Solid electrolytes and gas sensors

A solid electrolyte with controlled X-ray diffraction intensity ratios and phase transitions addresses the peeling issue in gas sensors, ensuring robust bonding and accurate readings under severe temperature fluctuations.

JP7593493B2Active Publication Date: 2024-12-03DENSO CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023525657
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-06-01
Filing Date
2022-04-21
Publication Date
2024-12-03
Estimated Expiration
2042-04-21

AI Technical Summary

Technical Problem

Conventional solid electrolytes experience peeling of the metal layer due to differences in thermal expansion coefficients when exposed to harsher cooling and heating cycles, leading to increased resistance fluctuations and decreased sensor accuracy in gas sensors.

Method used

A solid electrolyte made of partially stabilized zirconia with specific X-ray diffraction intensity ratios and phase transition properties, allowing for volume changes that maintain bonding strength with the metal layer during severe temperature cycles.

Benefits of technology

The solution effectively suppresses peeling of metal layers and electrodes, ensuring high sensor accuracy by maintaining interface bonding strength even under increased cooling and heating cycles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007593493000003
    Figure 0007593493000003
  • Figure 0007593493000004
    Figure 0007593493000004
  • Figure 0007593493000005
    Figure 0007593493000005
Patent Text Reader

Abstract

This solid electrolyte (1) is configured from partially stabilized zirconia and satisfies formulas 1 and 2. Formula 1: 0.05≤IM1 / ICT1≤0.4. Formula 2: −0.5≤(IM3×ICT2) / (IM2×ICT3)−1≤−0.1. In the formulas, IM1 is the X-ray diffraction intensity of a (11−1) plane of M phase at 27°C, ICT1 is the total X-ray diffraction intensity of a (111) plane of C phase and a (101) plane of T phase at 27°C, IM2 is the X-ray diffraction intensity of the (11−1) plane of M phase at 500°C, ICT2 is the total X-ray diffraction intensity of the (111) plane of C phase and the (101) plane of T phase at 500°C, IM3 is the X-ray diffraction intensity of the (11−1) plane of M phase at 850°C, and ICT3 is the total X-ray diffraction intensity of the (111) plane of C phase and the (101) plane of T phase at 850°C.
Need to check novelty before this filing date? Find Prior Art

Description

CROSS-REFERENCE TO RELATED APPLICATIONS

[0001] This application is based on Japanese Application No. 2021-92313 filed on June 1, 2021, the contents of which are incorporated herein by reference. [Technical field]

[0002] The present disclosure relates to a solid electrolyte and a gas sensor. [Background technology]

[0003] Conventionally, a solid electrolyte made of partially stabilized zirconia, in which a stabilizer such as yttria is dissolved in zirconia, has been known. This type of solid electrolyte may be used with a metal layer formed on the surface. For example, in the automotive field, a gas sensor is known in which an electrode or lead wire made of Pt or the like is formed on the surface of a solid electrolyte made of yttria partially stabilized zirconia.

[0004] Specifically, for example, Patent Document 1 describes a gas sensor that includes a solid electrolyte and an alumina substrate that is integrally provided with the solid electrolyte. In Patent Document 1, the solid electrolyte is made of partially stabilized zirconia in which C phase, M phase, and T phase are mixed. The difference in thermal expansion coefficient between the alumina substrate and the partially stabilized zirconia is within a range of 0% to 0.2%. In the partially stabilized zirconia, I(11-1) / I(111), which is the diffraction intensity ratio of the X-ray diffraction intensity of the (111) plane of the M phase to the X-ray diffraction intensity of the (11-1) plane of the C phase, is 0.05 to 0.4. The change in the diffraction intensity ratio after the solid electrolyte is heated to 200° C. for 1000 hours is within a range of −0.05 to +0.10. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 3873302 Summary of the Invention

[0006] In recent years, solid electrolytes have been exposed to more severe thermal cycles than before. For example, in the above-mentioned gas sensor, the sensor operating temperature has been increased due to changes in the sensor mounting position to be closer to the engine or catalytic converter in response to strict fuel consumption and exhaust gas regulations. In addition, in hybrid vehicles and idling-stop vehicles in which the engine is frequently stopped and started, the heater is turned off when the engine is stopped from the viewpoint of reducing power consumption. Therefore, in recent gas sensors, the number of repeated thermal cycles in which the sensor is rapidly cooled from a high sensor operating temperature to a low temperature, and then heated again from a low temperature to the sensor operating temperature is increasing. Therefore, recent gas sensors are exposed to repeated temperature changes between room temperature and the sensor operating temperature more than ever before.

[0007] When a metal layer is formed on the surface of a solid electrolyte, if the solid electrolyte is subjected to a thermal cycle that is more severe than the conventional one, the interfacial bonding strength decreases due to the difference in thermal expansion coefficient between the solid electrolyte and the metal layer, and the metal layer becomes easily peeled off from the solid electrolyte. For example, in the case of a gas sensor, if an electrode peels off from the solid electrolyte, the resistance fluctuation increases and the sensor accuracy decreases.

[0008] The present disclosure aims to provide a solid electrolyte capable of suppressing peeling of a metal layer even when the solid electrolyte has a metal layer formed on its surface and is exposed to more severe thermal cycles than conventional solid electrolytes, and a gas sensor using the solid electrolyte.

[0009] One aspect of the present disclosure is a solid electrolyte composed of partially stabilized zirconia in which a stabilizer is solid-dissolved in zirconia, The solid electrolyte satisfies the relationships of the following formulas 1 and 2. 0.05≦I M1 / I CT1 ≦0.4...Equation 1 -0.5≦(I M3 ×I CT2 ) / (I M2 ×I CT3 )-1≦-0.1...Equation 2 However, in formula 1 and formula 2, I M1: X-ray diffraction intensity of the (11-1) plane of the M phase at 27℃ I CT1 : The combined X-ray diffraction intensity of the (111) plane of the C phase and the (101) plane of the T phase at 27°C I M2 : X-ray diffraction intensity of the (11-1) plane of the M phase at 500℃ I CT2 : The combined X-ray diffraction intensity of the (111) plane of the C phase and the (101) plane of the T phase at 500℃ I M3 : X-ray diffraction intensity of the (11-1) plane of the M phase at 850℃ I CT3 : Combined X-ray diffraction intensity of the (111) plane of the C phase and the (101) plane of the T phase at 850℃

[0010] Another aspect of the present disclosure is a gas sensor having the above solid electrolyte.

