CURABLE COMPOSITION AND ORGANIC EL DISPLAY DEVICE

A curable composition with controlled dielectric constant and hysteresis loss addresses durability issues in organic EL display devices, improving their long-term performance by reducing electric field-induced distortion.

JP7590556B2Active Publication Date: 2024-11-26MITSUI CHEMICALS INC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023517476
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-04-28
Filing Date
2022-04-21
Publication Date
2024-11-26
Estimated Expiration
2042-04-21

AI Technical Summary

Technical Problem

Existing organic EL display devices face durability issues during long-term use due to degradation from moisture and oxygen, necessitating improved sealing materials.

Method used

A liquid curable composition is developed with specific components and properties, including a dielectric constant of 3.6 or less and hysteresis loss between 0% and 45%, using polymerizable compounds, photopolymerization initiators, and optional leveling agents, to enhance the durability of the sealing layer.

Benefits of technology

The composition improves the durability of organic EL display devices by reducing susceptibility to electric field distortion and enhancing long-term sealing properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007590556000008
    Figure 0007590556000008
  • Figure 0007590556000009
    Figure 0007590556000009
  • Figure 0007590556000010
    Figure 0007590556000010
Patent Text Reader

Abstract

Provided is a liquid curable composition used in the sealing of an organic EL element. The liquid curable composition includes (a) a polymerizable compound and (b) a polymerization initiator. A cured product of the curable composition cured under UV-LEDs having a wavelength of 395 nm, at an illuminance of 1500 mW / cm2 and a cumulative amount of light of 1500 mJ / cm2, has a dielectric constant at a frequency of 100 kHz of 3.6 or less. The hysteresis loss of a sample obtained as the cured product of the curable composition is 0% or more and 45% or less.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a curable composition and an organic electroluminescence display device. [Background technology]

[0002] Because of their low power consumption, organic EL elements are beginning to be used in displays, lighting devices, etc. Because organic EL elements are susceptible to deterioration due to moisture and oxygen in the air, it is being considered to use them sealed with a sealant.

[0003] Patent Document 1 (WO 2015 / 129670) describes a curable resin composition for encapsulating organic electroluminescence display elements, which contains a cycloalkene oxide-type alicyclic epoxy compound, a phenoxy resin, and a curing agent, and it is said that such a composition can give a cured product that is excellent in transparency, flexibility, and barrier properties. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2015 / 129670 Summary of the Invention [Problem to be solved by the invention]

[0005] However, after the inventors of the present invention have studied the technology described in Patent Document 1, it has become clear that there is room for improvement in the technology in terms of improving the durability of an organic EL display device when used for a long period of time. [Means for solving the problem]

[0006] The present inventors have conducted extensive research to improve the durability of organic EL display devices when used for a long period of time, and have found that the above-mentioned problems can be solved by forming a composition used for sealing an organic EL element into a liquid curable composition containing specific components and configuring the composition so that the dielectric constant and hysteresis loss are within specific ranges. That is, the present inventors have found that in a liquid curable composition containing specific components, the dielectric constant and hysteresis loss are effective design guidelines for improving the durability of organic EL display devices during long-term use, and have arrived at the present invention.

[0007] That is, according to the present invention, there are provided the following curable composition and organic EL display device. [1] A liquid curable composition for use in encapsulating an organic electroluminescence device, comprising: The following components (a) and (b): (a) polymerizable compound, (b) Polymerization initiator Including, UV-LED with wavelength of 395 nm and illuminance of 1500 mW / cm 2 , cumulative light intensity 1500mJ / cm 2 the dielectric constant of the cured product of the curable composition cured by the method is 3.6 or less at a frequency of 100 kHz, A curable composition, wherein a sample obtained under the following condition 1 has a hysteresis loss of 0% or more and 45% or less when measured under the following condition 2. (Condition 1) The curable composition is sealed between two pieces of glass sandwiching a 100 μm thick Teflon (registered trademark) sheet, and is irradiated with a UV-LED having a wavelength of 395 nm at an illuminance of 1000 mW / cm 2 , cumulative light intensity 1500mJ / cm 2 The cured product obtained by curing at the above temperature is cut into a size of 10 mm wide x 55 mm long, and the cured product having a thickness of 90 to 110 μm at a total of 5 points every 10 mm in the length direction is used as the sample. (Condition 2) One end of the sample is fixed, and the other end is fixed so that the chuck distance is 30 mm. At this time, the state in which the sample is not attached is set to 0 mN, and in order to eliminate the initial strain, the load is pulled until it reaches 0.05 N, and this point is set as the starting point. In a curve (stress-strain curve) in which the stress when a tensile test is performed in which the other end is pulled in a 180-degree direction at 23°C and 10 mm / sec (pulling speed) is taken as the vertical axis and the strain as the horizontal axis, A is the area of ​​the region enclosed by the vertical axis, the straight line of ``strain = 2%'', and the horizontal axis in graph 1 from the starting point of the tensile test to 2% elongation, and B is the area of ​​the region enclosed by the straight line of ``strain = 2%'', and the horizontal axis in graph 2 from 2% elongation to when the stress becomes zero, and the solution calculated by {(AB) / A} x 100 is the hysteresis loss. [2] The curable composition according to [1], wherein the component (a) comprises one or more compounds selected from the group consisting of a (meth)acrylic compound having two (meth)acrylic groups in one molecule, an epoxy compound having two epoxy groups in one molecule, and an oxetane compound having two oxetanyl groups in one molecule. [3] The curable composition according to [1] or [2], wherein the component (a) comprises two or more compounds selected from the group consisting of a (meth)acrylic compound having two (meth)acrylic groups in one molecule, an epoxy compound having two epoxy groups in one molecule, and an oxetane compound having two oxetanyl groups in one molecule. [4] The curable composition according to any one of [1] to [3], wherein the component (b) is a photocationic polymerization initiator. [5] The curable composition according to any one of [1] to [3], wherein the component (b) is a photoradical polymerization initiator. [6] The curable composition according to any one of [1] to [5], further comprising a component (c): a leveling agent. [7] The curable composition according to [6], wherein the component (c) is an acrylic leveling agent. [8] The curable composition according to any one of [1] to [7], wherein the viscosity of the curable composition measured at 25°C and 20 rpm using an E-type viscometer is 3 mPa s or more and 50 mPa s or less. [9] The curable composition according to any one of [1] to [8], wherein the component (a) contains two or more types of (meth)acrylic compounds having two (meth)acrylic groups in one molecule.

[10] A substrate; An organic electroluminescence element disposed on the substrate; a sealing layer that covers the organic EL element; wherein the sealing layer is formed from a cured product of the curable composition according to any one of [1] to [9]. Effect of the Invention

[0008] According to the present invention, it is possible to provide a technique for improving the durability of an organic EL display device during long-term use. [Brief description of the drawings]

[0009] [Figure 1] 1 is a cross-sectional view showing a configuration example of an organic EL display device according to an embodiment. [Diagram 2] FIG. 2 is a diagram illustrating an example of a stress-strain curve according to an embodiment. [Diagram 3] FIG. 2 is a top view for explaining a method for evaluating bending resistance in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In all drawings, similar components are given similar symbols and their explanations are omitted as appropriate. In the present embodiment, each component may be used alone or in combination of two or more. In the present specification, the symbol "to" indicating a numerical range includes both the lower limit and the upper limit.

[0011] (Curable composition) In this embodiment, the curable composition is a liquid composition used for sealing an organic EL device, and contains the following components (a) and (b): (a) Polymerizable compound (b) Polymerization initiator In addition, the curable composition was irradiated with a UV-LED having a wavelength of 395 nm and an illumination intensity of 1500 mW / cm 2 , cumulative light intensity 1500mJ / cm 2 The dielectric constant of the cured product at a frequency of 100 kHz is 3.6 or less. Furthermore, a sample obtained using the curable composition under the following condition 1 has a hysteresis loss measured under the following condition 2 of 0% or more and 45% or less. (Condition 1) The curable composition was sealed between two pieces of glass sandwiching a 100 μm thick Teflon (registered trademark) sheet, and irradiated with a UV-LED having a wavelength of 395 nm at an illuminance of 1000 mW / cm 2 , cumulative light intensity 1500mJ / cm 2 The cured product obtained by curing at the above temperature is cut into a size of 10 mm width x 55 mm length, and the cured product having a thickness of 90 to 110 μm at a total of 5 points every 10 mm in the length direction is used as a sample. (Condition 2) One end of the sample is fixed, and the other end is fixed so that the chuck distance is 30 mm. The state in which the sample is not attached is set to 0 mN, and in order to eliminate the initial strain, the load is pulled until it reaches 0.05 N, and this point is set as the starting point. A tensile test is performed by pulling the other end in a 180-degree direction at 23°C and 10 mm / sec (pulling speed), and in the curve (stress-strain curve) with the stress on the vertical axis and the strain on the horizontal axis, A is the area of ​​the region enclosed by the vertical axis, the straight line of ``strain = 2%'', and the horizontal axis of graph 1 from the start of the tensile test to 2% elongation, and B is the area of ​​the region enclosed by the straight line of ``strain = 2%'', and the horizontal axis of graph 2 from 2% elongation to when the stress becomes zero, and the solution calculated by {(AB) / A} x 100 is the hysteresis loss.

