Stainless steel flux-cored wire for LNG tank manufacturing

The stainless steel flux-cored wire with controlled Mn, Cr, and Mo compositions addresses the limitations of existing materials by ensuring high strength and cryogenic toughness in weld metals, suitable for diverse steel members.

JP7592085B2Active Publication Date: 2024-11-29ESAB SEAH CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2022531395
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-11-26
Filing Date
2020-11-25
Publication Date
2024-11-29
Estimated Expiration
2040-11-25

AI Technical Summary

Technical Problem

Existing materials for cryogenic storage tanks, such as Cr-Ni based stainless steels and 9% Ni steels, face issues like high production costs, low strength, and limited weldability, while nickel-free steels increase costs and strain heat treatment equipment, necessitating a welding material that overcomes these limitations and provides excellent cryogenic toughness.

Method used

A stainless steel flux-cored wire with controlled compositions of Mn, Cr, Mo, and Ni, along with specific oxide and impurity levels, satisfying relational expressions to ensure optimal weld metal properties, including {4(Na2O+K2O)/{0.5(TiO2+SiO2)+0.2(ZrO2)}<0.5, {Cr+Mo}/{Ni+Mn+30(C+N)}>1, and {Cr+Q}/{Ni+Mn+30(C+N)}>1, to achieve desired strength and toughness.

Benefits of technology

The wire enables weld metals with yield strength of 350 MPa or more, tensile strength of 600 MPa or more, elongation of 30% or more, and impact values greater than 27 J at -196°C, suitable for welding various steel members.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007592085000001
    Figure 0007592085000001
  • Figure 0007592085000002
    Figure 0007592085000002
  • Figure 0007592085000003
    Figure 0007592085000003
Patent Text Reader

Abstract

The present invention relates to a stainless steel flux-cored wire for manufacturing LNG tanks, and more particularly to a stainless steel flux-cored wire for manufacturing LNG tanks that can obtain a weld metal with excellent tensile strength and impact value by adjusting the contents of Mn, Mo, and Cr. The stainless steel flux-cored wire for manufacturing LNG tanks of the present invention is applicable to welding of all of 9% nickel steel, high manganese steel, and stainless steel, and has the effect of obtaining a weld metal with excellent cryogenic toughness in the weld region by adjusting the relationship between the contents of Mn, Mo, and Cr.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a stainless steel flux-cored wire for manufacturing LNG tanks, more particularly, the wire is made such that the contents of Mn, Cr and Mo are adjusted as desired, and the wire can be used to obtain a weld metal having excellent strength and cryogenic impact toughness. [Background technology]

[0002] Liquefied gases such as liquefied natural gas (LNG) with a boiling point of -164°C, liquid oxygen with a boiling point of -183°C, and liquid nitrogen with a boiling point of -196°C require cryogenic storage. Therefore, in order to store these gases, structures such as pressure vessels made of materials that have sufficient toughness and strength at cryogenic temperatures are required.

[0003] Cr-Ni-based stainless steel, 9% Ni steel, and 5000 series aluminum alloys have been commonly used as materials that can be used at low temperatures in liquefied gas environments. However, when using aluminum alloys, there are problems such as high alloy costs, large design thickness due to low strength, and limited specifications due to poor weldability. Cr-Ni-based stainless steel and 9% Ni steel overcome the low strength problem of aluminum, but they must contain excessive nickel, which increases manufacturing costs, making their application problematic.

[0004] Furthermore, as another technology for stainless steels used for liquefied gas, so-called nickel-free (Ni-free) high magnesium steels that do not use nickel at all have been used. However, such technology has problems such as increased costs and increased load on heat treatment equipment due to an increase in the number of heat treatment cycles. Therefore, as disclosed in Korean Patent No. 10-135843, a technology was developed to ensure cryogenic toughness by using austenite as the main structure instead of ferrite.

