Protective film and method for grinding backside of semiconductor wafer

A protective film with a deformable auxiliary layer addresses suction failures in semiconductor wafers with outer steps, ensuring reliable adhesion and preventing defects during back grinding.

JP7591054B2Active Publication Date: 2024-11-27MITSUI CHEM ICT MATERIA INC
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2022535380
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-07-10
Filing Date
2021-07-07
Publication Date
2024-11-27
Estimated Expiration
2041-07-07

AI Technical Summary

Technical Problem

Semiconductor wafers with steps on the outer periphery cause suction failures in fixtures due to variations in size and shape, leading to vacuum leaks during back grinding processes.

Method used

A protective film with an adhesive layer, a base layer, and an auxiliary layer is used, where the auxiliary layer has a tensile modulus of 5 MPa to 150 MPa and is made of materials like ethylene vinyl acetate copolymer, which elastically deforms to adhere the wafer to the fixture, ensuring consistent suction.

Benefits of technology

The protective film effectively suppresses suction failures and prevents defects like wafer cracking during back grinding, enhancing the manufacturing process's reliability and productivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591054000001
    Figure 0007591054000001
  • Figure 0007591054000002
    Figure 0007591054000002
  • Figure 0007591054000003
    Figure 0007591054000003
Patent Text Reader

Abstract

The present invention provides: a protective film which is capable of suppressing the occurrence of an adsorption failure; and a back grinding method for a semiconductor wafer. This protective film 30 protects a surface 11, on which a circuit has been formed, of a semiconductor wafer 10 when a back surface 12 of the semiconductor wafer 10 is ground, while having the surface 11 adsorbed onto a fixture 41. The protective film 30 comprises an adhesive layer 33, a base material layer 31 and an auxiliary layer 32. The adhesive layer 33 is bonded to the semiconductor wafer 10, while the auxiliary layer 32 comes into contact with the fixture 41. The semiconductor wafer 10 has a level difference 13 in the outer peripheral edge of the surface 11 on which circuit has been formed.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a protective film for protecting circuits on a semiconductor wafer when the surface on which the circuits are formed is attached to a fixture, and to a method for grinding the backside of a semiconductor wafer using the protective film. [Background technology]

[0002] During the manufacture of semiconductor components, after circuits and the like are formed on the front surface side of a semiconductor wafer, the back surface side is ground to make it thinner. In this back surface grinding method for grinding the back surface side, a protective film 130 is attached to the front surface 111 of a semiconductor wafer 110 on which circuits and the like are formed (see FIG. 9). The front surface 111 of the semiconductor wafer 110 is adsorbed to a fixture 141 via the protective film 130. The protective film 130 protects the circuits and the like by covering them. As a technique relating to the above-mentioned protective film and back grinding method, Patent Document 1 discloses a cutting step (trimming process) for a semiconductor wafer having a film layer formed on its surface and a chamfered portion formed on its outer circumferential side surface, in which a cutting blade is inserted from the surface of the semiconductor wafer to the outer circumferential edge while the semiconductor wafer is rotated, thereby cutting and removing at least the film layer on the chamfered portion in a circular shape. The trimmed semiconductor wafer 110 has a step 113 on the outer periphery of the surface 111. For this reason, the fixture 141 that adsorbs the semiconductor wafer 110 is designed taking the step 113 into consideration. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2012-43825 A Summary of the Invention [Problem to be solved by the invention]

[0004] It has been found that some semiconductor wafers 110 having the above-mentioned step 113 cause suction failures such as vacuum leaks in the fixture 141. This suction failure is considered to occur due to, for example, in the case of trimming processing, variations in the dimensions and shape of the step 113 caused by limitations in processing accuracy, etc.

[0005] The present invention has been made in view of the above problems, and an object of the present invention is to provide a protective film and a method for grinding the backside of a semiconductor wafer that can suppress the occurrence of suction failures. [Means for solving the problem]

[0006] As a means for solving the above problems, the present invention is as follows. [1] The invention described in claim 1 is a protective film for protecting a surface on which a circuit is formed when a back surface of a semiconductor wafer is ground while the surface on which a circuit is formed is held by suction to a fixture, comprising: The adhesive layer includes a base layer and an auxiliary layer. the pressure-sensitive adhesive layer is a layer to be attached to the semiconductor wafer, The auxiliary layer is a layer that is in contact with the fixing tool, The semiconductor wafer has a step on the outer periphery of the surface on which the circuit is formed. [2] The invention described in claim 2 is characterized in that, in the invention described in claim 1, the auxiliary layer is a layer having a tensile modulus of elasticity of 5 MPa or more and 150 MPa or less at a temperature of 25°C or more and 35°C or less. [3] The invention described in claim 3 is characterized in that, in the invention described in claim 1 or 2, the auxiliary layer contains one or more types selected from the group consisting of ethylene-vinyl acetate copolymers, polyolefin-based elastomers, styrene-based elastomers, polyester-based elastomers, and polyamide-based elastomers. [4] The invention described in claim 4 is characterized in that, in the invention described in any one of claims 1 to 3, the thickness of the auxiliary layer is 100 μm or more and 500 μm or less. [5] The invention described in claim 5 is characterized in that, in the invention described in any one of claims 1 to 4, the base material layer is a layer having a tensile modulus of elasticity of 5000 MPa or less at a temperature of 25°C or higher and 35°C or lower. [6] The invention described in claim 6 is characterized in that, in the invention described in any one of claims 1 to 5, the base material layer contains one or more types selected from the group consisting of polyester and polyamide. [7] The invention described in claim 7 is characterized in that, in the invention described in any one of claims 1 to 6, the thickness of the base material layer is 10 μm or more and 200 μm or less.

