Polymer-metal composites, tires, and polymer articles
The polymer-metal composite uses a modified copolymer with specific units and peroxide to enhance adhesion and stability, addressing environmental and processability issues in existing adhesion methods.
Patent Information
- Application Number
- JP2020206266
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-11
- Publication Date
- 2024-11-28
- Estimated Expiration
- 2040-12-11
Smart Images

Figure 0007591394000001 
Figure 0007591394000002 
Figure 0007591394000003
Abstract
Description
[Technical field]
[0001] The present invention relates to polymer-metal composites, tires, and polymer articles. [Background technology]
[0002] 2. Description of the Related Art Conventionally, direct vulcanization adhesion and indirect vulcanization adhesion methods have been widely used for bonding and compounding polymer members, such as diene-based rubber members, and metal members.
[0003] The direct vulcanization adhesion method is a bonding method in which a vulcanization system such as sulfur and, if necessary, an adhesion promoter such as a cobalt salt are mixed with a polymer member in advance, and an adhesive metal layer such as brass is formed in advance on the surface of a metal member, so that adhesion with the metal layer is achieved by the vulcanization reaction (crosslinking reaction) of the vulcanization system.On the other hand, the indirect vulcanization adhesion method is a bonding method in which an adhesive applied in advance to a polymer member and a metal member obtains vulcanization energy and achieves adhesion.
[0004] Regarding the above-mentioned adhesion method, the material of the polymer member itself is also being studied to improve adhesion. For example, Patent Document 1 discloses that SEBS (styrene-ethylene-butylene-styrene block copolymer) modified with maleic anhydride is blended with the rubber member to improve adhesion between the metal reinforcing material and the rubber member. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 8-225660 Summary of the Invention [Problem to be solved by the invention]
[0006] As described above, the direct vulcanization adhesion method requires the formation of a predetermined adhesive metal layer on the surface of the metal member to be bonded. In addition, there is a tendency to require a reduction in the amount of cobalt salt to be mixed into the polymer member in the direct vulcanization adhesion method from the viewpoint of reducing the environmental load. Furthermore, since sulfur, which is usually used as a vulcanization system in the direct vulcanization adhesion method, affects the deterioration of processability, heat deterioration, oxygen deterioration, etc., it is desirable to use a small amount of sulfur.
[0007] On the other hand, in the indirect vulcanization adhesion method, an organic solvent is usually used in the adhesive, but from the viewpoint of environmental load, it is desirable to use a small amount of organic solvent, and in particular to use no organic solvent at all.
[0008] In view of these circumstances, there is a need for improved techniques for firmly bonding polymeric and metallic components.
[0009] Therefore, an object of the present invention is to provide a polymer-metal composite in which a polymer member and a metal member are firmly bonded to each other. Another object of the present invention is to provide high-strength tires and polymer articles using such a polymer-metal composite. [Means for solving the problem]
[0010] The gist of the present invention for solving the above problems is as follows.
[0011] The polymer-metal composite of the present invention is a polymer-metal composite in which a polymer member containing a rubber component and / or a resin component and a metal member are bonded via an adhesive layer, The adhesive layer is characterized in that it contains a modified copolymer having conjugated diene units and non-conjugated olefin units, having no butylene units, and having a modifying group. In such a polymer-metal composite of the present invention, the polymer member and the metal member are firmly bonded to each other.
[0012] In the polymer-metal composite of the present invention, the modified copolymer preferably further contains an aromatic vinyl unit, which improves the fracture resistance of the copolymer itself and effectively suppresses peeling between the polymer member and the metal member.
[0013] In the polymer-metal composite of the present invention, the aromatic vinyl unit preferably contains an α-methylstyrene unit, an o-methylstyrene unit, an m-methylstyrene unit, or a p-methylstyrene unit, which makes it easier to introduce a modifying group and improves manufacturability.
[0014] In the polymer-metal composite of the present invention, from the same viewpoint as above, it is preferable that the aromatic vinyl units consist only of p-methylstyrene units.
[0015] In the polymer-metal composite of the present invention, the modifying group preferably has at least one selected from an oxygen atom, a nitrogen atom, a silicon atom, a sulfur atom, a halogen atom, and a metal atom, which can further improve the adhesive effect between the polymer member and the metal member.
[0016] In the polymer-metal composite of the present invention, from the viewpoint of more firmly adhering the polymer member and the metal member, it is preferable that the modifying group has at least one of a carbonyl moiety (-C(=O)-) and a thiocarbonyl moiety (-C(=S)-).
[0017] In the polymer-metal composite of the present invention, from the same viewpoint as above, it is more preferable that the modifying group has at least one of an ester bond (-C(=O)O-) and a dithioester bond (-C(=S)S-).
[0018] In the polymer-metal composite of the present invention, the proportion of the modifying group in the modified copolymer is preferably 0.1% by mass or more and 10.0% by mass or less, which allows the polymer member and the metal member to be more firmly bonded to each other and also allows gelation caused by a reaction between the modifying groups to be sufficiently suppressed.
[0019] In the polymer-metal composite of the present invention, the proportion of conjugated diene units in the modified copolymer is preferably 10 mol % or more, which can further improve the adhesion to the polymer member.
[0020] In the polymer-metal composite of the present invention, the proportion of conjugated diene units in the modified copolymer is preferably 25 mol % or more, which can further improve the adhesion to the polymer member.
[0021] In the polymer-metal composite of the present invention, from the viewpoint of more firmly adhering the polymer member and the metal member, it is preferable that in the modified copolymer, the conjugated diene unit is a butadiene unit and the non-conjugated olefin unit is an ethylene unit.
[0022] In the polymer-metal composite of the present invention, it is preferable that the polymer member does not substantially contain a cobalt-containing compound from the viewpoint of environmental regulations.
[0023] In the polymer-metal composite of the present invention, the polymer member preferably contains less than 3 parts by mass of sulfur per 100 parts by mass of the rubber component and / or the resin component, from the viewpoint of suppressing deterioration of processability, heat degradation, and oxygen degradation.
[0024] In the polymer-metal composite of the present invention, the adhesive layer preferably further contains a peroxide, in which case even if the composite is placed in a high-temperature environment, the polymer member and the metal member can maintain even stronger adhesion.
[0025] In the polymer-metal composite of the present invention, the one-hour half-life temperature of the peroxide is preferably higher than the melting point of the modified copolymer, which can effectively prevent the peroxide from reacting prematurely when kneading the peroxide with the modified copolymer in advance.
[0026] In the polymer-metal composite of the present invention, the one-hour half-life temperature of the peroxide is preferably 110° C. or higher. In this case, premature reaction of the peroxide can be effectively suppressed when the peroxide is kneaded in advance with the modified copolymer.
[0027] The tire of the present invention is characterized in that it comprises the above-mentioned polymer-metal composite, in which the polymer member contains a rubber component. Such a tire of the present invention has high strength.
[0028] The polymer article of the present invention is characterized by comprising the above-mentioned polymer-metal composite. Such a polymer article of the present invention has high strength. Effect of the Invention
[0029] According to the present invention, it is possible to provide a polymer-metal composite in which a polymer member and a metal member are firmly bonded to each other. Furthermore, according to the present invention, it is possible to provide high-strength tires and polymer articles using such a polymer-metal composite. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0030] Hereinafter, the present invention will be described in detail based on embodiments.
[0031] (Polymer-metal composites) In a polymer-metal composite according to one embodiment of the present invention (hereinafter sometimes referred to as the "composite according to the present embodiment"), a polymer member containing a rubber component and / or a resin component and a metal member are bonded via an adhesive layer. Moreover, in the composite according to the present embodiment, the adhesive layer contains a modified copolymer having conjugated diene units and non-conjugated olefin units, no butylene units, and having a modifying group (hereinafter sometimes simply referred to as the "modified copolymer").
[0032] In the composite of this embodiment, the modified copolymer contained in the adhesive layer can be highly bonded to the metal member by hydrogen bonds derived from the modified group. In addition, since the modified copolymer contained in the adhesive layer has a conjugated diene unit, it can form a bond with a member containing a rubber component by a co-crosslinking reaction. In addition, since the modified copolymer contained in the adhesive layer has a non-conjugated olefin unit, it can form a bond with a member containing a resin component by melting with each other. Due to these actions, it is considered that the polymer member and the metal member can be firmly bonded to each other through the above-mentioned adhesive layer in the composite of this embodiment.
[0033] Furthermore, in the composite of this embodiment, the above-mentioned modified copolymer may be used as the adhesive layer, that is, adhesiveness can be exhibited in a single layer, which is advantageous in that the composite is easy to manufacture.
[0034] The composite body of this embodiment can be used for various rubber articles such as tires, conveyor belts, hoses, crawlers, etc., which will be described later, or various resin articles.
[0035] <Metal parts> The shape of the metal member used in the composite of the present embodiment is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include a cord shape, a flat plate shape, etc. In particular, examples of cord-shaped metal members, typified by steel cords, include those made of a plurality of twisted metal wires (metal steel wires) or those made of a single metal wire.
[0036] Examples of the material of the metal member include iron, steel (stainless steel), lead, aluminum, copper, brass, bronze, Monel metal alloy, nickel, zinc, etc. However, in this embodiment, the material of the metal member is not particularly limited, and any material can exhibit strong adhesion with the polymer member. In addition, the metal member used in the composite of this embodiment may have a surface plated with any metal. In addition, when the metal member has a surface plated, the material of the main body of the metal member may be non-metallic. The surface plating is not particularly limited, but examples thereof include copper plating, zinc plating, brass plating, etc.
[0037] <Polymer materials> The polymer member in the composite of this embodiment is a member to be adhered to the metal member and contains a rubber component and / or a resin component. For convenience, the polymer member containing at least a rubber component can be called a "rubber member", and the polymer member containing at least a resin component can be called a "resin member". The polymer member may contain both a rubber component and a resin component.
