Negative plate and secondary battery

The dual-layer negative electrode plate design in lithium-ion batteries improves lithium ion transport and prevents precipitation, enhancing capacity retention and stability through controlled curvature and tortuosity.

JP7595149B2Active Publication Date: 2024-12-05BYD CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023510320
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-08-13
Filing Date
2021-04-15
Publication Date
2024-12-05
Estimated Expiration
2041-04-15

AI Technical Summary

Technical Problem

Lithium-ion batteries with single-coated negative electrodes face issues of non-uniform curvature leading to low lithium ion diffusion rates, fast cycle decay, and lithium precipitation, which affects capacity and safety.

Method used

A negative electrode plate design with two active material layers, where the second layer has a higher bending degree than the first, ensuring a tortuous path for electrolyte infiltration and uniform lithium insertion, while the first layer maintains solid phase transport efficiency.

Benefits of technology

The dual-layer design enhances capacity retention and stability by facilitating efficient lithium ion transport, preventing precipitation, and maintaining high capacity under high-rate cycling conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007595149000002
    Figure 0007595149000002
  • Figure 0007595149000003
    Figure 0007595149000003
  • Figure 0007595149000001
    Figure 0007595149000001
Patent Text Reader

Abstract

The negative electrode plate (100) includes a current collector (10), a first negative electrode active material layer (11), and a second negative electrode active material layer (12) sequentially provided on the current collector (10). The degree of bending of the first negative electrode active material layer (11) and the degree of bending of the second negative electrode active material layer (12) satisfy 1 < t1 ≤ 5, 1 < t2 ≤ 5, and 0.5 ≤ t2 - t1 ≤ 3.2, where t1 represents the degree of bending of the first negative electrode active material layer (11), t2 represents the degree of bending of the second negative electrode active material layer (12), and t2 - t1 represents the difference between the degree of bending of the second negative electrode active material layer (12) and the degree of bending of the first negative electrode active material layer (11).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] (CROSS REFERENCE TO RELATED APPLICATIONS) This application claims priority to Chinese Patent Application No. “202010811820.4” filed by BYD Company Limited on August 13, 2020, entitled “Negative Plate and Secondary Battery.”

[0002] The present application relates to the field of batteries, and in particular to negative plates and secondary batteries. [Background technology]

[0003] With the development of economy and science and technology, from portable electronic devices (mobile phones, tablet computers, notebook computers) to unmanned aerial vehicles and electric vehicles, these industries are in high demand for energy storage devices with higher energy density and higher power density. At present, in lithium ion batteries based on anodes such as graphite, the anode active material layer is a single coating, and the bending degree of the single anode active material layer after rolling is not uniform, and the bending degree of the surface layer away from the current collector is small. Therefore, when the battery is charged and discharged at a high rate, the diffusion speed of the liquid phase of lithium ions in the active material layer away from the current collector is low, which makes it difficult for the battery to achieve high capacity, causes fast cycle decay, and is prone to lithium precipitation on the surface of the negative plate, which greatly affects cycle performance and brings about potential safety risks. Summary of the Invention

[0004] The present application aims to solve at least one of the technical problems in the prior art by providing a negative electrode plate that can improve the capacity retention rate of a battery and prevent the occurrence of lithium precipitation in the battery.

[0005] The negative electrode plate includes a current collector, and a first negative electrode active material layer and a second negative electrode active material layer sequentially provided on the current collector. The degrees of bending of the first negative electrode active material layer and the second negative electrode active material layer satisfy 1 < t1 ≤ 5, 1 < t2 ≤ 5, and 0.5 ≤ t2 - t1 ≤ 3.2. In the formula, t1 represents the degree of bending of the first negative electrode active material layer, t2 represents the degree of bending of the second negative electrode active material layer, and t2 - t1 represents the difference between the degree of bending of the second negative electrode active material layer and the degree of bending of the first negative electrode active material layer.

