Beauty Methods
The application of a humidity-responsive polyvinyl alcohol film with a waterproof and moisture-permeable layer addresses moisture evaporation issues, providing effective skin moisturization and comfort across varying humidity levels.
Patent Information
- Application Number
- JP2021530024
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-07-03
- Filing Date
- 2020-06-29
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2040-06-29
AI Technical Summary
Existing beauty methods fail to provide sufficient moisturizing effects in low-humidity environments and cause sticky discomfort in high-humidity or sweaty conditions due to moisture evaporation issues.
Application of a moisturizing polyvinyl alcohol film to the skin, which exhibits humidity responsiveness by adjusting moisture evaporation based on environmental conditions, combined with a waterproof and moisture-permeable layer to manage moisture transfer.
Ensures effective skin moisturization in low-humidity environments while reducing sticky discomfort in high-humidity or sweaty conditions, enhancing skin health and appearance.
Smart Images

Figure 0007595008000003 
Figure 0007595008000004 
Figure 0007595008000005
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a cosmetic method utilizing moisturizing effects. [Background technology]
[0002] In recent years, various cosmetic methods have been proposed to improve skin problems.
[0003] Patent Document 1 discloses a beauty method for preventing acne and cleansing at the same time, which includes the steps of impregnating a sheet with a lotion containing component (A): an anti-inflammatory agent, component (B): a bactericide, component (C): a fatty acid ester nonionic surfactant, component (D): a moisturizer, and component (E): water, and wiping away dirt on the skin with the sheet impregnated with the lotion.
[0004] Patent Document 2 describes a cosmetic product that has a sheet base layer and an adhesive layer that can adhere to the skin surface after an emulsion cosmetic containing 5 to 50% by mass of an oily component is applied to the skin, and the water vapor permeability of the entire sheet including the sheet base layer and the adhesive layer is 200 to 2,000 g / m 2 A cosmetic method is disclosed in which a skin patch sheet is applied for 24 hours. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2016-132625 A [Patent Document 2] JP 2011-178693 A Summary of the Invention [Problem to be solved by the invention]
[0006] For example, in Japan, the humidity of the outdoor environment tends to be high during the rainy season, while the humidity tends to be quite low during the winter, when there is little rain. In recent years, with the use of air conditioners, the humidity may be quite low even in indoor workplaces or shopping centers. In such a low-humidity environment, moisture from the skin evaporates, causing the skin to lose moisture, and skin problems such as rough skin and wrinkles tend to occur.
[0007] In order to improve such skin troubles, moisturizers such as glycerin are generally applied to the skin. However, even if the moisturizer components applied to the skin temporarily retain the moisture generated from the skin and exert moisturizing performance, if the humidity of the outside air is low, the retained moisture will evaporate into the outside air over time, so it is not possible to obtain sufficient moisturizing effect. In addition, if the moisturizer is applied to the skin and the person sweats, the occlusion effect of the moisturizer spread over the skin makes it difficult for the sweat to evaporate into the outside air, which tends to cause sticky discomfort.
[0008] For example, the sheet described in Patent Document 2 always has a relatively low moisture permeability, so when a large amount of sweat is produced, the sheet cannot efficiently evaporate sweat into the outside air, which is likely to cause a sticky and uncomfortable feeling. In addition, since such a sheet is in a state where moisture from the skin is constantly evaporating through the sheet, such a sheet does not provide a sufficient moisturizing effect in a low humidity environment where moisture from the skin is likely to evaporate, and is therefore not likely to be able to fully improve skin problems such as rough skin.
[0009] Therefore, the subject of the present disclosure is to provide a beauty method that can ensure moisturizing of the skin while reducing sticky discomfort in a high humidity environment or when sweating, and can also ensure moisturizing of the skin and enhance the beauty effect even in a low humidity environment. [Means for solving the problem]
[0010] <Aspect 1> A cosmetic method in which a moisturizing polyvinyl alcohol film is applied to the body surface. <Aspect 2> 2. The cosmetic method according to aspect 1, wherein the application of the moisturizing polyvinyl alcohol film to a body surface is carried out by sticking it in the form of a free-standing film. <Aspect 3> The cosmetic method according to aspect 1, wherein the application of the moisturizing polyvinyl alcohol film to the body surface is carried out by spreading a composition containing polyvinyl alcohol and water on the body surface. <Aspect 4> The cosmetic method according to any one of Aspects 1 to 3, wherein the moisture-retaining polyvinyl alcohol film is applied to the body surface after a waterproof / moisture-permeable layer is applied to the body surface. <Aspect 5> The cosmetic method according to aspect 4, wherein the waterproof / moisture-permeable layer is applied to a body surface by attachment in the form of a free-standing film. Aspect 6 A cosmetic method according to aspect 4, wherein the application of the waterproof / moisture-permeable layer to a body surface is carried out by spreading components of the waterproof / moisture-permeable layer on the body surface. Aspect 7 The cosmetic method according to aspect 1 or 2, wherein a waterproof and moisture-permeable layer is applied to one side of the polyvinyl alcohol film for moisturizing, and then the polyvinyl alcohol film for moisturizing is applied to a body surface via the waterproof and moisture-permeable layer. <Aspect 8> The cosmetic method according to any one of aspects 1 to 7, wherein the moisture-retaining polyvinyl alcohol film has a thickness of 100 μm or less. <Aspect 9> The cosmetic method according to any one of aspects 1 to 8, wherein the moisturizing polyvinyl alcohol film contains unmodified polyvinyl alcohol. Aspect 10 A cosmetic method according to any one of aspects 4 to 9, wherein the waterproof and moisture-permeable layer is at least one selected from an oil layer containing at least one of petrolatum and liquid paraffin, a polylactic acid layer, and an artificial skin. <Aspect 11> The cosmetic method according to any one of aspects 1 to 10, wherein, when the moisture-retaining polyvinyl alcohol film or a laminate including the moisture-retaining polyvinyl alcohol film and the waterproof / moisture-permeable layer is evaluated in a moisture evaporation test, the amount of moisture evaporation measured in an environment of 23°C and 40% RH is less than the amount of moisture evaporation measured in an environment of 28°C and 70% RH. Effect of the Invention
[0011] According to the present disclosure, a beauty method can be provided that can ensure moisturizing of the skin while reducing sticky discomfort in a high humidity environment or when sweating, and can also ensure moisturizing of the skin and enhance the beauty effect even in a low humidity environment. [Brief description of the drawings]
[0012] [Figure 1] 1 is a schematic diagram showing the moisture blocking state when the moisture-retaining polyvinyl alcohol film of the present disclosure is applied to the skin in a low humidity environment. FIG. [Diagram 2] 1 is a schematic diagram showing the moisture permeation state when the moisture-retaining polyvinyl alcohol film of the present disclosure is applied to the skin in a high humidity environment. [Diagram 3] 1 is a schematic diagram showing the moisture permeation state when a thin moisturizing polyvinyl alcohol film of the present disclosure is applied to skin with a relatively high moisture content in a low humidity environment. [Figure 4] 1 is a schematic diagram showing the moisture blocking state when a waterproof / moisture permeable layer and a thin moisturizing polyvinyl alcohol film of the present disclosure are applied to skin with a relatively high moisture content in a low humidity environment. [Diagram 5] FIG. 2 is a schematic diagram of a measurement sample sealed with a polyvinyl alcohol film used in a moisture evaporation test. [Figure 6] 1 is a graph showing the amount of water evaporation from each sample in a water evaporation test under an environment of 28° C. and 70% RH (high humidity environment) and 23° C. and 40% RH (low humidity environment). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present disclosure is not limited to the following embodiments, and may be modified in various ways within the scope of the present invention.
