Thin film X-ray diffraction method
By using a high-density base film to create a total reflection interface with the thin film, X-ray diffraction methods overcome substrate interference, enabling accurate analysis of thin films with varied densities and expanding their applicability.
Patent Information
- Application Number
- JP2021039479
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-11
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-03-11
AI Technical Summary
Existing X-ray diffraction methods for thin films with low film density are affected by substrate halos, limiting the accuracy and scope of analysis, particularly when using glass substrates.
Forming a high-density base film, such as indium tin oxide, on the substrate surface to create a total reflection interface with the thin film, allowing X-rays to be incident at an angle between the critical angles of both films to minimize substrate influence and enhance analysis accuracy.
Accurate analysis of thin films is achieved by reducing substrate interference, enabling broader application to materials with varying densities and thicknesses, including copper oxide and nitride films.
Smart Images

Figure 0007593172000002 
Figure 0007593172000003 
Figure 0007593172000001
Abstract
Description
[Technical field]
[0001] The present invention relates to an X-ray diffraction method for identifying crystalline phases in thin films. [Background technology]
[0002] Thin films are used in various devices. The characteristics of these devices often depend on the crystalline structure of the thin film. X-ray diffraction is generally used to identify the crystalline phase of the thin film. When the thin film is on the order of a few nm thick, the in-plane XRD (X-ray diffraction) method and the GI-XRD (grazing incidence X-ray diffraction, also called out-of-plane GI-XRD) method, which have a small angle of incidence, are used. These X-ray diffraction methods are measurement techniques that use a thin film sample of a few nm thick formed on a substrate such as glass as the measurement object, and selectively obtain information about the thin film by fixing the X-ray incidence angle (ω) of the X-ray diffraction device used for the measurement to 0.1° to 1°.
[0003] For example, Patent Document 1 discloses a method in which X-rays are irradiated onto a sample having a thin film formed on a substrate, the X-rays are totally reflected at the interface between the thin film and the substrate, the diffracted X-rays are measured by an X-ray detector, and the X-ray detection intensity is counted. In this case, it is described that when two materials are in contact with each other at a sufficiently smooth interface, the total reflection phenomenon of X-rays occurs when X-rays are incident at a small angle to the interface from the material with low electron density to the material with high electron density. Then, X-rays are irradiated with energy that causes total reflection at the substrate, not total reflection at the surface of the thin film. In addition, glass is used as the substrate, and a thin film of metal or organic material is formed on the substrate.
[0004] Patent Document 2 also discloses a method for calculating the density of a sample, which involves irradiating X-rays onto a film on the surface of the sample at a predetermined angle, measuring the intensity of the reflected X-rays with a first detector while moving the sample in a direction perpendicular to the surface, measuring the intensity of diffracted X-rays among the incident X-rays with a second detector, calculating the film thickness from the difference between the height position of the sample at which the differential signal of the intensity of the diffracted X-rays is maximized and the height position of the sample at which the intensity of the reflected X-rays is maximized, and calculating the density of the film on the surface of the sample based on the film thickness and the X-ray intensity at each position. In this case, the material forming the substrate has a density of 2.0 to 2.3 g / cm. 3 The materials that make up the membrane are silicon and glass, etc., with a density of about 1 g / cm 3 It is said that the materials are carbon nanotubes and organic materials. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 2591650 [Patent Document 2] Patent No. 6171940 Summary of the Invention [Problem to be solved by the invention]
[0006] However, if the density of the film formed on the measurement target is low, the X-rays will penetrate all the way to the substrate, and information about the substrate will also be detected. For example, if glass is used as the substrate for an extremely thin film material with a low film density, the X-rays will penetrate the film, and not only will the X-ray diffraction peaks from the sample be detected, but also the halo (ring-shaped diffraction image) from the glass. In this regard, both patent documents irradiate X-rays at the critical angle for total reflection. However, in the region with a small diffraction angle, the X-rays are affected by the halo of the substrate. Therefore, their application is limited to objects that can be measured at a diffraction angle 2θ that is not affected by the halo (e.g., carbon as described in Patent Document 2).
