Resin composition

A resin composition with a maleimide compound and vinylphenyl or (meth)acryloyl groups addresses high viscosity and dielectric loss issues, enhancing copper plating peel strength and dielectric properties in printed wiring boards.

JP7593411B2Active Publication Date: 2024-12-03AJINOMOTO CO INC
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2022562210
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-11-12
Filing Date
2021-11-12
Publication Date
2024-12-03
Estimated Expiration
2041-11-12

AI Technical Summary

Technical Problem

Existing resin compositions for printed wiring boards face challenges with high minimum melt viscosity and high dielectric loss tangent (Df), compromising copper plating peel strength and dielectric properties.

Method used

Incorporating a maleimide compound with an isopropylidene group bonded to two aromatic carbon atoms and a resin with vinylphenyl or (meth)acryloyl groups to formulate a resin composition that suppresses minimum melt viscosity and reduces dielectric loss tangent (Df) while enhancing copper plating peel strength.

Benefits of technology

The resin composition achieves lower minimum melt viscosity, lower dielectric loss tangent (Df), and improved copper plating peel strength, resulting in better dielectric properties for printed wiring boards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007593411000001
    Figure 0007593411000001
  • Figure 0007593411000002
    Figure 0007593411000002
  • Figure 0007593411000003
    Figure 0007593411000003
Patent Text Reader

Abstract

The present invention addresses the problem of providing a resin composition such that the minimum melt viscosity can be further reduced, the dielectric loss factor (Df) is low, and a cured article having a superior copper plating peel strength can be obtained, and provides a resin composition containing (A) a maleimide compound that has a isopropylidene group bonded to two aromatic carbon atoms in different aromatic rings, and (B) a resin having a vinyl phenyl group and / or a (meth)acryloyl group.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition containing a maleimide compound, and further to a cured product, a sheet-like laminate material, a resin sheet, a printed wiring board, and a semiconductor device obtained by using the resin composition. [Background technology]

[0002] A known manufacturing technique for printed wiring boards is the build-up method, in which insulating layers and conductor layers are alternately stacked. In the build-up method, the insulating layer is generally formed by curing a resin composition. In recent years, there has been a demand for further improvement in the dielectric properties of the insulating layer, such as the dielectric constant, and further improvement in the copper adhesion. However, up to now, when a material with high copper plating peel strength is used, there have been problems with the high minimum melt viscosity of the resin composition and the high dielectric loss tangent (Df) of the material.

[0003] So far, maleimide compounds containing an isopropylidene group have been known (Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 6752390 Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present invention is to provide a resin composition which can reduce the minimum melt viscosity and give a cured product having a low dielectric tangent (Df) and excellent copper plating peel strength. [Means for solving the problem]

[0006] Means for Solving the Problems of the Invention The present inventors conducted intensive research in order to achieve the objects of the present invention and unexpectedly found that by using, as components of a resin composition, (A) a maleimide compound having an isopropylidene group bonded to two aromatic carbon atoms of different aromatic rings, and (B) a resin having a vinylphenyl group and / or a (meth)acryloyl group, it is possible to reduce the minimum melt viscosity of the resin composition and obtain a cured product having a low dielectric tangent (Df) and excellent copper plating peel strength, thereby completing the present invention.

[0007] That is, the present invention includes the following. [1] A resin composition comprising (A) a maleimide compound having an isopropylidene group bonded to two aromatic carbon atoms of different aromatic rings, and (B) a resin having a vinylphenyl group and / or a (meth)acryloyl group. [2] The component (A) is represented by the formula (A2):

[0008] [ka]

[0009] [In the formula, ring A and ring B each independently represent an aromatic ring which may have a substituent; and a represents an integer of 1 or more.] The resin composition according to the above [1], comprising a maleimide compound represented by the following formula: [3] The component (A) is represented by the formula (A-1):

[0010] [ka]

[0011] [In the formula, R 1 and R 2 each independently represents an alkyl group or an aryl group; a represents an integer of 1 or more; and x and y each independently represent 0, 1, 2, or 3. The resin composition according to the above [1] or [2], comprising a maleimide compound represented by the following formula: [4] The resin composition according to the above [2] or [3], wherein a is an integer of 2 to 10. [5] The resin composition according to any one of the above [1] to [4], wherein the component (B) is a thermoplastic resin having a vinylphenyl group and / or a (meth)acryloyl group. [6] The resin composition according to any one of the above [1] to [5], wherein the component (B) is a resin selected from a modified polyphenylene ether resin having a vinylphenyl group and / or a (meth)acryloyl group, and a modified polystyrene resin having a vinylphenyl group and / or a (meth)acryloyl group. [7] The resin composition according to any one of the above [1] to [6], wherein the content of the component (A) is 5% by mass to 30% by mass, based on 100% by mass of the non-volatile components in the resin composition. [8] The resin composition according to any one of the above [1] to [7], wherein the content of the component (B) is 5% by mass to 40% by mass, based on 100% by mass of the non-volatile components in the resin composition. [9] The resin composition according to any one of the above [1] to [8], wherein a mass ratio of the component (A) to the component (B) (component (A) / component (B)) is 0.3 to 3.

[10] The resin composition according to any one of the above [1] to [9], further comprising (C) an inorganic filler.

[11] The resin composition according to

[10] above, wherein the content of the component (C) is 40 mass% or more, based on 100 mass% of the non-volatile components in the resin composition.

[12] The resin composition according to the above

[10] or

[11] , wherein a mass ratio of the component (A) to the component (C) (component (A) / component (C)) is 0.1 to 1.

[13] The resin composition according to any one of the above [1] to

[12] , wherein a dielectric loss tangent (Df) of a cured product of the resin composition is 0.004 or less when measured at 5.8 GHz and 23°C.

[14] The resin composition according to any one of the above [1] to

[13] , wherein a cured product of the resin composition has a relative dielectric constant (Dk) of 3.5 or less when measured at 5.8 GHz and 23°C.

[15] A cured product of the resin composition according to any one of [1] to

[14] above.

[16] A sheet-like laminate material comprising the resin composition according to any one of [1] to

[14] above.

[17] A resin sheet comprising: a support; and a resin composition layer formed on the support, the resin composition being formed from the resin composition according to any one of [1] to

[14] above.

[18] A printed wiring board comprising an insulating layer made of a cured product of the resin composition according to any one of [1] to

[14] above.

[19] A semiconductor device comprising the printed wiring board according to

[18] above. Effect of the Invention

[0012] According to the resin composition of the present invention, the minimum melt viscosity can be reduced, and a cured product having a low dielectric loss tangent (Df) and excellent copper plating peel strength can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The present invention will be described in detail below with reference to preferred embodiments. However, the present invention is not limited to the following embodiments and examples, and can be modified and implemented as desired without departing from the scope of the claims of the present invention and their equivalents.

[0014] <Resin composition> The resin composition of the present invention contains (A) a maleimide compound having an isopropylidene group bonded to two aromatic carbon atoms of different aromatic rings (hereinafter sometimes referred to as a "specific maleimide compound"), and (B) a resin having a vinylphenyl group and / or a (meth)acryloyl group. By using such a resin composition, it is possible to further reduce the minimum melt viscosity and obtain a cured product having a low dielectric loss tangent (Df) and excellent copper plating peel strength.

[0015] The resin composition of the present invention may further contain optional components in addition to (A) the specific maleimide compound and (B) the resin having a vinylphenyl group and / or a (meth)acryloyl group. Examples of the optional components include (A') other maleimide compounds, (C) inorganic fillers, (D) radical polymerization initiators, (E) thermoplastic resins, (F) elastomers, (G) other additives, and (H) organic solvents. Each component contained in the resin composition will be described in detail below.

[0016] <(A) Specific Maleimide Compound> The resin composition of the present invention contains (A) a specific maleimide compound. The (A) specific maleimide compound may be used alone or in combination of two or more kinds in any ratio.

[0017] The maleimide compound means a compound having at least one maleimide group (2,5-dihydro-2,5-dioxo-1H-pyrrol-1-yl group) in one molecule. The maleimide group in the (A) specific maleimide compound may be bonded to an aromatic carbon atom or an aliphatic carbon atom, but preferably includes one bonded to an aromatic carbon atom, and more preferably, all of the maleimide groups in the (A) specific maleimide compound are bonded to aromatic carbon atoms. The number of maleimide groups in one molecule of the (A) specific maleimide compound is preferably 2 or more, more preferably 3 or more, more preferably 3 to 11, and even more preferably 3 to 6.

[0018] The (A) specific maleimide compound has at least one isopropylidene group (-C(CH3)2-) bonded to two aromatic carbon atoms of different aromatic rings in one molecule. The isopropylidene group contained in the (A) specific maleimide compound may be any of an isopropylidene group bonded to two aromatic carbon atoms, which is a combination of an aromatic carbon atom in an aromatic ring having a maleimide group and an aromatic carbon atom in an aromatic ring not having a maleimide group, an isopropylidene group bonded to an aromatic carbon atom in a different aromatic ring having a maleimide group, and an isopropylidene group bonded to an aromatic carbon atom in a different aromatic ring not having a maleimide group. The (A) specific maleimide compound preferably has an isopropylidene group bonded to two aromatic carbon atoms, which are a combination of an aromatic carbon atom in an aromatic ring having a maleimide group and an aromatic carbon atom in an aromatic ring not having a maleimide group, and particularly preferably, all of the isopropylidene groups contained in the (A) specific maleimide compound are isopropylidene groups bonded to two aromatic carbon atoms, which are a combination of an aromatic carbon atom in an aromatic ring having a maleimide group and an aromatic carbon atom in an aromatic ring not having a maleimide group. The number of such isopropylidene groups in one molecule of the (A) specific maleimide compound is preferably 2 or more, more preferably 4 or more, further preferably 4 to 20, and particularly preferably 4 to 10.

[0019] The aromatic ring means a ring conforming to the Huckel rule in which the number of electrons contained in the π electron system on the ring is 4p+2 (p is a natural number). The aromatic ring may be an aromatic carbocycle having a carbon atom as a ring-constituting atom, or an aromatic heterocycle having a heteroatom such as an oxygen atom, a nitrogen atom, or a sulfur atom in addition to a carbon atom as a ring-constituting atom, but in one embodiment, it is preferably an aromatic carbocycle. In one embodiment, the aromatic ring is preferably a 5-14-membered aromatic ring, more preferably a 5-10-membered aromatic ring, and even more preferably a 5- or 6-membered aromatic ring. Suitable specific examples of the aromatic ring include a benzene ring, a naphthalene ring, an anthracene ring, a phenanthrene ring, and the like, more preferably a benzene ring or a naphthalene ring, and particularly preferably a benzene ring.

[0020] (A) In one embodiment, the specific maleimide compound is preferably represented by formula (A1):

[0021] [ka]

[0022] [In the formula, ring A, ring B and ring C each independently represent an aromatic ring which may have a substituent; each X independently represents a single bond, -C(R x )2-, -O-, -CO-, -S-, -SO-, -SO2-, -CONH-, or -NHCO-; R x each independently represents a hydrogen atom, an alkyl group which may have a substituent, or an aryl group which may have a substituent; a represents an integer of 1 or more; b represents 0 or 1; and c represents 0, 1, 2, or 3. The maleimide compound includes a maleimide compound represented by the following formula: The a units and the c units may be the same or different for each unit.

[0023] Ring A, ring B and ring C each independently represent an aromatic ring which may have a substituent, preferably an aromatic carbocycle which may have a substituent, more preferably a benzene ring which may have a substituent or a naphthalene ring which may have a substituent, even more preferably a benzene ring which may be substituted with a group selected from an alkyl group and an aryl group, or a naphthalene ring which may be substituted with a group selected from an alkyl group and an aryl group, and particularly preferably a benzene ring which may be substituted with a group selected from an alkyl group and an aryl group.

[0024] In the present specification, the term "substituent" is not particularly limited, and examples thereof include monovalent substituents such as an alkyl group, an alkenyl group, an aryl group, an aryl-alkyl group, an alkyl-oxy group, an alkenyl-oxy group, an aryl-oxy group, an alkyl-carbonyl group, an alkenyl-carbonyl group, an aryl-carbonyl group, an alkyl-oxy-carbonyl group, an alkenyl-oxy-carbonyl group, an aryl-oxy-carbonyl group, an alkyl-carbonyl-oxy group, an alkenyl-carbonyl-oxy group, and an aryl-carbonyl-oxy group, and may also include divalent substituents such as an oxo group (=O) if substitutable.

[0025] The alkyl group means a linear, branched and / or cyclic monovalent aliphatic saturated hydrocarbon group. The alkyl group is preferably an alkyl group having 1 to 14 carbon atoms, unless otherwise specified. Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, a cyclopentyl group, a cyclohexyl group, a methylcyclohexyl group, a dimethylcyclohexyl group, a trimethylcyclohexyl group, a cyclopentylmethyl group, and a cyclohexylmethyl group. The alkenyl group means a linear, branched and / or cyclic monovalent aliphatic unsaturated hydrocarbon group having at least one carbon-carbon double bond. The alkenyl group is preferably an alkenyl group having 2 to 14 carbon atoms, unless otherwise specified. Examples of the alkenyl group include vinyl, propenyl, butenyl, pentenyl, hexenyl, heptenyl, octenyl, nonenyl, decenyl, and cyclohexenyl groups. The aryl group means a monovalent aromatic hydrocarbon group. Unless otherwise specified, the aryl group is preferably an aryl group having 6 to 14 carbon atoms. Examples of the aryl group include a phenyl group, a 1-naphthyl group, and a 2-naphthyl group.

