Positive electrode material for secondary battery and secondary battery using the same
By using a sulfur-containing positive electrode material with controlled electric double layer capacitance change, the cycle durability of secondary batteries is improved, addressing the discharge capacity degradation issue.
Patent Information
- Application Number
- JP2020202612
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-07
- Publication Date
- 2024-11-28
- Estimated Expiration
- 2040-12-07
AI Technical Summary
Secondary batteries using sulfur-containing positive electrode materials face issues with cycle durability, leading to a decrease in discharge capacity over time.
A positive electrode material is developed comprising a conductive material coated with a sulfur-containing active material and a solid electrolyte, with a controlled electric double layer capacitance change (ΔCdl) of 0.5 [F cm^2/g] or less, reducing the contact area between the solid electrolyte and conductive material to improve cycle durability.
The solution enhances the cycle durability of secondary batteries by minimizing the decomposition reaction of the solid electrolyte, resulting in improved discharge capacity retention.
Smart Images

Figure 0007591392000003 
Figure 0007591392000004 
Figure 0007591392000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a positive electrode material for a secondary battery and a secondary battery using the same. [Background technology]
[0002] In recent years, there has been a strong desire to reduce carbon dioxide emissions in order to combat global warming. In the automobile industry, there are high hopes for a reduction in carbon dioxide emissions through the introduction of electric vehicles (EVs) and hybrid electric vehicles (HEVs), and there has been active development of non-aqueous electrolyte secondary batteries, such as motor drive secondary batteries, which hold the key to putting these into practical use.
[0003] Secondary batteries for driving motors are required to have extremely high output characteristics and high energy compared to consumer lithium secondary batteries used in mobile phones, notebook computers, etc. Therefore, lithium secondary batteries, which have the highest theoretical energy of all practical batteries, have attracted attention and are currently being rapidly developed.
[0004] Currently, lithium secondary batteries in widespread use use flammable organic electrolytes as electrolytes, and these liquid-based lithium secondary batteries require stricter safety measures against leakage, short circuits, overcharging, etc. than other batteries.
[0005] In recent years, research and development of all-solid-state lithium secondary batteries using oxide-based or sulfide-based solid electrolytes has been actively conducted. A solid electrolyte is a material that is mainly composed of an ion conductor capable of ion conduction in a solid state. Therefore, in principle, all-solid-state lithium secondary batteries do not have various problems caused by flammable organic electrolytes, as in conventional liquid-based lithium secondary batteries. In addition, in general, the use of high-potential, large-capacity positive electrode materials and large-capacity negative electrode materials can significantly improve the output density and energy density of the battery. For example, elemental sulfur (S8) has an extremely large theoretical capacity of about 1670 mAh / g, and has the advantages of being low cost and abundant in resources.
[0006] In a secondary battery using a sulfur-containing positive electrode active material, in order to fully realize the high theoretical capacity that the active material potentially has, for example, Patent Document 1 discloses a cathode active material having a BET specific surface area of 1800 m 2 A technique is disclosed in which activated carbon having a carbon content of 0.1g or more and coated with sulfur having a thickness of 0.2 to 1.4 nm is used as a positive electrode material for an all-solid-state lithium-sulfur battery. According to Patent Document 1, it is possible to realize a very high discharge capacity by constructing an all-solid-state lithium-sulfur battery using a positive electrode material having such a configuration. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2015-88231 A Summary of the Invention [Problem to be solved by the invention]
[0008] However, according to the study by the present inventors, it was found that sufficient cycle durability may not be achieved when a secondary battery is constructed by adopting the technology described in Patent Document 1. In other words, it was found that the discharge capacity of the secondary battery may decrease over time when the technology described in Patent Document 1 is adopted.
[0009] Therefore, an object of the present invention is to provide a means for improving the cycle durability of a secondary battery using a positive electrode active material containing sulfur. [Means for solving the problem]
[0010] The present inventors have conducted extensive research to solve the above problems, and have found that the above problems can be solved by forming a secondary battery using a positive electrode material that includes a conductive material, a sulfur-containing positive electrode active material that coats the surface of the conductive material, and a solid electrolyte, and that has a small change in electric double layer capacity between full charge and full discharge, thereby completing the present invention.
[0011] One embodiment of the present invention is a secondary battery comprising a conductive material, a sulfur-containing positive electrode active material that coats a surface of the conductive material, and a solid electrolyte, the secondary battery being characterized in that the rate of change in electric double layer capacity per unit area of the positive electrode material between SOC 0% and SOC 100% (ΔC dl ) is 0.5 [F cm 2 / g] or less. Effect of the Invention
[0012] According to the present invention, it is possible to improve the cycle durability of a secondary battery using a positive electrode active material containing sulfur. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a perspective view showing the appearance of a flat laminated type all-solid-state lithium secondary battery, which is one embodiment of the lithium secondary battery according to the present invention. [Diagram 2] FIG. 2 is a cross-sectional view taken along line 2-2 shown in FIG. [Diagram 3] FIG. 3 is a Cole-Cole plot for explaining a method for calculating the electric double layer capacity (Cdl) value of a secondary battery, which is used to calculate the rate of change (ΔCdl) of the electric double layer capacity per unit area of the positive electrode material, based on the measurement results of AC impedance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, the above-mentioned embodiment of the present invention will be described with reference to the drawings, but the technical scope of the present invention should be determined based on the description of the claims, and is not limited to only the following embodiments. The dimensional ratios in the drawings are exaggerated for convenience of explanation and may differ from the actual ratios. Hereinafter, the present invention will be described by taking as an example a stacked type (internal parallel connection type) all-solid-state lithium secondary battery, which is one form of secondary battery. As described above, the solid electrolyte constituting the all-solid-state lithium secondary battery is a material mainly composed of an ion conductor capable of ion conduction in a solid. For this reason, the all-solid-state lithium secondary battery has the advantage that, in principle, various problems caused by a flammable organic electrolyte do not occur as in the conventional liquid-based lithium secondary battery. In addition, in general, there is also the advantage that the output density and energy density of the battery can be significantly improved by using a high-potential, large-capacity positive electrode material and a large-capacity negative electrode material.
[0015] One embodiment of the present invention is a secondary battery comprising a conductive material, a sulfur-containing positive electrode active material that coats a surface of the conductive material, and a solid electrolyte, the secondary battery being characterized in that the rate of change in electric double layer capacity per unit area of the positive electrode material between SOC 0% and SOC 100% (ΔC dl ) is 0.5 [F cm 2 / g] or less. According to the positive electrode material for secondary batteries according to the present embodiment, it is possible to improve cycle durability in secondary batteries using a positive electrode active material containing sulfur.
[0016] FIG. 1 is a perspective view showing the appearance of a flat laminated type all-solid-state lithium secondary battery which is one embodiment of the lithium secondary battery according to the present invention. FIG. 2 is a cross-sectional view taken along line 2-2 shown in FIG. 1. The laminated type allows the battery to be compact and have a high capacity. In this specification, the flat laminated type non-bipolar lithium secondary battery shown in FIG. 1 and FIG. 2 (hereinafter, also simply referred to as a "laminated type battery") will be described in detail as an example. However, in terms of the internal electrical connection form (electrode structure) of the lithium secondary battery according to this embodiment, it can be applied to both non-bipolar type (internal parallel connection type) batteries and bipolar type (internal series connection type) batteries.
[0017] 1, the stacked battery 10a has a flat rectangular shape, with a negative electrode current collector 25 and a positive electrode current collector 27 for extracting electric power extending from both sides. The power generating element 21 is wrapped in a battery exterior material (laminate film 29) of the stacked battery 10a, and the periphery is heat-sealed, with the power generating element 21 being sealed with the negative electrode current collector 25 and the positive electrode current collector 27 extending to the outside.
