Branched Metal-Organic Framework Nanoparticles and Related Methods
Branched MOF nanoparticles address the inefficiencies of traditional gas separation membranes by improving selectivity and permeability through controlled synthesis and uniform integration into polymer matrices, resulting in enhanced gas separation performance.
Patent Information
- Application Number
- JP2020568537
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-06-11
- Filing Date
- 2019-06-11
- Publication Date
- 2024-12-04
- Estimated Expiration
- 2039-06-11
AI Technical Summary
Existing gas separation membranes, particularly those based on polymeric materials, face challenges such as a trade-off between permeability and selectivity, plasticization issues, and poor compatibility between inorganic fillers and polymer matrices, leading to inefficient and non-selective separation processes.
The development of branched metal-organic framework (MOF) nanoparticles with controlled morphology and size, formed through the use of chemical modulators during synthesis, which are incorporated into mixed matrix membranes to enhance dispersion and compatibility with polymers, forming a uniform and interconnected network.
The branched MOF nanoparticles improve gas separation performance by maintaining high selectivity and permeability, reducing plasticization, and ensuring uniform distribution within the polymer matrix, thereby enhancing the efficiency of gas separation processes.
Smart Images

Figure 0007594280000015 
Figure 0007594280000016 
Figure 0007594280000017
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit under 35 U.S.C. § 119(e) of U.S. Provisional Patent Application No. 62 / 683,516, filed June 11, 2018, and entitled "Branched Metal-Organic Framework Nanoparticles in Mixed Matrix Membranes and Related Methods," which is incorporated by reference in its entirety for all purposes.
[0002] Technical Field The synthesis of nanoparticles comprising metal-organic frameworks is generally described. [Background technology]
[0003] background The chemical and petrochemical industries consume approximately 30% of the world's energy and emit 16% direct CO2. Approximately half of the energy consumption comes from separation processes, most notably thermal separations such as distillation. In the area of CO2 separation required for carbon capture applications and natural gas purification, amine absorption is the go-to technology. Although the process is efficient, it requires high-energy thermal regeneration cycles and the use of toxic amines. With improved material design, membranes can significantly reduce the energy consumption and costs associated with absorption processes and distillation, thereby providing an energy-efficient modular alternative to traditional unit operations.
[0004] To date, all commercially available gas separation membranes are formed using polymeric materials, and these gas separation membranes are difficult to fabricate due to the large areas (1,000–500,000 m) required for large-scale separations. 2) and can be formed into thin selective layers (approximately 100 nm). In contrast to these attractive processing advantages, polymeric membranes have several drawbacks. In terms of efficiency and productivity, traditional polymeric materials are often limited by the trade-off between permeability and selectivity. Furthermore, polymeric membranes are often vulnerable to a deleterious process known as plasticization, which is described as the swelling of linear polymers with intertwined chains in the presence of highly adsorptive molecular diluents that disrupt the chain packing. Plasticization often increases gas permeability but significantly reduces selectivity. Carbon dioxide is one of the most difficult substances to manipulate and exhibits this behavior. These drawbacks require novel membrane materials to improve transport properties and reduce plasticization in practical separation processes.
[0005] There has been much interest in mixed matrix membranes, where inorganic fillers are dispersed in polymers, to form composite membranes with relatively high mechanical integrity and better separation performance, while still using practical and process-friendly polymer-based systems. Inorganic materials such as various metal oxides, zeolites, and carbons have been incorporated into polymers to provide a molecular sieve effect, which defines the dimensions and size of the pores of the structure specifically for each structure. However, these inorganic materials lack the functionality of organic frameworks, and therefore the dispersed phase is not very compatible with the polymer. This compatibility problem leads to particle aggregation in the nascent composite membranes and no selectivity of the dispersion pathway. Metal-organic frameworks (MOFs) are an attractive platform of crystalline materials with metal ions or metal clusters bridged by organic ligands, which provide a variety of inorganic topologies, exceptionally high porosity and internal surface areas, tunable pore sizes, and chemical properties based on the selection of MOF building blocks. MOFs also have relatively flexible structures with tunable pore systems and better compatibility with polymer matrices, due to the organic composition of part of the structure. These features make MOFs easier to incorporate into polymers and may be preferable to other inorganic materials needed for efficient gas separation.
[0006] HKUST-1 (also called Cu(BTC)) is one of the MOFs being investigated for mixed matrix membrane applications. 2+ It is composed of paddlewheel units and benzene-1,3,5-tricarboxylic acid (trimesic acid) and displays a twisted cubic boron trilayer topology with two types of pores. These two types of pores have a main pore channel with a diameter of 9 Å, which is surrounded by a tetrahedral pocket with a diameter of 5 Å. One particularly interesting aspect is that HKUST-1 has coordinatively unsaturated (open) metal sites that are weakly bound to solvent molecules by coordination during synthesis, but can be exposed by solvent exchange and / or heating (so-called activation) processes. Once the weakly bound solvent molecules are removed, the exposed coordination vacancies of the copper metal sites are Lewis acidic and can strongly interact with Lewis basic polar gas molecules, thereby enhancing gas adsorption. For HKUST-1, the activation energy barrier for nucleation is approximately 71.6 kJ mol -1 and the activation energy barrier for growth is approximately 63.8 kJ mol -1 Thus, nucleation is typically much slower than growth, which results in the formation of micron-sized particles with a broader size distribution compared to other MOFs that energetically favor nucleation over growth, and therefore allows for the easier formation of uniformly structured nanoparticles. When typical micron-sized HKUST-1 particles are incorporated into a polymer matrix, they can undergo phase separation, which can lead to the MOF agglomeration into a "sleeve-in-cage" morphology, thereby creating nonselective interfacial voids between the bulk filler and the polymer, reducing gas selectivity. Thus, despite HKUST-1 itself having favorable properties for gas separation, it can be difficult to form defect-free HKUST-1 mixed matrix membranes. Summary of the Invention [Means for solving the problem]
[0007] Abstract Compositions comprising metal-organic frameworks and methods relating to the compositions are generally described. In some embodiments, branched nanoparticles made at least in part of the metal-organic frameworks are described. In some embodiments, the morphology and size of the branched nanoparticles are controlled by the presence of chemical regulators during synthesis. The subject matter of the present invention includes, in some cases, interrelated products, alternative solutions to a particular problem, and / or a plurality of different uses of one or more systems and / or articles.
[0008] In one aspect, a composition is described.In some embodiments, the composition comprises branched nanoparticles comprising a metal-organic framework, said metal-organic framework comprising a metal ion and a multidentate ligand.In some embodiments, the branched nanoparticles have a hydrodynamic diameter of 2 μm or less, an aspect ratio of at least 5, and a branch diameter of 200 nm or less.
[0009] In another aspect, a method is described. In some embodiments, the method includes combining a metal salt comprising a metal ion, a multidentate ligand, and a chemical modulator in a liquid to form branched nanoparticles, the branched nanoparticles comprising a metal-organic framework, the metal-organic framework comprising a metal ion and a multidentate ligand. In some embodiments, the metal salt, the multidentate ligand, and / or the chemical modulator are selected such that the presence of at least 0.1 equivalents of the chemical modulator relative to the concentration of the multidentate ligand increases the aspect ratio of the branched nanoparticles by at least 3-fold relative to particles formed under the same conditions in the absence of the chemical modulator.
[0010] Other advantages and novel features of the present invention will become apparent from the following detailed description of various non-limiting embodiments of the invention when considered in conjunction with the accompanying drawings. In the event that the present specification and any document incorporated by reference include conflicting and / or inconsistent disclosure, the present specification shall control. In an embodiment of the present invention, for example, the following items are provided: (Item 1) 1. A composition comprising: A branched nanoparticle comprising a metal-organic framework, the metal-organic framework comprising a metal ion and a multidentate ligand. Including, wherein the branched nanoparticles have a hydrodynamic diameter of 2 μm or less, an aspect ratio of at least 5, and branches with diameters of 200 nm or less. (Item 2) 2. The composition of claim 1, wherein the polydentate ligand comprises at least two carboxylate groups. (Item 3) 3. The composition according to any one of items 1 to 2, wherein the metal ion is a transition metal ion. (Item 4) 4. The composition according to any one of items 1 to 3, wherein the metal ion is copper. (Item 5) 5. The composition according to any one of items 1 to 4, wherein the metal-organic framework is HKUST-1. (Item 6) The composition according to any one of items 1 and 3-4, wherein the polydentate ligand comprises an imidazolate. (Item 7) 7. The composition according to any one of items 1 to 3 and 6, wherein the metal ion is zinc. (Item 8) 8. The composition according to any one of items 1 to 4 and 6 to 7, wherein the metal-organic framework is a zeolite-like imidazolate framework. (Item 9) The composition according to any one of items 1 to 4 and 6 to 8, wherein the metal-organic framework is ZIF-8. (Item 10) 10. The composition according to any one of items 1 to 9, wherein the branched nanoparticles are non-aggregated. (Item 11) 11. The composition according to any one of items 1 to 10, wherein the branched nanoparticles form an at least partially permeable network. (Item 12) 12. The composition according to any one of the preceding claims, wherein the branched nanoparticles comprise an amine associated with the metal-organic framework. (Item 13) The branched nanoparticles include an amine associated with the metal-organic framework, the amine having the formula NR 3 wherein each R is hydrogen, optionally substituted C 1~8 13. The composition according to any one of items 1 to 12, wherein the alkyl groups are independently selected from branched and unbranched alkyl, optionally substituted cycloalkyl, and optionally substituted aryl. (Item 14) 14. The composition according to any one of the preceding claims, wherein the branched nanoparticles comprise triethylamine associated with the metal organic framework. (Item 15) 1. A method comprising: combining a metal salt comprising a metal ion, a multidentate ligand, and a chemical modulator in a liquid to form branched nanoparticles, the branched nanoparticles comprising a metal-organic framework, the metal-organic framework comprising the metal ion and the multidentate ligand; Including, wherein the metal salt, multidentate ligand, and / or chemical modulator are selected such that when present in an amount of at least 0.1 equivalents relative to the concentration of the multidentate ligand, the aspect ratio of the branched nanoparticles increases by at least 3-fold relative to particles formed under the same conditions in the absence of the chemical modulator. (Item 16) 16. The method of claim 15, wherein the branched nanoparticles have a hydrodynamic diameter of 2 μm or less, an aspect ratio of at least 5, and branches with diameters of 200 nm or less. (Item 17) 17. The method according to any one of items 15 to 16, wherein the chemical regulator is a salt comprising a cation and an anion, and the anion has at least one carboxylate group. (Item 18) 18. The method of claim 17, wherein the anion is acetate. (Item 19) 17. The method of any one of items 15 to 16, wherein the chemical regulator comprises an amine. (Item 20) The chemical regulator has the formula NR 3 where each R is hydrogen, optionally substituted C 1~8 20. The method according to any one of items 15-16 and 19, wherein the alkyl groups are independently selected from branched and unbranched alkyl, optionally substituted cycloalkyl, and optionally substituted aryl. (Item 21) 20. The method of any one of items 15 to 16 and 19, wherein the chemical regulator comprises triethylamine. (Item 22) The pK of the chemical regulator in the liquid a is the pK of the multidentate ligand moiety that binds to the metal ion in the metal-organic framework. a 22. The method according to any one of items 15 to 21, wherein the method further comprises: (Item 23) The pK of the chemical regulator in the liquid a 23. The method according to any one of items 15 to 22, wherein the β-amino acid sequence is 3.0 or more. (Item 24) 24. The method according to any one of items 15 to 23, wherein the pKa of the chemical regulator in a liquid is 15.0 or less. (Item 25) 25. The method of any one of claims 15 to 24, wherein the chemical modulator is associated with the branched MOF nanoparticles after formation of the branched nanoparticles. (Item 26) 26. The method of any one of items 15 to 25, wherein the branched nanoparticles comprise an amine associated with the metal-organic framework. (Item 27) The branched nanoparticles include an amine associated with the metal-organic framework, the amine having the formula NR 3 wherein each R is hydrogen, optionally substituted C 1~8 27. The method according to any one of items 15 to 26, wherein the alkyl groups are independently selected from branched and unbranched alkyl, optionally substituted cycloalkyl, and optionally substituted aryl. (Item 28) 28. The method of any one of items 15 to 27, wherein the branched nanoparticles comprise triethylamine associated with the metal-organic framework. (Item 29) 29. The method according to any one of items 15 to 28, wherein the liquid is at least 99% by volume methanol. (Item 30) 30. The method of any one of items 15 to 29, wherein the combining step comprises mixing the liquids at a temperature of 15°C or greater and 60°C or less for at least 10 minutes. (Item 31) 31. The method according to any one of items 15 to 30, wherein the polydentate ligand comprises at least two carboxylate groups. (Item 32) 32. The method according to any one of items 15 to 31, wherein the metal ion is a transition metal ion. (Item 33) 33. The method according to any one of items 15 to 32, wherein the metal ion is copper. (Item 34) 34. The method according to any one of items 15 to 33, wherein the metal-organic framework is HKUST-1. (Item 35) 34. The method according to any one of items 15 to 30 and 32 to 33, wherein the polydentate ligand comprises an imidazolate. (Item 36) 36. The method according to any one of items 15 to 32 and 35, wherein the metal ion is zinc. (Item 37) 37. The method according to any one of items 15 to 30, 32 to 33, and 35 to 36, wherein the metal-organic framework is a zeolite-like imidazolate framework. (Item 38) The method according to any one of items 15 to 30, 32 to 33, and 35 to 37, wherein the metal-organic framework is ZIF-8. [Brief description of the drawings]
[0011] Non-limiting embodiments of the present invention are described by way of example with reference to the accompanying drawings, which are schematic and are not intended to be drawn to scale. In the drawings, each identical or nearly identical component shown is typically designated by a single numeral. For clarity, not all components in every drawing are labeled, nor are all components of each embodiment of the present invention shown labeled, unless such labeling is necessary for a person skilled in the art to understand the invention. The description of the figures is given below.
[0012] [Figure 1A-1B] 1A-1B show transmission electron microscopy (TEM) images of (FIG. 1A) branched HKUST-1 particles and (FIG. 1B) bulk HKUST-1 particles according to certain embodiments.
[0013] [Figure 2A] FIG. 2A shows a schematic diagram of an exemplary branched nanoparticle according to certain embodiments.
[0014] [Figure 2B] FIG. 2B shows a schematic diagram of an exemplary branched nanoparticle, according to certain embodiments.
