Filament and fishing line
A polyamide resin composed of xylylene diamine and α,ω-linear aliphatic dicarboxylic acid addresses the issue of strength retention in filaments post-water absorption, achieving high retention rates of linear and knot strength.
Patent Information
- Application Number
- JP2021525925
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-06-11
- Filing Date
- 2020-04-14
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-04-14
AI Technical Summary
Existing polyamide resins used in filaments, such as those derived from ε-caprolactam, ε-aminocaproic acid, and hexamethylenediamine, fail to maintain high linear and knot strength after water absorption treatment, necessitating improved retention rates.
A polyamide resin synthesized from xylylene diamine and α,ω-linear aliphatic dicarboxylic acid with specific molecular compositions is used, comprising 70 mol% or more xylylene diamine and 70 mol% or more α,ω-linear aliphatic dicarboxylic acid, enhancing retention rates.
The solution provides filaments with high linear and knot strength retention rates after water absorption treatment, achieving 90% or more retention of linear strength and 70% or more retention of knot strength.
Smart Images

Figure 0007593313000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a filament and a fishing line, and more particularly to a filament made of polyamide resin. [Background technology]
[0002] Conventionally, the use of polyamide resin for filaments has been considered. For example, Patent Document 1 discloses a monofilament containing a polyamide resin, the polyamide resin containing units derived from ε-caprolactam and / or ε-aminocaproic acid (hereinafter also referred to as "unit 1"), units derived from adipic acid (hereinafter also referred to as "unit 2"), and units derived from hexamethylenediamine (hereinafter also referred to as "unit 3"), and the proportion of units 1 is more than 60 mass% and less than 80 mass% of the total of units 1, 2, and 3. Furthermore, Patent Document 2 discloses polyamide filaments containing a polyamide resin obtained by polycondensation of an aliphatic diamine containing pentamethylenediamine as a main component and a dicarboxylic acid containing adipic acid as a main component. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2016-223037 A [Patent Document 2] JP 2010-281027 A Summary of the Invention [Problem to be solved by the invention]
[0004] As described above, polyamide resins are used for filaments. For example, when used for fishing lines, high retention of linear strength and knot strength is required after water absorption treatment. The present invention has an object to solve the above problems, and to provide a filament and a fishing line that have a high retention rate of straight strength and knot strength after a water absorption treatment. [Means for solving the problem]
[0005] In light of the above-mentioned problems, the present inventors conducted research and found that the above-mentioned problems can be solved by using filaments containing a polyamide resin synthesized from xylylenediamine and an α,ω-linear aliphatic dicarboxylic acid having 11 to 14 carbon atoms. Specifically, the above problems were solved by the following means. <1> A polyamide resin (A) is included, the polyamide resin (A) being composed of diamine-derived structural units and dicarboxylic acid-derived structural units, 70 mol % or more of the diamine-derived structural units being derived from xylylenediamine, and 70 mol % or more of the dicarboxylic acid-derived structural units being derived from an α,ω-linear aliphatic dicarboxylic acid having 11 to 14 carbon atoms. filament. <2> It is stretched, <1> The filament according to claim 1. <3> The xylylenediamine contains 10 to 90 mol % of metaxylylenediamine and 90 to 10 mol % of paraxylylenediamine (however, the total of metaxylylenediamine and paraxylylenediamine does not exceed 100 mol %). <1> or <2> The filament according to claim 1. <4> The xylylenediamine contains 40 to 80 mol % of metaxylylenediamine and 60 to 20 mol % of paraxylylenediamine (however, the total of metaxylylenediamine and paraxylylenediamine does not exceed 100 mol %). <1> or <2> The filament according to claim 1. <5> The xylylenediamine contains 51 to 75 mol % of metaxylylenediamine and 49 to 25 mol % of paraxylylenediamine (however, the total of metaxylylenediamine and paraxylylenediamine does not exceed 100 mol %). <1> or <2> The filament according to claim 1. <6> The dicarboxylic acid comprises 1,12-dodecanedioic acid. <1> ~ <5> 13. The filament according to any one of claims 1 to 12. <7> The linear strength X of the filament after drying at 40°C for 74 hours 1 The linear strength X of the filament after immersion in water at 23°C for 336 hours 2 Retention rate [(X 2 / X 1 ) × 100] is 90 or more, and the linear strength is a value measured in accordance with JIS L 1013:2010; <1> ~ <6> 13. The filament according to any one of claims 1 to 12. <8> The knot strength Y of the filament after drying at 40°C for 74 hours 1 The knot strength Y after immersion of the filament in water at 23°C for 336 hours 2 Retention rate [(Y 2 / Y 1 ) × 100] is 70 or more, and the knot strength is a value measured in accordance with JIS L 1013:2010; <1> ~ <7> 13. The filament according to any one of claims 1 to 12. <9> <1> ~ <8> A fishing line having the filament according to any one of claims 1 to 5. Effect of the Invention
[0006] According to the present invention, it is possible to provide a filament and a fishing line that have a high retention rate of straight strength and knot strength after a water absorption treatment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] The present invention will be described in detail below. In this specification, the word "to" is used to mean that the numerical values before and after it are included as a lower limit and an upper limit.
