Method for producing conductive carbon and method for producing electrode

Conductive carbon treated with oxidation and pulverization to spread like glue, addressing the issue of low energy density and stability in power storage devices by improving electrode density and maintaining stability under high temperatures.

JP7594725B2Active Publication Date: 2024-12-05NIPPON CHEMI CON CORP
View PDF 17 Cites 0 Cited by

Patent Information

Application Number
JP2020140403
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-08-21
Publication Date
2024-12-05
Estimated Expiration
2040-08-21

AI Technical Summary

Technical Problem

Existing conductive carbons used in power storage devices do not effectively increase energy density and maintain stability under high temperature conditions, as they do not efficiently spread and adhere to electrode active material particles, leading to gaps and reduced electrode density.

Method used

The use of conductive carbon that spreads like glue under pressure, subjected to oxidation and pulverization treatments, with a specific ratio of hybrid carbon determined by EELS analysis, to enhance adherence and density, thereby improving energy density and stability.

Benefits of technology

The conductive carbon effectively adheres to electrode active material particles, increasing electrode density and maintaining stability under high temperature conditions, enhancing the energy density of power storage devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007594725000003
    Figure 0007594725000003
  • Figure 0007594725000001
    Figure 0007594725000001
  • Figure 0007594725000002
    Figure 0007594725000002
Patent Text Reader

Abstract

To provide a conductive carbon which enables achievement of a power storage device having high energy density and improved in stability in high-temperature use, and a production method thereof.SOLUTION: A conductive carbon of the present invention has a property of expanding like a paste when receiving a pressure. As to the conductive carbon, a ratio of the number of carbon atoms taking part in SP2 hybrid orbitals to a total number of carbon atoms, determined from electron energy loss spectra falls in a range of 71.5-76.0%. The conductive carbon is produced by a method comprising: an oxidation step of performing an oxidizing process on a carbon material, thereby obtaining an oxidation-processed carbon having the property of expanding like a paste when receiving a pressure; and a pulverization step of pulverizing the oxidation-processed carbon in such a way that the ratio of the number of carbon atoms taking part in SP2 hybrid orbitals to a total number of carbon atoms, determined from electron energy loss spectra of the conductive carbon obtained by the pulverization step, falls in the range of 71.5-76.0%.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a conductive carbon used for an electricity storage device having high energy density and excellent high-temperature stability. The present invention also relates to a method for producing the conductive carbon and a method for producing an electrode for an electricity storage device using the conductive carbon. [Background technology]

[0002] Power storage devices such as secondary batteries, electric double layer capacitors, redox capacitors, and hybrid capacitors are devices whose applications are being considered widely as power sources for information devices such as mobile phones and notebook computers, motor drive power sources for low-pollution vehicles such as electric vehicles and hybrid vehicles, and energy regeneration systems. However, in order to meet the demand for higher performance and smaller size of these power storage devices, there is a demand for improving the energy density.

[0003] In these power storage devices, electrode active materials that exhibit capacity through a faradaic reaction involving the transfer of electrons with ions in an electrolyte (including an electrolytic solution) or a non-faradaic reaction not involving the transfer of electrons are used for energy storage. These active materials are generally used in the form of a composite material with a conductive agent. As the conductive agent, conductive carbons such as carbon black, natural graphite, artificial graphite, and carbon nanotubes are usually used. These conductive carbons are used in combination with active materials with low conductivity to impart conductivity to the composite material, but they also act as a matrix that absorbs volume changes associated with the reaction of the active material, and also play a role in ensuring an electronic conduction path even if the active material is mechanically damaged.

[0004] By the way, these composite materials of active material and conductive carbon are generally manufactured by a method of mixing active material particles with conductive carbon. Since conductive carbon does not basically contribute to improving the energy density of an electricity storage device, in order to obtain an electricity storage device with a high energy density, it is necessary to reduce the amount of conductive carbon per unit volume and increase the amount of active material. Therefore, studies have been conducted to increase the amount of active material per unit volume by improving the dispersibility of conductive carbon or reducing the structure of conductive carbon to reduce the distance between active material particles, but it is difficult to efficiently insert the conductive carbon as described above between active material particles, and therefore it is difficult to reduce the distance between active material particles to increase the amount of active material per unit volume.

[0005] In response to this problem, the applicant has proposed to use conductive carbon, which can be obtained by subjecting carbon raw materials to a strong oxidation treatment and has the property of spreading into a paste-like shape when subjected to pressure, for the electrodes of electricity storage devices (Patent Documents 1 to 15). Here, "paste-like" refers to a state in which the grain boundaries of primary carbon particles are not visible in an SEM photograph taken at a magnification of 25,000 times, and non-particulate, amorphous carbon is connected together.

[0006] Even when pressure is applied to conductive carbon such as carbon black, natural graphite, and carbon nanotubes, which are used as conductive agents in the electrodes of conventional power storage devices, the particle shape of the carbon is maintained. However, when these conductive carbons are subjected to an oxidation treatment, the surface of the particles is oxidized, and hydroxyl groups, carboxyl groups, carbonyl groups, ether bonds, etc. are introduced into the carbon, and the conjugated double bonds of the carbon are oxidized to form carbon single bonds, and carbon-carbon bonds are partially broken. By further increasing the intensity of the oxidation treatment, a conductive carbon can be obtained that has the property of spreading out like a paste under pressure.

[0007] The conductive carbon, which has the property of spreading like a paste under pressure, is characterized in that it easily adheres to the surface of the electrode active material particles, and when pressure is applied, it is compressed together and spreads like a paste, and is not easily broken apart. Therefore, when a mixture is obtained by mixing this conductive carbon with the electrode active material particles for an electrode of an electricity storage device, the conductive carbon adheres to the surface of the active material particles during the mixing process, covering the surface, and improving the dispersibility of the active material particles. If the pressure applied to the conductive carbon during the production of the mixture is large, at least a part of the conductive carbon spreads like a paste and partially covers the surface of the active material particles. Then, when an active material layer is formed on the current collector of the electrode using this mixture and pressure is applied to the active material layer, the conductive carbon further spreads like a paste and densifies while covering the surface of the electrode active material particles, and the active material particles approach each other, and accordingly the conductive carbon covers the surface of the active material particles and is pushed out into not only the gaps formed between adjacent active material particles but also the insides of the holes (including the gaps between primary particles recognized in secondary particles) present on the surface of the active material particles, and densely filled. Therefore, the amount of electrode active material per unit volume in the electrode is increased, and the electrode density is increased. In addition, the densely packed conductive carbon paste has sufficient conductivity to function as a conductive agent and does not inhibit the impregnation of the electrolyte in the power storage device. As a result, the energy density of the power storage device is improved.