[0018] The lithium secondary battery according to the present embodiment is not limited to a laminated flat shape. A wound lithium secondary battery may be cylindrical, or may be a rectangular flat shape obtained by deforming such a cylindrical shape, and is not particularly limited. The cylindrical shape may be a laminate film or a conventional cylindrical can (metal can) as an exterior material, and is not particularly limited. Preferably, the power generating element is housed inside a laminate film containing aluminum. This form can achieve weight reduction.
[0019] There is also no particular limitation on the removal of the current collectors (25, 27) shown in Fig. 1. The negative current collector 25 and the positive current collector 27 may be pulled out from the same side, or the negative current collector 25 and the positive current collector 27 may each be divided into a plurality of pieces and removed from each side, and are not limited to what is shown in Fig. 1. In addition, in a wound lithium battery, the terminals may be formed using, for example, a cylindrical can (metal can) instead of a tab.
[0020] 2, the stacked battery 10a of this embodiment has a structure in which a flat, generally rectangular power generating element 21, where charge and discharge reactions actually proceed, is sealed inside a laminate film 29, which is a battery exterior material. Here, the power generating element 21 has a structure in which a positive electrode, a solid electrolyte layer 17, and a negative electrode are laminated. The positive electrode has a structure in which positive electrode active material layers 15 containing a positive electrode active material are disposed on both sides of a positive electrode collector 11". The negative electrode has a structure in which negative electrode active material layers 13 containing a negative electrode active material are disposed on both sides of a negative electrode collector 11'. Specifically, the positive electrode, solid electrolyte layer, and negative electrode are stacked in this order such that one positive electrode active material layer 15 and an adjacent negative electrode active material layer 13 face each other with a solid electrolyte layer 17 interposed therebetween. As a result, the adjacent positive electrode, solid electrolyte layer, and negative electrode constitute one unit cell layer 19. Therefore, it can be said that the stacked battery 10a shown in FIG. 2 has a structure in which a plurality of unit cell layers 19 are stacked and electrically connected in parallel.
[0021] As shown in FIG. 2, the outermost negative electrode current collectors located on both outermost layers of the power generating element 21 each have a negative electrode active material layer 13 disposed on only one side, but active material layers may be provided on both sides. In other words, instead of using a current collector exclusively for the outermost layer with an active material layer provided on only one side, a current collector having active material layers on both sides may be used as it is as the outermost layer current collector. In some cases, the negative electrode active material layer 13 and the positive electrode active material layer 15 may be used as the negative electrode and positive electrode, respectively, without using the current collectors (11', 11").
[0022] Negative current collector 11′ and positive current collector 11″ are respectively attached with negative current collector plate (tab) 25 and positive current collector plate (tab) 27 that are electrically connected to the respective electrodes (positive and negative electrodes), and have a structure in which they are sandwiched between ends of laminate film 29, which is a battery exterior material, and are led out of laminate film 29. Positive current collector 27 and negative current collector 25 may be attached to positive current collector 11″ and negative current collector 11′ of each electrode by ultrasonic welding, resistance welding, or the like, respectively, via positive electrode leads and negative electrode leads (not shown) as necessary.
[0023] The main components of the lithium secondary battery according to this embodiment will be described below.
[0024] [Current collector] The current collector has a function of mediating the movement of electrons from the electrode active material layer. There are no particular limitations on the material constituting the current collector. For example, metals and conductive resins can be used as the material constituting the current collector.
[0025] The current collector may have a single layer structure made of a single material, or may have a laminate structure in which layers made of these materials are appropriately combined. From the viewpoint of reducing the weight of the current collector, it is preferable to include at least a conductive resin layer made of a resin having conductivity. In addition, from the viewpoint of blocking the movement of lithium ions between the single cell layers, a metal layer may be provided on a part of the current collector. Furthermore, if the negative electrode active material layer and the positive electrode active material layer described later are conductive by themselves and can perform a current collecting function, it is not necessary to use a current collector as a member separate from these electrode active material layers. In such a form, the negative electrode active material layer described later constitutes the negative electrode as it is, and the positive electrode active material layer described later constitutes the positive electrode as it is.
[0026] [Negative electrode (negative electrode active material layer)] In the stacked battery according to the embodiment shown in Fig. 1 and Fig. 2, the negative electrode active material layer 13 contains a negative electrode active material. The type of the negative electrode active material is not particularly limited, but may include a carbon material, a metal oxide, and a metal active material. Examples of the carbon material include natural graphite, artificial graphite, mesocarbon microbeads (MCMB), highly oriented graphite (HOPG), hard carbon, and soft carbon. Examples of the metal oxide include Nb2O5, Li4Ti5O 12and the like. Furthermore, silicon-based negative electrode active materials and tin-based negative electrode active materials may be used. Here, silicon and tin belong to the 14th group of elements, and are known to be negative electrode active materials that can greatly improve the capacity of non-aqueous electrolyte secondary batteries. These simple substances can absorb and release a large number of charge carriers (lithium ions, etc.) per unit volume (mass), and therefore become high-capacity negative electrode active materials. Here, it is preferable to use Si simple substance as the silicon-based negative electrode active material. Similarly, SiO 2 disproportionated into two phases, a Si phase and a silicon oxide phase, is also used. x It is also preferable to use silicon oxides such as (0.3≦x≦1.6). In this case, the range of x is more preferably 0.5≦x≦1.5, and even more preferably 0.7≦x≦1.2. Furthermore, an alloy containing silicon (silicon-containing alloy-based negative electrode active material) may be used. On the other hand, examples of negative electrode active materials containing tin element (tin-based negative electrode active materials) include simple Sn, tin alloys (Cu-Sn alloys, Co-Sn alloys), amorphous tin oxides, tin silicon oxides, and the like. Among these, examples of amorphous tin oxides include SnB 0.4 P 0.6 O 3.1 Examples of the tin silicon oxide include SnSiO3. Metals containing lithium may be used as the negative electrode active material. Such negative electrode active materials are not particularly limited as long as they are active materials containing lithium, and examples thereof include metallic lithium and lithium-containing alloys. Examples of the lithium-containing alloys include alloys of Li and at least one of In, Al, Si, and Sn. In some cases, two or more negative electrode active materials may be used in combination. Of course, negative electrode active materials other than the above may be used. The negative electrode active material preferably contains metallic lithium, a silicon-based negative electrode active material, or a tin-based negative electrode active material, and particularly preferably contains metallic lithium.
[0027] The shape of the negative electrode active material may be, for example, particulate (spherical, fibrous), thin film, etc. When the negative electrode active material is particulate, its average particle diameter (D 50) is, for example, preferably in the range of 1 nm to 100 μm, more preferably in the range of 10 nm to 50 μm, further preferably in the range of 100 nm to 20 μm, and particularly preferably in the range of 1 to 20 μm. In this specification, the average particle diameter (D 50 The value of can be measured by a laser diffraction scattering method.
[0028] The content of the negative electrode active material in the negative electrode active material layer is not particularly limited, but is, for example, preferably in the range of 40 to 99 mass %, and more preferably in the range of 50 to 90 mass %.
[0029] The negative electrode active material layer preferably further includes a solid electrolyte. By including the solid electrolyte in the negative electrode active material layer, the ionic conductivity of the negative electrode active material layer can be improved. Examples of the solid electrolyte include sulfide solid electrolytes and oxide solid electrolytes, and the sulfide solid electrolyte is preferable.
