Laminate, packaging material and anchor coating agent
The laminate structure with a specific anchor coat layer and vapor deposition layer on a polyolefin base material addresses adhesion and gas barrier issues in polypropylene film packaging, ensuring stability and performance after retort treatment.
Patent Information
- Application Number
- JP2024155310
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2044-09-09
AI Technical Summary
Existing laminates using polypropylene film for packaging materials face issues with insufficient adhesion between the polypropylene film and vapor-deposited films, leading to poor gas barrier properties, especially after retort treatment, and are prone to instability due to solvent-based adhesives.
A laminate structure comprising an anchor coat layer with a thickness of 0.05 to 1.5 μm, a vapor deposition layer, and a barrier coat layer on a polyolefin base material, using a resin material containing methyl (meth)acrylate, polar group-containing (meth)acrylic ester or (meth)acrylic acid, a curing agent, and a silane coupling agent, with specific polar groups and mixing ratios to enhance adhesion and gas barrier properties.
The laminate exhibits improved adhesion, lamination strength, retort resistance, and excellent gas barrier properties, maintaining performance even after retort treatment, with enhanced stability and blocking resistance.
Smart Images

Figure 0007595214000001 
Figure 0007595214000002 
Figure 0007595214000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminate, a packaging material, and an anchor coating agent. [Background technology]
[0002] In recent years, in order to improve the recyclability of packaging containers, a packaging material (mono-material) has been studied in which a polypropylene film is applied to the base material and a laminate made of the same material is used. However, due to concerns about a decrease in gas barrier properties, studies have been conducted to compensate for this by forming a vapor-deposited film on the surface of the polypropylene film, but the adhesion between the polypropylene film and the vapor-deposited film is insufficient, and the desired gas barrier properties are not achieved.
[0003] Patent Document 1 describes a laminate comprising at least a first substrate, a vapor-deposited film, a barrier coat layer, and a sealant layer, the first substrate being a biaxially oriented resin film comprising a polypropylene resin layer, a surface resin layer provided on one side of the polypropylene resin layer, and an adhesive resin layer between the polypropylene resin layer and the surface resin layer, the adhesive resin layer being provided on the polypropylene resin layer, the surface resin layer being provided on the adhesive resin layer, the vapor-deposited film being provided on the surface resin layer of the first substrate, the surface resin layer comprising a resin material having a melting point of 180°C or higher, the resin material being vinyl resin, nylon 6, nylon 6,6, MXD nylon, or polyester, the vapor-deposited film being made of an inorganic oxide, and the sealant layer comprising a polyolefin having a melting point of 110°C or higher. The laminate can be suitably used for mono-material packaging containers, can significantly improve interlayer adhesion between the substrate and the vapor-deposited film, can achieve favorable gas barrier properties, and can form a laminate having heat resistance.
[0004] Patent Document 2 describes a packaging bag including a barrier laminate including a first substrate, a first adhesive layer, a second substrate, a second adhesive layer, and a sealant layer in this order in the thickness direction, in which the first substrate is a polypropylene resin substrate that has been subjected to a stretching treatment, the second substrate is a barrier substrate including a polypropylene resin layer that has been subjected to a stretching treatment and a vapor deposition film composed of an inorganic oxide, the second substrate is disposed so that the vapor deposition film faces the first substrate side and the polypropylene resin layer faces the sealant layer side, the sealant layer is a polypropylene resin layer, the first adhesive layer has a thickness of 2 μm or less, and the second adhesive layer has a thickness of 2 μm or less. This packaging bag can improve gas barrier properties, and in particular can form a packaging bag that has excellent gas barrier properties even after retort treatment.
[0005] Patent Document 3 describes a packaging bag including a barrier laminate including a first substrate, a first adhesive layer, a second substrate, a second adhesive layer, and a sealant layer in this order in the thickness direction, in which the first substrate is a polypropylene resin substrate that has been subjected to a stretching treatment, the second substrate is a barrier substrate including a polypropylene resin layer that has been subjected to a stretching treatment and a vapor deposition film composed of an inorganic oxide, the second substrate is disposed so that the vapor deposition film faces the first substrate side and the polypropylene resin layer faces the sealant layer side, the sealant layer is a polypropylene resin layer, the first adhesive layer has a thickness of 10 μm or less, and the second adhesive layer has a thickness of 10 μm or less. This packaging bag can improve gas barrier properties, and in particular can form a packaging bag that has excellent gas barrier properties even after retort treatment.
[0006] However, in all of Patent Documents 1 to 3, the first adhesive layer and the second adhesive layer are composed of a solvent-based adhesive, which may deteriorate the deposition film and may cause the barrier laminate to become unstable. In addition, the inclusion of a resin material having a polar group in the coating layer (referred to as a surface resin layer in Patent Document 1, and as a surface coating layer or surface resin layer in Patent Documents 2 and 3) provided between the polypropylene resin layer and the deposition film is thought to contribute to improving the gas barrier properties, especially after retort treatment, but this alone may be insufficient.
[0007] Patent Document 4 describes a liquid sachet package comprising at least one transparent gas barrier film having a surface layer, the film comprising a substrate film made of a polyamide resin, an easy-adhesion layer formed on one side of the substrate film and containing nitrogen atoms, adipic acid, and bisphenol glycidyl ether, a vapor-deposition anchor coat layer formed on the easy-adhesion layer and containing a polyol, an isocyanate compound, and a reaction product thereof, the vapor-deposition anchor coat layer having a thickness of 0.08 μm to 0.3 μm, and an inorganic oxide layer formed on the anchor coat layer by a vapor phase deposition method, the laminate being laminated with thermal adhesive resin layers in sequence, the laminate being further used to form a packaging bag in which the surfaces of the thermal adhesive resin layers are stacked opposite each other and the edges around the periphery are fused, and the packaging bag is filled with contents through the opening, the packaging bag having high barrier properties and excellent laminate strength even in a wet state, is resistant to tearing, and is environmentally friendly. However, the inclusion of two layers, an easy-adhesion layer containing a water-dispersible polyurethane resin for imparting water resistance, heat resistance, adhesion and film cohesion, and a vapor deposition anchor coat layer containing a reaction product (urethane bonded) of a polyol, an isocyanate compound and a silane coupling agent for strengthening adhesion to the inorganic oxide layer, is thought to be effective for adhesion to a substrate film made of a polyamide resin, but there is a risk of poor adhesion with a polyolefin substrate. In addition, there is a description that it is preferable to provide an intermediate film for boiling and retort sterilization, but this is for increasing the bag-breaking strength, and the increase in the layer structure increases the environmental load and there is a risk of destabilizing the laminate.
[0008] Patent Document 5 describes a laminate in which at least a base film, a gas barrier precursor laminate, an adhesive layer, and a thermoplastic resin layer are laminated in this order, the gas barrier precursor laminate including a layer (A) containing a polycarboxylic acid polymer (A1) and at least one silicon-containing compound (A2) selected from the group consisting of a specific silane coupling agent, its hydrolysate, and its condensate, in a specific mass ratio, and a layer (B) containing a polyvalent metal compound, and further including an anchor coat layer formed on the base film; the laminate is capable of being treated with hot water and has excellent gas barrier properties. However, a gas barrier precursor laminate is laminated on the anchor coat layer, and the gas barrier precursor laminate contains a polycarboxylic acid polymer and is not a vapor deposition film. Comparative Examples 1 and 2 of Patent Document 5 include examples in which an alumina vapor deposition film and a silica vapor deposition film are formed, and it is clear that the effect of oxygen barrier properties after retorting is not exhibited, and it is clear that the problem cannot be solved even if a vapor deposition film is formed on the anchor coat layer formed using the anchor coat solution of Patent Document 5. As for the anchor coat layer, from the claims and the description, it can be interpreted that the anchor coat liquid used is composed of a composite of at least one metal compound (P) selected from the group consisting of trifunctional organosilanes (p1), metal alkoxides (p2) and their hydrolysates, a polyol compound (Q) and an isocyanate compound (R). However, since there is no specific disclosure, excessive trial and error will occur in selecting the anchor coat liquid in order to solve the problem of Patent Document 5.
[0009] Patent Document 6 describes a metal vapor deposition film in which at least an anchor coat layer and a metal thin film layer are successively formed on one side of a polypropylene film, in which the anchor coat layer is a layer containing at least a urethane cellulose resin that contains at least a urethane resin and a cellulose resin, and a hardener, and which maintains excellent adhesion between the polypropylene film and the metal thin film layer, and excellent adhesion at the heat sealed portion even after heat sealing processing. However, retort treatment is not anticipated at all, and there is no mention or suggestion of gas barrier properties after retort, which may result in inferior properties.
[0010] Patent Document 7 describes a gas barrier laminate obtained by laminating an inorganic oxide vapor deposition layer and a barrier coat layer in this order on one side of a base film made of a plastic material, in which an anchor coat layer is provided between the vapor deposition surface of the base film and the inorganic oxide vapor deposition layer, and the anchor coat layer is a layer obtained by reaction and curing of an anchor coat agent containing a hydroxyl group-containing acrylic resin, an isocyanate compound, and a silane coupling agent, and the barrier coat layer is a compound represented by the general formula R 1 n M(OR 2 ) m (In the formula, R 1 , R 2is an organic group having 1 to 8 carbon atoms, M is a metal atom, n is an integer of 0 or more, m is an integer of 1 or more, and n+m is the atomic valence of M), and a water-soluble polymer, the gas barrier composition being obtained by polycondensation using a sol-gel method, and the gas barrier laminate has good gas barrier properties and is not prone to delamination even under any stress. However, even the above-mentioned anchor coat layer may have poor adhesion to the vapor deposition layer, and in particular, may not be able to maintain high gas barrier properties after retort treatment. [Prior art documents] [Patent documents]
[0011] [Patent Document 1] JP 2023-075177 A [Patent Document 2] JP 2023-111747 A [Patent Document 3] JP 2023-111750 A [Patent Document 4] JP 2009-262992 A [Patent Document 5] JP 2021-020363 A [Patent Document 6] Patent Publication No. 2022-017007 [Patent Document 7] JP 2014-195953 A Summary of the Invention [Problem to be solved by the invention]
[0012] Therefore, an object of the present invention is to provide a laminate having blocking resistance, good adhesion between an anchor coat layer and a vapor deposition layer, lamination strength, retort resistance, and gas barrier properties, particularly good gas barrier properties even after retort treatment. [Means for solving the problem]
[0013] The present inventors have discovered a laminate comprising, on a polyolefin substrate, at least an anchor coat layer having a thickness of 0.05 to 1.5 μm, a vapor deposition layer, and a barrier coat layer, in this order, wherein the anchor coat layer is a layer made of an anchor coat agent containing a resin material containing methyl (meth)acrylate and a polar group-containing (meth)acrylic acid ester or (meth)acrylic acid, a curing agent, and a silane coupling agent, the polar group in the resin material being at least one polar group selected from a hydroxyl group, an amide group, an amino group, a phosphoric acid group, and an epoxy group, and the silane coupling agent is a layer made of an anchor coat agent containing a nitrogen atom. The present invention has been accomplished by finding that the above-mentioned object can be achieved by providing a laminate characterized in that the silane coupling agent contains at least one group selected from a polar group-containing group, a sulfur atom-containing group, and a vinyl group, the mixing ratio of the methyl (meth)acrylate and the polar group-containing (meth)acrylic ester or (meth)acrylic acid is 5 or more and less than 900 parts of polar group-containing (meth)acrylic ester or (meth)acrylic acid to 100 parts of methyl (meth)acrylate, and the contact angle of the anchor coat layer surface is 20 degrees or more and 75 degrees or less.
