Dispersion
A dispersion of small and large metal oxide particles with specific size and concentration ratios stabilizes the mixture, reducing viscosity and pressure loss by suppressing sedimentation and aggregation, improving dispersibility and heat transfer.
Patent Information
- Application Number
- JP2021045415
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-19
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-03-19
AI Technical Summary
Existing techniques for dispersing solid particles in a liquid lead to increased viscosity and pressure loss, particularly when used as a heat transport fluid, due to the agglomeration and sedimentation of particles.
A dispersion comprising small and large metal oxide particles with distinct size distributions and concentrations, where small particles with a diameter of 10 nm or less and large particles between 100 nm and 1 μm are used, along with a zeta potential of 35 mV or more, to suppress sedimentation and aggregation.
The dispersion effectively reduces viscosity and pressure loss, maintaining fluidity and stability by using osmotic pressure and repulsive forces between particles, thereby enhancing dispersibility and heat transfer properties.
Smart Images

Figure 0007593847000001 
Figure 0007593847000002 
Figure 0007593847000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a dispersion. [Background technology]
[0002] Conventionally, dispersions in which solid particles are dispersed in a liquid have been used in various industrial fields. For example, in order to improve the thermal conductivity of a heat transport fluid used in a heat exchanger, a technology has been proposed in which a dispersion in which solid particles are dispersed in a base liquid is used as the heat transport fluid. In addition, a dispersion in which a pigment (fine particles) is dispersed in a binder is used as a paint, a printing ink, etc.
[0003] A technique has been proposed for suppressing the aggregation of solid particles and improving the dispersibility in a dispersion in which solid particles are dispersed in a liquid (see, for example, Patent Document 1 and Non-Patent Document 1). Patent Document 1 discloses a technique for suppressing the aggregation of particles in a dispersion in which fine particles having a diamond structure are dispersed in a medium such as water by adding a bisphenol sulfonic acid polymer and a nitrogen-containing cationic polymer as dispersants. Non-Patent Document 1 also discloses a liquid dispersant and anti-settling agent whose main components are a wet oligomer and a high molecular weight polymer. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 5691007 [Non-patent literature]
[0005] [Non-Patent Document 1] Kyoeisha Chemical Co., Ltd., "KYOEI 2017 No.143", pages 9-10, "Dispersant for inorganic particles and silica, anti-settling agent "Floren DOPA-100"", [online], [Retrieved November 13, 2020], Internet <URL:https: / / www.kyoeisha.co.jp / wpja / wp-content / uploads / 2017 / 06 / 18f4991f62203ee64eee1fcafc585653.pdf> Summary of the Invention [Problem to be solved by the invention]
[0006] When the techniques described in Patent Document 1 and Non-Patent Document 1 are used to improve the dispersibility of solid molecules, the viscosity of the dispersion increases. Therefore, when the dispersion is used as a heat transport fluid, for example, there is a problem that the pressure loss increases when the dispersion is made to flow.
[0007] In view of the above problems, an object of the present invention is to provide another technique for suppressing settling of solid particles in a dispersion in which solid particles are dispersed in a liquid. [Means for solving the problem]
[0008] The present invention has been made to solve at least part of the above-mentioned problems, and can be realized in the following forms.
[0009] (1) According to one embodiment of the present invention, there is provided a dispersion comprising a base liquid, small metal oxide particles having a particle diameter D50 of 10 nm or less at 50% cumulative volume in a volume-based particle size distribution, and large metal oxide particles having a particle diameter D50 of more than 100 nm and less than 1 μm at 50% cumulative volume in a volume-based particle size distribution, and a concentration of the small particles in the dispersion of 0.16 wt % or less.
[0010] According to this configuration, the dispersion contains two types of metal oxide particles with significantly different sizes. When an appropriate amount of small particles, which are small metal oxide particles, are present between large particles, which are large metal oxide particles, the base liquid flows between the large particles due to osmotic pressure, suppressing aggregation of the large particles and suppressing sedimentation of the large particles.
[0011] (2) In the dispersion of the above form, the small particles may be crystallites and / or aggregates of the metal oxide, in which the particle diameter D50 at 50% cumulative volume in the volume-based particle size distribution is 0.8 nm or more and less than 4 nm, and the particle diameter D90 at 90% cumulative volume is 2.5 times or less than the particle diameter D50. Since such small particles have a uniform particle diameter, the dispersion state of the small particles is stabilized. Therefore, the sedimentation of the large particles can be further suppressed.