[0007] [8] The invention described in claim 8 includes a bonding step of bonding a protective film to a surface of a semiconductor wafer on which a circuit is formed; a suction step of interposing the protective film between the semiconductor wafer and a fixture that suction-holds the semiconductor wafer and suction-holding the semiconductor wafer to the fixture via the protective film; a grinding step of grinding a back surface of the semiconductor wafer while the semiconductor wafer is held by suction on the fixture via the protective film, The protective film has a pressure-sensitive adhesive layer, a base layer, and an auxiliary layer, the pressure-sensitive adhesive layer is a layer to be attached to the semiconductor wafer, The auxiliary layer is a layer that is in contact with the fixing tool, The semiconductor wafer has a step on the outer periphery of the circuit forming surface. [9] The invention described in claim 9 is characterized in that, in the invention described in claim 8, the auxiliary layer is a layer having a tensile modulus of elasticity of 5 MPa or more and 150 MPa or less at a temperature of 25°C or more and 35°C or less.

[10] The invention described in claim 10 is characterized in that, in the invention described in claim 8 or 9, the auxiliary layer contains one or more thermoplastic materials selected from the group consisting of ethylene-vinyl acetate copolymers, polyolefin-based elastomers, styrene-based elastomers, polyester-based elastomers, and polyamide-based elastomers.

[11] The invention described in claim 11 is characterized in that, in the invention described in any one of claims 8 to 10, the thickness of the auxiliary layer is 100 μm or more and 500 μm or less.

[12] The invention described in claim 12 is characterized in that, in the invention described in any of claims 8 to 11, the base material layer is a layer having a tensile modulus of elasticity of 5000 MPa or less at a temperature of 25°C or higher and 35°C or lower.

[13] The invention described in claim 13 is characterized in that, in the invention described in any of claims 8 to 12, the base material layer contains one or more thermoplastic materials selected from the group consisting of polyesters and polyamides.

[14] The invention described in claim 14 is characterized in that, in the invention described in any one of claims 8 to 13, the thickness of the base material layer is 10 μm or more and 200 μm or less. Effect of the Invention

[0008] According to the protective film and the method for grinding the backside of a semiconductor wafer of the present invention, the occurrence of suction failure can be suppressed. [Brief description of the drawings]

[0009] [Figure 1] FIG. 2 is an enlarged front cross-sectional view illustrating the protective film of the present invention. [Diagram 2] 1 is a front sectional view illustrating a semiconductor wafer according to the present invention. [Diagram 3] 1 is a front sectional view illustrating a trimming process for a semiconductor wafer according to the present invention. [Figure 4] FIG. 2 is a front sectional view illustrating a bonding step in the backgrinding method for a semiconductor wafer according to the present invention. [Diagram 5] 4 is a front sectional view illustrating a suction step in the backgrinding method for a semiconductor wafer according to the present invention. FIG. [Figure 6] 3 is a front sectional view illustrating a grinding step in the back grinding method for a semiconductor wafer according to the present invention. FIG. [Figure 7] 10 is a front sectional view illustrating another embodiment of a semiconductor wafer grinding process according to the present invention. FIG. [Figure 8]FIG. 11 is a front sectional view illustrating a semiconductor wafer according to another embodiment of the present invention. [Figure 9] FIG. 11 is a front sectional view illustrating a conventional method for suctioning a semiconductor wafer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present invention will be described below with reference to the drawings. The matters shown here are illustrative and are for illustrative purposes of the embodiments of the present invention, and are described for the purpose of providing what is believed to be the most effective and easy-to-understand explanation of the principles and conceptual features of the present invention. In this respect, it is not intended to show structural details of the present invention beyond a certain extent that are necessary for a fundamental understanding of the present invention, and the description in conjunction with the drawings will make it clear to those skilled in the art how some forms of the present invention are actually embodied.

[0011] [1] Protective film The protective film of the present invention protects the surface on which circuits are formed of a semiconductor wafer when the back surface of the semiconductor wafer is ground while the surface on which circuits are formed is held by suction to a fixture. The protective film has an adhesive layer, a base layer, and an auxiliary layer (see FIG. 1). The adhesive layer is a layer that is attached to a semiconductor wafer. The backing layer is the layer that is in contact with the fixture. The semiconductor wafer in the present invention is a semiconductor wafer having a step on the outer periphery of the surface on which the circuits are formed. Since a semiconductor wafer having this shape has a step on its outer periphery, when the back surface is ground, the surface area of ​​the surface that is adhered to the fixture (the surface on which the circuit is formed and to which the protective film is attached) may be smaller than that of a semiconductor wafer that does not have a step on its outer periphery. Therefore, since the semiconductor wafer in the present invention has a step on the outer peripheral edge of the surface on which the circuit is formed, it can also be said to be a semiconductor wafer in which the surface to be adsorbed to a fixture (the surface on which the circuit is formed) has a reduced adsorption area to the fixture. Hereinafter, in a semiconductor wafer, the surface on which circuits are formed is also referred to as the "non-ground surface," and the surface that is ground by the thinning process according to the back grinding method is also referred to as the "ground surface."

[0012] Specifically, as shown in FIG. 1, protective film 30 has a base layer 31, an auxiliary layer 32 provided on one side of base layer 31 (the bottom side in FIG. 1), and an adhesive layer 33 provided on the other side of base layer 31 (the top side in FIG. 1). In the adhering step of the backgrinding method, this protective film 30 is used with the adhesive layer 33 side facing the non-ground surface 11 of the semiconductor wafer 10. This adhesive layer 33 is adhered to the non-ground surface 11 of the semiconductor wafer 10 (see FIG. 4).

[0013] In addition, in the adsorption step in the backgrinding method, the protective film 30 is used with the auxiliary layer 32 side facing the fixture 41. The auxiliary layer 32 is brought into contact with the fixture 41 and adsorbed to the fixture 41 (see FIG. 5). Auxiliary layer 32 corresponds to the surface shape of non-ground surface 11 of semiconductor wafer 10 and the surface shape of fixture 41, and elastically deforms following these shapes. That is, auxiliary layer 32 elastically deforms to assist in adsorption of semiconductor wafer 10 to fixture 41 (see FIG. 6).

