Support, zeolite membrane composite, method for producing zeolite membrane composite, and separation method
By controlling support thickness variations, the zeolite membrane composite achieves uniform and thin zeolite films, enhancing separation efficiency in mixed substance applications.
Patent Information
- Application Number
- JP2020548086
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-09-28
- Filing Date
- 2019-08-02
- Publication Date
- 2024-11-27
- Estimated Expiration
- 2039-08-02
AI Technical Summary
Existing zeolite membrane composites face challenges in achieving uniform film thickness due to variations in support thickness, leading to non-uniform zeolite membrane formation and reduced yield of dense and thin films.
A porous cylindrical support with controlled thickness variations, where the maximum and minimum thickness values satisfy specific ratios, ensuring uniform zeolite membrane formation by hydrothermal synthesis.
The solution enables the production of a zeolite membrane composite with high uniformity and thickness, allowing for efficient separation of mixed substances, particularly gases with varying permeabilities.
Smart Images

Figure 0007590869000002 
Figure 0007590869000003 
Figure 0007590869000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a support used for supporting a zeolite membrane, a zeolite membrane composite including the support and a method for producing the same, and a method for separating a mixed substance by utilizing the zeolite membrane composite. [Background technology]
[0002] Currently, various research and development efforts are being conducted on forming a zeolite membrane composite on a porous support to utilize the molecular sieving action of zeolite for applications such as separation of specific molecules and adsorption of molecules.
[0003] For example, Japanese Patent Laid-Open Publication No. 9-71481 (Document 1) discloses a ceramic support used as a support for a zeolite membrane. Japanese Patent Laid-Open Publication No. 2012-66241 (Document 2) and International Publication No. 2007 / 105407 (Document 3) disclose a zeolite membrane composite in which a zeolite membrane is formed by hydrothermal synthesis on the outer surface of a cylindrical ceramic support.
[0004] Incidentally, cylindrical ceramic supports (hereinafter simply referred to as "supports") are generally produced by extrusion molding and surface polishing. Specifically, first, a clay prepared by kneading predetermined raw materials is fed into a die, and is extruded from the die while being formed into a cylindrical shape. Next, the roughly cylindrical molded body extruded from the die is fired, and then the outer surface of the fired body is polished so that the cross-sectional shape of the outer surface becomes roughly a perfect circle, thereby forming the support.
[0005] In the preparation of the cylindrical support, the radial thickness of the support may vary in the circumferential direction due to the variation in the feed rate when the clay is fed into the mold. The variation in the radial thickness of the support may also be caused by the unevenness of the amount of polishing when the outer surface is polished. Specifically, when the member is extruded from the mold, the cylindrical molded body may spread laterally due to gravity, and the cross-sectional shape of the outer surface and the inner surface may become a horizontally elongated approximately ellipse. In this case, in order to make the cross-sectional shape of the outer surface closer to a perfect circle, the amount of polishing of the side of the support is greater than the amount of polishing of the top and bottom. As a result, the thickness of the side of the support becomes thinner than the thickness of the top and bottom.
[0006] When attempting to form a zeolite membrane on a cylindrical support having such thickness variation, the amount of seed crystals applied per unit area varies greatly when the support surface is coated with seed crystals, resulting in a decrease in the uniformity of the membrane thickness. Therefore, it is difficult to form a dense and thin zeolite membrane with a high yield. However, no study has been conducted from the perspective of the extent to which the thickness variation of the support needs to be suppressed in order to form a dense and thin zeolite membrane. Summary of the Invention
[0007] The present invention is directed to a porous cylindrical support used to support a zeolite membrane. The support according to a preferred embodiment of the present invention comprises an inner surface having a substantially cylindrical shape centered on a central axis extending in the longitudinal direction, and an outer surface having a substantially cylindrical shape surrounding the periphery of the inner surface. The maximum value A and the minimum value B in the circumferential direction of the support thickness, which is the radial distance between the inner surface and the outer surface, are Over the entire length, 0.09≦ (AB) / (A+B)≦0.3 is satisfied, which can improve the uniformity of the thickness of the zeolite membrane.
[0008] good Preferably, in at least a portion in the longitudinal direction, the maximum value A and the minimum value B satisfy 0.18≦(AB) / (A+B)≦0.3. More preferably, the maximum value A and the minimum value B satisfy 0.18≦(AB) / (A+B)≦0.3 over the entire length in the longitudinal direction.
[0009] Preferably, the maximum value A and the minimum value B satisfy (AB) / (A+B)≦0.2 in at least a portion in the longitudinal direction.
[0010] Preferably, the average radius X and the circularity Y of the inner surface in the at least one portion in the longitudinal direction satisfy Y / X≦0.5.
[0011] Preferably, the support is formed of a sintered ceramic body.
[0012] The present invention is also directed to a zeolite membrane composite. A zeolite membrane composite according to a preferred embodiment of the present invention comprises the above-mentioned support and a zeolite membrane formed on the support.
[0013] Preferably, the maximum number of rings in the zeolite constituting the zeolite membrane is 8 or less.
[0014] Preferably, the zeolite membrane has a thickness of 1 μm or less. Preferably, the thickness a of the zeolite membrane in a portion where the support thickness is the maximum value A and the thickness b of the zeolite membrane in a portion where the support thickness is the minimum value B satisfy |ab| / ((a+b) / 2)≦10%.
[0015] The present invention is also directed to a method for producing a zeolite membrane composite. A method for producing a zeolite membrane composite according to a preferred embodiment of the present invention includes the steps of: a) preparing seed crystals; mentioned above and c) a step of growing zeolite from the seed crystals by hydrothermal synthesis to form a zeolite membrane on the support.
[0016] The present invention is also directed to a separation method. A separation method according to a preferred embodiment of the present invention comprises: d) mentioned aboveand e) supplying a mixed substance containing a plurality of types of gases or liquids to the zeolite membrane composite and separating a highly permeable substance in the mixed substance from the mixed substance by permeating the zeolite membrane composite.
[0017] Preferably, the mixture contains one or more of hydrogen, helium, nitrogen, oxygen, water, water vapor, carbon monoxide, carbon dioxide, nitrogen oxides, ammonia, sulfur oxides, hydrogen sulfide, sulfur fluoride, mercury, arsine, hydrogen cyanide, carbonyl sulfide, C1-C8 hydrocarbons, organic acids, alcohols, mercaptans, esters, ethers, ketones, and aldehydes.