[0012] (3) In the dispersion of the above form, the concentration of the large particles in the dispersion may be 10 wt % or less, thereby making it possible to suppress the viscosity of the dispersion.
[0013] (4) In the dispersion of the above form, the absolute value of the zeta potential of the large particles in the dispersion may be 35 mV or more, thereby making it possible to improve the dispersion stability.
[0014] The present invention can be realized in various aspects, for example, in the form of a heat transport system using a dispersion, or a system including the heat transport system. [Brief description of the drawings]
[0015] [Figure 1] FIG. 2 is an explanatory diagram showing an example of a particle size distribution of small particles. [Diagram 2] FIG. 2 is an explanatory diagram conceptually showing the dispersion of large particles in the dispersion of the present embodiment. [Diagram 3] Sample specifications are shown below. [Figure 4] FIG. 1 is a graph showing the effect of small particles in suppressing the settling of metal oxide particles. [Diagram 5] FIG. 1 is a graph showing the relationship between the concentration of small particles and the sedimentation suppression effect. [Figure 6] FIG. 1 is a graph showing the relationship between the type and average particle size of large particles and the sedimentation suppression effect of small particles. [Figure 7] FIG. 1 is a graph showing the relationship between the average particle size of large particles and the sedimentation suppression effect of small particles. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The dispersion of one embodiment of the present invention comprises a base liquid, small metal oxide particles having an average particle size of 10 nm or less, and large metal oxide particles having an average particle size of more than 100 nm and less than 1 μm.
[0017] (1) Base liquid The base liquid is not particularly limited, and may be, for example, water, an aqueous alcohol solution such as an aqueous ethylene glycol solution or an aqueous propylene glycol solution, paint, printing ink, recording medium, or a binder for cosmetic coloring materials.
[0018] (2) Small particles The small particles are not particularly limited in the type of metal as long as they are metal oxide particles. For example, various metal oxide particles such as zirconia particles, silica particles, alumina particles, magnesia particles, titania particles, etc. can be used. The small particles have an average particle diameter D50 of 10 nm or less, where the cumulative volume is 50% in the volume-based particle size distribution. The particle size distribution of the small particles is measured by dynamic light scattering.
[0019] The small particles are preferably crystallites and / or aggregates of the metal oxide, in which the particle diameter D50 at 50% cumulative volume in the volume-based particle size distribution is 0.8 nm or more and less than 4 nm, and the particle diameter D90 at 90% cumulative volume is 2.5 times or less than the particle diameter D50 at 50% cumulative volume. The volume-based particle size distribution and the mass-based particle size distribution are the same. Such small particles can be produced by the methods described in Japanese Patent No. 4784623, Japanese Patent No. 6658564, and Japanese Patent Publication No. 2011-143340, and are metal oxide particles contained in the metal colloid solution produced by the methods. Such small particles have a uniform particle diameter, so that the dispersion state of the small particles is stabilized. When such a metal colloid solution is added to a liquid in which large particles are added to a base liquid, the sedimentation of the large particles can be suppressed, and the metal colloid solution can be used as a dispersant. In the following description, the particle diameter D50 at which the cumulative volume in the volume-based particle size distribution becomes 50% is also simply referred to as the "average particle diameter."
[0020] Fig. 1 is an explanatory diagram showing an example of the particle size distribution of small particles, which is used in Sample 1 of an example described later, and the small particles are zirconia particles.
[0021] The concentration of the small particles in the dispersion is not particularly limited, but is preferably 0.16 wt % or less, since this keeps the viscosity of the dispersion at an appropriate level and inhibits aggregation of the large particles.
[0022] (3) Large particles The large particles are not particularly limited in the type of metal as long as they are metal oxide particles. For example, various metal oxide particles such as zirconia particles, silica particles, alumina particles, magnesia particles, titania particles, etc. can be used. The type of the large particles may be the same as or different from that of the small particles. The large particles have an average particle diameter D50 at which the cumulative volume in the volume-based particle size distribution is 50% and is greater than 100 nm and less than 1 μm. The particle size distribution of the large particles is also measured by dynamic light scattering, as with the small particles. Since the dispersion contains metal oxide particles, when the dispersion is used as a heat transport fluid, it can exhibit a heat transfer promotion effect.
