Method for evaluating the coating state of a protein adsorbent or the adsorption state of a protein
A method using fluorescent dyes and protein detection reagents allows for the non-destructive evaluation of protein adsorbent coating uniformity on complex cell culture substrates, addressing the challenge of assessing coating uniformity on diverse cell culture substrates.
Patent Information
- Application Number
- JP2022507617
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-09-20
- Filing Date
- 2020-09-11
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2040-09-11
AI Technical Summary
It is difficult to confirm the uniform coating of protein adsorbents on cell culture substrates with complex structures using non-destructive testing methods.
A method involving the combination of a fluorescent dye and a protein detection reagent with a polymer base material, where the coating state is evaluated by irradiating the material with light to detect the coloring state, allowing for visualization of the protein adsorbent coating on complex structures.
Enables the non-destructive evaluation of protein adsorbent coating and protein adsorption states on polymer base materials with complex structures, facilitating easy visualization and assessment of uniformity.
Smart Images

Figure 0007595066000008 
Figure 0007595066000009 
Figure 0007595066000010
Abstract
Description
[Technical field]
[0001] Technical Field The present invention relates to a method for evaluating the coating state of a protein adsorbent or the adsorption state of a protein. [Background technology]
[0002] background In recent years, cell culture techniques have been used in the development of regenerative medicine and drug discovery. In particular, the use of stem cells has attracted attention, and techniques to repair and replace damaged or defective tissues by using stem cells proliferated from donor cells are being actively researched. Most cells in animals, including humans, cannot survive in a suspended state, but are adhesive (anchorage-dependent) cells that survive while attached to something. For this reason, adhesive (anchorage-dependent) cells are cultured at high density to obtain cultured tissues similar to living tissues. For this purpose, cell culture substrates are coated with protein adsorbents (cell adhesion factors) such as fibronectin, collagen, and laminin.
[0003] Meanwhile, the structures of cell culture substrates (cell culture vessels) are becoming increasingly diversified, including not only the conventional flat dish (plate) structure but also hollow fiber structures (for example, Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Special Publication No. 2018-519800 Summary of the Invention
[0005] Summary of the Invention For culture vessels with such diverse and complicated structures, it is difficult or impossible to confirm by non-destructive testing whether the desired protein adsorbent has been uniformly coated on the cell culture substrate.
[0006] Therefore, the present invention has been made in consideration of the above circumstances, and has an object to provide a method capable of visualizing the coating state of a protein adsorbent even on a substrate having a complex structure.
[0007] The present inventors have conducted extensive research to solve the above problems, and as a result have found that the above problems can be solved by appropriately combining a fluorescent dye, a protein adsorbent, and a protein detection reagent, thereby completing the present invention.
[0008] That is, the above object is to provide a substrate 1 having a coating layer containing a protein adsorbent and a fluorescent dye formed on at least one surface of a polymer substrate, and detecting a color development state 1 of the substrate 1 by irradiating the substrate 1 with light; to provide a substrate 2 having a coating layer containing a protein adsorbent and a fluorescent dye and a coating layer containing a protein detection reagent formed in that order on at least one surface of a polymer substrate, and detecting a color development state 2 of the substrate 2 by irradiating the substrate 2 with light; to provide a substrate 3 having a coating layer containing a protein adsorbent and a fluorescent dye formed on at least one surface of a polymer substrate, and introducing a sample containing protein into the substrate 3 to obtain a substrate 4; This is achieved by a method for evaluating the coating state of a protein adsorbent or the adsorption state of a protein, comprising the steps of: irradiating light onto the substrate 4 to detect a color state 3 of the substrate 4; preparing a substrate 5 having a coating layer containing a protein adsorbent and a fluorescent dye formed on at least one surface of a polymer substrate, introducing a protein-containing sample into the substrate 5 to obtain substrate 6, introducing a protein detection reagent into the substrate 6 to obtain substrate 7, irradiating light onto the substrate 7 to detect a color state 4 of the substrate 7; and comparing the color state 1, 2 or 3 with the color state 4 to evaluate the coating state of the protein adsorbent or the adsorption state of the protein. [Brief description of the drawings]
[0009] [Figure 1]Fig. 1 is a diagram for explaining the method of the present invention. In Fig. 1, 10 denotes a polymer substrate, 20 denotes a coating layer containing a protein adsorbent and a fluorescent dye, 30 denotes a coating layer containing a protein detection reagent, 31 denotes a protein detection reagent, 40 denotes a protein, and 50 denotes light of a specific wavelength that excites the fluorescent dye. [Diagram 2] Figure 2 is a photograph showing the colored state of each substrate in Example 1. Figure 2A shows colored state 1 of substrate A. Figure 2B shows colored state 2 of substrate B. Figure 2C shows colored state 3 of substrate C. Figure 2D shows colored state 4 of substrate D. [Diagram 3] FIG. 3 is a photograph showing the color development state of each bioreactor in Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Detailed Description Hereinafter, an embodiment of the present invention will be described with reference to the drawings as appropriate. Note that the present invention is not limited to the following embodiment. In addition, each drawing is exaggerated for convenience of explanation, and the dimensional ratio of each component in each drawing may differ from the actual ratio. In addition, when an embodiment of the present invention is described with reference to the drawings, the same elements are given the same reference numerals in the description of the drawings, and duplicated explanations are omitted.
[0011] In this specification, the range "X to Y" includes X and Y and means "X or more and Y or less." Furthermore, unless otherwise specified, the operations and measurements of physical properties are performed under the conditions of room temperature (20 to 25°C) and relative humidity of 40 to 50% RH.
[0012] The present invention relates to (1) preparing a substrate 1 having a coating layer containing a protein adsorbent and a fluorescent dye formed on at least one surface of a polymer substrate, and detecting a color development state 1 of the substrate 1 by irradiating the substrate 1 with light (step (1)); (2) preparing a substrate 2 having a coating layer containing a protein adsorbent and a fluorescent dye and a coating layer containing a protein detection reagent formed in this order on at least one surface of a polymer substrate, and detecting a color development state 2 of the substrate 2 by irradiating the substrate 2 with light (step (2)); (3) preparing a substrate 3 having a coating layer containing a protein adsorbent and a fluorescent dye formed on at least one surface of a polymer substrate, introducing a protein-containing sample into the substrate 3 to obtain a substrate 4, and irradiating the substrate 4 with light to detect a color-developed state 3 of the substrate 4 (step (3)); (4) preparing a substrate 5 having a coating layer containing a protein adsorbent and a fluorescent dye formed on at least one surface of a polymer substrate, introducing a protein-containing sample into the substrate 5 to obtain a substrate 6, introducing a protein detection reagent into the substrate 6 to obtain a substrate 7, and irradiating the substrate 7 with light to detect a color development state 4 of the substrate 7 (step (4)); (5) A method for evaluating the coating state of a protein adsorbent or the adsorption state of a protein, comprising comparing the coloring state 1, 2 or 3 with the coloring state 4 to evaluate the coating state of the protein adsorbent or the adsorption state of the protein (step (5)). With the above configuration, the coating state of the protein adsorbent or the adsorption state of the protein can be easily observed visually. Furthermore, the coating state of the protein or the adsorption state of the protein can be evaluated by non-destructive testing even for substrates having complex structures. Here, the mechanism by which the above-mentioned action and effect of the configuration of the present invention is exhibited is presumed to be as follows. Note that the present invention is not limited to the following presumption.
[0013] With reference to FIG. 1, the mechanism of the above-mentioned effect of the configuration of the present invention will be described. In FIG. 1A, a substrate A (substrate 1 according to the present invention) is prepared in which a coating layer 20 containing a protein adsorbent and a fluorescent dye is formed on a polymer substrate 10. When this substrate A (substrate 1) is irradiated with light 50 (hereinafter simply referred to as "light 50") of a specific wavelength that excites the fluorescent dye, the fluorescent dye in the coating layer is excited by the light 50 and emits strong light when returning from the excited state to the ground state (coloring state 1 according to the present invention). In FIG. 1B, a substrate B (substrate 2 according to the present invention) is prepared in which a coating layer 20 containing a protein adsorbent and a fluorescent dye and a coating layer 30 containing a protein detection reagent 31 are sequentially formed on a polymer substrate 10. When the substrate B (substrate 2) is irradiated with light 50, the protein detection reagent 31 absorbs a part of the light 50. As a result, the intensity of the light 50 reaching the fluorescent dye in the coating layer decreases, and the emission intensity of the fluorescent dye excited by the light 50 decreases (coloring state 2 according to the present invention). Therefore, color state 2 is weaker than color state 1 (fluorescence intensity: color state 2<color state 1). In FIG. 1C, a substrate C (substrate 3 according to the present invention) is prepared in which a coating layer 20 containing a protein adsorbent and a fluorescent dye is formed on a polymer substrate 10. A sample containing a protein 40 is added (introduced) to this substrate C (substrate 4 according to the present invention). When light 50 is then irradiated onto substrate 4, protein 40 absorbs a portion of light 50. Here, the degree of light absorption is greater for protein detection reagent 31 than for protein 40. As a result, the intensity of light 50 reaching the fluorescent dye in the coating layer in FIG. 1C is lower than in the case of FIG. 1A (color state 1), but higher than in the case of FIG. 1B (color state 2). That is, the fluorescence intensity emitted from the fluorescent dye excited by light 50 (coloring state 3 according to the present invention) is lower than in the case of FIG. 1A (coloring state 1), but higher than in the case of FIG. 1B (coloring state 2) (fluorescence intensity: coloring state 2<coloring state 3<coloring state 1). In FIG. 1D, a substrate D (substrate 5 according to the present invention) is prepared in which a coating layer 20 containing a protein adsorbent and a fluorescent dye is formed on a polymer substrate 10. A sample containing protein 40 is added (introduced) to this substrate D (substrate 6 according to the present invention). The protein is then adsorbed to the protein adsorbent in the coating layer 20.Next, the protein detection reagent 31 is introduced into the substrate 6 (substrate 7 according to the present invention). Then, the protein detection reagent 31 and the protein 40 are bound (protein adsorbent-protein-protein detection reagent-bound body). Next, when the substrate is irradiated with light 50, the bound body strongly absorbs the light. As a result, the light 50 hardly reaches the fluorescent dye in the coating layer. That is, the emission intensity of the fluorescent dye excited by the light 50 is significantly reduced (colored state 4 according to the present invention). For this reason, the colored state 4 is weaker than the above-mentioned colored state 2 (and colored states 3 and 1) (fluorescence intensity: colored state 4<colored state 2<colored state 3<colored state 1). Therefore, by comparing the colored state 4 with the emission intensity 1, 2, or 3, the adsorption state of the protein can be evaluated. In addition, the location where the adsorption of the protein is observed corresponds to the location where the protein adsorbent is present. Therefore, by comparing the colored state 4 with the emission intensity 1, 2, or 3, the coating state of the protein adsorbent can also be evaluated. Furthermore, the comparison of the coloring states 1 or 3 with 4 is performed by adding the protein and the protein detection reagent to the substrate and then irradiating the substrate with light, and these operations can be performed regardless of the shape of the substrate. Furthermore, the comparison can be performed by a non-destructive test. Therefore, according to the above method, the coating state of the protein adsorbent and the adsorption state of the protein can be visualized even for substrates with complex structures.
[0014] Process (1) In this step, a substrate 1 is prepared in which a coating layer containing a protein adsorbent and a fluorescent dye is formed on at least one surface of a polymer substrate, and the substrate 1 is irradiated with light to detect a color development state 1 of the substrate 1. In the following, the "coating layer containing a protein adsorbent and a fluorescent dye" in this step (1) is also simply referred to as "coating layer 1."
