Packaging container for bean sprouts, method for manufacturing package containing bean sprouts, and method for preserving freshness of bean sprouts
A dual-layer packaging container with a higher melting point outer layer and optimized gas permeability addresses heat resistance and sealability issues, ensuring effective sealing and freshness maintenance for bean sprouts.
Patent Information
- Application Number
- JP2018127274
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2018-07-04
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2038-07-04
AI Technical Summary
Conventional packaging containers for bean sprouts face issues with heat resistance leading to hot plate removal during sealing, and maintaining freshness is a challenge due to poor heat sealability and gas permeability.
A packaging container composed of at least two layers, an outer surface layer and an inner surface layer, where the outer layer has a melting point 10 to 70°C higher than the inner layer, made from unstretched polypropylene and/or unstretched polyethylene, with specific gas permeability and thickness ratios to enhance heat sealability and freshness maintenance.
The solution effectively prevents hot plate removal and maintains bean sprout freshness by optimizing heat sealability and gas permeability, ensuring the container does not swell and retains the sprouts' appearance over time.
Smart Images

Figure 0007593731000002 
Figure 0007593731000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a packaging container for bean sprouts, a method for producing a package containing bean sprouts, and a method for preserving the freshness of bean sprouts. [Background technology]
[0002] Various studies have been conducted on the containers for packaging bean sprouts and the materials to be used for these containers.
[0003] For example, Patent Document 1 describes a laminated stretched film having at least two layers, in which a biaxially stretched polypropylene base layer is laminated on one side with a heat-sealable resin layer containing zinc oxide fine particles, and the heat-sealable resin layer is stretched at least in one direction. It also describes the use of the film to package bean sprouts. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2003-025524 A Summary of the Invention [Problem to be solved by the invention]
[0005] In a packaging container for bean sprouts (typically a bag), the bean sprouts are usually placed in the internal space of the container, and then the opening of the container is closed by a heat sealing process. However, according to the knowledge of the present inventor, some of the conventional packaging containers for bean sprouts are made of materials that lack heat resistance, which can cause a problem of "hot plate adhesion" in which a part of the molten packaging container adheres to the heat sealing device during heat sealing. One possible solution to the above problem is to increase the heat resistance of the container material, but simply increasing the heat resistance of the container material will result in poor heat sealability. In terms of "packaging bean sprouts," it is preferable that the freshness of the bean sprouts can be maintained for as long as possible.
[0006] The present invention has been made in view of the above circumstances. That is, one of the objects is to provide a packaging container for bean sprouts that is less susceptible to the problem of heat plate absorption and can maintain the freshness of the bean sprouts for a relatively long period of time. [Means for solving the problem]
[0007] As a result of extensive investigations, the present inventors have made the invention provided below and found that the above-mentioned objects can be achieved.
[0008] According to the present invention, A packaging container for bean sprouts, comprising: The container comprises at least an outer surface layer and an inner surface layer; the outer surface layer and the inner surface layer contain at least one selected from the group consisting of non-oriented polypropylene and non-oriented polyethylene; A packaging container in which the melting point of the outer surface layer is 10 to 70° C. higher than the melting point of the inner surface layer. is provided.
[0009] Further, according to the present invention, The method for producing a package containing bean sprouts includes the steps of: placing bean sprouts in the internal space of the packaging container for bean sprouts; and heat-sealing an opening of the packaging container while deaerating the packaging container containing the bean sprouts. is provided.
[0010] Further, according to the present invention, A method for preserving the freshness of bean sprouts, comprising: placing bean sprouts in the internal space of the packaging container for bean sprouts; and heat-sealing the opening of the packaging container while degassing the packaging container to produce a package containing bean sprouts, thereby preserving the freshness of the bean sprouts. is provided. Effect of the Invention
[0011] According to the present invention, a packaging container for bean sprouts is obtained which is less susceptible to the problem of heat plate absorption and is capable of maintaining the freshness of the bean sprouts for a relatively long period of time. [Brief description of the drawings]
[0012] [Figure 1] FIG. 2 is a diagram showing a schematic diagram of a packaging container for bean sprouts according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. The drawings are for illustrative purposes only, and the shapes and dimensional ratios of each component in the drawings do not necessarily correspond to actual articles.