[0014] The cosmetic method of the present disclosure involves applying a moisturizing polyvinyl alcohol film to a body surface.
[0015] Although not limited by the principle, it is believed that the principle of action of the cosmetic method of the present disclosure is as follows, by which the cosmetic method of the present disclosure can ensure moisturizing of the skin while reducing sticky discomfort in a high humidity environment or when sweating, and can ensure moisturizing of the skin and enhance the cosmetic effect even in a low humidity environment. Note that in the present disclosure, polyvinyl alcohol may be abbreviated as "PVA".
[0016] When exposed to dryness, moisture is robbed without our realizing it, and the stratum corneum on the skin surface may not be able to maintain its moisture level. When the skin lacks moisture, it is unable to produce the moisturizing ingredients (natural moisturizing factors (NMFs)) that it produces itself. As a result, the barrier function and moisturizing function of the skin surface are reduced, making the skin more susceptible to damage, which is thought to cause skin irritation and other problems.
[0017] In addition, if the stratum corneum on the skin's surface continues to lack moisture, the skin tries to quickly create new cells to repair the damaged stratum corneum, which speeds up the skin's regeneration (turnover) process and simultaneously produces a large number of immature and incomplete cells. As a result, the skin is not prepared to create a normal stratum corneum, and the skin surface cannot retain enough moisture, resulting in a vicious cycle of persistent rough skin.
[0018] It is generally known that PVA has excellent affinity with moisture. For example, as shown in FIG. 1, when a PVA film 101 is applied to the skin, moisture 105 evaporated from the skin binds to PVA molecules 103 in the film, and the PVA molecules 103 move so as to attract each other around the moisture 105, and it is considered that gaps 107 through which moisture passes are formed. However, when the humidity of the external environment is low, it is considered that the PVA molecules 103 do not move near the outermost surface of the PVA film 101, and therefore gaps 107 through which moisture passes are not formed. As a result, in a low humidity environment, moisture evaporated from the skin remains below the outermost surface of the PVA film and is not evaporated into the atmosphere, so that it is considered that the skin can be sufficiently moisturized even in a low humidity environment. This improves the function of generating moisturizing ingredients produced by the skin itself, and also improves the turnover disorder in the stratum corneum, so that it is considered that skin troubles such as rough skin are less likely to occur and the beauty effect is enhanced.
[0019] On the other hand, in a high humidity environment or when a large amount of sweat is produced, for example, as shown in Fig. 2, PVA molecules 203 near the outermost surface of the PVA film 201 also move around the moisture 205, so that gaps 207 that allow moisture to pass through are formed throughout the entire thickness of the film. As a result, under such circumstances, it is believed that excess moisture such as sweat can be evaporated from the skin, reducing the sticky discomfort. Furthermore, in a high humidity environment and when the skin is dry, it is believed that moisture in the environment can be provided to the skin through the PVA film 201.
[0020] As shown in FIG. 3, for example, when the PVA film 301 is thin and the skin has a high moisture content, gaps 307 that allow moisture to pass through may be formed even in a low humidity environment, and moisture from the skin may evaporate. In such a case, as shown in FIG. 4, by applying a waterproof and moisture-permeable layer 409 between the PVA film 401 and the skin, the formation of gaps 407 that allow moisture to pass through can be suppressed. Although the waterproof and moisture-permeable layer 409 has moisture permeability, it suppresses the movement of moisture from the exposed skin. Therefore, moisture 408 that passes through the waterproof and moisture-permeable layer 409 penetrates the PVA film 401 at a lower rate than when the waterproof and moisture-permeable layer 409 does not exist. Therefore, even in the above-mentioned case, gaps 407 that allow moisture to pass through due to the movement of PVA molecules 403 are not formed near the outermost surface of the PVA film 401, and it is believed that the skin can be moisturized and the beauty effect can be enhanced.
[0021] The definitions of terms used in this disclosure are as follows:
[0022] In the present disclosure, "humidity responsiveness" refers to the ability to change the amount of water evaporation in response to changes in the humidity environment, specifically, the ability to make the amount of water evaporation in a low humidity environment less than the amount of water evaporation in a high humidity environment.
[0023] In the present disclosure, a "low humidity environment" refers to an environment in which the relative humidity at atmospheric pressure and 23°C is 50% RH or less, 45% RH or less, 40% RH or less, 35% RH or less, or 30% RH or less. There is no particular restriction on the lower limit of the relative humidity, but it can be, for example, 3% RH or more, 5% RH or more, 7% RH or more, or 10% RH or more. In addition, the relative humidity can be converted into, for example, a weight absolute humidity that is not affected by temperature, and the weight absolute humidity can be 8.7 g / kg or less, 7.9 g / kg or less, 7.0 g / kg or less, 6.1 g / kg or less, or 5.2 g / kg or less, or 0.52 g / kg or more, 0.86 g / kg or more, 1.2 g / kg or more, or 1.7 g / kg or more.
[0024] In the present disclosure, a "high humidity environment" refers to an environment in which the relative humidity at atmospheric pressure and 28°C is 50% RH or more, 55% RH or more, 60% RH or more, 65% RH or more, 70% RH or more, or 75% RH or more. There is no particular limit to the upper limit of the relative humidity, but it can be, for example, 100% RH or less or less than 100% RH. In addition, the relative humidity can be converted into, for example, weight absolute humidity that is not affected by temperature, and the weight absolute humidity can be 12 g / kg or more, 13 g / kg or more, 14 g / kg or more, 15 g / kg or more, 17 g / kg or more, or 18 g / kg or more, and can be 24 g / kg or less or less than 24 g / kg.
