Side-fill resin composition, semiconductor device, and method for removing side-fill material
The photocurable side fill resin composition addresses thermal shock resistance and repairability issues in semiconductor devices by enhancing adhesion strength and enabling easy removal, thus improving the reliability and cost-effectiveness of semiconductor devices.
Patent Information
- Application Number
- JP2021575758
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-04-24
- Filing Date
- 2021-01-29
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2041-01-29
AI Technical Summary
Existing side fill materials in semiconductor devices suffer from reduced thermal shock resistance and poor repairability due to their adhesive properties, making it difficult to remove residues during repairs and leading to potential conduction defects in harsh thermal environments.
A photocurable side fill resin composition is used between the base material and the peripheral edge of mounted components, which can be easily removed by heating, thereby enhancing thermal shock resistance and repairability.
The composition provides high thermal shock resistance and excellent repairability by maintaining adhesion strength while allowing easy removal of the side fill material, reducing the likelihood of warping and conduction defects, and facilitating cost-effective repairs.
Smart Images

Figure 0007591720000002 
Figure 0007591720000003 
Figure 0007591720000001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a side-fill resin composition, a semiconductor device, and a method for removing a side-fill material, and more particularly, to a side-fill resin composition used to reinforce mounted components such as semiconductor elements, a semiconductor device including a side-fill material produced from the side-fill resin composition, and a method for removing the side-fill material. [Background technology]
[0002] Conventionally, in a semiconductor device including a substrate and a mounting component mounted on the substrate, in order to reinforce the connection between the substrate and the mounting component, a resin composition is supplied by filling or applying it into the gap between the substrate and the mounting component. There are an underfill method and a sidefill method for filling the gap between the substrate and the mounting component with a resin composition to reinforce the substrate and the mounting component.
[0003] In the underfill method, a resin composition is filled into the entire gap between the substrate and the mounted component, and the resin composition is cured to seal the gap between the substrate and the mounted component and reinforce the connection between the substrate and the mounted component.
[0004] On the other hand, in the side-fill method, a resin composition is applied only to a portion between the substrate and the mounting component, for example, the peripheral end surface of the mounting component in a plan view, and the resin composition is cured to reinforce the substrate and the mounting component, particularly the peripheral portion of the surface of the mounting component facing the substrate. Compared to the underfill material, the side-fill material has a smaller adhesion area with the substrate and the mounting component, so that if a defective component is found during inspection or use of the mounting component, the mounting component can be easily removed from the substrate and replaced with a good component, which is called excellent repairability. On the other hand, the side-fill method tends to reduce the reliability (particularly heat resistance reliability) of the semiconductor device.
[0005] Patent Document 1 discloses a liquid epoxy resin composition that contains an epoxy resin, a curing agent, and an inorganic filler, and that contains, as the inorganic filler, 0.1 to 30 mass% of a scaly inorganic material having an average aspect ratio of 2 to 150 relative to the total amount of the epoxy resin composition, and that has a thixotropic index of 3.0 to 8.0. The liquid epoxy resin composition is also disclosed as a side filler material that can encapsulate a substrate and an element mounted on the substrate. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2013-102167 A Summary of the Invention
[0007] An object of the present disclosure is to provide a side-fill resin composition that can impart excellent thermal shock resistance to a semiconductor device even when the peripheral portion of the surface of a mounted component of a semiconductor device that faces a substrate is reinforced with a side-fill and that has excellent side-fill repairability when repairing defects in the mounted component; a semiconductor device provided with a side-fill material made of a cured product of this side-fill resin composition; and a method for removing the side-fill material.
[0008] The side-fill resin composition according to one embodiment of the present disclosure is used to prepare a side-fill material interposed between a substrate and a peripheral portion of a surface of a mounted component that is surface-mounted on the substrate, the peripheral portion being opposed to the substrate, and has photocurability.
[0009] A semiconductor device according to an embodiment of the present disclosure includes a substrate and a side fill material interposed between the substrate and a peripheral portion of a surface of a mounting component that is to be surface-mounted on the substrate, the side fill material being made of a cured product of the side fill resin composition.
[0010] A method for removing a side fill material according to one embodiment of the present disclosure includes heating the side fill material in a semiconductor device to 200° C. or higher and removing the side fill material from between a peripheral portion of a mounted component and the substrate. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a schematic cross-sectional view showing a semiconductor device according to an embodiment of the present disclosure. [Diagram 2] Fig. 2A is a plan view showing a first example of a semiconductor device according to an embodiment of the present disclosure, in which a side fill material is interposed in the peripheral portion of a mounted component. Fig. 2B is a plan view showing a second example of a semiconductor device according to an embodiment of the present disclosure, in which a side fill material is interposed in the peripheral portion of a mounted component. Fig. 2C is a plan view showing a third example of a semiconductor device according to an embodiment of the present disclosure, in which a side fill material is interposed in the peripheral portion of a mounted component. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] 1. Overview First, the background to the present disclosure will be described.
[0013] In the liquid epoxy resin composition of Patent Document 1 (JP Patent Publication 2013-102167 A), when this liquid epoxy resin composition is cured and used as a side fill material, there is a problem that when a defective component mounted on a substrate is repaired, it is difficult to completely remove the residue of the side fill material from the substrate and the mounted component during repair. Also, in semiconductor devices, when the mounted components on the substrate are placed in a severe thermal environment, such as in vehicle applications, improved thermal shock resistance is required to prevent electrical continuity defects from occurring.
[0014] The inventors conducted intensive research to solve the above problems, and as a result, they have succeeded in realizing a side fill resin composition that can impart excellent thermal shock resistance to a semiconductor device even when the peripheral portion of the surface of a mounted component of a semiconductor device that faces a substrate is reinforced with a side fill, and that has excellent repairability as a side fill when repairing defects in the mounted component.
[0015] That is, the side fill resin composition according to the present embodiment is used to prepare a side fill material 4 interposed between the substrate 2 and the peripheral portion of the surface of the mounting component 3 facing the substrate 2, which is surface-mounted on the substrate 2. The side fill resin composition according to the present embodiment has photocurability. In the present disclosure, the "side fill material" is a material for reinforcing a mounting component such as a semiconductor element surface-mounted on the substrate. In the present embodiment, the side fill material 4 is made of a cured product of the side fill resin composition. The side fill material 4 can also be said to be a reinforcing material interposed between the substrate 2 and the peripheral portion of the surface of the mounting component 3 facing the substrate 2. The peripheral portion of the surface of the mounting component 3 facing the substrate 2 may be the entire peripheral portion of the mounting component 3 in a plan view, or at least a part of the entire peripheral portion.