[0030] Examples of sulfide solid electrolytes include LiI-Li2S-SiS2, LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, Li2S-P2S5, LiI-Li3PS4, LiI-LiBr-Li3PS4, and Li3PS 4、 Li2S-P2S5, Li2S-P2S5-LiI, Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-SiS2, Li2S-SiS2-LiI, Li2 S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, Li2S-P2S5-Z m S n (where m and n are positive numbers, and Z is Ge, Zn, or Ga), Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li x MO y(However, x and y are positive numbers, and M is any one of P, Si, Ge, B, Al, Ga, In, etc.). Note that the description of "Li2S-P2S5" means a sulfide solid electrolyte formed using a raw material composition containing Li2S and P2S5, and the same applies to other descriptions.
[0031] The sulfide solid electrolyte may, for example, have a Li3PS4 skeleton, a Li4P2S7 skeleton, or a Li4P2S6 skeleton. Examples of the sulfide solid electrolyte having a Li3PS4 skeleton include LiI-Li3PS4, LiI-LiBr-Li3PS 4、 Li3PS4. Also, examples of the sulfide solid electrolyte having a Li4P2S7 skeleton include a Li-P-S-based solid electrolyte called LPS (for example, Li7P3S 11 ). Also, as the sulfide solid electrolyte, for example, Li (4-x) Ge (1-x) P x S4 (where x satisfies 0 < x < 1), such as LGPS, may be used. Among them, the sulfide solid electrolyte contained in the active material layer is preferably a sulfide solid electrolyte containing the P element, and the sulfide solid electrolyte is more preferably a material mainly composed of Li2S-P2S5. Furthermore, the sulfide solid electrolyte may contain a halogen (F, Cl, Br, I). In a preferred embodiment, the sulfide solid electrolyte contains Li6PS5X (where X is Cl, Br, or I, preferably Cl).
[0032] Also, when the sulfide solid electrolyte is of the Li2S-P2S5 type, the ratio of Li2S and P2S5 is preferably in the range of Li2S:P2S5 = 50:50 to 100:0 in terms of molar ratio, and among them, Li2S:P2S5 = 70:30 to 80:20 is preferably.
[0033] The sulfide solid electrolyte may be sulfide glass, crystallized sulfide glass, or a crystalline material obtained by a solid phase method. The sulfide glass may be obtained, for example, by mechanical milling (ball mill, etc.) of the raw material composition. The crystallized sulfide glass may be obtained, for example, by heat treating the sulfide glass at a temperature equal to or higher than the crystallization temperature. The ionic conductivity (e.g., Li ion conductivity) of the sulfide solid electrolyte at room temperature (25° C.) is, for example, 1×10 -5 [S / cm] or more is preferable, and 1×10 -4 It is more preferable that the ionic conductivity of the solid electrolyte is equal to or higher than [S / cm]. The ionic conductivity of the solid electrolyte can be measured by an AC impedance method.
[0034] Examples of oxide solid electrolytes include compounds having a NASICON structure. An example of a compound having a NASICON structure is represented by the general formula Li 1+x Al x Ge 2-x Compounds represented by the formula (PO4)3 (0≦x≦2) (LAGP), general formula Li 1+x Al x Ti 2-x (PO4)3 (0≦x≦2) (LATP) and the like. Another example of an oxide solid electrolyte is LiLaTiO (for example, Li 0.34 La 0.51 TiO3), LiPON (e.g., Li 2.9 PO 3.3 N 0.46 ), LiLaZrO (e.g., Li7La3Zr2O 12 ) etc.
[0035] The shape of the solid electrolyte may be, for example, a particulate shape such as a spherical shape or an oval spherical shape, or a thin film shape. When the solid electrolyte is particulate, its average particle diameter (D 50 ) is not particularly limited, but is preferably 40 μm or less, more preferably 20 μm or less, and even more preferably 10 μm or less. 50) is preferably 0.01 μm or more, and more preferably 0.1 μm or more.
[0036] The content of the solid electrolyte in the negative electrode active material layer is, for example, preferably in the range of 1 to 60 mass %, and more preferably in the range of 10 to 50 mass %.
[0037] The negative electrode active material layer may further contain at least one of a conductive assistant and a binder, in addition to the above-mentioned negative electrode active material and solid electrolyte.
[0038] When the negative electrode active material layer contains a conductive assistant, the content of the conductive assistant in the negative electrode active material layer is not particularly limited, but is preferably 0 to 10 mass%, more preferably 2 to 8 mass%, and further preferably 4 to 7 mass% relative to the total mass of the negative electrode active material layer. If the content is within such a range, a stronger electron conduction path can be formed in the negative electrode active material layer, which can effectively contribute to improving the battery characteristics.
[0039] The thickness of the negative electrode active material layer differs depending on the intended configuration of the secondary battery, but is preferably within the range of, for example, 0.1 to 1000 μm.
[0040] [Solid electrolyte layer] In the stacked battery according to the embodiment shown in FIGS. 1 and 2, the solid electrolyte layer is interposed between the above-mentioned positive electrode active material layer and negative electrode active material layer, and is a layer that essentially contains a solid electrolyte.
[0041] The specific form of the solid electrolyte contained in the solid electrolyte layer is not particularly limited, and the solid electrolytes exemplified in the section on the negative electrode active material layer and their preferred forms can be similarly adopted. In some cases, a solid electrolyte other than the above-mentioned solid electrolytes may be used in combination.
[0042] The solid electrolyte layer may further contain a binder in addition to the above-mentioned predetermined solid electrolyte.
[0043] The thickness of the solid electrolyte layer varies depending on the configuration of the intended lithium secondary battery, but from the viewpoint of improving the volumetric energy density of the battery, it is preferably 600 μm or less, more preferably 500 μm or less, and even more preferably 400 μm or less. On the other hand, there is no particular restriction on the lower limit of the thickness of the solid electrolyte layer, but it is preferably 1 μm or more, more preferably 5 μm or more, and even more preferably 10 μm or more.
[0044] [Cathode active material layer] 1 and 2, the positive electrode active material layer contains the positive electrode material for a secondary battery according to one embodiment of the present invention. The positive electrode material for a secondary battery contains a conductive material, a sulfur-containing positive electrode active material that coats the surface of the conductive material, and a solid electrolyte.
[0045] (Conductive materials) There is no particular restriction on the specific form of the conductive material contained in the positive electrode material according to this embodiment, and a conventionally known conductive material can be appropriately adopted. In particular, from the viewpoint of increasing the surface area that can participate in the reaction in the positive electrode material, it is preferable that the conductive material has pores. In addition, from the viewpoint of excellent conductivity, ease of processing, and ease of designing the desired pore distribution, it is preferable that the conductive material having pores is a carbon material.
[0046] Examples of carbon materials having fine pores include activated carbon, Ketjen Black (registered trademark) (highly conductive carbon black), (oil) furnace black, channel black, acetylene black, thermal black, lamp black, and other carbon blacks, as well as carbon particles (carbon carriers) made of coke, natural graphite, artificial graphite, and the like. The carbon material is preferably made mainly of carbon. Here, "made mainly of carbon" means that the material contains carbon atoms as the main component, and is a concept that includes both the concept of being made only of carbon atoms and the concept of being made substantially of carbon atoms. "made substantially of carbon atoms" means that the inclusion of impurities of about 2 to 3 mass % or less is acceptable.
