Microchannel chip and method for manufacturing same

A microchannel chip with cyclic olefin polymer substrates and a thin bonding layer maintains strong bonding and prevents deformation during sterilization, addressing deformation and autofluorescence issues in existing microchannel chips.

JP7593400B2Active Publication Date: 2024-12-03ZEON CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2022526539
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-05-29
Filing Date
2021-05-24
Publication Date
2024-12-03
Estimated Expiration
2041-05-24

AI Technical Summary

Technical Problem

Microchannel chips made of cyclic olefin polymers face deformation during high-temperature, high-pressure sterilization, and conventional bonding methods using adhesive materials cause autofluorescence noise, compromising substrate bonding strength.

Method used

The microchannel chip is constructed with substrates and a bonding layer made of cyclic olefin polymers, where the bonding layer is thin (less than 50 μm) and has a specific glass transition temperature relationship (Tg of channel substrate > Tg of lid substrate > Tg of bonding layer), ensuring strong bonding without deformation during sterilization.

Benefits of technology

The solution maintains substrate integrity and prevents channel deformation during sterilization, while eliminating autofluorescence noise for effective optical signal detection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007593400000002
    Figure 0007593400000002
  • Figure 0007593400000003
    Figure 0007593400000003
  • Figure 0007593400000004
    Figure 0007593400000004
Patent Text Reader

Abstract

The purpose of the present invention is to provide: a microchannel chip in which strong joining performance between substrates is maintained and a channel is not deformed even if high-temperature and high-pressure sterilization treatment is performed; and a method for manufacturing the same. A microchannel chip according to the present invention includes: a channel substrate having at least one surface where a fine channel is formed; a lid substrate; and a joining layer that joins these substrates. The channel substrate, the lid substrate, and the joining layer are each formed from a cyclic olefin polymer. The relationship between the glass transition temperature Tgs1 of the cyclic olefin polymer that constitutes the channel substrate, the glass transition temperature Tgs2 of the cyclic olefin polymer that constitutes the lid substrate, and the glass transition temperature Tg2 of the cyclic olefin polymer forming the joining layer satisfies Tgs1>Tg2 and Tgs2>Tg2. The thickness of the joining layer is in a predetermined range.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a microchannel chip and a method for manufacturing the same. [Background technology]

[0002] In recent years, chips on which minute channels and reaction vessels on the order of micrometers are formed using microfabrication technology (microfluidic chips) have been used in a variety of fields, including the analysis and testing of biological materials such as DNA, RNA, and proteins, drug discovery and development, organic synthesis, and water quality analysis.

[0003] Moreover, as micro-channel chips, attention has been focused on micro-channel chips made of resin, which can be manufactured at low cost.

[0004] Resin microchannel chips are manufactured by interposing a bonding layer between a resin substrate having fine channels formed on at least one surface and a resin cover substrate serving as a lid material, and bonding the two together by heating (see, for example, Patent Documents 1 to 4). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 5948248 [Patent Document 2] JP 2008-304352 A [Patent Document 3] Patent No. 5948248 [Patent Document 4] International Publication No. 2014 / 178439 Summary of the Invention [Problem to be solved by the invention]

[0006] When a microchannel chip is subjected to high-temperature, high-pressure sterilization such as steam sterilization, if the bonding layer is thick, the flow channel may be deformed during the sterilization process. In addition, in a microchannel chip made of a transparent, low-autofluorescence cyclic olefin polymer as the substrate material, an adhesive material other than the cyclic olefin polymer has been used to strengthen the bonding between the substrates, and such a microchannel chip has a problem of noise during optical signal detection due to the autofluorescence of the adhesive material. A microchannel chip in which all components are made of cyclic olefin polymers and in which strong bonding between the substrates is maintained without using an adhesive material such as an autofluorescence material has not been known until now.

[0007] Therefore, an object of the present invention is to provide a microchannel chip in which the channels are not deformed even when subjected to high-temperature, high-pressure sterilization treatment and strong bonding between substrates is maintained even when a cyclic olefin polymer is used as the material for the entire microchannel chip, and a method for manufacturing the same. [Means for solving the problem]

[0008] As a result of intensive research into solving the above problems, the inventors have found that by making the bonding layer a thin film, it is possible to suppress deformation of the flow path due to high-temperature, high-pressure sterilization treatment, and that by using cyclic olefin polymers having a predetermined glass transition temperature relationship as the materials for the substrate and bonding layer, respectively, it is possible to maintain strong bonding between the substrates, thereby completing the present invention. Thus, according to the present invention, there are provided the following microchannel chip and its manufacturing method.

[0009] [1] A microchannel chip including a channel substrate having a fine channel formed on at least one surface thereof, a cover substrate, and a bonding layer bonding the two together, the flow channel substrate, the cover substrate, and the bonding layer are made of a cyclic olefin polymer; Glass transition temperature Tg of cyclic olefin polymer constituting the flow channel substrate s1 The glass transition temperature Tg of the cyclic olefin polymer constituting the cover substrate s2The relationship between the glass transition temperature Tg2 of the cyclic olefin polymer constituting the bonding layer is as follows: Tg s1 >Tg2, and Tg s2 > Tg2, The thickness of the bonding layer is less than 50 μm. Microfluidic chip. [2] Tg s1 and Tg s2 is 125°C or more, and Tg s1 ≧Tg2+10℃, Tg s2 ≧Tg2+10℃ The microchannel chip according to [1] above. [3] The flow path substrate and the cover substrate are joined by thermal fusion via a joining layer. A method for producing the microchannel chip according to [1] or [2] above. [4] forming a bonding layer on at least one of the flow path forming substrate and the cover substrate; A step of forming a flow path in a flow path forming substrate having a bonding layer formed thereon or in a flow path forming substrate having no bonding layer formed thereon to form a flow path substrate having a bonding layer formed thereon or in a flow path substrate having no bonding layer formed thereon; A step of bonding at least one of a combination of a flow path substrate on which a bonding layer is formed and a cover substrate on which a bonding layer is not formed, a combination of a flow path substrate on which a bonding layer is not formed and a cover substrate on which a bonding layer is formed, and a combination of a flow path substrate on which a bonding layer is formed and a cover substrate on which a bonding layer is formed by thermal fusion via the bonding layer. The method for producing the product according to [3] above, [5] forming a flow path substrate having a flow path formed on at least one surface; forming a bonding layer on a portion of at least one of the flow path substrate and the cover substrate other than a portion corresponding to the flow path on at least one surface of the flow path substrate; A step of bonding at least one of a combination of a flow path substrate on which a bonding layer is formed and a cover substrate on which a bonding layer is not formed, a combination of a flow path substrate on which a bonding layer is not formed and a cover substrate on which a bonding layer is formed, and a combination of a flow path substrate on which a bonding layer is formed and a cover substrate on which a bonding layer is formed by thermal fusion via the bonding layer. The method for producing the product according to [3] above, Effect of the Invention