[0018] The above and other objects, features, aspects and advantages will become apparent from the following detailed description of the invention which proceeds with reference to the accompanying drawings. [Brief description of the drawings]
[0019] [Figure 1] FIG. 2 is a cross-sectional view of a zeolite membrane composite. [Diagram 2] FIG. 2 is an enlarged cross-sectional view of a zeolite membrane composite. [Diagram 3] FIG. [Figure 4] FIG. 2 is a diagram showing a flow of production of a zeolite membrane composite. [Diagram 5] FIG. 2 shows a zeolite membrane composite in the process of being produced. [Figure 6] FIG. [Figure 7] FIG. 1 is a diagram showing the flow of separation of a mixed material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] Fig. 1 is a cross-sectional view of a zeolite membrane composite 1. Fig. 2 is an enlarged cross-sectional view of a portion of the zeolite membrane composite 1. The zeolite membrane composite 1 includes a porous support 11 and a zeolite membrane 12 formed on the support 11. In Fig. 1, the zeolite membrane 12 is drawn with a thick line. In Fig. 2, the zeolite membrane 12 is drawn with parallel oblique lines. Furthermore, in Fig. 2, the thickness of the zeolite membrane 12 is drawn thicker than it actually is.
[0021] The support 11 is a cylindrical member. The support 11 is a porous member that is permeable to gas and liquid. The support 11 has an inner side surface 113 that is substantially cylindrical and centered on a central axis J1 extending in the longitudinal direction (i.e., the left-right direction in FIG. 1), and an outer side surface 112 that is substantially cylindrical and surrounds the periphery of the inner side surface 113. The central axis J1 is the central axis of an imaginary cylinder disposed so as to circumscribe the inner side surface 113. In the radial direction (hereinafter also simply referred to as the "radial direction") centered on the central axis J1, the outer side surface 112 is located outside the inner side surface 113 and surrounds the periphery of the inner side surface 113. A zeolite membrane 12 is formed on the outer side surface 112. The zeolite membrane 12 covers substantially the entire surface of the outer side surface 112 of the support 11. In the following description, the substantially cylindrical space radially inside the inner side surface 113 is referred to as the "inner flow passage 111."
[0022] The length of the support 11 (i.e., the length in the left-right direction in FIG. 1) is, for example, 10 cm to 200 cm. The outer diameter of the support 11 is, for example, 0.5 cm to 30 cm. The radial distance between the inner surface 113 and the outer surface 112 of the support 11 (hereinafter also referred to as "support thickness") is, for example, 0.1 mm to 10 mm. The surface roughness (Ra) of the support 11 is, for example, 0.1 μm to 5.0 μm, and preferably 0.2 μm to 2.0 μm.
[0023] The material of the support 11 may be any of various substances (e.g., ceramics or metals) as long as it has chemical stability in the process of forming the zeolite membrane 12 on the surface. In this embodiment, the support 11 is formed of a ceramic sintered body. Examples of ceramic sintered bodies selected as the material of the support 11 include alumina, silica, mullite, zirconia, titania, yttria, silicon nitride, and silicon carbide. In this embodiment, the support 11 contains at least one of alumina, silica, and mullite.
[0024] The support 11 may contain an inorganic binder, which may be at least one of titania, mullite, sinterable alumina, silica, glass frit, clay minerals, and sinterable cordierite.
[0025] The average pore diameter of the support 11 near the surface where the zeolite membrane 12 is formed is preferably smaller than the average pore diameter of other parts of the support 11. To realize such a structure, the support 11 has a multilayer structure. When the support 11 has a multilayer structure, the materials of each layer can be those described above, and each layer may be the same or different. The average pore diameter of the support 11 can be measured by a mercury porosimeter, a perm porometer, a nanoperm porometer, or the like.
[0026] The average pore size of the support 11 is, for example, 0.01 μm to 70 μm, and preferably 0.05 μm to 25 μm. Regarding the pore size distribution of the support 11 near the surface on which the zeolite membrane 12 is formed, D5 is, for example, 0.01 μm to 50 μm, D50 is, for example, 0.05 μm to 70 μm, and D95 is, for example, 0.1 μm to 2000 μm. The porosity of the support 11 near the surface on which the zeolite membrane 12 is formed is, for example, 25% to 50%.
[0027] Fig. 3 is a diagram showing a cross section perpendicular to the longitudinal direction of the support 11 (i.e., a cross section perpendicular to the central axis J1). In Fig. 3, the position where the radial distance between the inner surface 113 and the outer surface 112 of the support 11 is maximum in the circumferential direction is indicated by an arrow, and the support thickness at that position is maximum support thickness A. In addition, the position where the radial distance between the inner surface 113 and the outer surface 112 of the support 11 is minimum in the circumferential direction is indicated by an arrow, and the support thickness at that position is minimum support thickness B.
[0028] In the support 11, the maximum value A and the minimum value B of the support thickness in one cross section perpendicular to the central axis J1 satisfy "(AB) / (A+B)≦0.3". In other words, the relationship between the maximum value A and the minimum value B is satisfied over at least a portion of the longitudinal direction of the support 11. Preferably, the relationship between the maximum value A and the minimum value B is satisfied over the entire longitudinal length of the support 11 (i.e., in each cross section in the longitudinal direction).
[0029] Also, preferably, the maximum value A and the minimum value B of the support thickness satisfy "(AB) / (A+B)≦0.2" in at least a part of the longitudinal direction of the support 11. More preferably, the relationship between the maximum value A and the minimum value B of the support thickness is satisfied over the entire longitudinal length of the support 11 (i.e., at each cross section in the longitudinal direction).
[0030] In the support 11, the average radius X and the roundness Y of the inner side surface 113 in the one cross section perpendicular to the central axis J1 satisfy "Y / X≦0.5". In other words, the relationship between the average radius X and the roundness Y is satisfied in at least a part of the longitudinal direction of the support 11. Preferably, the relationship between the average radius X and the roundness Y is satisfied over the entire longitudinal length of the support 11 (i.e., in each cross section in the longitudinal direction). The average radius X in one cross section of the support 11 is the arithmetic mean of the maximum radius and the minimum radius in the cross section. The roundness Y is calculated in accordance with JIS-B-0621. Specifically, in the cross section, the approximately circular shape (i.e., a circular shape) that is the inner side surface 113 is sandwiched between two concentric geometric circles, and the difference between the radii of the two geometric circles when the interval between the two geometric circles is the smallest is defined as the roundness Y.
[0031] The zeolite membrane 12 is a porous membrane having pores. The zeolite membrane 12 can be used as a separation membrane that separates a specific substance from a mixture of a plurality of types of substances by utilizing a molecular sieve effect. Other substances are less likely to permeate the zeolite membrane 12 than the specific substance. In other words, the permeation rate of the other substances through the zeolite membrane 12 is lower than the permeation rate of the specific substance.
