Semiconductor Device

The semiconductor device design with controlled surface roughness on metal patterns and insulating layers enhances adhesion, addressing the challenge of high-speed signal transmission and preventing short circuits, thus improving device performance.

JP7590931B2Active Publication Date: 2024-11-27RENESAS ELECTRONICS CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021100071
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-06-16
Publication Date
2024-11-27
Estimated Expiration
2041-06-16

AI Technical Summary

Technical Problem

The challenge is to increase the transmission speed of electrical signals in semiconductor devices while minimizing the device size and preventing short circuits between terminals, particularly in high-density signal transmission paths.

Method used

A semiconductor device design featuring a semiconductor chip with protruding electrodes and a wiring board that includes insulating layers and metal patterns with controlled surface roughness to enhance adhesion and prevent peeling, thereby reducing transmission loss and short circuits.

Benefits of technology

The design improves the performance of semiconductor devices by maintaining high signal transmission speeds with reduced size and minimizing short circuits, ensuring reliable electrical connections.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007590931000002
    Figure 0007590931000002
  • Figure 0007590931000003
    Figure 0007590931000003
  • Figure 0007590931000004
    Figure 0007590931000004
Patent Text Reader

Abstract

To improve the performance of a semiconductor device.SOLUTION: A wiring board SUB1 includes: an insulating layer 2e1; a metal pattern 2MP1 formed on the insulating layer 2e1; an insulating layer 2e2 formed on the insulating layer 2e1 so as to be in contact with the metal pattern 2MP1 and cover the metal pattern 2MP1; a metal pattern 2MP2 formed on the insulating layer 2e2; and an organic insulating film in contact with a part of the metal pattern 2MP2. The metal pattern 2MP1 has: a lower surface MP1b in contact with the insulating layer 2e1; and an upper surface MP1t in contact with the insulating layer 2e2. The metal pattern 2MP2 has: a lower surface MP2b in contact with the insulating layer 2e2; and an upper surface MP2t in contact with the organic insulating film. Surface roughness of the upper surface MP2 t of the metal pattern 2MP2 is greater than surface roughness of each of the lower surface MP2b of the metal pattern 2MP2, the upper surface MP1 t and the lower surface MP1b of the metal pattern 2MP1.SELECTED DRAWING: Figure 9
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a semiconductor device. [Background technology]

[0002] There is a technique for roughening the surface of a metal film from the viewpoint of improving adhesion between the metal film and an adhesive in contact with the metal film (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2014-236056 A Summary of the Invention [Problem to be solved by the invention]

[0004] As one of the demands for improving the performance of semiconductor devices, there is a demand for an increase in the transmission speed of electric signals or a demand for a smaller device. However, as the transmission speed increases, the size of the semiconductor device tends to increase. In order to suppress the increase in size of electronic devices that accompanies the increase in transmission speed, a technology is required for mounting a large number of signal transmission paths at a high density, for example, a technology that can prevent short circuits between adjacent terminals even when a large number of terminals are arranged at a high density.

[0005] Other objects and novel features will become apparent from the description of this specification and the accompanying drawings. [Means for solving the problem]

[0006] A semiconductor device according to an embodiment includes a semiconductor chip having a first surface on which a protruding electrode is disposed, and a wiring board having a second surface opposite to the first surface of the semiconductor chip. The wiring board includes a first insulating layer, a first metal pattern formed on the first insulating layer, a second insulating layer formed on the first insulating layer in contact with the first metal pattern and covering the first metal pattern, a second metal pattern formed on the second insulating layer, the second metal pattern having a first portion opposite to the protruding electrode and a second portion around the first portion, and an organic insulating film formed on the second insulating layer in contact with the second portion of the second metal pattern and exposing the first portion of the second metal pattern. The first metal pattern has a first lower surface in contact with the first insulating layer and a first upper surface located on the opposite side of the first lower surface and in contact with the second insulating layer. The second metal pattern has a second lower surface in contact with the second insulating layer and a second upper surface in contact with the organic insulating film at the second portion, and the second upper surface of the second metal pattern has a surface roughness greater than the surface roughness of the second lower surface of the second metal pattern, the first upper surface of the first metal pattern, and the first lower surface. Effect of the Invention

[0007] According to the above embodiment, the performance of the electronic device can be improved. [Brief description of the drawings]

[0008] [Figure 1] 1 is an explanatory diagram illustrating a configuration example of an electronic device including a semiconductor device according to an embodiment; [Diagram 2] 2 is an explanatory diagram showing an example of the configuration of a circuit included in the electronic device shown in FIG. 1; [Diagram 3] 2 is a top view of one of the two semiconductor devices shown in FIG. 1 according to an embodiment of the present invention; FIG. [Figure 4] 4 is a bottom view of the semiconductor device shown in FIG. 3. [Diagram 5] 4 is a plan view showing the internal structure of the semiconductor device on the wiring board with the cover member shown in FIG. 3 removed. [Figure 6] FIG. 4 is a cross-sectional view taken along line AA in FIG. [Figure 7] 7 is an enlarged plan view of the upper surface side of the wiring board shown in FIG. 6. [Figure 8] FIG. 8 is an enlarged cross-sectional view taken along line BB in FIG. [Figure 9] FIG. 8 is an enlarged cross-sectional view taken along line CC in FIG. [Figure 10] 8 is an enlarged plan view showing an example of the structure of a metal pattern disposed in a second wiring layer shown in FIG. 9 in an enlarged plane corresponding to FIG. 7. [Figure 11] FIG. 10 is an enlarged cross-sectional view showing a modification of FIG. [Figure 12] FIG. 12 is an enlarged cross-sectional view showing a modification of FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] (Description format, basic terms and usage in this application) In this application, the description of the embodiment is conveniently divided into multiple sections, etc., as necessary, but unless otherwise specified, these are not mutually independent and separate, and regardless of the description, each part of a single example, one is a partial detail of the other, or a partial or complete modified example, etc. In addition, as a general rule, repeated explanations of similar parts will be omitted. In addition, each component in the embodiment is not essential, unless otherwise specified, when it is theoretically limited to that number, or when it is clearly not from the context.

[0010] Similarly, in the description of the embodiments, when a material, composition, etc. is described as "X made of A," it does not exclude those containing elements other than A, unless otherwise specified or clearly indicated from the context. For example, when it comes to components, it means "X containing A as a main component." For example, when it comes to "silicon components," it goes without saying that it is not limited to pure silicon, but also includes SiGe (silicon germanium) alloys and other multi-component alloys whose main component is silicon, and components containing other additives. In addition, when it comes to gold plating, Cu layer, nickel plating, etc., it includes not only pure ones, but also components whose main components are gold, Cu, nickel, etc., unless otherwise specified.

[0011] Furthermore, even when a specific number or quantity is mentioned, unless otherwise specified, it may be a number greater than that specific number, or a number less than that specific number, unless it is theoretically limited to that number or unless it is clearly different from the context.

[0012] In addition, in each drawing of the embodiment, the same or similar parts are indicated by the same or similar symbols or reference numbers, and descriptions thereof will not be repeated as a general rule.

