Glass manufacturing method

By using a partition member and moving the mold relative to it to control melt flow, the method addresses oxidation suppression and productivity issues in glass manufacturing, enhancing production efficiency and quality.

JP7593070B2Active Publication Date: 2024-12-03NIPPON ELECTRIC GLASS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020191564
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-18
Publication Date
2024-12-03
Estimated Expiration
2040-11-18

AI Technical Summary

Technical Problem

Existing glass manufacturing methods, such as those described in Patent Document 1, require steps to suppress oxidation by creating an inert atmosphere, which hinders productivity.

Method used

A method involving the use of a partition member in the mold, where the mold is moved relative to the partition member to increase the inlet volume while flowing the melt, allowing the melt to flow into the mold without prolonged contact with air, thus suppressing oxidation and maintaining a constant melt thickness.

Benefits of technology

This method effectively suppresses oxidation and increases productivity by minimizing melt exposure to air, reducing the formation of foreign layers and striae in the glass, without the need for an inert atmosphere.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007593070000001
    Figure 0007593070000001
  • Figure 0007593070000002
    Figure 0007593070000002
  • Figure 0007593070000003
    Figure 0007593070000003
Patent Text Reader

Abstract

To provide a method for manufacturing glass that can readily suppress oxidation and improve productivity.SOLUTION: A method for manufacturing glass includes the steps of: flowing a molten liquid 11 of a molten glass raw material into a mold 13; and cooling the molten liquid 11 to obtain glass 18, where a partition member 16 is disposed in the mold 13 and an inflow part 17 is configured by being surrounded by the mold 13 and the partition member 16 and, in the step of flowing the molten liquid 11 into the mold 13, the molten liquid 11 is flown into the inflow part 17 while increasing the capacity of the inflow part 17 by moving the mold 13 relative to the partition member 16.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing glass. [Background technology]

[0002] In recent years, chalcogenide glass has been known as a material that is preferably used in the field of infrared optics. Chalcogenide glass is not only transparent to infrared rays, but also has advantages in terms of mass productivity and cost reduction due to its applicability to mold presses.

[0003] When manufacturing optical members such as lenses, for example, molten glass is quenched and cast to produce a glass ingot, which is then ground, polished, and cleaned to produce a glass preform, which is then molded by press molding or the like to produce an optical member such as a lens.

[0004] An example of a method for manufacturing a glass article is disclosed in the following Patent Document 1. In this manufacturing method, molten glass is poured into a bottomed cylindrical mold and cast to obtain a glass ingot. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2015-209364 A Summary of the Invention [Problem to be solved by the invention]

[0006] When forming glasses such as chalcogenide glasses, it is necessary to suppress oxidation. However, in the method described in Patent Document 1, the melt flowing into the mold is in contact with air over an area equivalent to the opening area of ​​the mold. Therefore, in order to suppress oxidation, a process such as making the molding environment an inert atmosphere is required, making it difficult to increase productivity.

[0007] An object of the present invention is to provide a method for producing glass, which can easily suppress oxidation and increase productivity. [Means for solving the problem]

[0008] The method for producing glass according to the present invention comprises a step of pouring a molten liquid obtained by melting glass raw materials into a forming mold, and a step of obtaining glass by cooling the molten liquid, wherein a partition member is disposed within the forming mold, and an inflow section is formed surrounded by the forming mold and the partition member, and in the step of pouring the molten liquid into the forming mold, the forming mold is moved relative to the partition member to increase the volume of the inflow section while causing the molten liquid to flow into the inflow section.

[0009] In the step of pouring the melt into the mold, it is preferable to keep the thickness of the melt constant when the mold is moved relative to the partition member.

[0010] In the step of pouring the melt into the mold, it is preferable to move only the mold.

[0011] The step of pouring the melt into the mold is preferably carried out in an air atmosphere.

