Method for manufacturing a crystal resonator wafer and a crystal resonator wafer
The method addresses excessive wafer protrusions in crystal resonator manufacturing by etching grooves and via holes, ensuring neat edges and enhancing device performance.
Patent Information
- Application Number
- JP2022132208
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-07-06
- Filing Date
- 2022-08-23
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-08-23
AI Technical Summary
Conventional crystal resonator wafer manufacturing methods, particularly in semiconductor micromachining, result in excessive wafer protrusions during packaging, affecting device performance.
A method involving etching crystal wafers to form grooves with specific widths and lengths, forming via holes, and creating shallow grooves to facilitate neat folding, thereby eliminating notches and protrusions, and enhancing device performance.
The method ensures neat edges on crystal resonator wafers, improving device performance by preventing notches and protrusions, and increasing production efficiency through batch processing.
Smart Images

Figure 0007592935000001 
Figure 0007592935000002 
Figure 0007592935000003
Abstract
Description
[Technical field]
[0001] The present invention relates to the technical field of resonators, and in particular to a method for fabricating a quartz resonator wafer and a quartz resonator wafer. [Background technology]
[0002] Quartz crystal resonators, as devices that generate oscillation signals, are widely used in fields such as communications, radar, precision calculations, precision balances, mobile phones, aviation, electronic watches, and automobiles. Conventional quartz crystal resonator wafers are formed using mechanical processing methods such as grinding, polishing, cutting the wafer along its dimensions, and drum grinding to its outer shape. However, with the development of smaller quartz crystal resonator dimensions and higher frequencies, the processing process is gradually evolving from mechanical processing to semiconductor micromachining.
[0003] However, in the semiconductor micromachining process, during the packaging use of the crystal resonator wafer, it is necessary to use a folding device to automatically or manually remove the wafer from the wafer to be processed, so that it is easy to cause a notch or excess protrusion of the wafer during the folding and removing process, as shown in Figure 1, the edge with this notch or protrusion is the dispensing fixing position of the wafer, which will affect the performance of the wafer.
[0004] Therefore, how to obtain neat edges after folding the wafer is currently a technical problem that needs to be urgently solved. Summary of the Invention [Problem to be solved by the invention]
[0005] In view of the above problems, the present invention is proposed to provide a method for fabricating a quartz resonator wafer and a quartz resonator wafer that overcomes or at least partially solves the above problems. [Means for solving the problem]
[0006] According to a first method, there is provided a method for producing a quartz crystal resonator wafer according to the present invention, comprising the steps of: Providing a quartz crystal wafer; Etching the front surface of the quartz crystal wafer to form N first grooves, and etching the back surface of the quartz crystal wafer to form N second grooves, the N first grooves and the N second grooves facing each other, each of the first grooves and each of the second grooves having a structure that is wider at the top and narrower at the bottom, the width of the second bottom end of each second groove is equal to the width of the first bottom end of the opposing first groove, the length of the second bottom end is equal to or longer than the length of the first bottom end, one end of the second bottom end faces one end of the first bottom end, the other end of the second bottom end exceeds the other end of the first bottom end or the other end of the second bottom end faces the other end of the first bottom end, and N is a positive integer; For each of the first grooves and the opposing second grooves, etching is performed from a position at one end of a first bottom end directly opposite one end of a second bottom end to the back surface to form a first via hole having a length equal to a width of the first bottom end; Etching from the other end of the second bottom end directly opposite the first bottom end to the back surface to form a second via hole having a length shorter than a width of the second bottom end; Etching a target edge of the second via hole on the front side, the target edge being an inward edge of a first bottom end, to form a shallow groove; and folding each of the crystal resonator wafers along a respective one of the shallow grooves to form N crystal resonator wafers.
[0007] Further, after etching the target edge of the second via hole on the front side to form a shallow groove, When the length of the second bottom end is longer than the length of the first bottom end, a first metal electrode is formed on the first bottom end of the first groove, on the second bottom end of the second groove, and extending from the first bottom end to the other end of the first bottom end and to the outside of the first groove; or When the length of the second bottom end is equal to the length of the first bottom end, the method further includes forming a second metal electrode on the first bottom end of the first groove and the second bottom end of the second groove.
[0008] Furthermore, etching the front surface of the crystal wafer to form N first grooves and etching the back surface of the crystal wafer to form N second grooves, forming a first chromium film layer and a first gold film layer in order from bottom to top on the front surface of the quartz crystal wafer; forming a first photoresist layer on the first gold film layer, and exposing and developing the first photoresist layer to form N first etching regions; Etching the N first etching regions to form N first grooves; forming a second chromium film layer and a second gold film layer in order from bottom to top on the rear surface of the quartz crystal wafer; forming a second photoresist layer on the second gold film layer, and exposing and developing the second photoresist layer to form N second etching regions; Etching the N second etching regions to form N second grooves.