[0012] As described above, the present inventors have found that the dielectric constant and hysteresis loss of a cured product of a liquid curable composition containing components (a) and (b) are effective design guidelines for realizing an encapsulant capable of improving the durability of an organic EL display device during long-term use. Based on the above findings, the present inventors have further studied the matter and found that an encapsulant capable of improving the durability of an organic EL display device during long-term use can be realized by using a curable composition having a dielectric constant of 3.6 or less and a hysteresis loss of 0% or more and 45% or less. The reason why the use of such a curable composition can improve the durability of an organic EL display device during long-term use is not necessarily clear, but it is thought that this is because the composition is less susceptible to the effects of the electric field of the organic EL element and the resin is less likely to return to its original shape, making it more susceptible to distortion.

[0013] The dielectric constant of the cured product of the curable composition is 3.6 or less, for example, 1.0 or more and 3.6 or less, preferably 1.0 or more and 3.5 or less, and more preferably 1.0 or more and 3.3 or less, from the viewpoint of improving the sealing properties of the sealing material. Here, the dielectric constant of the cured product is 1500mW / cm irradiance with a UV-LED of 395nm wavelength. 2 , cumulative light intensity 1500mJ / cm 2 The dielectric constant is measured at a frequency of 100 kHz for a cured product obtained by curing the curable composition under the above conditions.

[0014] From the viewpoint of improving the long-term durability of the encapsulant, the hysteresis loss of the cured product of the curable composition is 0% or more and 45% or less, preferably 0% or more and 40% or less, more preferably 0% or more and 35% or less, even more preferably 0% or more and 25% or less, and even more preferably 0% or more and 20% or less. The hysteresis loss of the cured product of the curable composition may be, for example, 5% or more.

[0015] Here, the hysteresis loss of the cured product of the curable composition is obtained by measuring a sample obtained under the above-mentioned condition 1 using the curable composition under the above-mentioned condition 2. In condition 1, the curable composition is first sealed between two pieces of glass sandwiching a 100 μm-thick Teflon (registered trademark) sheet. Then, the composition is irradiated with a UV-LED having a wavelength of 395 nm and an illuminance of 1000 mW / cm. 2 , cumulative light intensity 1500mJ / cm 2 The composition is cured at 40° C. to obtain a cured product having a thickness of approximately 100 μm. The obtained cured product is cut into a size of 10 mm wide x 55 mm long. Among the cut cured products, those having thicknesses of 90 to 110 μm at five points every 10 mm in the length direction are used as samples for measuring hysteresis loss.

[0016] The hysteresis loss is measured based on condition 2. For the measurement, a device capable of performing a tensile test, such as a universal material testing machine, can be used. One end of the sample is fixed to the chuck of the measuring device, and the other end is fixed so that the chuck distance is 30 mm. A tensile test is performed by pulling the other end in a 180 degree direction at 23°C and 10 mm / sec (tensile speed), and a curve (stress-strain curve) is obtained with stress on the vertical axis and strain on the horizontal axis. The state in which the sample is not attached to anything is set to 0 mN, and in order to eliminate the initial strain, the sample is pulled until the load reaches 0.05 N, and this point is set as the starting point. In other words, at the starting point, the strain is 0 mm and the load is 0.05 N. Here, the strain is ((pulling distance) / (chuck distance)). The chuck distance indicates the chuck distance at the starting point, and the pulling distance indicates the distance pulled in the 180 degree direction from the starting point. FIG. 2 is a diagram showing a schematic example of a stress-strain curve. In the stress-strain curve obtained from the tensile test, graph 1 from the start of the tensile test to 2% elongation is defined as A, and graph 2 is defined as the area enclosed by the vertical axis, the straight line of "strain = 2%", and the horizontal axis from 2% elongation until the stress becomes zero. Then, graph 2 is defined as the area enclosed by the straight line of "strain = 2%" and the horizontal axis, and hysteresis loss is calculated using the following formula. Hysteresis loss = {(AB) / A} x 100

[0017] In this embodiment, in order to adjust the dielectric constant and hysteresis loss of the cured product of the curable composition to be within the above-mentioned ranges, it is necessary to highly control, for example, the types and content ratios of components (a) and (b), the production method of the curable composition, etc. Among them, in the present embodiment, for example, one or more compounds selected from the group consisting of a (meth)acrylic compound having two or more (meth)acrylic groups in one molecule, an epoxy compound having two or more epoxy groups in one molecule, and an oxetane compound having two or more oxetanyl groups in one molecule are used as component (a); As component (b), for example, a photocationic polymerization initiator is used; adjusting the ratio of components (a) and (b); Adjusting the viscosity of the curable composition; Materials other than the polymerization initiator are heated and stirred under reduced pressure, for example at a temperature of 40°C or higher, and then the polymerization initiator is added; In obtaining a cured product of the curable composition, the oxygen concentration is adjusted during film formation (e.g., coating) and curing of the curable composition; These are examples of factors for controlling the dielectric constant and hysteresis loss of the cured product of the curable composition within the above-mentioned ranges. Among these, when preparing the curable composition, mixing and stirring are performed under reduced pressure, for example, at 200 Pa, and at a temperature of, for example, 40°C or higher. If the mixture is not stirred under reduced pressure, oxygen in the gas dissolves in the liquid, and the oxygen concentration in the liquid becomes high, so that desirable curing characteristics may not be obtained. Also, if the temperature is too low, oxygen in the liquid is difficult to remove, so that desirable curing characteristics may not be obtained. Furthermore, from the viewpoint of improving the reliability of the cured product during long-term use, coating for film formation is performed in an atmosphere with an oxygen concentration of, for example, 20.0 to 21.1%, and curing is performed, for example, in UV curing, at an oxygen concentration of 50 ppm to 1000 ppm.

[0018] In the present embodiment, the curable composition is preferably a sealant used for coating, and more preferably a sealant used for coating by an inkjet method. The viscosity of the curable composition, measured using an E-type viscometer at 25°C and 20 rpm, is preferably 3 mPa·s or more, more preferably 5 mPa·s or more, even more preferably 8 mPa·s or more, and still more preferably 10 mPa·s or more, from the viewpoint of improving inkjet dischargeability. From the viewpoint of improving the inkjet ejection properties, the viscosity of the curable composition is preferably 50 mPa·s or less, more preferably 30 mPa·s or less, even more preferably 27 mPa·s or less, and even more preferably 25 mPa·s or less.

[0019] Next, the components of the curable composition will be described with specific examples.

[0020] (Component (a)) Component (a) is a polymerizable compound. Specific examples of component (a) include compounds having a radically polymerizable functional group such as a (meth)acryloyl group or a vinyl group (hereinafter also referred to as "radical polymerizable compound"); Examples of the compound include compounds having a cationically polymerizable functional group such as an epoxy group, an oxetanyl group, or a vinyl ether group (hereinafter, also referred to as a "cationically polymerizable compound").

[0021] From the viewpoint of improving the durability of an organic EL display device during long-term use, component (a) preferably contains one or more compounds selected from the group consisting of a (meth)acrylic compound having two or more (meth)acrylic groups in one molecule, an epoxy compound having two or more epoxy groups in one molecule, and an oxetane compound having two or more oxetanyl groups in one molecule; more preferably contains one or more compounds selected from the group consisting of a (meth)acrylic compound having two (meth)acrylic groups in one molecule, an epoxy compound having two epoxy groups in one molecule, and an oxetane compound having two oxetanyl groups in one molecule; even more preferably contains two or more compounds selected from the group consisting of a (meth)acrylic compound having two (meth)acrylic groups in one molecule, an epoxy compound having two epoxy groups in one molecule, and an oxetane compound having two oxetanyl groups in one molecule, and even more preferably contains two or more compounds having two (meth)acrylic groups in one molecule. In this embodiment, (meth)acrylic means acrylic or methacrylic.