[0014] That is, the present invention provides (1) A laminate having an anchor coat layer having a thickness of 0.05 to 1.5 μm, a deposition layer, and a barrier coat layer, at least in this order, on a polyolefin substrate, the anchor coat layer is a layer made of an anchor coat agent containing a resin material including methyl (meth)acrylate and a polar group-containing (meth)acrylic acid ester or (meth)acrylic acid, a curing agent, and a silane coupling agent; the polar group in the resin material is at least one polar group selected from a hydroxyl group, an amide group, an amino group, a phosphate group, and an epoxy group; the silane coupling agent contains at least one group selected from a group containing a nitrogen atom, a group containing a sulfur atom, and a vinyl group; a mixing ratio of the methyl (meth)acrylate to the polar group-containing (meth)acrylic acid ester or (meth)acrylic acid is 5 or more and less than 900 of the polar group-containing (meth)acrylic acid ester or (meth)acrylic acid per 100 of the methyl (meth)acrylate; and a contact angle of the surface of the anchor coat layer is 20 degrees or more and 75 degrees or less. (2) A packaging material comprising the laminate according to (1). (3) An anchor coating agent for use in the laminate according to (1), the anchor coating agent comprises a resin material containing methyl (meth)acrylate and a polar group-containing (meth)acrylic acid ester or (meth)acrylic acid, a curing agent, and a silane coupling agent; the polar group in the resin material is at least one polar group selected from a hydroxyl group, an amide group, an amino group, a phosphate group, and an epoxy group; the silane coupling agent contains at least one group selected from a group containing a nitrogen atom, a group containing a sulfur atom, and a vinyl group; a mixing ratio of the methyl (meth)acrylate and the polar group-containing (meth)acrylic acid or (meth)acrylic acid is 5 or more and less than 900 of the polar group-containing (meth)acrylic acid ester or (meth)acrylic acid per 100 of the methyl (meth)acrylate; and an anchor coating agent characterized in that the contact angle of the surface of the anchor coating layer formed by printing the anchor coating agent is 20 degrees or more and 75 degrees or less. (4) providing a polyolefin substrate; forming an anchor coat layer having a thickness of 0.05 to 1.5 μm on at least one of the polyolefin substrates; forming a deposition layer on the anchor coat layer; forming a barrier coat layer on the deposition layer, in this order at least, the step of forming the anchor coat layer is a step of printing an anchor coat agent containing a resin material including methyl (meth)acrylate and a polar group-containing (meth)acrylic acid ester or (meth)acrylic acid, a curing agent, and a silane coupling agent; the polar group in the resin material is at least one group selected from a hydroxyl group, an amide group, an amino group, and a phosphate group, the silane coupling agent contains at least one group selected from a group containing a nitrogen atom, a group containing a sulfur atom, and a vinyl group; a mixing ratio of the methyl (meth)acrylate to the polar group-containing (meth)acrylic acid ester or (meth)acrylic acid is 5 or more and less than 900 of the polar group-containing (meth)acrylic acid ester or (meth)acrylic acid per 100 of the methyl (meth)acrylate; and a contact angle of the surface of the anchor coat layer formed in the anchor coat layer forming step is 20 degrees or more and 75 degrees or less. (5) The method for producing a laminate according to (4), wherein the step of forming the anchor coat layer is a gravure printing step. (6) The method for producing a laminate according to (4) or (5), further comprising a winding step after the anchor coat layer forming step. (7) The method for producing a laminate according to (6), further comprising a step of forming a deposition layer and a step of forming a barrier coat layer while rewinding the laminate after the winding step. This is regarding. Effect of the Invention
[0015] According to the present invention, it is possible to provide a laminate having blocking resistance, good adhesion between the anchor coat layer and the vapor deposition layer, laminate strength, retort resistance, and gas barrier properties, particularly good gas barrier properties even after retort treatment.
[0016] Hereinafter, an embodiment of the present invention will be described in detail. Note that this embodiment is merely one embodiment of the present invention, and the present invention is not limited to this embodiment, and various modifications and embodiments are possible without departing from the gist of the present invention.
[0017] In the following description, (meth)acrylic and (meth)acrylate mean acrylic and methacrylic, acrylate and methacrylate, respectively.
[0018] The laminate of the present invention is a laminate comprising an anchor coat layer having a thickness of 0.05 to 1.5 μm, a deposition layer, and a barrier coat layer, at least in this order, on a polyolefin substrate, the anchor coat layer being a layer made of a resin material containing methyl (meth)acrylate and a polar group-containing (meth)acrylic acid ester or (meth)acrylic acid, a curing agent, and a silane coupling agent, the polar group in the resin material being at least one polar group selected from a hydroxyl group, an amide group, an amino group, a phosphoric acid group, and an epoxy group, It is preferable that the silane coupling agent is a silane coupling agent containing at least one group selected from a group containing a nitrogen atom, a group containing a sulfur atom, and a vinyl group, that the mixing ratio of the methyl (meth)acrylate and the polar group-containing (meth)acrylic acid ester or (meth)acrylic acid is 5 or more and less than 900 parts of polar group-containing (meth)acrylic acid ester or (meth)acrylic acid per 100 parts of methyl (meth)acrylate, and that the contact angle on the surface of the anchor coat layer is 20 degrees or more and 75 degrees or less.
[0019] The anchor coat layer in the present invention is preferably a layer made of an anchor coat agent containing a resin material containing methyl (meth)acrylate and a polar group-containing (meth)acrylic acid ester or (meth)acrylic acid, a curing agent, and a silane coupling agent.
[0020] The polar group of the polar group-containing (meth)acrylic acid ester is preferably at least one group selected from the group consisting of a hydroxyl group, an amide group, an amino group, a phosphate group, and an epoxy group. The (meth)acrylic acid ester having a polar group improves wettability with a deposition layer, contributing to adhesion.
[0021] Examples of the hydroxyl-containing (meth)acrylic acid ester in which the polar group is a hydroxyl group include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and glycerol mono(meth)acrylate, and among these, 2-hydroxyethyl methacrylate is more preferable.
[0022] Examples of the amide group-containing (meth)acrylic acid ester in which the polar group is an amide group include N-(1,1-dimethyl-3-oxybutyl)(meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-dimethylaminopropyl(meth)acrylamide, N-isopropyl(meth)acrylamide, Nt-butyl(meth)acrylamide, N-(hydroxymethyl)acrylamide, and (2)-hydroxypropyl(meth)acrylamide. Of these, N-(1,1-dimethyl-3-oxybutyl)acrylamide is more preferable.
[0023] Examples of the amino group-containing (meth)acrylic acid ester in which the polar group is an amino group include N,N-dimethylaminoethyl (meth)acrylate and N,N-diethylaminoethyl (meth)acrylate, and among these, N,N-dimethylaminoethyl methacrylate is more preferable.
[0024] Examples of the phosphate group-containing (meth)acrylic acid ester in which the polar group is a phosphate group include (meth)acrylate phosphate, 2-(meth)acryloyloxyethyl acid phosphate, di-(2-methacryloyloxyethyl)-phosphate, 2-(meth)acryloyloxypropyl acid phosphate, 2-(meth)acryloyloxybutyl acid phosphate, acid phosphoxypolyoxypropylene glycol monomethacrylate, and acid phosphoxypolyoxyethylene glycol monomethacrylate, with 2-methacryloyloxyethyl acid phosphate being more preferred.
[0025] The epoxy group-containing (meth)acrylic acid ester in which the polar group is an epoxy group is, for example, glycidyl (meth)acrylate, β-methylglycidyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate glycidyl ether, 3,4-epoxycyclohexylmethyl (meth)acrylate, 3-epoxycyclo-2-hydroxypropyl (meth)acrylate, 6-methyl-3,4-epoxycyclohexylmethyl (meth)acrylate, 3,4-epoxybutyl (meth)acrylate, 6,7-epoxyheptyl (meth)acrylate, 6,7-epoxyheptyl α-ethyl (meth)acrylate, α-ethyl glycidyl acrylate, α-n-propyl glycidyl acrylate, and α-n-butyl glycidyl acrylate. Among these, glycidyl methacrylate, 4-hydroxybutyl (meth)acrylate glycidyl ether, and 3,4-epoxycyclohexylmethyl (meth)acrylate are more preferred.
[0026] The methyl (meth)acrylate and the polar group-containing (meth)acrylic ester or (meth)acrylic acid are preferably mixed in a ratio of 5 to 900, more preferably 10 to 500, and even more preferably 20 to 300, of 100 to 100 of methyl (meth)acrylate. If the ratio is less than 5, the contact angle may become large and the adhesion between the anchor coat layer and the vapor deposition layer may become poor, whereas if the ratio is 900 or more, the coating may become hard and the adhesion between the polyolefin substrate and the anchor coat layer may become poor. The use of a mixture of the methyl (meth)acrylate and the polar group-containing (meth)acrylic acid ester or the (meth)acrylic acid contributes to improving heat resistance and adhesion to a polyolefin substrate or a vapor deposition layer.
[0027] The amount of the resin material containing the methyl (meth)acrylate and the polar group-containing (meth)acrylic acid ester or (meth)acrylic acid is preferably 3 to 90% by mass, more preferably 5 to 80% by mass, and even more preferably 10 to 70% by mass, based on the total amount of the anchor coating agent (100%). These may be used alone or in combination of two or more kinds.
[0028] The curing agent is preferably a polyisocyanate-based compound, and is selected from conventionally known polyisocyanates without any particular limitation, and examples thereof include aliphatic polyisocyanates or aromatic aliphatic polyisocyanates, and examples thereof include aromatic diisocyanates such as tolylene diisocyanate and 4,4'-diphenylmethane diisocyanate, aliphatic diisocyanates such as hexamethylene diisocyanate, xylylene diisocyanate, isophorone diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, 4,4'-dicyclohexyl diisocyanate, and pentane-1,5-diisocyanate (Stabio PDI), and modified products thereof such as trimethylolpropane trimer, isocyanurate, biuret, and allophanate, and examples of commercially available products include LG Curing Agent C and LG Curing Agent D (both manufactured by Tokyo Ink Co., Ltd.). These may be used alone or in combination of two or more.
[0029] The amount of the curing agent added is preferably 1 to 20% by mass, more preferably 2 to 18% by mass, and even more preferably 4 to 15% by mass, based on the total amount of the anchor coating agent (100%). These may be used alone or in combination of two or more kinds.
[0030] The silane coupling agent preferably contains at least one group selected from a group containing a nitrogen atom, a group containing a sulfur atom, and a vinyl group. The inclusion of a silane coupling agent having the specific group contributes to improving the adhesion between the anchor coat layer and the deposition layer.
[0031] Examples of groups containing a nitrogen atom include amino groups, imino groups, isocyanate groups (-N=C=O), ureido groups (-NH-CO-NH2), nitro groups (=NO), carbamate groups (-O-CO-N<), and quaternary ammonium salts.
[0032] Examples of silane coupling agents having an amino group include 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltripropoxysilane, 3-aminopropylmethyldimethoxysilane, 3-aminopropylmethyldiethoxysilane, 3-triethoxysilyl-N-(1,3-dimethyl-butylidene)propylamine, bis(3-triethoxysilylpropyl)amine, bis(3-trimethoxysilylpropyl)amine, bis(3-methyldimethoxysilylpropyl)amine, bis(triethoxysilylmethyl)amine, N-(2-aminoethyl)-3 -aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldiethoxysilane, N-(n-butyl)-3-aminopropyltrimethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, N,N'-bis[3-(trimethoxysilyl)propyl]ethylenediamine, N-(vinylbenzyl)-2-aminoethyl-3-aminopropyltrimethoxysilane hydrochloride, etc. Among them, 3-aminopropyltrimethoxysilane and N-(2-aminoethyl)-3-aminopropyltrimethoxysilane are more preferred.
[0033] Commercially available products include KBP-64, KBP-90, KBE-9103P, KBE-903, KBM-6803, KBM-573, KBM-575, KBM-602, KBM-603, KBM-903, KBM-6103, X-12-1172ES, X-12-972F, X-12-5263HP, and X-88-475 (all manufactured by Shin-Etsu Chemical Co., Ltd.).
[0034] Examples of silane coupling agents having an isocyanate group include trialkoxysilanes such as 3-isocyanatepropyltrimethoxysilane, 3-isocyanatepropyltriethoxysilane, 3-isocyanatepropylmethyldimethoxysilane, and 3-isocyanatepropylmethyldiethoxysilane, as well as trimers (isocyanurates) of these compounds. Of these, 3-isocyanatepropyltrimethoxysilane is more preferred.
[0035] Commercially available products include KBE-9007N, X-12-1159, X-12-1159L, and KBM-9659 (all manufactured by Shin-Etsu Chemical Co., Ltd.), SILQUEST Silane A-1310, and SILQUEST Silane Y-5187 (all manufactured by Momentive Corporation).
[0036] Examples of silane coupling agents having a ureido group include trialkoxysilanes such as 3-ureidopropyltrialkoxysilane.
[0037] Commercially available products include KBE-585A and KBM-585 (both manufactured by Shin-Etsu Chemical Co., Ltd.).
[0038] Examples of silane coupling agents having a nitro group include trialkoxysilanes such as 3-nitropropyltrimethoxysilane and 3-nitropropyltriethoxysilane.
[0039] Examples of silane coupling agents having a carbamate group include (3-carbamate ethyl)propyl trimethoxy silane, (3-carbamate ethyl)propyl tripropoxy silane, (3-carbamate propyl)propyl triethoxy silane, (3-carbamate propyl)propyl trimethoxy silane, (3-carbamate propyl)propyl tripropoxy silane, (3-carbamate butyl)propyl triethoxy silane, (3-carbamate butyl)propyl trimethoxy silane, (3-carbamate butyl)propyl tripropoxy silane, (3-carbamate butyl)butyl tripropoxy silane, (3-carbamate butyl)propyl tripropoxy silane, Examples of the trialkoxysilane include (3-carbamate ethyl)propyl methyl diethoxysilane, (3-carbamate pentyl)propyl triethoxysilane, (3-carbamate hexyl)propyl triethoxysilane, (3-carbamate octyl)pentyl tributoxysilane, (3-carbamate ethyl)propyl silyl trichloride, (3-carbamate ethyl)propyl trimethylsilane, (3-carbamate ethyl)propyl dimethylsilane, (3-carbamate ethyl)propyl tributylsilane, (3-carbamate ethyl)ethyl-p-xylene triethoxysilane, and (3-carbamate ethyl)-p-phenylene triethoxysilane.