[0026] Each X is independently a single bond, -C(R x)2-, -O-, -CO-, -S-, -SO-, -SO2-, -CONH-, or -NHCO-, and preferably a single bond, -C(R x )2- or -O-, more preferably a single bond or -C(R x )2-, and particularly preferably a single bond. x each independently represents a hydrogen atom, an alkyl group which may have a substituent, or an aryl group which may have a substituent, more preferably a hydrogen atom, an alkyl group, or an aryl group, and even more preferably a hydrogen atom or an alkyl group.

[0027] a represents an integer of 1 or more, preferably 2 or more, more preferably an integer of 2 to 10, and even more preferably 2, 3, 4, or 5. In one embodiment, the (A) specific maleimide compound contains a maleimide compound represented by formula (A1) in which a is 1, and a maleimide compound represented by formula (A1) in which a is 2 or more, and preferably contains 1 mass %, more preferably 5 mass %, further preferably 8 mass %, and particularly preferably 10 mass % of the maleimide compound represented by formula (A1) in which a is 2 or more.

[0028] Each b independently represents 0 or 1, and preferably represents 1. Each c independently represents 0, 1, 2, or 3, and preferably represents 0, 1, or 2, more preferably represents 0 or 1, and particularly preferably represents 0.

[0029] In one embodiment, the specific maleimide compound (A) is more preferably represented by formula (A2):

[0030] [ka]

[0031] [In the formula, each symbol is as defined above.] The maleimide compound represented by the formula:

[0032] In another embodiment, the specific maleimide compound (A) is more preferably represented by the formulae (A-1) to (A-6):

[0033] [ka]

[0034] [In the formula, R 1 and R 2 each independently represents an alkyl group or an aryl group; x and y each independently represent 0, 1, 2, or 3; and other symbols are as defined above. In one embodiment, the maleimide compound is preferably a compound represented by formula (A-1), and in one embodiment, the maleimide compound is preferably a compound represented by formula (A-1a) or (A-1b):

[0035] [ka]

[0036] [In the formula, each symbol is the same as above.] In one embodiment, the compound represented by formula (A-1a) is particularly preferred.

[0037] R 1 and R 2 each independently represents an alkyl group or an aryl group, and is preferably an alkyl group. x and y each independently represent 0, 1, 2, or 3, and are preferably 0, 1, or 2, more preferably 0 or 1, and particularly preferably 0.

[0038] The weight average molecular weight (Mw) of the (A) specific maleimide compound is preferably 500 to 5000, more preferably 500 to 4000, and even more preferably 500 to 3000. The number average molecular weight (Mn) of the (A) specific maleimide compound is preferably 500 to 5000, more preferably 500 to 4000, and even more preferably 500 to 3000. The weight average molecular weight and number average molecular weight of the resin can be measured as polystyrene-equivalent values ​​by gel permeation chromatography (GPC).

[0039] The maleimide equivalent of the (A) specific maleimide compound is preferably 100 g / eq. to 1000 g / eq., more preferably 150 g / eq. to 400 g / eq. The maleimide equivalent of the (A) specific maleimide compound is the mass of the (A) specific maleimide compound per equivalent of maleimide group.

[0040] An example of a commercially available product of the (A) specific maleimide compound is "MIR-5000-60T" manufactured by Nippon Kayaku Co., Ltd.

[0041] The content of the (A) specific maleimide compound in the resin composition is not particularly limited, but is preferably 50% by mass or less, more preferably 40% by mass or less, even more preferably 30% by mass or less, even more preferably 25% by mass or less, and particularly preferably 20% by mass or less, when the non-volatile components in the resin composition are taken as 100% by mass. The lower limit of the content of the (A) specific maleimide compound in the resin composition is not particularly limited, but is preferably 0.1% by mass or more, more preferably 1% by mass or more, even more preferably 5% by mass or more, even more preferably 8% by mass or more, and particularly preferably 10% by mass or more, when the non-volatile components in the resin composition are taken as 100% by mass.

[0042] <(A') Other maleimide compounds> The resin composition of the present invention may further contain, as an optional component, (A') a maleimide compound other than the component (A). The (A') other maleimide compound may be used alone or in any combination of two or more kinds.

[0043] (A') Other maleimide compounds are not particularly limited, and may be either aliphatic maleimide compounds containing an aliphatic amine skeleton or aromatic maleimide compounds containing an aromatic amine skeleton. Commercially available products include, for example, "SLK-2600" manufactured by Shin-Etsu Chemical Co., Ltd., "BMI-1500", "BMI-1700", "BMI-3000J", "BMI-689", and "BMI-2500" (maleimide compounds containing a dimer diamine structure) manufactured by Designer Molecules, Inc., "BMI-6100" (aromatic maleimide compound) manufactured by Designer Molecules, and "MIR-3000-70MT" (biphenylaralkyl type maleimide compound) manufactured by Nippon Kayaku Co., Ltd. In addition, as (A') other maleimide compounds, the maleimide resin (maleimide compound containing an indane ring skeleton) disclosed in the Japan Institute of Invention and Innovation Disclosure Technical Journal No. 2020-500211 may be used.

[0044] The maleimide equivalent of the (A') other maleimide compound is preferably 100 g / eq. to 20,000 g / eq., more preferably 200 g / eq. to 15,000 g / eq., and even more preferably 300 g / eq. to 10,000 g / eq. The maleimide equivalent of the (A') other maleimide compound is the mass of the (A') other maleimide compound per equivalent of maleimide group.

[0045] The weight average molecular weight (Mw) of the (A') other maleimide compound is preferably 500 to 50,000, more preferably 700 to 20,000. The number average molecular weight (Mn) of the (A') other maleimide compound is preferably 500 to 50,000, more preferably 700 to 20,000.

[0046] The content of the (A') other maleimide compound in the resin composition is not particularly limited, but is preferably 50% by mass or less, more preferably 40% by mass or less, even more preferably 30% by mass or less, even more preferably 20% by mass or less, and particularly preferably 10% by mass or less, when the non-volatile components in the resin composition are taken as 100% by mass. The lower limit of the content of the (A') other maleimide compound in the resin composition is not particularly limited, but may be, for example, 0% by mass or more, 0.1% by mass or more, 1% by mass or more, 2% by mass or more, etc., when the non-volatile components in the resin composition are taken as 100% by mass.

[0047] The content of the specific maleimide compound (A) in the resin composition is preferably 10% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, and particularly preferably 50% by mass or more, when the total amount of the maleimide compounds in the resin composition (the sum of the components (A) and (A')) is taken as 100% by mass.

[0048] <(B) Resin Having a Vinylphenyl Group and / or a (Meth)acryloyl Group> The resin composition of the present invention contains (B) a resin having a vinylphenyl group and / or a (meth)acryloyl group. The (meth)acryloyl group means an acryloyl group or a methacryloyl group. The vinylphenyl group includes a 2-vinylphenyl group, a 3-vinylphenyl group, a 4-vinylphenyl group, or groups in which the aromatic carbon atom of these groups is further substituted with one or more alkyl groups. The component (B) is usually a resin having two or more vinylphenyl groups and / or (meth)acryloyl groups in one molecule.

[0049] The component (B) may be used alone or in any combination of two or more kinds in any ratio. In one embodiment, each molecule of the component (B) may react with other molecules of the component (B), or with molecules of the component (A) or (A').

[0050] The (B) component is preferably a thermoplastic resin having a vinylphenyl group and / or a (meth)acryloyl group. Examples of the thermoplastic resin include phenoxy resin, polyvinyl acetal resin, polystyrene resin, polyethylene resin, polypropylene resin, polybutadiene resin, polyimide resin, polyamideimide resin, polyetherimide resin, polysulfone resin, polyethersulfone resin, polyphenylene ether resin, polycarbonate resin, polyetheretherketone resin, and polyester resin. The (B) component may be a modified resin having a vinylphenyl group and / or a (meth)acryloyl group of these resins.

[0051] The (B) component is more preferably a resin selected from a modified polyphenylene ether resin having a vinylphenyl group and / or a (meth)acryloyl group (hereinafter may be abbreviated as "modified polyphenylene ether resin") and a modified polystyrene resin having a vinylphenyl group and / or a (meth)acryloyl group (hereinafter may be abbreviated as "modified polystyrene resin").

[0052] The modified polyphenylene ether resin is preferably represented by the formula (B-1):

[0053] [ka]

[0054] [In the formula, R 11 and R 12 each independently represents an alkyl group; R 13 , R 14 , R 21 , R 22 , R 23 and R 24 each independently represents a hydrogen atom or an alkyl group; R 31 and R 32 each independently represents a vinylphenyl group or a (meth)acryloyl group; Y represents a single bond, -C(R y )2-, -O-, -CO-, -S-, -SO-, or -SO2-; R yeach independently represents a hydrogen atom or an alkyl group; Z represents a single bond or an alkylene group; n and m each independently represent an integer of 1 or more; and p represents 0 or 1. The resin is represented by the formula: The n units and m units may be the same or different for each unit.

[0055] R 11 and R 12 R each independently represents an alkyl group, and is preferably a methyl group. 13 and R 14 R each independently represents a hydrogen atom or an alkyl group, and is preferably a hydrogen atom. 21 and R 22 R each independently represents a hydrogen atom or an alkyl group, preferably a hydrogen atom or a methyl group, and more preferably a methyl group. 23 and R 24 each independently represents a hydrogen atom or an alkyl group, preferably a hydrogen atom or a methyl group, and more preferably R 23 and R 24 One of these is a methyl group and the other is a hydrogen atom.

[0056] R 31 and R 32 are each independently a vinylphenyl group or a (meth)acryloyl group, and Z is a single bond or an alkylene group. The alkylene group means a linear, branched or cyclic divalent saturated hydrocarbon group. The alkylene group is preferably an alkylene group having 1 to 6 carbon atoms. Examples of the alkylene group include -CH2-, -CH2-CH2-, -CH(CH3)-, -CH2-CH2-CH2-, -CH2-CH(CH3)-, -CH(CH3)-CH2-, -C(CH3)2-, and the like. Preferably, R 31 and R 32 is a vinylphenyl group and Z is an alkylene group (particularly preferably -CH-), or R 31 and R 32 is a (meth)acryloyl group and Z is a single bond.

[0057] Y is a single bond, -C(R y )2-, -O-, -CO-, -S-, -SO-, or -SO2-, and preferably a single bond, -C(R y )2-, or -O-, and more preferably a single bond. y each independently represents a hydrogen atom or an alkyl group, and is preferably a hydrogen atom or a methyl group. n and m each independently represent an integer of 1 or more, and is preferably an integer of 1 to 200, and more preferably an integer of 1 to 100. p represents 0 or 1, and is preferably 1.

[0058] Commercially available modified polyphenylene ether resins include, for example, "OPE-2St 1200" and "OPE-2St 2200" (vinylbenzyl-modified polyphenylene ether resins) manufactured by Mitsubishi Gas Chemical Company, Inc.; and "SA9000" and "SA9000-111" (methacrylic-modified polyphenylene ether resins) manufactured by SABIC Innovative Plastics.

[0059] The modified polystyrene resin is preferably represented by the formula (B-2a):

[0060] [ka]

[0061] [In the formula, R 41 , R 42 and R 43 each independently represents a hydrogen atom or an alkyl group; R 44 each independently represents an alkyl group; and s represents an integer of 0 to 3. and a repeating unit represented by formula (B-2b):

[0062] [ka]

[0063] [In the formula, R 51 , R52 and R 53 each independently represents a hydrogen atom or an alkyl group; R 54 each independently represents an alkyl group; and t represents an integer of 0 to 3. The repeating unit of formula (B-2a) and the repeating unit of formula (B-2b) may be the same or different units.

[0064] R 41 , R 42 , R 43 , R 51 , R 52 and R 53 R each independently represents a hydrogen atom or an alkyl group, preferably a hydrogen atom or a methyl group, and more preferably a hydrogen atom. 44 and R 54 each independently represents an alkyl group, and is preferably an ethyl group or a methyl group. s represents an integer of 0 to 3, and is preferably 0 or 1, and is more preferably 0. t represents an integer of 0 to 3, and is preferably 0 or 1.

[0065] The molar content of the repeating unit of formula (B-2a) is preferably 8 mol % to 54 mol % when the total of the repeating units of formula (B-2a) and formula (B-2b) is taken as 100 mol %.

[0066] Commercially available modified polystyrene resins include, for example, "ODV-XET(X03)", "ODV-XET(X04)", and "ODV-XET(X05)" (styrene-divinylbenzene copolymers) manufactured by Nippon Steel Chemical & Material Co., Ltd.

[0067] The functional group equivalent of the component (B) is preferably 250 g / eq. to 2500 g / eq., more preferably 300 g / eq. to 1500 g / eq. The functional group equivalent of the component (B) represents the mass of the resin per equivalent of a vinylphenyl group or a (meth)acryloyl group.

[0068] The weight average molecular weight (Mw) of the component (B) is preferably 1000 to 40000, more preferably 1000 to 10000, and particularly preferably 1000 to 5000. The number average molecular weight (Mn) of the component (B) is preferably 1000 to 40000, more preferably 1000 to 10000, and particularly preferably 1000 to 5000. The weight average molecular weight and number average molecular weight of the resin can be measured as polystyrene-equivalent values ​​by gel permeation chromatography (GPC).

[0069] The content of the (B) component in the resin composition is not particularly limited, but is preferably 60% by mass or less, more preferably 50% by mass or less, even more preferably 40% by mass or less, even more preferably 30% by mass or less, and particularly preferably 25% by mass or less, when the non-volatile components in the resin composition are taken as 100% by mass. The lower limit of the content of the (B) component in the resin composition is not particularly limited, but is preferably 0.1% by mass or more, more preferably 1% by mass or more, even more preferably 5% by mass or more, even more preferably 10% by mass or more, and particularly preferably 15% by mass or more, when the non-volatile components in the resin composition are taken as 100% by mass.