[0006] Thus, by controlling the degrees of bending of the upper and lower two negative electrode active material layers so as to satisfy the above conditions, under the conditions of the same surface density and press density, the second active material layer with a higher degree of bending can provide more void structures. Therefore, during the cycling process of the battery, the electrolyte can infiltrate, the capacity of insertable lithium can be improved, and it helps to avoid the occurrence of lithium deposition phenomenon on the surface of the negative electrode plate. At the same time, the first active material layer with a smaller degree of bending has a compact structure, so it helps to maintain the solid-phase transport efficiency of lithium ions during the cycling process of the battery. Due to the appropriate difference in the degrees of bending between the two, when the battery cycles at a high rate, the capacity retention rate is high and the lithium deposition phenomenon does not occur.

[0007] The secondary battery includes the negative electrode plate as described above. When the secondary battery cycles at a high rate, it can maintain a high capacity and has high cycle stability.

[0008] Some of the additional aspects and advantages of the present application are shown in the following description, and some will become clear in the following description or will be understood by implementing the present application.

Brief Description of the Drawings

[0009] The above and / or additional aspects and advantages of the present application will become clear and easier to understand by describing the embodiments with reference to the following drawings.

[0010] [Figure 1] It is a schematic structural diagram of a negative electrode plate according to an embodiment of the present application. [Diagram 2]3 is a cycle curve at room temperature of a battery manufactured using a negative electrode plate according to an embodiment of the present invention and a negative electrode plate according to a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, the embodiments of the present application will be described in detail, and examples of the embodiments are shown in the drawings, and the same or similar reference numerals throughout indicate the same or similar parts or parts having the same or similar functions. The embodiments described below with reference to the drawings are illustrative and are only for interpreting the present application, and should not be understood as limiting the present application.

[0012] In addition, in the description of this application, the orientations or positional relationships indicated by the terms "center," "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," "outer," etc. are based on the orientations or positional relationships shown in the drawings, and are merely intended to facilitate and simplify the description of this application, and do not indicate or suggest that the devices or parts shown must have a specific orientation and be configured and operate in a specific orientation, and therefore should not be understood as limiting this application.

[0013] It should be noted that the terms "first" and "second" are for descriptive purposes only and should not be understood to indicate or suggest a relative importance or to imply a number of the technical features depicted. Thus, a feature qualified with "first" or "second" may explicitly or implicitly include one or more of the feature. In the description of this application, unless otherwise specified, "plurality" means two or more.

[0014] Hereinafter, the embodiments of the present application will be described with reference to the drawings.

[0015] As shown in FIG. 1, the negative electrode plate 100 according to the embodiment of the present application includes a current collector 10, a first negative electrode active material layer 11 and a second negative electrode active material layer 12 sequentially provided on the current collector. The degree of bending of the first negative electrode active material layer 11 and the second negative electrode active material layer 12 satisfies 1 < t1 ≦ 5, 1 < t2 ≦ 5, and 0.5 ≦ t2 - t1 ≦ 3. In the formula, t1 represents the degree of bending of the first negative electrode active material layer 11, t2 represents the degree of bending of the second negative electrode active material layer 12, and t2 - t1 represents the difference between the degree of bending of the second negative electrode active material layer 12 and the degree of bending of the first negative electrode active material layer 11.

[0016] In the present application, the degree of bending indicates the ratio of the lithium ion transport path to the layer thickness in the active material layer. In the above negative electrode plate, the degree of bending t2 of the second negative electrode active material layer 12 on the side away from the current collector 10 is greater than the degree of bending t1 of the first negative electrode active material layer 11 close to the current collector. Under the conditions of the same surface density and press density, the second negative electrode active material layer 12 with a high degree of bending can provide more void structures. Therefore, when the battery is in the cycle process, it is more infiltrated by the electrolyte, promoting the liquid-phase transport of lithium ions, improving the capacity of insertable lithium, and helping to avoid the occurrence of lithium deposition phenomenon at the interface between the negative electrode plate and the electrolyte. At the same time, the first active material layer 11 with a small degree of bending has a compact structure, which helps to maintain the solid-phase transport of lithium ions in the cycle process of the battery. Overall, due to the negative electrode plate having two layers of active material layers, when the battery manufactured with this negative electrode plate is charged, lithium is uniformly inserted into the negative electrode. Therefore, the battery has a high capacity and energy density, and has a high capacity retention rate in the cycle process, and the capacity decay is small.