[0009] Further, before etching a target edge of the second via hole on the front side, which is an edge toward the inside of the first bottom end, to form a shallow groove, the N crystal resonator wafer is formed. For each of the first grooves and the opposing second grooves, when the length of the second bottom end is longer than the length of the first bottom end, a third via hole and a fourth via hole are formed at both ends located in the width direction of the first bottom end at the other end position of the first bottom end, and the third via hole and the fourth via hole are both connected from the first bottom end to the opposing second bottom end; or When the length of the second bottom end is equal to the length of the first bottom end, a sixth via hole and a seventh via hole are formed at both ends in the width direction of the first bottom end located at a predetermined distance away from the second via hole, and the sixth via hole and the seventh via hole both communicate from the first bottom end to the opposing second bottom end.
[0010] Further, before etching a target edge of the second via hole on the front side, which is an edge close to the other end of the first bottom end, to form a shallow groove, the N crystal resonator wafer is formed. For each of the first grooves and the opposing second grooves, when the length of the second bottom end is longer than the length of the first bottom end, a fifth via hole is formed in the center of the first bottom end in the width direction at the other end position of the first bottom end, and the fifth via hole is connected from the first bottom end to the opposing second bottom end; or When the length of the second bottom end is equal to the length of the first bottom end, an eighth via hole is formed in a center portion of the width direction of the first bottom end, located at a position a predetermined distance away from the second via hole, and the eighth via hole further includes connecting from the first bottom end to the opposing second bottom end.
[0011] According to a second measure, the crystal resonator wafer of the present invention is The crystal wafer includes an oscillation region, an electrode region, and a frame region, which are arranged in sequence along the length of the crystal wafer, wherein the thickness of the electrode region is equal to or less than the thickness of the frame region; When the thickness of the electrode region is thinner than the thickness of the frame region, the contact point between the back surface of the electrode region and the back surface of the frame region transitions via a first slope, the front surface of the electrode region and the front surface of the frame region are flush with each other, the front surface of the electrode region includes a second slope and a top that is flush with the front surface of the frame region, and the back surface of the electrode region and the back surface of the oscillation region are flush with each other, or When the thickness of the electrode region is equal to the thickness of the frame region, the thickness of the electrode region is equal to the thickness of the oscillation region; The substrate further includes a second via hole having a shallow groove at a contact point between the front surface of the frame region and the front surface of the electrode region, the second via hole having the shallow groove as an edge in the frame region.
[0012] Furthermore, if the thickness of the electrode region is smaller than the thickness of the frame region, The semiconductor device further includes a third via hole and a fourth via hole located at the bottom end of the first slope, the third via hole and the fourth via hole being located at the boundary between the oscillation region and the second slope, and being located on both sides of the bottom of the first slope, and being used to weaken vibration of the oscillation frequency transmitted from the oscillation region to the electrode region.
[0013] Furthermore, if the thickness of the electrode region is smaller than the thickness of the frame region, The fifth via hole is located at the bottom end of the second slope, and is located at the boundary between the oscillation region and the first slope, facing the center of the first slope, and is used to weaken vibration of the oscillation frequency transmitted from the oscillation region to the electrode region.
[0014] Furthermore, if the thickness of the electrode region is equal to the thickness of the frame region, A sixth via hole and a seventh via hole at both ends along the width direction of the quartz crystal wafer at a location a predetermined distance away from the second via hole, which is the length of the electrode region, or The semiconductor device further includes an eighth via hole at a predetermined distance from the second via hole, in the central portion along the width direction of the quartz-crystal wafer.