[0025] In this disclosure, the term "film" includes not only films that can be carried alone, such as wrap films, but also thin films that cannot be carried alone, such as coating films. Here, in this disclosure, films that can be carried alone, such as wrap films, are sometimes referred to as "self-supporting films" and thin films that cannot be carried alone as "non-self-supporting films" to distinguish between them.
[0026] In the present disclosure, "beauty" or "beauty method" refers to applying the moisturizing polyvinyl alcohol film of the present disclosure to a body surface to beautify and smooth the condition of the body surface, or a method of beautifying and smoothing the condition of the body surface, and is different from methods of surgery, treatment, or diagnosis of humans.
[0027] In this disclosure, "body surface" means the skin surface of the body.
[0028] <Moisturizing polyvinyl alcohol film> The moisturizing polyvinyl alcohol film (sometimes simply referred to as a "polyvinyl alcohol film" or "PVA film") used in the cosmetic method of the present disclosure is a film that is humidity responsive. Such humidity responsiveness can be evaluated by the amount of moisture evaporation calculated by a moisture evaporation test. Here, the amount of moisture evaporation is sometimes called the moisture evaporation rate. In addition, since the moisturizing polyvinyl alcohol film can exert a cosmetic effect, a composition including such a moisturizing polyvinyl alcohol film may be called a "moisturizing film cosmetic" or simply a "cosmetic".
[0029] Evaluation method 1 As shown in FIG. 5, the amount of water evaporation can be calculated by covering the open part of a vial containing 20 mL of water with a measurement sample such as PVA film, leaving it to stand in a low humidity environment, for example, at 23°C and 40% RH, until it reaches an equilibrium state where the amount of evaporation is approximately constant over time, and then measuring the amount of water loss and calculating the amount of water loss per unit area and unit time.
[0030] The polyvinyl alcohol film of the present disclosure can exhibit humidity responsiveness, when evaluated in a moisture evaporation test using the amount of moisture evaporation, such that, for example, the amount of moisture evaporation measured in a low humidity environment of 23° C. and 40% RH is less than the amount of moisture evaporation measured in a high humidity environment of 28° C. and 70% RH. In contrast, in an open system or in a vial container covered with filter paper, the amount of moisture evaporation measured in a low humidity environment of 23° C. and 40% RH is greater than the amount of moisture evaporation measured in a high humidity environment of 28° C. and 70% RH.
[0031] Specifically, in the polyvinyl alcohol film of the present disclosure, the amount of water evaporation measured in a low humidity environment of 23°C and 40% RH is 0.20 mg / cm lower than the amount of water evaporation measured in a high humidity environment of 28°C and 70% RH. 2 / h or more, 0.25mg / cm 2 / h or more, 0.30mg / cm 2 / h or more, 0.40mg / cm 2 / h or more, 0.45mg / cm 2 / h or more, or 0.50 mg / cm 2 / h or more, and the upper limit is 1.3 mg / cm 2 / h or less, 1.2mg / cm 2 / h or less, 1.0mg / cm 2 / h or less, or 0.95 mg / cm 2 / h or less.
[0032] In addition, when the measurement environment is, for example, an environment with a lower humidity than an environment of 23°C and 40% RH, the polyvinyl alcohol film of the present disclosure can further suppress the evaporation of moisture. Therefore, the difference between the amount of evaporated moisture and the evaporation rate of moisture described later tends to increase as the difference in the humidity environment of the measurement environment increases.
[0033] Evaluation method 2 Humidity responsiveness can also be evaluated using the water evaporation rate (%) calculated as follows. First, an open vial containing 20 mL of water is left to stand in a low humidity environment of, for example, 23°C and 40% RH until the amount of evaporation is approximately constant over time and reaches equilibrium, and then the amount of water lost is measured, and the amount of water evaporation 1, which is the amount of water lost per unit area and unit time, is calculated. Next, as shown in FIG. 5, the open part of another vial containing 20 mL of water is covered with a measurement sample such as a PVA film, and left to stand in the same environment until it reaches equilibrium, and then the amount of water lost is measured, and the amount of water evaporation 2, which is the amount of water lost per unit area and unit time, is calculated. Then, the ratio of the amount of water evaporation 2 to the amount of water evaporation 1 is calculated as a percentage to calculate the water evaporation rate.
[0034] The polyvinyl alcohol film of the present disclosure can exhibit humidity responsiveness, when evaluated in a moisture evaporation test using a moisture evaporation rate, such that, for example, the moisture evaporation rate measured in a low humidity environment of 23° C. and 40% RH is less than the moisture evaporation rate measured in a high humidity environment of 28° C. and 70% RH. In contrast, in an open system or a vial container capped with filter paper, the amount of moisture evaporation measured in a low humidity environment of 23° C. and 40% RH is greater than the amount of moisture evaporation measured in a high humidity environment of 28° C. and 70% RH.
[0035] Specifically, in the polyvinyl alcohol film of the present disclosure, the moisture evaporation rate when measured in a low humidity environment of 23°C and 40% RH can be 2.0% or more, 2.5% or more, 3.0% or more, 3.5% or more, or 4.0% or more lower than the moisture evaporation rate when measured in a high humidity environment of 28°C and 70% RH, and the upper limit can be 10% or less, 9.5% or less, 9.0% or less, or 8.5% or less.
[0036] From the viewpoint of reducing or suppressing evaporation of moisture in a low humidity environment, the polyvinyl alcohol film is preferably a film in which openings are not always formed over the entire surface, rather than a film in which openings are always formed over the entire surface in order to impart moisture permeability, such as a nonwoven fabric or a film physically provided with through-holes. However, the polyvinyl alcohol film of the present disclosure may have through-holes partially formed in the film, for example, in order to improve air retention when the film is applied, as long as it can exhibit the above-mentioned humidity responsiveness.
[0037] <material> The material constituting the polyvinyl alcohol film of the present disclosure is not particularly limited as long as the resulting film exhibits humidity responsiveness, and polyvinyl alcohol or its derivatives can be used alone or in combination of two or more. Examples of polyvinyl alcohol derivatives include modified polyvinyl alcohol, polyvinyl acetate, polyvinyl butyral, etc. In addition, from the viewpoint of humidity responsiveness, it is preferable that such a film is composed of unmodified polyvinyl alcohol and / or modified polyvinyl alcohol.
