Semiconductor device manufacturing method and manufacturing jig set

The protective jig in the manufacturing method and jig set addresses solder scattering issues, ensuring reliable bonding and enhancing semiconductor device reliability by preventing solder piece scattering during the soldering process.

JP7593174B2Active Publication Date: 2024-12-03FUJI ELECTRIC CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021039909
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-12
Publication Date
2024-12-03
Estimated Expiration
2041-03-12

AI Technical Summary

Technical Problem

The scattering of solder pieces and generation of voids during the soldering process in semiconductor devices leads to poor electrical insulation and mechanical bonding, resulting in lower reliability due to short circuits and improper attachment of wiring members.

Method used

A manufacturing method and jig set that includes a protective jig with a protective surface and beam part to prevent solder pieces from scattering by aligning and supporting the components during the soldering process, ensuring electrical and mechanical bonding.

Benefits of technology

Prevents solder piece scattering, ensuring reliable electrical and mechanical bonding of wiring members, thereby improving the reliability of semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007593174000001
    Figure 0007593174000001
  • Figure 0007593174000002
    Figure 0007593174000002
  • Figure 0007593174000003
    Figure 0007593174000003
Patent Text Reader

Abstract

To prevent solder pieces from scattering, and surely joint wiring members or the like electrically and mechanically to be able to improve reliability.SOLUTION: A semiconductor chip 25 is arranged at an opening part 3a of a positioning jig 3 so that a front surface of the chip points to a front side, to position the semiconductor chip 25. Subsequently, a lead frame 26 is mounted on a main electrode of the semiconductor chip 25 arranged in the positioning jig 3, through a joining member 27. Then a protection part 4b of a protection jig 4 is arranged on the front surface so that a protection surface points to the main electrode, and the protection jig 4 is installed so that a beam portion 4a is supported by a support portion 3e. This allows the protection part 4b of the protection jig 4 to suppress pieces of the joining member 27 from scattering to a protection region, a control electrode 252 in particular. Further, the protection jig 4 can suppress the pieces of the joining member 27 from scattering to the control electrode while being lifted up, following warpage of the semiconductor chip 25.SELECTED DRAWING: Figure 8
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a semiconductor device and a manufacturing jig set. [Background technology]

[0002] The semiconductor device includes a power device and is used as a power conversion device. The power device includes a semiconductor chip. The semiconductor chip is, for example, an IGBT (Insulated Gate Bipolar Transistor) or a power MOSFET (Metal Oxide Semiconductor Field Effect Transistor). Such a semiconductor device may include at least a semiconductor module having a semiconductor chip and a ceramic circuit substrate on which the semiconductor chip is disposed, and a heat sink (such as a heat sink or a cooling unit) on which the ceramic circuit substrate is disposed.

[0003] In manufacturing such a semiconductor device, a semiconductor chip is bonded to a ceramic circuit board, and an alignment jig is used when the ceramic circuit board with the semiconductor chip bonded thereto is bonded to a heat sink (for example, Patent Documents 1 and 2).

[0004] In a semiconductor device, a semiconductor chip is placed on a solder material on a ceramic circuit board, which has solder material placed in a predetermined area, using an alignment jig. The solder material is then heated to melt and bond the semiconductor chip to the ceramic circuit board. Thereafter, the ceramic circuit board to which the semiconductor chip is bonded is similarly bonded to a heat sink by soldering. In some cases, wiring members such as a lead frame are also bonded to the semiconductor chip by soldering. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2019-36653 A [Patent Document 2] JP 2013-65662 A Summary of the Invention [Problem to be solved by the invention]

[0006] In the above soldering process of a semiconductor device, when the solder material is a cream solder containing flux, the flux may foam when the solder is heated and melted. When the flux foams, solder pieces fly off from the molten solder. When a plate solder not containing flux is used, voids are generated and solder pieces and solder fine particles fly off. When a fine metal particle bonding material such as a nano-silver particle sintered body is used, voids are generated and nano-metal particle lumps fly off. When these bonding material pieces and particles (solder pieces, etc.) fly off onto the circuit pattern of a ceramic circuit board, the surface of a semiconductor chip, and especially onto electrodes (protective areas), it becomes impossible to properly bond wiring members such as bonding wires to the circuit pattern and electrodes of the semiconductor chip. In addition, short circuits are likely to occur, the electrical insulation performance is reduced, and the reliability of the semiconductor device is also reduced. If the scattered solder pieces are to be removed, the number of complicated steps increases accordingly.

[0007] The present invention has been made in consideration of these points, and aims to provide a semiconductor device manufacturing method and manufacturing jig set that prevents solder chips from scattering, ensures reliable electrical and mechanical bonding of wiring members, etc., and improves reliability. [Means for solving the problem]

[0008] According to one aspect of the present invention, there is provided a method for manufacturing a semiconductor device, the method including: a preparation step of preparing a first component including a bonding region on a front surface thereof; a second component to be bonded to the bonding region; an alignment jig including an opening that is opened corresponding to a shape of the first component in a plan view and has a support portion formed at an opening edge; and a protective jig including a protective portion having a protective surface and a beam portion formed on the protective portion; an alignment step of arranging the first component with the front surface exposed in the opening of the alignment jig to align the first component; a mounting step of mounting a second component via a bonding member on the bonding region of the first component placed on the alignment jig; an installation step of placing the protective portion of the protective jig on the front surface with the protective surface facing the bonding region either before or after the installation step, and installing the protective jig so that the beam portion is supported by the support portion; and a heating step of heating the bonding member.

[0009] According to another aspect of the present invention, there is provided a manufacturing jig set for use in the above-described method for manufacturing a semiconductor device. Effect of the Invention

[0010] The above-mentioned semiconductor device manufacturing method and manufacturing jig set prevent solder pieces from scattering, ensure reliable electrical and mechanical bonding of wiring components, and make it possible to manufacture semiconductor devices in which a decrease in reliability is prevented. [Brief description of the drawings]

[0011] [Figure 1] FIG. 2 is a side view of the semiconductor device. [Diagram 2] 4 is a flowchart showing a method for manufacturing the semiconductor device according to the first embodiment. [Diagram 3] 1 is a side view of an assembly used in the method for manufacturing a semiconductor device according to a first embodiment. [Figure 4] 5 is a flowchart showing a bonding step included in the manufacturing method of the semiconductor device according to the first embodiment. [Diagram 5]3A to 3C are diagrams illustrating an alignment step included in the manufacturing method of the semiconductor device according to the first embodiment. [Figure 6] 1 is a diagram (part 1) showing a mounting step included in the manufacturing method of the semiconductor device according to the first embodiment; [Figure 7] 6 is a diagram (part 2) showing a mounting step included in the manufacturing method of the semiconductor device according to the first embodiment; FIG. [Figure 8] 5A to 5C are diagrams illustrating a heating step included in the manufacturing method of the semiconductor device according to the first embodiment. [Figure 9] 13 is a diagram showing a protective jig used in a semiconductor device manufacturing method according to a first modified example of the first embodiment. FIG. [Figure 10] 13 is a diagram showing a protective jig used in a semiconductor device manufacturing method according to Modification 2 of the first embodiment. FIG. [Figure 11] 13 is a diagram showing a protective jig used in a semiconductor device manufacturing method according to a third modified example of the first embodiment. FIG. [Figure 12] 13 is a diagram showing a protective jig used in a semiconductor device manufacturing method according to a fourth modified example of the first embodiment. FIG. [Figure 13] FIG. 11 is a side view of a semiconductor device according to a second embodiment. [Figure 14] 13 is a flowchart showing a bonding step included in the manufacturing method of the semiconductor device according to the second embodiment. [Figure 15] FIG. 13 is a side view of a semiconductor device according to a modified example of the second embodiment. [Figure 16] FIG. 13 is a plan view of a semiconductor device according to a third embodiment. [Figure 17] 13 is a plan view (part 1) showing a mounting step included in the manufacturing method of the semiconductor device according to the third embodiment. FIG. [Figure 18] 13 is a cross-sectional view (part 1) showing a mounting step included in the manufacturing method of the semiconductor device according to the third embodiment. FIG. [Figure 19] 13 is a plan view (part 2) showing a mounting step included in the manufacturing method of the semiconductor device according to the third embodiment. FIG. [Figure 20] 13 is a cross-sectional view (part 2) showing a mounting step included in the manufacturing method of the semiconductor device according to the third embodiment. FIG. [Figure 21] 13A and 13B are diagrams illustrating a protective jig used in a semiconductor device manufacturing method according to a modified example of the third embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, the embodiment will be described with reference to the drawings. In the present embodiment, the front surface (upper side) refers to the surface (direction) of the semiconductor device 20 in FIG. 1 facing upward. FIG. 1 shows a side view of the semiconductor device 20. For example, FIGS. 4 to 6 show the process of mounting a jig from the front surface. The back surface (lower side) refers to the surface (direction) facing downward in the semiconductor device 20 in FIG. 1. For example, the surface on which the ceramic circuit board 21 of the semiconductor device 20 is disposed is the back surface (lower side). In other than FIG. 1, the front surface (upper side) and the back surface (lower side) have the same orientation. In the following description, the term "main component" refers to a case where the component contains 80 vol% or more.

[0013] [First embodiment] First, a semiconductor device manufactured through a first bonding step (step S11 in FIG. 2) described in the first embodiment and a second bonding step (step S12 in FIG. 2) described in the second embodiment will be described with reference to FIG. 1. FIG. 1 is a side view of the semiconductor device. The semiconductor device 20 includes at least a ceramic circuit substrate 21, a semiconductor chip 25, a lead frame 26, and a heat sink 28. The semiconductor device 20 may be housed in a case, with appropriate electrical wiring between the semiconductor chip, the ceramic circuit substrate, etc., or may be sealed with a sealing member. Here, the minimum configuration of the semiconductor device 20 is shown.

[0014] The ceramic circuit board 21 includes an insulating plate 22, a circuit pattern 23 provided on the front surface of the insulating plate 22, and a metal plate 24 provided on the back surface of the insulating plate 22. The insulating plate 22 and the metal plate 24 may have chamfered corners. The outer shape of the circuit pattern 23 and the metal plate 24 is smaller than the outer shape of the insulating plate 22 in a plan view, and is formed inside the insulating plate 22. The number, arrangement position, and shape of the circuit patterns 23 are only an example, and the number, arrangement position, and shape can be selected by appropriate design without being limited to this case. The insulating plate 22 is made of a material that has insulation, low thermal resistance, and excellent thermal conductivity. Such an insulating plate 22 is preferably made of ceramics. The ceramics are aluminum oxide, aluminum nitride, silicon nitride, etc. The thickness of such an insulating plate 22 is 0.20 mm or more and 2.50 mm or less.