[0015] [Figure 3A]FIG. 3A shows X-ray diffraction (XRD) patterns of branched and bulk HKUST-1 particles according to certain embodiments.
[0016] [Figure 3B] FIG. 3B shows a number-average dynamic light scattering (DLS) plot of bulk and branched HKUST-1 particles according to certain embodiments.
[0017] [Figure 4A-4B] 4A-4B show cross-sectional SEMs of mixed matrix membranes containing bulk and branched nanoparticle HKUST-1 particles according to certain embodiments.
[0018] [Figure 5A-5E] 5A-5E show FIB-SEM images of 30 wt % branched HKUST-1 / 6FDA-DAM MMM at different magnifications according to certain embodiments (FIGS. 5A-5C) and reconstructed 3D images from FIB-SEM tomograms (FIGS. 5D-5E).
[0019] [Figures 6A-6D] 6A-6D show low magnification TEM images of a series of HKUST-1 particles formed with different sodium acetate concentrations according to certain embodiments.
[0020] [Figure 7A-7C] 7A-7C include FIB-SEM images of bulk HKUST-1 / 6FDA-DAM mixed matrix membranes according to certain embodiments.
[0021] [Figure 8A-8C] 8A-8C include FIB-SEM images of branched HKUST-1 / 6FDA-DAM MMMs using various HKUST-1 according to certain embodiments.
[0022] [Figure 9A-9B]9A-9B are charts showing FT-IR spectra of pure 6FDA-DAM polymer films and bulk HKUST-1 / 6FDA-DAM mixed matrix membranes with various HKUST-1 weight loadings, according to certain embodiments.
[0023] [Figure 10A-10B] 10A-10B are charts showing FT-IR spectra of pure 6FDA-DAM polymer films and branched HKUST-1 / 6FDA-DAM MMMs with various HKUST-1 weight loadings, according to certain embodiments.
[0024] [Figures 11A-11D] 11A-11D are charts illustrating certain gas permeabilities as a function of supply pressure according to certain embodiments.
[0025] [Figure 12A-12D] 12A-12D are charts illustrating certain gas permeabilities as a function of gas supply pressure according to certain embodiments.
[0026] [Figure 13A-13B] 13A-13B are charts showing the gas separation performance of various membranes according to certain embodiments.
[0027] [Figure 14A-14B] 14A-14B are charts showing the gas separation performance of two sets of pure 6FDA-DAM polymer thin films and bulk and branched HKUST-1 / 6FDA-DAM MMMs with various HKUST-1 weight loadings according to certain embodiments.
[0028] [Figure 15A-15D] 15A-15D include charts showing normalized CO 2 permeability as a function of CO 2 gas supply pressure for various membranes according to certain embodiments.
[0029] [Figure 16A-16B] 16A-16B include FIB-SEM images of a rhomboidal dodecahedral ZIF-8 / 6FDA-DAM mixed matrix membrane (FIG. 16A) and a branched ZIF-8 / 6FDA-DAM mixed matrix membrane according to certain embodiments.
[0030] [Figures 17A-17D] 17A-17D are charts showing the gas separation performance of mixed matrix membranes containing rhombic dodecahedral ZIF-8 nanoparticles (RDZ) and branched ZIF-8 nanoparticles (BZ) according to certain embodiments.
[0031] [Figure 18A-18B] 18A-18B are TEM images of ZIF-8 particles formed in the presence of pyridine (FIG. 18A) and triethylamine (FIG. 18B) according to certain embodiments. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0032] Detailed Description Compositions, devices, and methods related to particle synthesis, and inclusion of said particles in mixed matrix membranes for use in gas separation applications are generally described. In some embodiments, a synthesis scheme is provided for forming particles comprising metal-organic frameworks (MOFs). In some embodiments, the particles are branched nanoparticles. Branched nanoparticles, according to certain embodiments, have a relatively high aspect ratio and a relatively small hydrodynamic radius. In some embodiments, the branched nanoparticles have an interconnected structure. In some embodiments, the branched nanoparticles have a multi-dimensional structure. For example, branched nanoparticles, according to certain embodiments, have relatively narrow branches connected in an end-to-end manner, and the branches are not collinear. The branching dimensions and morphology of the branched nanoparticles may contribute to some of the favorable properties, such as limiting aggregation or agglomeration of suspensions in solution or forming multiple contact points in a multi-dimensional structure. The branched nanoparticles may comprise carboxylate-based MOFs. For example, the branched nanoparticles may comprise MOF HKUST-1, according to certain embodiments. In some embodiments, the branched nanoparticles comprise imidazolate-based MOFs. For example, in some embodiments, the branched MOF nanoparticle comprises MOF ZIF-8.
[0033] In some embodiments, branched nanoparticles can be formed by combining metal salts, polydentate ligands, and chemical regulators in liquid.For example, according to certain embodiments, a metal salt containing a metal ion (e.g., copper), a polydentate ligand containing at least two carboxylate groups (e.g., trimesic acid), and a chemical regulator containing a carboxylate group (e.g., sodium acetate) are combined in liquid (e.g., 100% methanol) at room temperature and 1 atm to form branched nanoparticles containing MOFs (e.g., HKUST-1).As another example, in some embodiments, a metal salt containing a metal ion (e.g., zinc), a polydentate ligand containing imidazolate (e.g., 2-methyl-imidazolate), and a chemical regulator containing amine (e.g., triethylamine) are combined in liquid (e.g., methanol) at room temperature and 1 atm to form branched nanoparticles containing MOFs (e.g., ZIF-8). The presence of chemical modulators and the conditions under which metal salts and polydentate ligands are combined can, in part, result in particles with high aspect ratios, branched morphology, and / or relatively small hydrodynamic radii. For example, in some embodiments, particles formed under the same conditions as branched particles, but in the absence of chemical modulators or in a different liquid, may lack the properties of branched nanoparticles. In other words, for example, the presence of a certain amount of chemical modulator (e.g., 0.1 equivalents relative to the concentration of polydentate ligands) may increase the aspect ratio of the resulting particles by about 3 times compared to particles formed under the same conditions. In some embodiments, metal salts, polydentate ligands, and / or chemical modulators are selected to result in particles with high aspect ratios, branched morphology, and / or relatively small hydrodynamic radii.
[0034] The particles may be incorporated into a mixed matrix membrane in another aspect. The mixed matrix membrane may, in some embodiments, include a matrix that includes a polymer. Throughout this disclosure, the term "polymer matrix" refers to a matrix that includes a polymer, where it should be understood that the matrix is limited to the polymer or that the matrix includes polymers and other materials. The mixed matrix membrane may be used to separate gases in some cases. In some embodiments, the particles that include MOFs are distributed uniformly throughout the polymer matrix rather than forming voids or undergoing phase separation, as is typically observed in mixed matrix membranes that include MOFs. In some embodiments, the uniform distribution of particles in the polymer matrix of the mixed matrix membrane is limited to the extent that convective transport of gases through the mixed matrix membrane is observed. In some embodiments, the mixed matrix membrane includes branched nanoparticles that include MOFs (e.g., HKUST-1). In some embodiments, the mixed matrix membrane includes branched nanoparticles that include MOFs, where the MOFs are zeolite-like imidazolate structures (e.g., ZIFs such as ZIF-8). Branched nanoparticles may form at least partially percolated networks in mixed matrix membranes according to certain embodiments. Such percolated networks may improve gas permeation. Such percolated networks may also improve selectivity, especially under mixed gas conditions where competitive adsorption may affect selectivity. For example, a mixed membrane network comprising a percolated network made from branched nanoparticles of HKUST-1 may have improved selectivity relative to a mixed membrane network comprising HKUST-1 particles that do not form a percolated network. As another example, a mixed matrix membrane network comprising a percolated network made from branched nanoparticles of ZIF-8 may have improved selectivity relative to a mixed membrane network comprising ZIF-8 particles that do not form a percolated network. In some embodiments, the branched nanoparticles may form multiple contact points with the polymer within the polymer matrix.These multiple contact points can improve the durability and structural integrity of the mixed matrix membrane and limit the extent to which the mixed matrix membrane undergoes plasticization upon adsorption of a particular gas. For example, in some embodiments, the plasticization pressure point for a gas (e.g., CO2) of a mixed matrix membrane containing branched nanoparticles is relatively high compared to the plasticization pressure point of a membrane made from the same polymer but lacking branched nanoparticles.
[0035] Certain embodiments relate to compositions. In some embodiments, the compositions include branched nanoparticles. In some embodiments, the branched nanoparticles include metal-organic frameworks (MOFs). For example, FIG. 1A shows a transmission electron microscopy image (TEM) of a branched nanoparticle including a MOF according to certain embodiments.
[0036] In some embodiments, the MOF comprises a metal ion. The metal ion can generally be any metal ion that can bind to a ligand. For example, the metal ion can be zinc, aluminum, or magnesium, according to certain embodiments. In some embodiments, the metal ion is zinc. In some embodiments, the metal ion is a transition metal ion. Non-limiting examples of transition metal ions that can be included in the MOF include iron, cobalt, nickel, manganese, zirconium, or chromium, according to certain embodiments. In some embodiments, the metal ion is copper.
[0037] In some embodiments, the MOF comprises a polydentate ligand. A polydentate ligand generally comprises at least two moieties (e.g., metal ions) capable of binding to a Lewis acid. In some embodiments, the polydentate ligand is an organic molecule. The polydentate ligand may be capable of binding to at least two, at least three, or at least four metals. In some embodiments, the polydentate ligand comprises at least two carboxylate groups. Non-limiting examples of some such groups include benzene-1,3,5-tricarboxylate, benzene-1,4-dicarboxylate, naphthalene-2,6-dicarboxylate, 1,3,5-tris(carboxyphenyl)benzene, 2-terephthalate, 2,5-dioxido-1,4-benzenedicarboxylate, and 5,5'-(9,10-anthracenediyl)di-isophthalate. In other embodiments, the polydentate ligand does not comprise multiple carboxylate groups. For example, in some embodiments, the polydentate ligand comprises an imidazolate. For example, the polydentate ligand may be, according to certain embodiments, an imidazolate. In some embodiments, the polydentate ligand is 2-methyl-imidazolate.
[0038] The branched nanoparticles can include various classes of MOFs. In some embodiments, the branched nanoparticles include carboxylate-based MOFs. Carboxylate-based MOFs generally include multidentate ligands that include at least two carboxylate groups. Non-limiting examples of carboxylate MOFs that the branched nanoparticles can include include UiO-66, MIL-53, MIL-96, MIL-100, MIL-101, MIL-125, and MOF-74. In some embodiments, the branched nanoparticles include HKUST-1, a carboxylate-based MOF. The names of the MOFs listed herein are generally known to those skilled in the art of metal-organic frameworks. Other classes of MOFs are also suitable, including zeolitic imidazolate frameworks (ZIFs). The zeolitic imidazolate frameworks can include any of a variety of metal ions. For example, in some embodiments, the zeolitic imidazolate frameworks include iron, cobalt, copper, or zinc ions, or combinations thereof. In some embodiments, the zeolite-like imidazolate structure comprises zinc ions. For example, in some embodiments, the branched MOF nanoparticle comprises ZIF-8. Modified MOFs may include multidentate ligands that are derivatized by the addition of various functional groups (e.g., hydroxyl, alkyl, amino, halo, thio, nitro, etc.), as well as MOFs in which at least a portion of the metal is replaced by a different metal (e.g., zinc is replaced by magnesium) can also be used in the branched nanoparticle.
[0039] As mentioned above, in some embodiments, the composition comprises branched nanoparticles. Nanoparticles generally refer to particles having at least one cross-sectional dimension of 500 nanometers or less as measured through the geometric center of the structure. Generally, a nanoparticle is branched if it comprises at least two branches, each of which has a relatively high aspect ratio (e.g., a relatively high length-to-width ratio) connected end-to-end, and at least two of the branches are not collinear. In some embodiments, the length-to-width ratio of the relatively high aspect ratio branches is 5 or more, 10 or more, and / or up to 15, up to 20, or more. For example, FIG. 2A shows a branched nanoparticle 100 comprising branch 1, branch 2, and branch 3 according to certain embodiments. Branch 1, branch 2, and branch 3 are connected end-to-end and are not all collinear. As another non-limiting example, FIG. 2B shows a branched nanoparticle 200 comprising branch 1, branch 2, branch 3, and branch 4 according to certain embodiments.
[0040] In some embodiments, the branched nanoparticles include branches that are non-planar with respect to one another. For example, returning to FIG. 2A, according to certain embodiments, branch 1, branch 2, and branch 3 are non-planar. In some embodiments, the branched nanoparticles may be considered to be interconnected. In some embodiments, the interconnected branches may result in a denser MOF framework structure than a relatively straight, one-dimensional rod, and may make devices easier to fabricate. One reason for this is that, according to some embodiments, there is little need to align the interconnected branched particles due to the fact that the branches of the interconnected branched particles are relatively randomly oriented, making it less likely that the interconnected branched nanoparticles will arbitrarily rotate and disrupt inter-particle contact with other interconnected branched nanoparticles. According to certain embodiments, such connections may occur when the interconnected branched nanoparticles make end-to-end connections with other interconnected branched nanoparticles, thereby forming a multidimensional MOF structure. Such structures may be formed in a continuous phase, such as a polymer matrix or solution, according to certain embodiments. Furthermore, the branched nanoparticles, in some embodiments, have closely spaced branching points (i.e., the angles between the branches are relatively small). Such closely spaced branching points allow for high density contact of MOF-polymers in the mixed matrix membrane due to the relatively small interstitial space between the branches.
[0041] In some embodiments, the branched nanoparticles have a relatively high aspect ratio. A high aspect ratio can help the branched particles form connected structures with long channels in some embodiments. The aspect ratio can be measured by dividing the hydrodynamic radius of the branched nanoparticle (as measured by dynamic light scattering) by the diameter of the branch in the branched particle with the largest diameter (as measured by TEM). In some embodiments, the branched nanoparticles have an aspect ratio of at least 5. In some embodiments, the branched nanoparticles have an aspect ratio of at least 8, at least 10, or more. In some embodiments, the aspect ratio is 20 or less, 15 or less, or less. Combinations of the above ranges are possible. For example, in some embodiments, the branched nanoparticles have an aspect ratio in the range of 5 to 20.