[0038] The shape of the polymer member is not particularly limited and can be appropriately selected depending on the purpose, for example, a flat plate shape. When the metal member is cord-shaped, the polymer member can cover the peripheral surface of the metal member (through an adhesive layer). When the polymer member in the composite of the present embodiment contains a rubber component, the polymer member can be a vulcanizate.
[0039] The polymer component can be made from a polymer composition that contains at least a rubber component or a resin component. When a rubber component is used, the rubber component preferably contains a diene rubber, and more preferably consists of only a diene rubber. This allows the polymer member and the modified copolymer contained in the adhesive layer to be co-crosslinked, thereby further improving adhesion. Examples of diene rubber include natural rubber (NR), isoprene rubber (IR), butadiene rubber (BR), styrene-butadiene rubber (SBR), styrene-isoprene-butadiene rubber (SIBR), butyl rubber, ethylene-propylene rubber (EPM), ethylene propylene diene rubber (EPDM), chloroprene rubber (CR), and acrylonitrile butadiene rubber (NBR). The rubber component may be used alone or in combination of two or more. In particular, from the viewpoint of high fracture properties, it is preferable to use natural rubber, isoprene rubber, butadiene rubber, styrene-butadiene rubber, butyl rubber, acrylonitrile butadiene rubber, chloroprene rubber, or ethylene-propylene rubber as the rubber component, and it is more preferable to use natural rubber.
[0040] When a resin component is used, the resin component can be appropriately selected according to the desired performance of the polymer article (resin article) finally produced, and examples thereof include homopolymers such as polyethylene, polypropylene, polybutene, polystyrene, etc.; copolymers such as ethylene-propylene copolymer, ethylene-methacrylic acid copolymer, ethylene-ethyl acrylate copolymer, ethylene-vinyl acetate copolymer, etc., and polyolefin resins such as ionomer resins thereof; polyvinyl alcohol resins such as vinyl alcohol homopolymer and ethylene-vinyl alcohol copolymer; poly(meth)acrylic acid resin and its ester resin; polyamide resins such as aliphatic polyamide resin and aromatic polyamide resin; polyethylene glycol resin; carboxyvinyl copolymer; styrene-maleic acid copolymer; polyvinylpyrrolidone resins such as vinylpyrrolidone homopolymer and vinylpyrrolidone-vinyl acetate copolymer; polyester resin; cellulose resin; mercaptomethanol; hydrogenated styrene-butadiene; syndiotactic polybutadiene, trans polybutadiene, trans polyisoprene, etc. The resin component may be used alone or in combination of two or more. Among these, from the viewpoint of affinity with the modified copolymer, the resin component is preferably a resin component having a non-conjugated olefin unit, more preferably a polyolefin resin, and further preferably polyethylene, polypropylene, polybutene, or an ethylene-propylene copolymer.
[0041] Furthermore, the polymer composition used to prepare the polymer member may contain, as necessary, appropriate additives depending on the purpose, such as fillers such as carbon black and silica, filler modifiers such as silane coupling agents, vulcanizing agents such as sulfur, vulcanization accelerators, vulcanization acceleration assistants such as zinc oxide, softeners such as oil, antioxidants, scorch inhibitors, processing aids, lubricants, tackifiers, colorants, and the like.
[0042] In addition, from the viewpoint of environmental regulations, it is preferable that the polymer composition used to prepare the polymer member does not substantially contain a cobalt-containing compound. Similarly, from the viewpoint of environmental regulations, it is preferable that the polymer member used in the composite of this embodiment does not substantially contain a cobalt-containing compound. Conventionally, cobalt-containing compounds such as cobalt salts have been mixed with rubber and the like for the purpose of improving adhesion, but in this embodiment, high adhesion to metal members can be achieved without using a cobalt-containing compound in the polymer member.
[0043] Moreover, the polymer composition used to prepare the polymer member preferably has a sulfur content of less than 3 mass parts by mass per 100 parts by mass of the rubber component and / or the resin component, from the viewpoint of suppressing deterioration of processability, heat degradation, and oxygen degradation. Similarly, the polymer member used in the composite of this embodiment preferably has a sulfur content of less than 3 mass parts by mass per 100 parts by mass of the rubber component and / or the resin component, from the viewpoint of suppressing deterioration of processability, heat degradation, and oxygen degradation. Conventionally, a large amount of sulfur has been blended into rubber and the like for the purpose of improving adhesion, but in this embodiment, high adhesion to metal members can be achieved without using a large amount of sulfur in the polymer member.
[0044] The polymer composition is not particularly limited, and can be prepared, for example, by blending and kneading the above-mentioned components according to a conventional method. A kneading machine such as a Banbury mixer or a kneader can be used for kneading. Furthermore, when the polymer composition is used to mold a polymer member into a sheet or strip shape, a known molding machine such as an extruder or a press can be used.
[0045] In addition, when the polymer composition contains a rubber component, the polymer composition may be vulcanized in a state in which it is in contact with an adhesive layer (modified copolymer) to form a polymer member.
[0046] <Adhesive layer (modified copolymer)> The adhesive layer used in the composite of the present embodiment contains at least a modified copolymer having conjugated diene units and non-conjugated olefin units, no butylene units, and a modifying group. Such an adhesive layer usually consists of only one layer containing the modified copolymer.
[0047] In addition, the adhesive layer may contain other additives such as peroxides (described later), fillers such as carbon black and silica, filler modifiers such as silane coupling agents, vulcanizing agents such as sulfur, vulcanization accelerators, vulcanization accelerator assistants such as zinc oxide, softeners such as oils, antioxidants, scorch inhibitors, processing assistants, lubricants, tackifiers, and colorants, as necessary, depending on the purpose. However, from the viewpoint of reliably obtaining the desired effect, the adhesive layer preferably contains 95% by mass or more of the modified copolymer, more preferably 98% by mass or more, and even more preferably 100% by mass (i.e., the adhesive layer is composed of only the modified copolymer).
[0048] The modified copolymer has at least a conjugated diene unit. Here, the conjugated diene unit is a structural unit corresponding to a unit derived from a conjugated diene compound as a monomer. The conjugated diene compound means a conjugated diene compound. Examples of the conjugated diene compound include 1,3-butadiene, isoprene, 1,3-pentadiene, and 2,3-dimethyl-1,3-butadiene. From the viewpoint of further improving the adhesion to the polymer member, the conjugated diene unit in the modified copolymer preferably contains a butadiene unit (a structural unit corresponding to a unit derived from 1,3-butadiene) and / or an isoprene unit, and more preferably consists of only a butadiene unit. The conjugated diene unit in the modified copolymer may be one type alone or two or more types in combination.
[0049] The proportion of the conjugated diene unit in the modified copolymer is preferably 10 mol% or more. If it is 10 mol% or more, the adhesion to the polymer material can be further improved. From the same viewpoint, the proportion of the conjugated diene unit in the modified copolymer is more preferably 25 mol% or more, and even more preferably 40 mol% or more, and is preferably 80 mol% or less, more preferably 70 mol% or less, and even more preferably 60 mol% or less.
[0050] The modified copolymer has at least a non-conjugated olefin unit. Here, the non-conjugated olefin unit is a structural unit corresponding to a unit derived from a non-conjugated olefin compound as a monomer. The non-conjugated olefin compound means an aliphatic unsaturated hydrocarbon having one or more carbon-carbon double bonds. Examples of the non-conjugated olefin compound include α-olefins such as ethylene, propylene, 1-pentene, 1-hexene, 1-heptene, and 1-octene, and heteroatom-substituted alkene compounds such as vinyl pivalate, 1-phenylthioethene, and N-vinylpyrrolidone. The non-conjugated olefin unit in the modified copolymer preferably contains an ethylene unit and / or a propylene unit, and more preferably consists of only an ethylene unit, from the viewpoint of more reliably exerting the desired effect. The non-conjugated olefin unit in the modified copolymer may be one type alone or a combination of two or more types.
[0051] The proportion of non-conjugated olefin units in the modified copolymer is preferably 20 mol% or more. If it is 20 mol% or more, the desired effect can be more reliably exhibited. From the same viewpoint, the proportion of non-conjugated olefin units in the modified copolymer is more preferably 30 mol% or more, and even more preferably 40 mol% or more. In addition, from the viewpoint of fully obtaining the effects exerted by the conjugated diene units, etc., the proportion of non-conjugated olefin units in the modified copolymer is more preferably 99 mol% or less, and even more preferably 90 mol% or less.
[0052] In order to reliably obtain the desired effect, the modified copolymer does not have a butylene unit, i.e., the modified copolymer preferably does not contain a polymer obtained by hydrogenating butadiene or a hydrogenated product of a styrene-butadiene copolymer such as styrene-ethylene / butylene-styrene (SEBS).
[0053] The modified copolymer preferably further contains an aromatic vinyl unit in addition to the conjugated diene unit and the non-conjugated olefin unit, which improves the fracture resistance of the copolymer itself and effectively suppresses peeling between the polymer member and the metal member.
[0054] Here, the aromatic vinyl unit is a structural unit corresponding to a unit derived from an aromatic vinyl compound as a monomer. The aromatic vinyl compound means an aromatic compound substituted with at least a vinyl group, and is not included in the conjugated diene compound. Examples of aromatic vinyl compounds include styrene; methylstyrenes such as α-methylstyrene, o-methylstyrene (2-methylstyrene), m-methylstyrene (3-methylstyrene), and p-methylstyrene (4-methylstyrene); o,p-dimethylstyrene; and ethylstyrenes such as o-ethylstyrene, m-ethylstyrene, and p-ethylstyrene. The aromatic vinyl unit in the modified copolymer preferably contains an α-methylstyrene unit, an o-methylstyrene unit, an m-methylstyrene unit, or a p-methylstyrene unit, from the viewpoint of facilitating the introduction of a modifying group and improving manufacturability. The aromatic vinyl unit may be one type alone or a combination of two or more types. However, from the same viewpoint as above, it is more preferable that the aromatic vinyl unit in the modified copolymer is composed of only a p-methylstyrene unit.