[0017] Generally, the greater the degree of bending, the sparser the coating, facilitating the transport of lithium ions. However, if the degree of bending is too large, the electronic conductivity drops sharply, increasing the impedance of the battery. In the examples of the present application, the degree of bending t2 of the second negative electrode active material layer 12 and the degree of bending t1 of the first negative electrode active material layer 11 are controlled so that both are within the range of (1,5), and both of these two negative electrode active material layers have excellent ionic conductivity and electronic conductivity. In addition, under the condition that the areal density and press density are constant, if t1 and t2 satisfy 0.5≦t2−t1≦3.2, the capacity retention rate when the battery is cycled at a high rate and the cycle stability are excellent. If t2-t1>3.2, lithium ions will mainly react in the second negative electrode active material layer, resulting in loss of the total capacity of the battery; if t2-t1<0.5, t2 and t1 are generally small due to the requirements of the surface density and press density of the negative electrode plate, and the second negative electrode active material layer is difficult to infiltrate, making it difficult for lithium ions to diffuse into the liquid phase in the entire negative electrode plate, which is likely to cause lithium precipitation, and the cycle curve of the battery at high rate will have a short-term sudden drop. Therefore, only when t2-t1 is controlled within an appropriate range can the battery have a high capacity retention rate and no lithium precipitation phenomenon occur when cycling at high rate.

[0018] In one embodiment of the present application, 0.5≦t2−t1≦3. In another embodiment of the present application, 1≦t2−t1≦3.

[0019] In general, the larger the D50 particle size of the active material, the greater the degree of tortuosity of the active material layer. In one embodiment of the present application, the first negative electrode active material layer 11 contains a first negative electrode active material, the second negative electrode active material layer 12 contains a second negative electrode active material, and the D50 particle size of the second negative electrode active material is larger than the D50 particle size of the first negative electrode active material, and the D50 particle size of both the first negative electrode active material and the second negative electrode active material are within the range of 8 μm to 20 μm. That is, the D50 particle size of the negative electrode active material in the second negative electrode active material layer 12 away from the current collector 10 (or "closer to the electrolyte") is set to be large, and the D50 particle size of the negative electrode active material in the first negative electrode active material layer 11 closer to the current collector 10 (or "away from the electrolyte") is set to be small. In this way, the second negative electrode active material layer 12 closer to the electrolyte is more infiltrated by the electrolyte during the battery cycle process, improving the battery's intercalable lithium capacity and preventing the occurrence of lithium precipitation, so that the battery has high cycle stability and can further ensure consistency in the lithium deintercalation / intercalation rates of the two negative electrode active material layers.

[0020] The D50 particle size of the first negative electrode active material is 8 μm to 13 μm, and the D50 particle size of the second negative electrode active material is 13 μm to 20 μm. The difference between the D50 particle size of the second negative electrode active material and the D50 particle size of the first negative electrode active material is 3 μm or more, which can better ensure that the difference between the tortuosity of the second negative electrode active material layer and the tortuosity of the first negative electrode active material layer is within an appropriate range, and can further contribute to the consistency of the lithium desorption / insertion rate of the two negative electrode active material layers. For example, the D50 particle size of the second negative electrode active material and the D50 particle size of the first negative electrode active material may be 13 μm and 8 μm, 15 μm and 13 μm, or 17 μm and 13 μm, respectively.

[0021] In another embodiment of the present application, the curvature of the first and second negative electrode active material layers may be changed by laser etching, a pore former, stepwise rolling, or the like.

[0022] In the present application, both the first negative electrode active material layer 11 and the second negative electrode active material layer 12 contain a conductive agent and a binder. That is, the first negative electrode active material layer 11 contains a first negative electrode active material, a conductive agent, and a binder, and the second negative electrode active material layer 12 contains a second negative electrode active material, a conductive agent, and a binder. The contents of the conductive agent, the binder, and the negative electrode active material are not limited. The weight of the first negative electrode active material accounts for 90% to 98% of the weight of the first negative electrode active material layer 11, and the weight of the second negative electrode active material accounts for 90% to 98% of the weight of the second negative electrode active material layer 12. This allows the negative electrode plate 100 to have a high amount of the negative electrode active material carried, thereby improving the energy density of the battery.

