Method for manufacturing glass articles

By controlling temperature differences and glass composition, the method addresses devitrification issues in glass ribbon molding, improving production efficiency and quality by reducing yttrium oxide elution and defects.

JP7591194B2Active Publication Date: 2024-11-28NIPPON ELECTRIC GLASS CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020210346
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-18
Publication Date
2024-11-28
Estimated Expiration
2040-12-18

AI Technical Summary

Technical Problem

Devitrification derived from yttrium-containing oxides occurs during the molding of glass ribbons, leading to defects and reducing production efficiency and quality in glass articles.

Method used

The method involves controlling the temperature difference between the molten glass in the groove part and the lower end of the molded body to 100°C or less, using an overflow down-draw method, and adjusting the glass composition to include specific proportions of SiO2, Al2O3, B2O3, Na2O, K2O, Li2O, MgO, and P2O5, while incorporating a Mg-rich layer to inhibit yttrium oxide elution.

Benefits of technology

This approach effectively reduces devitrification from yttrium-containing oxides, enhancing production efficiency and quality by preventing defects in glass ribbons and plates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591194000001
    Figure 0007591194000001
  • Figure 0007591194000002
    Figure 0007591194000002
  • Figure 0007591194000003
    Figure 0007591194000003
Patent Text Reader

Abstract

To mold a glass ribbon by the overflow downdraw method while the devitrified materials derived from yttrium-containing oxide contained in the molded body are positively reduced.SOLUTION: A method for producing a glass article comprises a molding step for flowing down a molten glass Gm overflowed from a groove 8 in a molded body 3 along both side surfaces 10 of the molded body 3 by the overflow downdraw method, and then merging the molten glass Gm flowing down along both side surfaces 10 into one at a lower end 3a of the molded body 3 to mold a glass ribbon Gr. The molded body 3 contains yttrium-containing oxide, and the molten glass Gm contains P2O5. In the molding step, the temperature difference (T1-T2) between the temperature T1 of the molten glass Gm in the groove 8 and the temperature T2 of the molten glass Gm in the lower end 3a is 100°C or less.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a glass article. [Background technology]

[0002] In a manufacturing process of glass products such as glass sheets and glass rolls, for example, by the overflow downdraw method, molten glass is caused to flow down along the surface of a forming body to continuously form a glass ribbon. The formed glass ribbon is cooled to about room temperature while being transported downstream, and then cut into predetermined lengths to obtain glass sheets, or wound into a roll to obtain a glass roll (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2018-062433 A Summary of the Invention [Problem to be solved by the invention]

[0004] In the above-mentioned compact, in order to improve the mechanical strength, an yttrium-containing oxide (e.g., a composite oxide of yttrium and aluminum, YAlO 12 ) may be added.

[0005] As a result of intensive research, the inventors of the present application have found for the first time that when a glass ribbon containing P2O5 is formed using a formed body containing an yttrium-containing oxide, yttrium oxide is dissolved or diffused from the yttrium-containing oxide contained in the formed body into molten glass, generating devitrified matter at the lower end of the formed body. Since such devitrified matter originating from the yttrium-containing oxide can become a defect in the glass ribbon and / or glass article, it is important to reduce the amount of devitrified matter generated from the viewpoints of production efficiency and quality improvement.

[0006] In addition, the devitrified matter derived from the yttrium-containing oxide is considered to be generated, for example, by a reaction between yttrium oxide (Y2O3) dissolved from the yttrium-containing oxide into the molten glass and P2O5 of the molten glass. In other words, the devitrified matter derived from the yttrium-containing oxide is considered to be, for example, a devitrified matter containing yttrium oxide and P2O5 (Y2O3-P2O5 crystal).

[0007] An object of the present invention is to reliably reduce the generation of devitrified matter originating from yttrium-containing oxides contained in a formed body when a glass ribbon is formed using an overflow downdraw method. [Means for solving the problem]

[0008] (1) The present invention, which has been invented to solve the above problems, is a method for producing a glass article, which includes a forming step in which molten glass overflowing from grooves of a forming body is caused to flow down both side surfaces of the forming body by an overflow downdraw method, and then fused at a lower end of the forming body to form a glass ribbon, wherein the forming body contains an yttrium-containing oxide and the molten glass contains P2O5, and in the forming step, the temperature difference between the molten glass in the grooves and the molten glass at the lower end is set to 100°C or less.