[0015] Furthermore, the shallow groove is specifically One of a continuous strip-like structure and a discontinuous dot-like structure; The dots in the discontinuous dot structure are specifically It is one of the following shapes: circular, rectangular, or diamond. Effect of the Invention
[0016] The technical solution of the present invention has at least the following technical effects or advantages:
[0017] A method for manufacturing a quartz resonator wafer according to the present invention includes providing a quartz wafer, etching a front surface of the quartz wafer to form N first grooves, and etching a rear surface of the quartz wafer to form N second grooves, the N first grooves and the N second grooves facing each other, each of the first grooves and each of the second grooves having a structure that is wider at the top and narrower at the bottom, a width of a second bottom end of each second groove is equal to a width of a first bottom end of the opposing first groove, a length of the second bottom end is equal to or longer than a length of the first bottom end, one end of the second bottom end faces one end of the first bottom end, and the other end of the second bottom end exceeds the other end of the first bottom end or faces the other end of the first bottom end, N is a positive integer, and each of the first grooves and the opposing second grooves are formed on a first surface of the quartz wafer. the second groove formed on the first bottom end from a position directly opposite one end of the second bottom end to the back surface to form a first via hole whose length is equal to or greater than the width of the first bottom end; the second groove formed on the first bottom end from a position directly opposite the other end of the second bottom end outside the other end of the first bottom end to the back surface to form a second via hole whose length is shorter than the width of the second bottom end; and the target edge of the second via hole on the front side, which is the edge closest to the other end of the first bottom end, is etched to form a shallow groove. When the formed quartz resonator wafer is folded, it can be folded along the shallow groove, so that the edge of the wafer is neat and free of notches or excess protrusions, further improving device performance. [Brief description of the drawings]
[0018] [Figure 1] FIG. 1 shows a schematic structural diagram of a crystal resonator wafer in the related art after folding, in which notches and excess protrusions exist; [Diagram 2] 2 shows a flowchart of a method for manufacturing a crystal resonator wafer in an embodiment of the present invention. [Diagram 3] FIG. 2 is a schematic diagram of forming N first grooves and N second grooves in an embodiment of the present invention; [Figure 4] FIG. 2 is a schematic diagram of forming N first grooves and N second grooves in an embodiment of the present invention; [Diagram 5]FIG. 2 is a schematic diagram of forming N first grooves and N second grooves in an embodiment of the present invention; [Figure 6] FIG. 2 is a schematic diagram of forming N first grooves and N second grooves in an embodiment of the present invention; [Figure 7] FIG. 2 is a schematic diagram of forming N first grooves and N second grooves in an embodiment of the present invention; [Figure 8] FIG. 2 is a schematic diagram of forming N first grooves and N second grooves in an embodiment of the present invention; [Figure 9] 1 shows a schematic diagram of forming a first via hole 312 and a second via hole 313 in a resonator wafer in an embodiment of the present invention. [Figure 10] 1 shows a schematic diagram of forming a first via hole 312 and a second via hole 313 in a resonator wafer in an embodiment of the present invention. [Figure 11] 1A and 1B show schematic diagrams of forming shallow trenches in an embodiment of the present invention. [Figure 12] 4A and 4B show schematic diagrams of forming a third via hole and a fourth via hole in an embodiment of the present invention. [Figure 13] FIG. 13 shows a schematic diagram of forming a fifth via hole in an embodiment of the present invention. [Figure 14] 1 shows a schematic diagram of forming a metal electrode in an embodiment of the present invention. [Figure 15] 1 shows a schematic diagram of forming a metal electrode in an embodiment of the present invention. [Figure 16] 1 shows a schematic diagram of forming a metal electrode in an embodiment of the present invention. [Figure 17] 1 shows a schematic diagram of forming a resonator wafer for a planar structure in an embodiment of the present invention. [Figure 18] 1 shows a schematic diagram of forming a resonator wafer for a planar structure in an embodiment of the present invention. [Figure 19] 1 shows a schematic diagram of forming a resonator wafer for a planar structure in an embodiment of the present invention. [Figure 20] 1 shows a schematic diagram of forming a resonator wafer for a planar structure in an embodiment of the present invention. [Figure 21a] 1 shows a schematic diagram of a structure of a crystal resonator wafer having bosses in an embodiment of the present invention. [Figure 21b] 1 is a schematic diagram showing the structure of a flat crystal resonator wafer according to an embodiment of the present invention; [Figure 22] 1 is a schematic diagram showing the structure of a crystal resonator wafer according to an embodiment of the present invention; [Figure 23] FIG. 13 is a schematic structural diagram of a crystal resonator wafer according to another embodiment of the present invention. [Figure 24] 1 shows a schematic diagram of shallow grooves with circular dot-like structures in an embodiment of the present invention. [Diagram 25] 1 shows the crystal resonator wafer edge structure after folding along the shallow groove of the circular dot structure in an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] Hereinafter, exemplary embodiments of the present