[0022] When component (a) is a radically polymerizable compound, the radically polymerizable compound is preferably a (meth)acrylic compound. The (meth)acrylic compound is preferably a (meth)acrylic compound having two or more (meth)acrylic groups in one molecule, and specific examples thereof include a di(meth)acrylic compound and a tri- or higher functional (meth)acrylic compound.

[0023] Specific examples of the di(meth)acrylic compound include one or more compounds selected from the group consisting of aliphatic di(meth)acrylic compounds and alicyclic di(meth)acrylic compounds. Examples of the aliphatic di(meth)acrylic compound include di(meth)acrylates of diols and di(meth)acrylates of (poly)alkylene glycols. More specifically, there are 1,6-hexanediol diacrylate (e.g., A-HD-N, manufactured by Shin-Nakamura Chemical Co., Ltd.), 1,9-nonanediol diacrylate (e.g., A-NOD-N, manufactured by Shin-Nakamura Chemical Co., Ltd.), 1,10-decanediol diacrylate (e.g., A-DOD-N, manufactured by Shin-Nakamura Chemical Co., Ltd.), neopentyl glycol diacrylate (e.g., A-NPG, manufactured by Shin-Nakamura Chemical Co., Ltd.), ethylene glycol diacrylate (e.g., SR206NS, manufactured by Arkema), polyethylene glycol diacrylate (e.g., A-400, manufactured by Shin-Nakamura Chemical Co., Ltd.), Examples of the dimethacrylate include polypropylene glycol diacrylate (e.g., APG-400, manufactured by Shin-Nakamura Chemical Co., Ltd.), tricyclodecane dimethanol diacrylate (e.g., A-DCP), 1,3-butanediol dimethacrylate (e.g., BG, manufactured by Shin-Nakamura Chemical Co., Ltd.), 1,4-butanediol dimethacrylate (e.g., BD, manufactured by Shin-Nakamura Chemical Co., Ltd.), 1,6-hexanediol dimethacrylate (e.g., HD-N, manufactured by Shin-Nakamura Chemical Co., Ltd.), 1,9-nonanediol dimethacrylate (e.g., NOD-N, manufactured by Shin-Nakamura Chemical Co., Ltd.), 1,10-decanediol dimethacrylate (e.g., DOD-N, manufactured by Shin-Nakamura Chemical Co., Ltd.), and neopentyl glycol dimethacrylate (e.g., NPG, manufactured by Shin-Nakamura Chemical Co., Ltd.). An example of the alicyclic di(meth)acrylic compound is dicyclopentanyl dimethacrylate (eg, DCP, manufactured by Shin-Nakamura Chemical Co., Ltd.).

[0024] From the viewpoint of maintaining a high crosslink density, the content of the di(meth)acrylic compound in the (meth)acrylic compound is preferably 50 parts by mass or more, more preferably 70 parts by mass or more, even more preferably 80 parts by mass or more, and even more preferably 90 parts by mass or more, when the total amount of the (meth)acrylic compound is 100 parts by mass. The content of the di(meth)acrylic compound in the (meth)acrylic compound may be, for example, 100 parts by mass or less, or, for example, 95 parts by mass or less.

[0025] Specific examples of the trifunctional or higher polyfunctional (meth)acrylic compound include trifunctional (meth)acrylic compounds such as trimethylolpropane triacrylate (e.g., A-TMPT, manufactured by Shin-Nakamura Chemical Co., Ltd.), ethoxylated trimethylolpropane triacrylate (e.g., A-TMPT-EO, manufactured by Shin-Nakamura Chemical Co., Ltd.), ethoxylated glycerin triacrylate (e.g., A-GLY-6E, manufactured by Shin-Nakamura Chemical Co., Ltd.), and propoxylated glycerin triacrylate (e.g., A-GLY-3P, manufactured by Shin-Nakamura Chemical Co., Ltd.); tetrafunctional (meth)acrylic compounds such as pentaerythritol tetraacrylate (e.g., A-TMMT, manufactured by Shin-Nakamura Chemical Co., Ltd.), ethoxylated pentaerythritol tetraacrylate (e.g., ATM-4E, manufactured by Shin-Nakamura Chemical Co., Ltd.), and ditrimethylolpropane tetraacrylate (e.g., AD-TMP-L, manufactured by Shin-Nakamura Chemical Co., Ltd.); Pentafunctional aliphatic acrylate compounds such as dipentaerythritol pentaacrylate (e.g., M-402, manufactured by Toagosei Co., Ltd.); and Examples of the compound include hexafunctional (meth)acrylic compounds such as dipentaerythritol pentahexaacrylate (for example, GM66G0H, manufactured by Kokusei Chemical Industry Co., Ltd.). On the other hand, examples of monofunctional (meth)acrylic compounds include monofunctional aliphatic (meth)acrylic compounds such as isostearyl acrylate; and monofunctional aromatic (meth)acrylic compounds such as benzyl acrylate and ethoxylated o-phenylphenol acrylate.

[0026] From the viewpoint of improving curability, the (meth)acrylic compound having two or more (meth)acrylic groups in one molecule is preferably a di(meth)acrylate of an aliphatic diol having from 8 to 12 carbon atoms, and more preferably one or more selected from the group consisting of 1,9-nonanediol diacrylate, 1,10-decanediol diacrylate, 1,9-nonanediol dimethacrylate, and 1,10-decanediol dimethacrylate. From a similar viewpoint, it is also preferable that the (meth)acrylic compound having two or more (meth)acrylic groups in one molecule includes an aliphatic di(meth)acrylic compound and an alicyclic di(meth)acrylic compound, and more preferably includes one or more selected from the group consisting of 1,9-nonanediol diacrylate, 1,10-decanediol diacrylate, 1,9-nonanediol dimethacrylate, and 1,10-decanediol dimethacrylate, and dicyclopentanyl dimethacrylate. Furthermore, the content of the monofunctional acrylate compound in the (meth)acrylic compound is preferably 30 mass% or less, more preferably 20 mass% or less, more preferably 15 mass% or less, even more preferably 12 mass% or less, even more preferably 8 mass% or less, even more preferably 5 mass% or less, and even more preferably 2 mass% or less, based on the total amount of the (meth)acrylic compound, and it is particularly preferable that the (meth)acrylic compound does not contain a monofunctional acrylate compound.

[0027] When component (a) is a cationically polymerizable compound, component (a) is preferably at least one selected from the group consisting of epoxy compounds and oxetane compounds, and more preferably an epoxy compound or an oxetane compound.

[0028] The epoxy compound is preferably an epoxy compound having two or more epoxy groups in one molecule, and specific examples thereof include difunctional epoxy compounds and trifunctional or higher epoxy compounds.

[0029] Specific examples of the difunctional epoxy compound include a difunctional alicyclic epoxy compound and a difunctional aliphatic epoxy compound. As the difunctional alicyclic epoxy compound, an alicyclic epoxy compound having a cycloalkene oxide structure is preferable.

[0030] An example of an alicyclic epoxy compound having a cycloalkene oxide structure is a compound represented by the following general formula (1).

[0031] [ka]

[0032] In the above general formula (1), X is a single bond or a linking group. The linking group can be, for example, a divalent hydrocarbon group, a carbonyl group, an ether group (ether bond), a thioether group (thioether bond), an ester group (ester bond), a carbonate group (carbonate bond), an amide group (amide bond), or a group in which a plurality of these are linked together.

[0033] Among X, examples of the divalent hydrocarbon group include an alkylene group having 1 to 18 carbon atoms and a divalent alicyclic hydrocarbon group. Examples of the alkylene group having 1 to 18 carbon atoms include a methylene group, a methylmethylene group, a dimethylmethylene group, an ethylene group, a propylene group, and a trimethylene group. Examples of the divalent alicyclic hydrocarbon group include a divalent cycloalkylene group (including a cycloalkylidene group) such as a 1,2-cyclopentylene group, a 1,3-cyclopentylene group, a cyclopentylidene group, a 1,2-cyclohexylene group, a 1,3-cyclohexylene group, a 1,4-cyclohexylene group, and a cyclohexylidene group.