[0009] In this way, even if yttrium oxide dissolves from the yttrium-containing oxide contained in the molded body into the molten glass, the temperature difference of the molten glass between the groove portion of the molded body and its lower end portion is small, so that it is possible to suppress the generation of devitrified matter derived from the yttrium-containing oxide (for example, devitrified matter containing yttrium oxide and P2O5) at the lower end portion of the molded body.

[0010] (2) In the above configuration (1), the temperature of the molten glass in the groove is preferably 1300° C. or less.

[0011] In this way, the viscosity of the molten glass is prevented from becoming too low, making it easier to form a glass ribbon from the molten glass.

[0012] (3) In the above configuration (1) or (2), the temperature of the molten glass at the lower end is preferably 1100° C. or higher.

[0013] In this way, the viscosity of the molten glass is prevented from becoming too high, making it easier to form a glass ribbon from the molten glass.

[0014] (4) In the above configurations (1) to (3), the molten glass preferably contains, as a glass composition, by mass%, 40 to 70% SiO2, 10 to 30% Al2O3, 0 to 3% B2O3, 5 to 25% Na2O, 0 to 5.5% K2O, 0.1 to 10% Li2O, 0 to 5.5% MgO, and 2 to 10% P2O5.

[0015] In this way, the aluminosilicate glass becomes suitable for chemically strengthened glass, and it becomes easier to achieve both high levels of ion exchange performance and high levels of devitrification resistance.

[0016] (5) In the above configurations (1) to (4), the molten glass preferably contains 0 to 1 mass % MgO.

[0017] When the molten glass has a high MgO content, a Mg-rich layer capable of suppressing the elution of yttrium oxide from the yttrium-containing oxide is formed on the surface of the molded body. For example, when the molded body is an alumina-based refractory, the Mg-rich layer is a layer mainly composed of spinel (MgAl2O4). Therefore, yttrium oxide is less likely to be eluted from the yttrium-containing oxide of the molded body into the molten glass. In contrast, when the MgO content of the molten glass is 1% by mass or less, a Mg-rich layer is less likely to be formed on the surface of the molded body. Therefore, yttrium oxide is more likely to be eluted from the yttrium-containing oxide of the molded body into the molten glass. Therefore, when the MgO content of the molten glass is 1% by mass or less, the effect of the present invention becomes remarkable.

[0018] (6) In the above configurations (1) to (5), the molded body preferably contains 1% by mass or more of an yttrium-containing oxide.

[0019] In this way, yttrium oxide is easily dissolved from the yttrium-containing oxide of the formed body into the molten glass, and the effect of the present invention becomes remarkable. Effect of the Invention

[0020] According to the present invention, when a glass ribbon is formed using the overflow downdraw method, it is possible to reliably reduce the generation of devitrified matter originating from an yttrium-containing oxide contained in a formed body. [Brief description of the drawings]

[0021] [Figure 1] 1 is a side view of a manufacturing apparatus for carrying out a method for manufacturing a glass article according to an embodiment of the present invention. [Diagram 2] 1 is a front view of a manufacturing apparatus for carrying out a method for manufacturing a glass article according to an embodiment of the present invention. [Diagram 3] FIG. 2 is an enlarged side view showing the periphery of the molded body of FIG. [Figure 4] FIG. 2 is a vertical cross-sectional view for explaining a heating test in an example of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] Hereinafter, an embodiment of the present invention will be described with reference to the accompanying drawings. In the Cartesian coordinate system consisting of XYZ shown in the drawings, the X and Y directions are horizontal directions, and the Z direction is vertical. In addition, a direction corresponding to the width direction of the glass ribbon Gr to be molded is called the width direction X, and a direction corresponding to the thickness direction of the glass ribbon Gr to be molded is called the thickness direction Y.