[0008] For example, Patent Document 6 shows the results of evaluating the content of hydrophilic parts in the conductive carbon. Here, the "hydrophilic part" of the conductive carbon has the following meaning. That is, 0.1 g of conductive carbon is added to 20 mL of an aqueous ammonia solution of pH 11, ultrasonic irradiation is performed for 1 minute, and the resulting liquid is left for 5 hours to precipitate the solid phase part. The part that does not precipitate and is dispersed in the aqueous ammonia solution of pH 11 is the "hydrophilic part". The content of the hydrophilic part relative to the entire conductive carbon is determined by the following method. After the precipitation of the solid phase part, the remaining part after removing the supernatant liquid is dried, and the weight of the solid after drying is measured. The weight obtained by subtracting the weight of the solid after drying from the initial weight of the conductive carbon of 0.1 g is the weight of the "hydrophilic part" dispersed in the aqueous ammonia solution of pH 11. The weight ratio of the weight of the "hydrophilic part" to the weight of the initial weight of the conductive carbon of 0.1 g is the content of the "hydrophilic part" in the conductive carbon.

[0009] Patent Document 6 shows that when the intensity of the oxidation treatment is increased so that the content of the hydrophilic portion exceeds 8 mass% of the entire conductive carbon, the electrode density of the electrode manufactured using the obtained conductive carbon begins to increase, and when the content of the hydrophilic portion exceeds 9 mass% of the entire conductive carbon, the electrode density begins to increase rapidly, and when the content of the hydrophilic portion exceeds 10 mass% of the entire conductive carbon, an extremely high electrode density is obtained (see Figure 2 of this document). This improvement in electrode density corresponds to the fact that the conductive carbon is given a property of spreading like a paste when pressure is applied as the intensity of the oxidation treatment is increased. In addition, it has been shown that when a lithium ion secondary battery having a positive electrode containing acetylene black as conductive carbon and a positive electrode active material and a lithium counter electrode and a lithium ion secondary battery having a positive electrode in which half or all of the acetylene black is replaced with the conductive carbon obtained by the above-mentioned strong oxidation treatment are constructed and the charge and discharge characteristics are evaluated, the latter shows better rate characteristics and charge and discharge cycle characteristics than the former (see Figures 6 to 11, 13, and 14 of this document). This improved charge-discharge cycle characteristic is believed to be due to the fact that the surface of the electrode active material is coated with conductive carbon spread in a paste-like form, thereby suppressing the dissolution of the active material in the electrolyte (see Table 1 in this document). [Prior art documents] [Patent documents]

[0010] [Patent Document 1] JP 2015-079678 A [Patent Document 2] JP 2015-079680 A [Patent Document 3] JP 2015-079681 A [Patent Document 4] WO2015 / 056759 issue [Patent Document 5] WO2015 / 056760 issue [Patent Document 6] WO2015 / 133586 [Patent Document 7] JP 2015-181089 A [Patent Document 8] JP 2015-181090 A [Patent Document 9] JP 2016-001592 A [Patent Document 10] JP 2016-096125 A [Patent Document 11] JP 2019-019014 A [Patent Document 12] JP 2019-021420 A [Patent Document 13] JP 2019-021421 A [Patent Document 14] JP 2019-021427 A [Patent Document 15] JP 2019-200866 A [Non-patent literature]

[0011] [Non-Patent Document 1] Surface & Coatings Technology 200(2005)739-743 [Non-Patent Document 2] Carbon 102(2016)198-207 Summary of the Invention [Problem to be solved by the invention]

[0012] In the evaluation of the lithium ion secondary battery in Patent Document 6, lithium is used as the counter electrode, but this can be said to be an evaluation of a half cell. Therefore, to evaluate the performance as a practical lithium ion secondary battery, a lithium ion secondary battery was constructed using a negative electrode containing hard carbon instead of a lithium counter electrode, and a high-temperature storage test was performed in which the battery was left at 60°C, and the change in direct current internal resistance (hereinafter referred to as "DCIR") was evaluated. It was found that the DCIR increased to more than 2.5 times the initial value after the test (see Comparative Example 1 in Table 1), in order to evaluate the performance as a practical lithium ion secondary battery, as described in detail later.

[0013] As described above, recent electricity storage devices are required to have higher energy density and smaller size, and are required to have stable performance under high temperature use so that they can be used in a highly integrated state. In response to this requirement, conductive carbon, which has the property of spreading like a paste under pressure, is excellent in providing electricity storage devices with high energy density, but it is desirable to further improve its stability under high temperature use.

[0014] It is therefore an object of the present invention to provide a conductive carbon and a method for producing the same which leads to an electricity storage device having high energy density and improved stability under high temperature use. [Means for solving the problem]

[0015] The inventors conducted research based on the conductive carbon, which has the property of spreading like a paste when subjected to pressure, and which is known to lead to a storage device with high energy density, and investigated the effect of pulverizing the conductive carbon. Then, a practical lithium-ion secondary battery was constructed with a positive electrode containing the pulverized conductive carbon and a positive electrode active material, and a negative electrode containing hard carbon, and a high-temperature storage test was performed at 60°C to evaluate the change in DCIR. It was found that the change in DCIR was suppressed at first as the pulverization was intensified, but the change in DCIR increased again when the pulverization was further intensified. Therefore, in order to obtain improved stability under high-temperature use, it was necessary to select appropriate pulverization conditions.

[0016] The inventors then performed the appropriate grinding to obtain conductive carbon, and then investigated the SP contained in the conductive carbon. 2 The ratio of hybridized carbon number to the total carbon number (hereinafter referred to as "SP 2 We tried to specify it by the SP ratio. 2 The ratio is expected to decrease, so SP is used to identify conductive carbon. 2 It is expected that the ratio can be effectively utilized.