[0034] Among the above, X is preferably a single bond or a linking group having an oxygen atom. The linking group having an oxygen atom is more preferably -CO- (carbonyl group), -O-CO-O- (carbonate group), -COO- (ester group), -O- (ether group), -CONH- (amide group), a group in which a plurality of these groups are linked, or a group in which one or more of these groups are linked to one or more divalent hydrocarbon groups. X is even more preferably a single bond.

[0035] Examples of epoxy compounds represented by general formula (1) are shown below. In the following formula, l represents an integer of 1 to 10, and m represents an integer of 1 to 30. R represents an alkylene group having 1 to 8 carbon atoms (preferably an alkylene group having 1 to 3 carbon atoms, such as a methylene group, an ethylene group, a propylene group, or an isopropylene group).

[0036] [ka]

[0037] [ka]

[0038] Commercially available alicyclic epoxy compounds having a cycloalkene oxide structure include, for example, Celloxide 2021P (3',4'-epoxycyclohexylmethyl 3,4-epoxycyclohexanecarboxylate), Celloxide 2081 (ε-caprolactone-modified 3',4'-epoxycyclohexylmethyl 3,4-epoxycyclohexanecarboxylate), Celloxide 8000, and Celloxide 8010 (all manufactured by Daicel Corporation).

[0039] Examples of bifunctional aliphatic epoxy compounds include neopentyl glycol diglycidyl ether (e.g., NPG(D), manufactured by Yokkaichi Chemical Co., Ltd.), 1,6-hexanediol diglycidyl ether (e.g., ED-503, manufactured by ADEKA Corporation), propylene glycol diglycidyl ether (e.g., SR-PG, manufactured by Sakamoto Pharmaceutical Co., Ltd.), and hydrogenated bisphenol A diglycidyl ether (e.g., EX252, manufactured by Nagase ChemteX Corporation). Specific examples of trifunctional or higher epoxy compounds include polyfunctional epoxy compounds such as trimethylolpropane polyglycidyl ether (eg, EX-321L, manufactured by Nagase ChemteX Corporation) and diglycerol polyglycidyl ether (eg, EX-421, manufactured by Nagase ChemteX Corporation).

[0040] From the viewpoint of improving curability, the epoxy compound having two or more epoxy groups in one molecule is preferably one or more selected from the group consisting of the compound in which X is a single bond in the above general formula (1), 3',4'-epoxycyclohexylmethyl 3,4-epoxycyclohexanecarboxylate, and neopentyl glycol diglycidyl ether.

[0041] From the viewpoint of increasing the initial reaction rate, the content of the epoxy compound in the cationic polymerizable compound is preferably 5 parts by mass or more, more preferably 15 parts by mass or more, and even more preferably 25 parts by mass or more, relative to 100 parts by mass of the entire cationic polymerizable compound. In addition, from the viewpoint of increasing the elongation reaction rate, the content of the epoxy compound in the cationic polymerizable compound is, for example, 100 parts by mass or less, preferably 50 parts by mass or less, more preferably 40 parts by mass or less, and even more preferably 30 parts by mass or less, relative to 100 parts by mass of the entire cationic polymerizable compound.

[0042] Next, the oxetane compound will be described. The oxetane compound is preferably an oxetane compound having two or more oxetanyl groups in one molecule, more preferably a bifunctional oxetane compound, and even more preferably a bifunctional oxetane compound represented by the following general formula (6) or (7).

[0043] [ka]

[0044] In the general formulas (6) and (7), R 5 are each independently a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an allyl group, an aryl group, an aralkyl group, a furyl group, or a thienyl group, and are preferably an alkyl group having 1 to 6 carbon atoms. 6 is a divalent organic residue. In addition, in the general formula (7), u is a number of 1 to 5, and preferably a number of 1 to 3, on average.

[0045] R 5 Among these, specific examples of the alkyl group having 1 to 6 carbon atoms include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, and a cyclohexyl group. Specific examples of the aryl group include a phenyl group, a naphthyl group, a tolyl group, and a xylyl group. Specific examples of the aralkyl group include a benzyl group and a phenethyl group.

[0046] Also, R 6 Specific examples of the alkylene group include an alkylene group, a polyoxyalkylene group, a phenylene group, a xylylene group, and a structure represented by the following general formula:

[0047] [ka]

[0048] In the above general formula, R 3 is an oxygen atom, a sulfur atom, -CH2-, -NH-, -SO-, -SO2-, -C(CF3)2- or -C(CH3)2-. Also, R 4 is an alkylene group or arylene group having 1 to 6 carbon atoms. Specific examples of the alkylene group having 1 to 6 carbon atoms include a methylene group, an ethylene group, a propylene group, a butylene group, and a cyclohexylene group.

[0049] Also, R 6 Among these, the number of carbon atoms in the polyoxyalkylene group is preferably 4 to 30, and more preferably 4 to 8. Specific examples of the polyoxyalkylene group include a polyoxyethylene group and a polyoxypropylene group.

[0050] A specific example of the compound shown in general formula (6) is 3-ethyl-3{[(3-ethyloxetan-3-yl)methoxy]methyl}oxetane (e.g., OXT-221, manufactured by Toagosei Co., Ltd.). A specific example of the compound shown in general formula (7) is a bifunctional oxetanyl compound such as xylylene bisoxetane (e.g., OXT121, manufactured by Toagosei Co., Ltd., u=1 to 3 in general formula (7)). From the viewpoint of improving curability, the oxetane compound having two or more oxetanyl groups in one molecule is preferably 3-ethyl-3{[(3-ethyloxetan-3-yl)methoxy]methyl}oxetane.

[0051] The oxetane compound may include a monofunctional oxetane compound, for example, a monofunctional aliphatic oxetane compound such as 3-ethyl-3-[(2-ethylhexyloxy)methyl]oxetane.

[0052] From the viewpoint of reducing the dielectric constant of the cured product of the curable composition, the content of the oxetane compound in the cationically polymerizable compound is preferably 30 parts by mass or more, more preferably 50 parts by mass or more, and even more preferably 70 parts by mass or more, based on 100 parts by mass of the entire cationically polymerizable compound. From the same viewpoint, the content of the oxetane compound in the cationically polymerizable compound is, for example, 100 parts by mass or less, preferably 95 parts by mass or less, more preferably 90 parts by mass or less, and even more preferably 85 parts by mass or less, when the total amount of the cationically polymerizable compound is 100 parts by mass.

[0053] From the viewpoint of improving the durability of an organic EL display device during long-term use, component (a) preferably contains one or more selected from the group consisting of a compound in which X is a single bond in the above general formula (1), neopentyl glycol diglycidyl ether, 3',4'-epoxycyclohexylmethyl 3,4-epoxycyclohexanecarboxylate, 3-ethyl-3{[(3-ethyloxetan-3-yl)methoxy]methyl}oxetane, 1,9-nonanediol diacrylate, 1,9-nonanediol dimethacrylate, and trimethylolpropane triacrylate, and more preferably contains one or more selected from the group consisting of 3-ethyl-3{[(3-ethyloxetan-3-yl)methoxy]methyl}oxetane, 1,9-nonanediol diacrylate, and 1,9-nonanediol dimethacrylate.

[0054] In addition, component (a) may contain one or more compounds selected from the group consisting of monofunctional (meth)acrylate compounds, monofunctional epoxy compounds, and monofunctional oxetane compounds. From the viewpoint of improving the durability of the encapsulant during long-term use, the curable composition preferably contains one or more compounds selected from the group consisting of monofunctional (meth)acrylate compounds and monofunctional oxetane compounds.

[0055] From the viewpoint of improving the strength of the cured product, the content of component (a) in the curable composition is preferably 60 to 99.9 mass%, more preferably 80 to 99.9 mass%, even more preferably 85 to 99.9 mass%, still more preferably 90 to 99.9 mass%, and even more preferably 90 to 98.0 mass%, based on the total composition of the curable composition.

[0056] (ingredient (b)) Component (b) is a polymerization initiator. Specific examples of the polymerization initiator include one or more selected from the group consisting of thermal radical initiators and photopolymerization initiators. From the viewpoint of stably forming a cured product at low temperatures, component (b) contains a polymerization initiator that generates radicals or ions when irradiated with light such as ultraviolet light (a photoradical polymerization initiator such as a UV radical initiator or a photocationic polymerization initiator such as a UV cationic initiator), and is more preferably a photocationic polymerization initiator.