[0011] The solid electrolyte has the above-mentioned configuration, and therefore, even when the solid electrolyte has a metal layer formed on its surface and is subjected to a thermal cycle more severe than in the past, the volume change associated with the phase transition maintains the bonding strength of the interface between the solid electrolyte and the metal layer during use, and peeling of the metal layer can be suppressed.

[0012] The gas sensor also contains the solid electrolyte. Therefore, even if the number of repeated cooling / heating cycles between the low temperature at engine stop / start (including restarting a hybrid vehicle or a vehicle equipped with an idling stop function) and the high temperature at which the sensor is used increases, the gas sensor can suppress peeling of the electrodes and lead wires made of metal layers. Therefore, the gas sensor can suppress resistance fluctuations and provide a gas sensor with high sensor accuracy.

[0013] Note that the reference characters in parentheses in the claims indicate the corresponding relationship with the specific means described in the embodiments described later, and are not intended to limit the technical scope of the present disclosure. [Brief description of the drawings]

[0014] The above and other objects, features and advantages of the present disclosure will become more apparent from the following detailed description taken in conjunction with the accompanying drawings, in which: [Figure 1] FIG. 1 is an explanatory diagram showing a schematic microstructure of the solid electrolyte of embodiment 1 (temperature 27° C.); [Diagram 2] FIG. 2 is an explanatory diagram showing an example of an XRD pattern (temperature: 850° C.) of the solid electrolyte of embodiment 1; [Diagram 3] FIG. 3 is an explanatory diagram showing a relationship between temperature and IM / ICT value for the solid electrolyte of the first embodiment and a conventional solid electrolyte; [Figure 4] FIG. 4 is an explanatory diagram showing a typical behavior of a conventional solid electrolyte having a metal layer formed on its surface when the temperature is changed from the initial state to 850° C. [Diagram 5] FIG. 5 is an explanatory diagram showing a typical behavior of the solid electrolyte of embodiment 1 having a metal layer formed on its surface when the temperature is changed from the initial state to 850° C. to 27° C.; [Figure 6] FIG. 6 is an explanatory diagram illustrating an outline of a method for producing a solid electrolyte according to the first embodiment; [Figure 7] FIG. 7 is an explanatory diagram showing a part of a phase diagram of zirconia in which Y2O3 is dissolved; [Figure 8] FIG. 8 is an explanatory view showing a schematic example of a method for producing a solid electrolyte according to the first embodiment; [Figure 9] FIG. 9 is an explanatory diagram illustrating an example of a crystal phase ratio in the solid electrolyte of the first embodiment; [Figure 10] FIG. 10 is an explanatory diagram of a method for determining an average particle size of an M phase in the solid electrolyte of the first embodiment; [Figure 11] FIG. 11 is a cross-sectional view of a gas sensor (cup-shaped) according to embodiment 2; [Figure 12] FIG. 12 is an enlarged cross-sectional view of a part of a gas sensor element included in the gas sensor of FIG. 11; [Figure 13] FIG. 13 is a cross-sectional view of a gas sensor (multilayer type) according to embodiment 3; [Figure 14] FIG. 14 is an enlarged cross-sectional view of the gas sensor element included in the gas sensor of FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] (Embodiment 1) The solid electrolyte of embodiment 1 will be described with reference to Figures 1 to 10. In the following, reference numerals other than those for the solid electrolyte 1 of embodiment 1 will be used only in the description that particularly refers to the drawings.

[0016] As illustrated in FIG. 1, the solid electrolyte 1 of this embodiment is made of partially stabilized zirconia in which a stabilizer is dissolved in zirconia.

[0017] Examples of the stabilizer include yttria (Y2O3), calcia (CaO), magnesia (MgO), scandia (Sc2O3), and ytterbia (Yb2O3). These can be used alone or in combination of two or more. The content of the stabilizer can be, for example, 3 mol% to 11 mol%. The content of the stabilizer means the amount of stabilizer contained in the entire solid electrolyte 1 (the amount of stabilizer doped in the solid electrolyte 1). From the viewpoint of chemical stability, the stabilizer can preferably contain yttria, and more preferably is yttria. The content of yttria can be 3 mol% to 11 mol% from the viewpoints of the strength of the solid electrolyte 1 and the suppression of peeling of the metal layer by reducing the difference in thermal expansion coefficient with the metal layer formed on the surface of the solid electrolyte 1.

[0018] The solid electrolyte 1 of the present embodiment satisfies the relationships of the following formulas 1 and 2. 0.05≦I M1 / I CT1 ≦0.4...Equation 1 -0.5≦(I M3 ×I CT2 ) / (I M2 ×I CT3 )-1≦-0.1...Equation 2 However, in formula 1 and formula 2, I M1 : X-ray diffraction intensity of the (11-1) plane of the M phase at 27℃ I CT1 : The combined X-ray diffraction intensity of the (111) plane of the C phase and the (101) plane of the T phase at 27°C I M2 : X-ray diffraction intensity of the (11-1) plane of the M phase at 500℃ I CT2 : The combined X-ray diffraction intensity of the (111) plane of the C phase and the (101) plane of the T phase at 500℃ I M3 : X-ray diffraction intensity of the (11-1) plane of the M phase at 850℃ I CT3 : Combined X-ray diffraction intensity of the (111) plane of the C phase and the (101) plane of the T phase at 850℃

[0019] The C phase, M phase, and T phase are crystalline phases, with the C phase being a cubic phase, the M phase being a monoclinic phase, and the T phase being a tetragonal phase. Miller indices indicating crystal planes in a crystal structure are generally expressed with a bar above the number when a minus (-) is added, but in this specification, they are expressed with a minus (-) before the number (for example, -1 in (11-1) of the above M phase).

[0020] Formula 1 and Formula 2 have the following technical significance. In a solid electrolyte 1 made of partially stabilized zirconia, at 27°C, the C phase, the M phase, and the T phase, or the C phase and the M phase may be mixed. When 27°C is a low temperature and 850°C is a high temperature, depending on the amount of the stabilizer dissolved in the M phase, when the temperature changes from a low temperature to a high temperature, the M phase may undergo a phase transition to the T phase, causing a volumetric contraction, and when the temperature changes from a high temperature to a low temperature, the T phase may undergo a phase transition to the M phase, causing a volumetric expansion. The temperature for the phase transformation between the M phase and the T phase is about 600°C. As a result of various experiments described later, the inventors have found that when the M phase is present at a specific abundance ratio at a low temperature of 27°C, and when 500°C, a temperature lower than the phase transition temperature, is used as the reference temperature in consideration of variation, when the M→T phase change rate, which indicates how much the abundance ratio of the M phase has decreased due to a temperature change from 500°C to a high temperature of 850°C relative to the abundance ratio of the M phase at 500°C, is within a specific range, peeling of the metal layer can be suppressed even when exposed to a thermal cycle that is more severe than before.