[0040] Examples of commercially available silane coupling agents having a quaternary ammonium salt include X-12-1126, KBM-9418-40, POLON-V8, X-12-1139, and X-12-1354-1 (all manufactured by Shin-Etsu Chemical Co., Ltd.).
[0041] Examples of the functional group containing a sulfur atom include a mercapto group and a sulfide group.
[0042] Examples of silane coupling agents having a mercapto group include trialkoxysilanes such as 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 3-mercaptopropyltripropoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropylmethyldiethoxysilane, 2-mercaptoethyltrimethoxysilane, and 2-mercaptoethyltriethoxysilane.
[0043] Commercially available products include KBM-802, KBM-803, X-12-1307, X-12-1056ES, and X-12-1154 (all manufactured by Shin-Etsu Chemical Co., Ltd.).
[0044] Examples of silane coupling agents having a sulfide group include bis(3-triethoxysilylpropyl)tetrasulfide, bis(2-triethoxysilylethyl)tetrasulfide, bis(4-triethoxysilylbutyl)tetrasulfide, bis(3-trimethoxysilylpropyl)tetrasulfide, Bis(2-trimethoxysilylethyl)tetrasulfide, bis(4-trimethoxysilylbutyl)tetrasulfide, bis(3-triethoxysilylpropyl)trisulfide, bis(2-triethoxysilylethyl)trisulfide, bis(4-triethoxysilylbutyl)trisulfide, bis(3-trimethoxysilylpropyl)trisulfide, bis(2-trimethoxysilylethyl)trisulfide, bis(4-trimethoxysilylbutyl)trisulfide, bis(3-triethoxysilylpropyl)disulfide, bis(2-triethoxysilylethyl)disulfide, bis(4-triethoxysilylbutyl)disulfide, bis(3-trimethoxysilylpropyl)disulfide, bis(2-triethoxysilylethyl)disulfide, bis(4-triethoxysilylbutyl)disulfide, bis(3-trimethoxysilylpropyl)disulfide, bis(2-trimethoxysilylethyl)disulfide Examples of the trialkoxysilanes include bis(4-trimethoxysilylbutyl) disulfide, 3-trimethoxysilylpropyl-N,N-dimethylthiocarbamoyl tetrasulfide, 3-triethoxysilylpropyl-N,N-dimethylthiocarbamoyl tetrasulfide, 2-triethoxysilylethyl-N,N-dimethylthiocarbamoyl tetrasulfide, 2-trimethoxysilylethyl-N,N-dimethylthiocarbamoyl tetrasulfide, 3-trimethoxysilylpropyl benzothiazolyl tetrasulfide, 3-triethoxysilylpropyl benzothiazole tetrasulfide, 3-triethoxysilylpropyl methacrylate monosulfide, and 3-trimethoxysilylpropyl methacrylate monosulfide.
[0045] Examples of silane coupling agents having a vinyl group include trialkoxysilanes such as vinyltrimethoxysilane, vinyltriethoxysilane, vinyltriisopropoxysilane, vinyltributoxysilane, vinylmethyldimethoxysilane, and vinylmethyldiethoxysilane.
[0046] Commercially available products include KBE-1003, KBM-1003, KBM-1083, and X-12-1290 (all manufactured by Shin-Etsu Chemical Co., Ltd.).
[0047] The amount of the silane coupling agent added is preferably 0.1 to 10 mass % relative to the total amount of the anchor coating agent (100%), more preferably 0.5 to 7 mass %, and even more preferably 1 to 5 mass %. These may be used alone or in combination of two or more kinds.
[0048] In addition to the resin material containing the methyl (meth)acrylate and the polar group-containing (meth)acrylic acid ester or (meth)acrylic acid, the curing agent, and the silane coupling agent, organic solvents, colorants, inorganic fillers, organic fillers, defoamers, leveling agents, pigment dispersants, antistatic agents, slip agents, plasticizers, tackifiers, etc. may also be added to the anchor coating agent as necessary. These may be added alone or in combination of two or more kinds.
[0049] The anchor coating agent of the present invention is preferably used in gravure printing, and can be applied as is, but can also be adjusted to a desired viscosity by diluting with a diluting solvent in a Zahn Cup #3 (manufactured by Rigo Co., Ltd.) depending on the coating conditions and coating effect. In this case, the viscosity is preferably 10 to 40 seconds at 25°C. If it is less than 10 seconds, it will tend to swim, and if it is more than 40 seconds, transferability during printing will be poor.
[0050] The anchor coat layer in the present invention is a layer made of the anchor coat agent, and is preferably formed by printing on a polyolefin substrate with a thickness of 0.05 to 1.5 μm by gravure printing, more preferably formed by printing with a thickness of 0.08 to 1.2 μm, and even more preferably formed by printing with a thickness of 0.1 to 1.0 μm. If the thickness is less than 0.05 μm, the deposition layer provided on the anchor coat layer is likely to crack due to the influence of substrate shrinkage caused by heat treatment such as retort treatment, and the gas barrier property may be poor, and if the thickness exceeds 1.5 μm, the adhesion to the polyolefin substrate and blocking resistance may be poor. In particular, it is more preferable to form the layer by printing with a gravure printing method using a multicolor gravure printer. This allows the anchor coat layer to be printed and wound by gravure printing. The anchor coat layer formed by the anchor coat agent of the present invention is stable after printing, and can be stored in a rolled-up state. Furthermore, a deposition layer and a barrier coat layer can be formed on the anchor coat layer.
[0051] The contact angle of the surface of the anchor coat layer in the present invention is preferably 20 degrees or more and 75 degrees or less, more preferably 30 degrees or more and 65 degrees or less, and even more preferably 40 degrees or more and 55 degrees or less. When the contact angle is within the above range, the adhesion between the polyolefin substrate and the deposition layer is dramatically improved, and the deposition layer is less likely to crack, so that good gas barrier properties, especially gas barrier properties after retort treatment, can be obtained. If the contact angle is less than 20 degrees, the adhesion with the deposition layer may be poor, and if the contact angle is more than 75 degrees, the polarity of the anchor coat layer itself may be high, and the adhesion with the polyolefin substrate may be poor.
[0052] The contact angle was measured at a temperature of 5° C. and a relative humidity of 50% (50% RH) by dropping distilled water in a drop amount of 2 μm onto the surface of the anchor coat layer, one second after the liquid had landed on the surface. The contact angle can be measured using a contact angle meter (portable contact angle meter PCA-1, manufactured by Kyowa Interface Science Co., Ltd.) or the like.
[0053] The laminate of the present invention preferably comprises a vapor-deposited layer on the anchor coat layer, and the vapor-deposited layer is a vapor-deposited film made of an inorganic oxide or a metal thin film.
[0054] Examples of the inorganic oxide include aluminum oxide (alumina), silicon oxide (silica), magnesium oxide, calcium oxide, zirconium oxide, titanium oxide, boron oxide, hafnium oxide, barium oxide, silicon carbide oxide (carbon-containing silicon oxide), and mixtures thereof. Among these, silica, silicon carbide oxide, and alumina are preferred, and silica is more preferred because it does not require aging treatment after the deposition film is formed. The metal used in the vapor-deposited film made of the metal thin film can be any of various conventionally known metals such as aluminum, chromium, tin, gold, silver, copper, zinc, and nickel, and may be appropriately selected depending on the desired purpose. The metal vapor-deposited film may be a thin film of an oxide, sulfide, or nitride of the conventionally known metal. The metal vapor-deposited film may be a single layer, or a multi-layer of two or more layers of the same or different kinds. Among these, aluminum is more preferable.
[0055] The deposition layer can be formed, for example, by using a physical vapor deposition (PVD) method such as vacuum deposition, sputtering, ion plating, or ion cluster beam, or by using a chemical vapor deposition (CVD) method such as plasma CVD, thermal CVD, photo CVD, or MOCVD. When using a vacuum deposition method, for example, an electron beam heating method, a resistance heating method, or an induction heating method can be used as a heating means for the evaporation material. When using an electron beam heating method, the degree of freedom in selecting the evaporation material is large. When a plasma assist method or an ion beam assist method is used during deposition, a denser deposition layer can be formed. In addition, when a reactive deposition method in which a gas such as oxygen is blown in is used during chemical deposition, a deposition layer with excellent transparency can be formed.
[0056] The thickness of the vapor-deposited layer is preferably in the range of 1 to 150 nm, more preferably in the range of 5 to 60 nm, and further preferably in the range of 10 to 40 nm. If the thickness is less than 1 nm, the desired gas barrier properties may not be exhibited, and if the thickness exceeds 150 nm, the polyolefin substrate may be deformed or altered by the heat generated when forming the vapor-deposited layer, and cracks may easily occur in the vapor-deposited layer, resulting in a loss of gas barrier properties.
[0057] The laminate of the present invention preferably has a barrier coat layer on the deposition layer, and the barrier coat layer is a coating film of a barrier coat agent having gas barrier properties obtained by polycondensing an alkoxide and a water-soluble polymer by a sol-gel method. A known coating method can be used as a coating method for forming the barrier coat layer, and for example, a printing method such as gravure printing or flexographic printing, or a wet coating method using a roll coater, a reverse roll coater, a gravure offset coater, a gravure coater, a microgravure coater, a knife coater, a bar coater, a wire bar coater, a die coater, a dip coater, a spin coater, a spray coater, etc. can be used. Among them, gravure printing, a roll coater, etc. are more preferable.
[0058] The alkoxide that can be used in the barrier coating agent having gas barrier properties is represented by the general formula R 1 n M(OR 2 ) m and at least one alkoxide selected from the group consisting of alkoxides represented by the formula: 1 , R 2 is an organic group having 1 to 8 carbon atoms, M is a metal atom, n is an integer of 0 or more, m is an integer of 1 or more, and n+m is the atomic valence of M.
[0059] The metal atom M is preferably, for example, silicon, zirconium, titanium, aluminum, etc. Furthermore, one or more alkoxides of different metal atoms may be mixed in the same solution.
[0060] In the alkoxide, R 1 The organic group represented by the formula (I) is an alkyl group, a cycloalkyl group, an aryl group, or an aralkyl group, which may have a substituent. Examples of the organic group include alkyl groups such as a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an n-hexyl group, and an n-octyl group.
[0061] Also, R 2 The organic group represented by the formula: is an alkyl group having a carbon number of 1 to 4. Examples thereof include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, and a sec-butyl group.
[0062] In addition, R 1 , R 2 In these, the alkyl groups may be the same or different.
[0063] The general formula R 1 n M(OR 2 ) m Examples of the alkoxides represented by the formula (I) and their hydrolysates include those in which the metal atom M is Si (in the case of Si, these are also called silane coupling agents), such as tetraethoxysilane (TEOS), tetramethoxysilane, tetrapropoxysilane, tetrabutoxysilane, methyltrimethoxysilane, ethyltrimethoxysilane, propyltrimethoxysilane, butyltrimethoxysilane, methyltriethoxysilane, ethyltriethoxysilane, propyltriethoxysilane, butyltriethoxysilane, methyltrippropoxysilane, ethyltrippropoxysilane, dimethyldimethoxysilane, diethyldimethoxysilane, dipropyldimethysilane, Examples of alkoxysilanes include alkoxysilanes such as xysilane, dimethyldiethoxysilane, diethyldiethoxysilane, γ-chloropropyltrimethoxysilane, γ-chloropropyltriethoxysilane, γ-mercaptopropyltrimethoxysilane, γ-mercaptopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, phenyltrippropoxysilane, diphenyldimethoxysilane, and diphenyldiethoxysilane. Of these, tetraethoxysilane and tetramethoxysilane are more preferred because they have good gas barrier properties.
[0064] The water-soluble polymer may be one or more water-soluble polymers selected from a vinyl alcohol polymer such as polyvinyl alcohol, an ethylene-vinyl alcohol polymer, a vinylpyrrolidone polymer, an acrylic acid polymer, starch, methyl cellulose, carboxymethyl cellulose, sodium alginate, etc., and is preferably one or more selected from a vinyl alcohol polymer, an ethylene-vinyl alcohol polymer, a vinylpyrrolidone polymer, and an acrylic acid polymer, since suitable gas barrier properties can be obtained.
[0065] The vinyl alcohol polymer can generally be one obtained by saponifying polyvinyl acetate. The saponification degree is preferably 95% or more. The polymerization degree is preferably 300 or more, more preferably 300 to 2400, and even more preferably 450 to 2000. If the saponification degree is 95% or more, sufficient gas barrier properties are easily obtained, and if the polymerization degree is 300 or more, the gas barrier properties and film cohesive strength are excellent. For example, commercially available polyvinyl alcohol products include Poval (manufactured by Kuraray Co., Ltd.) and Gohsenol (manufactured by Mitsubishi Chemical Corporation).
[0066] The ethylene vinyl alcohol copolymer may be a saponified copolymer of ethylene and vinyl acetate, i.e., a copolymer obtained by saponifying an ethylene-vinyl acetate random copolymer. For example, commercially available polyethylene vinyl alcohol products include EVAL (Kuraray Co., Ltd.) and Soarnol (Mitsubishi Chemical Co., Ltd.).