[0013] In the accompanying drawings, hatching and the like may be omitted even in cross sections if it would be too complicated or if the distinction from voids is clear. In relation to this, the background contour lines may be omitted even in the case of holes that are closed in plan view if it is clear from the explanation, etc. Furthermore, hatching or dot patterns may be added even if the drawing is not a cross section in order to clearly indicate that it is not a void or to clearly indicate the boundaries of the area.

[0014] <Electronic equipment> First, an example of use of the semiconductor device according to the present embodiment will be described below with reference to Figures 1 and 2. Figure 1 is an explanatory diagram showing an example of the configuration of an electronic device including the semiconductor device according to the present embodiment. Also, Figure 2 is an explanatory diagram showing an example of the configuration of a circuit included in the electronic device shown in Figure 1. Note that in Figure 1, in order to explicitly show that the semiconductor device PKG1 and the semiconductor device PKG2 are electrically connected, the signal transmission path SGP shown in Figure 2 is typically shown by a thick line.

[0015] The electronic device (electronic device) EDV1 shown in Fig. 1 has a wiring board (motherboard, mounting board) MB1, and semiconductor devices PKG1 and PKG2 mounted on the wiring board MB1. The semiconductor devices PKG1 and PKG2 are electrically connected to each other via a signal transmission path SGP formed on the wiring board MB1. Signals transmitted via the signal transmission path SGP include a signal SGT output from the semiconductor device PKG1 and a signal SGR input to the semiconductor device PKG1. The signal transmission path SGP also includes a signal transmission path SGPT through which the signal SGT is transmitted, and a signal transmission path SGPR through which the signal SGR is transmitted.

[0016] In the example shown in Fig. 1, the signal SGT is output from the semiconductor device PKG1 and is input to the semiconductor device PKG2. Also, the signal SGR is output from the semiconductor device PKG2 and is input to the semiconductor device PKG1. However, the output destination of the signal SGT and the output source of the signal SGR are not limited to the example shown in Fig. 1, and there are various modified examples. Since the semiconductor device PKG1 and the semiconductor device PKG2 shown in Fig. 1 have the same structure, the following will explain the semiconductor device PKG1 as a representative example.

[0017] As shown in FIG. 2, the electronic device EDV1 has a plurality of signal transmission paths SGP. The signal transmission path SGP is a high-speed transmission path (high-speed signal transmission path) through which a signal is transmitted at a transmission speed of, for example, 15 Gbps (Gigabit per second) or more. In order to realize a transmission speed of 15 Gbps through one signal transmission path, for example, the frequency of an electric signal flowing through the signal transmission path SGP needs to be 30 GHz (gigahertz) or more. In addition, in this embodiment, as an example of the signal transmission path SGP that is a high-speed transmission path, a so-called single-ended structure transmission path in which different signals are transmitted to each of the plurality of signal transmission paths SGP will be taken up and described. However, the technology described below can also be applied to a differential transmission path in which one signal is transmitted through a pair of signal transmission paths that constitute a differential pair.

[0018] As shown in Fig. 2, the semiconductor chip (semiconductor component, electronic component) CHP1 of the semiconductor device PKG1 has a plurality of electrodes (electrode terminals). The plurality of electrodes of the semiconductor chip CHP1 includes a signal electrode (signal electrode terminal) Tx through which a signal SGT (see Fig. 1) which is an output signal (transmission signal) is transmitted. The plurality of electrodes of the semiconductor chip CHP1 also includes a signal electrode (signal electrode terminal) Rx through which a signal SGR (see Fig. 1) which is an input signal (reception signal) is transmitted. Note that, hereinafter, the signal electrode Tx or the signal electrode Rx may be collectively referred to as a signal electrode Sx.

[0019] 2, two output signal transmission paths SGPT and two input signal transmission paths SGPR are representatively shown among the multiple signal transmission paths SGP included in the semiconductor device PKG1. However, the number of signal transmission paths SGP included in the semiconductor device PKG1 is greater than the number shown in FIG.

[0020] The multiple electrodes of the semiconductor chip CHP1 include an electrode (reference potential electrode, first potential electrode) Vs to which a reference potential (first potential) VSS is supplied, and an electrode (power potential electrode, second potential electrode) Vd to which a power supply potential (second potential) VDD is supplied. The electrode Vs constitutes a part of a reference potential supply path VSP. The electrode Vd constitutes a part of a power supply potential supply path VDP. The power supply potential VDD is supplied to the semiconductor chip CHP1 (more specifically, the circuits provided in the semiconductor chip CHP1) via the electrode Vd. The reference potential VSS is supplied to the semiconductor chip CHP1 (more specifically, the circuits provided in the semiconductor chip CHP1) via the electrode Vs. At least some of the multiple circuits provided in the semiconductor chip CHP1 are driven by a drive voltage generated by a potential difference between the power supply potential VDD and the reference potential VSS. The reference potential VSS is, for example, a ground potential, and the power supply potential VDD is higher than the reference potential VSS.

[0021] <Semiconductor device> Fig. 3 is a top view of a semiconductor device according to one embodiment of one of the two semiconductor devices shown in Fig. 1. Fig. 4 is a bottom view of the semiconductor device shown in Fig. 3. Fig. 5 is a plan view showing the internal structure of the semiconductor device on a wiring board with the cover member shown in Fig. 3 removed. Fig. 6 is a cross-sectional view taken along line AA in Fig. 3.

[0022] The semiconductor device PKG1 of this embodiment has a wiring board SUB1 and a semiconductor chip CHP1 (see FIG. 5) mounted on the wiring board SUB1. The semiconductor device PKG1 also has a heat dissipation sheet TIM arranged on the semiconductor chip CHP1, and a cover member LID that covers the entire semiconductor chip CHP1, the entire heat dissipation sheet TIM, and a part of the wiring board SUB1. Although not shown in the drawings, the technology described below can also be applied to a semiconductor device that does not have a heat dissipation sheet TIM or a cover member LID.

[0023] As shown in Fig. 6, the wiring board SUB1 has an upper surface (surface, main surface, chip mounting surface) 2t on which the semiconductor chip CHP1 is mounted, and a lower surface (surface, main surface, mounting surface) 2b opposite to the upper surface 2t. The wiring board SUB1 also has a plurality of side surfaces 2s (see Figs. 3 to 5) continuing to the outer edges of the upper surface 2t and the lower surface 2b. In the present embodiment, the upper surface 2t (see Fig. 3) and the lower surface 2b (see Fig. 4) of the wiring board SUB1 are each rectangular. The upper surface 2t is a chip mounting surface facing the front surface 3t of the semiconductor chip CHP1.

[0024] The wiring board SUB1 has a plurality of wiring layers (six layers in the example shown in FIG. 6) WL1, WL2, WL3, WL4, WL5, and WL6 that electrically connect terminals (pads 2PD) on the upper surface 2t, which is the chip mounting surface, and terminals (lands 2LD) on the lower surface 2b, which is the mounting surface. Each wiring layer is between the upper surface 2t and the lower surface 2b. Each wiring layer has a conductor pattern such as wiring that is a path for supplying electric signals and power. An insulating layer 2e is disposed between each wiring layer. Each wiring layer is electrically connected to each other through via wiring 2v, which is an interlayer conductive path penetrating the insulating layer 2e, or through-hole wiring 2THW. In this embodiment, a wiring board having eight wiring layers is illustrated as an example of the wiring board SUB1, but the number of wiring layers provided in the wiring board SUB1 is not limited to eight layers. For example, a wiring board having five or less wiring layers or seven or more wiring layers can be used as a modified example.

