Migration Resin Composition

A transition resin composition with vinyl chloride resin, plasticizer, and solvent forms a transition layer to restore flexibility and reduce stress in waterproof sheets by efficiently transferring plasticizer, addressing the issue of plasticizer volatilization.

JP7591624B2Active Publication Date: 2024-11-28S B SHEET WATERPROOF SYST +1
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
JP2023121037
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-07-25
Publication Date
2024-11-28
Estimated Expiration
2039-08-06

AI Technical Summary

Technical Problem

The flexibility of waterproof sheets in sheet waterproof structures deteriorates over time due to the volatilization of plasticizers, leading to stress generation and reduced waterproof properties.

Method used

A transition resin composition is applied to the waterproof sheet, containing a vinyl chloride resin, plasticizer, and solvent, with specific solubility parameters and viscosity modifiers, to form a transition layer that efficiently transfers plasticizer back to the sheet, restoring flexibility.

Benefits of technology

The transition layer effectively restores the flexibility of the waterproof sheet by transferring plasticizer, reducing stress and convex portions, thereby enhancing the waterproof properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591624000002
    Figure 0007591624000002
  • Figure 0007591624000003
    Figure 0007591624000003
  • Figure 0007591624000001
    Figure 0007591624000001
Patent Text Reader

Abstract

To provide a resin composition for transition allowing plasticizer to be efficiently transited from a transition layer by forming the transition layer in a waterproof sheet provided with a sheet waterproof structure.SOLUTION: A resin composite for transition of the present invention used for transition of plasticizer to a waterproof sheet 20 connected to a body 100 includes polyvinyl chloride resin, plasticizer, and solvent, configured to transit the plasticizer included in the resin composite for transition to the waterproof sheet 20 by drying the waterproof sheet 20 after being coated to form a transition layer 1, wherein when A is designated to a solution parameter of the polyvinyl chloride resin included in the resin composite for transition and B is designated to a solution parameter of the solvent included in the resin composite for transition, these difference of absolute value |A-B| meets |A-B|≤2.0.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to Migration Resin Composition Regarding. [Background technology]

[0002] 2. Description of the Related Art In recent years, with the demand for buildings to have high durability, sheet waterproofing structures in which resin sheets are laid down are being adopted on the rooftops, verandas, and the like of many buildings (see, for example, Patent Document 1).

[0003] In this sheet waterproofing structure, for example, a steel plate (metal plate) coated with polyvinyl chloride resin and formed to correspond to the shape of the boundary between the rooftop floor and a wall section erected along the outer edge of the floor is placed at the boundary, and at least a portion of this steel plate is covered with a waterproof sheet containing polyvinyl chloride resin and a plasticizer, thereby waterproofing the rooftop boundary.

[0004] Here, the shapes of rooftops, etc. on which waterproofing is to be applied are naturally various. Therefore, the steel plates are prepared in advance in a number of different shapes, and a number of plates that match the shapes of the boundary parts of the rooftops, etc. on which waterproofing is to be applied are selected. These steel plates are then arranged so that gaps are formed between adjacent plates in accordance with the shapes of the boundary parts, and in this state, they are covered with a waterproof sheet.

[0005] In a waterproof sheet structure of this kind, as time passes after construction, the plasticizer evaporates from the waterproof sheet due to exposure to sunlight and rainwater (muddy water), resulting in a decrease in the flexibility of the waterproof sheet. This causes stress in the waterproof sheet, which can lead to a decrease in the waterproofing properties of the waterproof sheet.

[0006] The generation of stress in this waterproof sheet is due to the evaporation of plasticizer from the waterproof sheet, so it has been proposed, for example in Patent Documents 2 and 3, to attach a transition (maintenance and repair) sheet containing polyvinyl chloride resin and plasticizer to the waterproof sheet.

[0007] By attaching the transfer sheet to the waterproof sheet in this manner, the plasticizer contained in the transfer sheet can be transferred (diffused) into the waterproof sheet, thereby restoring the flexibility of the waterproof sheet to excellent levels, thereby eliminating the generation of stress in the waterproof sheet.

[0008] There is a demand for the development of other configurations that can efficiently transfer plasticizer to a waterproof sheet, rather than being limited to the case where a transfer sheet is attached to the waterproof sheet as described above. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] JP 2007-70877 A [Patent Document 2] Japanese Patent Application Publication No. 8-207157 [Patent Document 3] JP 2015-196947 A Summary of the Invention [Problem to be solved by the invention]

[0010] The object of the present invention is to form a transfer layer on a waterproof sheet provided in a sheet waterproof structure, and to efficiently transfer a plasticizer from this transfer layer. Migration Resin Composition The purpose of this invention is to provide [Means for solving the problem]