[0015] Here, the polymer substrate is not particularly limited, and a substrate that requires evaluation of the coating state of the protein adsorbent or the adsorption state of the protein can be used. Specifically, the material constituting the polymer substrate is not limited to the following, but includes hydrophobic polymers such as polyamide (PA), polyaramid (PAA), polyethersulfone (PES), polyarylethersulfone (PAES), polysulfone (PSU), polyarylsulfone (PASU), polycarbonate (PC), polyether, polyurethane (PUR), polyetherimide, polypropylene, polyethylene, polystyrene, polyacrylonitrile, and polytetrafluoroethylene; and hydrophilic polymers such as polyvinylpyrrolidone (PVP), polyethylene glycol (PEG), polyglycolmonoester, water-soluble cellulose derivatives, polysorbate, and polyethylene-polypropylene oxide copolymer. The hydrophobic polymer may be used alone or in combination of two or more types. The hydrophilic polymer may be used alone or in combination of two or more types.
[0016] In one embodiment of the present invention, the polymer-based material preferably contains at least one selected from the group consisting of polyamide (PA), polyethersulfone (PES), polyarylethersulfone (PAES) and polyvinylpyrrolidone (PVP). Such a polymer-based material is preferably used as a hollow fiber membrane for a bioreactor.
[0017] The polymer substrate according to the present invention may be formed from a mixture of the hydrophobic polymer and the hydrophilic polymer, for example, a mixture (PAES / PVP / PA) of polyamide (PA), polyarylethersulfone (PAES) and polyvinylpyrrolidone (PVP). Such a polymer substrate is particularly suitable for use as a hollow fiber membrane for a bioreactor. When the polymer substrate is formed from a mixture of a hydrophobic polymer and a hydrophilic polymer, the content of the hydrophobic polymer may be 65 to 95% by weight and the content of the hydrophilic polymer may be 5 to 35% by weight, for example, based on the total amount of the hydrophobic polymer and the hydrophilic polymer.
[0018] The polymer substrate may have various structures (shapes), including, but not limited to, a planar structure, a structure with a porous body inserted, a hollow fiber structure, a porous membrane structure, a sponge structure, a cotton-like (glass wool) structure, etc. For example, in hollow fiber bioreactor applications, the polymer substrate has hollow fibers and is preferably a porous membrane (hollow fiber membrane) composed of a plurality of hollow fibers.
[0019] In the above preferred embodiment, the inner diameter (diameter) of the hollow fiber is not particularly limited, but is preferably about 50 to 1,000 μm, more preferably about 100 to 500 μm, and particularly preferably about 150 to 350 μm. The outer diameter (diameter) of the hollow fiber is not particularly limited, but is preferably about 100 to 1,200 μm, more preferably about 150 to 700 μm, and particularly preferably about 200 to 500 μm. The length of the hollow fiber is not particularly limited, but is preferably about 50 to 900 mm, more preferably about 100 to 700 mm, and particularly preferably about 150 to 500 mm. The number of hollow fibers constituting the hollow fiber membrane is not particularly limited, but is, for example, about 1,000 to 100,000, more preferably about 3,000 to 50,000, and particularly preferably about 5,000 to 25,000. In one embodiment, the polymeric substrate is composed of about 9000 hollow fibers having an average length of about 295 mm, an average inner diameter of 215 μm, and an average outer diameter of 315 μm.
[0020] The outer layer of the hollow fiber may have an open pore structure with a certain surface roughness. The opening (diameter) of the pores is not particularly limited, but is in the range of about 0.5 to about 3 μm. The number of pores on the outer surface of the hollow fiber is about 1 mm 2 (1 mm 2 The thickness of the outer layer of the hollow fiber may be in the range of about 10,000 to about 150,000 per 100 μm. The thickness of the outer layer of the hollow fiber is not particularly limited, but may be, for example, in the range of about 1 to about 10 μm. The hollow fiber may have a next layer (second layer) on the outside. In this case, the next layer (second layer) preferably has a sponge structure with a thickness of about 1 to about 15 μm. The second layer having such a structure can function as a support for the outer layer. In this embodiment, the hollow fiber may have a further next layer (third layer) on the outside of the second layer. In this case, the further next layer (third layer) preferably has a finger-like structure. The third layer having such a structure provides mechanical stability. In addition, a high void volume can be provided that reduces the membrane migration resistance of molecules. In this embodiment, the finger-like voids are filled with a fluid during use, and the fluid reduces the resistance in diffusion and convection compared to the case of a matrix having a sponge-filled structure with a small void volume. The third layer preferably has a thickness of about 20 to about 60 μm.
[0021] The method for producing the hollow fiber and the porous membrane is not particularly limited, and known production methods can be used in the same manner or with appropriate modifications. For example, the hollow fiber is preferably formed with micropores in the wall by a stretching method or a solid-liquid phase separation method.
[0022] The hollow fiber membrane used in the bioreactor is usually subjected to a hydrophilization treatment in order to exchange a culture medium between the inside and outside of the hollow fiber membrane. In one embodiment of the present invention, the polymer-based material is a hydrophilic polymer-based material.
[0023] The method for producing the hydrophilic polymer substrate is not particularly limited, and examples thereof include a method for producing a polymer substrate by a conventionally known method using the hydrophilic polymer or a mixture of the hydrophobic polymer and the hydrophilic polymer, and a method for producing a polymer substrate by a conventionally known method using the hydrophobic polymer or a mixture of the hydrophobic polymer and the hydrophilic polymer, and then hydrophilizing the surface of the polymer substrate by a conventionally known means such as plasma treatment, corona treatment, primer treatment, etc.
[0024] As the material constituting the polymer substrate, commercially available products may be used, for example, Polyflux (registered trademark) manufactured by Baxter Ltd., and Desmopan (registered trademark) manufactured by DIC Covestro Polymer Inc. Or, for example, JP-T-2010-523118 (Patent No. 5524824) (corresponding to WO 2008 / 124229 A2), JP-T-2013-524854 (Patent No. 6039547) (corresponding to WO 2011 / 140231 A1), JP-T-2013-507143 (Patent No. 5819835) (corresponding to WO 2011 / 045644 A1), JP-A-2013-176377 (corresponding to WO 2008 / 109674 A2), JP-T-2015-526093 (corresponding to WO 2014 / 031666 A1), JP-T-2016-537001 (WO The cell culture / growth systems described in, for example, JP 2015 / 073913 A1), JP 2016-536998 A (corresponding to WO 2015 / 073918 A1), JP 2017-509344 A (corresponding to WO 2015 / 148704 A1), and JP 2018-519800 A (corresponding to WO 2016 / 183350 A1); and further, substrates used in the Quantum cell growth system manufactured by Terumo BCT Corporation may be used as the polymer substrate according to the present invention.
[0025] A coating layer (coating layer 1) containing a protein adsorbent and a fluorescent dye, and a coating layer (coating layer 2) containing a protein detection reagent are formed on at least one surface of the polymer substrate to prepare a substrate 2.
[0026] Here, the coating layer 1 may be formed at least on the surface that requires evaluation of the coating state of the protein adsorbent or the adsorption state of the protein, but is preferably formed on only one surface. In addition, it is not necessary to form a coating layer on the entire surface of the polymer substrate, and the coating layer 1 is formed at least on the portion that requires evaluation of the coating state of the protein adsorbent or the adsorption state of the protein. Preferably, the coating layer 1 is formed on the entire surface of the polymer substrate. In addition, in bioreactor applications, a coating layer containing a cell adhesion factor may be formed on the polymer substrate. In this case, the cell adhesion factor acts as a protein adsorbent. In such a case, the coating layer containing the cell adhesion factor (protein adsorbent) may be further coated with a fluorescent dye to form the coating layer 1 (see below for details). That is, the coating layer 1 may be in a form in which a layer containing a protein adsorbent and a layer containing a fluorescent dye are laminated, or in a form in which a fluorescent dye is separately added to a layer containing a protein adsorbent.
[0027] The protein adsorbent used in the coating layer 1 is not particularly limited as long as it has protein adsorption ability. For example, cell adhesion factors such as fibronectin, collagen, laminin, etc. can be used. From the viewpoint of high protein adsorption ability, the protein adsorbent preferably has a constitutional unit represented by the following formula (1). That is, in a preferred embodiment of the present invention, the protein adsorbent has the following formula (1):
[0028] [ka]
[0029] In the formula (1), R 1 is a hydrogen atom or a methyl group, and R 2 is a group represented by the following formula (1-1) or the following formula (1-2):
[0030] [ka]
[0031] In the formula (1-1) and the formula (1-2), R 3 is an alkylene group having 1 to 3 carbon atoms; It has a structural unit derived from furfuryl (meth)acrylate.
[0032] In this specification, the structural unit derived from furfuryl (meth)acrylate of the above formula (1) is also referred to simply as a "furfuryl (meth)acrylate structural unit" or "structural unit (1)".
[0033] In this specification, "(meth)acrylate" includes both acrylate and methacrylate. Similarly, "(meth)acrylic acid" includes both acrylic acid and methacrylic acid, and "(meth)acryloyl" includes both acryloyl and methacryloyl.
[0034] In the above preferred embodiment, the protein adsorbent has a furfuryl (meth)acrylate-derived structural unit (structural unit (1)) of the above formula (1). The furfuryl (meth)acrylate-derived structural unit (structural unit (1)) of the above formula (1) imparts protein adsorption to the substrate. The structural unit (1) may be a single type, or a combination of two or more types. That is, the structural unit (1) may be composed of only one type of furfuryl (meth)acrylate-derived structural unit of the above formula (1), or may be composed of two or more types of furfuryl (meth)acrylate-derived structural units of the above formula (1). The multiple structural units (1) may be present in a block form or a random form.
[0035] In the above formula (1), R 1 is a hydrogen atom or a methyl group.
[0036] Also, R 2 is a group represented by the above formula (1-1) or (1-2). Among these, from the viewpoint of further improving the protein adsorption property, R 2 is preferably a group represented by the above formula (1-1).
[0037] In the above formula (1-1) and formula (1-2), R 3 is an alkylene group having 1 to 3 carbon atoms. Here, examples of the alkylene group having 1 to 3 carbon atoms include a methylene group (-CH2-), an ethylene group (-CH2CH2-), a trimethylene group (-CH2CH2CH2-), and a propylene group (-CH(CH3)CH2- or -CH2CH(CH3)-). Of these, from the viewpoint of further improving protein adsorption, R 3 is preferably a methylene group (-CH2-) or an ethylene group (-CH2CH2-), and more preferably a methylene group (-CH2-).
[0038] That is, examples of furfuryl (meth)acrylate include tetrahydrofurfuryl acrylate, 5-[2-(acryloyloxy)ethyl]tetrahydrofuran, 2-furylmethyl acrylate, 5-[2-(acryloyloxy)ethyl]furan, tetrahydrofurfuryl methacrylate, 5-[2-(methacryloyloxy)ethyl]tetrahydrofuran, 2-furylmethyl methacrylate, 5-[2-(methacryloyloxy)ethyl]furan, etc. Among these, from the viewpoint of further improving protein adsorption, tetrahydrofurfuryl (meth)acrylate is preferred, and tetrahydrofurfuryl acrylate (THFA) is more preferred.