[0025] Among the multiple wiring layers, the wiring layer WL1 arranged on the upper surface 2t side is covered with an organic insulating film SR1. An opening is provided in the organic insulating film SR1, and the multiple pads 2PD provided on the wiring layer WL1 are exposed from the organic insulating film SR1 at the opening. Among the multiple wiring layers, the wiring layer WL6 arranged at the position closest to the lower surface 2b side of the wiring board SUB1 is provided with multiple lands 2LD, and the wiring layer WL6 is covered with an organic insulating film SR2. Each of the organic insulating film SR1 and the organic insulating film SR2 is a solder resist film. Each of the multiple pads 2PD provided on the wiring layer WL1 and the multiple lands 2LD provided on the wiring layer WL6 is electrically connected via a conductor pattern (wires 2d and large-area conductor patterns) formed on each wiring layer of the wiring board SUB1, a via wiring 2v, and a through-hole wiring 2THW.

[0026] The wiring 2d, the pad 2PD, the via wiring 2v, the via land 2vL (see FIG. 9 described later), the through-hole wiring 2THW, the land 2LD, and the conductor pattern 2CP are each made of, for example, copper or a metal material containing copper as a main component.

[0027] The wiring board SUB1 is formed by stacking a plurality of wiring layers on the upper surface 2Ct and the lower surface 2Cb of an insulating layer (core material, core insulating layer) 2CR made of a prepreg in which glass fibers are impregnated with resin, by a build-up method. The wiring layer WL3 on the upper surface 2Ct side of the insulating layer 2CR and the wiring layer WL4 on the lower surface 2Cb side are electrically connected via a plurality of through-hole wirings 2THW embedded in a plurality of through holes (through holes) provided so as to penetrate from one side of the upper surface 2Ct to the other side of the lower surface 2Cb.

[0028] In the example shown in Fig. 6, the wiring board SUB1 is a wiring board in which a plurality of wiring layers are laminated on the upper surface 2Ct side and the lower surface 2Cb side of the insulating layer 2CR, which is a core material. However, as a modification of Fig. 6, a so-called coreless board may be used, which does not have the insulating layer 2CR made of a hard material such as a prepreg material, and is formed by sequentially laminating an insulating layer 2e and a conductor pattern such as wiring 2d. When a coreless board is used, no through-hole wiring 2THW is formed, and each wiring layer is electrically connected via a via wiring 2v.

[0029] In the example shown in FIG. 6, a solder ball (solder material, external terminal, electrode, external electrode) SB is connected to each of the multiple lands 2LD. The solder ball SB is a conductive member that electrically connects multiple terminals (not shown) on the motherboard side to the multiple lands 2LD when mounting the semiconductor device PKG1 on a motherboard (not shown). The solder ball SB is, for example, a solder material made of a Sn-Pb solder material containing lead (Pb) or a so-called lead-free solder that does not substantially contain Pb. Examples of lead-free solder include tin (Sn) only, tin-bismuth (Sn-Bi), tin-copper-silver (Sn-Cu-Ag), tin-copper (Sn-Cu), etc. Here, lead-free solder means a solder containing 0.1 wt% or less of lead (Pb), and this content is determined as a standard of the RoHS (Restriction of Hazardous Substances) Directive.

[0030] As shown in FIG. 4, the solder balls SB are arranged in a matrix. Although not shown in FIG. 4, the lands 2LD (see FIG. 6) to which the solder balls SB are bonded are also arranged in a matrix. A semiconductor device in which a plurality of external terminals (solder balls SB, lands 2LD) are arranged in a matrix on the mounting surface side of the wiring board SUB1 is called an area array type semiconductor device. The area array type semiconductor device is preferable in that the mounting surface (lower surface 2b) side of the wiring board SUB1 can be effectively used as a space for arranging the external terminals, and therefore the increase in the mounting area of ​​the semiconductor device can be suppressed even if the number of external terminals increases. In other words, a semiconductor device in which the number of external terminals increases with increasing functionality and integration can be mounted in a small space.

[0031] The semiconductor device PKG1 also includes a semiconductor chip CHP1 mounted on a wiring board SUB1. As shown in FIG. 6, each of the semiconductor chips CHP1 includes a surface (main surface, upper surface) 3t on which a plurality of protruding electrodes 3BP are arranged, and a back surface (main surface, lower surface) 3b opposite to the surface 3t. The semiconductor chip CHP1 also includes a plurality of side surfaces 3s intersecting the surface 3t and the back surface 3b. As shown in FIG. 5, the semiconductor chip CHP1 has a rectangular outer shape with a smaller planar area than the wiring board SUB1 in a plan view. In the example shown in FIG. 5, the semiconductor chip CHP1 is mounted in the center of the upper surface 2t of the wiring board SUB1, and each of the four side surfaces 3s of the semiconductor chip CHP1 extends along each of the four side surfaces 2s of the wiring board SUB1.

[0032] In addition, a plurality of electrodes (pads, electrode pads, bonding pads) 3PD are formed on the front surface 3t of the semiconductor chip CHP1. In the example shown in Fig. 6, the semiconductor chip CHP1 is mounted on the wiring board SUB1 with the front surface 3t facing the upper surface 2t of the wiring board SUB1. Such a mounting method is called a face-down mounting method or a flip-chip connection method.

[0033] Although not shown in the figure, a plurality of semiconductor elements (circuit elements) are formed on the main surface of the semiconductor chip CHP1 (more specifically, a semiconductor element formation region provided on an element formation surface of a semiconductor substrate that is the base material of the semiconductor chip CHP1). The plurality of electrodes 3PD are electrically connected to the plurality of semiconductor elements, respectively, via wiring (not shown in the figure) formed in a wiring layer arranged inside the semiconductor chip CHP1 (more specifically, between the surface 3t and the semiconductor element formation region, not shown).

[0034] The semiconductor chip CHP1 (more specifically, the substrate of the semiconductor chip CHP1) is made of, for example, silicon (Si). An insulating film (a passivation film 3PF shown in FIG. 9, which will be described later) that covers the substrate and wiring of the semiconductor chip CHP1 is formed on the surface 3t, and each of the multiple electrodes 3PD is partially exposed from the passivation film at an opening formed in the passivation film. Each of the multiple electrodes 3PD is made of a metal, and in this embodiment, is made of, for example, aluminum (Al).

[0035] 6, the electrodes 3PD are connected to protruding electrodes 3BP, and the electrodes 3PD of the semiconductor chip CHP1 and the pads 2PD of the wiring board SUB1 are electrically connected to each other via the protruding electrodes 3BP. The protruding electrodes (bump electrodes) 3BP are metal members (conductive members) formed so as to protrude from the surface 3t of the semiconductor chip CHP1. In this embodiment, the protruding electrodes 3BP are formed on the electrodes 3PD as pillar electrodes (so-called copper pillar electrodes), for example, made of copper, and have a structure in which a solder material is laminated on the tip of the pillar electrode. As the solder material laminated on the tip of the pillar electrode, a lead-containing solder material or a lead-free solder can be used, as in the case of the solder ball SB described above.