[0014] In addition, the base material layer 31 of the protective film 30 is attached to the non-ground surface 11 of the semiconductor wafer 10 by the adhesive layer 33 in the adhering step of the backgrinding method. This base material layer 31 covers the non-ground surface 11 of the semiconductor wafer 10 in the grinding step of the backgrinding method, and protects the circuits formed on the non-ground surface 11.

[0015] There is no particular limitation on the shape of the protective film 30. The protective film 30 may be, for example, circular or square in plan view. There is no particular limitation on the average thickness of the protective film 30. Specifically, the average thickness of the protective film 30 is preferably 150 to 1000 μm, more preferably 175 to 950 μm or more, and further preferably 200 to 750 μm. The average thickness is defined as the average value of the thicknesses actually measured on the film at 10 locations selected at least 2 cm apart.

[0016] Each layer of the protective film 30 will now be described. (1) Base material layer The base material layer 31 is a layer provided for the purpose of protecting the circuits formed on the non-ground surface 11 of the semiconductor wafer 10. The base material layer 31 is also a layer that improves the handleability, mechanical properties, and the like of the protective film 30. There are no particular limitations on the material used for the base layer 31 as long as it has the mechanical strength sufficient to withstand the external force in the grinding step of the back grinding method. Generally, the material of the base layer 31 is a synthetic resin film.

[0017] Examples of the synthetic resins mentioned above include one or more thermoplastic resins selected from polyolefins such as polyethylene, polypropylene, poly(4-methyl-1-pentene), poly(1-butene), etc.; ethylene-vinyl acetate copolymers; polyesters such as polyethylene terephthalate, polybutylene terephthalate, etc.; polyamides such as nylon-6, nylon-66, polymetaxylene adipamide, etc.; polyacrylates; polymethacrylates; polyvinyl chloride; polyetherimides; polyacrylonitrile; polycarbonates; polystyrenes; ionomers; polysulfones; polyethersulfones; polyphenylene ethers, etc.

[0018] The base layer 31 preferably contains one or more types selected from the group consisting of polyester and polyamide among the above-mentioned synthetic resins. When the base layer 31 contains them, the handleability of the protective film 30 can be made favorable. Additives can be added to the synthetic resins described above. Examples of additives include plasticizers, softeners (mineral oil, etc.), fillers (carbonates, sulfates, titanates, silicates, oxides (titanium oxide, magnesium oxide), silica, talc, mica, clay, fiber fillers, etc.), antioxidants, light stabilizers, antistatic agents, lubricants, colorants, etc. These additives may be used alone or in combination of two or more.

[0019] The film used as the material of the base layer 31 may be stretched or not. Any of non-stretched films and stretched films such as uniaxially stretched films and biaxially stretched films can be used. Stretched films are particularly useful from the viewpoint of improving mechanical strength. The above-mentioned film may be either a single-layer film or a multi-layer film having a plurality of layers. It is preferable to use a surface-treated film for the base layer 31. In this case, it is possible to improve adhesion to the auxiliary layer 32, etc. Specific examples of the surface treatment include corona treatment, plasma treatment, undercoat treatment, primer coat treatment, etc. The thickness of the base layer 31 is not particularly limited. 31 (see FIG. 1) is preferably 10 to 200 μm, more preferably 20 to 150 μm, and further preferably 30 to 100 μm. This thickness range is based on the viewpoint that the base layer 31 can obtain good characteristics.

[0020] Here, the tensile modulus of elasticity of the base layer 31 and the auxiliary layer 32 is obtained by reading data for each temperature from data obtained by measuring with a dynamic viscoelasticity measuring device (DMA) from 25° C. to 35° C. The measurement conditions are a sample size of 10 mm in width, a chuck length of 20 mm, a frequency of 1 Hz, and a heating rate of 5° C. / min. In the following, the tensile modulus of elasticity of the base layer 31 at 25° C. is defined as E′ 31 (25), the value at 35°C is E' 31 (35), and the value of each temperature between 25℃ and 35℃ is E' 31 Let (t). The tensile modulus of the auxiliary layer 32 at 25° C. is E′ 32 (25), the value at 35°C is E' 32 (35), and the value of each temperature between 25℃ and 35℃ is E' 32 Let (t).

[0021] The tensile modulus of the base layer 31 is usually E' 31 (t)≦5000 MPa. That is, in the temperature range of 25° C.≦t≦35° C., the tensile modulus of the base layer 31 is always 5000 MPa or less. Therefore, E′ 31 (25)≦5000MPa, E' 31 (35)≦5000 MPa. Also, usually, E' 31 (t)>E' 32 That is, in the temperature range of 25° C.≦t≦35° C., the tensile modulus of the base layer 31 is always higher than the tensile modulus of the auxiliary layer 32. There is no limitation on the degree of the difference, but E′ 31 (t) is E' 32 It is preferably 20 to 4850 MPa higher than (t), and more preferably 700 to 4850 MPa higher.

[0022] Therefore, at t=25° C., the difference (E′ 31 (25)-E' 32 (25)) is 20MPa ≦ E' 31 (25)-E' 32 (25) ≦4850MPa is preferable, and 700MPa ≦ E' 31 (25)-E' 32 (25)≦4850 MPa is more preferable. Similarly, at t=35° C., the difference (E′ 31 (35)-E' 32 (35)) is 20MPa ≦ E' 31 (35)-E' 32 (35) ≦4850MPa is preferable, and 700MPa ≦ E' 31 (35)-E' 32 (35)≦4850 MPa is more preferable.