[0010] According to the present invention, it is possible to provide a microchannel chip in which the channels are not deformed even when subjected to high-temperature, high-pressure sterilization treatment and strong bonding between the substrates is maintained, and a method for manufacturing the same. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a conceptual diagram of a method for producing a microchannel chip of the present invention, in which a channel is formed after the formation of an adhesive layer. [Diagram 2] FIG. 2 is a conceptual diagram of a method for producing a micro-channel chip of the present invention, in which a bonding layer is formed after the formation of a channel substrate on which a channel is formed. [Diagram 3] FIG. 3(a) is a plan view showing an example of a channel substrate of a micro-channel chip, and FIG. 3(b) is a plan view showing an example of a cover substrate of the micro-channel chip. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, an embodiment of the present invention will be described in detail.

[0013] (Microfluidic Chip) The micro-channel chip of the present invention includes a channel substrate s1 having a fine channel formed on at least one surface thereof, a cover substrate s2, and a bonding layer that bonds them together. The flow channel substrate s1, the cover substrate s2, and the bonding layer are made of a cyclic olefin polymer, Glass transition temperature Tg of cyclic olefin polymer constituting the flow channel substrate s1The glass transition temperature Tg of the cyclic olefin polymer constituting the cover substrate s2 The relationship between the glass transition temperature Tg2 of the cyclic olefin polymer constituting the bonding layer is as follows: Tg s1 >Tg2, and Tg s2 > Tg2, The thickness of the bonding layer is less than 50μ.

[0014] <Flow channel substrate> The flow channel substrate may be a substrate made of a cyclic olefin polymer having fine flow channels formed on at least one surface thereof, and the flow channel substrate is bonded to a cover substrate with the surface on which the fine flow channels are formed serving as a bonding surface.

[0015] Here, the width, depth and shape of the fine channel can be appropriately changed depending on the application of the microchannel chip, but is usually on the order of millimeters or less, may be on the order of nanometers, and is preferably on the order of micrometers. Specifically, the width of the fine channel is not particularly limited, and can be, for example, 10 μm or more and 800 μm or less.

[0016] The formation of a fine flow path in a substrate made of a cyclic olefin polymer can be carried out, for example, by using a microfabrication technique such as photolithography or thermal imprinting, cutting, injection molding, or the like. The formation of a flow path may be carried out on a flow path forming substrate on which no bonding layer is formed, or on a flow path forming substrate on which a bonding layer has been formed. The formation of a flow path in a flow path forming substrate on which no bonding layer is formed can be carried out, for example, by using a microfabrication technique such as photolithography or thermal imprinting, cutting, injection molding, or the like. The formation of a flow path in a flow path forming substrate on which a bonding layer has been formed can be carried out, for example, by applying a microfabrication technique such as photolithography or thermal imprinting, cutting, or the like to the surface on which the bonding layer of the flow path forming substrate is formed.

[0017] <Lid substrate> The cover substrate may be any substrate made of a cyclic olefin polymer capable of covering the fine flow paths formed in the flow path substrate. Specifically, the cover substrate may be a substrate having a smooth surface capable of covering the flow path substrate, and optionally having a through hole that serves as an inlet for injecting a sample or the like into the fine flow paths of the flow path substrate when the substrate is used to form a micro-flow path chip together with the flow path substrate. The cover substrate is bonded to the flow path substrate with the smooth surface side serving as the bonding surface. The cover substrate may be a substrate having a fine flow path formed on the surface opposite to the smooth surface side bonded to the flow path substrate.

[0018] The formation of through holes in a substrate made of a cyclic olefin polymer can be carried out, for example, by using microfabrication techniques such as photolithography and thermal imprinting, cutting, injection molding, etc. The formation of through holes can be carried out in a substrate for forming a flow path on which no bonding layer is formed, or in a substrate for forming a flow path on which a bonding layer has been formed. The formation of through holes in a substrate for forming a flow path on which no bonding layer is formed can be carried out, for example, by using microfabrication techniques such as photolithography and thermal imprinting, cutting, injection molding, etc. The formation of through holes in a substrate for forming a flow path on which a bonding layer has been formed can be carried out, for example, by applying microfabrication techniques such as photolithography and thermal imprinting, cutting, etc. to the surface of the substrate for forming a flow path on which the bonding layer has been formed.

[0019] <Joining layer> The bonding layer is a member formed on the flow path substrate or the cover substrate, and serves to bond the flow path substrate and the cover substrate together. The thickness of the bonding layer is less than 50 μm, preferably 40 μm or less, more preferably 10 μm or less, and even more preferably 5 μm or less. The thinner the bonding layer, the thinner the bonding layer becomes, so that deformation of the channel during steam sterilization of the microchannel chip is suppressed. The thickness of the bonding layer may be the minimum thickness that can ensure adhesion between the channel substrate and the cover substrate, and may be, for example, 0.1 μm or more, preferably 0.12 μm or more, more preferably 0.15 μm or more, and even more preferably 0.2 μm or more. The ratio of the thickness of the bonding layer to the depth of the flow channel may be, for example, 0.1 / 100 or more, preferably 0.12 / 100 or more, more preferably 0.15 / 100 or more, and even more preferably 0.2 / 100 or more. The ratio of the thickness of the bonding layer to the depth of the flow channel may be, for example, 50 / 100 or less, preferably 30 / 100 or less, more preferably 20 / 100 or less, and even more preferably 10 / 100 or less.