[0023] 1 to 3 are diagrams showing a manufacturing apparatus 1 for realizing a manufacturing method of a glass article according to the present embodiment. As shown in the drawings, the manufacturing apparatus 1 is an apparatus for manufacturing a glass sheet G as a glass article by an overflow downdraw method, and includes, from top to bottom, a forming furnace 2, an annealing furnace 4, a cooling chamber 5, and a cutting chamber 6. The forming furnace 2 and the annealing furnace 4, the annealing furnace 4 and the cooling chamber 5, and the cooling chamber 5 and the cutting chamber 6 are separated by partition members (e.g., floor surfaces of a building) F1, F2, and F3 each having an opening (e.g., a slit) through which the glass ribbon Gr passes.

[0024] The forming furnace 2 is a region for forming the glass ribbon Gr from the molten glass Gm by the overflow downdraw method. In the forming furnace 2, a forming body 3 for forming the glass ribbon Gr from the molten glass Gm and a first conveying roller 7 for cooling both ends in the width direction X of the glass ribbon Gr formed by the forming body 3 are arranged.

[0025] The molded body 3 is formed of a long refractory material along the width direction X. Examples of the refractory material include zircon, zirconia, alumina, magnesia, and xenotime.

[0026] A groove (overflow groove) 8 formed along the width direction X is provided at the top of the formed body 3. A supply pipe 9 is connected to one end side of the groove 8 in the width direction X. Molten glass Gm is supplied into the groove 8 through this supply pipe 9. The method of supplying the molten glass Gm is not limited to this. For example, the molten glass Gm may be supplied from both ends of the groove 8 in the width direction X, or the molten glass Gm may be supplied from above the groove 8.

[0027] The molded body 3 has a symmetrical shape in the thickness direction Y. Both side surfaces 10 of the molded body 3 in the thickness direction Y each have a vertical surface portion 11 that is a plane along the vertical direction, and an inclined surface portion 12 that is connected to the lower side of the vertical surface portion 11 and is a plane inclined with respect to the vertical direction. The vertical surface portions 11 are planes parallel to each other. The inclined surface portions 12 are planes that are inclined so as to approach each other in the thickness direction Y as they go downward. In other words, the molded body 3 has a wedge shape that tapers downward when viewed from the width direction X due to the formation of the inclined surface portions 12, and the corner where the inclined surface portions 12 intersect forms the lower end portion 3a of the molded body 3. The vertical surface portion 11 may be changed in shape to an inclined surface, a curved surface, or the like, or may be omitted.

[0028] In order to ensure mechanical strength, the molded body 3 is preferably made of an oxide containing 1 mass % or more of yttrium (e.g., a composite oxide of yttrium and aluminum, YAlO 12 ). In this embodiment, the formed body 3 is an alumina-based formed body containing an yttrium-containing oxide. The alumina-based formed body preferably has an alumina (Al2O3) content of 90 to 98 mass % and an yttrium-containing oxide content of 2 to 10 mass %. The formed body 3 may be a zircon-based formed body or the like as described above. However, in the case of a zircon-based formed body, when molten glass Gm having a specific tempered glass composition is allowed to flow down, zirconia derived from the formed body 3 may be mixed into the molten glass Gm, causing defects (streak-like defects, etc.) in the glass ribbon Gr and / or the glass sheet G. Therefore, from the viewpoint of preventing the occurrence of such defects due to zirconia, the formed body 3 is preferably an alumina-based formed body.

[0029] The first conveying rollers 7 are configured as a pair of rollers that sandwich each end of the glass ribbon Gr in the width direction X in the thickness direction Y directly below the forming body 3. The first conveying rollers 7 are cantilever type rollers, and are constantly internally cooled during the forming process. The first conveying rollers 7 are also called cooling rollers or edge rollers. The first conveying rollers 7 may be provided in multiple stages (for example, two stages) in the vertical direction Z. For example, in the case of two stages, it is preferable that the first conveying rollers 7 in the upper stage are drive rollers and the first conveying rollers 7 in the lower stage are free rollers.

[0030] The annealing furnace 4 is a region for reducing warpage and internal distortion of the glass ribbon Gr. The internal space of the annealing furnace 4 has a predetermined temperature gradient downward. The temperature gradient of the internal space of the annealing furnace 4 can be adjusted by, for example, a heating device such as a heater disposed on the inner wall of the annealing furnace 4.