[0008] The filament of the present invention is characterized in that it contains a polyamide resin (A), the polyamide resin (A) is composed of diamine-derived constituent units and dicarboxylic acid-derived constituent units, 70 mol % or more of the diamine-derived constituent units are derived from xylylenediamine, and 70 mol % or more of the dicarboxylic acid-derived constituent units are derived from an α,ω-linear aliphatic dicarboxylic acid having 11 to 14 carbon atoms. By adopting such a constitution, a filament having a high retention rate of linear strength and knot strength after water absorption treatment can be obtained.
[0009] <Polyamide resin (A)> The filament of the present invention contains a polyamide resin (A) that is composed of diamine-derived structural units and dicarboxylic acid-derived structural units, in which 70 mol % or more of the diamine-derived structural units are derived from xylylenediamine, and 70 mol % or more of the dicarboxylic acid-derived structural units are derived from an α,ω-linear aliphatic dicarboxylic acid having 11 to 14 carbon atoms. By using such polyamide resin (A), it is possible to increase the retention rate of linear strength and knot strength after water absorption treatment. The reason for this is speculation, but it is presumed that the polyamide resin (A) can increase these retention rates because the glass transition temperature after water absorption treatment is room temperature or higher. It is known that polyamide resins synthesized from xylylenediamine and α,ω-linear aliphatic dicarboxylic acids having 11 to 14 carbon atoms have low water absorption rates. However, there may be no correlation between low water absorption rates and the retention rates of physical properties after water absorption treatment. Furthermore, in the present invention, by using the polyamide resin (A), a filament having excellent transparency can be obtained. Also, by using the polyamide resin (A), a filament having high strength can be obtained.
[0010] In the polyamide resin (A), 70 mol % or more of the diamine-derived structural units are derived from xylylenediamine, preferably 80 mol % or more, more preferably 90 mol % or more, even more preferably 95 mol % or more, and even more preferably 99 mol % or more.
[0011] Xylylenediamine preferably contains 10-90 mol% metaxylylenediamine and 90-10 mol% paraxylylenediamine (however, the total of metaxylylenediamine and paraxylylenediamine does not exceed 100 mol%), more preferably contains 40-80 mol% metaxylylenediamine and 60-20 mol% paraxylylenediamine, and even more preferably contains 51-75 mol% metaxylylenediamine and 49-25 mol% paraxylylenediamine. In the xylylenediamine, the total of metaxylylenediamine and paraxylylenediamine preferably accounts for 95 mol% or more, more preferably 99 mol% or more, and even more preferably 100 mol%.