[0005] Conventional wires used for welding such structural steels have been developed to be selectively applied to 9% Ni steel, stainless alloy, or high magnesium steel according to the physical properties of the structural steels in order to satisfy the strength and impact resistance of the structure after welding. However, if the application is limited by the material of the structural steel, it causes confusion in the work process and is disadvantageous from an economic point of view. Therefore, there is a need to develop a welding material that can be welded without restrictions due to the material of the structural steel members and also provides excellent cryogenic toughness to the welded part. Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention aims to provide a stainless steel flux-cored wire for manufacturing LNG tanks, which has suitable physical properties required for LNG tanks. [Means for solving the problem]

[0007] In order to solve the above problems, the present invention provides an alloy flux-cored wire having an alloy sheath filled with flux, the wire has a wire composition including a sheath element and a flux element embedded in the sheath element, the wire composition containing 6.0-15.0 wt% Ni, 13.0-25.0 wt% Cr, 1.0-10.0 wt% Mn, 5.0 wt% or less (excluding 0 wt%) Mo, 0.05-1.0 wt% Si, and a C content of 0.05 wt% or less based on the total weight of the flux-cored wire. The amount of the alloy flux-cored wire is 0.5wt% or less (excluding 0wt%), the total content of P and S is 0.1wt% or less (excluding 0wt%), at least one of SiO2, TiO2, and ZrO2 is 5.0-18.0wt%, at least one of Na2O and K2O is 0.1-1.0wt%, and the balance is Fe and unavoidable impurities. The alloy flux-cored wire is a stainless steel flux-cored wire for manufacturing LNG tanks, which satisfies the following relationship 1. to provide. [Equation 1] {4(Na2O+K2O)} / {0.5(TiO2+SiO2)+0.2(ZrO2)}<0.5

[0008] In order to solve the above problems, the present invention provides a flux-filled alloy sheath. An alloy flux-cored wire, the wire composition including a sheath element and a flux element embedded in the sheath element, contains 6.0-15.0wt% Ni, 13.0-25.0wt% Cr, 1.0-10.0wt% Mn, 0.05-1.0wt% Si, 0.5wt% or less (excluding 0wt%) C based on the total weight of the flux-cored wire, the total content of P and S is 0.1wt% or less (excluding 0wt%), and the content of SiO2, TiO2, The present invention provides an alloy flux-cored wire, which is a stainless steel flux-cored wire for manufacturing LNG tanks, comprising at least one of ZrO2 at 5.0-18.0 wt%, at least one of Na2O and K2O at 0.1-1.0 wt%, at least one element selected from the group consisting of Mo, W and Nb in an amount of 0.1-5.0 wt%, with the balance being Fe and unavoidable impurities, and which satisfies the following relational expression 1. [Equation 1] {4(Na2O+K2O)} / {0.5(TiO2+SiO2)+0.2(ZrO2)}<0.5

[0009] The present invention provides an alloy flux-cored wire having an alloy sheath filled with flux, wherein the deposited metal obtained from the flux-cored wire contains 8.0-14.0 wt% Ni, 15.0-23.0 wt% Cr, 1.0-8.0 wt% Mn, 4.0 wt% or less (excluding 0 wt%) Mo, 0.05-1.0 wt% Si, the total content of C and N is limited to 0.01-0.5 wt%, the total content of P and S is limited to 0.1 wt% or less (excluding 0 wt%), the balance being Fe and unavoidable impurities, and the alloy flux-cored wire is a stainless steel flux-cored wire for manufacturing LNG tanks, and satisfies the following relational expression 2. [Equation 2] {Cr+Mo} / {Ni+Mn+30(C+N)}>1

[0010] The present invention provides an alloy flux-cored wire having an alloy sheath filled with flux, wherein the deposited metal obtained from the flux-cored wire contains 8.0-14.0wt% Ni, 15.0-23.0wt% Cr, 1.0-8.0wt% Mn, 0.05-1.0wt% Si, the total content of C and N is limited to 0.01-0.5wt%, the total content of P and S is limited to 0.1wt% or less (excluding 0wt%), at least one element (Q) selected from the group consisting of Mo, W and Nb is contained in an amount of 0.1-4.0wt%, and the balance is Fe and unavoidable impurities, and the alloy flux-cored wire is a stainless steel flux-cored wire for manufacturing LNG tanks, and satisfies the following relational formula 3. [Equation 3] {Cr+Q} / {Ni+Mn+30(C+N)}>1 Effect of the Invention

[0011] The stainless steel flux-cored wire for LNG tank manufacturing according to the present disclosure can be used for welding 9% nickel steel members, high manganese steel members, and stainless steel members by controlling the content of Mo and Cr. The stainless steel flux-cored wire has the effect of obtaining a weld metal having excellent cryogenic toughness at the welded portion. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The present invention will be described in detail below.