[0012] Preferably, the glass is a chalcogenide glass. Effect of the Invention

[0013] According to the present invention, it is possible to provide a method for producing glass that can easily suppress oxidation and increase productivity. [Brief description of the drawings]

[0014] [Figure 1] 1(a) to 1(c) are schematic cross-sectional views illustrating a process up to a step of heating a raw material in a glass manufacturing method according to a first embodiment of the present invention. [Diagram 2]1(a) and 1(b) are schematic cross-sectional views illustrating the process after stirring the melt in the glass manufacturing method according to the first embodiment of the present invention. [Diagram 3] 1(a) to 1(d) are schematic cross-sectional views illustrating the step of pouring a melt into a molding die in the glass manufacturing method according to the first embodiment of the present invention. [Figure 4] 2(a) to 2(d) are schematic cross-sectional views showing a method for producing glasses of Reference Examples. [Diagram 5] FIG. 4 is a schematic perspective view of a molding die used in a glass manufacturing method according to a second embodiment of the present invention. [Figure 6] FIG. 11 is a schematic perspective view of a molding die used in a glass manufacturing method according to a third embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Hereinafter, preferred embodiments will be described. However, the following embodiments are merely examples, and the present invention is not limited to the following embodiments. In addition, in the drawings, components having substantially the same functions may be referred to by the same reference numerals.

[0016] (Glass manufacturing method) (First embodiment) The present embodiment is characterized in that the melt of the raw material is poured into a mold. The manufacturing method of the present embodiment will be described below with reference to the drawings.

[0017] Fig. 1(a) to Fig. 1(c) are schematic cross-sectional views for explaining the process up to the step of heating the raw materials in the glass manufacturing method according to the first embodiment of the present invention. Fig. 2(a) and Fig. 2(b) are schematic cross-sectional views for explaining the process after the step of stirring the molten liquid in the glass manufacturing method according to the first embodiment of the present invention. Fig. 3(a) to Fig. 3(d) are schematic cross-sectional views for explaining the step of pouring the molten liquid into a forming die in the glass manufacturing method according to the first embodiment of the present invention. For convenience, coil 10A or coil 10B is omitted in some of the drawings.

[0018] The manufacturing method of this embodiment is a method for manufacturing chalcogenide glass as one example of the present invention, although the method of the present invention can also be applied to the manufacture of glasses other than chalcogenide glass.

[0019] As shown in Fig. 1(a), in this embodiment, a crucible is used as the container 1. The container 1 has a bottom 2 and a side wall 3. The container 1 is preferably made of quartz glass. This allows glass to be formed suitably in the following steps.

[0020] A pipe 4 is connected to the bottom 2 of the container 1. An outer tube 5 is disposed so as to surround the pipe 4. The pipe 4 passes through the inside of the outer tube 5. In this embodiment, the outer tube 5 is made of Pt. However, the outer tube 5 may be made of any suitable metal.

[0021] As shown in FIG. 1(a), glass raw material 6 is placed in container 1. In this embodiment, raw material 6 is a mixture containing components that constitute chalcogenide glass. In this embodiment, raw material 6 may contain metal. In the present invention, "metal" includes metal elements, semimetal elements, alkali metal elements, alkaline earth metal elements, and the like. Details of raw material 6 will be described later. It is preferable to melt a small amount of raw material 6 in advance to make a small amount of molten liquid 11, and to allow a small amount of molten liquid 11 to flow into pipe 4. The small amount of molten liquid 11 is cooled in pipe 4 and becomes a solidified material (solid glass). This allows plug 12 to be formed. By forming plug 12, raw material 6 can be stably placed even if pipe 4 is connected to bottom 2 of container 1.

[0022] Next, as shown in FIG. 1(b), a lid 7 is placed on the side wall 3 of the container 1. A gas supply pipe 8 and a gas exhaust pipe 9 are connected to the lid 7. Gas is exhausted from the container 1 through the gas exhaust pipe 9 to reduce the pressure. Next, an inert gas or a reducing gas is supplied into the container 1 through the gas supply pipe 8. By repeating this process, the inside of the container 1 is made into an inert atmosphere or a reducing atmosphere.