[0021] Here, the diffraction intensity ratio of the X-ray diffraction intensity of the (11-1) plane of the M phase at 27 °C to the total X-ray diffraction intensity of the (111) plane of the C phase and the (101) plane of the T phase at 27 °C is defined as I M1 / I CT1 Let us assume that M1 / I CT1 means the abundance ratio of the M phase at 27°C (300K). The diffraction intensity ratio of the X-ray diffraction intensity of the (11-1) plane of the M phase at 500°C to the combined X-ray diffraction intensity of the (111) plane of the C phase and the (101) plane of the T phase at 500°C is defined as I M2 / I CT2 Let us assume that M2 / I CT2 means the abundance ratio of the M phase at 500°C (773K). The diffraction intensity ratio of the X-ray diffraction intensity of the (11-1) plane of the M phase at 850°C to the combined X-ray diffraction intensity of the (111) plane of the C phase and the (101) plane of the T phase at 850°C is defined as I M3 / I CT3 Let us assume that M3 / I CT3means the abundance ratio of M phase at 850℃ (1123K). The diffraction intensity ratio of the X-ray diffraction intensity of the (11-1) plane of M phase at a given temperature to the total X-ray diffraction intensity of the (111) plane of C phase and the (101) plane of T phase at a given temperature is defined as I M / I CT Let us assume that M / I CT means the abundance ratio of the M phase at a given temperature. The X-ray diffraction intensity of a specific crystal plane of a given crystal phase at each temperature can be determined from the peak intensity of a specific crystal plane of a given crystal phase by measuring an X-ray diffraction pattern (XRD pattern) at each temperature using an X-ray diffraction method (X-ray source: CuKα, 2θ / θ measurement) for a surface of a solid electrolyte polished with a grit size of #1500. FIG. 2 shows an example of an X-ray diffraction pattern of solid electrolyte 1 at 850°C. In FIG. 2, the symbol 1M is the peak of the M phase (11-1) plane, and the symbol 1CT is the total peak of the C phase (111) plane and the T phase (101) plane.

[0022] As shown in Equation 1, I M1 / I CT1 is set to 0.05 or more and 0.4 or less. When the solid electrolyte 1 is applied to, for example, a gas sensor, a metal layer made of Pt or the like for an electrode or lead wire is formed on the surface of the solid electrolyte 1. The solid electrolyte 1 may be used not only with the metal layer but also with other members (different materials) such as alumina. M1 / I CT1 If I is less than 0.05, the amount of the M phase in the entire solid electrolyte 1 becomes too small, and the thermal expansion coefficient of the solid electrolyte 1 in the temperature range of 400° C. to 600° C. becomes large, and the matching of the thermal expansion coefficient with other members becomes poor. M1 / I CT1 If I exceeds 0.4, the amount of M phase in the entire solid electrolyte 1 becomes too large, and the thermal expansion coefficient of the solid electrolyte 1 in the temperature range of 400° C. to 600° C. becomes small, and the matching of the thermal expansion coefficient with other members decreases. From the viewpoint of the matching of the thermal expansion coefficient with the metal layer and other members, the solid electrolyte 1 is preferably in a range of 0.07≦I M1 / I CT1 ≦0.38, more preferably 0.09≦I M1 / ICT1 ≦0.35, more preferably 0.1≦I M1 / I CT1 ≦0.3. Specifically, the thermal expansion coefficient of the solid electrolyte 1 can be, for example, 7.0 ppm / ° C. or more and 9.5 ppm / ° C. or less. A method for measuring the thermal expansion coefficient of the solid electrolyte 1 will be described later in the Experimental Examples.

[0023] As shown in Equation 2, (I M3 ×I CT2 ) / (I M2 ×I CT3 )-1 is considered to be greater than or equal to -0.5 and less than or equal to -0.1. M3 ×I CT2 ) / (I M2 ×I CT3 Specifically, the M→T phase change rate, which indicates how much the proportion of the M phase has decreased (how much the M phase has changed to the T phase) due to a temperature change from 500°C to 850°C, relative to the proportion of the M phase at 500°C, can be calculated from the following formula. (I M3 / I CT3 -I M2 / I CT2 ) / (I M2 / I CT2 ) When this formula is calculated, it is shown in Equation 2 (I M3 ×I CT2 ) / (I M2 ×I CT3 )-1 is derived. Therefore, (I M3 ×I CT2 ) / (I M2 ×I CT3 )-1 means the M→T phase change rate.

[0024] Conventionally, a solid electrolyte made of partially stabilized zirconia containing a stabilizer such as yttria in an amount of about 3 mol % to 11 mol % in the entire solid electrolyte is known. This conventional solid electrolyte is generally prepared by mixing ZrO2 with a predetermined amount of stabilizer, granulating, molding, and firing. In the conventional solid electrolyte prepared in this manner, at least the C phase and the M phase are mixed at 27°C. However, in the solid electrolyte prepared by the above-mentioned method, the M phase contains almost no stabilizer, and does not undergo a phase transition to the T phase until the temperature exceeds the operating temperature of the gas sensor. Therefore, the conventional solid electrolyte has a diffraction intensity ratio I M / I CT There is almost no change in the linear thermal expansion coefficient of the solid electrolyte 9. Therefore, as shown in FIG. 4, even if a metal layer 91 (such as Pt plating forming an electrode or lead wire in the case of a gas sensor) is bonded to the surface of the solid electrolyte 9 in the initial state at a low temperature, when the temperature reaches a high temperature of 850° C., the metal layer 91 peels off from the solid electrolyte 9 due to the difference in thermal expansion coefficient between the solid electrolyte 9 and the metal layer 91, resulting in a peeled portion 92. For example, the linear thermal expansion coefficient of yttria-partially stabilized zirconia is about 8 ppm / K, and the linear thermal expansion coefficient of Pt is about 10 ppm / K. The double-ended arrow Y1 shown in FIG. 4 is a schematic example of the linear thermal expansion coefficient of yttria-partially stabilized zirconia, and the double-ended arrow Y2 shown in FIG. 4 is a schematic example of the linear thermal expansion coefficient of Pt. Thus, the linear thermal expansion coefficient of the metal constituting the metal layer is larger than the linear thermal expansion coefficient of the solid electrolyte. In the case of a gas sensor, when an electrode peels off from the solid electrolyte, the resistance fluctuation increases and the sensor accuracy decreases. Furthermore, if the lead wire peels off from the solid electrolyte, the lead wire may break, causing a loss of sensor function.