[0012] Diamine components other than xylylenediamine include aliphatic diamines such as tetramethylenediamine, pentamethylenediamine, 2-methylpentanediamine, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, nonamethylenediamine, decamethylenediamine, dodecamethylenediamine, 2,2,4-trimethylhexamethylenediamine, and 2,4,4-trimethylhexamethylenediamine; 1,3-bis(aminomethyl)cyclohexane; 1,4-bis(aminomethyl)cyclohexane; Examples of the diamines include alicyclic diamines such as bis(4-aminocyclohexyl)cyclohexane, 1,3-diaminocyclohexane, 1,4-diaminocyclohexane, bis(4-aminocyclohexyl)methane, 2,2-bis(4-aminocyclohexyl)propane, bis(aminomethyl)decalin, and bis(aminomethyl)tricyclodecane; and diamines having an aromatic ring such as bis(4-aminophenyl)ether, paraphenylenediamine, and bis(aminomethyl)naphthalene. These can be used alone or in combination of two or more.
[0013] In the polyamide resin (A), 70 mol % or more of the dicarboxylic acid-derived structural units are derived from an α,ω-straight-chain aliphatic dicarboxylic acid having 11 to 14 carbon atoms (preferably an α,ω-straight-chain aliphatic dicarboxylic acid having 12 to 14 carbon atoms, more preferably 1,12-dodecanedioic acid), preferably 80 mol % or more, more preferably 90 mol % or more, even more preferably 95 mol % or more, and even more preferably 99 mol % or more.
[0014] Examples of dicarboxylic acid components other than α,ω-linear aliphatic dicarboxylic acids having 11 to 14 carbon atoms include α,ω-linear aliphatic dicarboxylic acids having 10 or less carbon atoms, such as succinic acid, glutaric acid, pimelic acid, suberic acid, azelaic acid, adipic acid, and sebacic acid; phthalic acid compounds, such as isophthalic acid, terephthalic acid, and orthophthalic acid; and naphthalene dicarboxylic acids, such as 1,2-naphthalene dicarboxylic acid, 1,3-naphthalene dicarboxylic acid, 1,4-naphthalene dicarboxylic acid, 1,5-naphthalene dicarboxylic acid, 1,6-naphthalene dicarboxylic acid, 1,7-naphthalene dicarboxylic acid, 1,8-naphthalene dicarboxylic acid, 2,3-naphthalene dicarboxylic acid, 2,6-naphthalene dicarboxylic acid, and 2,7-naphthalene dicarboxylic acid. These can be used alone or in combination of two or more.
[0015] Here, "consisting of diamine-derived structural units and dicarboxylic acid-derived structural units" means that the amide bond constituting the polyamide resin (A) is formed by the bond between the dicarboxylic acid and the diamine. The polyamide resin (A) also contains other sites such as terminal groups in addition to the dicarboxylic acid-derived structural units and diamine-derived structural units. Furthermore, it may contain repeating units having amide bonds not derived from the bond between the dicarboxylic acid and the diamine, or trace amounts of impurities. Specifically, in addition to the diamine component and the dicarboxylic acid component, the polyamide resin (A) may also contain lactams such as ε-caprolactam and laurolactam, and aliphatic aminocarboxylic acids such as aminocaproic acid and aminoundecanoic acid as copolymerization components as long as the effects of the present invention are not impaired. In the present invention, preferably 90% by mass or more of the polyamide resin (A) is a diamine-derived structural unit or a dicarboxylic acid-derived structural unit, more preferably 95% by mass or more, and even more preferably 98% by mass or more.
[0016] The polyamide resin (A) used in the present invention preferably has a number average molecular weight (Mn) of 6,000 to 50,000, more preferably 8,000 to 48,000, and even more preferably 9,000 to 46,000. Within such a range, the molding processability is improved.
[0017] The number average molecular weight (Mn) referred to here can be determined from a standard polymethyl methacrylate (PMMA)-equivalent value measured by gel permeation chromatography (GPC).
[0018] In the present invention, the lower limit of the glass transition temperature of the polyamide resin (A) is preferably 30° C. or higher, more preferably 45° C. or higher, and even more preferably 50° C. or higher. Within this range, the retention rate of linear strength and knot strength after water absorption treatment tend to be higher. On the other hand, the upper limit of the glass transition temperature of the polyamide resin (A) is not particularly limited, and can be, for example, 200° C. or lower.