[0017] In Non-Patent Documents 1 and 2, the carbon K-edge absorption near edge fine structure (ELNES) in the electron energy loss spectrum (EELS) is used to determine the SP 2 The method for calculating the ratio is described, specifically, SP 2 The sample to be calculated and the SP 2 π from 1S orbital in standard EELS consisting of hybridized carbon only * Intensity corresponding to the excitation on the orbit I π * and σ from the 1S orbital * Intensity corresponding to the excitation on the orbit I σ * Using the above, SP is calculated by the following formula (1). 2 It is described that the ratio X is calculated (see formula (1) in Non-Patent Document 1 and formula (3) in Non-Patent Document 2). [ka]

[0018] FIG. 1 shows an example of the results of measuring EELS for carbon obtained by crushing conductive carbon that has the property of spreading like a paste when pressure is applied. In the present invention, the SP 2 To calculate the ratio X I π * and I σ * First, SP 2 EELS was obtained for the sample to be calculated and for graphite as a standard, and Fourier-ratio deconvolution was performed for each spectrum obtained. Next, the range of 270-294 eV of the deconvoluted EELS was extracted, Peak 1: 283.9-284.1 eV, half width 2.0-2.3 eV Peak 2: 286.5-286.7 eV, half-width 4.0-5.0 eV Peak 3: 289.6-289.1 eV, half width 3.9-4.3 eV Peak 4: 293.9-294.1 eV, half width 2.8-3.1 eV For the four components, the energy loss and half-width of each component are changed so as to fall within the above-mentioned ranges using a Gaussian / Lorentzian mixed function waveform, and waveform separation is performed using the least squares method. The area of ​​peak 1 obtained by waveform separation is I π * The integrated intensity of the spectrum between 292 and 307 eV of the EELS after deconvolution was I σ * From the spectrum between 292-307 eV, I σ * The reason for the determination is as follows. When the inventors investigated, it was found that the spectrum on the higher energy side than 310 eV changed even when the EELS was measured for the same sample, and the stable SP 2 The ratio was not calculated. Therefore, in Non-Patent Document 2, a stable I σ * From the integrated intensity of the spectrum between 292 eV and 307 eV, which is the recommended energy range from which I σ * We decided to ask for the following.

[0019] As a result of the study, the SP obtained from the EELS of conductive carbon was 2 It was found that by pulverizing the carbon material so that the ratio falls within the range of 71.5 to 76.0%, a conductive carbon can be obtained that leads to an electricity storage device having improved stability under high temperature use.

[0020] Therefore, the present invention provides a conductive carbon to be used as a conductive agent in an electrode of an electricity storage device, comprising: It has the property of spreading like a paste when subjected to pressure, and SP obtained from the EELS of the conductive carbon 2 The ratio is in the range of 71.5 to 76.0%. The present invention relates to a conductive carbon characterized by the above-mentioned.

[0021] The present invention also provides a method for producing the conductive carbon of the present invention, comprising the steps of: An oxidation step in which a carbon raw material is oxidized to obtain an oxidized carbon having a property of spreading like a paste under pressure; and The above-mentioned oxidation-treated carbon is subjected to a pulverization treatment, and the pulverization treatment is performed in accordance with the SP determined from the EELS of the obtained conductive carbon. 2 A crushing step is carried out so that the ratio is in the range of 71.5 to 76.0%. The present invention relates to a method for producing conductive carbon, comprising the steps of:

[0022] SP obtained from the EELS of the conductive carbon 2 By adjusting the ratio to the range of 71.5 to 76.0%, the stability of the electricity storage device obtained using the conductive carbon under high temperature use is improved. 2 By adjusting the ratio to within the range of 73.0 to 75.5%, a more preferable improvement is achieved.

[0023] In the conductive carbon of the present invention, it is preferable that the conductive carbon contains a hydrophilic portion and the content of the hydrophilic portion is 10 mass% or more of the entire conductive carbon, because the conductive carbon has a remarkable property of spreading like a paste when subjected to pressure.

[0024] By forming an electrode for an electricity storage device using the conductive carbon of the present invention, it is possible to obtain an electricity storage device having a high energy density and improved stability under high-temperature use. Therefore, the present invention also relates to a method for producing an electrode for an electricity storage device, comprising a mixing step of mixing electrode active material particles with the conductive carbon of the present invention to obtain a mixture in which at least a part of the conductive carbon spreads in a paste-like form and covers the surfaces of the electrode active material particles, and a pressurizing step of applying the mixture onto a current collector for the electrode to form an active material layer, and applying pressure to the obtained active material layer to further spread the conductive carbon in a paste-like form and densify it.

[0025] When the conductivity of the electrode active material contained in the electrode is low and it is desired to improve the conductivity of the electrode, it is preferable to further mix another conductive carbon having a higher conductivity than that of the conductive carbon in the mixing step to obtain a mixture in which at least a part of the conductive carbon spreads in a paste-like form and also covers the surface of the other conductive carbon. In producing this suitable mixture, it is preferable to carry out the mixing step by a method including a first mixing stage in which the conductive carbon and the other conductive carbon are mixed to obtain a conductive carbon mixture, and a second mixing stage in which the conductive carbon mixture is mixed with the electrode active material particles, since this further improves the conductivity of the obtained electrode. Effect of the Invention

[0026] Since the conductive carbon of the present invention has the property of easily adhering to the surface of active material particles and being compressed integrally and spread into a paste-like form when subjected to pressure, when pressure is applied to a mixture containing active material particles and the conductive carbon of the present invention in the manufacture of electrodes for electricity storage devices, the pressure causes the conductive carbon of the present invention to spread into a paste-like form and densify while covering the surfaces of the active material particles, thereby improving the energy density of the electricity storage device. Furthermore, electricity storage devices equipped with electrodes containing the conductive carbon of the present invention show improved stability under high temperature use. [Brief description of the drawings]

[0027] [Figure 1] FIG. 1 shows EELS of conductive carbon obtained by strong oxidation treatment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0028] (A) Conductive carbon and its manufacturing method The conductive carbon for the electrodes of the electricity storage device of the present invention has a property of spreading like a paste when subjected to pressure, and the SP 2 The conductive carbon is characterized in that the ratio is in the range of 71.5 to 76.0%. This conductive carbon is obtained by subjecting a carbon raw material to an oxidation treatment to obtain an oxidation-treated carbon having a property of spreading like a paste under pressure, and by subjecting the oxidation-treated carbon to a pulverization treatment, with the SP measured from EELS of the conductive carbon obtained by the pulverization treatment being in the range of 71.5 to 76.0%. 2 and a grinding step in which the ratio is in the range of 71.5 to 76.0%. Each step will be described in detail below.

[0029] (1) Oxidation stage In the oxidation step, the conductive carbon raw material is subjected to a relatively strong oxidation treatment. The carbon raw material used may be any conductive carbon used as a conductive agent for electrodes of conventional power storage devices, such as carbon blacks, such as Ketjen black, acetylene black, furnace black, and channel black, fullerene, carbon nanotubes, carbon nanofibers, graphene, amorphous carbon, carbon fibers, natural graphite, artificial graphite, graphitized Ketjen black, mesoporous carbon, and vapor-phase grown carbon fibers. From the viewpoint of ease of oxidation, however, porous carbon powder, Ketjen black, furnace black with voids, carbon nanofibers, and carbon nanotubes with voids are preferred. Among them, conductive carbons having a specific surface area of ​​300 m2 measured by the BET method are preferred. 2Conductive carbon having voids of 1000 nm or more per 1000 nm is preferred, and spherical conductive carbon such as Ketjen black and furnace black having voids is particularly preferred.