[0023] The tensile modulus of elasticity of the base layer 31 and the tensile modulus of elasticity of the auxiliary layer 32 have the above-mentioned relationship. When the semiconductor wafer 10 is attached to the fixture 41, the base material layer 31 has a tensile modulus that is always higher than the tensile modulus of the auxiliary layer 32, and therefore maintains a shape that covers the non-ground surface 11 to protect the circuits on the non-ground surface 11 of the semiconductor wafer 10 (see FIG. 5). On the other hand, auxiliary layer 32 elastically deforms because its tensile modulus is always lower than that of base layer 31. Regarding this elastic deformation of auxiliary layer 32, the back layer portion on the base layer 31 side conforms to the shape of base layer 31, and the front layer portion on the fixing device 41 side conforms to the surface shape of fixing device 41 (see FIG. 5).

[0024] (2) Auxiliary layer The auxiliary layer 32 is a layer provided for the purpose of assisting the semiconductor wafer 10 in being attached to the fixture 41 in the suction step of the back grinding method. Specifically, auxiliary layer 32 is a layer that can elastically deform in response to both the surface shape of semiconductor wafer 10 having steps 13 and the surface shape of fixture 41 (see FIG. 5). Then, the elastically deformed auxiliary layer 32 assists in adhering semiconductor wafer 10 to fixture 41. The flexibility of the auxiliary layer 32 is increased when the tensile modulus is reduced. In this case, the ability of the auxiliary layer 32 to conform to the surface shapes of the non-ground surface 11 of the semiconductor wafer 10 and the fixture 41 (such as a chuck table) can be improved. Furthermore, when the tensile modulus of elasticity of the auxiliary layer 32 is increased, the hardness of the auxiliary layer 32 is increased. In this case, the auxiliary layer 32 is prevented from sticking to the fixture 41 (such as a chuck table), and the ease of attachment and detachment between the auxiliary layer 32 and the fixture 41 can be improved.

[0025] The tensile modulus of the auxiliary layer 32 is preferably 5 MPa≦E′ 32(t)≦150 MPa. That is, the tensile modulus of the auxiliary layer 32 is 5 MPa or more and 150 MPa or less in the temperature range of 25° C.≦t≦35° C. In this case, the auxiliary layer 32 can exhibit sufficient elasticity (mechanical stretchability) at the environmental temperature where the backgrinding method is performed. More preferably, the tensile modulus E' is 6 MPa or less. 32 (t)≦120 MPa. More preferably, 7 MPa≦E′ 32 (t)≦80 MPa. Particularly preferably, 8 MPa≦E' 32 (t)≦60 MPa. Particularly preferably, 9 MPa≦E′ 32 (t)≦45 MPa.

[0026] There is no particular limitation on the material used for the auxiliary layer 32. The material for the auxiliary layer 32 is preferably a resin, and among resins, a resin having sufficient elasticity (mechanical stretchability) is more preferable, and a resin containing a thermoplastic material having elastomeric properties is particularly preferable. The thermoplastic material having elastomeric properties may be made of a block copolymer having a hard segment and a soft segment, may be made of a polymer alloy of a hard polymer and a soft polymer, or may have properties of both of these. Examples of the thermoplastic material include ethylene-vinyl acetate copolymers, polyolefin-based elastomers, styrene-based elastomers, polyester-based elastomers, polyamide-based elastomers, etc. These may be used alone or in combination of two or more.

[0027] When the material of the auxiliary layer 32 is a resin containing the above-mentioned thermoplastic material, the ratio of the thermoplastic material can be preferably 40 to 100 mass %, more preferably 60 to 100 mass %, and further preferably 80 to 100 mass %, based on the entire resin constituting the auxiliary layer 32. In other words, the resin constituting the auxiliary layer 32 may consist only of the above-mentioned thermoplastic material. Among the above-mentioned thermoplastic materials, ethylene-vinyl acetate copolymer is particularly preferred because its elasticity can be adjusted according to the vinyl acetate content. The vinyl acetate content in the ethylene-vinyl acetate copolymer is preferably 4 to 30% by mass, more preferably 5 to 25% by mass, and even more preferably 8 to 20% by mass, based on 100% by mass of the entire polymer. The thickness of the auxiliary layer 32 is not particularly limited. 32 (See FIG. 1) is preferably 100 to 500 μm, more preferably 100 to 400 μm, and further preferably 100 to 250 μm. This thickness range is based on the viewpoint of maintaining a margin sufficient to allow elastic deformation. In addition, the thickness T of the auxiliary layer 32 32 is usually 1.0 times or more the height H of the step 13 in the thickness direction of the semiconductor wafer 10 (see FIG. 2) (H≦T 32 ), preferably 1.5 times or more (1.5×H≦T 32 ), and more preferably 2.0 times or more (2.0×H≦T 32 ).

[0028] (3) Adhesive layer The adhesive layer 33 is a layer provided for the purpose of being attached to the non-ground surface 11 of the semiconductor wafer 10 in the attachment step in the backgrinding method. Specifically, the adhesive layer 33 can be formed by applying or laminating an adhesive or the like to the surface of the base layer 31 facing the non-ground surface 11 (the upper surface in FIG. 1).

[0029] The adhesive used in the adhesive layer 33 is not particularly limited. Examples of the adhesive include (meth)acrylic adhesives, silicone adhesives, urethane adhesives, rubber adhesives, energy ray curable adhesives, and acrylic, epoxy and silicone adhesives.

[0030] The adhesive strength of the adhesive layer 33 is not particularly limited. The adhesive strength is preferably 0.1 to 10 N / 25 mm, more preferably 0.2 to 9 N / 25 mm, and further preferably 0.3 to 8 N / 25 mm. The range of adhesive strength is determined from the viewpoint of ensuring good adhesion to the semiconductor wafer while suppressing adhesive residue on the semiconductor wafer when peeled off. The adhesive strength is the adhesive strength to a silicon wafer measured in accordance with JIS Z 0237. Specifically, it is the measured value when the tape is attached to the surface of a silicon wafer in an environment of 23°C temperature and 50% relative humidity, left for 60 minutes, and then peeled off from the surface of the silicon wafer.