disclosure will be described in more detail with reference to the drawings. Although the drawings show exemplary embodiments of the present disclosure, it should be understood that the present disclosure should not be limited to the embodiments described herein, but can be realized in various forms. On the contrary, these embodiments are provided to more fully understand the present disclosure and to fully convey the scope of the present disclosure to those skilled in the art. Various other advantages and benefits will become apparent to those skilled in the art upon reading the following detailed description of the preferred embodiments. The drawings are only for purposes of illustrating the preferred embodiments and are not to be construed as limiting the invention. Furthermore, the same reference numerals are used throughout the drawings to represent the same elements. EXAMPLES
[0020] The method for manufacturing a crystal resonator wafer according to the first embodiment of the present invention includes the following steps, as shown in FIG. S201 providing a quartz crystal wafer; Etching the front surface of the quartz crystal wafer to form N first grooves, and etching the back surface of the quartz crystal wafer to form N second grooves S202, where the N first grooves and the N second grooves face each other, each of the first grooves and each of the second grooves has a structure that is wider at the top and narrower at the bottom, the width of the second bottom end of each second groove is equal to the width of the first bottom end of the facing first groove, the length of the second bottom end is equal to or longer than the length of the first bottom end, one end of the second bottom end faces one end of the first bottom end, the other end of the second bottom end exceeds the other end of the first bottom end or faces the other end of the first bottom end, and N is a positive integer S202; Etching each of the first grooves and the opposing second grooves from a position at one end of the first bottom end directly opposite one end of the second bottom end to the back surface to form a first via hole having a length equal to the width of the first bottom end (S203); Etching from the other end of the second bottom end to the back surface directly opposite the first bottom end to form a second via hole having a length shorter than a width of the second bottom end (S204); Etching a front second via hole target edge, which is an inward edge of the first bottom end (S205), to form a shallow groove; and folding each crystal resonator wafer along a respective shallow groove to form N crystal resonator wafers S206.
[0021] The whole process of the crystal resonator wafer is taken as an example to be described in detail below.
[0022] As shown in FIG. 3, a quartz crystal wafer 301 is provided.
[0023] Then, as shown in FIGS. 4 to 8, the front surface of the quartz crystal wafer 301 is etched to form N first grooves 302, and the back surface of the quartz crystal wafer 301 is etched to form N second grooves 303.
[0024] Among them, N first grooves 302 and N second grooves 303 face each other, each of the first grooves 302 and each of the second grooves 303 has a structure in which the top is wider and the bottom is narrower, the width of the second bottom end of each second groove 303 is equal to the width of the first bottom end of the opposing first groove 303, the length of the second bottom end is longer than the length of the first bottom end, one end of the second bottom end faces one end of the first bottom end and the other end of the second bottom end exceeds the other end of the second bottom end, and N is a positive integer.
[0025] A specific etching method is as follows.
[0026] A first chromium film layer 304 and a first gold film layer 305 are formed in this order on the front surface of the quartz crystal wafer. forming a first photoresist layer 306 on the first gold film layer 305, and exposing and developing the first photoresist layer 306 to form N first etching regions 307; Etch the first etching region 307 to form N first grooves 302; Similarly, the N second grooves 303 on the back surface are formed in a similar manner.
[0027] A second chromium film layer 308 and a second gold film layer 309 are formed in this order on the back surface of the quartz crystal wafer 301. forming a second photoresist layer 310 on the second gold film layer 309, and exposing and developing the second photoresist layer 310 to form N second etching regions 311; The N second etching regions 311 are etched to form N second grooves 303 .
[0028] Among them, the first chromium film layer 304 and the second chromium film layer 308 are both 5 to 50 nm thick, and the first gold film layer 305 and the second gold film layer 309 are both thicker than 100 nm. The first photoresist 306 and the second photoresist 310 are both 0.5 μm thick.
[0029] Specifically, the etching of the first etching region 307 to form the N first grooves 302 includes the following steps: The method includes using an etching solution to etch the first gold film layer 305 and the first chromium film layer 304 in the first etching region 307 to form N first grooves 302 .
[0030] After forming the N number of first grooves 302, It further includes removing the first photoresist layer 306, the first gold film layer 305 and the first chromium film layer 304 except for the first etching region 307, where they are similarly removed using an etchant.
[0031] Etching the second etching region 311 to form N second grooves 303 Etching the second photoresist 310, the second gold film layer 309 and the second chromium film 308 in the second etching region 311 using an etching solution to form N second grooves 303; After forming N second grooves 303, The method further includes removing the second photoresist layer 310, the second gold film layer 309 and the second chromium film layer 308 except for the second etching region 311.