[0019] The melting point in the present invention means the temperature at the top of the endothermic peak during heating observed by DSC (differential scanning calorimetry). Specifically, the melting point means the temperature at the top of the endothermic peak observed when a DSC apparatus is used, a sample amount is 1 mg, nitrogen is flowed as the atmospheric gas at 30 mL / min, and a heating rate is 10°C / min, the polyamide resin is heated from room temperature (25°C) to a temperature above the expected melting point, the molten polyamide resin is then quenched with dry ice, and the temperature is raised again to a temperature above the melting point at a rate of 10°C / min. The glass transition temperature is the glass transition point measured by heating and melting a sample once to eliminate the effect of thermal history on crystallinity, and then heating it again. Specifically, a DSC device is used, the amount of sample is about 1 mg, nitrogen is flowed as the atmospheric gas at 30 mL / min, and the temperature is raised at a rate of 10°C / min. The polyamide resin is heated from room temperature to a temperature above the expected melting point and melted, and then quenched with dry ice and heated again at a rate of 10°C / min to a temperature above the melting point, to determine the glass transition temperature.
[0020] The lower limit of the relative viscosity (RV) of the polyamide resin (A) measured under the conditions of JIS K 69020-2 is preferably 2.0 or more, more preferably 2.1 or more, and even more preferably 2.3 or more. On the other hand, the upper limit of the relative viscosity of the polyamide resin (A) is preferably 4.0 or less, more preferably 3.9 or less, and even more preferably 3.8 or less. By setting it in such a range, the linear strength and knot strength tend to be further improved.
[0021] Furthermore, in the filament of the present invention, the polyamide resin (A) preferably accounts for 70 mass% or more of the mass of the filament, more preferably 80 mass% or more, and even more preferably 90 mass% or more, and may be 95 mass% or more. The filament of the present invention may contain only one type of polyamide resin (A), or may contain two or more types. When two or more types are contained, the total amount is preferably within the above range.
[0022] <Other resin components> The filament of the present invention may contain a polyamide resin other than the polyamide resin (A) or a thermoplastic resin other than polyamide. Examples of polyamide resins other than the polyamide resin (A) include polyamide 4, polyamide 6, polyamide 11, polyamide 12, polyamide 46, polyamide 66, polyamide 6 / 66, polyamide 610, polyamide 612, polyhexamethylene terephthalamide (polyamide 6T), polyhexamethylene isophthalamide (polyamide 6I), polyamide 66 / 6T, polyamide 9T, polyamide 9MT, polyamide 6I / 6T, polyamide XD6 (polyxylylene adipamide), polyamide XD10 (polyxylylene sebaceamide), and the like, with polyamide 6, polyamide 66, polyamide 666, polyamide 610, and polyamide 612 being preferred.
[0023] When the filament of the present invention contains polyamide resin (A) and a polyamide resin other than polyamide resin (A), the mass ratio thereof (polyamide resin (A): polyamide resin other than polyamide resin (A)) is preferably 100:1-100, and more preferably 100:10-90. The filament of the present invention may contain only one type of polyamide resin other than the polyamide resin (A), or may contain two or more types. When two or more types are contained, the total amount is preferably within the above range.
[0024] Examples of thermoplastic resins other than the polyamide resins include polyolefin resins such as polyethylene and polypropylene, polyester resins such as polyethylene terephthalate and polybutylene terephthalate, polycarbonate resins, polyoxymethylene resins, polyether ketones, polyether sulfones, and thermoplastic polyether imides. The filament of the present invention may be configured to be substantially free of thermoplastic resins other than polyamide resin (polyamide resin (A) and polyamide resins other than polyamide resin (A)). "Substantially free" means, for example, that the content of thermoplastic resins other than polyamide resins in the filament of the present invention is 5% by mass or less of the mass of the polyamide resin.
