Aqueous silica sol containing mercapto group-containing silica particles
The development of an aqueous silica sol with a pH of 2 to 7.5 stabilizes silica particles coated with mercapto group-containing silane compounds, addressing instability and aggregation issues, ensuring compatibility and stability with resins.
Patent Information
- Application Number
- JP2024532561
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-01-11
- Filing Date
- 2024-01-10
- Publication Date
- 2024-11-27
- Estimated Expiration
- 2044-01-10
AI Technical Summary
Existing silica sols with mercapto group-containing silane compounds face instability and aggregation issues due to pH fluctuations, leading to poor compatibility with resins and reduced stability.
An aqueous silica sol with a pH of 2 to 7.5 is developed, where silica particles are coated with a mercapto group-containing silane compound, allowing for stable dispersion and compatibility with resins by controlling pH within this range.
The solution ensures stable dispersion of silica particles with mercapto group-containing silane compounds, enhancing compatibility with resins and preventing aggregation, thus maintaining stability under pH changes.
Smart Images

Figure 0007590701000001 
Figure 0007590701000002 
Figure 0007590701000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an aqueous silica sol containing silica particles coated with a mercapto group-containing silane compound, and a method for producing the same. [Background technology]
[0002] Silica sols, in which colloidal silica particles are dispersed in a medium, are widely used, for example, as carriers, because of their excellent abrasion resistance and ability to impart irregularities due to the properties of the silica particles. There are various ways of using silica sols, such as coating liquids in which the silica sol is applied to the surface of a film or the like, or resin compositions in which the silica sol is mixed into a film-forming matrix and contained inside the film. There are also many silica sols containing silane-coated silica particles, in which the surfaces of silica particles are coated with a silane compound to utilize the properties of functional groups. For example, a method for producing an aqueous dispersion of silane-treated colloidal silica particles has been disclosed, which includes the step of mixing in an aqueous medium a) at least one silane compound containing epoxy functionality, b) at least one silane compound not having epoxy functionality (e.g., a functional group having a mercapto group) that is capable of modifying colloidal silica particles, and c) colloidal silica particles in any order to form an aqueous dispersion of silane-treated colloidal silica particles containing the silane compounds derived from a) and b) (see Patent Document 1). In a method for coating the surface layer of colloidal silica with a silane compound, a method has been disclosed in which an aqueous or alcoholic silica sol is mixed with a hydrolyzed compound of a glycidyl group-containing silane compound (see Patent Document 2). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2012-520227 A [Patent Document 2] JP 2002-511509 A Summary of the Invention [Problem to be solved by the invention]
[0004] The present invention provides an aqueous silica sol having a pH of 2 to 7.5, in which silica particles coated with a mercapto group-containing silane compound are dispersed in an aqueous medium. [Means for solving the problem]
[0005] As a first aspect, the present invention provides an aqueous silica sol having a pH of 2 to 7.5, which contains silica particles coated with a silane compound (a) containing a mercapto group or a hydrolysate thereof; As a second aspect, the silica particles are provided with a silane compound (a) containing a mercapto group represented by the formula (1): [ka] (In formula (1), R 1 is an alkyl group having 1 to 5 carbon atoms and containing a mercapto group, and is bonded to a silicon atom by a Si-C bond; R 2 represents an alkoxy group, and a represents an integer of 1 to 3; or a hydrolyzate thereof. As a third aspect, the aqueous silica sol according to the first aspect or the second aspect, in which a residual alcohol in the aqueous dispersion medium is 1.0 mass% or less. As a fourth aspect, the silica particles according to any one of the first to third aspects are A silane compound (a) containing a mercapto group or a hydrolyzate thereof and a compound represented by any one of the formulas (2) to (4): [ka] (In formula (2), R 3 R is an organic group having an alkenyl group, an aryl group, an epoxy group, a (meth)acryloyl group, an amino group, or a ureido group, and is bonded to a silicon atom by a Si-C bond; 4 each represents an alkoxy group, b represents an integer of 1 to 3, In formula (3) and formula (4), R 5 and R 7are aryl groups having 6 to 30 carbon atoms and bonded to silicon atoms by Si-C bonds, and R 6 and R 8 each represents an alkoxy group, Y represents an alkylene group, an NH group, or an oxygen atom, c is an integer of 1 to 3, d is an integer of 0 or 1, and e is an integer of 1 to 3.) As a fifth aspect, the silica sol according to the fourth aspect, which has a pH of 6.0 to 7.5. As a sixth aspect, the total amount of the silane compounds of the formulas (1) to (4) is, as a coating amount of the surface of the silica particles coated with the silane compounds of the formulas (1) to (4) or their hydrolysates, 0.3 silicon atoms / nm in terms of the number of silicon atoms in the silane compounds. 2 ~5.0 pieces / nm 2 The silica sol according to the fourth aspect, As a seventh aspect, the silica sol according to any one of the first to sixth aspects, in which an average particle size of silica particles contained in the silica sol is 5 nm to 200 nm as measured by a dynamic light scattering method. According to an eighth aspect, there is provided a resin composition comprising silica particles derived from the silica sol according to any one of the first to seventh aspects and a resin. According to a ninth aspect, there is provided an emulsion composition comprising silica particles derived from the silica sol according to any one of the first to seventh aspects, and a water-soluble resin having a hydroxyl group, a carboxyl group, an ester group, an amide group, or an ether bond; According to a tenth aspect, there is provided a coating composition comprising silica particles derived from the silica sol according to any one of the first to seventh aspects, and a hydrophobic resin containing a hydroxyl group, a carboxyl group, an ester group, an amide group, or an ether bond; According to an eleventh aspect, there is provided a polymerizable composition comprising silica particles derived from the silica sol according to any one of the first to seventh aspects, and a polymerizable resin. As a twelfth aspect, the method comprises the following steps (A) to (C): Step (A): A step of adjusting the pH of the aqueous silica sol to 2 to 7.5; Step (B): adding a silane compound (a) containing a mercapto group, or the silane compound (a) containing a mercapto group and at least one silane compound (b) selected from the group consisting of the silane compound represented by formulas (2) to (4) to the aqueous silica sol obtained in step (A); Step (C): a step of removing the alcohol having 1 to 5 carbon atoms from the aqueous medium of the aqueous silica sol obtained in step (B); The method for producing an aqueous silica sol according to any one of the first to seventh aspects, As a thirteenth aspect, there is provided a method for producing an aqueous silica sol according to the twelfth aspect, in which the step (B) is a step (B-1) of adding at least one silane compound (b) selected from the group consisting of formulae (2) to (4) to the aqueous silica sol obtained in the step (A), adjusting the pH to 6 to 7.5 with a basic substance, and then adding a silane compound (a) containing a mercapto group. Effect of the Invention
[0006] In the present invention, an aqueous silica sol containing silica particles coated with a silane compound having a mercapto group as a dispersoid is obtained by coating silica particles with a silane compound having a mercapto group in an aqueous medium, for example, an aqueous medium having a pH of 2 to 7.5. The aqueous medium having a pH of 2 to 7.5 containing silica particles is a silica sol having a pH of 2 to 7.5, which can be obtained by adding an acidic substance to the silica sol or by cation exchange. The aqueous silica sol having a pH of 2 to 7.5 obtained by coating a silane compound having a mercapto group in an aqueous medium having a pH of 2 to 7.5 remains stable even when the pH is subsequently increased or when the aqueous silica sol is mixed with a resin to produce a resin composition. If the pH value at the time of coating the silica particles with the silane compound having a mercapto group is outside the above-mentioned pH value, the above-mentioned effect cannot be obtained. When the function of the mercapto group as a functional group is coated on the surface of the silica particles in the above-mentioned pH range, the mercapto group on the surface of the silica particles is not modified, and the coated silica particles become stable. In addition, since the silane compound having a mercapto group is bonded to the silica particles, it can exist stably in an aqueous medium near neutral. This does not change even if the pH is changed or mixed with a resin afterwards. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] The present invention provides an aqueous silica sol having a pH of 2 to 7.5, which contains silica particles coated with a silane compound (a) containing a mercapto group or a hydrolysate thereof. By preparing an aqueous silica sol having a pH of 2 to 7.5, the silane compound (a) containing a mercapto group or a hydrolysate thereof is prevented from being denatured, and the silica particles are prevented from being aggregated and gelled. The sol of the present invention has a solid content of 0.1% by mass to 70% by mass, or 1% by mass to 60% by mass, or 10% by mass to 55% by mass, where the solid content is the total component of the sol excluding the solvent component. The silica particles of the present invention have an average primary particle diameter in the range of 5 nm to 200 nm, 5 nm to 150 nm, or 5 nm to 100 nm as measured by a nitrogen gas adsorption method (BET method), and an average particle diameter in the range of 5 nm to 200 nm, 5 nm to 150 nm, or 5 nm to 100 nm as measured by a dynamic light scattering method (DLS method).
[0008] Silica particles can be coated with the silane compound (a) containing a mercapto group, which is represented by the formula (1) or a hydrolysate thereof. In formula (1), R 1 is an alkyl group having 1 to 5 carbon atoms and containing a mercapto group, and is bonded to a silicon atom by a Si-C bond; R 2 represents an alkoxy group, and a represents an integer of 1 to 3.
[0009] Examples of the alkyl group having 1 to 5 carbon atoms and containing a mercapto group include a mercaptomethyl group and a mercaptopropyl group. Examples of the silane compound (a) include mercaptomethyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropylmethyldiethoxysilane, and mercaptomethyltriethoxysilane. These are available as silane compounds manufactured by Shin-Etsu Chemical Co., Ltd.
[0010] The residual alcohol content in the aqueous dispersion medium is preferably set to 1.0% by mass or less. The residual alcohol is mainly alcohol generated by hydrolysis of the silane compound, and this by-product alcohol is preferably removed from the system.
[0011] In the present invention, in an aqueous medium having a pH of 2 to 7.5, silica particles are coated with silane compound (b) or a hydrolysate thereof, and then coated with silane compound (a) having a mercapto group or a hydrolysate thereof, and the pH is further adjusted, and then the particles are coated with silane compound (a) having a mercapto group or a hydrolysate thereof.
[0012] In the present invention, the silica particles can be coated with a silane compound (a) or a hydrolysate thereof, and at least one silane compound (b) selected from the group consisting of formulas (2) to (4) or a hydrolysate thereof.