[0023] The thickness of the first negative electrode active material layer 11 and the thickness of the second negative electrode active material layer 12 are both within the range of 30 μm to 100 μm. If the thickness of each negative electrode active material layer is greater than 100 μm, the energy density of the battery is improved but the power density is reduced, and if the thickness is less than 30 μm, the power density of the battery is improved but the energy density is reduced. The thickness of the first negative electrode active material layer 11 and the thickness of the second negative electrode active material layer 12 are both within the range of 40 μm to 75 μm. The thickness of the first negative electrode active material layer 11 and the thickness of the second negative electrode active material layer 12 may or may not be equal. The sum of the thicknesses of the first negative electrode active material layer 11 and the second negative electrode active material layer 12 is within the range of 80 μm to 150 μm.

[0024] In general, the greater the porosity of the active material layer, the greater the degree of curvature of the active material layer. However, if the porosity of the active material layer is greater than 40%, the energy density of the battery is significantly reduced. The porosity of the first negative electrode active material layer 11 is 20% to 30%, the porosity of the second negative electrode active material layer 12 is 30% to 40%, and the porosity of the second negative electrode active material layer is greater than the porosity of the first negative electrode active material layer. For example, the porosities of the first negative electrode active material layer 11 and the second negative electrode active material layer 12 may be 20% and 30%, 25% and 36%, or 30% and 40%, respectively.

[0025] The surface density of the first negative electrode active material layer 11 and the surface density of the second negative electrode active material layer 12 are both 0.3 g / dm 2 ~0.8g / dm 2 is within the range.

[0026] The press density of the negative electrode plate 100 is 1.45-1.70 g / cm 3 It is.

[0027] In the present application, the current collector 10 may be a material applied as a current collector for a negative electrode plate, including but not limited to metal foil, alloy foil, composite foil of metal and polymer, etc. For example, it may be copper, nickel, stainless steel, etc. Preferably, the current collector 10 is a copper foil. The current collector 10 may be etched or roughened to form a secondary structure to facilitate intimate and effective contact with the first negative electrode active material layer 11.

[0028] The first and second negative electrode active materials are independently selected from one or more of graphite, soft carbon, hard carbon, lithium titanate, silicon-based materials, and tin-based materials. That is, the first and second negative electrode active materials may be made of the same material or different materials. Examples of silicon-based materials include silicon alone, silicon alloys, silicon oxides, and silicon carbon composite materials. Examples of tin-based materials include tin alone, tin oxides, and tin-based alloys.

[0029] In the present application, the binder and the conductive agent in the first negative electrode active material layer 11 and the second negative electrode active material layer 12 are not particularly limited, and may be any material commonly used in the field. For example, the binder may include one or more of styrene butadiene rubber (SBR), polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyvinyl alcohol (PVA), polyacrylonitrile (PAN), polyimide (PI), polyacrylic acid (PAA), polyacrylate (e.g., polymethyl methacrylate, polymethyl acrylate, polyethyl acrylate, etc.), polyolefin (e.g., polypropylene, polyethylene, etc.), carboxymethyl cellulose (CMC), sodium alginate, etc. For example, the conductive agent includes one or more of branched chain conductive agents, one-dimensional chain / linear conductive agents, two-dimensional plate-shaped conductive agents, three-dimensional spherical conductive agents, etc., but is not limited thereto. Specifically, the conductive agent may include one or more of polyacetylene, polythiophene, polypyrrole, polyaniline, carbon fiber, carbon nanotube, graphite, graphene, conductive carbon black, furnace black, mesocarbon microbeads, etc. Specifically, the conductive carbon black may include acetylene black, Ketjen black, Supper P, 350G carbon black, etc. Graphite may include natural graphite (e.g., flaky graphite, expanded graphite, etc.) and artificial graphite (e.g., KS-6, spherical graphite), etc.