[0016] As shown in FIG. 1, the side-fill resin composition according to this embodiment is preferably used as a reinforcing material (side-fill material 4) in a semiconductor device 1, which is interposed between a substrate 2 and a peripheral portion of a surface of a mounting component 3, such as a semiconductor chip, facing the substrate 2 and which is surface-mounted on the substrate 2, to reinforce the substrate 2 and the mounting component 3.
[0017] The side fill resin composition of this embodiment has photocurability. The photopolymerizable component having photocurability used in this embodiment often has a lower viscosity than the thermally polymerizable component. Therefore, even if the proportion of inorganic filler in the side fill resin composition is increased, the viscosity of the side fill resin composition is unlikely to increase. This makes it easy to adjust the linear expansion coefficient of the cured product low, and therefore the thermal shock resistance of the semiconductor device 1 including the cured product made from the side fill resin composition can be improved. Therefore, the semiconductor device 1 including the side fill material 4 made of the cured product of the side fill resin composition can have high heat resistance reliability.
[0018] In addition, in the semiconductor device 1, when the substrate 2 and the mounting component 3 surface-mounted on the substrate 2 are reinforced with, for example, a cured product of an underfill resin composition (underfill material), the underfill material supplies and fills the entire gap (joint) between the substrate 2 and the mounting component 3, even to the back of the gap. The resin composition is then cured to reinforce the connection between the substrate 2 and the mounting component 3. Therefore, when a defect occurs in the semiconductor device 1 and repair is performed, it may take time and effort to remove the underfill material formed over the entire gap between the substrate 2 and the mounting component 3, or the substrate 2 and the mounting component 3 may all have to be discarded, and there is a risk that residues of the sidefill material may remain on the substrate 2 and the mounting component 3.
[0019] In contrast, in this embodiment, the side fill material is prepared by photocuring the side fill resin composition, and therefore can be easily removed by heating. Therefore, in the semiconductor device 1 including the side fill material 4 made of the cured product of the side fill resin composition of this embodiment, the side fill material can have excellent repairability. The "repairability" here refers to the ease of removal from the substrate of the cured product (including the underfill material and the side fill material) prepared from the resin composition in the semiconductor device.
[0020] The reason why the side-fill resin composition of this embodiment has excellent repairability has not been precisely clarified, but it is believed to be due to the following reasons. With the side-fill resin composition of this embodiment, it is easy to adjust the adhesion strength between the base material 2 (substrate) in the semiconductor device 1 and the cured product of the side-fill resin composition, and even when removing a side-fill material made of the cured product of the side-fill resin composition on the substrate, the residue of the side-fill material is easy to remove from the substrate and the mounted components. For this reason, it is presumed that the side-fill resin composition can have excellent repairability.
[0021] In this manner, according to the present embodiment, the cured product made from the side-fill resin composition can be easily removed by heating. Therefore, even if a defect occurs in the semiconductor device 1, the side-fill resin composition of the present embodiment can be easily repaired.
[0022] In addition, since the side-fill resin composition of this embodiment is photocurable, when reinforcing the peripheral portion of the surface of the mounting component 3 facing the base material 2 between the base material 2 and the mounting component 3 surface-mounted on the base material 2 with the cured product of the side-fill resin composition, the tact time (for example, the time to form a cured product) can be shortened compared to a thermosetting resin component. In addition, the side-fill resin composition of this embodiment can suppress the inclusion of air bubbles before and after curing compared to the case of a thermosetting resin. Therefore, it is possible to make it difficult for voids to occur in the cured product, and as a result, even if the peripheral portion of the surface of the mounting component 3 facing the base material 2 is reinforced with the side-fill resin composition, it is possible to make it difficult for defects to occur in the semiconductor device 1. In addition, since it is not necessary to heat the side-fill resin composition to cure, the side-fill material 4 is not easily affected by the thermal history due to heating. Therefore, the side-fill resin composition can reinforce the base material 2 and the peripheral portion of the mounting component 3 facing the base material 2 by making it difficult for the mounting component 3 to come off from the semiconductor device 1, and can make it difficult for conductive defects to occur in the semiconductor device 1. As a result, when the side-fill resin composition is interposed between the base material 2 of the semiconductor device 1 and the peripheral portion of the surface of the mounting component 3 that faces the base material 2 and is surface-mounted on the base material 2 to reinforce the base material 2 and the mounting component 3, the side-fill material 4 can be produced in a short time and is less likely to retain heat history in the side-fill material 4. Therefore, warping and voids are less likely to occur in the reinforcing material produced from the side-fill resin composition.
[0023] In this way, the side-fill resin composition according to this embodiment can reinforce the connection between the substrate 2 of the semiconductor device 1 and the peripheral portion of the surface of the mounting component 3 mounted on the substrate 2 that faces the substrate 2. More specifically, the preferred characteristics of the side-fill resin composition can be realized by appropriately adjusting the components of the composition described below.
[0024] 2.Details The components that may be contained in the side fill resin composition according to this embodiment and the properties of the side fill resin composition will be described more specifically.
[0025] The sidefill resin composition of this embodiment preferably contains a photocurable component (A) and a photopolymerization initiator (B). In this case, the sidefill resin composition can be easily given photocurability. In addition, the sidefill material 4 prepared by photocuring the sidefill resin composition can be easily removed by heating compared to the cured product of the thermosetting component. Therefore, the semiconductor device 1 provided with the sidefill material 4 made of the cured product of the sidefill resin composition of this embodiment has high thermal shock resistance, and the sidefill material 4 in the semiconductor device 1 can have excellent repairability. In particular, when preparing a sidefill material from a thermosetting cured product, additives such as flexibility imparting agents have been added to improve repairability, but in this case, there was a problem that thermal properties such as heat resistance and thermal shock resistance may be reduced due to the influence of the flexibility imparting agent. In contrast, in the sidefill resin composition of this embodiment, the semiconductor device 1 can have excellent thermal shock resistance by providing a cured product prepared from the sidefill resin composition, and the sidefill material 4 can have excellent repairability even without adding additives such as flexibility imparting agents.
[0026] [Photopolymerizable component (A)] The photopolymerizable component (A) can impart photocurability to the sidefill resin composition. Examples of the photopolymerizable component (A) include compounds having appropriate photocurability. Examples of the photocurable compound include cationic polymerizable compounds and radical polymerizable compounds.
[0027] The mass ratio of the photocurable component (A) to the total solid content of the sidefill resin composition is preferably 10% by mass or more and 60% by mass or less. In this case, the sidefill resin composition can be imparted with higher photocurability. The mass ratio of the photocurable component (A) to the total solid content of the sidefill resin composition is more preferably 15% by mass or more and 55% by mass or less, and even more preferably 20% by mass or more and 50% by mass or less.
