Solder paste and solder joints

The solder paste with a Sn-containing first powder and Ni-Fe core powder with a Ni surface layer addresses void formation and maintains heat resistance by gradual flux release and high-melting-point compound formation, enhancing joint integrity in high-temperature applications.

JP7594229B1Active Publication Date: 2024-12-04SENJU METAL IND CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024008280
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-01-23
Publication Date
2024-12-04
Estimated Expiration
2044-01-23

AI Technical Summary

Technical Problem

Solder pastes containing flux generate voids during solidification due to gasified flux remaining in the molten solder, especially in high-temperature applications, and TLP pastes with high melting points suffer from decreased fluidity, making it difficult to release gasified flux, leading to void formation.

Method used

A solder paste comprising a first metal powder of Sn and a second metal powder with a core of Ni-Fe alloy and a Ni surface layer, where the Sn content is 20-100% by mass and the Ni-Fe core has 80-99% Ni and 1-20% Fe, with a surface layer thickness of 0.05-1.20 μm, enhancing heat resistance and void suppression.

Benefits of technology

The solder paste effectively suppresses void formation and maintains heat resistance by allowing gradual flux release and formation of high-melting-point compounds, improving joint integrity under high-temperature conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007594229000001_ABST
    Figure 0007594229000001_ABST
Patent Text Reader

Abstract

The present invention provides a solder paste that has excellent heat resistance and can further suppress the occurrence of voids during soldering, and a solder joint formed using the solder paste. [Solution] A solder paste containing a first metal powder, a second metal powder, and a flux is used. The first metal powder contains Sn. The second metal powder 20A has a core portion 201 made of an alloy containing Ni and Fe, and a surface layer 202 made of a metal containing Ni that covers the core portion 201. The Ni content in the metal forming the surface layer 202 of the second metal powder 20A is 50 mass% or more with respect to the total mass of the metal forming the surface layer 202 of the second metal powder 20A. The thickness of the surface layer 202 of the second metal powder 20A is 0.05 μm or more and less than 1.20 μm.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to solder paste and solder joints. [Background technology]

[0002] In recent years, as the operating environment of power semiconductor elements using silicon carbide (SiC) etc. becomes higher, the temperature of solder joints can reach approximately 250 to 280° C. For this reason, there is a demand for high-temperature solder that does not melt when operating under such high-temperature conditions.

[0003] In the manufacture of the above solder joints, various solder pastes are used as soldering materials, such as Ag paste that can be sintered at low temperatures and TLP (Transient Liquid Phase) paste that complies with the European Union's RoHS Directive. The TLP paste is a paste containing multiple types of solder powder. In the TLP paste, the solder powders form a compound with a high melting point when heated. As a result, even if the solder joint is reheated, remelting can be suppressed, and heat resistance can be improved. As such a TLP paste, for example, a paste in which Cu balls and Sn solder balls are dispersed via a flux has been proposed (see Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2012-91223 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, the solder paste containing the flux as described in Patent Document 1 has a problem in that the flux gasified when the solder powder is melted remains in the molten solder, and a large number of voids tend to occur when solidifying. In particular, in the TLP paste in which a compound with a high melting point is formed when solidifying, the fluidity decreases, and the gasified flux is difficult to release to the outside.

[0006] The present invention has been made in consideration of the above circumstances, and has an object to provide a solder paste that has excellent heat resistance and can further suppress the occurrence of voids during solder joining, and a solder joint formed using the solder paste. [Means for solving the problem]

[0007] The present invention includes the following aspects. [1] A solder paste containing a first metal powder, a second metal powder, and a flux, wherein the first metal powder contains Sn, and the second metal powder has a core portion made of an alloy containing Ni and Fe, and a surface layer covering the core portion and made of a metal containing Ni, the content of Sn in the first metal powder is 20 mass% or more and 100 mass% or less with respect to a total mass of the first metal powder, and the content of Ni in the metal forming the core portion of the second metal powder is 80 mass% or more and 99 mass% or less with respect to a total mass of the metal forming the core portion of the second metal powder. a content of Fe in the metal forming the core portion of the second metal powder is 1 mass % or more and 20 mass % or less, relative to a total mass of the metal forming the core portion of the second metal powder; a content of Ni in the metal forming the surface layer of the second metal powder is 50 mass % or more, relative to a total mass of the metal forming the surface layer of the second metal powder; a particle size of the first metal powder is 0.1 to 1000 μm, a particle size of the second metal powder is 0.2 to 1000 μm, and a thickness of the surface layer of the second metal powder is 0.05 μm or more and less than 1.20 μm. [2] The solder paste according to [1], wherein the content of the first metal powder is 30 to 99 mass% based on the total mass of the first metal powder and the second metal powder, and the content of the second metal powder is 1 to 70 mass% based on the total mass of the first metal powder and the second metal powder. [3] A solder joint formed using the solder paste according to [1] or [2]. Effect of the Invention

[0008] According to the present invention, it is possible to provide a solder paste that has excellent heat resistance and is capable of further suppressing the occurrence of voids during soldering. [Brief description of the drawings]

[0009] [Figure 1] 3 is a schematic diagram showing a cross section of a second metal powder 20A in the first embodiment of the solder paste. FIG. [Diagram 2] 13 is a schematic diagram showing a cross section of a second metal powder 20B in a second embodiment of the solder paste. FIG. [Diagram 3] 13 is a schematic diagram showing a cross section of a second metal powder 20C in a third embodiment of the solder paste. FIG. [Figure 4] 1 shows X-ray observation images of voids in solder joints in Examples 1 to 3, 5, and 6 and Comparative Examples 1 and 2. [Diagram 5] FIG. 1 is a diagram showing DSC curves for Examples 1 to 3 and 5 and Comparative Examples 1 and 2. [Figure 6] FIG. 2 is a graph showing the amounts of heat generated in Examples 1 to 3 and 5 and Comparative Examples 1 and 2. [Figure 7] 1 is a graph showing the ratio of the calorific value of Examples 1 to 3, 5, and Comparative Example 2 to the calorific value of Comparative Example 1. [Figure 8] 1 shows photographs of compound formation after reflow in the solder pastes of Examples 1 to 3, 5, and 6 and Comparative Examples 1 and 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] In this specification, the terms "comprise" and "containing" are concepts which encompass all of "comprise," "consist essentially of," and "consist of," respectively.

