Apparatus and method for fast charging of batteries - Patent application

Coating graphite anodes with Cu and/or Ni layers addresses lithium deposition issues in lithium-ion batteries, enabling ultra-fast charging with minimal capacity loss and maintaining energy density, thus supporting the widespread adoption of electric vehicles.

JP7595460B2Active Publication Date: 2024-12-06THE RES FOUNDATION FOR THE STATE UNIV OF NEW YORK +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020540390
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2019-01-18
Publication Date
2024-12-06
Estimated Expiration
2039-01-18

AI Technical Summary

Technical Problem

Current lithium-ion batteries face limitations in fast charging due to lithium metal deposition on graphite anodes, leading to capacity loss and reduced cycle life, which hinders the widespread adoption of electric vehicles.

Method used

Coating graphite anodes with ultrathin layers of copper (Cu) and/or nickel (Ni) metals to increase the overpotential for lithium nucleation, thereby suppressing lithium plating during ultra-fast charging.

Benefits of technology

The coated anodes enable lithium-ion batteries to achieve 500 cycles with less than 20% specific energy fade using a 10-minute fast charging protocol, maintaining energy density and cost comparable to current state-of-the-art batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007595460000001
    Figure 0007595460000001
  • Figure 0007595460000002
    Figure 0007595460000002
  • Figure 0007595460000003
    Figure 0007595460000003
Patent Text Reader

Abstract

An anode configured for fast charging a lithium-ion battery, comprising: an anode substrate; and a coating on a surface of the anode substrate that increases the overpotential of Li metal and inhibits Li metal plating during ultra-fast charging of a lithium-ion battery formed with the anode. The anode is fabricated by a process that applies a coating to the surface of the anode substrate, the coating comprising a nanolayer of Cu, a nanolayer of Ni, or a composite nanolayer of Cu and Ni. [Selected figure] Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] [Government support statement] This invention was made with Government support under DE-FOA-0001818, DE-EE0008356 and DE-SC0012704 awarded by the ETS Department of Energy. The United States Government has certain rights in this invention.

[0002] [CROSS REFERENCE TO RELATED APPLICATIONS] This application claims the benefit of U.S. national stage application PCT / US2019 / 014095, filed January 18, 2019, which has the benefit of the filing date of provisional application Ser. No. 62 / 618,116, filed January 17, 2018. The contents of the provisional application are incorporated herein by reference.

[0003] The present invention relates generally to lithium ion batteries, and more particularly to a lithium ion cell or battery for fast charging that includes an anode formed to increase the overpotential of Li metal nucleation and growth relative to an uncoated anode surface (e.g., graphite), thus inhibiting Li deposition ("metal plating") during ultra-fast charging, while still promoting Li ion diffusion into the graphite substrate. By mitigating Li plating, a cell or battery having a graphite anode so fabricated with a coating will meet the EERE goal of achieving 500 cycles with less than 20% fade in specific energy using a 10 minute fast charge protocol. The coating in the aggregate is about 2-200 nm thick, preferably about 2-10 nm (e.g., 5 nm). [Background technology]

[0004] Currently produced electric vehicles (EVs) rely on the use of lithium-ion battery technology due to its high energy and power density and its relative technological maturity compared to other emerging systems such as Li / S and Li / O2. Ahmed, S., et al., Enabling fast charging - A battery technology gap assessment. Journal of Power Sources (2017); 367(Supplement C): p. 250-262. However, a major barrier facing the adoption of electric vehicles is that currently utilized lithium-ion storage batteries require a significant amount of time to charge (approximately 30 minutes) compared to the time required to refuel an internal combustion engine-powered vehicle (less than 10 minutes). Thus, the need to develop Li-ion batteries that can be charged in approximately 10 minutes (at a 6C rate) without sacrificing range, cost, or cycle life is crucial for the widespread implementation of EVs.