[0028] The photopolymerizable component (A) preferably contains a photocationically polymerizable compound (A1). That is, the side-fill resin composition preferably contains a photocationically polymerizable compound (A1). In this case, even if the substrate 2 and the mounting component 3 are reinforced by interposing a cured product of the side-fill resin composition between the substrate 2 of the semiconductor device 1 and the peripheral portion of the surface of the mounting component 3 facing the substrate 2, the cured product can be easily removed by heating. Therefore, the side-fill resin composition can impart better repairability to the semiconductor device 1. In addition, when the side-fill resin composition contains the photocationically polymerizable compound (A1), the semiconductor device 1 can have excellent reliability in a heat cycle when the substrate 2 and the mounting component 3 are reinforced with the cured product of the side-fill resin composition. In the present disclosure, the "heat cycle" refers to a temperature cycle in which heating and cooling are repeated between a low temperature range (e.g., -40°C) and a high temperature range (e.g., 125°C).
[0029] The photocationically polymerizable compound (A1) is a component that, when irradiated with light, generates cationic species, for example, by the action of the photopolymerization initiator (B), and can polymerize the cationic species as a growing chain. The photopolymerization initiator (B) is mosquito Chion sexual light It is preferable that the composition contains a polymerization initiator (B1). mosquito Chion sexual light The polymerization initiator (B1) preferably has a function as, for example, a photoacid generator. A photoacid generator is a compound that absorbs irradiated light, decomposes to generate an acid, and polymerizes a photopolymerizable component.
[0030] The photocationically polymerizable compound (A1) preferably contains at least one selected from the group consisting of epoxy resins, oxetane resins, and vinyl ether resins.
[0031] The epoxy resin is, for example, a compound having at least one epoxy group in one molecule.Specifically, the epoxy resin may be at least one compound selected from the group consisting of biphenyl type epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, naphthalene ring-containing epoxy resin, anthracene ring-containing epoxy resin, alicyclic epoxy resin, dicyclopentadiene type epoxy resin having a dicyclopentadiene skeleton, phenol novolac type epoxy resin, cresol novolac type epoxy resin, triphenylmethane type epoxy resin, bromine-containing epoxy resin, aliphatic epoxy resin, aliphatic polyether type epoxy resin, and triglycidyl isocyanurate.The epoxy resin may have a glycidyl group.
[0032] The oxetane resin is, for example, a compound having at least one oxetane skeleton in one molecule. Specifically, the oxetane resin may be at least one compound selected from the group consisting of 3-ethyl-3-hydroxymethyloxetane, 2-ethylhexyloxetane, 3-ethyl-3-(2-ethylhexyloxymethyl)oxetane, 3-ethyl-3-(cyclohexyloxy)methyloxetane, and 3-ethyl-3-(phenoxymethyl)oxetane.
[0033] The vinyl ether resin is, for example, a compound having at least one vinyl ether skeleton in one molecule.Specific examples of the vinyl ether resin include at least one compound selected from the group consisting of ethylene glycol divinyl ether, diethylene glycol divinyl ether, triethylene glycol divinyl ether, polyethylene glycol divinyl ether, propylene glycol divinyl ether, butylene glycol divinyl ether, hexanediol divinyl ether, bisphenol A alkylene oxide divinyl ether, and bisphenol F alkylene oxide divinyl ether.
[0034] The photopolymerizable component (A) is a photocation heavy When the photocationically polymerizable compound (A1) is contained, the photocationically polymerizable compound (A1) preferably contains an epoxy resin and an oxetane resin. In this case, the photocuring of the side fill resin composition can be promoted more smoothly. When the photocationically polymerizable compound (A1) contains an epoxy resin and an oxetane resin, the mass ratio of the epoxy resin to the total amount of the epoxy resin and the oxetane resin is preferably 5 mass% or more and 95 mass% or less. In this case, the photocuring of the side fill resin composition can be promoted more smoothly. The photocationically polymerizable compound (A1) is not limited to the above, and may be a monomer or oligomer having appropriate cationic polymerizability.
[0035] The mass proportion of the photocationically polymerizable compound (A1) in the photocurable component (A) is preferably from 5 mass % to 100 mass % based on the total amount of the photocurable component (A).
[0036] The mass proportion of the oxetane resin in the photocationically polymerizable compound (A1) is preferably from 5 mass % to 100 mass % based on the total amount of the photocurable component (A).
[0037] The mass proportion of the oxetane resin in the photocurable component (A) is preferably from 5 mass % to 100 mass % based on the total amount of the photocurable component (A).
[0038] The mass proportion of the vinyl ether resin in the photocurable component (A) is preferably from 0 mass % to 30 mass % based on the total amount of the photocurable component (A).
[0039] In addition, the components that can be contained in the photopolymerizable component (A) in the side fill resin composition are not limited to those explained above, and the composition may contain resins other than those mentioned above.
[0040] [Photopolymerization initiator (B)] The photopolymerization initiator (B) can promote the curing reaction of the photocurable component (in this embodiment, the photopolymerizable component (A)) in the sidefill resin composition.
[0041] The photopolymerization initiator (B) preferably contains a cationic photopolymerization initiator (B1). That is, the sidefill resin composition preferably contains a cationic photopolymerization initiator (B1). In this case, the repairability of the sidefill material 4 in the semiconductor device 1 produced from the sidefill resin composition can be further improved. In particular, when the sidefill resin composition contains a cationic photopolymerization initiator (B1), the sidefill resin composition is preferably made of a cationic photopolymerization initiator (B1). compound (A1) and mosquito Thion light It is preferable that the resin composition contains a photocationically polymerizable compound (A1) and a cationic photopolymerization initiator (B1). In this case, the side fill material 4 made of a cured product produced from the side fill resin composition can be removed more easily in the semiconductor device 1. This is believed to be due to the following reasons. When the side fill resin composition containing the photocationically polymerizable compound (A1) and the cationic photopolymerization initiator (B1) is cured, an acid component by-produced from the cationic photopolymerization initiator (B1) remains in the cured product. When this cured product is heated to a higher temperature, the acid component reacts with the cured product, and the cured product is thermally decomposed. This is presumably because the physical properties of the cured product are reduced and it becomes easier to peel off.
[0042] When the side fill resin composition contains a cationic photopolymerization initiator (B1), the mass ratio of the cationic photopolymerization initiator (B1) to the photopolymerizable component (A) is preferably 0.01 mass% or more and 5 mass% or less, more preferably 0.1 mass% or more and 3 mass% or less, and even more preferably 0.5 mass% or more and 2 mass% or less.