[0013] In formula (2), R 3 R is an organic group having an alkenyl group, an aryl group, an epoxy group, a (meth)acryloyl group, an amino group, or a ureido group, and is bonded to a silicon atom by a Si-C bond; 4 each represents an alkoxy group, b represents an integer of 1 to 3, In formula (3) and formula (4), R 5 and R 7are aryl groups having 6 to 30 carbon atoms and bonded to silicon atoms by Si-C bonds, and R 6 and R 8 each represents an alkoxy group, Y represents an alkylene group, an NH group, or an oxygen atom, c is an integer of 1 to 3, d is an integer of 0 or 1, and e is an integer of 1 to 3.
[0014] The aryl group is an aryl group having 6 to 30 carbon atoms, and examples thereof include a phenyl group, a naphthyl group, an anthracene group, and a pyrene group. The alkenyl group is an alkenyl group having 2 to 10 carbon atoms, and examples of the alkenyl group include ethenyl group, 1-propenyl group, 2-propenyl group, 1-methyl-1-ethenyl group, 1-butenyl group, 2-butenyl group, 3-butenyl group, 2-methyl-1-propenyl group, 2-methyl-2-propenyl group, 1-ethylethenyl group, 1-methyl-1-propenyl group, 1-methyl-2-propenyl group, 1-pentenyl group, 2-pentenyl group, 3-pentenyl group, 4-pentenyl group, 1-n-propylethenyl group, 1-methyl-1-butenyl group, 1-methyl-2-butenyl group, 1-methyl-3-butenyl group, 2-ethyl-2-propenyl group, 2-methyl-1-butenyl group, 2-methyl-2-butenyl group, 2-methyl-3-butenyl group, Examples of such alkyl groups include, but are not limited to, a 3-methyl-1-butenyl group, a 3-methyl-2-butenyl group, a 3-methyl-3-butenyl group, a 1,1-dimethyl-2-propenyl group, a 1-i-propylethenyl group, a 1,2-dimethyl-1-propenyl group, a 1,2-dimethyl-2-propenyl group, a 1-cyclopentenyl group, a 2-cyclopentenyl group, a 3-cyclopentenyl group, a 1-hexenyl group, a 2-hexenyl group, a 3-hexenyl group, a 4-hexenyl group, a 5-hexenyl group, a 1-methyl-1-pentenyl group, a 1-methyl-2-pentenyl group, a 1-methyl-3-pentenyl group, a 1-methyl-4-pentenyl group, a 1-n-butylethenyl group, a 2-methyl-1-pentenyl group, and a 2-methyl-2-pentenyl group.
[0015] Examples of the organic group having an epoxy group include a 2-(3,4-epoxycyclohexyl)ethyl group, a 3-glycidoxypropyl group, and a 3-glycidoxypropylmethyl group.
[0016] The alkoxy group includes an alkoxy group having 1 to 10 carbon atoms, such as a methoxy group, an ethoxy group, an n-propoxy group, an i-propoxy group, an n-butoxy group, an i-butoxy group, an s-butoxy group, a t-butoxy group, an n-pentyloxy group, a 1-methyl-n-butoxy group, a 2-methyl-n-butoxy group, a 3-methyl-n-butoxy group, a 1,1-dimethyl-n-propoxy group, a 1,2-dimethyl-n-propoxy group, a 2,2-dimethyl-n-propoxy group, a 1-ethyl-n-propoxy group, and an n-hexyloxy group, but is not limited to these.
[0017] The (meth)acryloyl group refers to both an acryloyl group and a methacryloyl group. Examples of organic groups having a (meth)acryloyl group include a 3-methacryloxypropyl group and a 3-acryloxypropyl group. Examples of organic groups having an amino group include a 2-aminoethyl group, a 3-aminopropyl group, an N-2-(aminoethyl)-3-aminopropyl group, an N-(1,3-dimethyl-butylidene)aminopropyl group, an N-phenyl-3-aminopropyl group, and an N-(vinylbenzyl)-2-aminoethyl-3-aminopropyl group.
[0018] An example of the organic group having a ureido group is a 3-ureidopropyl group.
[0019] An example of the organic group having a cyano group is a 3-cyanopropyl group. The silane compound represented by the formula (2) is preferably a compound that forms an epoxy group or a hydrolyzate of an epoxy group on the surface of silica particles.
[0020] Preferred functional groups are epoxy groups, hydrolysates of epoxy groups, and the like, and corresponding silane compounds include 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane, and the like.
[0021] This is a process in which the silane compound reacts with a hydroxyl group on the surface of silica particles, for example, a silanol group in the case of silica particles, to coat the surface of the silica particles with the silane compound through a siloxane bond. The reaction temperature can be from 20°C to the boiling point of the dispersion medium, for example, in the range of 20°C to 100°C. The reaction time can be about 0.1 to 6 hours.
[0022] The content of sulfur atoms derived from the silane compound of the formula (1) is 0.3 / nm2 in terms of the number of sulfur atoms in the silane compound as a coating amount on the surface of the silica particles. 2 ~3.0 pieces / nm 2 The amount of the coating on the surface of the silica particles can be within the range of 0.3 sulfur atoms / nm2 in terms of the number of sulfur atoms in the silane compound. 2 ~3.0 pieces / nm 2 By doing so, when a coating film is formed on a metal plate (eg, a Cu plate) using the resin composition, the adhesion of the coating film can be improved.
[0023] The total amount of the silane compounds of the formulas (1) to (4) is, in terms of the coating amount of the silica particle surface coated with the silane compounds of the formulas (1) to (4) or their hydrolysates, 0.3 silicon atoms / nm in terms of the number of silicon atoms in the silane compounds. 2 ~5.0 pieces / nm 2The number of sulfur atoms derived from the silane compound of formula (1) and the number of silicon atoms in the silane compounds of formulas (1) to (4) can be set to a molar ratio of S:Si of 1:0 to 10.0, or 1:0 to 7.0. The coating amount on the silica particle surface can be set to 0.3 silicon atoms / nm2 in terms of the number of silicon atoms in the silane compound. 2 ~5.0 pieces / nm 2 By doing so, when a coating film is formed from the resin composition, the resin and the silica particles strongly interact with each other via the silane compound, thereby improving the scratch resistance of the coating film.
[0024] When the silane compound is coated without a catalyst, the silica particle surface is on the acidic side. When a catalyst is used, the hydrolysis catalyst can be a metal chelate compound, an organic acid, an inorganic acid, an organic base, or an inorganic base. Examples of the metal chelate compound as the hydrolysis catalyst include triethoxy mono(acetylacetonato)titanium and triethoxy mono(acetylacetonato)zirconium. Examples of the organic acid as the hydrolysis catalyst include acetic acid and oxalic acid. Examples of the inorganic acid as the hydrolysis catalyst include hydrochloric acid, nitric acid, sulfuric acid, hydrofluoric acid, and phosphoric acid. Examples of the organic base as the hydrolysis catalyst include pyridine, pyrrole, piperazine, and quaternary ammonium salts. Examples of the inorganic base as the hydrolysis catalyst include ammonia, sodium hydroxide, and potassium hydroxide.
[0025] The silica sol of the present invention can be produced by the following steps (A) to (C): Step (A): A step of adjusting the pH of the aqueous silica sol to 2 to 7.5; Step (B): adding a silane compound (a) containing a mercapto group, or the silane compound (a) containing a mercapto group and at least one silane compound (b) selected from the group consisting of the silane compound represented by formulas (2) to (4) to the aqueous silica sol obtained in step (A); Step (C): A step of removing the alcohol having 1 to 5 carbon atoms from the aqueous medium of the aqueous silica sol obtained in step (B). The step (B) may include a step (B-1) of adding the silane compound (b), adjusting the pH to 6 to 7.5 with a basic substance, and then adding the silane compound (a).
[0026] The basic substance added in step (B) is, in the case of an organic base, for example, pyridine, pyrrole, piperazine, or a quaternary ammonium salt, and in the case of an inorganic base, for example, ammonia, sodium hydroxide, or potassium hydroxide.
[0027] The step (C) may be a step of removing the alcohol having 1 to 5 carbon atoms from the aqueous medium of the aqueous silica sol.
[0028] In the present invention, an aqueous silica sol in which silica particles are coated with a silane compound (a) or its hydrolysate, or a silane compound (b) or its hydrolysate together with the silane compound (a) can exist stably as an aqueous silica sol by setting the residual amount of alcohol by-produced when the silane compound is hydrolyzed to 1.0 mass% or less in an aqueous medium. In an acidic aqueous silica sol having a mercapto group and a pH of 2 to 7.5, when the residual alcohol is 1.0 mass% or more, the compatibility of the coating agent with the alcohol may decrease, resulting in poor stability.
[0029] In the present invention, a resin composition can be produced that contains silica particles derived from the aqueous silica sol and a resin.
[0030] In the present invention, an emulsion composition containing silica particles derived from the aqueous silica sol and a water-soluble resin can be produced. The water-soluble resin can be a water-soluble resin containing a hydroxyl group, a carboxyl group, an ester group, an amide group, or an ether bond. The aqueous silica sol and the water-soluble resin can be mixed in any ratio to produce an aqueous resin emulsion composition. The silica in the aqueous resin emulsion composition is 0.1% by mass to 70% by mass, or 1% by mass to 60% by mass, or 10% by mass to 55% by mass as a solid content. The pH can be set in the range of 2 to 7.5, or 2 to 6.
[0031] In addition, the present invention can produce a coating composition containing the aqueous silica sol and a hydrophobic resin. The hydrophobic resin can be a hydrophobic resin containing a hydroxyl group, a carboxyl group, an ester group, or an ether bond. The silica in the hydrophobic resin is 0.10% by mass to 70% by mass, or 1% by mass to 60% by mass, or 10% by mass to 55% by mass, as a solid content. The pH can be set in the range of 2 to 7.5, or 2 to 6. The pH can be measured in a state where the hydrophobic resin and water are mixed in a mass ratio of 1:1, or the hydrophobic resin, methanol, and water are mixed in a mass ratio of 1:1:1. Examples of the water-soluble resin and hydrophobic resin containing a hydroxyl group include polyvinyl alcohol, carboxymethyl cellulose, methylol melamine resin, and resol type phenolic resin. Examples of the carboxyl group-containing resin include polyacrylic acid and polymethacrylic acid. Examples of the amide group-containing resin include urea resin, methylol urea resin, polyacrylamide, polyamide, polyimide, and polyamic acid. Examples of the ether bond-containing resin include polyethylene oxide, polypropylene glycol, polyphenylene oxide, and polysulfone.