[0013] The flux-cored wire described herein can be used to manufacture LNG tanks. The flux-cored wire has an alloy sheath filled with flux.

[0014] As used herein, the term "weld metal" refers to the metal resulting from solidification of a molten mixture of the weld metal and base metal during welding.

[0015] As used herein, the term "deposited metal" refers to metal transferred from the filler metal (i.e., wire), which is the metallic material added to the weld metal area during welding.

[0016] According to one aspect of the present invention, there is provided a stainless steel flux-cored wire for LNG tank manufacturing, the flux-cored wire having a sheath with embedded flux, the flux-cored wire having a composition including Mn, Mo, Cr and Ni in predetermined weight percents relative to a total weight of the wire.

[0017] More specifically, the wire has an alloy sheath filled with flux, and includes a wire component including a sheath element and a flux element embedded in the sheath element, the wire component including, based on the weight of the flux-cored wire, 6.0-15.0 wt% Ni, 13.0-25.0 wt% Cr, 1.0-10.0 wt% Mn, 5.0 wt% or less (excluding 0 wt%) Mo, and 0.05-1.0 wt% Si, and the C content is 0.5 wt% or less (excluding 0 wt%) based on the total weight of the flux-cored wire. The alloy flux-cored wire is a stainless steel flux-cored wire for manufacturing LNG tanks, and satisfies the following relational expression 1: [Equation 1] {4(Na2O+K2O)} / {0.5(TiO2+SiO2)+0.2(ZrO2)}<0.5

[0018] Ni: 6.0-15.0wt% Nickel (Ni) is a chemical component that stabilizes the austenite structure. If the nickel content is less than 6.0wt%, the austenite structure becomes unstable, which is not preferable. If the nickel content is more than 15.0wt%, the hot cracking resistance decreases, which is not preferable. Therefore, the nickel content is preferably limited to 6.0-15.0wt%.

[0019] Cr: 13.0-25.0wt% Chromium (Cr) is a chemical component that improves the strength of the weld metal and stabilizes the austenitic structure. If the chromium content is less than 13.0 wt%, sufficient strength cannot be obtained, which is undesirable. If the chromium content is more than 25.0 wt%, the low-temperature impact toughness of the weld metal decreases, which is undesirable. Therefore, it is preferable that the chromium content is limited to 13.0-25.0 wt%.

[0020] Mn: 1.0-10.0wt% Manganese (Mn) is a chemical component that stabilizes the austenite structure and improves deoxidation and weldability. If the manganese content is less than 1.0 wt%, it is not preferable because it does not provide sufficient deoxidation. If the manganese content is more than 10.0 wt%, the segregation of the weld metal in the final solidification region is accelerated, thereby lowering the melting point of the molten metal and reducing the hot cracking resistance. Therefore, it is preferable that the manganese content is limited to 1.0-10.0 wt%.

[0021] Mo: 5.0wt% or less (excluding 0wt%) Molybdenum (Mo) has the effect of improving the strength of the weld metal. If the Mo content is low, sufficient strength cannot be obtained, which is undesirable. If the Mo content is more than 5.0 wt%, the toughness of the weld metal decreases, and the segregation of Mo accelerates, which results in a decrease in hot cracking resistance, which is undesirable. Therefore, it is preferable that the Mo content is limited to a range of 5.0 wt% or less.