[0043] [Inorganic filler (C)] The resin composition for side fill material preferably further contains an inorganic filler (C). When the resin composition for side fill contains the inorganic filler (C), the coefficient of thermal expansion (CTE) of the cured product made from the resin composition for side fill can be reduced. Therefore, even if the resin composition for side fill is interposed between the substrate 2 of the semiconductor device 1 and the peripheral portion of the surface of the mounting component 3 facing the substrate 2, and the substrate 2 and the mounting component 3 are reinforced with the cured product, the side fill material 4 is less likely to warp. This makes it possible to further reduce the occurrence of defects due to heat generation, etc., of the semiconductor device 1.
[0044] When the inorganic filler (C) is contained, the mass ratio of the inorganic filler (C) to the total solid content of the side fill resin composition is preferably 30% by mass or more and 90% by mass or less. In this case, it is easier to lower the CTE of the cured product produced from the side fill resin composition. The mass ratio of the inorganic filler (C) to the total solid content of the side fill resin composition is more preferably 40% by mass or more and 80% by mass or less, and even more preferably 50% by mass or more and 75% by mass or less.
[0045] The inorganic filler (C) includes at least one material selected from the group consisting of, for example, silica, alumina, clay, mica, talc, aluminum hydroxide, magnesium hydroxide, calcium carbonate, and glass. The silica may be, for example, fused silica, crystalline silica, fumed silica, etc.
[0046] When the inorganic filler (C) contains silica, the silica may be surface-treated. If the silica is surface-treated, the photocurable component in the sidefill resin composition and the silica can be easily mixed, and the dispersibility of the sidefill resin composition can be improved. The surface treatment of the silica can be achieved, for example, by treating the silica with a silane coupling agent. Examples of the silane coupling agent include compounds having at least one functional group selected from the group consisting of an epoxy group, an amino group, a (meth)acryloyl group, and a phenyl group.
[0047] The average particle size of the inorganic filler (C) is preferably, for example, 2.5 μm or more and 200 μm or less. When the average particle size of the inorganic filler (C) is within this range, the side-fill resin composition can maintain better fluidity when it is interposed between the substrate 2 and the peripheral portion of the surface of the mounting component 3 facing the substrate 2. Here, the "average particle size" in the present disclosure is the median diameter D50. The median diameter D50 is calculated from the particle size distribution obtained by measurement using a laser diffraction / scattering method. The particle size distribution can be measured, for example, using a laser diffraction particle size distribution measuring device.
[0048] [Other ingredients] The side fill resin composition may contain components other than the components described above as long as the effects of the present disclosure are not impaired. For example, the side fill resin composition may contain a resin component other than the resin described above.
[0049] The encapsulating resin composition may contain an appropriate additive. Examples of the additive include a curing agent, a flux, a viscosity modifier, a surface modifier, a silane coupling agent, an antifoaming agent, a leveling agent, a stress reducing agent, and a pigment. For example, the side fill resin composition may contain a thixotropy imparting agent. In this case, when the side fill resin composition is supplied to the peripheral portion of the surface of the mounting component 3 facing the substrate 2 between the substrate 2 and the mounting component 3 of the semiconductor device 1, it is easy to ensure better fluidity and thixotropy of the side fill resin composition. This allows the side fill resin composition to have higher moldability, and even if the side fill material 4 that reinforces the peripheral portion of the mounting component 3 is produced from the side fill resin composition, the side fill material 4 can be given excellent strength.
[0050] It is also preferable that the side fill resin composition contains a photosensitizer. In this case, the curing reaction of the side fill resin composition can be accelerated. Therefore, when producing a cured product from the side fill resin composition, the takt time can be shortened.
[0051] It is preferable that the side fill resin composition does not contain an organic solvent, or the content of the organic solvent is 0.5 mass % or less.
[0052] The resin composition for side fill can be obtained, for example, by blending the above-mentioned components and adding appropriate additives as necessary. Specifically, the resin composition for side fill can be prepared, for example, by the following method.
[0053] First, the components that can be contained in the resin composition for side fill described above are mixed simultaneously or sequentially to obtain a mixture. The mixture is stirred and mixed while being subjected to a heating treatment or a cooling treatment as necessary.
[0054] Next, additives are added to the mixture as necessary, and the mixture is stirred again while being heated or cooled as necessary until it is uniformly dispersed. This allows the side fill resin composition to be obtained. For stirring the mixture, for example, a disperser, a planetary mixer, a ball mill, a three-roll mill, a bead mill, and the like can be used in appropriate combination as necessary.
[0055] The viscosity of the side-fill resin composition at 25°C is preferably 1000 Pa·s or less. In this case, the moldability of the side-fill resin composition is easily ensured. In addition, in this case, good filling properties can be achieved between the substrate 2 and the peripheral portion of the surface of the mounting component 3, such as a semiconductor chip, facing the substrate 2. The viscosity of the side-fill resin composition at 25°C can be measured using a B-type viscometer under the conditions of a rotor No. 7, a rotation speed of 1 to 50 rpm, and a measurement time of 60 to 180 seconds. The viscosity of the side-fill resin composition at 25°C is more preferably 500 Pa·s or less, and even more preferably 200 Pa·s or less.
[0056] The thixotropic index of the side fill resin composition at 25°C is preferably 2 or more. In this case, the moldability of the side fill resin composition is easily ensured. The thixotropic index of the side fill resin composition at 25°C is more preferably 3 or more. The thixotropic index of the side fill resin composition at 25°C can be calculated by dividing the viscosity value measured with a B-type viscometer using a rotor No. 7 at a rotation speed of 1 rpm by the viscosity at a rotation speed of 10 rpm.
[0057] As already described, the side fill resin composition of this embodiment has photocurability. Therefore, the side fill resin composition can be cured by irradiating light. The conditions for irradiating light, such as the irradiation wavelength of light, the irradiation intensity (amount of light), and the irradiation time of light, may be appropriately adjusted according to the type of component (e.g., photocurable component (A)) that can be contained in the side fill resin composition and the type of polymerization initiator (e.g., photopolymerization initiator (B)). The light source for irradiating the side fill resin composition with light can be an appropriate light source, and may be at least one light source selected from the group consisting of, for example, a chemical lamp, a low pressure mercury lamp, a medium pressure mercury lamp, a high pressure mercury lamp, an ultra-high pressure mercury lamp, a xenon lamp, a metal halide lamp, an LED, a YAG, g-line (436 nm), h-line (405 nm), i-line (365 nm), and a combination of two or more of g-line, h-line, and i-line. The light source is not limited to these, and may be any light source that can irradiate ultraviolet light that can cure the side fill resin composition.