[0070] The mass ratio of the specific maleimide compound (A) to the component (B) in the resin composition (component (A) / component (B)) is preferably 0.1 or more, more preferably 0.3 or more, and particularly preferably 0.5 or more. The upper limit of the mass ratio of the specific maleimide compound (A) to the component (B) in the resin composition (component (A) / component (B)) is preferably 5 or less, more preferably 3 or less, and particularly preferably 1.5 or less.

[0071] <(C) Inorganic filler> The resin composition of the present invention may contain an inorganic filler (C) as an optional component. The inorganic filler (C) is contained in the resin composition in the form of particles.

[0072] (C) An inorganic compound is used as the material of the inorganic filler. (C) Examples of the material of the inorganic filler include silica, alumina, aluminosilicate, glass, cordierite, silicon oxide, barium sulfate, barium carbonate, talc, clay, mica powder, zinc oxide, hydrotalcite, boehmite, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, magnesium oxide, boron nitride, aluminum nitride, manganese nitride, aluminum borate, strontium carbonate, strontium titanate, calcium titanate, magnesium titanate, bismuth titanate, titanium oxide, zirconium oxide, barium titanate, barium zirconate titanate, barium zirconate, calcium zirconate, zirconium phosphate, and zirconium tungstate phosphate. Among these, silica or aluminosilicate is preferred, and silica is particularly preferred. Examples of silica include amorphous silica, fused silica, crystalline silica, synthetic silica, and hollow silica. In addition, spherical silica is preferred as the silica. The (C) inorganic filler may be used alone or in combination of two or more kinds in any ratio.

[0073] Examples of commercially available (C) inorganic fillers include "UFP-30" manufactured by Denka Chemical Industry Co., Ltd.; "SP60-05" and "SP507-05" manufactured by Nippon Steel Chemical & Material Co., Ltd.; "YC100C", "YA050C", "YA050C-MJE", and "YA010C" manufactured by Admatechs Co., Ltd.; "UFP-30" manufactured by Denka Company; "Silfill NSS-3N", "Silfill NSS-4N", and "Silfill NSS-5N" manufactured by Tokuyama Corporation; "SC2500SQ", "SO-C4", "SO-C2", and "SO-C1" manufactured by Admatechs Co., Ltd.; "DAW-03" and "FB-105FD" manufactured by Denka Company; "BA-S" manufactured by JGC Catalysts and Chemicals Co., Ltd.; and "MG-005" manufactured by Taiheiyo Cement Corporation.

[0074] The average particle size of the (C) inorganic filler is not particularly limited, but is preferably 10 μm or less, more preferably 5 μm or less, even more preferably 2 μm or less, even more preferably 1 μm or less, and particularly preferably 0.7 μm or less. The lower limit of the average particle size of the (C) inorganic filler is not particularly limited, but is preferably 0.01 μm or more, more preferably 0.05 μm or more, even more preferably 0.1 μm or more, and particularly preferably 0.2 μm or more. The average particle size of the (C) inorganic filler can be measured by a laser diffraction / scattering method based on the Mie scattering theory. Specifically, the particle size distribution of the inorganic filler is created on a volume basis using a laser diffraction / scattering type particle size distribution measuring device, and the median diameter is taken as the average particle size. The measurement sample can be prepared by weighing 100 mg of the inorganic filler and 10 g of methyl ethyl ketone into a vial and dispersing it by ultrasonic waves for 10 minutes. The measurement sample was measured using a laser diffraction type particle size distribution measuring device with blue and red light source wavelengths, and the particle size distribution of the inorganic filler on a volume basis was measured using a flow cell method, and the average particle size was calculated as the median diameter from the particle size distribution obtained. An example of a laser diffraction type particle size distribution measuring device is the "LA-960" manufactured by Horiba, Ltd.

[0075] The specific surface area of ​​the (C) inorganic filler is not particularly limited, but is preferably 0.1 m 2 / g or more, more preferably 0.5m 2 / g or more, more preferably 1m 2 / g or more, particularly preferably 3m 2 The upper limit of the specific surface area of ​​the inorganic filler (C) is not particularly limited, but is preferably 100 m 2 / g or less, more preferably 70m 2 / g or less, more preferably 50m 2 / g or less, particularly preferably 40m 2 The specific surface area of ​​the inorganic filler is obtained by adsorbing nitrogen gas onto the surface of the sample using a specific surface area measuring device (Macsorb HM-1210 manufactured by Mountec Co., Ltd.) according to the BET method, and calculating the specific surface area using the BET multipoint method.

[0076] The (C) inorganic filler may be a non-hollow inorganic filler with a porosity of 0 volume % (preferably non-hollow silica, non-hollow aluminosilicate), a hollow inorganic filler with a porosity of more than 0 volume % (preferably hollow silica, hollow aluminosilicate), or may contain both. From the viewpoint of lowering the dielectric constant, the (C) inorganic filler preferably contains only a hollow inorganic filler (preferably hollow silica, hollow aluminosilicate), or contains both a non-hollow inorganic filler (preferably non-hollow silica, non-hollow aluminosilicate) and a hollow inorganic filler (preferably hollow silica, hollow aluminosilicate). The porosity of the hollow inorganic filler is preferably 90 volume % or less, more preferably 85 volume % or less. (C) The lower limit of the porosity of the inorganic filler is not particularly limited, but may be, for example, more than 0 volume %, 1 volume % or more, 5 volume % or more, 10 volume % or more, 20 volume % or more, 30 volume % or more, etc. The porosity P (volume %) of the inorganic filler is defined as the volume-based ratio of the total volume of one or more voids present inside the particle to the total volume of the particle based on the outer surface of the particle (total volume of voids / volume of particle), and is, for example, the measured value D of the actual density of the inorganic filler. M (g / cm 3 ), and the theoretical value of the material density of the material forming the inorganic filler D T (g / cm 3 ) is used to calculate according to the following formula (I).

[0077]

number

[0078] The actual density of the inorganic filler can be measured, for example, by using a true density measuring device. Examples of the true density measuring device include ULTRAPYCNOMETER 1000 manufactured by QUANTACHROME Co., Ltd. As the measurement gas, for example, nitrogen is used.

[0079] The inorganic filler (C) is preferably surface-treated with an appropriate surface treatment agent, which can enhance the moisture resistance and dispersibility of the inorganic filler (C). Examples of the surface treatment agent include vinyl-based silane coupling agents such as vinyltrimethoxysilane and vinyltriethoxysilane; epoxy-based silane coupling agents such as 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 3-glycidoxypropyltriethoxysilane; styryl-based silane coupling agents such as p-styryltrimethoxysilane; methacryl-based silane coupling agents such as 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, and 3-methacryloxypropyltriethoxysilane; acrylic-based silane coupling agents such as 3-acryloxypropyltrimethoxysilane; N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltriethoxysilane, and N-2-(aminoethyl)-3-aminopropyltriethoxysilane; Amino-based silane coupling agents such as trimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-triethoxysilyl-N-(1,3-dimethyl-butylidene)propylamine, N-phenyl-3-aminopropyltrimethoxysilane, N-phenyl-8-aminooctyltrimethoxysilane, and N-(vinylbenzyl)-2-aminoethyl-3-aminopropyltrimethoxysilane; isocyanurate-based silane coupling agents such as tris-(trimethoxysilylpropyl)isocyanurate; ureido-based silane coupling agents such as 3-ureidopropyltrialkoxysilane; mercapto-based silane coupling agents such as 3-mercaptopropylmethyldimethoxysilane and 3-mercaptopropyltrimethoxysilane; isocyanate-based silane coupling agents such as 3-isocyanatepropyltriethoxysilane; acid anhydride-based silane coupling agents such as 3-trimethoxysilylpropylsuccinic anhydride; and other silane coupling agents;Examples of the surface treatment agent include alkylalkoxysilane compounds such as methyltrimethoxysilane, dimethyldimethoxysilane, phenyltrimethoxysilane, methyltriethoxysilane, dimethyldiethoxysilane, phenyltriethoxysilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, hexyltrimethoxysilane, hexyltriethoxysilane, octyltriethoxysilane, decyltrimethoxysilane, 1,6-bis(trimethoxysilyl)hexane, and trifluoropropyltrimethoxysilane. The surface treatment agent may be used alone or in combination of two or more in any ratio.

[0080] Commercially available surface treatment agents include, for example, "KBM-1003" and "KBE-1003" (vinyl-based silane coupling agents), "KBM-303", "KBM-402", "KBM-403", "KBE-402", and "KBE-403" (epoxy-based silane coupling agents), "KBM-1403" (styryl-based silane coupling agents), "KBM-502", "KBM-503", "KBE-502", and "KBE-503" (methacrylic-based silane coupling agents), "KBM-5103" (acrylic-based silane coupling agents), "KBM-602", "KBM-603", "KBM-903", "KBE-903", "KBE-9103P", "KBM-573", and "KBM-575" (amino-based silane coupling agents), all of which are manufactured by Shin-Etsu Chemical Co., Ltd. coupling agent); "KBM-9659" (isocyanurate-based silane coupling agent); "KBE-585" (ureido-based silane coupling agent); "KBM-802", "KBM-803" (mercapto-based silane coupling agent); "KBE-9007N" (isocyanate-based silane coupling agent); "X-12-967C" (acid anhydride-based silane coupling agent); "KBM-13", "KBM-22", "KBM-103", "KBE-13", "KBE-22", "KBE-103", "KBM-3033", "KBE-3033", "KBM-3063", "KBE-3063", "KBE-3083", "KBM-3103C", "KBM-3066", "KBM-7103" (alkylalkoxysilane compound), and the like.

[0081] From the viewpoint of improving the dispersibility of the inorganic filler, the degree of surface treatment with the surface treatment agent is preferably within a predetermined range. Specifically, 100% by mass of the inorganic filler is preferably surface-treated with 0.2% to 5% by mass of the surface treatment agent, more preferably 0.2% to 3% by mass, and even more preferably 0.3% to 2% by mass.

[0082] The degree of surface treatment with the surface treatment agent can be evaluated by the amount of carbon per unit surface area of ​​the inorganic filler. From the viewpoint of improving the dispersibility of the inorganic filler, the amount of carbon per unit surface area of ​​the inorganic filler is set to 0.02 mg / m 2 More than 0.1 mg / m is preferable. 2 More preferably, 0.2 mg / m or more 2 On the other hand, from the viewpoint of preventing an increase in the minimum melt viscosity of the resin composition or the minimum melt viscosity in the form of a sheet, it is more preferable that the content is 1.0 mg / m 2 Less than 0.8 mg / m is preferred. 2 Less than 0.5 mg / m is more preferable. 2 The following is even more preferred:

[0083] (C) The amount of carbon per unit surface area of ​​the inorganic filler can be measured after the surface-treated inorganic filler is washed with a solvent (e.g., methyl ethyl ketone (MEK)). Specifically, a sufficient amount of MEK as a solvent is added to the inorganic filler that has been surface-treated with a surface treatment agent, and ultrasonic cleaning is performed at 25°C for 5 minutes. After removing the supernatant and drying the solid content, the amount of carbon per unit surface area of ​​the inorganic filler can be measured using a carbon analyzer. As the carbon analyzer, the "EMIA-320V" manufactured by Horiba, Ltd., or the like can be used.

[0084] The content of the inorganic filler (C) in the resin composition is not particularly limited, but when the non-volatile components in the resin composition are taken as 100 mass%, it may be preferably 90 mass% or less, more preferably 80 mass% or less, even more preferably 75 mass% or less, and particularly preferably 70 mass% or less. The lower limit of the content of the inorganic filler (C) in the resin composition is not particularly limited, but when the non-volatile components in the resin composition are taken as 100 mass%, it may be, for example, 0 mass% or more, 1 mass% or more, etc., preferably 10 mass% or more, more preferably 30 mass% or more, even more preferably 40 mass% or more, even more preferably 50 mass% or more, and particularly preferably 60 mass% or more.

[0085] The mass ratio of the specific maleimide compound (A) to the inorganic filler (C) in the resin composition (component (A) / component (C)) is preferably 0.05 or more, more preferably 0.1 or more, and particularly preferably 0.2 or more. The upper limit of the mass ratio of the specific maleimide compound (A) to the inorganic filler (C) in the resin composition (component (A) / component (C)) is preferably 2 or less, more preferably 1 or less, and particularly preferably 0.5 or less.

[0086] <(D) Radical Polymerization Initiator> The resin composition of the present invention may further contain a radical polymerization initiator (D) as an optional component. The radical polymerization initiator (D) may be, for example, a thermal polymerization initiator that generates free radicals when heated. The radical polymerization initiator (D) may be a polymerization initiator for the radical polymerizable components including the components (A) and (B) described above. The radical polymerization initiator (D) may be used alone or in any combination of two or more kinds.

[0087] (D) Examples of the radical polymerization initiator include peroxide-based radical polymerization initiators, azo-based radical polymerization initiators, etc. Among these, peroxide-based radical polymerization initiators are preferred.

[0088] Examples of the peroxide radical polymerization initiator include hydroperoxide compounds such as 1,1,3,3-tetramethylbutyl hydroperoxide; dialkyl peroxide compounds such as tert-butylcumyl peroxide, di-tert-butyl peroxide, di-tert-hexyl peroxide, dicumyl peroxide, 1,4-bis(1-tert-butylperoxy-1-methylethyl)benzene, and 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane; and diacyl peroxide compounds such as dilauroyl peroxide, didecanoyl peroxide, dicyclohexyl peroxydicarbonate, and bis(4-tert-butylcyclohexyl)peroxydicarbonate. peroxyester compounds such as tert-butyl peroxyacetate, tert-butyl peroxybenzoate, tert-butyl peroxyisopropyl monocarbonate, tert-butyl peroxy-2-ethylhexanoate, tert-butyl peroxyneodecanoate, tert-hexylperoxyisopropyl monocarbonate, tert-butyl peroxylaurate, (1,1-dimethylpropyl)2-ethylperhexanoate, tert-butyl 2-ethylperhexanoate, tert-butyl 3,5,5-trimethylperhexanoate, tert-butylperoxy-2-ethylhexyl monocarbonate, and tert-butylperoxymaleic acid.