[0067] The content of the water-soluble polymer is preferably in the range of 5 to 500 parts by mass relative to 100 parts by mass of the total amount of the alkoxides. If the content of the water-soluble polymer is less than 5 parts by mass, the gas barrier property is poor. If it exceeds 500 parts by mass, the heat resistance and water resistance are poor.
[0068] In polycondensation by the sol-gel method, it is preferable to include an acid or an amine compound as a sol-gel method catalyst. The amine compound is preferably a tertiary amine that is substantially insoluble in water and soluble in an organic solvent, such as N,N-dimethylbenzylamine, tripropylamine, tributylamine, tripentylamine, etc. Among them, N,N-dimethylbenzylamine is more preferable.
[0069] The amount of the catalyst for the sol-gel process is preferably in the range of 0.01 to 1.0 part by mass, and more preferably in the range of 0.03 to 0.3 part by mass, relative to 100 parts by mass of the alkoxide. By using a sol-gel catalyst in an amount of 0.01 parts by mass or more per 100 parts by mass of the alkoxide, the catalytic effect can be improved, and by using a sol-gel catalyst in an amount of 1.0 part by mass or less per 100 parts by mass of the alkoxide, the thickness of the barrier coat layer formed can be made uniform.
[0070] The barrier coating agent having gas barrier properties may further contain an acid. The acid is used as a sol-gel catalyst, mainly as a catalyst for hydrolysis of alkoxides and silane coupling agents. Examples of the acid include mineral acids such as sulfuric acid, hydrochloric acid, and nitric acid, and organic acids such as acetic acid and tartaric acid. The amount of the acid used is preferably 0.001 to 0.05 moles relative to the total moles of the alkoxide portion (e.g., silicate portion) of the alkoxide (or silane coupling agent). The catalytic effect can be improved by using an acid in an amount of 0.001 moles or more relative to the total molar amount of the alkoxide portion (e.g., silicate portion) of the alkoxide (or silane coupling agent).The thickness of the barrier coat layer formed can be made uniform by using an acid in an amount of 0.05 moles or less relative to the total molar amount of the alkoxide portion (e.g., silicate portion) of the alkoxide (or silane coupling agent).
[0071] The barrier coating agent having gas barrier properties preferably contains 0.1 to 100 moles of water, and more preferably 0.8 to 2 moles of water, per mole of the total molar amount of the alkoxides. The gas barrier properties of the laminate can be improved by controlling the water content to 0.1 mole or more per mole of the total amount of alkoxides, and the hydrolysis reaction can be carried out quickly by controlling the water content to 100 moles or less per mole of the total amount of alkoxides.
[0072] The barrier coating agent having gas barrier properties may contain an organic solvent, such as methyl alcohol, ethyl alcohol, n-propyl alcohol, isopropyl alcohol, and n-butanol.
[0073] If necessary, the barrier coating agent having gas barrier properties may contain coloring materials, inorganic fillers, organic fillers, defoamers, leveling agents, pigment dispersants, antistatic agents, slip agents, plasticizers, tackifiers, etc. These may be added alone or in combination of two or more.
[0074] The barrier coating agent having gas barrier properties is preferably used in gravure printing, and can be applied as is, but can also be adjusted to a desired viscosity by diluting with a diluting solvent in a Zahn Cup #3 (manufactured by Rigo Co., Ltd.) depending on the coating conditions and coating effect. In this case, the viscosity is preferably 12 to 15 seconds at 25°C. If it is less than 12 seconds, it tends to swim, and if it is more than 15 seconds, transferability during printing becomes poor.
[0075] The barrier coat layer is preferably coated with a barrier coating agent having gas barrier properties to a thickness of 0.01 to 10.0 μm, more preferably 1.0 to 5.0 μm, and even more preferably 2.0 to 5.0 μm. If the thickness is less than 0.01 μm, the gas barrier properties may be poor, and if the thickness exceeds 10.0 μm, the adhesion may be poor.
[0076] The polyolefin substrate may be polyethylene, polypropylene, ethylene-vinyl acetate, copolymers thereof, or co-extruded films thereof, which may be stretched. Alternatively, the substrate may be a sealant substrate such as low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), high-density polyethylene (HDPE), acid-modified polyethylene, non-oriented polypropylene (CPP), acid-modified polypropylene, or copolymer polypropylene. The thickness of the polyolefin substrate is not particularly limited as long as it does not interfere with printability or winding suitability, but is preferably 5 to 300 μm, and more preferably 6 to 250 μm.
[0077] The laminate of the present invention may include, in addition to the anchor coat layer, the vapor deposition layer, and the barrier coat layer, an adhesive layer, a pressure-sensitive adhesive layer, a printing layer, a heat seal layer, and other substrates. The laminate may have a configuration such as polyolefin substrate / anchor coat layer / vapor deposition layer / barrier coat layer / adhesive layer / printing layer / other substrate, polyolefin substrate / anchor coat layer / vapor deposition layer / barrier coat layer / printing layer / other substrate, heat seal layer / adhesive layer / polyolefin substrate / anchor coat layer / vapor deposition layer / barrier coat layer / adhesive layer / printing layer / other substrate, adhesive layer / polyolefin substrate / anchor coat layer / vapor deposition layer / barrier coat layer / adhesive layer / printing layer / other substrate, release layer / adhesive layer / polyolefin substrate / anchor coat layer / vapor deposition layer / barrier coat layer / adhesive layer / printing layer / other substrate, etc.
[0078] The other substrate is preferably a polyolefin substrate equivalent to that of the present invention, but may be a substrate generally used as a packaging material, and more preferably a substrate used as the outermost surface of the packaging material.
[0079] The adhesive layer is formed by dry lamination, non-solvent lamination, wet lamination, extrusion lamination, thermal lamination, or by applying an adhesive or adhesive ink.
[0080] When an adhesive is used for the lamination, a commercially available adhesive may be used, for example, two-component or one-component urethane resin adhesives, acrylic, epoxy, polyester, polyethyleneimine, polybutadiene, water-based urethane, isocyanate, organic titanium, starch-based water-soluble adhesives, and aqueous adhesives such as vinyl acetate emulsion.
[0081] The adhesive ink preferably contains a polyolefin resin, a chlorinated polyolefin resin, or a (meth)acrylic resin. Preferred examples of the polyolefin resins and chlorinated polyolefin resins include polyethylene, polypropylene, polybutene, ethylene-propylene copolymers, ethylene-vinyl acetate copolymers, and the like, or blends thereof, chlorinated polyethylene, chlorinated polypropylene, chlorinated ethylene-propylene copolymers, and acid anhydride modified versions of these, and among these, chlorinated polypropylene, acid-modified polyolefins, acid-modified chlorinated polyolefins, and chlorinated ethylene-vinyl acetate copolymers (chlorinated EVA) are more preferred.
[0082] The adhesive or adhesive ink may also contain other resins, solvents, inorganic fillers, organic fillers, defoamers, leveling agents, antiblocking agents, waxes, pigment dispersants, antistatic agents, slip agents, plasticizers, tackifiers, antioxidants, surfactants, UV absorbers, surface conditioners, pH adjusters, charge imparting agents, bactericides, deodorants, wetting agents, antiskinning agents, metal chelating agents, and the like.
[0083] The printing layer is a layer formed by applying a printing ink containing a resin used in general gravure printing inks, such as polyurethane resins, polyolefin resins, shellacs, rosin-modified maleic acid resins, rosin-modified phenolic resins, cellulose acetate, cellulose acetyl propionate, cellulose acetyl butyrate, chlorinated rubber, cyclized rubber, halogenated vinyl resins (e.g., vinyl chloride resins, fluorine-containing vinyl resins, etc.), polyvinyl acetate, vinyl chloride-vinyl acetate copolymers, polystyrene resins, acrylic resins, acrylic-styrene copolymers, polyacrylic esters, polyester resins, polyvinylidene chloride resins, ketone resins, polyamide resins, nitrocellulose resins, rosin resins, styrene-maleic acid resins, alkyd resins, and ethylene-vinyl alcohol resins. The printing ink may contain, in addition to the resin, a colorant, a solvent, an inorganic filler, an organic filler, an antifoaming agent, a leveling agent, an antiblocking agent, a wax, a pigment dispersant, an antistatic agent, a slip agent, a plasticizer, a tackifier, an antioxidant, a surfactant, an ultraviolet absorber, a surface conditioner, a pH adjuster, a charge imparting agent, a bactericide, a deodorant, a wetting agent, an antiskinning agent, a metal chelating agent, and the like.
[0084] The heat seal layer is preferably a layer to which heat sealability has been imparted, and may be the above-mentioned sealant substrate or a film generally called a sealant film. Examples of the sealant film include the above-mentioned polyolefin film, colored film, polystyrene film, polyacrylonitrile film, ethylene-vinyl alcohol resin film, etc., and may be either stretched or unstretched, and may be one or more types laminated. The heat seal layer is preferably a layer made of a sealant material having a melting point of 150° C. or more. This is because, when used as a packaging material such as a pouch for retort or boiling, when the pouch is filled with contents and then subjected to a retort treatment or boiling treatment, the heat seal layer is made of a sealant material having a melting point of 150° C. or more, and therefore the packaging material produced using the laminate having the heat seal layer can suppress deterioration in gas barrier properties and heat sealability even during heat treatment such as a retort treatment or boiling treatment. Here, the retort treatment is a process in which the contents are filled into a packaging material such as a retort pouch, sealed, and then the retort pouch is heated under pressure using steam or heated water. The retort treatment is carried out, for example, at 121°C for 30 minutes. The boiling treatment is carried out, for example, at 90°C for 30 minutes.
[0085] The adhesive layer is a layer formed by applying an adhesive. A release layer may be further formed.
[0086] The laminate of the present invention has gas barrier properties. Specifically, the oxygen permeability of the laminate in an atmosphere having a temperature of 23° C. and a relative humidity of 50% RH is 1 cc / m 2 In addition, the water vapor permeability of the laminate in an atmosphere of a temperature of 40°C and a relative humidity of 90% is preferably 1 g / m 2 Furthermore, it is preferable that the oxygen permeability or water vapor permeability of the packaging material using the laminate does not change before and after a retort treatment (for example, at a temperature of 121°C for 30 minutes) or a boiling treatment (for example, at a temperature of 90°C for 30 minutes).
[0087] The oxygen permeability of the laminate of the present invention can be measured using an oxygen gas permeability measuring device (OX-TRAN 2 / 22, manufactured by MOCON) under conditions of a measurement temperature of 23°C and a relative humidity of 50% RH based on JIS K 7126-2A:2006 (Plastics - Films and sheets - Gas permeability test methods - Part 2: isobaric method, Appendix A: Test method for oxygen gas permeability by electrolytic sensor method). For example, the measurement is performed by mounting the laminate in the measuring device so that the outermost surface side is in contact with oxygen gas, and measuring the oxygen permeability of the laminate with a permeation area of 50 cm. 2 This will be carried out under the following conditions.
[0088] The water vapor permeability of the laminate of the present invention can be measured using a water vapor permeability measuring device (PERMATRAN-W 3 / 34, manufactured by MOCON) under conditions of a measurement temperature of 40° C. and a relative humidity of 90% RH based on JIS K 7129-1:2019 (Plastics - Films and sheets - Determination of water vapor permeability - Part 1: Moisture sensor method). For example, the measurement is performed by mounting the laminate in the measuring device so that the outermost surface side is in contact with water vapor, and measuring the water vapor permeability of the laminate with a permeation area of 50 cm. 2 This will be carried out under the following conditions.
[0089] The packaging material of the present invention is preferably made using the laminate, and may be in the form of a packaging bag, a label, or a lid material (collectively referred to as "packaging material").
[0090] The heat-sealed layers of the laminate are joined together to form a packaging bag, which may have any of the well-known forms such as two-sided seal, three-sided seal, four-sided seal, pillow seal, standing pouch, envelope seal, gusset, and melt-cut seal.
[0091] The lid material may be in any known form, such as a cover, lid, or cap.
[0092] Furthermore, it is preferable that the container is sealed by being tightly attached to the container. The sealing with the container may be performed manually, or a machine such as an automatic sealing device may be used. These methods may be appropriately selected depending on the type, shape, size, and quantity of the food, the container to be sealed, the equipment, the environment, etc., and may be performed by a method using heat sealing (thermal pressure sealing), surface sealing, pasting or adhesion with an adhesive, etc. It is more preferable that the container is a cylindrical container with a bottom. In this case, it is preferable that a lid material covers the opening of the cylindrical container with a bottom and seals it, and it is more preferable that the sealing is performed by heat sealing. Examples of the resin used for the container include thermoplastic resins such as polyethylene, polypropylene, polyethylene terephthalate, polyvinyl chloride, polystyrene, and polyacrylonitrile.
[0093] The label can be produced, for example, by forming an adhesive layer or a pressure-sensitive adhesive layer on the polyolefin substrate on the other side of the barrier coat layer, and then forming a release layer. The adhesive layer or the pressure-sensitive adhesive layer may be any material that adheres to the substrate film and the release layer, such as a rubber-based adhesive material or an acrylic resin-based adhesive material, and that allows the release layer to be easily peeled off. The release layer may be any material, such as a polyethylene film, a polyester film, or paper (release paper).