[0022] Si: 0.05-1.0wt% Silicon (Si) is a chemical component that improves deoxidation and weldability. If the Si content is less than 0.05wt%, the deoxidation effect is insufficient. If the Si content is more than 1.0wt%, it is not preferable because it increases the cracking sensitivity due to the formation of Laves phase. Therefore, it is preferable to limit the Si content to 0.05-1.0wt%.

[0023] C: 0.5wt% or less (excluding 0wt%) Carbon (C) has the effect of improving the strength of the weld metal, but if it is added in excess, there is a problem that carbides are formed and the toughness is reduced. Therefore, the C content is set to 0.5 wt% or less based on the total weight of the wire. More specifically, the C content may be set to 0.1 wt% or less to prevent the toughness of the weld metal from being reduced.

[0024] P+S: 0.1wt% or less (excluding 0wt%) Phosphorus (P) and sulfur (S) are the elements that mainly affect hot cracking. P and S form compounds with low melting points, which may cause hot cracking. In the present invention, the total content of P and S is preferably less than 0.1 wt%.

[0025] SiO 2 , TiO 2 , ZrO 2 One or more oxides selected from: 5.0-18.0 wt% Si, Ti and Zr oxides may be added to increase the melting point of the slag to improve the workability of full-fine welding. If the total content of Si, Ti and Zr oxides is less than 5.0 wt%, the amount of slag is insufficient and the enveloping property of the slag is reduced. If it is more than 18.0 wt%, poor slag peeling may occur. Therefore, it is preferable to limit the total content of Si, Ti and Zr oxides to the range of 5.0-18.0 wt%.

[0026] Na 2 O and K 2 O: 0.1-1.0 wt% Alkali metal oxides should be added in an amount of 0.1wt% or more to facilitate arc generation, reduce the ionization potential of the arc during welding, and maintain a stable arc during welding. In addition, if the content of alkali metal oxides is more than 1.0wt%, excessive welding fumes may be generated due to high vapor pressure. Therefore, it is preferable to limit the content of alkali metal oxides to 0.1-1.0wt%. The alkali metal oxides may include either one or both of Na2O and K2O.

[0027] It may further contain K2SiF6, Bi2O3, Fe2O3, Al2O3, etc. The balance may be Fe and unavoidable impurities.

[0028] On the other hand, in the stainless steel flux-cored wire of the present invention, it is preferable to control the content of each oxide so as to satisfy the following [Relationship 1]. In particular, the control is preferably performed so that the value defined by [Relationship 1] is smaller than 0.5. If the value is 0.5 or more, the quality of the weld metal region is degraded due to the deterioration of weldability and cracking properties. [Equation 1] {4(Na2O+K2O)} / {0.5(TiO2+SiO2)+0.2(ZrO2)}<0.5

[0029] The stainless steel flux-cored wire of the present invention may further include copper (Cu) in an amount of 0.5wt% or less. Cu is a precipitation hardening element, and the Cu content is preferably limited to 0.5wt% or less. A Cu content greater than 0.5wt% is not preferred, since it increases the hardenability and thus reduces the low-temperature impact toughness.

[0030] Nitrogen (N) may be further included in an amount of 0.4wt% or less. N is a solid solution strengthening element, and it is preferable to limit the N content to 0.4wt% or less. If the N content is more than 0.4wt%, the low temperature impact toughness decreases and a fully austenitic structure occurs, which is undesirable because it decreases the hot cracking resistance and porosity resistance.

[0031] In the flux-cored wire of the present invention, the relationship between the contents of Mn, Cr and Mo is adjusted to obtain the physical properties required for the welded region. Specifically, when {Cr+Mo} / {Ni+Mn+30(C+N)}>1 is satisfied, the deposited metal obtained from the flux-cored wire has a yield strength of 350 MPa or more, a tensile strength of 600 MPa or more, and an elongation of 30% or more. Furthermore, the Charpy impact test shows that the deposited metal has an impact value of 27 J or more at -196°C.