[0032] The etching solutions include a gold etching solution, a chromium etching solution, and a BOE etching solution. The gold etching solution is a mixed aqueous solution of iodine and potassium iodide, and is used to corrode the first gold film layer 305 and the second gold film layer 309. The chromium etching solution is a mixed aqueous solution of nitric acid and cerium ammonium nitrate, and is used to corrode the first chromium film layer 304 and the second chromium film layer 308. The BOE etching solution is a mixed solution of hydrofluoric acid, ammonium bifluoride, and a corrosion inhibitor, and is used to corrode the crystal wafer 301. The specific corrosion depth is 40 to 190 μm, so that the frequency of the crystal wafer region after corrosion is greater than 60 MHz, and preferably 96 MHz. By using this BOE etching solution, it is possible to achieve an effect that the roughness in the pit region in the deep corrosion state does not change compared to before processing.
[0033] The photoresist may be removed by plasma desmear, chemical desmear, or the like.
[0034] There are two types of structures for the first groove 302 and the opposing second groove 303 thus formed.
[0035] First, in order to form a crystal resonator wafer having a boss, in this case, the length of the second bottom end of the second groove 303 is longer than the length of the first bottom end of the first groove 302 .
[0036] Secondly, to form a crystal resonator wafer with a flat plate structure, in this case, the length of the second bottom end of the second groove 303 is equal to the length of the first bottom end of the first groove 302 .
[0037] In a specific embodiment, when the thickness of the quartz crystal wafer is thinner than 10 μm, a quartz crystal resonator wafer having a boss can be formed, when the thickness of the quartz crystal wafer is between 10 and 30 μm, a quartz crystal resonator wafer having a boss or a quartz crystal resonator wafer having a flat structure can be formed, and when the thickness of the quartz crystal wafer is thicker than 30 μm, a quartz crystal resonator wafer having a flat structure can be formed.
[0038] The following will be described by taking as an example a case where the length of the second bottom end of the second groove 303 is longer than the length of the first bottom end of the first groove 302. As shown in Fig. 9, S203 is performed in which etching is performed from a position at one end of the first bottom end directly facing one end of the second bottom end to the back surface to form a first via hole 312 whose length is equal to the width of the first bottom end.
[0039] As shown in FIG. 10, in S204, etching is performed from the other end of the second bottom end to the front surface directly facing the second bottom end to form a second via hole 313 whose length is shorter than the width of the second bottom end.
[0040] In the process of forming the first via hole 312 and the second via hole 313, the chrome film layer, the gold film layer and the photoresist layer are formed in the same manner as described above, and the etching is performed by performing exposure and development again, which will not be described in detail here. The order of S204 and S203 may be reversed.
[0041] As shown in FIG. 11, S205 is performed to form a shallow groove 314 by etching a target edge of the front second via hole 313, which is an edge close to the other end of the first bottom end.
[0042] As shown in FIGS. 12 and 13, before S205, the first groove 302 may be etched to form a hollow structure, which can block the oscillation from the oscillation region of the quartz crystal wafer to the electrode region, thereby improving the performance of the device.
[0043] Specifically, as shown in FIG. 12, before S205, for each first groove 302 and the opposing second groove 303, at the other end position of the first bottom end, a third via hole 315 and a fourth via hole 316 are formed at both ends located in the width direction of the first bottom end, and the third via hole 315 and the fourth via hole 316 both further include communicating from the first bottom end to the opposing second bottom end.
[0044] In another embodiment, as shown in FIG. 13, before S205, for each first groove 302 and the opposing second groove 303, at the position of the other end of the first bottom end, a fifth via hole 317 is formed in the middle located in the width direction of the first bottom end, and this fifth via hole 317 further includes connecting from the first bottom end to the opposing second bottom end.
[0045] The process of forming the hollow structure also adopts the above etching method, which will not be described in detail here.
[0046] Before forming the hollow structure, the method further includes a process of forming an electrode, specifically, after S205, the method further includes forming a first metal electrode 318 on the first bottom end of the first groove 302, on the second bottom end of the second groove 303, and extending from the first bottom end to the outside of the other end of the first bottom end.
[0047] Of course, the first metal electrode 318 may be formed after the hollow structure is formed, and is not particularly limited here.
[0048] 14 to 16, the first metal electrode 318 is formed in the first groove 302, in the second groove 303, and extending from the first bottom end to the other end of the first bottom end and outside the first groove 302, and the vibration electrode and the pin electrode are left by etching. The etching method here is the same as the etching method described above.
[0049] Finally, each of the formed N crystal resonator wafers is folded along its respective shallow groove 314 to form N crystal resonator wafers, such that the resulting crystal resonator wafers are free of notches or protruding structures, further improving device performance.