[0025] <Additives> To the filament of the present invention, additives such as antioxidants, heat stabilizers, hydrolysis resistance improvers, weathering stabilizers, matting agents, UV absorbers, nucleating agents, plasticizers, dispersants, flame retardants, antistatic agents, coloring inhibitors, gelling inhibitors, colorants, release agents, surface activators, dyes, etc. can be added within the scope of not impairing the objects and effects of the present invention. For details of these, refer to the descriptions in paragraphs
[0130] to
[0155] of Japanese Patent No. 4894982, the descriptions in paragraph
[0021] of Japanese Patent Laid-Open No. 2010-281027, and the descriptions in paragraph
[0036] of Japanese Patent Laid-Open No. 2016-223037, the contents of which are incorporated herein by reference. Specific examples of the plasticizer include hexyldecyl p-hydroxybenzoate (manufactured by Kao Corporation, Exepar HD-PB), ethylhexyl p-hydroxybenzoate, ethylhexyl o-hydroxybenzoate, and N-butylbenzenesulfonamide. In addition, the descriptions in paragraphs 0033 to 0038 of International Publication No. 2017 / 010389 can also be taken into consideration, and the contents of these are incorporated herein by reference. The filament of the present invention may contain a filler such as carbon fiber, but is preferably substantially free of the filler, which means, for example, that the amount of the filler is 3% by mass or less of the filament of the present invention. In addition, the filament of the present invention can be given any surface property by performing plasma treatment. For details, refer to the descriptions of paragraphs 0019 to 0022 of JP-A-06-182195, the contents of which are incorporated herein by reference.
[0026] <Characteristics and properties of filament> The length (mass average length) of the filament of the present invention is not particularly limited, but is usually 2 cm or more, preferably 0.1 m or more, more preferably 1 m or more, and even more preferably 100 m or more. The upper limit of the length (mass average length) of the filament is preferably 20,000 m or less, more preferably 1,000 m or less, and even more preferably 100 m or less.
[0027] The lower limit of the fineness of the filament of the present invention is preferably 50d (denier) or more, more preferably 100d or more, even more preferably 300d or more, even more preferably 500d or more, and even more preferably 600d or more. The upper limit is preferably 1500d or less, more preferably 1300d or less, even more preferably 1200d or less, and particularly preferably 1100d or less. The fineness is measured by the method described in the Examples below.
[0028] The filament of the present invention may be a monofilament or a multifilament, preferably a monofilament, and may have a core-sheath structure. The cross section of the filament of the present invention is usually circular. Here, the circular shape includes not only a circular shape in a mathematical sense, but also a shape that is generally considered to be circular in the technical field of the present invention. The cross section of the filament of the present invention may be a shape other than a circular shape, for example, a flat shape such as an ellipse or an oval shape.
[0029] The filament of the present invention has a linear strength of X 1 Linear strength X after water absorption treatment 2 Retention rate [(X 2 / X 1 )×100] is preferably 90 or more, more preferably 92 or more, even more preferably 93 or more, and still more preferably 94 or more. The upper limit of the retention rate of linear strength after water absorption treatment is preferably 100. The knot strength of the filament in the dry state is Y1 Knot strength Y after water absorption treatment 2 Retention rate [(Y 2 / Y 1 )×100] is preferably 70 or more, more preferably 80 or more, even more preferably 85 or more, and still more preferably 90 or more. The upper limit of the knot strength retention rate after water absorption treatment is preferably 100. The retention rate of linear strength after water absorption treatment and the retention rate of knot strength after water absorption treatment are measured by the method described in the examples below.
[0030] <Stretching> The filament of the present invention may or may not be stretched, but is preferably stretched. The filament is preferably stretched in the longitudinal direction of the filament (filament length direction). The stretching ratio is preferably 2.5 times or more, more preferably 3.0 times or more, even more preferably 3.5 times or more, and even more preferably 3.8 times or more. The upper limit of the stretching ratio is preferably 8.0 times or less, more preferably 7.5 times or less, even more preferably 7.0 times or less, and even more preferably 6.5 times or less.