[0039] Here, the protein adsorbent may have only the furfuryl (meth)acrylate-derived structural unit of the above formula (1), or may further have a structural unit derived from another monomer in addition to the furfuryl (meth)acrylate-derived structural unit of the above formula (1). Here, the other monomer is not particularly limited as long as it does not inhibit the desired characteristic (protein adsorption). Specifically, the other monomer includes an ethylenically unsaturated monomer having a hydroxyl group, an alkoxyalkyl (meth)acrylate, an acrylamide, N,N-dimethylacrylamide, N,N-diethylacrylamide, methacrylamide, N,N-dimethylmethacrylamide, N,N-diethylmethacrylamide, ethylene, propylene, N-vinylacetamide, N-isopropenylacetamide, N-(meth)acryloylmorpholine, and the like. Among these, from the viewpoint of further improving the protein adsorption, the other monomer is preferably an ethylenically unsaturated monomer having a hydroxyl group and an alkoxyalkyl (meth)acrylate. In addition, when the protein adsorbent further has a structural unit derived from another monomer such as an ethylenically unsaturated monomer having a hydroxyl group and an alkoxyalkyl (meth)acrylate, the composition of the structural unit derived from the other monomer is not particularly limited as long as it does not inhibit the desired characteristic (protein adsorption), but is preferably more than 0 mol% and less than 10 mol%, more preferably about 3 to 8 mol%, based on the total structural units. That is, in a preferred embodiment, the protein adsorbent according to the present invention is composed only of a structural unit derived from furfuryl (meth)acrylate of the above formula (1) (preferred form A), or has a structural unit derived from furfuryl (meth)acrylate of the above formula (1) and a structural unit derived from an ethylenically unsaturated monomer having a hydroxyl group (preferred form B), or has a structural unit derived from furfuryl (meth)acrylate of the above formula (1) and a structural unit derived from an alkoxyalkyl (meth)acrylate represented by the following formula (3) (preferred form C). The above preferred forms A, B, and C will be described below.
[0040] [ka]
[0041] In the above formula (3), R 6 is a hydrogen atom or a methyl group; R 7 is an alkylene group having 2 to 3 carbon atoms; R 8 is an alkyl group having 1 to 3 carbon atoms.
[0042] (Preferred Form A) In the preferred form A, the protein adsorbent is a homopolymer of tetrahydrofurfuryl acrylate, 5-[2-(acryloyloxy)ethyl]tetrahydrofuran, 2-furylmethyl acrylate, 5-[2-(acryloyloxy)ethyl]furan, tetrahydrofurfuryl methacrylate, 5-[2-(methacryloyloxy)ethyl]tetrahydrofuran, 2-furylmethyl methacrylate, or 5-[2-(methacryloyloxy)ethyl]furan, or a copolymer of two or more of the above. Among these, from the viewpoint of further improving the protein adsorption, the protein adsorbent is preferably polytetrahydrofurfuryl acrylate (pTHFA) or polytetrahydrofurfuryl methacrylate, and more preferably polytetrahydrofurfuryl acrylate (pTHFA).
[0043] In this preferred form A, the weight-average molecular weight (Mw) of the protein adsorbent is not particularly limited, but is preferably 50,000 to 800,000. Within the above range, the solubility of the protein adsorbent in a solvent is improved, and it becomes easier to apply the protein adsorbent uniformly to a substrate. From the viewpoint of improving the coating film formability, the weight-average molecular weight of the protein adsorbent is more preferably 100,000 to 500,000, and particularly preferably 150,000 to 350,000.
[0044] In this specification, the "weight average molecular weight (Mw)" is a value measured by gel permeation chromatography (GPC) using polystyrene as a standard substance and tetrahydrofuran (THF) as a mobile phase. Specifically, a protein adsorbent is dissolved in tetrahydrofuran (THF) to a concentration of 10 mg / ml to prepare a sample. For the sample thus prepared, a GPC column LF-804 (Showa Denko K.K.) is attached to a GPC system LC-20 (Shimadzu Corporation), THF is run as a mobile phase, and polystyrene is used as a standard substance to measure the GPC of the protein adsorbent. After preparing a calibration curve with standard polystyrene, the weight average molecular weight (Mw) of the protein adsorbent is calculated based on this curve.
[0045] (Preferred Form B) In a preferred form B, the protein adsorbent has a structural unit (structural unit (1)) derived from furfuryl (meth)acrylate of the above formula (1) and a structural unit (structural unit (2)) derived from an ethylenically unsaturated monomer having a hydroxyl group. Here, the furfuryl (meth)acrylate (structural unit (1)) is considered to impart protein adsorptivity to the substrate. Also, the hydroxyl group (-OH) contained in the structural unit (2) is presumed to promote protein adsorptivity to the substrate surface. Note that the above is merely presumed, and the present invention is not limited thereto.
[0046] The structural unit (1) is the same as that described above, and therefore a detailed description thereof will be omitted here.
[0047] The structural unit (2) is a structural unit derived from an ethylenically unsaturated monomer having a hydroxyl group. Here, the ethylenically unsaturated monomer having a hydroxyl group forming the structural unit (2) is not particularly limited as long as it is a compound having one or more hydroxyl groups (-OH) and one or more ethylenically unsaturated groups in one molecule. Here, the "ethylenically unsaturated group" refers to a group formed by replacing a hydrogen atom of ethylene (CH2=CH2), and examples thereof include a (meth)acryloyl group, a vinyl group, an allyl group, and a vinyl ether group. Note that only one type of these groups may be contained in one molecule of the ethylenically unsaturated monomer, or two or more types may be contained.
[0048] Among them, the ethylenically unsaturated group is preferably a (meth)acryloyl group (CH2=CR-C(=O)-; R=hydrogen atom or methyl group). That is, according to a preferred embodiment of the present invention, the ethylenically unsaturated monomer has a (meth)acryloyl group. Therefore, the ethylenically unsaturated monomer is preferably a compound having one or more hydroxyl groups and one or more acryloyl groups or methacryloyl groups in one molecule. The upper limit of the number of hydroxyl groups and (meth)acryloyl groups contained in the ethylenically unsaturated monomer is not particularly limited, but from the viewpoint of protein adsorption, the number of hydroxyl groups in one molecule is preferably 3 or less, more preferably 2 or less, and particularly preferably 1. In addition, from the viewpoint of the ease of preparation of the protein adsorbent with furfuryl (meth)acrylate represented by the above formula (1), the controllability of the composition (molar ratio) of each constituent unit, and the controllability of protein adsorption, the number of (meth)acryloyl groups in one molecule is preferably 3 or less, more preferably 2 or less. In particular, from the viewpoint of further improving protein adsorption by controlling the composition (molar ratio) of each structural unit, it is particularly preferable that the number of (meth)acryloyl groups in one molecule is one.
[0049] According to a preferred embodiment of the present invention, the structural unit (2) is derived from a hydroxyalkyl (meth)acrylate represented by the following formula (2). That is, the ethylenically unsaturated monomer is preferably a hydroxyalkyl (meth)acrylate represented by the following formula (2). The structural unit (2) constituting the protein adsorbent may be a single type or a combination of two or more types. That is, the structural unit (2) may be composed of only a single type of structural unit derived from a hydroxyalkyl (meth)acrylate represented by the following formula (2), or may be composed of two or more types of structural units derived from a hydroxyalkyl (meth)acrylate represented by the following formula (2). The multiple structural units (2) may be present in a block form or a random form.
[0050] [ka]
[0051] In the above formula (2), R 4 R is a hydrogen atom or a methyl group. 5 is an alkylene group having 2 to 3 carbon atoms. Here, examples of the alkylene group having 2 to 3 carbon atoms include an ethylene group (-CH2CH2-), a trimethylene group (-CH2CH2CH2-), and a propylene group (-CH(CH3)CH2- or -CH2CH(CH3)-). Of these, from the viewpoint of further improving protein adsorption, R 5 is preferably an ethylene group (-CH2CH2-) or a trimethylene group (-CH2CH2CH2-), and more preferably an ethylene group (-CH2CH2-).
[0052] That is, examples of hydroxyalkyl (meth)acrylates include hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxyisopropyl acrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, and hydroxyisopropyl methacrylate. These hydroxyalkyl (meth)acrylates may be used alone or in combination of two or more. Among these, from the viewpoint of further improving protein adsorption, the hydroxyalkyl (meth)acrylate is preferably hydroxyethyl (meth)acrylate, and more preferably hydroxyethyl methacrylate (HEMA).
[0053] The composition of the structural unit (1) and the structural unit (2) is not particularly limited. From the viewpoint of protein adsorption, the protein adsorbent preferably has more than 20 mol% and less than 100 mol% of the structural unit (1) derived from furfuryl (meth)acrylate represented by the above formula (1) and more than 0 mol% and less than 80 mol% of the structural unit (2) derived from an ethylenically unsaturated monomer having a hydroxyl group. More preferably, the protein adsorbent has 35 mol% to 98 mol% of the structural unit (1) and 2 mol% to 65 mol% of the structural unit (2). Even more preferably, the protein adsorbent has 40 mol% to 95 mol% of the structural unit (1) and 5 mol% to 60 mol% of the structural unit (2). Even more preferably, the protein adsorbent has 50 mol% to 93 mol% of the structural unit (1) and 7 mol% to 50 mol% of the structural unit (2). Particularly preferably, the protein adsorbent comprises 55 mol% to 90 mol% of the structural unit (1) and 10 mol% to 45 mol% of the structural unit (2). Most preferably, the protein adsorbent comprises 60 mol% to 90 mol% of the structural unit (1) and 10 mol% to 40 mol% of the structural unit (2). The total of the structural units (1) and (2) is 100 mol%. When the structural unit (1) is composed of two or more types of structural units (1), the composition of the structural unit (1) is the ratio (molar ratio (mol%)) of the total of the structural units (1) to the total of the structural units (1) and (2). Similarly, when the structural unit (2) is composed of two or more types of structural units (2) (particularly preferably two or more types of structural units derived from a hydroxyalkyl (meth)acrylate represented by the above formula (2)), the composition of the structural unit (2) is the ratio (molar ratio (mol %)) of the total of the structural units (2) to the total of the structural units (1) and (2).
[0054] In this preferred form B, the protein adsorbent has the structural unit (1) and the structural unit (2), and, if necessary, structural units derived from other monomers as described above. Here, the arrangement of each structural unit is not particularly limited, and may be in a block form (block copolymer type protein adsorbent), a random form (random copolymer type protein adsorbent), or an alternating form (alternating copolymer type protein adsorbent). In consideration of further improvement of protein adsorption, it is preferable that the protein adsorbent is composed only of the structural unit (1) and the structural unit (2).
[0055] In this preferred form B, the weight-average molecular weight (Mw) of the protein adsorbent is not particularly limited, but is preferably 50,000 to 800,000. Within the above range, the solubility of the protein adsorbent in a solvent is improved, and it becomes easier to apply the protein adsorbent uniformly to a substrate. From the viewpoint of improving the coating film formability, the weight-average molecular weight of the protein adsorbent is more preferably 100,000 to 500,000, and particularly preferably 150,000 to 350,000.
[0056] (Preferred Form C) In a preferred form C, the protein adsorbent has a furfuryl (meth)acrylate-derived structural unit (structural unit (1)) of the above formula (1) and an alkoxyalkyl (meth)acrylate-derived structural unit (3) of the following formula (3). Here, the furfuryl (meth)acrylate (structural unit (1)) is considered to impart protein adsorptive properties to the substrate. Also, the alkoxyalkyl (meth)acrylate (structural unit (3)) is considered to impart protein adsorptive properties (and antithrombotic properties) to the substrate. Note that the above is merely speculation, and the present invention is not limited to the above.
[0057] The structural unit (1) is the same as that described above, and therefore a detailed description thereof will be omitted here.
[0058] The structural unit (3) is derived from an alkoxyalkyl (meth)acrylate of the following formula (3). The structural unit (3) constituting the protein adsorbent may be of one type alone or a combination of two or more types. That is, the structural unit (3) may be composed of only one type of structural unit derived from an alkoxyalkyl (meth)acrylate of the following formula (3), or may be composed of two or more types of structural units derived from an alkoxyalkyl (meth)acrylate of the following formula (3). The multiple structural units (3) may be present in a block form or a random form.