[0023] The concentration of the large particles in the dispersion is not particularly limited. As described in JP 2018-95845 A, a previous application by the inventors of the present application, it is preferable that the concentration of the large particles in the dispersion is 10 wt% or less, since the viscosity of the dispersion can be suppressed. For example, when the dispersion is used as a heat transport fluid, it is preferable because the pressure loss when the dispersion is made to flow can be suppressed.
[0024] The absolute value of the zeta potential of the large particles in the dispersion is not particularly limited, but it is preferable that the absolute value is 35 mV or more, since the dispersion stability can be improved. The zeta potential of the large particles in the dispersion can be changed by adjusting the type and average particle size of the large particles. In addition, it can be adjusted by the pH of the base fluid.
[0025] As mentioned above, the particle size of large particles and that of small particles differ by two orders of magnitude, so the average particle size of each of the large particles and the small particles in the dispersion can be determined by particle size distribution measurement using dynamic light scattering. In addition, the concentration of each of the large particles and the small particles can be estimated from the relationship between the particle volume and the average particle size D50 in the particle size distribution measurement.
[0026] The large particles and small particles in the dispersion can be identified by the method described in JP 2011-143340 A. That is, a part of the dispersion is dried to prepare a powdered sample, and the sample is subjected to electron diffraction measurement using a high-resolution transmission electron microscope (high-resolution TEM), and the structure and composition of the metal oxide can be identified from the obtained electron diffraction pattern.
[0027] FIG. 2 is an explanatory diagram conceptually showing the dispersion of large particles in the dispersion of this embodiment. The dispersion of this embodiment has a base liquid, small particles 10, and large particles 20. The small particles 10 are metal oxide particles with an average particle diameter of 10 nm or less, and the large particles 20 have an average particle diameter of more than 100 nm and less than 1 μm. In a dispersion having two types of metal oxide particles with a large difference in size, as shown in the figure, an appropriate amount of small particles 10 is present between the large particles 20, and the base liquid flows between the large particles 20 due to osmotic pressure, and a repulsive force acts between the large particles 20, resulting in an osmotic effect. This makes it possible to suppress the aggregation of the large particles 20 and to suppress sedimentation. In addition, even if the large particles 20 sediment over the course of days, the dispersion of this embodiment can easily disperse the large particles 20 and the small particles 10 by stirring.
[0028] According to the dispersion of the present embodiment, the aggregation of large particles can be suppressed by having small particles. Therefore, compared to the case where the aggregation of large particles is suppressed by adding a dispersant such as a surfactant or a polymer to improve the wettability of the solid-liquid interface or by manifesting a steric hindrance effect, the increase in the viscosity of the liquid can be suppressed. As a result, for example, when the dispersion is used in a fluidized state, such as when used as a heat transport fluid, the increase in pressure loss (pump power) can be suppressed. Even when the dispersion contains a dispersant such as a surfactant or a polymer, the amount of dispersant such as a surfactant or a polymer can be reduced compared to the case where the aggregation of large particles is suppressed only by a dispersant such as a surfactant or a polymer, so that the increase in the viscosity of the dispersion can be suppressed.
[0029] The dispersion of this embodiment can be used as a heat transport fluid used in, for example, a battery cooling circuit of an electric vehicle. At this time, a heat transfer promotion effect can be obtained by the dispersed large particles. Furthermore, when the large particles are porous particles capable of capturing ions inside the pores, an insulating effect can be obtained. The dispersion of this embodiment can be used as a heat transport fluid used in various objects such as automobiles other than electric vehicles, other moving objects, air conditioning equipment, fuel cells, inverters, motor generators, etc. The dispersion may also be used as a paint, printing ink, etc. EXAMPLES
[0030] The present invention will be described more specifically with reference to examples, but the present invention is not limited to the following examples. Fig. 3 shows the sample specifications. Using Samples 1 to 16 shown in Fig. 3, the effect of suppressing aggregation and sedimentation in a dispersion in which large particles and small particles are dispersed was confirmed. Samples 1 to 6 are examples, and Samples 7 to 16 are comparative examples.