[0007] The present invention has been made in consideration of the above circumstances, and has an object to provide a thin film X-ray diffraction method that can reduce the influence of the substrate, accurately analyze the object to be measured, and expand the range of application of the object. [Means for solving the problem]
[0008] The X-ray diffraction method for a thin film of the present invention includes forming an undercoat film made of a material having a higher density than the thin film to be measured on the surface of a substrate, forming the thin film on the undercoat film, and irradiating X-rays onto the thin film at an incident angle between the total reflection critical angle of the undercoat film and the total reflection critical angle of the thin film to identify the crystalline phase of the thin film.
[0009] When forming a film on the surface of a substrate, only objects with a density smaller than that of the substrate can be used to totally reflect X-rays on the surface of the substrate. Therefore, a base film made of a material with a density greater than that of the thin film to be measured is formed on the surface of the substrate, and total reflection occurs at the interface between the base film and the thin film. By adopting this method, the influence from the substrate can be reduced, and diffracted X-rays can be accurately captured for accurate analysis. In addition, by appropriately selecting the material of the base film, the angle of incidence can be made larger than when the surface of the substrate is used as the interface, expanding the range of applicable objects to be measured.
[0010] In this thin film X-ray diffraction method, the undercoat film may be an indium tin oxide film, which is widely used as a transparent electrode and can be easily formed by deposition or the like. In addition, the density of the indium tin oxide film is greater than that of glass (for example, glass has a density of 2.5 g / cm 3 In contrast, indium tin oxide has a density of 7.18 g / cm 3 ), by using it as an underlayer on the surface of a glass substrate, it is possible to accurately analyze thin films of materials with a density greater than that of glass.
[0011] In this thin film X-ray diffraction method, the thin film may be a film made of copper oxide. The density of the film made of copper oxide is, for example, about 3 g / cm.3 If a film is formed directly on a glass substrate and X-ray diffraction is performed, it will be affected by the glass halo. However, by using an indium tin oxide film as the base film, it is possible to accurately analyze the copper oxide in the measurement target.
[0012] In this thin film X-ray diffraction method, the undercoat film is preferably amorphous, which prevents the undercoat film from affecting the crystal growth and components of the measurement object formed thereon, thereby enabling accurate analysis of the measurement object.
[0013] In this X-ray diffraction method for a thin film, the substrate is made of glass, and the measurement includes a diffraction peak in the thin film having a diffraction angle 2θ of 20° or more and 35° or less. When no undercoat film is used, a large halo from the glass substrate appears in the range of diffraction angles 2θ between 20° and 35°, and the slight peaks of the diffraction lines of the object to be measured are buried in the halo and cannot be identified. With this diffraction method, an undercoat film is formed on the surface of the glass substrate, eliminating the effect of the substrate halo and making it possible to capture the slight peak lines of the thin film.
[0014] In this thin film X-ray diffraction method, the surface roughness Ra of the undercoat film is 5 nm or less. When the surface roughness Ra of the undercoat film is 5 nm or less, scattering at the undercoat film is suppressed, making it easier to detect diffracted X-rays and allowing accurate analysis.
[0015] In this case, the thickness of the thin film can be 10 nm or less. Even thin films of copper oxide can be accurately analyzed. Effect of the Invention
[0016] According to the present invention, it is possible to reduce the influence from the substrate, accurately analyze the measurement target, and expand the range of application of the target. [Brief description of the drawings]
[0017] [Figure 1]FIG. 2 is a perspective cross-sectional view showing a measurement sample in an embodiment of the present invention. [Diagram 2] This is an X-ray diffraction pattern measured after forming a thin film made of copper oxide on an undercoat film made of indium tin oxide. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Hereinafter, an embodiment of the present invention will be described. In the embodiment, the substance to be measured is, for example, copper oxide. In the measurement sample shown in FIG. 1, a thin film 3 made of copper oxide is formed on the surface of a substrate 1 via an undercoat film 2. The substrate 1 can be suitably made of glass, which is generally used in the XRD diffraction method. The undercoat film 2 is, for example, an indium tin oxide (ITO) film, which is an inorganic mixture of indium oxide (III) (In2O3) and tin oxide (IV) (SnO2). Indium tin oxide is preferably amorphous so as not to affect the crystal growth of the measurement object formed on the undercoat film 2 (for example, to prevent epitaxial growth or chemical reactions). The thickness of the undercoat film 2 is preferably 20 nm or more. In addition, the surface is preferably a mirror surface, and the arithmetic mean roughness Ra is preferably 5 nm or less. The thin film 3 to be measured is formed on the surface of the base film 2 to a thickness of approximately 8 nm.