[0032] In the present invention, a polymerizable composition containing silica particles derived from the aqueous silica sol and a polymerizable resin can be produced. The aqueous silica sol and the polymerizable resin can be mixed to obtain a polymerizable composition. The polymerizable composition can be used as a film-forming composition.
[0033] In the present invention, in the mixing of the aqueous silica sol and the polymerizable resin, a film-forming composition is obtained by selecting and mixing a thermosetting or photocurable resin as the polymerizable resin.These thermosetting and photocurable resins can contain a curing agent such as an amine-based curing agent, an acid anhydride-based curing agent, a radical generator-based curing agent (thermal radical generator, photoradical generator), or an acid generator-based curing agent (thermal acid generator, photoacid generator), and can be cured.
[0034] A film-forming composition containing an organic resin and a curing agent can be applied or filled to a substrate, and then heated, irradiated with light, or a combination thereof to form a cured product. Examples of organic resins (curable resins) include resins having functional groups such as epoxy groups or (meth)acryloyl groups, and isocyanate-based resins. For example, photocurable polyfunctional acrylates can be preferably used.
[0035] Examples of the polyfunctional acrylate include polyfunctional acrylates having difunctional, trifunctional, tetrafunctional or higher functional groups in the molecule, such as neopentyl glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, and dipentaerythritol hexa(meth)acrylate. As these polyfunctional acrylates, polyfunctional acrylates represented by the structural formulas shown below may be used. [ka] [ka] [ka] [ka]
[0036] The film-forming composition of the present invention may contain a surfactant (leveling agent). The surfactant (leveling agent) may be an anionic surfactant, a cationic surfactant, an amphoteric surfactant, a nonionic surfactant, or a silicone surfactant. The surfactant (leveling agent) may be added in an amount of 0.01 phr to 5 phr or 0.01 phr to 1 phr relative to the organic resin.
[0037] Anionic surfactants for use in the present invention include sodium and potassium salts of fatty acids, alkylbenzene sulfonates, higher alcohol sulfates, polyoxyethylene alkyl ether sulfates, α-sulfofatty acid esters, α-olefin sulfonates, monoalkyl phosphates, and alkanesulfonates. For example, alkylbenzenesulfonates include sodium salts, potassium salts and lithium salts, such as sodium C10-C16 alkylbenzenesulfonate, C10-C16 alkylbenzenesulfonic acid, and sodium alkylnaphthalenesulfonate.
[0038] Examples of higher alcohol sulfates include sodium dodecyl sulfate (sodium lauryl sulfate), which has 12 carbon atoms, triethanolamine lauryl sulfate, and triethanolammonium lauryl sulfate.
[0039] Examples of polyoxyethylene alkyl ether sulfates include sodium polyoxyethylene styrenated phenyl ether sulfate, ammonium polyoxyethylene styrenated phenyl ether sulfate, sodium polyoxyethylene decyl ether sulfate, ammonium polyoxyethylene decyl ether sulfate, sodium polyoxyethylene lauryl ether sulfate, ammonium polyoxyethylene lauryl ether sulfate, sodium polyoxyethylene tridecyl ether sulfate, and sodium polyoxyethylene oleyl cetyl ether sulfate. The α-olefin sulfonate salts include sodium α-olefin sulfonate.
[0040] Examples of the alkane sulfonate include sodium 2-ethylhexyl sulfate.
[0041] Examples of the cationic surfactant that can be used in the present invention include alkyltrimethylammonium salts, dialkyldimethylammonium salts, alkyldimethylbenzylammonium salts, and amine salt-based agents.
[0042] Alkyltrimethylammonium salts are quaternary ammonium salts that have a chloride ion or a bromide ion as a counterion. Examples include dodecyltrimethylammonium chloride, cetyltrimethylammonium chloride, coconut alkyltrimethylammonium chloride, and alkyl(C16-18)trimethylammonium chloride.
[0043] Dialkyldimethylammonium salts have two lipophilic main chains and two methyl groups. Examples include bis(hydrogenated tallow)dimethylammonium chloride. Examples include didecyldimethylammonium chloride, dicoconucleic acid alkyldimethylammonium chloride, dihydrogenated tallow alkyldimethylammonium chloride, and dialkyl(C14-18)dimethylammonium chloride.
[0044] Alkyl dimethyl benzyl ammonium salts are quaternary ammonium salts having one lipophilic main chain, two methyl groups, and a benzyl group, and examples thereof include benzalkonium chloride. For example, alkyl (C8-18) dimethyl benzyl ammonium chloride can be mentioned.
[0045] Amine salt agents include those in which the hydrogen atom of ammonia has been replaced with one or more hydrocarbon groups, such as N-methylbishydroxyethylamine fatty acid ester hydrochloride.
[0046] The amphoteric surfactants used in the present invention include N-alkyl-β-alanine type alkylamino fatty acid salts, alkylcarboxybetaine type alkylbetaines, and N,N-dimethyldodecylamine oxide type alkylamine oxides, examples of which include lauryl betaine, stearyl betaine, 2-alkyl-N-carboxymethyl-N-hydroxyethyl imidazolinium betaine, and lauryl dimethylamine oxide.
[0047] The nonionic surfactant used in the present invention is selected from polyoxyethylene alkyl ethers, polyoxyethylene alkylphenol ethers, alkyl glucosides, polyoxyethylene fatty acid esters, sucrose fatty acid esters, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, and fatty acid alkanolamides. For example, examples of polyoxyethylene alkyl ethers include polyoxyethylene dodecyl ether (polyoxyethylene lauryl ether), polyoxyalkylene lauryl ether, polyoxyethylene tridecyl ether, polyoxyalkylene tridecyl ether, polyoxyethylene myristyl ether, polyoxyethylene cetyl ether, polyoxyethylene oleyl ether, polyoxyethylene stearyl ether, polyoxyethylene behenyl ether, polyoxyethylene-2-ethylhexyl ether, and polyoxyethylene isodecyl ether.
[0048] Examples of polyoxyethylene alkylphenol ethers include polyoxyethylene styrenated phenyl ether, polyoxyethylene nonylphenyl ether, polyoxyethylene distyrenated phenyl ether, and polyoxyethylene tribenzyl phenyl ether.
[0049] The alkyl glucoside includes decyl glucoside and lauryl glucoside.
[0050] Examples of polyoxyethylene fatty acid esters include polyoxyethylene monolaurate, polyoxyethylene monostearate, polyoxyethylene monooleate, polyethylene glycol distearate, polyethylene glycol dioleate, and polypropylene glycol dioleate.
[0051] Examples of sorbitan fatty acid esters include sorbitan monocaprylate, sorbitan monolaurate, sorbitan monomyristate, sorbitan monopalmitate, sorbitan monostearate, sorbitan distearate, sorbitan tristearate, sorbitan monooleate, sorbitan trioleate, sorbitan monosesquioleate, and ethylene oxide adducts thereof.
[0052] Examples of polyoxyethylene sorbitan fatty acid esters include polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalmitate, polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan tristearate, polyoxyethylene sorbitan monooleate, polyoxyethylene sorbitan trioleate, and polyoxyethylene sorbitan triisostearate.
[0053] Examples of fatty acid alkanolamides include coconut oil fatty acid diethanolamide, beef tallow fatty acid diethanolamide, lauric acid diethanolamide, and oleic acid diethanolamide.
[0054] Further examples include polyoxyalkyl ethers or polyoxyalkyl glycols such as polyoxyethylene polyoxypropylene glycol, polyoxyethylene fatty acid esters, polyoxyethylene hydrogenated castor oil ether, sorbitan fatty acid ester alkyl ethers, alkyl polyglucosides, sorbitan monooleate, and sucrose fatty acid esters.
[0055] A silicone surfactant can be used as the surfactant (leveling agent). A silicone surfactant is a compound having a repeating unit containing a siloxane bond in the main chain. The weight average molecular weight of the silicone surfactant can be in the range of 500 to 50,000. These may be modified silicone surfactants, and examples of such surfactants include those having an organic group introduced into the side chain and / or end of a polysiloxane. Examples of the organic group include an amino group, an epoxy group, an alicyclic epoxy group, a carbinol group, a mercapto group, a carboxyl group, an aliphatic ester group, an aliphatic amide group, and a polyether group. Silicone surfactants include trade names such as Toray Silicone DC3PA, Toray Silicone SH7PA, Toray Silicone DC11PA, Toray Silicone SH21PA, Toray Silicone SH28PA, Toray Silicone SH29PA, Toray Silicone SH30PA, and Toray Silicone SH8400 (all manufactured by Toray Dow Corning Co., Ltd.), Silwet l-77, L-7280, L-7001, L-7002, L-7200, L-7210, L-7220, L-7230, L7500, L-7600, L-7602, L-7604, L-7605, L-7622, L-765 7, L-8500, and L-8610 (all manufactured by Momentive Performance Materials Co., Ltd.), KP-341, KF-6001, and KF-6002. (all manufactured by Shin-Etsu Silicones Co., Ltd.), BYK307, BYK323, BYK330 (all manufactured by BYK-Chemie Co., Ltd.), etc. For example, a product name L-7001 (manufactured by Dowsil Co., Ltd.) can be suitably used as a polyether-modified silicone.
[0056] In the present invention, a film-forming composition containing the aqueous silica sol and an organic resin is obtained. The film-forming composition can be obtained by removing the aqueous solvent from the aqueous silica sol to form a film-forming composition containing silica particles and an organic resin.
[0057] In the case of a thermosetting film-forming composition, the heat curing agent can be added in the range of 0.01 phr to 50 phr, or 0.01 phr to 10 phr, relative to the resin containing a functional group such as an epoxy group or a (meth)acryloyl group, and for example, the heat curing agent can be contained in a ratio of 0.5 equivalents to 1.5 equivalents, preferably 0.8 equivalents to 1.2 equivalents, relative to the functional group such as an epoxy group or a (meth)acryloyl group. The equivalent of the heat curing agent relative to the curable resin is represented by the equivalent ratio of the heat curing agent to the functional group.
[0058] Examples of the heat curing agent include phenol resins, amine-based curing agents, polyamide resins, imidazoles, polymercaptans, acid anhydrides, heat radical generators, heat acid generators, etc. In particular, radical generator-based curing agents, acid anhydride-based curing agents, and amine-based curing agents are preferred.
[0059] Even if these thermosetting agents are solid, they can be used by dissolving them in a solvent. However, evaporation of the solvent reduces the density of the cured product and creates pores, resulting in reduced strength and reduced water resistance. Therefore, it is preferable for the curing agent itself to be liquid at room temperature and normal pressure. Examples of the phenol resin include phenol novolac resin and cresol novolac resin.