[0031] <Sample preparation> 1. Sample 1 A first dispersion liquid was prepared by using an ethylene glycol aqueous solution with an ethylene glycol concentration of 50 wt% as a base liquid, and adding zirconia (ZrO2) with an average particle diameter of 300 nm as large particles to the base liquid so that the particle concentration was 10 wt%. Zirconia (ZrO2) was added as small particles to the first dispersion liquid. In the embodiment, zirconia (ZrO2) as small particles was added as a metal colloid solution (described later). As described above, the dispersibility of large particles is improved by adding small particles, so the metal colloid solution can be used as a dispersant. Therefore, in the following explanation and figures, the metal colloid solution is described as a dispersant. In sample 1, a metal colloid solution was added to the first dispersion liquid so that the dispersant concentration was 4.0 wt%, and a dispersion of sample 1 was prepared. The large particles contained in sample 1 are zirconia (ZrO2) with an average particle diameter of 300 nm, and the concentration is 7.0 wt%, and the small particles are zirconia (ZrO2) with an average particle diameter of 1 nm, and the concentration is 0.16 wt%. As described later, the metal colloid solution generally contains ACA (6-aminocaproic acid), which is used as a dispersant, and MEA (monoethanolamine), which is used as a neutralizing agent. Therefore, in FIG. 2, the ACA concentration / MEA concentration is written in parentheses as the concentration of the dispersant, along with the concentration of the metal colloid solution. The ACA concentration in sample 1 is 0.03 wt%, and the MEA concentration is 0.1 wt%.
[0032] 1-1. Metal colloid solution A metal colloid solution was prepared by the method described in Japanese Patent No. 4784623. In this example, 26.73 g of zirconyl nitrate (ZrO(NO3)2·2H2O) and 1.68 g of ACA (6-aminocaproic acid) were added to 100 mL of ethylene glycol aqueous solution with an ethylene glycol concentration of 50 wt%. 6.11 g of MEA (monoethanolamine) was added to 100 mL of ethylene glycol aqueous solution with an ethylene glycol concentration of 50 wt%. A metal colloid solution with a concentration of zirconia as small particles of ZrO20.357 mol / L was obtained by alternately discharging and stirring the A and B solutions using a commercially available homogenizer. The average particle size of the small particles in the metal colloid solution was measured at room temperature (25°C) using Malvern's Zetasizer Nano ZSP. Furthermore, the particle diameter D50 at which the cumulative mass in the particle size distribution reached 50% was 1 nm, and the particle diameter D90 at which the cumulative mass reached 90% was twice the particle diameter D50.
[0033] 2. Sample 2 A dispersion of Sample 2 was prepared by adding the same colloidal solution as Sample 1 as a dispersant to the same first dispersion as Sample 1 so that the dispersant concentration was 1.0 wt%. The large particles contained in Sample 2 were zirconia (ZrO2) with an average particle size of 300 nm, with a concentration of 7.0 wt%, and the small particles were zirconia (ZrO2) with an average particle size of 1 nm, with a concentration of 0.04 wt%.
[0034] 3. Sample 3 A dispersion of Sample 3 was prepared by adding the same colloidal solution as Sample 1 as a dispersant to the same first dispersion as Sample 1 so that the dispersant concentration was 3.0 wt%. The large particles contained in Sample 3 were zirconia (ZrO2) with an average particle diameter of 300 nm, with a concentration of 7.0 wt%, and the small particles were zirconia (ZrO2) with an average particle diameter of 1 nm, with a concentration of 0.12 wt%.
[0035] 4. Sample 4 As in sample 1, an ethylene glycol aqueous solution with an ethylene glycol concentration of 50 wt% was used as the base liquid, and silica (SiO2) with an average particle size of 300 nm was added as the large particles to the base liquid so that the particle concentration was 10 wt%, to prepare a second dispersion. The same metal colloid solution used in sample 1 was added as a dispersant to the second dispersion so that the dispersant concentration was 4.0 wt%, to prepare a dispersion of sample 4. The large particles contained in sample 4 were silica (SiO2) with an average particle size of 300 nm, with a concentration of 7.0 wt%, and the small particles were zirconia (ZrO2) with an average particle size of 1 nm, with a concentration of 0.16 wt%. In other words, sample 4 is the same as sample 1, except for the type of large particles.
[0036] 5. Sample 5 As in sample 1, an ethylene glycol aqueous solution with an ethylene glycol concentration of 50 wt% was used as the base liquid, and silica (SiO2) with an average particle size of 200 nm was added as the large particles to the base liquid so that the particle concentration was 10 wt%, to prepare a third dispersion. The same metal colloid solution as used in sample 1 was added as a dispersant to the third dispersion so that the dispersant concentration was 4.0 wt%, to prepare a dispersion of sample 5. The large particles contained in sample 5 were silica (SiO2) with an average particle size of 200 nm, with a concentration of 7.0 wt%, and the small particles were zirconia (ZrO2) with an average particle size of 1 nm, with a concentration of 0.16 wt%. In other words, sample 5 is similar to sample 4, except that the average particle size of the large particles in sample 5 is different from that in sample 4.