[0042] In some embodiments, the branched nanoparticles have a relatively small hydrodynamic diameter. Hydrodynamic diameter refers to the diameter of a hypothetical hard sphere that diffuses in the same manner as the particle being measured. As described below, a relatively small hydrodynamic radius allows the branched nanoparticles to avoid aggregation or agglomeration in suspension and to be well dispersed and uniformly distributed in the membrane structure. As described above, the hydrodynamic radius of the particle can be measured using dynamic light scattering (DLS). More specifically, the hydrodynamic radius can be measured by suspending the branched nanoparticles in a methanol (MeOH) solution, sonicating to uniformly disperse the branched nanoparticles, and then performing DLS measurements at 35° C. using a Zetasizer Nano S90 (Marvern). In some embodiments, the branched nanoparticles have a hydrodynamic diameter of 2 μm or less. In some embodiments, the branched nanoparticles have a hydrodynamic diameter of 1 μm or less, 500 nm or less, 400 nm or less, 300 nm or less, 200 nm or less, 150 nm or less, 100 nm or less, or less. In some embodiments, the branched nanoparticles have a hydrodynamic diameter of at least 20 nm, at least 30 nm, or more. Combinations of the above ranges are possible. For example, in some embodiments, the branched nanoparticles have a hydrodynamic diameter of at least 20 nm and less than 2 μm.
[0043] As mentioned above, the diameter of the branches of the branched nanoparticles is relatively small. Such diameter can be measured by TEM. The small diameter of the branches can be partially attributed to the formation of multidimensional structures with good transmission properties. In some embodiments, the diameter of the branches of the branched nanoparticles is 200 nm or less. In some embodiments, the diameter of the branches is 100 nm or less, 50 nm or less, 30 nm or less, 20 nm or less, 15 nm or less, 10 nm or less, or less. In some embodiments, the diameter of the branches is at least 2 nm, at least 5 nm, or more. Combinations of the above ranges are possible. For example, in some embodiments, the diameter of the branches of the branched nanoparticles is at least 2 nm and less than 200 nm. In some embodiments, at least 50% (e.g., at least 60%, at least 75%, at least 90%, or at least 95%) of the branched nanoparticles have a diameter of 200 nm or less. In some embodiments, at least 50% (e.g., at least 60%, at least 75%, at least 90%, or at least 95%) of the branched nanoparticles have a branch diameter of 100 nm or less, 50 nm or less, 30 nm or less, 20 nm or less, 15 nm or less, 10 nm or less, or less. In some embodiments, at least 50% (e.g., at least 60%, at least 75%, at least 90%, or at least 95%) of the branched nanoparticles have a branch diameter of at least 2 nm, at least 5 nm, or more. Combinations of the above ranges are possible. For example, in some embodiments, at least 50% (e.g., at least 60%, at least 75%, at least 90%, or at least 95%) of the branched nanoparticles have a branch diameter of at least 2 nm and less than 200 nm. The percentage of branched nanoparticles having branches with diameters in the above ranges can be determined using TEM.
[0044] Particles comprising MOFs can be formed in some embodiments by combining precursors in a solution. In some embodiments, particles comprising MOFs are formed by combining metal salts, polydentate ligands, and chemical modifiers in a liquid. For example, according to certain embodiments, copper nitrate is combined with benzene-1,3,5-carboxylic acid (trimesic acid) and sodium acetate in methanol to form branched nanoparticles comprising HKUST-1. As another example, in some embodiments, zinc nitrate hexahydrate (Zn(NO3)2·6H2O) hexahydrate (or any of Zn(acac)2, Zn(ClO4)2, ZnSO4, Zn(OAc)2, ZnCl2, ZnBr2, ZnI2, or combinations thereof) is combined with methyl-imidazole and triethylamine in methanol to form branched nanoparticles comprising ZIF-8.
[0045] In some embodiments, the presence of a certain amount of chemical modulator can affect the size and / or morphology of the resulting MOF particles. Chemical modulators generally refer to additives to a reaction mixture that, when present during the chemical reaction forming the particles, cause the particles to differ in size and / or morphology. In some embodiments, chemical modulators can compete with multidentate ligands to bind to metal ions of metal salts, thereby slowing the rate of particle growth. In some embodiments, chemical modulators can promote particle nucleation, thereby increasing the number of individual particles formed during the reaction. In some embodiments, chemical modulators can introduce defects into the crystal structure of the metal-organic framework, thereby affecting the surface energy of the crystal faces and the resulting morphology. In some embodiments, chemical modulators can affect the proton activity in solution (i.e., affecting the acid-base chemistry in the reaction mixture).
[0046] In some embodiments, the chemical regulator is a salt comprising a cation and an anion. In some embodiments, the anion has at least one carboxylate group. For example, in some embodiments, the anion is acetate. For example, in some embodiments, the chemical regulator is sodium acetate. In some but not all embodiments, the chemical regulator is sodium formate or sodium propionate.
[0047] In some embodiments, the chemical regulator comprises an amine. In some embodiments, the chemical regulator is an amine. The amine of the chemical regulator can be any of a variety of suitable amines. For example, in some embodiments, the amine is a primary amine. In some embodiments, the amine is a secondary amine. In some embodiments, the amine is a tertiary amine. The amine can comprise any of a variety of suitable substituents. For example, in some embodiments, the chemical regulator comprises an amine having the formula NR3, where each R is hydrogen, optionally substituted C 1~8 Independently selected from branched and unbranched alkyl, optionally substituted cycloalkyl, and optionally substituted aryl.As an example, in some embodiments, the chemical regulator is or comprises triethylamine.Other non-limiting examples of chemical regulators include trimethylamine, diethylamine, tri-n-butylamine, and n-butylamine.
[0048] As previously mentioned, in some instances, the chemical regulator may affect the acid-base chemistry of the reaction mixture. In some such cases, the chemical regulator may affect the acid-base chemistry of the reaction mixture within a certain range of pK a For example, in some embodiments, the pK of a chemical regulator that undergoes a chemical reaction in the liquid a is the pK of the multidentate ligand moiety that binds to the metal ion in the metal-organic framework. aFor example, in some embodiments where the multidentate ligand contains at least two carboxylate groups (and in the resulting MOF the carboxylate groups bind to the metal ion) and the solution in which synthesis occurs is methanol, the pK a is higher than the carboxylate group of the multidentate ligand in methanol. As another example, in some embodiments where the multidentate ligand includes an imidazolate group and the solution in which synthesis occurs is methanol, the pK a is the pK of the imidazolate ligand in methanol a In some embodiments, the pKa of the chemical regulator is relatively high. For example, in some embodiments, the pKa of the chemical regulator (e.g., acetate, amine, etc.) in methanol is a In some embodiments, the pK in methanol of the chemical modulator is 3.0 or higher, 4.0 or higher, 5.0 or higher, 6.0 or higher, 7.0 or higher, 7.5 or higher, 8.0 or higher, 8.0 or higher, 9.0 or higher. a is 15.0 or less, 12.0 or less, 11.5 or less, 11.0 or less, 10.5 or less, 10.0 or less, or less. Combinations of these ranges are possible. For example, in some embodiments, the pK in methanol of the chemical modulator is 15.0 or less, 12.0 or less, 11.5 or less, 11.0 or less, 10.5 or less, 10.0 or less, or less. a is greater than or equal to 3.0 and less than or equal to 15.0, greater than or equal to 5.0 and less than or equal to 12.0, or greater than or equal to 8.0 and less than or equal to 11.5.
[0049] In some embodiments, the metal salts, polydentate ligands, and / or chemical modulators that are combined in the liquid to form the branched nanoparticles comprising MOFs are selected to provide certain properties to the resulting branched nanoparticles. In some embodiments, the presence of at least 0.1 equivalents of the chemical modulator relative to the concentration of the polydentate ligand increases the aspect ratio of the branched nanoparticles by at least 3-fold relative to particles formed under the same conditions in the absence of the chemical modulator. In some embodiments, the metal salts, polydentate ligands, and / or chemical modulators are selected to provide at least 0.1, at least 0.15, at least 0.2, at least 0.3, at least 0.5, at least 1.0, at least 2.0, at least 5.0, or more equivalents of the chemical modulator relative to the concentration of the polydentate ligand increase the aspect ratio of the branched nanoparticles by at least 3-fold, at least 4-fold, at least 5-fold, at least 10-fold, or more relative to particles formed under the same conditions in the absence of the chemical modulator. Those skilled in the art having the benefit of this disclosure will know how to select the metal salt, the multidentate ligand, and / or the chemical modulator to achieve the above effects. For example, in some embodiments, the metal salt and the multidentate ligand are selected to form a desired MOF, and the chemical modulator is selected based on the relative pK of the chemical modulator compared to the binding moiety of the multidentate ligand. a or the ability of the metal salt to coordinate with the metal ion. Reactions carried out under the same conditions are generally considered to be reactions carried out in the same liquid (e.g., the same solvent mixture) at the same temperature and pressure for the same time, using the same concentration of reagents and the same mixing conditions (e.g., the same volume of reaction mixture and the same stirring speed), unless otherwise stated. For example, according to one particular embodiment, when copper nitrate trihydrate is mixed with trimesic acid in methanol at 23°C in the presence of 0.1 equivalent of sodium acetate relative to the concentration of trimesic acid, the aspect ratio of the resulting branched nanoparticles of HKUST-1 is at least 3 times higher than the aspect ratio of the HKUST-1 particles formed by mixing the same concentration of copper nitrate and trimesic acid in methanol at 23°C in the absence of 0.1 equivalent of sodium acetate.
[0050] In some embodiments, the liquid in which the metal salt, the polydentate ligand, and the chemical modifier are mixed comprises a relatively high volume percent of methanol. The high volume percent of methanol may contribute, at least in part, to the surprising size and morphology of the MOF-containing branched nanoparticles described herein. In some embodiments, the liquid is at least at least 99% methanol, or 100% methanol. It should also be understood that in some embodiments, other solvent mixtures are used. For example, in some embodiments, the liquid in which the branched nanoparticles are formed is a solvent mixture that contains less than 100% (e.g., less than 100% by volume), less than 99%, or less than methanol. In some embodiments, the liquid is a solvent mixture that does not contain methanol. Without wishing to be bound by any particular theory, differences in the miscibility of the protonated and deprotonated forms of the reaction mixture components (such as the polydentate ligand) may contribute, at least in part, to the formation of the branched MOF nanoparticles.
[0051] In some embodiments, the precursors are combined under relatively mild conditions. For example, in some embodiments, the liquids are mixed for at least 10 minutes at a temperature of 15° C. or greater and 60° C. or less. Such mild conditions may allow for easy production and processing of branched nanoparticles, including MOFs.
[0052] In some embodiments, the branched nanoparticles are non-agglomerated. That is, when suspended in a continuous phase, such as a liquid suspension, or in a polymer matrix, the branched nanoparticles do not aggregate, according to certain embodiments. In some embodiments, the branched nanoparticles do not agglomerate or aggregate in suspension in a continuous phase for at least one month. For example, in some embodiments, suspensions of HKUST-1 branched nanoparticles do not aggregate, clump, or settle for at least one month. As described below, the ability of the branched nanoparticles to avoid aggregation or agglomeration in a polymer suspension may contribute to the uniform distribution of particles in the mixed matrix membrane, without being bound by theory.
[0053] In some embodiments, the branched MOF nanoparticles include a compound associated with the MOF. In some such embodiments, a chemical modulator used during the synthesis of the branched nanoparticles is associated with the MOF after the formation of the branched nanoparticles. The compound (e.g., chemical modulator) may be associated with the MOF in any of a variety of ways, including, but not limited to, adsorption (e.g., physisorption, chemisorption), coordination with a portion of the MOF. For example, in some embodiments, the compound (e.g., chemical modulator) is a Lewis base that coordinates with a Lewis acid of the MOF (such as a metal ion of the MOF). In some embodiments, the branched nanoparticles include any of the chemical modulators described above, or a combination thereof. In some embodiments, the branched nanoparticles include a carboxylate group associated with the metal-organic framework (e.g., an acetate group associated with the MOF). In some embodiments, the branched nanoparticles include an amine. In some embodiments, the amine is associated with the MOF of the branched nanoparticle (e.g., coordinates with a metal ion of the MOF). The amine can be any amine described above. For example, in some embodiments, the branched nanoparticles comprise an amine having the formula NR3, where each R is hydrogen, optionally substituted C 1~8 Independently selected from branched and unbranched alkyl, optionally substituted cycloalkyl, and optionally substituted aryl. In some embodiments, the branched nanoparticle comprises triethylamine. The presence of the compound associated with the branched nanoparticle can be determined using analytical techniques such as, for example, X-ray photoelectron spectroscopy (XPS) or thermogravimetric analysis-mass spectrometry (TGA-MS).
[0054] In some embodiments, a device is described. In some embodiments, the device comprises a mixed matrix membrane. In some embodiments, the mixed membrane matrix comprises a matrix that includes a polymer ("polymer matrix"). A variety of polymers can be used for the mixed matrix membrane. Non-limiting examples of suitable polymers include polyimide, polycarbonate, polysulfone, cellulose triacetate, polyphenylene oxide, or derivatives or combinations thereof. In some embodiments, the polymer is a polymer with inherent porosity. In some embodiments, the polymer has the following structure: [ka] and 6FDA-DAM polyimide having the above structure.
[0055] As mentioned above, a matrix containing a polymer ("polymer matrix") refers to a matrix limited to a polymer or a matrix containing a polymer and other materials. Other materials that may be present in the polymer matrix in some embodiments include, but are not limited to, metal ions, residual chemical modulator molecules, additives (such as plasticizers, zeolites, carbon, and silica particles, or combinations thereof). In some embodiments, the polymer is present in the matrix in an amount of 50 weight percent (wt%) or more, 75 wt% or more, 90 wt% or more, 95 wt% or more, 99 wt% or more, or more, based on the weight of the matrix. In some embodiments, essentially all of the matrix is composed of a polymer. In some embodiments, all of the matrix is composed of a polymer.
[0056] In some embodiments, the mixed matrix membrane comprises particles comprising a metal-organic framework. In some embodiments, the particles are present in the mixed matrix membrane at a certain weight percentage. In some embodiments, the weight percentage of the particles in the mixed matrix membrane is at least 10%, at least 20%, at least 30%, or more. In some embodiments, the weight percentage of the particles in the mixed matrix membrane is up to 50%. In some embodiments, the weight percentage of the particles in the mixed matrix membrane is up to 40% or less. Combinations of the above ranges are possible. For example, in some embodiments, the weight percentage of the particles in the mixed matrix membrane is at least 5% and up to 50%. In some embodiments, the mixed matrix membrane comprises particles comprising HKUST-1. In some embodiments, the mixed matrix membrane comprises at least 90% particles of HKUST-1. In some embodiments, the mixed matrix membrane comprises particles comprising ZIF-8. In some embodiments, the mixed matrix membrane comprises at least 90% particles of ZIF-8. In some embodiments, the particles of the mixed matrix membrane are branched MOF nanoparticles described herein (e.g., branched HKUST-1 nanoparticles, branched ZIF-8 nanoparticles).