[0089] Examples of the azo radical polymerization initiator include azonitrile compounds such as 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), 1,1'-azobis(cyclohexane-1-carbonitrile), 1-[(1-cyano-1-methylethyl)azo]formamide, and 2-phenylazo-4-methoxy-2,4-dimethyl-valeronitrile; 2,2'-azobis[2-methyl-N-[1,1-bis(hydroxymethyl)-2-hydroxyethyl]propionamide], 2,2'-azobis[2-methyl-N-[1,1-bis(hydroxymethyl)-2-hydroxyethyl]propionamide], and the like. azo amide compounds such as 2,2'-azobis[2-methyl-N-[2-(1-hydroxybutyl)]-propionamide], 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)-propionamide], 2,2'-azobis(2-methylpropionamide) dihydrate, 2,2'-azobis[N-(2-propenyl)-2-methylpropionamide], 2,2'-azobis(N-butyl-2-methylpropionamide), and 2,2'-azobis(N-cyclohexyl-2-methylpropionamide); alkyl azo compounds such as 2,2'-azobis(2,4,4-trimethylpentane) and 2,2'-azobis(2-methylpropane); and the like.

[0090] (D) Commercially available radical polymerization initiators include, for example, “Perbutyl C”, “Perbutyl A”, “Perbutyl P”, “Perbutyl L”, “Perbutyl O”, “Perbutyl ND”, “Perbutyl Z”, “Perbutyl I”, “Percumyl P”, “Percumyl D”, “Perhexyl D”, “Perhexyl A”, “Perhexyl I”, “Perhexyl Z”, “Perhexyl ND”, “Perhexyl O”, “Perhexyl PV”, and “Perhexyl O”, all manufactured by NOF Corporation.

[0091] The content of the radical polymerization initiator (D) in the resin composition is not particularly limited, but when the non-volatile components in the resin composition are taken as 100 mass%, it may be preferably 5 mass% or less, more preferably 3 mass% or less, even more preferably 2 mass% or less, even more preferably 1 mass% or less, and particularly preferably 0.8 mass% or less. The lower limit of the content of the radical polymerization initiator (D) in the resin composition is not particularly limited, but when the non-volatile components in the resin composition are taken as 100 mass%, it may be, for example, 0 mass% or more, 0.0001 mass% or more, preferably 0.001 mass% or more, more preferably 0.01 mass% or more, even more preferably 0.05 mass% or more, even more preferably 0.1 mass% or more, and particularly preferably 0.3 mass% or more.

[0092] <(E) Thermoplastic resin> The resin composition of the present invention may further contain a thermoplastic resin (E) as an optional component. The thermoplastic resin (E) described here is a component other than those corresponding to the components (A) and (B) described above.

[0093] Examples of the thermoplastic resin as component (E) include phenoxy resin, polyvinyl acetal resin, polyolefin resin, polybutadiene resin, polyimide resin, polyamideimide resin, polyetherimide resin, polysulfone resin, polyethersulfone resin, polyphenylene ether resin, polycarbonate resin, polyetheretherketone resin, polyester resin, etc. Among them, from the viewpoint of obtaining the effect of the present invention remarkably, it is preferable that the thermoplastic resin (E) contains a resin selected from phenoxy resin and polyimide resin. Moreover, the thermoplastic resin may be used alone or in combination of two or more kinds.

[0094] Examples of the phenoxy resin include phenoxy resins having one or more skeletons selected from the group consisting of bisphenol A skeleton, bisphenol F skeleton, bisphenol S skeleton, bisphenolacetophenone skeleton, novolac skeleton, biphenyl skeleton, fluorene skeleton, dicyclopentadiene skeleton, norbornene skeleton, naphthalene skeleton, anthracene skeleton, adamantane skeleton, terpene skeleton, and trimethylcyclohexane skeleton. The terminal of the phenoxy resin may be any functional group such as a phenolic hydroxyl group or an epoxy group.

[0095] Specific examples of phenoxy resins include "1256" and "4250" manufactured by Mitsubishi Chemical Corporation (both of which are phenoxy resins containing a bisphenol A skeleton); "YX8100" manufactured by Mitsubishi Chemical Corporation (phenoxy resin containing a bisphenol S skeleton); "YX6954" manufactured by Mitsubishi Chemical Corporation (phenoxy resin containing a bisphenol acetophenone skeleton); "FX280" and "FX293" manufactured by Nippon Steel & Sumikin Chemical Co., Ltd.; "YL7500BH30", "YX6954BH30", "YX7553", "YX7553BH30", "YL7769BH30", "YL6794", "YL7213", "YL7290", "YL7482", and "YL7891T30" manufactured by Mitsubishi Chemical Corporation.

[0096] Examples of polyvinyl acetal resin include polyvinyl formal resin and polyvinyl butyral resin, and polyvinyl butyral resin is preferred.Specific examples of polyvinyl acetal resin include "Denka Butyral 4000-2", "Denka Butyral 5000-A", "Denka Butyral 6000-C", and "Denka Butyral 6000-EP" manufactured by Denki Kagaku Kogyo Co., Ltd.; S-LEC BH series, BX series (e.g. BX-5Z), KS series (e.g. KS-1), BL series, and BM series manufactured by Sekisui Chemical Co., Ltd.

[0097] Examples of polyolefin resins include ethylene-based copolymer resins such as low-density polyethylene, very low-density polyethylene, high-density polyethylene, ethylene-vinyl acetate copolymer, ethylene-ethyl acrylate copolymer, and ethylene-methyl acrylate copolymer; and polyolefin polymers such as polypropylene and ethylene-propylene block copolymer.

[0098] Specific examples of polyamide-imide resins include "Viromax HR11NN" and "Viromax HR16NN" manufactured by Toyobo Co., Ltd. Specific examples of polyamide-imide resins also include modified polyamide-imides such as "KS9100" and "KS9300" (polysiloxane skeleton-containing polyamide-imide) manufactured by Hitachi Chemical Co., Ltd.

[0099] A specific example of the polyethersulfone resin is "PES5003P" manufactured by Sumitomo Chemical Co., Ltd.

[0100] Specific examples of polysulfone resins include polysulfones "P1700" and "P3500" manufactured by Solvay Advanced Polymers.

[0101] Examples of the polyester resin include polyethylene terephthalate resin, polyethylene naphthalate resin, polybutylene terephthalate resin, polybutylene naphthalate resin, polytrimethylene terephthalate resin, polytrimethylene naphthalate resin, and polycyclohexane dimethyl terephthalate resin.

[0102] The polyimide resin also includes modified polyimide resins such as siloxane-modified polyimide resins. In one embodiment, the polyimide resin preferably includes an aromatic polyimide resin that does not have an aliphatic chain in the main chain.

[0103] In one embodiment, the polyimide resin is more preferably represented by formula (E1):

[0104] [ka]

[0105] [In the formula, X 1 , Y 1 and Y 2 each independently represents a single bond, -CR2-, -O-, -CO-, -S-, -SO-, -SO2-, -CONH-, or -NHCO-; R each independently represents a hydrogen atom or an alkyl group; Ring X a , Ring X b , and ring Y a each independently represents an aromatic ring which may have a substituent; R y1 each independently represents a substituent; Each y1 independently represents 0, 1, 2, or 3; xa and ya each independently represent 0, 1, 2, 3, 4, or 5; yb represents 0 or 1. The xa units may be the same or different for each unit. The ya units may be the same or different for each unit.

[0106] X 1 , Y 1 and Y 2 each independently represents a single bond, -CR2-, -O-, -CO-, -S-, -SO-, -SO2-, -CONH-, or -NHCO-; preferably, -CR2-, -O-, or -CO-; and more preferably, -CR2- or -O-.

[0107] R each independently represents a hydrogen atom or an alkyl group; preferably a hydrogen atom or a methyl group; and more preferably a methyl group.

[0108] Ring X a , Ring X b , and ring Y aeach independently represents an aromatic ring which may have a substituent; preferably a benzene ring which may be substituted with a group selected from an alkyl group, an alkenyl group, and an aryl group, or a naphthalene ring which may be substituted with a group selected from an alkyl group, an alkenyl group, and an aryl group; more preferably a benzene ring which may be substituted with a group selected from an alkyl group, an alkenyl group, and an aryl group; even more preferably a benzene ring which may be substituted with an alkyl group; and particularly preferably an (unsubstituted) benzene ring.

[0109] R y1 each independently represents a substituent; preferably an alkyl group, an alkenyl group, or an aryl group; more preferably an alkyl group.

[0110] Each y1 independently represents 0, 1, 2 or 3; preferably 0, 1 or 2; more preferably 0 or 1; particularly preferably 0. xa represents 0, 1, 2, 3, 4 or 5; preferably 1, 2, 3, 4 or 5; more preferably 2, 3, 4 or 5; even more preferably 3, 4 or 5; particularly preferably 4. ya represents 0, 1, 2, 3, 4 or 5; preferably 0, 1, 2, 3 or 4; more preferably 0, 1, 2 or 3; even more preferably 1, 2 or 3; particularly preferably 2. yb represents 0 or 1; preferably 1.

[0111] The structural unit represented by formula (E1) contains the formula (Ex):

[0112] [ka]

[0113] [wherein * indicates a binding site; other symbols are as defined above.] Specific examples of the partial structure represented by the formulae (Ex-1) to (Ex-24):

[0114] [ka]

[0115] [In the formula, * is the same as above.] Examples of the partial structure include those represented by any one of the following:

[0116] The structural unit represented by formula (E1) contains the formula (Ey):

[0117] [ka]

[0118] [wherein * indicates a binding site; other symbols are as defined above.] Specific examples of the partial structure represented by the formulae (Ey-1) to (Ey-25):

[0119] [ka]

[0120] [In the formula, * is the same as above.] Examples of the partial structure include those represented by any one of the following:

[0121] In one embodiment, the polyimide resin is more preferably represented by the formulas (E2-1) to (E2-4):

[0122] [ka]

[0123] [In the formula, X 11 , X 12 , X 13 , X 14 , Y 11 , Y 12 and Y 2 each independently represents a single bond, -CR2-, -O-, -CO-, -S-, -SO-, -SO2-, -CONH-, or -NHCO-; Ring X a1 , Ring X a2 , Ring X a3 , Ring X a4 , Ring X b , ring Y a1 and ring Y a2 each independently represents an aromatic ring which may have a substituent; Other symbols are as above.] In particular, it is preferable that the resin contains a resin having a repeating unit represented by formula (E2-1).

[0124] X 11 , X 12 , X 13 and X 14 each independently represents a single bond, -CR2-, -O-, -CO-, -S-, -SO-, -SO2-, -CONH-, or -NHCO-; preferably, -CR2-, -O-, or -CO-; more preferably, -CR2-, or -O-; and further preferably, X 11 and X 14 is -O- and X 12 and X 13 is -CR2-. Y 11 , Y 12 and Y 2 each independently represents a single bond, -CR2-, -O-, -CO-, -S-, -SO-, -SO2-, -CONH-, or -NHCO-; preferably, -CR2-, -O-, or -CO-; more preferably, -CR2- or -O-; and further preferably, Y 11 and Y 2 is -O- and Y 12 is -CR2-.

[0125] Ring X a1 , Ring X a2 , Ring X a3 , Ring X a4 , Ring X b , ring Y a1 and ring Y a2each independently represents an aromatic ring which may have a substituent; preferably a benzene ring which may be substituted with a group selected from an alkyl group, an alkenyl group, and an aryl group, or a naphthalene ring which may be substituted with a group selected from an alkyl group, an alkenyl group, and an aryl group; more preferably a benzene ring which may be substituted with a group selected from an alkyl group, an alkenyl group, and an aryl group; even more preferably a benzene ring which may be substituted with an alkyl group; and particularly preferably an (unsubstituted) benzene ring.

[0126] In one embodiment, the polyimide resin is more preferably represented by formula (E3):

[0127] [ka]

[0128] [In the formula, R x1 and R y2 each independently represents a substituent; x1 and y2 each independently represent 0, 1, 2, 3, or 4; Other symbols are as above.] The resin includes a resin having a repeating unit represented by the formula:

[0129] R x1 and R y2 each independently represents a substituent; preferably an alkyl group, an alkenyl group, or an aryl group; more preferably an alkyl group.

[0130] x1 and y2 each independently represent 0, 1, 2, 3, or 4; preferably, 0, 1, 2, or 3; more preferably, 0, 1, or 2; even more preferably, 0 or 1; and particularly preferably, 0.

[0131] The polyimide resin is not particularly limited, but can be obtained by a known synthesis method such as an imidization reaction between a diamine compound and a tetracarboxylic anhydride, an imidization reaction between a diisocyanate compound and a tetracarboxylic anhydride, etc. Commercially available polyimide resins may be used, and examples of commercially available polyimide resins include "Rikacoat SN20" and "Rikacoat PN20" manufactured by New Japan Chemical Co., Ltd.

[0132] The glass transition temperature of the (F) polyimide resin is not particularly limited, but is preferably 50°C to 400°C, more preferably 75°C to 350°C, further preferably 100°C to 300°C, and particularly preferably 125°C to 250°C.

[0133] From the viewpoint of significantly obtaining the effects of the present invention, the weight average molecular weight (Mw) of the (E) thermoplastic resin is preferably 8,000 or more, more preferably 10,000 or more, and particularly preferably 20,000 or more, and is preferably 70,000 or less, more preferably 60,000 or less, and particularly preferably 50,000 or less.