[0031] The second conveying rollers 13 are arranged in the annealing furnace 4. The second conveying rollers 13 are also referred to as annealer rollers. The second conveying rollers 13 are configured as a pair of rollers that sandwich each end of the width direction X of the glass ribbon Gr in the thickness direction Y. The second conveying rollers 13 may be double-supported rollers arranged to span the entire width direction X of the glass ribbon Gr, but in this embodiment, they are cantilever rollers. The second conveying rollers 13 are provided in a plurality of stages in the vertical direction Z.

[0032] The cooling chamber 5 is a region for cooling the glass ribbon Gr to approximately room temperature. The cooling chamber 5 is open to the outside atmosphere at room temperature, and does not include a heating device such as a heater.

[0033] The third conveying rollers 14 are disposed in the cooling chamber 5. The third conveying rollers 14 are configured as a pair of rollers that hold each end of the glass ribbon Gr in the width direction X in the thickness direction Y. The third conveying rollers 14 may be double-supported rollers disposed across the entire area of ​​the glass ribbon Gr in the width direction X, but in this embodiment, they are cantilever rollers. The third conveying rollers 14 are provided in a plurality of stages in the vertical direction Z.

[0034] Here, the second conveyor rollers 13 and / or the third conveyor rollers 14 may include rollers that do not pinch both ends of the glass ribbon Gr in the width direction X. In other words, the opposing distance between the roller pairs constituting the second conveyor rollers 13 and / or the third conveyor rollers 14 may be made larger than the thickness of both ends of the glass ribbon Gr in the width direction X, so that the glass ribbon Gr passes between the roller pairs. Note that in this embodiment, both ends in the width direction X of the glass ribbon Gr obtained by the manufacturing apparatus 1 include ear portions that are thicker than the central portion in the width direction X due to the influence of shrinkage during the molding process, etc.

[0035] The cutting chamber 6 is an area for cutting the glass ribbon Gr to a predetermined size to obtain a glass sheet G as a glass article. A cutting device (not shown) for cutting the glass ribbon Gr is disposed in the cutting chamber 6. In the present embodiment, the method for cutting the glass ribbon Gr by the cutting device is scribe cutting, in which a scribe line is formed on the glass ribbon Gr and then the glass ribbon Gr is bent and broken along the scribe line, but is not limited thereto. The cutting method of the cutting device may be, for example, laser cleaving or laser melting.

[0036] The glass plate G is a glass original plate (mother glass plate) from which one or more product glass plates are obtained. The thickness of the product glass plate is, for example, 0.05 mm to 10 mm, and the size of the product glass plate is, for example, 700 mm×700 mm to 3500 mm×3500 mm. The product glass plate is used, for example, as a substrate or cover glass of a display. Note that the substrate or cover glass of a display is not limited to a flat panel, and may be a curved panel or a foldable panel.

[0037] 3, the manufacturing apparatus 1 further includes, outside the forming furnace 2, a first side heater 15 for heating an upper side of the formed body 3, a second side heater 16 for heating a lower side of the formed body 3, and a ceiling heater 17 for heating the top of the formed body 3. The first side heater 15 is disposed on an upper outer wall of the side wall 2a of the forming furnace 2. The second side heater 16 is disposed on a lower outer wall of the side wall 2a of the forming furnace 2. The ceiling heater 17 is disposed on an outer wall of the ceiling 2b of the forming furnace 2.

[0038] The manufacturing apparatus 1 further includes, outside the forming furnace 2, a first side thermometer 18 for measuring the temperature of the side wall 2a at a position corresponding to the first side heater 15, a second side thermometer 19 for measuring the temperature of the side wall 2a at a position corresponding to the second side heater 16, and a ceiling thermometer 20 for measuring the temperature of the ceiling 2b at a position corresponding to the ceiling heater 17. The heaters 15, 16, and 17 may be divided into a plurality of parts in the width direction X and configured as a plurality of partial heaters. In this case, the thermometers 18, 19, and 20 may be provided for each partial heater.

[0039] Next, a method for producing a glass article according to this embodiment will be described.