[0057] As previously mentioned, the mixed matrix membrane, according to certain embodiments, can separate a first gas portion from a gas mixture including a first gas and a second gas. Some such separations can occur when the gas mixture passes through the mixed matrix membrane. For example, according to certain embodiments, the mixed matrix membrane can be configured to separate CO2 from CH4 or CO2 from N2. In some embodiments, the mixed matrix membrane can perform separations involving hydrocarbons. In some embodiments, the mixed matrix membrane can separate olefins from paraffins. For example, in some embodiments, the mixed matrix membrane can separate ethylene from ethane or propylene from propane.
[0058] In general, it is beneficial for a mixed matrix membrane to have relatively high selectivity and relatively high permeability or permeation during a gas separation process. The permeability of a gas through a membrane generally relates to the flow of the gas through the membrane divided by the thickness of the membrane. The selectivity of a first gas over a second gas in a gas mixture generally refers to the ratio of the permeability of the first gas to the permeability of the second gas. A common problem with mixed matrix membranes containing MOF particles is either low permeation or low selectivity. Such problems are often due to phase separation between the MOF particles and the polymer network or polymer matrix. An example of phase separation between a polymer and a MOF particle that is not a branched nanoparticle as described herein is shown in the TEM of FIG. 4B (described in Example 1 below), where the polymer phase forms an upper layer and the MOF particle phase forms an underlayer. Such phase separation can also result in voids between the MOF and the polymer matrix. Examples of such voids are shown in FIGS. 7A-7C (described in Example 1 below). Phase separation and the presence of voids in mixed matrix membranes reduces selectivity.
[0059] In some embodiments, the particles comprising the metal-organic framework are uniformly distributed in the mixed matrix membrane. In some such embodiments, the upper layer of the mixed matrix membrane and the lower layer of the mixed matrix membrane have the same uniform distribution of particles and polymers. Figure 4B shows an example of such a uniform distribution according to certain embodiments. This can be determined by using ATR-FTIR technique (the use of which is described in the examples below) to compare the spectra obtained in the upper and lower layers of the mixed matrix membrane (or vice versa). If the ATR-FTIR spectra do not show resolvable differences, the particles can be considered to be uniformly distributed.
[0060] In some embodiments, the mixed matrix membrane has a relatively small amount of voids. The voids in the mixed matrix membrane tend to allow gas to permeate by convection. Convective transport is observed when the gas permeability increases with increasing pressure of the non-plasticized gas. This tendency is characteristic of pressure-dependent pore flow due to interfacial defects in the polymer-metal-organic framework that have an effective dimension larger than the effective dimension of the pores in the metal-organic framework. In some embodiments, convective transport cannot be detected by permeation measurements.
[0061] In some embodiments, the mixed matrix membrane comprises branched nanoparticles comprising metal-organic frameworks. For example, in some embodiments, the particles of the mixed matrix membrane are any branched nanoparticles comprising metal-organic frameworks as described herein. In some embodiments, based on the weight of the particles in the membrane, at least 50 weight percent (wt%), at least 75 wt%, at least 90 wt%, at least 95 wt%, at least 99 wt%, or all of the metal-organic framework particles in the mixed matrix membrane are branched nanoparticles as described herein. In some embodiments, the mixed matrix membrane comprises branched nanoparticles comprising carboxylate-based branched nanoparticles. In some embodiments, the mixed matrix membrane comprises branched nanoparticles comprising HKUST-1. In some embodiments, the mixed matrix membrane comprises branched nanoparticles comprising ZIF-8.
[0062] The presence of metal-organic framework particles having a branched structure as described herein in a certain weight percentage can improve the gas separation performance of a mixed metal membrane according to certain embodiments (see below and Example 1 below). In some embodiments, the weight percentage of branched nanoparticles in the mixed matrix membrane is at least 5%. In some embodiments, the weight percentage of branched nanoparticles in the mixed matrix membrane is at least 10%, at least 20%, at least 30%, or more. In some embodiments, the weight percentage of branched nanoparticles in the mixed matrix membrane is up to 50%. In some embodiments, the weight percentage of branched nanoparticles in the mixed matrix membrane is up to 40% or less. Combinations of the above ranges are possible. For example, in some embodiments, the weight percentage of branched nanoparticles in the mixed matrix membrane is at least 5% and up to 50%.
[0063] In some embodiments, the branched nanoparticles form an at least partially leachable network. In some embodiments, the mixed matrix membrane comprises an at least partially leachable network. The at least partially leachable network can help improve the performance of the mixed matrix membrane during gas separation. Figures 5A-5E show examples of such leachable networks according to certain embodiments.
[0064] In some embodiments, the mixed matrix membrane is resistant to swelling or plasticization. Plasticization refers to the swelling of the polymer network or polymer matrix upon adsorption of a certain gas. The plasticization of the membrane can be monitored by monitoring the permeability of the gas through the membrane as a function of the pressure of the gas. At low pressure, the gas permeability decreases with increasing pressure. When plasticization occurs, a certain pressure point is reached, referred to herein as the plasticization pressure point, where the gas permeability begins to increase with increasing pressure due to swelling of the membrane. Such swelling generally reduces selectivity. In some embodiments, the plasticization pressure point of the mixed matrix membrane for a gas is at least 1.5 times that of a substantially identical membrane lacking the aforementioned particles. In some embodiments, the plasticization pressure point of the mixed matrix membrane for a gas (e.g., CO2) is at least 1.5 times, at least 2.0 times, at least 5.0 times, at least 10 times, at least 20 times, and / or up to 50 times that of a substantially identical membrane lacking the particles. In some embodiments, no plasticizing pressure point is observed even with gas at pressures above 750 psi. In some embodiments, the gas is CO2. In some embodiments, the gas is a hydrocarbon. The plasticizing pressure test tests multiple pressure points, first below and then above the observed plasticizing pressure, with at least 6× time lag θ (where θ=1 2 / (6 * In this equation, l is equal to the thickness of the mixed matrix membrane and D is the effective diffusion coefficient of CO2 in the membrane, which is determined experimentally.
[0065] The following examples are intended to illustrate certain embodiments of the present invention, but do not exemplify the full scope of the invention. EXAMPLES
[0066] Example 1 Synthesis of HKUST-1 particles HKUST-1 particles with various structures and sizes were synthesized using methanol (MeOH) solvent and carboxylate chemical modifier (sodium acetate) at room temperature for 1 h. Figure 1B shows a TEM image of typical HKUST-1 particles synthesized without chemical modifier, which are micron-sized (1-2 μm cross section) and have the morphology of octahedra, forming huge agglomerates. On the other hand, the introduction of modifier (0.3 molar equivalents relative to trimesic acid) during HKUST-1 synthesis resulted in branched structures as shown in Figure 1A. Figure 1A shows that these HKUST-1 particles exhibit end-to-end distances of approximately 100-300 nm in length and branches of approximately 10-30 nm in width, corresponding to an aspect ratio of approximately 5-20. Branched HKUST-1 particles were dispersed on TEM copper grids from the dried particle solution. A few meshes on the TEM grid showed well-dispersed branched HKUST-1 nanoparticles without any significant agglomerations. Furthermore, the TEM images shown in Figures 6A-6D demonstrated the effect of systematic variation of chemical modulator concentration (0, 0.1, 0.3, and 0.5 molar equivalents relative to trimesic acid, which correspond to Figures 6A, 6B, 6C, and 6D, respectively) on the size and structure of HKUST-1 particles. As the concentration of chemical modulator increased, the size of HKUST-1 particles decreased until a minimum size was reached at 0.3-0.5 molar equivalents of modulator relative to trimesic acid. This size also corresponds to a relatively high aspect ratio for the branched structure. To evaluate the effect of size and structure of HKUST-1 particles, micron-sized HKUST-1 particles synthesized without sodium acetate were selected as bulk HKUST-1 standard samples. Figure 1B shows a TEM image of bulk HKUST-1 particles. Figure 1A shows a TEM of HKUST-1 nanoparticles synthesized with 0.3 equivalents of sodium acetate relative to trimesic acid as a branched HKUST-1 sample. Figure 3A shows the XRD patterns for bulk and branched HKUST-1 particles. Both bulk and branched HKUST-1 particles showed the same crystalline phase of HKUST-1, but the peak width was broader for the branched HKUST-1 nanoparticles, indicating a smaller crystallite size.By applying the Scherrer equation to the main Bragg peak of the (222) plate, the crystallite size of the branched HKUST-1 nanoparticles was estimated to be approximately 16 nm. This feature size corresponds to the width of the branched structure. XRD results showed that increasing the sodium acetate concentration from 0 → 0.1 → 0.3 → 0.5 molar equivalents during HKUST-1 synthesis reduced the branch size of the crystallites, as suggested by the broader peak width, while the HKUST-1 crystal structure was still maintained. Figure 3B shows the particle distribution of bulk and branched HKUST-1 particles measured by DLS using a dilute suspension with MeOH as the solvent. While the bulk HKUST-1 particles roughly matched the 1-2 μm size particles observed by TEM, the HKUST-1 nanoparticles were much smaller, with diameters of approximately 100-300 nm. It should be noted that the particle size distribution calculated by DLS measurements was based on the hydrodynamic radius of a sphere using the Stokes-Einstein equation, which means that the DLS instrument cannot take into account the aspect ratio of the particles. Therefore, the DLS instrument assumed that the longer length of the particle was the radius of the skeleton hydrodynamic sphere. For this reason, the particle diameter of 100-300 nm estimated by DLS was strictly applied to the hydrodynamic radius of the interconnected branched structures. DLS measurements showed that varying the sodium acetate concentration during HKUST-1 synthesis varied the particle size distribution of HKUST-1 particles. Further addition of sodium acetate reduced the particle size distribution until the branched structures had the smallest particle size (100-200 nm). Overall, the branched HKUST-1 nanoparticles formed with sodium acetate modifier had branch widths of 10-30 nm and hydrodynamic diameters of 100-300 nm, as confirmed by TEM, XRD, and DLS analyses. These results suggested that the aspect ratios of these multidimensional MOFs were approximately 5–20.
[0067] Further characterization studies were performed on a series of HKUST-1 particles to investigate the effect of the concentration of chemical modifiers on the synthesis and chemical structure. Fourier transform infrared (FT-IR) spectra were acquired for the independent reagents (i.e., copper nitrate trihydrate and trimesic acid), chemical modifier (sodium acetate), and the product (branched HKUST-1 nanoparticles). The absorption bands of branched HKUST-1 nanoparticles were observed at 1649, 1448, and 1373 cm. -1 This indicates the coordination between the carboxylate group and the copper metal site (COO-Cu2), suggesting that the HKUST-1 structure was successfully formed. The unreacted trimesic acid was thoroughly washed away by multiple washing steps with fresh MeOH solvent at least three times and then with THF solvent at least three times. Furthermore, at approximately 490 cm -1 The absorption band at 1550 cm indicated a strong bond between the copper metal ion and the organic ligands via bridging carboxylate groups. To demonstrate the effect of chemical modifiers on HKUST-1 synthesis, FT-IR spectra were acquired for a series of HKUST-1 particles synthesized using various sodium acetate concentrations. The FT-IR spectra of HKUST-1 synthesized with 0, 0.1, 0.3, and 0.5 molar equivalents of sodium acetate were all similar in appearance and all showed the characteristic HKUST-1 peaks mentioned above. However, there was a slight increase in the peaks at approximately 1550 cm. -1 The intensity of the peak at 1550 cm gradually increased as the amount of sodium acetate increased. -1 The intensity of the peak at 177 cm increased. This change suggested that the acetate concentration from the sodium acetate modifier in the structure increased, resulting in defects in the crystal lattice of HKUST-1. These defects could be due to the substitution of a tridentate ligand (trimesic acid) characteristic of the HKUST-1 structure with a monodentate ligand (acetate ion). As the sodium acetate concentration increased during HKUST-1 synthesis, there were more defects due to sodium acetate substitution in HKUST-1. Nevertheless, the structure of HKUST-1 was retained. Raman spectra of a series of HKUST-1 particles formed using various sodium acetate concentrations were also acquired, revealing that all chemical bonds (Cu-Cu(177 cm)) in the HKUST-1 particles were clearly visible.-1 ), CH(745 and 829 cm -1 ), C=C (1005 and 1614 cm -1 ), and C-O2 (1462 and 1542 cm -1 ) vibrational forms) were located at the same position regardless of the sodium acetate concentration. However, when the Raman spectrum was expanded, the C-O2 functional group peak in the branched HKUST-1 nanoparticles had a peak at 1462 cm -1 From 1456cm -1 A small peak shift to Cu was detectable. This shift suggested that as the sodium acetate concentration during HKUST-1 synthesis increased, the position of the C-O2 functional group peak of the HKUST-1 particles approached the previously mentioned position of pure sodium acetate, thereby suggesting that only trimesic acid in the branched HKUST-1 structures was replaced by sodium acetate. Of particular interest, visual inspection of a series of HKUST-1 particles formed using various sodium acetate concentrations showed that they exhibited slightly different colors. The color difference was due to the Cu 2+ This indicates differences in particle size around the metal center and / or differences in the surrounding coordination environment. The color change occurs for both reasons. The branched HKUST-1 nanoparticles have a lower refractive index than the bulk HKUST-1 particles, and therefore a lower light reflectance. As the refractive index decreases with increasing particle size, these bulk particles appear dark blue. Furthermore, the branched HKUST-1 nanoparticles contain defects that cause the Cu 2+ The coordination environment around the metal center can also affect the color of the sample. Diffuse reflectance UV-Vis spectra were acquired for a series of HKUST-1 particles formed with various sodium acetate concentrations (0, 0.1, 0.3, and 0.5 molar equivalents of HKUST-1) when prepared with the powder pellet accessory. Overall, the diffuse reflectance UV-Vis absorption of HKUST-1 particles has two characteristic ranges: oxygen in the tricarboxylate group to Cu. 2+ Ligand-to-metal charge transfer (LMCT) to metal ions (wavelengths less than 500 nm) and Cu 2+dd transitions around the metal center (wavelengths above 500 nm). Compared to typical bulk HKUST-1 particles, branched HKUST-1 nanoparticles showed an increased peak shift in the wavelength range below 500 nm and a decreased peak shift in the wavelength range above 500 nm. Both peak shifts indicate defects such as substituted acetates and loss of linkers in the HKUST-1 structure.