[0011] In this specification, the terms "first metal," "second metal," and "third metal" may mean "particles made of the first metal," "particles made of the second metal," and "particles made of the third metal," respectively. In this specification, the terms "first metal powder," "second metal powder," and "third metal powder" may mean "a group of particles formed of a first metal," "a group of particles formed of a second metal," and "a group of particles formed of a third metal," respectively.

[0012] (Solder paste first embodiment) The solder paste according to the first embodiment contains a first metal powder, a second metal powder, and a flux. The first metal powder contains Sn. The second metal powder has a core portion made of an alloy containing Ni and Fe, and a surface layer containing Ni that covers the core portion.

[0013] <First metal powder> The metal constituting the first metal powder (hereinafter referred to as the first metal) is a metal containing Sn. The first metal may contain a metal other than Sn. Examples of metals other than Sn that may be included in the first metal include Ag, Cu, In, Bi, Ni, Ge, P, Co, Ga, Zn, Sb, Pb, Au, Al, Pt, Pd, Fe, Mn, Zr, and As. These metals other than Sn may include one type or two or more types. The group of metals other than Sn can be arbitrarily selected from these metals.

[0014] The metal that may be contained in the first metal may be each of simple substances Sn and a metal other than Sn, or may be an alloy of Sn and a simple substance of a metal other than Sn.

[0015] The first metal may be, for example, simple Sn, a mixture of Sn and a metal other than Sn, an alloy of Sn and a metal other than Sn, or a mixture of an alloy containing Sn and another metal.

[0016] The first metal may contain unavoidable impurities in addition to the above-mentioned metals. Even if the first metal contains unavoidable impurities, the effects of the present invention are not adversely affected. The first metal may be one type or two or more types.

[0017] The "melting point of a metal or a metal powder" as used herein refers to a melting point measured by differential scanning calorimetry (DSC). The melting point of the first metal can be measured, for example, using a DSC7020 manufactured by Hitachi High-Tech Science Corporation. The melting point of the second metal described below can be measured, for example, using a DSC404-F3Pegasus manufactured by NETZSCH.

[0018] The melting point of the first metal is preferably 300°C or lower, may be 250°C or lower, or may be in the range of 80 to 200°C. When the melting point of the first metal is equal to or lower than the upper limit of the above-mentioned preferable range, the wettability of the solder can be easily ensured.

[0019] The content of Sn in the first metal is 20% by mass or more and 100% by mass or less, based on the total mass of the first metal. In order to fully exhibit the properties of Sn, the content of Sn in the first metal is preferably 90% by mass or more, more preferably 95% by mass or more, and even more preferably 100% by mass, based on the total mass of the first metal.

[0020] In this specification, the "particle size of a metal or particle size of a metal powder" refers to the average particle size measured on a volume basis using a laser diffraction / scattering type particle size distribution measuring device. The average particle size can be measured, for example, using a laser diffraction / scattering particle size distribution measuring device (MT3300EXII) manufactured by Microtrack Bell.

[0021] The particle size of the first metal powder is 0.1 to 1000 μm, and preferably 1 to 100 μm. When the particle size of the first metal powder is equal to or larger than the lower limit of the above-mentioned preferred range, wettability is easily ensured, whereas when the particle size is equal to or smaller than the upper limit of the above-mentioned preferred range, an intermetallic compound is more easily formed.

[0022] <Second metal powder> As illustrated in FIG. 1, second metal powder 20A has a core portion 201 and a surface layer 202 that covers core portion 201 in its entirety. Rc means the core diameter of the core portion 201. Rs denotes the thickness of the surface layer 202. The metal forming the core portion 201 is made of an alloy containing Ni and Fe. The metal forming the surface layer 202 is made of a metal containing Ni.

[0023] ≪Surface layer≫ The metal forming the surface layer of the second metal powder may consist of only Ni, or may be a metal containing Ni and a metal other than Ni. The metal containing Ni and a metal other than Ni may be an alloy of Ni and a metal other than Ni. The metal forming the surface layer is preferably Ni alone.

[0024] Examples of metals other than Ni that may be included in the metal forming the surface layer include Ag, Cu, In, Bi, Ge, P, Co, Ga, Zn, Sb, Pb, Au, Al, Pt, Pd, Fe, Mn, Zr, Sn, and As. These metals other than Ni may include one type or may include two or more types. The group of metals other than Ni can be arbitrarily selected from these metals.

[0025] The metal forming the surface layer may contain unavoidable impurities in addition to the above-mentioned metals. Even if unavoidable impurities are contained, the effect of the present invention is not affected.

[0026] When the metal forming the surface layer is a metal containing Ni and a metal other than Ni, the Ni content in the metal forming the surface layer is 50 mass% or more and less than 100 mass%, preferably 70 mass% or more, more preferably 80 mass% or more, even more preferably 90 mass% or more, particularly preferably 95 mass% or more, and most preferably 98 mass% or more, relative to the total mass of the metal forming the surface layer. When the metal forming the surface layer contains Fe, the content of Fe in the metal forming the surface layer is preferably 0 mass % or more and less than 5 mass % with respect to the total mass of the metal forming the surface layer.

[0027] The thickness Rs of the surface layer is not less than 0.05 μm and less than 1.20 μm. The thickness Rs of the surface layer is preferably 0.05 μm, 0.10 μm, 0.15 μm, 0.20 μm, 0.25 μm, 0.30 μm, 0.35 μm, 0.40 μm, 0.45 μm, 0.50 μm, 0.55 μm, 0.60 μm, 0.70 μm, 0.75 μm, 0.80 μm, 0.90 μm, 1.00 μm, 1.10 μm, or 1.15 μm, and the upper and lower limits can be appropriately selected from these values. The thickness Rs of the surface layer may be 0.10 μm or more and less than 1.20 μm, 0.15 μm or more and less than 1.20 μm, 0.20 μm or more and less than 1.20 μm, 0.25 μm or more and less than 1.20 μm, 0.30 μm or more and less than 1.20 μm, 0.35 μm or more and less than 1.20 μm, 0.40 μm or more and less than 1.20 μm, 0.45 μm or more and less than 1.20 μm, or 0.50 μm or more and less than 1.20 μm. Alternatively, it may be 0.55 μm or more and less than 1.20 μm, 0.60 μm or more and less than 1.20 μm, 0.70 μm or more and less than 1.20 μm, 0.75 μm or more and less than 1.20 μm, 0.80 μm or more and less than 1.20 μm, 0.90 μm or more and less than 1.20 μm, 1.00 μm or more and less than 1.20 μm, 1.10 μm or more and less than 1.20 μm, or 1.15 μm or more and less than 1.20 μm. The thickness Rs of the surface layer may be 0.05 μm or more and 1.15 μm or less, 0.05 μm or more and 1.10 μm or less, 0.05 μm or more and 1.00 μm or less, 0.05 μm or more and 0.90 μm or less, 0.05 μm or more and 0.80 μm or less, 0.05 μm or more and 0.75 μm or less, 0.05 μm or more and 0.70 μm or less, 0.05 μm or more and 0.60 μm or less, or 0.05 μm or more and 0.55 μm or less. Alternatively, it may be 0.05 μm or more and 0.50 μm or less, 0.05 μm or more and 0.45 μm or less, 0.05 μm or more and 0.40 μm or less, 0.05 μm or more and 0.35 μm or less, 0.05 μm or more and 0.30 μm or less, 0.05 μm or more and 0.25 μm or less, 0.05 μm or more and 0.20 μm or less, 0.05 μm or more and 0.15 μm or less, or 0.05 μm or more and 0.10 μm or less.