[0032] Specifically, the present invention provides an alloy flux-cored wire having an alloy sheath filled with flux, and the wire components including the sheath elements and the flux elements embedded in the sheath elements contain, based on the total weight of the flux-cored wire, 6.0-15.0 wt% Ni, 13.0-25.0 wt% Cr, 1.0-10.0 wt% Mn, and 0.05-1.0 wt% Si, the C content is limited to 0.5 wt% or less (excluding 0 wt%), and the total content of P and S is 0.1 wt% or less. The alloy flux-cored wire is limited to the above (excluding 0wt%), contains at least one of SiO2, TiO2, ZrO2 in an amount of 5.0-18.0wt%, contains at least one of Na2O and K2O in an amount of 0.1-1.0wt%, contains at least one element selected from the group consisting of Mo, W and Nb in an amount of 0.1-5.0wt%, and the balance is Fe and unavoidable impurities, and the alloy flux-cored wire is a stainless steel flux-cored wire for manufacturing LNG tanks, and satisfies the following relational expression 1. [Equation 1] {4(Na2O+K2O)} / {0.5(TiO2+SiO2)+0.2(ZrO2)}<0.5

[0033] Mo, W, and Nb have the effect of improving the strength of the weld metal, and at least one of them may be selectively included. If the content of at least one element selected from the group consisting of Mo, W, and Nb is less than 0.1 wt%, sufficient strength cannot be obtained, which is not preferable. If the content of at least one element selected from the group consisting of Mo, W, and Nb is more than 5.0 wt%, the toughness of the weld metal decreases, and the hot cracking resistance decreases, which is not preferable. Therefore, it is preferable that the content of each element is limited to 0.1-5.0 wt%.

[0034] Specifically, the stainless steel flux-cored wire of the present invention may further contain W in an amount of 2.0 wt% or less instead of Mo. Tungsten (W) has the same effect as Mo. That is, W and Mo improve the strength of the weld metal. If the W content is more than 2.0 wt%, the toughness of the weld metal may decrease. Therefore, it is preferable that the W content is limited to the range of 2.0 wt% or less.

[0035] Furthermore, the stainless steel flux-cored wire of the present invention may further contain Nb in an amount of 1.5wt% or less instead of Mo. Niobium (Nb) has the same effect as Mo. That is, Ni and Mo improve the strength of the weld metal. If the Nb content is more than 1.5wt%, the toughness of the weld metal may decrease. Therefore, it is preferable that the Nb content is limited to the range of 1.5wt% or less.

[0036] According to another aspect of the present invention, there is provided an alloy flux-cored wire having an alloy sheath filled with flux, and a deposited metal obtained from the flux-cored wire contains 8.0-14.0 wt% Ni, 15.0-23.0 wt% Cr, 1.0-8.0 wt% Mn, 4.0 wt% or less (except 0 wt%) Mo, 0.05-1.0 wt% Si, 0.01-0.5 wt% C and N, the total content of P and S is limited to 0.1 wt% or less (except 0 wt%), the balance being Fe and unavoidable impurities, and the alloy flux-cored wire is a stainless steel flux-cored wire for LNG tank manufacturing, and satisfies the following [Relationship 2]. [Equation 2] {Cr+Mo} / {Ni+Mn+30(C+N)} > 1

[0037] Depending on the alloy composition of the flux-cored wire, the properties of the deposited metal obtained change, in particular those properties used in the manufacture of LNG tanks. The use of the flux-cored wire according to the invention makes it possible to obtain a deposited metal with excellent strength, toughness and impact value. The individual chemical components may be initially contained in the alloy sheath or may be added from the metal and alloy powders of the flux.

[0038] Nickel (Ni) is a chemical component that stabilizes the austenite structure. If the nickel content is less than 8.0wt%, the austenite structure becomes unstable, which is not preferable. If the nickel content is more than 14.0wt%, the hot cracking resistance decreases, which is not preferable. Therefore, the nickel content is preferably limited to the range of 8.0-15.0wt%.

[0039] Chromium (Cr) is a chemical component that improves the strength of the weld metal and stabilizes the austenite structure. If the chromium content is less than 15.0 wt%, sufficient strength cannot be obtained, which is undesirable. If the chromium content is more than 23.0 wt%, the low-temperature impact toughness of the weld metal decreases, which is undesirable. Therefore, it is preferable that the chromium content is limited to the range of 15.0-23.0 wt%.