[0134] The content of the (E) thermoplastic resin in the resin composition is not particularly limited, but when the non-volatile components in the resin composition are taken as 100 mass%, from the viewpoint of significantly obtaining the desired effects of the present invention, it may be preferably 20 mass% or less, more preferably 15 mass% or less, even more preferably 10 mass% or less, even more preferably 7 mass% or less, and particularly preferably 5 mass% or less. The lower limit of the content of the (E) thermoplastic resin in the resin composition is not particularly limited, but when the non-volatile components in the resin composition are taken as 100 mass%, it may be, for example, 0 mass% or more, 0.01 mass% or more, 0.05 mass% or more, preferably 0.1 mass% or more, more preferably 0.5 mass% or more, even more preferably 1 mass% or more, even more preferably 2 mass% or more, and particularly preferably 3 mass% or more.

[0135] <(F) Elastomer> The resin composition of the present invention may further contain an optional component (F) elastomer. The (F) elastomer described here is a component other than those corresponding to the components (A) and (B) described above.

[0136] The elastomer as component (F) is a flexible resin, and is preferably a resin having rubber elasticity or a resin exhibiting rubber elasticity by polymerization with other components. Examples of rubber elasticity include resins exhibiting an elastic modulus of 1 GPa or less when a tensile test is performed at a temperature of 25°C and a humidity of 40% RH according to the Japanese Industrial Standards (JIS K7161).

[0137] In one embodiment, the (F) elastomer is preferably a resin having, in the molecule, one or more structures selected from a polybutadiene structure, a polysiloxane structure, a poly(meth)acrylate structure, a polyalkylene structure, a polyalkyleneoxy structure, a polyisoprene structure, a polyisobutylene structure, a polycarbonate structure, and a polystyrene structure. "(Meth)acrylate" refers to methacrylate and acrylate.

[0138] In another embodiment, the (F) elastomer is preferably one or more selected from resins having a glass transition temperature (Tg) of 25° C. or less and resins that are liquid at 25° C. or less. The glass transition temperature of the resin having a glass transition temperature (Tg) of 25° C. or less is preferably 20° C. or less, more preferably 15° C. or less. The lower limit of the glass transition temperature is not particularly limited, but can usually be −15° C. or more. The resin that is liquid at 25° C. is preferably a resin that is liquid at 20° C. or less, more preferably a resin that is liquid at 15° C. or less. The glass transition temperature can be measured by DSC (differential scanning calorimetry).

[0139] The (F) elastomer is usually an amorphous resin component that can be dissolved in an organic solvent. The (F) elastomer may be used alone or in combination of two or more kinds in any ratio.

[0140] The (F) elastomer may be, for example, a resin containing a polybutadiene structure. The polybutadiene structure may be contained in the main chain or in the side chain. The polybutadiene structure may be partially or entirely hydrogenated. A resin containing a polybutadiene structure may be called a "polybutadiene resin." Specific examples of polybutadiene resins include "Ricon 130MA8", "Ricon 130MA13", "Ricon 130MA20", "Ricon 131MA5", "Ricon 131MA10", "Ricon 131MA17", "Ricon 131MA20", and "Ricon 184MA6" (polybutadiene containing an acid anhydride group) manufactured by Cray Valley Corporation; "GQ-1000" (polybutadiene having hydroxyl groups and carboxyl groups introduced therein), "G-1000", "G-2000", and "G-3000" (polybutadiene having hydroxyl groups at both ends), "GI-1000", "GI-2000", and "GI-3000" (polybutadiene having hydrogenated hydroxyl groups at both ends) manufactured by Nippon Soda Co., Ltd.; and "FCA-061L" (hydrogenated polybutadiene skeleton epoxy resin) manufactured by Nagase ChemteX Corporation. Specific examples of polybutadiene resins include hydroxyl-terminated polybutadiene, linear polyimides made from diisocyanate compounds and tetrabasic acid anhydrides (polyimides described in JP 2006-37083 A and WO 2008 / 153208 A), and phenolic hydroxyl-containing butadiene. The content of the butadiene structure in the polyimide resin is preferably 60% by mass to 95% by mass, more preferably 75% by mass to 85% by mass. For details of the polyimide resin, refer to the descriptions in JP 2006-37083 A and WO 2008 / 153208 A, the contents of which are incorporated herein by reference.

[0141] (F) Elastomers include, for example, resins containing a poly(meth)acrylate structure. Resins containing a poly(meth)acrylate structure are sometimes called "poly(meth)acrylic resins." Specific examples of poly(meth)acrylic resins include Teisan Resin manufactured by Nagase ChemteX Corporation, and ME-2000, W-116.3, W-197C, KG-25, and KG-3000 manufactured by Negami Chemical Industries, Ltd.

[0142] (F) elastomers include, for example, resins containing a polycarbonate structure. Resins containing a polycarbonate structure are sometimes called "polycarbonate resins". Specific examples of polycarbonate resins include "T6002" and "T6001" (polycarbonate diols) manufactured by Asahi Kasei Chemicals Corporation, and "C-1090", "C-2090", and "C-3090" (polycarbonate diols) manufactured by Kuraray Co., Ltd. In addition, linear polyimides made from hydroxyl-terminated polycarbonates, diisocyanate compounds, and tetrabasic acid anhydrides can also be used. The content of the carbonate structure in the polyimide resin is preferably 60% by mass to 95% by mass, more preferably 75% by mass to 85% by mass. For details of the polyimide resin, refer to the description in International Publication No. 2016 / 129541, the contents of which are incorporated herein by reference.

[0143] Examples of the (F) elastomer include resins containing a polysiloxane structure. Resins containing a polysiloxane structure are sometimes called "siloxane resins." Specific examples of siloxane resins include "SMP-2006," "SMP-2003PGMEA," and "SMP-5005PGMEA" manufactured by Shin-Etsu Silicones Co., Ltd., and linear polyimides made from amine-terminated polysiloxanes and tetrabasic acid anhydrides (see International Publication No. 2010 / 053185, JP 2002-12667 A, JP 2000-319386 A, etc.).

[0144] Examples of the (F) elastomer include resins containing a polyalkylene structure or a polyalkyleneoxy structure. A resin containing a polyalkylene structure may be referred to as an "alkylene resin". A resin containing a polyalkyleneoxy structure may be referred to as an "alkyleneoxy resin". The polyalkyleneoxy structure is preferably a polyalkyleneoxy structure having 2 to 15 carbon atoms, more preferably a polyalkyleneoxy structure having 3 to 10 carbon atoms, and particularly preferably a polyalkyleneoxy structure having 5 to 6 carbon atoms. Specific examples of the alkylene resin and the alkyleneoxy resin include "PTXG-1000" and "PTXG-1800" manufactured by Asahi Kasei Fibers Corporation.

[0145] (F) Elastomers include, for example, resins containing a polyisoprene structure. Resins containing a polyisoprene structure are sometimes called "isoprene resins." Specific examples of isoprene resins include "KL-610" and "KL613" manufactured by Kuraray Co., Ltd.

[0146] (F) Elastomers include, for example, resins containing a polyisobutylene structure. Resins containing a polyisobutylene structure are sometimes called "isobutylene resins." Specific examples of isobutylene resins include Kaneka Corporation's "SIBSTAR-073T" (styrene-isobutylene-styrene triblock copolymer) and "SIBSTAR-042D" (styrene-isobutylene diblock copolymer).

[0147] (F) Elastomers include, for example, resins containing a polystyrene structure. Resins containing a polystyrene structure are sometimes called "styrene resins". Examples of styrene resins include styrene-butadiene-styrene block copolymers (SBS), styrene-isoprene-styrene block copolymers (SIS), styrene-ethylene-butylene-styrene block copolymers (SEBS), styrene-ethylene-propylene-styrene block copolymers (SEPS), styrene-ethylene-ethylene-propylene-styrene block copolymers (SEEPS), styrene-butadiene-butylene-styrene block copolymers (SBBS), styrene-butadiene diblock copolymers, hydrogenated styrene-butadiene block copolymers, hydrogenated styrene-isoprene block copolymers, and hydrogenated styrene-butadiene random copolymers. Specific examples of styrene resins include hydrogenated styrene-based thermoplastic elastomers "H1041", "Tuftec H1043", "Tuftec P2000", and "Tuftec MP10" (manufactured by Asahi Kasei Corporation); epoxidized styrene-butadiene thermoplastic elastomers "Epofriend AT501" and "CT310" (manufactured by Daicel Corporation); modified styrene-based elastomers having hydroxyl groups "Septon HG252" (manufactured by Kuraray Co., Ltd.); modified styrene-based elastomers having carboxyl groups "Tuftec N503M", modified styrene-based elastomers having amino groups "Tuftec N501", modified styrene-based elastomers having acid anhydride groups "Tuftec M1913" (manufactured by Asahi Kasei Chemicals Corporation); unmodified styrene-based elastomers "Septon S8104" (manufactured by Kuraray Co., Ltd.); and styrene-ethylene / butylene-styrene block copolymers "FG1924" (manufactured by Kraton Co., Ltd.).

[0148] The number average molecular weight (Mn) of the (F) elastomer is preferably 1,000 or more, more preferably 1,500 or more, even more preferably 3,000 or more, particularly preferably 5,000 or more, and is preferably 1,000,000 or less, more preferably 900,000 or less. The number average molecular weight (Mn) can be measured in terms of polystyrene using GPC (gel permeation chromatography).

[0149] The content of the (F) elastomer in the resin composition is not particularly limited, but from the viewpoint of significantly obtaining the desired effect of the present invention, when the non-volatile components in the resin composition are taken as 100 mass%, it may be preferably 20 mass% or less, more preferably 15 mass% or less, even more preferably 10 mass% or less, even more preferably 7 mass% or less, and particularly preferably 5 mass% or less. The lower limit of the content of the (F) elastomer in the resin composition is not particularly limited, but when the non-volatile components in the resin composition are taken as 100 mass%, it may be, for example, 0 mass% or more, 0.01 mass% or more, 0.05 mass% or more, preferably 0.1 mass% or more, more preferably 0.5 mass% or more, even more preferably 1 mass% or more, even more preferably 2 mass% or more, and particularly preferably 3 mass% or more.

[0150] <(G) Other Additives> The resin composition of the present invention may further contain any additive as a non-volatile component.Examples of such additives include thermosetting resins such as epoxy resins, epoxy acrylate resins, urethane acrylate resins, urethane resins, cyanate resins, polyimide resins, benzoxazine resins, unsaturated polyester resins, phenolic resins, melamine resins, and silicone resins; curing accelerators such as imidazole-based curing accelerators, phosphorus-based curing accelerators, urea-based curing accelerators, guanidine-based curing accelerators, metal-based curing accelerators, and amine-based curing accelerators; phenol-based curing agents, naphthol-based curing agents, acid anhydride-based curing agents, thiol-based curing agents, and benzoxazine-based curing agents. curing agents such as cyanate ester curing agents, carbodiimide curing agents, imidazole curing agents, and active ester compounds; organic fillers such as rubber particles; organometallic compounds such as organocopper compounds, organozinc compounds, and organocobalt compounds; colorants such as phthalocyanine blue, phthalocyanine green, iodine green, diazo yellow, crystal violet, titanium oxide, and carbon black; polymerization inhibitors such as hydroquinone, catechol, pyrogallol, and phenothiazine; leveling agents such as silicone-based leveling agents and acrylic polymer-based leveling agents. agents; thickeners such as bentone and montmorillonite; defoamers such as silicone-based defoamers, acrylic-based defoamers, fluorine-based defoamers, and vinyl resin-based defoamers; ultraviolet absorbers such as benzotriazole-based ultraviolet absorbers; adhesion improvers such as urea silane; adhesion imparters such as triazole-based adhesion imparters, tetrazole-based adhesion imparters, and triazine-based adhesion imparters; antioxidants such as hindered phenol-based antioxidants and hindered amine-based antioxidants; fluorescent brighteners such as stilbene derivatives; surfactants such as fluorine-based surfactants and silicone-based surfactants; phosphorus-based flame retardants (for example Flame retardants such as phosphate ester compounds, phosphazene compounds, phosphinic acid compounds, red phosphorus), nitrogen-based flame retardants (e.g., melamine sulfate), halogen-based flame retardants, and inorganic flame retardants (e.g., antimony trioxide); dispersants such as phosphate ester-based dispersants, polyoxyalkylene-based dispersants, acetylene-based dispersants, silicone-based dispersants, anionic dispersants, and cationic dispersants; and stabilizers such as borate-based stabilizers, titanate-based stabilizers, aluminate-based stabilizers, zirconate-based stabilizers, isocyanate-based stabilizers, carboxylic acid-based stabilizers, and carboxylic anhydride-based stabilizers.The (G) other additives may be used alone or in any combination of two or more kinds at any ratio. The content of the (G) other additives can be appropriately determined by a person skilled in the art.

[0151] <(H) Organic Solvent> The resin composition of the present invention may further contain an arbitrary organic solvent as a volatile component in addition to the non-volatile components described above. As the (H) organic solvent, a known one can be appropriately used, and the type is not particularly limited. As the (H) organic solvent, for example, ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, etc.; ester-based solvents such as methyl acetate, ethyl acetate, butyl acetate, isobutyl acetate, isoamyl acetate, methyl propionate, ethyl propionate, γ-butyrolactone, etc.; ether-based solvents such as tetrahydropyran, tetrahydrofuran, 1,4-dioxane, diethyl ether, diisopropyl ether, dibutyl ether, diphenyl ether, anisole, etc.; alcohol-based solvents such as methanol, ethanol, propanol, butanol, ethylene glycol, etc.; 2-ethoxyethyl acetate, propylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, ethyl diglycol acetate, γ-butyrolactone, methoxypropionic acid, etc. Examples of suitable organic solvents include ether ester solvents such as methyl lactate, ethyl lactate, and methyl 2-hydroxyisobutyrate; ether alcohol solvents such as 2-methoxypropanol, 2-methoxyethanol, 2-ethoxyethanol, propylene glycol monomethyl ether, and diethylene glycol monobutyl ether (butylcarbitol); amide solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone; sulfoxide solvents such as dimethyl sulfoxide; nitrile solvents such as acetonitrile and propionitrile; aliphatic hydrocarbon solvents such as hexane, cyclopentane, cyclohexane, and methylcyclohexane; and aromatic hydrocarbon solvents such as benzene, toluene, xylene, ethylbenzene, and trimethylbenzene. (H) The organic solvent may be used alone or in combination of two or more in any ratio.