[0059] [ka]
[0060] In the above formula (3), R 6 R is a hydrogen atom or a methyl group. 7 is an alkylene group having 2 to 3 carbon atoms. Here, examples of the alkylene group having 2 to 3 carbon atoms include an ethylene group (-CH2CH2-), a trimethylene group (-CH2CH2CH2-), and a propylene group (-CH(CH3)CH2- or -CH2CH(CH3)-). Of these, from the viewpoints of further improving protein adsorptive properties (and antithrombotic properties) and achieving a good balance between protein adsorptive properties and antithrombotic properties, R 7 is preferably an ethylene group (-CH2CH2-) or a propylene group, more preferably an ethylene group (-CH2CH2-). 8 is an alkyl group having 1 to 3 carbon atoms. Examples of the alkyl group having 1 to 3 carbon atoms include a methyl group, an ethyl group, an n-propyl group, and an isopropyl group. Among these, from the viewpoints of further improving protein adsorptive properties (and antithrombotic properties) and achieving a good balance between protein adsorptive properties and antithrombotic properties, R 8 is preferably a methyl group or an ethyl group, and more preferably a methyl group.
[0061] That is, examples of alkoxyalkyl (meth)acrylates include methoxymethyl acrylate, methoxyethyl acrylate, methoxypropyl acrylate, ethoxymethyl acrylate, ethoxyethyl acrylate, ethoxypropyl acrylate, ethoxybutyl acrylate, propoxymethyl acrylate, butoxyethyl acrylate, methoxybutyl acrylate, methoxymethyl methacrylate, methoxyethyl methacrylate, ethoxymethyl methacrylate, ethoxyethyl methacrylate, propoxymethyl methacrylate, butoxyethyl methacrylate, etc. Among these, from the viewpoint of further improving protein adsorption, methoxyethyl (meth)acrylate, ethoxyethyl (meth)acrylate, and methoxybutyl (meth)acrylate are preferred, methoxyethyl (meth)acrylate is more preferred, and methoxyethyl acrylate (MEA) is particularly preferred.
[0062] The composition of the structural unit (1) and the structural unit (3) is not particularly limited. From the viewpoint of protein adsorption, the protein adsorbent preferably has 95 to 35 mol% of the structural unit (1) derived from furfuryl (meth)acrylate represented by formula (1) and 5 to 65 mol% of the structural unit (3) derived from an alkoxyalkyl (meth)acrylate represented by formula (3). More preferably, the protein adsorbent has 90 to 40 mol% of the structural unit (1) derived from furfuryl (meth)acrylate represented by formula (1) and 10 to 60 mol% of the structural unit (3) derived from an alkoxyalkyl (meth)acrylate represented by formula (3). Even more preferably, the protein adsorbent has 70 to 40 mol% of the structural unit (1) derived from furfuryl (meth)acrylate represented by formula (1) and 30 to 60 mol% of the structural unit (3) derived from an alkoxyalkyl (meth)acrylate represented by formula (3). Particularly preferably, the protein adsorbent has 60 to 40 mol % of the furfuryl (meth)acrylate-derived structural unit (1) of formula (1) and 40 to 60 mol % of the alkoxyalkyl (meth)acrylate-derived structural unit (3) of formula (3). A protein adsorbent having such a composition can exhibit a good balance between protein adsorption and antithrombotic properties. For this reason, it is particularly effective when the sample containing protein is blood. The total of the structural unit (1) and the structural unit (3) is 100 mol %. When the structural unit (1) is composed of two or more types of structural units (1), the composition of the structural unit (1) is the ratio (molar ratio (mol %)) of the total of the structural unit (1) to the total of the structural unit (1) and the structural unit (3). Similarly, when the structural unit (3) is composed of two or more types of structural units (3), the composition of the structural unit (3) is the ratio (molar ratio (mol %)) of the total of the structural unit (3) to the total of the structural unit (1) and the structural unit (3).
[0063] In this preferred form C, the protein adsorbent has the structural unit (1) and the structural unit (3), and, if necessary, structural units derived from other monomers as described above. Here, the arrangement of each structural unit is not particularly limited, and may be in a block form (block copolymer type protein adsorbent), a random form (random copolymer type protein adsorbent), or an alternating form (alternating copolymer type protein adsorbent). In consideration of further improvement of protein adsorption and an appropriate balance between protein adsorption and antithrombotic properties, it is preferable that the protein adsorbent is composed only of the structural unit (1) and the structural unit (3).
[0064] The weight-average molecular weight (Mw) of the protein adsorbent according to the present invention is not particularly limited, but is preferably 50,000 to 1,000,000. Within the above range, the solubility of the protein adsorbent in a solvent is improved, and it becomes easier to apply the protein adsorbent uniformly to a substrate. From the viewpoint of improving the coating film formability, the weight-average molecular weight of the protein adsorbent is more preferably 100,000 to 500,000, and particularly preferably 250,000 to 400,000.
[0065] The protein adsorbent according to the present invention is not particularly limited, and can be prepared by applying a conventionally known polymerization method such as bulk polymerization, suspension polymerization, emulsion polymerization, solution polymerization, living radical polymerization, polymerization using a macroinitiator, polycondensation, etc. Specifically, for example, when the protein adsorbent according to the present invention is made of a block copolymer, a living radical polymerization method or a polymerization method using a macroinitiator is preferably used. The living radical polymerization method is not particularly limited, and for example, the methods described in JP-A-11-263819, JP-A-2002-145971, JP-A-2006-316169, etc., as well as the atom transfer radical polymerization (ATRP) method, etc. can be applied in the same manner or with appropriate modifications.
[0066] Alternatively, for example, when the protein adsorbent of the present invention is composed of a random copolymer, a (co)polymerization method is preferably used which comprises stirring, in a polymerization solvent, one or more of the furfuryl (meth)acrylate of the above formula (1) (in the above preferred form A), and (in the above preferred form B) an ethylenically unsaturated monomer having a hydroxyl group (preferably a hydroxyalkyl (meth)acrylate of the above formula (2)) or (in the above preferred form C) an alkoxyalkyl (meth)acrylate of the above formula (3), and, if necessary, a monomer copolymerizable therewith (another monomer, a copolymerizable monomer), together with a polymerization initiator to prepare a monomer solution, and heating the monomer solution. In the following, "furfuryl (meth)acrylate of the above formula (1), and (in the above preferred form B) an ethylenically unsaturated monomer having a hydroxyl group (preferably, a hydroxyalkyl (meth)acrylate of the above formula (2)) or (in the above preferred form C) an alkoxyalkyl (meth)acrylate of the above formula (3), and one or more monomers (other monomers, copolymerizable monomers) that can be copolymerized with them if necessary" are referred to as "monomers for polymerization". In the above method, the polymerization solvent that can be used in the preparation of the monomer solution is not particularly limited as long as it can dissolve the monomers used. For example, water, methanol, ethanol, propanol, isopropanol, and other alcohols, polyethylene glycols, and other aqueous solvents; toluene, xylene, tetralin, and other aromatic solvents; and chloroform, dichloroethane, chlorobenzene, dichlorobenzene, trichlorobenzene, and other halogenated solvents can be mentioned. Among these, methanol is preferred in consideration of the ease of dissolving the monomer. The monomer concentration in the monomer solution is not particularly limited. The monomer concentration in the monomer solution is usually 1 to 60% by weight, more preferably 5 to 50% by weight, and particularly preferably 10 to 45% by weight. The monomer concentration means the total concentration of the monomers for polymerization.
[0067] The polymerization initiator is not particularly limited, and a known initiator may be used. A radical polymerization initiator is preferable because of its excellent polymerization stability. Specifically, persulfates such as potassium persulfate (KPS), sodium persulfate, and ammonium persulfate; peroxides such as hydrogen peroxide, t-butyl peroxide, and methyl ethyl ketone peroxide; azobisisobutyronitrile (AIBN), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane]disulfate dihydrate, 2,2'-azobis(2-methylpropionamidine)dihydrochloride, 2, Examples of the azo compounds include 2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine)]hydrate, 3-hydroxy-1,1-dimethylbutyl peroxyneodecanoate, α-cumyl peroxyneodecanoate, 1,1,3,3-tetrabutyl peroxyneodecanoate, t-butyl peroxyneodecanoate, t-butyl peroxyneoheptanoate, t-butyl peroxypivalate, t-amyl peroxyneodecanoate, t-amyl peroxypivalate, di(2-ethylhexyl) peroxydicarbonate, di(secondary butyl) peroxydicarbonate, and azobiscyanovaleric acid. In addition, the radical polymerization initiator may be used as a redox initiator by combining it with a reducing agent such as sodium sulfite, sodium hydrogen sulfite, or ascorbic acid. The amount of the polymerization initiator is preferably 0.0005 to 0.005 mol per 1 mol of the total amount of the polymerization monomers. With such an amount of the polymerization initiator, (co)polymerization of the polymerization monomers proceeds efficiently.
[0068] The polymerization initiator may be mixed with the polymerization monomer and the polymerization solvent as it is, or may be mixed with the polymerization monomer in the form of a solution in which it is dissolved in another solvent in advance. In the latter case, the other solvent is not particularly limited as long as it can dissolve the polymerization initiator, and examples thereof include the same solvent as the polymerization solvent. The other solvent may be the same as or different from the polymerization solvent, but is preferably the same as the polymerization solvent in consideration of ease of control of polymerization. The concentration of the polymerization initiator in the other solvent in this case is not particularly limited, but is preferably 0.1 to 10 parts by weight, more preferably 0.5 to 5 parts by weight, relative to 100 parts by weight of the other solvent in consideration of ease of mixing.
[0069] When the polymerization initiator is used in the form of a solution, a solution in which the monomer for polymerization is dissolved in the polymerization solvent may be degassed in advance before the polymerization initiator solution is added. The degassing treatment may be performed, for example, by bubbling the solution with an inert gas such as nitrogen gas or argon gas for about 0.5 to 5 hours. During the degassing treatment, the temperature of the solution may be adjusted to about 30°C to 80°C, preferably to the polymerization temperature in the polymerization step described below.
[0070] Next, the monomer solution is heated to (co)polymerize the monomers. Here, the (co)polymerization method may be a known polymerization method such as radical polymerization, anionic polymerization, or cationic polymerization, and preferably radical polymerization is used because it is easy to produce.
[0071] The (co)polymerization conditions are not particularly limited as long as the desired monomers for polymerization can be (co)polymerized. Specifically, the (co)polymerization temperature is preferably 30 to 80°C, more preferably 40 to 55°C. The (co)polymerization time is preferably 1 to 24 hours, more preferably 5 to 12 hours. Under the above conditions, the (co)polymerization of each monomer proceeds efficiently. Furthermore, gelation in the (co)polymerization step can be effectively suppressed or prevented, and high production efficiency can be achieved.
[0072] If necessary, a chain transfer agent, a polymerization rate regulator, a surfactant, and other additives may be appropriately used during the polymerization.
[0073] The atmosphere in which the (co)polymerization reaction is carried out is not particularly limited, and the reaction can be carried out in air or in an inert gas atmosphere such as nitrogen gas or argon gas, etc. During the (co)polymerization reaction, the reaction liquid may be stirred.
[0074] The (co)polymer after (co)polymerization can be purified by a general purification method such as a reprecipitation method (precipitation method), a dialysis method, an ultrafiltration method, or an extraction method.
[0075] The purified (co)polymer can be dried by any method such as freeze-drying, vacuum drying, spray drying, or heat drying. From the viewpoint of having little effect on the physical properties of the polymer, freeze-drying or vacuum drying is preferred.