[0068] Table 1 shows the results of N2 adsorption / desorption isotherms for a series of HKUST-1 particles formed with various sodium acetate concentrations. The BET surface area of the bulk HKUST-1 sample is approximately 1140 m 2 When sodium acetate was introduced in the synthesis, the BET surface area of the HKUST-1 particles was 1140 m 2 / g to 572m 2 / g. This decrease in the BET surface area of the HKUST-1 particles is due to a decrease in the micropore volume, indicating that certain defects formed may reduce the exposed surface area of the branched HKUST-1 nanoparticles compared to their bulk counterparts. These N2 adsorption isotherms also correlate with the decrease in crystalline strength determined by XRD, indicating that the bulk HKUST-1 particles have higher crystalline strength than the branched HKUST-1 nanoparticles.
[0069] [Table 1]
[0070] Thermogravimetric analysis (TGA) curves of bulk and branched HKUST-1 particles were determined by two different methods to observe the thermal behavior for as-prepared and activated samples. First, as-prepared bulk and branched HKUST-1 powder samples were loaded into a TGA pan and tested from room temperature to 800 °C at a heating rate of 20 °C / min under air. Branched HKUST-1 nanoparticles lost 20 wt% weight compared to 30 wt% weight loss for bulk samples before decomposition. The difference in solvent weight loss was attributed to reduced solvent capacity due to defects in branched HKUST-1 nanoparticles. For activation and decomposition procedures, bulk and branched HKUST-1 samples were activated at 150 °C for 2 hours under nitrogen atmosphere and after cooling to room temperature, a second TGA was performed in which the samples were gradually heated to 800 °C at the same rate as before. After activation, no significant weight change was observed up to 300 °C, indicating complete removal of the solvent during the activation process. At 300 °C, both bulk and branched HKUST-1 particles decomposed and converted to copper oxide. It should be noted that the final masses of bulk and branched HKUST-1 particles after annealing were used to back-calculate the actual weight loading of HKUST-1 particles in the mixed matrix membrane.
[0071] Preparation of mixed matrix membranes The dispersion stability of MOF particles in solution is a key factor that determines whether MOF particles can be incorporated into a polymer matrix in a homogeneously distributed state. Therefore, prior to fabricating the mixed matrix membranes, dispersion tests were performed on a series of HKUST-1 suspensions in MeOH (containing 0, 0.1, 0.3, and 0.5 molar equivalents of sodium acetate). These results demonstrated that all HKUST-1 suspensions showed good distribution immediately after strong stirring and sonication. However, when the suspensions were left on the benchtop for several hours, the bulk HKUST-1 began to settle to the bottom of the glass vial. After one day, all bulk HKUST-1 particles settled to the bottom of the glass vial, while all branched HKUST-1 suspensions retained their homogeneous distribution. Of particular interest, while HKUST-1 suspensions need to be well dispersed for up to 12 hours to incorporate homogeneously dispersed MOFs in the mixed matrix membranes, the branched HKUST-1 suspensions retained their homogeneous dispersion state for more than two weeks. Bulk and branched HKUST-1 mixed matrix membranes with various HKUST-1 weight loadings (10, 20, and 30 wt%) were fabricated using a solvent evaporation method with evaporation for approximately 6 hours to ensure uniform thickness of the thin film and homogeneous filler distribution in the composite. For the fabrication of the mixed matrix membranes, 6FDA-DAM polyimide was used as the matrix. Detailed characterization results of the polymer (i.e., purity and molecular weight) are shown in Table 2. Nuclear magnetic resonance (NMR) spectra confirmed the assignment and purity of the 6FDA-DAM polyimide matrix. It should be noted that the actual HKUST-1 weight loadings in the mixed matrix membranes from the TGA curves are all close to the targeted weight loadings, but the uncertainty for the samples independently prepared from different batches is ±1%. To demonstrate the dispersion and network formation of bulk and branched HKUST-1 in 6FDA-DAM polymer, Figure 4 shows cross-sectional images of bulk (Figure 4A) and branched (Figure 4B) HKUST-1 / 6FDA-DAM mixed matrix membranes with various HKUST-1 weight loadings. The mixed matrix membranes were fractured into two pieces using liquid nitrogen, and the cross sections were observed using FE-SEM.Figure 4A shows a cross-sectional FE-SEM image of a bulk HKUST-1 / 6FDA-DAM mixed matrix with a bulk HKUST-1 loading of 20 wt%. Membranes with incremental loadings of bulk HKUST-1 particles from 10 to 30 wt% were fabricated and observed using FE-SEM. The bulk HKUST-1 / 6FDA-DAM mixed matrix membranes exhibited an undesirably phase-separated structure into a MOF-rich phase and a polymer-rich phase, which was attributed to the rapid particle settling of bulk HKUST-1 that occurred during solvent evaporation. The thickness of the MOF-rich layer in the mixed matrix membranes increased with increasing weight loading of bulk HKUST-1. The thickness of the MOF-rich layer in the 30 wt% bulk HKUST-1 / 6FDA-DAM mixed matrix membranes was 20–25 μm, which was nearly half of the total thickness of the membrane (40–50 μm). Figure 4B shows the FE-SEM image of a branched HKUST-1 / 6FDA-DAM mixed matrix membrane with 20 wt% branched HKUST-1 particle loading. Membranes with 10-30 wt% branched HKUST-1 loading were fabricated and observed using FE-SEM. Compared to the bulk HKUST-1 / 6FDA-DAM mixed matrix membrane, the branched HKUST-1 nanoparticles were uniformly distributed in the 6FDA-DAM polymer matrix, resulting in a uniform morphology throughout the thin film. There did not appear to be any significant agglomeration of branched HKUST-1 particles even within the 30 wt% branched HKUST-1 sample. Furthermore, since the particle size and dispersibility differ between bulk HKUST-1 and branched HKUST-1, the cast HKUST-1 / 6FDA-DAM mixed matrix membranes showed a different appearance. The bulk HKUST-1 / 6FDA-DAM mixed matrix membrane was opaque due to the high reflectance caused by the large HKUST-1 particle agglomerates, whereas the branched HKUST-1 / 6FDA-DAM mixed matrix membrane was transparent due to the effective dispersion of small branched HKUST-1 nanoparticles. The image of the crystal structure of HKUST-1 can be clearly observed from behind the transparent branched HKUST-1 / 6FDA-DAM mixed matrix membrane, whereas the aforementioned image can be observed through the opaque bulk HKUST-1 / 6FDA-DAM mixed matrix membrane.
[0072]
Table 2
[0073] It was difficult to obtain clear cross-sectional images using fractured mixed matrix membranes. These cross-sectional SEM images, even at high resolution, did not clearly show localized HKUST-1 particle dispersion or interfacial voids between the HKUST-1 particles and the 6FDA-DAM polymer. To address these issues, bulk and branched HKUST-1 / 6FDA-DAM mixed matrix membranes were imaged by FIB-SEM for accurate cross-sectional analysis. Ga-ion milling was used for the FIB-SEM technique, which produced significantly smoother cross sections than liquid nitrogen fracturing. Images of branched HKUST-1 samples were obtained by milling the top of the mixed matrix membrane. However, because the bulk HKUST-1 particles settled to the bottom of the mixed matrix membrane, the membrane was inverted for FIB-SEM milling to analyze only the MOF-rich phase. Figure 7 shows FIB-SEM images of bulk HKUST-1 / 6FDA-DAM mixed matrix membranes. Various HKUST-1 weight loadings were used, all of which showed results consistent with those shown in Figures 7A-7C. In the FIB-SEM images, the bright areas are HKUST-1 particles, whereas the dark areas are 6FDA-DAM polymer. Consistent with the previous FE-SEM images, the thickness of the MOF-rich layer increased with increasing HKUST-1 weight loading. Of particular interest, there was a clear and visible interfacial void between the bulk HKUST-1 particles and the 6FDA-DAM polymer, which was consistent with the transmission results shown below. Furthermore, the curtain effect highlighted by the lines in Figure 19 is due to a density gradient associated with inefficient material packing, thereby providing further evidence of the giant voids. Figure 8 shows FIB-SEM images of branched HKUST-1 / 6FDA-DAM mixed matrix membranes with 30 wt% branched HKUST-1 loading at various magnifications (Figures 8A-8C). Remarkably, in contrast to FIG. 7, the branched HKUST-1 / 6FDA-DAM mixed matrix membrane in FIG. 20 had uniform dispersion of branched HKUST-1 nanoparticles in the polymer matrix, and no interfacial voids were observed between the particles and the polymer.Of particular interest, Figures 5A-5C show that the 30 wt% branched HKUST-1 / 6FDA-DAM mixed matrix membrane retains the percolated network characteristic of the cast particle morphology. Branched HKUST-1 nanoparticles were well distributed throughout the thin film, showing particle connectivity between free surfaces that benefit from the high aspect ratio of the branched structures. To more clearly assess the connectivity of branched HKUST-1 nanoparticles in the mixed matrix membrane, FIB-SEM cross-sectional tomography was obtained for a thin film section 11 μm long, 29 μm wide, and 4 μm deep. Figures 5D-5E show reconstructed 3D images of the 30 wt% branched HKUST-1 / 6FDA-DAM mixed matrix membrane using FIB-SEM tomography. A highly interconnected nanostructured composite thin film was formed from the branched HKUST-1 nanoparticles.
[0074] Figures 9A-9B show FT-IR spectra using an ATR accessory for pure 6FDA-DAM thin films and bulk HKUST-1 / 6FDA-DAM mixed matrix membranes with various HKUST-1 weight loadings. It should be noted that since the penetration depth of the ATR accessory is approximately 1-2 μm, it was possible to determine whether thin films with a thickness of approximately 50 μm had a uniform MOF distribution at both interfaces. Although the mixed matrix membranes had various bulk HKUST-1 weight loadings, the FT-IR spectrum of the upper side of the mixed matrix membrane (Figure 9A) showed the characteristic but identical functional group absorption bands of 6FDA-DAM, without any notable bulk HKUST-1 peaks. On the other hand, as shown in Figure 9B, the FT-IR spectrum of the lower side of the mixed matrix membrane showed the same 6FDA-DAM functional group absorption bands at 1645 cm regardless of the bulk HKUST-1 weight loading. -1 and 490cm -1The features showed almost identical HKUST-1 peak intensities at 1645 cm−1, indicating that most of the bulk HKUST-1 particles had settled to the lower side of the mixed matrix membrane. Figures 10A-10B show the FT-IR spectra of pure 6FDA-DAM thin film and branched HKUST-1 / 6FDA-DAM mixed matrix membranes with various HKUST-1 weight loadings using the same ATR accessory. Unlike the FT-IR spectra of the bulk HKUST-1 / 6FDA-DAM mixed matrix membranes, the FT-IR spectra of the branched HKUST-1 / 6FDA-DAM mixed matrix membranes showed an increase in the intensity of the HKUST-1 peak at 1645 cm−1 for both the upper and lower sides of the mixed matrix membrane as the branched HKUST-1 weight loading increased. -1 and 490cm -1 The results showed a gradual increase in the intensity of the branched HKUST-1 peak characteristic of the 6FDA-DAM polymer matrix, suggesting a uniform distribution of branched HKUST-1 nanoparticles in the 6FDA-DAM polymer matrix. These results further quantified the conclusion from the cross-sectional FE-SEM and FIB-SEM images that the bulk HKUST-1 particles settled at the lower side of the mixed matrix membrane, whereas the branched HKUST-1 nanoparticles showed a well-dispersed distribution in the mixed matrix membrane. X-ray diffraction (XRD) patterns were obtained for pure 6FDA-DAM polymer thin films as well as bulk and branched HKUST-1 / 6FDA-DAM mixed matrix membranes with various HKUST-1 weight loadings. In general, the higher the HKUST-1 weight loading, the stronger the crystalline peaks, independent of the HKUST-1 morphology, and the bulk HKUST-1 peaks were more intense than the branched HKUST-1 at similar weight loadings. These results indicated that crystallinity was maintained in the thin film preparations and that the structure of the bulk MOF was inherently more crystalline than the branched structure.
[0075] Permeation Test Prior to determining the gas permeation properties of the samples, we investigated the effect of activation temperature using a heating jacket covering the permeation cell while the mixed matrix membrane was held under vacuum and heated to activate the HKUST-1 particles. H2 and N2 gases were used as probe gases for the 20 wt% branched HKUST-1 / 6FDA-DAM mixed matrix membrane at 15, 30, and 45 psi. These results showed that the H2 and N2 permeability decreased with slight temperature increases, possibly due to increased polymer-MOF interfacial interactions or slight physical aging effects in the 6FDA-DAM polyimide phase, but also showed that the samples were thermally stable under these conditions. Furthermore, nearly identical XRD measurements for the 30 wt% branched HKUST-1 / 6FDA-DAM mixed matrix membrane obtained before and after activation using the heating jacket indicated that high HKUST-1 crystallinity was retained during activation. Therefore, we concluded that the high temperature activation process using the heating jacket did not significantly affect the gas transport properties and crystalline nature of the HKUST-1 particles. Furthermore, TGA analysis confirmed that the high temperature activation process aided in the complete removal of the solvent in the mixed matrix membranes.