[0020] <Materials for flow channel substrate, cover substrate, and bonding layer> A cyclic olefin polymer is used as the material for the flow channel substrate, the cover substrate, and the bonding layer. The cyclic olefin polymer is suitable for a micro-channel chip having excellent durability because the bonding strength and the optical stability are not decreased over time due to moisture absorption. In addition, the cyclic olefin polymer is a transparent and low autofluorescent material, and is therefore suitable for detecting optical signals from the fine flow channels of the micro-channel chip. By using cyclic olefin polymers as all the materials of the micro-channel chip and not using adhesive materials such as autofluorescent materials, noise during optical signal detection due to autofluorescence from adhesive materials can be suppressed. The cyclic olefin polymer used as the material for the flow channel substrate, the cover substrate, and the bonding layer satisfies the glass transition temperature relationship described below. By satisfying such a glass transition temperature relationship, even if all the materials of the micro-channel chip are cyclic olefin polymers, strong bonding between the substrates can be maintained. The type of cyclic olefin polymer used as the material for the flow channel substrate, the cover substrate, and the bonding layer may be appropriately selected from the specific examples described below, for example, one that satisfies the glass transition temperature relationship. The cyclic olefin polymer used as the material for the flow channel substrate, the cover substrate, and the bonding layer is preferably a cyclic olefin polymer having a water absorption rate of 0.01% by mass or less. The types of cyclic olefin polymers used as materials for the flow channel substrate and the cover substrate may be the same or different.

[0021] <<Glass transition temperature of cyclic olefin polymers>> The glass transition temperature Tg of the cyclic olefin polymer that is the material of the flow channel substrate s1 s1 , the glass transition temperature Tg of the cyclic olefin polymer which is the material of the cover substrate s2s2 and the glass transition temperature Tg2 of the cyclic olefin polymer that is the material of the bonding layer satisfies the following relationship. Tg s1 >Tg2, and Tg s2 >Tg2. By satisfying the above relationship, in the manufacture of a microchannel chip, the channel substrate and the cover substrate are bonded at a temperature higher than Tg2 and lower than Tg s1 and Tg s2 If the bonding is performed at a lower temperature, it is possible to soften only the bonding layer without softening, deforming or altering the flow channel substrate and the cover substrate, and bonding by thermal fusion becomes possible.

[0022] Tg s1 is preferably 125°C or higher, more preferably 130°C or higher. s1 When Tg is in this range, softening, deformation, and deterioration of the channel substrate due to heating during production and sterilization of the microchannel chip (e.g., autoclaving) can be suppressed. s1 is preferably 180° C. or less, more preferably 160° C. or less. s1 The difference between Tg and Tg2 is 10°C or more (i.e., Tg s1 ≧Tg2+10° C.), and preferably 15° C. or higher (i.e., Tg s1 ≧Tg2+15° C.), more preferably 20° C. or higher (i.e., Tg s1 ≧Tg2+20° C. is more preferable. s1 The larger the difference between Tg and Tg2, the easier it is to set the heating temperature in the manufacture of microchannel chips in order to soften only the bonding layer without softening, deforming, or altering the channel substrate. s1 The difference between Tg and Tg2 is preferably 100° C. or less, more preferably 90° C. or less, and even more preferably 80° C. or less. s1 The smaller the difference between Tg1 and Tg2, the better the temperature stability of the bonding layer.

[0023] Tg s2 is preferably 125°C or higher, more preferably 130°C or higher. s2When Tg is in this range, softening, deformation, and deterioration of the cover substrate due to heating during production and sterilization of the microchannel chip (e.g., autoclaving) can be suppressed. s2 is preferably 180° C. or less, more preferably 160° C. or less. s2 The difference between Tg and Tg2 is 10°C or more (i.e., Tg s2 ≧Tg2+10° C.), and preferably 15° C. or higher (i.e., Tg s2 ≧Tg2+15° C.), more preferably 20° C. or higher (i.e., Tg s2 ≧Tg2+20° C. is more preferable. s2 The larger the difference between Tg and Tg2, the easier it is to set the heating temperature in the manufacture of microchannel chips in order to soften only the bonding layer without softening, deforming, or altering the cover substrate. s2 The difference between Tg and Tg2 is preferably 100° C. or less, more preferably 90° C. or less, and even more preferably 80° C. or less. s2 The smaller the difference between Tg1 and Tg2, the better the temperature stability of the bonding layer.

[0024] Tg2 is preferably 50° C. or higher, and more preferably 65° C. or higher. When Tg2 is in this range, the temperature stability of the bonding layer is good. Furthermore, Tg2 is preferably 130° C. or lower, more preferably 110° C. or lower, and even more preferably 100° C. or lower. When Tg2 is in this range, it becomes easy to set the heating temperature for softening only the bonding layer in the manufacture of the microchannel chip.

[0025] In the present invention, the glass transition temperature can be measured by differential scanning calorimetry (DSC) based on JIS-K7121.

[0026] <<Types of cyclic olefin polymers>> The cyclic olefin polymer is, for example, a polymer or copolymer (hereinafter, sometimes collectively referred to as "polymer") obtained by polymerizing monomers as described below, or a hydrogenated product thereof. The cyclic olefin polymer may be crystalline or amorphous, but is preferably amorphous. Preferred examples of the monomer for the cyclic olefin polymer include norbornene-based monomers. The norbornene-based monomer is a monomer containing a norbornene ring. Examples of the norbornene-based monomer include bicyclic monomers such as bicyclo[2.2.1]hept-2-ene (common name: norbornene), 5-ethylidene-bicyclo[2.2.1]hept-2-ene (common name: ethylidenenorbornene), and derivatives thereof (those having a substituent on the ring); tricyclo[5.2.1.0 2,6 ]Deca-3,8-diene (common name: dicyclopentadiene) and its derivatives, etc.; tetracyclo[7.4.0.0 2,7 .1 10,13 ]Tetradeca-2,4,6,11-tetraene (common name: methanotetrahydrofluorene), tetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-4-ene (common name: tetracyclododecene), 9-ethylidenetetracyclo[6.2.1.1 3,6 .0 2,7 ]dodec-4-ene, and tetracyclic monomers such as their derivatives; and the like. These monomers may have a substituent at any position. Examples of the substituent include an alkyl group, an alkylene group, a vinyl group, an alkoxycarbonyl group, and an alkylidene group, and the above norbornene monomers may have two or more of these. Specific examples of the derivatives include 8-methoxycarbonyl-tetracyclo[4.4.0.1 2,5 .1 7,10 ]dodec-3-ene, 8-methyl-8-methoxycarbonyl-tetracyclo[4.4.0.1 2,5 .1 7,10 ]dodec-3-ene, 8-ethylidene-tetracyclo[4.4.0.1 2,5 .1 7,10]dodec-3-ene and the like. These norbornene-based monomers may be used alone or in combination of two or more. The cyclic olefin polymer may be an addition polymer, a ring-opening polymer, or a hydrogenated product thereof, but is preferably a ring-opening polymer or a ring-opening polymer hydrogenated product. The cyclic olefin polymer used as the material for the substrate (channel substrate, cover substrate) is preferably a polymer obtained by polymerizing a monomer having a methanotetrahydrofluorene (MTF) content of 25 parts by weight or more per 100 parts by weight of the total monomers. The cyclic olefin polymer used as the material for the bonding layer is preferably a polymer obtained by polymerizing a monomer having a dicyclopentadiene (DCPD) content of 30 parts by weight or more per 100 parts by weight of the total monomers.