[0037] 6. Sample 6 As in sample 1, an ethylene glycol aqueous solution with an ethylene glycol concentration of 50 wt% was used as the base liquid, and silica (SiO2) with an average particle size of 500 nm was added as the large particles to the base liquid so that the particle concentration was 10 wt%, to prepare a fourth dispersion. The same metal colloid solution used in sample 1 was added as a dispersant to the fourth dispersion so that the dispersant concentration was 4.0 wt%, to prepare a dispersion of sample 6. The large particles contained in sample 6 were silica (SiO2) with an average particle size of 500 nm, with a concentration of 7.0 wt%, and the small particles were zirconia (ZrO2) with an average particle size of 1 nm, with a concentration of 0.16 wt%. In other words, sample 6 is similar to samples 4 and 5, except that the average particle size of the large particles is different from samples 4 and 5.
[0038] 7. Sample 7 A dispersion of Sample 7 was prepared by adding the same metal colloid solution used in Sample 1 as a dispersant to the first dispersion liquid used in Sample 1 so that the dispersant concentration was 5.0 wt%. The large particles contained in Sample 7 were zirconia (ZrO2) with an average particle size of 300 nm and had a concentration of 7.0 wt%, and the small particles were zirconia (ZrO2) with an average particle size of 1 nm and had a concentration of 0.20 wt%. In other words, Sample 7 is similar to Sample 1 except for the concentration of the small particles and the concentration of the dispersant, which are different from Sample 1.
[0039] 8. Sample 8 A dispersion of Sample 8 was prepared by adding the same metal colloid solution used in Sample 1 as a dispersant to the first dispersion liquid used in Sample 1 so that the dispersant concentration was 7.0 wt%. The large particles contained in Sample 8 were zirconia (ZrO2) with an average particle size of 300 nm and their concentration was 7.0 wt%, and the small particles were zirconia (ZrO2) with an average particle size of 1 nm and their concentration was 0.28 wt%. In other words, Sample 8 is similar to Sample 1 except for the concentration of the small particles and the concentration of the dispersant, which are different from Sample 1.
[0040] 9. Sample 9 A surfactant was added as a dispersant to the first dispersion liquid used in Sample 1 so that the dispersant concentration became 4.0 wt%, to prepare the dispersion of Sample 9. The surfactant used was Leocon 1020H manufactured by Lion Specialty Chemicals Co., Ltd. The large particles contained in Sample 9 were zirconia (ZrO2) with an average particle diameter of 300 nm, the same as Sample 1, and the concentration was 7.0 wt%, and no small particles were included.
[0041] 10. Sample 10 A dispersion of Sample 10 was prepared by adding polyethylene glycol as a dispersant to the first dispersion liquid used in Sample 1 so that the dispersant concentration became 4.0 wt%. The large particles contained in Sample 10 were zirconia (ZrO2) with an average particle diameter of 300 nm, the same as in Sample 1, and the concentration was 7.0 wt%, and no small particles were contained.
[0042] 11. Sample 11 ACA / MEA was added as a dispersant to the first dispersion liquid used in Sample 1 to prepare a dispersion of Sample 11. The ACA concentration was 0.03 wt%, and the MEA concentration was 0.1 wt%. The dispersant concentration was added to 4.0 wt%, to prepare a dispersion of Sample 10. The large particles contained in Sample 11 are zirconia (ZrO2) with an average particle diameter of 300 nm, the same as Sample 1, and their concentration is 7.0 wt%, and no small particles are included. The concentration of ACA / MEA is the same as that of ACA / MEA contained in Sample 1.
[0043] 12. Sample 12 The first dispersion liquid used in Sample 1 was diluted with the base liquid so that the concentration of large particles was 7.0 wt%, and used as Sample 12. In other words, Sample 12 does not contain a dispersant. The large particles contained in Sample 12 are zirconia (ZrO2) with an average particle diameter of 300 nm, the same as Sample 1, and the concentration is 7.0 wt%, and no small particles are included.