[0050] By batch processing the entire crystal wafer to form N crystal resonator wafers, the efficiency of obtaining crystal resonator wafers with relatively excellent performance can be improved, and production efficiency can be further improved.
[0051] The above is a description of a crystal resonator wafer having bosses, and the following is a description of a crystal resonator wafer having a flat structure.
[0052] Specifically, as shown in FIG. 17, in S202, when the second groove 303 is formed, the length of the second bottom end of the second groove 303 is equal to the length of the first bottom end of the first groove 302.
[0053] 18, in steps S203 and S204, when the first via hole 312 and the second via hole 313 are formed, the first via hole 312 and the second via hole 313 are both located within the first groove 302. In steps S203 and S204, as shown in FIG.
[0054] At the same time, a third via hole and a fourth via hole can be formed in the first groove 302, or a fifth via hole, ie, a hollow structure can be directly formed.
[0055] Specifically, as shown in FIG. 19, for each first groove 302 and the opposing second groove 303, a sixth via hole 1901 and a seventh via hole 1902 are formed at both ends in the width direction of the first bottom end at a location at a predetermined distance from the second via hole 313 at the first bottom end, and both the sixth via hole 1901 and the seventh via hole 1902 connect from the first bottom end to the opposing second bottom end.
[0056] As shown in FIG. 20, an eighth via hole 2001 is formed in the center of the width of the first bottom end, located at a predetermined distance away from the second via hole 313, and the eighth via hole 2001 connects from the first bottom end to the opposing second bottom end.
[0057] The purpose of the above two types of openings is to block the transmission of oscillation vibration from the oscillation region of the crystal resonator wafer to the electrode region, thereby improving the performance of the device.
[0058] Next, when the length of the second bottom end is equal to the length of the first bottom end, a second metal electrode is formed at the first bottom end of the first groove 302 and the second bottom end of the second groove 303, which will not be described in detail here.
[0059] Finally, the crystal resonator wafer is folded along the shallow groove 314, resulting in a more perfect edge of the crystal resonator wafer and improving the performance of the device.
[0060] The shallow groove 314 is specifically a continuous strip-like structure or a discontinuous dot-like structure, in which the dots in the discontinuous dot-like structure are specifically circular, rectangular or diamond-shaped.
[0061] One or more technical solutions in the embodiments of the present invention have at least the following technical effects or advantages:
[0062] A method for manufacturing a quartz resonator wafer according to the present invention includes providing a quartz wafer, etching a front surface of the quartz wafer to form N first grooves, and etching a rear surface of the quartz wafer to form N second grooves, the N first grooves and the N second grooves facing each other, each of the first grooves and each of the second grooves having a structure that is wider at the top and narrower at the bottom, a width of a second bottom end of each second groove is equal to a width of a first bottom end of the opposing first groove, a length of the second bottom end is equal to or longer than a length of the first bottom end, one end of the second bottom end faces one end of the first bottom end, and the other end of the second bottom end exceeds the other end of the second bottom end or faces the other end of the first bottom end, N is a positive integer, and each of the first grooves and the second grooves are formed on a first surface of the quartz wafer. and etching from the other end of the second bottom end to the back surface facing the other end of the second bottom end to form a second via hole whose length is shorter than the width of the second bottom end. And etching a target edge of the second via hole on the front side, which is the edge close to the other end of the first bottom end, to form a shallow groove. When the formed crystal resonator wafer is folded, it can be folded along the shallow groove, so that the edge of the wafer is neat and free of notches or excess protrusions, and further improving the performance of the device. EXAMPLES
[0063] The second embodiment of the present invention further provides a crystal resonator wafer, as shown in Figs. 21a and 21b, The crystal wafer includes an oscillation region 2101, an electrode region 2102, and a frame region 2103, which are arranged in sequence along the length of the crystal wafer. The thickness of the electrode region 2102 is equal to or less than the thickness of the frame region 2103, When the thickness of the electrode region 2102 is thinner than the thickness of the frame region 2101, the contact point between the back surface of the electrode region 2102 and the back surface of the frame region 2103 transitions via the first slope 2105, the front surface of the electrode region 2102 and the front surface of the frame region 2103 are flush with each other, the front surface of the electrode region 2102 includes the second slope 2104 and a top that is flush with the front surface of the frame region 2103, the back surface of the electrode region 2102 and the back surface of the oscillation region 2101 are flush with each other, When the thickness of the electrode region 2102 is equal to the thickness of the frame region 2101, the thickness of the electrode region 2102 is equal to the thickness of the oscillation region 2101; A shallow groove 314 is formed at the contact point between the front surface of the frame region 2103 and the front surface of the electrode region 2102 , and a second via hole 313 is further included in the frame region 2103 with the shallow groove 314 as its edge.