[0025] In contrast, in the solid electrolyte 1 of the present embodiment, the M phase exists within a range that satisfies the formula 1. The diffraction intensity ratio I M / I CTAs shown in L2 of FIG. 3, changes greatly in the temperature range from 500°C to 850°C. Specifically, the solid electrolyte 1 of this embodiment can undergo a phase transition from the M phase to the T phase within a range that satisfies formula 2 by a temperature change from 500°C to a high temperature of 850°C. Therefore, in the case where a metal layer 91 (Pt plating forming an electrode or lead wire in the example of a gas sensor) is bonded to the surface of the solid electrolyte 1 of this embodiment as shown in FIG. 5, when the temperature rises from a low-temperature initial state to a high temperature of 850°C, a part of the M phase contained in the solid electrolyte 1 undergoes a phase transition to the T phase, causing a volume reduction, and a gap 93 is generated around the part. Then, a part of the metal layer 91 softened at high temperature enters the gap. After that, when the temperature drops to a low temperature, the T phase undergoes a phase transition to the M phase, causing a volume expansion, and a compressive stress 94 is generated around the part of the metal layer 91 that has entered the gap 93, and an anchor effect is generated by a part of the metal layer 91 biting into the surface of the solid electrolyte 1.

[0026] Due to the above-mentioned estimated mechanism, even when the solid electrolyte 1 of the present embodiment, with a metal layer formed on its surface, is subjected to a more severe thermal cycle than in the past, the volume change associated with the phase transition maintains the bonding strength of the interface between the solid electrolyte and the metal layer during use, making it possible to suppress peeling of the metal layer.

[0027] As shown in Equation 2 (I M3 ×I CT2 ) / (I M2 ×I CT3 )-1 becomes less than -0.5, I M1 / I CT1 When is relatively large, the phase transition strain becomes large and the strength of the solid electrolyte 1 decreases. On the other hand, when (I M3 ×I CT2 ) / (I M2 ×I CT3 If (I )-1 exceeds -0.1, the bonding strength of the interface between the solid electrolyte 1 and the metal layer decreases when exposed to severe thermal cycles, causing the metal layer to peel off. As a result, the resistance fluctuation increases. From the viewpoint of the balance between strength and the prevention of peeling of the metal layer during thermal cycles, the solid electrolyte 1 preferably satisfies -0.48≦(I M3 ×ICT2 ) / (I M2 ×I CT3 ) - 1 ≤ -0.12, more preferably, -0.45 ≤ (I M3 ×I CT2 ) / (I M2 ×I CT3 ) - 1 ≤ -0.15, even more preferably, -0.43 ≤ (I M3 ×I CT2 ) / (I M2 ×I CT3 ) - 1 ≤ -0.17, even more preferably, -0.4 ≤ (I M3 ×I CT2 ) / (I M2 ×I CT3 ) - 1 ≤ -0.2 can be satisfied.

[0028] The solid electrolyte 1 of the present embodiment can be manufactured, for example, as follows. In the conventional method for manufacturing a solid electrolyte, a stabilizer such as Y2O3 in a predetermined amount x mol% (for example, when producing partially stabilized zirconia in which 7 mol% of a stabilizer is dissolved, x = 7 mol%) and ZrO2 that are finally required are mixed, granulated, molded, and fired to produce a solid electrolyte.

[0029] In contrast, in the method for manufacturing the solid electrolyte 1 of the present embodiment, as shown in the outline in FIG. 6, ZrO2 containing a stabilizer in an amount capable of undergoing a phase transition from the M phase to the T phase with a temperature change from 500°C to 850°C (hereinafter, this may be referred to as the easily phase-transitionable M phase 102) is separately produced. When the amount of the stabilizer contained in the easily phase-transitionable M phase 102 is y mol%, 0 < y < x is satisfied. That is, a part of the partially stabilized zirconia raw material is first made into the easily phase-transitionable M phase 102. Then, the easily phase-transitionable M phase 102 is added to the mixed raw material containing the stabilizer 103 and ZrO2 104 so that partially stabilized zirconia in which a predetermined amount x mol% of the stabilizer is finally dissolved can be obtained, and granulated to obtain granulated powder 105. Next, the granulated powder 105 is molded into a molded body. Next, the molded body is fired to obtain a fired body. Thereby, the solid electrolyte 1 of the present embodiment can be manufactured.

[0030] The manufacturing method of the solid electrolyte 1 of this embodiment will be described in more detail using the case where the solid electrolyte 1 is made of yttria partially stabilized zirconia as an example. FIG. 7 shows a part of a phase diagram of zirconia in which Y2O3 is dissolved. In the phase diagram, the horizontal axis is the amount of Y2O3 dissolved (mol%), and the vertical axis is temperature (°C). According to the phase diagram, when Y2O3 is not dissolved, it is understood that the M phase does not undergo a phase transition to the T phase in the temperature range from 500°C to 850°C. In contrast, when the amount of Y2O3 dissolved is 1 mol% or more, it is understood that the phase transition from the M phase to the T phase occurs by 850°C. Note that when the amount of Y2O3 dissolved exceeds 2 mol%, the concentration of Y2O3 increases in the process after the preparation process of the easy-to-phase-transition M phase, and there is a tendency for the easy-to-phase-transition M phase to become a T phase rather than an M phase. Therefore, it is preferable that the easy-to-phase-transition M phase is composed of ZrO2 in which 1 mol% to 2 mol% of Y2O3 is dissolved. Although the case where Y2O3 is selected as the stabilizer is shown here, it is possible to form an easy-to-transition M phase for other stabilizers using a similar approach based on the respective phase diagrams.

[0031] 8 shows a specific example of a method for producing the solid electrolyte 1 of this embodiment. Here, a case will be described in which an easy-to-phase-transition M phase 102 made of ZrO2 with 1 mol % of Y2O3 dissolved therein is used to produce a solid electrolyte 1 made of partially stabilized zirconia with, for example, 7 mol % of Y2O3 dissolved therein as a whole, but the present invention is not limited to this. As shown in FIG. 8, a powder of Y2O3103y and a powder of ZrO2104 are prepared as starting materials. First, a powder of the easy-to-phase-transition M phase 102 is produced through a first pulverizing step, a first firing step, and a second pulverizing step.