[0014] In this specification, the expression "a to b" in the explanation of a numerical range means from a to b, unless otherwise specified. For example, 0 to 100°C means from 0°C to 100°C. In the description of groups (atomic groups) in this specification, when a description is made without specifying whether the group is substituted or unsubstituted, the description includes both groups having no substituents and groups having a substituent. For example, an "alkyl group" includes not only an alkyl group having no substituents (unsubstituted alkyl group) but also an alkyl group having a substituent (substituted alkyl group). In this specification, the term "(meth)acrylic" refers to a concept that includes both acrylic and methacrylic. The same applies to similar terms such as "(meth)acrylate."
[0015] <Packaging container for bean sprouts> FIG. 1 is a schematic diagram of a packaging container 1 for bean sprouts (hereinafter, also referred to as packaging container 1) according to this embodiment. As an example, the packaging container 1 is in a bag shape as shown in the drawing. Of course, the shape of the packaging container 1 is not limited to a bag shape, and as another example, it may be in a cup shape or the like. The packaging container 1 is typically made of a film 10 . The film 10 includes at least an outer surface layer 11 and an inner surface layer 12. The outer surface layer 11 and the inner surface layer 12 each contain at least one selected from the group consisting of unstretched polypropylene and unstretched polyethylene. In the film 10, the melting point of the outer surface layer 11 is higher than the melting point of the inner surface layer 12 by 10 to 70°C.
[0016] The packaging container 1 configured as above can prevent the problem of being caught by the hot plate and can improve the heat sealability. In other words, by making the packaging container 1 not a single layer but two layers, that is, the outer surface layer 11 and the inner surface layer 12, and setting the melting point of the outer surface layer 11, which can directly contact the hot plate of the heat sealing device, higher, the problem of being caught by the hot plate can be prevented from occurring. On the other hand, by setting the melting point of the inner surface layer 12 lower than that of the outer surface layer 11, it is believed that it is possible to obtain sufficiently good heat sealability without deteriorating the heat sealability.
[0017] The melting point of the outer surface layer 11 is usually 135 to 170° C., and preferably 140 to 165° C. The melting point of the inner surface layer 12 is usually 100 to 140° C., and preferably 110 to 135° C. Designing the melting points of the outer surface layer 11 and the inner surface layer 12 to satisfy these numerical ranges is believed to optimize the heat sealability under heat seal conditions conventionally applied in packaging bean sprouts.
[0018] The packaging container 1 is typically composed of a film 10 having a specific outer surface layer 11 and inner surface layer 12. As a result, the packaging container 1 not only reduces the problem of hot plate adhesion and has good heat sealability, but also has a certain degree of effect of suppressing deterioration of the contained bean sprouts (preserving freshness). According to the findings of the present inventors, the film made of unstretched polypropylene and / or unstretched polyethylene has a suitable gas permeability for preventing deterioration (preserving freshness) of bean sprouts due to its molecular structure, orientation, etc. This is believed to have the effect of preventing deterioration (preserving freshness) of bean sprouts. In addition, this suitable gas permeability can prevent the problem of the packaging container 1 swelling due to respiration of the bean sprouts after they are placed in the packaging container 1.
[0019] The packaging container 1 will be described in more detail below.
[0020] Materials for the outer surface layer 11 and the inner surface layer 12 The outer surface layer 11 and the inner surface layer 12 are typically made of a film containing unstretched polypropylene and / or unstretched polyethylene, respectively, and have the melting point difference described above. The outer surface layer 11 preferably contains at least one selected from the group consisting of a propylene homopolymer, a propylene block copolymer, and a propylene random copolymer, and more preferably contains a propylene homopolymer. The inner surface layer 12 preferably contains at least one selected from the group consisting of a random copolymer of propylene, a low density polyethylene, and a linear low density polyethylene. In this way, it becomes easier to design a film having the above-mentioned difference in melting point by selecting the materials and properties of the outer surface layer 11 and the inner surface layer 12. As a result, it becomes easier to obtain a packaging container for bean sprouts that is less susceptible to the problem of being caught by the hot plate and has good heat sealability.