[0040] 1 to 3, the present manufacturing method includes a molding step, a slow cooling step, and a cutting step, each of which is carried out using the manufacturing apparatus 1 described above.

[0041] In the forming step, in the forming furnace 2, the molten glass Gm is supplied to the grooves 8 of the forming body 3, and the molten glass Gm overflowing on both sides of the grooves 8 flows down along the vertical surfaces 11 and the inclined surfaces 12 and joins again at the lower end 3a. In this way, a belt-shaped glass ribbon Gr is continuously formed from the molten glass Gm.

[0042] The molten glass Gm is an aluminosilicate glass containing P2O5. In detail, the molten glass Gm preferably contains, in mass%, SiO2 40-70%, Al2O3 10-30%, B2O3 0-3%, Na2O 5-25%, K2O 0-5.5%, Li2O 0.1-10%, MgO 0-5.5%, and P2O5 2-10% as a glass composition. By restricting the glass composition range in this way, it becomes easier to achieve both ion exchange performance and devitrification resistance at a high level in the glass ribbon Gr. Therefore, a glass ribbon Gr (glass plate G) suitable for a chemically strengthened glass plate used for cover glass of mobile phones, digital cameras, PDAs (mobile terminals), touch panel displays, etc. can be obtained.

[0043] MgO is a component that reduces high-temperature viscosity, improves meltability and formability, and increases strain point and Young's modulus. Among alkaline earth metal oxides, MgO is a component that has a large effect of improving ion exchange performance. However, if the content of MgO is too high, the density and thermal expansion coefficient tend to increase, and the glass tends to devitrify. Therefore, the preferable upper limit range of MgO is 5.5 mass% or less, 4 mass% or less. Here, if the content of MgO is 0 to 1 mass%, it becomes difficult to form a Mg-rich layer that functions as a diffusion suppression layer for yttrium-containing oxide on the surface of the molded body 3, so that temperature management of the molten glass Gm described later becomes particularly important.

[0044] P2O5 is a component that enhances ion exchange performance when chemically strengthening glass, and in particular increases the stress depth of the compressive stress layer. As the content of P2O5 increases, glass becomes more susceptible to phase separation. The lower limit of P2O5 is preferably 2 mass% or more, and more preferably 4 mass% or more. On the other hand, the upper limit of P2O5 is preferably 10 mass% or less, more preferably 9.5 mass% or less, and even more preferably 9 mass% or less.

[0045] Li2O is an ion exchange component, and also a component that reduces high-temperature viscosity and improves melting and moldability. It also increases Young's modulus. Li2O is also a component that dissolves during ion exchange treatment and deteriorates the ion exchange solution. Therefore, the preferred lower limit range of Li2O is, in mass%, 0.1% or more, 0.5% or more, 1.0% or more, 1.5% or more, 2.0% or more, particularly 2.5% or more, and the preferred upper limit range is 10% or less, 8% or less, 5% or less, 4.5% or less, 4.0% or less, particularly less than 3.5%.

[0046] In the forming process, the temperature difference (T1-T2) between the temperature T1 of the molten glass Gm in the groove 8 of the formed body 3 and the temperature T2 of the molten glass Gm at the lower end 3a of the formed body 3 is controlled to 100°C or less. The temperature difference (T1-T2) is preferably 90°C or less, 80°C or less, particularly 70°C or less. In this way, even if yttrium oxide is dissolved from the yttrium-containing oxide contained in the formed body 3 into the molten glass Gm, the temperature difference (T1-T2) of the molten glass Gm is small, so that it is possible to suppress the generation of devitrified matter (e.g., Y2O3-P2O5 crystals) derived from the yttrium-containing oxide at the lower end 3a of the formed body 3. In other words, it is possible to suppress the generation of defects caused by devitrified matter derived from the yttrium-containing oxide in the glass ribbon Gr or the glass sheet G, thereby improving production efficiency and quality. The lower limit of the temperature difference (T1-T2) of the molten glass Gm can be, for example, 0°C or more.