[0023] When forming chalcogenide glass, it is necessary to prevent the heated raw material 6 from reacting with oxygen or moisture. In this embodiment, the air in the container 1 is replaced with an inert gas or a reducing gas, so that oxygen and moisture are removed from the container. Therefore, chalcogenide glass can be suitably formed without using a sealed container kept in a vacuum state. In this embodiment, as described later, the formed glass can be discharged from the container 1 through the pipe 4, so that it is not necessary to destroy the container 1 to take out the formed glass, and the container 1 can be reused.

[0024] Incidentally, as shown in FIG. 1(c), coil 10A is arranged so as to surround at least a part of side wall 3 of container 1. Specifically, coil 10A is arranged so as to surround the part of container 1 where raw material 6 is placed. Raw material 6 is induction-heated by passing a current through coil 10A. Specifically, an induced magnetic field generated by passing a current through coil 10A generates an induced current. Raw material 6 contains a metal, and metal has an internal resistance. Therefore, when an induced current flows through the metal, the metal contained in raw material 6 becomes a heat source, and the entire raw material 6 is heated. This induction heating turns raw material 6 into a melt 11 as shown in FIG. 2(a).

[0025] By passing a current through coil 10A, an induced magnetic field and an induced current are generated, and a Lorentz force is applied to melt 11. This Lorentz force can stir melt 11. In this manner, in this embodiment, melt 11 can be stirred without using a means for stirring melt 11 by directly contacting a member therewith, such as a stirrer. However, a stirrer or the like may also be used to stir melt 11.

[0026] As described above, a part of the melt 11 flows into the pipe 4. The melt 11 in the pipe 4 is cooled and solidifies (solid glass). This forms the plug 12. Therefore, a small amount of the melt 11 sufficient to form the plug 12 flows into the pipe 4, but the outflow of the remaining melt 11 is stopped by the plug 12. However, a lid, a plunger, or the like may be used instead of the plug 12.

[0027] As shown in FIG. 2(b), a coil 10B is disposed around the outer tube 5. By passing a current through the coil 10B, the outer tube 5 is induction heated. The pipe 4 and the plug 12 in the pipe 4 are heated by radiant heat from the outer tube 5. Note that the plug 12 is solid glass and does not contain a simple metal or alloy, and is therefore not induction heated. The plug 12 melts as a result of the above heating, and the molten liquid 11 flows out of the container 1.

[0028] It should be noted that the methods shown in FIGS. 1(a) to 1(c) and 2(a) and (b) are merely examples, and the methods for the step of melting the raw material 6 and the step of causing the melt 11 to flow are not limited to those described above.

[0029] As shown in FIG. 3(a), the melt 11 that has flowed out is caused to flow into a mold 13. In this embodiment, the mold 13 is a container having a rectangular parallelepiped outer shape. The mold 13 has a bottom surface portion 14 and a wall portion 15. The side of the mold 13 that faces the bottom surface portion 14 is open. A rectangular parallelepiped partition member 16 is disposed within the mold 13. Specifically, the partition member 16 is in contact with the bottom surface portion 14 and the wall portion 15 of the mold 13. This forms an inlet portion 17 surrounded by the bottom surface portion 14 and the wall portion 15 of the mold 13 and the partition member 16. The wall portion 15 includes an opposing portion 15a. The opposing portion 15a forms the inlet portion 17 and faces the partition member 16.

[0030] First, as shown in FIG. 3(a), melt 11 is allowed to flow into inlet 17 until melt 11 in mold 13 reaches a certain thickness (i.e., a certain liquid level height). In FIG. 3(a), the thickness of melt 11 is shown typically as the thickness up to the top end of wall 15, but the certain thickness of melt 11 is not limited to this. In this embodiment, the step of allowing melt 11 to flow into mold 13 and the step of cooling melt 11, which will be described later, are performed in an air atmosphere. In this case, in chalcogenide glass melt 11, the longer the contact time with the outside air, the more likely a heterogeneous layer 11a is formed on the surface. The heterogeneous layer 11a is composed of oxidized impurities and / or devitrified substances and / or glass solidified by quenching.