[0011] Such objectives are as follows: 8 This is achieved by the present invention described in (1) A waterproof sheet that is joined to a structure having a floor is used to transfer a plasticizer, and contains a polyvinyl chloride resin, a plasticizer, and a solvent. and at least a part of the vinyl chloride resin and the plasticizer is dissolved in the solvent. A transitional resin composition, The composition is configured such that the plasticizer contained in the migration resin composition migrates to the waterproof sheet by applying the composition to the waterproof sheet and then drying the composition to form a migration layer that covers the waterproof sheet; The solubility parameter of the vinyl chloride resin contained in the migration resin composition is A [(cal / cm 3 ) 1 / 2 ], and the solubility parameter of the solvent contained in the transition resin composition is B[(cal / cm 3 ) 1 / 2 ], the absolute value of the difference |AB| is 1.0≦|AB|≦1.5 Satisfying the relationship death, In the transition resin composition, the content of the vinyl chloride resin, the content of the plasticizer, and the content of the solvent are 5 wt% or more and 10 wt% or less, 30 wt% or more and 40 wt% or less, and 20 wt% or more and 40 wt% or less, respectively. A transfer resin composition comprising:

[0012] (2) The solubility parameter A is 9.0 (cal / cm 3 ) 1 / 2 More than 11.0(cal / cm 3 ) 1 / 2 The transfer resin composition according to the above (1), which is:

[0013] (3) The component contained in the transfer resin composition The above The solvent is a mixed solvent, The transition resin composition according to the above (1) or (2), wherein the solvent having the lowest boiling point has a boiling point of 60°C or higher, and the solvent having the highest boiling point has a boiling point of 125°C or lower.

[0014] (4) The transition resin composition according to any one of (1) to (3) above, further comprising a viscosity modifier.

[0015] (5) The transitional resin composition according to any one of (1) to (4) above, which is in a cream form.

[0016] (6) The transition resin composition according to any one of (1) to (5) above, wherein the transition resin composition has a viscosity of 5,500 mPa or more and 9,500 mPa or less.

[0017] (7) The structure further has a wall portion erected from the floor portion, and the waterproof sheet contains a polyvinyl chloride resin and a plasticizer, A sheet waterproofing structure having the above-mentioned structure, a first placement member and a second placement member arranged side by side at the boundary between the above-mentioned floor portion and the above-mentioned wall portion with a gap formed therebetween, and the above-mentioned waterproof sheet joined so as to cover at least a portion of both the above-mentioned first placement member and the above-mentioned second placement member while including the above-mentioned gap, The transitional resin composition is a transitional resin composition according to any one of (1) to (6) above, which is used for forming the transitional layer that covers the waterproof sheet.

[0018] (8) The waterproof sheet has a convex portion due to deterioration at a position corresponding to the gap, and the transfer layer is provided corresponding to the convex portion. Effect of the Invention

[0020] According to the transfer resin composition of the present invention, a transfer layer can be formed that can efficiently transfer a plasticizer to a waterproof sheet from which the plasticizer has volatilized, which is provided in a sheet waterproof structure. [Brief description of the drawings]

[0021] [Figure 1] This is a partial oblique view of a transitional sheet waterproof structure in which a transitional layer is formed on a waterproof sheet provided in a sheet waterproof structure applied to a structural body. [Diagram 2] 2 is a cross-sectional view taken along line AA of the transition sheet waterproof structure shown in FIG. 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] The present invention will be described below. Migration Resin Composition The above will now be described in detail with reference to the preferred embodiments shown in the accompanying drawings.

[0023] First, before describing the transitional resin composition of the present invention, a sheet waterproofing structure was preserved and repaired by a transitional layer formed using the transitional resin composition of the present invention. Transition sheet waterproof structure An example of the above will be described.

[0024] <Transition sheet waterproof structure> Fig. 1 is a partial perspective view of a transitional sheet waterproof structure in which a transitional layer is formed on a waterproof sheet included in the sheet waterproof structure applied to a structural body, and Fig. 2 is a cross-sectional view of the transitional sheet waterproof structure shown in Fig. 1 taken along line AA. In the following explanation, the upper side in Fig. 1 and Fig. 2 will be referred to as "upper" and the lower side as "lower." For the sake of convenience, Fig. 1 does not show the entire sheet waterproof structure, but only partially illustrates the vicinity of the boundary between the floor and wall parts of the structural body.

[0025] In the following, a transitional sheet waterproof structure 500 in which a sheet waterproof structure 10 applied to a body 100 (structural body) such as a rooftop or a balcony is preserved and repaired with a transitional layer 1 will be described as an example.

[0026] In this embodiment, as shown in FIG. 1, the body 100 has a floor portion 101 and a wall portion 102 that is provided upright along and surrounds the outer edge of the floor portion 101.

[0027] The sheet waterproof structure 10 is applied to this main body 100, i.e., to a wall portion 102 forming a frame and a floor portion 101 forming the bottom of the wall portion 102, and has a waterproof sheet 20 and a placement member 50.

[0028] A plurality of placement members 50 are arranged side by side along the boundary 103 between the floor 101 and the wall 102, and in this state, the waterproof sheet 20 covers adjacent placement members 50 so as to straddle them, thereby ensuring waterproofing at the boundary 103 of the structure 100. That is, the boundary 103 of the structure 100 is a position where cracks and other fissures are likely to occur when exposed to sunlight or rainwater, but this boundary 103 is prevented from being directly exposed to sunlight or rainwater, and the placement members 50 and the waterproof sheet 20 are exposed to sunlight and rainwater, ensuring waterproofing at the boundary 103 of the structure 100.