[0015] The circuit pattern 23 is made of a material having excellent electrical conductivity. Examples of such materials include copper, aluminum, and an alloy containing at least one of these. The thickness of the circuit pattern 23 is preferably 0.10 mm or more and 2.00 mm or less, and more preferably 0.20 mm or more and 1.00 mm or less. It is also possible to perform plating processing on the circuit pattern 23 using a material having excellent corrosion resistance. Examples of such materials include nickel and an alloy containing nickel. The circuit pattern 23 is formed in the center of the insulating plate 22, and a gap is provided between the edge of the circuit pattern 23 and the edge of the insulating plate 22 in a plan view.

[0016] The metal plate 24 is made of a metal having excellent thermal conductivity. Examples of such materials include copper, aluminum, and an alloy containing at least one of these. The thickness of the metal plate 24 is preferably 0.10 mm or more and 2.00 mm or less, and more preferably 0.20 mm or more and 1.00 mm or less. In order to improve corrosion resistance, a material such as nickel may be formed on the surface of the metal plate 24 by plating or the like.

[0017] The semiconductor chip 25 is a power device made of a semiconductor material such as silicon, silicon carbide, or gallium nitride. The semiconductor chip 25 is a switching element or a diode element. The switching element is a power MOSFET, an IGBT, or the like. Such a semiconductor chip 25 has, for example, a drain electrode (positive electrode, a collector electrode in an IGBT) as a main electrode on the back surface, a gate electrode as a control electrode, and a source electrode (negative electrode, an emitter electrode in an IGBT) as a main electrode (joined region) on the front surface. The diode element is an SBD (Schottky Barrier Diode) or a FWD (Free Wheeling Diode) of a PiN (P-intrinsic-N) diode. Such a semiconductor chip 25 has a cathode electrode as a main electrode on the back surface, and an anode electrode as a main electrode on the front surface. The thickness of the semiconductor chip 25 is 80 μm or more and 500 μm or less, for example, 200 μm. In the first embodiment, the semiconductor chip 25 on the ceramic circuit substrate 21 is an example of a switching element. A main electrode 251 and a control electrode 252 are provided on the front surface of the semiconductor chip 25 (see FIG. 6). The region (first region) of the main electrode 251 is provided in the approximate center of the front surface of the semiconductor chip 25. The region (second region) of the control electrode 252 is provided away from the main electrode 251 on the front surface of the semiconductor chip 25 toward the outer edge. Also, the semiconductor chips 25 of the switching element and the diode element may each be used according to a desired design.

[0018] Alternatively, the semiconductor chip 25 is an RC (Reverse Conducting)-IGBT. The RC-IGBT is a single chip that includes an IGBT, which is a switching element, and an FWD, which is a diode element. Such a semiconductor chip 25 includes, for example, a collector electrode (positive electrode) and an anode electrode as main electrodes on the back surface, and a gate electrode as a control electrode, and an emitter electrode (negative electrode) and a cathode electrode as main electrodes on the front surface.

[0019] The semiconductor chip 25 has its back surface joined to the predetermined circuit pattern 23 by a joining member 27. The joining member 27 is, for example, a solder material. The solder material is made of lead-free solder mainly composed of a predetermined alloy. The solder material may be, for example, Sn-Bi (tin-bismuth)-based, Sn-Ag-Cu (tin-silver-copper)-based, Sn-Sb (tin-antimony)-based, Sn-Sb-Ag (tin-antimony-silver)-based, Sn-Cu (tin-copper)-based, Sn-Sb-Ag-Cu (tin-antimony-silver-copper)-based, Sn-Cu-Ni (tin-copper-nickel)-based, or Sn-Ag (tin-silver)-based. Such a solder material may further contain an additive element. The additive element may be, for example, nickel, germanium, or phosphorus. However, when the solder material is Sn-Sb, Sn-Cu, or Sn-Ag, or when these solder materials contain at least one element of silver, copper, or nickel, the liquidus temperature (melting point) is easily scattered at 210°C or higher. When using such solder materials, the manufacturing jig set 9 described later is particularly effective. In addition, when joining the semiconductor chip 25 and the circuit pattern 23, a plate-shaped solder material (plate solder) or a paste-like cream solder may be used. The plate solder is made of the above-mentioned alloy. The cream solder contains a flux having a reducing agent in the above-mentioned alloy or alloy powder. In addition, a joining material (fine metal particle sintered body) containing fine metal particles such as a sintered body of nano-silver particles may be used as the joining member 27. The fine metal particle sintered body includes a nanoparticle sintered body and a microparticle sintered body, and the nanoparticle sintered body refers to a porous metal body in which a group of metal particles having an average particle diameter of about 1 nm or more and 200 nm or less is sintered and the particles are bonded and connected to each other. Microparticle sintered bodies are porous metal bodies in which metal particles with an average particle size of about 1 nm or more and 10 μm or less are sintered and bonded together. There are also mixed particle sintered bodies in which nanoparticles and microparticles are mixed. The bonding material before sintering (micrometal sintered body bonding material) includes bonding materials in which the metal particle surface is covered with an organic substance to prevent aggregation and improve dispersibility in the solvent, and bonding materials in which silver oxide and a reducing solvent with a reducing action are made into a paste as metal particles.

[0020] The thickness of the solder material (before heat bonding) can be 0.05 mm or more and 0.30 mm or less. In particular, it is preferable that the thickness be 0.10 mm or more and 0.20 mm or less. If the thickness is within this range, the bonding strength is sufficient, there is little scattering, and thermal resistance is suppressed.

[0021] The lead frame 26 is, for example, a wiring member that electrically connects the semiconductor chip 25 (particularly the electrodes on the front surface) to the circuit pattern 23 and external terminals. The lead frame 26 is made of a material with excellent conductivity. Examples of such materials include copper, aluminum, and an alloy containing at least one of these. The thickness of the lead frame 26 is preferably 0.20 mm or more and 4.00 mm or less, and more preferably 0.50 mm or more and 1.50 mm or less. In order to improve corrosion resistance, a material such as nickel may be formed on the surface of the lead frame 26 by plating or the like. The shape of the lead frame 26 in the first embodiment is an example. A specific example of the lead frame 26 will be described in the third embodiment. The back side of the lead frame 26 is also bonded to a predetermined semiconductor chip 25 by a bonding member 27.

[0022] The heat sink 28 is joined to the ceramic circuit board 21 by a joining member 27 or the like, and has a function of discharging heat generated by the semiconductor chip 25 to a cooling unit or the like. The heat sink 28 is flat and has a rectangular shape in a plan view. The heat sink 28 may have a convex portion or a concave portion that protrudes upward from the front surface, laterally from the side surface, or downward from the back surface. The heat sink 28 is made of a metal having excellent thermal conductivity. Examples of such materials include aluminum, iron, silver, copper, or an alloy containing at least one of these. Examples of such alloys include metal composites such as aluminum-silicon carbide or magnesium-silicon carbide. In order to improve corrosion resistance, a material such as nickel may be formed on the surface of the heat sink 28 by plating or the like. A cooling unit may be provided on the back surface of the heat sink 28 of the semiconductor device 20. The cooling unit is, for example, a water-cooled jacket. The cooling unit is not limited to a water-cooled jacket, and may be a heat sink having one or more fins. The heat sink is made of, for example, a metal with excellent thermal conductivity. The metal is aluminum, iron, silver, copper, or an alloy containing at least one of these. The heat sink 28 itself may be the cooling unit. In this case, protrusions such as an inlet and an outlet may be provided on the lower and sides.

[0023] In addition, when the lead frame 26 is bonded to the semiconductor chip 25 by the bonding member 27, if the bonded part is the first part and the bonding part is the second part, the semiconductor chip 25 corresponds to the first part and the lead frame 26 corresponds to the second part. The front surface of the semiconductor chip 25 includes a bonded area and a protective area. The bonded area is an area where the lead frame 26 (second part) is bonded to the main electrode 251 on the front surface of the semiconductor chip 25 (first part). The protective area corresponds to an area of ​​the front surface of the semiconductor chip 25 excluding the bonded area. In particular, when the first part is a semiconductor chip, the protective area may be an area around the bonded area on the front surface of the semiconductor chip 25 (first part). That is, the protective area is an outer edge part that is at least a predetermined distance away from the bonded area. The predetermined distance is, for example, 0.30 mm or more and 0.50 mm or less. The outer edge part includes the control electrode 252.

[0024] Similarly, when semiconductor chip 25 is bonded to circuit pattern 23 with bonding material 27, circuit pattern 23 corresponds to the first component, and semiconductor chip 25 corresponds to the second component. The front surface of circuit pattern 23 includes a bonded area and a protected area. The bonded area corresponds to the arrangement area of ​​semiconductor chip 25 on the front surface of circuit pattern 23, and the protected area corresponds to the area of ​​the front surface of circuit pattern 23 excluding the arrangement area.

[0025] Similarly, when ceramic circuit board 21 is joined to heat sink 28 with joining member 27, heat sink 28 corresponds to the first component, and ceramic circuit board 21 corresponds to the second component. The front surface of heat sink 28 includes a joined area and a protected area. The joined area corresponds to the arrangement area of ​​ceramic circuit board 21 on the front surface of heat sink 28, and the protected area corresponds to the area on the front surface of heat sink 28 excluding the arrangement area.

[0026] Next, a method for manufacturing such a semiconductor device 20 will be described with reference to Fig. 2. Fig. 2 is a flow chart showing the method for manufacturing the semiconductor device according to the first embodiment. First, a preparation step is performed to prepare components required for the semiconductor device 20 (step S10 in Fig. 2). As examples of the required components, a semiconductor chip 25, a ceramic circuit board 21, a case, a sealing member, a lead frame 26, a heat sink 28, etc. are prepared.

[0027] Next, a first bonding step is performed in which a semiconductor chip 25 is bonded to the prepared ceramic circuit board 21, and a lead frame 26 is bonded to the semiconductor chip 25 (step S11 in FIG. 2). In the first embodiment, the first bonding step will be described in detail later.

[0028] Next, a second bonding step is performed to bond the thus bonded ceramic circuit board 21 to a heat sink (step S12 in FIG. 2). This second bonding step will be described in the second embodiment.