[0030] The negative electrode plate according to the first aspect of the present application may be manufactured by a method known in the art. For example, the manufacturing method of the negative electrode plate may include the steps of applying a first negative electrode active material slurry and a second negative electrode active material slurry to one surface of a current collector, drying and pressing the slurry, and then sequentially forming a first negative electrode active material layer and a second negative electrode active material layer on the current collector.

[0031] Specifically, the coating method may include one or a combination of methods selected from the group consisting of drop coating, brush coating, spray coating, dip coating, knife coating, and spin coating. The coating time and temperature may be set according to actual needs, and the coating operation may be performed in a dry room or in a protective atmosphere. The first negative electrode active material slurry may include a first negative electrode active material, a conductive agent, a binder, and a solvent, and the second negative electrode active material slurry may include a second negative electrode active material, a conductive agent, a binder, and a solvent. In one embodiment of the present application, the first negative electrode active material slurry and the second negative electrode active material slurry are coated in sequence using a two-layer coating die head.

[0032] An embodiment of the present application further provides a secondary battery including the negative electrode plate.

[0033] The secondary battery further includes a positive electrode plate, a separator disposed between the positive electrode plate and the negative electrode plate, and an electrolyte.

[0034] The positive electrode plate may be a positive electrode plate applied to a secondary battery, specifically including, but not limited to, one or a combination of a lithium iron phosphate positive electrode plate, a nickel-cobalt-manganese ternary positive electrode plate, a nickel-cobalt-aluminum ternary positive electrode plate, a lithium cobalt oxide positive electrode plate, and a lithium manganese oxide positive electrode plate.

[0035] The separator may be various separators applied to secondary batteries in this field, specifically including, but not limited to, one or more of polyethylene, polypropylene, nonwoven fabric, polyfiber material, etc., and multi-layer composite films thereof, etc. The electrolyte includes an electrolyte salt and an organic solvent, and the specific types and compositions of the electrolyte salt and the organic solvent are all common choices in the battery field and can be selected according to actual needs.

[0036] The technical solutions of the present application are further described below with reference to several specific embodiments. EXAMPLES

[0037] The negative electrode plate includes a copper foil having a thickness of 6 μm, and a first negative electrode active material layer and a second negative electrode active material layer disposed in that order on the copper foil, the first negative electrode active material layer having a tortuosity of 3.42, the second active material layer having a tortuosity of 4.55, and the difference between the tortuosity of the second active material layer and the tortuosity of the first negative electrode active material layer being 1.13.

[0038] In Example 1, the D50 particle size of the negative electrode active material (specifically, graphite) in the first negative electrode active material layer was 11 μm, the D50 particle size of the negative electrode active material (specifically, graphite) in the second negative electrode active material layer was 17 μm, and the first negative electrode active material layer had a thickness of 40 μm and an areal density of 0.675 g / dm 2 The second negative electrode active material layer has a thickness of 42 μm and an areal density of 0.688 g / dm 2 It is.

[0039] The method for producing the negative electrode plate includes the steps of: (1) A negative electrode active material (specifically, graphite), a conductive agent Supper P, carboxymethyl cellulose (CMC), styrene butadiene rubber (SBR), and water were prepared into two slurries in a weight ratio of 100:2:1.6:1.8:128, the solid content of each of the two slurries was 45.2%, the slurry viscosity of each of the two slurries was 2300 cps, the D50 particle size of the graphite in the first negative electrode active material slurry was 11 μm, and the D50 particle size of the graphite in the second negative electrode active material slurry was 17 μm, (2) Using a two-layer coating die head, the negative electrode active material slurry and the second negative electrode active material slurry were uniformly coated in sequence on a copper foil having a thickness of 6 μm, baked in an oven at 120° C. for 15 min, cooled, and then rolled at 2 MPa to obtain a negative electrode plate. The negative electrode plate had an areal density of 1.363 g / dm 2 and the press density is 1.60 g / cm 3 The sum of the thicknesses of the two active material layers is 82 μm.