[0027] The ring-opening polymer can be produced by a method using a ring-opening polymerization catalyst. As the ring-opening polymerization catalyst, for example, a catalyst consisting of a halide of a metal such as ruthenium or osmium, a nitrate or an acetylacetone compound, and a reducing agent, or a catalyst consisting of a halide or an acetylacetone compound of a metal such as titanium, zirconium, tungsten, or molybdenum, and an organoaluminum compound can be used. The ring-opening polymer can be produced by a method using a metathesis reaction catalyst (ring-opening polymerization catalyst) such as a ruthenium carbene complex catalyst described in International Publication No. 2010 / 110323, and a method using a ring-opening polymerization catalyst such as a tungsten(phenylimide)tetrachloride-tetrahydrofuran complex or tungsten hexachloride described in Japanese Patent Application Laid-Open No. 2015-54885, and the like. The above-mentioned addition polymer can be obtained by polymerizing a monomer using a known addition polymerization catalyst, for example, a catalyst consisting of a titanium, zirconium or vanadium compound and an organoaluminum compound. The addition polymer can be produced, for example, by addition copolymerizing a monomer of a cyclic olefin polymer and, if necessary, a monomer capable of addition copolymerization (another monomer) in the presence of a metallocene catalyst described in International Publication No. 2017 / 199980.

[0028] Examples of other monomers capable of undergoing ring-opening copolymerization with norbornene monomers include monocyclic olefin monomers such as cyclohexene, cycloheptene, and cyclooctene. These norbornene-based monomers and other monomers capable of ring-opening copolymerization can be used alone or in combination of two or more. When a norbornene-based monomer and other monomers capable of ring-opening copolymerization with it are ring-opening copolymerized, the ratio of the structural unit derived from the norbornene-based monomer to the structural unit derived from the other monomers capable of ring-opening copolymerization in the ring-opening polymer is appropriately selected so as to be usually in the range of 70:30 to 99:1, preferably 80:20 to 99:1, more preferably 90:10 to 99:1 by weight ratio.

[0029] Examples of other monomers capable of addition copolymerization with norbornene-based monomers include α-olefins having 2 to 20 carbon atoms, such as ethylene, propylene, 1-butene, 1-pentene, and 1-hexene, and derivatives thereof; cycloolefins, such as cyclobutene, cyclopentene, cyclohexene, cyclooctene, and 3a,5,6,7a-tetrahydro-4,7-methano-1H-indene, and derivatives thereof; and non-conjugated dienes, such as 1,4-hexadiene, 4-methyl-1,4-hexadiene, 5-methyl-1,4-hexadiene, and 1,7-octadiene. Among these, α-olefins are preferred, and ethylene is particularly preferred. These other monomers capable of addition copolymerization with norbornene-based monomers can be used alone or in combination of two or more. When a norbornene-based monomer and another monomer capable of addition copolymerization with it are addition copolymerized, the ratio of the structural unit derived from the norbornene-based monomer to the structural unit derived from the other monomer capable of addition copolymerization in the addition polymer is appropriately selected so as to be usually in the range of 30:70 to 99:1, preferably 50:50 to 97:3, more preferably 70:30 to 95:5 by weight ratio.

[0030] Furthermore, examples of the method for producing a hydrogenated ring-opening polymer containing an alicyclic structure by hydrogenating a ring-opening polymer include a method using a hydrogenation catalyst described in International Publication No. 2010 / 110323. In addition, for example, after producing an alicyclic structure-containing polymer using the above-mentioned ruthenium carbene complex catalyst as a ring-opening polymerization catalyst, the ruthenium carbene catalyst can be used as a hydrogenation catalyst as it is to hydrogenate the alicyclic structure-containing ring-opening polymer to produce a hydrogenated ring-opening polymer containing an alicyclic structure.

[0031] The glass transition temperature (Tg) of the cyclic olefin polymer can be appropriately adjusted depending on the type and blending ratio of the monomers used in the polymerization, the average molecular weight and molecular weight distribution of the polymer, and the like.

[0032] In the micro-channel chip of the present invention, at least one of the channel substrate, the cover substrate, and the bonding layer may be composed of two or more layers having different Tg's.

[0033] (Method of manufacturing a microchannel chip) The microchannel chip of the present invention can be produced, for example, by the production method described below (hereinafter referred to as the "production method of the present invention").

[0034] The manufacturing method of the present invention includes bonding the flow path substrate and the cover substrate via a bonding layer by thermal fusion.