[0044] 13. Sample 13 As in Sample 1, an ethylene glycol aqueous solution with an ethylene glycol concentration of 50 wt% was used as the base liquid, and alumina (Al2O3) with an average particle size of 4000 nm was added as the large particles to the base liquid so that the particle concentration was 10 wt%, to prepare a fifth dispersion. The same metal colloid solution as used in Sample 1 was added as a dispersant to the fifth dispersion so that the dispersant concentration was 4.0 wt%, to prepare a dispersion of Sample 13. The large particles contained in Sample 13 were alumina (Al2O3) with an average particle size of 4000 nm, with a concentration of 7.0 wt%, and the small particles were zirconia (ZrO2) with an average particle size of 1 nm, with a concentration of 0.16 wt%. That is, Sample 13 is similar to Sample 1 except for the type and average particle size of the large particles.
[0045] 14. Sample 14 As in Sample 1, an ethylene glycol aqueous solution with an ethylene glycol concentration of 50 wt% was used as the base liquid, and titanium dioxide (TiO2) with an average particle diameter of 6000 nm was added as the large particles to the base liquid so that the particle concentration was 10 wt%, to prepare a sixth dispersion. The same metal colloid solution as used in Sample 1 was added as a dispersant to the sixth dispersion so that the dispersant concentration was 4.0 wt%, to prepare a dispersion of Sample 14. The large particles contained in Sample 14 were titanium dioxide (TiO2) with an average particle diameter of 6000 nm, with a concentration of 7.0 wt%, and the small particles were zirconia (ZrO2) with an average particle diameter of 1 nm, with a concentration of 0.16 wt%. That is, Sample 14 is similar to Sample 1 except for the type and average particle diameter of the large particles.
[0046] 15. Sample 15 As in Sample 1, an ethylene glycol aqueous solution with an ethylene glycol concentration of 50 wt% was used as the base liquid, and silica (SiO2) with an average particle size of 100 nm was added as the large particles to the base liquid so that the particle concentration was 10 wt%, to prepare a seventh dispersion. The same metal colloid solution used in Sample 1 was added as a dispersant to the seventh dispersion so that the dispersant concentration was 4.0 wt%, to prepare a dispersion of Sample 15. The large particles contained in Sample 15 were silica (SiO2) with an average particle size of 100 nm, with a concentration of 7.0 wt%, and the small particles were zirconia (ZrO2) with an average particle size of 1 nm, with a concentration of 0.16 wt%. In other words, Sample 15 is similar to Sample 1, except for the type and average particle size of the large particles.
[0047] 16. Sample 16 As in Sample 1, an ethylene glycol aqueous solution with an ethylene glycol concentration of 50 wt% was used as the base liquid, and silica (SiO2) with an average particle size of 1000 nm was added as the large particles to prepare an 8th dispersion so that the particle concentration was 10 wt%. The same metal colloid solution as used in Sample 1 was added as a dispersant to the 8th dispersion so that the dispersant concentration was 4.0 wt% to prepare a dispersion of Sample 16. The large particles contained in Sample 16 were silica (SiO2) with an average particle size of 1000 nm, with a concentration of 7.0 wt%, and the small particles were zirconia (ZrO2) with an average particle size of 1 nm, with a concentration of 0.16 wt%. In other words, Sample 15 is the same as Sample 1, except for the type and average particle size of the large particles.
[0048] The time (days) required for settling, the viscosity ratio (the viscosity of each sample relative to the composition not including the dispersant), and the zeta potential of the large particles were measured using Samples 1 to 16. The measurement methods are as follows.
[0049] <Time required for sinking> After preparing the sample, it was left to stand and visually confirmed whether or not there was phase separation. If a transparent supernatant portion amounting to 50% or more of the liquid height appeared, it was judged that sedimentation had occurred.
[0050] <Viscosity ratio> The viscosity was measured at 25°C using a TA Instruments dynamic viscoelasticity measuring device ARES-G2 in accordance with the JIS Z 8803:2011 method for measuring viscosity using a coaxial double cylindrical rotational viscometer.
[0051] <Zeta potential of large particles> Measurements were performed at 25°C using a Malvern Panalytical Zetasizer Nano ZSP in accordance with JIS Z 8836:2017 electrophoretic light scattering (ELS) method.