[0047] The temperature T1 of the molten glass Gm in the grooves 8 of the forming body 3 is preferably 1300° C. or less, 1250° C. or less, particularly 1220° C. or less. This prevents the viscosity of the molten glass Gm from becoming too low, making it easier to form the molten glass Gm into a glass ribbon Gr. In addition, when the temperature T1 is 1220° C. or less, the amount of yttrium oxide eluted from the yttrium-containing oxide of the forming body 3 can be significantly reduced, so that devitrification products derived from the yttrium-containing oxide can be more reliably suppressed.

[0048] The temperature T2 of the molten glass Gm at the lower end 3a of the forming body 3 is preferably 1130°C or higher, 1150°C or higher, particularly 1180°C or higher. This prevents the viscosity of the molten glass Gm from becoming too high, making it easier to form the glass ribbon Gr from the molten glass Gm. In addition, since the temperature T2 is relatively high, it becomes easier to control the temperature difference (T1-T2) to 100°C or lower.

[0049] The temperature T1 of the molten glass Gm in the groove portion 8 of the forming body 3, the temperature T2 of the molten glass Gm at the lower end portion 3a of the forming body 3, and the temperature difference (T1-T2) can be adjusted, for example, by heaters 15 to 17. Furthermore, the temperatures T1 and T2 can be measured, for example, by a radiation thermometer or estimated from the furnace wall temperature of the forming furnace 2 measured by thermometers 18 to 20.

[0050] The time required for the molten glass Gm to pass through the lower end 3a of the formed body 3 after overflowing the grooves 8 of the formed body 3 is, for example, 10 to 600 seconds, and more preferably 60 to 300 seconds.

[0051] In the annealing step, the glass ribbon Gr formed in the forming step is annealed in an annealing furnace 4.

[0052] In the cooling step, the glass ribbon Gr that has been slowly cooled in the slow cooling step is cooled to approximately room temperature in the cooling chamber 5.

[0053] In the cutting step, in the cutting chamber 6, the glass ribbon Gr cooled in the cooling step is cut to obtain a glass sheet G. The cutting step includes a first cutting step of cutting the glass ribbon Gr in the width direction X at predetermined lengths to obtain a glass sheet G, and a second cutting step of cutting and removing the edge portions at both ends of the glass sheet G in the width direction X.

[0054] The process after the cutting process is not particularly limited, and may include, for example, a cutting process for cutting a glass sheet of a desired size from the glass sheet G, an edge processing process, a cleaning process, an inspection process, a packaging process, a chemical strengthening process, etc. In the inspection process, it is preferable to inspect whether the glass sheet G contains devitrified matter derived from yttrium-containing oxide.

[0055] Although a glass article manufacturing apparatus and a method for manufacturing the same according to an embodiment of the present invention have been described, the embodiment of the present invention is not limited thereto, and various modifications can be made without departing from the gist of the present invention.

[0056] In the above embodiment, the glass article is the glass sheet G. However, the glass article may be, for example, a glass roll obtained by winding up a glass ribbon Gr in a roll shape.

[0057] In the above embodiment, the case where the molten glass Gm is an aluminosilicate glass has been exemplified, but the molten glass Gm may be a glass containing P2O5 other than an aluminosilicate glass. EXAMPLES

[0058] Examples of the present invention will be described below, but the present invention is not limited to these examples.

[0059] As shown in FIG. 4, a specimen 101 for the comparison test of Examples 1 and 2 and Comparative Example was prepared by placing molten glass 102 on refractory 103 and bringing both 102 and 103 into contact with each other. The molten glass 101 is an aluminosilicate glass containing the same material as the molten glass Gm, P2O5 (8.7% by mass) and MgO (0.1% by mass), and the refractory 103 is a rod-shaped alumina-based refractory containing the same material as the molded body, yttrium-containing oxide (3% by mass). In other words, the contact portion between the molten glass 102 and refractory 103 reproduces the contact portion between the molten glass Gm flowing down the surface of the molded body 3 and the molded body 3. The configuration of the specimen 101 is common to Examples 1 and 2 and Comparative Example.

[0060] A heating test was conducted in which each test specimen 101 of Examples 1 and 2 and Comparative Example was heated in an electric furnace 104 having a heater 104a. In the heating test, test specimen 101 was heated at a relatively high first temperature that reproduced the temperature of molten glass Gm in groove portion 8 of formed body 3, and then heated at a relatively low second temperature that reproduced the temperature of molten glass Gm at lower end portion 3a of formed body 3. Note that each temperature shown below is the atmospheric temperature of electric furnace 104, but the temperature of molten glass 102 can also be considered to be the same temperature.