[0058] The glass transition temperature (Tg) of the cured product of the resin composition for side fill is preferably 130°C or higher. If the glass transition temperature is 130°C or higher, the cured product of the resin composition for side fill can have heat resistance. The glass transition temperature can be measured, for example, by TMA (Thermomechanical Analysis). In addition, if the glass transition temperature is 130°C or higher, the cured product of the resin composition for side fill can be prevented from softening even in a high temperature range (for example, around 125°C) in a heat cycle test. Therefore, the resin composition for side fill can ensure high heat resistance reliability in the semiconductor device 1. In particular, in the semiconductor device 1, when the mounted components on the board are reinforced with a side fill material made of a cured product of a conventional resin composition, there was a problem that poor conduction is likely to occur between the board and the mounted components when the semiconductor device 1 is placed in a severe thermal environment (for example, below -40°C and above 125°C). In contrast, when a side fill material for reinforcing the mounted components 3 on the substrate 2 in the semiconductor device 1 is produced from the side fill resin composition of this embodiment, the cured product of the side fill resin composition can impart high thermal shock resistance to the semiconductor device 1.
[0059] The coefficient of linear expansion (CTE) of the cured product of the sidefill resin composition below the glass transition temperature Tg is also preferably less than 40 ppm / °C. In this case, below the glass transition temperature, the sidefill material 4 made of the cured product of the sidefill resin composition is less likely to warp, and the cured product of the sidefill resin composition is less likely to peel off from the substrate 2 and the mounting components 3. Therefore, the cured product of the encapsulating resin composition is less likely to crack. Therefore, the sidefill material 4 made from the sidefill resin composition can further improve the heat resistance reliability of the semiconductor device 1. The CTE of the cured product of the sidefill resin composition below the Tg is more preferably 35 ppm / °C or less, and even more preferably 30 ppm / °C or less. The CTE of the cured product of the sidefill resin composition below the Tg can be obtained by calculating the slope of the tangent based on the dimensional change between any two temperatures below the Tg.
[0060] The shear strength of the cured product of the side-fill resin composition at 125°C is preferably 3 MPa or more, and the shear strength at 200°C is preferably less than 0.1 MPa. When the shear strength of the cured product at 125°C is 3 MPa or more, the adhesive strength of the cured product is unlikely to decrease up to a temperature range near the Tg of the cured product, so that the stress in the solder bump due to thermal shock can be suppressed. In other words, the dimensional change due to heating of the cured product of the side-fill resin composition is unlikely to occur. Therefore, the side-fill resin composition of this embodiment can impart superior heat resistance reliability to the semiconductor device 1, for example, in a temperature cycle (heat cycle) from a low temperature range of about -40°C to a high temperature range of about 125°C. On the other hand, when the shear strength at 200°C is less than 0.1 MPa, the adhesive strength of the cured product of the side-fill resin composition decreases at a temperature in a repair work, for example, a heating temperature of about 240°C, so that when a defect occurs in the semiconductor device 1, only the defective part can be easily replaced. That is, the cured product of the side-fill resin composition can be easily removed from the substrate 2 in the semiconductor device 1, and the semiconductor device 1 can be repaired. Therefore, the cured product of the side-fill resin composition of this embodiment can provide excellent repairability. The shear strength of the cured product of the side-fill resin composition of this embodiment is the adhesion strength of the cured product to the substrate measured by a bond tester when the side-fill resin composition is cured on a solder resist-treated glass epoxy substrate. Specifically, the shear strength of the side-fill resin composition can be obtained as follows. First, a solder resist layer is prepared on an appropriate glass epoxy substrate. In this embodiment, the glass epoxy substrate is more specifically FR4 (board thickness 0.6 mm) manufactured by Panasonic Corporation. The solder resist layer is prepared from an appropriate solder resist composition, cured by UV curing, heat curing, or the like, and then subjected to a development treatment such as alkaline development, as necessary.The composition of the solder resist composition may be, for example, a two-liquid type liquid solder resist composition consisting of an active energy ray curable resin obtained by adding a saturated or unsaturated polybasic acid anhydride to a reaction product of a novolac type epoxy compound and an unsaturated monocarboxylic acid, a photopolymerization initiator, a diluent, and an epoxy compound. Specifically, for example, it is prepared from a resist PSR4000 manufactured by Taiyo Ink Mfg. Co., Ltd. The method of preparing the solder resist layer is not limited to the above, and for example, the solder resist composition may be composed of either one-liquid or two-liquid. The curing of the solder resist composition may be either heat curing, photo curing, or a combination of heat curing and photo curing. The solder resist composition may be in the form of a liquid or a dry film. The glass epoxy substrate can be covered with a solder resist layer by treating the glass epoxy substrate with this resist. Next, a side fill resin composition is applied onto the solder resist layer and then photo cured to prepare a cured product of the side fill resin composition on the solder resist layer. As already mentioned, the photocuring conditions of the side fill resin composition can be appropriately adjusted depending on the components that can be contained in the side fill resin composition, but the curing conditions of the side fill resin composition for measuring the shear strength of the cured product of the side fill resin composition are an irradiation wavelength of 365 nm and a light irradiation intensity (light amount) of 1000 mW / cm. 2The exposure time is 4 seconds. Next, the solder resist layer on the glass epoxy substrate and the cured product on the solder resist layer are heated to 125°C or 200°C, and the adhesion strength between the cured product and the solder resist layer is measured by a bond tester. The measurement conditions are a test height (distance between the substrate surface and the tip of the measuring tool) of 50 μm and a test speed of 500 μm / s, and the measurement sample is a cylindrical cured product with a diameter of 3 mm and a height of 1 mm. The heating is controlled by the stage temperature of the device. This allows the shear strength of the cured product of the side-fill resin composition to be obtained. For the bond tester, a measuring device such as Nordson Advanced Technology Co., Ltd.'s product name Nordson DAGE 4000 Optima can be used. Note that the above description is the condition for measuring the shear strength of the cured product of the side-fill resin composition specified in this embodiment, and is not intended to limit the target to which the side-fill resin composition is applied to the solder resist layer.
[0061] As described above, the side-fill resin composition of the present embodiment can be suitably used as a side-fill material. The side-fill resin composition can be suitably used as a post-supply type side-fill material in flip chip mounting.
