Manufacturing method of brazing sheet
The method addresses flux-related issues in brazing by using a specific Al-Si-Mg alloy and inorganic acid etching to enhance brazing properties and productivity in flux-free brazing processes.
Patent Information
- Application Number
- JP2020069976
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-04-08
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2040-04-08
AI Technical Summary
Existing brazing methods for aluminum materials face issues such as flux residue, high equipment costs, reduced productivity, and poor brazing properties, particularly in flux-free and vacuum brazing processes.
A method for manufacturing a brazing sheet involving lamination, hot rolling, cold rolling, and etching with an inorganic acid-based etching solution to create a clad plate with an Al-Si-Mg alloy, ensuring excellent brazing properties without flux, using specific chemical compositions and etching processes to weaken the oxide film.
The method produces a brazing sheet with enhanced brazing properties and improved productivity, reducing flux-related issues and maintaining quality in flux-free brazing atmospheres.
Smart Images

Figure 0007591872000004 
Figure 0007591872000001 
Figure 0007591872000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a brazing sheet. [Background technology]
[0002] Aluminum products such as heat exchangers and machine parts have many parts made of aluminum materials (including aluminum and aluminum alloys; the same applies below). These parts are often brazed with a brazing sheet having a core material and a brazing material applied on at least one surface of the core material. The core material of the brazing sheet is generally made of an aluminum alloy with a solidus temperature of 620°C or higher. The brazing material is made of an Al-Si (aluminum-silicon) alloy with a solidus temperature of about 577°C.
[0003] A commonly used brazing method for aluminum materials is the flux brazing method, in which flux is applied to the surfaces of the parts to be joined, that is, the parts to be joined by brazing, before brazing. However, when brazing is performed using the flux brazing method, the flux and its residue adhere to the surface of the aluminum product after brazing is completed. Depending on the application of the aluminum product, these fluxes and their residues may cause problems. Furthermore, pickling is required to remove the flux and its residues, and in recent years, the cost burden of this treatment has become a problem.
[0004] To avoid the above problems associated with the use of flux, some aluminum products are brazed in a vacuum without applying flux to the surface of the parts to be joined, which is called vacuum brazing. However, the vacuum brazing method has problems such as lower productivity than the flux brazing method and the quality of the brazed joint is easily deteriorated. In addition, the brazing furnace used in the vacuum brazing method has higher equipment and maintenance costs than general brazing furnaces.
[0005] Therefore, a so-called flux-free brazing method has been proposed, in which brazing is performed in an inert gas atmosphere without applying flux to the surface of the parts to be joined. The core material of the brazing sheet and the brazing material used in the flux-free brazing method contain metal elements such as Mg (magnesium) that are more easily oxidized than Al (aluminum). These metal elements have the effect of destroying the oxide film that exists on the brazing sheet itself and on the surface of the mating material to be joined to the brazing sheet during brazing. In flux-free brazing, aluminum materials are brazed together by utilizing the effects of these metal elements.
[0006] Furthermore, Patent Document 1 proposes a method for producing a brazing sheet in which, after the brazing sheet is produced, an oxide film present on the surface is removed by etching. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Special Publication No. 2017-505231 Summary of the Invention [Problem to be solved by the invention]
[0008] However, the brazing sheet obtained by the manufacturing method described in Patent Document 1 may have poor brazeability depending on the chemical components of the core material and brazing material.
[0009] The present invention has been made in view of the above background, and aims to provide a method for manufacturing a brazing sheet having excellent brazing properties in flux-free brazing. [Means for solving the problem]
[0010] One aspect of the present invention is a method for producing a brazing sheet for brazing aluminum materials in an inert gas atmosphere without using a flux, A lamination process for producing a clad ingot including a core ingot made of an aluminum material and a brazing material ingot made of an Al-Si-Mg alloy and disposed on at least one surface of the core ingot; a hot rolling process for producing a clad plate including a core material made of the core material ingot and a brazing material made of the brazing material ingot and disposed on at least one surface of the core material ingot by hot rolling the clad ingot; A cold rolling step of subjecting the clad plate to one or more passes of cold rolling; In the cold rolling process, between passes of cold rolling or after completion of the cold rolling process, an inorganic acid is added. and salts containing iron ions and an etching step of etching the surface of the clad plate using an etching solution containing death, the Al-Mg-Si alloy constituting the brazing material ingot has a chemical composition comprising: Si: 3% by mass or more and 13% by mass or less, Mg: 0.1% by mass or more and 2.0% by mass or less, Bi: 0% by mass or more and 1.0% by mass or less, Li: 0% by mass or more and 0.30% by mass or less, Cu: 0% by mass or more and 2.0% by mass or less, Zn: 0% by mass or more and 6.5% by mass or less, Sn: 0% by mass or more and 0.10% by mass or less, In: 0% by mass or more and 0.10% by mass or less, Sr: 0% by mass or more and 0.030% by mass or less, Na: 0% by mass or more and 0.030% by mass or less, and Sb: 0% by mass or more and 0.030% by mass or less, with the balance being Al and unavoidable impurities; The core block is made of an aluminum alloy containing Mg: 0.10% by mass or more and 4.0% by mass or less and Si: more than 0% by mass and 1.0% by mass or less, The etching amount in the etching step was 0.05 g / m 2 More than 1g / m 2 Below is the The manufacturing method of the brazing sheet. Effect of the Invention
[0011] In the method for producing the brazing sheet, the clad ingot is subjected to hot rolling and cold rolling to produce a clad plate. A brazing material made of an Al-Si-Mg alloy is placed on at least one side of the clad plate. The surface of the clad plate is etched with an etching solution containing an inorganic acid and not containing fluorine atoms, thereby producing a brazing sheet with excellent brazing properties in flux-free brazing. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a side view of a test specimen used in a gap filling test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] <Lamination process> In the method for manufacturing the brazing sheet, first, a plurality of aluminum ingots are prepared, including a core ingot that will eventually become the core material of the brazing sheet and a brazing filler ingot that will eventually become the brazing filler of the brazing sheet. Then, a lamination process is performed in which these aluminum ingots are stacked in a desired order to produce a clad ingot. The stacking order and number of layers of the aluminum ingots in the clad ingot may be appropriately set according to the desired layer structure and number of layers of the brazing sheet.