[0060] Examples of the amine curing agent include piperidine, N,N-dimethylpiperazine, triethylenediamine, 2,4,6-tris(dimethylaminomethyl)phenol, benzyldimethylamine, 2-(dimethylaminomethyl)phenol, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, diethylaminopropylamine, N-aminoethylpiperazine, di(1-methyl-2-aminocyclohexyl)methane, menthenediamine, isophoronediamine, diaminodicyclohexylmethane, 1,3-diaminomethylcyclohexane, xylylenediamine, metaphenylenediamine, diaminodiphenylmethane, diaminodiphenylsulfone, 3,3'-diethyl-4,4'-diaminodiphenylmethane, and diethyltoluenediamine. Of these, liquid diethylenetriamine, triethylenetetramine, tetraethylenepentamine, diethylaminopropylamine, N-aminoethylpiperazine, di(1-methyl-2-aminocyclohexyl)methane, menthenediamine, isophoronediamine, diaminodicyclohexylmethane, 3,3'-diethyl-4,4'-diaminodiphenylmethane, diethyltoluenediamine, etc. can be preferably used.
[0061] The polyamide resin is produced by condensation of dimer acid and polyamine, and is a polyamide amine having a primary amine and a secondary amine in the molecule.
[0062] Examples of the imidazoles include 2-methylimidazole, 2-ethyl-4-methylimidazole, 1-cyanoethyl-2-undecylimidazolium trimellitate, and epoxy imidazole adduct.
[0063] The polymercaptan is, for example, one having a mercaptan group at the end of a polypropylene glycol chain or one having a mercaptan group at the end of a polyethylene glycol chain, and is preferably in a liquid form.
[0064] As the acid anhydride curing agent, the anhydride of the compound having a plurality of carboxyl groups in one molecule is preferable.As these acid anhydride curing agents, phthalic anhydride, trimellitic anhydride, pyromellitic anhydride, benzophenone tetracarboxylic anhydride, ethylene glycol bis trimellitate, glycerol tris trimellitate, maleic anhydride, tetrahydrophthalic anhydride, methyl tetrahydrophthalic anhydride, endomethylene tetrahydrophthalic anhydride, methyl endomethylene tetrahydrophthalic anhydride, methyl butenyl tetrahydrophthalic anhydride, dodecenyl succinic anhydride, hexahydrophthalic anhydride, methyl hexahydrophthalic anhydride, succinic anhydride, methylcyclohexene dicarboxylic anhydride, chlorendic anhydride, etc. can be mentioned.
[0065] Examples of the thermal acid generator include sulfonium salts and phosphonium salts, with sulfonium salts being preferred. For example, the following compounds can be mentioned. [ka] R is an alkyl group having 1 to 12 carbon atoms or an aryl group having 6 to 20 carbon atoms, and is particularly preferably an alkyl group having 1 to 12 carbon atoms.
[0066] Among these, the following are preferred, which are liquid at room temperature and pressure: methyltetrahydrophthalic anhydride, methyl-5-norbornene-2,3-dicarboxylic anhydride (methylnadic anhydride, methylhimic anhydride), hydrogenated methylnadic anhydride, methylbutenyltetrahydrophthalic anhydride, dodecenylsuccinic anhydride, methylhexahydrophthalic anhydride, and a mixture of methylhexahydrophthalic anhydride and hexahydrophthalic anhydride. These liquid acid anhydrides have a viscosity of about 10 mPa·s to 1000 mPa·s when measured at 25°C.
[0067] Examples of thermal radical generators include 2,2'-azobis(isobutyronitrile), 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis(2-methylpropionate)dimethyl, 2,2'-azobis(2-methylpropionamidine)dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride, tert-butyl hydroperoxide, cumene hydroperoxide, di-tert-butyl peroxide, dicumyl peroxide, benzoyl peroxide, etc. These can be obtained from Tokyo Chemical Industry Co., Ltd.
[0068] In addition, when obtaining the cured product, a curing assistant may be used in combination as appropriate. Examples of the curing assistant include organic phosphorus compounds such as triphenylphosphine and tributylphosphine, quaternary phosphonium salts such as ethyltriphenylphosphonium bromide and methyltriphenylphosphonium diethyl phosphate, and quaternary ammonium salts such as 1,8-diazabicyclo(5,4,0)undecane-7-ene, salts of 1,8-diazabicyclo(5,4,0)undecane-7-ene and octylic acid, zinc octylate, and tetrabutylammonium bromide. These curing assistants can be contained in a ratio of 0.001 to 0.1 parts by mass relative to 1 part by mass of the curing agent.
[0069] The composition is a thermosetting varnish obtained by mixing a resin, a curing agent, and optionally a curing aid, which can be mixed in a reaction vessel using a stirring blade or a kneader. The mixing is carried out by a hot mixing method at a temperature of 60° C. to 100° C. for 0.5 to 1 hour. The obtained curable film-forming composition is a thermosetting coating composition, and has a suitable viscosity for use as, for example, a liquid sealant. The liquid thermosetting film-forming composition can be prepared to any viscosity, and can be partially sealed at any desired location for use as a transparent sealant for LEDs, etc., by casting, potting, dispenser, printing, etc. The liquid thermosetting composition is directly mounted on an LED, etc., in the liquid state, by the above-mentioned method, and then dried and cured to obtain a cured epoxy resin body. The thermosetting film-forming composition (thermosetting coating composition) is applied to a substrate and heated at a temperature of 80°C to 200°C to obtain a cured product.
[0070] In the case of a photocurable resin composition in the film-forming composition, a photocuring agent (photoradical generator, photoacid generator) can be added in the range of 0.01 phr to 50 phr, or 0.01 phr to 10 phr, to a resin containing a functional group such as an epoxy group or a (meth)acryloyl group. For example, the photocuring agent (photoradical generator, photoacid generator) can be contained in a ratio of 0.5 equivalents to 1.5 equivalents, preferably 0.8 equivalents to 1.2 equivalents, to a functional group such as an epoxy group or a (meth)acryloyl group. The equivalent of the photocuring agent to the curable resin is represented by the equivalent ratio of the photocuring agent to the functional group. The photoradical generator is not particularly limited as long as it generates radicals directly or indirectly upon irradiation with light. Examples of the photoradical generator include photoradical polymerization initiators such as imidazole compounds, diazo compounds, bisimidazole compounds, N-arylglycine compounds, organic azide compounds, titanocene compounds, aluminate compounds, organic peroxides, N-alkoxypyridinium salt compounds, and thioxanthone compounds.
[0071] Examples of the organic azide compound include p-azidobenzaldehyde, p-azidoacetophenone, p-azidobenzoic acid, p-azidobenzalacetophenone, 4,4'-diazidochalcone, 4,4'-diazidodiphenyl sulfide, and 2,6-bis(4'-azidobenzal)-4-methylcyclohexanone.
[0072] Examples of the diazo compound include 1-diazo-2,5-diethoxy-4-p-tolylmercaptobenzene borofluoride, 1-diazo-4-N,N-dimethylaminobenzene chloride, and 1-diazo-4-N,N-diethylaminobenzene borofluoride.
[0073] Examples of the bisimidazole compound include 2,2'-bis(o-chlorophenyl)-4,5,4',5'-tetrakis(3,4,5-trimethoxyphenyl)1,2'-bisimidazole, and 2,2'-bis(o-chlorophenyl)4,5,4',5'-tetraphenyl-1,2'-bisimidazole.
[0074] Titanocene compounds include dicyclopentadienyl-titanium-dichloride, dicyclopentadienyl-titanium-bisphenyl, dicyclopentadienyl-titanium-bis(2,3,4,5,6-pentafluorophenyl), dicyclopentadienyl-titanium-bis(2,3,5,6-tetrafluorophenyl), dicyclopentadienyl-titanium-bis(2,4,6-trifluorophenyl), dicyclopentadienyl-titanium-bis(2,6-difluorophenyl), dicyclopentadienyl Examples of such aryl groups include dicyclopentadienyl-titanium-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)-phenyl), dicyclopentadienyl-titanium-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)-phenyl), dicyclopentadienyl-titanium-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)-phenyl), and dicyclopentadienyl-titanium-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)-phenyl).
[0075] Further examples of photoradical generators include 1,3-di(tert-butyldioxycarbonyl)benzophenone, 3,3',4,4'-tetrakis(tert-butyldioxycarbonyl)benzophenone, 3-phenyl-5-isoxazolone, 2-mercaptobenzimidazole, 2,2-dimethoxy-1,2-diphenylethan-1-one, 1-hydroxy-cyclohexyl-phenyl-ketone, and 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone.
[0076] These photoradical polymerization agents are available, for example, under the trade name Irgacure TPO (the component is 2,4,6-trimethylbenzoyldiphenylphosphine oxide) (c1-1-1) manufactured by BASF, under the trade name Omnirad819 (the component is bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide) (c1-1-2) manufactured by IGM RESINS, and under the trade name Irgacure 184 (the component is 1-hydroxycyclohexyl phenyl ketone) (c1-1-3) manufactured by IGM RESINS. [ka]
[0077] The photoacid generator is not particularly limited as long as it generates an acid directly or indirectly upon irradiation with light.
[0078] Specific examples of the photoacid generator that can be used include triazine-based compounds, acetophenone derivative compounds, disulfone-based compounds, diazomethane-based compounds, sulfonic acid derivative compounds, onium salts such as iodonium salts, sulfonium salts, phosphonium salts, and selenium salts, metallocene complexes, and iron arene complexes.
[0079] The onium salt used as the photoacid generator includes, for example, an iodonium salt, such as diphenyliodonium chloride, diphenyliodonium trifluoromethanesulfonate, diphenyliodonium mesylate, diphenyliodonium tosylate, diphenyliodonium bromide, diphenyliodonium tetrafluoroborate, diphenyliodonium hexafluoroantimonate, diphenyliodonium hexafluoroarsenate, bis(p-tert-butylphenyl)iodonium hexafluorophosphate, bis(p-tert-butylphenyl)iodonium mesylate, bis(p-tert-butylphenyl)iodonium tosylate, bis(p-tert-butylphenyl)iodonium trifluoromethanesulfonate, and bis(p-tert-butylphenyl)iodonium trifluoromethanesulfonate. Examples of the iodonium salt include iodonium tetrafluoroborate, bis(p-tert-butylphenyl)iodonium chloride, bis(p-chlorophenyl)iodonium chloride, bis(p-chlorophenyl)iodonium tetrafluoroborate, and further bis(4-t-butylphenyl)iodonium hexafluorophosphate. Examples of the iodonium salt include bis(alkylphenyl)iodonium salts such as bis(4-t-butylphenyl)iodonium hexafluorophosphate, alkoxycarbonylalkoxy-trialkylaryliodonium salts (e.g., 4-[(1-ethoxycarbonyl-ethoxy)phenyl]-(2,4,6-trimethylphenyl)-iodonium hexafluorophosphate, and the like), and bis(alkoxyaryl)iodonium salts (e.g., bis(alkoxyphenyl)iodonium salts such as (4-methoxyphenyl)phenyliodonium hexafluoroantimonate, and the like).