[0052] FIG. 4 is a diagram showing the effect of small particles in suppressing the precipitation of metal oxide particles. As shown in the figure, sample 1 and samples 9 to 12 have the same type, average particle size, and concentration of large particles. No dispersant was added to sample 12, and the time required for precipitation was 5.0 days. In contrast, sample 11 contains the same amount (wt%) of ACA / MEA contained in the metal colloid solution used as the dispersant in sample 1 as in sample 1. The time required for precipitation in sample 11 is 5.0 days, which is the same as that in sample 12 to which no dispersant was added. In other words, the type and amount (wt%) of the dispersant in sample 11 does not exhibit the effect of suppressing precipitation.
[0053] In contrast, in samples 9 and 10, the amount of dispersant was increased to 4.0 wt% and the type of dispersant was changed. As a result, the time required for settling was 7.5 days for sample 9 and 6.0 days for sample 10, demonstrating the effect of suppressing settling. However, sample 10 has a viscosity ratio of 1.1, resulting in large pressure loss.
[0054] Sample 1 contains 4.0 wt% of metal colloid solution containing the above-mentioned small particles (zirconia particles with an average particle size of 1 nm) as a dispersant, the same amount as Samples 9 and 10. Sample 1 took 12 days to settle, and was more effective in suppressing settling than Samples 9 and 10. In addition, the viscosity ratio was 1.0, which was the same viscosity as Sample 12, which did not contain a dispersant, and the increase in viscosity could be suppressed. In addition, Sample 1 is a dispersion equivalent to Sample 11 to which small particles were added, and it can be said that the addition of small particles provided a settling suppression effect. From the above, it can be said that the settling of particles is suppressed by including large particles and small particles in the dispersion.
[0055] FIG. 5 is a diagram showing the relationship between the concentration of small particles and the sedimentation suppression effect. All of the samples shown in FIG. 5 have zirconia particles with an average particle diameter of 300 nm as the large particles and zirconia particles with an average particle diameter of 1 nm as the small particles. As described above, the small particles are contained in a metal colloid solution as a dispersant. In the samples shown in FIG. 5, the concentration (wt%) of small particles increases as you go down the row of the table. Samples 1 to 3 took longer to settle than samples 9 to 12 (FIG. 4) that did not contain small particles, and a sedimentation suppression effect was obtained. On the other hand, samples 7 and 8 both took 0.2 days to settle, which was shorter than samples 9 to 12 (FIG. 4) that did not contain small particles, and no sedimentation suppression effect was observed. Samples 7 and 8 had high viscosity, with viscosity ratios of 1.9 and 2.1, respectively. It is considered that the high concentration of small particles in samples 7 and 8 caused poor fluidity, making aggregation and sedimentation more likely to occur. From the results shown in FIG. 5, it is possible to suitably suppress the settling of metal oxide particles when the concentration of small particles is 0.16 wt % or less.
[0056] FIG. 6 is a diagram showing the relationship between the type and average particle size of large particles and the sedimentation suppression effect of small particles. All of the samples shown in FIG. 6 have zirconia particles with an average particle size of 1 nm as small particles, and their concentration is 0.16 wt%. As described above, the small particles are contained in a metal colloid solution as a dispersant. The samples shown in the figure have different types and average particle sizes of large particles. In addition to the zeta potential, time required for sedimentation, and viscosity ratio of the large particles, FIG. 6 shows the time required for each sample to sediment without a dispersant (a dispersion of only base liquid and large particles) to show the sedimentation suppression effect of the small particles.
[0057] As shown in the figure, for Samples 1 and 4, the time required for settling without a dispersant was 5.0 days, whereas for Samples 1 and 4 containing small particles, the time required for settling was 12 days, which indicates that the small particles have an effect of suppressing settling. 13 and sample 14 For the sample without dispersant, the time required for settling was 0.2 days, whereas the time required for settling was 1.1 days for the sample with small particles. 13 and sample 14 The time required for settling was 0.2 days for the sample, and the time required for settling did not change even when small particles were added. 13 and sample 14 In Sample 1 and Sample 2, the effect of suppressing sedimentation by small particles was not obtained. 4 Although the types of large particles are different, the average particle size is 300 nm, and the sample 13 and sample 14 The average particle diameters of the large particles in Samples 1 and 2 are 4000 nm and 6000 nm, respectively, which are significantly larger than those in Samples 1 and 4. From these results, it is considered that, regardless of the type of large particles, when the average particle diameter of the large particles is on the order of μm, the aggregation suppression effect cannot be obtained by adding small particles.