[0047] The BET specific surface area of the conductive material (preferably a carbon material) having pores is preferably 200 m 2 / g or more, more preferably 500 m 2 / g or more, still more preferably 800 m 2 / g or more, particularly preferably 1200 m 2 / g or more, and most preferably 1500 m 2 / g or more. Also, the pore volume of the conductive material (preferably a carbon material) having pores is preferably 1.0 mL / g or more, more preferably 1.3 mL / g or more, and still more preferably 1.5 mL / g or more. If the BET specific surface area and pore volume of the conductive material are within such ranges, a sufficient amount of pores can be retained, and thus a sufficient amount of the positive electrode active material can be retained. Note that the values of the BET specific surface area and pore volume of the conductive material can be measured by nitrogen adsorption / desorption measurement. This nitrogen adsorption / desorption measurement is performed using BELSORP mini manufactured by MicrotracBEL Corp. at a temperature of -196 °C by the multi-point method. The BET specific surface area is determined from the adsorption isotherm in the relative pressure range of 0.01 < P / P0 < 0.05. Also, the pore volume is determined from the volume of adsorbed N2 at a relative pressure of 0.96.
[0048] The average pore diameter of the conductive material is not particularly limited, but is preferably 50 nm or less, and particularly preferably 30 nm or less. If the average pore diameter of the conductive material is within these ranges, when the sulfur-containing positive electrode active material is disposed inside the pores, electrons can be sufficiently supplied to the active material existing at a position away from the pore wall. Note that the value of the average pore diameter of the conductive material can be calculated by nitrogen adsorption / desorption measurement in the same manner as when obtaining the values of the BET specific surface area and pore volume.
[0049] When the conductive material is particulate, the average particle diameter (primary particle diameter) is not particularly limited, but is preferably 0.05 to 50 μm, more preferably 0.1 to 20 μm, and even more preferably 0.5 to 10 μm. In this specification, the "particle diameter of the conductive material" refers to the maximum distance L between any two points on the contour line of the conductive material. The value of the "average particle diameter of the conductive material" is calculated as the average value of particle diameters of particles observed in several to several tens of fields of view using an observation means such as a scanning electron microscope (SEM) or a transmission electron microscope (TEM).
[0050] (Sulfur-containing positive electrode active material) The sulfur-containing positive electrode active material is a material that contains sulfur and can function as a positive electrode active material. The type of sulfur-containing positive electrode active material is not particularly limited, but may be, in addition to elemental sulfur (S), particles or thin films of organic or inorganic sulfur compounds, and may be any material that can release lithium ions during charging and absorb lithium ions during discharging by utilizing the oxidation-reduction reaction of sulfur. Examples of the organic sulfur compound include disulfide compounds, sulfur-modified polyacrylonitrile, sulfur-modified polyisoprene, rubeanic acid (dithiooxamide), polycarbonate sulfide, etc., as typified by the compounds described in the pamphlet of International Publication No. 2010 / 044437. Among them, disulfide compounds, sulfur-modified polyacrylonitrile, and rubeanic acid are preferred, and sulfur-modified polyacrylonitrile is particularly preferred. As the disulfide compound, a dithiobiurea derivative, a compound having a thiourea group, a thioisocyanate, or a thioamide group is more preferred. Here, the sulfur-modified polyacrylonitrile is a modified polyacrylonitrile containing sulfur atoms, which is obtained by mixing sulfur powder with polyacrylonitrile and heating the mixture under an inert gas or under reduced pressure. Its estimated structure is, for example, as shown in Chem. Mater. 2011, 23, 5024-5028, in which polyacrylonitrile is ring-closed to form a polycyclic ring, and at least a part of S is bonded to C. The compound described in this document has a peak at 1330 cm in the Raman spectrum. -1and 1560cm -1 There is a strong peak signal near 307 cm -1 , 379cm -1 , 472cm -1 , 929cm -1 There is a peak around 1000 nm. On the other hand, inorganic sulfur compounds are preferred because of their excellent stability, and specific examples thereof include sulfur element (S), TiS2, TiS3, TiS4, NiS, NiS2, CuS, FeS2, Li2S, MoS2, MoS3, MnS, MnS2, CoS, CoS2, and the like. Among them, S, S-carbon composite, TiS2, TiS3, TiS4, FeS2, and MoS2 are preferred, sulfur element (S), TiS2, and FeS2 are more preferred, and sulfur element (S) is particularly preferred from the viewpoint of high capacity. As the sulfur element (S), α-sulfur, β-sulfur, or γ-sulfur having an S8 structure can be used.
[0051] The positive electrode material according to the present embodiment may further include a positive electrode active material that does not contain sulfur in addition to the sulfur-containing positive electrode active material. Examples of the positive electrode active material that does not contain sulfur include layered rock salt active materials such as LiCoO2, LiMnO2, LiNiO2, LiVO2, and Li(Ni-Mn-Co)O2, LiMn2O4, LiNi 0.5 Mn 1.5 Examples of oxide active materials other than those mentioned above include spinel-type active materials such as LiFePO4 and LiMnPO4, olivine-type active materials such as Li2FeSiO4 and Li2MnSiO4, and Si-containing active materials such as Li4Ti5O 12 Examples include:
[0052] In some cases, two or more kinds of positive electrode active materials may be used in combination. Here, the content ratio of the sulfur-containing positive electrode active material in the total amount of the positive electrode active material (100 mass%) is preferably 50 mass% or more, more preferably 70 mass% or more, even more preferably 80 mass% or more, still more preferably 90 mass% or more, particularly preferably 95 mass% or more, and most preferably 100 mass%.
[0053] (solid electrolyte) The positive electrode material according to the present embodiment essentially contains a solid electrolyte. There is no particular limitation on the specific form of the solid electrolyte contained in the positive electrode material according to the present embodiment, and the solid electrolytes exemplified in the section on the negative electrode active material layer and their preferred forms can be similarly adopted. In some cases, a solid electrolyte other than the above-mentioned solid electrolytes may be used in combination.
[0054] In particular, from the viewpoint of excellent ion conductivity and durability, the solid electrolyte contained in the positive electrode material according to this embodiment is preferably a sulfide solid electrolyte. In another preferred embodiment, the solid electrolyte contained in the positive electrode material contains an alkali metal atom. Here, examples of the alkali metal that can be contained in the solid electrolyte include Li, Na, and K, and Li is preferred in terms of excellent ion conductivity. In yet another preferred embodiment, the solid electrolyte contained in the positive electrode material contains an alkali metal atom (e.g., Li, Na, or K; preferably Li) and a phosphorus atom and / or a boron atom. Examples of sulfide solid electrolytes containing such alkali metal atoms and phosphorus atoms and / or boron atoms include LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, Li2S-P2S5, LiI-Li3PS4, LiI-LiBr ... 4、 Li3PS 4、 Li2S-P2S5, Li2S-P2S5-LiI, Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, Li2S-P2S5-Z m S n (where m and n are positive numbers, and Z is Ge, Zn, or Ga), Li2S-SiS2-Li3PO4, etc. Examples of sulfide solid electrolytes having a Li4P2S7 skeleton include Li-PS-based solid electrolytes called LPS (for example, Li7P3S 11 ) can be mentioned. For example, Li (4-x) Ge (1-x) P xAn LGPS or the like represented by S4 (where 0 < x < 1) may be used. Among them, the sulfide solid electrolyte contained in the positive electrode material is preferably a sulfide solid electrolyte containing a phosphorus atom, and more preferably, the sulfide solid electrolyte is a material mainly composed of Li2S-P2S5. Further, the sulfide solid electrolyte may contain a halogen (F, Cl, Br, I). In a preferred embodiment, the sulfide solid electrolyte contains Li6PS5X (where X is Cl, Br, or I, preferably Cl). Since these solid electrolytes have high ionic conductivity, they can also effectively contribute to the manifestation of the effects of the present invention.