[0029] As described above, the placement member 50 is placed near the boundary portion 103 between the floor portion 101 and the wall portion 102.

[0030] The arrangement member 50 is made of a metal plate (steel plate) whose surface is coated with resin, and has a bottom portion 51 and a rising surface 52 as shown in FIG. The bottom portion 51 has a rectangular shape bounded by four sides in a plan view facing the floor portion 101.

[0031] In addition, the rising surface 52 stands up from the edge of the bottom 51, i.e., one of the four long sides, and when viewed in a plan view facing the wall portion 102, forms a rectangular shape surrounded by four sides, with long sides having the same length as the long sides of the bottom 51.

[0032] The bottom portion 51 and the rising surface 52 are positioned so as to correspond to the floor portion 101 and the wall portion 102, respectively, when placed on the boundary portion 103.

[0033] In this embodiment, two arrangement members 50 (a first arrangement member and a second arrangement member) having the above-described configuration are arranged side by side along the boundary portion 103 with a gap 55 formed therebetween.

[0034] In this embodiment, two placement members 50 of the same shape are placed at the boundary 103, but since the shape of the structure 100 to be waterproofed naturally varies, placement members 50 of a plurality of different shapes are prepared in advance, and a plurality of placement members 50 that match the shape of the boundary 103 of the structure 100 to be actually applied are selected. These placement members 50 are then arranged in a state in which a gap 55 is formed so as to correspond to the shape of the boundary 103.

[0035] As described above, the arrangement member 50 is made of a metal plate whose surface is coated with resin. By coating the metal plate with resin in this manner, corrosion of the metal plate can be reliably prevented.

[0036] The metal plate is not particularly limited, but examples thereof include steel plates such as stainless steel plates and iron plates, aluminum plates, and copper plates, with steel plates being preferred, as this allows the positioning member 50 to have excellent strength.

[0037] The thickness of the metal plate is not particularly limited, but is preferably about 0.1 mm or more and 3 mm or less, and more preferably about 0.3 mm or more and 2.5 mm or less.

[0038] Examples of the resin include vinyl chloride resins such as polyvinyl chloride, polyolefin resins, ethylene-vinyl acetate copolymers, etc., and one or more of these may be used in combination, but polyvinyl chloride is preferred. Polyvinyl chloride has excellent solvent welding and heat fusion properties, and can more reliably prevent corrosion of the metal plate.

[0039] The thickness of the resin covering the metal plate is not particularly limited, but is preferably about 0.03 mm or more and 2 mm or less, and more preferably about 0.1 mm or more and 0.7 mm or less.

[0040] As shown in Figure 1, the waterproof sheet 20 is in the form of a sheet (plate) and covers two adjacent positioning members 50 (a first positioning member and a second positioning member) while including the gap 55 formed between them.

[0041] This prevents the boundary portion 103 from being directly exposed to sunlight or rainwater, and instead exposes the placement member 50 and the waterproof sheet 20 to sunlight and rainwater, thereby ensuring waterproofing at the boundary portion 103 of the main body 100.

[0042] Such a waterproof sheet 20 is made of a vinyl chloride resin sheet containing a vinyl chloride resin such as polyvinyl chloride and a plasticizer. According to the waterproof sheet 20 having such a configuration, by laminating the waterproof sheet 20 in a heated state, the two placement members 50 can be covered with the waterproof sheet 20 across the gap 55.

[0043] The thickness of the waterproof sheet 20 is not particularly limited, but is preferably, for example, about 0.1 mm to 5 mm, and more preferably about 0.3 mm to 2 mm. This allows the waterproof sheet 20 to reliably cover the placement member 50 as well as the floor portion 101 and the wall portion 102.

[0044] In the sheet-type waterproof structure 10 having the above-mentioned configuration, as time passes after construction, the plasticizer volatilizes from the waterproof sheet 20 due to exposure to sunlight and rainwater. As a result, the flexibility of the waterproof sheet 20 decreases, and stress is generated in the waterproof sheet 20 due to the deterioration of the waterproof sheet 20.

[0045] Here, in the sheet waterproofing structure 10 configured as in this embodiment, gaps 55 are formed between adjacent positioning members 50, and because the waterproof sheet 20 is not joined to the positioning members 50, stress is generated in the waterproof sheet 20, causing a hemispherical convex portion 25 (protrusion) to form on the waterproof sheet 20 that protrudes toward the opposite side of the floor portion 101.As a result, there may be a concern that the waterproofness of the waterproof sheet 20 will be reduced around this convex portion 25.

[0046] Therefore, if the plasticizer that has evaporated in the waterproof sheet 20 can be resupplied around the protrusions 25, the flexibility of the waterproof sheet 20 can be restored to excellent levels. This makes it possible to eliminate the generation of stress in the waterproof sheet 20 and set the height of the protrusions 25 low, i.e., to reduce the amount of floating of the waterproof sheet 20 at the positions corresponding to the protrusions 25.