[0028] From the viewpoint of ensuring sufficient heat resistance and further enhancing the void suppression ability, the thickness Rs of the surface layer is preferably 0.10 μm or more and less than 1.20 μm. From the viewpoint of ensuring sufficient void suppression ability and further enhancing heat resistance, the surface layer thickness Rs is preferably 0.05 μm or more and 1.0 μm or less, more preferably 0.05 μm or more and 0.75 μm or less, even more preferably 0.05 μm or more and 0.30 μm or less, particularly preferably 0.05 μm or more and 0.25 μm or less, most preferably 0.05 μm or more and 0.20 μm or less, and may be 0.05 μm or more and 0.15 μm or less, or may be 0.05 μm or more and 0.10 μm or less. When the thickness Rs of the surface layer is equal to or greater than the lower limit, the void suppression ability can be further improved. When the thickness Rs of the surface layer is equal to or less than the upper limit, the heat resistance can be further improved.

[0029] In this specification, the thickness Rs of the surface layer and the core diameter Rc of the core portion of the second metal powder, as well as the thickness Ri of the intermediate layer of the second metal powder in the second embodiment described below and the thickness Rm of the metal layer of the second metal powder in the third embodiment can be measured from the cross-sectional structure of the second metal powder using an optical microscope, SEM, transmission electron microscope (TEM), etc. Alternatively, the thickness Rs of the surface layer of the second metal can be measured using an Auger electron spectrometer based on Auger electron spectroscopy.

[0030] Alternatively, the core diameter Rc of the core portion of the second metal powder can be measured as follows: When producing the second metal powder, the particle diameter of the metal powder prepared for use as the core portion can be taken as the core diameter Rc.

[0031] The melting point of the metal forming the surface layer is preferably above 300°C, more preferably 500°C or higher, and further preferably 600 to 1600°C.

[0032] The surface layer may be a plated layer formed by a plating process. Examples of the plating method include known electroplating and electroless plating.

[0033] At least a part of the surface of the core portion is covered with the surface layer, whereas in Fig. 1, the entire surface of the core portion is covered with the surface layer. The proportion of the surface area of ​​the core portion that is covered by the surface layer relative to the total surface area (100%) of the core portion is preferably 50% or more and 100% or less, more preferably 70% or more and 100% or less, even more preferably 90% or more and 100% or less, particularly preferably 95% or more and 100% or less, and most preferably 100%.

[0034] <Core> The core portion of the second metal powder is made of an alloy containing Ni and Fe. The alloy in the core portion contains Ni and Fe, and has a higher melting point than the first metal powder. The melting point of the alloy in the core portion is preferably above 300°C, more preferably 500°C or higher, and further preferably 600 to 1600°C. When the melting point of the alloy in the core portion is above the lower limit of the above-mentioned preferred range, the heat resistance can be increased, and the shear strength of the soldered joint can be easily increased.

[0035] The alloy in the core portion may contain a metal other than Ni and Fe. That is, the second metal may be an alloy of Ni and Fe, or an alloy of Ni, Fe, and a metal other than these, and among these, an alloy of Ni and Fe is preferable.

[0036] Examples of metals other than Ni and Fe that may be included in the alloy in the core portion include Ag, Cu, In, Bi, Ge, P, Co, Ga, Zn, Sb, Pb, Au, Al, Pt, Pd, Mn, Zr, Sn, and As. These metals other than Ni and Fe may include one type or two or more types. The group of metals other than Ni and Fe can be arbitrarily selected from these metals.

[0037] The metal forming the core part may contain inevitable impurities in addition to the above-mentioned metals. Even if inevitable impurities are contained, the effect of the present invention is not affected. The second metal may be one type or two or more types.

[0038] The Ni content in the metal forming the core portion is 80 mass % or more and 99 mass % or less, and preferably 85 mass % or more and 95 mass % or less, based on the total mass of the metal forming the core portion. The content of Fe in the metal forming the core part is from 1 mass % to 20 mass %, and preferably from 5 mass % to 15 mass %, based on the total mass of the metal forming the core part. When the contents of Ni and Fe in the metal forming the core portion are within the above-mentioned preferred ranges, intermetallic compounds are formed at an earlier stage, and heat resistance can be improved.

[0039] The core diameter Rc of the core portions 201 of the second metal powder 20A is preferably 0.1 to 1000 μm, more preferably 3 to 300 μm, further preferably 5 to 100 μm, and particularly preferably 10 to 50 μm.

[0040] For the second metal powder 20A, the ratio of the core diameter Rc of the core portion 201 to the thickness Rs of the surface layer 202, expressed as Rc / Rs, is preferably 0.2 to 20,000, more preferably 2 to 2,000, even more preferably 10 to 1,000, particularly preferably 20 to 500, most preferably 30 to 500, and may be 30 to 452. The ratio represented by Rc / Rs is preferably 452, 400, 350, 300, 250, 226, 65, 45, or 30, and the upper and lower limits can be appropriately selected from these values. When Rc / Rs is within the above range, heat resistance is easily improved and voids are easily suppressed.

[0041] The second metal powder has a particle size of 0.2 to 1000 μm, preferably 1 to 100 μm, and more preferably 5 to 50 μm. When the particle size of the second metal is at least the lower limit of the above-mentioned preferred range, wettability is easily ensured, and when it is at most the upper limit of the above-mentioned preferred range, an intermetallic compound is more easily formed.

[0042] The second metal powder 20A may be of one type or of two or more types.