[0055] The proportion of aromatic vinyl units in the modified copolymer is preferably 0.1 mol% or more. If it is 0.1 mol% or more, the effect of improving the fracture resistance of the modified copolymer can be sufficiently obtained. From the same viewpoint, the proportion of aromatic vinyl units in the modified copolymer is more preferably 0.3 mol% or more, and even more preferably 0.5 mol% or more. In addition, from the viewpoint of sufficiently obtaining the effects exerted by the conjugated diene unit and the non-conjugated olefin unit, the proportion of aromatic vinyl units in the modified copolymer is more preferably 20 mol% or less, even more preferably 10 mol% or less, and particularly preferably 5 mol% or less.
[0056] The modified copolymer preferably has a weight average molecular weight (Mw) of 10,000 or more and 10,000,000 or less in terms of polystyrene. When the modified copolymer has an Mw of 10,000 or more, it is possible to ensure sufficient mechanical strength, and when the modified copolymer has an Mw of 10,000 or less, it is possible to maintain high workability. From the same viewpoint, the modified copolymer preferably has an Mw of 100,000 or more, more preferably 150,000 or more, more preferably 9,000,000 or less, and even more preferably 8,000,000 or less.
[0057] The modified copolymer preferably has a polystyrene-equivalent number average molecular weight (Mn) of 10,000 or more and 10,000,000 or less. When the modified copolymer has an Mn of 10,000 or more, it is possible to ensure sufficient mechanical strength, and when the modified copolymer has an Mn of 10,000 or less, it is possible to maintain high workability. From the same viewpoint, the modified copolymer preferably has an Mn of 50,000 or more, more preferably 100,000 or more, more preferably 9,000,000 or less, and even more preferably 8,000,000 or less.
[0058] The modified copolymer preferably has a molecular weight distribution [Mw / Mn (weight average molecular weight / number average molecular weight)] of 1.00 or more and 4.00 or less. If the molecular weight distribution of the modified copolymer is 4.00 or less, sufficient homogeneity can be obtained in the physical properties of the modified copolymer. From the same viewpoint, the molecular weight distribution of the modified copolymer is more preferably 3.50 or less, and even more preferably 3.00 or less. In addition, the molecular weight distribution of the modified copolymer is more preferably 1.50 or more, and even more preferably 1.80 or more.
[0059] The weight average molecular weight (Mw), number average molecular weight (Mn) and molecular weight distribution (Mw / Mn) are determined by gel permeation chromatography (GPC) using polystyrene as a standard substance.
[0060] The modified copolymer preferably has a melting point of 30°C or higher, and preferably 180°C or lower, as measured by a differential scanning calorimeter (DSC). If the melting point of the modified copolymer is 30°C or higher, the crystallinity of the modified copolymer is increased, and the crack resistance is further improved. If the melting point is 180°C or lower, there is no need to excessively increase the heating temperature during heating, and workability is further improved. From the same viewpoint, the melting point of the modified copolymer is more preferably 140°C or lower. If the copolymer has two or more melting points, the highest melting point is used.
[0061] The modified copolymer has a crystallinity (ΔH / ΔH 0 × 100, also referred to as "crystalline amount") is preferably 0.5% or more, and more preferably 50% or less. If the crystallinity of the modified copolymer is 0.5% or more, the crystallinity due to the non-conjugated olefin unit is sufficiently secured, and the crack resistance is further improved. If the crystallinity of the modified copolymer is 50% or less, the workability during kneading and the like is improved, and the tackiness of the modified copolymer is improved, so that the workability when attaching molded members made from the copolymer to each other is also improved. From the same viewpoint, the crystallinity of the modified copolymer is more preferably 1% or more, more preferably 1.5% or more, and more preferably 45% or less. The degree of crystallinity is the crystalline melting energy (ΔH 0 ) versus the endothermic peak energy (ΔH 1 ) ratio (ΔH 1 / ΔH 0 × 100). The heat of crystalline fusion (crystalline fusion energy) of polyethylene is 293 J / g.
[0062] The main chain of the modified copolymer may have a cyclic structure, or the main chain may be composed of only acyclic structures. When the main chain is composed of only acyclic structures, the crack growth resistance can be further improved. In addition, NMR is mainly used as a measuring means to confirm whether the main chain of the copolymer has a cyclic structure or not. Specifically, peaks derived from the cyclic structures present in the main chain (for example, for three-membered to five-membered rings, 13 When the peak (which appears at 10 to 24 ppm in a C-NMR spectrum chart) is not observed, it indicates that the main chain of the copolymer is composed of only a non-cyclic structure, whereas when the peak is observed, it indicates that the main chain of the copolymer has a cyclic structure.
[0063] The modified copolymer preferably consists of only conjugated diene units and non-conjugated olefin units, or only conjugated diene units, non-conjugated olefin units and aromatic vinyl units, as monomer units. In the modified copolymer, from the viewpoint of more firmly adhering the polymer member and the metal member, it is preferable that the conjugated diene units are butadiene units and the non-conjugated olefin units are ethylene units. As a copolymer having a conjugated diene unit, a non-conjugated olefin unit, and an aromatic vinyl unit, for example, the copolymer described in WO2017 / 065301A1 can be preferably used, and as a copolymer having a conjugated diene unit and a non-conjugated olefin unit, for example, the copolymer described in WO2012 / 105258A1 and WO2012 / 014463A1 can be preferably used.
[0064] Next, the modified group will be described. The modified group in the modified copolymer is not particularly limited as long as it can increase the polarity of the copolymer. However, it is preferable that the modified group in the modified copolymer has at least one selected from oxygen atom, nitrogen atom, silicon atom, sulfur atom, halogen atom and metal atom. In this case, the adhesive effect between the polymer member and the metal member can be further improved.
[0065] The modifying group, particularly the modifying group containing at least one selected from the above oxygen atom, nitrogen atom, silicon atom, sulfur atom, halogen atom and metal atom, can be introduced into the copolymer by using a modifying agent. As the modifying agent, for example, at least one compound selected from the following compounds (a) to (l) can be preferably mentioned.
[0066] The compound (a) is a compound represented by the following general formula (1).
[0067] [ka]
[0068] In the general formula (1), X 11 ~X 15 each independently represents a hydrogen atom or a monovalent functional group containing at least one selected from the group consisting of a halogen atom, a carbonyl group, a thiocarbonyl group, an isocyanate group, a thioisocyanate group, an epoxy group, a thioepoxy group, a halogenated silyl group, a hydrocarbyloxysilyl group, and a sulfonyloxy group, and containing no active proton or onium salt; X 11 ~X 15 At least one of the is not a hydrogen atom. R 11 ~R 15 R each independently represents a single bond or a divalent hydrocarbon group having 1 to 18 carbon atoms. 11 ~R 15Typical examples of the divalent hydrocarbon group include an alkylene group having 1 to 18 carbon atoms, an alkenylene group having 2 to 18 carbon atoms, an arylene group having 6 to 18 carbon atoms, and an aralkylene group having 7 to 18 carbon atoms. Among these, an alkylene group having 1 to 18 carbon atoms is preferred, and an alkylene group having 1 to 10 carbon atoms is more preferred. The alkylene group and alkenylene group may be linear, branched, or cyclic, and linear ones are preferred. Examples of linear alkylene groups include a methylene group, an ethylene group, a trimethylene group, a tetramethylene group, a pentamethylene group, a hexamethylene group, an octamethylene group, and a decamethylene group. Also, X 11 ~X 15 and R 11 ~R 15 In addition, in the general formula (1), X 11 is a hydrogen atom, and R 11 is preferably not simultaneously satisfied as a single bond.
[0069] Typical examples of the modifying agent represented by the general formula (1) include 1-acetylaziridine, 1-propionylaziridine, 1-butylaziridine, 1-isobutylaziridine, 1-valerylaziridine, 1-isovalerylaziridine, 1-pivaloylaziridine, 1-acetyl-2-methylaziridine, 2-methyl-1-propionylaziridine, 1-butyl-2-methylaziridine, 2-methyl-1-isobutylaziridine, 2-methyl-1-valerylaziridine, and 1-isovaleryl-2-methylaziridine. -Methylaziridine, 2-methyl-1-pivaloylaziridine, ethyl 3-(1-aziridinyl)propionate, propyl 3-(1-aziridinyl)propionate, butyl 3-(1-aziridinyl)propionate, ethylene glycol bis[3-(1-aziridinyl)propionate], trimethylolpropane tris[3-(1-aziridinyl)propionate], ethyl 3-(2-methyl-1-aziridinyl)propionate, propyl 3-(2-methyl-1-aziridinyl ) propionate, butyl 3-(2-methyl-1-aziridinyl)propionate, ethylene glycol bis[3-(2-methyl-1-aziridinyl)propionate], trimethylolpropane tris[3-(2-methyl-1-aziridinyl)propionate], neopentyl glycol bis[3-(1-aziridinyl)propionate], neopentyl glycol bis[3-(2-methyl-1-aziridinyl)propionate], di(1-aziridinylcarbonyl)methane, 1,2 -di(1-aziridinylcarbonyl)ethane, 1,3-di(1-aziridinylcarbonyl)propane, 1,4-di(1-aziridinylcarbonyl)butane, 1,5-di(1-aziridinylcarbonyl)pentane, di(2-methyl-1-aziridinylcarbonyl)methane, 1,2-di(2-methyl-1-aziridinylcarbonyl)ethane, 1,3-di(2-methyl-1-aziridinylcarbonyl)propane, 1,4-di(2-methyl-1-aziridinylcarbonyl)butane, and the like. As the compound (a), the above compounds can be used alone or in combination of two or more.
[0070] The compound (b) is a halogenated organometallic compound, a halogenated metal compound, or an organometallic compound represented by the following general formulas (2-1) to (2-5).
[0071] [ka]
[0072] In the general formulas (2-1) to (2-5), R 21 ~R 23 each independently represents a hydrocarbon group having 1 to 20 carbon atoms; R 24 represents a hydrocarbon group having 1 to 20 carbon atoms, which may contain a carbonyl group or an ester group in the side chain; M 21 represents a tin atom, a silicon atom, a germanium atom, or a phosphorus atom; Z 21 indicates a halogen atom, n 21 represents an integer from 0 to 3.