[0014] For example, to obtain a brazing sheet having a two-layer structure including a core material and a brazing material laminated on one side of the core material, the clad ingot may be made of two aluminum ingots: a core material ingot and a brazing material ingot laminated on one side of the core material ingot. Similarly, to obtain a brazing sheet having a three-layer structure including a core material and a brazing material ingot laminated on both sides of the core material, the clad ingot may be made of three aluminum ingots: a core material ingot and a brazing material ingot laminated on both sides of the core material ingot.
[0015] In addition, when preparing the aluminum ingot, an aluminum ingot having a different chemical composition from the core material ingot and the brazing material ingot is prepared, and the aluminum ingot is layered on the core material ingot and the brazing material ingot to form a clad ingot, thereby obtaining a brazing sheet having layers different from the core material and the brazing material. For example, when preparing the aluminum ingot, an intermediate material ingot having a different chemical composition from the core material ingot and the brazing material ingot is prepared, and the core material ingot, the intermediate material ingot, and the brazing material ingot are layered in this order to form a clad ingot, thereby finally obtaining a brazing sheet having an intermediate material made of the intermediate material ingot between the core material and the brazing material. In addition, when preparing the aluminum ingot, a sacrificial anode material ingot made of an aluminum alloy having a lower natural electrode potential than the core material ingot is prepared, and the sacrificial anode material ingot, the core material ingot, and the brazing material ingot are layered in this order to form a clad ingot, thereby finally obtaining a brazing sheet having a brazing material layered on one side of the core material and a sacrificial anode material made of the sacrificial anode material ingot on the other side.
[0016] Each aluminum block contained in the clad ingot can be produced by a conventional method. Each aluminum block contained in the clad ingot may have the following configuration:
[0017] (Lump for heartwood) The core ingot is an aluminum ingot that becomes the core of the brazing sheet after the clad ingot is hot-rolled and cold-rolled. The aluminum material constituting the core ingot can be an aluminum material having a higher solidus temperature than the Al-Si-Mg alloy constituting the brazing material ingot. The core ingot may be made of, for example, JIS A1000 series aluminum, A3000 series alloy, A5000 series alloy, or A6000 series alloy.
[0018] More specifically, the core ingot may have a chemical composition consisting of Al and unavoidable impurities. The core ingot may also contain, in addition to Al and unavoidable impurities, one or more alloy elements selected from the group consisting of Mg (magnesium), Mn (manganese), Si (silicon), Fe (iron), Cu (copper), Zn (zinc), Ti (titanium), Cr (chromium) and Zr (zirconium). The chemical composition of the core in the brazing sheet is the same as that of the core ingot.
[0019] ·Mg: 0.10 mass% or more and 4.0 mass% or less The aluminum alloy constituting the core block contains 0.10% to 4.0% by mass of Mg. This allows A brazing sheet having a core material made of an aluminum alloy containing Mg can be obtained. The Mg in the core material diffuses and migrates to the brazing material due to heating during brazing. The Mg that migrates to the brazing material destroys the oxide film present on the surface of the brazing material and the surface of the mating material together with the Mg in the brazing material, thereby further improving the brazing property in flux-free brazing.
[0020] From the viewpoint of further improving brazing properties in flux-free brazing, the Mg content in the core ingot is preferably 0.20 mass% or more, more preferably 0.30 mass% or more, and even more preferably 0.40 mass% or more.
[0021] On the other hand, if the Mg content in the core ingot is excessively high, the amount of Mg that reaches the surface of the brazing material during brazing is likely to be large. If this Mg is oxidized on the surface of the brazing material, it may lead to deterioration of brazing properties. By setting the Mg content in the core ingot to 4.0 mass% or less, preferably 1.5 mass% or less, and more preferably 1.0 mass% or less, the amount of Mg oxide generated during brazing can be further reduced, and thus deterioration of brazing properties can be avoided.
[0022] ·Mn: 0.05 mass% or more and 1.60 mass% or less The aluminum alloy constituting the core ingot may contain 0.05% by mass to 1.60% by mass of Mn, in which case it is possible to obtain a brazing sheet having a core made of an aluminum alloy containing Mn.
[0023] By making the Mn content in the core ingot 0.05 mass% or more, preferably 0.30 mass% or more, and more preferably 0.60 mass% or more, the strength of the core in the brazing sheet can be further improved, and the potential of the core can be adjusted to further improve the corrosion resistance.
[0024] However, if the Mn content in the core ingot is excessively high, the core is more likely to crack during the manufacturing process of the brazing sheet. By setting the Mn content in the core ingot to 1.6 mass% or less, preferably 1.4 mass% or less, it is possible to avoid deterioration in the manufacturability of the brazing sheet.
[0025] ·Si: More than 0 mass% and 1.0 mass% or less The aluminum alloy constituting the core block contains more than 0 mass% and not more than 1.0 mass% Si. This willIn this way, a brazing sheet having a core material made of an aluminum alloy containing Si can be obtained. The Si in the core material of the brazing sheet has the effect of improving the strength of the core material. However, if the content of Si in the core material is excessively high, the melting point of the core material decreases, which may lead to deterioration of brazing properties. By setting the content of Si in the core material ingot to 1.0 mass % or less, preferably 0.7 mass % or less, and more preferably 0.5 mass % or less, it is possible to further improve the strength of the core material while avoiding deterioration of brazing properties.