[0055] As described above, the positive electrode material according to this embodiment includes a conductive material, a sulfur-containing positive electrode active material that coats the surface of the conductive material, and a solid electrolyte. However, the change rate (ΔC dl ) of the electric double layer capacitance per unit area of the positive electrode material between SOC0% and SOC100% of the secondary battery is 2 characterized in that it is 0.5 [F·cm
[0056] / g] or less. dl The electric double layer is a thin film-like layer formed at the interface where an ion conductor and an electron conductor are adjacent. Here, electrons and cations are arranged opposite to each other, or holes and anions are aligned opposite to each other. Therefore, the electric double layer can be regarded as a capacitor in which positive charges and negative charges are opposed to each other, and the concept of electric double layer capacitance (C
[0057] dl dlIn this specification, as described in the Examples section below, a test cell is prepared using the positive electrode material, and the test cell is subjected to an initial charge treatment and an initial discharge treatment, and then the AC impedance is measured by the EIS method to obtain the electric double layer capacity (C dl The method for producing the test cell, the method for charge / discharge treatment, and the method for measuring the AC impedance are the same as those described in the Examples below.
[0058] According to the study by the present inventors, when the state of charge (SOC) of a secondary battery changes, the electric double layer capacity (C dl ) also changed in the same way. Specifically, as the state of charge (SOC) of the secondary battery increases, the electric double layer capacity (C dl ) value becomes smaller. This is thought to be because when the state of charge (SOC) is low (during discharging), the solid electrolyte exists in a reduced state with high ionic conductivity, whereas when the state of charge (SOC) is high (during charging), the solid electrolyte exists in an oxidized state with low ionic conductivity. For example, taking the argyrodite-type sulfide solid electrolyte (Li6PS5Cl) used in the examples as an example, it becomes in a reduced state during discharging and exists in the states of Li2S, Li3P, LiCl, etc., of which Li3P is present at 10 -3 It has a high ionic conductivity of the order of [S / cm]. On the other hand, during charging, it becomes oxidized and exists in the form of S, P2S5, LiCl, etc., of which LiCl has an ionic conductivity of 10 -7 It is extremely low, on the order of [S / cm]. "SOC (state of charge)" refers to the ratio of the capacity at the current time to the capacity at the fully charged state. Therefore, "SOC 0%" means that the capacity at the current time is 0 (zero), and "SOC 100%" means that the capacity at the current time is equal to the capacity at the fully charged state.
[0059] As a result of further investigations, the inventors of the present invention found that the rate of change in electric double layer capacity per unit area of the positive electrode material between the fully discharged state (SOC 0%) and the fully charged state (SOC 100%) of the secondary battery (ΔC dl ) is 0.5 [F cm 2 / g] or less, the cycle durability is significantly improved.
[0060] In the positive electrode material according to the present invention, the rate of change in electric double layer capacity per unit area of the positive electrode material (ΔC dl ) is 0.5[F cm 2 / g] or less. However, from the viewpoint of further improving the cycle characteristics of the secondary battery, the rate of change (ΔC dl ) is preferably 0.4 [F cm 2 / g] or less, and more preferably 0.3 [F cm 2 / g] or less, and particularly preferably 0.2 [F cm 2 / g] or less, and most preferably 0.1 [F cm 2 / g] or less. Note that the "rate of change in electric double layer capacity per unit area of the positive electrode material (ΔC dl The method for calculating "(a)" will be the same as that described in the Examples section below.
[0061] According to the positive electrode material of the present embodiment having the above-mentioned configuration, it is possible to improve the cycle characteristics of a secondary battery such as an all-solid-state lithium secondary battery using a positive electrode active material containing sulfur. Although the mechanism by which such an excellent effect is achieved by adopting the configuration of the present embodiment is not completely clear, the following mechanism is presumed. First, as described above, according to the study by the present inventors, when a secondary battery is constructed by adopting the technology described in Patent Document 1, the discharge capacity of the secondary battery may decrease over time. In searching for the cause of this, the present inventors focused on the fact that some of the values of the discharge capacity per sulfur described in Table 1 of Patent Document 1 exceed the theoretical capacity of sulfur. In other words, since such an abnormal value was measured, it was thought that in the positive electrode material prepared in the example of Patent Document 1, the conductive material (carbon) and the solid electrolyte contact with each other, which causes the solid electrolyte to contribute to charging and discharging, and as a result, the decomposition reaction of the solid electrolyte proceeds.
[0062] Based on this idea, the inventors have used the electric double layer capacitance (C dl ), if the contact area between the solid electrolyte and the conductive material (carbon) is reduced, the electric double layer capacity (C dl ) change rate (ΔC dl We hypothesized that the electric double layer capacity (C) would also be reduced by devising a method for preparing the positive electrode material to reduce the contact area between the solid electrolyte and the conductive material (carbon). dl ) change rate (ΔC dl ) and confirmed that such a positive electrode material has excellent cycle durability, thereby proving the above hypothesis and completing the present invention.
[0063] In the positive electrode material according to the present embodiment, when the conductive material is a conductive material having pores, it is preferable that at least a part of the solid electrolyte is arranged inside the pores so as to contact the sulfur-containing positive electrode active material and not to contact the conductive material. With such a configuration, a three-phase interface in which the conductive material, the sulfur-containing positive electrode active material, and the solid electrolyte coexist is sufficiently formed, while the progress of the decomposition reaction of the solid electrolyte is suppressed, and as a result, a secondary battery having excellent capacity characteristics and charge / discharge rate characteristics can be provided. It is possible to confirm whether the positive electrode active material or the solid electrolyte is arranged inside the pores of the conductive material by using various conventionally known methods. For example, it is possible to perform element mapping from each material using energy dispersive X-ray spectroscopy (EDX) for an image of a cross section of a conductive material observed by a transmission electron microscope (TEM), and to confirm the arrangement form of each material using the obtained element map and the count number of elements from each material relative to the count number of all elements as an index. For example, in the case where the solid electrolyte contains phosphorus atoms and / or boron atoms, if there is no possibility that the phosphorus atoms and / or boron atoms are derived from other materials, it is possible to obtain the above element map for phosphorus and / or boron and confirm the arrangement of the solid electrolyte from its distribution. It is also possible to confirm the arrangement of the solid electrolyte from the ratio of the count number of phosphorus and / or boron to the count number of all elements in EDX. When the arrangement of the solid electrolyte is confirmed using the count number of elements derived only from the solid electrolyte as an index in EDX, if the ratio of the count number of elements derived only from the solid electrolyte to the count number of all elements in EDX is 0.10 or more, it can be determined that the solid electrolyte is arranged inside the pores of the conductive material. In addition, the value of the ratio is preferably 0.15 or more, more preferably 0.20 or more, even more preferably 0.26 or more, and particularly preferably 0.35 or more. The larger this value is, the more the solid electrolyte is arranged on the inner surface of the pores of the conductive material. Therefore, when the value of the ratio is within these ranges, the effect of the present invention can be more significantly exhibited.There is no particular restriction on the preferred upper limit of the ratio, but a preferred upper limit is, for example, 0.50 or less, and more preferably 0.45 or less.
[0064] Although there is no particular limitation on the manufacturing method of the positive electrode material according to the present embodiment having the above-mentioned configuration, an example of the manufacturing method will be briefly described below, taking as an example a case where a conductive material having pores is used. As described in the Examples section below, first, the conductive material is immersed in a melt or solution of the sulfur-containing positive electrode active material, and the sulfur-containing positive electrode active material is impregnated into the pores of the conductive material. Next, the impregnated material is subjected to a drying treatment as necessary. Thereafter, a solid electrolyte is added and mixed using a mixing means to obtain a positive electrode material. At this time, a so-called bead mill is used as a mixing means, and the positive electrode material according to the present embodiment can be obtained by mixing under mild mixing conditions of about 100 rpm.