[0032] The thickness of the zeolite membrane 12 is, for example, 0.05 μm to 30 μm, preferably 0.1 μm to 20 μm, and more preferably 0.5 μm to 10 μm. The thickness of the zeolite membrane 12 is the minimum value of the distance from the surface of the support 11 to the surface of the zeolite membrane 12 in the entire zeolite membrane 12 excluding defects (i.e., the minimum thickness). The same applies to the following description. In this embodiment, the thickness of the zeolite membrane 12 is 1 μm or less. The average thickness of the zeolite membrane 12 is preferably 5 μm or less, more preferably 3 μm or less, and more preferably 2 μm or less. The separation performance is improved by making the zeolite membrane 12 thicker. The permeation rate is increased by making the zeolite membrane 12 thinner. The surface roughness (Ra) of the zeolite membrane 12 is, for example, 5 μm or less, preferably 2 μm or less, more preferably 1 μm or less, and more preferably 0.5 μm or less.
[0033] The zeolite constituting the zeolite membrane 12 may be a zeolite in which the atom (T atom) located at the center of the oxygen tetrahedron (TO4) constituting the zeolite is only Si or is composed of Si and Al, an AlPO type zeolite in which the T atom is composed of Al and P, a SAPO type zeolite in which the T atom is composed of Si, Al and P, a MAPSO type zeolite in which the T atom is composed of magnesium (Mg), Si, Al and P, or a ZnAPSO type zeolite in which the T atom is composed of zinc (Zn), Si, Al and P. Some of the T atoms may be substituted with other elements.
[0034] When the maximum number of rings in the zeolite constituting the separation membrane 12 is n, the average pore diameter is the arithmetic average of the short diameter and long diameter of the n-membered ring pores. An n-membered ring pore is a pore in which the number of oxygen atoms in a portion in which an oxygen atom is bonded to a T atom to form a ring structure is n. When a zeolite has multiple n-membered ring pores with the same n, the arithmetic average of the short diameter and long diameter of all the n-membered ring pores is the average pore diameter of the zeolite. In this way, the average pore diameter of a zeolite membrane is uniquely determined by the skeletal structure of the zeolite, and is calculated based on the skeletal structure of the zeolite membrane, as described in the "Database of Zeolite Structures" [online] of the International Zeolite Society, the Internet, and the like.<URL:http: / / www.iza-structure.org / databases / > The values can be obtained from the values disclosed in the
[0035] The average pore diameter of the zeolite membrane 12 is preferably 0.2 nm or more and 0.8 nm or less, more preferably 0.3 nm or more and 0.6 nm or less, and even more preferably 0.3 nm or more and 0.5 nm or less. The average pore diameter of the zeolite membrane 12 is smaller than the average pore diameter of the support 11 in the vicinity of the surface on which the zeolite membrane 12 is formed.
[0036] The type of zeolite constituting the zeolite membrane 12 is not particularly limited, but from the viewpoint of increasing the amount of CO2 permeation and improving separation performance, it is preferable that the maximum number of rings of the zeolite is 8 or less (e.g., 6 or 8). The zeolite membrane 12 is, for example, a DDR-type zeolite. In other words, the zeolite membrane 12 is a zeolite membrane composed of zeolite whose structure code is "DDR" defined by the International Zeolite Society. In this case, the intrinsic pore diameter of the zeolite constituting the zeolite membrane 12 is 0.36 nm x 0.44 nm, and the average pore diameter is 0.40 nm.
[0037] The zeolite membrane 12 may be, for example, an AEI type, AEN type, AFN type, AFV type, AFX type, BEA type, CHA type, ERI type, ETL type, FAU type (X type, Y type), GIS type, LEV type, LTA type, MEL type, MFI type, MOR type, PAU type, RHO type, SAT type, SOD type, or other zeolite membrane.
[0038] The zeolite membrane 12 contains, for example, silicon (Si). The zeolite membrane 12 may contain, for example, any two or more of Si, aluminum (Al) and phosphorus (P). The zeolite membrane 12 may contain an alkali metal. The alkali metal is, for example, sodium (Na) or potassium (K). When the zeolite membrane 12 contains Si atoms, the Si / Al ratio in the zeolite membrane 12 is, for example, 1 or more and 100,000 or less. The Si / Al ratio is preferably 5 or more, more preferably 20 or more, and even more preferably 100 or more, and the higher the ratio, the more preferable it is. The Si / Al ratio in the zeolite membrane 12 can be adjusted by adjusting the mixing ratio of the Si source and the Al source in the raw material solution described later.
[0039] Next, an example of a manufacturing flow of the zeolite membrane composite 1 will be described with reference to FIG. 4. When the zeolite membrane composite 1 is manufactured, the support 11 is first formed (step S11). Specifically, ceramic particles, inorganic binder, water, a dispersant, and a thickener are first kneaded to prepare a clay as a raw material of the support 11. The clay is then extruded to form a roughly cylindrical molded body. The molded body is then fired to obtain a roughly cylindrical fired body. The outer surface of the fired body is then polished to form a support member. After that, an intermediate layer, which is a ceramic porous membrane having a pore size smaller than that of the support member, is formed on the outer surface of the support member, and a surface layer, which is a ceramic porous membrane having an even smaller pore size, is formed on the intermediate layer to form the support 11 having a multilayer structure.
[0040] In preparing the above-mentioned clay, for example, 0.1 parts by mass to 50 parts by mass (20 parts by mass in this embodiment) of inorganic binder are added to 100 parts by mass of ceramic particles (alumina particles in this embodiment). The average particle size of the alumina particles is, for example, 1 μm to 200 μm, and is 50 μm in this embodiment. The firing temperature of the above-mentioned molded body is, for example, 1000° C. to 1800° C., and is 1250° C. in this embodiment. The firing time of the above-mentioned molded body is, for example, 0.1 hours to 100 hours, and is 1 hour in this embodiment.
[0041] The outer surface of the sintered body is polished, for example, by a belt-type polishing machine using a fixed grindstone made of fixed diamond abrasive grains, in a belt centerless manner. The polishing method in the polishing process and the type of polishing machine used for the polishing process may be changed in various ways. The intermediate layer and the surface layer described above are, for example, a porous alumina film having a thickness of several μm to several hundred μm. The intermediate layer and the surface layer are formed, for example, by a filtration membrane formation method. The intermediate layer and the surface layer may be formed by other methods. The average pore diameter of the intermediate layer is, for example, 0.1 μm to 10 μm, and in this embodiment, it is 0.5 μm. The average pore diameter of the surface layer is, for example, 0.01 μm to 5 μm, and in this embodiment, it is 0.1 μm.
[0042] Next, seed crystals to be used in manufacturing the zeolite membrane 12 are prepared (step S12). For example, a powder of DDR-type zeolite is produced by hydrothermal synthesis, and the seed crystals are obtained from the powder. The powder of zeolite may be used as the seed crystals as it is, or the powder may be processed by pulverization or the like to obtain the seed crystals. Note that step S12 may be performed in parallel with step S11 or before step S11.