[0047] Therefore, in the present invention, as shown in Figures 1 and 2, for the purpose of supplying a plasticizer to a waterproof sheet 20 from which plasticizer volatilization is observed, a transition resin composition containing a vinyl chloride resin, a plasticizer, and a solvent is applied to the waterproof sheet 20 and then dried to form a transition layer 1 covering the waterproof sheet 20 at a position that includes the convex portion 25 of the waterproof sheet 20.

[0048] As described above, by using the transfer resin composition to form the transfer layer 1 on the waterproof sheet 20 in a position that corresponds to the position that includes the protrusions 25, the plasticizer can be efficiently transferred to the waterproof sheet 20 located in the area that includes the protrusions 25. This makes it possible to restore the flexibility of the waterproof sheet 20. This makes it possible to eliminate the generation of stress in the waterproof sheet 20 and reliably set the height of the protrusions 25 low, i.e., to reliably reduce the amount of floating of the waterproof sheet 20 at the position that corresponds to the protrusions 25.

[0049] In addition, a transition layer 1 can be formed in the area including the convex portion 25 of the waterproof sheet 20 by the relatively simple process of applying a transition resin composition containing a vinyl chloride resin, a plasticizer, and a solvent to the waterproof sheet 20 and then drying it.

[0050] <Transfer resin composition> The transfer layer 1 is formed using the transfer resin composition of the present invention.

[0051] The transition resin composition of the present invention is used to transfer a plasticizer to the waterproof sheet 20, and contains a vinyl chloride resin, a plasticizer, and a solvent. The solubility parameter (SP value) of the vinyl chloride resin contained in the transition resin composition is A[(cal / cm 3 ) 1 / 2 ], and the solubility parameter of the solvent contained in the transition resin composition is B[(cal / cm 3 ) 1 / 2 ], the absolute value of the difference |AB| satisfies the relationship |AB|≦2.0.

[0052] By setting the absolute value |AB| of the difference between the solubility parameter A of the vinyl chloride resin and the solubility parameter B of the solvent within the above range, the vinyl chloride resin can be dissolved in the solvent with excellent solubility. Therefore, the transition resin composition can be made creamy (paste-like). Therefore, the transition layer 1 can be reliably formed in the area including the convex portion 25 of the waterproof sheet 20 by a relatively simple process of applying the transition resin composition to the waterproof sheet 20 and then drying it. Then, the plasticizer contained in the transition resin composition can be efficiently transferred from the transition layer 1 to the waterproof sheet 20, so that the flexibility of the waterproof sheet 20 can be restored.

[0053] In this specification, the solubility parameter (SP value) refers to the Hansen solubility parameter, which is obtained by dividing the solubility parameter introduced by Hildebrand into three components, namely, the dispersion term δD, the polarity term δP, and the hydrogen bonding term δH, and expressing them in a three-dimensional space.

[0054] The dispersion term ΔD represents the effect due to dispersion forces, the polar term ΔP represents the effect due to dipole-dipole forces, and the hydrogen bond term ΔH represents the effect due to hydrogen bonding forces. δD: Energy derived from intermolecular dispersion forces δP: Energy derived from intermolecular polar forces δH: Energy derived from hydrogen bonding forces between molecules (Note that the units are MPa.) 0.5 ).

[0055] The following relationship is found between Hildebrand's SP score and Hansen's HSP. Hildebrand's SP 2 = δD 2 +δP 2 +δH 2

[0056] The definition and calculation of HSP are described in Hansen Solubility Parameters: A Users Handbook by Charles M. Hansen (CRC Press, 2007).

[0057] Here, the dispersion term reflects van der Waals forces, the polar term reflects dipole moments, and the hydrogen bond term reflects the effects of water, alcohol, etc. Also, it can be determined that substances with similar HSP vectors have high solubility.

[0058] The HSP distance (Ra) can be calculated, for example, by the following formula when the HSP of the solute (vinyl chloride resin) is (ΔD1, ΔP1, ΔH1) and the HSP of the solvent is (ΔD2, ΔP2, ΔH2).

[0059] HSP distance (Ra)= {4×(δD1-δD2) 2 +(δP1-δP2) 2 +(δH1-δH2) 2} 0.5

[0060] In addition, the Hansen HSP of a mixed solvent can be calculated using the following formula, using the volume as the mixing ratio.

[0061] [δDm, δPm, δHm] = [(a×(δD1+b×δD2),(a×(δP1+b×δP2),(a×(δH1+b×δH2)] / (a+b)

[0062] The various constituent materials contained in the transition resin composition of the present invention having the above-mentioned composition will be described below. As described above, the transition resin composition of the present invention contains a vinyl chloride resin, a plasticizer, and a solvent.

[0063] (a) Vinyl chloride resin The vinyl chloride resin is contained in the transition resin composition as the main material thereof so that when the transition resin composition is applied to the waterproof sheet 20 and then dried, the dried product, i.e., the transition layer 1, will be layered.