[0073] The halogenated organometallic compounds and halogenated metal compounds represented by the general formulas (2-1) to (2-3) include M 21 When is a tin atom, typical examples include triphenyltin chloride, tributyltin chloride, triisopropyltin chloride, trihexyltin chloride, trioctyltin chloride, diphenyltin dichloride, dibutyltin dichloride, dihexyltin dichloride, dioctyltin dichloride, phenyltin trichloride, butyltin trichloride, octyltin trichloride, tin tetrachloride, and the like.
[0074] M 21 When is a silicon atom, typical examples include triphenylchlorosilane, trihexylchlorosilane, trioctylchlorosilane, tributylchlorosilane, trimethylchlorosilane, diphenyldichlorosilane, dihexyldichlorosilane, dioctyldichlorosilane, dibutyldichlorosilane, dimethyldichlorosilane, methyldichlorosilane, phenylchlorosilane, hexyltridichlorosilane, octyltrichlorosilane, butyltrichlorosilane, methyltrichlorosilane, silicon tetrachloride, and the like.
[0075] M 21 When M' is a germanium atom, typical examples include triphenylgermanium chloride, dibutylgermanium dichloride, diphenylgermanium dichloride, butylgermanium trichloride, germanium tetrachloride, etc. Furthermore, when M' in formula (V) is a phosphorus atom, examples of the component (b) include phosphorus trichloride, etc.
[0076] Examples of the compound (b) include organometallic compounds represented by the above general formula (2-4) containing an ester group in the molecule, and organometallic compounds represented by the above general formula (2-5) containing a carbonyl group in the molecule. As the compound (b), the above compounds can be used alone or in combination of two or more.
[0077] Compound (c) is a heterocumulene compound, and contains Y in the molecule. 01 =C=Y 02 Bond (where Y 01 represents a carbon atom, an oxygen atom, a nitrogen atom, or a sulfur atom; Y 02 represents an oxygen atom, a nitrogen atom, or a sulfur atom.
[0078] Compound (c) is Y 01 is a carbon atom and Y 02 When Y is an oxygen atom, it is a ketene compound. 01 is a carbon atom and Y 02 When Y is a sulfur atom, it is a thioketene compound. 01 is a nitrogen atom, and Y 02 When Y is an oxygen atom, it is an isocyanate compound. 01 is a nitrogen atom, and Y 02 When Y is a sulfur atom, it is a thioisocyanate compound. 01 and Y 02 When both are nitrogen atoms, the compound is a carbodiimide compound, and Y 01 and Y 02 When both are oxygen atoms, it is carbon dioxide, and Y 01 is an oxygen atom, Y02 If Y is a sulfur atom, it is a carbonyl sulfide. 01 and Y 02 When both are sulfur atoms, it is carbon disulfide. 01 and Y 02 is not limited to the above combinations.
[0079] Typical examples of the ketene compound include ethyl ketene, butyl ketene, phenyl ketene, and toluyl ketene. Typical examples of the thioketene compound include ethylene thioketene, butyl thioketene, phenyl thioketene, and toluyl thioketene. Typical examples of the isocyanate compound include phenyl isocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, diphenylmethane diisocyanate, polymeric diphenylmethane diisocyanate, and hexamethylene diisocyanate. Typical examples of the thioisocyanate compound include phenyl thioisocyanate, 2,4-tolylene dithioisocyanate, and hexamethylene dithioisocyanate. Typical examples of the carbodiimide compound include N,N'-diphenylcarbodiimide, N,N'-ethylcarbodiimide, and the like. As the compound (c), the above compounds can be used alone or in combination of two or more.
[0080] Compound (d) is a three-membered heterocyclic compound having a bond represented by the following general formula (3).
[0081] [ka]
[0082] In the general formula (3), Y 31 represents an oxygen atom or a sulfur atom. Compound (d) is Y 31When is an oxygen atom, it is an epoxy compound, and when is a sulfur atom, it is a thiirane compound. Here, typical examples of epoxy compounds include ethylene oxide, propylene oxide, cyclohexene oxide, styrene oxide, epoxidized soybean oil, and epoxidized natural rubber. Typical examples of thiirane compounds include thiirane, methylthiirane, and phenylthiirane. As the compound (d), the above compounds can be used alone or in combination of two or more.
[0083] Compound (e) is a halogenated isocyano compound. Examples of the halogenated isocyano compound include >N=CX 01 Join(X 01 is a halogen atom.
[0084] Typical examples of halogenated isocyano compounds include 2-amino-6-chloropyridine, 2,5-dibromopyridine, 4-chloro-2-phenylquinazoline, 2,4,5-tribromoimidazole, 3,6-dichloro-4-methylpyridazine, 3,4,5-trichloropyridazine, 4-amino-6-chloro-2-mercaptopyrimidine, 2-amino-4-chloro-6-methylpyrimidine, 2-amino-4,6-dichloropyrimidine, 6-chloro-2,4-dimethoxypyrimidine, 2-chloropyrimidine, imidine, 2,4-dichloro-6-methylpyrimidine, 4,6-dichloro-2-(methylthio)pyrimidine, 2,4,5,6-tetrachloropyrimidine, 2,4,6-trichloropyrimidine, 2-amino-6-chloropyrazine, 2,6-dichloropyrazine, 2,4-bis(methylthio)-6-chloro-1,3,5-triazine, 2,4,6-trichloro-1,3,5-triazine, 2-bromo-5-nitrothiazole, 2-chlorobenzothiazole, and 2-chlorobenzoxazole. As the compound (e), the above compounds can be used alone or in combination of two or more.
[0085] The compound (f) is a carboxylic acid, an acid halide, an ester compound, a carbonate ester, or an acid anhydride represented by the following general formulas (4-1) to (4-6).
[0086] [ka]
[0087] In general formulas (4-1) to (4-6), R 41 ~R 49 each independently represents a hydrocarbon group having 1 to 50 carbon atoms; Z 41 is a halogen atom, n 41 represents an integer from 1 to 5.
[0088] Typical examples of the carboxylic acid represented by the general formula (4-1) include acetic acid, stearic acid, adipic acid, maleic acid, benzoic acid, acrylic acid, methacrylic acid, phthalic acid, isophthalic acid, terephthalic acid, trimellitic acid, pyromellitic acid, mellitic acid, polymethacrylic acid ester compounds, and total or partial hydrolysates of polyacrylic acid compounds.
[0089] Typical examples of the acid halide of general formula (4-2) include acetic acid chloride, propionic acid chloride, butanoic acid chloride, isobutanoic acid chloride, octanoic acid chloride, acrylic acid chloride, benzoic acid chloride, stearic acid chloride, phthalic acid chloride, maleic acid chloride, oxalic acid chloride, acetyl iodide, benzoyl iodide, acetyl fluoride, and benzoyl fluoride.
[0090] Typical examples of the ester compound represented by the general formula (4-3) include ethyl acetate, ethyl stearate, diethyl adipate, diethyl maleate, methyl benzoate, ethyl acrylate, ethyl methacrylate, diethyl phthalate, dimethyl terephthalate, tributyl trimellitate, tetraoctyl pyromellitate, hexaethyl melliticate, phenyl acetate, polymethyl methacrylate, polyethyl acrylate, and polyisobutyl acrylate. Examples of the carbonate compound represented by the general formula (4-4) include dimethyl carbonate, diethyl carbonate, dipropyl carbonate, dihexyl carbonate, and diphenyl carbonate.
[0091] Examples of the acid anhydride include intermolecular acid anhydrides represented by the general formula (4-5), such as acetic anhydride, propionic anhydride, isobutyric anhydride, isovaleric anhydride, heptanoic anhydride, benzoic anhydride, and cinnamic anhydride; and acid anhydrides represented by the general formula (4-6), such as succinic anhydride, methylsuccinic anhydride, maleic anhydride, glutaric anhydride, citraconic anhydride, phthalic anhydride, and styrene-maleic anhydride copolymer. As the compound (f), the above compounds can be used alone or in combination of two or more.
[0092] The compounds listed as the compound (f) may contain aprotic polar groups such as ether groups, tertiary amino groups, etc., within the scope of the present invention. In addition, the compound (f) may contain compounds containing free alcohol groups or phenol groups as impurities. As the compound (f), the above compounds can be used either individually or in combination of two or more.
[0093] The compound (g) is a metal salt of a carboxylic acid represented by the following general formulas (5-1) to (5-3).
[0094] [ka]
[0095] In general formulas (5-1) to (5-3), R 51 ~R 57 each independently represents a hydrocarbon group having 1 to 20 carbon atoms; M 51 represents a tin atom, a silicon atom, or a germanium atom; n 51 represents an integer from 0 to 3, and n 52 represents an integer of 0 or 1.