[0026] Fe: More than 0% by mass and up to 1.0% by mass The aluminum alloy constituting the core ingot may contain Fe from more than 0% by mass to 1.0% by mass or less. In this case, a brazing sheet having a core made of an aluminum alloy containing Fe can be obtained. The Fe in the core of the brazing sheet has the effect of improving the strength of the core. However, if the content of Fe in the core is excessively high, the corrosion resistance of the core may deteriorate. In addition, in this case, large precipitates are likely to be formed in the core, which may lead to a decrease in the formability of the brazing sheet. By setting the content of Fe in the core ingot to 1.0% by mass or less, preferably 0.7% by mass or less, and more preferably 0.5% by mass or less, it is possible to further improve the strength of the core while avoiding these problems.
[0027] ·Cu: More than 0 mass% and 2.0 mass% or less The aluminum alloy constituting the core ingot may contain Cu in an amount of more than 0% by mass and not more than 2.0% by mass. In this case, a brazing sheet having a core made of an aluminum alloy containing Cu can be obtained. The Cu in the core has the effect of improving the strength of the core. In addition, Cu has the effect of adjusting the electric potential of the core and improving the corrosion resistance. However, if the content of Cu in the core is excessively high, intergranular corrosion is likely to occur. In addition, in this case, the melting point of the core is lowered, which may lead to deterioration of brazing properties. By setting the content of Cu in the core ingot to 2.0% by mass or less, preferably 1.0% by mass or less, and more preferably 0.5% by mass or less, it is possible to further improve the strength and corrosion resistance of the core while avoiding these problems.
[0028] ·Zn: More than 0 mass% and 6.5 mass% or less The aluminum alloy constituting the core block may contain Zn in an amount of more than 0% by mass and not more than 6.5% by mass. In this case, a brazing sheet having a core made of an aluminum alloy containing Zn can be obtained. The Zn in the core has the effect of making the natural electrode potential of the core less potent. By making the natural potential of the core less potent, the core can function as a sacrificial anode in the aluminum product after brazing. However, if the Zn content is excessively high, the natural electrode potential of the core will be excessively reduced, and the sacrificial corrosion protection effect may be impaired early. By making the Zn content in the core block not more than 6.5% by mass, the sacrificial corrosion protection effect of the core can be maintained for a longer period of time.
[0029] ·Ti: More than 0% by mass and 0.20% by mass or less The aluminum alloy constituting the core ingot may contain Ti in a range of more than 0% by mass to 0.20% by mass or less. In this case, a brazing sheet having a core made of an aluminum alloy containing Ti can be obtained. The Ti in the core causes the corrosion of the core to progress in layers, suppressing the progress of corrosion in the depth direction. However, if the Ti content is excessively high, huge precipitates are likely to be formed in the core ingot, which may lead to deterioration of the rolling properties in hot rolling and cold rolling. In this case, there is also a risk of the corrosion resistance of the core being deteriorated. By setting the Ti content in the core ingot to 0.20% by mass or less, it is possible to more effectively suppress the progress of corrosion in the depth direction of the core while avoiding such problems.
[0030] ·Cr: More than 0% by mass and 0.50% by mass or less The aluminum alloy constituting the core ingot may contain Cr from more than 0% by mass to 0.50% by mass or less. In this case, a brazing sheet having a core made of an aluminum alloy containing Cr can be obtained. Cr has the effect of increasing the crystal grain size of the core and suppressing the occurrence of erosion. However, if the Cr content in the core ingot is excessively high, cracks are likely to occur in the core during the manufacturing process of the brazing sheet. By setting the Cr content in the core ingot to 0.50% by mass or less, the occurrence of erosion can be more effectively suppressed while avoiding deterioration of the manufacturability of the brazing sheet.
[0031] ·Zr: More than 0 mass% and 0.50 mass% or less The aluminum alloy constituting the core ingot may contain more than 0% to 0.50% by mass of Zr. In this case, a brazing sheet having a core made of an aluminum alloy containing Zr can be obtained. Zr has the effect of increasing the crystal grain size of the core and suppressing the occurrence of erosion. However, if the Zr content in the core ingot is excessively high, cracks are likely to occur in the core during the manufacturing process of the brazing sheet. By setting the Zr content in the core to 0.50% by mass or less, the occurrence of erosion can be more effectively suppressed while avoiding deterioration of the manufacturability of the brazing sheet.
[0032] (Brazing lump) The brazing material ingot is an aluminum ingot that becomes the brazing material of the brazing sheet after the clad ingot is subjected to hot rolling and cold rolling. As the aluminum material constituting the brazing material ingot, an Al-Si-Mg alloy, which is an aluminum alloy containing Mg and Si, can be adopted. The brazing material ingot may be composed of an Al-Si-Mg alloy having chemical components containing, for example, 3.0 mass% to 13.0 mass% Si, 0.10 mass% to 2.0 mass% Mg, and the balance being Al and unavoidable impurities. The chemical components of the brazing material in the brazing sheet are the same as those of the brazing material ingot.
[0033] ·Si: 3.0 mass% or more and 13.0 mass% or less The Al-Si-Mg alloy constituting the brazing material ingot contains 3.0 mass% or more and 13.0 mass% or less of Si. There are By setting the Si content in the brazing filler metal ingot within the above-mentioned specific range, brazing properties in flux-free brazing can be further improved.
[0034] ·Mg: 0.10 mass% or more and 2.0 mass% or less The Al-Si-Mg alloy that constitutes the brazing material ingot contains 0.10 mass% to 2.0 mass% Mg. There areMg in the brazing filler metal has the effect of destroying the oxide film present on the surface of the brazing filler metal and the surface of the mating material during brazing. By making the Mg content in the brazing filler metal lump 0.10 mass% or more, more preferably 0.20 mass% or more, the oxide film present on the surface of the brazing filler metal and the surface of the mating material can be sufficiently destroyed, and the brazing property in flux-free brazing can be further improved.