[0032] In the first pulverization step, a stabilizer powder of Y2O3103y is added to the powder of ZrO2104 to a concentration of 1 mol%, and the mixture is dry-pulverized and mixed to prepare a raw material for the easy-to-transition M phase.

[0033] The average particle size of the easy-phase-transition M phase raw material can be 0.1 μm or more and 1 μm or less. When the average particle size of the easy-phase-transition M phase raw material is 0.1 μm or more, a solid electrolyte 1 that is easily converted to an M phase at 27° C. is obtained. When the average particle size of the easy-phase-transition M phase raw material is 1 μm or less, a solid electrolyte 1 in which particles of the easy-phase-transition M phase 102 are less likely to localize is obtained. The average particle size of the easy-phase-transition M phase raw material is the particle size (diameter) d50 when the volume-based cumulative frequency distribution measured by a laser diffraction / scattering method shows 50%.

[0034] In the first firing step, the easy-to-transition M-phase raw material produced in the first pulverization step is fired to dissolve Y2O3103y in the M-phase. The firing temperature can be set to a temperature equal to or lower than the firing temperature in the second firing step described below, and to a range of 1200°C to 1400°C.

[0035] In the second pulverization step, the aggregates of the raw material obtained in the first firing step are broken down, whereby powder of the easy phase transition M phase 102 can be produced.

[0036] Next, the solid electrolyte 1 is produced through a third pulverizing step, a mixing step, a granulating step, a molding step, and a second firing step.

[0037] In the third pulverization step, a stabilizer powder of Y2O3103y is added to the powder of ZrO2104, and the powder is pulverized and mixed in a dry manner to produce a mixed raw material powder 106. At this time, taking into consideration the amount of Y2O3 solid solution contained in the powder of the easy phase transition M phase 102 added after the third pulverization step, the amount of Y2O3103y powder added can be adjusted so that a partially stabilized zirconia having a predetermined amount of Y2O3 solid solution (7 mol% in this case) is finally obtained.

[0038] In the mixing step, the mixed raw material powder 106 obtained in the third pulverization step, the powder of the easy phase transition M phase 102 obtained in the second pulverization step, and water are mixed together to prepare a slurry.

[0039] In the granulation process, the slurry obtained in the mixing process is used to produce a granulated powder 105 having fluidity. The granulated powder 105 contains ZrO2104 particles, Y2O3103y particles, and particles of the easy-to-transition M phase 102. The granulated powder 105 can be, for example, a spray-dried powder suitable for powder compaction.

[0040] In the molding step, the granulated powder 105 is molded into, for example, an arbitrary shape to produce a molded body. The molded body can be molded into, for example, the shape of the solid electrolyte 1 used in the gas sensor element. The molded body can be appropriately ground or otherwise processed.

[0041] In the second firing step, the compact obtained in the molding step is fired to produce a fired body. The firing temperature can be 1300° C. to 1500° C. In this manner, the solid electrolyte 1 of the present embodiment can be produced.

[0042] In the above-mentioned method for producing the solid electrolyte 1, the final amount of Y2O3 in the solid solution, the sintering temperature in the second sintering step, etc. are adjusted to obtain the I of formula 1 in the solid electrolyte 1. M1 / I CT1 Specifically, by increasing the final amount of Y2O3, the value of I M1 / I CT1 In addition, by increasing the firing temperature in the second firing step, the value of I M1 / I CT1 In addition, by adjusting the amount of powder of the easy-to-transition M phase added to the entire solid electrolyte raw material in the mixing process, the value of (I M3 ×I CT2 ) / (I M2 ×I CT3 Specifically, by increasing the amount of powder of the easy-to-transition M phase, the value of (I M3 ×I CT2 ) / (I M2 ×I CT3 )-1 can be made smaller.

[0043] The solid electrolyte 1 obtained by the above-mentioned manufacturing method includes at least the C phase 11 and the M phase 10 at 27°C, as exemplified in Figs. 1, 6, and 9. Furthermore, the M phase 10 specifically includes a normal M phase 101 that contains almost no yttria and does not transition to the T phase, and an easy-to-transition M phase 102 that contains yttria and can transition from the M phase to the T phase with a temperature change from 500°C to 850°C. The C phase 11 is a phase that mainly contributes to the oxygen ion conductivity of the solid electrolyte 1. The easy-to-transition M phase 102 is a phase that contributes to the expression of the effect of suppressing the peeling of the metal layer by the above-mentioned estimated mechanism. The C phase 11 and the normal M phase 101 are mainly formed from the mixed raw material powder 106 prepared in the above-mentioned third pulverization step. The easy-to-transition M phase 102 is mainly formed from the powder of the easy-to-transition M phase 102 prepared in the above-mentioned second pulverization step. 1 and 6, more specifically, a solid electrolyte 1 including particles of a C phase 11 and particles of an M phase 10 is illustrated. The particles of the M phase 10 usually include particles of an M phase 101 and particles of an easy phase transition M phase 102. As illustrated in FIGS. 1 and 6, the solid electrolyte 1 may include pores 13 (voids).

[0044] In the above-mentioned method for producing the solid electrolyte 1, one or more additives such as silica, alumina, etc. can be added in the steps up to the mixing step (including the mixing step). In this case, the solid electrolyte 1 is obtained that is made of partially stabilized zirconia containing one or more additives such as silica, alumina, etc.

[0045] The solid electrolyte 1 may contain a small amount of T phase in addition to the above-mentioned C phase and M phase. This T phase is pushed by surrounding particles during the temperature drop process in the second firing step, and cannot expand and return to the M phase. When the solid electrolyte 1 contains silica, the silica may exist at the grain boundaries of the solid electrolyte 1. In this case, the silica at the grain boundaries is dissolved by etching the surface of the solid electrolyte 1, and the grain boundaries are cut (widened), so that the T phase can be returned to the M phase. In other words, this M phase is an M phase containing yttria in a solid solution, which can exist in the T phase up to low temperatures, and can exhibit the action and effect of the above-mentioned estimated mechanism. Therefore, when the solid electrolyte 1 contains silica, the effect of suppressing peeling of the metal layer can be enhanced by having grain boundaries from which silica is missing exist on the surface of the solid electrolyte 1. The content of silica can be, for example, 0.01 parts by mass or more and 1 part by mass or less, preferably 0.01 parts by mass or more and 0.6 parts by mass or less, relative to 100 parts by mass of the solid electrolyte 1.