[0038] The polyvinyl alcohol can be prepared, for example, using a fully saponified polyvinyl alcohol having a saponification degree of 99% or more, a partially saponified polyvinyl alcohol having a saponification degree of 90% or more but less than 99%, or a partially saponified polyvinyl alcohol having a saponification degree of 70% or more but less than 90%. These polyvinyl alcohols can be used alone or in combination of two or more. Among them, from the viewpoint of humidity responsiveness, particularly the effect of suppressing water evaporation in a low humidity environment, fully saponified polyvinyl alcohol and partially saponified polyvinyl alcohol are preferred, and fully saponified polyvinyl alcohol is more preferred. Examples of the modification treatment of polyvinyl alcohol include diol modification, anion modification, and cation modification.
[0039] From the viewpoint of humidity responsiveness, particularly the effect of suppressing water evaporation in a low humidity environment, unmodified polyvinyl alcohol or diol-modified polyvinyl alcohol is preferred, and unmodified polyvinyl alcohol is more preferred.
[0040] Such polyvinyl alcohol may be a commercially available product. Examples of unmodified fully saponified polyvinyl alcohol include Gohsenol (trademark) NL-05 (manufactured by Mitsubishi Chemical Corporation), KURARAY POVAL (trademark) PVA-117H (manufactured by Kuraray Co., Ltd.), and KURARAY POVAL (trademark) PVA-124 (manufactured by Kuraray Co., Ltd.). Examples of anion-modified fully saponified polyvinyl alcohol include Gohsenex (trademark) T-330H (manufactured by Mitsubishi Chemical Corporation). Examples of diol-modified fully saponified polyvinyl alcohol include Nichigo G Polymer (trademark) OKS-1089 and Nichigo G Polymer (trademark) OKS-1109 (both manufactured by Mitsubishi Chemical Corporation).
[0041] An example of an unmodified partially saponified polyvinyl alcohol is KURARAY POVAL (trademark) PVA-617 (manufactured by Kuraray Co., Ltd.), and an example of a diol-modified partially saponified polyvinyl alcohol is Nichigo G Polymer (trademark) OKS-8096 (manufactured by Mitsubishi Chemical Corporation).
[0042] Examples of unmodified partially saponified polyvinyl alcohol include GOHSENOL (trademark) GM-14, GOHSENOL (trademark) PVA EG-05, GOHSENOL (trademark) PVA EG-40 (all manufactured by Mitsubishi Chemical Corporation), and KURARAY POVAL (trademark) PVA-235 (manufactured by Kuraray Co., Ltd.). Examples of cation-modified partially saponified polyvinyl alcohol include GOHSENOL (trademark) PVA K-434 (manufactured by Mitsubishi Chemical Corporation).
[0043] <Thickness> The thickness of the polyvinyl alcohol film is not particularly limited, and can be appropriately adjusted depending on the part to which the polyvinyl alcohol film is applied, the purpose of use, the amount of sweat glands or the amount of moisture evaporation from the skin of the user, or the balance of humidity responsiveness when combined with a waterproof and moisture-permeable layer described below, etc. For example, the thickness of the polyvinyl alcohol film can be 100 μm or less, 70 μm or less, 50 μm or less, 20 μm or less, 15 μm or less, 13 μm or less, 10 μm or less, 7 μm or less, 5 μm or less, 3 μm or less, 1 μm or less, or 0.5 μm or less, and can be 0.01 μm or more, 0.05 μm or more, 0.1 μm or more, 0.2 μm or more, or 0.3 μm or more. In particular, when used in combination with a waterproof and moisture-permeable layer described later, the thickness of the polyvinyl alcohol film can be as thin as 15 μm or less, 13 μm or less, 10 μm or less, 7 μm or less, 5 μm or less, 3 μm or less, 1 μm or less, 0.7 μm or less, or 0.5 μm or less, and can be 0.01 μm or more, 0.05 μm or more, 0.1 μm or more, 0.2 μm or more, or 0.3 μm or more.
[0044] When the polyvinyl alcohol film is a free-standing film, the thickness of the polyvinyl alcohol film can be defined as the average value calculated by measuring the thickness of any part of the film at least five times using a high-precision digital micrometer (MDH-25MB, manufactured by Mitutoyo Corporation). When the thickness of the polyvinyl alcohol film is too thin to be measured with a high-precision digital micrometer, the thickness of the polyvinyl alcohol film can be determined by a similar method using a scanning electron microscope as described below.
[0045] When the polyvinyl alcohol film is combined with a waterproof / moisture-permeable layer (described later) to form a laminate and the waterproof / moisture-permeable layer cannot be separated from the laminate, a scanning electron microscope is used to measure the thickness direction cross section of the laminate. The average thickness of at least five arbitrary points on the polyvinyl alcohol film in the laminate can be defined as the thickness of the polyvinyl alcohol film.
[0046] <Basic weight> The polyvinyl alcohol film may be specified by basis weight instead of thickness. Here, basis weight in this disclosure is the weight per 1 cm of the film. 2 The basis weight of a polyvinyl alcohol film is, for example, 0.0010 mg / cm. 2 More than 0.0060mg / cm 2 More than 0.010mg / cm 2 More than 0.025mg / cm 2 More than 0.035mg / cm 2 More than 0.050mg / cm 2 More than 0.070mg / cm 2 More than 0.10mg / cm 2 More than 0.15mg / cm 2 More than 0.30mg / cm 2 or more than 0.45 mg / cm 2 and 12.0 mg / cm or more. 2 Below, 8.5mg / cm 2 Below, 6.0mg / cm 2 Below, 4.5mg / cm 2 Below 2.5mg / cm 2 Below 2.0mg / cm 2 Below 1.5mg / cm 2 Below, 1.2mg / cm 2 Below 1.0mg / cm 2 Below 0.80mg / cm 2 Below, 0.60mg / cm 2 Below, 0.35mg / cm 2 Below, 0.15mg / cm 2 Below, 0.10mg / cm 2 Below, 0.085mg / cm 2 or less than 0.060 mg / cm 2 It can be as follows:
[0047] <Optional ingredients> Various components can be appropriately blended into the polyvinyl alcohol film of the present disclosure as long as they do not affect the effects of the present invention. Examples of the various components include moisturizers, polymers (e.g., carboxyvinyl polymers, (N,N-dimethylacrylamide-2-acrylamidodimethylpropanesulfonic acid) crosslinked copolymers, copolymers of 2-methacryloyloxyphosphorylcholine (MPC) and n-butyl methacrylate (BMA), rubbers, elastomers, pressure sensitive adhesives, adhesives, adhesion modifiers, adhesion modifiers, UV absorbers, antioxidants, preservatives, antioxidant assistants, crosslinking agents, light diffusing agents, fillers, skin nutrients, vitamins, pharmaceuticals, quasi-drugs, various drugs applicable to cosmetics, etc., organic powders, pigments, dyes, colorings, and fragrances. These optional components can be used alone or in combination of two or more. Here, glycerin, which is a moisturizer, may increase moisture permeability in a low humidity environment, so that moisturizers other than glycerin, such as dipropylene glycol, POE(14)POP(7)dimethyl ether, etc., are preferred. Here, POE means polyoxyethylene, and POP means polyoxypropylene.