[0043] Next, a seed crystal is attached onto the outer surface 112 of the support 11 (step S13). In step S13, the seed crystal is attached to the support 11 by, for example, a filtration method. Specifically, first, the lower end opening of the support 11, which is erected so that the central axis J1 is parallel to the vertical direction, is sealed liquid-tight, and a substantially cylindrical opening member 83 made of a liquid-tight material is liquid-tightly attached to the upper end opening. Next, as shown in FIG. 5, the support 11 is inserted from the lower end side (i.e., the side to which the seal member 82 is attached) into a storage tank 80 in which a solution 81 in which seed crystals are dispersed is stored, and the support 11 is immersed in the solution 81. The upper end opening of the opening member 83 attached to the upper end of the support 11 is located above the liquid level of the solution 81, and the outer surface 112 of the support 11 is located in the solution 81. As a result, the solvent of the solution 81 moves from the outer surface 112 of the support 11 through the support 11 to the inner flow path 111, as shown by the arrows pointing in the left-right direction in FIG. 5. On the other hand, the seed crystals in the solution 81 do not pass through the support 11, but are left on the outer surface 112 of the support 11 and adhere to the outer surface 112. In this way, a seed crystal-adhered support is produced.
[0044] When step S13 is completed, the support 11 with the seed crystal attached thereto is pulled out of the solution 81 and dried. The dried support 11 with the seed crystal attached thereto is immersed in the raw material solution. The raw material solution is prepared by dissolving and dispersing, for example, a Si source and a structure-directing agent (hereinafter also referred to as "SDA") in a solvent. Water or an alcohol such as ethanol may be used as the solvent for the raw material solution. The SDA contained in the raw material solution is, for example, an organic substance. For example, 1-adamantanamine can be used as the SDA.
[0045] Then, the seed crystals are used as nuclei to grow DDR-type zeolite by hydrothermal synthesis, thereby forming a DDR-type zeolite membrane 12 on the support 11 (step S14). The temperature during the hydrothermal synthesis is preferably 120 to 200° C., for example, 160° C. The hydrothermal synthesis time is preferably 10 to 100 hours, for example, 30 hours.
[0046] After the hydrothermal synthesis is completed, the support 11 and the zeolite membrane 12 are washed with pure water. The washed support 11 and the zeolite membrane 12 are dried, for example, at 80° C. After the support 11 and the zeolite membrane 12 are dried, the zeolite membrane 12 is heat-treated to burn off the SDA in the zeolite membrane 12 almost completely, thereby penetrating the micropores in the zeolite membrane 12 (step S15). As a result, the above-mentioned zeolite membrane composite 1 is obtained.
[0047] In the above-mentioned production of the zeolite membrane composite 1, if there is a large variation in the support thickness in the support 11, the amount of seed crystals attached in step S13 will vary. Specifically, in the portion of the support 11 where the support thickness is thin, the resistance when the solvent of the above-mentioned solution permeates the support 11 is small, so the amount of solvent permeates is large, and the amount of seed crystals attached to the outer surface 112 is also large. On the other hand, in the portion of the support where the support thickness is thick, the resistance when the solvent permeates the support 11 is large, so the amount of solvent permeates is small, and the amount of seed crystals attached to the outer surface 112 is also small. As a result, in the zeolite membrane composite 1, the zeolite membrane 12 is thick in the portion of the support where the support thickness is thin, and the zeolite membrane 12 is thin in the portion of the support where the support thickness is thick, so that the thickness of the zeolite membrane 12 varies.
[0048] Table 1 shows the relationship between the variation in the support thickness of the support 11 in the zeolite membrane composite 1 and the variation in the membrane thickness of the zeolite membrane 12. The approximately cylindrical support 11 in Examples 1 to 7 has an outer diameter of 20 mm and a longitudinal length of 15 cm. The same is true for the support in Comparative Example 1. The zeolite membranes 12 in Examples 1 to 3 and the zeolite membrane in Comparative Example 1 are DDR type zeolite membranes. The zeolite membranes 12 in Examples 4 to 5 are CHA type zeolite membranes. The zeolite membranes 12 in Examples 6 to 7 are AEI type zeolite membranes.
[0049] The zeolite membrane composite 1 of Examples 1 to 7 and the zeolite membrane composite of Comparative Example were produced by substantially the same production method as the production method shown in the above-mentioned steps S11 to S15. Detailed production conditions etc. are shown below.
[0050] In the manufacture of the DDR-type zeolite membrane 12 of Examples 1 to 3, in step S13, a seeding slurry liquid prepared so that the concentration of seed crystals of DDR-type zeolite dispersed in water was 0.1 mass % was used as the above-mentioned solution 81. Then, the support 11 to which the seed crystals were attached was dried by ventilation under predetermined conditions (room temperature, wind speed of 5 m / sec, 10 minutes). In step S14, 88.0 g of 30 wt % silica sol (product name: Snowtex S, manufactured by Nissan Chemical Industries, Ltd.), 6.59 g of ethylenediamine (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), 1.04 g of 1-adamantanamine (manufactured by Sigma-Aldrich Japan LLC), and 104.4 g of pure water were mixed to prepare the above-mentioned raw material solution. In addition, the zeolite membrane 12 was formed by performing hydrothermal synthesis for 10 hours in a hot air dryer at 130°C. The SDA was removed by heating the support 11 on which the zeolite membrane 12 was formed in an electric furnace at 450° C. for 50 hours. The same procedure was followed for the production of the DDR type zeolite membrane of Comparative Example 1.
[0051] In the manufacture of the CHA-type zeolite membrane 12 of Examples 4 to 5, in step S12, seed crystals of CHA-type zeolite were prepared by a structure conversion method of Y-type zeolite or hydrothermal synthesis of an aluminosilicate aqueous solution. In step S13, a seeding slurry liquid adjusted so that the concentration of the CHA-type zeolite seed crystals dispersed in water was 0.1 mass % was used as the above-mentioned solution 81. Then, the support 11 to which the seed crystals were attached was dried by ventilation under predetermined conditions (room temperature, wind speed of 5 m / sec, 10 minutes). In step S14, 21.3 g of 30 wt % silica sol (trade name: Snowtex S, manufactured by Nissan Chemical Industries, Ltd.), 0.90 g of potassium hydroxide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), 1.18 g of sodium aluminate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), 3.58 g of 25 mass % N,N,N-trimethyl-1-adamantan ammonium hydroxide aqueous solution (manufactured by Seichem Co., Ltd.), and 173.1 g of pure water were mixed to prepare the above-mentioned raw material solution. The zeolite membrane 12 was formed by hydrothermal synthesis for 30 hours in a hot air dryer at 160°C. The SDA was removed by heating the support 11 on which the zeolite membrane 12 was formed at 550°C for 10 hours.