[0035] In one embodiment, the manufacturing method of the present invention may be carried out in the order of forming a bonding layer on the entire surface of a substrate and then forming a flow path on the substrate. That is, the manufacturing method of the present invention may be carried out in the following steps. (1) forming a bonding layer on at least one of a flow path forming substrate and a cover substrate; (2) A step of forming a flow path on a flow path forming substrate on which a bonding layer is formed or on which a bonding layer is not formed, for example, by cutting, photolithography, or thermal imprinting to form a flow path substrate on which a bonding layer is formed or on which a bonding layer is not formed; (3) A process of bonding at least one of a combination of a flow path substrate having a bonding layer formed thereon and a lid substrate having no bonding layer formed thereon, a combination of a flow path substrate having no bonding layer formed thereon and a lid substrate having a bonding layer formed thereon, and a combination of a flow path substrate having a bonding layer formed thereon and a lid substrate having a bonding layer formed thereon by thermal fusion via the bonding layer. An example of a conceptual diagram of the manufacturing method according to this embodiment is shown in FIG.

[0036] In this embodiment, the bonding layer may be formed by applying a solution of the cyclic olefin polymer, which is the material of the bonding layer, to the entire surface of the substrate in a thin film form and evaporating the solvent. Examples of the solvent include organic solvents such as cyclohexane, tetrahydrofuran, toluene, xylene, decalin, methylcyclohexane, and ethylcyclohexane, and may be used as a mixed solvent. The evaporation of the solvent may be performed, for example, by drying at a temperature lower than the glass transition temperature of the cyclic olefin polymer, which is the material of the bonding layer (e.g., heat drying, room temperature drying), heating and vacuum (reduced pressure) drying, or a combination of these.

[0037] In addition, in this embodiment, when a flow path is formed in a flow path forming substrate on which a bonding layer is formed, the surface of the flow path forming substrate on which the bonding layer is formed is processed by, for example, cutting, photolithography, thermal imprinting, or the like, and the flow path forming portion of the flow path forming substrate is removed together with the bonding layer.

[0038] In another embodiment, the manufacturing method of the present invention may be carried out in the following order: after preparing a substrate (channel substrate) on which a channel is formed, a bonding layer is formed on a portion of the surface of the substrate (channel substrate, lid substrate) other than the portion corresponding to the channel. That is, the manufacturing method of the present invention may be carried out in the following steps. (1) forming a flow path substrate having a flow path formed on at least one surface thereof; (2) forming a bonding layer on a portion of at least one of the flow path substrate and the cover substrate other than the portion corresponding to the flow path on at least one surface of the flow path substrate; (3) A process of bonding at least one of a combination of a flow path substrate having a bonding layer formed thereon and a lid substrate having no bonding layer formed thereon, a combination of a flow path substrate having no bonding layer formed thereon and a lid substrate having a bonding layer formed thereon, and a combination of a flow path substrate having a bonding layer formed thereon and a lid substrate having a bonding layer formed thereon by thermal fusion via the bonding layer. An example of a conceptual diagram of the manufacturing method according to this embodiment is shown in FIG.

[0039] In this embodiment, the flow path substrate having a flow path formed on at least one surface thereof may be formed, for example, by injection molding a cyclic olefin polymer that is the material of the substrate, or may be formed on a flow path forming substrate by, for example, microfabrication techniques such as photolithography and thermal imprinting, or by cutting.

[0040] In this embodiment, the bonding layer may be formed by applying a solution of a cyclic olefin polymer, which is the material of the bonding layer, in a pattern by screen printing on the parts of the substrate other than the parts corresponding to the flow paths, or by spray coating after masking the parts corresponding to the flow paths on the substrate, and then evaporating the solvent.

[0041] From the viewpoint of ease of manufacture, the manufacturing method of the present invention is preferably carried out in an embodiment that involves forming a bonding layer on the entire surface of the substrate.

[0042] The thermal fusion is performed by overlapping the flow path substrate and the cover substrate with a bonding layer interposed therebetween to form a temporary bonded assembly, and then heating the temporary bonded assembly to a temperature higher than Tg2 and Tg s1 and Tg s2 Heating is performed at a lower temperature. Examples of means for performing heat fusion include an autoclave, a heat press, and a roll press. The temperature for performing heat fusion is preferably Tg2+5°C or higher, more preferably Tg2+10°C or higher. The temperature for performing heat fusion is preferably Tg2+50°C or lower, more preferably Tg2+40°C or lower. Before performing heat fusion, it is preferable to remove trapped air from the temporarily bonded bonded body and perform pressure bonding, but since a small amount of air bubbles will diffuse during autoclave processing, there is no problem as long as large air bubbles are not trapped.

[0043] In the production method of the present invention, at least one of the flow path substrate, the lid substrate, and the bonding layer may be composed of two or more layers having different Tg values.

Example

[0044] Hereinafter, the present invention will be specifically described based on examples, but the present invention is not limited to these examples.

[0045] <Measurement and Evaluation Methods of Physical Properties> The measurement and evaluation of various physical properties were carried out according to the following methods.

[0046] (Measurement Method of Weight-Average Molecular Weight Mw) The weight-average molecular weight Mw was measured by gel permeation chromatography (GPC) using cyclohexane as an eluent and determined as a standard polyisoprene conversion value. As the standard polyisoprene, standard polyisoprene manufactured by Tosoh Corporation was used. When the sample was insoluble in cyclohexane, it was measured by GPC using tetrahydrofuran (THF) as an eluent and determined as a standard polystyrene conversion value. As the standard polystyrene, standard polystyrene manufactured by Tosoh Corporation was used.

[0047] (Measurement Method of Glass Transition Temperature) The glass transition temperature (Tg) was measured using a differential scanning calorimeter (manufactured by Nanotechnology Co., Ltd., product name: DSC6220SII) under the condition of a heating rate of 10 °C / min based on JIS-K7121.

[0048] [1-1. Production of Cyclic Olefin Polymer (COP)] <Production of COP-1> (1-1-1) Production of Ring-Opening Polymer: In a glass reaction vessel with the inside replaced with nitrogen, 200 parts by weight of dehydrated cyclohexane, 0.75 mol% of 1-hexene, 0.15 mol% of diisopropyl ether, and 0.44 mol% of triisobutylaluminum were placed in the reactor at room temperature relative to a total of 100 parts by weight of the monomers described below, and mixed. Thereafter, while maintaining the temperature at 45°C, 28 parts by weight of methanotetrahydrofluorene (MTF), 35 parts by weight of tetracyclododecene (TCD), and 37 parts by weight of dicyclopentadiene (DCPD), as monomers, and 0.02 mol% of tungsten hexachloride (0.65 wt% toluene solution) were continuously added in parallel to the reactor over a period of 2 hours, and polymerization was performed. Next, 0.2 mol% of isopropyl alcohol was added to the polymerization solution to inactivate the polymerization catalyst, and the polymerization reaction was stopped. In the above explanation, the amount indicated by the unit "mol%" is a value in which the total amount of the monomers is 100 mol%. The weight-average molecular weight Mw of the resulting norbornene ring-opening polymer was 2.8×10 4 The molecular weight distribution (Mw / Mn) was 2.1, and the conversion rate of monomer to polymer was 100%.