[0029] Next, the ceramic circuit board 21 etc. thus bonded is housed in a case and a housing process of bonding is performed (step S13 in FIG. 2). Next, a wiring process is performed in which the ceramic circuit board 21 etc. housed in the case is electrically connected and wired by bonding wires (step S14 in FIG. 2). Note that the housing process may be performed after the wiring process. Finally, a sealing process is performed in which the ceramic circuit board 21 etc. housed in the case is sealed with a sealing member (step S15 in FIG. 2). As a result of the above, the semiconductor device 20 shown in FIG. 1 is further housed in a case to complete it.

[0030] Next, the first bonding step in step S11 of the flow chart in FIG. 2 will be described. In the first bonding step described in the first embodiment, the ceramic circuit board 21, the semiconductor chip 25, and the lead frame 26 are bonded to each other by the bonding member 27. First, the manufacturing jig set 9 used when bonding the ceramic circuit board 21, the semiconductor chip 25, and the lead frame 26 in the first bonding step will be described with reference to FIG. 3. FIG. 3 is a side view of an assembly used in the manufacturing method of the semiconductor device of the first embodiment. In FIG. 3, the ceramic circuit board 21, the semiconductor chip 25, and the lead frame 26 to which the manufacturing jig set 9 is attached are collectively referred to as the assembly 1.

[0031] The manufacturing jig set 9 included in the assembly 1 includes alignment jigs 2 and 3, a protective jig 4, and a weight 5. The manufacturing jig set 9 may include jigs other than these jigs. The alignment jigs 2 and 3 and the protective jig 4 of the manufacturing jig set 9 are each made of a material that has excellent heat resistance and a small linear expansion coefficient. Examples of such materials include carbon and composite ceramic materials. The weight 5 is made of stainless steel, for example.

[0032] The alignment jig 2 is a jig for arranging the ceramic circuit board 21 at a predetermined position. The alignment jig 2 includes a bottom 2c and a frame 2b. The bottom 2c is flat and is configured to be larger than the area of ​​the ceramic circuit board 21 in a plan view, and the ceramic circuit board 21 is arranged on the bottom 2c. The frame 2b is integrally formed on the front surface of the bottom 2c. The frame 2b surrounds an alignment area 2a formed in a concave shape corresponding to the shape (rectangular) of the ceramic circuit board 21 in a plan view. It is preferable that the height of the alignment area 2a is approximately equal to the height of the ceramic circuit board 21. In other words, the upper surface of the frame 2b of the alignment jig 2 and the upper surface of the ceramic circuit board 21 (the upper surface of the circuit pattern 23) form the same plane. This is because the alignment jig 3 is arranged on the frame 2b and the ceramic circuit board 21.

[0033] The alignment jig 3 has a flat plate shape and includes a frame 3b surrounding an opening 3a that is opened on the front surface in a plan view corresponding to the shape of the semiconductor chip 25. The alignment jig 3 may also include a recess 3c formed in an annular shape along the opening 3a on the front surface of the frame 3b on the side of the opening 3a, and a protrusion 3d formed in an annular shape on the back surface of the frame 3b. The recess 3c is used to determine the position of the weight 5 to be mounted on the alignment jig 3, which will be described later. The height of the protrusion 3d in this case preferably corresponds to the height of the circuit pattern 23 of the ceramic circuit board 21. The width of the protrusion 3d (X direction in FIG. 3) preferably corresponds to the gap (length) between the outer edge of the circuit pattern 23 and the outer edge of the insulating plate 22 in a plan view of the ceramic circuit board 21. By setting the protrusion 3d to the above height and width, the alignment jig 3 can be easily positioned at a predetermined position on the front surface of the alignment jig 2 and the ceramic circuit board 21. Further, the alignment jig 3 includes a support portion 3e formed on the inner wall surface of the opening 3a. As shown in Fig. 6, the support portion 3e has a rectangular shape in a plan view, protrudes perpendicularly from the inner wall surface of the opening 3a of the alignment jig 3 to the opening 3a, and faces the control electrode 252 of the semiconductor chip 25. As will be described later, a beam portion 4a of the protection jig 4 is disposed on the front surface of the support portion 3e.

[0034] A protective jig 4 used when bonding a lead frame 26 (second component) to a semiconductor chip 25 (first component) via a bonding member 27 will be described. The protective jig 4 includes a protective portion 4b having a protective surface 4c and a beam portion 4a formed on the protective portion 4b, and is installed on the support portion 3e and the front surface of the semiconductor chip 25. The beam portion 4a and the protective portion 4b are each formed in a flat plate shape, and as shown in FIG. 3, are integrally connected to each other in an L-shape in side view. That is, the beam portion 4a is formed perpendicular to the protective portion 4b from the end of the protective portion 4b, and forms an L-shape in side view. The corner where the beam portion 4a and the protective portion 4b are connected is not limited to a right angle as shown in FIG. 3, but may be rounded. Such a beam portion 4a is supported by the support portion 3e. Moreover, the protective portion 4b is disposed on the front surface of the semiconductor chip 25 (first component) with the protective surface 4c (see Figures 3 and 7, etc.) facing the lead frame 26 side (the joining area side). The protective surface 4c is not necessarily flat. As will be described later, the protective surface 4c may be curved as long as it can prevent the joining material pieces (solder pieces) from scattering. The width of the protective jig 4 (Y direction in Figures 3 and 7) corresponds to the width of the support portion 3e of the alignment jig 3.

[0035] It is important that the protective surface 4c of the protective jig 4 protects against scattered joining material pieces (solder pieces) and prevents the solder pieces from adhering to the front surface (protected area) of the semiconductor chip 25. The protected area of ​​the semiconductor chip 25 is the area of ​​the front surface including the control electrode 252 but excluding the main electrode 241 on the front surface. For this reason, the protective part 4b of the protective jig 4 is disposed in the protected area. More specifically, it is preferable that the tip of the protective part 4b of the protective jig 4 is disposed so as to contact the edge of the protective area. In addition, the protective part 4b of the protective jig 4 may be disposed at a predetermined distance in the protective area in the direction from the main electrode 252 toward the outer edge of the semiconductor chip 25. The predetermined distance is the direction from the main electrode 252 toward the outer edge of the semiconductor chip 25, up to just before the control electrode 252. Although the predetermined distance depends on the size of the semiconductor chip 25, it is, for example, in the range of 0.20 mm or more and 0.50 mm or less. Moreover, the protective portion 4b is not limited to being disposed at the control electrode 252, but may be disposed up to the outer edge of the protective region (including the control electrode 252).

[0036] The protection area of ​​the circuit pattern 23 is the area on the front surface excluding the arrangement area of ​​the semiconductor chip 25. The protection area of ​​the heat sink 28 is the area on the front surface excluding the arrangement area of ​​the ceramic circuit board 21. With respect to the circuit pattern 23 and the heat sink 28, the protective part 4b of the protective jig 4 is preferably arranged in the vicinity of the arrangement area in the protection area.

[0037] In addition, in a state where the protective jig 4 is mounted on the alignment jig 3 and the semiconductor chip 25, it is preferable that at least the protective portion 4b has a structure that allows it to move upward and then downward again, as described below.

[0038] Specifically, the back surface of the beam portion 4a of the protective jig 4 is supported vertically upward (in the +Z direction) by the support portion 3e, and the protective portion 4b is disposed in a protective area on the front surface of the semiconductor chip 25. Since the back surface of the beam portion 4a is only supported by the support portion 3e, the protective jig 4 itself can move vertically upward (in the opening direction of the opening portion 3e) relative to the alignment jig 3 (see FIG. 8).

[0039] Alternatively, the end of the beam 4a on the alignment jig 3 side is held by the support 3e of the alignment jig 3, and the beam 4a and the protective part 4b rotate counterclockwise around the end as an axis. As a result, the protective part 4b can move up and down (see FIG. 12).

[0040] In addition, the protective surface 4c may be roughened so that scattered solder pieces and the like can adhere to it and maintain the adhesion state. The protective surface 4c may be roughened by, for example, blasting or etching to a center line surface roughness (Ra) of about 0.1 μm to 1 μm.

[0041] The weight 5 has a flat plate shape, and has an opening 5a formed on the front surface thereof in a plan view corresponding to the shape of the lead frame 26, and a frame portion 5b surrounding the opening 5a. The weight 5 is preferably formed with the opening 5a to such an extent that the protective jig 4 is covered when the weight 5 is mounted on the alignment jig 3. The weight 5 does not necessarily require the opening 5a. That is, the weight 5 may be configured to cover the opening 3a of the alignment jig 3. The weight 5 may also have a protrusion 5d formed on the back surface of the frame portion 5b. The protrusion 5d is formed on the frame portion 5b along the edge of the opening 5a. The protrusion 5d is formed so that the weight 5 fits into the recess 3c of the alignment jig 3 when the weight 5 is placed on the alignment jig 3.

[0042] Next, the details of step S11 (first bonding step) in the flowchart of FIG. 2 will be described with reference to FIG. 3 as well as FIG. 4 to FIG. 8. FIG. 4 is a flowchart showing the bonding step included in the manufacturing method of the semiconductor device of the first embodiment. FIG. 5 is a diagram showing the alignment step included in the manufacturing method of the semiconductor device of the first embodiment. FIGS. 6 and 7 are diagrams showing the mounting step included in the manufacturing method of the semiconductor device of the first embodiment. FIG. 8 is a diagram showing the heating step included in the manufacturing method of the semiconductor device of the first embodiment. Note that FIG. 5 corresponds to step S11a, FIG. 6 corresponds to step S11b, and FIG. 7 corresponds to steps S11c and S11d, and are shown in plan view. FIG. 8 corresponds to step S11f, and is shown in side view.

[0043] In particular, the prevention of scattering of solder pieces (joining material pieces) when joining semiconductor chip 25 and lead frame 26 will be described. In the first joining step, semiconductor chip 25 is placed on ceramic circuit board 21 via joining material 27, and lead frame 26 is further placed on semiconductor chip 25 via joining material 27. After that, a heat treatment is performed to join ceramic circuit board 21, semiconductor chip 25, and lead frame 26 at once.

[0044] However, the ceramic circuit board 21 and the semiconductor chip 25 may be bonded separately, for example, by bonding the semiconductor chip 25 and the lead frame 26 thereafter. In this case, the protective jig 4 is used to prevent the bonding member 27 from scattering. For example, when the semiconductor chip 25 is bonded to the ceramic circuit board 21 via the bonding member 27, the protective jig 4 can be placed on the support portion 8e1 to prevent the bonding member 27 from scattering, as shown in FIG. 15 described later. The same applies to the case where the lead frame 26 is not used. Now, a specific description will be given below. The following description will be given by taking the case where the bonding member 27 is a solder material as an example.