[0040] Manganese (Mn) is a chemical component that stabilizes the austenite structure and improves deoxidation and weldability. If the manganese content is less than 1.0 wt%, it is not preferable because it does not provide sufficient deoxidation. If the manganese content is more than 8.0 wt%, the segregation of the weld metal in the final solidification region is accelerated, thus reducing the hot cracking resistance. Therefore, it is preferable that the manganese content is limited to the range of 1.0-8.0 wt%.

[0041] Molybdenum (Mo) has the effect of improving the strength of the weld metal. If the Mo content is low, sufficient strength cannot be obtained, which is undesirable. If the Mo content is more than 4.0 wt%, the toughness of the weld metal decreases, segregation accelerates, and therefore the hot cracking resistance decreases. Therefore, it is preferable that the Mo content is limited to a range of 4.0 wt% or less.

[0042] If the Si content is less than 0.05wt%, the deoxidizing effect is insufficient. If the Si content is more than 1.0wt%, the cracking sensitivity increases due to the formation of Laves phase, which is not preferable. Therefore, the Si content is preferably limited to the range of 0.05-1.0wt%.

[0043] Carbon (C) has the effect of improving the strength of the weld metal, but if it is added in excess, carbides are formed, which causes a problem of reduced toughness. N is a solid solution strengthening element, and if added in excess, it reduces low-temperature impact toughness and produces a fully austenitic structure, which is undesirable because it reduces hot cracking resistance and porosity resistance. Therefore, the total content of C and N is preferably limited to the range of 0.01-0.5wt%.

[0044] Phosphorus (P) and sulfur (S) are the elements that mainly affect hot cracking. P and S form compounds with low melting points, which may cause hot cracking. In the present invention, the total content of P and S is preferably less than 0.1 wt%.

[0045] The deposited metal obtained from the stainless steel flux-cored wire of the present invention may further contain copper (Cu) in an amount of 0.5wt% or less. Cu is a precipitation hardening element, and the Cu content is preferably limited to the range of 0.5wt% or less. A Cu content greater than 0.5wt% is not preferred because it increases the hardenability and therefore reduces the low-temperature impact toughness.

[0046] On the other hand, in the stainless steel flux-cored wire of the present invention and the weld metal obtained from the wire, it is preferable to control the content of each chemical component so as to satisfy the following [Relationship 2].

[0047] [Equation 2] {Cr+Mo} / {Ni+Mn+30(C+N)}>1 In particular, it is preferable that the control is carried out so that the value defined by the relation 2 is greater than 1. If the value is less than 1, it is difficult to ensure the strength and cryogenic toughness (i.e., values ​​related to impact), resulting in a deterioration of the quality of the weld metal area.

[0048] Further, there is provided an alloy flux-cored wire having a sheath filled with flux, wherein a deposited metal obtained from the alloy flux wire contains 8.0-14.0 wt% Ni, 15.0-23.0 wt% Cr, 1.0-8.0 wt% Mn, 0.05-1.0 wt% Si, 0.01-0.5 wt% C and N, the total content of P and S is limited to a range of 0.1 wt% or less (excluding 0 wt%), at least one element selected from the group (Q) consisting of Mo, W and Nb is contained in an amount of 0.1-4.0 wt%, and the balance is Fe and unavoidable impurities, and the alloy flux-cored wire is a stainless steel flux-cored wire for manufacturing LNG tanks, and satisfies the following [Relationship 3]. [Equation 3] {Cr+Q} / {Ni+Mn+30(C+N)}>1

[0049] When the composition further contains W or Nb, or when Mo is replaced with W or Nb, the stainless steel flux-cored wire of the present invention or the deposited metal obtained therefrom preferably satisfies the following Relation 3. In Relation 3, Q may be any one of Mo, [Mo+W], [Mo+Nb], [Mo+W+Nb], W, Nb, and [W+Nb]. More strictly, Relation 3 may be 1.5>{Cr+Q} / {Ni+Mn+30(C+N)}>1. When the value of Relation 3 is 1.5 or more or 1 or less, it is difficult to ensure strength and cryogenic toughness (i.e., values ​​related to impact), resulting in a deterioration of the quality of the weld metal area.