[0052] In the manufacture of the AEI zeolite membranes 12 of Examples 6 and 7, in step S12, seed crystals of AEI zeolite were prepared by hydrothermal synthesis of an aluminophosphate aqueous solution or the like. In step S13, a seeding slurry liquid adjusted so that the concentration of the seed crystals of AEI zeolite dispersed in water was 0.1 mass % was used as the above-mentioned solution 81. Then, the support 11 to which the seed crystals were attached was subjected to ventilation drying under predetermined conditions (room temperature, wind speed of 2 m / sec to 7 m / sec, 30 minutes). In step S13, the application of the seeding slurry liquid and ventilation drying were performed twice. In step S14, 4.72 g of aluminum triisopropoxide (Kanto Chemical Co., Ltd.), 30.71 g of 35 mass % tetraethylammonium hydroxide aqueous solution (Sigma-Aldrich Japan LLC), 8.41 g of 85% phosphoric acid (Sigma-Aldrich Japan LLC), and 156.17 g of pure water were mixed to prepare the above-mentioned raw material solution. The zeolite membrane 12 was formed by hydrothermal synthesis at 150°C for 30 hours. The SDA was removed by heating the support 11 on which the zeolite membrane 12 was formed at 400°C for 10 hours.
[0053] [Table 1]
[0054] The variation in support thickness in Table 1 is the above-mentioned "(AB) / (A+B)" in one cross section of support 11. In other words, the variation in support thickness is the difference between the maximum value A and the minimum value B of the support thickness in one cross section of support 11 divided by the sum of the maximum value A and the minimum value B. The larger this value is, the greater the variation in support thickness is.
[0055] The variation in thickness in Table 1 is calculated by dividing the absolute value of the difference between thickness a and thickness b by the arithmetic mean of thickness a and thickness b, where a is the thickness of the zeolite membrane 12 at the portion of the cross section of the support 11 where the support thickness is maximum value A and b is the thickness of the zeolite membrane 12 at the portion of the cross section of the support 11 where the support thickness is minimum value B (i.e., "|ab| / ((a+b) / 2)"). In Table 1, the value is shown as a percentage. The larger the value, the greater the variation in thickness of the zeolite membrane 12.
[0056] The above-mentioned maximum thickness A and minimum thickness B of the support, as well as film thickness a and film thickness b, were determined by cutting the support 11 along a plane perpendicular to the central axis J1 and observing the cross section produced by the cutting using a scanning electron microscope (SEM).
[0057] As shown in Comparative Example 1, when the support thickness variation "(AB) / (A+B)" was greater than 0.3, the thickness variation "|ab| / ((a+b) / 2)" of the DDR-type zeolite membrane 12 was greater than 10%. On the other hand, as shown in Examples 1 to 3, when the support thickness variation "(AB) / (A+B)" was 0.3 or less, the thickness variation "|ab| / ((a+b) / 2)" of the DDR-type zeolite membrane 12 was 10% or less.
[0058] Similarly, for the CHA-type zeolite membrane 12, when the support thickness variation "(AB) / (A+B)" was 0.3 or less, the thickness variation "|ab| / ((a+b) / 2)" of the zeolite membrane 12 was 10% or less (Examples 4 to 5). Similarly, for the AEI-type zeolite membrane 12, when the support thickness variation "(AB) / (A+B)" was 0.3 or less, the thickness variation "|ab| / ((a+b) / 2)" of the zeolite membrane 12 was 10% or less (Examples 6 to 7).
[0059] Next, separation of a mixed substance using the zeolite membrane composite 1 will be described with reference to Fig. 6 and Fig. 7. Fig. 6 is a diagram showing a separation device 2. Fig. 7 is a diagram showing a flow of separation of a mixed substance by the separation device 2.
[0060] In the separation device 2, a mixed substance containing multiple types of fluids (i.e., gases or liquids) is supplied to the zeolite membrane composite 1, and a highly permeable substance in the mixed substance is separated from the mixed substance by permeating the zeolite membrane composite 1. The separation in the separation device 2 may be performed, for example, for the purpose of extracting a highly permeable substance from the mixed substance, or for the purpose of concentrating a less permeable substance.
[0061] The mixed substance (i.e., mixed fluid) may be a mixed gas containing multiple types of gases, a mixed liquid containing multiple types of liquids, or a gas-liquid two-phase fluid containing both gas and liquid.
[0062] In the separation device 2, the CO2 permeation amount (permeance) of the zeolite membrane composite 1 at 20°C to 400°C is, for example, 100 nmol / m 2 s Pa or more. The ratio of the CO2 permeation amount / CH4 leakage amount (permeance ratio) of the zeolite membrane composite 1 at 20°C to 400°C is, for example, 100 or more. The permeance and permeance ratio are those when the partial pressure difference of CO2 between the supply side and the permeation side of the zeolite membrane composite 1 is 1.5 MPa.
[0063] The mixture of substances may include one or more of the following: hydrogen (H2), helium (He), nitrogen (N2), oxygen (O2), water (H2O), water vapor (H2O), carbon monoxide (CO), carbon dioxide (CO2), nitrogen oxides, ammonia (NH3), sulfur oxides, hydrogen sulfide (H2S), sulfur fluoride, mercury (Hg), arsine (AsH3), hydrogen cyanide (HCN), carbonyl sulfide (COS), C1 to C8 hydrocarbons, organic acids, alcohols, mercaptans, esters, ethers, ketones, and aldehydes.
[0064] Nitrogen oxides are compounds of nitrogen and oxygen. Examples of the above-mentioned nitrogen oxides include nitric oxide (NO), nitrogen dioxide (NO2), nitrous oxide (also called dinitrogen monoxide) (N2O), dinitrogen trioxide (N2O3), dinitrogen tetroxide (N2O4), dinitrogen pentoxide (N2O5), etc. X The gas is called NOX.
[0065] Sulfur oxides are compounds of sulfur and oxygen. The above-mentioned sulfur oxides include, for example, sulfur dioxide (SO2), sulfur trioxide (SO3), and other SO X The gas is called SOXX.
[0066] Sulfur fluoride is a compound of fluorine and sulfur. The above-mentioned sulfur fluoride is, for example, disulfur difluoride (FSSF, S = SF2), sulfur difluoride (SF2), sulfur tetrafluoride (SF4), sulfur hexafluoride (SF6) or disulfur decafluoride (S2F 10 ) etc.
[0067] C1-C8 hydrocarbons are those with 1 to 8 carbon atoms. C3-C8 hydrocarbons may be straight-chain compounds, side-chain compounds, or cyclic compounds. C2-C8 hydrocarbons may be saturated hydrocarbons (i.e., those with no double or triple bonds in the molecule) or unsaturated hydrocarbons (i.e., those with double or triple bonds in the molecule). C1-C4 hydrocarbons are, for example, methane (CH4), ethane (C2H6), ethylene (C2H4), propane (C3H8), propylene (C3H6), normal butane (CH3(CH2)2CH3), isobutane (CH(CH3)3), 1-butene (CH2=CHCH2CH3), 2-butene (CH3CH=CHCH3), or isobutene (CH2=C(CH3)2).