[0040] In this application, the degree of curvature of each active material layer in Example 1 is measured using FIB-SEM (focused particle beam-scanning electron microscope), and the measurement method is to FIB slice the measurement sample, slice it once for every 50 nm thickness, and then perform SEM scanning. Repeat multiple times, and reconstruct all the scanning results in three dimensions to obtain a 3D image of the electrode plate, which is then analyzed by specialized software to obtain the degree of curvature. EXAMPLES

[0041] The negative electrode plate includes a copper foil having a thickness of 6 μm, and a first negative electrode active material layer and a second negative electrode active material layer disposed in that order on the copper foil, the first negative electrode active material layer having a tortuosity of 1.88, the second active material layer having a tortuosity of 4.06, and the difference between the tortuosity of the second active material layer and the tortuosity of the first negative electrode active material layer being 2.18.

[0042] In Example 2, the D50 particle size of the negative electrode active material (specifically, graphite) in the first negative electrode active material layer is 8 μm, and the D50 particle size of the negative electrode active material (specifically, graphite) in the second negative electrode active material layer is 15 μm. EXAMPLES

[0043] The negative electrode plate includes a copper foil having a thickness of 6 μm, and a first negative electrode active material layer and a second negative electrode active material layer disposed in that order on the copper foil, the first negative electrode active material layer having a tortuosity of 1.75, the second active material layer having a tortuosity of 4.92, and the difference between the tortuosity of the second active material layer and the tortuosity of the first negative electrode active material layer being 3.17.

[0044] In Example 3, the D50 particle size of the negative electrode active material (specifically, graphite) in the first negative electrode active material layer is 8 μm, and the D50 particle size of the negative electrode active material (specifically, graphite) in the second negative electrode active material layer is 20 μm. EXAMPLES

[0045] The negative electrode plate includes a copper foil having a thickness of 6 μm, and a first negative electrode active material layer and a second negative electrode active material layer disposed in that order on the copper foil, the first negative electrode active material layer having a tortuosity of 2.33, the second active material layer having a tortuosity of 3.02, and the difference between the tortuosity of the second active material layer and the tortuosity of the first negative electrode active material layer being 0.69.

[0046] In Example 4, the D50 particle size of the negative electrode active material (specifically, graphite) in the first negative electrode active material layer is 9 μm, and the D50 particle size of the negative electrode active material (specifically, graphite) in the second negative electrode active material layer is 11 μm. EXAMPLES

[0047] The negative electrode plate includes a copper foil having a thickness of 6 μm, and a first negative electrode active material layer and a second negative electrode active material layer disposed in that order on the copper foil, the first negative electrode active material layer having a tortuosity of 1.81, the second active material layer having a tortuosity of 4.62, and the difference between the tortuosity of the second active material layer and the tortuosity of the first negative electrode active material layer being 2.81.

[0048] In Example 5, the D50 particle size of the negative electrode active material (specifically, graphite) in the first negative electrode active material layer is 8 μm, and the D50 particle size of the negative electrode active material (specifically, graphite) in the second negative electrode active material layer is 17 μm.

[0049] In order to highlight the beneficial effects of the examples of the present application, the following Comparative Examples 1 to 4 are particularly provided. Comparative Example 1

[0050] The negative electrode plate includes a copper foil having a thickness of 6 μm, and a first negative electrode active material layer and a second negative electrode active material layer disposed in that order on the copper foil, the first negative electrode active material layer having a tortuosity of 2.97, the second active material layer having a tortuosity of 3.11, and the difference between the tortuosity of the second active material layer and the tortuosity of the first negative electrode active material layer being 0.14.

[0051] In Comparative Example 1, the D50 particle size of the negative electrode active material (specifically, graphite) in the first negative electrode active material layer is 14 μm, and the D50 particle size of the negative electrode active material (specifically, graphite) in the second negative electrode active material layer is 15 μm. Comparative Example 2

[0052] The negative electrode plate includes a copper foil having a thickness of 6 μm, and a first negative electrode active material layer and a second negative electrode active material layer disposed in that order on the copper foil, the first negative electrode active material layer having a tortuosity of 3.90, the second active material layer having a tortuosity of 2.01, and the difference between the tortuosity of the second active material layer and the tortuosity of the first negative electrode active material layer being −1.89.