[0076] Gas permeation tests were performed on pure 6FDA-DAM polymer thin films as well as bulk and branched HKUST-1 / 6FDA-DAM mixed matrix membranes with various HKUST-1 weight loadings. Prior to testing, all membrane samples were annealed at 150 °C for 2 h using a heating jacket to activate the HKUST-1 particles in the mixed matrix membranes. Figures 11A-11D show the transport properties of H2, CH4, N2, O2, and CO2 gases as a function of gas supply pressure at 35 °C for pure 6FDA-DAM polymer membranes and bulk HKUST-1 / 6FDA-DAM mixed matrix membranes with various weight loadings (10, 20, and 30 wt%). As the gas supply pressure increased, the light gases H2, CH4, N2, and O2 showed a slight decrease in permeability, while CO2, which has a higher characteristic gas-phase activity, showed an initial decrease in permeability associated with dual-mode and Langmuir adsorption effects, followed by an increase in permeability due to plasticization at higher pressures. The addition of bulk HKUST-1 particles into the 6FDA-DAM polymer matrix significantly increased gas permeability and decreased gas selectivity for the gas pairs of interest (i.e., CO2 / CH4 and CO2 / N2). For example, a 30 wt% bulk HKUST-1 / 6FDA-DAM mixed matrix membrane exhibited a CO2 gas permeability of approximately 2500 Barrer at 15 psi, which was 2.5 times that of pure 6FDA-DAM (i.e., 1000 Barrer), while the CO2 / CH4 selectivity was slightly decreased from 19 to 15. Figures 12A-12D show the permeability of H2, CH4, N2, O2, and CO2 as a function of gas supply pressure at 35 °C for pure 6FDA-DAM polymer thin films and branched HKUST-1 / 6FDA-DAM mixed matrix membranes with various weight loadings (10, 20, 30 wt%). As a function of increasing HKUST-1 weight loading, the branched HKUST-1 / 6FDA-DAM mixed matrix membranes showed a significant concomitant increase in gas permeability similar to that of the bulk HKUST-1 / 6FDA-DAM mixed matrix membranes.In comparison, the 30 wt% branched HKUST-1 / 6FDA-DAM mixed matrix membrane showed a CO2 permeability of approximately 2500 Barrer at 15 psi, which was similar to that of the 30 wt% bulk HKUST-1 / 6FDA-DAM mixed matrix membrane. However, the branched HKUST-1 / 6FDA-DAM mixed matrix membrane showed a smaller loss of selectivity for CO2 / CH4 and CO2 / N2 separation compared to that of the pure 6FDA-DAM polymer thin film. To investigate the gas transport trends as a function of HKUST-1 particle type and weight loading, Figures 13A-13B show the transport properties at 35 °C and 15 psi of the pure 6FDA-DAM polymer thin film, bulk and branched HKUST-1 / 6FDA-DAM mixed matrix membranes with various HKUST-1 weight loadings (10, 20, and 30 wt%) for CO2 / CH4 and CO2 / N2 separation at the upper bound. As the bulk and branched HKUST-1 weight loadings in the mixed matrix membranes increased, the CO2 gas permeability increased in a similar manner. However, the branched HKUST-1 / 6FDA-DAM mixed matrix membranes had more limited selectivity loss, which shifted the gas transport properties of the branched mixed matrix membrane closer to the upper bound than those of the bulk mixed matrix membrane. The bulk HKUST-1 / 6FDA-DAM mixed matrix membranes lost selectivity in parallel to the upper bound. The theoretical gas transport properties of the mixed matrix membranes with the lowest HKUST-1 weight loading (i.e., 10 wt%) and the pure 6FDA-DAM polymer thin films could not be predicted from the Maxwell model. The two assumptions of the Maxwell model are: 1) the dispersed (i.e., filler) particles must be uniformly dispersed in the continuous (i.e., polymer) matrix, and 2) the dispersed (i.e., filler) particles must be spherical to apply a shape factor (n) of 1 / 3. However, the branched HKUST-1 nanoparticles were not spherical, and the bulk HKUST-1 particles were not uniformly distributed in the 6FDA-DAM polymer matrix.As a result, the addition of 10 wt% branched HKUST-1 nanoparticles (or even 10 wt% bulk HKUST-1 particles) significantly increased the gas transport performance far beyond the theoretically predicted gas transport properties. In particular, the high aspect ratio of the branched HKUST-1 nanoparticles (5-20) results in a low permeation threshold with a shape factor of less than 0.1 and less than 10 vol%, but fitting the low shape factor to a Maxwellian model still did not provide a reasonable fit when compared to the pure HKUST-1 transport properties reported in the literature. It is possible that the highly unconventional structure and defects of these novel branched particles may have more beneficial intrinsic transport properties that were not modulated in HKUST-1, but experimentally determining the permeability of pure branched MOFs (i.e., without polymer support) remains a significant and challenging task. Figures 14A-B show the trends of gas transport properties from 0 to 100 wt% HKUST-1 weight loadings predicted by the Maxwell model using a shape factor of 1 / 3 using pure 6FDA-DAM polymer thin film data and HKUST-1 polycrystalline membranes on porous supports derived from data in the literature based on interpolation. Two sets of gas transport data points for pure 6FDA-DAM polymer thin films and bulk and branched HKUST-1 / 6FDA-DAM mixed matrix membranes with various HKUST-1 weight loadings (10, 20, and 30 wt%) are included in Figures 14A-B along with the Maxwell model predictions. Notably, the branched HKUST-1 / 6FDA-DAM mixed matrix membranes showed significantly improved gas transport properties over the theoretically predicted gas transport trends using HKUST-1 polycrystalline membranes. These results may suggest a non-standard transport mechanism in these composite systems, possibly related to the interconnected multidimensional branched structures. An additional feature of branched multidimensional MOFs is their exceptional stability against plasticization imparted to their polymeric supports. To quantify this effect, Figure 15A-B shows the normalized CO2 permeability of pure 6FDA-DAM polymer thin films, as well as bulk and branched HKUST-1 / 6FDA-DAM mixed matrix membranes with various HKUST-1 weight loadings.Addition of bulk HKUST-1 to 6FDA-DAM polymers slightly shifted the CO2 plasticization pressure point, suggesting a slight improvement in plasticization resistance. On the other hand, addition of branched HKUST-1 to 6FDA-DAM significantly shifted the CO2 plasticization pressure point, indicating a substantial improvement in plasticization resistance. Particularly interestingly, the 30 wt% branched HKUST-1 / 6FDA-DAM mixed matrix membrane showed no observable plasticization pressure point even up to 750 psi, indicating that this membrane has high CO2 resistance. To further investigate the CO2 plasticization behavior, the difference in normalized CO2 permeability between the hysteresis curves and the initial permeation isotherm at the same CO2 pressure points was calculated. To the extent that these calculations could resolve, bulk HKUST-1 / 6FDA-DAM mixed matrix membranes did not change significantly in normalized CO2 permeability as a function of increasing MOF loading, whereas branched HKUST-1 / 6FDA-DAM mixed matrix membranes showed a significant decrease in normalized CO2 permeability as a function of increasing MOF loading. These results were consistent with a molecular-level interpretation of decreased polymer chain mobility resulting from increased surface contact between the polymer chains and branched HKUST-1 nanoparticles leading to increased plasticization resistance.
[0077] Materials and methods and characterization The materials used for the following examples are as follows: Copper(II) nitrate trihydrate (Cu(NO3)2·3H2O), trimesic acid (C9H6O6, 95%), sodium acetate (NaAc, C2H3NaO2, ≥ 99.0%), methanol (MeOH, CH4O ≥ 99.9%), tetrahydrofuran (THF, C4H8O, ≥ 99.0%), N-methylpyrrolidone (NMP, C5H9NO anhydride, 99.5%) were purchased from Sigma-Aldrich and used as received. Monomeric 4,4'-(hexafluoroisopropylidene)diphthalic anhydride (6FDA, C 19H6F6O6 >99% and 2,4-diaminomesitylene (DAM, (CH3)3C6H(NH2)2 >99%) were purchased from Akron Polymer Systems. 6FDA was dried overnight in vacuum at 160 °C before use to cyclize diacid contaminants, and DAM was dried overnight in vacuum at 70 °C before use. Triethylamine (Et3N, CH6H 15 N 99%) and o-dichlorobenzene (o-DCB >98%) were used as received from Fisher. Ethanol (EtOH, C2H6O 99.5%) was used as received from VWR. Gas cylinders of H2 (HY UHP300, 100%), CH4 (ME UHP300, 100%), N2 (NI UHP300, 100%), O2 (OX UHP300, 100%), and CO2 (CD UP300, 99.999%) were purchased from Airgas.
[0078] Synthesis of HKUST-1 particles For branched HKUST-1 nanoparticles, copper precursor solutions and organic ligand solutions were prepared separately. Copper nitrate trihydrate (0.9 g, 3.7 mmol) and trimesic acid (0.43 g, 2 mmol) were dissolved in separate MeOH solutions (100 mL) along with the corresponding sodium acetate concentrations (0.2, 0.6, and 1 mmol) (0.1, 0.3, and 0.5 molar equivalents relative to trimesic acid). The two separate solutions were immediately mixed and the mixture was stirred vigorously (approximately 800 rpm) at room temperature for 1 h. After centrifugation of the final solution, at least three washing steps with fresh MeOH (100 mL) were performed, in which the MeOH was exposed to the sample for several hours at room temperature to remove unreacted monomers and chemical modifiers. The HKUST-1 suspension in MeOH was stored until use for characterization and formation of mixed matrix films. For bulk HKUST-1 particle synthesis, the same procedure as above was used, except that sodium acetate was not added.
[0079] Synthesis of 6FDA-DAM polymer 6FDA-DAM polyimide was synthesized via the ester acid route to complete imidization. A three-neck 250 mL round bottom flask and all further glassware were dried overnight at 200 °C before use. The glassware was removed from the oven and cooled under a nitrogen stream, and the monomer was cooled in a desiccator under vacuum. 6FDA (17.7695 g, 40 mmol) was transferred to a three-neck flask containing 125 mL of EtOH. The reaction flask was equipped with a Dean-Stark trap fitted with a mechanical stirrer, nitrogen inlet, and condenser. The Dean-Stark trap was charged with EtOH, and Et3N (10 mL) was added to the reaction flask. The reaction was heated to reflux under a nitrogen stream and stirred for 1 h. The Dean-Stark trap was drained and the excess Et3N and EtOH were distilled off until a viscous ester acid solution remained. DAM (6.0088 g, 40 mmol) was added along with NMP (128 mL) and o-DCB (32 mL). After completion of distillation of EtOH and Et3N, the Dean-Stark trap was charged with o-DCB and the reaction was heated to 175-180 °C. The reaction was heated and stirred under nitrogen for 48 h to give the fully cyclized polyimide. The viscous polymer solution was precipitated dropwise into stirring MeOH to give white polymer beads. The polymer beads were blended and Soxhlet extracted overnight with MeOH to remove additional NMP. The polymer was dried to a constant weight of 21.4 g (Mw=149 kDa, D=4.1, 96% yield).
[0080] Preparation of mixed matrix membranes The HKUST-1 particles were not dried before mixing with the polymer to prevent agglomeration. The solvent containing the HKUST-1 suspension was exchanged from MeOH to THF by repeated centrifugation and washing steps. For this step, the sample was centrifuged in a centrifuge tube, the supernatant was removed, and fresh THF (100 mL) was used to top the sample and exchange with MeOH at room temperature for several hours. At least three centrifugation and washing steps were used to complete the solvent exchange. To load the desired HKUST-1 weight in the mixed matrix membrane, the concentration of HKUST-1 in the stock solution was first determined by removing a small amount (0.5 ml) of the sonicated HKUST-1 suspension in THF. The volume was measured immediately after removal, followed by complete evaporation of the solution in a vacuum oven. Once the HKUST-1 particles had turned purple due to adsorption of atmospheric gases and vapors, the vial containing the dried HKUST-1 particles was weighed again, which allowed an approximation of the concentration of the HKUST-1 solution to be determined. Using the approximation of the concentration of the known HKUST-1 solution, mixed matrix membranes were prepared as follows. 6FDA-DAM polymer was dissolved in THF solvent and stirred with a stir bar for 3-4 h to obtain a homogeneous solution. The total mass of the casting solution for membrane fabrication was kept constant at 0.15 g. Thus, for the pure polymer thin film, 0.15 g of 6FDA-DAM polymer was used. For the mixed matrix membranes, 0.015, 0.03, and 0.045 g of HKUST-1 particles were added into 0.135, 0.12, and 0.105 g of 6FDA-DAM to obtain weight loadings of 10, 20, and 30 wt.% HKUST-1 in the mixed matrix membranes, respectively. The HKUST-1 solution was sonicated with a horn (Qsonica, Q500) for 1 min to further disperse the HKUST-1 particles, after which the HKUST-1 solution was mixed with the 6FDA-DAM polymer solution. The mixture was stirred for 3-4 h to homogenously disperse the HKUST-1 particles in the 6FDA-DAM polymer. The mixture was sonicated using a horn for 1 min, poured into a glass Petri dish, and covered with an aluminum foil cap with a small hole to allow the THF solvent to evaporate slowly.The thin films were cast in an oven at 50° C. overnight, resulting in a film with a thickness of 40–50 μm. The free-standing thin films were peeled off from the glass Petri dish and dried in a vacuum oven for 24 h to remove residual THF solution.
[0081] Pure gas permeation measurements Pure gas permeation measurements were performed using an automated custom-built constant volume variable pressure pure gas permeation system (Maxwell Robotics). A stock disk of brass shim with an outer diameter of 47 mm and an internal concentric hole was specially machined for the thin film support. The thin film was cut to an area larger than the hole in the brass disk, and the thickness of the thin film was measured using a micrometer before making a coupon. The thin film was placed over the hole in the support disk and attached and sealed to the small area of the exposed thin film with an impermeable epoxy adhesive (Devcon, 5 Minute Epoxy, 14250). The working area of the thin film was determined five times using a scanner and Image J software (NIH), and the average working area was used in the permeability calculations. The thin film was mounted in a stainless steel filter holder for the permeation experiments. Prior to gas permeation testing, all thin films were activated in situ under dynamic vacuum at 150°C for 2 hours using a custom-built heating jacket (HTS / Amptek) in the permeation cell. After activation, the permeation cell was allowed to cool naturally overnight to allow the temperature in the permeation cell to return to room temperature. To precisely control the test temperature, the permeation equipment was immersed in a constant temperature water bath heated to 35°C using an immersion circulator (ThermoFisher Scientific, SC150). Leak tests were performed under static vacuum by closing all valves in the permeation system, which was performed before the gas permeation tests. Gas permeability was calculated by subtracting the leak rate from the measured gas transport rate. It should be noted that for all gas permeation tests, the leak rate was less than 1% of the gas transport rate. Pure H2, CH4, N2, O2, and CO2 gases were continuously supplied for multi-pressure tests at 35°C. The first two supply pressures considered were 15 psi and 75 psi. Then, the pressure was systematically increased in 75 psi increments up to 900 psi for all gases except CO2, which was tested up to 750 psi for its saturated vapor pressure. To investigate the hysteresis effect after pressurization, the CO2 gas supply pressure was gradually decreased in units that matched our first pressurization step. After the depressurization step was completed, the sample was kept under dynamic vacuum conditions for 2 hours. Then, the same pressurization protocol as the first considered pressurization protocol was repeated.Each gas was tested for permeation at different hold times at each pressure: H2 was held for 18 minutes, CH4 for 30 minutes, N2 for 30 minutes, O2 for 24 minutes, and CO2 for 3.6 minutes. To reliably assess steady-state permeation, gas transport rates were calculated using at least 6x time lag at each pressure point. Time lag is defined as the distance from pressure (y-axis) of the intersection of the line obtained by extrapolating the time plot to the linear portion of the steady-state permeation pressure increase with the time axis (x-axis). Pure gas permeability (P. i ) is the unit of Barrer (1 Barrer = 10 -10 (cm 3 (STP)·cm) / (cm 2 Calculated in s cmHg):
number
number
number
number
number
[0082] [Table 3]
[0083] [Table 4]
[0084] [Table 5] The Maxwell model (4) was used to predict the theoretical gas transport properties of the mixed matrix membranes.
number
[0085] At high feed pressures, it was necessary to consider non-ideal gas phase behavior, especially for gases such as CO2. Therefore, the fugacity (f) was calculated to more accurately assess the permeability. The fugacity-based permeability was calculated as Equation (5) below:
number
[0086] The fugitive potential was estimated at 35 °C using a virial equation including the second and third virial coefficients. Gas-phase activity (f / f sat ) was calculated by dividing the estimated fugacity by the estimated fugacity at the theoretical saturation pressure point for CO2 at 35°C using data tables from NIST. Since CO2 is a supercritical gas at this temperature, T -1 Note that the extrapolation was done by extrapolating the saturated fugacity through the critical point when plotting the ln of fugacity as a function of .