[0062] [Semiconductor Devices] As described above, the side-fill resin composition according to the present embodiment can be suitably used to prepare a side-fill material 4 that reinforces the substrate 2 and the mounting component 3 in the semiconductor device 1. In particular, the side-fill resin composition can reinforce the substrate 2 and the mounting component 3 to make the mounting component 3 less likely to come off and to make poor conduction less likely to occur by simply supplying the side-fill resin composition between the substrate 2 and the peripheral portion of the surface of the mounting component 3 facing the substrate 2, so that the amount of resin composition to be supplied can be reduced compared to an underfill material that fills the entire gap between the substrate 2 and the mounting component 3. Furthermore, in the case of a connection failure occurring between the substrate 2 and the mounting component 3 in the semiconductor device 1, only the side-fill material 4 that supports the substrate 2 and the mounting component 3 (specifically, the side-fill material 4 interposed in the peripheral portion of the mounting component 3) needs to be peeled off, so that the semiconductor device 1 can be repaired without discarding the normal portion of the member. The side-fill material 4 of the present embodiment can be easily removed without heating to an excessively high temperature. Therefore, the side fill material 4 produced from the side fill resin composition of the present embodiment has excellent repairability in the semiconductor device 1. Furthermore, as described above, when repairing the semiconductor device 1, it is possible to reduce the waste of parts other than the defective parts, and therefore, compared to the underfill material, it can also contribute to reducing costs when defects occur.
[0063] The semiconductor device 1 of this embodiment includes a base material 2, a mounting component 3, and a side fill material 4. The mounting component 3 is surface-mounted on the base material 2. The side fill material 4 is interposed between the mounting component 3 and the peripheral edge of the surface facing the base material 2. The side fill material 4 is made of a cured product of the side fill resin composition described above.
[0064] 1 shows an example of a semiconductor device 1 according to this embodiment. The semiconductor device 1 includes a base material 2 that supports a mounting component 3 such as a semiconductor chip, the mounting component 3 that is surface-mounted face-down on the base material 2, and a side fill material 4 that is interposed between the base material 2 and the mounting component 3, between the base material 2 and the peripheral portion of the surface of the mounting component 3 that faces the base material 2. The side fill material 4 can support the base material 2 and the mounting component 3 between the base material 2 and the peripheral portion of the mounting component 3.
[0065] The side fill material 4 is formed by supplying the side fill resin composition between the substrate 2 and the mounting component 3 to a part or all of the peripheral portion of the surface of the mounting component 3 facing the substrate 2, and photocuring the composition. The distance by which the side fill resin composition penetrates between the substrate 2 and the mounting component 3 to a position inside the surface of the mounting component 3 facing the substrate 2 in a plan view may be appropriately adjusted, but for example, the penetration distance is preferably more than 0% and 5% or less of the length dimension of the mounting component 3. The penetration distance is the length by which the side fill resin composition penetrates from a position corresponding to the outer periphery of the mounting component 3 in a plan view on the surface of the mounting component 3 facing the substrate 2 to a position inside the surface where the mounting component 3 and the substrate 2 face each other.
[0066] The semiconductor device 1 and the manufacturing method thereof will now be described in detail.
[0067] The semiconductor device 1 includes a substrate 2 having conductor wiring 21, a mounting component 3 such as a semiconductor chip having bump electrodes 33 and mounted on the substrate 2 by bonding the bump electrodes 33 to the conductor wiring 21, and a side fill material 4. The side fill material 4 is a cured product of the side fill resin composition described above.
[0068] The substrate 2 is, for example, a mother substrate, a package substrate, or an interposer substrate. For example, the substrate 2 includes an insulating substrate made of glass epoxy, polyimide, polyester, ceramic, or the like, and conductor wiring 21 made of a conductor such as copper formed on the surface of the insulating substrate. The conductor wiring 21 includes, for example, an electrode pad.
[0069] The mounting component 3 is, for example, a semiconductor chip. The semiconductor chip is, for example, a flip-chip type chip such as a BGA (ball grid array), an LGA (land grid array), or a CSP (chip size package). The semiconductor chip may be a PoP (package on package) type chip.
[0070] The mounting component 3 may include a plurality of bump electrodes 33. The bump electrodes 33 include solder. For example, as shown in Fig. 1, the bump electrodes 33 include a pillar 31 and a solder bump 32 provided at the tip of the pillar 31. The solder bump 32 is made of solder, and therefore the bump electrodes 33 include solder. The pillars 31 are made of copper, for example.
[0071] The melting point of the solder (for example, the solder in the solder bump 32) of the bump electrode 33 is not particularly limited, but may be a temperature that can melt at or below the mounting temperature (for example, 220 to 260°C) when mounting the mounting component 3 such as a semiconductor chip. The composition of the solder is not particularly limited and may be an appropriate composition, for example, Sn-Ag solder and Sn-Ag-Cu solder. The structure of the bump electrode 33 with solder is not limited to the above, and for example, the bump electrode 33 may have only a spherical solder bump 32 (solder ball). In other words, the bump electrode 33 does not need to have a pillar.
[0072] 1, the side fill material 4 fills only the gap between the substrate 2 and the mounting component 3, and between the substrate 2 and a part of the peripheral edge of the surface of the mounting component 3 facing the substrate 2. As a result, the side fill material 4 reinforces the mounting component 3 surface-mounted on the substrate 2 at the peripheral edge of the mounting component 3.
[0073] An example of a method for manufacturing the semiconductor device 1 will be described below. The method for manufacturing the semiconductor device 1 is not limited to the method described below, and it is sufficient that the above-described side-fill resin composition is supplied to the semiconductor device 1 so as to be interposed in a part or the whole of the peripheral portion of the surface of the mounting component 3 that is surface-mounted on the substrate 2 and faces the substrate 2.
[0074] First, a substrate 2 having conductor wiring 21 and a mounting component 3 having bump electrodes 33 are prepared, the mounting component 3 is placed on the substrate 2, and the bump electrodes 33 are placed on the conductor wiring 21. The conductor wiring 21 and the bump electrodes 33 may be electrically connected by, for example, heating.
[0075] Next, the side fill resin composition is supplied to the peripheral portion of the surface of the mounting component 3 that faces the base material 2, which is surface-mounted on the base material 2, and then the supplied side fill resin composition is irradiated with light to cure the side fill resin composition. This produces a side fill material 4 on the base material 2 and the peripheral portion of the mounting component 3 that faces the base material 2. The curing conditions for the side fill resin composition are as already described.
[0076] The above order does not have to be as described above. As long as the side-fill resin composition can be disposed so as to be interposed between the substrate 2 and a part or the whole of the peripheral portion of the surface of the mounting component 3 facing the substrate 2 during the manufacturing process, the side-fill resin composition may be disposed at any time and in any position on the mounting component 3 and the substrate 2.