[0036] When mounting the semiconductor chip CHP1 on the wiring board SUB1, a bonding material (e.g., a base metal film or solder paste) having good bonding properties with solder is formed in advance on the multiple pads 2PD. The solder material at the tip of the columnar electrode is brought into contact with the bonding material on the pad 2PD and a heat treatment (reflow treatment) is performed, whereby the solder is integrated to form a protruding electrode 3BP. As a modification of this embodiment, a columnar electrode made of nickel (Ni), or a so-called solder bump in which a micro solder ball is formed on the electrode 3PD via a base metal film, may be used as the protruding electrode 3BP.

[0037] As shown in FIG. 6, an underfill resin (insulating resin) UF is disposed between the semiconductor chip CHP1 and the wiring board SUB1. The underfill resin UF is disposed so as to fill the space between the surface 3t of the semiconductor chip CHP1 and the upper surface 2t of the wiring board SUB1. Each of the plurality of protruding electrodes 3BP is sealed with the underfill resin UF. The underfill resin UF is made of an insulating (non-conductive) material (e.g., a resin material) and disposed so as to seal the electrical connection portion (the joint portion of the plurality of protruding electrodes 3BP) between the semiconductor chip CHP1 and the wiring board SUB1. In this way, by covering the joint portion between the plurality of protruding electrodes 3BP and the plurality of pads 2PD with the underfill resin UF, the stress generated in the electrical connection portion between the semiconductor chip CHP1 and the wiring board SUB1 can be relaxed. The stress generated in the joint portion between the plurality of electrodes 3PD of the semiconductor chip CHP1 and the plurality of protruding electrodes 3BP can also be relaxed. Furthermore, the main surface on which the semiconductor element (circuit element) of the semiconductor chip CHP1 is formed can also be protected.

[0038] A cover member (lid, heat spreader, heat dissipation member) LID is disposed on the back surface 3b of the semiconductor chip CHP1. The cover member LID is, for example, a metal plate having a higher thermal conductivity than the wiring board SUB1, and has a function of dissipating heat generated in the semiconductor chip CHP1 to the outside. The cover member LID is thermally connected to the semiconductor chip CHP1 via a heat dissipation sheet TIM. The heat dissipation sheet TIM is in contact with both the semiconductor chip CHP1 and the cover member LID.

[0039] <Surrounding structure of wiring board pads> Next, a detailed structure around the connection portion of the protruding electrode 3BP shown in Fig. 6 will be described. Fig. 7 is an enlarged plan view of the upper surface side of the wiring board shown in Fig. 6. Fig. 8 is an enlarged cross-sectional view taken along line BB in Fig. 7. Fig. 9 is an enlarged cross-sectional view taken along line CC in Fig. 7. Fig. 10 is an enlarged plan view showing an example of the structure of a metal pattern arranged on the second wiring layer shown in Fig. 9 in an enlarged plane corresponding to Fig. 7. Figs. 8 and 9 show protruding electrodes 3BP connected to each of a plurality of pads 2PD in order to show the positional relationship between the protruding electrodes 3BP and the pads 2PD.

[0040] The upper surface 2t of the wiring board SUB1 shown in Fig. 7 and each of the multiple wiring layers shown in Fig. 6 have a region CHR1 (see Fig. 7) overlapping with the semiconductor chip CHP1 in a plan view seen from the semiconductor chip CHP1 side, and a region CHR2 (see Fig. 7) that does not overlap with the semiconductor chip CHP1 and is located around the region CHR1. Each of the multiple wiring layers has a boundary line CBL1 (see Fig. 7) that is a boundary between the region CHR1 and the region CHR2 and overlaps with one of the side surfaces 3s (see Fig. 5) of the semiconductor chip CHP1 in a plan view. In the following description, in a sentence using the boundary line CBL1, the part "boundary line CBL1" can be read as "one of the side surfaces 3s of the semiconductor chip CHP1 in a plan view seen from the semiconductor chip CHP1 side."

[0041] As shown in Fig. 7, the pads 2PD are arranged in a matrix (array) in an area CHR1 overlapping with the semiconductor chip CHP1 (see Fig. 6). Although a plan view is omitted, the protruding electrodes 3BP and the pads 2PD arranged on the front surface 3t of the semiconductor chip CHP1 are arranged in positions facing each other, as shown in Fig. 8. Similarly, the electrodes 3PD and the pads 2PD arranged on the front surface 3t of the semiconductor chip CHP1 are arranged in positions facing each other.

[0042] Each of the pads 2PD shown in FIG. 7 has a central portion (portion) PDc facing the protruding electrode 3BP (see FIG. 8) and a peripheral portion (portion) PDp around the central portion PDc. The peripheral portion (portion) PDp of each of the pads 2PD is covered with the organic insulating film SR1, and the central portion (portion) PDc of each of the pads 2PD is exposed from the organic insulating film SR1 at an opening SRh formed in the organic insulating film SR1. As shown in FIG. 9, the portion of the pad 2PD exposed from the opening SRh is joined to the protruding electrode 3BP. The pads 2PD of the wiring board SUB1 are included in an electric signal transmission path (for example, the signal transmission path SGP shown in FIG. 2), a reference potential supply path VSP (see FIG. 2), or a power supply potential supply path VSD (see FIG. 2).

[0043] As shown in Fig. 8, a passivation film 3PF is formed on the surface 3t side of the semiconductor chip 3. The passivation film 3PF is an infinite insulating film having a surface 3t. An opening PFh is formed in the passivation film 3PF, and the electrode 3PD is exposed from the passivation film 3PF at the opening PFh. One end of the protruding electrode 3BP is in contact with the electrode 3PD. The other end of the protruding electrode 3BP is in contact with a bonding material 3BM made of solder.

[0044] An organic insulating film SR1 is formed on the upper surface 2t side of the wiring board SUB1. The organic insulating film is a solder resist film that has the property of suppressing the wetting and spreading of solder. The organic insulating film SR1 has an upper surface 2t. A plurality of openings SRh are formed in the organic insulating film SR1, and the pads 2PD are exposed from the organic insulating film SR1 at the openings SRh. A metal film 2UBM is formed on the exposed surface of the pad 2PD. The metal film 2UBM is called an under-bump metal, and is a film provided to improve the electrical connection characteristics between the protruding electrodes 3BP and the pads 2PD. The protruding electrodes 3BP and the metal film 2UBM are electrically connected via solder (bonding material 3BM).

[0045] As described with reference to FIG. 1 and FIG. 2, a high-frequency signal is transmitted through the signal transmission path SGP, and therefore, noise countermeasures are required for the signal transmission path SGP. For example, in the example shown in FIG. 9, the wiring 2d constituting a part of the signal transmission path SGP (see FIG. 2) is arranged on the wiring layer WL2 (see FIG. 6). In the thickness direction of the wiring board SUB1, the wiring 2d is arranged between the conductor pattern 2CP formed on the wiring layer WL1 and the conductor pattern 2CP formed on the wiring layer WL3 (see FIG. 6). A reference potential is supplied to the conductor pattern 2CP. The conductor pattern to which the reference potential is supplied is called a ground plane. The wiring structure illustrated in FIG. 9 is called a strip line structure, and the ground planes arranged to sandwich the wiring 2d function as an electromagnetic shield that prevents electromagnetic waves generated by the transmission of a high-frequency signal through the wiring 2d from diffusing to the surroundings.