[0049] (1-1-2) Preparation of norbornene-based cyclic olefin polymer (COP-1) by hydrogenation: Next, 300 parts by weight of the reaction solution containing the ring-opened polymer obtained in the above step (1-1-1) was transferred to an autoclave equipped with a stirrer, and 3 parts by weight of a diatomaceous earth supported nickel catalyst ("T8400RL" manufactured by JGC Chemical Industries, Ltd., nickel loading rate 57%) was added, followed by autoclaving at a hydrogen pressure of 4.5 MPa and 160°C for 4 hours to carry out a hydrogenation reaction.

[0050] After the hydrogenation reaction, the obtained solution was pressure-filtered at a pressure of 0.25 MPa using Radiolite #500 as a filter bed (a "Hundaback Filter" manufactured by Ishikawajima-Harima Heavy Industries Co., Ltd.) to remove the hydrogenation catalyst and obtain a colorless and transparent solution. The obtained solution was poured into a large amount of isopropanol to precipitate a norbornene-based cyclic olefin polymer (COP-1) as a hydride of the ring-opening polymer. After filtering the precipitated norbornene-based cyclic olefin polymer (COP-1), it was dried in a vacuum dryer (220 °C, 1 Torr) for 6 hours to obtain a norbornene-based cyclic olefin polymer (COP-1). The weight average molecular weight of the norbornene-based cyclic olefin polymer (COP-1) was 3.5×10 4 , and the molecular weight distribution Mw / Mn was 2.3.

[0051] The glass transition temperature Tg of the obtained norbornene-based cyclic olefin polymer (COP-1) was 134 °C.

[0052] (1-1-3) Production of thermoplastic norbornene resin: The norbornene-based cyclic olefin polymer (COP-1) obtained in the above step (1-1-2) was charged into a twin-screw extruder and formed into a strand-shaped molded body by hot melt extrusion molding. This molded body was shredded using a strand cutter to obtain pellets of a thermoplastic norbornene resin containing the norbornene-based cyclic olefin polymer (COP-1).

[0053] <Production of COP-2> Except that 33 parts by weight of tetracyclododecene (TCD), 33 parts by weight of dicyclopentadiene (DCPD), and 34 parts by weight of norbornene (NB) were used as monomers, in the same manner as the production of COP-1, a norbornene-based cyclic olefin polymer (COP-2) and pellets of a thermoplastic norbornene resin containing COP-2 were obtained. The glass transition temperature Tg of COP-2 was 70 °C.

[0054] <Production of COP-3> Except that 22 parts by weight of tetracyclododecene (TCD), 73 parts by weight of dicyclopentadiene (DCPD), and 5 parts by weight of norbornene (NB) were used as monomers, pellets of a norbornene-based cyclic olefin polymer (COP-3) and a thermoplastic norbornene-based resin containing COP-3 were obtained in the same manner as the production of COP-1. The glass transition temperature Tg of COP-3 was 104 °C.

[0055] <Production of COP-4> Except that 8 parts by weight of methanotetrahydrofluorene (MTF), 36 parts by weight of tetracyclododecene (TCD), and 56 parts by weight of dicyclopentadiene (DCPD) were used as monomers, pellets of a norbornene-based cyclic olefin polymer (COP-4) and a thermoplastic norbornene-based resin containing COP-4 were obtained in the same manner as the production of COP-1. The glass transition temperature Tg of COP-4 was 124 °C.

[0056] <Production of COP-5> Except that 40 parts by weight of methanotetrahydrofluorene (MTF), 56 parts by weight of tetracyclododecene (TCD), and 4 parts by weight of dicyclopentadiene (DCPD) were used as monomers, pellets of a norbornene-based cyclic olefin polymer (COP-5) and a thermoplastic norbornene-based resin containing COP-5 were obtained in the same manner as the production of COP-1. The glass transition temperature Tg of COP-5 was 156 °C.

[0057] [1-2. Production of cyclic olefin copolymer (COC)] To a reaction vessel charged with 258 liters of cyclohexane, bicyclo[2.2.1]hept-2-ene (hereinafter referred to as "NB") (120 kg) was added under normal temperature and a nitrogen stream, and stirring was carried out for 5 minutes. Further, triisobutylaluminum was added so that the concentration in the system became 1.0 mL / liter. Subsequently, ethylene was circulated at normal pressure while stirring to make the inside of the system an ethylene atmosphere. The internal temperature of the autoclave was maintained at 70 °C, and the internal pressure was 6 kg / cm with gauge pressure by ethylene 2After stirring for 10 minutes, 0.4 liters of a toluene solution containing isopropylidene(cyclopentadienyl)(indenyl)zirconium dichloride and methylalumoxane was added to the system to initiate the copolymerization reaction of ethylene and NB. The catalyst concentrations at this time were 0.018 mmol / liter of isopropylidene(cyclopentadienyl)(indenyl)zirconium dichloride and 8.0 mmol / liter of methylalumoxane relative to the total system.

[0058] During polymerization, ethylene was continuously fed into the system to maintain the temperature at 70°C and the internal pressure at 6 kg / cm (gauge pressure). 2 After 60 minutes, the polymerization reaction was stopped by adding isopropyl alcohol. After depressurization, the polymer solution was taken out and then added with 1 ml of water. 3 The mixture was allowed to stand, and the aqueous phase was separated and removed, and then washed twice with water to separate the polymerized liquid phase.