[0065] The content of the positive electrode active material in the positive electrode active material layer is not particularly limited, but is preferably within the range of 35 to 99 mass %, and more preferably within the range of 40 to 90 mass %. Note that this content value is calculated based on the mass of only the positive electrode active material excluding the conductive material and the solid electrolyte.
[0066] The positive electrode active material layer may further contain a conductive assistant (one that does not hold the positive electrode active material or solid electrolyte inside the pores) and / or a binder.
[0067] [Positive and negative current collectors] The material constituting the current collector plates (25, 27) is not particularly limited, and any known highly conductive material conventionally used as a current collector plate for a secondary battery may be used. As the material constituting the current collector plates, for example, metal materials such as aluminum, copper, titanium, nickel, stainless steel (SUS), and alloys thereof are preferable. From the viewpoints of light weight, corrosion resistance, and high conductivity, aluminum and copper are more preferable, and aluminum is particularly preferable. The positive electrode current collector plate 27 and the negative electrode current collector plate 25 may be made of the same material or different materials.
[0068] [Positive and negative leads] Although not shown in the figures, the current collectors (11', 11") and the current collecting plates (25, 27) may be electrically connected via positive and negative electrode leads. As the materials for the positive and negative electrode leads, materials used in known lithium secondary batteries may be used. Note that the parts removed from the exterior are preferably covered with a heat-resistant insulating heat-shrink tube or the like to prevent them from coming into contact with peripheral devices or wiring, causing electric leakage and affecting products (e.g., automobile parts, particularly electronic devices, etc.).
[0069] [Battery exterior materials] As the battery exterior material, a known metal can case can be used, and a bag-shaped case using a laminate film 29 containing aluminum, which can cover the power generating element as shown in Figs. 1 and 2, can be used. The laminate film can be, for example, a three-layer laminate film formed by laminating PP, aluminum, and nylon in this order, but is not limited thereto. A laminate film is preferable from the viewpoint of being excellent in high output and cooling performance and being suitable for use in batteries for large equipment such as EVs and HEVs. In addition, a laminate film containing aluminum is more preferable as the exterior body because it can easily adjust the group pressure applied to the power generating element from the outside.
[0070] The stacked battery according to the present embodiment has a configuration in which a plurality of unit cell layers are connected in parallel, and thus has high capacity and excellent cycle durability, and is therefore suitable for use as a driving power source for EVs and HEVs.
[0071] While one embodiment of the lithium secondary battery has been described above, the present invention is not limited to the configuration described in the above embodiment, and may be modified as appropriate based on the claims.
[0072] For example, the type of battery to which the lithium secondary battery according to the present invention can be applied includes a bipolar battery including a bipolar electrode having a positive electrode active material layer electrically bonded to one surface of a current collector and a negative electrode active material layer electrically bonded to the opposite surface of the current collector.
[0073] In addition, the secondary battery according to the present embodiment may not be an all-solid-state type. That is, the solid electrolyte layer may further contain a conventionally known liquid electrolyte (electrolytic solution). There is no particular limit to the amount of liquid electrolyte (electrolytic solution) that can be contained in the solid electrolyte layer, but it is preferable that the amount is such that the shape of the solid electrolyte layer formed by the solid electrolyte is maintained and the liquid electrolyte (electrolytic solution) does not leak. In addition, as the liquid electrolyte (electrolytic solution), a solution having a form in which a conventionally known lithium salt is dissolved in a conventionally known organic solvent is used. The liquid electrolyte (electrolytic solution) may further contain additives other than the organic solvent and the lithium salt. These additives may be used alone or in combination of two or more. In addition, the amount of additives used in the electrolyte solution can be appropriately adjusted.
[0074] [Battery pack] A battery pack is a device that consists of multiple batteries connected together. More specifically, it is a device that uses at least two batteries and is configured in series or parallel or both. By connecting them in series or parallel, it is possible to freely adjust the capacity and voltage.
[0075] A small, removable assembled battery can be formed by connecting a plurality of batteries in series or in parallel. Then, a large capacity, high output assembled battery (battery module, battery pack, etc.) suitable for a vehicle driving power source or an auxiliary power source that requires a high volumetric energy density and a high volumetric output density can be formed by further connecting a plurality of such small, removable assembled batteries in series or in parallel. How many batteries are connected to form an assembled battery, and how many stages of small assembled batteries are stacked to form a large capacity assembled battery can be determined according to the battery capacity and output of the vehicle (electric vehicle) in which the battery is to be installed.
[0076] [vehicle] The battery or a battery pack formed by combining a plurality of batteries can be mounted on a vehicle. In the present invention, a battery with excellent long-term reliability and long life can be configured, and thus, by mounting such a battery, a plug-in hybrid electric vehicle with a long EV driving distance or an electric vehicle with a long driving distance per charge can be configured. For example, if the battery or a battery pack formed by combining a plurality of batteries is used in a hybrid vehicle, a fuel cell vehicle, or an electric vehicle (all of which include four-wheeled vehicles (commercial vehicles such as passenger cars, trucks, and buses, and light vehicles, etc.), as well as two-wheeled vehicles (motorcycles) and three-wheeled vehicles), the vehicle will have a long life and high reliability. However, the application is not limited to automobiles, and the battery pack can be applied to, for example, various power sources for other vehicles, such as moving bodies such as trains, and can also be used as a mounted power source for an uninterruptible power supply device or the like. EXAMPLES
[0077] The present invention will be described in more detail below with reference to examples, although the technical scope of the present invention is not limited to the following examples.
[0078] Example of test cell preparation [Example 1] (Hot sulfur impregnation) In a glove box with an argon atmosphere at a dew point of -68°C or less, 0.060g of carbon (Kansai Thermochemical Co., Ltd., activated carbon, MSC-30) (conductive material with fine pores) was added to 0.140g of sulfur (Aldrich) and mixed thoroughly in an agate mortar, and the mixed powder was then placed in a sealed pressure-resistant autoclave and heated at 170°C for 3 hours to melt the sulfur and impregnate the carbon with the sulfur. This resulted in a sulfur / carbon composite material.
[0079] (Preparation of sulfur-containing positive electrode material) In a glove box in an argon atmosphere with a dew point of -68°C or less, 0.5 g of zirconia balls with a diameter of 2 mm, 0.120 g of the sulfur / carbon composite material prepared above, and 0.080 g of an argyrodite-type sulfide solid electrolyte (Li6PS5Cl, manufactured by Ampcera) were placed in a sample bottle with a capacity of 10 mL, and treated with a tabletop rotating roller (VMR-3R, manufactured by AS ONE Corporation) (bead mill) at 100 rpm for 0.5 hours to obtain a powder of a sulfur-containing positive electrode material. The composition of the sulfur-containing positive electrode material was sulfur: solid electrolyte: carbon = 42: 40: 18 (mass ratio). In addition, when the obtained sulfur-containing positive electrode material was observed using a scanning electron microscope (SEM), it was confirmed that the conductive material carbon was covered with the positive electrode active material sulfur (the same applies to the following examples).
[0080] (Production of all-solid-state lithium secondary batteries) An all-solid-state lithium secondary battery was fabricated in a glove box with an argon atmosphere at a dew point of -68°C or lower by the following method.