[0064] 21a shows a crystal resonator wafer with bosses, ie, the thickness of the electrode region 2102 is thinner than the thickness of the frame region 2103. FIG.
[0065] FIG. 21b shows a quartz crystal resonator wafer with a flat structure, ie, the thickness of the electrode region 2102 is equal to the thickness of the frame region 2103. FIG.
[0066] In one optional embodiment, when the thickness of the electrode region 2102 is thinner than that of the frame region 2103, the crystal resonator wafer further includes a third via hole 315 and a fourth via hole 316 located at the bottom end of the second slope 2104, the third via hole 315 and the fourth via hole 316 located at the boundary between the oscillation region 1701 and the second slope 2104, located on both sides of the bottom of the second slope 2104, and used to weaken the vibration of the oscillation frequency transmitted from the oscillation region 1701 to the electrode region 2102. As shown in FIG. 22, the function of the third via hole 315 and the fourth via hole 316 is to weaken the vibration of the oscillation frequency transmitted from the oscillation region 1701 to the electrode region 1702, thereby improving the performance of the device.
[0067] In one optional embodiment, when the thickness of the electrode region 2102 is thinner than that of the frame region 2103, the crystal resonator wafer further includes a fifth via hole 317 located at the bottom end of the second slope 2104, which is located at the boundary between the oscillation region 1701 and the second slope 1704, facing the middle of the second slope 2104, and is used to weaken the vibration of the oscillation frequency transmitted from the oscillation region to the electrode region. As shown in FIG. 23, the function of the fifth via hole 317 is to weaken the vibration of the oscillation frequency transmitted from the oscillation region 2101 to the electrode region 2102, thereby improving the performance of the device.
[0068] Of course, this crystal resonator wafer further includes a first metal electrode 318 located in the oscillation region 2101 and the electrode region 2102, of which the one located in the oscillation region 2101 is an oscillation electrode and the one located in the electrode region 2102 is a pin electrode, which will not be described in detail here.
[0069] In one alternative embodiment, as shown in Figs. 19 and 20, when the thickness of the electrode region 2102 is equal to the thickness of the frame region 2103, the crystal resonator wafer has: The sixth via hole 1901 and the seventh via hole 1902 at both ends along the width direction of the quartz-crystal wafer at a location away from the second via hole 313 by a preset distance that is the length of the electrode region 2102, or It further includes an eighth via hole 2001 at a location a preset distance away from the second via hole 313 and in the central portion along the width direction of the quartz-crystal wafer.
[0070] Similarly, using the sixth via hole 1901, the seventh via hole 1902, or directly using the eighth via hole 2001, is to weaken the oscillation frequency vibration transmitted from the oscillation region 2101 to the electrode region 2102, thereby improving the performance of the device.
[0071] Of course, when the thickness of the electrode region 2102 is equal to the thickness of the frame region 2103, the crystal resonator wafer further includes a second metal electrode located in the oscillation region 2101 and the electrode region 2102, among which the one located in the oscillation region 2101 is an oscillation electrode, and the one located in the electrode region 2102 is a pin electrode, which will not be described in detail here.
[0072] The shallow grooves on the above two types of crystal resonator wafers are specifically One of a continuous strip-like structure and a discontinuous dot-like structure; Among them, the dots in the discontinuous dot structure are specifically It is one of the following shapes: circular, rectangular, or diamond.
[0073] Specifically, the shallow grooves 314 shown in FIG. 21b are discontinuous dot-like structures, of which rectangular dots are taken as an example for schematic illustration.
[0074] The shallow groove 314 shown in Fig. 24 is a discontinuous dot structure, among which the dot is a circular structure. After folding along the shallow groove 314 of the circular dot structure, the edge structure shown in Fig. 25 is formed.
[0075] The shallow grooves allow for easy folding.
[0076] Although the preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they have grasped the basic creative concept. Therefore, it is intended that the appended claims be interpreted to include the preferred embodiments and all changes and modifications that are within the scope of the present invention.