[0068] The organic acid may be a carboxylic acid or a sulfonic acid. The carboxylic acid may be, for example, formic acid (CH2O2), acetic acid (C2H4O2), oxalic acid (C2H2O4), acrylic acid (C3H4O2), or benzoic acid (C6H5COOH). The sulfonic acid may be, for example, ethanesulfonic acid (C2H6O3S). The organic acid may be a chain compound or a cyclic compound.
[0069] The above-mentioned alcohols are, for example, methanol (CH3OH), ethanol (C2H5OH), isopropanol (2-propanol) (CH3CH(OH)CH3), ethylene glycol (CH2(OH)CH2(OH)) or butanol (C4H9OH).
[0070] Mercaptans are organic compounds that have hydrogenated sulfur (SH) at the end, and are also called thiols or thioalcohols. Examples of the mercaptans mentioned above include methyl mercaptan (CH3SH), ethyl mercaptan (C2H5SH), and 1-propanethiol (C3H7SH).
[0071] The esters mentioned above are, for example, formates or acetates.
[0072] The above-mentioned ethers are, for example, dimethyl ether ((CH3)2O), methyl ethyl ether (C2H5OCH3) or diethyl ether ((C2H5)2O).
[0073] The above-mentioned ketones are, for example, acetone ((CH3)2CO), methyl ethyl ketone (C2H5COCH3) or diethyl ketone ((C2H5)2CO).
[0074] The above-mentioned aldehydes are, for example, acetaldehyde (CH3CHO), propionaldehyde (C2H5CHO) or butanal (butyraldehyde) (C3H7CHO).
[0075] In the following description, it is assumed that the mixed substance separated by the separation device 2 is a mixed gas containing a plurality of types of gases.
[0076] The separation device 2 includes a zeolite membrane composite 1, a plugging section 21, an outer cylinder 22, a seal member 23, a supply section 26, a first recovery section 27, and a second recovery section 28. The zeolite membrane composite 1, the plugging section 21, and the seal member 23 are housed in the outer cylinder 22. The supply section 26, the first recovery section 27, and the second recovery section 28 are disposed outside the outer cylinder 22 and connected to the outer cylinder 22.
[0077] The sealing parts 21 are attached to both ends of the support 11 in the longitudinal direction (i.e., the left-right direction in FIG. 6) and are members that cover and seal both longitudinal end faces of the support 11 and the outer surfaces near the both end faces. The sealing parts 21 prevent the inflow and outflow of gas from both end faces of the support 11, which are substantially annular. The sealing parts 21 are, for example, plate-like members made of glass or resin. The material and shape of the sealing parts 21 may be changed as appropriate. The right sealing part 21 in FIG. 6 has an opening that overlaps with the inner flow passage 111 of the support 11, so that the right end opening of the inner flow passage 111 is not covered by the sealing part 21. Therefore, the gas in the inner flow passage 111 can flow out from the end opening to the outside of the zeolite membrane composite 1. On the other hand, the left sealing part 21 in FIG. 6 has no opening, so that the gas cannot flow in or out from the left end opening of the inner flow passage 111.
[0078] The outer cylinder 22 is a tubular member having a substantially cylindrical shape. The outer cylinder 22 is formed of, for example, stainless steel or carbon steel. The longitudinal direction of the outer cylinder 22 is substantially parallel to the longitudinal direction of the zeolite membrane composite 1 (i.e., the direction in which the central axis J1 faces). A supply port 221 and a first discharge port 222 are provided on the outer surface of the outer cylinder 22. The supply port 221 and the first discharge port 222 are disposed, for example, on opposite sides in the radial direction (i.e., positions 180° apart in the circumferential direction) across the zeolite membrane composite 1. A second discharge port 223 is provided on one end of the outer cylinder 22 in the longitudinal direction (i.e., the end on the right side in FIG. 6). The supply port 221 is connected to the supply unit 26. The first discharge port 222 is connected to the first recovery unit 27. The second discharge port 223 is connected to the second recovery unit 28. The internal space of the outer cylinder 22 is a sealed space isolated from the space surrounding the outer cylinder 22 .
[0079] The seal member 23 is disposed in the longitudinal direction of the zeolite membrane composite 1. Mukaidate The outer cylinder 22 is disposed between the outer surface of the zeolite membrane composite 1 and the inner surface of the outer cylinder 22 around the entire circumference. . The seal member 23 is a substantially annular member made of a material that is gas impermeable. The seal member 23 is, for example, an O-ring made of a flexible resin. The seal member 23 is in close contact with the outer surface of the zeolite membrane composite 1 and the inner surface of the outer tube 22 over the entire circumference. In the example shown in FIG. 6, the seal member 23 is in close contact with the outer surface of the plug 21 on the right side of the figure, and indirectly in contact with the outer surface of the zeolite membrane composite 1 via the plug 21. The gap between the seal member 23 and the outer surface of the zeolite membrane composite 1 and the gap between the seal member 23 and the inner surface of the outer tube 22 are sealed, and gas is hardly or completely prevented from passing through. The seal member 23 may be provided between the longitudinal end face of the zeolite membrane composite 1 and the outer tube 22.
[0080] The supply unit 26 supplies the mixed gas to the internal space of the outer cylinder 22 via the supply port 221. The supply unit 26 is, for example, a blower or a pump that pressure-feeds the mixed gas toward the outer cylinder 22. The blower or pump includes a pressure adjustment unit that adjusts the pressure of the mixed gas supplied to the outer cylinder 22. The first recovery unit 27 and the second recovery unit 28 are, for example, a storage container that stores the gas derived from the outer cylinder 22, or a blower or a pump that transfers the gas.
[0081] When the mixed gas is separated, the above-mentioned separation device 2 is prepared, and the zeolite membrane composite 1 is prepared (step S21). Then, the supply unit 26 supplies the mixed gas containing a plurality of types of gases having different permeabilities to the zeolite membrane 12 to the internal space of the outer casing 22. For example, the main components of the mixed gas are CO2 and CH4. The mixed gas may contain gases other than CO2 and CH4. The pressure of the mixed gas supplied from the supply unit 26 to the internal space of the outer casing 22 (i.e., the introduction pressure) is, for example, 0.1 MPa to 20.0 MPa. The temperature at which the mixed gas is separated is, for example, 10°C to 150°C.