[0096] Typical examples of the compound (g) represented by the general formula (5-1) include triphenyltin laurate, triphenyltin-2-ethylhexatate, triphenyltin naphthate, triphenyltin acetate, triphenyltin acrylate, tri-n-butyltin laurate, tri-n-butyltin-2-ethylhexatate, tri-n-butyltin naphthate, tri-n-butyltin acetate, tri-n-butyltin acrylate, tri-t-butyltin laurate, tri-t-butyltin-2-ethylhexatate, tri-t-butyltin naphthate, t-butyltin acetate, tri-t-butyltin acrylate, triisobutyltin laurate, triisobutyltin-2-ethylhexatate, triisobutyltin naphthate, triisobutyltin acetate, triisobutyltin acrylate, triisopropyltin laurate, triisopropyltin-2-ethylhexatate, triisopropyltin naphthate, triisopropyltin acetate, triisopropyltin acrylate, trihexyltin laurate, trihexyltin-2-ethylhexatate, trihexyltin tin acetate, trihexyl tin acrylate, trioctyl tin laurate, trioctyl tin 2-ethylhexate, trioctyl tin naphthate, trioctyl tin acetate, trioctyl tin acrylate, tri-2-ethylhexyl tin laurate, tri-2-ethylhexyl tin 2-ethylhexate, tri-2-ethylhexyl tin naphthate, tri-2-ethylhexyl tin acetate, tri-2-ethylhexyl tin acrylate, tristearyl tin laurate, tristearyl tin 2-ethylhexate, tristearyl Lyltin naphthate, tristearyltin acetate, tristearyltin acrylate, tribenzyltin laurate, tribenzyltin-2-ethylhexatate, tribenzyltin naphthate, tribenzyltin acetate, tribenzyltin acrylate, diphenyltin dilaurate, diphenyltin-2-ethylhexatate, diphenyltin distearate, diphenyltin dinaphthate, diphenyltin diacetate, diphenyltin diacrylate, di-n-butyltin dilaurate, di-n-butyltin di-2-ethylhexatate,Di-n-butyltin distearate, di-n-butyltin dinaphthate, di-n-butyltin diacetate, di-n-butyltin diacrylate, di-t-butyltin dilaurate, di-t-butyltin di-2-ethylhexatate, di-t-butyltin distearate, di-t-butyltin dinaphthate, di-t-butyltin diacetate, di-t-butyltin diacrylate, diisobutyltin dilaurate, diisobutyltin di-2-ethylhexatate, diisobutyltin distearate, diisobutyltin dinaphthate, diisobutyltin di acetate, diisobutyltin diacrylate, diisopropyltin dilaurate, diisopropyltin 2-ethylhexate, diisopropyltin distearate, diisopropyltin dinaphthate, diisopropyltin diacetate, diisopropyltin diacrylate, dihexyltin dilaurate, dihexyltin di-2-ethylhexate, dihexyltin distearate, dihexyltin dinaphthate, dihexyltin diacetate, dihexyltin diacrylate, di-2-ethylhexyltin dilaurate, di-2-ethylhexyltin Dioctyltin 2-ethylhexate, di-2-ethylhexyltin distearate, di-2-ethylhexyltin dinaphthate, di-2-ethylhexyltin diacetate, di-2-ethylhexyltin diacrylate, dioctyltin dilaurate, dioctyltin di-2-ethylhexate, dioctyltin distearate, dioctyltin dinaphthate, dioctyltin diacetate, dioctyltin diacrylate, distearyltin dilaurate, distearyltin di-2-ethylhexate, distearyltin distearate, distearyltin tin dinaphthate, distearyltin diacetate, distearyltin diacrylate, dibenzyltin dilaurate, dibenzyltin di-2-ethylhexatate, dibenzyltin distearate, dibenzyltin dinaphthate, dibenzyltin diacetate, dibenzyltin diacrylate, phenyltin trilaurate, phenyltin tri-2-ethylhexatate, phenyltin trinaphthate, phenyltin triacetate, phenyltin triacrylate, n-butyltin trilaurate, n-butyltin tri-2-ethylhexatate,n-butyltin trinaphthate, n-butyltin triacetate, n-butyltin triacrylate, t-butyltin trilaurate, t-butyltin tri-2-ethylhexatate, t-butyltin trinaphthate, t-butyltin triacetate, t-butyltin triacrylate, isobutyltin trilaurate, isobutyltin tri-2-ethylhexatate, isobutyltin trinaphthate, isobutyltin triacetate, isobutyltin triacrylate, isopropyltin trilaurate, isopropyltin tri-2-ethylhexatate, isopropyltin trinaphthate, isopropyltin triacetate, isopropyltin triacrylate, hexyltin trilaurate, hexyltin tri-2-ethylhexatate, hexyltin trinaphthate, hexyltin triacetate, Examples of the tin esters include hexyltin triacrylate, octyltin trilaurate, octyltin tri-2-ethylhexatate, octyltin trinaphthate, octyltin triacetate, octyltin triacrylate, 2-ethylhexyltin trilaurate, 2-ethylhexyltin tri-2-ethylhexatate, 2-ethylhexyltin trinaphthate, 2-ethylhexyltin triacetate, 2-ethylhexyltin triacrylate, stearyltin trilaurate, stearyltin tri-2-ethylhexatate, stearyltin trinaphthate, stearyltin triacetate, stearyltin triacrylate, benzyltin trilaurate, benzyltin tri-2-ethylhexatate, benzyltin trinaphthate, benzyltin triacetate, and benzyltin triacrylate.
[0097] Typical examples of the compound (g) represented by the general formula (5-2) include diphenyltin bismethyl malate, diphenyltin bis-2-ethylhexate, diphenyltin bisoctyl malate, diphenyltin bisoctyl malate, diphenyltin bisbenzyl malate, di-n-butyltin bismethyl malate, di-n-butyltin bis-2-ethylhexate, di-n-butyltin bisoctyl malate, di-n-butyltin bisbenzyl malate, di-t-butyltin bismethyl malate, di-t-butyltin bis-2-ethylhexate, tin, di-t-butyltin bisoctyl malate, di-t-butyltin bisbenzyl malate, diisobutyltin bismethyl malate, diisobutyltin bis-2-ethylhexatate, diisobutyltin bisoctyl malate, diisobutyltin bisbenzyl malate, diisopropyltin bismethyl malate, diisopropyltin bis-2-ethylhexatate, diisopropyltin bisoctyl malate, diisopropyltin bisbenzyl malate, dihexyltin bismethyl malate, dihexyltin bis-2-ethylhexatate, dihexyltin Bisoctyl malate, dihexyltin bisbenzyl malate, di-2-ethylhexyltin bismethyl malate, di-2-ethylhexyltin bis-2-ethylhexate, di-2-ethylhexyltin bisoctyl malate, di-2-ethylhexyltin bisbenzyl malate, dioctyltin bismethyl malate, dioctyltin bis-2-ethylhexate, dioctyltin bisoctyl malate, dioctyltin bisbenzyl malate, distearyltin bismethyl malate, distearyltin bis-2-ethylhexate, distearyl Tin bisoctyl malate, distearyl tin bisbenzyl malate, dibenzyl tin bismethyl malate, dibenzyl tin bis-2-ethylhexatate, dibenzyl tin bisoctyl malate, dibenzyl tin bisbenzyl malate, diphenyl tin bismethyl agitate, diphenyl tin bis-2-ethylhexatate, diphenyl tin bisoctyl agitate, diphenyl tin bisbenzyl agitate, di-n-butyl tin bismethyl agitate, di-n-butyl tin bis-2-ethylhexatate, di-n-butyl tin bisoctyl agitate,Di-n-butyltin bisbenzyl agitate, di-t-butyltin bismethyl agitate, di-t-butyltin bis-2-ethylhexatate, di-t-butyltin bisoctyl agitate, di-t-butyltin bisbenzyl agitate, diisobutyltin bismethyl agitate, diisobutyltin bis-2-ethylhexatate, diisobutyltin bisoctyl agitate, diisobutyltin bisbenzyl agitate, diisopropyltin bismethyl agitate, diisopropyltin bis-2-ethylhexatate, diisopropyltin bisoctyl agitate, diisopropyltin bisbenzyl agitate, dihexyltin bismethyl agitate, dihexyltin bis-2-ethylhexatate, dihexyltin bismethyl agitate, dihexyltin bisbenzyl agitate di-2-ethylhexyltin bismethyl aditate, di-2-ethylhexyltin bis-2-ethylhexate, di-2-ethylhexyltin bisoctyl aditate, di-2-ethylhexyltin bisbenzyl aditate, dioctyltin bismethyl aditate, dioctyltin bis-2-ethylhexate, dioctyltin bisoctyl aditate, dioctyltin bisbenzyl aditate, distearyltin bismethyl aditate, distearyltin bis-2-ethylhexate, distearyltin bisoctyl aditate, distearyltin bisbenzyl aditate, dibenzyltin bismethyl aditate, dibenzyltin bis-2-ethylhexate, dibenzyltin bisoctyl aditate, dibenzyltin bisbenzyl aditate, and the like.
[0098] Typical examples of the compound (g) represented by the general formula (5-3) include diphenyl tinmarate, di-n-butyl tinmarate, di-t-butyl tinmarate, diisobutyl tinmarate, diisopropyl tinmarate, dihexyl tinmarate, di-2-ethylhexyl tinmarate, dioctyl tinmarate, distearyl tinmarate, dibenzyl tinmarate, diphenyl tin agitate, di-n-butyl tin agitate, di-t-butyl tin agitate, diisobutyl tin agitate, diisopropyl tin agitate, dihexyl tin diacetate, di-2-ethylhexyl tin agitate, dioctyl tin agitate, distearyl tin agitate, and dibenzyl tin agitate. As the compound (g), the above compounds can be used alone or in combination of two or more.
[0099] Compound (h) is an N-substituted aminoketone, an N-substituted aminothioketone, an N-substituted aminoaldehyde, an N-substituted aminothioaldehyde or an N-substituted aminoketone having -C-(=M 01 )-N<bond(M 01 represents an oxygen atom or a sulfur atom.
[0100] Typical examples of compound (h) include N-substituted aminoketones and corresponding N-aminothioketones such as 4-dimethylaminoacetophenone, 4-diethylaminoacetophenone, 1,3-bis(diphenylamino)-2-propanone, 1,7-bis(methylethylamino)-4-heptanone, 4-dimethylaminobenzophenone, 4-diethylaminobenzophenone, 4-di-t-butylaminobenzophenone, 4-diphenylaminobenzophenone, 4,4'-bis(dimethylamino)benzophenone, 4,4'-bis(diethylamino)benzophenone, and 4,4'-bis(diphenylamino)benzophenone; N-substituted aminoaldehydes and corresponding N-substituted aminothioaldehydes such as 4-dimethylaminobenzaldehyde, 4-diphenylaminobenzaldehyde, and 4-divinylaminobenzaldehyde; and N-methyl-β-propionamide. Lactam, N-phenyl-β-propiolactam, N-methyl-2-pyrrolidone, N-phenyl-2-pyrrolidone, Nt-butyl-2-pyrrolidone, N-phenyl-5-methyl-2-pyrrolidone, N-methyl-2-piperidone, N-phenyl-2-piperidone, N-methyl-ε-caprolactam, N-phenyl-ε-caprolactam, N-methyl-ω-caprolactam, N-phenyl-ω-caprolactam, N-methyl-ω N-substituted lactams such as N-laurilolactam and N-vinyl-ω-laurilolactam and the corresponding N-substituted thiolactams, as well as N-substituted cyclic ureas such as 1,3-dimethylethyleneurea, 1,3-divinylethyleneurea, 1,3-diethyl-2-imidazolidinone, 1-methyl-3-ethyl-2-imidazolidinone, 1,3-dimethyl-2-imidazolidinone and the corresponding N-substituted cyclic thioureas, 01 )-N<bond(M 01 represents an oxygen atom or a sulfur atom; As the compound (h), the above compounds can be used alone or in combination of two or more.