[0076] The fluorescent dye used in the coating layer 1 is not particularly limited as long as it is excited when irradiated with light such as ultraviolet light and emits specific fluorescence. From the viewpoint of visibility, the fluorescent dye is preferably a xanthene dye. Specific examples of xanthene dyes include, but are not limited to, coumarin, cyanine, benzofuran, quinoline, quinazolinone, indole, benzazole, borapolyazaindacene, fluorescein, rhodamine, and rhodol. In addition, from the viewpoints of the film strength of the coating layer 1, the effect of suppressing the elution of the dye, and the adhesion to the polymer substrate, a fluorescent dye having a polymerizable group such as a (meth)acrylic group is preferably used. Here, the fluorescent dye may be synthesized or a commercially available product may be used. An example of a commercially available product is R13 (color: fluorescent purple, polymerizable group: methacryl group, acrylic equivalent: 1.2×10 3 g / eq, maximum absorption wavelength: 559 nm; Fujifilm Wako Pure Chemical Industries, Ltd.), R60 (color: red, polymerizable group: methacrylic group, acrylic equivalent: 1.2 × 10 3 g / eq, maximum absorption wavelength: 499 nm; Fujifilm Wako Pure Chemical Industries, Ltd.), K01 (color: black, polymerizable group: methacryl group, acrylic equivalent: 1.3 × 10 3xanthene dyes such as Y03 (color: yellow, polymerizable group: methacryl group, acrylic equivalent: 1.1×10 3 cyanine dyes such as G01 (color: green, polymerizable group: methacryl group, acrylic equivalent: 1.2 × 10 g / eq, maximum absorption wavelength: 419 nm; Fujifilm Wako Pure Chemical Industries, Ltd.); 3 g / eq, maximum absorption wavelength: 643 nm; Fujifilm Wako Pure Chemical Industries, Ltd.), B01 (color: blue, polymerizable group: methacryl group, acrylic equivalent: 1.2 × 10 3 g / eq, maximum absorption wavelength: 624 nm; Fujifilm Wako Pure Chemical Industries, Ltd.) and other triarylmethane dyes.
[0077] The method for forming the coating layer 1 on the polymer substrate is not particularly limited, and known methods can be applied in the same manner or with appropriate modifications. For example, a method can be used in which a coating liquid (coating liquid (1)) containing a protein adsorbent and a fluorescent dye is prepared and the coating liquid (1) is applied to the polymer substrate. Alternatively, in a bioreactor or the like, when a layer containing a protein adsorbent (cell adhesion factor) is formed on the polymer substrate in advance, a coating liquid (coating liquid (1')) containing a fluorescent dye is prepared and the coating liquid (1') is applied to the coating layer containing the protein adsorbent (cell adhesion factor) of the polymer substrate to form the coating layer 1. That is, when a coating layer containing a protein adsorbent is formed on the polymer substrate in advance, in step (1), a coating layer containing a fluorescent dye is formed on the surface of the polymer substrate having a coating layer containing a protein adsorbent on the side where the coating layer is located, or a fluorescent dye is added to the coating layer of the polymer substrate having a coating layer containing a protein adsorbent, to prepare the substrate 1. The substrate 1 is irradiated with light to detect the color development state 1 of the substrate 1.
[0078] Here, the solvent used to prepare the coating liquid (1) and (1') is not particularly limited and can be appropriately selected depending on the type of protein adsorbent and fluorescent dye. Specifically, examples of the solvent include water; ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ester-based solvents such as butyl acetate, ethyl acetate, carbitol acetate, and butyl carbitol acetate; ether-based solvents such as methyl cellosolve, ethyl cellosolve, butyl ether, and tetrahydrofuran; alkane-based solvents such as butane and hexane; aromatic solvents such as benzene, toluene, and xylene; halogen-based solvents such as dichloroethane, chloroform, and methylene chloride; and alcohol-based solvents such as methanol, ethanol, n-propanol, isopropanol, and ethylene glycol. The above solvents may be used alone or in combination of two or more. The protein adsorbent and the fluorescent dye may be dissolved in the same solvent to obtain the coating liquid (1), or the protein adsorbent and the fluorescent dye may be dissolved in different solvents and then these solutions may be mixed to obtain the coating liquid (1). The mixing ratio of the protein adsorbent and the fluorescent dye in the coating liquid (1) is not particularly limited. From the viewpoint of the balance between the desired protein adsorption properties and the fluorescence intensity (ease of observation), the mixing ratio of the protein adsorbent and the fluorescent dye (weight ratio of protein adsorbent: fluorescent dye) is preferably 2 to 200: 1, more preferably 7.5 to 150: 1. The concentration of the protein adsorbent in the coating liquid (1) is not particularly limited, but is preferably 0.05 to 2 wt%, more preferably 0.05 to 1 wt%. The concentration of the fluorescent dye in the coating liquids (1) and (1') is not particularly limited, but is preferably 0.005 to 0.1 wt%, more preferably 0.01 to 0.05 wt%. Within such ranges, the coating liquids (1) and (1') have good applicability, and a uniform coating layer 1 of desired thickness can be easily obtained by a single coating.
[0079] The amount of coating liquid (1) to be applied is not particularly limited, but is preferably an amount that results in a thickness (dry film thickness) of the coating layer 1 of 1 to 5 μm. The amount of coating liquid (1') to be applied is not particularly limited, but may be an amount that allows the coating layer 1 to emit sufficient fluorescence when irradiated with light. Specifically, the amount of coating liquid (1') to be applied is 0.15 to 0.45 g / cm. 3 The amount is preferably such that one coating layer is formed.
[0080] Before applying the coating liquid (1), the surface of the polymer substrate may be pretreated by ultraviolet irradiation treatment, plasma treatment, corona discharge treatment, flame treatment, oxidation treatment, silane coupling treatment, phosphoric acid coupling treatment, or the like. For example, the surface of the polymer substrate is made hydrophilic by subjecting the surface of the polymer substrate to plasma treatment. This improves the wettability of the coating liquid (1) to the surface of the polymer substrate, and allows the formation of a uniform coating layer 1.
[0081] The method for applying the coating liquid (1) or (1') to the polymer substrate is not particularly limited, and any conventionally known method can be applied, such as a coating / printing method, a dipping method (dipping method, dip coating method), a spray method, a spin coating method, or a mixed solution impregnated sponge coating method. Among these, the dipping method (dipping method, dip coating method) is preferred. Alternatively, in the case of a bioreactor or the like, the above-mentioned coating liquid (1) or (1') may be introduced or circulated to the polymer substrate in the bioreactor.
[0082] After the coating liquid (1) is applied to the polymer substrate, it is preferable to dry the coating film. Here, the drying conditions are not particularly limited as long as the solvent can be removed from the coating film, and hot air treatment using a dryer or the like may be performed, or natural drying may be performed. In the case of a bioreactor or the like, dry air may be introduced or circulated into the bioreactor. Furthermore, the pressure conditions during drying are also not particularly limited, and drying may be performed under normal pressure (atmospheric pressure), or under pressure or reduced pressure. For example, an oven, a reduced pressure dryer, or the like can be used as the drying means (apparatus), but in the case of natural drying, no particular drying means (apparatus) is required.
[0083] By the above method, the coating layer 1 is formed on the polymer substrate to obtain the substrate 1. Next, the substrate 1 thus obtained is irradiated with light, and the color development state 1 of the substrate 1 is detected.
[0084] Here, the light to be irradiated is appropriately selected depending on the type of fluorescent reagent. Specifically, ultraviolet light (UV), visible light, infrared light, electron beam, gamma ray, etc. can be used. Preferred is ultraviolet light or electron beam, and more preferably ultraviolet light in consideration of the effect on the human body. When irradiating with ultraviolet light, the wavelength of irradiation can be appropriately selected from wavelengths that can excite the fluorescent dye. Specifically, the wavelength range of ultraviolet light is preferably 200 to 400 nm, more preferably 220 to 320 nm. Moreover, ultraviolet light irradiation is preferably performed at a temperature of 10 to 50°C, more preferably 20 to 40°C. The irradiation intensity of ultraviolet light is not particularly limited, but is preferably 1 to 5,000 mW / cm. 2 , more preferably 1 to 100 mW / cm 2 , and more preferably 1 to 10 mW / cm 2 The integrated amount of ultraviolet light (integrated amount of ultraviolet light on the substrate 1 before the surface lubricating layer is applied) is not particularly limited, but is preferably 1 to 5,000 mJ / cm. 2 and more preferably 1 to 100 mJ / cm 2 Examples of devices for irradiating ultraviolet rays include high pressure mercury lamps, low pressure mercury lamps, metal halide lamps, xenon lamps, and halogen lamps.
[0085] The above-mentioned irradiation causes the fluorescent dye in the coating layer 1 to develop color, and this colored state (colored state 1) is detected (FIG. 1A).
[0086] Process (2) In this step, a substrate 2 is prepared in which a coating layer containing a protein adsorbent and a fluorescent dye and a coating layer containing a protein detection reagent are successively formed on at least one surface of a polymer substrate, and the substrate 2 is irradiated with light to detect a color development state 2 of the substrate 2. In the following, the "coating layer containing a protein adsorbent and a fluorescent dye" and the "coating layer containing a protein detection reagent" in this step (2) are also simply referred to as "coating layer 1'" and "coating layer 2'", respectively.
[0087] Here, the polymer substrate is not particularly limited, and any substrate that requires evaluation of the coating state of the protein adsorbent or the adsorption state of the protein can be used in the same manner. Specifically, the same polymer substrate as in the above step (1) can be used. The polymer substrate used in this step (2) is preferably the same as that used in the above step (1).
[0088] A coating layer (coating layer 1') containing a protein adsorbent and a fluorescent dye, and a coating layer (coating layer 2') containing a protein detection reagent are formed on at least one surface of the polymer substrate to prepare a substrate 2.
[0089] Here, the coating layer 1' only needs to be formed on the surface that requires evaluation of the coating state of the protein adsorbent or the adsorption state of the protein, but is preferably formed on only one surface. Moreover, it is not necessary to form a coating layer on the entire surface of the polymer substrate, and the coating layer 1' is formed at least on the portion that requires evaluation of the coating state of the protein adsorbent or the adsorption state of the protein. Preferably, the coating layer 1' is formed on the entire surface of the polymer substrate. It is preferable that the coating layer 1' is formed in the same manner as the coating layer 1, since comparison of the color development state is easier and more accurate.
[0090] The protein adsorbent used in coating layer 1' is not particularly limited as long as it has protein adsorption ability. Specifically, the same protein adsorbent as in step (1) above can be used, and therefore a description thereof will be omitted here. It is particularly preferable that the protein adsorbent used in coating layer 1' is the same as the protein adsorbent used in coating layer 1, from the viewpoint of easier and more accurate comparison of color development state, etc.
[0091] The fluorescent dye used in the coating layer 1' is not particularly limited as long as it is excited when irradiated with light such as ultraviolet light and emits specific fluorescence. Specifically, the same fluorescent dye as in the above step (1) can be used, and therefore a description thereof will be omitted here. From the viewpoint of easier and more accurate comparison of color development states, etc., it is preferable that the fluorescent dye used in the coating layer 1' is the same as the fluorescent dye used in the coating layer 1.
[0092] The method for forming the coating layer 1' on the polymer substrate is not particularly limited, and a known method can be applied in the same manner or with appropriate modifications. Specifically, the same method as in the above step (1) can be used, and therefore a description thereof will be omitted here. It is preferable that the coating layer 1' is formed on the polymer substrate by the same method as the coating layer 1, from the viewpoint of easier and more accurate comparison of the color development state, etc.
[0093] The method for forming the coating layer 1' on the polymer substrate is not particularly limited, and a known method can be applied in the same manner or with appropriate modification. Specifically, the same method as in the above step (1) can be used, and therefore the explanation is omitted here. For example, in a bioreactor or the like, when a layer containing a protein adsorbent (cell adhesion factor) is formed on the polymer substrate in advance, a coating liquid (coating liquid (1')) containing a fluorescent dye is prepared, and the coating liquid (1') is applied to the coating layer containing the protein adsorbent (cell adhesion factor) of the polymer substrate to form the coating layer 1'. That is, when the substrate has a coating layer containing a protein adsorbent, in step (2), a substrate 2 is prepared in which a coating layer containing a fluorescent dye and a coating layer containing a protein detection reagent are sequentially formed on the surface of the polymer substrate having a coating layer containing a protein adsorbent on the side where the coating layer is located. The substrate 2 is irradiated with light to detect the color development state 2 of the substrate 2. It is preferable that the coating layer 1' is formed on the polymer substrate by the same method as the coating layer 1, from the viewpoint of easier and more accurate comparison of the color development state.