[0031] Next, as shown in Fig. 3(b) and Fig. 3(c), while melt 11 is flowing into mold 13, mold 13 is moved relative to partition member 16. As a result, melt 11 is caused to flow into mold 13 while increasing the volume of inflow portion 17. Specifically, mold 13 is slid while maintaining a state in which partition member 16 is in contact with bottom portion 14 and wall portion 15 of mold 13. Mold 13 is moved in a direction in which opposing portion 15a of wall portion 15 moves away from partition member 16. At this time, in this embodiment, partition member 16 and the above-mentioned piping 4 are not moved, and only mold 13 is moved. As a result, the opening area of ​​inflow portion 17 is increased, and the volume of inflow portion 17 is increased.

[0032] Next, as shown in FIG. 3(d), the melt 11 is cooled in the forming die 13 to form glass 18. In this embodiment, a rectangular columnar glass 18 can be obtained. A glass preform can be produced by grinding, polishing, and cleaning the glass 18. In addition, an optical member such as a lens can be produced by performing mold press molding or the like on the preform glass. Note that an optical member such as a lens may be produced directly from the glass 18 without producing a glass preform. In addition, the heterogeneous layer 11a can be removed by grinding, polishing, or the like.

[0033] The feature of this embodiment is that melt 11 is caused to flow into forming die 13 while moving forming die 13 relative to partition member 16 and increasing the volume of inflow portion 17. This makes it possible to easily suppress oxidation of melt 11 and increase the productivity of glass 18. Furthermore, striae in glass 18 can be suppressed. These details will be described below.

[0034] When melt is introduced into a conventional mold, the distance between the pipe and the melt surface gradually decreases as the melt is supplied, but the melt is supplied in a state where it is in contact with the outside air for a long time. The melt supplied while in contact with the outside air for a long time contains heterogeneous parts, and the liquid surface is constantly replaced by such melt. Therefore, in an area equivalent to the opening area of ​​the mold, the newly added melt containing heterogeneous parts and the previously supplied melt are constantly mixed together, and the glass melt accumulates in a heterogeneous state.

[0035] In contrast, as shown in FIG. 3(b) and FIG. 3(c), in this embodiment, after the melt 11 is allowed to flow into the inflow section 17 until the melt 11 in the mold 13 reaches a certain thickness, the melt 11 is allowed to flow into the mold 13 while increasing the volume of the inflow section 17. Here, when the melt 11 in the mold 13 reaches a certain thickness, a heterogeneous layer 11a is formed on the liquid surface of the melt 11. Therefore, the melt 11 that is allowed to flow into the mold 13 while increasing the volume of the inflow section 17 flows between the bottom section 14 and the heterogeneous layer 11a without contacting the outside air for a long time. Note that as the opening area of ​​the inflow section 17 increases, the area of ​​the heterogeneous layer 11a also increases. As a result, even if the mold 13 is slid, the inflow section 17 is covered by the heterogeneous layer 11a. Therefore, the melt 11 newly introduced into the mold 13 is prevented from coming into contact with the outside air by the heterogeneous layer 11a. This suppresses oxidation of the melt 11. This makes it possible to increase productivity.

[0036] Furthermore, according to the method of the present invention, the area of ​​melt 11 exposed to the outside air is not maximum from the beginning, but gradually increases as forming die 13 moves relative to partition member 16. This makes it possible to reduce the integrated value of the area of ​​melt 11 exposed to the outside air and the time. This makes it possible to easily suppress oxidation without going through a step of creating an inert atmosphere. This makes it possible to increase productivity.

[0037] The effect of suppressing the formation of striae in the glass in this embodiment will be described in detail below.

[0038] 4(a) to 4(d) are schematic cross-sectional views showing a manufacturing method of glass of a reference example. In the reference example, as shown in FIG. 4(a), melt 11 is made to flow into inflow section 17. Next, as shown in FIG. 4(b) and FIG. 4(c), partition member 16 is moved to increase the volume of inflow section 17, and melt 11 is made to flow into mold 13. At this time, melt 11 is relatively easily cooled at the portion of mold 13 in contact with facing portion 15a. Then, as shown in FIG. 4(b), melt 11 that first flows into inflow section 17 is cooled and solidified at the portion in contact with facing portion 15a, and even after solidification, high-temperature melt 11 continues to be supplied from pipe 4 to the vicinity of the solidified portion. Therefore, a part of the solidified portion is melted by high-temperature melt 11. Furthermore, as shown by the dashed arrow in FIG. 4(b), a liquid that is a part of the solidified portion is mixed with supplied melt 11. This tends to result in inhomogeneity of the melt 11. Furthermore, as shown in Fig. 4(d), the melt 11 as described above is cooled to form glass 18, which tends to result in striae.