[0087] Characterization Nuclear magnetic resonance (NMR) spectroscopy was performed using an Ascend™ 500 spectrometer (Bruker) equipped with a TopSpin™ 3.2. 1H-NMR spectra were acquired at 500 MHz. All spectra were obtained from 0.7 mL of DMSO-d6 solutions at 1–5% (w / v). Gel permeation chromatography (GPC) measurements were performed by Intertek (Allentown, PA) using a Waters 2695 chromatographic system, THF mobile phase, and refractive index detection. Solutions were analyzed using a polystyrene / divinylbenzene column set from Agilent Technologies. Sample solutions were prepared as 2 mg / mL THF solutions and filtered using a 0.45 μm nylon filter. Samples were shaken manually until completely dissolved. Molecular weights were measured using online light scattering and intrinsic viscosity signals. Narrow-range polystyrene standards ranging from 6 M to 162 Daltons were used for calibration. Fourier transform infrared (FT-IR) spectra were obtained by an Alpha II FT-IR spectrometer (Bruker) equipped with an attenuated total reflectance (ATR) accessory at a resolution of 4 cm with 32 scans. -1The measurements were performed using a TA instrument (TGA500) with a heating rate of 20°C / min for the MOF powders and the MOF mixed matrix membranes. To determine the mass of the remaining metal oxides after complete burn-off of the MOFs, the MOF powders were first activated in a TGA furnace at 150°C for 2 hours (the same conditions used for activation in the gas permeation measurements) under nitrogen atmosphere. The furnace was then cooled to room temperature and, once the temperature was stable, the ramp was run to 700°C under air with a heating rate of 20°C / min. The final product was pure metal oxides due to oxidation. To determine the actual MOF weight loading in the mixed matrix membranes, the same protocol was followed for the MOF mixed matrix membranes. Once the polymer matrix was completely decomposed under air at 700°C and only the metal oxides remained, the ratio of final weight (mixed matrix membrane) / final weight (MOF powder) was determined and is reported herein as a percentage of weight loading. Glass transition temperatures were determined from the third trajectory of a repeated heating protocol carried out between room temperature and 420°C at a heating rate of 20°C / min using a TA Instruments Differential Scanning Calorimeter (DSC250). Number-average particle size distributions were obtained from dynamic light scattering (DLS) analysis. DLS measurements were performed at 35°C using a Zetasizer Nano S90 (Marvern) after sonication of the diluted MOF suspension in MeOH to uniformly disperse the MOF particles. The diffuse reflectance of the MOF powder was measured by a UV-Vis spectrophotometer (Perkin Elmer Lambda 1050). For the preparation of UV-Vis samples, the MOF powder was fully packed into a circular powder pellet cell designed for the measurement of solid samples. Raman spectra were obtained using a Renishaw Invia Reflex Micro Raman spectroscopy using a charge-coupled device (CCD) camera with a 532 nm laser and a 1200 l / mm grating for the MOF powder on the substrate. Powder X-ray diffraction (XRD) measurements were obtained using a Bruker D8 Discover diffractometer equipped with a copper tube (l = 0.15418 nm) and a VANTEC-500 area detector. Data were recorded in the range of 5-40°. Nitrogen physisorption measurements were performed on a Micromeritics ASAP 2460 at -196 °C.Prior to measurements, all samples were degassed overnight at 150 °C under vacuum in a Micromeritics Smart VacPrep. Apparent surface areas were determined using the Brunauer-Emmett-Teller (BET) method in the P / P0 range of 0.02-0.10. Micropore volumes (V) were calculated using the t-plot method. mic) was estimated. Transmission electron microscope (TEM) images were obtained by FEI Tecnai (G2 Spirit TWIN) operating at 120 kV. A drop of diluted MOF solution with a concentration of less than 0.5% in MeOH was cast onto a copper TEM grid, and the TEM grid was allowed to air dry for several hours to allow complete evaporation of the MeOH solvent. Cross-sectional field emission scanning electron microscope (FE-SEM) images of the thin films were collected using a FE-SEM instrument (Zeiss Merlin). The thin films were cryo-fractured into two pieces in liquid nitrogen to observe the cross-sections. The cross-sections of the thin films were sputtered with gold (Au) to create a thin conductive layer (3–5 nm) for dissipating charge on the non-conductive thin films. To observe smoother cross-sections, focused ion beam scanning electron microscope (FIB-SEM) imaging was performed using an FEI Helios Nanolab 600 Dual Beam System with gallium (Ga)-ion milling. The thin film surface was similarly coated with gold (Au) using a sputtering machine to create a thin conductive layer of the same thickness. Using an e-beam position, a rectangular platinum (Pt) thin layer was coated, and the sample was tilted at 52°, after which the location below this Pt layer was subjected to Ga-ion milling at an appropriate beam current, such as 6.5 nA, using a regular cross-section. Further Ga-ion milling was performed at a lower current using a cleaning cross-section mode to create a smooth cross-section before imaging. Note that for consistent FIB-SEM imaging, all thin films were investigated with the same protocol and conditions, regardless of the morphology of HKUST-1. For reconstruction of FIB-SEM tomographic images, an e-beam was used to deposit a protective Pt / C mixture (about 250 nm) on the area to be sectioned and on the adjacent square area for alignment reference. Then, a Ga-ion beam was used to deposit a platinum layer (about 1 μm) on these same areas, engraving an X-shape within the alignment square. The initial trench was milled using an accelerating voltage of 30 kV and a current of 2.5 nA. A final milling step at a lower current (30 kV, 80 pA) was used to smooth the cross section and remove material damaged during the initial trenching.Micrograph sections with 5 nm side spacing were then acquired using software routines provided by FEI. The SEM was operated in backscattering mode (3 kV, 0.4 nA) using a through-lens detection system to increase the contrast between materials with different atomic weights to take the final micrographs. The Avizo software package (FEI) was used for data processing, during which images were aligned, cropped, and stacked. An adaptive histogram equalization routine was used to remove artifacts from depth shadowing, and a frequency domain FFT filter was used to remove curtain artifacts. An adaptive 3D histogram and edge detection routine was combined with smart thresholding techniques to find edges with large intensity changes, and then a noise reduction routine was used to eliminate single pixel regions. Different intensity regimes were assigned to the polymer material, copper material, or void regions (bubbles), and then a 3D reconstruction file was created for the copper material net. The final images of the 3D tomographic reconstruction for the copper net were created using open source software (Blender).
[0088] Example 2 This example describes the synthesis and characterization of branched nanoparticles of the metal-organic framework ZIF-8. In this example, triethylamine was used as a chemical modifier during the synthesis of ZIF-8 branched nanoparticles. Triethylamine has a higher pKa value and is more soluble in methanol than sodium acetate. The metal precursor was prepared by dissolving 0.5 g of zinc nitrate hexahydrate (Zn(NO3)26H2O, 1.68 mmol) in 20 mL of methanol (0.99 mmol), and the ligand precursor was prepared by dissolving 0.5 g of 2-methylimidazole (C4H6N2, 6.10 mmol). The ligand solution was poured into the stirred metal solution at room temperature and atmospheric pressure. Immediately after mixing, 0.2 mL of pure triethylamine (1.43 mmol) was added dropwise. The reaction solution was stirred at 600 rpm for 1 h to obtain multidimensional ZIF-8 nanoparticles. The particles were purified by washing with methanol and centrifugation of the suspension at 11,000 rpm for 90 min. Between each washing and centrifugation step, the particles were resuspended in 40 mL of fresh methanol and sonicated by indirect sonication for 30 min, direct sonication for 90 s, and processed with a vortex device at 2000 rpm for more than 2 h. Three washing steps were used for each sample. The multidimensionally branched ZIF-8 nanoparticles had previously unrecognized surface terminations, which led to different dispersion behavior in the solvents. The branched ZIF-8 nanoparticles were suspended in various solvents in different glass vials. The solvents used were dichloromethane, chloroform (solubility parameter 9.2 (cal / cm 3 ) 1 / 2 ), tetrahydrofuran (solubility parameter 9.3 (cal / cm 3 ) 1 / 2 ), dimethylformamide (solubility parameter 12.1 (cal / cm 3 ) 1 / 2 ), and methanol (solubility parameter 14.5 (cal / cm 3 ) 1 / 2). For most of the solvents considered, it was difficult to form a stable ZIF-8 suspension, but a uniform dispersion could be formed in dimethylformamide (DMF), which is also a good solvent for use in making casting solutions for certain polymers (such as certain polyimide polymers).
[0089] Example 3 This example describes the preparation and characterization of mixed matrix membranes containing branched nanoparticles of the metal-organic framework ZIF-8.
[0090] Using the 6FDA-DAM polymer matrix, mixed matrix films containing branched ZIF-8 nanoparticles were fabricated. The branched multidimensional ZIF-8 nanoparticles described in Example 2 (hereafter referred to as branched ZIF-8 or BZ) showed small hierarchical particle size (approximately 60 nm) and uniform distribution in the 6FDA-DAM polymer matrix. As a result, the BZ / 6FDA-DAM MMM was transparent. On the other hand, the rhombic dodecahedral ZIF-8 particles (called RDZ) used as a control sample had a particle size of 100-500 nm and showed agglomeration when mixed with the 6FDA-DAM polymer matrix to form the RDZ / 6FDA-DAM MMM. This agglomeration of the RDZ particles reduced the transparency of the thin film, and the RDZ-6FDA-DAM sample was opaque due to its higher reflective index. In addition, a film (called CZ / 6FDA-DAM MMM) containing commercially available ZIF-8 particles (called CZ) was fabricated. The CZ / 6FDA-DAM MMM resulted in significant aggregation of the MOF particles, which resulted in a noticeable pattern on the thin films, and therefore the BZ and RDZ mixed matrix membrane samples were used for the fabrication of mixed matrix membranes to accurately compare the effect of MOF particle structure on the transport properties.
[0091] Cross-sectional SEM images of BZ / 6FDA-DAM MMMs with various BZ loadings (10, 20, 30, and 40 wt%) were acquired. The thin films were fractured into two pieces in liquid nitrogen. The cross-sectional SEM images of 10 wt% BZ / 6FDA-DAM MMMs showed a very rough and uneven torn cross-section due to enhanced matrix elongation during thin film fracturing in liquid nitrogen. However, as the BZ MOF loading increased, the cross-sections became smoother due to immediate fracture without significant matrix elongation. Higher magnification cross-sectional SEMs were acquired, demonstrating that the FE-SEM images of BZ / 6FDA-DAM MMMs showed uniform MOF distribution regardless of MOF loading.
[0092] To further investigate the dispersion of branched ZIF-8 particles within the membrane and whether these particles form a percolated network, 30 wt. % RDZ / 6FDA-DAM MMM and 30 wt. % BZ / 6FDA-DAM MMM were imaged by FIB-SEM. Figure 16A shows a FIB-SEM image showing that 30 wt. % RDZ / 6FDA-DAM MMM contained nearly spherical ZIF-8 nanoparticles (100-500 nm) in the 6FDA-DAM polymer matrix. At this weight loading, the ZIF-8 (0.97 g cm) -3 ) and 6FDA-DAM (1.3 g cm -3 Considering the density of RDZ nanoparticles, the volume fraction of loading was determined to be 36%. Nevertheless, the 30 wt% RDZ / 6FDA-DAM MMM did not show clear evidence of a percolated network in the FIB-SEM images. It is possible that the polymer interacts favorably with the RDZ ZIF-8 particles to provide a coating layer on the MOF during casting, thereby preventing interparticle contact. Such a feature is useful for preventing defects, but it also cannot surpass the ability of the Maxwell model to predict the transport properties of MMMs. On the other hand, Figure 16B shows FIB-SEM images showing that the 30 wt% BZ / 6FDA-DAM MMM exhibited a percolated network and maintained a uniform distribution throughout the thin film. Such a percolated network may be due to the characteristic interconnected structure of branched ZIF-8 nanoparticles and increase the gas transport properties.