[0030] For the oxidation treatment of the carbon raw material, a known oxidation method can be used without any particular limitation. For example, the carbon raw material can be treated in a solution of an acid or hydrogen peroxide to obtain the oxidation-treated carbon. As the acid, nitric acid, a mixture of nitric acid and sulfuric acid, an aqueous solution of hypochlorous acid, etc. can be used. The carbon raw material can be heated in an oxygen-containing atmosphere, water vapor, or carbon dioxide to obtain the oxidation-treated carbon. Furthermore, the carbon raw material can be mixed with an alkali metal hydroxide, heated in an oxygen-containing atmosphere, and the alkali metal can be removed by washing with water or the like to obtain the oxidation-treated carbon. The carbon raw material can be subjected to a plasma treatment, ultraviolet light irradiation, corona discharge treatment, and glow discharge treatment in an oxygen-containing atmosphere, a treatment with ozone water or ozone gas, or an oxygen bubbling treatment in water to obtain the oxidation-treated carbon.

[0031] When a carbon raw material, preferably a carbon raw material having the above-mentioned voids, is subjected to oxidation treatment, the surface of the carbon particles is oxidized, hydroxyl groups, carboxyl groups, and ether bonds are introduced into the carbon, and the conjugated double bonds of the carbon are oxidized to form carbon single bonds, and carbon-carbon bonds are partially cut, resulting in the formation of hydrophilic parts on the particle surface. Then, by increasing the intensity of the oxidation treatment, the proportion of hydrophilic parts in the carbon particles increases, and it is possible to obtain oxidation-treated carbon that has the property of spreading like a paste under pressure. The content of hydrophilic parts in the oxidation-treated carbon is preferably 10% by mass or more of the entire oxidation-treated carbon. Such oxidation-treated carbon is easily compressed as a whole and spreads like a paste under pressure, and is easily densified.

[0032] Oxidized carbon containing 10% or more by mass of hydrophilic moieties is (a1) treating a porous carbon raw material with an acid; (b1) mixing the product after the acid treatment with a transition metal compound; (c1) grinding the mixture to cause a mechanochemical reaction; (d1) heating the product of the mechanochemical reaction in a non-oxidizing atmosphere; and (e1) A step of removing the transition metal compound and / or its reaction product from the product after heating. The compound can be suitably obtained by the first production method comprising the steps of:

[0033] In step (a1), the carbon raw material having voids is immersed in acid and left to stand. Ultrasonic irradiation may be used during this immersion. The acid may be an acid normally used in the oxidation treatment of carbon, such as nitric acid, a mixture of nitric acid and sulfuric acid, or an aqueous solution of hypochlorous acid. The immersion time depends on the concentration of the acid and the amount of the carbon raw material to be treated, but is generally in the range of 5 minutes to 5 hours. After the acid treatment, the carbon is thoroughly washed with water and dried, and then mixed with a transition metal compound in step (b1).

[0034] As the transition metal compound added to the carbon raw material in the (b1) step, inorganic metal salts such as halides, nitrates, sulfates, and carbonates of transition metals, organic metal salts such as formates, acetates, oxalates, methoxides, ethoxides, and isopropoxides, or mixtures thereof can be used. These compounds may be used alone or in combination of two or more. Compounds containing different transition metals may be mixed and used in a predetermined amount. In addition, as long as they do not adversely affect the reaction, compounds other than the transition metal compound, such as alkali metal compounds, may be added together. Since the conductive carbon of the present invention is used by being mixed with active material particles in the manufacture of electrodes for power storage devices, it is preferable to add compounds of elements constituting the active material to the carbon raw material, since this can prevent the active material from being contaminated with elements that may become impurities.

[0035] In step (c1), the mixture obtained in step (b1) is pulverized to cause a mechanochemical reaction. Examples of pulverizers for this reaction include a Raikai mill, a ball mill, a bead mill, a rod mill, a roller mill, an agitator mill, a planetary mill, a vibration mill, a hybridizer, a mechanochemical composite device, and a jet mill. The pulverization time depends on the pulverizer used and the amount of carbon to be treated, and is not strictly limited, but is generally in the range of 5 minutes to 3 hours. Step (d1) is performed in a non-oxidizing atmosphere such as a nitrogen atmosphere or an argon atmosphere. The heating temperature and heating time are appropriately selected depending on the transition metal compound used. In the subsequent step (e1), the transition metal compound and / or its reaction product are removed from the product after heating by means of dissolving it in an acid, etc., and then the product is thoroughly washed and dried to obtain an oxidation-treated carbon.

[0036] In the first manufacturing method, in the step (c1), the transition metal compound acts to promote the oxidation of the carbon raw material through a mechanochemical reaction, and the oxidation of the carbon raw material proceeds rapidly. By this oxidation, an oxidized carbon containing hydrophilic portions of 10 mass % or more of the entire conductive carbon is obtained.

[0037] The oxidized carbon containing 10% by mass or more of a hydrophilic portion is also (a2) mixing a void-containing carbon raw material with a transition metal compound; (b2) heating the resulting mixture in an oxidizing atmosphere; and (c2) removing the transition metal compound and / or its reaction product from the product after heating; It can also be suitably obtained by the second production method including the steps of:

[0038] As the transition metal compound added to the carbon raw material in the (a2) step, inorganic metal salts such as transition metal halides, nitrates, sulfates, and carbonates, organic metal salts such as formates, acetates, oxalates, methoxides, ethoxides, and isopropoxides, or mixtures thereof can be used. These compounds may be used alone or in combination of two or more. Compounds containing different metals may be mixed and used in a predetermined amount. In addition, as long as they do not adversely affect the reaction, compounds other than the transition metal compound, such as alkali metal compounds, may be added together. Since this conductive carbon is mixed with active material particles in the manufacture of electrodes for power storage devices, it is preferable to add compounds of elements constituting the active material to the carbon raw material, since this can prevent the active material from being contaminated with elements that may become impurities.