[0031] The thickness of the adhesive layer 33 is not particularly limited. The thickness T of the adhesive layer 33 33 (See FIG. 1) is preferably 1 to 50 μm, more preferably 2 to 45 μm, and even more preferably 3 to 40 μm. This thickness range is based on the viewpoint of exhibiting suitable adhesive strength while enabling peeling without leaving any adhesive residue.

[0032] The adhesive layer 33 of the protective film 30 only needs to be provided on the surface of the base layer 31 on the side of the non-ground surface 11 when the protective film 30 is attached to the semiconductor wafer 10. For example, a laminate of base layer 31 and auxiliary layer 32 is prepared in advance, and just before this laminate is attached to semiconductor wafer 10, an adhesive or the like is applied or laminated to the laminate or semiconductor wafer 10, and then the laminate and semiconductor wafer 10 are bonded together to form adhesive layer 33.

[0033] (4) Other layers The protective film 30 is not limited to the configuration having the above-mentioned layers, and may have other layers.

[0034] As another layer, for example, in the case of a semiconductor wafer 10 having bumps 15 as exemplified in FIG. 8, an unevenness absorbing layer that absorbs the uneven shape caused by the bumps 15 can be mentioned. The irregularity absorbing layer can be formed by laminating one surface of the base layer 31 on the non-ground surface 11 side, particularly between the base layer 31 and the adhesive layer 33. The material of this irregularity absorbing layer is not particularly limited as long as it has irregularity absorbing properties due to the expression of fluidity or plasticity. Examples of such materials include acrylic resins, olefin resins, and ethylene-polar monomer copolymers. The thickness of the irregularity absorbing layer is not particularly limited as long as it is thick enough to absorb the irregularities caused by the bumps 15. The thickness is preferably 20 μm or more, more preferably 80 μm or more, and even more preferably 170 μm or more.

[0035] Moreover, a layer having the same configuration as the auxiliary layer 32 can be provided on one surface of the base material layer 31 that is the non-ground surface 11 side, particularly between the base material layer 31 and the adhesive layer 33. In this case, the protective film 30 can prevent warping of the semiconductor wafer 10 to which it is attached.

[0036] Further, other layers include, for example, an interface strength improving layer that improves the interface strength with the adhesive layer 33, a migration prevention layer that suppresses the migration of low molecular weight components to the surface of the adhesive layer 33, and an antistatic layer that prevents the protective film 30 from becoming static. The above-mentioned other layers may be used alone or in combination of two or more.

[0037] [2] Semiconductor wafers The semiconductor wafer used in the present invention is used for manufacturing semiconductor parts, and is not particularly limited in terms of material or shape, as long as it has a circuit formed on one surface (non-ground surface). Usually, the semiconductor wafer is formed into a disk shape using silicon as the material (see FIG. 2). This semiconductor wafer is thinned by grinding the back surface (ground surface) opposite to the surface on which the circuits are formed (non-ground surface).

[0038] The protective film of the present invention is used in a back grinding method for thinning a semiconductor wafer. The semiconductor wafer to which this protective film is applied may be one that does not have a step on the outer periphery of the surface (non-ground surface) on which a circuit is formed, but may also be suitably used for one that has a step on the outer periphery of the surface (non-ground surface) on which a circuit is formed. That is, when the back surface of the semiconductor wafer is ground, a protective film is attached to the non-ground surface in order to protect the non-ground surface. The semiconductor wafer with the protective film attached is fixed to a fixture by vacuum suction or the like on the surface to which the protective film is attached (non-ground surface). When a protective film is attached to the non-ground surface of a semiconductor wafer and fixed to a fixture, a semiconductor wafer having a step on the outer periphery of the non-ground surface may have a smaller adsorption area to the fixture of the non-ground surface than a semiconductor wafer having no step on the outer periphery of the non-ground surface. In this way, the protective film of the present invention can be suitably used for a semiconductor wafer having a step on the outer periphery of the surface (non-ground surface) on which a circuit is formed and a smaller adsorption area to the fixture of the non-ground surface. Therefore, since the semiconductor wafer in the present invention has a step on the outer peripheral edge of the surface on which the circuit is formed, it can also be said to be a semiconductor wafer in which the surface to be adsorbed to a fixture (the surface on which the circuit is formed) has a reduced adsorption area to the fixture.

[0039] Specifically, the semiconductor wafer 10 is formed in a plate shape as shown in Fig. 2. Circuits are formed on the non-ground surface 11 of the semiconductor wafer 10. The semiconductor wafer 10 is thinned to a desired thickness by grinding the ground surface 12 (see Fig. 6). Furthermore, as shown in FIG. 7, the present invention can also be used for grinding the grinding surface 12 in DBG (dicing before gridding) or SDBG (stealth dicing before gridding). The semiconductor wafer 10 has arcuate surfaces 14 at the portions extending from the non-ground surface 11 or the ground surface 12 to the outer surface due to the chamfering process. In the trimming process, the arcuate surfaces 14 on the non-ground surface 11 side are cut and removed (see FIG. 3). The trimmed semiconductor wafer 10 has a concave step 13 on the outer periphery of the non-ground surface 11 (see FIG. 2).

[0040] Here, the above-mentioned trimming process will be described. An example of a trimming device 20 used in the trimming process includes a chuck table 21 that adheres to the semiconductor wafer 10 by vacuum suction, and a trimming blade 22, as shown in FIG. During trimming, the semiconductor wafer 10 is fixed to the chuck table 21 with the grinding surface 12 being attracted to the chuck table 21 . The trimming process is performed by pressing a trimming blade 22 against the outer periphery of the non-ground surface 11 of the semiconductor wafer 10 while rotating a chuck table 21 to which the semiconductor wafer 10 is fixed by suction. In the trimmed semiconductor wafer 10, the arcuate surface 14 on the non-ground surface 11 side is cut and removed by the trimming blade 22, so that a concave step 13 is formed on the outer periphery of the non-ground surface 11.