[0064] The vinyl chloride resin is not particularly limited as long as it is a polymer containing vinyl chloride, that is, an oligomer, a prepolymer, or a polymer, but examples thereof include a monomer polymer of vinyl chloride, a copolymer of vinyl chloride with vinyl acetate, ethylene, or propylene, and a mixture of two or more of these polymers. By using these as the vinyl chloride resin, the plasticizer contained in the transition layer 1 formed using the transition resin composition can be reliably transferred to the waterproof sheet 20 side from the transition layer 1. In addition, among these, the vinyl chloride resin is preferably a vinyl chloride-vinyl acetate copolymer. This can improve the solubility of the vinyl chloride resin in the transition resin composition and can increase the viscosity of the vinyl chloride resin. In addition, the retention of the plasticizer in the transition layer 1 formed can be improved.

[0065] This vinyl chloride resin has a solubility parameter A of 9.0 (cal / cm 3 ) 1 / 2 More than 11.0(cal / cm 3 ) 1 / 2 It is preferable that the calorie content is 9.5 (cal / cm 3 ) 1 / 2 More than 10.5(cal / cm3 ) 1 / 2 It is more preferable that |AB| is equal to or less than 2.0. This makes it relatively easy to set the absolute value of the difference |AB| so as to satisfy the relationship |AB|≦2.0.

[0066] The content of the vinyl chloride resin in the transition resin composition is preferably 3 wt% or more and 20 wt% or less, and more preferably 5 wt% or more and 10 wt% or less. By setting the content of the vinyl chloride resin within the above range, the transition resin composition can be used to reliably form a layered transition layer 1. Furthermore, the plasticizer contained in the transition layer 1 can be reliably transferred from the transition layer 1 formed using the transition resin composition to the waterproof sheet 20 side.

[0067] (b) Plasticizer The plasticizer is contained as a material that migrates from the transfer layer 1 formed by applying the transfer resin composition to the waterproof sheet 20 and then drying it, to the waterproof sheet 20.

[0068] The plasticizer is not particularly limited, but examples thereof include phthalate ester plasticizers such as DOP (dioctyl phthalate), DBP (dibutyl phthalate), DIBP (diisobutyl phthalate), DINP (diisononyl phthalate), and DHP (diheptyl phthalate), aliphatic dibasic acid ester plasticizers such as DOA (di-2-ethylhexyl adipate), DIDA (diisodecyl adipate), and DOS (di-2-ethylhexyl sebacate), aromatic carboxylate ester plasticizers such as ethylene glycol benzoates, and trimellitic acid ester plasticizers such as TOTM (trioctyl trimellitate), and one or more of these can be used in combination. By using these as plasticizers, the flexibility of the waterproof sheet 20, which has decreased when the plasticizer migrates from the transfer layer 1 to the waterproof sheet 20, can be reliably improved again.

[0069] The solubility parameter (SP value) of this plasticizer is 8.0 (cal / cm3 ) 1 / 2 More than 10.0(cal / cm 3 ) 1 / 2 It is preferable that the calorie content is 8.5 (cal / cm 3 ) 1 / 2 More than 9.5(cal / cm 3 ) 1 / 2 This makes it possible to dissolve not only the vinyl chloride resin but also the plasticizer in the solvent with excellent solubility in the transition resin composition.

[0070] The content of the plasticizer in the transition resin composition is preferably 20 wt% to 50 wt%, more preferably 30 wt% to 40 wt%. By setting the content of the plasticizer within the above range, the plasticizer can be reliably transferred from the transition layer 1 formed using the transition resin composition to the waterproof sheet 20.

[0071] (c) Solvent The solvent is contained in the transition resin composition in order to dissolve the vinyl chloride resin, thereby making the transition resin composition cream-like (paste-like).

[0072] The solvent is not particularly limited, but examples thereof include hydrocarbon solvents such as n-hexane, toluene, and o-xylene, ketone solvents such as acetone, methyl ethyl ketone (MEK), and cyclohexanone, ester solvents such as ethyl acetate and isobutyl acetate, ether solvents such as diethyl ether and tetrahydrofuran (THF), and alcohol solvents such as methanol, ethanol, and 1-propanol, and one or more of these can be used in combination. By using these as solvents, the vinyl chloride resin can be dissolved in the transition resin composition, and the transition resin composition can be made into a cream (paste) form.

[0073] This solvent has a solubility parameter B of 7.5 (cal / cm 3 ) 1 / 2More than 10.5(cal / cm 3 ) 1 / 2 It is preferable that the calorie content is 8.5 (cal / cm 3 ) 1 / 2 More than 9.5(cal / cm 3 ) 1 / 2 It is more preferable that the absolute value of the difference |AB| is equal to or less than 2.0. This makes it relatively easy to set the absolute value of the difference |AB| to satisfy the relationship of |AB|≦2.0, and the transfer layer 1 obtained by drying the transfer resin composition can be formed to exhibit appropriate adhesion to the waterproof sheet 20.