[0039] Step (b2) is carried out in an oxygen-containing atmosphere, for example, air, at a temperature at which carbon is partially but not completely lost, preferably at a temperature of 200 to 350° C. In the subsequent step (c2), the transition metal compound and / or its reaction product is removed from the product after heating by means of dissolving it in an acid or the like, and then the product is thoroughly washed and dried to obtain oxidized carbon.

[0040] In the second manufacturing method, the transition metal compound acts as a catalyst to oxidize the carbon raw material in the heating step in an oxidizing atmosphere, and the oxidation of the carbon raw material proceeds rapidly. This oxidation produces oxidized carbon containing hydrophilic portions that account for 10 mass % or more of the entire conductive carbon.

[0041] A suitable oxidized carbon containing hydrophilic portions of 10 mass% or more of the total amount can be obtained by subjecting a carbon raw material to a strong oxidation treatment, and it is also possible to promote the oxidation of the carbon raw material by a method other than the first production method and the second production method.

[0042] (2) Crushing stage In the pulverization step, the above-mentioned oxidation-treated carbon is subjected to pulverization treatment to obtain the conductive carbon of the present invention. 2 The ratio is set to be in the range of 71.5-76.0%. 2 By adjusting the ratio to the range of 73.0 to 75.5%, the stability when used at high temperatures is more preferably improved.

[0043] For the pulverization, a grinding mill, a stone mill, a ball mill, a bead mill, a rod mill, a roller mill, an agitator mill, a planetary mill, a vibration mill, a hybridizer, a mechanochemical composite device, and a jet mill can be used. The pulverization time varies depending on the amount of the oxidized carbon to be pulverized and the mixing device used, but is generally between 10 minutes and 1 hour.

[0044] (B) Electrode manufacturing method The conductive carbon of the present invention is used in an electrode of a power storage device such as a secondary battery, an electric double layer capacitor, a redox capacitor, and a hybrid capacitor in a form mixed with particles of an electrode active material that exhibits capacitance through a Faraday reaction involving the transfer of electrons with ions in an electrolyte of the power storage device or a non-Faraday reaction not involving the transfer of electrons. A power storage device essentially comprises a pair of electrodes (positive electrode, negative electrode) and an electrolyte disposed between them, and at least one of the positive electrode and the negative electrode is manufactured using a mixture containing the conductive carbon of the present invention and particles of an electrode active material.

[0045] The electrolyte placed between the positive and negative electrodes in the power storage device may be an electrolyte solution held in a separator, a solid electrolyte, or a gel electrolyte, and any electrolyte used in conventional power storage devices can be used without any particular limitation. Representative electrolytes are shown below. For lithium ion secondary batteries, an electrolyte solution in which a lithium salt such as LiPF6, LiBF4, LiCF3SO3, or LiN(CF3SO2)2 is dissolved in a solvent such as ethylene carbonate, propylene carbonate, butylene carbonate, or dimethyl carbonate is used in a state held by a separator such as a polyolefin fiber nonwoven fabric or a glass fiber nonwoven fabric. In addition, Li5La3Nb2O 12 , Li 1.5 Al 0.5 Ti 1.5 (PO4)3, Li7La3Zr2O 12 , Li7P3S 11 Inorganic solid electrolytes such as ethylene glycol, organic solid electrolytes consisting of a complex of lithium salt and polymer compounds such as polyethylene oxide, polymethacrylate, and polyacrylate, and gel electrolytes in which electrolyte is absorbed in polyvinylidene fluoride, polyacrylonitrile, etc. are also used. For electric double layer capacitors and redox capacitors, electrolytes in which quaternary ammonium salts such as (C2H5)4NBF4 are dissolved in solvents such as acrylonitrile and propylene carbonate are used. For hybrid capacitors, electrolytes in which lithium salts are dissolved in propylene carbonate, etc. and electrolytes in which quaternary ammonium salts are dissolved in propylene carbonate, etc. are used.

[0046] The positive or negative electrode of the power storage device using the conductive carbon of the present invention is generally produced by a method including a mixing step of mixing electrode active material particles and the conductive carbon of the present invention together with a solvent in which a binder is dissolved as necessary to obtain a mixture in which at least a part of the conductive carbon spreads in a paste-like form to cover the surface of the electrode active material particles, and a pressurizing step of applying the mixture onto a current collector for the electrode to form an active material layer, and applying pressure to the obtained active material layer to further spread the conductive carbon in a paste-like form and densify it. When a solid electrolyte or gel electrolyte is used as the electrolyte between the positive electrode and the negative electrode, a solid electrolyte is added to a mixture containing the conductive carbon of the present invention and the electrode active material particles in order to ensure an ion conduction path in the active material layer, and these are thoroughly kneaded together with a solvent in which a binder is dissolved as necessary, and the obtained mixture is used to form an active material layer on the current collector. As the current collector, conductive materials such as platinum, gold, nickel, aluminum, titanium, steel, and carbon can be used. The shape of the current collector can be any shape such as a film, foil, plate, net, expanded metal, or cylinder.

[0047] In the mixing step, the conductive carbon of the present invention adheres to the surface of the active material particles to cover the surface, so that the aggregation of the active material particles can be suppressed. In addition, when the pressure applied to the conductive carbon of the present invention in the mixing step is large, at least a part of the conductive carbon spreads in a paste-like form to partially cover the surface of the active material particles. In addition, the pressure applied to the active material layer in the pressurizing step causes the conductive carbon of the present invention to further spread in a paste-like form to cover the surface of the active material particles while densifying, and the active material particles approach each other, and accordingly, the conductive carbon of the present invention is pushed out not only into the gaps formed between the adjacent active material particles while covering the surface of the active material particles, but also into the inside of the holes present on the surface of the active material particles, and densely filled. Therefore, the amount of active material per unit volume in the electrode increases, and the electrode density increases. In addition, the densely filled paste-like conductive carbon has sufficient conductivity to function as a conductive agent and does not suppress the impregnation of the electrolyte in the electricity storage device. As a result, the energy density of the electricity storage device is improved.

[0048] As the positive electrode active material and the negative electrode active material to be mixed with the conductive carbon of the present invention in the mixing step, any electrode active material used in a conventional power storage device can be used without any particular limitation. The active material may be a single compound or a mixture of two or more compounds.