[0021] Examples of the random copolymer or block copolymer of propylene in the outer surface layer 11 and the inner surface layer 12 include a random copolymer or block copolymer of a propylene monomer and an α-olefin having 2 or 4 to 10 carbon atoms, and a random copolymer or block copolymer of propylene and ethylene is preferred. Regarding the melting point, when ethylene is selected as the copolymerization component, the melting point tends to be lower as the ethylene content increases. When an α-olefin having 4 or more carbon atoms is selected as the copolymerization component, the melting point tends to be higher as the content of the structural unit increases.
[0022] When the inner surface layer 12 contains a random copolymer of propylene, the copolymer is preferably a random copolymer of propylene and ethylene from the viewpoint of ensuring sufficient heat sealability at low temperatures. In addition, in the random copolymer of propylene and ethylene, it is preferable that 3 mol % or more of the total structural units are structural units derived from ethylene, more preferably 5 mol % or more of the structural units derived from ethylene, and even more preferably 10 mol % or more of the structural units derived from ethylene. There is no particular upper limit, but it is, for example, 95 mol % or less.
[0023] The low-density polyethylene (often abbreviated as LDPE) and linear low-density polyethylene (often abbreviated as LLDPE) that may be contained in the inner surface layer 12 are not particularly limited, and known or commercially available materials may be appropriately used. Examples of copolymerization components of LLDPE with ethylene include 1-butene, 1-hexene, 4-methylpentene-1, and 1-octene. The production method (polymerization method) of LDPE and LLDPE is also not particularly limited. LDPE or LLDPE produced by any method, such as gas phase polymerization, liquid phase polymerization, or polymerization using a metallocene catalyst, can be used.
[0024] In order to make the outer surface layer 11 have a higher melting point than the inner surface layer 12, it is considered preferable to use a propylene homopolymer or a random copolymer or block copolymer of a propylene monomer and an α-olefin having 4 to 10 carbon atoms.
[0025] Of course, it is also possible to use a random copolymer of propylene and ethylene (carbon number: 2) for the outer surface layer 11. However, in terms of creating a difference in melting point with the inner surface layer 12, it is preferable that the copolymer contains a smaller amount of structural units derived from ethylene. Specifically, when the outer surface layer 11 is composed of a random copolymer or block copolymer of propylene, the content of structural units derived from ethylene in the copolymer is preferably 50 mol % or less, more preferably 45 mol % or less, and even more preferably 40 mol % or less. There is no particular lower limit, but it is, for example, 3 mol % or more. From yet another viewpoint, when both the outer surface layer 11 and the inner surface layer 12 are composed of a random copolymer or block copolymer of propylene (e.g., a random copolymer or block copolymer of propylene and ethylene), the ratio of propylene-derived structural units in the copolymer constituting the outer surface layer 11 is preferably 10 to 50 mol % greater than the ratio of propylene-derived structural units in the copolymer constituting the inner surface layer 12, and more preferably 20 to 50 mol % or more greater.
[0026] In this specification, the melting points of the outer surface layer 11 and the inner surface layer 12 are, for example, B1 / S B2 The peak top temperature of the endothermic peak of melting in the DSC curve obtained by DSC measurement to obtain the value of can be taken as the melting point.
[0027] Thermal properties of the outer surface layer 11 and the inner surface layer 12 One method for further reducing the problem of hot plate adhesion and further improving the heat sealability is to use a material having specific thermal properties for the outer surface layer 11 and the inner surface layer 12. Specifically, the crystallization peak area per unit mass of the outer surface layer in differential scanning calorimetry is SB1 , the crystallization peak area per unit mass of the inner surface layer is S B2 Then, S B1 / S B2 It is preferable to design the outer surface layer 11 and the inner surface layer 12 so that the value of S is less than 1. B1 / S B2 The value of S is more preferably less than 0.95, and even more preferably less than 0.9. B1 / S B2 The value of is typically greater than 0.1.