[0041] The step 13 resulting from the above-mentioned trimming process has a width W in the radial direction of the semiconductor wafer 10 of preferably 1 to 10 mm, more preferably 2 to 8 mm, and particularly preferably 3 to 7 mm (see FIG. 2). Moreover, the height H of this step 13 in the thickness direction of the semiconductor wafer 10 is preferably 10 to 100 μm, more preferably 20 to 80 μm, and particularly preferably 30 to 70 μm (see FIG. 2).

[0042] The step 13 is not limited to that caused by the trimming process. Examples of the semiconductor wafer 10 having the step 13 on the outer periphery of the non-ground surface 11 other than that caused by the trimming process include the semiconductor wafer 10 having the following configuration. In the semiconductor wafer 10 shown in FIG. 8, a plurality of bumps 15 are formed on the non-ground surface 11, resulting in a step 13 being generated on the outer periphery on the non-ground surface 11 side. Although not specifically shown, the semiconductor wafer having the above-mentioned step may also be a wafer having a multilayer film formed on the non-ground surface.

[0043] Regarding the above-mentioned step 13, the width W and height H are respectively the average values ​​of the measured widths and heights of four step portions selected to be spaced at central angle intervals of 10 to 90 degrees. In the present invention, the step 13 on the semiconductor wafer 10 includes a step caused by trimming processing, and further a step caused by the formation of a bump or a multilayer film. Specifically, the step 13 caused by the formation of the bump or multilayer film has a height difference (height H in the thickness direction of the semiconductor wafer 10) of 10 to 300 μm within a width W in the radial direction of the semiconductor wafer 10 from the outer peripheral edge of the semiconductor wafer 10 that is within a range of 1 to 30 mm (see Figure 8).

[0044] The protective film of the present invention can be used for any type of semiconductor wafer 10. In particular, a wafer having a reduced suction area for a fixture such as a chuck table is useful as the semiconductor wafer 10. A trimmed wafer is particularly an example of the semiconductor wafer 10 with a reduced suction area. In this trimmed semiconductor wafer 10, the outer peripheral edge of the non-ground surface 11 is trimmed (notched) to provide a step 13, thereby reducing the suction area for the fixture 41 (such as a chuck table). Here, the above-mentioned "attachment area" refers to an area on which the suction force of fixture 41 can act.

[0045] More specifically, the trimmed semiconductor wafer 10 has a step 13 formed by cutting the outer periphery of the non-ground surface 11 into a concave shape. On the non-ground surface 11 of the semiconductor wafer 10, the step 13 and a portion other than the step 13 do not come into contact with the fixture 41 on the same plane. For this reason, the suction force of the fixture 41 does not act easily or does not act at the step 13. Here, the actual suction area ar1 on the non-ground surface 11 of the semiconductor wafer 10 is a value obtained by subtracting the planar area of ​​the portion corresponding to the step 13 from the planar area ar2 of the semiconductor wafer 10 (see FIG. 2). In other words, in the semiconductor wafer 10 having the step 13 on the outer periphery of the non-ground surface 11, the suction force of the fixture 41 acts only on the suction area ar1 which is smaller than the planar area ar2. In other words, the semiconductor wafer 10 has a step 13 on the outer peripheral edge of the non-ground surface 11, and therefore the adsorption area ar1 of the non-ground surface 11 with respect to the fixing device 41 is subtracted from the planar area ar2 of the semiconductor wafer 10 (non-ground surface 11).

[0046] [3] Back grinding method The method for grinding the backside of a semiconductor wafer according to the present invention includes a bonding step, a suction step, and a grinding step. The adhesion step is a step of adhering a protective film to the surface of the semiconductor wafer on which the circuits are formed. The suction step is a step in which a protective film is interposed between the semiconductor wafer and a fixture that suctions the semiconductor wafer, and the semiconductor wafer is suction-attached to the fixture via the protective film. The grinding step is a step of grinding the back surface of the semiconductor wafer while the semiconductor wafer is held by suction on a fixture via a protective film. The protective film includes a pressure-sensitive adhesive layer, a base layer, and an auxiliary layer. The adhesive layer is a layer that is attached to a semiconductor wafer. The backing layer is the layer that is in contact with the fixture. The semiconductor wafer in the present invention is a semiconductor wafer having a step on the outer periphery of the surface on which the circuit is formed. Since a semiconductor wafer having such a shape has a step on the outer periphery, when the back surface is ground, the surface to be adsorbed to a fixture (the surface on which the circuit is formed and to which the protective film is attached) may have a smaller adsorption area to the fixture than a semiconductor wafer having no step on the outer periphery. Therefore, the semiconductor wafer in the present invention has a step on the outer peripheral edge of the surface on which the circuit is formed, and therefore has a reduced area for adsorption to the fixture of the surface to be adsorbed to the fixture (the surface on which the circuit is formed).

[0047] Specifically, the back surface grinding method is a method for thinning the semiconductor wafer 10 by grinding the back surface of the semiconductor wafer 10. This back grinding method is performed using a processing device 40 equipped with a fixture 41 that adsorbs and fixes the semiconductor wafer 10, and a grinding tool 42 that grinds the grinding surface 12 of the semiconductor wafer 10, as shown in Figures 5 and 6. In the back grinding method, the protective film 30 is used to protect the circuits formed on the non-ground surface 11 when the back surface of the semiconductor wafer 10 is ground. As described above, the protective film 30 has the base layer 31, the auxiliary layer 32, and the adhesive layer 33. As described above, semiconductor wafer 10 has step 13 on the outer periphery of non-ground surface 11 (surface on which circuits are formed), and the adhesion area of ​​non-ground surface 11 to fixture 41 is reduced. The adhering step, the suction step, and the grinding step will be described below.