[0046] Furthermore, in the case of a semiconductor device PKG1 used for high-speed signal transmission, there is a demand for increasing the number of signal transmission paths SGP to increase the bus width in addition to increasing the frequency of one signal transmission path SGP. In order to increase the number of signal transmission paths SGP, it is necessary to increase the number of pads 2PD. However, due to the demand for miniaturization of semiconductor devices, it is necessary to suppress an increase in the overall size of the semiconductor device PKG1 even if the pads 2PD are increased. As a result, the arrangement density of the multiple pads 2PD increases. In the example shown in FIG. 7, the diameter 2PDD of each of the multiple pads 2PD is, for example, about 90 μm to 150 μm, and the minimum value of the center-to-center distance 2PDP between adjacent pads 2PD is about 110% to 130% of the diameter 2PDD.

[0047] As shown in Fig. 7, when the arrangement density of the multiple pads 2PD is increased, a technique for preventing short-circuiting between adjacent pads 2PD is required. For example, in the example shown in Fig. 8, when the adhesive interface between the organic insulating film SR1 and the pad 2PD peels off, solder may enter into the gap caused by the peeling. When the peeling progresses in the planar direction, the adjacent pads 2PD may communicate with each other through the gap caused by the peeling, depending on the extent of the progress of the peeling. When solder enters this communicated gap, there is a concern that the adjacent pads 2PD may be short-circuited via the solder.

[0048] From the viewpoint of preventing the above-mentioned short circuit, it is preferable to improve the adhesion between the pad 2PD and the organic insulating film SR1. Therefore, the inventors of the present application have investigated a method for suppressing the peeling between the pad 2PD and the organic insulating film SR1 by roughening the surface of the pad 2PD that is in contact with the organic insulating film SR1.

[0049] By the way, improving the adhesion between the metal pattern and the insulating layer containing an organic material such as resin is preferable from the viewpoint of protecting the metal pattern from damage. If peeling between the metal pattern and the insulating layer can be prevented, the metal pattern can be prevented from being broken by an external force caused by the progress of peeling. From this viewpoint, it is preferable that the roughened metal pattern is not only the pad 2PD shown in FIG. 8, but also the adhesion interface between each of the multiple wirings 2d formed in the wiring layer WL2 (see FIG. 6) and the insulating layer 2e2.

[0050] However, according to the study of the present inventors, it was found that increasing the surface roughness of the wiring 2d constituting the signal transmission path, particularly the transmission path of a high-frequency signal, increases the transmission loss. In addition, the wiring width of the wiring 2d tends to become narrower due to high density. If the surface roughness of the wiring 2d is increased while the wiring width is narrow, this causes a decrease in accuracy when forming the pattern. If the shape accuracy of the wiring pattern in the signal transmission path decreases, the signal transmission characteristics will vary.

[0051] Based on the above-mentioned examination results, the structure of the semiconductor device PKG1 of this embodiment will be described with reference to FIG. 9. In the following description, the metal pattern formed on the wiring layer WL1 (see FIG. 6) will be described as the metal pattern 2MP2. Any of the multiple pads 2PD corresponds to the metal pattern 2MP2. Also, the metal pattern formed on the wiring layer WL2 (see FIG. 6) will be described as the metal pattern 2MP1. The metal pattern 2MP1 corresponds to a pattern in which the via land 2vL and the wiring 2d are integrally formed, the conductor pattern 2CP (see FIG. 6), etc. Also, although the details will be described later, the metal pattern formed on the wiring layer WL3 (see FIG. 6) will be described as the metal pattern 2MP3. The metal pattern 2MP3 corresponds to multiple conductor patterns 2CP to which a power supply potential or a reference potential is supplied, a through-hole land (reference numerals omitted) connected to the through-hole wiring 2THW shown in FIG. 6, etc.

[0052] As shown in FIG. 9, the semiconductor device PKG1 has a semiconductor chip CHP1 and a wiring board SUB1 having an upper surface 2t facing the surface 3t of the semiconductor chip CHP1. The wiring board SUB1 includes an insulating layer 2e1 and a metal pattern 2MP1 formed on the insulating layer 2e1. The wiring board SUB1 also includes an insulating layer 2e2 formed on the insulating layer 2e1 in contact with the metal pattern 2MP1 and so as to cover the metal pattern 2MP1, and a metal pattern 2MP2 formed on the insulating layer 2e2. The metal pattern 2MP2 has a first portion (a central portion PDc shown in FIG. 7) facing the protruding electrode 3BP and a second portion (a peripheral portion PDp shown in FIG. 7) around the first portion. The wiring board SUB1 also includes an organic insulating film formed on the insulating layer 2e2 in contact with the second portion of the metal pattern 2MP2 and so as to expose the first portion of the metal pattern 2MP2. The metal pattern 2MP1 has a lower surface MP1b in contact with the insulating layer 2e1 and an upper surface MP1t located on the opposite side of the lower surface MP1b and in contact with the insulating layer 2e2. The metal pattern 2MP2 has a lower surface MP2b in contact with the insulating layer 2e2 and an upper surface MP2t in contact with the organic insulating film in the second portion. The surface roughness of the upper surface MP2t of the metal pattern 2MP2 is larger than the surface roughness of the lower surface MP2b of the metal pattern 2MP2, the upper surface MP1t of the metal pattern 2MP1, and the lower surface MP1b.

[0053] For example, when the surface roughness index is expressed using the arithmetic mean roughness Ra, the following ranges are preferable: The surface roughness (Ra) of the upper surface MP2t of the metal pattern 2MP2 is preferably 0.3 μm or more. On the other hand, the surface roughness Ra of each of the lower surface MP2b of the metal pattern 2MP2, the upper surface MP1t of the metal pattern 2MP1, and the lower surface MP1b is preferably less than 0.3 μm.

[0054] The arithmetic mean roughness Ra mentioned above is calculated as follows. First, a reference length L is extracted from the surface roughness curve in the direction of the mean line. Next, the X-axis is taken in the direction of the mean line of the extracted portion, and the Y-axis is taken in the direction perpendicular to the mean line, and the roughness curve is expressed as y = f(x). At this time, the arithmetic mean roughness Ra is calculated by the following formula.

[0055]

number

[0056] In the above-mentioned configuration, first, the surface roughness of the pads 2PD of the wiring layer WL1 (see FIG. 6), which is most likely to cause a short circuit between adjacent pads 2PD due to peeling of the organic insulating film SR1, is made rough. Meanwhile, the surface roughness of the lower surface MP2b of the metal pattern 2MP2, the upper surface MP1t of the metal pattern 2MP1, and the lower surface MP1b thereof, which are not in contact with the organic insulating film SR1, are each smaller than the surface roughness of the pads 2PD. Therefore, for example, even when a high-frequency signal is transmitted to the wiring 2d shown in FIG. 9, the transmission loss can be reduced.