[0028] S B1 / S B2 A value of less than 1 means that the outer surface layer 11 undergoes less structural change due to crystallization than the inner surface layer 12. In other words, it is believed that the problem of being caught by the hot plate can be reduced. Also, the fact that the peak area of the inner surface layer 12 is larger means that the inner surface layer 12 undergoes greater microstructural change due to heat than the outer surface layer 11, which is believed to contribute to high heat sealability. In other words, in addition to the index of the melting point difference, S B1 / S B2 By taking these indicators into consideration when designing the packaging container 1, it is expected that the problem of hot plate adhesion can be further reduced and the heat sealability can be improved.
[0029] The differential scanning calorimetry can be performed, for example, at a measurement temperature of 25 to 300° C., at a temperature rise rate of 5° C. / min, in a nitrogen atmosphere (flow rate: 30 ml / min). As a measuring device, for example, DSC6220 manufactured by SII Corporation can be used.
[0030] · Thickness of outer surface layer 11 and inner surface layer 12 In the packaging container 1, when the thickness of the outer surface layer 11 of the film 10 is D1 and the thickness of the inner surface layer 12 is D2, the value of D1 / D2 is preferably 0.1 to 5, more preferably 0.1 to 4, and further preferably 0.1 to 3. It is believed that by setting the value within this range, the problem of hot plate absorption can be reduced to a greater extent. In addition, by adjusting D1 / D2 within the above range, it is believed that pinhole resistance (durability when impact is applied due to dropping, etc.) can be improved. As the inventors have found, for example, when the outer surface layer contains a propylene homopolymer, there is a slight tendency for pinholes to be generated by the impact of dropping. Therefore, when the outer surface layer 11 contains a propylene homopolymer, it is preferable to make the inner surface layer 12 relatively thick by not making the outer surface layer 11 too thick (the value of D1 / D2 is 5 or less), or to use a propylene random copolymer (rather than a propylene homopolymer) for the inner surface layer.
[0031] The thickness D1 is preferably 0.5 to 24 μm, more preferably 1 to 23 μm. The thickness D2 is preferably 0.5 to 24 μm, more preferably 1 to 23 μm. By setting the values of D1 and D2 within appropriate numerical ranges, it is believed that the gas permeation amount described below can be appropriately adjusted.
[0032] Components that the outer surface layer 11 and / or the inner surface layer 12 may contain The outer surface layer 11 and / or the inner surface layer 12 are mainly composed of a specific polypropylene and / or polyethylene, but may contain various other additives. Specifically, additives such as anti-fogging agents and anti-blocking agents, adhesive resins such as urethane resins, urea resins, melamine resins, epoxy resins, crystal nucleating agents, elastomer resins, petroleum resins, and alkyd resins, silane coupling agents, etc. may be contained. The amount (total) of these added components in each surface layer is typically 0.01 to 10 parts by mass when the total amount of the unstretched polypropylene and the unstretched polyethylene is taken as 100 parts by mass.
[0033] Of the additive components, the antifogging agent may be any known antifogging agent such as a fatty acid ester of a polyhydric alcohol, an ethylene oxide adduct of a higher aliphatic amine, etc. Specific examples thereof include glycerin monostearate, diglycerin laurate, decaglycerin laurate, and sorbitan stearate. When an antifogging agent is used, it is preferably used at least in the inner surface layer 12. When an antifogging agent is used in the inner surface layer 12, the amount used (addition amount) is typically 0.01 to 10 parts by mass, preferably 0.1 to 9 parts by mass, relative to 100 parts by mass of the polypropylene constituting the inner surface layer 12.
[0034] Additional layers The packaging container 1 may have an additional layer other than the outer surface layer 11 and the inner surface layer 12. For example, it may further have various coating layers or laminate layers such as a lubricating layer, an antistatic layer, etc. The location of the additional layer is not particularly limited, and may be, for example, between the outer surface layer 11 and the inner surface layer 12, further outside the outer surface layer 11, further inside the inner surface layer 12, etc. In one embodiment, an intermediate layer may be present between the outer surface layer 11 and the inner surface layer 12. This intermediate layer may be made of at least one material selected from the group consisting of homopolypropylene, random polypropylene, block polypropylene, low-density polyethylene, linear low-density polyethylene, and high-density polyethylene. The presence of the intermediate layer may, for example, provide an appropriate adjustment of gas permeability and improve the strength of the container.