[0152] In one embodiment, the content of the (H) organic solvent is not particularly limited, but when all components in the resin composition are taken as 100 mass%, it can be, for example, 60 mass% or less, 40 mass% or less, 30 mass% or less, 20 mass% or less, 15 mass% or less, 10 mass% or less, etc.

[0153] <Method of producing resin composition> The resin composition of the present invention can be produced, for example, by adding (A) a specific maleimide compound, (B) a resin having a vinylphenyl group and / or a (meth)acryloyl group, if necessary (A') other maleimide compounds, if necessary (C) an inorganic filler, if necessary (D) a radical polymerization initiator, if necessary (E) a thermoplastic resin, if necessary (F) an elastomer, if necessary (G) other additives, if necessary, and if necessary (H) an organic solvent in any order and / or all at once and mixing them in any preparation vessel. In addition, the temperature can be appropriately set during the process of adding and mixing each component, and heating and / or cooling may be performed temporarily or throughout. In addition, during or after the process of adding and mixing, the resin composition may be stirred or shaken using a stirring device or shaking device such as a mixer to disperse uniformly. In addition, degassing may be performed under low pressure conditions such as under vacuum at the same time as stirring or shaking.

[0154] <Characteristics of resin composition> The resin composition of the present invention contains (A) a specific maleimide compound and (B) a resin having a vinylphenyl group and / or a (meth)acryloyl group. By using such a resin composition, the minimum melt viscosity can be reduced, and a cured product having a low dielectric loss tangent (Df) and excellent copper plating peel strength can be obtained.

[0155] The cured product of the resin composition of the present invention may be characterized by excellent copper plating peel strength. Thus, in one embodiment, as in the following Test Example 2, a copper plating conductor layer is formed on the cured product, and the copper plating peel strength calculated from the load when the copper plating conductor layer is peeled off in the vertical direction may be preferably 0.1 kgf / cm or more, more preferably 0.2 kgf / cm or more, even more preferably 0.25 kgf / cm or more, particularly preferably 0.3 kgf / cm or more, 0.35 kgf / cm or more. The upper limit is not particularly limited, but may be, for example, 10 kgf / cm or less.

[0156] The cured product of the resin composition of the present invention may be characterized by a low dielectric loss tangent (Df). Thus, in one embodiment, the dielectric loss tangent (Df) of the cured product of the resin composition, as measured at 5.8 GHz and 23° C. as in Test Example 1 below, may be preferably 0.020 or less, 0.010 or less, more preferably 0.009 or less, 0.008 or less, even more preferably 0.007 or less, 0.006 or less, 0.005 or less, and particularly preferably 0.004 or less, 0.0035 or less, 0.003 or less.

[0157] The resin composition of the present invention may be characterized by a low minimum melt viscosity. Thus, in one embodiment, the minimum melt viscosity measured using a dynamic viscoelasticity measuring device at a frequency of 1 Hz, a strain of 5 degrees, a load of 100 g, a heating rate of 5°C / min, and a temperature range of 60°C to 180°C as in Test Example 4 below may be preferably 2500 poise or less, more preferably 2000 poise or less, and even more preferably 1800 poise or less.

[0158] In one embodiment, the cured product of the resin composition of the present invention may be characterized by a low dielectric constant (Dk). Thus, in one embodiment, the dielectric constant (Dk) of the cured product of the resin composition, as measured at 5.8 GHz and 23° C. as in the following Test Example 1, is preferably 5.0 or less, more preferably 4.0 or less, even more preferably 3.5 or less, particularly preferably 3.2 or less, and may be 3.0 or less.

[0159] In one embodiment, the cured product of the resin composition of the present invention may be characterized by a low arithmetic mean roughness (Ra) of the surface after roughening treatment. Therefore, in one embodiment, the arithmetic mean roughness (Ra) of the cured product surface after roughening treatment measured as in the following Test Example 3 may be preferably 300 nm or less, more preferably 200 nm or less, even more preferably 150 nm or less, even more preferably 130 nm or less, and particularly preferably 110 nm or less. The lower limit is not particularly limited, and may be, for example, 1 nm or more, 2 nm or more, etc.

[0160] <Applications of resin composition> The resin composition of the present invention can be suitably used as a resin composition for insulating purposes, particularly as a resin composition for forming an insulating layer. Specifically, it can be suitably used as a resin composition for forming an insulating layer (resin composition for forming an insulating layer for forming a conductor layer) for forming a conductor layer (including a rewiring layer) formed on an insulating layer. In addition, in a printed wiring board described later, it can be suitably used as a resin composition for forming an insulating layer of a printed wiring board (resin composition for forming an insulating layer of a printed wiring board). The resin composition of the present invention can also be used in a wide range of applications requiring a resin composition, such as a resin sheet, a sheet-like laminate material such as a prepreg, a solder resist, an underfill material, a die bonding material, a semiconductor encapsulant, a hole filling resin, and a component embedding resin.

[0161] In addition, for example, when a semiconductor chip package is manufactured through the following steps (1) to (6), the resin composition of the present invention can be suitably used as a resin composition for a rewiring formation layer (resin composition for forming a rewiring formation layer) as an insulating layer for forming a rewiring layer, and as a resin composition for sealing a semiconductor chip (resin composition for sealing a semiconductor chip). When a semiconductor chip package is manufactured, a rewiring layer may be further formed on the sealing layer. (1) A step of laminating a temporary fixing film onto a substrate; (2) a step of temporarily fixing a semiconductor chip on a temporary fixing film; (3) forming an encapsulation layer on the semiconductor chip; (4) peeling the substrate and the temporary fixing film from the semiconductor chip; (5) forming a rewiring formation layer as an insulating layer on the surface of the semiconductor chip from which the base material and the temporary fixing film have been peeled off; and (6) A process of forming a rewiring layer as a conductor layer on the rewiring formation layer.

[0162] Furthermore, the resin composition of the present invention provides an insulating layer with good component embedding properties, and therefore can be suitably used when the printed wiring board is a circuit board with built-in components.

[0163] <Sheet-type laminated material> The resin composition of the present invention can be used by coating in the form of a varnish, but from an industrial perspective, it is generally preferred to use the resin composition in the form of a sheet-like laminate material containing the resin composition.

[0164] As the sheet-like laminate material, the following resin sheets and prepregs are preferred.

[0165] In one embodiment, the resin sheet includes a support and a resin composition layer provided on the support, and the resin composition layer is formed from the resin composition of the present invention.

[0166] The thickness of the resin composition layer is preferably 50 μm or less, more preferably 40 μm or less, from the viewpoint of making the printed wiring board thinner and being able to provide a cured product with excellent insulation even if the cured product of the resin composition is a thin film. The lower limit of the thickness of the resin composition layer is not particularly limited, but can usually be 5 μm or more, 10 μm or more, etc.

[0167] Examples of the support include films made of plastic materials, metal foils, and release papers, with films made of plastic materials and metal foils being preferred.

[0168] When a film made of a plastic material is used as the support, examples of the plastic material include polyesters such as polyethylene terephthalate (hereinafter sometimes abbreviated as "PET") and polyethylene naphthalate (hereinafter sometimes abbreviated as "PEN"), polycarbonate (hereinafter sometimes abbreviated as "PC"), acrylics such as polymethyl methacrylate (PMMA), cyclic polyolefins, triacetyl cellulose (TAC), polyether sulfide (PES), polyether ketone, polyimide, etc. Among these, polyethylene terephthalate and polyethylene naphthalate are preferred, and inexpensive polyethylene terephthalate is particularly preferred.

[0169] When a metal foil is used as the support, examples of the metal foil include copper foil, aluminum foil, etc., and copper foil is preferred. As the copper foil, a foil made of a single metal, copper, or an alloy of copper and another metal (e.g., tin, chromium, silver, magnesium, nickel, zirconium, silicon, titanium, etc.) may be used.

[0170] The surface of the support to be bonded to the resin composition layer may be subjected to a matte treatment, a corona treatment, or an antistatic treatment.

[0171] In addition, as the support, a support with a release layer having a release layer on the surface to be bonded to the resin composition layer may be used. The release agent used in the release layer of the support with a release layer may be, for example, one or more release agents selected from the group consisting of alkyd resins, polyolefin resins, urethane resins, and silicone resins. The support with a release layer may be a commercially available product, for example, "SK-1", "AL-5", and "AL-7" manufactured by Lintec Corporation, "Lumirror T60" manufactured by Toray Industries, Inc., "Purex" manufactured by Teijin Limited, and "Unipeel" manufactured by Unitika Limited, which are PET films having a release layer mainly composed of an alkyd resin-based release agent.

[0172] The thickness of the support is not particularly limited, but is preferably in the range of 5 μm to 75 μm, and more preferably in the range of 10 μm to 60 μm. When a support with a release layer is used, it is preferable that the total thickness of the support with a release layer is in the above range.

[0173] In one embodiment, the resin sheet may further include an optional layer as necessary. For example, such an optional layer may be a protective film equivalent to the support provided on the surface of the resin composition layer that is not bonded to the support (i.e., the surface opposite to the support). The thickness of the protective film is not particularly limited, but is, for example, 1 μm to 40 μm. By laminating the protective film, adhesion of dirt and the like to the surface of the resin composition layer and scratches can be suppressed.

[0174] The resin sheet can be produced, for example, by preparing a liquid resin composition as is or a resin varnish by dissolving the resin composition in an organic solvent, applying this onto a support using a die coater or the like, and then drying to form a resin composition layer.

[0175] The organic solvent may be the same as the organic solvent described as a component of the resin composition. The organic solvent may be used alone or in combination of two or more kinds.

[0176] Drying may be performed by a known method such as heating or hot air blowing. Drying conditions are not particularly limited, but drying is performed so that the content of the organic solvent in the resin composition layer becomes 10% by mass or less, preferably 5% by mass or less. Although it varies depending on the boiling point of the organic solvent in the resin composition or resin varnish, for example, when a resin composition or resin varnish containing 30% by mass to 60% by mass of the organic solvent is used, the resin composition layer can be formed by drying at 50°C to 150°C for 3 minutes to 10 minutes.

[0177] The resin sheet can be stored in a rolled state. When the resin sheet has a protective film, it can be used by peeling off the protective film.

[0178] In one embodiment, the prepreg is formed by impregnating a sheet-like fiber substrate with the resin composition of the present invention.

[0179] The sheet-like fiber substrate used for the prepreg is not particularly limited, and can be a substrate commonly used for prepreg, such as glass cloth, aramid nonwoven fabric, liquid crystal polymer nonwoven fabric, etc. From the viewpoint of thinning the printed wiring board, the thickness of the sheet-like fiber substrate is preferably 50 μm or less, more preferably 40 μm or less, even more preferably 30 μm or less, and particularly preferably 20 μm or less. The lower limit of the thickness of the sheet-like fiber substrate is not particularly limited. It is usually 10 μm or more.

[0180] The prepreg can be produced by a known method such as a hot melt method or a solvent method.

[0181] The thickness of the prepreg may be in the same range as that of the resin composition layer in the above-mentioned resin sheet.

[0182] The sheet-like laminate material of the present invention can be suitably used for forming an insulating layer of a printed wiring board (for an insulating layer of a printed wiring board), and can be more suitably used for forming an interlayer insulating layer of a printed wiring board (for an interlayer insulating layer of a printed wiring board).

[0183] <Printed wiring board> The printed wiring board of the present invention includes an insulating layer made of a cured product obtained by curing the resin composition of the present invention.

[0184] The printed wiring board can be produced, for example, by using the above-mentioned resin sheet by a method including the following steps (I) and (II). (I) A step of laminating a resin sheet on an inner layer substrate such that a resin composition layer of the resin sheet is bonded to the inner layer substrate. (II) A step of curing (e.g., heat curing) the resin composition layer to form an insulating layer.

[0185] The "inner layer substrate" used in step (I) is a member that becomes the substrate of the printed wiring board, and examples thereof include a glass epoxy substrate, a metal substrate, a polyester substrate, a polyimide substrate, a BT resin substrate, and a thermosetting polyphenylene ether substrate. The substrate may have a conductor layer on one or both sides, and the conductor layer may be patterned. An inner layer substrate having a conductor layer (circuit) formed on one or both sides of the substrate may be called an "inner layer circuit substrate". In addition, an intermediate product on which an insulating layer and / or a conductor layer is to be formed during the manufacture of a printed wiring board is also included in the "inner layer substrate" of the present invention. When the printed wiring board is a circuit board with built-in components, an inner layer substrate with built-in components may be used.

[0186] The lamination of the inner layer substrate and the resin sheet can be carried out, for example, by thermocompression bonding the resin sheet to the inner layer substrate from the support side. Examples of the member for thermocompression bonding the resin sheet to the inner layer substrate (hereinafter also referred to as the "thermocompression bonding member") include a heated metal plate (such as a SUS plate) or a metal roll (SUS roll). It is preferable to press the thermocompression member not directly onto the resin sheet, but via an elastic material such as heat-resistant rubber so that the resin sheet can sufficiently follow the surface irregularities of the inner layer substrate.