[0059] Next, the purified and separated polymer solution was contacted with three times the amount of acetone under strong stirring to precipitate the copolymer, and the solid portion (copolymer) was collected by filtration and thoroughly washed with acetone. Furthermore, in order to extract the unreacted monomers present in the polymer, this solid portion was filtered and thoroughly washed with acetone at 40 kg / m 3 After being poured into acetone so that the mixture became a solid, extraction was performed at 60°C for 2 hours. After the extraction process, the solid portion was collected by filtration and dried for 12 hours at 130°C and 350 mmHg under a nitrogen flow to obtain an ethylene-NB copolymer (cyclic olefin copolymer: COC). 100 parts by weight of the obtained ethylene-NB copolymer (COC) and 0.1 parts by weight of an antioxidant (Irganox (registered trademark) 1010) were kneaded in a twin-screw kneader to obtain pellets of a thermoplastic norbornene-based resin containing ethylene-NB copolymer (COC).

[0060] The Tg of the ethylene-NB copolymer (COC) obtained in this manner was 137°C, and the NB unit content was 51 mol%.

[0061] [2. Manufacturing of circuit boards] In Examples 1 to 10 and Comparative Examples 1 and 2, the cyclic olefin polymer or cyclic olefin copolymer for substrate shown in Table 1 (pellets of thermoplastic norbornene resin: COP-1, COP-5, or COC) was dried for 5 hours at Tg-20° C. Then, the pellets were injection molded by a conventional method using an injection molding machine (FANUC ROBOSHOT (registered trademark) α100B, manufactured by FANUC CORPORATION) at a resin temperature of Tg+150° C., a mold temperature of Tg-10° C., and a holding pressure of 80 MPa to obtain substrates (flow path forming substrate and cover substrate) as molded products of flat plates of 100 mm×100 mm×2 mm.

[0062] [3. Formation of bonding layer on substrate] (3-1. Formation of bonding layer in Examples 1 to 8 and Comparative Examples 1 and 2) 20 parts by weight of pellets of the thermoplastic norbornene-based resin for the bonding layer (COP-2, COP-3, COP-4, or COP-1) shown in Table 1 and 80 parts by weight of cyclohexane (special grade: manufactured by Wako Pure Chemical Industries) were sealed in a glass airtight container (Pyrex (registered trademark) medium bottle: manufactured by Corning) and shaken to dissolve at room temperature to prepare a cyclohexane solution (solution for the bonding layer) with a solid concentration of 20% by weight. The obtained bonding layer solution was cast onto the flat plate 100mm x 100mm x 2mm molded product (channel forming substrate: COP-1 or COC) obtained above, and wet coating was performed using a small automatic film applicator (manufactured by Allgood Co., Ltd.). The coated flat plate molded product was dried at room temperature for about 10 minutes, and then heated and dried in an oven at 80°C for 1 hour to obtain a molded product coated with a bonding layer (channel forming substrate with a bonding layer formed thereon).

[0063] (3-2. Formation of bonding layer in Example 9) 20 parts by weight of pellets of the thermoplastic norbornene-based resin for the bonding layer (COP-2) shown in Table 1 and 80 parts by weight of xylene (special grade: manufactured by Wako Pure Chemical Industries) were sealed in a glass airtight container (Pyrex (registered trademark) medium bottle: manufactured by Corning), and the mixture was shaken at room temperature to dissolve, creating a xylene solution (solution for the bonding layer) with a solids concentration of 20% by weight. The obtained bonding layer solution was cast onto the flat plate 100mm x 100mm x 2mm molded product (channel forming substrate: COP-1) obtained above, and wet coating was performed using a small automatic film applicator (manufactured by Allgood Co., Ltd.). The coated flat plate molded product was dried at room temperature for about 10 minutes, and then heated and dried in an oven at 120°C for 5 minutes to obtain a molded product coated with a bonding layer (channel forming substrate with a bonding layer formed thereon).

[0064] (3-3. Formation of bonding layer in Example 10) 20 parts by weight of pellets of the thermoplastic norbornene-based resin for the bonding layer (COP-3) shown in Table 1 and 80 parts by weight of cyclohexane (special grade: manufactured by Wako Pure Chemical Industries) were sealed in a glass airtight container (Pyrex (registered trademark) medium bottle: manufactured by Corning), and the mixture was shaken at room temperature to dissolve, thereby preparing a cyclohexane solution (solution for the bonding layer) with a solid concentration of 20% by weight. The obtained bonding layer solution was cast onto the flat plate 100mm x 100mm x 2mm molded product (channel forming substrate: COP-5) obtained above, and wet coating was performed using a small automatic film applicator (manufactured by Allgood Co., Ltd.). The coated flat plate molded product was dried at room temperature for about 10 minutes, and then heated and dried in an oven at 80°C for 5 minutes to obtain a molded product coated with a bonding layer (channel forming substrate with a bonding layer formed thereon).

[0065] [4. Cutting the channel in the substrate] The molded product coated with the bonding layer (a flow path forming substrate with a bonding layer formed thereon) was subjected to flow path cutting and external shape processing using an ultra-high precision, high speed micromachining machine Android II (manufactured by Rokuroku Sangyo Co., Ltd.) to obtain a flow path substrate 10 with a bonding layer formed thereon (thickness: 2.0 mm, external dimensions: 76.0 mm × 26.0 mm) having four flow paths 11 (width: 100 μm, depth: 100 μm) on one side in the pattern as shown in Figure 3(a). 3(b), eight through holes 21 (injection ports) having a diameter of 2.0 mm were formed in the cover substrate obtained in [2. Manufacturing of Substrate] above, and the cover substrate 20 (thickness: 2.0 mm, outer dimensions: 76.0 mm × 26.0 mm) was obtained by external processing. The positions of the through holes 21 were set to correspond to the ends 12 of the flow paths 11 of the flow path substrate 10.

[0066] [5. Bonding substrates together] After the flow channel substrate and the cover substrate on which the bonding layer was formed were overlapped, they were pressed several times with a rubber roll to remove trapped air and to perform pressure bonding to prepare a temporarily bonded bonded body A. Since a small amount of air bubbles will disperse during autoclave processing, there is no problem as long as no large amount of air is trapped. The temporarily bonded bonded body A was inserted into a retort pouch bag (manufactured by Meiwa Pax) and degassed and packaged using a vacuum packaging machine (TECHNOVAC T1000; manufactured by Nippon Packaging Machinery). This degassed package was placed in an autoclave container (Tandelion DL-2010; manufactured by Hanyuda Iron Works) and autoclaved at the temperature shown in Table 1, 0.8 MPa, and a heating and pressurizing time of 90 minutes to perform bonding and defoaming treatment, and a microflow chip was obtained as a bonded body.