[0094] That is, the coating layer 1 ′ is preferably the same as the coating layer 1 .
[0095] Next, a coating layer (coating layer 2') containing a protein detection reagent is placed on coating layer 1'. Here, coating layer 2' may be formed at least on the surface that requires evaluation of the coating state of the protein adsorbent or the adsorption state of the protein, but is preferably formed on at least a part of coating layer 1', and more preferably formed on the entire surface of coating layer 1'.
[0096] The protein detection reagent used in the coating layer 2' is not particularly limited as long as it has the ability to detect proteins, and can be appropriately selected depending on the type of protein to be detected. Specifically, bicinchoninic acid, Coomassie blue, ninhydrin, etc. can be used. Of these, the protein detection reagent preferably has a quinoline structure, and more preferably is bicinchoninic acid (BCA). In a preferred embodiment, proteins are detected by the bicinchoninic acid method (BCA method). In the BCA method, the peptide bonds of proteins are converted to cupric ions (Cu 2+ ) is reduced to tetradentate cuprous ion (Cu 1+ ) complex, which reacts with BCA to form (Cu 1+ Each BCA molecule (2 BCA molecules) produces a strong purple color. For this reason, in the BCA method, proteins are measured at 562 nm. The BCA method is preferably used because it has high protein detection ability, high compatibility with interfering compounds, is simple, and has a wide linear action range (excellent quantitative performance). It is also preferable because the absorption spectrum of bicinchoninic acid (BCA) overlaps widely with the excitation spectrum of xanthene fluorescent dyes.
[0097] The method for forming the coating layer 2' on the coating layer 1' is not particularly limited, and a known method can be applied in the same manner or with appropriate modifications. For example, a method can be used in which a coating liquid (coating liquid (2)) containing a protein detection reagent is prepared and the coating liquid (2) is applied to the coating layer 1'. The solvent used to prepare the coating liquid (2) is not particularly limited as long as it can dissolve the protein detection reagent. Specifically, the same solvent as that used to prepare the coating liquid (1) in the above step (1) can be used. The concentration of the protein detection reagent in the coating liquid (2) is not particularly limited, but is preferably 2.0 to 20.0% by weight, and more preferably 5.0 to 15.0% by weight. Within such a range, the coating property of the coating liquid (2) is good. In addition, a uniform coating layer 2' of a desired thickness can be easily obtained by one coating.
[0098] The amount of the coating liquid (2) to be applied is not particularly limited, but is preferably an amount such that the thickness (dry film thickness) of the coating layer 2' is 0.1 to 2 μm. Alternatively, the amount of the coating liquid (2) to be applied is preferably 0.1 to 0.3 g / cm. 3 It is preferable that the amount be such that a coating layer 2' is formed.
[0099] The method of applying the coating liquid (2) to the covering layer 1' is not particularly limited, and the same method as the method of applying the coating liquid (1) in the above step (1) can be applied. Among these, the immersion method (dipping method, dip coating method) is preferable. Alternatively, in the case of a bioreactor or the like, the coating liquid (2) may be introduced or circulated to the polymer substrate in the bioreactor.
[0100] After the coating liquid (2) is applied to the coating layer 1', it is preferable to dry the coating film. Here, the drying conditions are not particularly limited as long as the solvent can be removed from the coating film, and hot air treatment using a dryer or the like may be performed, or natural drying may be performed. In the case of a bioreactor or the like, dry air may be introduced or circulated into the bioreactor. Furthermore, the pressure conditions during drying are also not particularly limited, and drying may be performed under normal pressure (atmospheric pressure), or under pressure or reduced pressure. For example, an oven, a reduced pressure dryer, or the like can be used as the drying means (apparatus), but in the case of natural drying, no particular drying means (apparatus) is required.
[0101] By the above method, coating layers 1' and 2' are successively formed on the polymer substrate to obtain substrate 2. Next, light is irradiated onto substrate 2 thus obtained to detect color-developed state 2 of substrate 2. Here, the light to be irradiated is appropriately selected depending on the type of fluorescent reagent. Specifically, the same light and irradiation conditions and methods as those in step (1) above can be used, and therefore a description thereof will be omitted here. It is particularly preferable to detect color-developed state 2 by the same method and conditions as those in step (1) above, because comparison of color-developed states is easier and more accurate.
[0102] The above-mentioned irradiation causes the fluorescent dye in the coating layer 1' to develop color, and this colored state (colored state 2) is detected (FIG. 1B).
[0103] Process (3) In this step, a substrate 3 is prepared, which is a polymer substrate having a coating layer containing a protein adsorbent and a fluorescent dye formed on at least one surface thereof, a sample containing a protein is introduced into the substrate 3 to obtain a substrate 4, and the substrate 4 is irradiated with light to detect the color-developed state 3 of the substrate 4. In the following, the "coating layer containing a protein adsorbent and a fluorescent dye" in step (3) is also referred to simply as "coating layer 1''.
[0104] Here, the polymer substrate is not particularly limited, and any substrate that requires evaluation of the coating state of the protein adsorbent or the adsorption state of the protein can be used in the same manner. Specifically, the same polymer substrate as in step (1) above can be used. The polymer substrate used in step (3) is preferably the same as that used in step (1) or (2) above, and is preferably the same as that used in steps (1) and (2) above.
[0105] A coating layer (coating layer 1 ″) containing a protein adsorbent and a fluorescent dye is formed on at least one surface of the polymer substrate to prepare a substrate 3 .
[0106] Here, coating layer 1" only needs to be formed on at least the surface that requires evaluation of the coating state of the protein adsorbent or the adsorption state of the protein, but is preferably formed on only one surface. Also, it is not necessary for a coating layer to be formed on the entire surface of the polymer substrate, and coating layer 1" is formed at least on the portion that requires evaluation of the coating state of the protein adsorbent or the adsorption state of the protein. Preferably, coating layer 1" is formed on the entire surface of the polymer substrate. From the standpoint of easier and more accurate comparison of the color development state, etc., it is preferable that coating layer 1" is formed in the same manner as coating layer 1 or 1', and it is preferably formed in the same manner as coating layers 1 and 1'.
[0107] The protein adsorbent used in coating layer 1" is not particularly limited as long as it has protein adsorbing ability. Specifically, the same protein adsorbent as in step (1) above can be used, and therefore a detailed explanation will be omitted here. From the standpoint of easier and more accurate comparison of color development states, it is preferable that the protein adsorbent used in coating layer 1" is the same as the protein adsorbent used in coating layer 1 or 1', and it is more preferable that it is the same as the protein adsorbent used in coating layers 1 and 1'.
[0108] There are no particular limitations on the fluorescent dye used in coating layer 1", so long as it is excited when irradiated with light such as ultraviolet light and emits specific fluorescence. Specifically, the same fluorescent dye as in step (1) above can be used, and therefore a detailed explanation is omitted here. From the standpoint of easier and more accurate comparison of the color development state, it is preferable that the fluorescent dye used in coating layer 1" is the same as the fluorescent dye used in coating layer 1 or 1', and it is more preferable that it is the same as the fluorescent dye used in coating layers 1 and 1'.
[0109] The method for forming coating layer 1" on the polymer substrate is not particularly limited, and known methods can be applied in the same manner or with appropriate modifications. Specifically, the same method as in step (1) above can be used, and therefore a description thereof will be omitted here. From the standpoint of easier and more accurate comparison of the color development state, it is preferable that coating layer 1" be formed on the polymer substrate by the same method as coating layer 1 or 1', and it is more preferable that coating layer 1" be formed on the polymer substrate by the same method as coating layers 1 and 1'.
[0110] That is, coating layer 1'' is preferably the same as coating layer 1 or coating layer 1', and more preferably the same as coating layer 1 and coating layer 1'.
[0111] Next, a sample containing protein is introduced (substrate 4) to substrate 3, which has coating layer 1'' formed on a polymer substrate. This causes the protein to be adsorbed to the protein adsorbent in coating layer 1''.
[0112] Here, the protein is not particularly limited, and examples thereof include the protein itself, a mixture of proteins such as serum, and cells. The method of introducing the sample is also not particularly limited, so long as the protein in the sample can come into contact with coating layer 1" (protein adsorbent). Specifically, the method includes impregnating substrate 3 with the sample, applying the sample to substrate 3, and the like. Alternatively, in the case of a bioreactor or the like, the sample may be introduced or circulated into substrate 3 (polymer substrate on which coating layer 1" is formed) in the bioreactor.
[0113] Next, the substrate 4 to which the protein-containing sample has been introduced is irradiated with light to detect the color-developed state 3 of the substrate 4. Here, the light to be irradiated is appropriately selected depending on the type of fluorescent reagent. Specifically, the same light and irradiation conditions and methods as those in the above step (1) can be used, and therefore a description thereof will be omitted here. From the viewpoint of easier and more accurate comparison of the color-developed states, it is preferable to detect the color-developed state 3 by the same method and conditions as those in the above step (1) or (2), and it is more preferable to detect the color-developed state 3 by the same method and conditions as those in the above steps (1) and (2).
[0114] The above-mentioned irradiation causes the fluorescent dye in the coating layer 1'' to develop color, and this colored state (colored state 3) is detected (FIG. 1C).
[0115] Process (4) In this step, a substrate 5 is prepared, which is a polymer substrate having a coating layer containing a protein adsorbent and a fluorescent dye formed on at least one surface thereof, a protein-containing sample is introduced into the substrate 5 to obtain substrate 6, a protein detection reagent is introduced into the substrate 6 to obtain substrate 7, and light is applied to the substrate 7 to detect the color development state 4 of the substrate 7. In the following, the "coating layer containing the protein adsorbent and the fluorescent dye" in step (4) is also referred to simply as "coating layer 1'"".
[0116] Here, the polymer substrate is not particularly limited, and any substrate that requires evaluation of the coating state of the protein adsorbent or the adsorption state of the protein can be used in the same manner. Specifically, the same polymer substrate as in step (1) above can be used. The polymer substrate used in step (4) is preferably the same as that used in steps (1), (2) or (3) above, and more preferably the same as that used in steps (1), (2) and (3) above.
[0117] A coating layer (coating layer 1'") containing a protein adsorbent and a fluorescent dye is formed on at least one surface of the polymer-based material to prepare a substrate 5.
[0118] Here, coating layer 1'" only needs to be formed on at least the surface that requires evaluation of the coating state of the protein adsorbent or the adsorption state of the protein, but is preferably formed on only one surface. Moreover, it is not necessary for a coating layer to be formed on the entire surface of the polymer substrate, and coating layer 1'" is formed at least on the portion that requires evaluation of the coating state of the protein adsorbent or the adsorption state of the protein. Preferably, coating layer 1'" is formed on the entire surface of the polymer substrate. From the standpoint of easier and more accurate comparison of the color development state, etc., it is preferable that coating layer 1'" is formed in the same manner as coating layer 1, coating layer 1' or coating layer 1", and it is more preferable that coating layer 1'" is formed in the same manner as coating layer 1, coating layer 1' and coating layer 1".
[0119] The protein adsorbent used in coating layer 1'" is not particularly limited as long as it has protein adsorbing ability. Specifically, the same protein adsorbent as in step (1) above can be used, and therefore a description thereof will be omitted here. From the standpoint of easier and more accurate comparison of color development states, it is preferable that the protein adsorbent used in coating layer 1'" is the same as the protein adsorbent used in coating layer 1, coating layer 1' or coating layer 1", and it is more preferable that the protein adsorbent used in coating layer 1, coating layer 1' and coating layer 1" is the same.