[0045] First, as shown in Fig. 5, an alignment step is performed in which the ceramic circuit board 21 is placed and aligned in the alignment area 2a of the alignment jig 2 (step S11a in Fig. 4). This prevents the ceramic circuit board 21 from being misaligned in the X and Y directions (horizontal directions). This allows each component to be mounted in an appropriate position in the subsequent mounting step.

[0046] Next, the alignment jig 3 is mounted on the alignment jig 2, and a first mounting step is performed in which the semiconductor chip 25 is mounted on the front surface of the ceramic circuit board 21 through the bonding member 27 with its front surface (main electrodes 251 and control electrodes 252) exposed based on the opening 3a of the alignment jig 3 (step S11b in FIG. 4). In this case, the ceramic circuit board 21 corresponds to the first component, and the semiconductor chip 25 corresponds to the second component.

[0047] In the first mounting step, the convex portion 3d formed on the back surface of the frame portion 3b of the alignment jig 3 is fitted into the gap between the outer edge of the circuit pattern 23 of the ceramic circuit board 21 and the opening edge of the alignment region 2a of the frame portion 2b of the alignment jig 2. As a result, the ceramic circuit board 21 is reliably fixed to the alignment jig 2. The opening portion 3a of the alignment jig 3 mounted in this manner corresponds to the arrangement region of the semiconductor chip 25 on the front surface of the ceramic circuit board 21. With such an opening portion 3a, as shown in FIG. 6 (and FIG. 3), the semiconductor chip 25 is mounted on the circuit pattern 23 of the ceramic circuit board 21 via the bonding member 27. Due to the opening portion 3a of the alignment jig 3, the movement (displacement) of the semiconductor chip 25 in the horizontal direction (X direction and Y direction) is restricted with respect to the stacking direction (+Z direction) in which the semiconductor chip 25 is stacked on the ceramic circuit board 21. As shown in FIG. 3 and FIG. 8, the opening portion 3a is opened wider than the semiconductor chip 25. At this time, the clearance between the end of the opening 3a and the end of the semiconductor chip 25 is preferably 0.30 mm or more and 1.00 mm or less. The back surface of the alignment jig 3, which faces the upper surface of the circuit pattern 23, is arranged so as to cover the circuit pattern 23. The alignment jig 3 covers the protective area of ​​the circuit pattern 23, so that the scattering of the bonding material 27 that bonds the circuit pattern 23 and the semiconductor chip 25 can be suppressed. In addition, at this time, the support portion 3e of the alignment jig 3 may be arranged to face the control electrode 252 of the semiconductor chip 25 in a plan view. In particular, in order to prevent solder pieces from adhering to the control electrode 252, it is preferable to arrange the support portion 3e of the alignment jig 3 near the control electrode 252 and mount the protection jig 4.

[0048] Next, a second mounting process is performed in which the lead frame 26 (second component) is mounted on the main electrodes 251 of the semiconductor chip 25 (first component) via the bonding members 27 (step S11c in FIG. 4). In the second mounting process, the lead frame 26 is also mounted on the main electrodes 251 of the semiconductor chip 25 via the bonding members 27 through the openings 3a, as shown in FIG. 7 (and FIG. 3).

[0049] Next, a step of installing the protective jig 4 over the alignment jig 3 and the semiconductor chip 25 is performed (step S11d in FIG. 4). In the step of installing, as shown in FIG. 7 (and FIG. 3), the protective surface 4c of the protective portion 4b of the protective jig 4 faces the main electrode 251 of the semiconductor chip 25 and is mounted between the main electrode 251 and the control electrode 252. Furthermore, the beam portion 4a of the protective jig 4 is supported by the support portion 3e. Specifically, the back surface of the beam portion 4a is placed on the front surface of the support portion 3e. In this manner, the protective jig 4 is installed between the support portion 3e and the front surface of the semiconductor chip 25. That is, the protective jig 4, which is L-shaped in side view, has the beam portion 4a leaned against the support portion 3e and the protective portion 4b placed in the protective area on the semiconductor chip 25. As a result, the control electrode 252 included in the protective area of ​​the semiconductor chip 25 is covered by the protective jig 4. It is preferable that the protective jig 4 covers not only the control electrodes 252 but also the outer edge of the front surface of the semiconductor chip 25 including the control electrodes 252 .

[0050] The order of the second mounting step and the erection step may be reversed. That is, the first mounting step may be followed by the erection step, and then the second mounting step.

[0051] Next, a third mounting step is performed in which the weight 5 is mounted on the alignment jig 3 (step S11e in FIG. 4). At this time, the convex portion 5d on the back surface of the weight 5 is fitted into the concave portion 3c of the alignment jig 3. This completes the assembly 1 shown in FIG. 3. At this time, the protective jig 4 is covered by the back surface of the weight 5.

[0052] Next, a heating step is performed (step S11f in FIG. 4). The assembly 1 shown in FIG. 3 is heated to melt the bonding members 27. The bonding temperature at this time is a heating peak temperature that is 20° C. or more and 50° C. or less higher than the liquidus temperature (melting point) of the solder material. An example of the bonding temperature is, for example, about 250° C. or more and 350° C. or less. The heat treatment time at this time is maintained for about 0.5 minutes or more and 30 minutes or less, preferably about 1 minute or more and 5 minutes or less.

[0053] The bonding atmosphere is a nitrogen atmosphere or an active atmosphere such as hydrogen or formic acid. In particular, when using plate solder, it is preferable to use a gas such as hydrogen or formic acid that has a reducing effect. When bonding is performed in an active gas atmosphere having such a reducing effect, it is preferable to set the temperature at which the gas effectively reduces oxides, for example, 250°C or higher and 280°C or lower. In actual bonding, a temperature distribution of several degrees Celsius or more is achieved, and a stable bonding quality is obtained by securing a certain temperature and time or higher in order to bond. Thereafter, the molten solder is solidified by cooling at a predetermined temperature drop rate to form a solder bonding layer. The temperature rise rate of this heat treatment is about 1°C / sec, and the temperature drop rate is 5°C / sec or higher. Preferably, it is 8°C / sec or higher and 15°C / sec or lower. In the conventional bonding method, the temperature drop rate of the heat treatment for forming the solder bonding layer was 1°C / sec. In this case, the fine crystals in the plating layer are easily coarsened. In addition, by setting the temperature drop rate within the above range, it is easy to obtain a solder bonding layer having a predetermined configuration.

[0054] At this time, for example, if the bonding member 27 is cream solder, when the flux contained in the bonding member 27 between the semiconductor chip 25 and the lead frame 26 foams, pieces of the bonding member 27 will fly off (for example, as indicated by the dashed arrow in FIG. 3). Even if the bonding member 27 is a plate solder or a fine metal particle sintered material, voids will be generated during melting, causing the pieces of the bonding member 27 to fly off. However, the protective portion 4b of the protective jig 4 prevents the pieces of the bonding member 27 from flying off toward the outer edge of the front surface of the semiconductor chip 25, in particular the control electrode 252.

[0055] In addition, the semiconductor chip 25 and the lead frame 26 have different linear expansion coefficients. Therefore, when heated, the semiconductor chip 25 may warp due to the difference in linear expansion coefficients. The protective jig 4 is merely installed between the support 3e and the front surface of the semiconductor chip 25. Therefore, as shown in FIG. 8, the protective jig 4 follows the warp of the semiconductor chip 25. That is, the beam 4a of the protective jig 4 is lifted in the Z direction relative to the support 3e and moves (slides) while sliding on the inner wall surface of the opening 5a. Accordingly, the protective part 4b also moves in the Z direction, so that it is possible to suppress the scattering of the piece of the bonding member 27 to the control electrode 252.

[0056] Thereafter, the manufacturing jig set 9 is removed from the assembly 1, and the ceramic circuit board 21, the semiconductor chip 25, and the lead frame 26 are bonded together. This particularly prevents the bonding material 27 from scattering onto the control electrode 252, and ensures that the wiring material is electrically and mechanically connected to the control electrode 252. By the above-described first bonding process, the ceramic circuit board 21, the semiconductor chip 25, and the lead frame 26 can be bonded together.

[0057] Therefore, in the first bonding step of the manufacturing method for the above-mentioned semiconductor device 20, there are prepared a semiconductor chip 25 including a main electrode 251 on its front surface, a lead frame 26 bonded to the main electrode 251, an alignment jig 3 including an opening 3a that is opened corresponding to the shape of the semiconductor chip 25 in a plan view and has a support portion 3e formed at the opening edge, and a protective jig 4 including a protective portion 4b with a protective surface 4c and a beam portion 4a formed on the protective portion 4b.

[0058] Next, the semiconductor chip 25 is placed in the opening 3a of the alignment jig 3 with its front surface facing the front side, and the semiconductor chip 25 is aligned. Next, the lead frame 26 is mounted via the bonding member 27 on the main electrode 251 of the semiconductor chip 25 placed on the alignment jig 3. Next, the protective portion 4b of the protective jig 4 is placed on the front surface with the protective surface 4c facing the main electrode 251, and the protective jig 4 is erected so that the beam portion 4a is supported by the support portion 3e.

[0059] Therefore, the protective portion 4b of the protective jig 4 prevents the pieces of the bonding members 27 from scattering onto the protected area, particularly onto the control electrode 252. Furthermore, the protective jig 4 follows the warping of the semiconductor chip 25 and can prevent the pieces of the bonding members 27 from scattering onto the control electrode 252 while being lifted up.

[0060] Next, a description will be given of modified examples of the alignment jig 3 and the protective jig 4 included in such a manufacturing jig set 9. Note that the alignment jig 3 and the protective jig 4 are not limited to these examples, and any structure may be used as long as the protective jig 4 mounted on the alignment jig 3 can be moved in the vertical direction.

[0061] [Variation 1] A first modification of the alignment jig 3 and the protective jig 4 will be described with reference to Fig. 9. Fig. 9 is a diagram showing a protective jig used in a semiconductor device manufacturing method according to a first modification of the first embodiment. Fig. 9 shows an enlarged view of the surroundings including the protective jig 4 installed on the alignment jig 3. Fig. 9(A) shows a plan view, and Fig. 9(B) shows a cross-sectional view taken along dashed line YY in Fig. 9(A).