[0048] (1) Pasting process The adhering step is a step for adhering the above-mentioned protective film 30 to the semiconductor wafer 10. As shown in FIG. 4, in the adhering step, the protective film 30 is adhered to the non-ground surface 11 of the semiconductor wafer 10. In the adhering step, the protective film 30 is adhered to the unground surface 11 of the semiconductor wafer 10 so as to cover the uneven shape of the unground surface 11 of the semiconductor wafer 10, particularly the steps 13 on the outer periphery. Furthermore, a resin such as an adhesive layer can be interposed between the protective film 30 and the non-ground surface 11 of the semiconductor wafer 10. In this case, the interposed resin can more reliably protect the non-ground surface 11 of the semiconductor wafer 10. In the adhering step, there is no particular limitation on the method and device for adhering the protective film 30 to the semiconductor wafer 10. Existing methods and devices can be used for the method and device.

[0049] (2) Adsorption process The suction step is a step for the purpose of suctioning the semiconductor wafer 10 to which the above-mentioned protective film 30 is attached, onto the fixture 41. By this suction process, a protective film 30 is interposed between the non-ground surface 11 of the semiconductor wafer 10 and a fixture 41 that adsorbs the semiconductor wafer 10, and the semiconductor wafer 10 is adsorbed to the fixture 41 via the protective film 30.

[0050] Specifically, as shown in FIG. 5, the semiconductor wafer 10 to which the protective film 30 has been attached in the above-mentioned attachment step is adsorbed to a fixture 41 with the non-ground surface 11 facing the fixture 41 side. In this adsorption step, the surface layer portion of auxiliary layer 32 of protective film 30 on the side of fixing tool 41 is elastically deformed to conform to the surface shape of fixing tool 41 . In other words, the auxiliary layer 32 of the protective film 30 elastically deforms so as to maintain the adsorption area ar3 with respect to the fixture 41 at approximately the same size as the area ar4 of the surface of the fixture 41, without being affected by the surface shape of the non-ground surface 11, and in particular, regardless of the adsorption area ar1 which becomes uncertain due to variations in the step 13, etc.

[0051] In other words, by having the elastically deformable auxiliary layer 32, the protective film 30 can maintain an adsorption area ar3 that allows it to be reliably adsorbed to the fixing device 41 without being affected by the surface shape of the semiconductor wafer 10, such as steps 13. Therefore, since the protective film 30 has the auxiliary layer 32, the occurrence of poor adhesion of the semiconductor wafer 10 due to the step 13 is suppressed. Therefore, the protective film 30 of the present invention is particularly useful in a method for grinding the back surface of a semiconductor wafer 10 having a step 13 caused by a trimming process.

[0052] (3) Grinding process The grinding step is a step for the purpose of thinning the semiconductor wafer 10 by grinding the grinding surface 12 of the semiconductor wafer 10. As shown in FIG. 6, in the grinding step, a grinding tool 42 is brought into contact with the grinding surface 12 of the semiconductor wafer 10 while the semiconductor wafer 10 is kept in a state of being sucked by the fixture 41 in the above-mentioned suction step. In the processing device 40, the grinding tool 42 is configured to be rotatable about an axis extending in the thickness direction of the semiconductor wafer 10 as the center of rotation, and is also configured to be movable in the thickness direction of the semiconductor wafer 10. In addition, in the processing device 40, the fixing tool 41 is configured to be rotatable about its center as the axis. Then, while the grinding tool 42 and the fixing tool 41 are each rotated, the grinding tool 42 moves to keep the grinding tool 42 in contact with the grinding surface 12, thereby grinding the grinding surface 12 and thinning the semiconductor wafer 10.

[0053] The present invention can also be used in back grinding of DBG and SDBG. That is, as shown in FIG. 7, in DBG and SDBG, the semiconductor wafer 10 has a plurality of half-cut portions 17 on the non-ground surface 11 in the case of DBG, and a plurality of modified layers 17 in the case of SDBG. In a processing step, the ground surface 12 of the semiconductor wafer 10 is ground to thin the wafer, and the wafer is separated at each half-cut portion 17 or each modified layer 17 into a plurality of chips 10A. EXAMPLES

[0054] The present invention will now be described in detail with reference to examples. [Protective film] The protective film 30 used was for a 12-inch screen. The configuration of the protective film 30, the base layer 31, and the auxiliary layer 32 are as follows. (1) Base material layer 31 Material: Polyethylene terephthalate film, E' 31 (25): 4726MPa, E' 31 (35): 4581 MPa. Thickness: 50μm. (2) Adhesive layer 33 Material: UV-curable acrylic adhesive Thickness: 20μm. (3) Auxiliary layer 32 Example 1 Material: Ethylene vinyl acetate copolymer (vinyl acetate content: 19%), E' 32 (25): 21MPa, E' 32 (35): 17 MPa. Thickness: 120μm. Example 2 Material: Ethylene vinyl acetate copolymer (vinyl acetate content: 9%), E' 32 (25): 40MPa, E' 32 (35): 34 MPa. Thickness: 120μm. Example 3 Material: Ethylene vinyl acetate copolymer (vinyl acetate content: 9%), E' 32 (25): 40MPa, E' 32 (35): 34 MPa. Thickness: 160μm. Comparative Example 1 The auxiliary layer 32 was not provided.

[0055] [Semiconductor wafers] The following was used as the semiconductor wafer 10 provided with circuits. (1) Specifications Diameter: 300mm. Thickness: 810μm. Material: Silicon. (2) Step 13 The width W was set to 5 mm and the height H to 50 μm, and trimming was performed to form a step 13 (see FIG. 2).

[0056] [Back grinding method] (1) Pasting process A tape application machine (manufactured by Nitto Seiki, product number "DR-3000II") was prepared, and protective film 30 was applied to non-ground surface 11 of semiconductor wafer 10, and excess portion was cut off to obtain samples of Examples 1 to 3 and Comparative Example 1.