[0080] Examples of sulfonium salts include triphenylsulfonium salts such as triphenylsulfonium chloride, triphenylsulfonium bromide, tri(p-methoxyphenyl)sulfonium tetrafluoroborate, tri(p-methoxyphenyl)sulfonium hexafluorophosphonate, tri(p-ethoxyphenyl)sulfonium tetrafluoroborate, triphenylsulfonium triflate, triphenylsulfonium hexafluoroantimonate, and triphenylsulfonium hexafluorophosphate; and sulfonium salts such as (4-phenylthiophenyl)diphenylsulfonium hexafluoroantimonate, (4-phenylthiophenyl)diphenylsulfonium hexafluorophosphate, bis[4-(diphenylsulfonio)phenyl]sulfide-bis-hexafluoroantimonate, bis[4-(diphenylsulfonio)phenyl]sulfide-bis-hexafluorophosphate, and (4-methoxyphenyl)diphenylsulfonium hexafluoroantimonate.
[0081] Examples of phosphonium salts include phosphonium salts such as triphenylphosphonium chloride, triphenylphosphonium bromide, tri(p-methoxyphenyl)phosphonium tetrafluoroborate, tri(p-methoxyphenyl)phosphonium hexafluorophosphonate, tri(p-ethoxyphenyl)phosphonium tetrafluoroborate, 4-chlorobenzenediazonium hexafluorophosphate, and benzyltriphenylphosphonium hexafluoroantimonate. Examples include selenium salts such as triphenylselenium hexafluorophosphate, and metallocene complexes such as (η5 or η6-isopropylbenzene)(η5-cyclopentadienyl)iron(II) hexafluorophosphate.
[0082] In addition, the following compounds can also be used as the photoacid generator. [ka] [ka] [ka] [ka] [ka] [ka] [ka] [ka] [ka]
[0083] As the photoacid generator, sulfonium salt compounds and iodonium salt compounds are preferred. The anion species thereof is CF3SO3 - , C4F9SO3 - , C8F 17 SO3 - , camphorsulfonate anion, tosylate anion, BF4 - , PF6 - , AsF6 - and SbF6 - In particular, anion species such as phosphorus hexafluoride and antimony hexafluoride, which exhibit strong acidity, are preferred.
[0084] The film-forming composition of the present invention may contain conventional additives as necessary. Examples of such additives include pigments, colorants, thickeners, sensitizers, defoamers, coating improvers, lubricants, stabilizers (antioxidants, heat stabilizers, light resistance stabilizers, etc.), plasticizers, dissolution promoters, fillers, antistatic agents, etc. These additives may be used alone or in combination of two or more.
[0085] Examples of methods for applying the coating composition of the present invention include flow coating, spin coating, spray coating, screen printing, casting, bar coating, curtain coating, roll coating, gravure coating, dipping, and slit coating.
[0086] In the present invention, the photocurable coating composition (film-forming composition) can be applied onto a substrate and cured by irradiation with light. It can also be heated before or after irradiation with light.
[0087] The thickness of the coating film can be selected from the range of about 0.01 μm to 10 mm depending on the application of the cured product. For example, when used as a photoresist, it can be about 0.05 μm to 10 μm (particularly 0.1 μm to 5 μm), when used as a printed wiring board, it can be about 5 μm to 5 mm (particularly 100 μm to 1 mm), and when used as an optical thin film, it can be about 0.1 μm to 100 μm (particularly 0.3 μm to 50 μm).
[0088] When a transparent coating is obtained, the coating can have a visible light transmittance of 80% or more, or 90% or more, typically 90 to 96%.
[0089] When a photoacid generator is used, the light to be irradiated or exposed may be, for example, gamma rays, X-rays, ultraviolet rays, visible light, etc., and is usually visible light or ultraviolet rays, particularly ultraviolet rays. The wavelength of the light is, for example, about 150 nm to 800 nm, preferably 150 to 600 nm, and more preferably about 150 nm to 400 nm. The amount of irradiation light varies depending on the thickness of the coating film, but is, for example, 2 mJ / cm. 2 ~20000mJ / cm 2 , preferably 5 mJ / cm 2 ~5000mJ / cm 2The light source can be selected according to the type of light to be exposed, and for example, in the case of ultraviolet light, a low pressure mercury lamp, a high pressure mercury lamp, an ultra-high pressure mercury lamp, a deuterium lamp, a halogen lamp, or a laser beam (helium-cadmium laser, excimer laser, etc.) can be used. Such light irradiation causes the curing reaction of the composition to proceed.
[0090] When a thermal acid generator is used, or when a photoacid generator is used, the coating film is heated as necessary after light irradiation, for example at 60° C. to 350° C., and preferably at about 100° C. to 300° C. The heating time can be selected within a range of 3 seconds or more (for example, about 3 seconds to 5 hours), for example, 5 seconds to 2 hours, preferably about 20 seconds to 30 minutes, and usually about 1 minute to 3 hours (for example, about 5 minutes to 2.5 hours). Furthermore, when forming a pattern or an image (for example, when manufacturing a printed wiring board, etc.), the coating film formed on the substrate may be pattern-exposed, and this pattern exposure may be performed by scanning with laser light or by irradiating light through a photomask. A pattern or an image can be formed by developing (or dissolving) the non-irradiated area (unexposed part) generated by such pattern exposure with a developer.
[0091] The developer may be an aqueous alkaline solution or an organic solvent. Examples of the alkaline aqueous solution include aqueous solutions of alkali metal hydroxides such as potassium hydroxide, sodium hydroxide, potassium carbonate, and sodium carbonate; aqueous solutions of quaternary ammonium hydroxides such as tetramethylammonium hydroxide, tetraethylammonium hydroxide, and choline; and aqueous solutions of amines such as ethanolamine, propylamine, and ethylenediamine.
[0092] The alkaline developer is generally an aqueous solution of 10% by mass or less, and preferably an aqueous solution of 0.1% by mass to 3.0% by mass, etc. Furthermore, alcohols and surfactants may be added to the developer, and each of these is preferably 0.05 parts by mass to 10 parts by mass relative to 100 parts by mass of the developer. Of these, an aqueous solution of 0.1% by mass to 2.38% by mass of tetramethylammonium hydroxide can be used. In addition, the organic solvent used as the developer can be a general organic solvent, such as acetone, acetonitrile, toluene, dimethylformamide, methanol, ethanol, isopropanol, propylene glycol methyl ether, propylene glycol ethyl ether, propylene glycol propyl ether, propylene glycol butyl ether, propylene glycol methyl ether acetate, propylene glycol ethyl ether acetate, propylene glycol propyl ether acetate, propylene glycol butyl ether acetate, ethyl lactate, cyclohexanone, etc., and these can be used alone or in combination of two or more. In particular, propylene glycol methyl ether, propylene glycol methyl ether acetate, ethyl lactate, etc. can be preferably used.
[0093] In the present invention, an adhesion promoter can be added for the purpose of improving the adhesion to the substrate after development. These adhesion promoters include chlorosilanes such as trimethylchlorosilane, dimethylvinylchlorosilane, methyldiphenylchlorosilane, and chloromethyldimethylchlorosilane, alkoxysilanes such as trimethylmethoxysilane, dimethyldiethoxysilane, methyldimethoxysilane, dimethylvinylethoxysilane, diphenyldimethoxysilane, and phenyltriethoxysilane, silazanes such as hexamethyldisilazane, N,N'-bis(trimethylsilyl)urea, dimethyltrimethylsilylamine, and trimethylsilylimidazole, vinyltrichlorosilane, 3-chloropropyltrimethoxysilane, 3-chloropropyltrimethoxysilane, and 3-chloropropyltrimethoxysilane. Examples of the adhesion promoter include silanes such as aminopropyltriethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, and 3-(N-piperidinyl)propyltrimethoxysilane, heterocyclic compounds such as benzotriazole, benzimidazole, indazole, imidazole, 2-mercaptobenzimidazole, 2-mercaptobenzothiazole, 2-mercaptobenzoxazole, urazole, thiouracil, mercaptoimidazole, and mercaptopyrimidine, and ureas such as 1,1-dimethylurea and 1,3-dimethylurea, or thiourea compounds. The adhesion promoters may be used alone or in combination of two or more. The amount of these adhesion promoters added is usually 18% by mass or less, preferably 0.0008% by mass to 9% by mass, and more preferably 0.04% by mass to 9% by mass, based on the solid content.
[0094] The present invention may contain a sensitizer. Examples of sensitizers that can be used include anthracene, phenothiazene, perylene, thioxanthone, and benzophenone thioxanthone. Examples of sensitizing dyes include thiopyrylium salt dyes, merocyanine dyes, quinoline dyes, styrylquinoline dyes, ketocoumarin dyes, thioxanthene dyes, xanthene dyes, oxonol dyes, cyanine dyes, rhodamine dyes, and pyrylium salt dyes. Anthracene sensitizers are particularly preferred, and when used in combination with a cationic curing catalyst (radiation-sensitive cationic polymerization initiator), they dramatically improve sensitivity and also have a radical polymerization initiation function, and in the hybrid type in which the cationic curing system of the present invention and the radical curing system are used in combination, the catalyst species can be simplified. Specific examples of anthracene compounds that are effective include dibutoxyanthracene and dipropoxyanthraquinone. The amount of the sensitizer added is 0.01% by mass to 20% by mass, preferably 0.01% by mass to 10% by mass, based on the solid content.
[0095] The composition of the present invention can be photocured or thermally cured using a photoradical generator, a thermal radical generator, a photoacid generator, or a thermal acid generator. When a photoacid generator or a thermal acid generator is used, for example, commonly used epoxy curing agents (e.g., amines and acid anhydrides) are not used, or even if they are used, the content of these agents is extremely small, so that the storage stability of the composition is improved.