[0039] 3(a) to 3(d), in contrast, forming die 13 is moved. At this time, in the portion near partition member 16, the relative position between bottom surface portion 14 and partition member 16 changes, so that immediate solidification of melt 11 does not occur in the portion near partition member 16.

[0040] On the other hand, the melt 11 is relatively easy to solidify in the portion in contact with the facing portion 15a of the mold 13. Here, in this embodiment, the facing portion 15a is moved away from the partition member 16 and the pipe 4. Therefore, when the melt 11 that first flows into the inlet portion 17 is cooled and solidified, the facing portion 15a is away from the pipe 4. Therefore, the high-temperature melt 11 is unlikely to come into contact with the solidified portion. Therefore, it is unlikely that a part of the solidified portion melts as in the reference example, and the melt 11 is unlikely to become inhomogeneous. Therefore, the striae of the glass 18 can be suppressed.

[0041] In the step of pouring melt 11 into mold 13, it is desirable to keep the thickness of melt 11 constant. This makes it possible to keep the distance between the tip of pipe 4 and the surface of melt 11 short, and to prevent melt 11 being supplied from coming into excessive contact with the outside air. This makes it possible to effectively prevent melt 11 from being oxidized.

[0042] When melt 11 is poured into forming die 13, it is preferable to move only forming die 13 as in this embodiment. In other words, it is preferable not to move partition member 16 in the step of pouring melt 11 into forming die 13. This makes it easier to keep the thickness of melt 11 constant. This makes it possible to more reliably suppress solidification of melt 11 near pipe 4, and more reliably suppress melting of the solidified portion. Therefore, it is possible to more reliably suppress striae in glass 18.

[0043] Alternatively, the flow of melt 11 into mold 13 may be started with bottom portion 14 of mold 13 brought close to pipe 4, and melt 11 may be allowed to flow into mold 13 while mold 13 is moved away from pipe 4, and after melt 11 reaches a certain thickness in mold 13, melt 11 may be allowed to flow into mold 13 while mold 13 is slid as described above. This can further prevent melt 11 from coming into contact with the outside air. This is particularly suitable when inflow portion 17 is thick.

[0044] The ratio of materials contained in the raw material 6 of this embodiment is adjusted so as to obtain glass 18 having the following composition. In the description of the composition of glass 18, "%" means "mol %." For example, the total content of A, B, and C may be expressed as "content of A+B+C" or "A+B+C."

[0045] The glass 18 formed by the method of the present embodiment has a glass composition containing, in molar ratios, from greater than 0% to 50% Ge, from greater than 0% to 50% Ga, from 30% to 90% Te, from greater than 0% to 40% Ag+Al+Ti+Cu+In+Sn+Bi+Cr+Zn+Mn, and from 0% to 50% F+Cl+Br+I.

[0046] Ge is a component for forming a glass skeleton. Ge is a semimetal element. The Ge content is more than 0% to 50%, preferably 2% to 40%, more preferably 4% to 35%, even more preferably 5% to 30%, even more preferably 7% to 25%, and even more preferably 10% to 20%. If the Ge content is too low, vitrification becomes difficult. On the other hand, if the Ge content is too high, Ge-based crystals tend to precipitate easily and the raw material cost tends to increase.

[0047] Ga is a component for increasing the thermal stability (vitrification stability) of glass. Ga is a metal element. The Ga content is more than 0% to 50%, preferably 1% to 45%, more preferably 2% to 40%, even more preferably 4% to 30%, even more preferably 5% to 25%, and even more preferably 10% to 20%. If the Ga content is too low, vitrification becomes difficult. On the other hand, if the Ga content is too high, Ga-based crystals tend to precipitate easily and the raw material cost tends to increase.