[0046] Furthermore, when the solid electrolyte 1 contains alumina, the grain size of the solid electrolyte 1 can be made finer, and the grain boundary area that exerts the above-mentioned anchor effect can be increased. Therefore, in this case, the effect of suppressing peeling of the metal layer can be enhanced. The content of alumina can be, for example, 0.1 parts by mass or more and 10 parts by mass or less, preferably 0.5 parts by mass or more and 10 parts by mass or less, relative to 100 parts by mass of the solid electrolyte 1.

[0047] In the solid electrolyte 1, the average particle size of the M phase may be 0.1 μm or more from the viewpoint of facilitating formation of the M phase at 27° C., etc. Also, the average particle size of the M phase may be 1 μm or less from the viewpoint of suppressing localization of the M phase particles and facilitating the achievement of the above-mentioned effects, etc.

[0048] The average particle size of the M phase is measured as follows. A measurement sample is cut out from the solid electrolyte 1. The size of the measurement sample can be, for example, 5 mm wide, 20 mm long, and 2 mm thick. After polishing the surface of this measurement sample, a thermal etching process is performed. The thermal etching process is performed by heating the measurement sample at a temperature of 1200°C for 1 hour. Next, a composition analysis is performed by SEM / EDX analysis, and element mapping of the specific element derived from the stabilizer is performed for five regions. For example, when the stabilizer is yttria, element mapping can be performed for the Y element. Next, for each observed particle, the M phase is identified from the specific element concentration at the particle center, and the particle size of the M phase is measured. The specific element concentration identified as the M phase can be determined from a phase diagram of zirconia in which the specific element is dissolved. For example, when the stabilizer is Y2O3, the maximum Y2O3 amount of the M phase can be a particle having an yttrium concentration of 4.7 mol% or less (Y2O3 concentration of 2.35 mol% or less in terms of Y2O3) that is the boundary between the M phase, the M phase-T phase, and the M phase-C phase. In the phase diagram of FIG. 7, the point marked with a circle is a point where the Y2O3 concentration (solid solution amount) is 2.35 mol%. The center of the particle is the center of gravity of a rectangle covered by the maximum width of the particle P in the horizontal and vertical directions, as shown in FIG. 10. The observation conditions of the SEM can be an acceleration voltage of 5 kV, a WD setting of 8.0 mm, a current of 10 mA, and a magnification of 20,000 times. For the SEM, for example, SU8220 manufactured by Hitachi High-Technologies Corporation can be used. The measurement conditions by EDX can be an acceleration voltage of 5 kV, a WD setting of 14 mm, a current of 5 to 15 mA, and a magnification of 50,000 times. The current is adjusted so that the detection amount is 40 to 55 kcps. For the EDX, for example, Xflash6160 manufactured by Bruker Corporation can be used. The average grain size of the M phase is the arithmetic mean value of the grain size measurements of the M phase, which is represented by the arithmetic mean value of the horizontal length T1 and the vertical length T2 of a rectangle covered by the maximum width of the particle P in the horizontal and vertical directions, as shown in FIG. 10.

[0049] (Embodiment 2) The gas sensor of the second embodiment will be described with reference to Fig. 11 and Fig. 12. Note that, among the reference characters used in the second and subsequent embodiments, the reference characters that are the same as those used in the previous embodiments represent the same components, etc. as those in the previous embodiments, unless otherwise specified.

[0050] As illustrated in FIGS. 11 and 12, the gas sensor of this embodiment has a solid electrolyte 1A to which the solid electrolyte 1 of the first embodiment is applied.

[0051] Specifically, the gas sensor 2 can be configured to include a gas sensor element 3 having a solid electrolyte 1A, a housing 4 into which the gas sensor element 3 is inserted and held, a cover 5 for protecting the tip portion of the gas sensor element 3, and a heater 6 for heating the gas sensor element 3.

[0052] The gas sensor 2 can be configured as a cup-shaped gas sensor 2 as illustrated in FIG. 11. In this case, the gas sensor element 3 can include a solid electrolyte 1A formed in a bottomed cylindrical shape (so-called cup-shaped) with one end closed and the other end open, as illustrated in FIG. 11 and FIG. 12, a reference electrode 31 provided on the cylindrical inner surface of the solid electrolyte 1A for contacting a reference gas such as air, and a measurement electrode 32 provided on the cylindrical outer surface of the solid electrolyte 1A for contacting an exhaust gas to be measured. A lead wire (not shown) formed on the cylindrical inner surface of the solid electrolyte 1A is connected to the reference electrode 31. Also, a lead wire (not shown) provided on the cylindrical outer surface of the solid electrolyte 1A is connected to the measurement electrode 32. The reference electrode 31, the measurement electrode 32, and each lead wire can be made of, for example, Pt, a Pt alloy, or the like.

[0053] In FIG. 12, the surface of the measurement electrode 32 may be covered with one or more protective layers 33. FIG. 12 illustrates a configuration in which the surface of the measurement electrode 32 is covered with a first protective layer 331, the surface of the first protective layer 331 is covered with a second protective layer 332, and the surface of the second protective layer 332 is covered with a third protective layer 333. The protective layer 33 can be configured to be porous in order to protect the measurement electrode 32 from sulfur (S), phosphorus (P), glassy poisoning substances, etc. contained in the exhaust gas, and to adjust the amount of gas reaching the measurement electrode 32. The material, porosity, thickness, etc. of each protective layer 33 can be appropriately changed depending on the purpose. For other configurations of the gas sensor 2, known techniques can be appropriately applied.

[0054] The gas sensor 2 of this embodiment has a solid electrolyte 1A to which the solid electrolyte 1 of this embodiment 1 is applied. Therefore, the gas sensor 2 of this embodiment can suppress peeling of the electrodes (reference electrode 31 and measurement electrode 32) made of a metal layer and the lead wires even if the number of repeated cold-hot cycles between the low temperature at engine stop / start (including restart of a hybrid vehicle or a vehicle equipped with an idling stop function) and the high temperature at which the sensor is used increases. Therefore, according to the gas sensor 2 of this embodiment, a cup-shaped gas sensor 2 with suppressed resistance fluctuation and high sensor accuracy can be obtained.

[0055] (Embodiment 3) The gas sensor of the third embodiment will be described with reference to Fig. 13 and Fig. 14. As illustrated in Fig. 13 and Fig. 14, the gas sensor 2 of the present embodiment has a solid electrolyte 1B to which the solid electrolyte 1 of the first embodiment is applied.