[0048] Waterproof and breathable layer The waterproof / moisture-permeable layer used in the cosmetic method of the present disclosure is a layer that has waterproof properties and moisture permeability, and does not exhibit humidity responsiveness by itself.
[0049] As shown in Fig. 3, for example, when polyvinyl alcohol film 301 is thin and the skin has a high moisture content, gaps 307 that allow moisture to pass through may be formed even in a low humidity environment, causing moisture to evaporate from the skin. In such a case, as shown in Fig. 4, by applying a waterproof moisture-permeable layer 409 between polyvinyl alcohol film 401 and the skin, the formation of gaps 407 that allow moisture to pass through can be suppressed, and moisture retention can be ensured.
[0050] In addition, as the polyvinyl alcohol film becomes thicker, its rigidity increases, which may make it difficult to apply to the skin and may also make the appearance worse. Even if the waterproof / moisture-permeable layer is relatively thin, when combined with the polyvinyl alcohol film, the laminate containing them can provide sufficient humidity responsiveness similar to the humidity responsiveness performance of the polyvinyl alcohol film described above, so that the overall thickness can be reduced. As a result, the laminate having such a configuration can improve the applicability to the skin and the appearance compared to the case where a thick polyvinyl alcohol film is used.
[0051] Since the surface of the polyvinyl alcohol film opposite to the body surface side is used to adjust the moisture permeability to the external environment, it is preferable that no waterproof moisture permeable layer or any additional layer is formed on this surface. Therefore, when a waterproof moisture permeable layer is applied to the polyvinyl alcohol film in advance for use, it is preferable that the waterproof moisture permeable layer is configured to be disposed closer to the body surface side than the polyvinyl alcohol film.
[0052] The waterproof and moisture-permeable layer may be a single layer or a laminate. The waterproof and moisture-permeable layer may be in the form of a free-standing or non-free-standing film. The waterproof and moisture-permeable layer may be configured to be applied to the entire surface or a part of the polyvinyl alcohol film.
[0053] <material> The waterproof and moisture-permeable layer is not particularly limited as long as it is a layer that can exhibit the above-mentioned humidity responsiveness when combined with the polyvinyl alcohol film. Examples of the waterproof and moisture-permeable layer include at least one selected from an oil layer, a polylactic acid layer, and an artificial skin.
[0054] Examples of materials for the oil layer include polar oils such as ester oils, and non-polar oils such as hydrocarbon oils. Among these, non-polar oils are preferred from the viewpoint of humidity responsiveness.
[0055] Examples of non-polar oils include petrolatum, liquid paraffin, tetraisobutane, hydrogenated polydecene, olefin oligomer, isododecane, isohexadecane, squalane, polybutene, hydrogenated polybutene, polyisobutene, hydrogenated polyisobutene, etc. These can be used alone or in combination of two or more. Among them, petrolatum and liquid paraffin are preferred from the viewpoint of humidity responsiveness.
[0056] Examples of materials that can be used to form the artificial skin include rubbers or elastomers such as urethane rubber, olefin rubber, silicone rubber, acrylic rubber, and natural rubber, as well as α-gel. These can be used alone or in combination of two or more. Among these, silicone rubber is preferred from the viewpoints of flexibility, humidity responsiveness, and the like.
[0057] <Thickness> The thickness of the waterproof and moisture-permeable layer is not particularly limited, and can be appropriately adjusted depending on the area to which the waterproof and moisture-permeable layer is applied, the purpose of use, the amount of sweat glands or the amount of moisture evaporated from the skin of the user, the balance of humidity responsiveness when combined with the above-mentioned polyvinyl alcohol film, and the like.
[0058] <Basic weight> The waterproof and moisture-permeable layer can be specified, for example, by basis weight. The basis weight of the waterproof and moisture-permeable layer is, for example, 1.0 mg / cm 2 More than 1.2mg / cm 2 or more than 1.4 mg / cm 2 and 2.0 mg / cm or more. 2 Below 1.8mg / cm 2 or less than 1.6 mg / cm 2 It can be as follows:
[0059] <Optional ingredients> The waterproof and moisture-permeable layer of the present disclosure may be appropriately blended with various components within a range that does not affect the effects of the present invention. Examples of the various components include moisturizers, polymers, rubbers, elastomers, pressure-sensitive adhesives, adhesives, adhesion modifiers, adhesion modifiers, UV absorbers, antioxidants, preservatives, antioxidant assistants, light diffusing agents, fillers, skin nutrients, vitamins, various drugs applicable to medicines, quasi-drugs, cosmetics, etc., organic powders, pigments, dyes, colorants, and fragrances. These optional components may be used alone or in combination of two or more.
[0060] 《Optional composition layer》 The moisture-retaining polyvinyl alcohol film of the present disclosure can be used in combination with any constituent layer within a range that does not affect the effects of the present invention. Examples of such constituent layers include a moisture-permeable adhesive layer (e.g., an adhesive layer having through holes), a protective film having peeling properties, and a release sheet, which can be used alone or in combination of two or more. For example, a protective film can be applied to one side of the polyvinyl alcohol film, and / or a release sheet can be applied to the opposite side. Here, the surface of the protective film and the release sheet may be subjected to a release treatment such as silicone. In addition, the release performance of the protective film and the release sheet against the polyvinyl alcohol film may be the same or different. From the viewpoint of ease of peeling from the polyvinyl alcohol film, it is preferable that these release performances are different.