[0074] The solvent is a mixed solvent, and the solvent having the lowest boiling point is preferably 60° C. or higher, more preferably 65° C. or higher, and the solvent having the highest boiling point is preferably 125° C. or lower, more preferably 120° C. or lower. This makes it possible to more reliably make the transition resin composition creamy before drying, and also makes it possible to form the transition layer 1 obtained by drying the transition resin composition so as to exhibit excellent adhesion to the waterproof sheet 20.

[0075] Considering the relationship between the solubility parameter B and the boiling point of the mixed solvent as described above, specific combinations of solvents include, for example, a combination of at least one of toluene, ethyl acetate, and isobutyl acetate with at least one of methyl ethyl ketone and tetrahydrofuran, and in consideration of environmental safety, a combination of at least one of ethyl acetate and isobutyl acetate with tetrahydrofuran is exemplary.

[0076] The content of the solvent in the transition resin composition is preferably 20 wt% or more and 50 wt% or less, more preferably 30 wt% or more and 40 wt% or less. By setting the content of the solvent within the above range, the vinyl chloride resin can be dissolved in the transition resin composition. Furthermore, the transition resin composition can be used to reliably form a layered transition layer 1.

[0077] (d) Viscosity modifier In addition to the vinyl chloride resin, plasticizer and solvent, the transition resin composition preferably further contains a viscosity modifier.

[0078] By including a viscosity adjuster in the transition resin composition, the viscosity of the transition resin composition can be set within an appropriate range, ensuring that the transition resin composition is creamy.

[0079] The viscosity modifier is not particularly limited, but examples thereof include titanium oxide, clay, silica, calcium carbonate, barium sulfate, etc., and one or more of these may be used in combination. Among these, calcium carbonate is preferable. This can reliably increase the viscosity of the transition resin composition.

[0080] The viscosity modifier is preferably particulate and has an average particle size of 0.5 μm to 20 μm, more preferably 0.5 μm to 10 μm. By setting the average particle size within the above range, the dispersibility of the viscosity modifier in the transition resin composition can be improved.

[0081] The content of the viscosity modifier in the transition resin composition is preferably 5 wt% to 20 wt%, more preferably 10 wt% to 15 wt%. By setting the content of the viscosity modifier within the above range, the viscosity of the transition resin composition can be set within an appropriate range relatively easily.

[0082] Furthermore, in addition to the above-mentioned constituent materials, the transition resin composition may contain stabilizers, stabilizing aids, ultraviolet absorbers, colorants, lubricants, etc.

[0083] The stabilizer may be, for example, zinc glycine, and the stabilizing aid in this case may be, for example, organic phosphates such as tricresyl phosphate (TCP), trixylyl phosphate (TXP), tributyl phosphate (TBP), tri-2-ethylhexyl phosphate, and 2-ethylhexyl diphenyl phosphate.

[0084] In such a transition resin composition, the absolute value |AB| of the difference between the solubility parameter A of the vinyl chloride resin and the solubility parameter B of the solvent may satisfy the relationship |AB|≦2.0, preferably the relationship 0.8≦|AB|≦1.7, and more preferably the relationship 1.0≦|AB|≦1.5. This allows the vinyl chloride resin to be dissolved in the solvent with better solubility, so that the transition resin composition can have a better creamy consistency, and furthermore, since the difference between the solubility parameter A of the vinyl chloride resin and the solubility parameter B of the solvent is not too small, it becomes possible to peel off the waterproof sheet having the transition layer and the convex portion.

[0085] Furthermore, when the transition resin composition is cream-like, the viscosity of the transition resin composition is preferably 5,500 mPa or more and 9,500 mPa or less, and more preferably 6,500 mPa or more and 7,500 mPa or less. This makes it possible to supply the transition resin composition to the waterproof sheet 20 relatively easily, and the transition resin composition supplied to the waterproof sheet 20 can be made to follow the shape of the protrusions 25 formed on the waterproof sheet 20. Therefore, the transition layer 1 formed by drying the transition resin composition can also be formed to follow the shape of the protrusions 25.

[0086] Furthermore, the thickness of the transfer layer 1 formed by drying the transfer resin composition is preferably 0.5 mm to 2 mm, more preferably 1 mm to 2 mm, in the regions not corresponding to the convex portions 25. This allows the transfer layer 1 to be formed as a layer even in the regions corresponding to the convex portions 25 without being broken by the convex portions 25, and also allows the plasticizer to be reliably transferred from the transfer layer 1 to the waterproof sheet 20 side.

[0087] In addition, as described above, the transition layer 1 is formed by drying the transition resin composition, and its adhesion to the waterproof sheet 20 is set to a level that allows it to be peeled off relatively easily by manual peeling. Therefore, after the formation of the transition layer 1, the transition layer 1 can be peeled off at the point where it is confirmed that the floating amount of the waterproof sheet 20 has been reduced at the position corresponding to the convex portion 25, and then the transition sheet as described in the background art can be attached to the waterproof sheet 20. In other words, the transition layer 1 can be said to be an emergency repair layer that reduces the degree of deterioration of the waterproof sheet 20 before the transition sheet is attached.