[0035] On the other hand, if the amount of Mg in the brazing material is too high, Mg oxides are likely to be formed on the surface of the brazing sheet. If the amount of Mg oxides is too high, it may cause deterioration of brazing properties. By setting the Mg content in the brazing material lump to 2.0 mass% or less, more preferably 1.5 mass% or less, the amount of Mg oxides formed on the surface of the brazing sheet can be further reduced, and thus deterioration of brazing properties can be avoided.
[0036] The aluminum alloy constituting the brazing material ingot may contain, in addition to the essential components Si and Mg, one or more alloying elements selected from the group consisting of Bi (bismuth), Li (lithium), Cu, Zn, Sn (tin), In (indium), Sr (strontium), Na (sodium) and Sb (antimony).
[0037] ·Bi: 0.05 mass% or more and 1.0 mass% or less The aluminum alloy constituting the brazing material ingot may contain 0.05% by mass or more and 1.0% by mass or less of Bi. In this case, a brazing sheet having a brazing material made of an Al-Si-Mg alloy containing Bi can be obtained. Bi has the effect of reducing the surface tension of the molten brazing material generated during brazing. By making the Bi content in the brazing material ingot 0.05% by mass or more, more preferably 0.10% by mass or more, the brazing property can be further improved.
[0038] However, if the Bi content in the brazing filler metal ingot is excessively high, it becomes difficult to obtain the effect of improving brazing property commensurate with the Bi content. In addition, in this case, the brazing filler metal after brazing is likely to discolor, which may result in poor appearance. By setting the Bi content in the brazing filler metal ingot to 1.0 mass% or less, preferably 0.70 mass% or less, and more preferably 0.50 mass% or less, it is possible to avoid these problems and further improve the brazing property.
[0039] ·Li: 0.0010 mass% or more and 0.30 mass% or less The Al-Si-Mg alloy constituting the brazing filler metal ingot may contain 0.0010% by mass to 0.30% by mass of Li. In this case, a brazing sheet having a brazing filler metal made of an Al-Si-Mg alloy containing Li can be obtained. The Li in the brazing filler metal has the effect of destroying the oxide film present on the surface of the brazing filler metal and the surface of the mating material during brazing.
[0040] By setting the Li content in the brazing filler metal ingot to 0.0010 mass % or more, and more preferably 0.0040 mass % or more, the brazing property in flux-free brazing can be further improved.
[0041] However, if the Li content in the brazing material ingot is excessively high, Li oxides are likely to be formed on the surface of the brazing sheet. If the Li oxides are excessively high, it may lead to deterioration of brazing properties. By setting the Li content in the brazing material ingot to 0.30 mass% or less, more preferably 0.10 mass% or less, it is possible to avoid deterioration of brazing properties due to oxidation of Li.
[0042] ·Cu: More than 0 mass% and 2.0 mass% or less The Al-Si-Mg alloy constituting the brazing material ingot may contain Cu in an amount of more than 0 mass% and not more than 2.0 mass%. In this case, a brazing sheet including a brazing material made of an Al-Si-Mg alloy containing Cu can be obtained. The Cu in the brazing material has the effect of making the natural electrode potential of the brazing material more noble and lowering the melting point. By setting the Cu content in the brazing material ingot to the specific range, the natural electrode potential of the brazing material can be appropriately increased and the corrosion resistance of the brazing material can be improved. In addition, by setting the Cu content in the brazing material ingot to the specific range, the fluidity of the molten brazing material can be increased and the brazing property can be further improved.
[0043] ·Zn: More than 0% by mass and not more than 6.5% by mass, Sn: More than 0% by mass and not more than 0.10% by mass, In: More than 0% by mass and not more than 0.10% by mass The Al-Si-Mg alloy constituting the brazing material ingot may contain one or more elements selected from the group consisting of more than 0% by mass and up to 6.5% by mass of Zn, more than 0% by mass and up to 0.10% by mass of Sn, and more than 0% by mass and up to 0.10% by mass of In. The Zn, Sn, and In in the brazing material all have the effect of making the natural electrode potential of the brazing material less noble. By setting the Zn content, Sn content, and In content in the brazing material ingot to the above-mentioned specific ranges, the brazing material can function as a sacrificial anode, and the corrosion resistance of the aluminum product after brazing can be further improved.
[0044] ·Sr: More than 0% by mass and not more than 0.030% by mass, Na: More than 0% by mass and not more than 0.030% by mass, Sb: More than 0% by mass and not more than 0.030% by mass The Al-Si-Mg alloy constituting the brazing material ingot may contain one or more elements selected from the group consisting of more than 0% by mass and 0.030% by mass or less Sr, more than 0% by mass and 0.030% by mass or less Na, and more than 0% by mass and 0.030% by mass or less Sb. Sr, Na, and Sb in the brazing material all have the effect of refining Si particles in the brazing material and improving the fluidity of the molten brazing material. By setting the Sr content, Na content, and Sb content in the brazing material ingot to the specific ranges, the fluidity of the molten brazing material can be increased and the brazing property can be further improved.
[0045] (Intermediate material block) When preparing the clad ingot, an intermediate ingot is placed between the core ingot and the brazing material ingot, thereby obtaining a brazing sheet in which an intermediate material made of the intermediate ingot is provided between the core material and the brazing material. As the aluminum alloy constituting the intermediate ingot, for example, an aluminum alloy having a chemical composition different from that of the core material ingot and the brazing material ingot can be used. The chemical composition of the intermediate material is the same as that of the intermediate ingot.