[0019] The crystal phase of the sample thus constructed is identified by the in-plane XRD method or the GI-XRD method. In the in-plane XRD method or the GI-XRD method, in order to perform an accurate analysis, it is important to cause total reflection of X-rays between the thin film 3 and the undercoat film 2 of the measurement object. It is known that the critical angle α for total reflection of a film can be calculated by multiplying the wavelength of the incident X-rays by the square root of the mass density of the target material. Specifically, the critical angle α for total reflection is expressed by the following formula:
[0020]
number
[0021] The indium tin oxide undercoat film 2 is effective in causing total reflection at the interface with the copper oxide thin film 3. That is, the copper oxide thin film 3 has a density of approximately 3 g / cm 3 and the density of the undercoat film 2 made of indium tin oxide is approximately 7 g / cm 3 In the case of indium tin oxide, the critical angle of total reflection α is approximately 0.4°. Therefore, if X-rays are incident at an angle smaller than this critical angle of total reflection α, they will be totally reflected on the surface of the base film 2. Note that since the refractive index of materials with respect to X-rays is approximately 1, the effects of refraction are ignored. On the other hand, in the case of the thin film 3 of copper oxide, which is the substance to be measured, the total reflection critical angle α is approximately 0.25°. Therefore, it is advisable to make the X-rays incident at an incident angle ω between the total reflection critical angle of the base film 2 and the total reflection critical angle of the thin film 3 to be measured, for example, 0.3° in this case.
[0022] In this way, by irradiating X-rays on the thin film 3 at an incident angle (ω) between the total reflection critical angle of the undercoat film 2 and the total reflection critical angle of the thin film 3 to be measured, it is possible to achieve almost total reflection at the interface between the undercoat film 2 and the thin film 3. When the total reflection phenomenon occurs, the X-rays generate evanescent waves parallel to the sample surface and hardly penetrate into the sample. In other words, by inducing the total reflection phenomenon on the surface of the undercoat film 2 formed directly below the measurement target, it is possible to reduce the generation of diffracted X-rays, amorphous halos, and characteristic X-rays by the undercoat film 2 and the substrate 1. Therefore, the crystalline phase of the thin film 3 to be measured can be accurately identified.
[0023] Furthermore, by providing a base film 2 in this manner and performing measurements at an incidence angle ω, a more accurate analysis can be performed, and the measurement object can be applied not only to copper oxide but also to a wide range of materials that satisfy the incidence angle ω, such as nitride films.
[0024] The present invention is not limited to the configuration of the above embodiment, and various changes can be made to the details of the configuration without departing from the spirit of the present invention. For example, although the substrate is made of glass, it may be made of silicon. Alternatively, a silicon wafer coated with amorphous silicon may be used as the substrate. In addition, since a base film is formed, the material of the substrate is not particularly limited as long as it can have a smooth surface.
[0025] Furthermore, the base film 2 may be any film having a large total reflection critical angle (e.g., larger than that of glass), and in addition to the indium tin oxide film described in the embodiment, a film made of zinc oxide (ZnO), tin oxide (SnO2), titanium oxide (TiO2), niobium oxide (NbO2), etc. may be used. EXAMPLES
[0026] In order to confirm the specific effects of the present invention, the results of a qualitative analysis of a thin film made of copper oxide using an in-plane XRD method are shown below. The substrate was made of glass, and the undercoat film was made of indium tin oxide. The undercoat film had a thickness of 40 nm. The arithmetic mean roughness Ra of the surface was approximately 2 nm. A thin film made of copper oxide was formed on the undercoat film to a thickness of 8 nm. As a comparative example, a thin film made of copper oxide was also formed directly on the glass substrate by sputtering.