[0057] (2) Adsorption process A processing device (Disco Corp., product number "DGP8760") was prepared, and each of the samples of Examples 1 to 3 and Comparative Example 1 was attached to fixture 41, and the presence or absence of attachment failure was observed. In this observation, each sample was adsorbed to the fixture 41 three times, and the number of occurrences of adsorption failure was counted. As a result of the observation, in Examples 1 to 3, no adsorption failure occurred at all. On the other hand, in Comparative Example 1, adsorption failure occurred in all three adsorption attempts. The above results show that the protective film 30 having the auxiliary layer 32 can prevent poor adsorption.

[0058] (3) Grinding process In the above-mentioned (2) adsorption step, no poor adsorption occurred at all. For Examples 1 to 3, the grinding step was carried out using the above-mentioned processing device. In this grinding process, three pieces of each sample were ground on the backside, and the number of defects such as wafer cracks was measured. As a result, in Examples 1 to 3, no defects such as wafer cracking occurred. The above results show that the protective film 30 having the auxiliary layer 32 can prevent defects such as wafer cracking during the grinding process. [Industrial Applicability]

[0059] The protective film of the present invention is widely used in applications for manufacturing semiconductor parts. In particular, since the protective film has a property of suitably suppressing poor adhesion to a fixture in a semiconductor wafer having a step on its outer periphery, it is suitably used for manufacturing parts with excellent productivity. [Explanation of symbols]

[0060] 10;Semiconductor wafer, 11: Non-ground surface (surface on which a circuit is formed), 12; grinding surface, 13;Steps, 14; Arc surface, 15;Bump, 17: Half-cut portion or modified layer 20;Trimming device, 21; Chuck table, 22; trimming blade, 30; protective film, 31; base material layer, 32; auxiliary layer, 33; adhesive layer, 40; processing equipment; 41; Fixtures; 42;Grinding tools.

Claims

1. A protective film for protecting a surface on which circuits are formed when a back surface of a semiconductor wafer is ground in a state in which the surface on which circuits are formed of the semiconductor wafer is held by suction to a fixture, the protective film comprising: The adhesive layer includes a base layer and an auxiliary layer. the pressure-sensitive adhesive layer is a layer to be attached to the semiconductor wafer, The auxiliary layer is a layer that is in contact with the fixing tool, the semiconductor wafer has a step on an outer periphery of the surface on which the circuit is formed, A protective film characterized in that, when the thickness of the auxiliary layer is T 32 and the height of the step is H, T 32 is 100 to 500 μm, H is 10 to 100 μm, and the relationship H≦T 32 is satisfied.

2. The protective film according to claim 1 , wherein the auxiliary layer has a tensile modulus of elasticity of 10 MPa or more and 200 MPa or less at a temperature of 25° C. or more and 35° C. or less.

3. A protective film as described in claim 1 or 2, wherein the auxiliary layer comprises a thermoplastic material having elastomeric properties.

4. The protective film according to claim 3 , wherein the thermoplastic material having elastomeric properties comprises one or more selected from the group consisting of ethylene-vinyl acetate copolymers, polyolefin-based elastomers, styrene-based elastomers, polyester-based elastomers, and polyamide-based elastomers.

5. The protective film according to claim 1 , wherein the base layer is a layer having a tensile modulus of elasticity of 5000 MPa or less at a temperature of 25° C. or more and 35° C. or less.

6. The protective film according to claim 1 , wherein the base layer comprises one or more materials selected from the group consisting of polyesters and polyamides.

7. 7. The protective film according to claim 1, wherein the thickness of the base layer is from 10 μm to 200 μm.

8. a bonding step of bonding a protective film to a surface of the semiconductor wafer on which a circuit is formed; a suction step of interposing the protective film between the semiconductor wafer and a fixture that suction-holds the semiconductor wafer and suction-holding the semiconductor wafer to the fixture via the protective film; a grinding step of grinding a back surface of the semiconductor wafer while the semiconductor wafer is held by suction on the fixture via the protective film, The protective film has a pressure-sensitive adhesive layer, a base layer, and an auxiliary layer, the pressure-sensitive adhesive layer is a layer to be attached to the semiconductor wafer, The auxiliary layer is a layer that is in contact with the fixing tool, the semiconductor wafer has a step on an outer periphery of the surface on which the circuit is formed, The method for grinding the backside of a semiconductor wafer, wherein, when the thickness of the auxiliary layer is T 32 and the height of the step is H, T 32 is 100 to 500 μm, H is 10 to 100 μm, and the relationship H≦T 32 is satisfied.

9. 9. The method for grinding the backside of a semiconductor wafer according to claim 8, wherein the auxiliary layer has a tensile modulus of elasticity of 10 MPa or more and 200 MPa or less at a temperature of 25° C. or more and 35° C. or less.

10. A method for grinding the back surface of a semiconductor wafer as described in claim 8 or 9, wherein the auxiliary layer contains a thermoplastic material having elastomeric properties.

11. 11. The method for grinding the backside of a semiconductor wafer according to claim 10, wherein the thermoplastic material having elastomeric properties includes one or more selected from the group consisting of ethylene-vinyl acetate copolymers, polyolefin-based elastomers, styrene-based elastomers, polyester-based elastomers, and polyamide-based elastomers.

12. 12. The method for grinding the backside of a semiconductor wafer according to claim 8, wherein the base layer is a layer having a tensile modulus of elasticity of 5000 MPa or less at a temperature of 25° C. to 35° C.

13. 13. The method for grinding the backside of a semiconductor wafer according to claim 8, wherein the base layer contains one or more materials selected from the group consisting of polyester and polyamide.

14. 14. The method for grinding the backside of a semiconductor wafer according to claim 8, wherein the thickness of the base layer is 10 μm or more and 200 μm or less.

Citation Information

Patent Citations

  • Method and apparatus for manufacturing semiconductor device

    JP2000173961A

  • Adhesive film for protecting semiconductor wafer and method for processing back of semiconductor wafer using the same

    JP2002069396A

  • Wafer processing method

    JP2012043825A

  • Base film and pressure-sensitive adhesive sheet with base film

    JP2013077758A

  • Processing method for wafer

    JP2017069489A