[0057] Specific examples of photocationic polymerization initiators include aromatic sulfonium salts, aromatic iodonium salts, aromatic diazonium salts, aromatic ammonium salts, etc., from the viewpoint of stably forming a cured product. The anion portion of these salts is, for example, BF4 - , (R f ) n PF 6-n (R f is an organic group, and n is an integer of 1 to 5.) PF6 - , SbF6 - , or BY4 - (Y is a phenyl group substituted with at least two fluorine or trifluoromethyl groups.)

[0058] Specific examples of aromatic sulfonium salts include bis[4-(diphenylsulfonio)phenyl]sulfide bishexafluorophosphate, bis[4-(diphenylsulfonio)phenyl]sulfide bishexafluoroantimonate, bis[4-(diphenylsulfonio)phenyl]sulfide bistetrafluoroborate, bis[4-(diphenylsulfonio)phenyl]sulfide tetrakis(pentafluorophenyl)borate, diphenyl-4-(phenylthio)phenylsulfonium hexafluorophosphate, diphenyl-4-(phenylthio)phenylsulfonium hexafluoroantimonate, and diphenyl-4-(phenylthio)phenylsulfonium tetrafluoroborate.

[0059] Specific examples of aromatic iodonium salts include diphenyliodonium hexafluorophosphate, diphenyliodonium hexafluoroantimonate, diphenyliodonium tetrafluoroborate, diphenyliodonium tetrakis(pentafluorophenyl)borate, bis(dodecylphenyl)iodonium hexafluorophosphate, bis(dodecylphenyl)iodonium hexafluoroantimonate, bis(dodecylphenyl)iodonium tetrafluoroborate, and bis(dodecylphenyl)iodonium tetrakis(pentafluorophenyl)borate.

[0060] Specific examples of aromatic diazonium salts include phenyldiazonium hexafluorophosphate, phenyldiazonium hexafluoroantimonate, phenyldiazonium tetrafluoroborate, and phenyldiazonium tetrakis(pentafluorophenyl)borate.

[0061] Specific examples of aromatic ammonium salts include 1-benzyl-2-cyanopyridinium hexafluorophosphate, 1-benzyl-2-cyanopyridinium hexafluoroantimonate, and the like.

[0062] Specific examples of commercially available photocationic polymerization initiators include Irgacure 250, Irgacure 270, Irgacure 290 (all manufactured by BASF), CPI-100P, CPI-101A, CPI-200K, CPI-210S, CPI-310B, CPI-400PG (all manufactured by San-Apro), SP-150, SP-170, SP-171, SP-056, SP-066, SP-130, SP-140, SP-601, SP-606, SP-701 (all manufactured by ADEKA). From the viewpoint of stably obtaining a cured film, the photocationic polymerization initiator is preferably a sulfonium salt such as Irgacure270, Irgacure290, CPI-100P, CPI-101A, CPI-200K, CPI-210S, CPI-310B, CPI-400PG, SP-150, SP-170, SP-171, SP-056, SP-066, SP-601, SP-606, or SP-701.

[0063] Specific examples of the photoradical polymerization initiator include acylphosphine oxide photopolymerization initiators such as 2,4,6-trimethylbenzoyldiphenylphosphine oxide.

[0064] From the viewpoint of improving curability, the content of component (b) in the curable composition is preferably 0.1 mass % or more, more preferably 0.3 mass % or more, and even more preferably 0.5 mass % or more, based on the total composition of the curable composition. In addition, from the viewpoint of suppressing coloration of the curable composition, the content of component (b) in the curable composition is preferably 10 mass % or less, more preferably 6 mass % or less, and even more preferably 4 mass % or less, based on the total composition of the curable composition.

[0065] The curable composition may contain components other than components (a) and (b). For example, the curable composition may further contain component (c): a leveling agent.

[0066] (component (c)) When the curable composition contains the leveling agent as component (c), the flatness of the film formed from the curable composition can be improved. Specific examples of the component (c) include silicone-based leveling agents such as polyester-modified polydimethylsiloxane (e.g., BYK-310, manufactured by BYK-Chemie Japan) and polyether-modified siloxane (e.g., BYK-345, manufactured by BYK-Chemie Japan); Acrylic leveling agents such as acrylic copolymers (e.g., BYK-350, manufactured by BYK Japan; KL700, manufactured by Kyoeisha Chemical Co., Ltd.); Examples of the fluorine-based leveling agent include fluorine-modified polymers (e.g., BYK-340, manufactured by BYK Japan Co., Ltd.) and perfluoroalkyl-containing oligomers (e.g., Surflon S-611 (manufactured by AGC Seimi Chemical Co., Ltd.)).

[0067] From the viewpoint of improving the flatness when the curable composition is applied to inkjet printing, component (c) is preferably one or more types selected from the group consisting of acrylic copolymers, polyester-modified polydimethylsiloxanes, and fluorine-modified polymers. From the same viewpoint, it is also preferred that component (c) is an acrylic leveling agent.

[0068] From the viewpoint of improving the flatness of the film formed by the curable composition, the content of component (c) in the curable composition is preferably 0.01 mass % or more, more preferably 0.03 mass % or more, and even more preferably 0.05 mass % or more, based on the total composition of the curable composition. In addition, from the viewpoint of stabilizing the surface hardness of the cured product, the content of component (c) in the curable composition is preferably 5 mass % or less, more preferably 3 mass % or less, and even more preferably 2 mass % or less, based on the total composition of the curable composition.

[0069] Examples of other components in the curable composition include a tackifier, a sensitizer, and a coupling agent such as a silane coupling agent.

[0070] For example, by including a tackifier in the curable composition, the viscosity of the curable composition can be adjusted, for example, preferably increased, without significantly changing the dielectric constant of the cured product of the curable composition. Specific examples of tackifiers include one or more selected from the group consisting of petroleum resins such as aliphatic hydrocarbon resins, alicyclic hydrocarbon resins, and aromatic hydrocarbon resins; terpene resins; phenols such as phenolic resins; and rosin resins.

[0071] As petroleum resins, for example, C5 monomers or oligomers thereof obtained from pentene, pentadiene, isoprene, etc.; C9 monomers or oligomers thereof derived from indene, methylindene, vinyltoluene, styrene, α-methylstyrene, β-methylstyrene, etc.; Copolymers of C5 and C9 monomers (C5-C9 copolymer resins); Alicyclic monomers or polymers thereof obtained from cyclopentadiene, dicyclopentadiene, etc.; Aromatic monomers or polymers thereof, such as isopropenyl toluene; Hydrogenated products of the above-mentioned various monomers or their polymers; Examples of the modified petroleum resins include those obtained by modifying the above-mentioned various monomers or their polymers with maleic anhydride, maleic acid, fumaric acid, (meth)acrylic acid, phenol, or the like. From the viewpoint of excellent compatibility with component (a), the petroleum resin used as a tackifier is preferably a styrene-based oligomer. From the same viewpoint, it is also preferable that component (a) is a petroleum resin produced from dicyclopentadiene as a main raw material, and more preferably a petroleum resin produced from dicyclopentadiene as a main raw material and having an ester group in the molecule (e.g., QTN1500, manufactured by Zeon Corporation).

[0072] Examples of the terpene resin include α-pinene resin, β-pinene resin, α-pinene monomer, and aromatic modified terpene resin obtained by copolymerizing terpenes such as β-pinene monomer with an aromatic monomer such as styrene.

[0073] Specific examples of phenols include phenol compounds such as phenol, m-cresol, 3,5-xylenol, p-alkylphenol, and resorcinol. Specific examples of phenolic resins include resols obtained by addition reaction of these phenolic compounds with formaldehyde using an alkali catalyst, novolacs obtained by condensation reaction using an acid catalyst, etc. The phenolic resin also includes rosin phenolic resins obtained by adding phenol to rosin using an acid catalyst and thermally polymerizing the resulting mixture.