[0096] The composition has been found to be applicable to photocationic polymerization. It has a higher curing speed than conventional liquid epoxy compounds (e.g., alicyclic epoxy compounds having an epoxycyclohexyl ring). Because of the fast curing speed, it is possible to reduce the amount of acid generator added and to use weak acid generators. Reducing the amount of acid generator is important for preventing metal corrosion, since acid active species may remain even after UV irradiation. Because of the fast curing speed, thick film curing is possible.
[0097] Curing by UV irradiation can be applied to materials (equipment) that are sensitive to heat. The film-forming composition of the present invention can be used as a coating agent for steel sheets, and the film formed on the surface of the steel sheet has excellent adhesion to the steel sheet.
[0098] The thermosetting and photocuring materials using the film-forming composition of the present invention have characteristics such as fast curing, transparency, and small shrinkage on curing, and can be used for coating and bonding electronic parts, optical parts (anti-reflection coating), and precision mechanical parts. For example, they can be used for bonding mobile phone and camera lenses, optical elements such as light-emitting diodes (LEDs) and semiconductor lasers (LDs), liquid crystal panels, biochips, camera lenses and prisms, magnetic parts of hard disks of personal computers, CD and DVD player pickups (parts that capture optical information reflected from the disk), speaker cones and coils, motor magnets, circuit boards, electronic parts, etc. As a hard coating material for surface protection of electrical appliances, building materials, plastics, etc., it can be applied to, for example, plastic lenses of glasses, mobile phones, game consoles, optical films, ID cards, etc. Examples of ink materials for printing on metals such as aluminum and plastics include credit cards, membership cards, and other cards, switches for electrical appliances and office equipment, printing ink for keyboards, and inkjet printer ink for CDs, DVDs, etc. Examples of applications include a technology that can be used in combination with 3D CAD to harden resin and create complex three-dimensional objects, photolithography for producing models of industrial products, and optical fiber coatings, adhesives, optical waveguides, and thick-film resists. The film-forming composition of the present invention can also be suitably used as an insulating resin for electronic materials, such as anti-reflection films, semiconductor encapsulation materials, adhesives for electronic materials, printed wiring board materials, interlayer insulating film materials, and encapsulants for power modules, as well as an insulating resin for use in high-voltage equipment, such as generator coils, transformer coils, and gas-insulated switchgear. EXAMPLES
[0099] (Analysis method) [Measurement of SiO2 concentration] The silica sol was placed in a crucible and dried at 100°C. The resulting gel was then fired at 1000°C for 30 minutes, and the firing residue was weighed and calculated. [Measurement of average primary particle size (particle size by nitrogen adsorption method)] The specific surface area of the acidic silica sol powder dried at 300° C. was measured using a specific surface area measuring device (trade name: Monosorb MS-16, manufactured by Yuasa Ionics Co., Ltd.), and the average primary particle size was calculated. [Measurement of average particle size by dynamic light scattering method] Measurement was performed using a dynamic light scattering particle size measurement device (manufactured by Malvern Instruments LTD, trade name ZETASIZER Nano series). For the aqueous silica sol, the sample was diluted with a 0.15 mass % NaCl aqueous solution and then measured. [Measurement of Viscosity] The viscosity of the silica sol at 20° C. was measured using an Ostwald viscometer. [Measurement of the amount of methanol] Equipment used: GC-2014S (manufactured by Shimadzu Corporation) The measurement was performed by gas chromatography. [pH Measurement] Equipment used: MM-43X (manufactured by DKK Toa Corporation) In the case of aqueous silica sol: The silica sol was measured as it was with a pH meter. [Method for Analyzing Sulfur Atom Content Based on Thiol Groups Bonded to Silica Particles] 2g of silica sol and 4g of pure water were put into a 15ml centrifugal filter unit (trade name: Amicon Ultra-15, Merck Ltd.), and centrifuged for 30 minutes at a centrifugal force of 2770G (3000rpm). After centrifugation, the liquid discharged from the bottom of the unit was discarded, and the same mass of pure water as the discarded liquid was added to the concentrated silica sol on the filter to redisperse it, and then centrifuged again for 30 minutes at a rotation speed of 3000rpm. The above process was repeated a total of four times to obtain an aqueous silica sol from which unbonded silane had been removed. 1 g of the aqueous silica sol from which the unbonded silane had been removed was placed in a glass petri dish, heated and dried on a hot plate to remove water, and then pulverized in a mortar. The resulting powder was placed in a 20 ml glass sample tube and vacuum dried (heating temperature 60°C, 30 minutes) to obtain a powder for measurement. The powder thus obtained was measured using an automatic combustion ion chromatograph analyzer (manufactured by JFE Techno-Research Corporation) to obtain the sulfur content S (mass%) in the powder. From the obtained value, the sulfur atom content (sulfur atoms / nm2) based on the thiol groups bonded to the silica particles per unit area was calculated using the following formula: 2 ) was sought. [Sulfur atom content based on thiol groups bound to silica particles per unit area] (pieces / nm 2 )= (S / 32.07×6.02×10 23 ) / (2720 / (average primary particle diameter nm)×10 20 )
[0100] Example 1 An aqueous silica sol, trade name Snowtex O-33 (average primary particle size by BET method: 12 nm, silica concentration: 33.5 mass %, pH: 2.6, manufactured by Nissan Chemical Industries, Ltd.) was prepared. 200 g of the aqueous silica sol was placed in a 1 L recovery flask, and 4.3 g of mercaptomethyltrimethoxysilane (product name X-12-1307, manufactured by Shin-Etsu Chemical Co., Ltd.) was added while stirring the aqueous silica sol with a magnetic stirrer, and the liquid temperature was then maintained at 80° C. for 4 hours. Thereafter, the pressure was adjusted to 150 Torr using a rotary evaporator, and the solvent was evaporated and distilled off at a bath temperature of 80°C. While gradually lowering the pressure to 110 Torr, 80 g of water was supplied to obtain a mercapto group-containing surface-treated aqueous silica sol (silica concentration 30.6 mass%, viscosity (20°C) 4.2 mPa s, methanol 0.01 mass%, pH 2.7, average particle size by dynamic light scattering method 22 nm, sulfur atom content based on thiol groups bound to silica particles per unit area 0.97 / nm 2 ) 224g was obtained. The obtained mercapto group-containing surface-treated aqueous silica sol was placed in a sealed glass container and kept at 50°C for 14 days. After this, the average particle size measured by dynamic light scattering was 26 nm and the viscosity (20°C) was 7.0 mPa·s.
[0101] Example 2 An aqueous silica sol, trade name Snowtex O-33 (average primary particle size by BET method: 12 nm, silica concentration: 33.5 mass %, pH: 2.6, manufactured by Nissan Chemical Industries, Ltd.) was prepared. 500 g of the aqueous silica sol was charged into a 1 L eggplant flask, and while stirring the aqueous silica sol with a magnetic stirrer, 15.26 g of 3-glycidoxypropyltrimethoxysilane (trade name KBM-403, manufactured by Shin-Etsu Chemical Co., Ltd.) was added, and the liquid temperature was maintained at 80° C. for 2 hours. The pH of the resulting sol was 2.8. Next, 5.43 g of mercaptomethyltrimethoxysilane (trade name X-12-1307, manufactured by Shin-Etsu Chemical Co., Ltd.) was added, and the liquid temperature was maintained at 80° C. for 2 hours. Thereafter, the pressure was adjusted to 150 Torr using a rotary evaporator, and the solvent was evaporated and distilled off at a bath temperature of 80°C while the pressure was gradually lowered to 110 Torr while 190 g of water was supplied to obtain a mercapto group-containing surface-treated aqueous silica sol (silica concentration 30.3 mass%, viscosity (20°C) 4.4 mPa s, methanol 0.05 mass%, pH 2.7, average particle size by dynamic light scattering method 21 nm, sulfur atom content based on thiol groups bound to silica particles per unit area 0.44 / nm 2 ) 572g was obtained. The obtained mercapto group-containing surface-treated aqueous silica sol was placed in a sealed glass container and kept at 50°C for 14 days. After that, the average particle size measured by dynamic light scattering was 22 nm, and the viscosity (20°C) was 4.9 mPa·s, indicating that the sol was stable.
[0102] Example 3 An aqueous silica sol, trade name Snowtex O-33 (average primary particle size by BET method: 12 nm, silica concentration: 33.5 mass %, pH: 2.6, manufactured by Nissan Chemical Industries, Ltd.) was prepared. 500 g of the aqueous silica sol was charged into a 1 L eggplant flask, and 15.26 g of 3-glycidoxypropyltrimethoxysilane (trade name KBM-403, manufactured by Shin-Etsu Chemical Co., Ltd.) was added while stirring the aqueous silica sol with a magnetic stirrer, and the liquid temperature was then maintained at 80°C for 2 hours. Next, 1.96 g of an aqueous NaOH solution (10.22 mass%) was added to adjust the pH of the surface-treated aqueous silica sol to 7.0. Thereafter, the liquid temperature was maintained at 80°C for 2 hours. The pH of the obtained sol was 7.2. 5.43 g of mercaptomethyltrimethoxysilane (trade name X-12-1307, manufactured by Shin-Etsu Chemical Co., Ltd.) was added, and the liquid temperature was maintained at 80°C for 2 hours. Thereafter, the pressure was adjusted to 150 Torr using a rotary evaporator, and the solvent was evaporated and distilled off at a bath temperature of 80°C while gradually lowering the pressure to 110 Torr while supplying 190 g of water to obtain a mercapto group-containing surface-treated aqueous silica sol (silica concentration 30.5 mass%, viscosity (20°C) 7.7 mPa s, methanol 0.05 mass%, pH 7.5, average particle size by dynamic light scattering method 21 nm, sulfur atom content based on thiol groups bound to silica particles per unit area 0.47 / nm 2 )568g was obtained. The obtained mercapto group-containing surface-treated aqueous silica sol was placed in a sealed glass container and kept at 50°C for 14 days. After that, the average particle size measured by dynamic light scattering was 20 nm, and the viscosity (20°C) was 6.0 mPa·s, indicating that the sol was stable.