[0062] In the first modification, the support portion 3e of the alignment jig 3 is formed in a concave shape on the opening 3a side of the front surface of the frame portion 3b. That is, the support portion 3e is recessed in the -Z direction from the front surface of the frame portion 3b on the opening 3a side, and in the -X direction from the inner wall surface on the front surface side of the frame portion 3b. The width of such a support portion 3e in the Y direction is approximately equal to the width of the protective jig 4. Moreover, the length of the support portion 3e in the -X direction is such that the beam portion 4a of the protective jig 4 is stably supported.

[0063] When the protective jig 4 is mounted on the alignment jig 3 and the semiconductor chip 25, the beam 4a of the protective jig 4 is fitted into the concave support 3e as shown in FIG. 9. That is, as described later, the beam 4a is arranged to be movable (slidable) while sliding up and down (±Z direction) along the support 3e. In addition, the protective surface 4c of the protective part 4b faces the main electrode 251 (the joint of the lead frame 26) of the semiconductor chip 25, and the protective area, specifically, the protective part 4b is mounted between the main electrode 251 and the control electrode 252 or the outer edge part. In this manner, the protective jig 4 is mounted between the support 3e and the front surface of the semiconductor chip 25.

[0064] When the semiconductor chip 25 is heated in this state, as shown in FIG. 8, warpage occurs in the semiconductor chip 25. The protective jig 4 moves in the Z direction following the warpage of the semiconductor chip 25. In the case of the first modification, both side surfaces in the width direction of the concave support portion 3e serve as guides, and the beam portion 4a of the protective jig 4 can reliably and stably move (slide) while sliding in the Z direction along the both side surfaces of the support portion 3e. As the beam portion 4a moves, the protective portion 4b can also reliably and stably move up and down along the Z direction. Therefore, even if the semiconductor chip 25 is warped unevenly or is subjected to an external impact, the protective jig 4 does not deviate from the support portion 3e, and the scattering of the bonding member 27 can be reliably suppressed. Note that, since the beam portion 4a and both side surfaces of the concave support portion 3e are in contact with each other, it is preferable to perform a treatment to reduce frictional resistance on at least one of the surfaces of the beam portion 4a and the support portion 3e so that the protective jig 4 including the beam portion 4a can move up and down smoothly. Specifically, the surfaces of the beam portion 4a and the support portion 3e may be covered with carbon or NiP (nickel-phosphorus plating) having self-lubricating properties.

[0065] [Variation 2] Modification 2, which is a variation of Modification 1 of the alignment jig 3 and the protective jig 4, will be described with reference to Fig. 10. Fig. 10 is a diagram showing a protective jig used in a semiconductor device manufacturing method according to Modification 2 of the first embodiment. Fig. 10 shows an enlarged plan view of the surroundings including the protective jig 4 installed on the alignment jig 3. Fig. 9(B) can be referred to for a cross-sectional view taken along dashed line YY in Fig. 10.

[0066] In the second modification, similarly to the first modification, the support portion 3e in the alignment jig 3 is formed in a concave shape on the opening 3a side of the frame portion 3b. That is, the support portion 3e is recessed in the -Z direction from the front surface of the frame portion 3b on the opening 3a side, and in the -X direction from the inner wall surface on the front surface side of the frame portion 3b. In the case of the second modification, the support portion 3e is formed so that the back side of the recess in the -X direction from the inner wall surface on the front surface side of the frame portion 3b forms a curved surface. Accordingly, the tip portion of the beam portion 4a of the protection jig 4 is also shaped to match the curved surface.

[0067] When mounting the protective jig 4 on such an alignment jig 3 and semiconductor chip 25, as shown in Fig. 10, the beam portion 4a of the protective jig 4 is fitted into the support portion 3e, and the tip portion of the beam portion 4a coincides with the inner side (in the -X direction) of the support portion 3e. Furthermore, the protective surface 4c of the protective portion 4b faces the main electrode 251 of the semiconductor chip 25, and is mounted between the main electrode 251 and the control electrode 252. In this manner, the protective jig 4 is installed between the support portion 3e and the front surface of the semiconductor chip 25.

[0068] In this protective jig 4, as in the first modification, both side surfaces in the width direction of the concave support portion 3e serve as guides, and the beam portion 4a of the protective jig 4 can reliably and stably move (slide) in the Z direction while sliding along the both side surfaces of the support portion 3e. As the beam portion 4a moves, the protective portion 4b can also reliably and stably move up and down along the Z direction. Therefore, even if the semiconductor chip 25 is warped unevenly or is subjected to an external impact, the protective jig 4 does not deviate from the support portion 3e, and the scattering of the bonding member 27 can be reliably suppressed. In addition, in the second modification, the inner side of the support portion 3e and the tip portion of the beam portion 4a of the protective jig 4 form a curved surface, so that the beam portion 4a can easily fit into the support portion 3e. Therefore, the protective jig 4 can be easily attached to the alignment jig 3. The beam portion 4a and the surface of the support portion 3e may be subjected to a friction reduction treatment similar to that of the first modification.

[0069] [Variation 3] Modification 3 of the alignment jig 3 and the protective jig 4 will be described with reference to Fig. 11. Fig. 11 is a diagram showing a protective jig used in a semiconductor device manufacturing method according to modification 3 of the first embodiment. Fig. 11 shows an enlarged view of the surroundings including the protective jig 4 installed on the alignment jig 3. Fig. 11(A) is a plan view, and Fig. 11(B) is a cross-sectional view taken along dashed line YY in Fig. 11(A).

[0070] In the third modification, the support 3e in the alignment jig 3 protrudes perpendicularly in the X direction (towards the opening 3a) from the inner wall surface of the opening 3a of the frame 3b. Furthermore, the support 3e extends in the -Z direction from the front surface of the frame 3b to the inner wall surface of the frame 3b. That is, the support 3e protrudes in a rectangular parallelepiped shape from the inner wall surface of the frame 3b perpendicularly in the X direction (towards the opening 3a). The protection jig 4 shown in FIG. 3 is also used in the third modification. However, in the third modification, a concave recess is formed in the tip of the flat beam 4a of the protection jig 4 in plan view in correspondence with the support 3e protruding in a rectangular parallelepiped shape. The recess of the beam 4a at this time is large enough to fit into the support 3e. Therefore, the width of the support 3e in the Y direction and the width of the recess of the beam 4a are approximately equal in plan view in FIG. 11(A). In addition, the thickness (depth) of the support 3e in the X direction in a plan view may be substantially equal to or longer than the depth of the beam 4a. The length of the support 3e in the -Z direction may be lower than the back surface of the beam 3e when the protection jig 4 is mounted on the alignment jig 3 and the semiconductor chip 25, as described later.

[0071] When the protective jig 4 is installed on such an alignment jig 3 and semiconductor chip 25, as shown in FIG. 11, the recess of the beam 4a of the protective jig 4 is fitted into the support 3e, and the beam 4a is leaned against the support 3e. That is, the beam 4a is arranged so as to be movable (slidable) while sliding up and down (in the ±Z direction) along the support 3e. The protective surface 4c of the protective part 4b is directed toward the main electrode 251 of the semiconductor chip 25, and the protective part 4b is mounted between the main electrode 251 and the control electrode 252. In this manner, the protective jig 4 is installed between the support 3e and the front surface of the semiconductor chip 25. The surfaces of the beam 4a and the support 3e may be subjected to a friction reduction treatment similar to that of the first modification.

[0072] When heated in this state, the protective jig 4 moves in the Z direction following the warpage of the semiconductor chip 25. In the case of the third modification, the support portion 3e protruding in a rectangular parallelepiped shape serves as a guide, and the beam portion 4a of the protective jig 4, whose recess at the tip end is fitted into the support portion 3e, can slide reliably and stably in the Z direction while sliding along the support portion 3e. As the beam portion 4a moves, the protective portion 4b can also move up and down reliably and stably along the Z direction. Therefore, even if the semiconductor chip 25 varies in warpage or is subjected to an external impact, the protective jig 4 does not deviate from the support portion 3e, and scattering of the bonding member 27 can be reliably suppressed.

[0073] In addition, in the modification 3, the support portion 3e of the alignment jig 3 and the beam portion 4a of the protection jig 4 are rectangular in plan view. However, this is not limited to this case, and they may be curved, uneven, or the like, as in the modification 2.

[0074] [Variation 4] A fourth modification of the alignment jig 3 and the protective jig 4 will be described with reference to Fig. 12. Fig. 12 is a diagram showing a protective jig used in a semiconductor device manufacturing method according to a fourth modification of the first embodiment. Fig. 12 shows an enlarged view of the surroundings including the protective jig 4 installed on the alignment jig 3. Fig. 12(A) is a plan view, and Fig. 12(B) is a cross-sectional view taken along dashed line YY in Fig. 12(A). Also, the protective jig 4 is not shown in Fig. 12(A).

[0075] In the fourth modification, the support 3e in the alignment jig 3 includes a recess 3e1 and a shaft 3e2. The recess 3e1 is formed in a concave shape on the opening 3a side of the front surface of the frame 3b, similar to the support 3e in the first modification (see FIG. 9). That is, the support 3e is recessed in the -Z direction from the front surface of the frame 3b on the opening 3a side, and in the -X direction from the inner wall surface of the front surface of the frame 3b. The shaft 3e2 is integral with the bottom of the recess 3e1 on the opening 3a side, and is formed in the width direction (Y direction). That is, the shaft 3e2 is formed in a convex shape parallel to the side of the edge of the opening. The side of the edge of the opening is the edge of the opening 3a facing the outer edge where the control electrode 252 of the semiconductor chip 25 is arranged. Alternatively, the shaft 3e2 may be saddle-shaped, and the front side may be semi-cylindrical.

[0076] On the other hand, a bearing portion 4a5 is formed on the back surface of the tip of the beam portion 4a of the protective jig 4 along the width direction (Y direction) of the beam portion 4a. That is, the bearing portion 4a5 is formed in a concave shape parallel to the side of the opening edge portion. The bearing portion 4a5 has a shape similar to an inverted shaft portion 3e2 of the support portion 3e.

[0077] When the protective jig 4 is set up on such an alignment jig 3 and semiconductor chip 25, as shown in FIG. 12, the bearing portion 4a5 of the beam portion 4a of the protective jig 4 is placed on the shaft portion 3e2 of the support portion 3e, and the protective surface 4c of the protective portion 4b faces the main electrode 251 of the semiconductor chip 25, and is mounted between the main electrode 251 and the control electrode 252. That is, the beam portion 4a is arranged so as to be rotatable (slidable) while sliding with the shaft portion 3e2 provided on the support portion 3e as a fulcrum. In this manner, the protective jig 4 is set up between the support portion 3e and the front surface of the semiconductor chip 25. The surfaces of the beam portion 4a and the support portion 3e may be subjected to a friction reduction treatment similar to that of the first modification.