[0094] The anchor coating agent of the present invention is used for laminates, and comprises a resin material containing methyl (meth)acrylate and a polar group-containing (meth)acrylic ester or (meth)acrylic acid, a curing agent, and a silane coupling agent, wherein the polar group in the resin material is at least one polar group selected from a hydroxyl group, an amide group, an amino group, a phosphate group, and an epoxy group, and the silane coupling agent is a silane coupling agent containing at least one group selected from a group containing a nitrogen atom, a group containing a sulfur atom, and a vinyl group, and the mixing ratio of the methyl (meth)acrylate and the polar group-containing (meth)acrylic acid or (meth)acrylic acid is 10 to 900 polar group-containing (meth)acrylic ester or (meth)acrylic acid per 100 methyl (meth)acrylate, and the contact angle of the surface of the anchor coating layer formed by printing the anchor coating agent is preferably 20 degrees to 75 degrees.
[0095] The anchor coating agent of the present invention preferably contains a resin material containing methyl (meth)acrylate and a polar group-containing (meth)acrylic ester or (meth)acrylic acid, a curing agent, and a silane coupling agent.
[0096] The polar group of the polar group-containing (meth)acrylic acid ester is preferably at least one group selected from the group consisting of a hydroxyl group, an amide group, an amino group, a phosphate group, and an epoxy group. The (meth)acrylic acid ester having a polar group improves wettability with a deposition layer, contributing to adhesion.
[0097] Examples of the hydroxyl-containing (meth)acrylic acid ester in which the polar group is a hydroxyl group include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and glycerol mono(meth)acrylate, and among these, 2-hydroxyethyl methacrylate is more preferable.
[0098] Examples of the amide group-containing (meth)acrylic acid ester in which the polar group is an amide group include N-(1,1-dimethyl-3-oxybutyl)(meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-dimethylaminopropyl(meth)acrylamide, N-isopropyl(meth)acrylamide, Nt-butyl(meth)acrylamide, N-(hydroxymethyl)acrylamide, and (2)-hydroxypropyl(meth)acrylamide. Of these, N-(1,1-dimethyl-3-oxybutyl)acrylamide is more preferable.
[0099] Examples of the amino group-containing (meth)acrylic acid ester in which the polar group is an amino group include N,N-dimethylaminoethyl (meth)acrylate and N,N-diethylaminoethyl (meth)acrylate, and among these, N,N-dimethylaminoethyl methacrylate is more preferable.
[0100] Examples of the phosphate group-containing (meth)acrylic acid polypropylene film phosphate (meth)acrylate, in which the polar group is a phosphate group, include 2-(meth)acryloyloxyethyl acid phosphate, di-(2-methacryloyloxyethyl)-phosphate, 2-(meth)acryloyloxypropyl acid phosphate, 2-(meth)acryloyloxybutyl acid phosphate, acid phosphooxy polyoxypropylene glycol monomethacrylate, and acid phosphooxy polyoxyethylene glycol monomethacrylate, and among these, 2-methacryloyloxyethyl acid phosphate is more preferred.
[0101] The epoxy group-containing (meth)acrylic acid ester in which the polar group is an epoxy group is, for example, glycidyl (meth)acrylate, β-methylglycidyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate glycidyl ether, 3,4-epoxycyclohexylmethyl (meth)acrylate, 3-epoxycyclo-2-hydroxypropyl (meth)acrylate, 6-methyl-3,4-epoxycyclohexylmethyl (meth)acrylate, 3,4-epoxybutyl (meth)acrylate, 6,7-epoxyheptyl (meth)acrylate, 6,7-epoxyheptyl α-ethyl (meth)acrylate, α-ethyl glycidyl acrylate, α-n-propyl glycidyl acrylate, and α-n-butyl glycidyl acrylate. Among these, glycidyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate glycidyl ether, and 3,4-epoxycyclohexylmethyl (meth)acrylate are more preferred.
[0102] The methyl (meth)acrylate and the polar group-containing (meth)acrylic ester or (meth)acrylic acid are preferably mixed in a ratio of 5 to 900, more preferably 10 to 500, and even more preferably 20 to 300, of 100 to 100 of methyl (meth)acrylate. If the ratio is less than 5, the contact angle may become large and the adhesion between the anchor coat layer and the vapor deposition layer may become poor, whereas if the ratio is 900 or more, the coating may become hard and the adhesion between the polyolefin substrate and the anchor coat layer may become poor.
[0103] The amount of the resin material containing the methyl (meth)acrylate and the polar group-containing (meth)acrylic acid ester or (meth)acrylic acid is preferably 3 to 90% by mass, more preferably 5 to 80% by mass, and even more preferably 10 to 70% by mass, based on the total amount of the anchor coating agent (100%). These may be used alone or in combination of two or more kinds.
[0104] The curing agent is preferably a polyisocyanate-based compound, and is selected from conventionally known polyisocyanates without any particular limitation, and examples thereof include aliphatic polyisocyanates or aromatic aliphatic polyisocyanates, and examples thereof include aromatic diisocyanates such as tolylene diisocyanate and 4,4'-diphenylmethane diisocyanate, aliphatic diisocyanates such as hexamethylene diisocyanate, xylylene diisocyanate, isophorone diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, 4,4'-dicyclohexyl diisocyanate, and pentane-1,5-diisocyanate (Stabio PDI), and modified products thereof such as trimethylolpropane trimer, isocyanurate, biuret, and allophanate, and examples of commercially available products include LG Curing Agent C and LG Curing Agent D (both manufactured by Tokyo Ink Co., Ltd.). These may be used alone or in combination of two or more.
[0105] The amount of the curing agent added is preferably 1 to 20% by mass, more preferably 2 to 18% by mass, and even more preferably 4 to 15% by mass, based on the total amount of the anchor coating agent (100%). These may be used alone or in combination of two or more kinds.
[0106] The silane coupling agent preferably contains at least one group selected from a group containing a nitrogen atom, a group containing a sulfur atom, and a vinyl group. The inclusion of a silane coupling agent having the specific group contributes to improving the adhesion between the anchor coat layer and the deposition layer.
[0107] Examples of groups containing a nitrogen atom include amino groups, imino groups, isocyanate groups (-N=C=O), ureido groups (-NH-CO-NH2), nitro groups (=NO), carbamate groups (-O-CO-N<), and quaternary ammonium salts.
[0108] Examples of silane coupling agents having an amino group include 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltripropoxysilane, 3-aminopropylmethyldimethoxysilane, 3-aminopropylmethyldiethoxysilane, 3-triethoxysilyl-N-(1,3-dimethyl-butylidene)propylamine, bis(3-triethoxysilylpropyl)amine, bis(3-trimethoxysilylpropyl)amine, bis(3-methyldimethoxysilylpropyl)amine, bis(triethoxysilylmethyl)amine, N-(2-aminoethyl)-3 -aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldiethoxysilane, N-(n-butyl)-3-aminopropyltrimethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, N,N'-bis[3-(trimethoxysilyl)propyl]ethylenediamine, N-(vinylbenzyl)-2-aminoethyl-3-aminopropyltrimethoxysilane hydrochloride, etc. Among them, 3-aminopropyltrimethoxysilane and N-(2-aminoethyl)-3-aminopropyltrimethoxysilane are more preferred.
[0109] Commercially available products include KBP-64, KBP-90, KBE-9103P, KBE-903, KBM-6803, KBM-573, KBM-575, KBM-602, KBM-603, KBM-903, KBM-6103, X-12-1172ES, X-12-972F, X-12-5263HP, and X-88-475 (all manufactured by Shin-Etsu Chemical Co., Ltd.).
[0110] Examples of silane coupling agents having an isocyanate group include trialkoxysilanes such as 3-isocyanatepropyltrimethoxysilane, 3-isocyanatepropyltriethoxysilane, 3-isocyanatepropylmethyldimethoxysilane, and 3-isocyanatepropylmethyldiethoxysilane, as well as trimers (isocyanurates) of these compounds. Of these, 3-isocyanatepropyltrimethoxysilane is more preferred.
[0111] Commercially available products include KBE-9007N, X-12-1159, X-12-1159L, and KBM-9659 (all manufactured by Shin-Etsu Chemical Co., Ltd.), SILQUEST Silane A-1310, and SILQUEST Silane Y-5187 (all manufactured by Momentive Corporation).
[0112] Examples of silane coupling agents having a ureido group include trialkoxysilanes such as 3-ureidopropyltrialkoxysilane.
[0113] Commercially available products include KBE-585A and KBM-585 (both manufactured by Shin-Etsu Chemical Co., Ltd.).
[0114] Examples of silane coupling agents having a nitro group include trialkoxysilanes such as 3-nitropropyltrimethoxysilane and 3-nitropropyltriethoxysilane.
[0115] Examples of silane coupling agents having a carbamate group include (3-carbamate ethyl)propyl trimethoxy silane, (3-carbamate ethyl)propyl tripropoxy silane, (3-carbamate propyl)propyl triethoxy silane, (3-carbamate propyl)propyl trimethoxy silane, (3-carbamate propyl)propyl tripropoxy silane, (3-carbamate butyl)propyl triethoxy silane, (3-carbamate butyl)propyl trimethoxy silane, (3-carbamate butyl)propyl tripropoxy silane, (3-carbamate butyl)butyl tripropoxy silane, (3-carbamate butyl)propyl tripropoxy silane, Examples of the trialkoxysilane include (3-carbamate ethyl)propyl methyl diethoxysilane, (3-carbamate pentyl)propyl triethoxysilane, (3-carbamate hexyl)propyl triethoxysilane, (3-carbamate octyl)pentyl tributoxysilane, (3-carbamate ethyl)propyl silyl trichloride, (3-carbamate ethyl)propyl trimethylsilane, (3-carbamate ethyl)propyl dimethylsilane, (3-carbamate ethyl)propyl tributylsilane, (3-carbamate ethyl)ethyl-p-xylene triethoxysilane, and (3-carbamate ethyl)-p-phenylene triethoxysilane.
[0116] Examples of commercially available silane coupling agents having a quaternary ammonium salt include X-12-1126, KBM-9418-40, POLON-V8, X-12-1139, and X-12-1354-1 (all manufactured by Shin-Etsu Chemical Co., Ltd.).
[0117] Examples of the functional group containing a sulfur atom include a mercapto group and a sulfide group.
[0118] Examples of silane coupling agents having a mercapto group include trialkoxysilanes such as 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 3-mercaptopropyltripropoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropylmethyldiethoxysilane, 2-mercaptoethyltrimethoxysilane, and 2-mercaptoethyltriethoxysilane.
[0119] Commercially available products include KBM-802, KBM-803, X-12-1307, X-12-1056ES, and X-12-1154 (all manufactured by Shin-Etsu Chemical Co., Ltd.).
[0120] Examples of silane coupling agents having a sulfide group include bis(3-triethoxysilylpropyl)tetrasulfide, bis(2-triethoxysilylethyl)tetrasulfide, bis(4-triethoxysilylbutyl)tetrasulfide, bis(3-trimethoxysilylpropyl)tetrasulfide, bis(2-trimethoxysilylethyl)tetrasulfide, bis(4-trimethoxysilylbutyl)tetrasulfide, bis(3-triethoxysilylpropyl)trisulfide, bis(2-triethoxysilylethyl)trisulfide, bis(4-trimethoxysilylbutyl)trisulfide, bis(3-trimethoxysilylpropyl)trisulfide, bis(2-trimethoxysilylethyl)trisulfide, bis(4-trimethoxysilylbutyl)trisulfide, bis(3-trimethoxysilylpropyl)trisulfide, bis(2-trimethoxysilylethyl)trisulfide, bis(4-trimethoxysilylbutyl)trisulfide, bis(3-triethoxysilylpropyl)disulfide, bis(2-triethoxysilylethyl)disulfide, Examples of trialkoxysilanes include (4-triethoxysilylbutyl) disulfide, bis(3-trimethoxysilylpropyl) disulfide, bis(2-trimethoxysilylethyl) disulfide, bis(4-trimethoxysilylbutyl) disulfide, 3-trimethoxysilylpropyl-N,N-dimethylthiocarbamoyl tetrasulfide, 3-triethoxysilylpropyl-N,N-dimethylthiocarbamoyl tetrasulfide, 2-triethoxysilylethyl-N,N-dimethylthiocarbamoyl tetrasulfide, 2-trimethoxysilylethyl-N,N-dimethylthiocarbamoyl tetrasulfide, 3-trimethoxysilylpropyl benzothiazolyl tetrasulfide, 3-triethoxysilylpropyl benzothiazole tetrasulfide, 3-triethoxysilylpropyl methacrylate monosulfide, and 3-trimethoxysilylpropyl methacrylate monosulfide.
[0121] Examples of silane coupling agents having a vinyl group include vinyltrimethoxysilane, vinyltriethoxysilane, vinyltriisopropoxysilane, Examples of the silane include trialkoxysilanes such as vinyltributoxysilane, vinylmethyldimethoxysilane, and vinylmethyldiethoxysilane.