[0050] Specifically, the deposited metal obtained by welding the stainless steel flux-cored wire of the present invention may further contain W in an amount of 2.0 wt% or less instead of Mo. Tungsten (W) has the same effect as Mo. That is, W and Mo improve the strength of the weld metal. If the W content is more than 2.0 wt%, the toughness of the weld metal decreases. Therefore, it is preferable that the W content is limited to the range of 2.0 wt% or less.

[0051] Specifically, the deposited metal obtained by welding the stainless steel flux-cored wire of the present invention may further contain Nb in an amount of 1.5 wt% or less instead of Mo. Niobium (Nb) has the same effect as Mo. That is, Nb and Mo improve the strength of the weld metal. If the Nb content is more than 1.5 wt%, the toughness of the weld metal decreases. Therefore, it is preferable that the Nb content is limited to the range of 1.5 wt% or less.

[0052] In connection with the stainless steel flux-cored wire according to the present invention, the physical properties of the weld metal region according to the relationship between the contents of Cr, Mo and Mn will be described in detail with reference to the following examples and comparative examples, but the scope of the present invention is not limited by these examples.

[0053] A stainless steel flux-cored arc welding wire was prepared having the chemical composition shown in Table 1. [Table 1]

[0054] Flux cored arc welding (FCAW) was performed with each welding material. For FCAW, welding was performed with a heat input of 8.0-12.0 kJ / cm in a 100% CO2 protective gas environment. A wire with a diameter of 1.2 mm was used for FCAW. A bevel was formed with a bevel angle of 22.5° on the bevel surface of a 20 mm thick 9% Ni steel plate, which is one of the base materials used to manufacture LNG tanks. Next, the base materials were arranged with a root gap of 12 mm, and the same stainless steel material as the base material was placed on the side where the bevel narrows (the root side). Welding was performed with this bevel to form a welded joint.

[0055] Visual inspection was performed for arc stability of the welded joint, slag removability, crack resistance of the welded joint, and porosity on the outer surface of the bead. The inspection results were evaluated on a four-point scale: ◎: excellent, O: good, △: fair, X: poor. The results are shown in Table 2 below. [Table 2]

[0056] Referring to Table 2, it can be seen that in the case of No. 11, which does not satisfy the relational expression 1, the arc stability and bead appearance were not satisfactory. Numbers 12 and 14 It was found that the percentage of cracks was high in the case of No. 1. It was found that cracks occurred in the cases of No. 20 and No. 27 depending on the range of Mn.

[0057] The yield strength (YS), tensile strength (TS), elongation (EL) and Charpy impact energy (at -196°C) of the welded joints were then measured and the results are shown in Table 3 below. [Table 3]

[0058] Referring to Table 3, the yield point, tensile strength and especially the impact value are If relational expression 2 is not satisfied in number 12-20 On the other hand, in the case of Nos. 1 to 10, which correspond to the composition range of the present invention, a yield point of 420 MPa or more, a tensile strength of 650 MPa or more, an elongation of 38% or more, and an impact value of 35 J or more were ensured.

[0059] Furthermore, regarding the content of Mo, W or Nb, a stainless steel flux-cored wire having the chemical composition shown in Table 4 was prepared according to Relation 3. The evaluation results of the properties of the welded joint after welding are shown in Table 5 below. [Table 4] [Table 5]

[0060] Referring to Tables 4 and 5, when W or Nb is added or MoIt was found that when Mn and W or Nb are added instead of Mo, and the value of the relationship between Mn and W or Nb is in the range of 25-28, which is outside the range of the composition of the present invention, the low temperature impact value is low. Furthermore, it was confirmed that when the value is in the range of 29-35 and does not satisfy the relationship 3, the impact value is also low. Therefore, when W and Nb are added or instead of Mo, Mn When added, the content ratio of the chemical components is Equation 3 It can be seen that it is preferable to adjust the amount of the ion exchange resin according to the following formula:

[0061] The stainless steel flux-cored wire according to the present invention has a feature that the weld metal having excellent strength and cryogenic impact toughness can be obtained from the stainless steel flux-cored wire, since the manganese content is limited to a range of 10wt% or less and the Mo and Cr contents are appropriately controlled. The stainless steel flux-cored wire according to the present invention is applicable to welding of 9% nickel steel, high manganese steel and stainless steel, and has an advantageous effect of obtaining a weld metal having excellent cryogenic toughness in the welded region.