[0077] 2A to 2C, specific examples of positions where the side fill material 4 is disposed in the semiconductor device 1 will be described. However, the positions of the side fill material 4 in the semiconductor device 1 are not limited to these.
[0078] In FIG. 2A to FIG. 2C, in a plan view, in the semiconductor device 1, a side-fill resin composition is supplied between the substrate 2 and the peripheral portion of the surface of the mounting component 3 mounted on the substrate 2, facing the substrate 2, and cured to produce a side-fill material 4. That is, FIG. 2A to FIG. 2C show examples (first to third examples) of a state in which the substrate 2 and the peripheral portion of the mounting component 3 are reinforced with the side-fill material 4. In the semiconductor device 1 shown in FIG. 2A to C, the side-fill resin composition is not supplied to the back of the gap between the substrate 2 and the mounting component 3, for example, the entire portion including the lower center portion of the mounting component 3. This is because the side-fill resin composition of this embodiment can reinforce the substrate 2 and the mounting component 3 in the semiconductor device 1 even if it is only supplied to the peripheral portion of the mounting component 3. In particular, the side-fill material 4 produced from the side-fill resin composition supports the peripheral portion of the mounting component 3 in the semiconductor device 1. Therefore, the mounting component 3 is less likely to warp.
[0079] In the first example shown in Fig. 2A, a side fill material 4 made of a cured product of a side fill resin composition is formed on the entire periphery of the surface of the mounting component 3 facing the base material 2. In this case, the strength reinforcing the base material 2 and the mounting component 3 in the semiconductor device 1 can be increased, and warping of the base material 2 and the mounting component 3 can be made less likely to occur. Furthermore, in this case, repairs in the event of a defect in the semiconductor device 1 are easier than in the case of an underfill material.
[0080] In the second example shown in Fig. 2B, a side fill material 4 made of a cured product of a side fill resin composition is formed on the substrate 2 and on multiple corners (more specifically, on the four corners of the mounting component 3, which is substantially rectangular in plan view) of the peripheral portion of the surface of the mounting component 3 facing the substrate 2. In this case, the strength reinforcing the substrate 2 and the mounting component 3 in the semiconductor device 1 can be maintained, and warping of the substrate 2 and the mounting component 3 can be made less likely to occur. Furthermore, in this case, it is easier to repair a defect in the semiconductor device 1 than in the case of an underfill material.
[0081] In the third example shown in Fig. 2C, a side fill material made of a cured product of a side fill resin composition is formed on the corners of the peripheral portion of the surface of the mounting component 3 facing the base material 2 and on two opposing sides. In this case, the strength reinforcing the base material 2 and the mounting component 3 in the semiconductor device 1 can be maintained, and warping of the base material 2 and the mounting component 3 can be made less likely to occur. Furthermore, in this case, repairs in the event of a defect in the semiconductor device 1 are easier than in the case of an underfill material.
[0082] In this embodiment, a method for removing the side fill material will be described.
[0083] In the method for removing the side fill material of the present embodiment, the side fill material in the semiconductor device 1 is heated to 200° C. or higher, and the side fill material 4 is removed from between the periphery of the mounted component 3 and the base material 2. In repairing a defective portion of the semiconductor device 1, it is necessary to melt the solder material such as the solder bumps 32 in order to remove the electrical connection between the base material 2 and the mounted component 3. In this embodiment, the side fill material 4 can be removed by heating to the melting temperature (approximately 200° C.) or higher of the solder material. Therefore, according to the method for removing the side fill material 4 of the present embodiment, the semiconductor device 1 can be easily repaired. EXAMPLES
[0084] Specific examples of the present disclosure will be presented below, but the present disclosure is not limited to the examples.
[0085] 1. Preparation of resin composition for side fill material [Examples 1 to 9 and Comparative Examples 1 to 3] The components shown in Table 1 below were charged into a planetary mixer in the mixing ratios (parts by mass) shown in Table 1, stirred and mixed, and uniformly dispersed using a three-roll mill to obtain a resin composition. Details of the components shown in Table 1 are as follows. (Photopolymerizable component) Epoxy resin 1: DIC Corporation, product name: Epiclon 840A. Epoxy resin 2: Made by Daicel Corporation. Product name: Celloxide 2021. Epoxy resin 3: Nagase ChemteX Corporation, product name EX-192. -Oxetane resin: Toagosei Co., Ltd. Product name: OXT-221. (Polymerization initiator) Photopolymerization initiator 1: San-Apro Ltd. Product name CPI-200K. Photopolymerization initiator 2: WPI-170 manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. (Others (additives, etc.)) Photosensitizer: Fujifilm Wako Pure Chemical Industries, Ltd. Product name: 2-Isopropylthioxanthone. Heat hardener 1: Acid anhydride (DIC Corporation product name B650). -Heat curing agent 2: Imidazole (2MAOK manufactured by Shikoku Chemical Industry Co., Ltd.). Inorganic filler: Denka Co., Ltd. Product name QS-6 (30μm cut). Thixotropic agent: Nippon Aerosil Co., Ltd., product name RY200. -Flexibility enhancer: Kuraray Co., Ltd. Product name LBR-302.
[0086] 2.Evaluation Test 2.1. Glass transition temperature and loss modulus (elastic modulus when hot) In Examples 1 to 9, the side fill resin composition prepared in 1 above was irradiated with an LED UV irradiator (Model Aicure UD40, manufactured by Panasonic Industrial Devices SUNX Co., Ltd.) at an illuminance of 1000 mW / cm 2 The resin composition was irradiated with light for 4 seconds under the conditions of and cured. The obtained cured product of the resin composition for side fill was cut into a size of 5 mm in width, 50 mm in length, and 0.2 mm in thickness to prepare a test piece. In Comparative Examples 1 to 3, the resin composition for side fill was cured by heating under the conditions of a heating temperature of 150°C and a heating time of 1 hour. The obtained cured product of the resin composition for side fill was cut into a size of 5 mm in width, 50 mm in length, and 0.2 mm in thickness to prepare a test piece.
[0087] The prepared test pieces were measured in bending mode using a viscoelasticity spectrometer (Model DMA7100, Hitachi High-Tech Science Corporation), and the glass transition temperature and hot elastic modulus were calculated by the DMA method. The glass transition temperatures (℃) of the cured products obtained are shown in Table 1.
[0088] 2.2. Linear expansion coefficient (α1) In Examples 1 to 9, photocuring was performed under the same light irradiation conditions as in 2.1 above to obtain a cured product of the side fill resin composition, which was then cut to a width of 3 mm, a length of 15 mm, and a thickness of 3 mm to prepare a test piece. In Comparative Example 1, heat curing was performed under the same heating conditions as in 2.1 above to obtain a cured product of the side fill resin composition, which was then cut to a width of 3 mm, a length of 15 mm, and a thickness of 3 mm to prepare a test piece.