[0122] Commercially available products include KBE-1003, KBM-1003, KBM-1083, and X-12-1290 (all manufactured by Shin-Etsu Chemical Co., Ltd.).
[0123] The amount of the silane coupling agent added is preferably 0.1 to 10 mass % relative to the total amount of the anchor coating agent (100%), more preferably 0.5 to 7 mass %, and even more preferably 1 to 5 mass %. These may be used alone or in combination of two or more kinds.
[0124] In addition to the resin material containing the methyl (meth)acrylate and the polar group-containing (meth)acrylic acid ester or (meth)acrylic acid, the curing agent, and the silane coupling agent, organic solvents, colorants, inorganic fillers, organic fillers, defoamers, leveling agents, pigment dispersants, antistatic agents, slip agents, plasticizers, tackifiers, etc. may also be added to the anchor coating agent of the present invention, if necessary. These may be added alone or in combination of two or more kinds.
[0125] The anchor coating agent of the present invention may be an anchor coat set including a resin solution A containing a resin material containing the methyl (meth)acrylate and a polar group-containing (meth)acrylic acid ester or (meth)acrylic acid, and an organic solvent, a curing liquid B containing a curing agent and an organic solvent, and a silane coupling liquid C containing a silane coupling agent and an organic solvent. Note that the anchor coat set may be a two-liquid anchor coat set obtained by mixing the components contained in the silane coupling liquid C with the resin solution A and the curing liquid B.
[0126] The resin solution A, the curing solution B, and the silane coupling solution C in the anchor coat set may contain, as necessary, an organic solvent, a coloring material, an inorganic filler, an organic filler, an antifoaming agent, a leveling agent, a pigment dispersant, an antistatic agent, a slip agent, a plasticizer, a tackifier, etc. Any known and commonly used agent may be appropriately selected within a range that does not impair the properties as a curing agent.
[0127] The methyl (meth)acrylate and the polar group-containing (meth)acrylic ester or (meth)acrylic acid used in the resin solution A are preferably mixed in a ratio of 100 methyl (meth)acrylate to 5 or more and less than 900, more preferably 10 or more and less than 500, and even more preferably 20 or more and less than 300. If the mixing ratio is less than 5, the contact angle may become large and the adhesion between the anchor coat layer and the vapor deposition layer may become poor, and if the mixing ratio is 900 or more, the coating may become hard and the adhesion between the polyolefin substrate and the anchor coat layer may become poor.
[0128] The anchor coat set uses the resin solution A, the curing liquid B, and the silane coupling liquid C. That is, it is used as a three-liquid mixture. The content ratio of the resin solution A, the curing liquid B, and the silane coupling liquid C is preferably resin solution A / curing liquid B / silane coupling liquid C=91 / 3 / 6 to 40 / 25 / 35, more preferably 85 / 5 / 10 to 45 / 23 / 32, and even more preferably 80 / 6 / 14 to 50 / 20 / 30. By using the resin solution A, the curing liquid B, and the silane coupling liquid C in the above range as three liquids, excellent adhesion is achieved. In addition, the components contained in the silane coupling liquid C may be mixed with the resin solution A and used as a two-liquid mixture together with the curing liquid B.
[0129] The three-liquid mixture can be produced by mixing or dispersing the resin solution A, the curing liquid B, and the silane coupling liquid C by a known method. In particular, it is more preferable to mix or disperse them at a printing factory or the like. Mixing or dispersing can be easily performed by manual stirring, but various stirrers or dispersers such as dissolvers, paint shakers, and homomixers can also be used. These devices may be used alone or in combination of two or more types. When a two-liquid mixture is used, it can be produced in the same manner.
[0130] The three-liquid mixture is preferably used in gravure printing, and can be applied as is, but can also be adjusted to a desired viscosity by diluting with a diluting solvent in a Zahn Cup #3 (manufactured by Rigo Co., Ltd.) depending on the coating conditions and coating effect. In this case, the viscosity is preferably 10 to 40 seconds at 25°C. If it is less than 10 seconds, it tends to swim, and if it is more than 40 seconds, transferability during printing becomes poor.
[0131] The dilution solvent may be any solvent that can adjust the viscosity of the three-liquid mixture, and may be any organic solvent. Commercially available solvents may also be used, and are not particularly limited. Commercially available solvents include TS32 solvent (ester solvent), PU533 solvent (toluene-containing solvent), PU515 solvent (non-toluene-containing solvent), SL9155 solvent (non-toluene-containing solvent), CN104 solvent (non-toluene-containing solvent), AC372 solvent (non-toluene-containing solvent), PP575 solvent (toluene-containing solvent), SL9164 solvent (non-ketone-based solvent), and SL9170 solvent (non-ketone-based solvent) (all manufactured by Tokyo Ink Co., Ltd.).
[0132] The resin solution A can be produced by a known method by uniformly dissolving or dispersing methyl (meth)acrylate, a polar group-containing (meth)acrylic acid ester or (meth)acrylic acid, and various additives in the organic solvent. For dissolving or dispersing, various stirrers or dispersers such as a dissolver, a roll mill, a ball mill, a bead mill, a sand mill, an attritor, a paint shaker, an agitator, a Henschel mixer, a colloid mill, a pearl mill, an ultrasonic homogenizer, a wet jet mill, a kneader, or a homomixer can be used. These devices may be used alone or in combination of two or more. If air bubbles or coarse particles are contained in the resin solution, they are preferably removed using a known filter or centrifuge, since they reduce printability and print quality.
[0133] The curing liquid B can be produced by a known method by uniformly dissolving or dispersing a polyisocyanate compound and various additives in the organic solvent. For dissolving or dispersing, various stirrers or dispersers such as a dissolver, a roll mill, a ball mill, a bead mill, a sand mill, an attritor, a paint shaker, an agitator, a Henschel mixer, a colloid mill, a pearl mill, an ultrasonic homogenizer, a wet jet mill, a kneader, or a homomixer can be used. These devices may be used alone or in combination of two or more. If air bubbles or coarse particles are contained in the curing liquid, they are preferably removed using a known filter or centrifuge, since they deteriorate the printability and the quality of the printed matter.
[0134] The silane coupling liquid C can be produced by a known method by uniformly dissolving or dispersing the silane coupling agent and various additives in the organic solvent. For dissolving or dispersing, various stirrers or dispersers such as a dissolver, a roll mill, a ball mill, a bead mill, a sand mill, an attritor, a paint shaker, an agitator, a Henschel mixer, a colloid mill, a pearl mill, an ultrasonic homogenizer, a wet jet mill, a kneader, and a homomixer can be used. These devices may be used alone or in combination of two or more. If air bubbles or coarse particles are contained in the silane coupling liquid, they are preferably removed using a known filter or centrifuge, since they reduce printability and print quality.
[0135] Using the anchor coat set, it is preferable to form an anchor coat layer having a thickness of 0.05 to 1.5 μm on a polyolefin substrate by gravure printing, more preferably to form an anchor coat layer having a thickness of 0.08 to 1.2 μm, and even more preferably to form an anchor coat layer having a thickness of 0.1 to 1.0 μm. If the thickness is less than 0.05 μm, the deposition layer provided on the anchor coat layer is likely to crack due to the influence of substrate shrinkage caused by heat treatment such as retort treatment, and the gas barrier property may be poor, and if the thickness exceeds 1.5 μm, the adhesion to the polyolefin substrate and blocking resistance may be poor. In particular, it is more preferable to print and form the anchor coat layer by gravure printing using a multicolor gravure printer. This allows the anchor coat layer to be formed by gravure printing and wound up. The anchor coat layer formed using the anchor coat set is stable after printing, so that it can be stored in a rolled up state. Furthermore, a deposition layer and a barrier coat layer can be formed on the anchor coat layer.
[0136] The contact angle of the surface of the anchor coat layer in the present invention is preferably 20 degrees or more and 75 degrees or less, more preferably 30 degrees or more and 65 degrees or less, and even more preferably 40 degrees or more and 55 degrees or less. When the contact angle is within the above range, the adhesion between the polyolefin substrate and the deposition layer is dramatically improved, and the deposition layer is less likely to crack, so that good gas barrier properties, especially gas barrier properties after retort treatment, can be obtained. If the contact angle is less than 20 degrees, the adhesion with the deposition layer may be poor, and if the contact angle is more than 75 degrees, the polarity of the anchor coat layer itself may be high, and the adhesion with the polyolefin substrate may be poor.
[0137] The contact angle was measured at a temperature of 5° C. and a relative humidity of 50% (50% RH) by dropping distilled water in a drop amount of 2 μm onto the surface of the anchor coat layer, one second after the liquid had landed on the surface. The contact angle can be measured using a contact angle meter (portable contact angle meter PCA-1, manufactured by Kyowa Interface Science Co., Ltd.) or the like.
[0138] The method for producing a laminate of the present invention comprises, at least in this order, a step of preparing a polyolefin substrate, a step of forming an anchor coat layer having a thickness of 0.05 to 1.5 μm on at least one of the polyolefin substrates, a step of forming a vapor deposition layer on the anchor coat layer, and a step of forming a barrier coat layer on the vapor deposition layer, wherein the step of forming the anchor coat layer is a step of printing an anchor coat agent containing a resin material containing methyl (meth)acrylate and a polar group-containing (meth)acrylic acid ester or (meth)acrylic acid, a curing agent, and a silane coupling agent, and the polar group in the resin material is a hydroxyl group, an amide group, It is preferable that the polar group-containing (meth)acrylic ester or (meth)acrylic acid is at least one group selected from an amino group, a phosphate group, the silane coupling agent contains at least one group selected from a group containing a nitrogen atom, a group containing a sulfur atom, and a vinyl group, the mixing ratio of the methyl (meth)acrylate and the polar group-containing (meth)acrylic ester or (meth)acrylic acid is 5 or more and less than 900 parts of polar group-containing (meth)acrylic ester or (meth)acrylic acid to 100 parts of methyl (meth)acrylate, and the contact angle of the surface of the anchor coat layer formed in the anchor coat layer formation process is 20 degrees or more and 75 degrees or less.
[0139] The step of forming the anchor coat layer is preferably a step of gravure printing the anchor coat agent on a polyolefin substrate with a thickness of 0.05 to 1.5 μm, more preferably a step of gravure printing with a thickness of 0.08 to 1.2 μm, and even more preferably a step of gravure printing with a thickness of 0.1 to 1.0 μm. If the thickness is less than 0.05 μm, the deposition layer provided on the anchor coat layer is likely to crack due to the influence of substrate shrinkage caused by heat treatment such as retort treatment, and the gas barrier property may be poor, and if the thickness exceeds 1.5 μm, the adhesion to the polyolefin substrate and blocking resistance may be poor. In particular, it is more preferable to carry out gravure printing using a multicolor gravure printer. This allows the step of forming the anchor coat layer by the gravure printing step to include a winding step.
[0140] Since the anchor coat layer formed in the step of forming the anchor coat layer in the present invention is stable, a winding step may be provided after the anchor coat layer forming step, which allows storage in a wound state.
[0141] After the winding step, a step of forming a vapor deposition layer and a step of forming a barrier coat layer, which will be described later, can be included while unwinding the film.
[0142] The contact angle of the surface of the anchor coat layer formed by the gravure printing process is preferably 20 degrees or more and 75 degrees or less, more preferably 30 degrees or more and 65 degrees or less, and even more preferably 40 degrees or more and 55 degrees or less. When the contact angle is within the above range, the adhesion between the polyolefin substrate and the deposition layer is dramatically improved, and the deposition layer is less likely to crack, so that good gas barrier properties, especially gas barrier properties after retort treatment, can be obtained. If the contact angle is less than 20 degrees, the adhesion with the deposition layer may be poor, and if the contact angle is more than 75 degrees, the polarity of the anchor coat layer itself may be high, and the adhesion with the polyolefin substrate may be poor.
[0143] The contact angle was measured at a temperature of 5° C. and a relative humidity of 50% (50% RH) by dropping distilled water in a drop amount of 2 μm onto the surface of the anchor coat layer, one second after the liquid had landed on the surface. The contact angle can be measured using a contact angle meter (portable contact angle meter PCA-1, manufactured by Kyowa Interface Science Co., Ltd.) or the like.
[0144] The method for producing a laminate of the present invention preferably includes a step of forming a vapor-deposited layer on the anchor coat layer, and the step of forming the vapor-deposited layer is a step of forming a vapor-deposited film made of an inorganic oxide or a metal thin film.
[0145] The process of forming the deposition layer can be, for example, a vacuum deposition process, a sputtering process, an ion plating process, an ion cluster beam process, etc., of the physical vapor deposition (PVD) method, or a plasma CVD process, a thermal CVD process, a photo CVD process, an MOCVD process, etc., of the chemical vapor deposition (CVD) method. When using a vacuum deposition process, for example, an electron beam heating, a resistance heating, or an induction heating method can be used as a heating means for the evaporation material. When using an electron beam heating method, the degree of freedom in selecting the evaporation material is large. When a plasma assist process or an ion beam assist process is used during deposition, a denser deposition layer can be formed. In addition, when reactive deposition in which a gas such as oxygen is blown in during chemical deposition is used, a deposition layer with excellent transparency can be formed.