[0088] In this embodiment, the transition layer 1 is provided at a position corresponding to the gap 55 between the two placement members 50 so as to cover the convex portion 25 formed on the waterproof sheet 20, and the height of the convex portion 25 is reduced by transferring the plasticizer contained in the transition layer 1 to the waterproof sheet 20. However, the position where the transition layer 1 is provided is not limited to this case. Specifically, for example, before the convex portion 25 is formed, the transition layer 1 may be formed on the waterproof sheet 20 at a position corresponding to the gap 55, or the transition layer 1 may be formed on the waterproof sheet 20 at a position directly covering the floor portion 101 without covering the placement member 50. In these cases, the plasticizer contained in the transition layer 1 can be transferred to the waterproof sheet 20 to restore the flexibility of the waterproof sheet 20, that is, the deterioration of the waterproof sheet 20 can be reduced.

[0089] As described above, Migration Resin CompositionHowever, the present invention is not limited to these.

[0090] For example, in the transition sheet waterproof structure of the present invention, each component can be replaced with any component that can exert a similar function, or any component can be added. EXAMPLES

[0091] Next, specific examples of the present invention will be described. However, the present invention is not limited to the descriptions in these examples.

[0092] 1. Preparation of raw materials First, the raw materials used in the preparation of the transition resin compositions of the Examples and Comparative Examples are shown below.

[0093] (Vinyl chloride resin) As a vinyl chloride resin, a vinyl chloride-vinyl acetate copolymer (manufactured by Tosoh Corporation, "Ryuron Best 952", SP value: 10.4 (cal / cm 3 ) 1 / 2 ) was prepared.

[0094] (Plasticizer) As a plasticizer, DINP (manufactured by JPlus, SP value: 8.9 (cal / cm 3 ) 1 / 2 ) was prepared.

[0095] (solvent) As a solvent, toluene (manufactured by Mitsubishi Chemical Corporation, boiling point: 111°C, SP value: 8.9 (cal / cm 3 ) 1 / 2 ), ethyl acetate (Showa Denko K.K., boiling point: 77°C, SP value: 9.1 (cal / cm 3 ) 1 / 2 ), isobutyl acetate (KH Neochem, boiling point: 118°C, SP value: 8.3 (cal / cm 3 ) 1 / 2 ), MEK (Maruzen Petrochemical Co., Ltd., boiling point: 80°C, SP value: 9.3 (cal / cm 3 ) 1 / 2), THF (Mitsubishi Chemical Corporation, boiling point: 66°C, SP value: 9.5 (cal / cm 3 ) 1 / 2 ) was prepared.

[0096] (Viscosity modifier) As a viscosity adjuster, calcium carbonate (Bihoku Funka Kogyo Co., Ltd., "Softon 2200", average particle size: 1 μm) was prepared.

[0097] (Stabilizer) As the stabilizer, a Ca-Zn liquid stabilizer (manufactured by ADEKA Corporation, "SC-32") was prepared.

[0098] (Coloring agent) As colorants, titanium oxide (manufactured by Ishihara Sangyo Kaisha, Ltd., "R-680") and carbon black (manufactured by Mitsubishi Chemical Corporation, "Mitsubishi Carbon Black #45") were prepared.

[0099] 2. Preparation of the migration resin composition [Example 1] First, vinyl chloride-vinyl acetate copolymer (9.0 wt%) as a vinyl chloride resin, DINP (36.0 wt%) as a plasticizer, calcium carbonate (14.0 wt%) as a viscosity modifier, toluene (17.0 wt%) and THF (19.0 wt%) as solvents, the stabilizer (4.0 wt%), and the colorant (1.0 wt%) were uniformly mixed using a mixer at 25°C to prepare the transition resin composition of Example 1.

[0100] [Examples 2 to 4, Comparative Examples 1 to 5] The transition resin compositions of Examples 2 to 4 and Comparative Examples 1 to 5 were prepared in the same manner as in Example 1, except that the type and content of the solvent contained in the transition resin composition were changed as shown in Table 1.

[0101] 3. Formation of transfer layer 1 on waterproof sheet using transfer resin composition Next, a transfer layer 1 was formed on a waterproof sheet 20 having protrusions 25 using the transfer resin composition of each of the Examples and Comparative Examples.

[0102] More specifically, a sheet waterproof structure 10 as shown in Figure 1 was prepared, which included a waterproof sheet 20 having a hemispherical convex portion 25 with a diameter of φ23 mm and a floating amount of the waterproof sheet 20 of 4 mm.The transition resin composition of each example and comparative example was applied to the waterproof sheet 20 in this sheet waterproof structure 10, and then dried to form a transition layer 1 with an average thickness of 2 mm that covers the waterproof sheet 20 to correspond to the convex portion 25, thereby obtaining a transition sheet waterproof structure 500.

[0103] The waterproof sheet 20 used was one containing 50 parts by weight of plasticizer for 100 parts by weight of vinyl chloride resin. The convex portions 25 on the waterproof sheet 20 were formed by attaching butyl tape to the waterproof sheet 20, and then treating it in an oven at 80°C for 3 days to extract the plasticizer, thereby setting the plasticizer residual rate at 70%.