[0043] <Relationship between the content of the first metal powder and the second metal powder> In the solder paste of the first embodiment, the mixing ratio of the first metal powder to the second metal powder is such that the content of the first metal powder is preferably 30 to 99 mass%, more preferably 60 to 95 mass%, even more preferably 70 to 95 mass%, and particularly preferably 80 to 95 mass%, relative to the total content of the first metal powder and the second metal powder (100 mass%). The mixing ratio of the first metal powder and the second metal powder is preferably such that the content of the second metal powder is 1 to 70 mass% relative to the total content of the first metal powder and the second metal powder (100 mass%), more preferably 5 to 40 mass%, even more preferably 5 to 30 mass%, and particularly preferably 5 to 20 mass%.

[0044] In the solder paste according to the first embodiment, the ratio of the content of the first metal powder to the content of the second metal powder, expressed as a mass ratio (content of first metal powder / content of second metal powder), is preferably 4, 8, or 9, and the upper and lower limits can be appropriately selected from these values. The mass ratio expressed as the content of the first metal powder / the content of the second metal powder may be, for example, 1 to 20, 3 to 15, 6 to 10, or 4 to 9.

[0045] <Flux> The solder paste according to the first embodiment contains flux. The components contained in the flux are not particularly limited as long as they produce the effects of the present invention, and examples thereof include resin components such as rosin, activators, thixotropic agents, solvents, metal deactivators, surfactants, silane coupling agents, antioxidants, colorants, and the like.

[0046] Rosins include natural resins containing abietic acid as a main component, mixtures of abietic acid and its isomers, and chemically modified natural resins.

[0047] Examples of the activator include organic acids, amines, and halogen compounds. Examples of the thixotropic agent include ester-based thixotropic agents, amide-based thixotropic agents, and sorbitol-based thixotropic agents.

[0048] The content of the flux in the solder paste is preferably 5 to 30 mass % and more preferably 8 to 15 mass % based on the total mass of the solder paste.

[0049] The solder paste according to the first embodiment described above contains a first metal powder, a second metal powder, and a flux. The first metal powder contains Sn. The second metal powder has a core portion made of an alloy containing Ni and Fe, and a surface layer containing Ni that covers the core portion. In the solder paste of the first embodiment, Sn and an alloy containing Ni and Fe form a high-melting point compound during soldering, so that remelting can be suppressed even if the solder joint is reheated.

[0050] In the solder paste according to the first embodiment, the second metal powder has a core and a surface layer containing Ni that covers the core. The Ni content in the metal that forms the surface layer is 50 mass% or more with respect to the total mass of the metal that forms the surface layer. The thickness of the surface layer is 0.05 μm or more and less than 1.20 μm. In the solder paste according to the first embodiment, since the second metal powder has the above-mentioned surface layer, it has excellent heat resistance and can further suppress the generation of voids during soldering. The reason why such an effect is obtained is not clear, but is presumed to be as follows.

[0051] The surface layer of the second metal powder protects the core of the second metal powder until a certain time has elapsed since the start of reflow. Ni contained in the surface layer of the second metal powder is less reactive with Sn than an alloy containing Ni and Fe, so it is possible to suppress the sudden formation of a compound between the alloy containing Ni and Fe and Sn. As a result, the gasified flux is easily discharged from the solder paste, and the occurrence of voids during solder joining can be further suppressed. By making the thickness of the surface layer 0.05 μm or more, it is possible to suppress the rapid formation of compounds between the alloy containing Ni and Fe and Sn, and it is possible to further suppress the occurrence of voids.

[0052] As the time passes after the start of reflow, the Ni on the surface gradually diffuses into the molten Sn. As the Ni on the surface disappears, the Ni and Fe-containing alloy in the core reacts with the Sn to form a compound with a high melting point. By making the thickness of the surface layer less than 1.20 μm, the Ni in the surface layer can easily diffuse into the molten Sn, forming a compound with a high melting point, thereby improving the heat resistance of the solder joint.

[0053] The solder paste of the first embodiment has improved heat resistance during reflow because the core of the second metal powder, which is an alloy containing Ni and Fe, and the Sn of the first metal powder form a high-melting point compound.

[0054] The reaction that forms the high melting point compound is an exothermic reaction. The calorific value of the first metal powder and the second metal powder contained in the solder paste according to this embodiment is preferably within the following range.

[0055] First, a mixed powder made of a first metal powder and a second metal powder contained in the target solder paste according to this embodiment is prepared (hereinafter, this mixed powder is referred to as a "target sample"). The mixing ratio (mass ratio) of the first metal powder and the second metal powder in the target sample is set to be the same as the mixing ratio (mass ratio) of the first metal powder and the second metal powder in the target solder paste according to this embodiment.

[0056] A mixed powder is prepared that is identical to the target sample except that the second metal powder is replaced with the metal powder of the core portion of the second metal powder (hereinafter, this mixed powder is referred to as a "reference sample"). In the reference sample, the mixing ratio (mass ratio) of the first metal powder to the metal powder of the core portion of the second metal powder is set to be the same as the mixing ratio (mass ratio) of the first metal powder to the second metal powder in the target solder paste according to this embodiment.

[0057] First, the calorific value of a reference sample is measured by differential scanning calorimetry (DSC) according to the following procedure. In the measurement, an EXSTAR DSC7020 (manufactured by Hitachi High-Tech Science Corporation) is used as the measuring device, and the sample is placed in an aluminum pan for measurement. The measurement program is set to 100 to 350°C, with a heating rate of 5°C / min.

[0058] The results of differential scanning calorimetry are shown as follows: the horizontal axis represents time t, and the vertical axis represents heat flow (units are [W] or [J][s] -1 ) or as a DSC curve with the horizontal axis being temperature T and the vertical axis being heat flow. The obtained DSC curve has a large negative value (that is, a large heat absorption) in the vicinity of 235° C. at which the first metal powder containing Sn melts.

[0059] Based on the DSC curve, the heat flow per unit mass (mg) of the reference sample is integrated over time to calculate the integral value Q0' (unit: [J]) per unit mass (mg) of the reference sample from time t0 to time t. Here, time t0 is the time when the temperature of the reference sample reaches 200°C. The time t at which the integrated value Q0' of the heat flow of the reference specimen becomes minimum in the range from 200°C to 350°C is defined as tin0 At time t in0 is the time when the reference sample starts to generate heat. in0 The calorific value from time t to time t is the calorific value of the reference sample (hereinafter, this is referred to as "reference calorific value Q0"). The reference calorific value Q0 is the calorific value per unit mass (mg) of the reference sample.