[0061] The material of the optional constituent layer is not particularly limited, but from the viewpoint of handling, examples of the material include polyolefins such as polyethylene and polypropylene, polyesters such as polyethylene terephthalate, cotton, paper, etc. The optional constituent layer may be in the form of a film, or in the form of a nonwoven fabric, knitted fabric, woven fabric, etc.
[0062] <<Beauty treatment using moisturizing polyvinyl alcohol film>> The cosmetic method of the present disclosure is carried out by applying a moisturizing polyvinyl alcohol film to the body surface. The moisturizing polyvinyl alcohol film applied to the skin can reduce or inhibit evaporation of moisture from the skin in a low humidity environment, and can sufficiently moisturize the skin even in a low humidity environment. As a result, the function of producing moisturizing components produced by the skin itself is improved, and the turnover disorder in the stratum corneum is also improved, so that skin troubles such as rough skin are less likely to occur, and the cosmetic effect can be improved.
[0063] The means for applying the polyvinyl alcohol film to a body surface is not particularly limited. For example, the polyvinyl alcohol film may be attached to the body surface in the form of a free-standing film, or the polyvinyl alcohol film-making composition described below may be applied to the body surface.
[0064] As a means for attaching the polyvinyl alcohol film to the body surface in the form of a self-supporting film, for example, when the polyvinyl alcohol film has a moisture-permeable adhesive layer, the polyvinyl alcohol film can be attached to the body surface via the adhesive layer. Alternatively, since the polyvinyl alcohol film becomes adhesive when it comes into contact with water, the film may be attached to the body surface part to which the film is to be applied after applying water or lotion, or the polyvinyl alcohol film may be applied to the body surface after spreading water or lotion.
[0065] The composition for producing a polyvinyl alcohol film may be applied to the body surface, for example, by spraying the composition from a spray container so as to form a film, or by pouring the composition into a container without a spray function, taking an appropriate amount of the composition from the container onto a finger or the like, and spreading it over the body surface.
[0066] The application of the polyvinyl alcohol film to the body surface may be carried out after the waterproof and moisture-permeable layer is applied to the body surface. In this case, the application of the waterproof and moisture-permeable layer to the body surface may be carried out, for example, by attaching it in the form of a free-standing film, or by applying the waterproof and moisture-permeable layer components to the body surface. Here, the application of the polyvinyl alcohol film to the waterproof and moisture-permeable layer may be carried out in the same manner as the application of the polyvinyl alcohol film to the body surface, or, if the waterproof and moisture-permeable layer itself has adhesiveness, the polyvinyl alcohol film may be attached by utilizing the adhesiveness.
[0067] As a means for attaching the waterproof / moisture-permeable layer to the body surface in the form of a self-supporting film, for example, if the waterproof / moisture-permeable layer itself has adhesiveness, the waterproof / moisture-permeable layer in such a form can be attached to the body surface as is. If the waterproof / moisture-permeable layer itself does not have adhesiveness, for example, the waterproof / moisture-permeable layer in such a form can be attached to the body surface via an adhesive layer having moisture permeability or another waterproof / moisture-permeable layer having adhesiveness.
[0068] The waterproof and moisture-permeable layer components can be applied to the body surface by preparing a composition containing the various components that make up the waterproof and moisture-permeable layer, and applying the composition in the same manner as in the case of the composition for producing the polyvinyl alcohol film described above.
[0069] The application of the polyvinyl alcohol film to the body surface may be performed by applying a waterproof and moisture-permeable layer to one side of the polyvinyl alcohol film, and then applying the polyvinyl alcohol film to the body surface via the waterproof and moisture-permeable layer. Here, when the waterproof and moisture-permeable layer itself has adhesiveness, the waterproof and moisture-permeable layer can be applied to the polyvinyl alcohol film by utilizing its adhesiveness. In addition, when the waterproof and moisture-permeable layer does not have adhesiveness, the waterproof and moisture-permeable layer can be applied to the polyvinyl alcohol film via a moisture-permeable adhesive layer or another waterproof and moisture-permeable layer having adhesiveness. In this case, a moisture-permeable adhesive layer or another waterproof and moisture-permeable layer having adhesiveness is also applied to the body surface side of the waterproof and moisture-permeable layer, or a moisture-permeable adhesive layer or another waterproof and moisture-permeable layer having adhesiveness is applied to the body surface, so that the polyvinyl alcohol film having a non-adhesive waterproof and moisture-permeable layer can be applied to the body surface.
[0070] <Areas to which moisturizing polyvinyl alcohol film should be applied> The polyvinyl alcohol film for moisturizing can be applied to any part of the skin surface of the body, that is, any part of the body surface. For example, it can be applied appropriately to the skin surface of the face (lips, eyes, nose, cheeks, forehead, etc.), neck, ears, hands, arms, legs, feet, chest, abdomen, back, etc. Here, the skin also includes nails that have hardened due to changes in the keratin of the epidermis of the skin.
[0071] <<Method for producing a moisture-retaining polyvinyl alcohol film>> The moisturizing polyvinyl alcohol film of the present disclosure can be produced, for example, by using a commercially available polyvinyl alcohol film of a predetermined thickness, or by using a composition for producing a polyvinyl alcohol film.
[0072] In a production method using a composition for producing a polyvinyl alcohol film, for example, the composition can be applied onto a release sheet by any means, for example, a known coating means such as offset printing, gravure coating, bar coating, knife coating, spray coating, etc., and the film can be continuously prepared by optionally applying, for example, a drying step, a crosslinking step, a step of applying a waterproof and moisture-permeable layer, a step of laminating constituent layers such as a protective film, a winding step, etc.
[0073] The moisturizing polyvinyl alcohol film of the present disclosure can also be prepared discontinuously using a composition for preparing a polyvinyl alcohol film. For example, a predetermined amount of such a composition may be added to a container or a mold, and dried to prepare a polyvinyl alcohol film. At this time, for example, a waterproof moisture-permeable layer, a protective film, a release sheet, etc. may be applied to the obtained polyvinyl alcohol film as necessary. Alternatively, the composition may be poured into, for example, a tube container, a spray container, etc., and the composition may be applied to a body surface from such a container, or the composition may be applied to a waterproof moisture-permeable layer previously applied to the body surface and dried to directly form a polyvinyl alcohol film on the body surface.
[0074] The size and shape of the moisture retaining polyvinyl alcohol film or a laminate including the film can be appropriately adjusted using known cutting means such as half cutting or laser cutting depending on the area to be applied.