[0120] The fluorescent dye used in coating layer 1'" is not particularly limited as long as it is excited when irradiated with light such as ultraviolet light and emits inherent fluorescence. Specifically, the same fluorescent dye as in step (1) above can be used, and therefore a description thereof will be omitted here. From the standpoint of easier and more accurate comparison of the color development state, it is preferable that the fluorescent dye used in coating layer 1'" is the same as the fluorescent dye used in coating layer 1, coating layer 1' or coating layer 1", and it is more preferable that the fluorescent dye used in coating layer 1, coating layer 1' and coating layer 1" is the same.
[0121] The method for forming coating layer 1'" on the polymer substrate is not particularly limited, and known methods can be applied in the same manner or with appropriate modifications. Specifically, the same method as in step (1) above can be used, and therefore a description thereof will be omitted here. From the standpoint of easier and more accurate comparison of the color development state, it is preferable that coating layer 1'" be formed on the polymer substrate by the same method as coating layer 1, coating layer 1' or coating layer 1", and it is more preferable that coating layer 1'" be formed on the polymer substrate by the same method as coating layer 1, coating layer 1' and coating layer 1".
[0122] That is, coating layer 1'" is preferably the same as coating layer 1, coating layer 1' or coating layer 1", and more preferably the same as coating layer 1, coating layer 1' and coating layer 1".
[0123] Next, a sample containing protein is introduced (substrate 6) to substrate 5, which has coating layer 1''' formed on the polymer substrate. This causes the protein to be adsorbed to the protein adsorbent in coating layer 1'''.
[0124] Here, the method of introducing the sample is not particularly limited as long as the protein in the sample can come into contact with coating layer 1''' (protein adsorbent). Specifically, the same method as in step (3) above can be used, and therefore a description thereof will be omitted here. From the standpoint of easier and more accurate comparison of color development states, etc., it is preferable to introduce the sample by the same method as in step (3) above.
[0125] Next, a protein detection reagent is introduced to the substrate 6 to which the protein-containing sample has been introduced (substrate 7). The protein detection reagent used here is not particularly limited as long as it can detect the protein present in the substrate 6, and can be appropriately selected depending on the type of protein to be detected. Specifically, the same protein detection reagent as in step (2) above can be used, and therefore a description thereof will be omitted here. It is particularly preferable that the protein detection reagent is the same as the protein detection reagent used in the coating layer 2', from the standpoint of easier and more accurate comparison of the color development state, etc. That is, the protein detection reagent preferably has a quinoline structure, and is more preferably bicinchoninic acid (BCA).
[0126] Next, the substrate 7 to which the protein detection reagent has been introduced is irradiated with light to detect the color development state 4 of the substrate 7. Here, the light to be irradiated is appropriately selected depending on the type of fluorescent reagent. Specifically, the same light, irradiation conditions, and method as those in the above step (1) can be used, and therefore a description thereof will be omitted here. From the viewpoint of easier and more accurate comparison of the color development state, it is preferable that the type of light, and the irradiation conditions and method are the same as those in the above steps (1), (2), or (3), and more preferably the same as those in the above steps (1), (2), and (3).
[0127] The above-mentioned irradiation causes the fluorescent dye in the coating layer 1''' to develop color, and this colored state (colored state 4) is detected (FIG. 1D).
[0128] Process (5) In this step, the color state 1 detected in step (1), the color state 2 detected in step (2), or the color state 3 detected in step (3) is compared with the color state 4 detected in step (4) to evaluate the coating state of the protein adsorbent or the adsorption state of the protein.
[0129] As described above, when the same amount of protein is adsorbed, the degree of light emission (fluorescence intensity) of each coloring state 1 to 4 is higher in the order of coloring state 1, coloring state 3, coloring state 2, and coloring state 4 (coloring state 4<coloring state 2<coloring state 3<coloring state 1). Therefore, when the coloring state 4 has a lower fluorescence intensity than the coloring states 1, 2, or 3, it can be evaluated that the protein is adsorbed onto the substrate, or that the protein adsorbent is effectively present on the polymer substrate. That is, when the fluorescence intensity of the coloring state 4 is lower than that of the coloring states 1, 2, or 3, the coating state of the protein adsorbent and the adsorption state of the protein can be evaluated. In one embodiment of the present invention, when the coloring state 4 is generated by suppressing the absorption of light of the fluorescent dye compared to the coloring states 1, 2, or 3, it is evaluated that the protein is adsorbed onto the polymer substrate, or that the protein adsorbent is coated on the polymer substrate.
[0130] In this step, as described above, the difference between color state 4 and color state 1 or 3 is relatively large. For this reason, from the viewpoint of ease of comparison, it is preferable to compare color state 4 with color state 1 or 3, and more preferable to compare color state 1. Here, in the case of a bioreactor or the like in which a layer containing a protein adsorbent (cell adhesion factor) is formed in advance on a polymer substrate, the coating state of the protein adsorbent (cell adhesion factor) can be easily evaluated by a simple operation of circulating a coating liquid containing a fluorescent dye around the coating layer of the protein adsorbent (cell adhesion factor) on the polymer substrate (color state 1), circulating a coating liquid containing a fluorescent dye and a sample containing a protein in sequence (color state 3), or circulating a coating liquid containing a fluorescent dye, a sample containing a protein, and a coating liquid containing a protein detection reagent in sequence (color state 4).
[0131] After evaluating the coating state of the protein adsorbent or the adsorption state of the protein in step (4) above, each substrate (substrates 1, 2, 4, 7) may be washed with physiological saline, a buffer solution such as a phosphate buffer solution, ion-exchanged water, pure water, RO water, or other water.
[0132] According to the method of the present invention, the coating state of the protein adsorbent or the adsorption state of the protein can be visualized simply and quickly by comparing the coloring state after the introduction of the protein. For example, in the case of coloring state 4, when the fluorescence intensity is uniform over the entire surface of the polymer substrate, it can be evaluated that the protein adsorbent is uniformly present on the polymer substrate. Furthermore, the structure of the substrate is not limited in this method. Therefore, according to the method of the present invention, even in a culture vessel having a diversified and complicated structure (shape) such as the hollow fiber bioreactor described above, it is possible to evaluate by a non-destructive test whether or not the cell adhesion factor (protein adsorbent) has been uniformly arranged on the hollow fiber membrane.
[0133] In addition, the fluorescence intensity in the coloring states 3 to 4 is proportional to the amount of protein. That is, for a desired protein whose presence / absence is to be confirmed, a calibration curve of fluorescence intensity versus protein amount is prepared using the protein whose amount is known in advance, and the amount of protein in the sample can be measured based on this calibration curve and the fluorescence intensity in the coloring state 4. In detail, for a sample whose protein amount is known in advance, the same operation as in the above (step (4)) is performed to measure the fluorescence intensity of the protein, and a calibration curve of the protein amount and fluorescence intensity is prepared. Here, the method of measuring the fluorescence intensity is not particularly limited, and a known method can be used. For example, a fluorometer (fluorescence scanner) or an image processing system can be used. The calibration curve obtained is not dependent on external factors and is constant, so it is effective as a calibration curve. Therefore, by using this calibration curve, the amount of protein in the sample can be accurately measured. EXAMPLES
[0134] The effects of the present invention will be described using the following examples and comparative examples. However, the technical scope of the present invention is not limited to the following examples. In the following examples, unless otherwise specified, the operations were performed at room temperature (25°C). Furthermore, unless otherwise specified, "%" and "parts" mean "% by weight" and "parts by weight", respectively.
[0135] Preparation Example 1: Synthesis of protein adsorbent (pTHFA) 1 Polytetrahydrofurfuryl acrylate (pTHFA) 1 (weight average molecular weight: 600,000) was synthesized by the following method.
[0136] A 300 mL four-neck flask was charged with 90 g of methanol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.). Next, 60 g of tetrahydrofurfuryl acrylate (THFA) was added to the four-neck flask, stirred, and subjected to nitrogen bubbling for about 1 hour to prepare a 40 wt % THFA solution. Furthermore, 0.06 g of 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile) (FUJIFILM Wako Pure Chemical Industries, Ltd., V-70) was added to this THFA solution as a polymerization initiator, and a radical polymerization reaction was carried out in an oil bath at 45°C for 6 hours. After the reaction for a predetermined time, the reactant was transferred to a beaker and left to stand for 3 to 4 hours to precipitate the polymer (polytetrahydrofurfuryl acrylate), and the supernatant was discarded. Next, acetone was added to the beaker and stirred to dissolve the polymer, and the solution was dropped into cyclohexane to reprecipitate the polymer. The precipitate was collected and vacuum dried at 60°C overnight to obtain polytetrahydrofurfuryl acrylate (pTHFA) 1. The weight average molecular weight (Mw) of the obtained polytetrahydrofurfuryl acrylate (pTHFA) 1 was measured and found to be approximately 600,000.
[0137] Preparation Example 2: Synthesis of protein adsorbent (pTHFA) 2 Polytetrahydrofurfuryl acrylate (pTHFA)2 (weight average molecular weight: 200,000) was synthesized by the following method.
[0138] A 300 mL four-neck flask was charged with 190 g of methanol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.). Next, 60 g of tetrahydrofurfuryl acrylate (THFA) was added to the four-neck flask, stirred, and subjected to nitrogen bubbling for about 1 hour to prepare a 24 wt % THFA solution. Furthermore, 0.06 g of 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile) (FUJIFILM Wako Pure Chemical Industries, Ltd., V-70) was added to the THFA solution as a polymerization initiator, and radical polymerization reaction was carried out in an oil bath at 45°C for 6 hours. After the reaction for a predetermined time, the reactant was transferred to a beaker and left to stand for 3 to 4 hours to precipitate the polymer (polytetrahydrofurfuryl acrylate), and the supernatant was discarded. Next, acetone was added to the beaker and stirred to dissolve the polymer, and the solution was dropped into cyclohexane to reprecipitate the polymer. The precipitate was collected and vacuum dried at 60°C overnight to obtain polytetrahydrofurfuryl acrylate (pTHFA)2. The weight average molecular weight (Mw) of the obtained polytetrahydrofurfuryl acrylate (pTHFA)2 was measured and found to be approximately 200,000.
[0139] Preparation Example 3: Synthesis of protein adsorbent (pTHFA) 3 Polytetrahydrofurfuryl acrylate (pTHFA) 3 (weight average molecular weight: 100,000) was synthesized by the following method.
[0140] A 300 mL four-neck flask was charged with 220 g of methanol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.). Next, 30 g of tetrahydrofurfuryl acrylate (THFA) was added to the four-neck flask, stirred, and subjected to nitrogen bubbling for about 1 hour to prepare a 12 wt % THFA solution. Furthermore, 0.06 g of 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile) (FUJIFILM Wako Pure Chemical Industries, Ltd., V-70) was added to this THFA solution as a polymerization initiator, and a radical polymerization reaction was carried out in an oil bath at 45°C for 6 hours. After the reaction for a predetermined time, the reactant was transferred to a beaker and left to stand for 3 to 4 hours to precipitate the polymer (polytetrahydrofurfuryl acrylate), and the supernatant was discarded. Next, acetone was added to the beaker and stirred to dissolve the polymer, and the solution was dropped into cyclohexane to reprecipitate the polymer. The precipitate was collected and vacuum dried at 60°C overnight to obtain polytetrahydrofurfuryl acrylate (pTHFA)3. The weight average molecular weight (Mw) of the obtained polytetrahydrofurfuryl acrylate (pTHFA)3 was measured and found to be approximately 100,000.
[0141] Example 1 (Detection of color state 1) 3 g of pTHFA3 (Mw=100,000) (protein adsorbent) obtained in Production Example 3 was mixed with 300 g of methanol to obtain a pTHFA solution. The pTHFA solution was added with a polymerizable dye, fluorescent purple R13 (color: fluorescent purple, polymerizable group: methacryl group, acrylic equivalent: 1.2×10 3 g / eq, maximum absorption wavelength: 559 nm; Fujifilm Wako Pure Chemical Industries, Ltd.) (fluorescent dye) (20 mg) was added to prepare a dispersion.