[0046] ·Mg: 0.40 mass% or more and 6.0 mass% or less The aluminum alloy constituting the intermediate ingot may have a chemical composition containing, for example, 0.40% by mass to 6.0% by mass of Mg, with the balance being Al and unavoidable impurities. By disposing such an intermediate ingot between the core ingot and the brazing material ingot in the clad ingot, a brazing sheet can be obtained in which an intermediate material containing Mg is provided between the core material and the brazing material.
[0047] The Mg in the intermediate material, like the Mg in the core material, diffuses and migrates to the brazing material due to heating during brazing. The Mg that migrates to the brazing material destroys the oxide film present on the surface of the brazing material and the surface of the mating material together with the Mg in the brazing material, thereby further improving the brazing property in flux-free brazing. From the viewpoint of further improving the brazing property in flux-free brazing, it is preferable that the Mg content in the intermediate material ingot is within the above-mentioned specific range.
[0048] The intermediate ingot may contain, in addition to Al and unavoidable impurities, one or more elements selected from the group consisting of Mn, Si, Fe, Cu, Zn, Ti, Cr and Zr.
[0049] ·Mn: More than 0 mass% and 2.0 mass% or less The aluminum alloy constituting the intermediate material ingot may contain more than 0 mass% and not more than 2.0 mass% Mn. In this case, a brazing sheet having an intermediate material made of an aluminum alloy containing Mn can be obtained. By setting the Mn content in the intermediate material ingot to the above-mentioned specific range, the strength of the intermediate material in the brazing sheet can be further improved, and the potential of the intermediate material can be adjusted to further improve the corrosion resistance.
[0050] ·Si: More than 0 mass% and 1.0 mass% or less The aluminum alloy constituting the intermediate material ingot may contain more than 0 mass% and 1.0 mass% or less of Si. In this case, a brazing sheet having an intermediate material made of an aluminum alloy containing Si can be obtained. By setting the Si content in the intermediate material ingot to the above-mentioned specific range, the strength of the intermediate material in the brazing sheet can be further improved.
[0051] Fe: More than 0% by mass and up to 1.0% by mass The aluminum alloy constituting the intermediate material ingot may contain more than 0 mass% and 1.0 mass% or less of Fe. In this case, a brazing sheet having an intermediate material made of an aluminum alloy containing Fe can be obtained. By setting the Fe content in the intermediate material ingot to the above-mentioned specific range, the strength of the intermediate material in the brazing sheet can be further improved.
[0052] ·Cu: More than 0 mass% and 2.0 mass% or less The aluminum alloy constituting the intermediate material ingot may contain Cu in an amount of more than 0 mass% and not more than 2.0 mass%. In this case, a brazing sheet having an intermediate material made of an aluminum alloy containing Cu can be obtained. By setting the Cu content in the intermediate material ingot to the above-mentioned specific range, the strength of the intermediate material in the brazing sheet can be further improved. Also, in this case, the potential of the intermediate material can be adjusted to further improve the corrosion resistance.
[0053] ·Zn: More than 0 mass% and 6.5 mass% or less The aluminum alloy constituting the intermediate material ingot may contain Zn in an amount of more than 0 mass% and not more than 6.5 mass%. In this case, a brazing sheet can be obtained that includes an intermediate material made of an aluminum alloy containing Zn. The Zn in the intermediate material, like the Zn in the core material, has the effect of making the natural electrode potential of the intermediate material less noble. By setting the Zn content in the intermediate material in the specific range, the intermediate material can function as a sacrificial anode, further improving corrosion resistance.
[0054] ·Ti: More than 0 mass% and 0.20 mass% or less The aluminum alloy constituting the intermediate material ingot may contain Ti in a range of more than 0% by mass and not more than 0.20% by mass. In this case, a brazing sheet having an intermediate material made of an aluminum alloy containing Ti can be obtained. By setting the Ti content in the intermediate material ingot to the above-mentioned specific range, corrosion of the intermediate material can be caused to progress in layers, and the progress of corrosion in the depth direction can be more effectively suppressed.
[0055] ·Cr: More than 0 mass% and less than 0.50 mass%, Zr: More than 0 mass% and less than 0.50 mass% The aluminum alloy constituting the intermediate ingot may contain one or two elements selected from the group consisting of more than 0% by mass and 0.50% by mass or less of Cr and more than 0% by mass and 0.50% by mass or less of Zr. Cr and Zr have the effect of increasing the grain size of the intermediate material. By setting the Cr content and Zr content in the intermediate ingot to the above-mentioned specific ranges, the occurrence of erosion can be more effectively suppressed.
[0056] (Sacrificial anode material block) When preparing the clad block, a brazing material block is placed on one side of a core material block, and a sacrificial anode material block is placed on the other side, thereby obtaining a brazing sheet in which the brazing material is provided on one side of the core material and the sacrificial anode material is provided on the other side. As the aluminum alloy constituting the sacrificial anode material block, for example, an aluminum alloy having a lower natural electrode potential than the aluminum alloy constituting the core material can be used. The chemical composition of the sacrificial anode material is the same as that of the sacrificial anode material block.
[0057] ·Zn: More than 0% by mass and not more than 6.5% by mass, Sn: More than 0% by mass and not more than 0.10% by mass, In: More than 0% by mass and not more than 0.10% by mass The aluminum alloy constituting the sacrificial anode material ingot may have a chemical composition containing, for example, one or more elements selected from the group consisting of more than 0% by mass and not more than 6.50% by mass of Zn, more than 0% by mass and not more than 0.10% by mass of Sn, and more than 0% by mass and not more than 0.10% by mass of In, with the balance being Al and unavoidable impurities. In this case, a brazing sheet provided with a sacrificial anode material made of an aluminum alloy containing Zn, Sn, or In can be obtained.