[0056] The gas sensor 2 is configured as a laminated gas sensor 2. In this case, as illustrated in Fig. 14, the gas sensor element 3 includes a layered solid electrolyte 1B, a reference electrode 31 provided on one side of the solid electrolyte 1B for contacting a reference gas such as the atmosphere, and a measurement electrode 32 provided on the other side of the solid electrolyte 1B for contacting an exhaust gas to be measured. A lead wire (not shown) formed on one side of the solid electrolyte 1B is connected to the reference electrode 31. Also, a lead wire (not shown) provided on the other side of the solid electrolyte 1B is connected to the measurement electrode 32.

[0057] In FIG. 14, an exhaust gas inlet (not shown) is formed at the tip of the gas sensor element 3 to introduce exhaust gas into the inside. A reference gas space 310 through which a reference gas flows is provided on one side of the solid electrolyte 1B, and a reference electrode 31 is arranged on the reference gas space 310 side. An exhaust gas space 320 through which exhaust gas flows is provided on the other side of the solid electrolyte 1B, and a measurement electrode 32 is arranged on the exhaust gas space 320 side. The other side of the solid electrolyte 1B is held by an insulating holding layer 34. A heater 6 for heating the gas sensor element 3 is built in the holding layer 34. A protective layer 33 is formed on the outer peripheral surface of the gas sensor element 3 to protect the gas sensor element 3 from poisoning, water, and the like. Other configurations of the gas sensor 2 can be appropriately applied to known techniques.

[0058] The gas sensor 2 of this embodiment has a solid electrolyte 1B to which the solid electrolyte 1 of this embodiment 1 is applied. Therefore, the gas sensor 2 of this embodiment can suppress peeling of the electrodes (reference electrode 31 and measurement electrode 32) made of metal layers and the lead wires even if the number of repeated cold-hot cycles between the low temperature at engine stop / start (including restart of a hybrid vehicle or a vehicle equipped with an idling stop function) and the high temperature at which the sensor is used increases. Therefore, according to the gas sensor 2 of this embodiment, a laminated gas sensor 2 having suppressed resistance fluctuation and high sensor accuracy can be obtained.

[0059] (Experimental Example 1) According to the above-mentioned manufacturing method, the solid electrolytes of Samples 1-1 to 1-7 were prepared. In this experimental example, the type of the solid electrolyte was yttria partially stabilized zirconia with an yttria content in the range of 3 mol % to 11 mol %. For each solid electrolyte, the X-ray diffraction intensity was measured, and the I M1 / I CT1 The thermal expansion coefficient of each solid electrolyte was also measured.

[0060] <X-ray diffraction intensity of solid electrolyte> Using an X-ray diffraction device "UltimaIII" manufactured by Rigaku Corporation and a horizontal goniometer (D / teX) as a detector, the X-ray diffraction intensity of the (11-1) plane of the M phase, the (111) plane of the C phase, and the total X-ray diffraction intensity of the (101) plane of the T phase were measured for each solid electrolyte. At this time, the X-ray diffraction intensity was measured at sample surface temperatures of 27°C, 500°C, and 850°C. In addition, the measurement was performed in a range of 2θ=27.5 to 32.5° with a sampling interval of 0.02° by continuous 2θ / θ scanning. In addition, CuKα radiation was used as the X-ray source, with an acceleration voltage of 40 kV and a current of 30 mA. From the measured X-ray diffraction intensities, the I in formula 1 for the solid electrolyte of each sample was calculated. M1 / I CT1 (X-ray diffraction intensity ratio) was obtained.

[0061] <Thermal expansion coefficient of solid electrolyte> Each solid electrolyte was cut to a size of about 5 mm wide and 45 mm long. The thermal expansion behavior of this sample between 27°C and 1050°C was measured by thermomechanical analysis (TMA). In this case, an alumina sintered body was used as the standard sample. The measurement was performed five times for each sample. The slope of the linear section from 400°C to 600°C in the thermal expansion behavior was defined as the thermal expansion coefficient, and the arithmetic average value of the measured thermal expansion coefficient was calculated as the thermal expansion coefficient of each sample. From the viewpoint of the compatibility of the thermal expansion coefficient with different materials, a thermal expansion coefficient of 7.0 ppm / °C or more and 9.5 ppm / °C or less was considered to be acceptable.

[0062] The above results are summarized in Table 1.

[0063] [Table 1]

[0064] From Table 1, the following can be seen. The solid electrolytes of Samples 1-2 to 1-6 satisfy Formula 1. Therefore, the solid electrolytes of Samples 1-2 to 1-6 can ensure the matching of the thermal expansion coefficient with other members such as metal layers and alumina. In contrast, the solid electrolyte of Sample 1-1 does not satisfy the I shown in Formula 1. M1 / I CT1 Since the thermal expansion coefficient is less than 0.05, it is difficult to ensure the consistency of the thermal expansion coefficient with other components. This is because the amount of M phase in the entire solid electrolyte is too small, and the thermal expansion coefficient of the solid electrolyte in the temperature range from 400°C to 600°C becomes large. In addition, the solid electrolyte of Sample 1-7 has a thermal expansion coefficient of I M1 / I CT1 Since the thermal expansion coefficient exceeds 0.4, it is difficult to ensure consistency in thermal expansion coefficient with other components. This is because the amount of M phase in the entire solid electrolyte becomes too large, and the thermal expansion coefficient of the solid electrolyte becomes small in the temperature range from 400°C to 600°C.

[0065] (Experimental Example 2) According to the above-mentioned manufacturing method, the solid electrolytes of Samples 2-1 to 2-10 were prepared. In this experimental example, the type of the solid electrolyte was yttria partially stabilized zirconia with an yttria content in the range of 3 mol % to 11 mol %. For each solid electrolyte, the X-ray diffraction intensity was measured in the same manner as in Experimental Example 1, and the I M1 / I CT1 (X-ray diffraction intensity ratio), (I M3 ×I CT2 ) / (I M2 ×I CT3 The rate of change in resistance and bending strength of each solid electrolyte were measured by the following test methods.

[0066] <Resistance change rate of solid electrolyte> A metal layer was formed on the surface of each solid electrolyte, and the resistance change rate was measured. Specifically, a solid electrolyte having a cup-shaped configuration with an electrode made of Pt plating assumed to be a gas sensor element was used for measuring the electrical resistance of the solid electrolyte. In this experimental example, in the molding step in the manufacturing method of the solid electrolyte described above, granulated powder was molded into a cup-shaped shape by a rubber press method, and ground to obtain a cup-shaped molded body. This cup-shaped molded body was fired in the second firing step to form a cup-shaped solid electrolyte, and then an electrode made of Pt plating (average film thickness 1 μm) was formed on the surface.