[0060] The standard heat generation amount Q0 is the temperature T in0 It can also be said that the amount of heat generated from temperature T. Here, time t in0 The temperature of the reference sample at in0 and the temperature of the reference sample at time t is T. T in0 is the temperature of the reference specimen when the integral value Q0' of the heat flow of the reference specimen is minimum in the range from 200°C to 350°C.

[0061] Next, a DSC curve is obtained for the target sample by differential scanning calorimetry in the same manner as for the reference sample. T of the reference sample in0 Similarly, the T in Calculate the temperature T in The calorific value from the temperature T to the target temperature is calculated (hereinafter, this is referred to as the "target calorific value Q"). The target calorific value Q is the calorific value per unit mass (mg) of the target sample. The target heat generation amount Q is the temperature T in It can also be said that the amount of heat generated from temperature T. Here, time t in The temperature of the target sample at in and the temperature of the target sample at time t is T. T in is the temperature of the target sample when the integral value of the heat flow of the target sample is minimum in the range from 200°C to 350°C.

[0062] As will be described later in the Examples, the temperature T in The target heat generation amount Q from temperature T to temperature T is calculated, for example, as shown in FIG. in0 The reference calorific value Q0 from to temperature T is the calorific value in Comparative Example 1.

[0063] temperature T in The ratio of the target calorific value Q of the target sample in the temperature range from temperature T in0 It is preferable that the calorific value is 10% or more and less than 100% relative to the reference calorific value Q0 (100%) of a reference sample in the temperature range of 0.1 to 300°C. The lower limit of the proportion of the target calorific value is preferably 10% or more, more preferably 15% or more, even more preferably 20% or more, particularly preferably 25% or more, and most preferably 30% or more, and may be 40% or more, 50% or more, or 60% or more. The upper limit of the proportion of the target calorific value is not particularly limited, but may be less than 100%, or may be 80% or less.

[0064] As will be described later in the Examples, the temperature T in0 The temperature T of the target sample for the reference calorific value Q0 (100%) in the range from in The ratio of the target calorific value Q in the range of from 0 to 300° C. is calculated, for example, as shown in FIG.

[0065] In summary, the calorific values ​​of the first metal powder and the second metal powder are preferably as follows. Temperature of the target sample per unit mass (mg) measured by differential scanning calorimetry, T in The ratio of the target calorific value Q in the range of 0 to 300°C is the temperature T of the reference sample per unit mass (mg). in0 It is preferable that the calorific value is 10% or more and less than 100% with respect to the reference calorific value Q0 (100%) in the range of from 0.1 to 300°C. The target sample is a mixed powder consisting of a first metal powder and a second metal powder. The mixing ratio (mass ratio) of the first metal powder to the second metal powder in the target sample is the same as the mixing ratio (mass ratio) of the first metal powder to the second metal powder in the solder paste. The reference sample is a mixed powder consisting of a first metal powder and a core metal powder of a second metal powder. The mixing ratio (mass ratio) of the first metal powder and the core metal powder of the second metal powder in the reference sample is the same as the mixing ratio (mass ratio) of the first metal powder and the second metal powder in the solder paste. temperature T in is the temperature of the target sample when the integral value of the heat flow of the target sample is minimum in the range from 200°C to temperature T. The temperature T of the target sample can be from 200°C to 350°C. temperature T in0 is the temperature of the target sample when the integral value of the heat flow of the reference sample is minimum in the range from 200°C to temperature T. The temperature T of the reference sample can be from 200°C to 350°C.

[0066] When the main component of the surface layer of the second metal powder is Cu, Au, Ag, or Pd instead of Ni, Cu, Au, Ag, and Pd are more likely to diffuse into molten Sn than Ni, and therefore the surface layer mainly composed of Cu, Au, Ag, or Pd cannot sufficiently suppress the sudden formation of a compound between the alloy containing Ni and Fe and Sn. Even if the main component of the surface layer of the second metal powder is Bi rather than Ni, Bi dissolves into Sn, so it is not possible to sufficiently prevent the alloy containing Ni and Fe from suddenly forming a compound with Sn. If the main component of the surface layer of the second metal powder is a low-melting point metal such as In rather than Ni, the surface layer will melt within a short time after reflow begins, and it will not be possible to sufficiently prevent the alloy containing Ni and Fe from suddenly forming a compound with Sn.

[0067] In addition, Cu, Au, Ag, and Pd react more easily with Sn to form compounds than Ni, so the surface layer containing Cu, Au, Ag, or Pd forms compounds with Sn, preventing Sn from forming a high-melting compound with an alloy containing Ni and Fe, and as a result, the heat resistance of the solder joint is not sufficiently improved.

[0068] The embodiment of the present invention is not limited to the first embodiment, and may be other embodiments other than the first embodiment. As other embodiments, second to fourth embodiments will be described.

[0069] Second embodiment The solder paste according to the second embodiment is the same as the solder paste according to the first embodiment, except that second metal powder 20A is changed to second metal powder 20B. The solder paste according to the second embodiment is similar to the first, third or fourth embodiment, except that it contains second metal powder 20B. Examples of the core portion 201 and the surface layer 202 in the second metal powder 20B include the same as those described above for the second metal powder 20A.

[0070] As illustrated in FIG. 2, second metal powder 20B has intermediate layer 203 covering core portion 201 between core portion 201 and surface layer 202 covering core portion 201. As illustrated in FIG.

[0071] The intermediate layer may cover a part of the surface of the core portion, or may cover the entire surface of the core portion, and preferably covers the entire surface of the core portion. In FIG. 2, the intermediate layer 203 covers the entire surface of the core portion 201. The proportion of the surface area of ​​the core portion that is covered by the intermediate layer relative to the total surface area of ​​the core portion (100%) is preferably 50% or more and 100% or less, more preferably 70% or more and 100% or less, even more preferably 90% or more and 100% or less, particularly preferably 95% or more and 100% or less, and most preferably 100%.

[0072] Ri denotes the thickness of the intermediate layer 203 . The intermediate layer may be one layer or two or more layers. In the second metal powder 20B illustrated in FIG. 2, the intermediate layer 203 is one layer.

[0073] The composition of the metal forming the intermediate layer 203 is different from the metal forming the core portion 201 and the metal forming the surface layer 202 . The metal forming the intermediate layer may be one kind of elemental metal, or may be an alloy formed of two or more kinds of metal elements.