[0049] Examples of positive electrode active materials for secondary batteries include layered rock salt LiMO2, layered Li2MnO3-LiMO2 solid solution, and spinel LiM2O4 (wherein M is Mn, Fe, Co, Ni, or a combination thereof). Specific examples of these include LiCoO2, LiNiO2, LiNi 4 / 5 Co 1 / 5 O2, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, LiNi 1 / 2 Mn 1 / 2 O2, LiFeO2, LiMnO2, Li2MnO3-LiCoO 2、 Li2MnO3-LiNiO2, Li2MnO3-LiNi 1 / 3 Co1 / 3 Mn 1 / 3 O2, Li2MnO3-LiNi 1 / 2 Mn 1 / 2 O2, Li2MnO3-LiNi 1 / 2 Mn 1 / 2 O2-LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, LiMn2O4, LiMn 3 / 2 Ni 1 / 2 O4. Sulfur and Li2S, TiS2, MoS2, FeS2, VS2, Cr 1 / 2 V 1 / 2 Sulfides such as S2, selenides such as NbSe3, VSe2, NbSe3, Cr2O5, Cr3O8, VO2, V3O8, V2O5, V6O 13 In addition to oxides such as LiNi 0.8 Co 0.15 Al 0.05 O2, LiVOPO4, LiV3O5, LiV3O8, MoV2O8, Li2FeSiO4, Li2MnSiO4, LiFePO4, LiFe 1 / 2 Mn 1 / 2 Examples include complex oxides such as PO4, LiMnPO4, and Li3V2(PO4)3.

[0050] Examples of negative electrode active materials for secondary batteries include oxides such as Fe2O3, MnO, MnO2, Mn2O3, Mn3O4, CoO, Co3O4, NiO, Ni2O3, TiO, TiO2, SnO, SnO2, SiO2, RuO2, WO, WO2, and ZnO, metals such as Sn, Si, Al, and Zn, LiVO2, Li3VO4, and Li4Ti5O 12 Complex oxides such as Li 2.6 Co 0.4 Nitrides such as N, Ge3N4, Zn3N2, and Cu3N.

[0051] Examples of the active material in the polarizable electrode of the electric double layer capacitor include carbon materials with a large specific surface area, such as activated carbon, carbon nanofibers, carbon nanotubes, phenolic resin carbide, polyvinylidene chloride carbide, and microcrystalline carbon. In the hybrid capacitor, the positive electrode active material exemplified for the secondary battery can be used for the positive electrode, and in this case, the negative electrode is composed of a polarizable electrode using activated carbon or the like. Also, the negative electrode active material exemplified for the secondary battery can be used for the negative electrode, and in this case, the positive electrode is composed of a polarizable electrode using activated carbon or the like. Examples of the positive electrode active material of the redox capacitor include metal oxides such as RuO2, MnO2, and NiO, and the negative electrode is composed of an active material such as RuO2 and a polarizable material such as activated carbon.

[0052] There is no limitation on the shape or particle size of the active material particles, but it is preferable that the average particle size is greater than 2 μm and not more than 25 μm. Such active material particles having a relatively large particle size not only improve the electrode density by themselves, but also promote the pasting of the conductive carbon in the mixing process by the pressing force of the active material particles. In addition, in the process of applying pressure to the active material layer on the current collector in the electrode production, the active material particles having such a relatively large particle size further press the conductive carbon that has at least partially turned into a paste, further spreading the conductive carbon into a paste and densifying it. As a result, the electrode density is further increased, and the energy density of the electricity storage device is further improved.

[0053] In addition, it is preferable that the active material particles are composed of fine particles having an average particle size of 0.01 to 2 μm and coarse particles having an average particle size of more than 2 μm and not more than 25 μm, which can act as an active material of the same polarity as the fine particles. In the mixing step, the conductive carbon of the present invention adheres to and covers not only the surfaces of the fine particles but also the surfaces of the coarse particles, so that the aggregation of the active material particles can be suppressed and the mixed state of the active material particles and the conductive carbon can be made uniform. In addition, as described above, the coarse particles promote the pasting and densification of the conductive carbon of the present invention, increase the electrode density, and improve the energy density of the electricity storage device. Furthermore, by the pressure applied to the active material layer formed on the current collector by the rolling process in the electrode production, the fine particles are pushed out and filled into the gaps formed between the adjacent coarse particles together with the conductive carbon spread in a paste-like form while pressing the conductive carbon of the present invention, thereby further increasing the electrode density and further improving the energy density of the electricity storage device.

[0054] When the conductivity of the electrode active material contained in the electrode is low and it is desired to improve the conductivity of the electrode, it is preferable to further mix another conductive carbon having a higher conductivity than the conductive carbon in the mixing step, and obtain a mixture in which at least a part of the conductive carbon spreads in a paste-like form and also covers the surface of the other conductive carbon. Examples of the other conductive carbon include carbon blacks such as ketjen black, acetylene black, furnace black, and channel black, which are used for electrodes of conventional power storage devices, fullerenes, carbon nanotubes, carbon nanofibers, graphene, amorphous carbon, carbon fibers, natural graphite, artificial graphite, graphitized ketjen black, mesoporous carbon, and vapor-grown carbon fibers. The mass ratio of the conductive carbon to the other conductive carbon is generally in the range of 3:1 to 1:3.

[0055] In this embodiment, in the mixing step, at least a part of the conductive carbon of the present invention spreads in a paste-like form and adheres to and covers not only the surface of the electrode active material but also the surface of the other conductive carbon, thereby suppressing aggregation of the other conductive carbon. Furthermore, by the pressure applied to the active material layer formed on the current collector in the pressurizing step, the other conductive carbon, together with the conductive carbon of the present invention that has spread in a paste-like form, is densely filled in the gaps formed by adjacent active material particles, improving the conductivity of the entire electrode, and further improving the energy density of the electricity storage device.

[0056] In producing a suitable mixture containing the other conductive carbon, it is preferable to carry out the mixing step by a method including a first mixing stage in which the conductive carbon is mixed with the other conductive carbon to obtain a conductive carbon mixture, and a second mixing stage in which the conductive carbon mixture is mixed with the electrode active material particles, since this further improves the conductivity of the electrode obtained after the pressurizing step.

[0057] There is no particular limitation on the mixing method for carrying out the mixing step, and a known mixing method can be used. However, it is preferable to mix the active material particles, the conductive carbon of the present invention, and another conductive carbon used in combination as necessary by dry mixing, and then mix with a solvent in which a binder is dissolved as necessary. For dry mixing, a Raikai device, a ball mill, a bead mill, a rod mill, a roller mill, an agitation mill, a planetary mill, a vibration mill, a hybridizer, a mechanochemical composite device, and a jet mill can be used. In order to obtain a power storage device having a high energy density, the ratio of the active material particles to the conductive carbon of the present invention or the total of the conductive carbon of the present invention and another conductive carbon used in combination as necessary is preferably in the range of 90:10 to 99.5:0.5 by mass ratio, and more preferably in the range of 95:5 to 99:1. If the ratio of the conductive carbon is less than the above range, the conductivity of the active material layer tends to be insufficient, and the coverage rate of the active material particles by the conductive carbon tends to decrease. Also, if the ratio of the conductive carbon is more than the above range, the electrode density tends to decrease, and the energy density of the power storage device tends to decrease.