[0062] The features and technical advantages of the present invention have been described above in a broad manner so that the appended claims may be better understood. Those skilled in the art will appreciate that the present invention may be embodied in other different forms without departing from the technical spirit or basic characteristics of the illustrated embodiments. It will therefore be understood that the above-described examples are for illustrative purposes only and are not limiting in all respects. The scope of the present invention is defined by the following claims, not the above detailed description, and all changes or modifications that come within the meaning and scope of the claims, and their equivalents, should be construed as being within the scope of the present invention.

Claims

1. An alloy flux-cored wire having an alloy sheath filled with flux, The wire composition including the sheath element and the flux element embedded in the sheath element contains, based on the total weight of the flux-cored wire, 8.0-14.0 wt% Ni, 15.0-23.0 wt% Cr, 1.0-8.0 wt% Mn, 4.0 wt% or less (excluding 0 wt%) Mo, and 0.05-1.0 wt% Si; The total content of C and N is limited to 0.01-0.5 wt%, the total content of P and S is limited to 0.1 wt% or less (excluding 0 wt%), and SiO 2 , TiO 2 , ZrO 2 At least one of the following is contained in an amount of 5.0-18.0 wt %; 2 O and K 2 At least one of O is contained in an amount of 0.1-1.0 wt%, and the balance is Fe and unavoidable impurities, The alloy flux-cored wire is a stainless steel flux-cored wire for manufacturing LNG tanks, and satisfies the following Relational Formula 1 and Relational Formula 2. [Relationship 1] {4(Na2O+K2O)} / {0.5(TiO2+SiO2)+0.2(ZrO2)}<0.5 [Relationship 2] {Cr+Mo} / {Ni+Mn+30(C+N)}>1

2. An alloy flux-cored wire having an alloy sheath filled with flux, The wire composition, including the sheath element and the flux element embedded in the sheath element, comprises, based on the total weight of the flux-cored wire, 8.0-14.0 wt. % Ni, 15.0-23.0 wt. % Cr, 1.0-8.0 wt. % Mn, 0.05-1.0 wt. % Si, and 0.01-0.5 wt. % C and N; The total content of P and S is limited to 0.1 wt% or less (excluding 0 wt%), and SiO 2 , TiO 2 , ZrO 2 At least one of the following is contained in an amount of 5.0-18.0 wt %; 2 O and K 2 At least one of O is contained in an amount of 0.1-1.0 wt%, at least one element selected from the group (Q) consisting of Mo, W and Nb is contained in a total amount of 0.1-4.0 wt%, and the balance is Fe and unavoidable impurities; The alloy flux-cored wire is a stainless steel flux-cored wire for manufacturing LNG tanks, and satisfies the following Relational Formula 1 and Relational Formula 3. [Relationship 1] {4(Na2O+K2O)} / {0.5(TiO2+SiO2)+0.2(ZrO2)}<0.5 [Relationship 3] 1.5>{Cr+Q} / {Ni+Mn+30(C+N)}>1

Citation Information

Patent Citations

  • Flux-cored wire for pure argon gas shield welding for lower temperature steel

    CN107838579A

  • Welding wire powder, stainless steel flux-cored wire and preparation method and application thereof

    CN108453415A

  • Deposited metal of austenitic stainless steel having resistance to chloride stress corrosion cracking

    JP1984127991A

  • Flux cored wire for welding and weld joint for steel structure

    JP2005279768A

  • Flux cored wire for welding high-strength stainless steel

    JP2007160314A