[0089] The test pieces were heated at a temperature rise rate of 5°C / min at measurement temperatures of 30 to 260°C using a thermal analyzer (Model TMA7100, Hitachi High-Tech Science Corporation), and the linear expansion coefficient was calculated by the TMA method. The linear expansion coefficient (ppm / °C) of the cured product thus obtained is shown in Table 1.
[0090] 2.3.Repairability A test piece having a cured product of the side-fill resin composition on the substrate was prepared by applying 10 mg of the side-fill resin composition prepared in 1. above onto a solder resist-treated glass epoxy substrate (substrate: Panasonic Corporation, FR4, plate thickness 0.6 mm / resist: Taiyo Ink Mfg. Co., Ltd. PSR4000) and curing the composition. The curing conditions for Examples 1 to 9 were the same as the light irradiation conditions in 2.1 above, and for Comparative Examples 1 to 3, the heating conditions were the same as those in 2.1 above.
[0091] The test piece was placed on a hot plate and heated for 10 minutes so that the surface temperature of the substrate reached 200°C. The cured product was then peeled off from the substrate using a bamboo skewer. The condition of the cured product and the substrate were visually inspected and evaluated according to the following criteria. The results are shown in Table 1. A: The cured product can be peeled off from the substrate, and no residue of the cured product remains on the substrate. B: The cured product can be peeled off from the substrate, but a residue of the cured product remains on the substrate. C: The cured product could not be peeled off from the substrate, and remained on the substrate.
[0092] 2.4. Temperature cycle (TC) properties A TEG (Test Element Group) was prepared by mounting an IC chip (WLP TEG <0.3 mm pitch BGA>, 6 mm, manufactured by Waltz) on an FR-4 circuit board (WALTS KIT WLP300P, manufactured by Waltz) having daisy chain electrodes. The side fill resin composition prepared in 1. above was applied between the substrate and the peripheral portion of the surface of the IC chip facing the substrate in the TEG, so as to have a width of 0.8 mm and a height of 0.4 mm, so as to have a planar shape shown in FIG. 2B. The length of the contact portion between the side fill resin composition and the IC chip was set to 2.5 mm. The applied side fill resin composition was cured to prepare a test piece having a cured product of the side fill resin composition on the TEG. The curing conditions were the same as the light irradiation conditions in 2.1 above for Examples 1 to 9, and the same as the heating conditions in 2.1 above for Comparative Examples 1 to 3.
[0093] The prepared test specimens were subjected to a total of 2000 temperature cycles in a gas phase, with one cycle being -40°C for 30 minutes and 125°C for 30 minutes, using a thermal shock tester (Model TSE-12-A, manufactured by Espec Corporation). Operation was confirmed by measuring the resistance of the test specimens every 100 cycles. Test specimens whose resistance had increased by 10% or more from the start of the test were determined to be inoperable, and were evaluated according to the following criteria. The results are shown in Table 1. A: No malfunction occurs even after 2000 cycles. B: Malfunction occurs between 500 and 2000 cycles. C: Malfunction occurs within less than 500 cycles.
[0094] 2.5. Thixotropy test The side fill resin composition prepared in 1 above was placed in a cylindrical container, and the viscosity was measured using a B-type viscometer (Toki Sangyo, model number TVB10) with rotor No. 7, a rotation speed of 10 rpm, and a measurement time of 60 seconds. The thixotropic index was calculated by dividing the viscosity value at 1 rpm by the viscosity value at 10 rpm.
[0095] 2.6. Adhesion strength (shear strength) test A solder resist layer was prepared by treating a glass epoxy board (base material: Panasonic Corporation's FR4 board thickness 0.6 mm) with a resist (Taiyo Ink Mfg. Co., Ltd.'s PSR4000). This produced a glass epoxy board covered with a solder resist layer. Next, a 1 mm thick silicon plate with a circular hole with a diameter of 3 mm was placed on the produced board, and the side-fill resin composition produced in 1 above was filled into the hole and cured. The silicon plate was then removed to produce a test piece for measuring shear strength. The side-fill resin composition was cured using an LED UV irradiator (Panasonic Industrial Devices SUNX Co., Ltd.'s Model Aicure UD40) under the curing conditions of an irradiation wavelength of 365 nm and a light irradiation intensity (light amount) of 1000 mW / cm. 2 , the exposure time is 4 seconds.
[0096] The shear strength of the prepared test pieces was measured using a bond tester (Nordson DAGE 4000 Optima) under the conditions of a load cell S of 200KG, a test height of 50 μm, and a test speed of 500 μm / s.
[0097] [Table 1] [Explanation of symbols]
[0098] 1 Semiconductor device 2 Base material 3. Mounting parts 4 Side fill material
Claims
1. A side-fill resin composition used for producing a side-fill material interposed between a substrate and a peripheral portion of a surface of a mounting component that is surface-mounted on the substrate and faces the substrate, It has light curing properties, When the side fill resin composition is cured on a solder resist-treated glass epoxy substrate to produce a cured product, the shear strength of the cured product against the substrate, as measured by a bond tester, is 3 MPa or more when the temperature of the cured product is 125° C., and is 0.3 MPa or less when the temperature of the cured product is 200° C. Resin composition for side fill.
2. The glass transition temperature of the cured product is 130° C. or higher, and the linear expansion coefficient of the cured product at a temperature equal to or lower than the glass transition temperature is less than 40 ppm / ° C. The resin composition for side fill according to claim 1.
3. A composition comprising a photocationically polymerizable compound (A1) and a cationic photopolymerization initiator (B1), The resin composition for side fill according to claim 1 or 2.
4. Contains an inorganic filler (C), The resin composition for a side fill according to any one of claims 1 to 3.
5. A substrate, a mounting component to be surface-mounted on the substrate, and a side fill material interposed between the substrate and a peripheral portion of a surface of the mounting component facing the substrate, The side fill material is made of a cured product of the side fill resin composition according to any one of claims 1 to 4. Semiconductor device.
6. In the semiconductor device according to claim 5, the side fill material is heated to 200°C or higher, and the side fill material is removed from between the peripheral portion of the mounting component and the substrate. How to remove side fill material.
Citation Information
Patent Citations
Mounting method for semiconductor device
JP1996213428A
Semiconductor device with hollow structure
JP2004273554A
Side filling material for flip chip mounting, and semiconductor device
JP2005105243A
Flame-retardant sidefill material for mounting and semiconductor device
JP2009007467A
Semiconductor device
JP2013102167A