[0104] 4. Evaluation For the transfer layer 1 formed using the transfer resin composition of each Example, the effect of reducing the lifting amount of the waterproof sheet 20 at the convex portions 25 was evaluated using the following method.

[0105] <Effect of reducing floating amount of waterproof sheet 20 at convex portion 25> The transfer layer 1 formed on the waterproof sheet 20 having the projections 25 using the transfer resin composition of each Example was stored at a temperature of 80° C. for one week, and then the amount of lifting of the waterproof sheet 20 at the projections 25 was measured, and the effect of reducing the amount of lifting of the waterproof sheet 20 at the projections 25 was evaluated based on the evaluation criteria shown below. The evaluation results are shown in Table 1.

[0106] [Evaluation Criteria] ◎: The floating amount of the waterproof sheet 20 is less than 3 mm. A clear reduction in the amount of floating was observed. ○: The floating amount of the waterproof sheet 20 is 3 mm or more and less than 4 mm. The effect of reducing the amount of floating was observed. ×: The floating amount of the waterproof sheet 20 was 4 mm, and no effect of reducing the floating amount was observed.

[0107] [Table 1]

[0108] As shown in Table 1, in each Example, the magnitude of the absolute value of the difference |AB| was set to 2.0 or less, and as a result, the transfer resin composition was in a cream form, and a transfer layer 1 could be formed on the waterproof sheet 20 on which the convex portions 25 were formed. Then, the plasticizer could be transferred from this transfer layer 1 to the waterproof sheet 20, and as a result, the amount of lift of the waterproof sheet 20 at the positions corresponding to the convex portions 25 was reduced.

[0109] In contrast to this, in each of the comparative examples, the effect of reducing the amount of floating was not observed because the magnitude of the absolute value of the difference |AB| could not be set to 2.0 or less. [Explanation of symbols]

[0110] 1. Transition Layer 10 Sheet waterproof structure 20. Tarpaulin 25 Convex 50 Placement parts 51 Bottom 52 Rising surface 55 Gap 100 skeleton 101 Floor section 102 Wall section 103 Boundary 500 Transition Sheet Waterproof Structure

Claims

1. A transfer resin composition is used to transfer a plasticizer to a waterproof sheet joined to a building frame having a floor portion, the transfer resin composition comprising a vinyl chloride resin, a plasticizer, and a solvent, in which at least a portion of the vinyl chloride resin and the plasticizer are dissolved in the solvent, The composition is configured such that the plasticizer contained in the migration resin composition migrates to the waterproof sheet by applying the composition to the waterproof sheet and then drying the composition to form a migration layer that covers the waterproof sheet; The solubility parameter of the vinyl chloride resin contained in the transition resin composition is A [(cal / cm 3 ) 1 / 2 ], and the solubility parameter of the solvent contained in the transition resin composition is B [(cal / cm 3 ) 1 / 2 ], the absolute value of the difference |A-B| satisfies the relationship 1.0≦|A-B|≦1.5, In the transition resin composition, the content of the vinyl chloride resin, the content of the plasticizer, and the content of the solvent are, respectively, 5 wt% or more and 10 wt% or less, 30 wt% or more and 40 wt% or less, and 20 wt% or more and 40 wt% or less.

2. The solubility parameter A is 9.0 (cal / cm 3 ) 1 / 2 More than 11.0 (cal / cm 3 ) 1 / 2 2. The transfer resin composition of claim 1, wherein:

3. The solvent contained in the transition resin composition is a mixed solvent, 3. The transfer resin composition according to claim 1, wherein the solvent having the lowest boiling point has a boiling point of 60° C. or higher, and the solvent having the highest boiling point has a boiling point of 125° C. or lower.

4. 4. The transition resin composition of claim 1, further comprising a viscosity modifier.

5. 5. The transitional resin composition according to claim 1, wherein the transitional resin composition is in a cream form.

6. 6. The transition resin composition according to claim 1, wherein the transition resin composition has a viscosity of 5,500 mPa or more and 9,500 mPa or less.

7. The structure further has a wall portion erected from the floor portion, and the waterproof sheet contains a polyvinyl chloride resin and a plasticizer, A sheet waterproof structure having the structure, a first placement member and a second placement member arranged side by side at the boundary between the floor and the wall with a gap formed therebetween, and the waterproof sheet joined so as to cover at least a portion of both the first placement member and the second placement member while including the gap, 7. The transitional resin composition according to claim 1, which is used to form the transitional layer that covers the waterproof sheet.

8. The transfer resin composition according to claim 7, wherein the waterproof sheet has a convex portion due to deterioration at a position corresponding to the gap, and the transfer layer is provided corresponding to the convex portion.

Citation Information

Patent Citations

  • Coating method

    JP1995070346A

  • Production of conductive resin molding

    JP1995196828A

  • Life prolonging / Restoring method of existing secular degraded waterproof sheet and coating material therefor

    JP1996004225A

  • Resin composition for mending waterproof sheet

    JP1996207154A

  • Resin sheet for mending waterproof sheet

    JP1996207157A