[0146] The thickness of the vapor-deposited layer formed in the step of forming the vapor-deposited layer is preferably in the range of 1 to 150 nm, more preferably in the range of 5 to 60 nm, and even more preferably in the range of 10 to 40 nm. If the thickness is less than 1 nm, the desired gas barrier properties may not be exhibited, and if the thickness exceeds 150 nm, the polyolefin substrate may be deformed or altered by heat during the step of forming the vapor-deposited layer, and cracks may easily occur in the vapor-deposited layer, which may impair the gas barrier properties.
[0147] The method for producing a laminate of the present invention preferably includes a step of forming a barrier coat layer on the deposition layer, and the step of forming the barrier coat layer is a step of forming a coating film of a gas barrier composition obtained by polycondensing an alkoxide and a water-soluble polymer by a sol-gel method. As the step of forming the barrier coat layer, a known step can be used, and for example, a printing step such as gravure printing or flexographic printing, or a wet coating step using a roll coater, a reverse roll coater, a gravure offset coater, a gravure coater, a microgravure coater, a knife coater, a bar coater, a wire bar coater, a die coater, a dip coater, or the like can be used. Among them, a printing step using gravure printing and a wet coating step using a roll coater are more preferable.
[0148] The step of preparing the polyolefin substrate may be a step of preparing polyethylene, polypropylene, ethylene-vinyl acetate, copolymers thereof, co-extruded films thereof, or the like, and may be a step of preparing a stretched product. It may also be a step of preparing a sealant substrate such as low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), high-density polyethylene (HDPE), acid-modified polyethylene, non-oriented polypropylene (CPP), acid-modified polypropylene, or copolymer polypropylene. There is no particular restriction on the thickness of the polyolefin substrate as long as it is within a range that does not interfere with printability, winding suitability, or the like, but it is preferably 5 to 300 μm, more preferably 6 to 250 μm.
[0149] The method for producing the laminate of the present invention may include, in addition to the steps of forming the anchor coat layer, forming the vapor deposition layer, and forming the barrier coat layer, a step of forming an adhesive layer, a step of forming a pressure-sensitive adhesive layer, a step of forming a printing layer, a step of forming a heat seal layer, and a step of preparing other substrates.
[0150] The step of preparing another substrate is preferably a step of preparing a polyolefin substrate equivalent to that of the present invention, but may be a step of preparing a substrate generally used as a packaging material, and more preferably a step of preparing a substrate used as the outermost surface of the packaging material.
[0151] The step of forming the adhesive layer may be a dry lamination step, a non-solvent lamination step, a wet lamination step, an extrusion lamination step, a thermal lamination step, or a coating step of applying an adhesive or an adhesive ink.
[0152] When an adhesive is used in the lamination step, a commercially available adhesive may be used, and examples of such adhesives include two-component or one-component urethane resin adhesives, acrylic, epoxy, polyester, polyethyleneimine, polybutadiene, water-based urethane, isocyanate, organic titanium, and starch-based water-soluble adhesives, and aqueous adhesives such as vinyl acetate emulsions.
[0153] The adhesive ink preferably contains a polyolefin resin, a chlorinated polyolefin resin, or a (meth)acrylic resin. Preferred examples of the polyolefin resins and chlorinated polyolefin resins include polyethylene, polypropylene, polybutene, ethylene-propylene copolymers, ethylene-vinyl acetate copolymers, and the like, or blends thereof, chlorinated polyethylene, chlorinated polypropylene, chlorinated ethylene-propylene copolymers, and acid anhydride modified versions of these, and among these, chlorinated polypropylene, acid-modified polyolefins, acid-modified chlorinated polyolefins, and chlorinated ethylene-vinyl acetate copolymers (chlorinated EVA) are more preferred.
[0154] The adhesive or adhesive ink may also contain other resins, solvents, inorganic fillers, organic fillers, defoamers, leveling agents, antiblocking agents, waxes, pigment dispersants, antistatic agents, slip agents, plasticizers, tackifiers, antioxidants, surfactants, UV absorbers, surface conditioners, pH adjusters, charge imparting agents, bactericides, deodorants, wetting agents, antiskinning agents, metal chelating agents, and the like.
[0155] The step of forming the printed layer is a step of applying a printing ink containing a resin used in general gravure printing inks, such as polyurethane resins, polyolefin resins, shellacs, rosin-modified maleic acid resins, rosin-modified phenolic resins, cellulose acetate, cellulose acetyl propionate, cellulose acetyl butyrate, chlorinated rubber, cyclized rubber, halogenated vinyl resins (e.g., vinyl chloride resins, fluorine-containing vinyl resins, etc.), polyvinyl acetate, vinyl chloride-vinyl acetate copolymers, polystyrene resins, acrylic resins, acrylic-styrene copolymers, polyacrylic esters, polyester resins, polyvinylidene chloride resins, ketone resins, polyamide resins, nitrocellulose resins, rosin resins, styrene-maleic acid resins, alkyd resins, and ethylene-vinyl alcohol resins. The printing ink may contain, in addition to the resin, a colorant, a solvent, an inorganic filler, an organic filler, an antifoaming agent, a leveling agent, an antiblocking agent, a wax, a pigment dispersant, an antistatic agent, a slip agent, a plasticizer, a tackifier, an antioxidant, a surfactant, an ultraviolet absorber, a surface conditioner, a pH adjuster, a charge imparting agent, a bactericide, a deodorant, a wetting agent, an antiskinning agent, a metal chelating agent, and the like.
[0156] The step of forming the heat seal layer is preferably a step of imparting heat sealability, and may be a step of preparing the sealant substrate or a general sealant film. Examples of the step of preparing a sealant film include a step of preparing the polyolefin film, colored film, polystyrene film, polyacrylonitrile film, ethylene-vinyl alcohol resin film, etc., which may be stretched or unstretched, and may be a step of preparing a film in which one or more types are laminated.
[0157] The step of forming the adhesive layer is preferably a step of applying an adhesive, and may further include a step of forming a release layer. EXAMPLES
[0158] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited thereto. In the examples and comparative examples, "parts" means "parts by mass" and "%" means "% by mass."
[0159] [Preparation of resin solution A] (Production Example 1) 100 parts of methyl methacrylate (MMA), 200 parts of 2-hydroxyethyl methacrylate (HEMA), and 1200 parts of a mixed solvent of n-propyl acetate / isopropyl alcohol=6 / 4 were charged into a beaker and stirred at 600 rpm for 30 minutes to prepare Liquid A1. Similarly, resin solutions of Production Examples 2 to 12 were prepared according to the formulations in Tables 1 and 2. Production Example 12 is similar to Example 2 of Patent Document 1.
[0160] [Preparation of hardening liquid B] (Production Example 21) 50 parts of tolylene diisocyanate TMP (trimethylolpropane) trimer (TDI3TMP) and 50 parts of ethyl acetate were charged into a beaker and stirred at 600 rpm for 30 minutes to prepare liquid B1. Similarly, each of the curing liquids of Production Examples 22 to 25 was prepared according to the formulations in Table 3. Production Example 25 is similar to Example 2 of Patent Document 1.
[0161] [Preparation of Silane Coupling Liquid C] (Production Example 31) 10 parts of KBM-903 (3-aminopropyltrimethoxysilane, Shin-Etsu Chemical Co., Ltd.) and 90 parts of a mixed solvent of n-propyl acetate / isopropyl alcohol=7 / 3 were placed in a beaker and stirred at 600 rpm for 30 minutes to prepare Liquid C1. Similarly, silane coupling solutions of Production Examples 32 to 35 were prepared according to the formulations in Table 4. Production Example 35 used a silane coupling agent that did not contain at least one of a group containing a nitrogen atom, a group containing a sulfur atom, and a vinyl group.
[0162] The materials used were as follows: MA: Methyl acrylate DAAM: Diacetone acrylamide (N-(1,1-dimethyl-3-oxybutyl)acrylamide) DAM: N,N-dimethylaminoethyl methacrylate Kayamer PM-1: 2-methacryloyloxyethyl acid phosphate, manufactured by Nippon Kayaku Co., Ltd. GMA: glycidyl methacrylate MAA: Methacrylic acid HDI3TMP: Hexamethylene diisocyanate trimethylolpropane trimer HDI nurate: Isocyanurate of hexamethylene diisocyanate XDI3TMP: Xylylene diisocyanate trimethylolpropane trimer TDI: Tolylene diisocyanate KBE-9007N: 3-isocyanatepropyltriethoxysilane (Shin-Etsu Chemical Co., Ltd.) KBM-803: 3-mercaptopropyltrimethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd. KBE-1003: Vinyltriethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd. KBE-403: 3-glycidoxypropyltriethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd.
[0163] [Table 1]
[0164] [Table 2]
[0165] [Table 3]
[0166] [Table 4]
[0167] [Preparation of anchor coating agent] Anchor Coating Agent 1 (Example 1) 100 parts of A liquid 1, 15 parts of B liquid 1, and 30 parts of C liquid 1 were charged into a beaker and stirred at 600 rpm for 30 minutes to prepare 145 parts of anchor coating agent 1 of Example 1.
[0168] Similarly, anchor coating agents of Examples 2 to 20 and Comparative Examples 1 to 7 were prepared according to the formulations in Tables 5 to 7. Comparative Example 7 is similar to Example 2 of Patent Document 1.
[0169] [Table 5]
[0170] [Table 6]
[0171] [Table 7]
[0172] [Preparation of barrier coating agent] 385g of water, 67g of isopropyl alcohol, and 9.1g of 0.5N hydrochloric acid were mixed to obtain a solution with a pH of 2.2. 175g of tetraethoxysilane as a metal alkoxide and 9.2g of glycidoxypropyltrimethoxysilane as a silane coupling agent were mixed into this solution while cooling to 10°C to obtain solution A. Solution B was obtained by mixing 14.7 g of polyvinyl alcohol having a saponification degree of 99% or more and a polymerization degree of 2400 as a water-soluble polymer, 324 g of water, and 17 g of isopropyl alcohol. The solution A and the solution B were mixed in a ratio of 6.5:3.5 by mass to obtain a barrier coating agent 1.
[0173] [Laminated body production] (Example 30) Using a two-head coater, anchor coating agent 1 was printed in a first unit on one side of a 20 μm-thick OPP film (P2171, abbreviated as OPP, manufactured by Toyobo Co., Ltd.) as a polyolefin substrate so as to have a film thickness of 1.0 μm, forming an anchor coating layer coating film to produce AC laminate 1. At this time, anchor coating agent 1 was diluted with WA734 (non-toluene-based solvent, manufactured by Tokyo Ink Co., Ltd.) and adjusted to a viscosity of 17 seconds using Zahn cup No. 3. Similarly, AC laminates 2 to 24 and AC laminates 31 to 40 were obtained by changing the anchor coating agent and film thickness according to Tables 8 to 10.
[0174] Furthermore, a silicon oxide film (vapor deposition layer) having a thickness of 12 nm was formed by PVD on the anchor coat layer coating of the AC laminate 1 to produce a vapor deposition laminate 1. Similarly, vapor deposition laminates 2 to 24 and vapor deposition laminates 31 to 41 were obtained according to Tables 8 to 10.
[0175] Further, the barrier coating agent 1 was coated on the vapor deposition layer of the vapor deposition laminate 1 by a roll coater, and heat treatment was performed in an oven at 80° C. for 60 seconds to form a barrier coating layer coating having a thickness of 300 nm, thereby producing a barrier laminate 1. Similarly, according to Tables 8 to 10, barrier laminates 2 to 24 and barrier laminates 31 to 40 were obtained.
[0176] Further, Takelac A-525 / Takenate A-52 (abbreviation: DL, manufactured by Mitsui Chemicals, Inc.) was applied onto the barrier coat layer coating film of the barrier laminate 1 using A-Bar OSP-10 (manufactured by OSG System Products, Inc.), and a 60 μm-thick non-oriented polypropylene film for retort use, ZK207 (abbreviation: Reto CP, manufactured by Toray Film Processing Co., Ltd.), was laminated, and aging was performed at 40° C. for 72 hours to obtain a laminate 1 of OPP / anchor coat layer / vapor deposition layer / barrier coat layer / DL / Reto CP. According to Tables 8 to 10, laminates 2 to 24 and laminates 31 to 41 were obtained in the same manner as in Example 30. In addition, the laminate 38 did not have an anchor coat layer coating film (a vapor deposition layer film was formed on a polyolefin substrate), and the laminate 41 did not have a barrier coat layer (a heat seal layer was produced on a vapor deposition layer film).