[0074] Examples of metals that may be contained in the intermediate layer include Ag, Cu, In, Bi, Ni, Ge, P, Co, Ga, Zn, Sb, Pb, Au, Al, Pt, Pd, Fe, Mn, Zr, Sn, and As. These metals may be contained alone or in combination of two or more. The metal group that may be contained in the intermediate layer can be arbitrarily selected from these metals.

[0075] The intermediate layer may contain unavoidable impurities in addition to the above-mentioned metals. Even if the intermediate layer contains unavoidable impurities, the effects of the present invention are not adversely affected. The intermediate layer may be formed of one type of metal, or two or more types of metal.

[0076] The thickness Ri of the intermediate layer may be, for example, 0.01 μm or more and 100 μm or less, 0.05 μm or more and 50 μm or less, or 0.1 μm or more and 10 μm or less.

[0077] The intermediate layer may be a plating formed by a plating process. Examples of the plating method include known electroplating and electroless plating.

[0078] The second metal powder 20B may be of one type or of two or more types.

[0079] Since second metal powder 20B has intermediate layer 203, surface layer 202 of second metal powder 20B can be easily provided.

[0080] Third embodiment In the solder paste according to the third embodiment, the surface layer of the second metal powder is covered with a metal layer. The solder paste according to the third embodiment is similar to the first, second or fourth embodiment, except that the second metal powder has a metal layer.

[0081] As illustrated in FIG. 3, second metal powder 20C has a core portion 201, a surface layer 202 covering core portion 201, and a metal layer 204 covering surface layer 202.

[0082] At least a part of the surface of the surface layer is covered with a metal layer 204. In FIG. The proportion of the surface area of ​​the surface layer covered by the metal layer relative to the total surface area (100%) of the surface layer is preferably 50% or more and 100% or less, more preferably 70% or more and 100% or less, even more preferably 90% or more and 100% or less, particularly preferably 95% or more and 100% or less, and most preferably 100%.

[0083] The metal layer may be one layer or two or more layers. In the second metal powder 20C illustrated in FIG. 3, the metal layer is one layer.

[0084] The composition of the metal forming the metal layer 204 is different from the metal forming the surface layer. The metal forming the metal layer may be one kind of elemental metal, or may be an alloy formed of two or more kinds of metal elements.

[0085] Examples of metals that may be included in the metal layer include Ag, Cu, In, Bi, Ni, Ge, P, Co, Ga, Zn, Sb, Pb, Au, Al, Pt, Pd, Fe, Mn, Zr, Sn, and As. These metals may be included in one type or in two or more types. The metal group that may be included in the core part can be arbitrarily selected from these metals.

[0086] The metal layer may contain unavoidable impurities in addition to the above-mentioned metals. Even if the metal layer contains unavoidable impurities, the effect of the present invention is not affected. The metal layer may be formed of one type of metal, or two or more types of metals.

[0087] When the metal forming the metal layer contains Fe, the content of Fe in the metal forming the metal layer is preferably 0 mass % or more and less than 5 mass % with respect to the total mass of the metal forming the metal layer.

[0088] The thickness Rm of the metal layer may be, for example, 0.01 μm or more and 100 μm or less, 1 μm or more and 50 μm or less, or 2 μm or more and 10 μm or less.

[0089] The metal layer may be a plating formed by a plating process. Examples of the plating method include known electroplating and electroless plating.

[0090] Since the second metal powder 20C has the metal layer 204, and the metal layer contains Sn, wettability is improved when the solder paste melts, and voids can be reduced. The metal layer melts after heating is started to melt the solder paste, and the surface layer of the third metal is exposed, so the effect of the present application is not hindered.

[0091] (Fourth embodiment) The solder paste according to the fourth embodiment further contains a metal powder other than the first metal powder and the second metal powder (hereinafter, this may be referred to as a "third metal powder"). The solder paste according to the fourth embodiment is similar to the first, second or fourth embodiment except that it further contains a third metal powder.

[0092] There are no particular limitations on the composition of the third metal powder as long as it is different from the first metal powder and the second metal powder. For example, powders made of any of the elemental metals Ni, Ag, Cu, In, Bi, Ge, P, Co, Ga, Zn, Sb, Pb, Au, Al, Pt, Pd, Fe, Mn, Zr, Sn, and As, or alloys formed of two or more of these elemental metals, are preferred.

[0093] The third metal powder may have, for example, a core portion and a surface layer that covers the core portion and is made of a metal containing Ni. The core portion is not particularly limited in composition as long as it is different from the core portion of the first and second embodiments, and is preferably, for example, a powder of one of the elemental metals Ni, Ag, Cu, In, Bi, Ge, P, Co, Ga, Zn, Sb, Pb, Au, Al, Pt, Pd, Fe, Mn, Zr, Sn, and As, or an alloy formed of two or more of these elemental metals.

[0094] The third metal powder preferably has a particle size of 0.1 to 1000 μm, more preferably 1 to 100 μm, and even more preferably 5 to 50 μm. The third metal powder may contain one type of metal or two or more types of metals. The third metal powder may be of one type or of two or more types.

[0095] By including the third metal powder, it is possible to increase the thermal conductivity of the solder paste.

[0096] (solder joint) A solder joint according to the present invention is formed using the solder paste according to the above embodiment. There is no particular limitation on the objects to be joined by the solder joints, but for example, a semiconductor element and a substrate can be joined by the solder joints. Examples of semiconductor elements include silicon carbide (SiC) chips and Si chips. Examples of the substrate include a circuit board, a ceramic substrate, a metal substrate, a DCB (Direct Copper Bonding) substrate, etc. The electrode on the substrate may be, for example, a Cu electrode, or a Cu electrode plated with Sn, Ni, Ni-Au, Ni-Pd, or Ni-Pd-Au.

[0097] The solder paste according to the embodiment may be used to bond objects to each other by a reflow method, for example. The conditions for the reflow method may be appropriately set by referring to known methods. The pressure inside the reflow furnace may be reduced during the reflow process, which facilitates the discharge of gasified flux from the solder paste and makes it easier to prevent voids from occurring. The temperature when bonding the semiconductor element and the substrate is, for example, preferably 120° C. or more and 400° C. or less, and may be 200° C. or more and 400° C. or less, or may be 250° C. or more and 400° C. or less. The atmosphere in which the objects are joined may be an air atmosphere, an inert atmosphere such as a nitrogen atmosphere, or a reducing atmosphere.

[0098] As described above, the solder joint of the present invention has excellent heat resistance and shear strength because it uses the solder paste of the above embodiment, which contains a first metal powder, a second metal powder, and a flux. The solder joint according to the present invention is particularly useful in applications requiring high-temperature solder that does not melt during operation under high-temperature conditions, such as in power semiconductor devices. EXAMPLES

[0099] The present invention will be described below with reference to examples, but the present invention is not limited to the following examples.