[0031] <Manufacturing method> The filament of the present invention is obtained by molding a polyamide resin (A) or a composition containing a polyamide resin (A). The molding method is arbitrary, and the filament may be molded into a desired shape by any conventionally known molding method such as melt spinning. For example, the description in paragraphs 0051 to 0058 of International Publication No. 2017 / 010389 can be referred to, and the contents of these paragraphs are incorporated herein by reference. The molding conditions and the shape after molding may be appropriately selected and determined depending on the application, for example, filaments for fishing lines, filaments for fishing nets, filaments for industrial materials, filaments for woven fabrics such as clothing and carpets, and strings for rackets.
[0032] <Application> The filament of the present invention may be used as it is, or may be processed into a molding material such as a blended yarn, a braided cord, a twisted cord, etc. It is also preferably used as a molding material for a woven fabric, a knitted fabric, a nonwoven fabric, etc. The filaments of the present invention are widely used in automobile and other transportation vehicle parts, general machine parts, precision machine parts, electronic and electrical device parts, office equipment parts, building materials and housing related parts, medical devices, leisure sports goods (e.g., fishing lines), play equipment, medical supplies, food packaging films, everyday items such as clothing, defense and aerospace products, etc. The filament of the present invention may be wound around a core, i.e., a wound body having a core and a filament wound around the core may be formed. EXAMPLES
[0033] The present invention will be described in more detail below with reference to examples. The materials, amounts, ratios, processing contents, processing procedures, etc. shown in the following examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the scope of the present invention is not limited to the specific examples shown below.
[0034] raw material <Synthesis of polyamide MP12> A precisely weighed 60.00 mol of 1,12-dodecanedioic acid was placed in a jacketed reactor equipped with a stirrer, a partial condenser, a cooler, a thermometer, a dropping tank and a nitrogen gas inlet tube, and the mixture was thoroughly replaced with nitrogen. The temperature was then raised to 180°C under a small amount of nitrogen flow to dissolve the 1,12-dodecanedioic acid and make it into a homogeneous fluid state. 60 mol of para / meta-xylylenediamine, in which 40 mol% of the diamine component was para-xylylenediamine and 60 mol% was meta-xylylenediamine, was dropped into the mixture over a period of 160 minutes while stirring. During this time, the internal pressure of the reaction system was kept at normal pressure, and the internal temperature was continuously raised to 250°C. Water distilled with the dropping of para / meta-xylylenediamine was removed from the system through the partial condenser and cooler. After the dropping of para / meta-xylylenediamine was completed, the liquid temperature was kept at 250°C and the reaction was continued for 10 minutes. After that, the pressure inside the reaction system was continuously reduced to 600 Torr over 10 minutes, and the reaction was continued for 20 minutes. During this time, the reaction temperature was continuously raised to 260 ° C. After the reaction was completed, the inside of the reaction vessel was pressurized with nitrogen gas at 0.3 MPa, and the polymer was taken out as a strand from a nozzle at the bottom of the polymerization vessel, and after cooling with water, it was cut into pellets to obtain pellets of a molten polymerized product. The obtained pellets were charged at room temperature into a tumbler (rotary vacuum vessel) having a jacket for heating a heat medium. While rotating the tumbler, the inside of the vessel was reduced in pressure (0.5 to 10 Torr), the circulating heat medium was heated to 190 ° C, and the pellet temperature was raised to 180 ° C and maintained at that temperature for 5 hours. Then, nitrogen was introduced again to return to normal pressure, and cooling was started. When the temperature of the pellets became 70 ° C or less, the pellets were taken out of the vessel, and a solid-phase polymerized product was obtained. The resulting polyamide resin (MP12) had a melting point of 216° C., a glass transition temperature of 57° C., and a relative viscosity of 2.36.
[0035] Polyamide 612: 7034B manufactured by Ube Industries, Ltd. The melting point of polyamide 612 was 205° C., the glass transition temperature was 25° C., and the relative viscosity was 3.86.