[0075] <Polyvinyl alcohol film preparation composition> The polyvinyl alcohol film for moisture retention of the present disclosure can be prepared using a composition for preparing a polyvinyl alcohol film. Such a composition can be prepared by appropriately mixing the above-mentioned polyvinyl alcohol, water, and the following optional components.
[0076] (optional ingredient) The composition for preparing the polyvinyl alcohol film of the present disclosure can be appropriately blended with various components within a range that does not affect the effects of the present invention. Examples of various components include lower alcohols, polyhydric alcohols, higher alcohols, oils, various extracts, anionic surfactants, cationic surfactants, amphoteric surfactants, nonionic surfactants, moisturizing agents, polymers, rubbers, elastomers, pressure sensitive adhesives, adhesives, adhesion modifiers, adhesion modifiers, UV absorbers, antioxidants, preservatives, antioxidant assistants, crosslinking agents, light diffusing agents, fillers, gelling agents (thickeners), skin nutrients, vitamins, various drugs applicable to medicines, quasi-drugs, cosmetics, etc., organic powders, pigments, dyes, colorants, and fragrances. These optional components can be used alone or in combination of two or more.
[0077] Cosmetic kit The moisturizing polyvinyl alcohol film of the present disclosure can be provided in the form of a cosmetic kit including a polyvinyl alcohol film or a composition for producing the polyvinyl alcohol film.
[0078] <Optional parts> The cosmetic kit may further include optional components. Examples of such optional components include the above-mentioned components to which the waterproof / moisture-permeable layer can be applied, a cutter, scissors, a mirror, etc. These optional components may be provided in the cosmetic kit alone or in combination of two or more. EXAMPLES
[0079] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0080] Examples 1 to 3 and Comparative Examples 1 to 2 The polyvinyl alcohol (PVA) films obtained by the manufacturing methods described in Examples 1 to 3, as well as the filter paper (Comparative Example 1) and polylactic acid film (Comparative Example 2) used for comparison, were evaluated for humidity responsiveness by the moisture evaporation test shown below. The results are shown in Table 1 and Figure 6. As a reference example, the results of the open system sample are shown in Table 1.
[0081] <Water Evaporation Test> The circular opening (radius: 0.7 cm, area: 1.54 cm) of a vial containing 20 mL of water 2 ) was capped with each measurement sample, and the vial was placed in a thermostatic chamber under the specified temperature and humidity conditions. After leaving it for about 2 to 3 days until the amount of evaporation was equilibrated with time, the amount of water lost in the vial was measured, and the amount of water evaporation, which is the amount of water lost per unit area and unit time, was calculated. Here, the test was carried out in two environments: a low humidity environment of 23°C and 40% RH, and a high humidity environment of 28°C and 70% RH.
[0082] Example 1 A composition for producing a polyvinyl alcohol film was prepared by mixing unmodified fully saponified polyvinyl alcohol, KURARAY POVAL™ PVA-117H (manufactured by Kuraray Co., Ltd.), which is a polyvinyl alcohol, in a 10 mL vial and stirring the mixture so that the polyvinyl alcohol concentration was 5.0% by mass. The resulting 5.0% by mass aqueous solution of the composition was then poured into a 19.6 cm2 film. 2 3.0 g of the mixture was added to a roughly circular petri dish and dried to obtain a measurement sample with a thickness of approximately 60 μm and a basis weight of approximately 7.6 mg / cm. 2 A polyvinyl alcohol film was prepared.
[0083] Example 2 A polyvinyl alcohol film as a measurement sample was prepared in the same manner as in Example 1, except that the concentration of polyvinyl alcohol was changed to 1.0 mass %. The thickness of the obtained film was about 10 μm, and the basis weight was about 1.5 mg / cm 2 It was.
[0084] Example 3 A polyvinyl alcohol film as a measurement sample was prepared in the same manner as in Example 1, except that the concentration of polyvinyl alcohol was changed to 0.5% by mass. The thickness of the obtained film was about 6 μm, and the basis weight was about 0.76 mg / cm 2 It was.
[0085] Comparative Example 1 Thickness 250μm, basis weight 14mg / cm 2 Filter paper #133 manufactured by ADVANTEC was used as a measurement sample in Comparative Example 1.
[0086] Comparative Example 2 A 0.1% by mass solution of polylactic acid prepared using tetrahydrofuran was used to spin coat a film with a thickness of approximately 200 nm and a basis weight of approximately 0.025 mg / cm. 2 A polylactic acid film having the above formula was prepared. Two of these polylactic acid films were stacked together and used as a measurement sample for Comparative Example 2.
[0087] <Reference example 1> As a reference example, an open sample was used in which the open part of the vial was not capped.
[0088] [Table 1]
[0089] <result> 6, in the case of the filter paper of Comparative Example 1 and the polylactic acid film of Comparative Example 2, the amount of water evaporation was greater in a low humidity environment than in a high humidity environment, and no humidity responsiveness was observed. On the other hand, in the case of the polyvinyl alcohol films of Examples 1 to 3, the amount of water evaporation in a low humidity environment was clearly lower than the amount of water evaporation in a high humidity environment, and it was confirmed that the films exhibited humidity responsiveness.
[0090] Examples 4 and 5 and Comparative Example 3 The amount of water evaporation from human skin was evaluated, and the results are summarized in Table 2. Here, the amount of water evaporation was measured using a VAPO METER manufactured by Keystone Corporation in two environments: a low humidity environment of 23°C and 40% RH, and a high humidity environment of 28°C and 70% RH.
[0091] Example 4 The polyvinyl alcohol film (thickness: about 10 μm) obtained in Example 2 was attached to the skin surface on the inside of a human left arm.
[0092] Example 5 Vaseline (Sunwhite P-1, manufactured by Nikko Rica Corporation) was applied at a dose of approximately 1.5 mg / cm to the skin surface of the inside of the left arm of a human. 2 The waterproof / moisture-permeable layer was formed by coating in a ratio of 10 μm to 200 μm, and the polyvinyl alcohol film (thickness: about 10 μm) obtained in Example 2 was laminated thereon.
[0093] Comparative Example 3 The amount of water lost from bare skin was measured.