[0067] For each of the obtained samples, the electrical resistance of the solid electrolyte body was measured initially and after the thermal cycle using the following measuring device and measuring software. The measuring devices used were an impedance / gain-phase analyzer "1260" manufactured by Solartron Analytical and a potentiostat / galvanostat "SI1287" manufactured by Solartron Analytical, and the measuring software used was "Z Plot" manufactured by Solartron Analytical. The measuring conditions were: Initial Frequency (Hz): 0.1, Final Frequency (Hz): 10 6 , DC Potential (Volts): 0, AC Amplitude (mV): 20, VS Reference, Logarthimic, steps / Decade: 10. Note that VS Reference applies a voltage based on 0V, Logarthimic sets the output to be logarithmic, and steps / Decade: 10 means that there are 10 measurement points each time a digit of the logarithmic frequency increases.

[0068] In the measurement of the electrical resistance, a thermal cycle from 27°C to 1100°C was repeated 1000 times at a temperature increase / decrease rate of ±300°C / h. If the rate of change in electrical resistance from the initial endurance period was 30% or less, it was deemed to have passed the test, since it was possible to suppress peeling of the electrodes even when exposed to severe thermal cycles and the output function as a gas sensor element could be maintained. On the other hand, if the rate of change in electrical resistance from the initial endurance period exceeded 30%, it was deemed to have failed, since the electrodes peeled off due to the severe thermal cycles and it was not possible to suppress peeling of the electrodes.

[0069] <Strength of solid electrolyte after thermal cycle> Each solid electrolyte was cut to a size of about 5 mm wide and about 45 mm long. For this sample, a thermal cycle from 27°C to 1100°C was repeated 1000 times at a temperature increase and decrease rate of ±300°C / h. Next, a test piece for strength evaluation was prepared from this sample in accordance with the four-point bending test specified in JIS R 1601, and a four-point bending test was performed to measure the four-point bending strength of each solid electrolyte. The four-point bending test was performed 10 times for each test piece (N=10), and the arithmetic average value was taken as the bending strength of each test piece. When the bending strength was 250 MPa or more, the occurrence of cracks could be suppressed even when exposed to severe thermal cycles, and the test piece was deemed to have passed the test because it was able to function as a solid electrolyte. On the other hand, when the bending strength was less than 250 MPa, the solid electrolyte was destroyed by the severe thermal cycles, and it was deemed to have failed the test because it was unable to function as a solid electrolyte.

[0070] The above results are summarized in Table 2.

[0071] [Table 2]

[0072] From Table 2, the following can be seen. The solid electrolytes of Samples 2-1 to 2-9 are composed of partially stabilized zirconia, and satisfy the relationships of Formulas 1 and 2. Therefore, even when the solid electrolytes of Samples 2-1 to 2-10 are exposed to more severe thermal cycles than before with a metal layer formed on their surfaces, the volume change associated with the phase transition maintains the bonding strength of the interface between the solid electrolyte and the metal layer during use, and peeling of the metal layer can be suppressed. In contrast, the solid electrolyte of Sample 2-9 satisfies the relationship (I) shown in Formula 2. M3 ×I CT2 ) / (I M2 ×I CT3 )-1 exceeded -0.1, resulting in a large resistance fluctuation. This is because the bonding strength at the interface between the solid electrolyte and the metal layer was reduced due to exposure to severe thermal cycles, causing the metal layer to peel off. In addition, the solid electrolyte of sample 2-10 has a resistance fluctuation of 0.01% as shown in formula 2 (I M3 ×I CT2 ) / (I M2 ×I CT3 )-1 was less than -0.5, the strength of the solid electrolyte was reduced because the phase transition strain became too large.

[0073] In the measurement of the resistance change rate of the solid electrolyte in this experimental example, a metal layer was formed on the surface of the solid electrolyte by plating. However, similar results were obtained when a metal layer was formed on the surface of the solid electrolyte by applying a paste to the surface of the molded body and firing it.

[0074] The present disclosure is not limited to the above-mentioned embodiments and experimental examples, and various modifications are possible within the scope of the gist of the disclosure. That is, although the present disclosure has been described based on the embodiments, it is understood that the present disclosure is not limited to the embodiments, structures, etc. The present disclosure also includes various modified examples and modifications within the equivalent range. In addition, various combinations and forms, and further other combinations and forms including only one element, more than one element, or less than one element, are also within the scope and concept of the present disclosure. Also, the configurations shown in each embodiment and each experimental example can be arbitrarily combined. Also, in the second and third embodiments, the solid electrolyte of the first embodiment is applied to a gas sensor, but the solid electrolyte of the first embodiment can also be applied to other applications such as a solid oxide fuel cell (SOFC).

Claims

1. A solid electrolyte (1) comprising partially stabilized zirconia in which a stabilizer is dissolved in zirconia, A solid electrolyte (1) that satisfies the relationships of the following formulas 1 and 2. 0.05≦I M1 / I CT1 ≦0.4...Formula 1 −0.5≦(I M3 ×I CT2 ) / (I M2 ×I CT3 )-1≦-0.1...Formula 2 However, in Formula 1 and Formula 2, I M1 : X-ray diffraction intensity of the (11-1) plane of the M phase at 27 ° C. I CT1 : Total X-ray diffraction intensity of the (111) plane of the C phase and the (101) plane of the T phase at 27 ° C. I M2 : X-ray diffraction intensity of the (11-1) plane of the M phase at 500 ° C. I CT2 : Total X-ray diffraction intensity of the (111) plane of the C phase and the (101) plane of the T phase at 500 ° C. I M3 : X-ray diffraction intensity of the (11-1) plane of the M phase at 850 ° C. I CT3 : Total X-ray diffraction intensity of the (111) plane of the C phase and the (101) plane of the T phase at 850 ° C.

2. the stabilizer is yttria, The content of the yttria is 3 mol% or more and 11 mol% or less. The solid electrolyte according to claim 1 .

3. A gas sensor (2) comprising a solid electrolyte according to claim 1 or 2.

Citation Information

Patent Citations

  • Solid electrolyte body for oxygen sensor

    JP1981111455A

  • Zirconia oxygen sensor element

    JP1988210063A

  • Laminated oxygen sensor element

    JP1997026409A

  • Stacked oxygen sensor element

    JP3873302B2

  • Solid electrolyte, method for producing same and gas sensor

    WO2019087735A1