[0061] (1) Example 1 In Example 1, the test piece 101 was heated in the electric furnace 104 at 1250°C for 72 hours, and then heated at 1180°C for 48 hours. 1250°C is a first temperature that reproduces the temperature of the molten glass Gm in the groove portion 8 of the molded body 3, and 1180°C is a second temperature that reproduces the temperature of the molten glass Gm in the lower end portion 3a of the molded body 3. That is, in Example 1, the temperature difference (T1-T2) is 70°C obtained by subtracting the second temperature from the first temperature. The reason for making the heating time at the first temperature (1250°C) longer than the heating time at the second temperature (1180°C) is to ensure sufficient time for yttrium oxide to dissolve from the yttrium-containing oxide of the refractory (molded body) 103. In Example 2 and Comparative Example, the heating time at the first temperature is also made longer than the heating time at the second temperature for the same reason.

[0062] (2) Example 2 In Example 2, test specimen 101 was heated in electric furnace 104 at 1220°C for 72 hours, and then heated at 1150°C for 48 hours. 1220°C is a first temperature that reproduces the temperature of molten glass Gm in groove portion 8 of formed body 3, and 1150°C is a second temperature that reproduces the temperature of molten glass Gm in lower end portion 3a of formed body 3. That is, in Example 2, the temperature difference (T1-T2) is 70°C.

[0063] (3) Comparative Example In the comparative example, the test piece 101 was heated in the electric furnace 104 at 1250°C for 72 hours, and then heated at 1120°C for 48 hours. 1250°C is a first temperature that reproduces the temperature of the molten glass Gm in the groove portion 8 of the formed body 3, and 1120°C is a second temperature that reproduces the temperature of the molten glass Gm in the lower end portion 3a of the formed body 3. That is, in the comparative example, the temperature difference (T1-T2) is 130°C.

[0064] Then, after each of the molten glasses 102 that had undergone the above heating tests was cooled to room temperature, the particles in each of the glasses obtained by cooling were confirmed with SEM images, and the particles found were then confirmed by EPMA to be devitrified matter (Y2O3-P2O5 crystals) derived from yttrium-containing oxides. As a result, in Example 1 and Example 2 in which the temperature difference (T1-T2) was 100°C or less, no devitrified matter derived from yttrium-containing oxides was found in the glass obtained by cooling the molten glass 102. On the other hand, in the comparative example in which the temperature difference (T1-T2) was more than 100°C, devitrified matter derived from yttrium-containing oxides was found in the glass obtained by cooling the molten glass 102.

[0065] Based on the test results of Example 1, in the forming step, the temperature of the molten glass Gm in the grooves 8 of the formed body 3 was set to 1220°C, and the temperature of the molten glass Gm at the lower end 3a of the formed body 3 was set to 1150°C to form a glass ribbon Gr. At that time, the time required for the molten glass Gm to overflow the grooves 8 of the formed body 3 and pass the lower end 3a of the formed body 3 was set to about 300 seconds. As a result, no devitrified matter derived from yttrium-containing oxide was confirmed in the obtained glass sheet G.

[0066] Based on the test results of Example 2, in the forming step, the temperature of the molten glass Gm in the grooves 8 of the formed body 3 was set to 1250° C., and the temperature of the molten glass Gm at the lower end 3a of the formed body 3 was set to 1180° C. to form a glass ribbon Gr. At that time, the time required for the molten glass Gm to overflow the grooves 8 of the formed body 3 and pass the lower end 3a of the formed body 3 was set to about 300 seconds. As a result, no devitrified matter derived from yttrium-containing oxide was confirmed in the obtained glass sheet G.

[0067] Based on the test results of the comparative example, in the forming step, the temperature of the molten glass Gm in the grooves 8 of the forming body 3 was set to 1250° C., and the temperature of the molten glass Gm at the lower end 3a of the forming body 3 was set to 1120° C. to form a glass ribbon Gr. At that time, the time required for the molten glass Gm to overflow the grooves 8 of the forming body 3 and pass through the lower end 3a of the forming body 3 was set to about 300 seconds. As a result, devitrified matter derived from yttrium-containing oxide was confirmed in a part of the obtained glass sheet G.