[0067] [6. Evaluation] <Adhesive strength> The adhesive strength was measured in accordance with JIS K 6854-2 (180° peel). A 10 mm wide cut was made on the sheet (lid substrate) side of the bonded body, penetrating the sheet and the adhesive layer, as shown in Figure 3. The 10 mm wide cut was exposed from the edge so that it could be fixed with a chuck, and the molding plate (flow path substrate) side was fixed to the lower chuck of a universal testing machine with oven (Autograph AGS-X10kN; Shimadzu Corporation), and the sheet side was fixed to the upper chuck, and the bonded body was held at room temperature for 5 minutes. After holding, a 180° peel was performed with a peel width of 10 mm and a peel speed of 100 mm / min to determine the peel strength, which was taken as the adhesive strength.

[0068] <Liquid transfer test> For five samples, the ink solution was injected from the injection port into each channel of the fabricated microchannel chip using a pressure-controlled non-pulsating pump P-Pump (manufactured by Takasago Electric Co., Ltd.). The outlet side was sealed with silicone rubber, and the liquid delivery pressure was increased to 650 kPa and maintained for three minutes. Then, the presence or absence of bleeding of the ink solution from the channel to the joint was visually confirmed.

[0069] <Observation of joint cross section, measurement of joint layer thickness> The resulting bonded body (microchannel chip) was cross-sectioned in cryo-milling mode using an ion milling device IM4000PLUS (Hitachi High-Tech Corporation). The cross-section was observed with a field emission scanning electron microscope FE-SEM8220 (Hitachi High-Tech Corporation), and the thickness of the bonded layer was measured.

[0070] <Evaluation of flow path cross section before and after steam sterilization> (Steam sterilization) The resulting assembly (microchannel chip) was steam sterilized using a small high-pressure steam sterilizer under the conditions of 121°C, 0.12 MPa, and 30 min.

[0071] (Flow path cross-section evaluation) The cross-sectional area S1 before steam sterilization and the area S2 after steam sterilization were measured using a field emission scanning electron microscope FE-SEM8220 (Hitachi High-Technologies Corporation). The flow channel shape retention rate was calculated as S2 / S1×100(%).

[0072] [7. Results] The types of cyclic olefin polymers used in the substrates (channel substrate and cover substrate) and bonding layer, the glass transition temperatures Tg, the thicknesses of the bonding layers, and the evaluation results are shown in Table 1. The evaluation symbols have the following meanings. <Liquid transfer test> 〇: No leakage ×: Leaking <Evaluation of flow path cross section after steam sterilization> Flow channel shape retention rate ◎: 95% or more ○: 90% or more but less than 95% △: 80% or more but less than 90% ×: Less than 80%

[0073] [Table 1] [Industrial Applicability]

[0074] According to the present invention, it is possible to provide a microchannel chip in which the channels are not deformed even when subjected to high-temperature, high-pressure sterilization treatment and strong bonding between the substrates is maintained, and a method for manufacturing the same. [Explanation of symbols]

[0075] 10 Flow channel substrate 11 Flow Path 12 Both ends 20 Lid substrate 21 Through hole

Claims

1. A microchannel chip including a channel substrate having a fine channel formed on at least one surface thereof, a cover substrate, and a bonding layer bonding the two together, the flow channel substrate, the cover substrate, and the bonding layer are made of a cyclic olefin polymer; Glass transition temperature Tg of the cyclic olefin polymer constituting the flow channel substrate s1 , the glass transition temperature Tg of the cyclic olefin polymer constituting the cover substrate s2 The glass transition temperature Tg of the cyclic olefin polymer constituting the bonding layer 2 The relationship is as follows: Tg s1 >Tg 2 ,and Tg s2 >Tg 2 and The thickness of the bonding layer is less than 50 μm. Microfluidic chip.

2. Tg s1 and Tg s2 is 125° C. or more, and Tg s1 ≧Tg 2 +10℃、 Tg s2 ≧Tg 2 +10℃ The microchannel chip according to claim 1 ,

3. and bonding the flow path substrate and the cover substrate by thermal fusion via a bonding layer. A method for producing the microchannel chip according to claim 1 or 2.

4. forming a bonding layer on at least one of the flow path forming substrate and the cover substrate; A step of forming a flow path in a flow path forming substrate having a bonding layer formed thereon or in a flow path forming substrate having no bonding layer formed thereon to form a flow path substrate having a bonding layer formed thereon or in a flow path substrate having no bonding layer formed thereon; A step of bonding at least one of a combination of a flow path substrate on which a bonding layer is formed and a cover substrate on which a bonding layer is not formed, a combination of a flow path substrate on which a bonding layer is not formed and a cover substrate on which a bonding layer is formed, and a combination of a flow path substrate on which a bonding layer is formed and a cover substrate on which a bonding layer is formed by thermal fusion via the bonding layer. The method of claim 3, comprising:

5. A step of forming a flow path substrate having a flow path formed on at least one surface thereof; forming a bonding layer on a portion of at least one of the flow path substrate and the cover substrate other than a portion corresponding to the flow path on at least one surface of the flow path substrate; A step of bonding at least one of a combination of a flow path substrate on which a bonding layer is formed and a cover substrate on which a bonding layer is not formed, a combination of a flow path substrate on which a bonding layer is not formed and a cover substrate on which a bonding layer is formed, and a combination of a flow path substrate on which a bonding layer is formed and a cover substrate on which a bonding layer is formed by thermal fusion via the bonding layer. The method of claim 3, comprising:

Citation Information

Patent Citations

  • Attaching structure of radiator grill

    JP1984048248A

  • Channel device and method for bonding channel device-use board

    JP2008304352A

  • Method of joining microchip substrate

    JP2012066518A

  • Filter for capturing target substance

    JP2013217918A

  • Method and apparatus for producing resinous micro-flow path device

    JP2015199340A