[0058] Zn, Sn, and In in the sacrificial anode material have the effect of making the natural electrode potential of the sacrificial anode material less noble. By setting the Zn content, Sn content, and In content in the sacrificial anode material to the specific ranges, the corrosion resistance of the aluminum product after brazing can be further improved.
[0059] <Hot rolling process> In the method for manufacturing the brazing sheet, a hot rolling step is performed after the lamination step. In the hot rolling step, the clad ingot obtained in the lamination step is hot rolled. This makes it possible to obtain a clad plate in which adjacent aluminum ingots are bonded together. The rolling conditions in the hot rolling step may be appropriately set depending on the configuration of the clad ingot and the configuration of the brazing sheet to be finally obtained. Furthermore, after the hot rolling step, the clad plate may be heated and subjected to a homogenization treatment as necessary.
[0060] <Cold rolling process> After the hot rolling process, a cold rolling process is performed in which the obtained clad plate is subjected to one or more passes of cold rolling. By performing cold rolling on the clad plate, the thickness of the clad plate is reduced to the desired thickness of the brazing sheet. The number of passes and rolling conditions in the cold rolling process may be appropriately set according to the configuration of the clad plate and the desired configuration of the brazing sheet. In addition, the clad plate may be heated and annealed as necessary before, during, or after cold rolling.
[0061] <Etching process> On the surface of the brazing sheet obtained by cold rolling, there is an oxide film formed by the high temperature of the clad plate or brazing sheet during the above-mentioned hot rolling or heat treatment. In order to weaken this oxide film, in the etching process, an etching solution is brought into contact with the surface of the brazing sheet to perform etching. The etching process may be performed between passes of cold rolling in the cold rolling process, or after the cold rolling process is completed. When the etching process is performed after the cold rolling process is completed, etching may be performed in the state of a coil material before being cut to a desired size, or etching may be performed after processing such as cutting and pressing is performed to form the brazing sheet into a desired shape.
[0062] In the etching step, an aqueous solution containing an inorganic acid and not containing fluorine atoms can be used as the etching solution. As described above, the brazing material of the brazing sheet contains Mg as an essential component. Therefore, if fluorine atoms are present in the etching solution, the fluorine atoms react with Mg in the brazing material, and a compound containing Mg and fluorine atoms is formed on the surface of the brazing material. This compound has the effect of preventing the destruction of the oxide film by Mg during brazing, so if etching is performed using an etching solution containing fluorine atoms, brazing properties may be reduced.
[0063] In contrast, the etching solution does not contain fluorine atoms, and therefore it is possible to prevent fluorine atoms from remaining on the surface of the brazing sheet and to prevent the formation of compounds between fluorine atoms and Mg. Therefore, by performing etching using the specific etching solution, it is possible to further improve the brazeability of a brazing sheet that contains Mg in the brazing material.
[0064] Examples of inorganic acids that can be used in the etching solution include sulfuric acid, nitric acid, and phosphoric acid. These inorganic acids may be used alone or in combination of two or more. From the viewpoint of further improving the brazing properties of the brazing sheet, the etching solution preferably contains sulfuric acid as an inorganic acid, and more preferably contains both sulfuric acid and nitric acid. The concentration of sulfuric acid in the etching solution is preferably 0.10% by mass or more and 4.0% by mass or less, and more preferably 0.20% by mass or more and 2.0% by mass or less. The concentration of nitric acid in the etching solution is preferably 0.02% by mass or more and 0.50% by mass or less.
[0065] In addition to inorganic acids, etching solutions contain salts that contain iron ions. There areAs such salts, for example, ferric sulfate, ferric nitrate, ferric perchlorate, etc. can be used. These salts may be used alone or in combination of two or more. By performing etching using an etching solution containing an inorganic acid and a salt containing iron ions, the storage stability of the brazing sheet can be further improved and the deterioration of brazing property during storage can be suppressed for a longer period of time. In this case, even if oil such as rolling oil is not applied to the surface of the brazing sheet after etching, the deterioration of brazing property during storage can be suppressed for a longer period of time.
[0066] As the salt containing iron ions, ferric sulfate is preferably used. In this case, the concentration of ferric sulfate in the etching solution is preferably 0.05% by mass or more and 1.0% by mass or less, and more preferably 0.10% by mass or more and 1.0% by mass or less.
[0067] From the viewpoint of further improving the brazing properties of the brazing sheet as well as the storage stability of the brazing sheet, it is particularly preferable that the etching solution contains 0.20 mass % or more and 2.0 mass % or less of sulfuric acid, 0.02 mass % or more and 0.50 mass % or less of nitric acid, and 0.10 mass % or more and 1.0 mass % or less of ferric sulfate.
[0068] The etching solution preferably further contains at least one of a surfactant and a reaction accelerator, and more preferably contains both. By performing etching using an etching solution containing a surfactant and a reaction accelerator, the time required for etching can be further shortened, unevenness in the reaction can be suppressed, and the entire brazing sheet can be etched uniformly.
[0069] In the above-mentioned etching, the thickness of the oxide film present on the surface of the brazing sheet may be made thinner than before etching, or the oxide film may be completely removed. In the former case, the thickness of the oxide film after etching is thinner than before etching, so that the oxide film after etching can be made weaker than before etching. In the latter case, the oxide film is formed on the surface of the brazing material by contacting the surface of the clad plate with the outside air after removing the oxide film. However, the oxide film formed in this way is weaker than the oxide film formed during the manufacturing process of the clad plate, i.e., the oxide film that existed before etching.
[0070] Therefore, by etching the surface of the clad plate, the oxide film present on the surface of the brazing material can be weakened. By weakening the oxide film, the oxide film can be easily broken during brazing. As a result, the brazing property in flux-free brazing can be further improved.