[0058] As the binder mixed with the active material particles, the conductive carbon of the present invention, and another conductive carbon used in combination as required, known binders such as polytetrafluoroethylene, polyvinylidene fluoride, tetrafluoroethylene-hexafluoropropylene copolymer, polyvinyl fluoride, and carboxymethyl cellulose are used. The content of the binder is preferably 1 to 30% by mass with respect to the total amount of the mixed materials. If it is 1% by mass or less, the strength of the active material layer is insufficient, and if it is 30% by mass or more, problems such as a decrease in the discharge capacity of the electrode and excessive internal resistance occur. As the solvent mixed with the active material particles, the conductive carbon of the present invention, and another conductive carbon used in combination as required, a solvent that does not adversely affect other materials, such as N-methylpyrrolidone, can be used without any particular limitation. EXAMPLES

[0059] The present invention will be described with reference to the following examples, but the present invention is not limited to the following examples.

[0060] Comparative Example 1 10g of Ketjen Black (product name EC300J, Ketjen Black International) was added to 300mL of 40% nitric acid, and the resulting solution was irradiated with ultrasonic waves for 10 minutes, then filtered to recover Ketjen Black. The recovered Ketjen Black was washed with water three times and dried to obtain acid-treated Ketjen Black. 1.8g of this acid-treated Ketjen Black, 0.5g of Fe(CH3COO)2, 0.19g of Li(CH3COO), 0.28g of C6H8O7·H2O, 0.33g of CH3COOH, 0.33g of H3PO4, and 250mL of distilled water were mixed, and the resulting mixture was stirred with a stirrer for 1 hour, then evaporated to dryness at 100℃ in air, and the mixture was collected. The resulting mixture was then introduced into a vibration ball mill and milled at 20Hz for 10 minutes. The ground powder was heated in nitrogen at 700°C for 3 minutes to obtain a composite of LiFePO4 supported on Ketjen Black.

[0061] 1 g of the resulting composite was added to 100 mL of a 30% aqueous hydrochloric acid solution, and the resulting solution was irradiated with ultrasonic waves for 15 minutes to dissolve the LiFePO4 in the composite, and the remaining solid was filtered, washed with water, and dried. A part of the dried solid was heated to 900°C in air by TG analysis to measure the weight loss. The above-mentioned process of dissolving LiFePO4 in an aqueous hydrochloric acid solution, filtering, washing with water, and drying was repeated until it was confirmed that the weight loss was 100%, that is, no LiFePO4 remained, to obtain LiFePO4-free oxidation-treated carbon.

[0062] Next, 0.1 g of the obtained oxidized carbon was added to 20 mL of an aqueous ammonia solution of pH 11, and ultrasonic irradiation was performed for 1 minute. The obtained liquid was left to stand for 5 hours to allow the solid phase to precipitate. After the solid phase precipitated, the supernatant liquid was removed and the remaining part was dried, and the weight of the dried solid was measured. The weight ratio of the weight of the dried solid subtracted from the weight of the initial oxidized carbon (0.1 g) to the weight of the initial oxidized carbon (0.1 g) was determined as the content of the "hydrophilic portion" in the oxidized carbon. The content of the hydrophilic portion was 10.2% of the total oxidized carbon.

[0063] In addition, EELS was measured for the obtained oxidized carbon and the graphite standard using a scanning transmission microscope HD2700 manufactured by Hitachi High-Technologies Corporation. Fourier-ratio deconvolution was performed for each of the obtained spectra using Gaten's software, and then the range of 270-294 eV of the EELS after deconvolution was extracted using the fitting analysis software of the analysis software (spectra manager) and analyzed by the above-mentioned method. I π * From the integrated intensity of the spectrum between 292-307 eV of the EELS after deconvolution, I σ * Then, using the above formula (1), SP 2 The ratio was calculated.

[0064] In addition, 96 parts by mass of commercially available LiNi 0.5 Mn 0.3 Co 0.2 An appropriate amount of N-methylpyrrolidone was added to O2 particles (average particle size 5 μm), 2 parts by mass of the above-mentioned oxidized carbon, and 2 parts by mass of polyvinylidene fluoride, and thoroughly kneaded to form a slurry. This slurry was applied to an aluminum foil and dried, and then pressed three times under a condition of 1.5 t / cm to obtain a positive electrode for a lithium-ion secondary battery.

[0065] In addition, 93 parts by mass of hard carbon, 1 part by mass of acetylene black, and 6 parts by mass of polyvinylidene fluoride were mixed with an appropriate amount of N-methylpyrrolidone to form a slurry. This slurry was applied onto a copper foil, dried, and then pressed to obtain a negative electrode for a lithium ion secondary battery having an electrode density of 1.0 g / cc. The ratio of the positive electrode capacity to the negative electrode capacity was 1:1.2.

[0066] The obtained positive and negative electrodes were vacuum dried at 100°C for 12 hours, and then a lithium ion secondary battery was fabricated using a 1M LiPF6 solution in ethylene carbonate / dimethyl carbonate / propylene carbonate (1:1:1) as an electrolyte.

[0067] A high-temperature storage test was performed on the obtained battery. First, the obtained battery was charged until the SOC (remaining capacity (Ah) / full charge capacity (Ah) x 100) was 50%, then discharged at a constant current for 10 seconds, and the initial DCIR was calculated from the voltage drop. Next, the battery was charged to 4V and left in a thermostatic chamber at 60°C for 2 weeks, after which the battery was removed from the thermostatic chamber, charged until the SOC was 50%, then discharged at a constant current for 10 seconds, and the DCIR after storage was calculated from the voltage drop. The resistance increase rate of the DCIR after storage from the initial DCIR was calculated as a measure of high-temperature storage stability.

[0068] Example 1 The LiFePO4-free oxidation-treated carbon obtained in Comparative Example 1 was introduced into a vibration ball mill and pulverized for 20 minutes under the condition of 10 Hz. A lithium ion secondary battery was produced in the same manner as in Comparative Example 1 using the obtained pulverized conductive carbon instead of the oxidation-treated carbon of Comparative Example 1, and the obtained battery was subjected to a high-temperature storage test in the same manner as in Comparative Example 1.