[0035] Gas permeability As described above, the packaging container 1 is expected to have an effect of suppressing deterioration (preserving freshness) of the bean sprouts contained therein. By appropriately designing the oxygen permeability and carbon dioxide permeability of the packaging container 1, it is expected that the effect of suppressing deterioration of the bean sprouts can be further enhanced.
[0036] Specifically, when the bean sprouts are sealed using the packaging container 1 (for example, if the packaging container 1 is a bag, the bean sprouts are placed inside the bag and the opening of the bag is closed by heat sealing), it is preferable that the oxygen transmission rate To per 100 g of bean sprouts at 23°C and 60% RH is not less than 40 cc / 100g·day·atm and not more than 400 cc / 100g·day·atm. In addition to the above, when the bean sprouts are sealed using the packaging container 1 (for example, if the packaging container 1 is a bag, the bean sprouts are placed inside the bag and the opening of the bag is closed by heat sealing), it is preferable that Tc / To is 1 or more (the relationship Tc≧To holds).
[0037] Bean sprouts continue to respire even after harvest. Therefore, during storage, distribution or preservation after harvest, the sprouts consume energy through their own respiration, causing a deterioration in freshness. In order to maintain the freshness of bean sprouts, it is considered effective to create a low oxygen and high carbon dioxide concentration state inside the packaging container 1 by balancing the respiration rate of the sprouts and the gas permeability of the packaging container 1.
[0038] In the packaging container 1, it is believed that the inside of the packaging body can be made to have a low oxygen concentration and a high carbon dioxide concentration to some extent by using a specific polypropylene or polyethylene for the outer surface layer 11 and the inner surface layer 12. In addition, it is believed that an even more ideal low oxygen concentration and high carbon dioxide concentration state can be made by setting the oxygen permeability To and the carbon dioxide permeability Tc as described above.
[0039] More specifically, by designing the oxygen permeability To and carbon dioxide permeability Tc of the packaging container 1 as described above, it is possible to more effectively prevent the bean sprouts from suffering from anoxia (oxygen deficiency) and the gas concentration conditions inside the packaging from becoming excessively oxygen-rich. This is preferable for stably maintaining the freshness of the bean sprouts for a long period of time. In addition, by designing the oxygen permeability To and carbon dioxide permeability Tc of the packaging container 1 as described above, it is possible to more effectively suppress the increase in oxygen concentration in the packaging body over time after the bean sprouts are packaged. In other words, it is possible to suppress an increase in the respiration rate of the bean sprouts. As a result, it is expected that the appearance (appearance) of the packaging body can be maintained in a good condition for a long period of time in that the packaging body can be prevented from expanding over time after the bean sprouts are packaged.
[0040] The carbon dioxide permeation rate Tc is preferably 70 to 2000 cc / 100 g·day·atm, more preferably 100 to 1600 cc / 100 g·day·atm, and further preferably 150 to 1500 cc / 100 g·day·atm.
[0041] The oxygen transmission rate To can be calculated as follows. First, the oxygen transmission rate Tx [cc / m 2 ·day·atm] is measured using an oxygen permeability measuring device manufactured by MOCON (OXYTRAN (registered trademark) OX-TRAN 2 / 21) according to the method in accordance with Appendix B of JIS K7126-2. Next, the oxygen transmission rate Tx [cc / m 2 The measured value for oxygen transmission rate T1 [cc / 100g m 2 ·day·atm] can be calculated. The oxygen permeability T1 [cc / 100g m 2 ·day·atm], and the inner surface area [m 2 ], the oxygen transmission rate To [cc / 100g day atm] per 100g of bean sprouts at 23°C and 60% RH can be calculated.
[0042] The carbon dioxide permeation rate Tc can be calculated as follows. First, the carbon dioxide permeation rate Ty [cc / m 2 ·day·atm] is measured using a carbon dioxide permeability measuring device (PERMATRAN-C 4 / 41) manufactured by MOCON, in accordance with Appendix B of JIS K7126-2. Next, the carbon dioxide permeation amount Ty [cc / m 2 The measured value for the carbon dioxide permeation rate T2 [cc / 100g m 2 ·day·atm] can be calculated. And the above-mentioned carbon dioxide permeability T2 [cc / 100g m 2 ·day·atm], and the inner surface area [m 2 ], the carbon dioxide permeation rate Tc [cc / 100g day atm] per 100g of bean sprouts at 23°C and 60% RH can be calculated.