[0177] <Contact angle of the anchor coat layer surface> Distilled water was dropped in a drop amount of 2 μm onto the coating surface of the anchor coat layer of the AC laminate 1, and the contact angle was measured 1 second after the liquid arrived at the coating surface under conditions of a measurement temperature of 25°C and a relative humidity of 50% (50% RH) using a contact angle meter (portable contact angle meter PCA-1, manufactured by Kyowa Interface Science Co., Ltd.). A contact angle of 20 degrees or more and 75 degrees or less results in good adhesion between the polyolefin substrate and the vapor deposition layer. The contact angle was evaluated on the following five-level scale. Similarly, the contact angles were measured for AC laminates 2 to 24 and AC laminates 31 to 40. The results are shown in Tables 8 to 10. Note that the contact angle of laminate 38, which did not have an anchor coat layer coating, was not measured and its contact angle was recorded as "-". ◎: Contact angle is between 40 degrees and 55 degrees ○: Contact angle is 30 degrees or more and less than 40 degrees, or more than 55 degrees and less than 65 degrees △: Contact angle is 20 degrees or more and less than 30 degrees, or more than 65 degrees and less than 75 degrees (no problem in practical use) ×: Contact angle is 10 degrees or more and less than 20 degrees, or more than 75 degrees and 85 degrees or more ××: Contact angle is less than 10 degrees or more than 85 degrees
[0178] For Laminates 1 to 24 and Laminates 31 to 41, the adhesion, blocking resistance, lamination strength, gas barrier properties, and retort resistance were evaluated and the results are shown in Tables 8 to 10.
[0179] <Adhesion> An adhesive tape (cellophane tape, 28 mm, manufactured by Nichiban Co., Ltd.) was applied to the barrier coat layer coating surface of the barrier laminate 1 and rubbed strongly with a thumb five times, and then the adhesive tape was slowly peeled off, and then rapidly peeled off halfway through. The degree to which the barrier coat layer coating surface or the anchor coat layer coating surface was attached to the adhesive tape was visually observed and evaluated. Those that were least attached to the adhesive tape were judged to have good adhesion. The degree to which the adhesive tape was removed was evaluated on a four-point scale: ◎: not at all, ○: slightly removed (0 to less than 10% of the peeled area per area), △: a little removed (10 to less than 20% of the peeled area per area, no practical problem), ×: almost all removed (20% or more of the peeled area per area). Similarly, the adhesion was evaluated for the barrier laminates 2 to 24 and the barrier laminates 31 to 40. The results are shown in Tables 8 to 10. Note that the adhesion of the laminate 41, which did not have a barrier coat layer coating, was not measured and was given a "-" mark.
[0180] <Blocking resistance> Two sheets of the barrier laminate 1 cut into a size of 3 cm x 3 cm were stacked with the barrier coat layer coating surface and the polyolefin substrate surface opposite the barrier coat layer coating surface, and subjected to a pressure of 20 N / cm at 50°C for 24 hours. 2After applying a load of this magnitude, the overlapping portion of the barrier coat layer coating surface and the polyolefin substrate surface opposite the barrier coat layer coating surface were peeled off, and the peeling state between the polyolefin substrate and the anchor coat layer coating surface, or between the anchor coat layer coating surface and the barrier coat layer coating surface, was confirmed, and the ink peeling and peeling resistance at this time were evaluated. Ink peeling and peeling resistance were evaluated on a two-level scale: ◯: peeled off without resistance, no peeling of the coating surface; ×: high resistance during peeling, peeling of the coating surface observed. Similarly, the blocking resistance was evaluated for the barrier laminates 2 to 24 and the barrier laminates 31 to 40. The results are shown in Tables 8 to 10. Note that no measurement was made for the laminate 41 on which no barrier coat layer film was formed, and the blocking resistance was given a "-" mark.
[0181] <Lamination strength> The laminate 1 was cut into a 15 mm wide strip to prepare a test piece, and five of these test pieces were prepared and subjected to T-peel and tensile tests at a tensile speed of 300 mm / min using a universal tensile tester (RTE-1210, manufactured by Orientec Co., Ltd.), and the laminate strength of each test piece was measured five times and the average value was calculated. The same test was also performed on laminate 38 (a polyolefin substrate coated with a vapor deposition layer and a barrier coat layer, a blank test piece) to which no anchor coating agent was applied, and the average value was calculated. The laminate strength was evaluated on a two-level scale: ◯: the laminate strength was 50% or more compared to the average value of the blank test pieces; ×: the laminate strength was less than 50% compared to the average value of the blank test pieces. Similarly, the laminate strength was evaluated for Laminates 2 to 24 and Laminates 31 to 41. The results are shown in Tables 8 to 10. The laminate strength of Laminate 38 was given the mark "-".
[0182] <Oxygen barrier properties> The oxygen permeability of the laminate 1 was measured using an oxygen gas permeability measuring device (OX-TRAN 2 / 22, manufactured by MOCON) under conditions of a measurement temperature of 23° C. and a humidity of 50% RH. The measurement was performed three times for each laminate under the same conditions, and the average was taken as the oxygen permeability of the laminate before retorting. Furthermore, the same packages as those prepared in <Retort resistance> described later were prepared, and the same retort treatment was carried out, and the packages were opened. The oxygen permeability of the laminates after the retort treatment was measured under the same conditions as described above. The measurements were carried out three times for each laminate under the same conditions, and the average was taken as the oxygen permeability of the laminates after retort. The change in oxygen transmission rate of the laminate before and after retorting was evaluated. The smaller the change in oxygen transmission rate, the better the oxygen barrier property. The oxygen permeability was evaluated on a three-point scale: ◯: no change at all, △: change rate of 0.1% to less than 10% (no practical problem), ×: change rate of 10% or more. Similarly, the oxygen barrier properties were evaluated for Laminates 2 to 24 and Laminates 31 to 41. The results are shown in Tables 8 to 10.
[0183] <Water vapor barrier properties> The water vapor permeability of the laminate 1 was measured using a water vapor permeability measuring device (PERMATRAN-W 3 / 34, manufactured by MOCON) under conditions of a measurement temperature of 40° C. and a relative humidity of 90% RH. The measurement was performed three times for each laminate under the same conditions, and the average was taken as the water vapor permeability of the laminate before retorting. Furthermore, the same packaging as that prepared in <Retort resistance> described later was used, and the same retort treatment was carried out, and the laminate after the retort treatment was opened, and the water vapor permeability was measured under the same conditions as above. Each laminate was measured three times under the same conditions, and the average was taken as the water vapor permeability of the laminate after retort. The change in water vapor permeability of the laminate before and after retorting was evaluated. The smaller the change in water vapor permeability, the better the water vapor barrier property. The water vapor permeability was evaluated on a three-point scale: ◯: no change at all, △: change rate of 0.1% to less than 10% (no practical problem), ×: change rate of 10% or more. Similarly, the water vapor barrier properties were evaluated for the laminates 2 to 24 and the laminates 31 to 41. The results are shown in Tables 8 to 10.
[0184] <Retort resistance> Two sheets of laminate 1 are subjected to 3kgf / cm 2 The pieces were bonded by heat sealing under conditions of 180° C. for 1 second to obtain a packaging bag 1 having an opening and a size of 15 cm×10 cm. Packaging bag 1 was filled with a 1 / 1 / 1 mixture of salad oil / ketchup / vinegar as the contents, and the opening was sealed by heat sealing under the same conditions as above to create a package. This packaging bag was retorted at 120°C for 40 minutes using a hot water shower, and the appearance of the package was visually observed and evaluated. The appearance of the package was evaluated as to whether swelling due to peeling of the anchor coat layer and the deposition layer could be confirmed. Packages in which no swelling was confirmed were judged to have good retort resistance. The appearance of the package was evaluated on a three-point scale: ◯: no change at all, △: slight swelling could be confirmed (no practical problem), ×: swelling could be confirmed. Similarly, the retort resistance was evaluated for packaging bags 2 to 24 and packaging bags 31 to 41. The results are shown in Tables 8 to 10.
[0185] [Table 8]
[0186] [Table 9]
[0187] [Table 10]
[0188] According to Tables 8 to 10, in Laminates 1 to 24 of Examples 30 to 53 using the anchor coating agents of Examples 1 to 20, the contact angle of the anchor coating layer is within a specific range, and therefore it is clear that the adhesion between the polyolefin substrate and the anchor coating layer or between the anchor coating layer and the deposition layer is excellent. It is also clear that the blocking resistance is also excellent. Furthermore, it is clear that the laminate strength, gas barrier properties, and retort resistance are also excellent. The laminate 31 of Comparative Example 10, which uses an anchor coating agent 21 (Comparative Example 1) containing a resin material that does not contain at least one polar group selected from the group consisting of a hydroxyl group, an amide group, an amino group, a phosphate group, and an epoxy group, has a contact angle of the anchor coating layer outside the specific range, and it is clear that the laminate 31 has inferior adhesion, blocking resistance, lamination strength, gas barrier properties, and retort resistance. The laminate 32 of Comparative Example 11, which used an anchor coating agent 22 (Comparative Example 2) that does not contain a silane coupling agent, has a contact angle of the anchor coating layer outside the specific range, and it is clear that the laminate has inferior adhesion, blocking resistance, lamination strength, gas barrier properties, and retort resistance. Laminates 33 to 35 of Comparative Examples 12 to 14, which use anchor coating agents 23 to 25 (Comparative Examples 3 to 5) containing silane coupling agents that do not contain at least one of a nitrogen-atom-containing group, a sulfur-atom-containing group, and a vinyl group, have contact angles of the anchor coating layer outside the specific range, and are clearly inferior in adhesion, blocking resistance, lamination strength, gas barrier properties, and retort resistance. The laminate 36 of Comparative Example 15, which used an anchor coating agent 26 (Comparative Example 6) containing a resin material in which the mixing ratio of methyl methacrylate (MMA) and the polar group-containing methacrylic acid ester (HEMA) was outside the range, had a contact angle of the anchor coating layer outside the specific range, and it was clear that the laminate had inferior adhesion, blocking resistance, lamination strength, gas barrier properties, and retort resistance. The laminate 37 of Comparative Example 16, which uses an anchor coating agent 27 (Comparative Example 7) that does not contain a silane coupling agent similar to that in Patent Document 1, has a contact angle of the anchor coating layer outside the specific range, and it is clear that the laminate has inferior adhesion, blocking resistance, lamination strength, gas barrier properties, and retort resistance. It is clear that the laminate 38 of Comparative Example 17, which does not have an anchor coat layer, is inferior in adhesion, blocking resistance, gas barrier properties, and retort resistance. Note that the laminate 38 has a certain degree of laminate strength. The laminate 39 of Comparative Example 18, in which the thickness of the anchor coat layer is outside the range, has a contact angle of the anchor coat layer within a specific range, but it is clear that the adhesion, blocking resistance, lamination strength, gas barrier properties, and retort resistance are inferior. In the laminate 40 of Comparative Example 19, in which the thickness of the anchor coat layer is outside the range, the contact angle of the anchor coat layer is outside the specific range, and it is clear that the adhesion, blocking resistance, lamination strength, gas barrier properties, and retort resistance are inferior. It is clear that the laminate 41 of Comparative Example 20, which does not have a barrier coat layer, is inferior in lamination strength, gas barrier properties, and retort resistance.
Claims
1. A laminate comprising, on a polyolefin substrate, an anchor coat layer having a thickness of 0.05 to 1.5 μm, a deposition layer, and a barrier coat layer, at least in this order, the anchor coat layer is a layer made of an anchor coat agent containing a resin material including methyl (meth)acrylate and a polar group-containing (meth)acrylic acid ester or (meth)acrylic acid, a curing agent, and a silane coupling agent; the polar group in the resin material is at least one polar group selected from a hydroxyl group, an amide group, an amino group, a phosphate group, and an epoxy group; the silane coupling agent contains at least one group selected from a group containing a nitrogen atom, a group containing a sulfur atom, and a vinyl group; a mixing ratio of the methyl (meth)acrylate to the polar group-containing (meth)acrylic acid ester or (meth)acrylic acid is 5 or more and less than 900 parts by weight of the polar group-containing (meth)acrylic acid ester or (meth)acrylic acid per 100 parts by weight of the methyl (meth)acrylate; and a contact angle of the surface of the anchor coat layer is 20 degrees or more and 75 degrees or less.
2. A packaging material comprising the laminate according to claim 1.
3. An anchor coating agent for use in the laminate according to claim 1, the anchor coating agent comprises a resin material containing methyl (meth)acrylate and a polar group-containing (meth)acrylic acid ester or (meth)acrylic acid, a curing agent, and a silane coupling agent; the polar group in the resin material is at least one polar group selected from a hydroxyl group, an amide group, an amino group, a phosphate group, and an epoxy group; the silane coupling agent contains at least one group selected from a group containing a nitrogen atom, a group containing a sulfur atom, and a vinyl group; a mixing ratio of the methyl (meth)acrylate and the polar group-containing (meth)acrylic acid or (meth)acrylic acid is 5 or more and less than 900 of the polar group-containing (meth)acrylic acid or (meth)acrylic acid per 100 of the methyl (meth)acrylate; The anchor coating agent is characterized in that the contact angle of the surface of the anchor coating layer formed by printing the anchor coating agent is 20 degrees or more and 75 degrees or less.
Citation Information
Patent Citations
Barrier film and laminated material using it
JP2006116733A
Small liquid bag package
JP2009262992A
Gas barrier laminate
JP2014195953A
Gas barrier film
JP2017094556A
Laminate, packaging container using the same, and method for producing them
JP2021020363A