[0053] In Comparative Example 2, the D50 particle size of the negative electrode active material (specifically, graphite) in the first negative electrode active material layer is 14 μm, and the D50 particle size of the negative electrode active material (specifically, graphite) in the second negative electrode active material layer is 9 μm. Comparative Example 3

[0054] The negative electrode plate includes a copper foil having a thickness of 6 μm, and a first negative electrode active material layer and a second negative electrode active material layer disposed in that order on the copper foil, the first negative electrode active material layer having a tortuosity of 1.18, the second active material layer having a tortuosity of 5.22, and the difference between the tortuosity of the second active material layer and the tortuosity of the first negative electrode active material layer being 4.04. Comparative Example 4

[0055] The negative electrode plate includes a copper foil having a thickness of 6 μm and a negative electrode active material layer having a thickness of 82 μm disposed on the copper foil. The graphite in the active material layer has a D50 particle size of 15 μm. The degree of curvature of the negative electrode active material layer is 3.06, and the degree of curvature of the surface layer is slightly smaller.

[0056] In order to strongly support the beneficial effects of the technical solutions of the embodiments of the present application, the negative plate in each of the above examples is manufactured into a corresponding battery by the following method: in a glove box, the positive plate, the separator and the negative plate are stacked in order to obtain a bare cell, and then the cell is put into a case, baked and dried, and then an electrolyte specially for ternary batteries is injected, welded and sealed, and a battery is obtained through processes such as high temperature aging, chemical formation and aging.

[0057] For each battery manufactured with the negative electrode plate in each of the above examples, the following direct current resistance (DCIR) measurement and cycle performance measurement were performed. The results of the DCIR measurement are summarized in Table 1, the results of the cycle performance measurement are summarized in Table 1, and the cycle curves of some examples are shown in Figure 2.

[0058] DCIR measurement method: 1) At room temperature (25°C), discharge the battery at 0.2C until the cutoff voltage is 2.5V, leave it for 30 minutes, charge it at 0.2C until the cutoff voltage is 4.2V at room temperature, leave it for 30 minutes, and discharge it at 0.2C until the cutoff voltage is 2.5V at room temperature to calculate the initial capacity C0 of the battery, and adjust the battery's state of charge (SOC) to 50% SOC by charging it at 0.2C (50% C0), 2) leave it at -10°C for 12 hours, and measure the DCIR after charging at a rate of 1C for 30 seconds.

[0059] Cycle performance measurement method: 1) Charge: Charge at 25°C at a constant current of 1C to 4.1V, then charge at 0.5C to 4.15V, and then charge at 0.2C to 4.2V, and leave for 30 minutes; 2) Discharge: Discharge at a constant current of 1C to 2.5V, and leave for 30 minutes; 3) End condition: Cycle 500 times in this manner. [Table 1]

[0060] As can be seen from Table 1, the DCIR values ​​of the batteries manufactured with the negative plates of the examples of the present application are much lower than those of the comparative examples, which explains that the batteries of the examples of the present application have excellent power performance.

[0061] As can be seen from FIG. 2 and Table 1, the capacity retention rates of the batteries manufactured using the negative electrode plates of Examples 1 and 2 were the highest, and the capacity retention rates of the batteries manufactured using the negative electrode plates of Examples 3 to 5 were lower than those of Examples 1 and 2, but were all much higher than the capacity retention rates of the batteries manufactured using the negative electrode plates of each comparative example. The reason is that the tortuosity of the two active material layers in the negative electrodes of the examples of the present application all meets 0.5≦t2-t1≦3.2, so that under high-rate conditions, the upper second negative electrode active material layer can provide more void structure, which is infiltrated by the electrolyte and helps to promote the liquid-phase transport of liquid-phase lithium ions, and the first active material layer has a more compact structure, which helps to maintain the solid-phase transport and electron transport of lithium ions during cycling. When t2-t1>3 (Comparative Example 3), the capacity retention rate of the battery is reduced, which is because the lithium ions mainly react in the second negative electrode active material layer, and the solid-phase conductivity of the lithium ions in the first negative electrode active material layer is low and the impedance is high, resulting in a loss of the total capacity of the battery. When t2-t1<0.5 (Comparative Examples 1-2), the cycle curve of the battery shows a short-term sharp drop, which is because the liquid-phase diffusion of lithium ions is difficult and lithium precipitation occurs.