[0043] Manufacturing method for packaging containers for bean sprouts The packaging container for bean sprouts of this embodiment (for example, the above-mentioned packaging container 1) can be produced using known polypropylene, polyethylene, or the like as a raw material.
[0044] The film (film 10) constituting the packaging container for bean sprouts of this embodiment can be manufactured by an extrusion method (T-die method, inflation method), calendaring method, or the like. When forming the film, additives such as the above-mentioned anti-fogging agent may be kneaded as necessary. In addition, a coating may be applied to the film surface to impart some function.
[0045] In the production of the film, it is particularly important to highly control the various factors related to the following conditions in order to obtain the desired values for the specific melting point, crystallization peak area, oxygen and carbon dioxide permeation amount, etc. In other words, the film (film 10) constituting the packaging container for bean sprouts of this embodiment can be produced only by using a film obtained by a production method that highly controls the various factors related to the following conditions. Note that the film constituting the packaging container for bean sprouts of this embodiment can be produced by combining other known production conditions as long as the various factors related to the following conditions are highly controlled. (1) Combination of resin materials used to form the film (2) Combination of film layer structure, thickness of each layer, film-making method, etc.
[0046] The method for producing a packaging container for bean sprouts using the obtained film includes, for example, the following method. First, the film produced by the above-mentioned method is prepared. Next, the film is cut into two pieces of the desired size, and the two pieces of film are overlapped and heat-sealed on three sides using a sealer to form heat-sealed portions (the seal width is typically about 10 mm). Through this series of steps, the bean sprout packaging container of this embodiment can be produced.
[0047] The inner surface area of the bean sprout packaging container is not particularly limited, but is typically 200 to 2000 cm 2 , preferably 600 to 1600 cm 2 It is.
[0048] ·others The packaging container 1 may be perforated with micropores in order to adjust the amount of permeation of various gases. However, in this embodiment, it is preferable that the packaging container is not perforated with micropores in order to prevent the packaging container from slightly expanding over time after packaging the bean sprouts, thereby causing a change in its appearance.
[0049] <Manufacturing method of bean sprout-containing package> The method for producing a package containing bean sprouts according to the present embodiment uses the above-mentioned packaging container for bean sprouts (eg, the above-mentioned packaging container 1) to produce a package containing bean sprouts.
[0050] As a specific manufacturing procedure, for example, first, a packaging container for bean sprouts manufactured by the above-mentioned method is prepared, and a predetermined amount of bean sprouts is placed in its internal space. Then, a heat seal (heat sealing process) is applied to one side of the packaging bag where a heat-sealed portion has not yet been formed, to form a heat-sealed portion (seal width is typically about 10 mm). By the above procedure, a package containing bean sprouts can be obtained in which the bean sprouts are placed (sealed) in the internal space of the packaging container. The amount of bean sprouts to be stored in one bean sprout packaging container is typically 50 to 500 g, and preferably 100 to 400 g.
[0051] In addition, the heat sealing (heat sealing process) in the above-mentioned production method is preferably performed while degassing the air in the packaging container. Such heat sealing while degassing can be performed by using a known degassing sealer, for example.
[0052] In the above manufacturing method, the temperature of heat sealing (heat sealing process) is preferably higher than the melting point of the inner surface layer 12 and lower than the melting point of the outer surface layer 11. This more reliably prevents the problem of being caught by the hot plate and ensures good heat sealing properties. More specifically, the temperature is preferably 120 to 155°C, more preferably 125 to 145°C.