[0101] Compound (i) is a compound having an N≡C bond. There are no particular limitations on the compound (i) so long as it is a compound having an N≡C bond, and examples thereof include organic cyano compounds represented by the general formula R-CN, such as 2-cyanopyridine, 3-cyanopyridine, and acrylonitrile. As the compound (i), the above compounds can be used alone or in combination of two or more.
[0102] Compound (j) is a compound having a phosphate residue represented by the following general formula (6).
[0103] [ka]
[0104] In the general formula (6), R 61 and R 62 each independently represents an alkyl group having 1 to 20 carbon atoms, a monovalent alicyclic hydrocarbon group having 3 to 20 carbon atoms, a monovalent aromatic hydrocarbon group having 6 to 20 carbon atoms, or a hydrogen atom.
[0105] A typical example of the phosphate residue represented by general formula (6) is a phosphate residue represented by the following general formula (7).
[0106] [ka]
[0107] As the compound (j), the above compounds can be used alone or in combination of two or more.
[0108] Compound (k) is an electrophilic compound containing at least one atom selected from oxygen, nitrogen, and silicon atoms. Preferred examples of the electrophilic compound include electrophilic compounds such as ketones, aldehydes, and epoxies, such as benzaldehyde, benzophenone, 4,4'-bis(diethylamino)benzophenone, 3-glycidoxypropyltrimethoxysilane, and allyl glycidyl ether. As the compound (k), the above compounds can be used alone or in combination of two or more.
[0109] Compound (l) is a vinyl compound having a vinyl group containing at least one atom selected from oxygen, nitrogen and silicon atoms. Preferred examples of the vinyl compound include vinyl phosphate, vinyl acetate ether, vinyl pivaloyl, vinyl trimethylsilane, triethoxyvinylsilane, etc. As the compound (l), the above compounds can be used alone or in combination of two or more.
[0110] Another method for producing a modified copolymer includes the steps of: (i) adding an alkali metal compound to an unmodified copolymer (a copolymer having conjugated diene units and non-conjugated olefin units, but no butylene units); and (ii) reacting the product obtained in step (i) with a specific modifying agent to introduce a modifying group into the copolymer.
[0111] Examples of the alkali metal atom (M) of the alkali metal compound added in the above step (i) include Li, Na, K, Rb, and Cs. Examples of the alkali metal compound include organic alkali metal compounds and organic alkaline earth metal compounds. The alkali metal compound is preferably an organic alkali metal compound.
[0112] Organoalkali metal compounds include, for example, hydrocarbyl lithium and lithium amide compounds.
[0113] The hydrocarbyllithium is preferably, for example, one having a hydrocarbyl group having 2 to 20 carbon atoms, and examples thereof include ethyllithium, n-propyllithium, isopropyllithium, n-butyllithium, isobutyllithium, sec-butyllithium, tert-butyllithium, tert-octyllithium, n-decyllithium, phenyllithium, 2-naphthyllithium, 2-butylphenyllithium, 4-phenylbutyllithium, cyclohexyllithium, cyclopentyllithium, and a reaction product of diisopropenylbenzene and butyllithium.
[0114] Examples of the lithium amide compound include lithium hexamethylene imide, lithium pyrrolidide, lithium piperidide, lithium heptamethylene imide, lithium dodecamethylene imide, lithium dimethylamide, lithium diethylamide, lithium dibutylamide, lithium dipropylamide, lithium diheptylamide, lithium dihexylamide, lithium dioctylamide, lithium di-2-ethylhexylamide, lithium didecylamide, lithium-N-methylpiberazide, lithium ethylpropylamide, lithium ethylbutylamide, lithium ethylbenzylamide, and lithium methylphenethylamide.
[0115] From the viewpoint of more efficiently introducing the modifying group into the copolymer, the alkali metal compound used in step (i) is preferably sec-butyllithium.
[0116] By adding an alkali metal compound in step (i), an alkali metal atom is introduced into a portion of the polymer main chain of the copolymer other than one end (e.g., in the middle of the polymer main chain) (a hydrogen atom of the hydrocarbon chain is replaced with an alkali metal atom), and the introduced alkali metal atom reacts with the modifying agent to introduce a modifying group.
[0117] In the step (i), the portion into which the alkali metal atom is introduced may be, for example, a tertiary carbon atom at the bonding portion of the styrene unit to the polymer main chain when the copolymer contains a styrene unit as an aromatic vinyl unit. In addition, for example, when the copolymer contains a p-methylstyrene unit as an aromatic vinyl unit, an alkali metal atom is introduced to a tertiary carbon atom at the bonding portion of the p-methylstyrene unit to the polymer main chain and a primary carbon atom of a methyl group at the 4th position. In this case, since the primary carbon atom has a smaller steric hindrance than the tertiary carbon atom, it is considered that the alkali metal atom is preferentially introduced to the primary carbon atom. In addition, when the copolymer does not contain an aromatic vinyl unit, the activity is inferior to that when the copolymer contains an aromatic vinyl unit, but it is considered that the hydrogen atom at the allyl position reacts with the alkali metal atom of the additionally added alkali metal compound, and the alkali metal atom is introduced.
[0118] The modifying agent used in step (ii) includes, for example, carbon dioxide gas, carbon disulfide, aldehyde, etc. From the viewpoint of more easily introducing the modifying group, the modifying agent used in step (ii) is preferably carbon dioxide gas.
[0119] When carbon dioxide gas is used as the modifying agent, the modifying group can be -C(=O)OM (M is an alkali metal atom). When carbon disulfide is used as the modifying agent, the modifying group can be -C(=S)SM (M is an alkali metal atom). When an aldehyde such as acetaldehyde is used as the modifying agent, the modifying group can be -OM (M is an alkali metal atom).
[0120] Further, as another method for producing a modified copolymer, there can be mentioned a method in which any of basic monomers such as conjugated diene compounds, non-conjugated olefin compounds, aromatic vinyl compounds, etc., to which a modifying group has been previously imparted, is used as a monomer and copolymerized.
[0121] From the viewpoint of more firmly adhering the polymer member and the metal member, the modified group in the modified copolymer preferably has at least one of a carbonyl portion (-C(=O)-) and a thiocarbonyl portion (-C(=S)-). From the same viewpoint, the modified group in the modified copolymer more preferably has at least one of an ester bond (-C(=O)O-) and a dithioester bond (-C(=S)S-). Examples of such modified groups include groups corresponding to carboxylates, i.e., -C(=O)OR (R is any group), and groups corresponding to dithiocarboxylates, i.e., -C(=S)SR (R is any group), and in particular, groups corresponding to metal carboxylates, i.e., -C(=O)OM (M is an alkali metal atom), and groups corresponding to metal dithiocarboxylates, i.e., -C(=S)SM (M is an alkali metal atom). Such modified copolymers can be appropriately prepared, for example, by selecting an appropriate modifier from the above-mentioned compounds (a) to (l), employing a method including the above-mentioned steps (i) and (ii), or the like.
[0122] The proportion of the modifying group in the modified copolymer is preferably 0.1% by mass or more and 10.0% by mass or less. If the proportion of the modifying group is 0.1% by mass or more, the polymer member and the metal member can be more firmly bonded. If the proportion of the modifying group is 10.0% by mass or less, gelation due to the reaction between the modifying groups can be sufficiently suppressed. From the same viewpoint, the proportion of the modifying group in the modified copolymer is more preferably 0.3% by mass or more, even more preferably 0.5% by mass or more, even more preferably 1.0% by mass or more, and more preferably 7.0% by mass or less, even more preferably 5.0% by mass or less, and even more preferably 3.0% by mass or less. The proportion of modifying groups in the modified copolymer can be increased, for example, by increasing the amount of modifier added, increasing the amount of the alkali metal compound added, increasing the amount of aromatic vinyl units in the copolymer, or increasing the amount of methylstyrene-based units (α-methylstyrene units, o-methylstyrene units, m-methylstyrene units, or p-methylstyrene units) as aromatic vinyl units. The ratio of the modifying group in the modified copolymer is 1 It can be calculated from the H-NMR spectrum.
[0123] In the composite of this embodiment, it is preferable that the adhesive layer further contains a peroxide in addition to the modified copolymer. In this case, since the softening of the modified copolymer caused by the presence of olefin units is significantly suppressed, even if the composite is placed in a high-temperature environment, the adhesive layer is prevented from self-rupturing or self-peeling, and stronger adhesion between the polymer member and the metal member can be maintained. When the peroxide is used, it is preferable to blend the peroxide with the modified copolymer in advance and knead them according to a conventional method. In addition, in the adhesive layer, the peroxide may form a crosslinked structure in the modified copolymer.
[0124] Examples of peroxides include ketone peroxides, peroxyketals, dialkyl peroxides, hydroperoxides, diacyl peroxides, peroxy esters, and peroxydicarbonates.
[0125] An example of the ketone peroxide is methyl ethyl ketone peroxide.
[0126] Examples of peroxyketals include 1,1-di(t-butylperoxy)cyclohexane, 2,2-di(t-butylperoxy)butane, n-butyl 4,4-di(t-butylperoxy)valerate, ethyl 3,3-di(t-butylperoxy)butyrate, and 1,1-di(t-amylperoxy)cyclohexane.