[0100] <Preparation of paste> (Examples 1 to 7, Comparative Examples 1 to 2) Metal powders having the compositions shown in Table 1 were mixed with flux to prepare pastes for the examples and comparative examples. In each of the pastes of Examples 1 to 5 and 7, the flux was 12 mass %, and the total mass of the first metal powder and the second metal powder was 88 mass %. The paste of Example 6 contains 12 mass % of flux, and the total mass of the first metal powder, the second metal powder, and metal powder C is 88 mass %. The paste of Comparative Example 1 contained 12 mass % of flux and 88 mass % of the total mass of the first metal powder and metal powder B. The paste of Comparative Example 2 contained 12 mass % of flux and the total mass of the first metal powder and metal powder A was 88 mass %. The numerical values ​​in the table indicate the content of each metal powder relative to the total mass (100 mass%) of the metal powder in the paste. A blank in the table indicates "0."

[0101] The particle size of the metal powder and the particle size Rc of the core portion were measured by measuring the average particle size on a volume basis using a laser diffraction / scattering type particle size distribution measuring device (MT3300EXII) manufactured by Microtrack Bell. The melting points of the metal powders were determined by differential scanning calorimetry (DSC). The melting points of the first metal powder were measured using a DSC7020 manufactured by Hitachi High-Tech Science Corporation, and the melting points of the second metal powder and metal powders A to C were measured using a DSC404-F3Pegasus manufactured by NETZSCH. The thicknesses Rs of the surface layers of the second metal powders (1) to (5), metal powder A and metal powder C were measured using an Auger electron spectrometer based on Auger electron spectroscopy.

[0102] First metal powder: Metal powder containing 100% Sn by mass (100% Sn powder) The first metal powder had a size (particle size distribution) that satisfied symbol 4 in the powder size classification in Table 2 of JIS Z 3284-1:2004. That is, the content of particles having a particle diameter of 38 μm or less in the first metal powder was 99 mass % or more based on the total mass of the first metal powder. The average particle diameter of the first metal powder was 34.54 μm. The melting point of the first metal powder was 232°C.

[0103] Second metal powder (1)~(5): In the second metal powders (1) to (5), the core portion was a metal powder made of an alloy of 90 mass % Ni and 10 mass % Fe (Ni-10 mass % Fe powder). The Ni-10% by mass Fe powder, which was the core part, had a size (particle size distribution) that satisfied symbol 5 in the powder size classification in Table 2 of JIS Z 3284-1:2004. That is, the content of particles with a particle diameter of 25 μm or less in the Ni-10% by mass Fe powder was 99% by mass or more with respect to the total mass of the Ni-10% by mass Fe powder. The particle diameter (i.e., core diameter Rc) of the Ni-10% by mass Fe powder, which was the core part, was 22.59 μm. The melting point of the core was 1444°C.

[0104] In the second metal powders (1) to (5), metal powder A, and metal powder C, the metal forming the surface layer covering the entire surface of the core portion was a metal containing 100 mass % Ni. This surface layer was formed by coating the entire core portion with Ni plating. All of these Ni platings were formed by electroplating. The surface layer thicknesses Rs (i.e., the thickness of the Ni plating) were (1) 0.05 μm, (2) 0.10 μm, (3) 0.35 μm, (4) 0.50 μm, and (5) 0.75 μm, respectively. The melting point of the Ni that forms the surface layer was 1455°C.

[0105] Metal powder A~C: Metal powder A had a core and a surface layer made of Ni that covered the core. Metal powder A was the same as second metal powder (1) except that the surface layer had a thickness Rs of 1.20 μm. The particle size of the core portion of Metal Powder A (ie, core diameter Rc) was 22.59 μm. The melting point of the core was 1444°C, and the melting point of the Ni that formed the surface layer was 1455°C.

[0106] The same metal powder (Ni-10 mass % Fe powder) used as the core portion of the second metal powders (1) to (5) was used as the metal powder B. The third metal powder was a metal powder having no surface layer. Metal powder B had a particle size of 22.59 μm. The melting point of metal powder B was 1444°C.

[0107] Metal powder C had a core and a surface layer made of Ni that covered the core. The thickness of the surface layer of the metal powder was 1 to 3 μm. The core portion was made of metal powder made of Cu (Cu powder containing 100% by mass). The particle size of the core portion of Metal Powder C (ie, core diameter Rc) was 55.3 μm. The melting point of the core was 1085°C. The melting point of the Ni that formed the surface layer was 1455°C.

[0108] As the flux, SDC5 (manufactured by Senju Metal Industry Co., Ltd.) was used.

[0109] According to the evaluation methods described in the following <Evaluation>, <Evaluation of void suppression ability>, <Evaluation of compound formation>, and <Evaluation of heat resistance> were performed. The evaluation results are shown in Table 1 and Figure 8.

[0110] <Evaluation> <Evaluation of void suppression ability> (1) Evaluation method Using a mask (opening: size 3mm x 3mm, thickness 0.15mm) and a squeegee, the paste of each example was printed on a Cu substrate (size 50mm x 50mm, thickness 0.3mm), and after mounting a Si chip (size 3mm x 3mm), reflow was performed. The reflow profile was a temperature rise rate of 3°C / sec from 30°C to the peak temperature (250°C). The nitrogen atmosphere was set to a peak time of 2.5 minutes, and the pressure was reduced for the first 2 minutes of the peak. After that, the voids were observed using an X-ray observation device.

[0111] (2) Judgment criteria A small amount of voids occurred, similar to when the paste of Comparative Example 2 was used. B: The amount of voids generated was greater than when the paste of Comparative Example 2 was used, but less than when the paste of Comparative Example 1 was used. C A large number of voids were generated, similar to the case where the paste of Comparative Example 1 was used.

[0112] X-ray observation images of Examples 1 to 3, 5, and 6 and Comparative Examples 1 and 2 are shown in Fig. 4. It was confirmed that voids were suppressed in Examples 1 to 3, 5, and 6 and Comparative Example 2 compared to Comparative Example 1. Although photographed images are not shown, it was confirmed that voids were suppressed in Example 4 to the same extent as in Examples 3 and 5. Although photographed images are not shown, it was confirmed that voids were suppressed in Example 7 compared to Comparative Example 1.