[0053] <How to keep bean sprouts fresh> The method for preserving the freshness of bean sprouts in this embodiment uses the above-mentioned packaging container for bean sprouts (e.g., the above-mentioned packaging container 1) to prepare a package containing bean sprouts and preserve the freshness of the bean sprouts. Specifically, the method preserves the freshness of the bean sprouts (suppresses deterioration of the freshness of the bean sprouts) by obtaining a package containing bean sprouts by, for example, the method described above in <Production method of package containing bean sprouts>. In order to enhance the effect of preserving freshness, the package containing the bean sprouts is preferably stored in an environment of 2 to 10°C.
[0054] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can be adopted. Furthermore, the present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of the present invention are included in the present invention. EXAMPLES
[0055] The embodiments of the present invention will be described in detail based on examples and comparative examples. However, the present invention is not limited to the examples.
[0056] <Film manufacturing> As the raw material polypropylene, the following product numbers manufactured by Japan Polypropylene Corporation were prepared. [Raw material for outer surface layer: propylene homopolymer or propylene random copolymer] Novatec PP FB3B (propylene homopolymer) or Wintec WFW5T (propylene random copolymer) [Raw material for inner surface layer: Random copolymer of propylene] Wintech WFX4TA or Wintech WFW4
[0057] Furthermore, as the raw linear low-density polyethylene, metallocene linear low-density polyethylene "Evolue (registered trademark) SP2040" manufactured by Prime Polymer Co., Ltd. was prepared.
[0058] The combinations of the raw materials for the outer surface layer and the inner surface layer were as shown in Table 1 below.
[0059] The raw materials for the outer surface layer and the inner surface layer were melted and extruded using a multi-die. The extrusion amount of each raw material was adjusted so that the final film had a thickness of 25 μm and a thickness ratio D B1 / D B2 (DB1 is the thickness of the outer surface layer, D B2 represents the thickness of the inner surface layer) was adjusted to the value shown in Table 1. The extruded molten film was cooled with a cooling roll to obtain the unstretched films of Examples 1-6 and Comparative Examples 1-2. In Comparative Example 2, the film was further stretched 4 times in the longitudinal direction and 4 times in the transverse direction according to a conventional method to obtain a stretched film.
[0060] <Manufacturing of packaging containers (bags)> The films obtained in each of the Examples and Comparative Examples were cut to a predetermined size and then heat sealed using an impulse sealer (manufactured by Fuji Impulse Co., Ltd., FI-400Y-10PK) leaving an opening to obtain a bag.
[0061] <Bean sprout packaging> 210g of mung bean sprouts were placed in the inner space of the bag (inner dimensions: 180mm x 210mm) obtained above. Next, a vacuum sealer (Fuji Impulse, V-301) was used to form a 10mm wide heat seal at the opening of the bag while visually checking that the inner space of the bag was in a vacuum state. The sealing time was about 2 seconds. Apart from the problem of the hot plate being absorbed, all the bags were sealed without any problems in terms of airtightness. As a result, a package containing bean sprouts was obtained. The internal surface area of the obtained package containing bean sprouts was 7.2×10 -2 m 2 It was.
[0062] <Measurements of various values> The melting points (and melting point difference) of the inner and outer surface layers, and the crystallization peak area ratio (S B1 / S B2 ) was determined using an SII Corporation device (model number: DSC6220) at a measurement temperature of 25 to 300°C, a temperature increase rate of 5°C / min, and in a nitrogen atmosphere (flow rate: 30 ml / min), as described above. To and Tc were also calculated using the above-mentioned calculation method.
[0063] <Evaluation> -Whether or not the heat plate is removed In the above-mentioned "bean sprout packaging", when a 10 mm wide heat-sealed portion was formed at the opening of the bag, an evaluation was made as to whether or not the bag was broken by the hot plate.
[0064] - Drop test (whether pinholes occur due to impact) The bean sprout-containing package obtained above was dropped onto the floor from a height of 1 m, and an evaluation was performed to see whether pinholes were formed in the film.
[0065] Freshness retention (whether or not it expands) The package containing the bean sprouts obtained above was stored at 10°C for 72 hours, and then the package was observed for swelling. The presence of swelling indicates that the respiration of the bean sprouts is not well controlled, which is undesirable in terms of freshness retention. Conversely, the absence of swelling indicates that it is desirable in terms of freshness retention.
[0066] The bag composition, various values, evaluation results, etc. are summarized in Table 1.