[0103] Example 4 An aqueous silica sol, trade name Snowtex O-33 (average primary particle size by BET method: 12 nm, silica concentration: 33.5 mass %, pH: 2.6, manufactured by Nissan Chemical Industries, Ltd.) was prepared. 500 g of the aqueous silica sol was charged into a 1 L eggplant flask, and 22.89 g of 3-glycidoxypropyltrimethoxysilane (trade name KBM-403, manufactured by Shin-Etsu Chemical Co., Ltd.) was added while stirring the aqueous silica sol with a magnetic stirrer, and the liquid temperature was then maintained at 80° C. for 2 hours. The pH of the resulting sol was 2.8. Next, 3.83 g of 3-mercaptopropyltrimethoxysilane (trade name KBM-803, manufactured by Shin-Etsu Chemical Co., Ltd.) was added, and the liquid temperature was then maintained at 80° C. for 2 hours. Thereafter, the pressure was adjusted to 150 Torr using a rotary evaporator, and the solvent was evaporated and distilled off at a bath temperature of 80°C while gradually lowering the pressure to 110 Torr while supplying 190 g of water to obtain a mercapto group-containing surface-treated aqueous silica sol (silica concentration 30.5 mass%, viscosity (20°C) 6.9 mPa s, methanol 0.02 mass%, pH 2.7, average particle size by dynamic light scattering method 23 nm, sulfur atom content based on thiol groups bound to silica particles per unit area 0.20 / nm 2 )565g was obtained. The obtained mercapto group-containing surface-treated aqueous silica sol was placed in a sealed glass container and kept at 50°C for 14 days. After this, the average particle size measured by dynamic light scattering was 26 nm and the viscosity (20°C) was 9.3 mPa·s.
[0104] Example 5 An aqueous silica sol, trade name Snowtex O-40 (average primary particle size by BET method: 22 nm, silica concentration: 40.5% by mass, pH: 2.4, manufactured by Nissan Chemical Industries, Ltd.) was prepared. 500 g of the aqueous silica sol was charged into a 1 L eggplant flask, and while stirring the aqueous silica sol with a magnetic stirrer, 10.13 g of 3-glycidoxypropyltrimethoxysilane (trade name KBM-403, manufactured by Shin-Etsu Chemical Co., Ltd.) was added, and the liquid temperature was maintained at 80° C. for 2 hours. The pH of the resulting sol was 2.7. Next, 7.22 g of mercaptomethyltrimethoxysilane (trade name X-12-1307, manufactured by Shin-Etsu Chemical Co., Ltd.) was added, and the liquid temperature was maintained at 80° C. for 2 hours. Thereafter, 429 g of water was supplied while evaporating and distilling off the solvent in a rotary evaporator at a pressure of 150 Torr to 110 Torr and a bath temperature of 80°C, to obtain a mercapto group-containing surface-treated aqueous silica sol (silica concentration 30.9 mass%, viscosity (20°C) 4.7 mPa s, methanol 0.04 mass%, pH 3.4, average particle size by dynamic light scattering method 36 nm, sulfur atom content based on thiol groups per unit area bonded to silica particles 0.93 / nm 2 )672g was obtained. The obtained mercapto group-containing surface-treated aqueous silica sol was placed in a sealed glass container and kept at 50°C for 14 days. After that, the average particle size measured by dynamic light scattering was 38 nm, and the viscosity (20°C) was 4.9 mPa·s, indicating that the sol was stable.
[0105] Example 6 An aqueous silica sol, trade name Snowtex OL (average primary particle size by BET method: 45 nm, silica concentration: 20.5 mass %, pH: 2.7, manufactured by Nissan Chemical Industries, Ltd.) was prepared. 500 g of the aqueous silica sol was charged into a 1 L eggplant flask, and 2.42 g of 3-glycidoxypropyltrimethoxysilane (trade name KBM-403, manufactured by Shin-Etsu Chemical Co., Ltd.) was added while stirring the aqueous silica sol with a magnetic stirrer, and the liquid temperature was then maintained at 80° C. for 2 hours. The pH of the resulting sol was 3.0. Next, 1.68 g of mercaptomethyltrimethoxysilane (trade name X-12-1307, manufactured by Shin-Etsu Chemical Co., Ltd.) was added, and the liquid temperature was then maintained at 80° C. for 2 hours. Thereafter, 160 g of water was supplied while evaporating and distilling off the solvent in a rotary evaporator at a pressure of 150 Torr to 110 Torr and a bath temperature of 80°C, to obtain a mercapto group-containing surface-treated aqueous silica sol (silica concentration 30.8 mass%, viscosity (20°C) 3.0 mPa·s, methanol 0.01 mass%, pH 2.9, average particle size by dynamic light scattering method 76 nm, sulfur atom content based on thiol groups per unit area bonded to silica particles 0.62 / nm 2 ) 337g was obtained. The obtained mercapto group-containing surface-treated aqueous silica sol was placed in a sealed glass container and kept at 50°C for 14 days. After that, the average particle size measured by dynamic light scattering was 77 nm, and the viscosity (20°C) was 3.1 mPa·s, indicating that the sol was stable.
[0106] Example 7 An aqueous silica sol, trade name Snowtex O-40 (average primary particle size by BET method: 22 nm, silica concentration: 40.5% by mass, pH: 2.4, manufactured by Nissan Chemical Industries, Ltd.) was prepared. 300 g of the aqueous silica sol was charged into a 1 L eggplant flask, and while stirring the aqueous silica sol with a magnetic stirrer, 6.08 g of 3-glycidoxypropyltrimethoxysilane (trade name KBM-403, manufactured by Shin-Etsu Chemical Co., Ltd.) was added, and the liquid temperature was maintained at 80°C for 2 hours. The pH of the obtained sol was 2.7. Next, 2.17 g of mercaptomethyltrimethoxysilane (trade name X-12-1307, manufactured by Shin-Etsu Chemical Co., Ltd.) was added, and the liquid temperature was maintained at 80°C for 2 hours. The pH of the obtained sol was 2.7. Next, 0.60 g of 3-acryloxypropyltrimethoxysilane (trade name KBM-5103, manufactured by Shin-Etsu Chemical Co., Ltd.) was added, and the liquid temperature was maintained at 80°C for 2 hours. Thereafter, 333 g of water was supplied while evaporating and distilling off the solvent in a rotary evaporator at a pressure of 150 Torr to 110 Torr and a bath temperature of 80°C, to obtain a mercapto group-containing surface-treated aqueous silica sol (silica concentration 31.2 mass%, viscosity (20°C) 4.6 mPa s, methanol 0.01 mass%, pH 3.8, average particle size by dynamic light scattering method 36 nm, sulfur atom content based on thiol groups per unit area bonded to silica particles 0.42 / nm 2 ) 398g was obtained. The obtained mercapto group-containing surface-treated aqueous silica sol was placed in a sealed glass container and kept at 50°C for 14 days. After that, the average particle size measured by dynamic light scattering was 37 nm, and the viscosity (20°C) was 4.5 mPa·s, indicating that the sol was stable.
[0107] Example 8 An aqueous silica sol, trade name Snowtex O-40 (average primary particle size by BET method: 22 nm, silica concentration: 40.5% by mass, pH: 2.4, manufactured by Nissan Chemical Industries, Ltd.) was prepared. 300 g of the aqueous silica sol was charged into a 1 L eggplant flask, and 9.12 g of 3-glycidoxypropyltrimethoxysilane (trade name KBM-403, manufactured by Shin-Etsu Chemical Co., Ltd.) was added while stirring the aqueous silica sol with a magnetic stirrer, and the liquid temperature was maintained at 80°C for 2 hours. The pH of the obtained sol was 2.7. Next, 2.17 g of mercaptomethyltrimethoxysilane (trade name X-12-1307, manufactured by Shin-Etsu Chemical Co., Ltd.) was added, and the liquid temperature was maintained at 80°C for 2 hours. The pH of the obtained sol was 2.7. Next, 0.60 g of 3-acryloxypropyltrimethoxysilane (trade name KBM-5103, manufactured by Shin-Etsu Chemical Co., Ltd.) was added, and the liquid temperature was maintained at 80°C for 2 hours. Thereafter, 333 g of water was supplied while evaporating and distilling off the solvent in a rotary evaporator at a pressure of 150 Torr to 110 Torr and a bath temperature of 80°C, to obtain a mercapto group-containing surface-treated aqueous silica sol (silica concentration 30.5 mass%, viscosity (20°C) 5.1 mPa s, methanol 0.01 mass%, pH 3.5, average particle size by dynamic light scattering method 35 nm, sulfur atom content based on thiol groups per unit area bonded to silica particles 0.25 / nm 2 ) 409g was obtained. The obtained mercapto group-containing surface-treated aqueous silica sol was placed in a sealed glass container and kept at 50°C for 14 days. After that, the average particle size measured by dynamic light scattering was 35 nm, and the viscosity (20°C) was 5.1 mPa·s, indicating that the sol was stable.
[0108] Comparative Example 1 An aqueous silica sol, trade name Snowtex O-33 (average primary particle size by BET method: 12 nm, silica concentration: 33.5 mass %, pH: 2.6, manufactured by Nissan Chemical Industries, Ltd.) was prepared. 500 g of the aqueous sol was placed in a 1 L recovery flask, and 22.89 g of 3-glycidoxypropyltrimethoxysilane (product name KBM-403, manufactured by Shin-Etsu Chemical Co., Ltd.) was added while stirring the sol with a magnetic stirrer, and the liquid temperature was then maintained at 80° C. for 4 hours. Thereafter, 190 g of water was supplied while evaporating and distilling off the solvent in a rotary evaporator at a pressure of 150 Torr to 110 Torr and a bath temperature of 80°C, yielding 561 g of an aqueous surface-treated silica sol (silica concentration 30.5 mass%, viscosity (20°C) 5.2 mPa s, methanol 0.01 mass%, pH 2.8, average particle size measured by dynamic light scattering method 22 nm).
[0109] Comparative Example 2 An aqueous silica sol, trade name Snowtex O-33 (average primary particle size by BET method: 12 nm, silica concentration: 33.5 mass %, pH: 2.6, manufactured by Nissan Chemical Industries, Ltd.) was prepared. 500 g of the aqueous silica sol was charged into a 1 L eggplant flask, and 15.26 g of 3-glycidoxypropyltrimethoxysilane (trade name KBM-403, manufactured by Shin-Etsu Chemical Co., Ltd.) was added while stirring the aqueous silica sol with a magnetic stirrer, and the liquid temperature was then maintained at 80° C. for 2 hours. Next, 8.30 g of an aqueous NaOH solution (10.22 mass%) was added to adjust the pH of the surface-treated aqueous silica sol to 9.0. Then, the liquid temperature was maintained at 80° C. for 2 hours. Next, mercaptomethyltrimethoxysilane (trade name KBM-803, manufactured by Shin-Etsu Chemical Co., Ltd.) was added, and the entire sol gelled.