[0127] Examples of dialkyl peroxides include dicumyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, 1,3-di(2-t-butylperoxyisopropyl)benzene, di-t-butyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexyne-3, and di-t-amyl peroxide.
[0128] Examples of the hydroperoxide include 1,1,3,3-tetramethylbutyl hydroperoxide, t-butyl hydroperoxide, and t-amyl hydroperoxide.
[0129] Examples of the diacyl peroxide include diisononanoyl peroxide, dilauroyl peroxide, and dibenzoyl peroxide.
[0130] Examples of peroxyesters include 3-hydroxy-1,1-dimethylbutyl peroxyneodecanoate, α-cumyl peroxyneodecanoate, 1,1,3,3-tetramethylbutyl peroxyneodecanoate, 1,1,3,3-tetramethylbutyl peroxy-2-ethylhexanoate, t-butyl peroxyneodecanoate, t-butyl peroxyneoheptanoate, t-butyl peroxypivalate, and t-butyl peroxy-2-ethylhexanoate. t-butyl peroxyisobutyrate, t-butyl peroxyacetate, t-butyl peroxyisononanoate, t-butyl peroxybenzoate, t-amyl peroxyneodecanoate, t-amyl peroxypivalate, t-amyl peroxy-2-ethylhexanoate, t-amyl peroxynormal octoate, t-amyl peroxyacetate, t-amyl peroxyisononanoate, and t-amyl peroxybenzoate.
[0131] Examples of peroxydicarbonates include di(2-ethylhexyl) peroxydicarbonate and di(sec-butyl) peroxydicarbonate.
[0132] Among the above, as the peroxide, dialkyl peroxide and hydroperoxide are preferable, and in particular, dicumyl peroxide and 2,5-dimethyl-2,5-di(t-butylperoxy)hexane are more preferable.
[0133] The peroxide preferably has a one-hour half-life temperature higher than the melting point of the modified copolymer. In this case, the peroxide can be effectively prevented from reacting prematurely when kneading with the modified copolymer in advance. The peroxide having such a one-hour half-life temperature can be appropriately selected from the above-mentioned peroxides, taking into consideration the melting point of the modified copolymer to be used.
[0134] The peroxide preferably has a one-hour half-life temperature of 110° C. or higher. In this case, the peroxide can be effectively prevented from reacting prematurely when kneading with the modified copolymer in advance. From the same viewpoint, the one-hour half-life temperature of the peroxide is more preferably 120° C. or higher, and further preferably 125° C. or higher. The peroxide having such a one-hour half-life temperature can be appropriately selected from those described above.
[0135] The content of the peroxide in the adhesive layer is preferably 0.1 parts by mass or more relative to 100 parts by mass of the modified copolymer. In this case, the effect of blending the peroxide can be fully obtained. From the same viewpoint, the content of the peroxide relative to 100 parts by mass of the modified copolymer is more preferably 0.5 parts by mass or more, and even more preferably 1 part by mass or more. In addition, the content of the peroxide relative to 100 parts by mass of the modified copolymer is not particularly limited, and is preferably 5 parts by mass or less.
[0136] <Production of polymer-metal composites> The method for producing the composite of the present embodiment is not particularly limited, and a polymer-metal composite can be produced by arranging the metal member, the adhesive layer, and the polymer member in this order so that they are in contact with each other. In addition, when the polymer member contains a rubber component, a polymer-metal composite can be produced by arranging the metal member, the adhesive layer, and the polymer member (unvulcanized) in this order so that they are in contact with each other, and vulcanizing the polymer-metal composite.
[0137] When vulcanization is performed, the vulcanization temperature can be 120 to 200°C, particularly 130 to 170°C, and the vulcanization time can be 3 minutes to 6 hours. However, when the above-mentioned peroxide is used, the vulcanization temperature is preferably equal to or higher than the one-hour half-life temperature of the peroxide. More specifically, the vulcanization temperature is preferably 140°C or higher, 145°C or higher, or 150°C or higher. In this case, the crosslinking effect (and thus the softening suppression effect) of the peroxide can be effectively exerted during vulcanization.
[0138] In addition, when vulcanization is performed and the above-mentioned peroxide is used, the peroxide may be blended in advance with the modified copolymer and kneaded according to a conventional method. In this case, the kneading temperature is preferably equal to or higher than the melting point of the modified copolymer, and is preferably lower than the one-hour half-life temperature of the peroxide. In this case, kneading is made easier and the premature reaction of the peroxide before vulcanization can be effectively suppressed. The kneading time can be 1 to 10 minutes.
[0139] During kneading, the amount of peroxide to be blended into the modified copolymer is preferably 0.1 parts by mass or more per 100 parts by mass of the modified copolymer. In this case, the effect of blending the peroxide can be fully obtained. From the same viewpoint, the amount of peroxide to be blended into 100 parts by mass of the modified copolymer is more preferably 0.5 parts by mass or more, and even more preferably 1 part by mass or more. In addition, the amount of peroxide to be blended into 100 parts by mass of the modified copolymer is not particularly limited, and is preferably 5 parts by mass or less.
[0140] Furthermore, in the above-mentioned manufacturing method, the metal member and the adhesive layer may be heated and welded together before the polymer member is brought into contact with the adhesive layer. At that time, the welding temperature may be, for example, 100 to 160°C.
[0141] (tire) A tire according to one embodiment of the present invention is characterized in that it comprises the above-mentioned polymer-metal composite, in which the polymer member contains a rubber component. Such a tire has high strength because it uses the above-mentioned polymer-metal composite (rubber-metal composite) in which the polymer member (rubber member) and the metal member are firmly bonded. In one embodiment of a tire, the above-mentioned polymer-metal composite can be preferably applied to a carcass, a belt, a bead core, and the like.
[0142] (Polymer Articles) A polymer article according to one embodiment of the present invention is characterized by comprising the above-mentioned polymer-metal composite. Such a polymer article has high strength because it uses the above-mentioned polymer-metal composite in which the polymer member and the metal member are firmly bonded to each other. Rubber articles (polymer articles having a polymer-metal composite in which the polymer member contains a rubber component) are not particularly limited, and examples thereof include, in addition to tires, conveyor belts, hoses, rubber crawlers, seismic isolation devices, vibration-proof devices, and coated electric wires. The resin article (polymer article having a polymer-metal composite in which the polymer member contains a resin component) is not particularly limited, and examples thereof include resin-coated electric wires. EXAMPLES
[0143] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples and can be modified as appropriate without departing from the gist of the present invention.
[0144] (Preparation of Modified Copolymer A1) Into a thoroughly dried 2000 mL pressure-resistant stainless steel reactor, 16 g of styrene as an aromatic vinyl compound and 364 g of toluene were placed. In a glove box under a nitrogen atmosphere, mono(bis(1,3-tert-butyldimethylsilyl)indenyl)bis(bis(dimethylsilyl)amide) gadolinium complex (1,3-[(t-Bu)Me 2 Si] 2 C 9 H 5 Gd[N(SiHMe 2 ) 2 ] 2 ) 0.025mmol, Trityltetrakis(pentafluorophenyl)borate [Ph 3 CB(C 6 F 5 ) 4 0.025 mmol of 1,000 mmol of toluene and 0.75 mmol of triisobutylaluminum were added to prepare a catalyst solution, which was then added to the pressure-resistant stainless steel reactor and heated to 60°C. Next, ethylene as a non-conjugated olefin compound was added to the pressure-resistant stainless steel reactor at a pressure of 0.6 MPa, and copolymerization was carried out for 61 minutes at 75° C. In addition, 260 g of a toluene solution containing 80 g of 1,3-butadiene as a conjugated diene compound was continuously added at a rate of 4.0 to 7.0 mL / min. Next, 1 mL of 5% by mass of 2,2'-methylene-bis(4-ethyl-6-t-butylphenol) (NS-5) in isopropanol was added to the pressure-resistant stainless steel reactor to stop the reaction. Then, separation was performed using a large amount of methanol and vacuum drying at 50°C to obtain copolymer A0 (before the introduction of the modifying group).
[0145] 20 g of the copolymer and 380 g of cyclohexane were added to a 1 L glass bottle, and the mixture was stirred in a water bath at 80° C. for 2 hours to dissolve the copolymer in cyclohexane. Next, a hexane solution containing 3.4 mmol of sec-butyl lithium and 3.4 mmol of tetramethylethylenediamine were added to the glass bottle, and the mixture was reacted at 80° C. for 1 hour. After the reaction, the glass bottle was removed from the water bath, and carbon dioxide gas (CO 2) was added by bubbling for 1 minute. The mixture was then left to stand overnight at room temperature to complete the modification reaction. Then, separation was performed using a large amount of methanol and vacuum drying was performed at 50°C, and finally, a copolymer A1 having a modified group (-C(=O)OLi) (especially mainly on the tertiary carbon atom of the bond portion with the polymer main chain of the styrene unit) was obtained.
[0146] (Preparation of Modified Copolymer B1) Into a thoroughly dried 2000 mL pressure-resistant stainless steel reactor, 7 g of p-methylstyrene as an aromatic vinyl compound and 373 g of toluene were placed. In a glove box under a nitrogen atmosphere, mono(bis(1,3-tert-butyldimethylsilyl)indenyl)bis(bis(dimethylsilyl)amide) gadolinium complex (1,3-[(t-Bu)Me 2 Si] 2 C 9 H 5 Gd[N(SiHMe 2 ) 2 ] 2 ) 0.025mmol, Trityltetrakis(pentafluorophenyl)borate [Ph 3 CB(C 6 F 5 ) 4 0.025 mmol of 1,000 mmol of toluene and 0.75 mmol of triisobutylaluminum were added to prepare a catalyst solution, which was then added to the pressure-resistant stainless steel reactor and heated to 60°C. Next, ethylene as a non-conjugated olefin compound was added to the pressure-resistant stainless steel reactor at a pressure of 0.6 MPa, and copolymerization was carried out for 117 minutes at 75° C. In addition, 260 g of a toluene solution containing 80 g of 1,3-butadiene as a conjugated diene compound was continuously added at a rate of 2.0 to 4.0 mL / min. Next, 1 mL of 5% by mass of 2,2'-methylene-bis(4-ethyl-6-t-butylphenol) (NS-5) in isopropanol was added to the pressure-resistant stainless steel reactor to stop the reaction. Then, separation was performed using a large amount of methanol and vacuum drying at 50°C to obtain copolymer B0 (before the introduction of the modifying group).