[0048] Te, a chalcogen element, is a component that is essential for forming a glass skeleton. Te is also a metalloid element. The content of Te is 30% to 90%, preferably 40% to 89%, more preferably 50% to 88%, even more preferably 60% to 86%, and even more preferably 70% to 85%. If the content of Te is too low, vitrification becomes difficult. On the other hand, if the content of Te is too high, Te-based crystals are likely to precipitate.

[0049] Ag+Al+Ti+Cu+In+Sn+Bi+Cr+Zn+Mn are metal elements. The glass contains the above metal elements, which can enhance thermal stability. The content of Ag+Al+Ti+Cu+In+Sn+Bi+Cr+Zn+Mn is 0% to 40%, preferably more than 0% to 30%, more preferably more than 0% to 20%, and even more preferably 0.1% to 10%. If the content of Ag+Al+Ti+Cu+In+Sn+Bi+Cr+Zn+Mn is too low or too high, vitrification becomes difficult. The content of each component of Ag+Al+Ti+Cu+In+Sn+Bi+Cr+Zn+Mn is 0% to 40%, preferably 0% to 30% (at least one of them is more than 0%), more preferably 0% to 20% (at least one of them is more than 0%), and even more preferably 0.1% to 10%. Among these, it is preferable to use Ag and / or Sn, since they have a particularly large effect of increasing the thermal stability of the glass.

[0050] The glass formed in this embodiment may contain, in addition to the above components, the following components, for example.

[0051] F, Cl, Br, and I are also components that enhance the thermal stability of glass. The content of F+Cl+Br+I is 0% to 50%, preferably 1% to 40%, more preferably 1% to 30%, even more preferably 1% to 25%, and particularly preferably 1% to 20%. If the content of F+Cl+Br+I is too high, vitrification becomes difficult and weather resistance is easily reduced. The contents of each of F, Cl, Br, and I are each 0% to 50%, preferably 1% to 40%, more preferably 1% to 30%, even more preferably 1% to 25%, and particularly preferably 1% to 20%. Among them, it is preferable to use I, since elemental raw materials can be used and the effect of enhancing glass stability is particularly large.

[0052] By including Si, Sb, and Cs, the thermal stability can be improved. Here, Si and Sb are semimetals. The content of Si+Sb+Cs is preferably 0% to 40%, more preferably 0% to 30%, even more preferably 0% to 20%, and even more preferably 0.1% to 10%.

[0053] S is a component that expands the vitrification range and tends to increase the thermal stability of glass. Its content is preferably 0% to 30%, more preferably 0% to 20%, further preferably 0% to 10%, and particularly preferably 0% to 3%. If the S content is too high, the transmittance of infrared rays having a wavelength of 10 μm or more tends to decrease.

[0054] Se and As are components that expand the vitrification range and increase the thermal stability of glass. The content of each of these elements is preferably 0% to 10%, and more preferably 0.5% to 5%. However, since these substances are toxic, it is preferable that they are not substantially contained from the viewpoint of reducing the impact on the environment and human body, as described above.

[0055] It is preferable that the glass does not substantially contain the toxic substances Cd, Tl and Pb, where "substantially not containing" means that the content is 0.1% or less.

[0056] The ratio of metal in the raw material 6 is preferably 80% or more, 85% or more, particularly 90% or more by volume. In this way, the raw material 6 can be easily melted by induction heating. Therefore, the temperature can be increased or decreased more easily and quickly than by heating by radiation, and productivity can be improved. The upper limit is not particularly limited, but can be, for example, 100%, 99%, particularly 98% or less.

[0057] Second embodiment 5 is a schematic perspective view of a molding die used in a glass manufacturing method according to the second embodiment. This embodiment differs from the first embodiment in that the outer shape of the molding die 23 is semi-cylindrical. In this embodiment, glass is formed in the same manner as in the first embodiment.