[0057] One example of a method for increasing the surface roughness of the pad 2PD (i.e., the metal pattern 2MP2) is sandblasting, which is a method for increasing the surface roughness of a target by colliding a group of fine particles made of an inorganic material with the target.

[0058] The surface to be treated to increase the surface roughness (hereinafter referred to as the roughening treatment) preferably includes at least the upper surface MP2t of the pad 2PD. The upper surface MP2t is a surface that is likely to become a starting point for peeling of the organic insulating film SR1. Furthermore, if peeling can be prevented on the upper surface MP2t, it is possible to prevent the intrusion of the bonding material 3BM made of solder.

[0059] In the example shown in FIG. 9, the metal pattern 2MP2 has a side surface MP2s that is continuous with the upper surface MP2t and in contact with the organic insulating film SR1. The surface roughness of the side surface 2s of the metal pattern 2MP2 is greater than the surface roughness of the lower surface MP2b of the metal pattern 2MP2, the upper surface MP1t of the metal pattern 2MP1, and the lower surface MP1b. The surface roughness of the side surface 2s of the metal pattern 2MP2 is approximately the same as the surface roughness of the upper surface MP2t, and the arithmetic mean roughness Ra is preferably 0.3 μm or more. By making the surface roughness of the side surface MP2s approximately the same as the surface roughness of the upper surface MP2t, it is possible to prevent a peeling mode in which peeling that occurs on the side surface MP2s progresses to the upper surface MP2t side. However, although not shown, there is a case in which the side surface MP2s is not roughened and the upper surface MP2t is selectively roughened as a modified example of FIG. 9. Even in this modified example, peeling starting from the upper surface MP2t can be prevented.

[0060] In addition, in addition to the pads 2PD, metal patterns such as a conductor pattern 2CP are formed on the wiring layer WL1 (see FIG. 6). When roughening the upper surfaces MP2t of the pads 2PD, the roughening can be selectively performed on only the pads 2PD formed on the wiring layer WL1, or on some of the pads 2PD. However, from the viewpoint of suppressing peeling between the organic insulating film SR1 and the metal patterns formed on the wiring layer WL1, it is particularly preferable to roughen all of the metal patterns formed on the wiring layer WL1, including the upper surface of the conductor pattern 2CP. In this case, the surface roughness of the upper surfaces of all the metal patterns formed on the wiring layer WL1 is greater than the surface roughness of the lower surface MP2b of the metal pattern 2MP2, the upper surface MP1t, and the lower surface MP1b of the metal pattern 2MP1.

[0061] 9, a metal film 2UBM is formed on the central portion (part) of the metal pattern 2MP2, and the protruding electrode 3BP and the metal film 2UBM are electrically connected via solder (bonding material 3BM). In this case, if peeling (interface peeling) occurs at the interface between the upper surface MP2t of the metal pattern 2MP2 and the organic insulating film SR1, the peeling propagates (advances) into the organic insulating film SR1, and there is a possibility that solder will enter the gap that has propagated into the organic insulating film SR1.

[0062] In addition, in the transmission path of the high frequency signal described above, in a long pattern such as a wiring pattern, the effect of reducing the transmission loss by reducing the surface roughness is particularly large. In the example shown in Fig. 9, the protruding electrode 3BP is electrically connected to the metal pattern 2MP1. The metal pattern 2MP1 is electrically connected to the metal pattern 2MP2 through the via wiring 2v formed so as to penetrate the insulating layer 2e2. The metal pattern 2MP1 includes a via land (via land portion) 2vL to which the via wiring 2v is joined, and a wiring (wiring portion) 2d formed integrally with the via land 2vL and extending along the X direction.

[0063] 7, the pad 2PD corresponding to the metal pattern 2MP2 (see FIG. 9) is disposed in a region CHR1 overlapping with the semiconductor chip CHP1 in a plan view. As shown in FIG. 10, the wiring 2d of the metal pattern 2MP1 extends from the region CHR1 toward the region CHR2 surrounding the region CHR1 in a plan view. In other words, the wiring 2d straddles the boundary line CBL1 between the region CHR1 and the region CHR2. In yet other words, in a plan view, the pad 2PD does not overlap with the side surface 3s (see FIG. 9) of the semiconductor chip CHP1 (see FIG. 9), and the wiring 2d overlaps with one of the side surfaces 3s of the semiconductor chip CHP1.

[0064] The length of the wiring 2d shown in FIG. 9 is longer than the lengths of the metal pattern 2MP2, the via wiring 2v, and the via land portion 2vL. In the above, the length of the wiring 2d is defined as the length of the wiring 2d from the connection portion with the via land 2vL shown in FIG. 9 to the connection portion with the via wiring 2v connecting the wiring layer WL2 and the wiring layer WL3 shown in FIG. 6. The length of the metal pattern 2MP2 is defined as the length from the connection portion with the protruding electrode 2BP shown in FIG. 9 to the connection portion with the via wiring 2v connecting the wiring layer WL1 and the wiring layer WL2. The length of the via wiring 2v is defined as the length of the via wiring 2v in the Z direction shown in FIG. 9. The length of the via land 2vL is defined as the length of the via land 2vL from the connection portion with the via wiring 2v connecting the wiring layer WL1 and the wiring layer WL2 to the connection portion with the wiring 2d. In addition, an electric signal (for example, the signal SGT or the signal SGR shown in FIG. 1) is transmitted to the metal pattern 2MP1 and the metal pattern 2MP2. In other words, the metal pattern 2MP1 and the metal pattern 2MP2 are included in the signal transmission path SGP (see FIG. 2). In addition, in this embodiment, the electric signal flowing through the signal transmission path SGP is a high-frequency signal of 30 GHz (gigahertz) or more. Therefore, if the surface roughness of a portion (corresponding to the wiring 2d) that extends longer than other portions of the transmission path of the high-frequency signal of 30 GHz or more is increased, the adhesion between this portion (the wiring 2d) and the insulating layer 2e1 or 2e2 that contacts this portion is improved, but it is susceptible to the influence of transmission loss due to this roughening. That is, the scattering loss due to the skin effect of the high-frequency signal (the phenomenon that the higher the frequency of the signal, the more the current flows only on the surface of the wiring) increases. On the other hand, according to this embodiment, the surface roughness of the wiring 2d that constitutes the signal transmission path is smaller than the surface roughness of the upper surface MP2t of the metal pattern 2MP2, for example, so that the transmission loss can be reduced.

[0065] Peeling between the metal pattern and the insulating film occurs due to the difference in linear expansion coefficient caused by the materials constituting each member. Therefore, when the difference in linear expansion coefficient between the metal pattern and the insulating film is small, peeling is unlikely to occur, and when the difference in linear expansion coefficient is large, peeling is likely to occur. For example, in the example shown in FIG. 9, the thermal expansion coefficient (specifically, the linear expansion coefficient) of the organic insulating film SR1 is larger than the thermal expansion coefficient (specifically, the linear expansion coefficient) of the insulating layer 2e2. Also, the storage elastic modulus of the organic insulating film SR1 is softer than the storage elastic modulus of the insulating layer 2e2. In addition to electrical insulation properties, the organic insulating film SR1 is required to function as a solder resist film as described above. Also, since the organic insulating film SR1 is a film located on the outermost surface (outermost layer) of each material constituting the wiring board SUB1, it is also required to function as a protective film. On the other hand, the insulating layer 2e1 and the insulating layer 2e2 located in the inner layer of the wiring board SUB1 than the organic insulating film SR1 are required to have high rigidity in order to suppress warping and deformation of the wiring board SUB1 in addition to electrical insulation properties. For this reason, it is preferable to select a material that reduces the thermal expansion coefficient of the insulating layer 2e2 so as to bring it closer to the thermal expansion coefficient of the metal pattern 2MP1. This can reduce the occurrence of peeling at the interface between the metal pattern 2MP1 and the insulating layer 2e2. On the other hand, peeling can be suppressed at the interface between the organic insulating film SR1 and the metal pattern 2MP2 by increasing the surface roughness of the upper surface MP2t as described above.