[0074] Examples of rosin resins include gum rosin, wood rosin, or tall oil rosin, stabilized rosins or polymerized rosins obtained by disproportionating or hydrogenating these rosins, modified rosins obtained by modifying these rosins with maleic anhydride, maleic acid, fumaric acid, (meth)acrylic acid, phenol, or the like, and esters thereof. The alcohol used to obtain the esters is preferably a polyhydric alcohol. Examples of polyhydric alcohols include dihydric alcohols such as ethylene glycol, diethylene glycol, propylene glycol, and neopentyl glycol; trihydric alcohols such as glycerin, trimethylolethane, and trimethylolpropane; tetrahydric alcohols such as pentaerythritol and diglycerin; and hexahydric alcohols such as dipentaerythritol.

[0075] From the viewpoint of obtaining a preferable viscosity of the curable composition, the content of the tackifier in the curable composition is preferably 1 mass % or more, more preferably 3 mass % or more, and even more preferably 5 mass % or more, relative to the total composition of the curable composition, and is preferably 30 mass % or less, more preferably 25 mass % or less, and even more preferably 20 mass % or less.

[0076] The curable composition may further include a sensitizer, such as a cationic photosensitizer. Specific examples of sensitizers include thioxanthone compounds such as 2,4-diethylthioxanthone, 2,2-dimethoxy-1,2-diphenylethan-1-one, benzophenone, 2,4-dichlorobenzophenone, methyl o-benzoylbenzoate, 4,4'-bis(dimethylamino)benzophenone, 4-benzoyl-4'-methyldiphenyl sulfide, and 9,10-dibutoxyanthracene.

[0077] From the viewpoint of improving the curability of the curable composition, the content of the sensitizer in the curable composition is preferably 0.01 mass % or more, more preferably 0.03 mass % or more, and even more preferably 0.05 mass % or more, based on the total composition of the curable composition. From the viewpoint of obtaining favorable visible light transmittance of the cured product, the content of the sensitizer in the curable composition is preferably 20 mass % or less, more preferably 10 mass % or less, even more preferably 5 mass % or less, and even more preferably 1 mass % or less.

[0078] Next, a method for producing the curable composition will be described. In the present embodiment, the method for producing the curable composition includes, for example, a step of obtaining a liquid curable composition by mixing components (a) and (b) and other components, and then curing the obtained curable composition to obtain a cured product. At this time, as described above, by highly controlling the types and content ratios of components (a) and (b), the manufacturing method of the curable composition, etc., the dielectric constant and hysteresis loss of the cured product of the curable composition can be stably adjusted within the above-mentioned range. For example, the curable composition can be obtained by mixing the above-mentioned components using a mixer such as a homodisper, homomixer, universal mixer, planetary mixer, kneader, or three-roll mixer. From the viewpoint of stably mixing the curable composition, it is more preferable to mix components other than component (b) and then mix component (b). It is also preferable to adjust the degree of vacuum when mixing and stirring the raw materials of the curable composition, the mixing temperature, and the oxygen concentration when obtaining the cured product. By such a method, the liquid can be adjusted uniformly, a cured product without unevenness can be obtained, and the dielectric constant and hysteresis loss of the cured product of the curable composition can be easily controlled within the above-mentioned range.

[0079] The curable composition obtained in this embodiment is suitably used for sealing, for example, a display device, preferably an organic EL display device. By using the cured product of the curable composition obtained in this embodiment as a sealant for a display device, preferably an organic EL display device, it is possible to obtain a display device that is excellent in durability when used for a long period of time. Below, an example of the configuration of a display device will be given, taking an organic EL display device as an example.

[0080] (Organic EL display device) In this embodiment, the organic EL display device has a layer constituted of a cured product of a curable composition. Fig. 1 is a cross-sectional view showing an example of the configuration of an organic EL display device in this embodiment. The display device 100 shown in Fig. 1 is an organic EL display device, and includes a substrate (base layer 50), an organic EL element (light-emitting element 10) disposed on the base layer 50, and a sealing layer 22 (which may be an overcoat layer 22 or a barrier layer 22) that covers the light-emitting element 10. For example, the sealing layer 22 is formed of a cured product of the curable composition in this embodiment. 1, the display device 100 has a barrier layer 21 (which may be a touch panel layer 21 or a surface protective layer 21), a sealing layer 22 (which may be an overcoat layer 22 or a barrier layer 22), a planarization layer 23 (which may be a sealing layer 23), and a barrier layer 24 as layers located closer to the observation side than the light-emitting element 10. The planarization layer 23 is provided on the base layer 50 so as to cover the light-emitting element 10, and the barrier layer 24 is provided on the surface of the planarization layer 23. The sealing layer 22 is provided on the base layer 50 so as to cover the planarization layer 23 and the barrier layer 24. In addition, the barrier layer 21 is provided on the sealing layer 22.

[0081] The specific configuration of each layer is not limited, and an appropriate configuration can be adopted based on generally known information. Moreover, such a display device 100 can be manufactured based on generally known information. EXAMPLES

[0082] EXAMPLES Hereinafter, the present invention will be described with reference to examples and comparative examples, but the present invention is not limited to these.

[0083] First, the materials used in the following examples are listed. ((a) Polymerizable compound) Polymerizable compound 1: Difunctional alicyclic epoxy compound, Celloxide CEL8010 (manufactured by Daicel Corporation, compound represented by the following formula (estimated))

[0084] [ka]

[0085] Polymerizable compound 2: Difunctional aliphatic epoxy compound, NPG(D), manufactured by Yokkaichi Synthetic Co., Ltd., neopentyl glycol diglycidyl ether Polymerizable compound 3: Bifunctional aliphatic oxetane compound, OXT221, manufactured by Toagosei Co., Ltd., 3-ethyl-3{[(3-ethyloxetan-3-yl)methoxy]methyl}oxetane Polymerizable compound 4: Difunctional alicyclic methacrylate compound, DCP, Shin-Nakamura Chemical Co., Ltd., dicyclopentanyl dimethacrylate Polymerizable compound 5: Difunctional aliphatic methacrylate compound, NOD-N, manufactured by Shin-Nakamura Chemical Co., Ltd., 1,9-nonanediol dimethacrylate Polymerizable compound 6: Difunctional aliphatic acrylate compound, A-NOD-N, manufactured by Shin-Nakamura Chemical Co., Ltd., 1,9-nonanediol diacrylate Polymerizable compound 7: Monofunctional aliphatic acrylate compound, manufactured by Shin-Nakamura Chemical Co., Ltd., isostearyl acrylate Polymerizable compound 8: Trifunctional aliphatic acrylate compound, A-TMPT, manufactured by Shin-Nakamura Chemical Co., Ltd., trimethylolpropane triacrylate Polymerizable compound 9: 5-functional aliphatic acrylate compound, M-402, manufactured by Toagosei Co., Ltd., dipentaerythritol pentaacrylate Polymerizable compound 10: Monofunctional aliphatic oxetane compound, OXT212, manufactured by Toagosei Co., Ltd., 3-ethyl-3-[(2-ethylhexyloxy)methyl]oxetane Polymerizable compound 11: Monofunctional aromatic acrylate compound, A-LEN-10, manufactured by Shin-Nakamura Chemical Co., Ltd., ethoxylated o-phenylphenol acrylate Polymerizable compound 12: Monofunctional aromatic acrylate compound, Viscoat 160, manufactured by Osaka Organic Chemical Industry Co., Ltd., benzyl acrylate ((b) Polymerization initiator) Polymerization initiator 1: Photocationic initiator, CPI210S, manufactured by San-Apro Co., Ltd. Polymerization initiator 2: Photoradical initiator, TPO, BASF, 2,4,6-trimethylbenzoyl-diphenyl phosphine oxide (c) Leveling agent Leveling agent 1: Acrylic copolymer, KL700, manufactured by Kyoeisha Chemical Co., Ltd. (Other ingredients) Other component 1 (tackifier): styrene oligomer (homopolymer of isopropenyl toluene (IPT) (styrene oligomer, weight average molecular weight: 1200, number average molecular weight: 800)) Other component 2 (photocationic sensitizer): 9,10-dibutoxyanthracene, UVS-1331, manufactured by Kawasaki Kasei Chemical Industries, Ltd.