[0078] When the semiconductor chip 25 is heated in this state, as shown in FIG. 12, warpage may occur in the semiconductor chip 25. The protective jig 4 rotates in the direction from the X-axis to the Z-axis in FIG. 12(B) with the bearing portion 4a5 as a fulcrum in response to the warpage of the semiconductor chip 25. In the case of the modified example 4, the bearing portion 4a5 of the beam portion 4a of the protective jig 4 rotates while sliding on the shaft portion 3e2 of the support portion 3e, and rotates counterclockwise with the bearing portion 4a5 as an axis. With the rotation of the beam portion 4a, the protective portion 4b can also move up and down along the Z direction reliably and stably. Therefore, even if the semiconductor chip 25 is warped unevenly or is subjected to an external impact, the protective jig 4 does not deviate from the support portion 3e, and the scattering of the bonding member 27 can be reliably suppressed. Furthermore, even when the protective part 4b rotates around the shaft part 3e2 of the support part 3e as a fulcrum (Figure 12 (B)), the tip of the protective part 4b moves in the vertical direction, so it can be understood that the protective jig 4 is movable in the vertical direction.

[0079] The shaft portion 3e2 of the support portion 3e does not necessarily have to be formed on the bottom surface of the recess 3e1. The shaft portion 3e2 may be formed with a gap from the bottom of the recess 3e1. The concave and convex shapes of the shaft portion 3e2 of the support portion 3e and the bearing portion 4a5 of the beam portion 4a may be reversed. That is, the shaft portion 3e2 may be formed concavely on the bottom of the support portion 3e, and the bearing portion 4a5 may be formed convexly on the back surface of the beam portion 4a so as to fit into the concave shaft portion 3e. It is sufficient that the protective jig 4 can rotate around the shaft portion 3e2 and the bearing portion 4a5.

[0080] [Second embodiment] In the second embodiment, the second bonding step of step S12 in the flowchart of the manufacturing method of the semiconductor device 20 shown in FIG. 2 will be described. In the second bonding step, the heat sink 28 is bonded by the bonding member 27 to the back surface of the ceramic circuit board 21 in which the semiconductor chip 25 and the lead frame 26 bonded by the bonding member 27 in step S11 of FIG. 2 are laminated in order. Here, the manufacturing jig set used when bonding the heat sink 28 to the back surface of the ceramic circuit board 21 in which the semiconductor chip 25 and the lead frame 26 are laminated in order and the second bonding step will be described in detail with reference to FIG. 13 and FIG. 14. FIG. 13 is a side view of the semiconductor device of the second embodiment. FIG. 14 is a flowchart showing the bonding step included in the manufacturing method of the semiconductor device of the second embodiment. Note that FIG. 13 shows a side view of an assembly 1a in which the ceramic circuit board 21, the semiconductor chip 25, and the lead frame 26 are further provided with the heat sink 28 and the manufacturing jig set 9 is attached.

[0081] The second embodiment particularly describes how, when ceramic circuit board 21 to which semiconductor chip 25 and lead frame 26 are bonded and heat sink 28 are heat-bonded with bonding material 27, the bonding material 27 between already-bonded semiconductor chip 25 and lead frame 26, and between ceramic circuit board 21 and semiconductor chip 25 is remelted, and the bonding material 27 (solder pieces, etc.) is prevented from scattering.

[0082] 13 includes a manufacturing jig set 9 that houses a heat sink 28, a ceramic circuit board 21, a semiconductor chip 25, and a lead frame 26. That is, in the second embodiment, a heat sink 28 is further bonded to the ceramic circuit board 21, the semiconductor chip 25, and the lead frame 26 that are bonded in the first embodiment.

[0083] The manufacturing jig set 9 includes alignment jigs 3, 7, 12, a protective jig 4, and a base jig 6. Although the weight 5 is omitted from the manufacturing jig set 9, the weight 5 may be included. As described in the first embodiment, the manufacturing jig set 9 is made of a material having excellent heat resistance and a small linear expansion coefficient. Examples of such materials include carbon and composite ceramic materials.

[0084] The base jig 6 is flat, and the heat sink 28 is disposed on the front surface in a plan view. The alignment jig 7 is flat, and has an opening formed therein and a frame portion 7b surrounding the opening. The alignment jig 7 also has a protrusion 7d formed along the opening on the inner wall surface of the frame portion 7b and protruding toward the opening side. The height of the frame portion 7b to the protrusion 7d corresponds to the thickness of the heat sink 28. Therefore, the alignment jig 7 is disposed on the heat sink 28 on the base jig 6, and the outer edge of the heat sink 28 is restricted by the protrusion 7d and the frame portion 7b relative to the base jig 6. In addition, when the heat sink 28 is a cooler, an inlet / outlet and an outlet, which become a protrusion at the bottom in FIG. 13, may be provided on the back surface of the heat sink 28.

[0085] The alignment jig 12 is flat, has an opening 12a formed therein, and includes a frame portion 12b surrounding the opening 12a. Such an alignment jig 12 is disposed on the front surface of the heat sink 28, in the opening of the alignment jig 7, in contact with the protrusion 7d. At this time, the opening 12a of the alignment jig 12 corresponds to the arrangement position of the ceramic circuit board 21 of the heat sink 28. Then, the opening 12a of the alignment jig 12 allows the ceramic circuit board 21 to be disposed on the front surface of the heat sink 28 via the bonding member 27. The thickness of such an alignment jig 12 is approximately equal to the thickness of the ceramic circuit board 21. The alignment jig 3 and the protection jig 4 are the same as those in the first embodiment.

[0086] The second joining step S12 in the flow chart of FIG. 2 using such an assembly 1a is performed as follows. First, an alignment step is performed to align the heat sink 28 with respect to the base jig 6 (step S12a in FIG. 14). Here, the heat sink 28 is mounted in a predetermined area of ​​the base jig 6. Furthermore, by placing the alignment jig 7 on the base jig 6 and the heat sink 28, the heat sink 28 is restrained to the base jig 6 by the convex portion 7d of the alignment jig 7. The positional deviation of the heat sink 28 in the X direction and the Y direction (horizontal direction) is suppressed. Therefore, each component can be mounted in an appropriate position in the subsequent mounting step. Furthermore, the alignment jig 12 is mounted in the opening of the alignment jig 7.

[0087] Next, a first mounting process is performed in which the ceramic circuit board 21, to which the lead frame 26 and the semiconductor chip 25 are bonded in sequence, is mounted on the heat sink 28 via the bonding member 27 based on the opening 12a of the alignment jig 12 (step S12b in FIG. 14).

[0088] Next, the alignment jig 3 is mounted on the ceramic circuit board 21 and the alignment jig 12, and a step of bridging the protection jig 4 with respect to the alignment jig 3 and the semiconductor chip 25 is performed (step S12c in FIG. 14). In the bridging step, the convex portion 3d formed on the back surface of the frame portion 3b of the alignment jig 3 is fitted into the gap between the outer edge portion of the circuit pattern 23 of the ceramic circuit board 21 and the opening edge portion of the alignment region 2a of the frame portion 12b of the alignment jig 12. This ensures that the ceramic circuit board 21 is fixed to the alignment jig 12. Then, as in the first embodiment, the protection surface 4c of the protection portion 4b of the protection jig 4 faces the main electrode 251 of the semiconductor chip 25 and is mounted between the main electrode 251 and the control electrode 252. Furthermore, the beam portion 4a of the protection jig 4 is supported by the support portion 3e. In this manner, the protection jig 4 is bridging between the support portion 3e and the front surface of the semiconductor chip 25. That is, the protective jig 4 having an L-shape in a side view has its beam portion 4a leaned against the support portion 3e and its protective portion 4b disposed on the semiconductor chip 25. As a result, the control electrode 252 of the semiconductor chip 25 is covered by the protective jig 4.

[0089] Next, a second mounting step is performed in which the weight 5 is mounted on the alignment jig 3 (step S12d in FIG. 14). Next, a heating step is performed (step S12e in FIG. 14). When the assembly 1a shown in FIG. 13 is heated, the bonding member 27 between the heat sink 28 and the ceramic circuit board 21 melts. At the same time, the bonding member 27 between the semiconductor chip 25 and the lead frame 26 may remelt. When the bonding member 27 remelts, there is a risk that pieces of the bonding member 27 may fly off, as in the case of the first embodiment. However, in this case, the protective jig 4 prevents the pieces from flying off. By the above-mentioned second bonding step, the ceramic circuit board 21 on which the semiconductor chip 25 and the lead frame 26 are laminated in order, and the heat sink 28 can be bonded.

[0090] In this manner, the semiconductor device 20 is constructed, and the ceramic circuit board 21 is bonded to the heat sink 28. The manufacturing jig set 9 is removed from the assembly 1a manufactured in this manner, to obtain the semiconductor device 20. In such a semiconductor device 20, scattering of the bonding member 27 onto the control electrode 252 is suppressed, and the wiring member can be reliably connected to the control electrode 252 electrically and mechanically.

[0091] Next, a modified example of the manufacturing jig set 9 used when joining the ceramic circuit board 21 to such a heat sink 28 will be described.

[0092] [Variations] A modified example of the manufacturing jig set 9 will be described with reference to Fig. 15. Fig. 15 is a side view of a semiconductor device according to a modified example of the second embodiment. Fig. 15 shows an enlarged view of an end side of an assembly 1b in which a semiconductor device 20 is included in the manufacturing jig set 9.

[0093] The modified assembly 1b is as follows. First, it has a protective jig 4 (first protective jig) for preventing scattering of the bonding members 27 that bond the semiconductor chip 25 and the lead frame 26. It has a protective jig (second protective jig) for preventing scattering of the bonding members 27 that bond the ceramic circuit board 21 and the semiconductor chip 25. It also has a protective jig 4 (third protective jig) for preventing scattering of the bonding members 27 that bond the ceramic circuit board 21 and the heat sink 28.

[0094] The assembly 1b shown in FIG. 15 includes a manufacturing jig set 9 in which a heat sink 28, a ceramic circuit board 21, a semiconductor chip 25, and a lead frame 26 are housed. The manufacturing jig set 9 includes alignment jigs 17 and 8, three protective jigs 4, and a base jig 6. Although the manufacturing jig set 9 omits the weight 5, the weight 5 may be included and is mounted on the alignment jig 8. As described in the first embodiment, the manufacturing jig set 9 is made of a material that has excellent heat resistance and a small linear expansion coefficient. For example, carbon or a composite ceramic material is used as such a material.