[0066] In addition, as in the example shown in FIG. 6, when the metal pattern (metal pattern 2MP3 shown in FIG. 9) formed on the wiring layer WL3 is formed on the insulating layer 2CR, which is the core insulating layer, peeling is unlikely to occur at the interface between the insulating layer 2CR and the metal pattern 2MP3. As described above, the insulating layer 2CR is an insulating layer made of a prepreg in which glass fibers are impregnated with resin. In this case, the linear expansion coefficient of the insulating layer 2CR can be reduced. On the other hand, the organic insulating film SR1, the insulating layer 2e1, and the insulating layer 2e2 do not contain glass fibers. Therefore, the linear expansion coefficients of the organic insulating film SR1, the insulating layer 2e1, and the insulating layer 2e2 are each larger than the linear expansion coefficient of the insulating layer 2CR.

[0067] 9, the thickness TSR of the organic insulating film SR1 is thinner than the thickness Te2 of the insulating layer 2e2. The organic insulating film SR1, which is thinner than the insulating layer 2e2, is more likely to expand or contract in response to the environmental temperature than the insulating layer 2e2. Therefore, it is particularly important to take measures against peeling by roughening the adhesive interface between the organic insulating film SR1 and the metal pattern 2MP2.

[0068] FIG. 11 is an enlarged cross-sectional view showing a semiconductor device which is a modification of FIG. 9. The semiconductor device PKG3 shown in FIG. 11 is similar to the semiconductor device PKG1 shown in FIG. 9, except that the upper surface MP3t of the metal pattern 2MP3 is roughened as described below. Therefore, the overlapping description will be omitted. The semiconductor device PKG3 shown in FIG. 11 further includes a core insulating layer (insulating layer) 2CR (see FIG. 6) and a metal pattern 2MP3 formed on the insulating layer 2CR. The metal pattern 2MP3 is a conductor pattern 2CP formed on the wiring layer WL3 (see FIG. 6). A reference potential or a power supply potential is supplied to the conductor pattern 2CP shown in FIG. 9, but a reference potential is supplied to the conductor pattern 2CP. The metal pattern 2MP3 has a lower surface MP3b in contact with the insulating layer 2CR (see FIG. 6) and an upper surface MP3t located on the opposite side of the lower surface MP3b and in contact with the insulating layer 2e1. The surface roughness of the upper surface MP3t of the metal pattern 2MP3 is larger than the surface roughness of the lower surface MP2b of the metal pattern 2MP2, the upper surface MP1t of the metal pattern 2MP1, and the lower surface MP1b. For example, the metal pattern 2MP3 is subjected to a roughening treatment similar to that of the metal pattern 2MP2, and the surface roughness (Ra) of the upper surface MP3t is preferably 0.3 μm or more. The supply path of the reference potential is less susceptible to transmission loss due to roughening compared to the signal transmission path. On the other hand, the metal pattern 2MP3 is a large-area pattern having an area three times or more larger than that of the wiring 2d. The large-area metal pattern 2MP3 has a large value of stress generated when thermally contracted or thermally expanded. For this reason, peeling is likely to occur at the adhesive interface between the metal pattern 2MP3 and the insulating layer 2e1 due to stress. Therefore, it is preferable to perform a roughening treatment on the metal pattern 2MP3, similar to the metal pattern 2MP2.

[0069] However, even if peeling occurs between the metal pattern 2MP3 and the insulating layer 2e1, insulation failure or the like does not occur immediately. Therefore, the metal pattern 2MP1 has a higher priority in the roughening process than the metal pattern 2MP3. Therefore, as in the semiconductor device PKG1 shown in FIG. 9, the surface roughness of the upper surface MP3t of the metal pattern 2MP3 may be approximately the same as the surface roughness of the upper surface MP1t of the metal pattern 2MP1.

[0070] Incidentally, in FIG. 9, the surfaces of the metal patterns other than the upper surface MP2t, the side surface MP2s, and the upper surface MP3t of the metal pattern 2MP3 are illustrated as flat surfaces. However, when a process called a desmear process is performed in the process of manufacturing the wiring board SUB1, the other surfaces may not be flat. FIG. 12 is an enlarged cross-sectional view showing a modification of FIG. 11. The semiconductor device PKG4 shown in FIG. 12 is similar to the semiconductor device PKG3 shown in FIG. 11, except that it has uneven surfaces caused by the desmear process described below. Therefore, a duplicated description will be omitted.

[0071] In the manufacturing process of the wiring board SUB1, for example, when a build-up method is adopted, an insulating layer is formed on the lower wiring layer, and then holes are drilled to provide the via wiring 2v. At this time, in order to remove the residue of the insulating layer remaining after the drilling process, for example, plasma is irradiated onto the non-processed surface. This process is called a desmear process (sometimes called a plasma desmear process). By performing the desmear process, the adhesion between the metal film and the insulating layer can be improved. On the other hand, since the insulating layer is irradiated with plasma in the desmear process, the surface roughness of the insulating layer, which is the base layer of the metal pattern, becomes larger compared to the case where the desmear process is not performed. When the metal pattern is formed after this desmear process, the lower surface of the metal pattern becomes uneven following the unevenness of the insulating layer that has been desmeared.

[0072] As shown in FIG. 12, the lower surface MP1b of the metal pattern 2MP1 and the lower surface MP2b of the metal pattern 2MP2 each have an uneven surface caused by the desmear process, rather than a flat surface. However, in the case of an uneven surface caused by the desmear process, the surface roughness can be suppressed from becoming extremely large, compared with the roughening process such as the sandblasting process described above. Therefore, even in the case of the modified example shown in FIG. 12, the following can be said. That is, the surface roughness of the upper surface MP2t of the metal pattern 2MP2 is larger than the surface roughness of the lower surface MP2b of the metal pattern 2MP2, the upper surface MP1t, and the lower surface MP1b of the metal pattern 2MP1. In addition, the surface roughness of the side surface 2s of the metal pattern 2MP2 is larger than the surface roughness of the lower surface MP2b of the metal pattern 2MP2, the upper surface MP1t, and the lower surface MP1b of the metal pattern 2MP1. Moreover, the surface roughness of the upper surface MP3t of the metal pattern 2MP3 is greater than the surface roughness of the lower surface MP2b of the metal pattern 2MP2, and the upper surface MP1t and lower surface MP1b of the metal pattern 2MP1.