[0081] A SUS cylindrical convex punch (10 mm diameter) was inserted into one side of a cylindrical tube jig made by Macor (inner diameter 10 mm, outer diameter 23 mm, height 20 mm), and 80 mg of an argyrodite-type sulfide solid electrolyte (Li6PS5Cl, made by Ampcera) was placed into the cylindrical tube jig from the top. Then, another SUS cylindrical convex punch was inserted to sandwich the solid electrolyte, and the solid electrolyte was pressed for 3 minutes at a pressure of 75 MPa using a hydraulic press to form a solid electrolyte layer with a diameter of 10 mm and a thickness of approximately 0.6 mm in the cylindrical tube jig.
[0082] Next, the cylindrical convex punch inserted from the top was removed once, 8.2 mg of the sulfur-containing positive electrode material prepared above was placed on one side of the solid electrolyte layer in the cylindrical tube, and a cylindrical convex punch (also serving as a positive electrode current collector) was inserted from the top again and pressed at a pressure of 300 MPa for 3 minutes to form a positive electrode active material layer with a diameter of 10 mm and a thickness of about 0.06 mm on one side of the solid electrolyte layer. Next, the lower cylindrical convex punch (also serving as a negative electrode current collector) was removed, and a lithium foil (manufactured by Nilaco, thickness 0.20 mm) punched to a diameter of 8 mm and an indium foil (manufactured by Nilaco, thickness 0.30 mm) punched to a diameter of 9 mm were stacked, and the indium foil was inserted from the bottom of the cylindrical tube jig so that it was located on the solid electrolyte layer side, and the cylindrical convex punch was inserted again and pressed at a pressure of 75 MPa for 3 minutes to form a lithium-indium negative electrode.
[0083] In this manner, an all-solid-state lithium secondary battery was produced in which the negative electrode current collector, the lithium-indium negative electrode, the solid electrolyte layer, the positive electrode active material layer, and the positive electrode current collector were laminated.
[0084] (Evaluation of charge / discharge characteristics of all-solid-state lithium secondary batteries) Using an electrochemical diagnostic device (VSP-300, manufactured by BioLogic) in a constant temperature bath set at 25° C., the charge / discharge characteristics of the all-solid-state lithium secondary battery prepared above were evaluated by the following method.
[0085] The battery was placed in a thermostatic chamber, and after the cell temperature had stabilized, the battery was conditioned at 0.2 mA / cm 2 The cell was discharged at a constant current density of 0.5 V to a cell voltage of 0.5 V, followed by a constant current / constant voltage charge to 2.5 V at the same current density (cut-off current 0.01 mA / cm 2 )-constant current discharge (voltage 0.5 V) were performed for 10 cycles as a conditioning charge-discharge cycle. From the charge-discharge capacity value obtained after this conditioning charge-discharge cycle and the mass value of the sulfur active material contained in the positive electrode active material layer, the capacity value per mass of sulfur (mAh / g) was calculated.
[0086] The cycle characteristics were evaluated by fully charging the battery at 25°C under the conditions of 0.05C-2.5V constant current / constant voltage charging with a cutoff current of 0.01C, and then discharging at 0.05C with a cutoff voltage of 0.5V. The 10th cycle discharge capacity retention rate [%] was calculated as the percentage of the discharge capacity at the 10th cycle to the discharge capacity at the first cycle. The results are shown in Table 1 below.
[0087] (Evaluation of AC impedance of all-solid-state lithium secondary batteries) After a 1.0 hour rest period was provided at the end of charging (SOC 100%) and at the end of discharging (SOC 0%) in the first cycle of the cycle characteristic evaluation described above, the measurement frequency f was set to 7MHz to 10mHz, the voltage amplitude ΔV was set to ±5mV relative to the open circuit voltage (OCV) of the cell, and the AC impedance of the battery was evaluated by electrochemical impedance measurement (EIS). Note that the evaluation was also performed using the same electrochemical diagnostic device as above.
[0088] Next, from the evaluation results of the AC impedance, the electric double layer capacity (C dl ), and the rate of change in electric double layer capacity per unit area of the positive electrode material (ΔC dl ) was calculated.
[0089] First, the equivalent circuit of this battery system was simulated using a general Randolph equivalent circuit shown below.
[0090]
number
[0091] Then, calculate the angular frequency ω (=2πf) from the measured frequency f, and set the X-axis to ω -2 and the Y axis is the imaginary part of the impedance Z img and the angular frequency ω (1 / ωZ img) and a Cole-Cole plot is created. The intersection of the straight line extrapolated from the low-frequency side and the Y-axis is the electric double-layer capacitance C of the positive electrode material. dl [mF] (see Figure 3). In this way, the electric double layer capacity (C dl,SOC100% ) and the electric double layer capacity (C dl,SOC0% ) were calculated respectively.
[0092] Next, the two Cs calculated above dl The difference between the values of (C dl,SOC0% -C dl,SOC100% ) [mF] is the weight of the positive electrode material [mg / cm 2 ] to obtain the rate of change in electric double layer capacity per unit area of the positive electrode material between the end of discharge (SOC 0%) and the end of charge (SOC 100%) (ΔC dl )[F cm 2 The results are shown in Table 1 below.
[0093] [Example 2] In the preparation of the sulfur / carbon composite material, the amount of carbon used was changed to 0.033 g, and the amount of sulfur used was changed to 0.167 g, but an all-solid-state lithium secondary battery was produced in the same manner as in Example 1 described above. In addition, the charge / discharge characteristics and AC impedance of the all-solid-state lithium secondary battery were evaluated in the same manner as above, and the 10th cycle discharge capacity retention rate and the rate of change in electric double layer capacity per unit area of the positive electrode material (ΔC dl The results are shown in Table 1 below.
[0094] [Example 3] In preparing the sulfur / carbon composites, the solution impregnation method described below was used.
[0095] That is, 1000 mg of sulfur and 20 g of cyclohexane were placed in a 50 mL screw tube, and the sulfur was dissolved by stirring with a magnetic stirrer while heating to 60°C. Next, 300 mg of carbon (Kansai Thermochemical Industry Co., Ltd., activated carbon, MSC-30) was immersed in the cyclohexane solution of sulfur, and ultrasonic treatment (output 100 W, oscillation frequency 28 Hz, 40 minutes) was performed to disperse the carbon. Then, the mixture was stirred with a magnetic stirrer at 25°C for 7 days to adsorb sulfur to the carbon, thereby preparing a sulfur / carbon composite material.
[0096] Here, about 2 g of the dispersion liquid after sulfur adsorption was extracted, the carbon covered with sulfur was precipitated by centrifugation, and the solid content of the supernatant sulfur solution was measured. As a result, the solid content was 1.478 mass%. Since the concentration of the original sulfur solution was 4.762 mass%, 700 mg of sulfur covered 300 mg of carbon. And the mass ratio of sulfur in the carbon to which sulfur was adsorbed was calculated to be 70 mass%.
[0097] The entire remaining amount, except for about 2 g extracted for calculating the amount of sulfur coating, was suction filtered to separate the sulfur-adsorbed carbon from the sulfur solution. The carbon was then heated at 160°C for 1 hour to obtain 862 mg (yield 86.2%) of a sulfur / carbon composite material.
[0098] Except for using the sulfur / carbon composite material thus obtained, an all-solid-state lithium secondary battery was produced in the same manner as in Example 1 described above. In addition, the charge / discharge characteristics and AC impedance of the all-solid-state lithium secondary battery were evaluated in the same manner as above, and the 10th cycle discharge capacity retention rate and the rate of change in electric double layer capacity per unit area of the positive electrode material (ΔC dl The results are shown in Table 1 below.