[0082] The mixed gas supplied from the supply unit 26 to the outer cylinder 22 flows toward the outer surface of the zeolite membrane composite 1 as shown by the arrow 251. A gas having high permeability in the mixed gas (e.g., CO2, hereinafter referred to as a "highly permeable substance") permeates the zeolite membrane 12 provided on the outer surface 112 of the support 11 and the support 11, and is discharged from the inner surface 113 of the support 11 to the inner flow passage 111. As a result, the highly permeable substance is separated from a gas having low permeability in the mixed gas (e.g., CH4, hereinafter referred to as a "lowly permeable substance") (step S22). The gas discharged from the inner surface 113 of the support 11 to the inner flow passage 111 (hereinafter referred to as a "permeating substance") is recovered by the second recovery unit 28 through the second discharge port 223 as shown by the arrow 253. The pressure of the gas recovered by the second recovery section 28 through the second discharge port 223 (i.e., the permeation pressure) is, for example, about 1 atmosphere (0.101 MPa). The permeating substance may include substances other than the above-mentioned highly permeable substances.
[0083] Furthermore, gases other than the gas that has permeated the zeolite membrane 12 and the support 11 (hereinafter referred to as "non-permeating substances") in the mixed gas pass between the outer surface of the zeolite membrane composite 1 and the inner surface of the outer cylinder 22 from the top to the bottom in the figure, and are recovered by the first recovery section 27 through the first discharge port 222, as shown by arrow 252. The pressure of the gas recovered by the first recovery section 27 through the first discharge port 222 is, for example, approximately the same as the introduction pressure. The non-permeating substances may include highly permeable substances that have not permeated the zeolite membrane 12, in addition to the low permeable substances described above.
[0084] As described above, the porous cylindrical support 11 used to support the zeolite membrane 12 includes a substantially cylindrical inner surface 113 centered on a central axis J1 extending in the longitudinal direction, and a substantially cylindrical outer surface 112 surrounding the periphery of the inner surface 113. The zeolite membrane 12 is formed on the outer surface 112. The maximum value A and minimum value B in the circumferential direction of the support thickness, which is the radial distance between the inner surface 113 and the outer surface 112, satisfy "(AB) / (A+B)≦0.3" in at least a portion of the longitudinal direction of the support 11.
[0085] In the support 11, by suppressing the variation in the support thickness in this way, as described above, it is possible to improve the uniformity of the thickness of the zeolite membrane 12 formed on the support 11. Therefore, even when forming a zeolite membrane 12 with a thin average thickness, it is possible to prevent a part of the zeolite membrane 12 from becoming too thin and being damaged. As a result, a dense and thin zeolite membrane 12 can be formed on the support 11.
[0086] As described above, it is preferable that the maximum value A and the minimum value B of the circumferential thickness of the support 11 satisfy "(AB) / (A+B)≦0.3" over the entire longitudinal length of the support 11. This can further improve the uniformity of the thickness of the zeolite membrane 12 formed on the support 11.
[0087] As described above, in the support 11, the maximum value A and the minimum value B of the support thickness in the circumferential direction preferably satisfy "(AB) / (A+B)≦0.2" and more preferably satisfy "(AB) / (A+B)≦0.1" in at least a part of the longitudinal direction of the support 11. This can further improve the uniformity of the thickness of the zeolite membrane 12 formed on the support 11.
[0088] As described above, in the support 11, it is more preferable that the maximum value A and the minimum value B of the support thickness in the circumferential direction satisfy "(AB) / (A+B)≦0.2" and particularly preferable that they satisfy "(AB) / (A+B)≦0.1" over the entire longitudinal length of the support 11. This can further improve the uniformity of the thickness of the zeolite membrane 12 formed on the support 11.
[0089] As described above, in the support 11, the average radius X and the circularity Y of the inner side surface 113 in at least a portion of the longitudinal direction of the support 11 preferably satisfy "Y / X≦0.5", more preferably satisfy "Y / X≦0.3", and further preferably satisfy "Y / X≦0.1". In this way, if the cross-sectional shape of the inner side surface 113 perpendicular to the central axis J1 is relatively close to a perfect circle, the uniformity of the thickness of the support in the circumferential direction can be improved when the outer side surface 112 is brought closer to a perfect circle by polishing or the like during the formation of the support 11. Therefore, the support 11 that satisfies "(AB) / (A+B)≦0.3" in at least a portion of the longitudinal direction can be formed with good yield.
[0090] As described above, in the support 11, it is more preferable that the average radius X and the circularity Y of the inner surface 113 satisfy "Y / X≦0.5" over the entire length of the support 11, more preferably "Y / X≦0.3", and particularly preferably "Y / X≦0.1". This makes it possible to form the support 11 that satisfies "(AB) / (A+B)≦0.3" over the entire length of the support 11 with an even higher yield.
[0091] As described above, it is preferable that the support 11 is made of a sintered ceramic body. This makes it possible to increase the bonding strength between the zeolite membrane 12 and the support 11 compared to a case where the support is made of a material other than the sintered ceramic body, and therefore to stably support the zeolite membrane 12.
[0092] The zeolite membrane composite 1 includes the above-mentioned support 11 and a zeolite membrane 12 formed on the outer surface 112 of the support 11. This makes it possible to provide a zeolite membrane composite 1 including a zeolite membrane 12 with high thickness uniformity. It is therefore possible to provide a zeolite membrane composite 1 including a dense and thin zeolite membrane 12. In other words, in the zeolite membrane composite 1, a thin zeolite membrane 12 can be achieved.
[0093] As described above, in the zeolite membrane composite 1, the zeolite membrane 12 can be made thin, and therefore the structure of the zeolite membrane composite 1 is particularly suitable for zeolite membrane composites in which the thickness (minimum membrane thickness) of the zeolite membrane 12 is 1 μm or less.
[0094] As described above, the maximum number of rings in the zeolite constituting the zeolite membrane 12 is preferably 8 or less. As a result, when the zeolite membrane 12 is used for separating a mixture of substances, selective permeation of a substance to be permeated, such as CO2, which has a relatively small molecular diameter, can be suitably realized, and the substance to be permeated can be efficiently separated from the mixture of substances.
[0095] The above-mentioned method for producing the zeolite membrane composite 1 includes a step of preparing seed crystals (step S12), a step of attaching the seed crystals to the support 11 (step S13), and a step of growing zeolite from the seed crystals by hydrothermal synthesis to form the zeolite membrane 12 on the support 11 (step S14). This makes it possible to provide the zeolite membrane composite 1 including the zeolite membrane 12 with high thickness uniformity. Therefore, it is also possible to provide the zeolite membrane composite 1 including the dense and thin zeolite membrane 12.
[0096] The above-mentioned separation method includes a step (step S21) of preparing the zeolite membrane composite 1, and a step (step S22) of supplying a mixed substance containing a plurality of types of gases or liquids to the zeolite membrane 12 and separating a highly permeable substance in the mixed substance from the mixed substance by permeating the zeolite membrane composite 1. This makes it possible to suitably separate a highly permeable substance (i.e., a highly permeable substance) from the mixed substance.