[0068] From the above, it can be seen that by controlling the temperature difference (T1-T2) between the temperature T1 of the molten glass Gm in the groove portion 8 of the molding body 3 and the temperature T2 of the molten glass Gm at the lower end portion 3a of the molding body 3 to be 100°C or less, it is possible to suppress devitrification products derived from yttrium-containing oxides.

[0069] In the comparative example, the temperature T1 of the molten glass Gm in the grooves 8 of the molded body 3 was set to 1250°C, and devitrification due to yttrium-containing oxide occurred in a part of the obtained glass sheet G. As in the comparative example, the temperature T1 of the molten glass Gm in the grooves 8 of the molded body 3 in Example 2 was set to 1250°C, so it is presumed that the molten glass Gm in Example 2 contains the same amount of yttrium oxide as in the comparative example. It is presumed that the devitrification of yttrium oxide was prevented in Example 2 by increasing the temperature T2 of the molten glass Gm in the lower end 3a of the molded body 3 to 1180°C and reducing the temperature difference (T1-T2) compared to the comparative example.

[0070] In addition, it is presumed that in Example 1, the temperature T1 of the molten glass Gm in the groove portion 8 of the formed body 3 was lowered to 1220°C than in the comparative example and Example 2, and therefore the dissolution of yttrium oxide into the molten glass Gm was reduced. For this reason, it is presumed that even if the temperature T2 of the molten glass Gm in the lower end portion 3a of the formed body 3 was lowered to 1150°C than in Example 2 in Example 1, devitrification of yttrium oxide could be prevented as long as the temperature difference (T1-T2) was maintained. [Explanation of symbols]

[0071] 1. Glass product manufacturing equipment 2 Molding furnace 3. Molded body 3a Bottom end 4 Annealing furnace 5 Cooling room 6 Cutting chamber 7 First conveyor roller 8 Groove 9 Supply Pipe 13 Second conveyor roller 14 Third conveyor roller 15 First side heater 16 Second side heater 17 Ceiling heater 18 First side thermometer 19 Second side thermometer 20 Ceiling thermometer G Glass plate Gm Molten Glass Gr Glass ribbon

Claims

1. A method for producing a glass article, comprising a forming step of causing molten glass overflowing from a groove of a forming body to flow down along both side surfaces of the forming body by an overflow downdraw method, and then fusing the molten glass at a lower end of the forming body to form a glass ribbon, The formed body contains an yttrium-containing oxide, and the molten glass contains P 2 O 5 Including, A method for manufacturing a glass article, wherein in the forming step, a temperature difference between the molten glass in the groove portion and the molten glass at the lower end portion is set to 100° C. or less.

2. The method for manufacturing a glass article according to claim 1 , wherein the temperature of the molten glass in the groove is 1300° C. or less.

3. The method for producing a glass article according to claim 1 or 2, wherein the temperature of the molten glass at the lower end is 1100°C or higher.

4. The molten glass has a glass composition, in mass%, of SiO 2 40-70%, Al 2 O 3 10-30%, B 2 O 3 0-3%, Na 2 O 5-25%, K 2 O 0-5.5%, Li 2 O 0.1-10%, MgO 0-5.5%, P 2 O 5 The method for producing a glass article according to any one of claims 1 to 3, wherein the content is 2 to 10%.

5. The method for producing a glass article according to any one of claims 1 to 4, wherein the molten glass contains 0 to 1 mass % of MgO.

6. The method for producing a glass article according to any one of claims 1 to 5, wherein the formed body contains 1 mass % or more of an yttrium-containing oxide.

Citation Information

Patent Citations

  • Process for making sheet glass by overflow downdraw fusion process

    JP2005514302A

  • Method for manufacturing glass substrate for flat panel display

    JP2013212943A

  • Large-scale xenotime ceramic block and dry process for its fabrication

    JP2013542166A

  • Method and equipment for manufacturing glass article

    JP2018062433A