[0071] The amount of etching in the etching process is 0.05 g / m 2 More than 1g / m 2 Below do. Etching amount: 0.05g / m 2 More preferably, 0.1 g / m 2 By setting the etching amount at 1 g / m or more, the oxide film present on the surface of the clad plate can be weakened sufficiently, and the oxide film can be more easily broken during brazing. 2 Less than 0.5 g / m 2 By setting the amount of etching to the amount below, it is possible to sufficiently weaken the oxide film while shortening the time required for etching, and thus to further improve the productivity of the brazing sheet.
[0072] The brazing sheet obtained by the above-mentioned manufacturing method can be used for flux-free brazing, that is, brazing performed without applying flux in an inert gas atmosphere. Examples of the inert gas that can be used include nitrogen, argon, and helium.
[0073] In flux-free brazing, excessively high oxygen concentration and dew point in the inert gas atmosphere may lead to deterioration of brazing properties. However, as described above, the brazing sheet has an oxide film on the surface of the brazing material that is weakened in advance, so that deterioration of brazing properties can be avoided even at relatively high oxygen concentrations and dew points. The brazing sheet can be used for flux-free brazing in an inert gas atmosphere with an oxygen concentration of 100 volume ppm or less and a dew point of -30°C or less.
[0074] Although the heating conditions in flux-free brazing are not particularly limited, if the time required from the start of brazing heating until the brazing material melts is excessively long, the oxidation of the surface of the brazing material may progress, leading to a deterioration in brazing properties. In order to avoid such a problem, it is preferable to perform brazing under heating conditions in which the time required from the time the temperature of the brazing sheet reaches 300°C until the time it reaches the solidus temperature of the brazing material is 40 minutes or less. EXAMPLES
[0075] Examples of the method for producing the brazing sheet are described below. Note that the embodiment of the method for producing the brazing sheet according to the present invention is not limited to the embodiment shown below, and the configuration can be appropriately changed without departing from the spirit of the present invention.
[0076] The chemical compositions of the brazing filler metal ingots A1 to A3 and the core material ingot B1 used in this example are as shown in Table 1. These brazing filler metal ingots and core material ingots can be produced by standard methods. In Table 1, the symbol "Bal." indicates that the remainder is present, and the symbol "-" indicates that the alloy element is not actively added.
[0077] [Table 1]
[0078] Example 1 First, a clad ingot is produced by stacking either the brazing material ingot A1 or A2 on one side of the core material ingot B1 (lamination process). This clad ingot is hot-rolled to produce a clad plate in which the brazing material is stacked on one side of the core material (hot-rolling process). The thickness of the clad plate is 3.0 mm.
[0079] This clad plate is subjected to one or more passes of cold rolling and then annealed to produce a brazing sheet with a thickness of 0.8 mm (cold rolling process). The cladding ratio of the brazing material in the obtained brazing sheet, that is, the ratio of the brazing material thickness to the brazing sheet thickness, is 8%.
[0080] After cold rolling, the brazing sheet is degreased and washed to remove rolling oil from the surface of the brazing sheet. Next, an etching solution having the composition shown in Table 2 is brought into contact with the brazing sheet to etch the surface of the brazing sheet (etching process). The temperature of the etching solution brought into contact with the brazing sheet and the etching time are as shown in Table 2. After etching is completed, the brazing sheet is washed with water to remove the etching solution, and then the brazing sheet is dried. Note that the symbol "-" in Table 2 indicates that the component in question is not contained.
[0081] The brazing properties of the brazing sheets C1 to C14 obtained as described above can be evaluated by a gap filling test. In the gap filling test, first, a test specimen 1 shown in FIG. 1 is assembled. As shown in FIG. 1, the test specimen 1 has a horizontal plate 2 made of the brazing sheets C1 to C14 and a vertical plate 3 made of a JIS A3003 alloy and having a thickness of 1.0 mm. The horizontal plate 2 is horizontally arranged with the brazing material 21 facing upward and the core material 22 facing downward. The vertical plate 3 is arranged so as to be perpendicular to the horizontal plate 2. One end 31 of the vertical plate 3 in the longitudinal direction is in contact with the brazing material 21 of the horizontal plate 2. The horizontal plate 2 has a width of 25 mm and a length of 60 mm. The vertical plate 3 has a width of 25 mm and a length of 55 mm.
[0082] A spacer 4 is interposed between the other end 32 of the vertical plate 3 in the longitudinal direction and the horizontal plate 2. This forms a gap S between the horizontal plate 2 and the vertical plate 3, which gradually widens from one end 31 of the vertical plate 3 toward the spacer 4. The spacer 4 is specifically a stainless steel round wire with a diameter of 1.6 mm, and is disposed 55 mm horizontally from the position where the vertical plate 3 abuts against the horizontal plate 2 (i.e., one end 31 of the vertical plate 3).
[0083] The brazing of the test specimen is performed using a nitrogen gas furnace. Specifically, the atmosphere in the furnace is first set to a nitrogen gas atmosphere with an oxygen concentration of 10 ppm by volume or less, and the test specimen is placed in the furnace with the temperature in the furnace being 100°C or less. The test specimen is left in the furnace for 10 minutes, and then brazing heating is started. The brazing heating is performed by increasing the temperature of the test specimen to 600°C, and then maintaining the temperature at 600°C for 3 minutes. After the brazing heating is completed, the test specimen is slowly cooled in the furnace until the temperature drops to a certain extent, and then the test specimen is taken out of the furnace.
[0084] In the gap filling test, brazeability can be evaluated based on the length L and shape of the fillet F formed after brazing (see Figure 1). Table 2 shows the length L of the fillet F in the test specimens using each brazing sheet.