[0077] Obviously, those skilled in the art can make various modifications and variations to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. 1. A method for fabricating a quartz crystal resonator wafer, comprising the steps of: Providing a quartz crystal wafer; Etching the front surface of the quartz crystal wafer to form N first grooves, and etching the back surface of the quartz crystal wafer to form N second grooves, the N first grooves and the N second grooves facing each other, each of the first grooves and each of the second grooves having a structure that is wider at the top and narrower at the bottom, the width of a second bottom end of each second groove is equal to the width of a first bottom end of the opposing first groove, the length of the second bottom end is equal to or longer than the length of the first bottom end, one end of the second bottom end in the length direction faces one end of the first bottom end in the length direction, the other end of the second bottom end exceeds the other end of the first bottom end in the length direction or faces the other end of the first bottom end in the length direction, and N is a positive integer; etching each of the first grooves and the opposing second grooves from a position at one end of the first bottom end in a longitudinal direction directly opposite one end of the second bottom end to the back surface to form a first via hole having a length equal to a width of the first bottom end; Etching from the other end of the second bottom end in the length direction to the front surface directly facing the first bottom end to form a second via hole having a length shorter than a width of the second bottom end; Etching a target edge of the second via hole on the front side, which is an edge close to the other end in the length direction of the first bottom end, to form a shallow groove, the shallow groove being formed at a boundary between a frame region and an electrode region of the quartz crystal wafer; and folding each crystal resonator wafer along a respective one of said shallow grooves to form N crystal resonator wafers.
2. After etching the target edge of the second via hole on the front side to form a shallow groove, When the length of the second bottom end is longer than the length of the first bottom end, a first metal electrode is formed on the first bottom end of the first groove, on the second bottom end of the second groove, and extending from the first bottom end to the other end in the length direction of the first bottom end and to the outside of the first groove; or 2. The method for fabricating a quartz crystal resonator wafer as claimed in claim 1, further comprising: forming a second metal electrode on the first bottom end of the first groove and the second bottom end of the second groove when the length of the second bottom end is equal to the length of the first bottom end.
3. Etching the front surface of the quartz crystal wafer to form N first grooves, and etching the back surface of the quartz crystal wafer to form N second grooves. forming a first chromium film layer and a first gold film layer in order from bottom to top on the front surface of the quartz crystal wafer; forming a first photoresist layer on the first gold film layer, and exposing and developing the first photoresist layer to form N first etching regions; Etching the N first etching regions to form N first grooves; forming a second chromium film layer and a second gold film layer in order from bottom to top on the rear surface of the quartz crystal wafer; forming a second photoresist layer on the second gold film layer, and exposing and developing the second photoresist layer to form N second etching regions; 2. The method for manufacturing a quartz crystal resonator wafer as claimed in claim 1, further comprising: etching said N number of second etching regions to form N number of second grooves.
4. before etching a target edge of the front second via hole, the target edge being an inward edge of the first bottom end, to form a shallow trench; For each of the first grooves and the opposing second grooves, when the length of the second bottom end is longer than the length of the first bottom end, a third via hole and a fourth via hole are formed at both ends located in the width direction of the first bottom end at the other end position of the first bottom end in the length direction, and the third via hole and the fourth via hole are both connected from the first bottom end to the opposing second bottom end; or 2. The method for manufacturing a quartz crystal resonator wafer according to claim 1, further comprising: forming a sixth via hole and a seventh via hole at both ends in a width direction of the first bottom end located at a position a predetermined distance away from the second via hole in the first bottom end when the length of the second bottom end is equal to the length of the first bottom end, and the sixth via hole and the seventh via hole both communicate from the first bottom end to the opposing second bottom end.
5. before etching a target edge of the second via hole on the front side, which is an edge close to the other end in the length direction of the first bottom end, to form a shallow groove; For each of the first grooves and the opposing second grooves, when the length of the second bottom end is longer than the length of the first bottom end, a fifth via hole is formed in a central portion located in a width direction of the first bottom end at the other end position of the first bottom end in the length direction, and the fifth via hole is connected from the first bottom end to the opposing second bottom end; or 2. The method for manufacturing a quartz crystal resonator wafer according to claim 1, further comprising: forming an eighth via hole in a central portion of the first bottom end in a width direction thereof, the eighth via hole being located at a predetermined distance from the second via hole in the first bottom end when the length of the second bottom end is equal to the length of the first bottom end, the eighth via hole being connected from the first bottom end to the opposing second bottom end.
Citation Information
Patent Citations
Piezoelectric oscillator element and manufacturing method thereof, and piezoelectric device
JP2003110388A
Piezoelectric wafer and piezoelectric device
JP2007142526A
Method of manufacturing piezoelectric vibration chip, piezoelectric vibration chip, and piezoelectric device
JP2007214942A
Piezoelectric device and manufacturing method thereof
JP2009065520A
Piezoelectric substrate, method of manufacturing the same, and method of manufacturing piezoelectric vibrating reed
JP2012105074A