[0099] [Comparative Example 1] No thermal impregnation with sulfur was performed. Instead, 40 g of 5 mm diameter zirconia balls, 0.138 g of an argyrodite-type sulfide solid electrolyte (Li6PS5Cl, manufactured by Ampcera) and 0.062 g of carbon (activated carbon, MSC-30, manufactured by Kansai Thermochemical Industry Co., Ltd.) were placed in a glove box in an argon atmosphere with a dew point of -68°C or lower and placed in a 45 mL zirconia container and processed at 370 rpm for 6 hours in a planetary ball mill to obtain a powder of the positive electrode material of this comparative example.
[0100] Except for using the positive electrode material thus obtained, an all-solid-state lithium secondary battery was produced in the same manner as in Example 1 described above. In addition, the charge / discharge characteristics and AC impedance of the all-solid-state lithium secondary battery were evaluated in the same manner as above, and the 10th cycle discharge capacity retention rate and the rate of change in electric double layer capacity per unit area of the positive electrode material (ΔC dl The results are shown in Table 1 below.
[0101] [Comparative Example 2] In the preparation of the sulfur / carbon composite material, the amount of carbon used was changed to 0.102 g, and the amount of sulfur used was changed to 0.098 g, but other than this, an all-solid-state lithium secondary battery was produced in the same manner as in Example 1 described above. In addition, the charge / discharge characteristics and AC impedance of the all-solid-state lithium secondary battery were evaluated in the same manner as above, and the 10th cycle discharge capacity retention rate and the rate of change in electric double layer capacity per unit area of the positive electrode material (ΔC dl The results are shown in Table 1 below.
[0102] [Comparative Example 3] In the preparation of the sulfur / carbon composite, the mixed powder was placed in an unsealed glass container and heated at 170°C for 3 hours to melt the sulfur and impregnate the carbon with the sulfur. After that, the furnace was evacuated with a diaphragm pump while heating at 250°C for 3 hours to sublimate the sulfur, and the sulfur that was not impregnated and remained on the carbon surface was removed (reduced pressure thermal impregnation process).
[0103] Except for using the sulfur / carbon composite material thus obtained, an all-solid-state lithium secondary battery was produced in the same manner as in Example 1 described above. In addition, the charge / discharge characteristics and AC impedance of the all-solid-state lithium secondary battery were evaluated in the same manner as above, and the 10th cycle discharge capacity retention rate and the rate of change in electric double layer capacity per unit area of the positive electrode material (ΔC dl The results are shown in Table 1 below.
[0104] [Comparative Example 4] In the preparation of the sulfur-containing positive electrode material, 0.5 g of zirconia balls with a diameter of 2 mm was replaced with 40 g of zirconia balls with a diameter of 5 mm, and the treatment using a tabletop rotating roller was replaced with treatment using a planetary ball mill (Fritsch, Premium line P-7) (370 rpm for 6 hours). Except for this, an all-solid-state lithium secondary battery was produced in the same manner as in Example 1 described above. In addition, the charge / discharge characteristics and AC impedance of the all-solid-state lithium secondary battery were evaluated in the same manner as above, and the 10th cycle discharge capacity retention rate and the rate of change in electric double layer capacity per unit area of the positive electrode material (ΔC dl The results are shown in Table 1 below.
[0105] [Comparative Example 5] In the preparation of the sulfur-containing positive electrode material, 0.5 g of zirconia balls with a diameter of 2 mm was changed to 40 g of zirconia balls with a diameter of 5 mm, and the treatment using a tabletop rotating roller was changed to treatment using a planetary ball mill (Fritsch, Premium line P-7) (370 rpm for 6 hours). Except for this, an all-solid-state lithium secondary battery was produced in the same manner as in Example 3 described above. In addition, the charge / discharge characteristics and AC impedance of the all-solid-state lithium secondary battery were evaluated in the same manner as above, and the 10th cycle discharge capacity retention rate and the rate of change in electric double layer capacity per unit area of the positive electrode material (ΔC dl The results are shown in Table 1 below.
[0106] [Table 1]
[0107] From the results shown in Table 1, the specified ΔC dl It can be seen that the all-solid-state lithium secondary batteries of Examples 1 to 3 using the positive electrode material having the above structure exhibit a higher discharge capacity retention rate than the batteries of Comparative Examples 1 to 5. In addition, from the comparison of Examples 1 to 3, ΔC dl It can also be seen that the smaller the value of is, the more the discharge capacity retention rate can be improved.
[0108] In Comparative Example 2, ΔC dl The reason why the value of is large is considered to be that the carbon content in the sulfur / carbon composite is relatively high, so that even if the solid electrolyte is mixed using a bead mill, the contact area between the solid electrolyte and the carbon becomes large, and the decomposition reaction of the solid electrolyte during charging and discharging cannot be suppressed. dl The reason why the value of is large is considered to be that the contact area between the solid electrolyte and the carbon is increased because the sulfur remaining on the carbon surface during the reduced pressure heat impregnation treatment is removed by sublimation, and the decomposition reaction of the solid electrolyte during charging and discharging cannot be suppressed as described above. Furthermore, in Comparative Examples 4 and 5, a large amount of relatively large zirconia balls are used, and the mixing treatment is performed using a planetary ball mill under stricter mixing conditions. For this reason, the sulfur that covered the carbon in the sulfur / carbon composite material falls off, and as a result, the contact area between the solid electrolyte and the carbon becomes large, and the decomposition reaction of the solid electrolyte during charging and discharging cannot be suppressed. [Explanation of symbols]
[0109] 10a Stacked battery, 11' negative electrode current collector, 11” positive electrode current collector, 13 negative electrode active material layer, 15 positive electrode active material layer, 17 solid electrolyte layer, 19 cell layer, 21 Power generation elements, 25 negative current collector plate, 27 Positive current collector, 29 Laminating film.
Claims
1. A conductive material, a sulfur-containing positive electrode active material that coats a surface of the conductive material, and a solid electrolyte, The rate of change in electric double layer capacity per unit area of the positive electrode material between SOC 0% and SOC 100% of the secondary battery (ΔC dl ) is 0.5 [F cm 2 / g] or less.
2. The rate of change (ΔC dl ) is 0.2 [F cm 2 2. The positive electrode material for a secondary battery according to claim 1, wherein the molecular weight of the positive electrode material is 100% or less.
3. 3. The positive electrode material for a secondary battery according to claim 1, wherein the conductive material has pores.
4. The positive electrode material for a secondary battery according to claim 3 , wherein the conductive material has a pore volume of 1.0 mL / g or more.
5. 5. The positive electrode material for a secondary battery according to claim 3, wherein the conductive material has an average pore size of 50 nm or less.
6. 6. The positive electrode material for a secondary battery according to claim 3, wherein at least a part of the solid electrolyte is arranged inside the pores so as to be in contact with the sulfur-containing positive electrode active material and not in contact with the conductive material.
7. The positive electrode material for a secondary battery according to any one of claims 1 to 6, wherein the conductive material is a carbon material.
8. The positive electrode material for secondary batteries according to any one of claims 1 to 7, wherein the solid electrolyte is a sulfide solid electrolyte.
9. 9. The positive electrode material for a secondary battery according to claim 1, wherein the solid electrolyte contains an alkali metal atom and a phosphorus atom and / or a boron atom.
10. The positive electrode material for a secondary battery according to claim 9 , wherein the alkali metal atom is lithium.
11. A secondary battery comprising the positive electrode material for secondary batteries according to any one of claims 1 to 10.
12. The secondary battery according to claim 11 , which is an all-solid-state lithium secondary battery.
Citation Information
Patent Citations
Thin film sulfur-coated activated carbon, positive electrode mixture, and all-solid-state lithium sulfur battery
JP2015088231A
Composite material
WO2014162693A1