[0095] The alignment jig 17 is flat, has an opening 17a formed therein, and includes a frame 17b surrounding the opening. The alignment jig 17 may also include a protrusion 17d formed on the rear surface of the frame 17b. The inner wall surface of the frame 17b of the alignment jig 17 includes a support 17e formed to protrude into the opening 17a. The support 17e is configured to have the same shape as the support 4a shown in FIG. 3 so that the protective jig 4 can be placed thereon. The front surface of the alignment jig 17 is located above the front surface of the semiconductor chip 25 on the ceramic circuit board 21 on the heat sink 28. The alignment jig 17 is placed on the base jig 6 and the heat sink 28, and the heat sink 28 is regulated by the protrusion 17d of the frame 17b.

[0096] Next, the protective jig 4 (third protective jig) is placed over the alignment jig 17 and the heat sink 28. That is, as explained above, the protective portion 4b of the protective jig 4 is mounted with the protective surface 4c of the protective portion 4b facing the ceramic circuit board 21. At this time, the protective portion 4b is mounted on the side closer to the ceramic circuit board 21. Furthermore, the beam portion 4a of the protective jig 4 is supported by the support portion 17e. In this manner, the protective jig 4 is placed between the support portion 17e and the front surface of the heat sink 28.

[0097] The alignment jig 8 is flat, has an opening 8a formed therein, and includes a frame 8b surrounding the opening 8a. The alignment jig 8 includes a convex portion 8d formed on the back surface of the frame 8b, surrounding the opening 8a, and protruding downward. In addition, a support portion 8e1 protruding toward the opening 8a is formed on the inner wall surface of the convex portion 8d facing the opening 8a. The support portion 8e1 is configured to have a shape similar to that of the support portion 4a shown in FIG. 3 so that the protective jig 4 is disposed thereon. However, the support portion 8e1 extends toward the semiconductor chip 25 so that the tip of the support portion 8e1 is close to the semiconductor chip 25. In addition, a support portion 8e2 protruding toward the opening 8a is formed on the inner wall surface of the frame 8b facing the opening 8a. The support portions 8e1 and 8e2 are configured to have a shape similar to that of the support portion 4a shown in FIG. 3 so that the protective jig 4 is disposed thereon. However, the supporting portion 8e1 extends toward the semiconductor chip 25 so that the tip of the supporting portion 8e1 is close to the semiconductor chip 25.

[0098] Such an alignment jig 8 is mounted on the alignment jig 17 and the ceramic circuit board 21. That is, the back surface of the frame portion 8b of the alignment jig 8 is placed on the front surface of the alignment jig 17, and the protrusion portion 8d is placed between the outer edge portion of the circuit pattern 23 of the ceramic circuit board 21 and the outer edge portion of the insulating plate 22. Next, the protective jig 4 (second protective jig) is mounted on the alignment jig 8 and the ceramic circuit board 21. That is, the protective portion 4b of the protective jig 4 is mounted with the protective surface 4c of the protective portion 4b facing the semiconductor chip 25. The beam portion 4a of the protective jig 4 is supported by the support portion 8e1. At this time, the support portion 8e1 is lengthened so that the protective portion 4b of the protective jig 4 with the beam portion 4a supported by the support portion 8e1 can be brought close to the semiconductor chip 25. In this manner, the protective jig 4 is installed between the support portion 8e1 and the front surface of the ceramic circuit board 21. In addition, the protective jig 4 (first protective jig) is also installed on the supporting portion 8e2 of the alignment jig 8 and the semiconductor chip 25 in the same manner as in the first embodiment.

[0099] When heated, the bonding members 27 between the ceramic circuit board 21 and the heat sink 28 melt. At the same time, even if the bonding members 27 between the semiconductor chip 25 and the lead frame 26 and between the semiconductor chip 25 and the ceramic circuit board 21 remelt and pieces of the bonding members 27 fly off, the protective jig 4 prevents the pieces from flying off.

[0100] The manufacturing jig set 9 of the modified example can also be used when the heat sink 28, the ceramic circuit board 21, the semiconductor chip 25, and the lead frame 26 are bonded together at once with the bonding members 27. This is not limited to this case, and each component may be bonded separately with the bonding members 27.

[0101] When the ceramic circuit board 21 and the heat sink 28 are joined via the joining member 27, the protective jig 4 (third protective jig) can be placed on the support portion 17e of the positioning jig 17 and joined by heat treatment.

[0102] When a semiconductor chip 25 is bonded to a ceramic circuit board 21 having a heat sink 28 bonded thereto via a bonding member 27, an alignment jig 8 having at least a support portion 8e1 as shown in Fig. 15 is disposed. Then, a protection jig 4 (second protection jig) can be placed on the support portion 8e1 and bonded by heating.

[0103] Furthermore, when the lead frame 26 is joined to the semiconductor chip 25 via the joining member 27, the protective jig 4 (first protective jig) can be placed on the alignment jig 8 having the support portion 8e2 and joined by heating.

[0104] In this manner, the ceramic circuit board 21 is bonded to the heat sink 28. When the manufacturing jig set 9 is removed from the assembly 1b manufactured in this manner, the semiconductor device 20 is obtained. In such a semiconductor device 20, scattering of the bonding member 27 onto the control electrode 252 is suppressed, and the wiring member can be reliably connected to the control electrode 252 electrically and mechanically.

[0105] The modifications 1 to 4 described in the first embodiment can be applied to the supports 3e, 8e1, 8e2, and 17e and the protective jig 4 in the second embodiment. The supports 3e and the protective jig 4 for the alignment jig 3 in the first embodiment may also be provided for the bonding member 27 between the ceramic circuit board 21 and the semiconductor chip 25, similarly to the second embodiment.

[0106] [Third embodiment] In the third embodiment, a protective jig different from those in the first and second embodiments will be described as an example. First, an example of a ceramic circuit board 21 used in the third embodiment will be described with reference to FIG. 16. FIG. 16 is a plan view of a semiconductor device in the third embodiment. This ceramic circuit board 21 has a similar configuration to those in the first and second embodiments. However, in the ceramic circuit board 21 of the third embodiment, circuit patterns 23a, 23b, and 23c are formed on the front surface of an insulating plate 22 as shown in FIG. 16.

[0107] Circuit pattern 23a is formed along the X-direction end of insulating plate 22, bent in a U-shape in plan view at the -Y-direction end of insulating plate 22, and extends from its center in the +Y direction on the front surface of insulating plate 22. Semiconductor chips 25a are provided on circuit pattern 23a, aligned in the Y direction.

[0108] Circuit pattern 23b is formed on the front surface of insulating plate 22, extending in the Y direction between circuit patterns 23a which are U-shaped in a plan view. Circuit pattern 23c is formed extending in the Y direction along the end of insulating plate 22 in the -X direction. Semiconductor chips 25b are provided on circuit pattern 23c, aligned in the Y direction. Semiconductor chips 25a and 25b are similar to semiconductor chip 25.

[0109] Furthermore, the ceramic circuit board 21 and the main electrodes of the semiconductor chips 25a and 25b are electrically connected by lead frames 26a and 26b, respectively. The lead frame 26a electrically and mechanically connects the main electrodes of the semiconductor chip 25a to the circuit pattern 23b. The lead frame 26b electrically and mechanically connects the main electrodes of the semiconductor chip 25b to the circuit pattern 23a.

[0110] Next, a method for manufacturing a semiconductor device 20 including such a ceramic circuit board 21 will be described with reference to FIGS. 17 to 20 based on the manufacturing method of the third embodiment. FIGS. 17 and 19 are plan views showing a mounting process included in the manufacturing method of the semiconductor device of the third embodiment. FIGS. 18 and 20 are cross-sectional views showing a mounting process included in the manufacturing method of the semiconductor device of the third embodiment. Note that FIGS. 17 and 18 are steps corresponding to step S11b (FIG. 6) in FIG. 4 of the first embodiment. Also, FIGS. 19 and 20 are steps corresponding to step S11d (FIG. 7) in FIG. 3 of the first embodiment. Also, FIGS. 18 and 20 are cross-sectional views taken along dashed line YY in FIGS. 17 and 19. Note that this is an example in which a first protective jig is used to prevent the joining member 27 from scattering when joining the semiconductor chip 25 and the lead frame 26.

[0111] Steps S11a to S11c are performed in the same manner as in the flowchart of the first embodiment. In the third embodiment, the alignment jig 3 is mounted on the alignment jig 2 (see FIG. 18). The alignment jig 3 is flat, and openings 3a are formed at locations corresponding to the semiconductor chips 25a, 25b and the lead frames 26a, 26b in a plan view. When the alignment jig 3 is mounted on the alignment jig 2, the semiconductor chips 25a, 25b and the lead frames 26a, 26b are exposed from the openings 3a as shown in FIG. 17. Furthermore, the alignment jig 3 has a support portion 3e formed in the opening 3a. The support portion 3e is formed on a part of the side of the opening 3a that corresponds to the side of the semiconductor chips 25a, 25b. Such support portion 3e is recessed in the -Z direction from the front surface of frame portion 3b on the opening 3a side and in the -X direction from the inner wall surface on the front surface side of frame portion 3b, as shown in Figures 17 and 18. In the third embodiment, support portion 3e is formed at the corner portion of opening 3a.

[0112] Next, a step of installing the protective jig 4 on the alignment jig 3 and the semiconductor chip 25 is performed (step S11d in FIG. 3). The protective jig 4 used at this time includes a protective portion 4b as shown in FIG. 19 and FIG. 20. The protective portion 4b is formed in a block shape that fills the gap between the inner wall surface of the opening 3a of the alignment jig 3 and the area where the lead frame 28 is placed when the lead frames 26a, 26b are placed on the alignment jig 3 in a plan view. The block-shaped protective portion 4b is formed in a U-shape or an L-shape in a plan view. That is, the protective portion 4b is a rectangular parallelepiped that fills the gap between the lead frames 26a, 26b and the inner wall surface of the opening 3a for each inner wall surface and is connected in an L-shape or a U-shape. The protective jig 4 further has a beam portion 4a formed on the protective portion 4b. The beam portion 4a may be flush with the front surface of the protective portion 4b, and protrudes outward from the protective portion 4b. The beam portion 4a is formed at a portion of the protective portion 4b that corresponds to the support portion 3a when the protective portion 4b is disposed in the gap between the lead frames 26a, 26b and the inner wall surface of the opening 3a. Therefore, in the installation process, the protective portion 4b of the protective jig 4 is mounted on the semiconductor chips 25a, 25b so as to fit between the lead frames 26a, 26b and the inner wall surface of the opening 3a. At this time, the beam portion 4a is supported by the support portion 3e.