[0073] 9. The semiconductor device PKG4 of the modified example shown in FIG. 12 is similar to the semiconductor device PKG1 shown in FIG. 9 in that the metal pattern 2MP1 is not roughened. Therefore, the following relationship is established between the surface roughness of the upper surface MP1t and the lower surface MP1b of the metal pattern 2MP1. That is, the surface roughness of the upper surface MP1t of the metal pattern 2MP1 is smaller than the surface roughness of the lower surface MP1b of the metal pattern 2MP1. The surface roughness of the upper surface MP1t of the metal pattern 2MP1 is also smaller than the surface roughness of the upper surface MP2t, the lower surface MP2b, and the side surface MP2s of the metal pattern 2MP2.

[0074] The invention made by the inventor has been specifically described above based on an embodiment, but it goes without saying that the present invention is not limited to the above embodiment and can be modified in various ways without departing from the gist of the invention. [Explanation of symbols]

[0075] 2b Bottom surface (surface, main surface, mounting surface) 2Cb bottom surface 2CP Conductor pattern (Conductor plane) 2CR Insulation layer (core material, core insulation layer) 2Ct top surface 2d Wiring (wiring section) 2e,2e1,2e2 Insulating layer 2LD Land 2MP1, 2MP2, 2MP3 Metal pattern 2PD Pad 2PDD diameter 2PDP center distance 2s side 2t Top surface (main surface, chip mounting surface) 2THW Through hole wiring 2UBM metal membrane 2v via wiring 2vL Beerland (Beerland Department) 3. Semiconductor chips 3b Back side (main side, bottom side) 3BM bonding material 3BP Protruding electrode (bump electrode) 3PD electrodes (pads, electrode pads, bonding pads) 3PF insulating film 3PF passivation film 3s side 3t surface (main surface, top surface) CBL1 border CHP1 Semiconductor chips (semiconductor parts, electronic parts) CHR1,CHR2 area EDV1 Electronic equipment (electronic equipment) LID Cover parts (lids, heat spreaders, heat dissipation parts) MB1 Wiring board (motherboard, mounting board) MP1b, MP2b, MP3b bottom side MP1t, MP2t, MP3t top surface PDc central part (part) PDp peripheral area (part) PFh opening PKG1, PKG2, PKG3, PKG4 Semiconductor device Rx, Sx, Tx signal electrode (signal electrode terminal) SB Solder ball (solder material, external terminal, electrode, external electrode) SGP signal transmission path SGPR input signal transmission path SGPT output signal transmission path SGR, SGT signal (electrical signal) SR1, SR2 Organic insulating film SRh opening SUB1 Wiring board TIM Heat dissipation sheet UF underfill resin (insulating resin) Vd electrode (power supply potential electrode, second potential electrode) VDD power supply potential (second potential) Vs electrode (reference potential electrode, first potential electrode) VSD Power supply potential supply path VSP Reference potential supply path VSS Reference potential (1st potential) WL1,WL2,WL3,WL3,WL4,WL5,WL6 wiring layers

Claims

1. a semiconductor chip having a first surface on which protruding electrodes are arranged; a wiring substrate having a second surface opposed to the first surface of the semiconductor chip; having The wiring board includes: A first insulating layer; a first metal pattern formed on the first insulating layer; a second insulating layer formed on the first insulating layer so as to contact the first metal pattern and cover the first metal pattern; a second metal pattern formed on the second insulating layer, the second metal pattern having a first portion facing the protruding electrode and a second portion surrounding the first portion; an organic insulating film formed on the second insulating layer in contact with the second portion of the second metal pattern and such that the first portion of the second metal pattern is exposed; A third insulating layer; a third metal pattern formed on the third insulating layer and supplied with a reference potential; Including, The first metal pattern is a first lower surface in contact with the first insulating layer; a first upper surface located opposite the first lower surface and in contact with the second insulating layer; having The second metal pattern is a second lower surface in contact with the second insulating layer; a second upper surface in contact with the organic insulating film in the second portion; having The third metal pattern is a third lower surface in contact with the third insulating layer; a third upper surface located opposite the third lower surface and in contact with the first insulating layer; having the surface roughness of the second upper surface of the second metal pattern is greater than the surface roughness of the second lower surface of the second metal pattern and the surface roughness of the first upper surface of the first metal pattern; A semiconductor device, wherein the surface roughness of the third upper surface of the third metal pattern is greater than the surface roughness of the second lower surface of the second metal pattern and the surface roughness of the first upper surface of the first metal pattern.

2. In claim 1, the bump electrode is electrically connected to the first metal pattern; the first metal pattern is electrically connected to the second metal pattern through a via wiring formed to penetrate the second insulating layer; The first metal pattern is a via land portion to which the via wiring is joined; a wiring portion formed integrally with the via land portion and extending along a first direction; 13. A semiconductor device comprising:

3. In claim 2, the second metal pattern is disposed in a first region overlapping the semiconductor chip in a plan view; A semiconductor device, wherein the wiring portion of the first metal pattern extends from the first region toward a second region surrounding the first region in a plan view.

4. In claim 2, The first metal pattern and the second metal pattern are included in a signal transmission path.

5. In claim 4, a length of the wiring portion is longer than a length of each of the second metal pattern, the via wiring, and the via land portion; The semiconductor device, wherein the electrical signal flowing through the signal transmission path is a high-frequency signal of 30 GHz or more.

6. In claim 1, a surface roughness of the second upper surface of the second metal pattern is greater than a surface roughness of each of the second lower surface of the second metal pattern, the first upper surface of the first metal pattern, and the first lower surface of the first metal pattern; A semiconductor device, wherein the surface roughness of the third upper surface of the third metal pattern is greater than the surface roughness of the second lower surface of the second metal pattern, the first upper surface of the first metal pattern, and the first lower surface of the first metal pattern.

7. In claim 1, The semiconductor device, wherein the organic insulating film has a coefficient of thermal expansion greater than a coefficient of thermal expansion of the second insulating layer.

8. In claim 7, The organic insulating film has a linear expansion coefficient larger than a linear expansion coefficient of the second insulating layer.

9. In claim 1, a third insulating layer containing glass fiber, but the organic insulating film, the first insulating layer, and the second insulating layer each not containing glass fiber.

10. In claim 1, A semiconductor device, wherein the organic insulating film has a thickness smaller than a thickness of the second insulating layer.

11. In claim 1, A semiconductor device, wherein the surface roughness of the first upper surface of the first metal pattern is smaller than the surface roughness of the first lower surface of the first metal pattern.

12. In claim 1, a metal film is formed on the first portion of the second metal pattern; The bump electrode and the metal film are electrically connected to each other via solder.

13. In claim 1, the second metal pattern is continuous with the second upper surface and has a side surface in contact with the organic insulating film; A semiconductor device, wherein the surface roughness of the side surface of the second metal pattern is greater than the surface roughness of the second lower surface of the second metal pattern, the first upper surface of the first metal pattern, and the first lower surface of the first metal pattern.

Citation Information

Patent Citations

  • Method of manufacturing multilayer circuit board

    JP2010267712A

  • Wiring board and method for manufacturing the same

    JP2012209418A

  • Semiconductor device

    JP2013048285A

  • Multilayer printed wiring board, and method of manufacturing the same

    JP2014090130A

  • Semiconductor device

    JP2014236056A