[0187] The lamination of the inner layer substrate and the resin sheet may be performed by a vacuum lamination method. In the vacuum lamination method, the thermocompression temperature is preferably in the range of 60°C to 160°C, more preferably in the range of 80°C to 140°C, the thermocompression pressure is preferably in the range of 0.098MPa to 1.77MPa, more preferably in the range of 0.29MPa to 1.47MPa, and the thermocompression time is preferably in the range of 20 seconds to 400 seconds, more preferably in the range of 30 seconds to 300 seconds. The lamination may be performed under reduced pressure conditions, preferably at a pressure of 26.7hPa or less.

[0188] The lamination can be performed by a commercially available vacuum laminator, such as a vacuum pressure laminator manufactured by Meiki Seisakusho Co., Ltd., a vacuum applicator manufactured by Nikko Materials Co., Ltd., or a batch type vacuum pressure laminator.

[0189] After lamination, the laminated resin sheet may be smoothed under normal pressure (atmospheric pressure), for example, by pressing a thermocompression member from the support side. The pressing conditions for the smoothing treatment may be the same as the thermocompression conditions for the lamination. The smoothing treatment may be performed using a commercially available laminator. The lamination and smoothing treatment may be performed consecutively using the commercially available vacuum laminator.

[0190] The support may be removed between step (I) and step (II) or after step (II).

[0191] In step (II), the resin composition layer is cured (for example, thermally cured) to form an insulating layer made of a cured product of the resin composition. The curing conditions for the resin composition layer are not particularly limited, and conditions that are usually adopted when forming an insulating layer for a printed wiring board may be used.

[0192] For example, the thermal curing conditions for the resin composition layer vary depending on the type of resin composition, etc., but in one embodiment, the curing temperature is preferably 120° C. to 240° C., more preferably 150° C. to 220° C., and even more preferably 170° C. to 210° C. The curing time is preferably 5 minutes to 120 minutes, more preferably 10 minutes to 100 minutes, and even more preferably 15 minutes to 100 minutes.

[0193] Before the resin composition layer is thermally cured, the resin composition layer may be preheated at a temperature lower than the curing temperature. For example, prior to thermally curing the resin composition layer, the resin composition layer may be preheated at a temperature of 50° C. to 120° C., preferably 60° C. to 115° C., more preferably 70° C. to 110° C. for 5 minutes or more, preferably 5 minutes to 150 minutes, more preferably 15 minutes to 120 minutes, and even more preferably 15 minutes to 100 minutes.

[0194] In manufacturing a printed wiring board, the steps of (III) drilling holes in the insulating layer, (IV) roughening the insulating layer, and (V) forming a conductor layer may be further carried out. These steps (III) to (V) may be carried out according to various methods known to those skilled in the art for use in manufacturing printed wiring boards. When the support is removed after step (II), the support may be removed between step (II) and step (III), between step (III) and step (IV), or between step (IV) and step (V). In addition, the formation of the insulating layer and the conductor layer in steps (II) to (V) may be repeated to form a multilayer wiring board, as necessary.

[0195] In another embodiment, the printed wiring board of the present invention can be manufactured using the above-mentioned prepreg. The manufacturing method is basically the same as when a resin sheet is used.

[0196] Step (III) is a step of drilling holes in the insulating layer, which allows holes such as via holes and through holes to be formed in the insulating layer. Step (III) may be performed using, for example, a drill, a laser, plasma, etc., depending on the composition of the resin composition used to form the insulating layer. The dimensions and shape of the holes may be appropriately determined depending on the design of the printed wiring board.

[0197] Step (IV) is a step of roughening the insulating layer. Usually, smears are also removed in this step (IV). The procedure and conditions of the roughening treatment are not particularly limited, and known procedures and conditions that are usually used when forming an insulating layer of a printed wiring board can be adopted. For example, the insulating layer can be roughened by carrying out a swelling treatment with a swelling liquid, a roughening treatment with an oxidizing agent, and a neutralization treatment with a neutralizing liquid in this order.

[0198] The swelling liquid used in the roughening treatment is not particularly limited, but includes an alkaline solution, a surfactant solution, etc., and is preferably an alkaline solution, and more preferably a sodium hydroxide solution or a potassium hydroxide solution. Examples of commercially available swelling liquids include "Swelling Dip Securigans P" and "Swelling Dip Securigans SBU" manufactured by Atotech Japan. The swelling treatment using the swelling liquid is not particularly limited, but can be performed by immersing the insulating layer in a swelling liquid at 30°C to 90°C for 1 to 20 minutes, for example. From the viewpoint of suppressing the swelling of the resin of the insulating layer to an appropriate level, it is preferable to immerse the insulating layer in a swelling liquid at 40°C to 80°C for 5 to 15 minutes.

[0199] The oxidizing agent used in the roughening treatment is not particularly limited, but examples thereof include an alkaline permanganate solution in which potassium permanganate or sodium permanganate is dissolved in an aqueous solution of sodium hydroxide. The roughening treatment using an oxidizing agent such as an alkaline permanganate solution is preferably performed by immersing the insulating layer in an oxidizing agent solution heated to 60°C to 100°C for 10 minutes to 30 minutes. The concentration of permanganate in the alkaline permanganate solution is preferably 5% by mass to 10% by mass. Examples of commercially available oxidizing agents include alkaline permanganate solutions such as "Concentrate Compact CP" and "Dosing Solution Securigans P" manufactured by Atotech Japan.

[0200] The neutralizing solution used in the roughening treatment is preferably an acidic aqueous solution, and a commercially available product such as "Reduction Solution Securigant P" manufactured by Atotech Japan can be mentioned.

[0201] The treatment with the neutralizing solution can be carried out by immersing the surface that has been roughened with an oxidizing agent in a neutralizing solution at 30° C. to 80° C. for 5 to 30 minutes. From the viewpoint of workability, etc., a method in which the object that has been roughened with an oxidizing agent is immersed in a neutralizing solution at 40° C. to 70° C. for 5 to 20 minutes is preferred.

[0202] In one embodiment, the root mean square roughness (Rq) of the insulating layer surface after the roughening treatment is preferably 500 nm or less, more preferably 400 nm or less, and even more preferably 300 nm or less. The lower limit is not particularly limited, and may be, for example, 1 nm or more, 2 nm or more, etc. The root mean square roughness (Rq) of the insulating layer surface can be measured using a non-contact surface roughness meter.

[0203] Step (V) is a step of forming a conductor layer, and the conductor layer is formed on the insulating layer. The conductor material used for the conductor layer is not particularly limited. In a preferred embodiment, the conductor layer contains one or more metals selected from the group consisting of gold, platinum, palladium, silver, copper, aluminum, cobalt, chromium, zinc, nickel, titanium, tungsten, iron, tin and indium. The conductor layer may be a single metal layer or an alloy layer, and examples of the alloy layer include layers formed from alloys of two or more metals selected from the above group (e.g., nickel-chromium alloy, copper-nickel alloy and copper-titanium alloy). Among these, from the viewpoints of versatility in forming the conductor layer, cost, ease of patterning, and the like, a single metal layer of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver, or copper, or an alloy layer of a nickel-chromium alloy, a copper-nickel alloy, or a copper-titanium alloy is preferred, a single metal layer of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver, or copper, or an alloy layer of a nickel-chromium alloy is more preferred, and a single metal layer of copper is even more preferred.

[0204] The conductor layer may be a single-layer structure or a multi-layer structure in which two or more single metal layers or alloy layers made of different kinds of metals or alloys are laminated. When the conductor layer has a multi-layer structure, the layer in contact with the insulating layer is preferably a single metal layer of chromium, zinc or titanium, or an alloy layer of a nickel-chromium alloy.

[0205] The thickness of the conductor layer depends on the desired design of the printed wiring board, but is generally 3 μm to 35 μm, and preferably 5 μm to 30 μm.

[0206] In one embodiment, the conductor layer may be formed by plating. For example, a conductor layer having a desired wiring pattern can be formed by plating the surface of the insulating layer by a conventionally known technique such as a semi-additive method or a full-additive method, and from the viewpoint of ease of production, it is preferable to form the conductor layer by the semi-additive method. An example of forming the conductor layer by the semi-additive method will be described below.

[0207] First, a plating seed layer is formed on the surface of an insulating layer by electroless plating. Next, a mask pattern is formed on the formed plating seed layer to expose a part of the plating seed layer corresponding to a desired wiring pattern. After a metal layer is formed on the exposed plating seed layer by electrolytic plating, the mask pattern is removed. Thereafter, unnecessary plating seed layer is removed by etching or the like to form a conductor layer having a desired wiring pattern.

[0208] In another embodiment, the conductor layer may be formed using a metal foil. When the conductor layer is formed using a metal foil, it is preferable to carry out step (V) between steps (I) and (II). For example, after step (I), the support is removed, and a metal foil is laminated on the exposed surface of the resin composition layer. The lamination of the resin composition layer and the metal foil may be carried out by a vacuum lamination method. The lamination conditions may be the same as those described for step (I). Next, step (II) is carried out to form an insulating layer. Thereafter, a conductor layer having a desired wiring pattern can be formed by a conventionally known technique such as a subtractive method or a modified semi-additive method, using the metal foil on the insulating layer.

[0209] The metal foil can be produced by a known method such as an electrolytic method, a rolling method, etc. Commercially available metal foils include, for example, HLP foil and JXUT-III foil manufactured by JX Nippon Mining & Metals Corporation, and 3EC-III foil and TP-III foil manufactured by Mitsui Mining & Smelting Co., Ltd.

[0210] <Semiconductor device> The semiconductor device of the present invention includes the printed wiring board of the present invention. The semiconductor device of the present invention can be manufactured by using the printed wiring board of the present invention.

[0211] Examples of the semiconductor device include various semiconductor devices used in electric appliances (for example, computers, mobile phones, digital cameras, and televisions) and vehicles (for example, motorcycles, automobiles, trains, ships, and aircraft). EXAMPLES

[0212] The present invention will be specifically described below with reference to examples. The present invention is not limited to these examples. In the following, "parts" and "%" representing amounts mean "parts by mass" and "% by mass", respectively, unless otherwise specified. Unless otherwise specified, the temperature and pressure conditions are room temperature (23°C) and atmospheric pressure (1 atm).

[0213] <Synthesis Example 1: Polyimide resin 1> A monomer composition was obtained by mixing 49.6g of 2,2-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride (BPADA), 50.4g of 4,4'-[1,4-phenylenebis[(1-methylethylidene)-4,1-phenyleneoxy]]bisbenzenamine (BPPAN), and 40g of toluene as a solvent in 400g of N,N-dimethylacetamide, and the mixture was stirred and reacted at room temperature and atmospheric pressure for 3 hours. As a result, a polyamic acid solution was obtained.

[0214] Subsequently, the polyamic acid solution was heated, and the temperature was kept at about 160°C, and the condensed water was removed azeotropically with toluene under a nitrogen stream. It was confirmed that a predetermined amount of water had accumulated in the water content receiver, and that no water was flowing out. After confirmation, the reaction solution was further heated and stirred at 200°C for 1 hour. Then, it was cooled. As a result, a varnish containing 20% ​​by mass of polyimide resin 1 (a polyimide resin having a repeating unit represented by the following formula (E)) as a non-volatile component was obtained. The glass transition temperature Tg of polyimide resin 1 was measured according to the above-mentioned method, and was found to be 210°C.

[0215] [ka]

[0216] <Example 1> The mixture consisted of 23 parts of an isopropylidene group-containing maleimide compound ("MIR-5000-60T" manufactured by Nippon Kayaku Co., Ltd., a toluene solution containing 60% by mass of non-volatile components, main component (non-volatile component): a maleimide compound represented by the following formula (A)), 20 parts of a vinylbenzyl-modified polyphenylene ether resin ("OPE-2St 1200" manufactured by Mitsubishi Gas Chemical Co., Ltd., a number average molecular weight of 1200, a toluene solution containing 65% by mass of non-volatile components), 0.5 parts of a polymerization initiator (peroxide "Perbutyl (registered trademark) C" manufactured by NOF Corporation), 0.5 parts of an inorganic filler (spherical silica ("SO-C2" manufactured by Admatechs Co., Ltd., average particle size 0.5 μm, specific surface area 5.8 m) surface-treated with an amine-based alkoxysilane compound ("KBM573" manufactured by Shin-Etsu Chemical Co., Ltd.), 2 A resin composition (resin varnish) was obtained by mixing 50 parts of a methyl ketone (100 parts by weight / g) and 10 parts of an ester-type phenoxy resin ("YL7891T30" manufactured by Mitsubishi Chemical Corporation, a 1:1 solution of MEK and cyclohexanone with a solid content of 30% by mass) and dispersing the mixture uniformly using a high-speed rotating mixer.

[0217] [ka]

[0218] <Example 2> A resin composition (resin varnish) was obtained in the same manner as in Example 1, except that 20 parts of a styrene-divinylbenzene copolymer ("ODV-XET(X04)" manufactured by Nippon Steel Chemical & Material Co., Ltd., weight average molecular weight 3110, vinyl group equivalent 380 g / eq., 65 mass% solution) was used instead of 20 parts of a vinylbenzyl-modified polyphenylene ether resin ("OPE-2St 1200" manufactured by Mitsubishi Gas Chemical Co., Ltd.).

[0219] <Example 3> A resin composition (resin varnish) was obtained in the same manner as in Example 1, except that 20 parts of a methacrylic-modified polyphenylene ether resin (SABIC Corp.'s "SA9000-111", number average molecular weight 1850 to 1950) was used instead of 20 parts of a vinylbenzyl-modified polyphenylene ether resin (Mitsubishi Gas Chemical Co., Inc.'s "OPE-2St 1200").