[0027] As shown diagrammatically in FIG. 1, the measurement angle range (angle of the scanning axis) 2θ was set to 10° to 90°, and the X-ray incident angle ω was set to 0.3°. The diffraction patterns of the example and comparative example are shown in Figure 2. The horizontal axis is the diffraction angle (2θ), and the vertical axis is the diffracted X-ray intensity (counts: the number of diffracted X-rays captured by the detector per second). The diffraction pattern of the example is indicated by the symbol E, and the diffraction pattern of the comparative example is indicated by the symbol C. P1 to P6 indicate the positions of the diffraction peaks due to copper oxide.
[0028] In the case of the comparative example, a broad peak is observed in the region near 2θ=20° indicated by H due to the influence of the glass halo. This indicates that the X-ray penetration depth of the formed copper oxide thin film is about 400 nm when ω=0.3° (the material is Cu2O, and the depth at which diffracted X-ray intensity for incident X-rays is 99% or more is calculated as the X-ray penetration depth), which is much greater than the film thickness of 8 nm, and therefore the X-ray penetrates all the way to the glass layer of the substrate.
[0029] In contrast, in the case of the embodiment in which an undercoat film made of amorphous indium tin oxide, which is a material that satisfies the above-mentioned requirements, is formed between the glass substrate and the thin film made of copper oxide, it is clear that the influence of the glass halo is not observed, as shown in E of Figure 2. Furthermore, if diffraction lines are generated from the undercoat film, which is the amorphous indium tin oxide film, a broad peak should be observed near 2θ=32°, but it can be seen that this does not appear either. Also, the increase in background is suppressed.
[0030] Furthermore, in the case of the comparative example, due to the influence of the glass halo as described above, no peaks assumed to be diffraction peaks of copper oxide were visible in the region around 2θ=10° to 35°, whereas in the case of the example, a small diffraction peak derived from CuO in the region around 2θ=30° (see P1) was visible.
[0031] From these diffraction results, it can be said that the method of this embodiment is a technique that can measure copper oxide thin films of nm order with high sensitivity by reducing the influence of the substrate and the underlayer as much as possible. Also, as shown in the above formula (1), from the relationship between the critical angle of total reflection of the indium tin oxide film, α ≒ 0.4°, and the critical angle of total reflection of the copper oxide thin film, α ≒ 0.25°, it is estimated that theoretically, total reflection occurs sufficiently at the X-ray incident angle ω = 0.3° set in this experiment, and it was found that a highly visible diffraction peak can be obtained even for an extremely thin film sample of 8 nm. [Explanation of symbols]
[0032] 1 Board 2. Base film 3. Thin film to be measured
Claims
1. 1. A method for X-ray diffraction of a thin film, comprising: forming an undercoat film on a surface of a substrate, the undercoat film being a material having a higher density than a thin film made of copper oxide and being made of any one of indium tin oxide, zinc oxide, tin oxide, titanium oxide, and niobium oxide; forming the thin film on the undercoat film; and irradiating X-rays onto the thin film at an incident angle between the total reflection critical angle of the undercoat film and the total reflection critical angle of the thin film to identify a crystalline phase of the thin film.
2. 2. The method for X-ray diffraction of a thin film according to claim 1, wherein the undercoat film is amorphous.
3. 3. The method for X-ray diffraction of a thin film according to claim 1, wherein the substrate is made of glass, and the measurement includes diffraction peaks in the thin film having a diffraction angle 2θ of 20° or more and 35° or less.
4. 4. The thin film X-ray diffraction method according to claim 1, wherein the undercoat film has a surface roughness Ra of 5 nm or less.
Citation Information
Patent Citations
Tool exchange device
JP1986071940A
X-ray crystal analysis method
JP2014052223A
Humidity sensor
JP2014178137A
X-ray analysis method and x-ray analysis device
JP2015129666A
Thin film transistor
JP2016111324A