[0113] The protective portion 4b of the protective jig 4 is provided in accordance with the joining locations of the lead frames 26a, 26b to the semiconductor chips 25a, 25b. For example, for the opening 3a at the upper left of Fig. 19, the protective portion 4b is disposed corresponding to two perpendicular sides of the semiconductor chip 25b around the lead frame 26b. For the opening 3a at the lower left of Fig. 19, the protective portion 4b is disposed corresponding to three sides of the semiconductor chip 25b around the lead frame 26b.

[0114] Next, a weight 5 is mounted (step S11e in FIG. 3), and a heating process is performed (step S11f in FIG. 3). At this time, the protective portion 4b of the protective jig 4 prevents pieces of the bonding material 27 between the semiconductor chip 25 and the lead frame 26 from scattering onto the control electrode 252.

[0115] Furthermore, even if the semiconductor chip 25 is warped, the protective jig 4 is merely installed between the support portion 3e and the front surface of the semiconductor chip 25. The protective portion 4b is arranged to be movable (slidable) while sliding up and down (in the ±Z direction) between the lead frames 26a, 26b and the inner wall surface of the opening 3a. Therefore, the protective jig 4 can suppress the scattering of the pieces of the bonding member 27 to the control electrode 252 while being lifted in the Z direction in accordance with the warp of the semiconductor chip 25. Next, modified examples of the protective jig 4 included in such a manufacturing jig set 9 will be described.

[0116] [Variations] A modified example of the protective jig 4 will be described with reference to FIG. 21. FIG. 21 is a diagram showing a protective jig used in a semiconductor device manufacturing method according to a modified example of the third embodiment. FIG. 21 corresponds to FIG. 19. That is, the protective portion 4b of the protective jig 4 is divided into a plurality of portions corresponding to the gaps between the lead frames 26a, 26b and the respective inner wall surfaces of the opening 3a. For example, for the opening 3a at the lower left of FIG. 21, the protective portion 4b is divided into block-shaped protective members 4b1, 4b2, and 4b3 and arranged in the gaps between the lead frame 26b and the inner wall surface of the opening 3a on three sides. That is, the protective portion 4b is divided in correspondence with each side of the opening edge of the opening 3a and arranged in each gap between the lead frame 26b and the inner wall surface of the opening 3a.

[0117] In addition, beams 4a1, 4a2, and 4a3 are formed on the protective members 4b1, 4b2, and 4b3 of the protective portion 4b, respectively, which are flush with the front surfaces of the protective members 4b1, 4b2, and 4b3 and protrude outward from the protective members 4b1, 4b2, and 4b3. Furthermore, support parts corresponding to the beams 4a1, 4a2, and 4a3 are formed on the opening edge of the opening 3a of the alignment jig 3 when the protective members 4b1, 4b2, and 4b3 are respectively arranged in the gaps between the lead frames 26a and 26b and the inner wall surfaces of the opening 3a. The protective members 4b1, 4b2, and 4b3 are arranged to be movable (slidable) while sliding up and down (in the ±Z direction) between the lead frames 26a and 26b and the inner wall surfaces of the opening 3a. Moreover, the upper left part of FIG. 21 shows a case where protective portion 4b is divided and arranged in the gap between lead frame 26b and two sides of the inner wall surface of opening 3a.

[0118] In this case, the protective part 4b of the protective jig 4 also prevents pieces of the bonding member 27 between the semiconductor chip 25 and the lead frame 26 from scattering onto the control electrode 252. Even if the semiconductor chip 25 is warped, the protective jig 4 is merely installed between the support part 3e and the front surface of the semiconductor chip 25. In particular, in this modified example, since the protective part 4b is divided, it is easy to follow the warping of the semiconductor chips 25a and 25b, and is easy to lift compared to the case of FIG. 19. Therefore, the protective jig 4 can follow the warping of the semiconductor chip 25 and be lifted in the Z direction (movable in the vertical direction), while preventing pieces and particles of the bonding member 27 from scattering onto the control electrode 252. It is possible to prevent scattering onto not only the control electrode 252 but also the front surface of the semiconductor chip 25. [Explanation of symbols]

[0119] 1,1a,1b Assembly 2,3,7,8,12,17 Alignment jig 2a Alignment area 2b,3b,5b,7b,8b,12b,17b Frame 2c bottom 3a,5a,8a,12a,17a opening 3c,3e1 Concave 3d,5d,7d,8d,17d Convex part 3e,8e1,8e2,17e Support part 3e2 Shaft 4 Protective fixture 4a, 4a1, 4a2, 4a3 Beam section 4a5 bearing part 4b Protective part 4b1, 4b2, 4b3 Protective materials 4c Protective surface 5 Weight 6 Base jig 9 Manufacturing jig set 20 Semiconductor Devices 21 Ceramic circuit board 22 Insulating plate 23, 23a, 23b, 23c Circuit patterns 24 Metal plate 25, 25a, 25b Semiconductor chip 26, 26a, 26b Lead frame 27 Joining materials 28 Heat sink 251 Main electrode 252 Control Electrode

Claims

1. a preparation process for preparing a first component including a joining region on its front surface, a second component to be joined to the joining region, an alignment jig including an opening that is opened to correspond to the shape of the first component in a plan view and has a support portion formed on the opening edge, and a protection jig including a protection portion having a protection surface and a beam portion formed on the protection portion; an alignment step of placing the first component in the opening of the alignment jig with the front surface exposed, and aligning the first component; a mounting step of mounting a second component on the to-be-joined region of the first component placed on the alignment jig via a joining member; an erection process, either before or after the mounting process, of placing the protective portion of the protective jig on the front surface with the protective surface facing the welded region, and erecting the protective jig so that the beam portion is supported by the support portion; a heating step of heating the joining member; A method for manufacturing a semiconductor device having the above structure.

2. the first component further includes a protective region on the front surface excluding the region to be joined, In the installation step, the protective portion of the protective jig is disposed at a predetermined distance from the welded region of the protective region. The method for manufacturing a semiconductor device according to claim 1 .

3. The beam portion is formed by extending perpendicularly to the end portion of the protective portion of the installed protective jig.

3. The method for manufacturing a semiconductor device according to claim 1.

4. The support portion supports the back surface of the beam portion of the installed protective jig vertically upward. The method for manufacturing a semiconductor device according to claim 3 .

5. the support portion protrudes perpendicularly to the opening from an inner wall surface of the opening of the alignment jig in a plan view, In the erection step, the back surface of the beam portion of the protective jig is placed on the front surface of the support portion. The method for manufacturing a semiconductor device according to claim 4 .

6. The support portion is formed as a recessed portion on the front surface of the alignment jig toward the opening portion, In the erection step, the beam portion of the protective jig is fitted into the recess portion of the support portion, and the beam portion is arranged to be movable while sliding up and down along the support portion. The method for manufacturing a semiconductor device according to claim 4 .

7. The support portion protrudes perpendicularly from an inner wall surface of the opening of the alignment jig toward the opening in a rectangular parallelepiped shape in a plan view, A recess having a concave shape in a plan view is formed at the tip of the beam portion of the protective jig, In the erection step, the recess of the beam portion of the protective jig is fitted into the support portion, and the beam portion is arranged to be movable while sliding up and down along the support portion. The method for manufacturing a semiconductor device according to claim 3 .

8. a shaft portion parallel to a side of the opening edge portion on which the support portion is formed is formed in the recess of the support portion, a bearing portion parallel to a side of the opening edge portion is formed on a back surface of a region of the protective jig that is fitted to the support portion of the beam portion, In the erection step, the shaft portion of the support portion is fitted into the bearing portion of the beam portion of the protective jig, and the beam portion is disposed on the support portion so that the protective jig can rotate around the bearing portion as an axis. The method for manufacturing a semiconductor device according to claim 6 .

9. The protective jig has a flat protective portion and a flat beam portion, and the beam portion is formed perpendicular to the protective portion from an end of the protective portion.

9. The method for manufacturing a semiconductor device according to claim 1.

10. the protective portion has a block shape in a plan view when the first component is placed on the alignment jig, the block shape filling a gap between an inner wall surface of the opening of the alignment jig and the second component.

9. The method for manufacturing a semiconductor device according to claim 1.

11. the protective portion is divided into a plurality of portions corresponding to sides of the opening edge portion of the opening and includes a plurality of protective members disposed in the gap, the beam portions are formed in the same plane as the front surfaces of the plurality of protection members and protrude outward from the plurality of protection members; the support portions are formed on the opening edge portion in correspondence with the plurality of beam portions formed on the plurality of protection members arranged in the gap; The method for manufacturing a semiconductor device according to claim 10.

12. the first component placed in the opening of the alignment jig is constrained by the opening from moving in a horizontal direction relative to a stacking direction in which the second component is stacked relative to the first component; The method for manufacturing a semiconductor device according to any one of claims 1 to 11.

13. the first component is a semiconductor chip, the second component is a wiring member; The method for manufacturing a semiconductor device according to any one of claims 1 to 12.

14. the bonded region is a main electrode of the semiconductor chip; The method for manufacturing a semiconductor device according to claim 13.

15. the first component is a circuit pattern, the second component is a semiconductor chip; The method for manufacturing a semiconductor device according to any one of claims 1 to 12.

16. the first component is a heat sink; the second component is an insulating circuit board; The method for manufacturing a semiconductor device according to any one of claims 1 to 12.

17. an alignment jig including an opening that is opened on a front surface thereof in accordance with a shape in a plan view of a component that includes a region to be joined, and has a support portion formed on an edge of the opening; a protective jig including a protective portion having a protective surface and a beam portion formed on the protective portion, the protective portion being disposed on the front surface of the component with the protective surface facing the joining region, and the beam portion being supported by the support portion; A semiconductor device manufacturing jig set having the same.

18. The beam portion of the protective jig supported by the support portion is supported by the support portion so as to be movable upward relative to the support portion. The semiconductor device manufacturing jig set according to claim 17.

Citation Information

Patent Citations

  • Positioning jig of semiconductor chip and manufacturing method of semiconductor device

    JP2013065662A

  • Semiconductor device

    JP2017037892A

  • Manufacturing method of semiconductor device and soldering auxiliary tool

    JP2019036653A

  • Manufacturing method of semiconductor module and assembly jig set

    JP2020155457A

  • Assembly jig set and manufacturing method of semiconductor module

    JP2020178026A