[0036] Examples 1 to 4, Comparative Examples 1 and 2 <Filament manufacturing> Polyamide MP12 was melted using a single screw extruder, spun through a spinneret at a spinning temperature of 260°C, taken up in a water bath at 50°C, and continuously stretched without being taken up. The stretching was carried out in two stages and one stage of heat setting, with a 70°C hot water bath in the first stage stretching zone and a 200°C dry air bath in the second stage as the stretching means, and the stretching conditions were a total stretch ratio of 3 to 6, a second stage stretch ratio of 1.0 to 1.5, and a relaxation rate of 5%. A filament was obtained by the above method. The obtained filaments were dried at 40°C for 74 hours (dry state). The dry filaments were immersed in water at 23°C for 336 hours (water absorption treatment). Various evaluations were performed on the dry filaments and the filaments after water absorption treatment. The results are shown in Table 1 below.
[0037] <Fineness> The filament fineness (positive fineness) was measured in a dry state and after water absorption treatment in accordance with the provisions of JIS L 1013:2010. The unit is denier (d).
[0038] <Straight line strength> The linear strength of the filaments in the dry state and after water absorption treatment was measured in accordance with JIS L 1013: 2010. The unit of linear strength is gf / d.
[0039] <Knot strength> The knot strength of the filaments in the dry state and after water absorption treatment was measured according to JIS L 1013: 2010. The unit of knot strength is gf / d.
[0040] <Maintenance rate of linear strength after water absorption treatment and maintenance rate of knot strength after water absorption treatment> The retention rate of linear strength after water absorption treatment is linear strength in dry state x 1 Linear strength X after water absorption treatment 2 Retention rate [(X 2 / X 1 ) × 100]. The knot strength retention rate after water absorption treatment is the knot strength Y 1 Knot strength Y after water absorption treatment 2Retention rate [(Y 2 / Y 1 ) × 100].
[0041] [Table 1]
[0042] As is clear from the above results, the filaments containing polyamide resin (A) had a high retention rate of linear strength and knot strength after the water absorption treatment.
[0043] When the filament obtained in Example 4 was attached to a fishing line as a leader and used, it could be used for sea fishing without any problems.
Claims
1. Contains a polyamide resin (A), The polyamide resin (A) is composed of a diamine-derived structural unit and a dicarboxylic acid-derived structural unit, 70 mol % or more of the diamine-derived constitutional units are derived from xylylenediamine, 70 mol % or more of the dicarboxylic acid-derived constitutional units are derived from an α,ω-linear aliphatic dicarboxylic acid having 11 to 14 carbon atoms, The xylylenediamine contains 10 to 90 mol % of metaxylylenediamine and 90 to 10 mol % of paraxylylenediamine (however, the total of metaxylylenediamine and paraxylylenediamine does not exceed 100 mol %); filament.
2. The filament of claim 1 which is drawn.
3. The filament according to claim 1 or 2, wherein the xylylenediamine contains 40 to 80 mol % of metaxylylenediamine and 60 to 20 mol % of paraxylylenediamine (provided that the sum of metaxylylenediamine and paraxylylenediamine does not exceed 100 mol %).
4. The filament according to claim 1 or 2, wherein the xylylenediamine contains 51 to 75 mol % metaxylylenediamine and 49 to 25 mol % paraxylylenediamine (provided that the sum of metaxylylenediamine and paraxylylenediamine does not exceed 100 mol %).
5. The filament of any one of claims 1 to 4, wherein the dicarboxylic acid comprises 1,12-dodecanedioic acid.
6. The linear strength X of the filament after drying at 40° C. for 74 hours 1 The linear strength X of the filament after immersion in water at 23° C. for 336 hours 2 Retention rate [(X 2 / X 1 6. The filament according to claim 1, wherein the linear strength is a value measured in accordance with JIS L 1013:2010.
7. The knot strength Y of the filament after drying at 40° C. for 74 hours 1 The knot strength Y after immersion of the filament in water at 23° C. for 336 hours 2 Retention rate [(Y 2 / Y 1 ) × 100] is 70 or more, and the knot strength is a value measured in accordance with JIS L 1013:2010. The filament according to any one of claims 1 to 6.
8. A fishing line comprising the filament according to any one of claims 1 to 7.
Citation Information
Patent Citations
Polyamides
GB1129074A
JP1973063050A
Monofilament
JP1993044109A
Polyamide monofilament and its production
JP2000154426A
Xylyene group-containing polyamide resin
JP2003026797A