[0069] Example 2 The LiFePO4-free oxidation-treated carbon obtained in Comparative Example 1 was introduced into a vibration ball mill and pulverized for 20 minutes under the condition of 15 Hz. A lithium ion secondary battery was produced in the same manner as in Comparative Example 1 using the obtained pulverized conductive carbon instead of the oxidation-treated carbon of Comparative Example 1, and the obtained battery was subjected to a high-temperature storage test in the same manner as in Comparative Example 1.

[0070] Example 3 The LiFePO4-free oxidation-treated carbon obtained in Comparative Example 1 was introduced into a vibration ball mill and pulverized for 30 minutes under the condition of 15 Hz. A lithium ion secondary battery was produced in the same manner as in Comparative Example 1 using the obtained pulverized conductive carbon instead of the oxidation-treated carbon of Comparative Example 1, and the obtained battery was subjected to a high-temperature storage test in the same manner as in Comparative Example 1.

[0071] Example 4 The LiFePO4-free oxidation-treated carbon obtained in Comparative Example 1 was introduced into a vibration ball mill and pulverized for 60 minutes under the condition of 20 Hz. A lithium ion secondary battery was produced in the same manner as in Comparative Example 1 using the obtained pulverized conductive carbon instead of the oxidation-treated carbon of Comparative Example 1, and the obtained battery was subjected to a high-temperature storage test in the same manner as in Comparative Example 1.

[0072] Example 5 The LiFePO4-free oxidation-treated carbon obtained in Comparative Example 1 was introduced into a vibration ball mill and pulverized for 20 minutes under the condition of 30 Hz. A lithium ion secondary battery was produced in the same manner as in Comparative Example 1 using the obtained pulverized conductive carbon instead of the oxidation-treated carbon of Comparative Example 1, and the obtained battery was subjected to a high-temperature storage test in the same manner as in Comparative Example 1.

[0073] Comparative Example 2 The LiFePO4-free oxidation-treated carbon obtained in Comparative Example 1 was introduced into a vibration ball mill and pulverized for 60 minutes under the condition of 30 Hz. A lithium ion secondary battery was produced in the same manner as in Comparative Example 1 using the obtained pulverized conductive carbon instead of the oxidation-treated carbon of Comparative Example 1, and the obtained battery was subjected to a high-temperature storage test in the same manner as in Comparative Example 1.

[0074] Table 1 shows the SPs obtained from the EELS of the conductive carbon for Examples 1 to 5 and Comparative Examples 1 and 2. 2 The ratio and the resistance increase rate calculated in a high-temperature storage test of the lithium ion secondary battery are shown together. [Table 1]

[0075] As can be clearly seen from Table 1, when the oxidized carbon of Comparative Example 1 is pulverized and then the obtained conductive carbon is used to construct a practical lithium ion secondary battery, the resistance increase rate in the high temperature storage test is preferably decreased, but when the intensity of the pulverization is increased, the resistance increase rate in the high temperature storage test, which had decreased once, starts to increase again. Therefore, in order to obtain an electricity storage device having a high energy density and improved stability under high temperature use, it is necessary to select the SP determined by EELS. 2 The oxidized carbon must be crushed to a ratio of 71.5 to 76.0%. In order to obtain stability under high temperature conditions for the storage device, the SP determined by EELS must be 2It is important to pulverize the oxidized carbon so that the ratio falls within the range of 73.0 to 75.5%. [Industrial Applicability]

[0076] By using the conductive carbon of the present invention, it is possible to obtain an electricity storage device having a high energy density and improved stability under high temperature use.

Claims

1. A method for producing conductive carbon to be used as a conductive agent in an electrode of an electricity storage device, the conductive carbon having a property of spreading like a paste under pressure, and the ratio of the number of SP 2 hybridized carbons to the total number of carbons of the conductive carbon determined from an electron energy loss spectrum of the conductive carbon being in the range of 71.5 to 76.0%, An oxidation step in which a carbon raw material is oxidized to obtain an oxidized carbon having a property of spreading like a paste under pressure; and The oxidized carbon is subjected to a pulverization treatment, and the pulverization treatment is performed in accordance with the SP determined from the electron energy loss spectrum of the resulting conductive carbon. 2 A grinding step is carried out so that the ratio of the number of hybrid carbon atoms to the number of total carbon atoms is in the range of 71.5 to 76.0%. A method for producing conductive carbon, comprising:

2. In the pulverization step, the pulverization process is performed according to the SP determined from the electron energy loss spectrum of the obtained conductive carbon. 2 The method for producing conductive carbon according to claim 1, wherein the method is carried out so that the ratio of the number of hybrid carbon atoms to the total number of carbon atoms falls within the range of 73.0 to 75.5%.

3. 3. The method for producing conductive carbon according to claim 1, wherein in the oxidation step, the oxidation treatment is carried out so that the content of hydrophilic portions in the obtained oxidized carbon is 10 mass% or more of the total oxidized carbon.

4. A method for producing an electrode for an electricity storage device, comprising the steps of: A carbon production step of obtaining conductive carbon by the production method according to any one of claims 1 to 3; a mixing step of mixing the electrode active material particles with the conductive carbon to obtain a mixture in which at least a part of the conductive carbon spreads in a paste-like form and covers the surfaces of the electrode active material particles; and a pressurizing step of applying the mixture onto a current collector for the electrode to form an active material layer, and applying pressure to the active material layer to further spread the conductive carbon into a paste-like form and densify it; A method for producing an electrode, comprising:

5. 5. The method for producing an electrode according to claim 4, wherein in the mixing step, another conductive carbon having a higher conductivity than that of the conductive carbon is further mixed to obtain a mixture in which at least a portion of the conductive carbon spreads in a paste-like form and also covers a surface of the other conductive carbon.

6. The mixing step comprises: a first mixing step of mixing the conductive carbon with the other conductive carbon to obtain a conductive carbon mixture; and A second mixing step of mixing the conductive carbon mixture with the electrode active material particles. A method for producing the electrode of claim 5, comprising:

Citation Information

Patent Citations

  • Negative electrode for lithium secondary battery, lithium secondary battery and method of manufacturing negative electrode for lithium secondary battery

    JP2011258348A

  • Conductive carbon and method for manufacturing the same

    JP2015079678A

  • Conductive carbon and method for manufacturing the same

    JP2015079680A

  • Electrode material for lithium ion secondary batteries, and lithium ion secondary battery arranged by use thereof

    JP2015079681A

  • Conductive carbon, electrode material including conductive carbon, and electrode using the electrode material

    JP2015181089A