[0110] [Adhesion evaluation test] <Silica sol> The following silica sols were prepared: Aqueous surface-treated silica sols prepared in Examples 1 to 8 and Comparative Example 1 Product name: Snowtex 30 (average primary particle size by BET method: 12 nm, silica concentration: 30.5% by mass, pH: 9.9, manufactured by Nissan Chemical Industries, Ltd.) Product name: Snowtex O-33 (average primary particle size by BET method: 12 nm, silica concentration: 33.5% by mass, pH: 2.6, manufactured by Nissan Chemical Industries, Ltd.) <Resin> The following resin emulsions were prepared: Product name: Polysol S-65 (main component: vinyl acetate resin, solid content: 50.5% by mass, manufactured by Showa Denko K.K.) Product name: Hydran AP-40F (main component: polyester resin, solid content: 22.5% by mass, manufactured by DIC Corporation) <How to prepare the coating solution> The silica sol of Examples 1 to 8 or Comparative Example 1 was added to the resin emulsion so that the amount of silica added to the resin was 67 phr, and then the coating liquid was diluted with pure water to a solid content of 20 mass % to prepare a silica-containing resin emulsion coating liquid (Table 1). In addition, in Reference Example 1, when only the resin emulsion was used, the coating liquid was diluted with pure water to a solid content of 20 mass %. In Reference Examples 2 and 3, Snowtex 30 (trade name) or Snowtex O-33 (trade name) was added, and then the coating liquid was diluted with pure water to a solid content of 20 mass % to prepare a silica-containing resin emulsion coating liquid. <Coating method> The following Cu plates were prepared: Plate thickness: 0.5 mm, dimensions: width 200 mm x length 365 mm, Cu plate (product name HC0526, manufactured by Hikari Co., Ltd.) The protective sheet was removed from the Cu plate and the plate was wiped with acetone to degrease it. Then, each coating liquid was dropped onto the Cu plate and coated at a speed of 0.5 m / min with a wet coating thickness of 41 μm using a tabletop wire bar coater (PM-9050MC, manufactured by SMT Corporation). The plate was then dried at 80°C for 5 minutes to obtain a Cu plate with a coating.
[0111] <Adhesion evaluation> The adhesion of the coating film to the Cu plate was evaluated by the cross-cut method according to the following method, with reference to JIS K5600-5-6. A cutting tool was used to cut 100 1.5 mm square grid patterns (10 rows x 10 columns) on the coating surface, and 20 mm wide cellophane adhesive tape was placed over the grids. The tape was then gripped by its edge and peeled off in 0.5 to 1.0 seconds, and the presence or absence of peeling on the coating film and the number of peeled areas (number of grids) were visually checked and evaluated according to the following criteria. <Judgment criteria> A: 90 or more squares that do not peel off B: Number of unpeeled squares is 60 or more but less than 90 C: Number of unpeeled squares is between 40 and 60 D: The number of grids that do not peel off is 40 or less. <Coating solution composition and adhesion evaluation results> The coating solution composition and the results of the adhesion evaluation are shown in Tables 1 and 2.
[0112] [Table 1]
[0113] [Table 2]
[0114] [Scratch Resistance Evaluation Test] <Silica sol> The following silica sols were prepared: Aqueous surface-treated silica sols prepared in Examples 1, 2, 4 and Comparative Example 1 Product name: Snowtex 30 (average primary particle size by BET method: 12 nm, silica concentration: 30.5% by mass, pH: 9.9, manufactured by Nissan Chemical Industries, Ltd.) Product name: Snowtex O-33 (average primary particle size by BET method: 12 nm, silica concentration: 33.5% by mass, pH: 2.6, manufactured by Nissan Chemical Industries, Ltd.) <Resin> A product name UAW-1000W30 (main component: 10-functional urethane acrylate resin emulsion, solvent: water, solid content: 30% by mass, manufactured by Kyoeisha Chemical Co., Ltd.) was prepared. <How to prepare the coating solution> The silica sols of Examples 2, 4, and 5 to 8 and Comparative Example 1 were added to the resin emulsion so that the amount of silica added to the resin was 50 phr, and then the mixture was diluted with pure water so that the solid content of the coating liquid was 30 mass %. A photopolymerization initiator, Omnirad2959, was added in an amount of 4 mass % relative to the resin component to prepare a silica-blended resin emulsion coating liquid. In addition, in the case of only the resin emulsion in Reference Example 1, the same amount of photopolymerization initiator was added to prepare a resin emulsion coating solution. In Reference Examples 2 and 3, after adding Snowtex 30 or Snowtex O-33, the coating solution was diluted with pure water so that the solid content of the coating solution became 30% by mass. A photopolymerization initiator, Omnirad 2959, was added in an amount of 4% by mass relative to the resin component to prepare a silica-blended resin emulsion coating solution. <Coating method> The following PET films were prepared: Film thickness: 0.1 mm, dimensions: width 210 mm x length 297 mm PET film (product name: Cosmos Shine A4100#100, manufactured by Toyobo Co., Ltd.) Each coating solution was dropped onto a PET film and coated at a speed of 1.0 m / min using a wire bar coater (wet coating thickness 31 μm), and then dried at 80° C. for 3 minutes. Then, a conveyor-type UV curing device (product name EYE INVERTOR GRANDAGE (4KW) manufactured by EYE GRAPHICS Co., Ltd.) was used to apply the coating solution at an irradiation dose of 620 mJ / cm. 2 The resulting cured film was evaluated for transparency by visual inspection. <Scratch resistance evaluation (steel wool (SW) resistance test)> The surface of the obtained coating film (the surface of the low refractive index layer) was attached to a reciprocating abrasion tester (product name: HEIDON TRIBOGEAR TYPE: 30S, manufactured by Shinto Scientific Co., Ltd.), and the surface of the coating film was repeatedly rubbed 10 times with steel wool under a load of 1.0 kg, and the number of scratches on the surface was visually confirmed. The coating solution composition and the abrasion resistance results are shown in Tables 3 and 4. <Coating liquid composition and abrasion evaluation results>
[0115] [Table 3]
[0116] [Table 4] [Industrial Applicability]
[0117] The present invention provides an aqueous silica sol having a pH of 2 to 7.5, in which silica particles coated with a mercapto group-containing silane compound are dispersed in an aqueous medium.
Claims
1. An aqueous silica sol having a pH of 2 to 7.5, comprising silica particles coated with a silane compound (a) containing a mercapto group or a hydrolysate thereof, The silica particles are represented by the formula (1): [Formula 1] (in formula (1), R 1 is an alkyl group having 1 to 5 carbon atoms containing a mercapto group and bonded to a silicon atom via a Si-C bond, R 2 is an alkoxy group, and a is an integer of 1 to 3), or an aqueous silica sol coated with a silane compound represented by the following formula (1):
2. 2. The aqueous silica sol according to claim 1, wherein the residual alcohol content in the aqueous dispersion medium is 1.0% by mass or less.
3. The silica particles according to claim 1 , comprising a silane compound (a) containing a mercapto group or a hydrolyzate thereof and a compound represented by any one of the formulas (2) to (4): [Case 2] (In formula (2), R 3 are each an alkenyl group, an aryl group, or an organic group having an epoxy group, a (meth)acryloyl group, an amino group, or a ureido group, and are bonded to a silicon atom by a Si-C bond; R 4 each represents an alkoxy group; b represents an integer of 1 to 3; In formula (3) and formula (4), R 5 and R 7 are each an aryl group having 6 to 30 carbon atoms and bonded to a silicon atom by a Si—C bond, R 6 and R 8 each represents an alkoxy group, Y represents an alkylene group, an NH group, or an oxygen atom, c is an integer of 1 to 3, d is an integer of 0 or 1, and e is an integer of 1 to 3.)
4. The silica sol according to claim 3, having a pH of 6.0 to 7.
5.
5. The total amount of the silane compounds of the formulas (1) to (4) is, in terms of the coating amount of the silica particle surface coated with the silane compounds of the formulas (1) to (4) or their hydrolysates, 0.3 silicon atoms / nm in terms of the number of silicon atoms in the silane compounds. 2 ~5.0 pieces / nm 2 The silica sol according to claim 3, wherein the range is
6. 2. The silica sol according to claim 1, wherein the average particle size of silica particles contained in the silica sol is 5 nm to 200 nm as measured by a dynamic light scattering method.
7. A resin composition comprising silica particles derived from the silica sol according to any one of claims 1 to 6 and a resin.
8. 7. An emulsion composition comprising silica particles derived from the silica sol according to claim 1 and a water-soluble resin having a hydroxyl group, a carboxyl group, an ester group, an amide group, or an ether bond.
9. A coating composition comprising silica particles derived from the silica sol according to any one of claims 1 to 6 and a hydrophobic resin containing a hydroxyl group, a carboxyl group, an ester group, an amide group, or an ether bond.
10. A polymerizable composition comprising silica particles derived from the silica sol according to claim 1 and a polymerizable resin.
11. The following steps (A) to (C): Step (A): preparing an aqueous silica sol having a pH of 2 to 7.5; Step (B): The aqueous silica sol obtained in step (A) is treated with a silane compound having a mercapto group ( a step of adding a silane compound (a) containing a mercapto group and at least one silane compound (b) selected from the group consisting of the following formulas (2) to (4); Step (C): A step of removing the alcohol having 1 to 5 carbon atoms from the aqueous medium of the aqueous silica sol obtained in step (B); The method for producing the aqueous silica sol according to any one of claims 1 to 6, comprising:
12. The method for producing an aqueous silica sol according to claim 11, wherein the step (B) is a step (B-1) of adding at least one silane compound (b) selected from the group consisting of formula (2) to formula (4) to the aqueous silica sol obtained in the step (A), adjusting the pH to 6 to 7.5 with a basic substance, and then adding a silane compound (a) containing a mercapto group.
Citation Information
Patent Citations
Organic-inorganic hybrid copolymer and method for producing the same
JP2003226706A
Aqueous siloxane coating composition and its production method, surface treatment agent, surface-treated steel material, and coated steel material
JP2011246636A
Aqueous silane-treated silica dispersion
JP2012520227A
Coated particle and conductive material containing the same
JP2021097040A
Coating composition containing polymer-type silane coupling agent having alkoxysilyl group and mercapto group on side chain