[0094] [Table 2]
[0095] <result> As is clear from Table 2, the amount of moisture evaporation from the bare skin itself was greater in a low humidity environment than in a high humidity environment. On the other hand, in the case of Examples 4 and 5 in which the polyvinyl alcohol film was applied, no sticky discomfort was observed in a high humidity environment, and the amount of moisture evaporation in a low humidity environment was suppressed to be lower than that in a high humidity environment, and it was confirmed that the moisturizing performance of the skin in a low humidity environment can be improved. In addition, in a high humidity environment, the amount of moisture evaporation from the bare skin in Example 4 was greater than that in Comparative Example 3. This is thought to be due to the fact that the measurement site of the bare skin in Comparative Example 3 was different from the site where the PVA film in Example 4 was applied to the bare skin, that is, the amount of moisture evaporation from the bare skin at each measurement site was different. [Explanation of symbols]
[0096] 100, 200, 300, 400 Moisturizing film cosmetic 101, 201, 301, 401 Polyvinyl alcohol film 103, 203, 303, 403 Polyvinyl alcohol molecule 105, 205, 305, 405 Moisture 107, 207, 307, 407 Moisture-permeable gaps 408 Water passing through waterproof / breathable layer 409 Waterproof and breathable layer
Claims
1. A cosmetic method (excluding medical procedures) in which a waterproof / moisture-permeable layer is applied to a body surface, and then a moisturizing polyvinyl alcohol film is applied to the body surface, or a cosmetic method (excluding medical procedures) in which a waterproof / moisture-permeable layer is applied to one side of a moisturizing polyvinyl alcohol film, and then the moisturizing polyvinyl alcohol film is applied to the body surface via the waterproof / moisture-permeable layer, The waterproof and moisture-permeable layer is at least one selected from an oil layer, a polylactic acid layer, and an artificial skin, When a laminate including the moisture-retaining polyvinyl alcohol film and the waterproof / moisture-permeable layer is evaluated in a moisture evaporation test, the amount of moisture evaporation measured in an environment of 23° C. and 40% RH is less than the amount of moisture evaporation measured in an environment of 28° C. and 70% RH. Beauty method.
2. A cosmetic method (excluding medical procedures) in which a waterproof and moisture-permeable layer is applied to a body surface, and then a moisturizing polyvinyl alcohol film is applied to the body surface, The waterproof and moisture-permeable layer is at least one selected from an oil layer, a polylactic acid layer, and an artificial skin, When a laminate including the moisture-retaining polyvinyl alcohol film and the waterproof / moisture-permeable layer is evaluated in a moisture evaporation test, the amount of moisture evaporation measured in an environment of 23° C. and 40% RH is less than the amount of moisture evaporation measured in an environment of 28° C. and 70% RH. Beauty method.
3. The thickness of the moisture-retaining polyvinyl alcohol film is 100 μm or less. The cosmetic method according to claim 1 or 2.
4. The thickness of the moisture-retaining polyvinyl alcohol film is 10 μm or less. The cosmetic method according to claim 3.
5. When the moisture-retaining polyvinyl alcohol film is evaluated in a moisture evaporation test, the moisture evaporation amount measured in an environment of 23° C. and 40% RH is less than the moisture evaporation amount measured in an environment of 28° C. and 70% RH. The cosmetic method according to any one of claims 1 to 4.
6. The waterproof and moisture-permeable layer is the oil layer, and the oil layer contains at least one of Vaseline and liquid paraffin. The cosmetic method according to any one of claims 1 to 5.
7. The waterproof and moisture-permeable layer is at least one selected from a polylactic acid layer and an artificial skin. The cosmetic method according to any one of claims 1 to 5.
8. The application of the moisturizing polyvinyl alcohol film to the body surface is carried out by attaching it in the form of a self-supporting film; The cosmetic method according to any one of claims 1 to 7.
9. The application of the moisturizing polyvinyl alcohol film to a body surface is carried out by applying a composition containing polyvinyl alcohol and water to the body surface. The cosmetic method according to any one of claims 1 to 7.
10. The moisture-retaining polyvinyl alcohol film contains unmodified polyvinyl alcohol. The cosmetic method according to any one of claims 1 to 9.
11. The thickness of the moisture-retaining polyvinyl alcohol film is 7 μm or less. The cosmetic method according to any one of claims 1 to 10.
12. A cosmetic method (excluding medical procedures) in which a waterproof and moisture-permeable layer is applied to a body surface, and then a moisturizing polyvinyl alcohol film is applied to the body surface, the application of the moisture-retaining polyvinyl alcohol film to a body surface is carried out by applying a composition containing polyvinyl alcohol and water to the body surface; The application of the waterproof and moisture-permeable layer to the body surface is carried out by attaching it in the form of a free-standing film, The waterproof and moisture-permeable layer is at least one selected from an oil layer, a polylactic acid layer, and an artificial skin. Beauty method.
13. A cosmetic method (excluding medical procedures) in which a waterproof and moisture-permeable layer is applied to a body surface, and then a moisturizing polyvinyl alcohol film is applied to the body surface, the application of the moisture-retaining polyvinyl alcohol film to a body surface is carried out by applying a composition containing polyvinyl alcohol and water to the body surface; The application of the waterproof and moisture-permeable layer to the body surface is carried out by applying a waterproof and moisture-permeable layer component to the body surface, The waterproof and moisture-permeable layer is at least one selected from an oil layer, a polylactic acid layer, and an artificial skin. Beauty method.
14. A polyvinyl alcohol film for use in the cosmetic method according to any one of claims 1 to 13, or A composition for producing the polyvinyl alcohol film, A member to which a waterproof / moisture-permeable layer can be applied, the waterproof / moisture-permeable layer being at least one selected from an oil layer, a polylactic acid layer, and an artificial skin; A cosmetic kit comprising:
15. A polyvinyl alcohol film; A waterproof and moisture-permeable layer disposed on one side of the polyvinyl alcohol film; A cosmetic kit comprising: The waterproof and moisture-permeable layer is at least one selected from an oil layer, a polylactic acid layer, and an artificial skin, When the laminate including the polyvinyl alcohol film and the waterproof moisture-permeable layer is evaluated in a moisture evaporation test, the moisture evaporation amount measured in an environment of 23°C and 40% RH is less than the moisture evaporation amount measured in an environment of 28°C and 70% RH. Cosmetic kit.
16. Further comprising a component layer used in combination with the polyvinyl alcohol film, The constituent layer has a pressure-sensitive adhesive layer having through holes, The cosmetic kit according to claim 15.
Citation Information
Patent Citations
Skin-simulating function film and preparation method thereof
CN103251511A
Quartery nitrogen modified polyvinyl alcohol polymer
JP1985133008A
Skin external preparation
JP1991005411A
Emulsion composition, emulsion cosmetic, medicine and antiallergic agent containing the same
JP2002308729A
Pack cosmetic
JP2006131616A