[0086] (Examples 1 to 8, Comparative Examples 1 to 3) A liquid curable composition was obtained by mixing each component on a scale of 11 kg in total so as to obtain the composition shown in Table 1. At that time, all components except the polymerization initiator were mixed, the pressure in the system was reduced by a vacuum pump, and mixing and stirring were performed for 4 hours at 80°C under an atmosphere of reduced pressure of 190 Pa to 210 Pa, and after cooling to room temperature, the liquid was transferred to a tank containing the polymerization initiator by nitrogen extrusion to prevent oxygen from being mixed in, and mixing and stirring were performed for 1 hour at 40°C under an atmosphere of reduced pressure of 190 Pa to 210 Pa. In addition, coating for film formation was performed in an atmosphere with an oxygen concentration of 20.0 to 21.1%, and curing was performed at an oxygen concentration of 50 ppm to 1000 ppm during UV curing. The physical properties of the curable composition or the cured product thereof obtained in each example were measured by the following methods. The measurement results are shown in Table 1.

[0087] (Viscosity of Curable Composition) The viscosity of the curable composition obtained in each example was measured at 25° C. and 20 rpm using an E-type viscometer (LV-DV-II+, manufactured by BROOKFIELD Corporation). The evaluation criteria for the viscosity shown in Table 1 are as follows: A: 3mPa·s or more and 50mPa·s or less B: Less than 3 mPa s or more than 50 mPa s

[0088] (Hysteresis Loss of Cured Product of Curable Composition) A cured product of the curable composition was prepared according to the above-mentioned method, and the hysteresis loss was determined from the results of a tensile test on the cured product. That is, first, the curable composition was sealed between two pieces of glass sandwiching a 100 μm-thick Teflon (registered trademark) sheet (MSF-100, manufactured by Chukoh Chemical Industries, Ltd.). Then, the composition was irradiated with a UV-LED having a wavelength of 395 nm and an illuminance of 1000 mW / cm. 2 , cumulative light intensity 1500mJ / cm 2 The mixture was cured at 40° C. to obtain a cured product having a thickness of about 100 μm. The obtained cured product was cut into a size of 10 mm wide x 55 mm long. Of the cut cured products, those with thicknesses ranging from 90 to 110 μm at a total of five points every 10 mm in the length direction were used as samples for measuring hysteresis loss. One end of the sample was fixed to a chuck, and a tensile test was performed by pulling the other end in a 180 degree direction at 23°C and 10 mm / sec (pulling speed) using a universal material testing machine AG-X-Plus (Shimadzu Corporation). A curve (stress-strain curve) was obtained with stress on the vertical axis and strain on the horizontal axis. The state in which the sample was not attached was set to 0 mN, and the load was pulled until it reached 0.05 N to eliminate the initial strain, and this point was set as the starting point. Therefore, at the starting point, the strain was 0 mm and the load was 0.05 N. In the stress-strain curve, the area of ​​the region enclosed by the vertical axis, the straight line of ``strain = 2%'', and the horizontal axis from the start of the tensile test to 2% elongation was set as A, and the area of ​​the region enclosed by the vertical axis, the straight line of ``strain = 2%'', and the horizontal axis ... horizontal axis from 2% elongation to 0% elongation was set as Graph 2. The area of ​​the region enclosed by the line of "strain = 2%" and the horizontal axis was defined as B, and the hysteresis loss was calculated by the following formula. Hysteresis loss = {(AB) / A} x 100 The evaluation criteria for hysteresis loss shown in Table 1 are as follows. A: 0% or more and 45% or less B: More than 45%

[0089] (Dielectric constant of the cured product of the curable composition) A coating film for obtaining a cured product for measuring the dielectric constant was prepared by the following method. That is, the obtained curable composition was introduced into an inkjet cartridge DMC-11610 (manufactured by Fujifilm Dimatix). The inkjet cartridge was set in an inkjet device DMP-2831 (manufactured by Fujifilm Dimatix), and after adjusting the discharge state, the composition was applied to a substrate in which aluminum was vapor-deposited to a thickness of 100 nm on non-alkali glass, with a size of 5 cm x 5 cm, so that the thickness after curing was 10 μm. The oxygen concentration at this time was 20.6%. The resulting coating was left at room temperature (25°C) for 1 minute, and then exposed to a UV-LED with a wavelength of 395 nm and an illumination intensity of 1500 mW / cm 2 , cumulative light intensity 1500mJ / cm 2 The curing was carried out at an oxygen concentration of 1000 ppm or less. Then, aluminum was evaporated onto the inkjet coated surface to a thickness of 100 nm, and the dielectric constant was measured at 100 kHz using an LCR meter HP4284A (Agilent Technologies) by the automatic balancing bridge method. The evaluation criteria for the dielectric constants shown in Table 1 are as follows: A: 3.6 or less B: Over 3.6

[0090] In addition, the curable compositions obtained in each example were evaluated for flex resistance and EL element damage as indicators of long-term durability when used as encapsulants for display devices. The evaluation methods are as follows. The evaluation results are also shown in Table 1.

[0091] (Evaluation method) (Bending resistance) As an index of flex resistance, the haze after a 300,000-fold folding endurance test was evaluated by the following method. The curable composition obtained in each example was introduced into an inkjet cartridge DMC-11610 (manufactured by Fujifilm Dimatix). The inkjet cartridge was set into an inkjet device DMP-2831 (manufactured by Fujifilm Dimatix), and after adjusting the discharge state, it was applied to a 6 cm x 6 cm PET film (25 μm, A31) in a size of 5 cm x 5 cm so that the thickness after curing would be 10 μm. The oxygen concentration at this time was within the range of 20.0% to 21.1%. The obtained coating film was left at room temperature (25°C) for 1 minute, and then was exposed to a UV-LED with a wavelength of 395 nm at an illuminance of 1000 mW / cm. 2 , cumulative light intensity 1500mJ / cm 2 The curing was carried out at an oxygen concentration of 1000 ppm or less. The obtained cured product was used as a measurement sample to evaluate the bending resistance. FIG. 3 is a top view for explaining the method of evaluating bending resistance. The bending radius was set to 1 mm in a bending tester (DML HP, manufactured by Yuasa System Co., Ltd.), and the measurement sample (sample 31 in FIG. 3, arranged so that the PET film was on the lower surface and the cured film was on the upper surface) was fixed to a sample fixing plate 33 with double-sided tape 35 (Nistack NW-15, manufactured by Nichiban Co., Ltd.) as shown in FIG. 3, and a bending test was performed 300,000 times at a bending speed of 30 times per minute. After 1000 bendings, the appearance was visually confirmed within 10 minutes, and the presence or absence of cloudiness was evaluated. After 300,000 bendings, the appearance was visually confirmed within 10 minutes, and the presence or absence of cloudiness was evaluated. Those without cloudiness at the end of 1000 bendings (A and B below) were considered to have passed. The evaluation criteria are as follows: A: No cloudiness B: There was no cloudiness after 1,000 bending cycles, but there was cloudiness after 300,000 bending cycles. C: Cloudy after 1000 bending cycles

[0092] (EL element damage) As an index of damage to the EL element, the reliability of the organic EL display element was evaluated by the following method. The glass substrate on which the ITO electrode was formed was treated with a UV-ozone treatment device (PL21-200(S) / UVE-200J, manufactured by Sen Tokushu Genkougen Co., Ltd.), and then ultrasonically cleaned with an alkaline aqueous solution, pure water, acetone, and isopropyl alcohol for 15 minutes each, and finally ultrasonically cleaned with acetone for 10 minutes. Next, this substrate was fixed in a substrate holder of a vacuum deposition apparatus, 200 mg of Dipyrazino[2,3-f:2',3'-h]quinoxaline-2,3,6,7,10,11,hexacarbonitrile (HAT-CN) was placed in an unglazed crucible, and 200 mg of 9-Phenyl-3,6-bis(9-phenyl-9Hcarbazol-3-yl)-9H-carbazole (Tris-PCz) was placed in another unglazed crucible, and the inside of the vacuum chamber was heated to 1 × 10 -4The pressure was reduced to 1×10 Pa. The crucible containing HAT-CN was then heated, and HAT-CN was deposited on the substrate at a deposition rate of 0.4 Å / s to form a film with a thickness of 100 nm. Next, the crucible containing Tris-PCz was heated, and HAT-CN was deposited on the substrate at a deposition rate of 1.0 Å / s to form a film with a thickness of 400 nm. Next, 200 mg of Tris(8-hydroxyquinolinato)aluminium (Alq3) was placed in another unglazed crucible, and the vacuum chamber was again heated to 1×10 4 The pressure in the vacuum chamber was reduced to 1×10 Pa. Then, the crucible containing Alq3 (tris(8-quinolinolato)aluminum) was heated, and a 700 nm thick film was formed at a deposition rate of 0.5 Å / s. After that, 200 mg of lithium fluoride was placed in a tungsten resistance heating boat, and the vacuum chamber was heated to 1×10 -4 The pressure was reduced to 10 Pa, and lithium fluoride was deposited at a deposition rate of 0.03 Å / s to form a 5 nm film. Finally, 1 g of magnesium and 200 mg of silver were placed in a tungsten resistance heating boat, and the vacuum chamber was heated to 1×10 -4 The pressure was reduced to 100 Pa, and magnesium was deposited at a deposition rate of 0.9 Å / s and silver at a deposition rate of 0.1 Å / s to form a 150 nm film with a magnesium / silver ratio of 1 / 9. The pressure inside the deposition chamber was returned to normal pressure using nitrogen, and the substrate on which the 8 mm x 8 mm laminate having the organic light-emitting material layer was placed was removed. To this laminate having an organic light-emitting material layer, 30 mg of the curable composition obtained in each example to serve as a sealant was dropped under a nitrogen atmosphere, the laminate was covered with glass, and the sealant was cured by irradiating with 395 nm light at 400 mW for 4 seconds using a UV irradiation device. The obtained organic EL display element was exposed to an environment at a temperature of 85° C. for 96 hours, and then a voltage of 3 V was applied to the organic EL display element, and the light emitting state of the organic EL display element was visually confirmed. The evaluation criteria are as follows. A and B below were considered to be acceptable. A: No dark spots when the element emits light. B: Dark spots are partially present when the element emits light. C: When the element emits light, dark spots are present all over the surface, and the light-emitting area is also reduced.