[0142] 10 mL of this dispersion was cast into a petri dish and naturally dried in a draft for 4 hours to form a film (dry film thickness: 2 μm) (substrate A-1) containing pTHFA and R13 in the petri dish (petri dish A). The substrate A-1 was removed from the petri dish A to prepare substrate A.
[0143] This substrate A was irradiated with light having a wavelength of 254 nm and an intensity of 2.02 mW / cm 2 , Irradiation distance: 50mm, Accumulated light quantity: 2.02mJ / cm 2 The substrate A was irradiated with ultraviolet (UV) rays from a low-pressure mercury lamp under the irradiation conditions shown in Figure 2A.
[0144] (Detection of color state 2) Bicachininic acid (BCA), a protein detection reagent, is used as a copper ion chelator (composition: bicinchoninic acid Cu + Complex (manufactured by Thermo Fisher Scientific, product name: BCA Protein Assay) to a concentration of 1% by weight to prepare a BCA solution.
[0145] In the same manner as described above (detection of color development state 1), a substrate A-1 was prepared in a petri dish (petri dish A). 10 mL of the above BCA solution was cast into petri dish A and naturally dried in a draft for one day to form a BCA film (dry film thickness: 1 μm) (substrate B-1) on the substrate A-1. This substrate B-1 was removed from the petri dish to prepare substrate B.
[0146] This substrate B was irradiated with light having a wavelength of 254 nm and an intensity of 2.02 mW / cm 2 , Irradiation distance: 50mm, Accumulated light quantity: 2.02mJ / cm 2 The substrate B was irradiated with ultraviolet (UV) rays from a low-pressure mercury lamp under the irradiation conditions shown in Figure 2B.
[0147] (Detection of color state 3) Fetal bovine serum (FBS) was added to a phosphate buffer solution (PBS, pH=7.4) to a concentration of 10% by volume to prepare a protein solution.
[0148] Substrate A-1 was prepared in a petri dish (petri dish A) in the same manner as described above (detection of color development state 1). 50 mL of the above protein solution was poured into petri dish A and left for 30 minutes. After a predetermined time had passed, the protein solution was discarded from petri dish A (petri dish C-1). Petri dish C-1 was washed three times with 50 mL of phosphate buffered saline (PBS, pH 7.4) (petri dish C-2). After washing, petri dish C-2 was naturally dried for 4 hours in a fume hood to obtain substrate C-1 in a petri dish (petri dish C-3). Substrate C-1 was removed from petri dish C-3 to prepare substrate C.
[0149] For this substrate C, wavelength: 254 nm, irradiation intensity: 2.02 mW / cm 2 , Irradiation distance: 50mm, Accumulated light quantity: 2.02mJ / cm 2 The substrate C was irradiated with ultraviolet (UV) rays from a low-pressure mercury lamp under the irradiation conditions shown in Figure 2C.
[0150] (Detection of color state 4) A BCA solution was prepared in the same manner as above (detection of color development state 2).
[0151] Substrate C-1 was prepared in a petri dish (petri dish C-3) in the same manner as described above (detection of color development state 3). 10 mL of the BCA solution was added to petri dish C-3, and then incubated at 37°C for 1 hour to react FBS with BCA (substrate D-1). Substrate D-1 was removed from the petri dish to prepare substrate D.
[0152] This substrate D was irradiated with light having a wavelength of 254 nm and an irradiation intensity of 2.02 mW / cm 2 , Irradiation distance: 50mm, Accumulated light quantity: 2.02mJ / cm 2 The substrate D was irradiated with ultraviolet (UV) rays from a low-pressure mercury lamp under the irradiation conditions shown in FIG. 2D.
[0153] From FIG. 2, it can be seen that in color state 4 of substrate D, the fluorescence is significantly lost compared to color state 1 of substrate A, color state 2 of substrate B, and color state 3 of substrate C. Furthermore, the fluorescence is lost overall in substrate D. Therefore, it is considered that in substrate D, the protein adsorbent pTHFA is uniformly and entirely disposed. Furthermore, it is expected that the amount of protein in the coating layer can be measured by measuring the absorption spectrum (fluorescence intensity).
[0154] From the above results, it is considered that the method of the present invention can easily and quickly visualize the coating state of a protein adsorbent or the adsorption state of a protein. Furthermore, it is considered that the method of the present invention can visualize the coating state of a protein adsorbent or the adsorption state of a protein by non-destructive testing, even for a substrate having a complex structure.
[0155] Example 2 (Detection of color state 1) A PAES / PVP / PA porous hollow fiber membrane with an inner diameter of 215±10μm and a wall thickness of 50±5μm was placed in the housing, and the membrane area was 2.1m 2 Bioreactor 1 was prepared.
[0156] 3 g of pTHFA3 (Mw=100,000) (protein adsorbent) obtained in Production Example 3 was mixed with 300 g of methanol to obtain a pTHFA solution. The pTHFA solution was added with a polymerizable dye, fluorescent purple R13 (color: fluorescent purple, polymerizable group: methacryl group, acrylic equivalent: 1.2×10 3 g / eq, maximum absorption wavelength: 559 nm; Fujifilm Wako Pure Chemical Industries, Ltd.) (fluorescent dye) (20 mg) was added to prepare a dispersion.
[0157] The above dispersion was circulated in the lumen of the hollow fiber membrane of the bioreactor 1 at a flow rate of 20 ml / min for 30 minutes using a rotary pump, and then incubated at 37°C for 1 hour to form a coating layer X containing pTHFA and R13 on the inner surface of the hollow fiber membrane (bioreactor 1').
[0158] In this bioreactor 1', wavelength: 254 nm, irradiation intensity: 2.02 mW / cm 2 , Irradiation distance: 50mm, Accumulated light quantity: 2.02mJ / cm 2 The bioreactor 1' was irradiated with ultraviolet (UV) rays from a low-pressure mercury lamp under the irradiation conditions shown in FIG.
[0159] (Detection of color state 3) Fetal bovine serum (FBS) was added to a phosphate buffer solution (PBS, pH=7.4) to a concentration of 10% to prepare a protein solution.
[0160] The protein solution prepared above was circulated in the hollow fiber membrane of the bioreactor 1' prepared above with a rotary pump at a flow rate of 20 ml / min for 30 minutes, and then incubated at 37°C for 1 hour (bioreactor 2). 2 , Irradiation distance: 50mm, Accumulated light quantity: 2.02mJ / cm 2 The bioreactor 2 was irradiated with ultraviolet (UV) rays from a low-pressure mercury lamp under the irradiation conditions shown in FIG.
[0161] (Detection of color state 4) Bicachininic acid (BCA), a protein detection reagent, is used as a copper ion chelator (composition: bicinchoninic acid Cu + Complex (manufactured by Thermo Fisher Scientific, product name: BCA Protein Assay) to a concentration of 10% by weight to prepare a BCA solution.
[0162] Bioreactor 2 was prepared in the same manner as above (detection of color development state 3). The BCA solution prepared above was circulated in the hollow fiber membrane of this bioreactor 2 with a rotary pump at a flow rate of 20 ml / min for 30 minutes, and then the bioreactor was kept in an incubator at 37°C for 1 hour (bioreactor 3). This bioreactor 3 was irradiated with light having a wavelength of 254 nm and an irradiation intensity of 2.02 mW / cm. 2 , Irradiation distance: 50mm, Accumulated light quantity: 2.02mJ / cm2 The bioreactor 3 was irradiated with ultraviolet (UV) rays from a low-pressure mercury lamp under the irradiation conditions shown in FIG.
[0163] From FIG. 3, it can be seen that in color state 4 of bioreactor 3, the fluorescence has been significantly lost compared to color state 1 of bioreactor 1' and color state 3 of bioreactor 2. Furthermore, in color state 4 of bioreactor 3, a pink area is observed in the upper left part. It is presumed that no protein is adsorbed in this area (i.e., the protein adsorbent is not sufficiently arranged). Therefore, it is expected that the method of the present invention will make it possible to easily confirm the coating state of the protein adsorbent. Furthermore, it is expected that the amount of protein in the coating layer will be able to be measured by measuring the absorption spectrum (fluorescence intensity).
[0164] In addition, from the above results, it is considered that the method of the present invention can easily and quickly visualize the coating state of a protein adsorbent or the adsorption state of a protein, and further, it is considered that the method of the present invention can visualize the coating state of a protein adsorbent or the adsorption state of a protein by non-destructive testing, even for a substrate having a complex structure.
[0165] Although the embodiments of the present invention have been described and illustrated in detail, the disclosed embodiments are made for purposes of illustration and example only and are not limiting, and the scope of the present invention should be interpreted by the appended claims.
[0166] The disclosure of Japanese Patent Application No. 2019-172049, filed on September 20, 2019, is hereby incorporated by reference in its entirety. [Explanation of symbols]
[0167] 10...polymer base material, 20...a coating layer containing a protein adsorbent and a fluorescent dye; 30... a coating layer containing a protein detection reagent; 31...Protein detection reagent, 40…protein, 50...Light of a specific wavelength that causes a fluorescent dye to become excited.
Claims
1. A substrate 1 is prepared, which is a polymer substrate having a coating layer formed on at least one surface thereof, the coating layer containing a protein adsorbent and a fluorescent dye, and the substrate 1 is irradiated with light to detect a color development state 1 of the substrate 1; A substrate 2 is prepared in which a coating layer containing a protein adsorbent and a fluorescent dye and a coating layer containing a protein detection reagent are successively formed on at least one surface of a polymer substrate, and a color development state 2 of the substrate 2 is detected by irradiating the substrate 2 with light; A substrate 3 is prepared in which a coating layer containing a protein adsorbent and a fluorescent dye is formed on at least one surface of a polymer substrate, a sample containing a protein is introduced into the substrate 3 to obtain a substrate 4, and a color development state 3 of the substrate 4 is detected by irradiating the substrate 4 with light; A substrate 5 is prepared in which a coating layer containing a protein adsorbent and a fluorescent dye is formed on at least one surface of a polymer substrate, a sample containing a protein is introduced into the substrate 5 to obtain a substrate 6, a protein detection reagent is introduced into the substrate 6 to obtain a substrate 7, and a color development state 4 of the substrate 7 is detected by irradiating the substrate 7 with light; comparing the color-developed state 1, 2 or 3 with the color-developed state 4 to evaluate the coating state of the protein adsorbent or the adsorption state of the protein; The protein adsorbent has the following formula (1): 【Chemistry 1】 In formula (1), R 1 is a hydrogen atom or a methyl group, and R 2 is a group represented by the following formula (1-1) or the following formula (1-2): 【Chemistry 2】 In formula (1-1) and formula (1-2), R 3 is an alkylene group having 1 to 3 carbon atoms; The furfuryl (meth)acrylate-derived structural unit is A method for evaluating the coating state of a protein adsorbent or the adsorption state of a protein, wherein the fluorescent dye has a methacryl group.
2. The method of claim 1, wherein a protein is evaluated as being adsorbed onto a polymer substrate or a protein adsorbent is coated onto a polymer substrate when the color-formed state 4 is produced by suppressing the absorption of light by the fluorescent dye compared to the color-formed states 1, 2 or 3.
3. The method of claim 1 or 2, wherein the protein detection reagent has a quinoline structure.
4. The method of claim 3 , wherein the protein detection reagent is bicinchoninic acid.
5. The method according to any one of claims 1 to 4, wherein the fluorescent dye is a xanthene dye.
Citation Information
Patent Citations
Light-fixing solid-phase carrier and manufacturing method therefor
JP2008170241A
Multiligand scavengers and related compositions, methods and systems
JP2011525187A
Cell proliferation
JP2018519800A
Porous substrate for culturing pluripotent stem cells and method for culturing pluripotent stem cells while maintaining undifferentiation
JP2019080561A