[0220] <Example 4> A resin composition (resin varnish) was obtained in the same manner as in Example 1, except that the amount of isopropylidene group-containing maleimide compound ("MIR-5000-60T" manufactured by Nippon Kayaku Co., Ltd.) used was changed from 23 parts to 18 parts, and further, 5 parts of a biphenylaralkyl type maleimide compound ("MIR-3000-70MT" manufactured by Nippon Kayaku Co., Ltd., a MEK / toluene mixed solution with a non-volatile content of 70%) was used.

[0221] <Example 5> A resin composition (resin varnish) was obtained in the same manner as in Example 1, except that the amount of isopropylidene group-containing maleimide compound ("MIR-5000-60T" manufactured by Nippon Kayaku Co., Ltd.) used was changed from 23 parts to 21 parts, and further, 2 parts of a liquid aliphatic maleimide compound ("BMI-1500" manufactured by Designer Molecules Inc.) was used.

[0222] <Example 6> A resin composition (resin varnish) was obtained in the same manner as in Example 1, except that 3 parts of an elastomer ("FG1924" styrene-ethylene / butylene-styrene block copolymer manufactured by Kraton) was used instead of 10 parts of an ester-type phenoxy resin ("YL7891T30" manufactured by Mitsubishi Chemical Corporation, a 1:1 solution of MEK with a solid content of 30% by mass and cyclohexanone).

[0223] <Example 7> A resin composition (resin varnish) was obtained in the same manner as in Example 1, except that the amount of ester-type phenoxy resin ("YL7891T30" manufactured by Mitsubishi Chemical Corporation, a 1:1 solution of MEK and cyclohexanone with a solid content of 30 mass %) was changed from 10 parts to 5 parts, and 7 parts of the polyimide resin 1 obtained in Synthesis Example 1 were added.

[0224] <Example 8> A resin composition (resin varnish) was obtained in the same manner as in Example 6, except that the amount of "SO-C2" manufactured by Admatechs was changed from 50 parts to 40 parts, and 10 parts of an inorganic filler having hollow portions (spherical silica having hollow portions ("BA-S" manufactured by JGC Catalysts and Chemicals, average particle size 2.6 μm) surface-treated with an amine-based alkoxysilane compound ("KBM573" manufactured by Shin-Etsu Chemical Co., Ltd.)) was used instead.

[0225] <Comparative Example 1> A resin composition (resin varnish) was obtained in the same manner as in Example 1, except that no isopropylidene group-containing maleimide compound ("MIR-5000-60T" manufactured by Nippon Kayaku Co., Ltd.) was used, and the amount of vinylbenzyl-modified polyphenylene ether resin ("OPE-2St 1200" manufactured by Mitsubishi Gas Chemical Co., Ltd.) used was changed from 20 parts to 40 parts.

[0226] <Comparative Example 2> A resin composition (resin varnish) was obtained in the same manner as in Example 1, except that no isopropylidene group-containing maleimide compound ("MIR-5000-60T" manufactured by Nippon Kayaku Co., Ltd.) was used, and 40 parts of a styrene-divinylbenzene copolymer ("ODV-XET(X04)" manufactured by Nippon Steel Chemical & Material Co., Ltd.) was used instead of 20 parts of a vinylbenzyl-modified polyphenylene ether resin ("OPE-2St 1200" manufactured by Mitsubishi Gas Chemical Co., Ltd.).

[0227] <Comparative Example 3> A resin composition (resin varnish) was obtained in the same manner as in Example 1, except that no isopropylidene group-containing maleimide compound ("MIR-5000-60T" manufactured by Nippon Kayaku Co., Ltd.) was used, and 40 parts of a methacrylic-modified polyphenylene ether resin ("SA9000-111" manufactured by SABIC Corporation, number average molecular weight 1850 to 1950) was used instead of 20 parts of a vinylbenzyl-modified polyphenylene ether resin ("OPE-2St 1200" manufactured by Mitsubishi Gas Chemical Co., Ltd.).

[0228] <Comparative Example 4> A resin composition (resin varnish) was obtained in the same manner as in Example 1, except that 20 parts of a biphenylaralkyl-type maleimide compound ("MIR-3000-70MT" manufactured by Nippon Kayaku Co., Ltd., a MEK / toluene mixed solution with a non-volatile content of 70%) was used instead of the isopropylidene group-containing maleimide compound ("MIR-5000-60T" manufactured by Nippon Kayaku Co., Ltd.).

[0229] <Test Example 1: Measurement of relative dielectric constant (Dk) and dielectric loss tangent (Df)> A polyethylene terephthalate film with a release layer ("AL5" manufactured by Lintec Corporation, thickness 38 μm) was prepared as a support. On the release layer of this support, the resin compositions (resin varnishes) obtained in the examples and comparative examples were uniformly applied so that the thickness of the resin composition layer after drying was 40 μm. Thereafter, the resin compositions were dried at 80°C to 100°C (average 90°C) for 4 minutes to obtain a resin sheet including a support and a resin composition layer.

[0230] The obtained resin sheet was heated at 190°C for 90 minutes to heat-cure the resin composition layer. The support was then peeled off to obtain a cured product of the resin composition. This cured product was cut into a test piece having a width of 2 mm and a length of 80 mm. The relative dielectric constant (Dk) and dielectric loss tangent (Df) of the test piece were measured at a measurement frequency of 5.8 GHz and a measurement temperature of 23°C by a cavity resonance perturbation method using an Agilent Technologies "HP8362B". Measurements were performed on three test pieces, and the average values ​​are shown in Table 1 below.

[0231] <Test Example 2: Measurement of copper plating peel strength> (1) Surface preparation for inner layer circuit boards A glass cloth-based epoxy resin double-sided copper-clad laminate (copper foil thickness 18 μm, board thickness 0.4 mm, Panasonic "R1515A") with inner layer circuits (copper foil) on both sides was prepared as an inner layer circuit board. Both sides of this inner layer circuit board were etched by 1 μm using MEC's ​​"CZ8101" to roughen the copper surface.

[0232] (2) Lamination of resin sheet The resin sheet obtained in Test Example 1 was laminated on both sides of the inner layer circuit board using a batch type vacuum pressure laminator (Nikko Materials Co., Ltd., 2-stage build-up laminator, CVP700). This lamination was performed so that the resin composition layer of the resin sheet was in contact with the inner layer circuit board. This lamination was also performed by reducing the pressure for 30 seconds to 13 hPa or less, and pressing at 130°C and a pressure of 0.74 MPa for 45 seconds. Next, a heat press was performed at 120°C and a pressure of 0.5 MPa for 75 seconds.

[0233] (3) Curing of the resin composition The laminated resin sheet and the inner layer circuit board were heated at 130° C. for 30 minutes, and then heated at 170° C. for 30 minutes to harden the resin composition and form an insulating layer. The support was then peeled off to obtain a laminated substrate having an insulating layer, an inner layer circuit board, and an insulating layer in this order.

[0234] (4) Roughening treatment The laminated substrate was immersed in a swelling solution (Atotech Japan's Swelling Dip Securigant P (aqueous solution of glycol ethers and sodium hydroxide) containing diethylene glycol monobutyl ether). The laminated substrate was then immersed in a roughening solution (Atotech Japan's Concentrate Compact P (aqueous solution of KMnO4: 60 g / L and NaOH: 40 g / L)) at 80°C for 20 minutes. The laminated substrate was then immersed in a neutralizing solution (Atotech Japan's Reduction Shalusin Securigant P (aqueous solution of sulfuric acid)) at 40°C for 5 minutes. The laminated substrate was then dried at 80°C for 30 minutes to obtain "Evaluation Substrate A."

[0235] (5) Semi-additive plating: Evaluation substrate A was immersed in an electroless plating solution containing PdCl2 at 40°C for 5 minutes, and then immersed in an electroless copper plating solution at 25°C for 20 minutes. It was then heated at 150°C for 30 minutes and annealed. An etching resist was then formed, and a pattern was formed by etching. Copper sulfate electrolytic plating was then performed to form a conductor layer with a thickness of 20 μm. An annealing process was then performed at 190°C for 60 minutes to obtain "evaluation substrate B."

[0236] (6) Measurement of copper plating peel strength A cut was made in the conductor layer of evaluation board B to surround a rectangular portion 10 mm wide and 100 mm long. One end of the rectangular portion was peeled off and held with a gripper (Autocom type testing machine "AC-50C-SL" manufactured by TSE Corporation). The rectangular portion was peeled off vertically at room temperature with the gripper at a speed of 50 mm / min, and the load (kgf / cm) when 35 mm had been peeled off was measured as the copper plating peel strength, and is shown in Table 1 below.

[0237] <Test Example 3: Measurement of surface roughness Ra> The arithmetic mean roughness Ra of the surface of the insulating layer of the evaluation substrate A produced in Test Example 2(4) was measured. The measurement was performed using a non-contact surface roughness meter (WYKO NT3300 manufactured by B-CO Instruments) in VSI mode with a 50x lens, with a measurement range of 121 μm × 92 μm. This measurement was performed at 10 measurement points, and the average values ​​are shown in Table 1 below.

[0238] <Test Example 4: Measurement of minimum melt viscosity> The resin sheet obtained in Test Example 1 was peeled off from the support film and measured using a dynamic viscoelasticity measuring device G-3000 manufactured by UBM at a frequency of 1 Hz, a strain of 5 degrees, a load of 100 g, a heating rate of 5°C / min, and a temperature range of 60°C to 180°C.

[0239] The amounts of raw materials used and the non-volatile component contents of the resin compositions of the Examples and Comparative Examples, as well as the measurement results of the Test Examples, are shown in Table 1 below.

[0240] [Table 1]

[0241] Referring to Table 1, in Comparative Examples 1 to 3 in which no maleimide compound was used, the copper plating peel strength was low. In Comparative Example 4 in which an aromatic polymaleimide compound having no isopropylidene group was used as the maleimide compound, the minimum melt viscosity was high and the dielectric loss tangent (Df) was also high. In contrast, it can be seen that these problems can be overcome when the resin composition of the present invention containing (A) the specific maleimide compound and (B) a resin having a vinylphenyl group and / or a (meth)acryloyl group is used.

[0242] This application is based on patent application No. 2020-189016 (filed on November 12, 2020) filed with the Japan Patent Office, the contents of which are incorporated in their entirety herein.

Claims

1. A resin composition comprising: (A) a maleimide compound having an isopropylidene group bonded to two aromatic carbon atoms of different aromatic rings; (B) a resin having a vinylphenyl group; and (C) an inorganic filler, The component (A) is represented by the formula (A2): 【Chemistry 1】 [In the formula, ring A and ring B each independently represent an aromatic ring which may have a substituent; and a represents an integer of 1 or more.] The maleimide compound is represented by the formula: The content of the (B) component is 5% by mass to 25% by mass, based on 100% by mass of the non-volatile components in the resin composition; A resin composition, wherein the content of the component (C) is 50% by mass to 90% by mass, assuming that the total amount of non-volatile components in the resin composition is 100% by mass.

2. The component (A) is represented by the formula (A-1): 【Chemistry 2】 [In the formula, R 1 and R 2 each independently represents an alkyl group or an aryl group; a represents an integer of 1 or more; and x and y each independently represent 0, 1, 2, or 3. The resin composition according to claim 1 , comprising a maleimide compound represented by the formula:

3. The resin composition according to claim 1 or 2, wherein a is an integer from 2 to 10.

4. The resin composition according to any one of claims 1 to 3, wherein the component (B) is a thermoplastic resin having a vinyl phenyl group.

5. The resin composition according to any one of claims 1 to 4, wherein the component (B) is a resin selected from a modified polyphenylene ether resin having a vinylphenyl group and a modified polystyrene resin having a vinylphenyl group.

6. The resin composition according to any one of claims 1 to 5, wherein the content of the component (A) is 5% by mass to 30% by mass, based on 100% by mass of non-volatile components in the resin composition.

7. The resin composition according to any one of claims 1 to 6, wherein the content of the component (B) is 15% by mass to 25% by mass, based on 100% by mass of non-volatile components in the resin composition.

8. The resin composition according to any one of claims 1 to 7, wherein a mass ratio of the component (A) to the component (B) (component (A) / component (B)) is 0.3 to 3.

9. The resin composition according to any one of claims 1 to 8, wherein the content of the component (C) is 50% by mass to 80% by mass, based on 100% by mass of non-volatile components in the resin composition.

10. The resin composition according to any one of claims 1 to 9, wherein a mass ratio of the component (A) to the component (C) (component (A) / component (C)) is 0.1 to 1.

11. The resin composition according to any one of claims 1 to 10, further comprising: (E) a thermoplastic resin and / or (F) an elastomer.

12. The resin composition according to any one of claims 1 to 11, wherein the dielectric loss tangent (Df) of a cured product of the resin composition is 0.004 or less when measured at 5.8 GHz and 23 ° C.

13. The resin composition according to any one of claims 1 to 12, wherein the dielectric constant (Dk) of a cured product of the resin composition is 3.5 or less when measured at 5.8 GHz and 23°C.

14. A cured product of the resin composition according to any one of claims 1 to 13.

15. A sheet-like laminate material comprising the resin composition according to any one of claims 1 to 13.

16. A resin sheet comprising a support and a resin composition layer formed from the resin composition according to any one of claims 1 to 13 provided on the support.

17. A printed wiring board comprising an insulating layer made of a cured product of the resin composition according to any one of claims 1 to 13.

18. A semiconductor device comprising the printed wiring board according to claim 17.

Citation Information

Patent Citations

  • Resin composition and resin sealing type semiconductor apparatus

    JP1997296105A

  • Curable electron donor compound

    JP2002060364A

  • Thermosetting resin composition and semiconductor device using the same

    JP2016164257A

  • Maleimide resin, curable resin composition and cured product thereof

    JP6752390B1

  • JPP6752390B