[0085] [Table 2]
[0086] As shown in Table 2, the brazing sheets C1 to C11 etched using an etching solution containing an inorganic acid and no fluorine atoms can have a longer fillet length L than the brazing sheets C12 and C13 etched using an etching solution containing fluorine atoms.
[0087] In the brazing sheet C14 in which the brazing material does not contain Mg, destruction of the oxide film by Mg is insufficient, so that the brazing property cannot be improved even if the brazing sheet C14 is etched with an etching solution that does not contain fluorine.
[0088] From these results, it can be seen that the brazing properties in flux-free brazing can be improved by etching a brazing sheet having a brazing material made of an Al-Mg-Si alloy using an etching solution that contains an inorganic acid and does not contain fluorine atoms.
[0089] Example 2 In this example, the storage stability of the brazing sheet is evaluated. First, the brazing material ingot A3 is layered on one side of the core material ingot B1 shown in Table 1 to produce a clad ingot (lamination process). This clad ingot is hot rolled to produce a clad plate with a thickness of 3.0 mm (hot rolling process). Next, the clad plate is cold rolled to obtain a brazing sheet with a thickness of 0.4 mm (cold rolling process). The clad ratio of the brazing material in the obtained brazing sheet is 10%.
[0090] After cold rolling, the brazing sheet is annealed. Next, the brazing sheet is degreased and washed to remove rolling oil from the surface of the brazing sheet. After that, the brazing sheet is brought into contact with an etching solution having the composition shown in Table 3 to etch the surface of the brazing sheet (etching process). The temperature of the etching solution brought into contact with the brazing sheet and the etching time are as shown in Table 3. After etching is completed, the brazing sheet is washed with water to remove the etching solution, and then the brazing sheet is dried. In this manner, brazing sheets D1 to D4 are obtained. Note that the symbol "-" in Table 3 indicates that the corresponding component is not contained.
[0091] In this example, in order to simulate the condition of brazing sheets stored for a long period of time, the dried brazing sheets D1 to D4 are left to stand for 7 days in a thermohygrostat at a temperature of 40°C and a relative humidity of 80% RH. Then, a gap filling test is performed in the same manner as in Example 1. Table 3 shows the length L of the fillet F in the test specimens using each brazing sheet.
[0092] [Table 3]
[0093] As shown in Table 3, the brazing sheets D1 and D2 etched using an etching solution containing an inorganic acid and ferric sulfate can have a longer length L of the fillet F than the brazing sheets D3 and D4 etched using an etching solution that does not contain ferric sulfate.
[0094] From these results, it can be seen that by etching the brazing sheet using an etching solution containing an inorganic acid and iron ions, the storage stability of the brazing sheet can be further improved and deterioration of brazing ability during storage can be suppressed for a longer period of time. [Explanation of symbols]
[0095] 1. Test specimen 2 horizontal plate 21 Brazing material 22 Heartwood 3 vertical plates 4 Spacer F Fillet L Fillet length
Claims
1. A method for manufacturing a brazing sheet for brazing aluminum materials in an inert gas atmosphere without using a flux, comprising: a lamination step of producing a clad ingot including a core ingot made of an aluminum material and a brazing material ingot made of an Al-Si-Mg alloy and disposed on at least one surface of the core ingot; a hot rolling process for producing a clad plate including a core material made of the core material ingot and a brazing material made of the brazing material ingot and disposed on at least one surface of the core material ingot by hot rolling the clad ingot; A cold rolling step of subjecting the clad plate to one or more passes of cold rolling; an etching step of etching a surface of the clad sheet using an etching solution containing an inorganic acid and a salt containing iron ions and not containing fluorine atoms between passes of cold rolling in the cold rolling step or after completion of the cold rolling step; the Al-Mg-Si alloy constituting the brazing material ingot has a chemical composition comprising Si: 3% by mass or more and 13% by mass or less, Mg: 0.1% by mass or more and 2.0% by mass or less, Bi: 0% by mass or more and 1.0% by mass or less, Li: 0% by mass or more and 0.30% by mass or less, Cu: 0% by mass or more and 2.0% by mass or less, Zn: 0% by mass or more and 6.5% by mass or less, Sn: 0% by mass or more and 0.10% by mass or less, In: 0% by mass or more and 0.10% by mass or less, Sr: 0% by mass or more and 0.030% by mass or less, Na: 0% by mass or more and 0.030% by mass or less, and Sb: 0% by mass or more and 0.030% by mass or less, with the balance being Al and unavoidable impurities; The core ingot is made of an aluminum alloy containing Mg: 0.10% by mass or more and 4.0% by mass or less and Si: more than 0% by mass and 1.0% by mass or less, A method for producing a brazing sheet, wherein an etching amount in the etching step is 0.05 g / m 2 or more and 1 g / m 2 or less.
2. 2. The method for producing a brazing sheet according to claim 1, wherein the etching solution contains ferric sulfate as the salt containing iron ions.
3. 3. The method for producing a brazing sheet according to claim 2, wherein the etching solution contains sulfuric acid and nitric acid as the inorganic acid.
4. 4. The method for producing a brazing sheet according to claim 3, wherein the etching solution has a sulfuric acid concentration of 0.20 mass% or more and 2.0 mass% or less, a nitric acid concentration of 0.02 mass% or more and 0.50 mass% or less, and a ferric sulfate concentration of 0.10 mass% or more and 1.0 mass% or less.
Citation Information
Patent Citations
Production of non-oxidizing gas atmosphere non-flux brazing material and brazing method
JP1998180489A
Drawn cup laminated type heat exchanger and brazing method
JP2000225461A
Acidic detergent for chemical conversion film of heat exchanger, method for pickling heat exchanger, method for treating heat exchanger and heat exchanger
JP2001158983A
Flux-free joining of aluminum composites
JP2017505231A
Brazing sheet for flux-free brazing and method for producing same
WO2013105637A1