[0113] [Table 1]

[0114] <Heat resistance evaluation> (1) Evaluation method The Sn contained in the solder paste and an alloy containing Ni and Fe form a compound with a high melting point, which enhances the heat resistance of the solder joint. The reaction that forms this compound is an exothermic reaction. Therefore, the heat resistance was evaluated by measuring the amount of heat generated during the compound formation.

[0115] First, mixed powders were prepared from the metal powders contained in each of the solder pastes of Examples 1 to 3 and 5 and Comparative Examples 1 and 2. Hereinafter, these mixed powders are referred to as the mixed powders of Examples 1 to 3, 5 and Comparative Examples 1 and 2, respectively. In each mixed powder, the mixing ratio (mass ratio) of each metal powder was set to be the same as the mixing ratio (mass ratio) in the solder paste.

[0116] Each mixed powder was placed in an aluminum pan, and the exothermic peak was measured by DSC. The measurement device used was EXSTAR DSC7020 (manufactured by Hitachi High-Tech Science Corporation). The measurement program was set to 100 to 350°C, with a heating rate of 5°C / min.

[0117] The measurement results (DSC curves) of the exothermic peak (heat flow) per unit mass (mg) for each of the mixed powders of Examples 1 to 3 and 5 and Comparative Examples 1 and 2 are shown in Fig. 5. In Fig. 5, the large peak near 230°C indicates the endothermic peak when Sn melts.

[0118] Next, based on the DSC curves, the heat flow per unit mass (mg) was integrated over time to calculate the integral value (unit: [J]) per unit mass (mg) for each mixed powder of Examples 1 to 3 and 5 and Comparative Examples 1 to 2. In the mixed powder of Comparative Example 1, the temperature T at which the heat generation amount becomes the minimum in the range of 200°C to 350°C is defined as T in0 In each mixed powder of Examples 1 to 3 and 5 and Comparative Example 2, the temperature T at which the integral value becomes the minimum in the range of 200° C. to 350° C. is defined as T in It was decided. temperature T in The calorific value per unit mass (mg) of each mixed powder in Examples 1 to 3, 5, and Comparative Example 2 in the range from 0 to 350 ° C., and T in0 The calorific value per unit mass (mg) of the mixed powder of Comparative Example 1 in the range from 0 to 350° C. is shown in FIG.

[0119] Then, the temperature T in The ratio of the calorific value of each mixed powder of Examples 1 to 3, 5, and Comparative Example 2 in the range of from 0 to 300 ° C. was in0 The calorific value was calculated as a percentage of the calorific value (100%) of the mixed powder of Comparative Example 1 in the range from 0 to 300°C. The calculation results of the calorific value percentage are shown in Figure 7. A higher calorific value percentage means that compound formation progresses more during soldering, and heat resistance is improved.

[0120] From the above, it was confirmed that in the examples, the thicker the Ni plating, the slower the onset of the exothermic reaction and the more the reaction to form compounds is suppressed.

[0121] (2) Judgment criteria The proportion of the calorific value of the mixed powder A to the calorific value of the mixed powder of Comparative Example 1 was 60% or more. The ratio of the calorific value of the mixed powder B to the calorific value of the mixed powder of Comparative Example 1 was 20% or more and less than 60%. C The ratio of the calorific value of the mixed powder to the calorific value of the mixed powder of Comparative Example 1 was less than 20%.

[0122] It was confirmed that Examples 1 to 7 and Comparative Example 1 had higher heat resistance than Comparative Example 2.

[0123] <Evaluation of compound formation> As in the evaluation of void suppression ability, the paste of each example was printed on a substrate and reflowed without mounting a Si chip. The solder after reflow was photographed.

[0124] The photographed images of Examples 1 to 3, 5, and 6 and Comparative Examples 1 and 2 are shown in FIG. The white areas in the photographed image have a weak metallic luster and represent an alloy of Ni and Fe and a compound of Sn. The black areas in the photographed images have a strong metallic luster and represent unreacted Sn that has not yet been converted into a compound.

[0125] It was confirmed that more compounds were formed in Examples 1 to 3, 5, and 6 and Comparative Example 1 compared to Comparative Example 2. Although no photographic images are shown, in Example 4, compounds were formed to the same extent as in Examples 3 and 5. Although no photographic images are shown, in Example 7, more compounds were formed compared to Comparative Example 2. It is presumed that in Comparative Example 2, the Ni plating was too thick, so that the core portion was not completely exposed during bonding, and a sufficient amount of compounds was not formed between the core portion and the first metal to exhibit heat resistance. From these results, it was confirmed that Examples 1 to 7 and Comparative Example 1 had higher heat resistance than Comparative Example 2. [Explanation of symbols]

[0126] 20A, 20B, 20C 2nd metal powder 201 Core 202 Surface layer 203 Middle Class 204 Metal layer Rc Core diameter Rs Surface layer thickness Ri Interlayer thickness Rm Metal layer thickness

Claims

1. A solder paste containing a first metal powder, a second metal powder, and a flux, The first metal powder contains Sn, The second metal powder has a core portion made of an alloy containing Ni and Fe, and a surface layer covering the core portion and made of a metal containing Ni, The content of Sn in the first metal powder is 20 mass% or more and 100 mass% or less with respect to the total mass of the first metal powder, The content of Ni in the metal forming the core portion of the second metal powder is 80 mass% or more and 99 mass% or less with respect to the total mass of the metal forming the core portion of the second metal powder, The content of Fe in the metal forming the core portion of the second metal powder is 1 mass% or more and 20 mass% or less with respect to the total mass of the metal forming the core portion of the second metal powder, A content of Ni in the metal forming the surface layer of the second metal powder is 50 mass% or more with respect to a total mass of the metal forming the surface layer of the second metal powder, The particle size of the first metal powder is 0.1 to 1000 μm; The particle size of the second metal powder is 0.2 to 1000 μm; The thickness of the surface layer of the second metal powder is 0.05 μm or more and 0.30 μm or less. Solder paste.

2. The content of the first metal powder is 30 to 99 mass% with respect to the total mass of the first metal powder and the second metal powder, The content of the second metal powder is 1 to 70 mass% with respect to the total mass of the first metal powder and the second metal powder. The solder paste of claim 1.

3. A solder joint formed by using the solder paste according to claim 1 or 2.

Citation Information

Patent Citations

  • Iron-nickel alloy coating with good weldability and uses thereof

    CN101041901A

  • Electronic circuit module part and method for manufacturing the same

    JP2012076097A

  • Pb-FREE SOLDER

    JP2012091223A

  • Electronic circuit module component

    JP2016083695A