[0093] To investigate the transport performance, permeation tests of neat 6FDA-DAM polymer film, RDZ / 6FDA-DAM MMM, and BZ / 6FDA-DAM MMM were conducted at 35 °C and 15 psi for the separation of light gases (H2 separation from CH4, N2, and CO2, as well as O2 / N2 separation). The MMMs used various MOF loadings (10, 20, 30, and 40 wt%). The results of the permeation tests are shown in FIGS. 17A - D. As the MOF loading increased, an increase in selectivity was observed for BZ / 6FDA-DAM MMM, while RDZ / 6FDA-DAM MMM showed nearly constant selectivity. This surprising result indicated that the branched ZIF-8 sample exhibited molecular sieving behavior for gases smaller than those traditionally considered to be separated using this material (such as propylene / propane separation). The kinetic diameters of the gases were considered to increase in the following order: H2 (2.89 Å) < CO2 (3.30 Å) < O2 (3.46 Å) < N2 (3.64 Å) < CH4 (3.80 Å). Based on the findings shown in FIG. 17D, a molecular sieving window for O2 / N2 separation was available in the BZ / 6FDA-DAM membrane, suggesting that the BZ sample had effective pore openings between the sizes of O2 and N2. In particular, the mixed matrix membranes containing branched ZIF-8 nanoparticles showed selectivity for light gases greater than 15 (such as H2 / N2) and even greater than 20. Without wishing to be bound by any particular theory, it is thought that the chemical regulator (triethylamine) is incorporated into the crystal structure of the ZIF-8 MOF of the BZ particles, thereby tethering to the organic polydentate ligand (2-methylimidazole) or inhibiting the gate-opening effect (mobility), resulting in smaller effective pore openings.
[0094] Example 4 This example describes attempts at the synthesis of branched ZIF-8 nanoparticles in methanol using various different potent chemical regulators. The different chemical regulators tested were pyridine (pK a = 5.44 (in methanol), pK a = 5.22 (in H2O)), aniline (pKa = 6.05 (in methanol), pK a = 4.6 (in H2O), p-phenylenediamine (pPDA, pK a = 6.2 (in H2O), 4-ethoxyaniline (p-phenetidine, pK a = 6.92 (in methanol), pK a = 5.32 (in HO), N,N-dimethylpropargylamine (pK a = 7.97 (in methanol), pK a =8.04 (in H2O), sodium formate (pK a = 8.87 (in methanol), sodium acetate (pK a = 9.63 (in methanol), sodium propionate (pK a = 9.71 (in methanol), trimethylamine (TMA, pK a = 9.8 (in methanol), pK a = 9.74 (in H2O), triethylamine (pK a = 10.78 (in methanol), pK a = 10.67 (in H2O), diethylamine (pK a = 11.2 (in methanol), pK a = 10.72 (in HO), tri-n-butylamine (TBA, pK a = 10.89 (in HO), and n-butylamine (pK a = 11.48 (in methanol), pK a = 10.6 (in H2O). ZIF-8 nanoparticles were synthesized by the procedure described in Example 2 using identical molar amounts of modulators of different structures; the ligand source (0.5 g of C4H6N2 dissolved in 20 mL of methanol) was poured into the metal source (0.5 g of Zn(NO3)6H2O dissolved in 20 mL of methanol). 1.43 mmol of each modulator was added dropwise (or, if the modulator was solid, it was dissolved in the ligand solution before mixing), stirred for 1 h under ambient conditions, and then washed three times with fresh methanol as described in Example 2.
[0095] It was found that ZIF-8 nanoparticles synthesized using pyridine, aniline, pPDA, sodium formate, sodium acetate, and sodium propionate were not branched, but instead had the RDZ morphology described in Example 2 above. Branched ZIF-8 nanoparticles were found to form when any one of the following was used as a chemical modifier: trimethylamine, triethylamine, diethylamine, tri-butylamine, and n-butylamine. Figure 18 shows images of ZIF-8 nanoparticles formed in the presence of aniline (Figure 18A, unbranched) and triethylamine (Figure 18B, branched). The pK of the basic nitrogen of the 2-methylimidazolate multidentate ligand of the ZIF-8 MOF a (pK a pK approximately 7.97) or higher a It was observed that branched ZIF-8 nanoparticles were formed with each chemical modulator having a pK of 0.01 to 0.01. This result was due to the fact that in some cases, without wishing to be bound by any particular theory, the pK of the multidentate ligand moiety that binds to the metal ion in the metal-organic framework was a or higher pK a This shows that the use of chemical modulators having the formula (I) can contribute to the formation of branched morphologies of branched MOF nanoparticles.
[0096] X-ray photoelectron spectroscopy was also performed on RDZ and BZ ZIF-8 nanoparticles (BZ particles were synthesized using triethylamine as a chemical modifier). The XPS data was used to determine the mole percentages of elements in the two types of nanoparticles, as summarized in Table 6.
[0097] [Table 6]
[0098] As seen in Table 6, there is a significant difference in composition between the RDZ ZIF-8 nanoparticles and the BZ ZIF-8 nanoparticles. The difference in composition can be explained by the coordination of the triethylamine chemical modulator to the zinc ions in the BZ nanoparticles.
[0099] While several embodiments of the invention have been described and illustrated herein, those skilled in the art will readily envision various other means and / or structures for performing the functions and / or results and / or obtaining one or more advantages described herein, and each such variation and / or modification is deemed to be within the scope of the present invention. More generally, those skilled in the art will readily recognize that all parameters, dimensions, materials, and configurations described herein are intended to be exemplary, and that the actual parameters, dimensions, materials, and / or configurations will depend on the particular application(s) for which the teachings of the present invention are used. Those skilled in the art will recognize, or be able to ascertain, using no more than routine experimentation, numerous equivalents to the specific embodiments of the invention described herein. Thus, the foregoing embodiments are presented by way of example only, and it should be understood that, within the scope of the appended claims and their equivalents, the invention may be practiced otherwise than as specifically described and claimed. The present invention relates to each individual feature, system, article, material, and / or method described herein. Furthermore, any combination of two or more such features, systems, articles, materials, and / or methods is included within the scope of the present invention, provided that such features, systems, articles, materials, and / or methods are not mutually inconsistent.
[0100] The indefinite articles "a" and "an," as used herein and in the claims, unless clearly indicated otherwise, should be understood to mean "at least one."
[0101] The phrase "and / or" as used herein and in the claims should be understood to mean "either or both" of the elements connected by the phrase (i.e., the elements may coexist or may exist separately). Unless expressly indicated otherwise, other elements may be present, whether in association with or not with the elements specifically identified, other elements than the elements specifically identified by the "and / or" clause may be present as appropriate. Thus, as a non-limiting example, "A and / or B," when used in conjunction with open-ended language such as "comprising," can refer to, in one embodiment, A without B (optionally including elements other than B); in another embodiment, B without A (optionally including elements other than A); in yet another embodiment, both A and B (optionally including other elements), and so forth.
[0102] As used herein and in the claims, "or" should be understood to have the same meaning as "and / or" as defined above. For example, when separating items in a list, "or" or "and / or" shall be construed as inclusive (i.e., including at least one of a number or list of elements and, where appropriate, more than one of additional unlisted items). Clearly exclusive terms such as "only one" or "exactly one," or, when used in the claims, "consisting of," shall refer to the inclusion of exactly one element of a number or list of elements. In general, the term "or" as used herein shall be construed to indicate exclusive alternatives only (i.e., "one or the other, but not both") when preceded by a term of exclusivity such as "either," "one of," "only one of," or "exactly one of." "Consisting essentially of," when used in the claims, shall have its ordinary meaning as used in the field of patent law.
[0103] As used herein and in the claims, the phrase "at least one," when referring to a list of one or more elements, should be understood to mean at least one element selected from any one or more elements in the list of elements, but not necessarily including at least one of each and every element specifically listed in the list of elements, and not excluding any combination of elements in the list of elements. This definition also allows that there may optionally be elements other than those specifically identified in the list of elements to which the phrase "at least one" refers, whether or not related to the specifically identified elements. Thus, as a non-limiting example, "at least one of A and B" (or, equivalently, "at least one of A or B" or, equivalently, "at least one of A and / or B") can refer to, in one embodiment, at least one A (optionally including more than one A) in the absence of B (and optionally including elements other than B); in another embodiment, at least one B (optionally including more than one B) in the absence of A (and optionally including elements other than A); in yet another embodiment, at least one A (optionally including more than one A) and at least one B (optionally including more than one B) (and optionally including other elements), etc.
[0104] In the claims and the above specification, all transitional phrases such as "comprising," "including," "carrying," "having," "containing," "involving," and "holding" are to be understood to be open-ended (i.e., meaning "including, but not limited to"). Only the transitional phrases "consisting of" and "consisting essentially of" shall be closed or semi-closed transitional phrases, respectively, as set forth in Section 2111.03 of the United States Patent Office Manual of Patent Examining Procedures.
Claims
1. 1. A composition comprising: A branched nanoparticle comprising a metal-organic framework, the metal-organic framework comprising a metal ion and a multidentate ligand. Including, wherein the branched nanoparticles have a hydrodynamic diameter of 2 μm or less as measured by dynamic light scattering, an aspect ratio of at least 5, and branches having diameters of 200 nm or less, wherein the aspect ratio is measured by dividing the hydrodynamic radius of the branched nanoparticle by the diameter of the branch in the branched nanoparticle having the largest diameter; the metal-organic framework is HKUST-1 or a zeolite-like imidazolate framework; composition.
2. The composition of claim 1 , wherein the metal ion is a transition metal ion.
3. The composition of any one of claims 1 to 2, wherein the metal ion is copper.
4. The composition according to any one of claims 1 to 3, wherein the metal-organic framework is HKUST-1.
5. The composition according to any one of claims 1 to 2, wherein the metal ion is zinc.
6. The composition according to any one of claims 1 to 3 and 5, wherein the metal-organic framework is a zeolite-like imidazolate framework.
7. The composition according to any one of claims 1 to 3 and 5 to 6, wherein the metal-organic framework is ZIF-8.
8. The composition of any one of claims 1 to 7, wherein the branched nanoparticles are non-aggregated.
9. The composition of any one of claims 1 to 8, wherein the branched nanoparticles form an at least partially permeable network.
10. The composition of any one of claims 7 to 9, wherein the branched nanoparticles comprise an amine associated with the metal-organic framework.
11. The branched nanoparticles comprise an amine associated with the metal-organic framework, the amine having the formula NR 3 where each R is hydrogen, optionally substituted C 1~8 The composition of any one of claims 7 to 10, wherein the alkyl groups are independently selected from branched and unbranched alkyl, optionally substituted cycloalkyl, and optionally substituted aryl.
12. The composition of any one of claims 7 to 11, wherein the branched nanoparticles comprise triethylamine associated with the metal organic framework.
13. The composition of any one of claims 1 to 11, wherein each of the branched nanoparticles comprises at least two branches that are connected end-to-end and are not collinear.
14. The composition of claim 13 , wherein the at least two branches have a length to width ratio of 5 or greater.
15. 1. A method for forming branched nanoparticles, comprising: A step of combining, in a liquid, a metal salt comprising a metal ion, a multidentate ligand, and a chemical modulator to form branched nanoparticles, the branched nanoparticles comprising a metal-organic framework, the metal-organic framework comprising the metal ion and the multidentate ligand. Including, wherein the branched nanoparticles have a hydrodynamic diameter of 2 μm or less as measured by dynamic light scattering, an aspect ratio of at least 5, and branches with diameters of 200 nm or less; the metal-organic framework is HKUST-1 or a zeolitic imidazolate framework; the metal salt, the multidentate ligand, and / or the chemical modifier are selected such that, when present in an amount of at least 0.1 equivalents relative to the concentration of the multidentate ligand, the aspect ratio of the branched nanoparticles increases by at least 3-fold relative to particles formed under the same conditions in the absence of the chemical modifier; wherein the aspect ratio is measured by dividing the hydrodynamic radius of the branched nanoparticle by the diameter of the branch in the branched nanoparticle having the largest diameter.
16. 16. The method of claim 15, wherein the metal-organic framework is HKUST-1 and the chemical modulator is a salt comprising a cation and an anion, the anion having at least one carboxylate group.
17. 17. The method of claim 16, wherein the anion is acetate.
18. 16. The method of claim 15, wherein the metal-organic framework is a zeolite-like imidazolate framework and the chemical modulator comprises an amine.
19. The chemical regulator has the formula NR 3 where each R is hydrogen, optionally substituted C 1~8 20. The method of claim 18, wherein the alkyl groups are independently selected from branched and unbranched alkyl, optionally substituted cycloalkyl, and optionally substituted aryl.
20. 20. The method of claim 18, wherein the chemical regulator comprises triethylamine.
21. The pK of the chemical regulator in the liquid a is the pK of the portion of the multidentate ligand that binds to the metal ion in the metal-organic framework. a 21. The method of any one of claims 15 to 20, wherein the
22. The pK of the chemical regulator in the liquid a The method of any one of claims 15 to 21, wherein is 3.0 or greater.
23. The method of any one of claims 15 to 22, wherein the pKa of the chemical regulator in the liquid is 15.0 or less.
24. 24. The method of any one of claims 15 to 23, wherein the chemical modulator is associated with the branched MOF nanoparticles after formation of the branched nanoparticles.
25. 16. The method of claim 15, wherein the metal-organic framework is a zeolitic imidazolate framework and the branched nanoparticles comprise an amine associated with the metal-organic framework.
26. The branched nanoparticles comprise an amine associated with the metal-organic framework, the amine having the formula NR 3 where each R is hydrogen, optionally substituted C 1~8 26. The method of claim 25, wherein the alkyl groups are independently selected from branched and unbranched alkyl, optionally substituted cycloalkyl, and optionally substituted aryl.
27. The method of any one of claims 25 to 26, wherein the branched nanoparticles comprise triethylamine associated with the metal-organic framework.
28. The method of any one of claims 15 to 27, wherein the liquid is at least 99% by volume methanol.
29. 29. The method of any one of claims 15 to 28, wherein the combining step comprises mixing the liquids at a temperature of 15°C or greater and 60°C or less for at least 10 minutes.
30. The method according to any one of claims 15 to 29, wherein the metal ion is a transition metal ion.
31. The method of any one of claims 15 to 30, wherein the metal ion is copper.
32. 16. The method of claim 15, wherein the metal-organic framework is HKUST-1.
33. The method of any one of claims 15 to 30, wherein the metal ion is zinc.
34. The method of claim 15, wherein the metal-organic framework is a zeolite-like imidazolate framework.
35. The method of claim 15, wherein the metal-organic framework is ZIF-8.
36. The method of any one of claims 15 to 35, wherein each of the branched nanoparticles comprises at least two branches that are connected end-to-end and are not collinear.
37. 37. The method of claim 36, wherein the at least two branches have a length to width ratio of 5 or greater.
Citation Information
Patent Citations
Method for manufacturing composite
JP2014028792A
Method for producing a porous metal-organic structure made of zinc methylimidazolate
JP2014523898A
EMM-19*: Novel zeolite imidazolate skeleton material, method for producing the same, and its uses.
JP2015519299A
Supermolecule metal-organic structure material and manufacturing method therefor