[0097] The separation method is particularly suitable for separating mixtures containing one or more of the following substances: hydrogen, helium, nitrogen, oxygen, water, water vapor, carbon monoxide, carbon dioxide, nitrogen oxides, ammonia, sulfur oxides, hydrogen sulfide, sulfur fluoride, mercury, arsine, hydrogen cyanide, carbonyl sulfide, C1-C8 hydrocarbons, organic acids, alcohols, mercaptans, esters, ethers, ketones, and aldehydes.
[0098] The support 11, the zeolite membrane composite 1 and the production method thereof, and the method for separating a mixed substance described above can be modified in various ways.
[0099] For example, the support 11 does not necessarily have to be made of a sintered ceramic body, and may be made of other materials such as metal. Furthermore, in the support 11, the average radius X and the circularity Y of the inner surface 113 do not necessarily have to satisfy "Y / X≦0.5". Furthermore, the central axis of the outer surface 112 of the support 11 does not necessarily have to coincide with the central axis J1 of the inner surface 113, and may be different.
[0100] In the zeolite membrane composite 1, the thickness of the zeolite membrane 12 is not limited to 1 μm or less and may be variously changed. The maximum number of rings of the zeolite constituting the zeolite membrane 12 may be greater than or less than eight.
[0101] The support 11 may be manufactured by a manufacturing method different from that of the above example. For example, the polishing of the outer surface may not be performed.
[0102] The above-mentioned zeolite membrane composite 1 may be produced by a production method different from that of the above example. For example, the attachment of the seed crystals to the support 11 may be performed by a method different from that of the above example. In addition, the zeolite membrane 12 may be formed on the inner surface 113 of the support 11, or may be formed on both the outer surface 112 and the inner surface 113 of the support 11.
[0103] The structure of the separation device 2 shown in Fig. 6 may be modified in various ways. For example, an opening overlapping with the inner flow path 111 may be provided in the sealing portion 21 on the left side in Fig. 6, similar to the sealing portion 21 on the right side in Fig. 6, and a sealing member 23 may be provided for sealing, and a second discharge port 223 connected to the second recovery portion 28 may also be provided in the left end face of the outer cylinder 22.
[0104] In the above-described separation device 2 and separation method, substances other than the substances exemplified in the above description may be separated from the mixed substance.
[0105] The zeolite membrane 12 of the zeolite membrane composite 1 does not necessarily have to be used for separating a highly permeable substance from a mixed substance, but may be used for other purposes, such as an adsorption membrane or a pervaporation membrane.
[0106] The configurations in the above-described embodiment and each of the modified examples may be combined as appropriate as long as they are not mutually inconsistent.
[0107] Although the invention has been particularly illustrated and described, it is to be understood that the above description is illustrative and not restrictive, and therefore numerous modifications and variations are possible without departing from the scope of the invention. [Industrial Applicability]
[0108] The support of the present invention can be used, for example, as a support for a zeolite membrane that can be used as a gas separation membrane. The zeolite membrane composite of the present invention can be used in various fields in which zeolites are used as gas separation membranes, separation membranes for materials other than gas, and adsorption membranes for various substances. [Explanation of symbols]
[0109] 1 Zeolite membrane composite 11 Support 12 Zeolite membrane 112 (of support) outer surface 113 (of the support) inner surface A (support thickness in the circumferential direction) Maximum B (support thickness in circumferential direction) minimum J1 center axis S11~S15, S21~S22 steps
Claims
1. A porous cylindrical support used to support a zeolite membrane, comprising: A generally cylindrical inner surface having a central axis extending in a longitudinal direction as a center; A generally cylindrical outer surface surrounding the inner surface; Equipped with The maximum value A and minimum value B in the circumferential direction of the support thickness, which is the radial distance between the inner surface and the outer surface, satisfy 0.09≦(A−B) / (A+B)≦0.3 over the entire longitudinal length.
2. 2. The support according to claim 1, In at least a portion in the longitudinal direction, the maximum value A and the minimum value B satisfy 0.18≦(A−B) / (A+B)≦0.
3.
3. A support according to claim 2, Over the entire length in the longitudinal direction, the maximum value A and the minimum value B satisfy 0.18≦(A−B) / (A+B)≦0.
3.
4. A support according to any one of claims 1 to 3, The maximum value A and the minimum value B satisfy (A−B) / (A+B)≦0.2 in at least a portion in the longitudinal direction.
5. A support according to any one of claims 1 to 4, The average radius X and the circularity Y of the inner surface in at least the portion in the longitudinal direction satisfy Y / X≦0.
5.
6. A support according to any one of claims 1 to 5, It is made of a sintered ceramic body.
7. A zeolite membrane composite, A support according to any one of claims 1 to 6, A zeolite membrane formed on the support; and Equipped with.
8. The zeolite membrane composite according to claim 7, The maximum number of ring members of the zeolite constituting the zeolite membrane is 8 or less.
9. The zeolite membrane composite according to claim 7 or 8, The zeolite membrane has a thickness of 1 μm or less.
10. The zeolite membrane composite according to any one of claims 7 to 9, a thickness a of the zeolite membrane in a portion where the support thickness is the maximum value A, and a thickness b of the zeolite membrane in a portion where the support thickness is the minimum value B, satisfy |a-b| / ((a+b) / 2)≦10%.
11. A method for producing a zeolite membrane composite, comprising the steps of: a) providing a seed crystal; b) depositing said seed crystals on a support according to any one of claims 1 to 6; c) growing zeolite from the seed crystals by hydrothermal synthesis to form a zeolite membrane on the support; Equipped with.
12. A method of separation comprising the steps of: d) preparing a zeolite membrane composite according to any one of claims 7 to 10; e) supplying a mixed substance containing a plurality of types of gases or liquids to the zeolite membrane composite, and separating a highly permeable substance in the mixed substance from the mixed substance by permeating the highly permeable substance through the zeolite membrane composite; Equipped with.
13. 13. The method of claim 12, further comprising the steps of: The mixture of substances includes one or more of hydrogen, helium, nitrogen, oxygen, water, water vapor, carbon monoxide, carbon dioxide, nitrogen oxides, ammonia, sulfur oxides, hydrogen sulfide, sulfur fluoride, mercury, arsine, hydrogen cyanide, carbonyl sulfide, C1-C8 hydrocarbons, organic acids, alcohols, mercaptans, esters, ethers, ketones, and aldehydes.
Citation Information
Patent Citations
Composite membrane
JP2006231123A
Manufacturing method of zeolite separation membrane
JP2007090233A
Process for producing DDR type zeolite membrane
WO2007105407A1