[0058] The mold 23 has a wall 25. The wall 25 includes a curved surface portion in a semi-cylindrical shape and a pair of semi-circular surfaces. A semi-cylindrical partition member 26 is disposed in the mold 23. The partition member 26 is in contact with the wall 25 of the mold 23. A portion of the wall 25 that corresponds to one of the pair of semi-circular surfaces is the opposing portion 25a. The mold 23 may be supported by a guide rail, an appropriate support, or the like. The shape of the mold is not limited to the shapes in the first embodiment and this embodiment.

[0059] In this embodiment, as in the first embodiment, oxidation of the melt 11 can be easily suppressed, and glass productivity can be increased. Furthermore, striae in the glass can be suppressed. According to this embodiment, columnar glass having a semicircular bottom surface can be obtained. Preform glass can also be produced by grinding, polishing, and cleaning the glass. Moreover, optical members such as lenses can be produced by subjecting the preform glass to mold press molding or the like.

[0060] (Third embodiment) 6 is a schematic perspective view of a molding die used in a glass manufacturing method according to a third embodiment. This embodiment differs from the first embodiment in that the outer shape of molding die 33 is approximately cylindrical. In this embodiment, glass is formed in the same manner as in the first embodiment.

[0061] The mold 33 has a wall 35. The wall 35 includes a curved surface portion in a substantially cylindrical shape and a pair of substantially circular surfaces. A substantially cylindrical partition member 36 is disposed within the mold 33. The partition member 36 is in contact with the wall 35 of the mold 33. A portion of the wall 35 that corresponds to one of the pair of substantially circular surfaces is the opposing portion 35a. The mold 33 may be supported by a guide rail, an appropriate support, or the like. The shape of the mold is not limited to the shapes in the first embodiment and this embodiment.

[0062] In this embodiment, as in the first embodiment, oxidation of the melt 11 can be easily suppressed, and glass productivity can be increased. Furthermore, striae in the glass can also be suppressed. According to this embodiment, a substantially cylindrical glass can be obtained. Preform glass can also be produced by grinding, polishing, and cleaning the glass. In addition, optical members such as lenses can be produced by performing mold press molding or the like on the preform glass. Since optical members such as lenses often have a circular planar shape, if a substantially cylindrical glass is formed according to this embodiment, the processing required to produce a lens can be reduced, and the yield can be improved. [Explanation of symbols]

[0063] 1…Container 2…Bottom 3…Side wall 4. Piping 5...Mantle tube 6...Raw materials 7…Lid 8...Gas supply pipe 9...Gas exhaust pipe 10A…Coil 10B…Coil 11…Melted liquid 11a…heterogeneous layer 12…Seal 13…Mold 14…Bottom part 15...Wall part 15a...Opposing part 16...Partition member 17…Inflow part 18...Glass 23...Molding mold 25…Wall part 25a...Opposing part 26...Partition member 33…Mold 35…Wall part 35a…Facing part 36...Partition member

Claims

1. A step of pouring a molten liquid obtained by melting a glass raw material into a mold; cooling the melt to obtain glass; Equipped with the glass is a chalcogenide glass, A partition member is disposed in the mold, and an inlet portion is formed surrounded by the mold and the partition member, The step of pouring the melt into the mold is carried out under an air atmosphere; a step of flowing the melt into the forming mold, the forming mold being moved relative to the partition member to increase the volume of the inlet while forming a heterogeneous layer on a liquid surface of the melt flowed into the inlet, and the melt being flowed into a space between a bottom portion of the inlet and the heterogeneous layer.

2. 2. The method for producing glass according to claim 1, wherein in the step of flowing the melt into the mold, a thickness of the melt is kept constant when the mold is moved relative to the partition member.

3. The method for producing glass according to claim 1 , wherein in the step of pouring the melt into the mold, only the mold is moved.

Citation Information

Patent Citations

  • Method of molding low-melting glass and molded article of low-melting glass

    JP1994279040A

  • Apparatus and method for forming glass

    JP2013001586A

  • Method for manufacturing glass article

    JP2015209364A

  • System and method for vapor pressure controlled growth of infrared chalcogenide glasses

    US20040206119A1