[0058] FIG. 7 is a diagram showing the relationship between the average particle size of large particles and the sedimentation suppression effect of small particles. All of the samples shown in FIG. 7 have zirconia particles with an average particle size of 1 nm as small particles, and their concentration is 0.16 wt%, similar to the sample shown in FIG. 6. The small particles are contained in a metal colloid solution as a dispersant, as described above. All of the samples shown in the figure contain silica (SiO2) as large particles, but the average particle sizes are different from each other. In FIG. 7, in addition to the zeta potential, time required for sedimentation, and viscosity ratio of the large particles, in order to show the sedimentation suppression effect of the small particles, the time required for sedimentation in each sample without a dispersant (a dispersion of only the base liquid and large particles) is shown, similar to FIG. 6.
[0059] As shown in the figure, sample 15 did not settle for 12 days or more regardless of the presence or absence of small particles. For sample 16, the time required for settling was 2.0 days without a dispersant, whereas sample 16 with small particles also took 2.0 days to settle, and there was no change in the time required for settling even when small particles were added. That is, sample 16 did not obtain a settling suppression effect due to small particles. For sample 5, the time required for settling was 6.0 days without a dispersant, whereas sample 5 with small particles took 12 days to settle. For sample 4, the time required for settling was 5.0 days without a dispersant, whereas sample 4 with small particles took 12 days to settle. For sample 6, the time required for settling was 3.0 days without a dispersant, whereas sample 6 with small particles took 6.0 days to settle. Thus, it can be said that for samples 4 to 6, a settling suppression effect due to small particles was obtained. The samples shown in Figure 7 have the same type of large particles but different average particle diameters. From the results shown in Figures 6 and 7, it is believed that the effect of suppressing sedimentation by small particles can be obtained when the average particle diameter is greater than 100 nm and smaller than 1000 nm (1 μm), regardless of the type of large particles. As shown in Figures 6 and 7, Samples 1 and 4 to 6 have absolute values of the zeta potential of the large particles of 35 mV or more, which means that they have high dispersibility.
[0060] In addition, as shown in Figures 4 to 7, Samples 1 to 6 have a viscosity ratio of 1.0, and the increase in viscosity and the decrease in fluidity can be suppressed. In other words, by using a metal colloid solution containing small particles as a dispersant, the amount of surfactant and polymer dispersant used can be reduced. This makes it possible to suppress the viscosity of the dispersion.
[0061] As described above, according to the present invention, in a dispersion containing metal oxide particles, sedimentation of the metal oxide particles can be suppressed.
[0062] The present invention has been described above based on the embodiments and examples, but the above-mentioned embodiments are intended to facilitate understanding of the present invention and do not limit the present invention. The present invention may be modified or improved without departing from the spirit and scope of the claims, and the present invention includes equivalents thereof. Furthermore, if a technical feature is not described as essential in this specification, it may be deleted as appropriate. [Explanation of symbols]
[0063] 10…Small particles 20...Large particles
Claims
1. A dispersion comprising: A base liquid; Small particles which are metal oxide particles and have a particle diameter D50 of 10 nm or less at a cumulative volume of 50% in a volume-based particle size distribution; Metal oxide particles, which are large particles having a particle diameter D50 at 50% cumulative volume in a volume-based particle size distribution of more than 100 nm and less than 1 μm; Including, the concentration of the small particles in the dispersion is 0.16 wt % or less; The small particles are colloidal particles. Dispersion.
2. 2. The dispersion of claim 1 , The concentration of the large particles in the dispersion is 10 wt % or less. Dispersion.
3. 3. The dispersion according to claim 1 or claim 2, The small particles are crystallites and / or aggregates of the metal oxide having a particle diameter D50 at 50% cumulative volume in a volume-based particle size distribution of 0.8 nm or more and less than 4 nm, and a particle diameter D90 at 90% cumulative volume of 2.5 times or less than the particle diameter D50. Dispersion.
4. 3. The dispersion according to claim 1 or claim 2, the absolute value of the zeta potential of the large particles in the dispersion is 35 mV or more; Dispersion.
Citation Information
Patent Citations
Production of polyester fiber
JP1981091007A
Abrasive slurry excellent in dispersion stability, and manufacturing method for substrate
JP2004331852A
Aqueous dispersion
JP2005179682A
Method for producing catalytic material, catalytic material produced thereby and catalytic body
JP2009172529A
Filler containing liquid composition
JP2013204030A