[0093] [Table 1]

[0094] As can be seen from Table 1, the curable compositions obtained in the respective Examples had a dielectric constant of 3.6 or less and a hysteresis loss in the range of 0% to 45%. By using the curable compositions in the respective Examples for sealing a display device, a display device having excellent durability during long-term use can be obtained.

[0095] This application claims priority based on Japanese Patent Application No. 2021-076201, filed on April 28, 2021, the disclosure of which is incorporated herein in its entirety. [Explanation of symbols]

[0096] 10 Light emitting element 21 Barrier layer, touch panel layer or surface protection layer 22 Sealing layer, overcoat layer, or barrier layer 23 Planarization or sealing layer 24 Barrier layer 31 Sample 33 Sample Fixing Plate 35 Double-sided tape 50 Base material layer 100 display device

Claims

1. A liquid curable composition for use in sealing an organic EL element, comprising: The following components (a) and (b): (a) polymerizable compound, (b) Polymerization initiator Including, UV-LED with wavelength of 395 nm and illuminance of 1500 mW / cm 2 , cumulative light amount 1500 mJ / cm 2 the dielectric constant of the cured product of the curable composition at a frequency of 100 kHz is 3.3 or less, A sample obtained under the following condition 1 has a hysteresis loss of 0% or more and 45% or less when measured under the following condition 2, The curable composition, wherein the component (b) is a photocationic polymerization initiator. (Condition 1) The curable composition was sealed between two pieces of glass sandwiching a 100 μm-thick Teflon (registered trademark) sheet, and irradiated with a UV-LED having a wavelength of 395 nm at an illuminance of 1000 mW / cm 2 , cumulative light amount 1500 mJ / cm 2 The cured product obtained by curing at the above temperature is cut into a size of 10 mm width x 55 mm length, and the cured product having a thickness of 90 to 110 μm at a total of 5 points every 10 mm in the length direction is used as the sample. (Condition 2) One end of the sample is fixed, and the other end is fixed so that the chuck distance is 30 mm. At this time, the state in which the sample is not attached is set to 0 mN, and in order to eliminate the initial strain, the load is pulled until it reaches 0.05 N, and this point is set as the starting point. In a curve (stress-strain curve) in which the stress when a tensile test is performed in which the other end is pulled in a 180-degree direction at 23° C. and 10 mm / sec (tensile speed) is the vertical axis and the strain is the horizontal axis, A is the area of ​​the region enclosed by the vertical axis, the straight line of ``strain = 2%'', and the horizontal axis in graph 1 from the starting point of the tensile test to 2% elongation, and B is the area of ​​the region enclosed by the straight line of ``strain = 2%'', and the horizontal axis in graph 2 from 2% elongation to when the stress becomes zero, and the solution calculated by {(A-B) / A} x 100 is the hysteresis loss.

2. The curable composition according to claim 1, wherein the component (a) comprises at least one selected from the group consisting of an epoxy compound having two epoxy groups in one molecule, and an oxetane compound having two oxetanyl groups in one molecule.

3. 3. The curable composition according to claim 1, wherein the component (a) comprises two or more compounds selected from the group consisting of an epoxy compound having two epoxy groups in one molecule and an oxetane compound having two oxetanyl groups in one molecule.

4. A liquid curable composition for use in encapsulating an organic electroluminescence (EL) element, comprising: The following components (a) and (b): (a) polymerizable compound, (b) Polymerization initiator Including, the curable composition is cured with a UV-LED having a wavelength of 395 nm at an illuminance of 1500 mW / cm 2 and an accumulated light quantity of 1500 mJ / cm 2 , and the cured product has a dielectric constant of 3.6 or less at a frequency of 100 kHz; A sample obtained under the following condition 1 has a hysteresis loss of 0% or more and 45% or less when measured under the following condition 2, The component (a) contains a (meth)acrylic compound, A curable composition, wherein the content of the monofunctional acrylate compound in the (meth)acrylic compound is 15 mass % or less based on the total amount of the (meth)acrylic compound. (Condition 1) The curable composition is enclosed between two pieces of glass sandwiching a 100 μm thick Teflon (registered trademark) sheet, and cured with a UV-LED having a wavelength of 395 nm at an illuminance of 1000 mW / cm 2 and an accumulated light quantity of 1500 mJ / cm 2. The cured product obtained is cut into a size of 10 mm wide x 55 mm long, and the sample is determined to have a thickness of 90 to 110 μm at a total of 5 points every 10 mm in the length direction. (Condition 2) One end of the sample is fixed, and the other end is fixed so that the chuck distance is 30 mm. At this time, the state in which the sample is not attached is set to 0 mN, and in order to eliminate the initial strain, the load is pulled until it reaches 0.05 N, and this point is set as the starting point. In a curve (stress-strain curve) in which the stress when a tensile test is performed in which the other end is pulled in a 180-degree direction at 23° C. and 10 mm / sec (tensile speed) is the vertical axis and the strain is the horizontal axis, A is the area of ​​the region enclosed by the vertical axis, the straight line of ``strain = 2%'', and the horizontal axis in graph 1 from the starting point of the tensile test to 2% elongation, and B is the area of ​​the region enclosed by the straight line of ``strain = 2%'', and the horizontal axis in graph 2 from 2% elongation to when the stress becomes zero, and the solution calculated by {(A-B) / A} x 100 is the hysteresis loss.

5. The curable composition according to claim 4 , wherein the component (b) is a photoradical polymerization initiator.

6. The curable composition described in claim 4 or 5, wherein the component (a) contains one or more (meth)acrylic compounds having two (meth)acrylic groups in one molecule.

7. The curable composition according to claim 6 , wherein the component (a) contains two or more kinds of (meth)acrylic compounds having two (meth)acrylic groups in one molecule.

8. The curable composition of claim 1 or 4, further comprising component (c): a leveling agent.

9. The curable composition of claim 8 , wherein the component (c) is an acrylic leveling agent.

10. 5. The curable composition according to claim 1, wherein the viscosity of the curable composition measured at 25°C and 20 rpm using an E-type viscometer is 3 mPa·s or more and 50 mPa·s or less.

11. A substrate; an organic electroluminescence element disposed on the substrate; a sealing layer that covers the organic EL element; The organic electroluminescence display device according to claim 1 , wherein the sealing layer is formed of a cured product of the curable composition according to claim 1 .

Citation Information

Patent Citations

  • UV curable resin composition for organic el element encapsulation, manufacturing method of organic el light emitting device, organic el light-emitting device, and touch panel

    JP2020057580A

  • UV curable resin composition, manufacturing method of light emitting device, light emitting device, and touch panel

    JP2021064541A

  • Curable resin composition for sealing organic electroluminescent display element, curable resin sheet for sealing organic electroluminescent display element, and organic electroluminescent display element

    WO2015129670A1

  • Sealing agent for organic el display element, and organic el display device