[0062] According to the above results, when a negative electrode plate includes two negative electrode active material layers, and the difference between the tortuosity of the second negative electrode active material layer away from the current collector and the tortuosity of the first negative electrode active material layer close to the current collector is 0.5 to 3.2, it can be ensured that the battery manufactured with the negative electrode plate has a low DCIR value, still has stable cycle performance at a high rate, and has a longer service life.

[0063] Although embodiments of the present application have been shown and described, as will be understood by those skilled in the art, various changes, modifications, substitutions and variations can be made to these embodiments without departing from the principles and spirit of the present application, and the scope of the present application is limited by the claims and their equivalents.

Claims

1. A negative electrode plate including a current collector and a first negative electrode active material layer and a second negative electrode active material layer disposed in that order on the current collector, The bending degree of the first negative electrode active material layer and the second negative electrode active material layer is 1<t 1 ≦5, 1<t 2 ≦5 and 0.5≦t 2 -t 1 ≦3.2 is satisfied, In the formula, the above t 1 represents the bending degree of the first negative electrode active material layer, and the t 2 represents the bending degree of the second negative electrode active material layer, and the t 2 -t 1 represents a difference between the bending degree of the second negative electrode active material layer and the bending degree of the first negative electrode active material layer, a porosity of the first negative electrode active material layer is 20% to 30%, a porosity of the second negative electrode active material layer is 30% to 40%, and the porosity of the second negative electrode active material layer is greater than the porosity of the first negative electrode active material layer.

2. 2. The negative electrode plate of claim 1, wherein the first negative electrode active material layer includes a first negative electrode active material, the second negative electrode active material layer includes a second negative electrode active material, a D50 particle size of the first negative electrode active material and a D50 particle size of the second negative electrode active material are both within a range of 8 μm to 20 μm, and the D50 particle size of the second negative electrode active material is larger than the D50 particle size of the first negative electrode active material.

3. The negative electrode plate according to claim 2 , wherein the first negative electrode active material has a D50 particle size of 8 μm to 13 μm, and the second negative electrode active material has a D50 particle size of 13 μm to 20 μm.

4. The negative electrode plate according to claim 2 , wherein a difference between a D50 particle size of the second negative electrode active material and a D50 particle size of the first negative electrode active material is 3 μm or more.

5. The negative electrode plate according to any one of claims 1 to 4, wherein the thickness of the first negative electrode active material layer and the thickness of the second negative electrode active material layer are both within a range of 30 μm to 100 μm.

6. The surface density of the first negative electrode active material layer and the surface density of the second negative electrode active material layer are both 0.30 g / dm 2 ~0.73 g / dm 2 The negative electrode plate according to any one of claims 1 to 4, characterized in that the range of

7. 5. The negative electrode plate of claim 4, wherein a weight of the first negative electrode active material accounts for 90% to 98% of a weight of the first negative electrode active material layer, and a weight of the second negative electrode active material accounts for 90% to 98% of a weight of the second negative electrode active material layer.

8. 3. The negative electrode plate according to claim 2, wherein the first negative electrode active material and the second negative electrode active material are independently selected from one or more of graphite, soft carbon, hard carbon, lithium titanate, silicon-based materials, and tin-based materials.

9. A secondary battery comprising the negative electrode plate according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Cathode for lithium ion secondary battery, and lithium ion secondary battery

    JP2005071918A

  • Anode and lithium ion secondary battery

    JP2008251250A

  • Nonaqueous electrolyte secondary battery

    JP2010192230A

  • Nonaqueous electrolyte secondary battery

    JP2014143152A

  • Electrode, nonaqueous electrolyte battery and battery pack

    JP2014154317A