[0147] 20 g of the copolymer and 380 g of cyclohexane were added to a 1 L glass bottle, and the mixture was stirred in a water bath at 80° C. for 2 hours to dissolve the copolymer in cyclohexane. Next, a hexane solution containing 3.4 mmol of sec-butyl lithium and 3.4 mmol of tetramethylethylenediamine were added to the glass bottle, and the mixture was reacted at 80° C. for 1 hour. After the reaction, the glass bottle was removed from the water bath, and carbon dioxide gas (CO 2 ) was added by bubbling for 1 minute. Then, the mixture was left to stand overnight at room temperature to complete the modification reaction. Then, separation was performed using a large amount of methanol and vacuum drying was performed at 50°C, and finally, copolymer B1 having a modified group (-C(=O)OLi) (especially mainly at the methyl moiety at the 4-position of the p-methylstyrene unit) was obtained.
[0148] The copolymer was analyzed by gel permeation chromatography (GPC: HLC-8220GPC / HT manufactured by Tosoh Corporation, column: GMH manufactured by Tosoh Corporation). HR Using a -H(S)HT x 2, detector: differential refractometer (RI), the weight average molecular weight (Mw), number average molecular weight (Mn), and molecular weight distribution (Mw / Mn) in terms of polystyrene were determined using monodisperse polystyrene as a standard. The measurement temperature was 140°C. The results are shown in Table 1.
[0149] In addition, a differential scanning calorimeter (DSC, manufactured by TA Instruments Japan, "DSCQ2000") was used to heat the copolymer from -150°C to 150°C at a rate of 10°C / min, and the endothermic peak energy (ΔH 1 ) and the endothermic peak energy at 100℃ to 150℃ (ΔH 2 The crystalline melting energy (ΔH 0 ) value, the crystalline melting energy (ΔH 0 ) to the endothermic peak energy of the copolymer ((ΔH 1 / ΔH 0 ) × 100, (ΔH 2 / ΔH 0)×100), the crystallinity of the copolymer at 0°C to 100°C and at 100°C to 150°C were calculated. The results are shown in Table 1. Note that the above crystallinity is the crystallinity in the range of 0 to 150°C. For example, when the crystallinity is separately indicated for 0 to 100°C and for 100 to 150°C, the sum of these is the crystallinity at 0 to 150°C.
[0150] The proportions (mol%) of the conjugated diene units (1,3-butadiene units), non-conjugated olefins (ethylene units), and aromatic vinyl units (styrene units, p-methylstyrene units) in the copolymer are 1 The results were calculated from the integral ratio of each peak in the H-NMR spectrum (100°C, d-tetrachloroethane standard: 6 ppm). The results are shown in Table 1.
[0151] The ratio of the modifying group in the copolymer is 1 The results were calculated from the H-NMR spectrum and are shown in Table 1.
[0152] In addition, regarding the above copolymer, 13 The C-NMR spectrum was measured. 13 No peaks were observed in the range of 10 to 24 ppm in the C-NMR spectrum chart, confirming that the main chain of each of the synthesized copolymers was composed solely of acyclic structures.
[0153] [Table 1]
[0154] (Preparation of polymer components) A polymer composition (rubber composition) was prepared by kneading using a Banbury mixer according to the compounding recipe shown in Table 2. The obtained rubber composition was molded into a shape of 150 mm × 150 mm × thickness of 4 mm to prepare a polymer member (rubber member) (unvulcanized).
[0155] [Table 2]
[0156] *1 Antioxidant A: N-phenyl-N-isopropyl-p-phenylenediamine *2 Vulcanization accelerator A: Nt-butyl-2-benzothiazolyl sulfenamide *3 Vulcanization accelerator B: Diphenyl guanidine
[0157] (Preparation of polymer-metal composites) In each example, one of the copolymers (modified copolymer A1 or modified copolymer B1) shown in Table 1 was placed to a thickness of 0.3 mm directly on a metal member (made of brass) processed to 100 mm × 25 mm × thickness 1 mm to obtain a metal member-copolymer (adhesive layer) laminate. The obtained laminate was sandwiched between two flat molds with a thickness of 1.8 mm, welded at 130°C for 10 minutes, and then cooled for 10 minutes. Next, the welded laminate was placed at room temperature on a sufficiently large flat mold having a thickness of 3 mm, with the metal member facing the mold, at intervals. Next, the above-mentioned polymer member (unvulcanized) was placed so as to cover the above-mentioned laminates and to be in contact with the copolymer. Then, while pressing with another flat mold, vulcanization was performed at 160°C for 20 minutes, and then cooled for 10 minutes. In this way, a polymer-metal composite in which the polymer member and the metal member were bonded via an adhesive layer (modified copolymer A1 or modified copolymer B1) was produced.
[0158] (Evaluation of Adhesion) The adhesive strength (N / 25 mm width) of the polymer-metal composites prepared as described above was measured in accordance with Japanese Industrial Standard JIS K 6854-2. As a result, the adhesive strength was 30 N / 25 mm for the polymer-metal composite using copolymer A1 as the adhesive layer, and 90 N / 25 mm for the polymer-metal composite using copolymer B1 as the adhesive layer. From these results, it is understood that the use of a specific copolymer having a modifying group, such as modified copolymer A1 and modified copolymer B1, results in adhesion between the polymer member and the metal member. In contrast, when a copolymer without a modifying group is used, it is considered that interfacial peeling occurs between the polymer member and the metal member, and the desired adhesion is not achieved.
[0159] Here, in modified copolymer A1, at least modified group is introduced into styrene group, while in modified copolymer B1, at least modified group is introduced into p-methylstyrene group. And, as the above result shows, modified copolymer B1 exhibits higher adhesiveness than modified copolymer A1. This is presumably because the efficiency of modifying group introduction of p-methylstyrene is higher than that of styrene.
[0160] In the above embodiment, a flat metal member and a flat polymer member are bonded together, but the present invention is not limited to this and can also be applied to, for example, bonding a cord-shaped metal member, such as a steel cord, to a coating rubber that covers the metal member. [Industrial Applicability]
[0161] According to the present invention, it is possible to provide a polymer-metal composite in which a polymer member and a metal member are firmly bonded to each other. Furthermore, according to the present invention, it is possible to provide high-strength tires and polymer articles using such a polymer-metal composite.
Claims
1. A polymer-metal composite in which a polymer member containing a rubber component and / or a resin component and a metal member are bonded via an adhesive layer, The adhesive layer contains a modified copolymer having a conjugated diene unit and a non-conjugated olefin unit, having no butylene unit, and having a modifying group; the modifying group has at least one selected from the group consisting of an oxygen atom, a nitrogen atom, a silicon atom, a sulfur atom, a halogen atom, and a metal atom, The adhesive layer has a content of the modified copolymer of 95% by mass or more, The modified copolymer does not contain a hydrogenated styrene-butadiene copolymer.
2. 2. The polymer-metal composite of claim 1, wherein the modified copolymer further comprises an aromatic vinyl unit.
3. 3. The polymer-metal composite of claim 2, wherein the aromatic vinyl units comprise α-methylstyrene units, o-methylstyrene units, m-methylstyrene units, or p-methylstyrene units.
4. 4. The polymer-metal composite of claim 3, wherein the aromatic vinyl units consist solely of p-methylstyrene units.
5. 5. The polymer-metal composite of claim 1, wherein the modifying group comprises at least one of a carbonyl moiety (-C(=O)-) and a thiocarbonyl moiety (-C(=S)-).
6. 6. The polymer-metal composite according to claim 5, wherein the modifying group comprises at least one of an ester bond (-C(=O)O-) and a dithioester bond (-C(=S)S-).
7. The polymer-metal composite according to any one of claims 1 to 6, wherein the proportion of the modifying group in the modified copolymer is 0.1% by mass or more and 10.0% by mass or less.
8. 8. The polymer-metal composite according to claim 1, wherein the proportion of conjugated diene units in the modified copolymer is 10 mol % or more.
9. 9. The polymer-metal composite according to claim 8, wherein the proportion of conjugated diene units in the modified copolymer is 25 mol % or more.
10. 10. The polymer-metal composite according to claim 1, wherein in said modified copolymer, the conjugated diene unit is a butadiene unit and the non-conjugated olefin unit is an ethylene unit.
11. The polymer-metal composite of any one of claims 1 to 10, wherein the polymer member is substantially free of cobalt-containing compounds.
12. The polymer-metal composite according to any one of claims 1 to 11, wherein the polymer member has a sulfur content of less than 3 parts by mass per 100 parts by mass of a rubber component and / or a resin component.
13. The polymer-metal composite according to any one of claims 1 to 12, wherein the adhesive layer further comprises a peroxide.
14. 14. The polymer-metal composite of claim 13, wherein the one-hour half-life temperature of the peroxide is higher than the melting point of the modified copolymer.
15. The polymer-metal composite according to claim 13 or 14, wherein the peroxide has a one-hour half-life temperature of 110° C. or higher.
16. A tire comprising the polymer-metal composite according to any one of claims 1 to 15, wherein the polymer member comprises a rubber component.
17. A polymer article comprising the polymer-metal composite according to any one of claims 1 to 15.
Citation Information
Patent Citations
adhesive rubber composition
JP1994506004A
Use of maleated styrene-ethylene-butylene-styrene triblock polymer for improving adhesive properties
JP1996225660A
Tire consisting of thermo-reversible crosslinked polymer composition
JP2001097002A
Epoxy resin composition and insulating adhesive for polyimide
JP2013170214A
Polyamide resin composition for laser marking and molded body thereof
JP2015143312A