[0067] [Table 1]
[0068] As shown in the above table, when bean sprouts were packaged (sealed by heat sealing) in packaging containers (Examples 1 to 6) that had outer and inner surface layers containing specific materials and in which the melting point of the outer surface layer was 10 to 70°C higher than that of the inner surface layer, the occurrence of hot plate sticking was sufficiently suppressed. In addition, the freshness of the bean sprouts was well maintained. On the other hand, in a packaging container in which the difference in melting point between the outer surface layer and the inner surface layer is less than 10° C. (7° C.), the heat plate breakage could not be sufficiently suppressed (Comparative Example 1). Furthermore, the packaging container made of a stretched film was rated poorly for freshness retention (Comparative Example 2), presumably due to insufficient gas permeability.
[0069] When the example is analyzed in more detail, the melting point difference between the outer surface layer and the inner surface layer is 17°C, SB1 / S B2 In Example 4, where the value of S is 0.7, some heat loss occurred. B1 / S B2 In Examples 1 to 3, 5 and 6, in which the value of was smaller, no hot plate adhesion occurred.
[0070] In addition, pinholes were generated in the drop test in Example 5, but no pinholes were generated in the other examples. This is because FB3B (a homopolymer of propylene) was used as the material for the outer surface layer, and the outer surface layer was relatively thick (D B1 / D B2 It is assumed that this is related to 6). [Explanation of symbols]
[0071] 1. Packaging containers (packaging containers for bean sprouts) 10 Film 11 Outer surface layer 12 Inner surface layer
Claims
1. A packaging container for bean sprouts, comprising: The container comprises at least an outer surface layer and an inner surface layer; the outer surface layer and the inner surface layer contain at least one selected from the group consisting of non-oriented polypropylene and non-oriented polyethylene; The melting point of the outer surface layer is 10 to 70° C. higher than the melting point of the inner surface layer; The crystallization peak area per unit mass of the outer surface layer in differential scanning calorimetry is S B1 The crystallization peak area per unit mass of the inner surface layer is S B2 When this is done, S B1 / S B2 is less than 1, The outer surface layer and the inner surface layer are in direct contact with each other, with no additional layers present between the two layers.
2. The bean sprout packaging container according to claim 1, the outer surface layer comprises at least one selected from the group consisting of a propylene homopolymer, a propylene block copolymer, and a propylene random copolymer; The packaging container, wherein the inner surface layer comprises at least one selected from the group consisting of a random copolymer of propylene, a low density polyethylene, and a linear low density polyethylene.
3. The packaging container for bean sprouts according to claim 1 or 2, When bean sprouts are sealed in the packaging container for bean sprouts, the oxygen transmission amount To per 100 g of bean sprouts at 23° C. and 60% RH is 40 cc / 100 g day atm or more and 400 cc / 100 g day atm or less; When bean sprouts are sealed in the packaging container, Tc / To is 1 or more, where Tc is the amount of carbon dioxide permeation per 100 g of bean sprouts at 23° C. and 60% RH.
4. The packaging container for bean sprouts according to any one of claims 1 to 3, The thickness of the outer surface layer is D B1 and the thickness of the inner surface layer is D B2 When this is done, D B1 / D B2 A packaging container having a value of 0.1 to 5.
5. A step of placing bean sprouts in an internal space of the packaging container for bean sprouts according to any one of claims 1 to 4; a step of heat-sealing an opening of the packaging container containing the bean sprouts while degassing the packaging container; A method for producing a package containing bean sprouts, comprising the steps of:
6. A method for preserving the freshness of bean sprouts, comprising: placing bean sprouts in the internal space of a packaging container for bean sprouts described in any one of claims 1 to 4; heat-sealing an opening of the packaging container while degassing the packaging container to produce a package containing bean sprouts, thereby preserving the freshness of the bean sprouts.
Citation Information
Patent Citations
Gas high-permeable multilayer film
JP1996216307A
Laminated stretched film
JP2003025524A
Separator for battery
JP2013048081A
Easily tearable multilayer film
JP2015139961A
Package containing bean sprout, and method for retaining freshness of bean sprout
JP2017190144A