[0005] A major barrier preventing ultrafast charging of state-of-the-art lithium-ion batteries is the occurrence of lithium metal deposition, or lithium plating, on the graphite anode, as reported by Nitta, N., et al., Li-ion battery materials: present and future. Mater. Today (Oxford, UK) (2015); 18(5): p. 252-264. Graphite anodes have been shown to have a low anode degradation rate of 0.05-0.1 V vs as reported in Waldmann, T., et al., Interplay of Operational Parameters on Lithium Deposition in Lithium-Ion Cells: Systematic Measurements with Reconstructed 3 -Electrode Pouch Full Cells. Journal of The Electrochemical Society (2016); 163(7): p. A1232-A1238 and Liu, Q., et al., Understanding undesirable anode lithium plating issues in lithium-ion batteries. RSC Adv. (2016); 6(91): p. 88683-88700; Agubra, V. and J. Fergus, (Degradation mechanisms of lithium-ion battery anodes) Materials (2013)6 (4): p. 1310. It operates at an operating potential of Li / Li+.

[0006] Thus, the operating voltage is very close to that of metallic Li deposition. Under normal charging conditions at low rates, Li+ ions intercalate into the graphite anode. However, under high-rate charging conditions, the rate of transport of Li+ ions to the anode surface is greater than the rate of Li+ diffusivity in graphite, resulting in the accumulation of Li+ ions on the electrode surface. Waldmann, T., et al., Interplay of Operational Parameters on Lithium Deposition in Lithium-Ion Cells: Systematic Measurements with Reconstructed 3-Electrode Pouch Full Cells, Journal of The Electrochemical Society (2016); 163(7): p. A1232-A1238. These conditions cause polarization of the electrode below the 0V threshold for Li deposition, resulting in Li plating. Lithium deposition depends on the charging conditions, with high rates, low temperatures and high states of charge (SOC) all increasing electrode polarization and thus facilitating Li deposition. Liu, Q., et al., Understanding undesirable anode lithium plating issues in lithium-ion batteries. RSC Adv (2016); 6(91): p. 88683-88700.

[0007] Lithium deposition depends on the charging conditions, with fast rates, low temperatures and high states of charge (SOC) all increasing the anode polarization that facilitates Li deposition. Q. Liu, et al. RSC Adv., 6, 88683 (2016). The fast charging capability of state-of-the-art Li-ion batteries is limited by the occurrence of Li plating on the graphite anode, which operates at operating potentials of 0.05-0.1 V vs. Li / Li+. T. Waldmann, et al. J. Electrochem. Soc., 163, A1232 (2016); Q. Liu, et al. RSC Adv., 6, 88683 (2016); 5. V. Agubra, et al. Materials, 6, 1310 (2013).

[0008] When the anode is polarized below 0 V, Li deposition on the graphite surface is favored over intercalation, resulting in plating. Due to the high reactivity of Li metal, subsequent reactions with the electrolyte occur, consuming some of the active lithium and resulting in battery capacity loss.

[0009] To suppress Li plating, multiple strategies have been demonstrated with limited effectiveness, including optimization of the electrolyte composition to increase ionic conductivity and / or control the SEI resistance. Jones, JP, et al., The Effect of Electrolyte Composition on Lithium Plating During Low Temperature Charging of Li-Ion Cells. ECS Transactions (2017); 75(21): p. 1-11; Liu, QQ, et al., Effects of Electrolyte Additives and Solvents on Unwanted Lithium Plating in Lithium-Ion Cells. Journal of The Electrochemical Society (2017) 164(6): p. A1173-A1183, 13. Jumg, S., et al., Low-Temperature Performance Improvement of Graphite Electrode by Allyl Sulfide Additive and Its Film-Forming Mechanism. Journal of The Electrochemical Society (2016); 163(8): p. A1798-A1804. Smart, MC and BV Ratnakumar, Effects of Electrolyte Composition on Lithium Plating in Lithium-Ion Cells. Journal of The Electrochemical Society (2011); 158(4): p. A379- A389; Smart, MC, et al., Lithium-Ion Electrolytes Containing Ester Cosolvents for Improved Low Temperature Performance Journal of The Electrochemical Society (2010); 157(12): p. A1361-A1374; Smart, MC, BV Ratnakumar, and S. Surampudi, Use of Organic Esters as Cosolvents in Electrolytes for Lithium-Ion Batteries with Improved Low Temperature Performance Journal of The Electrochemical Society (2002); 149(4): p. A361-A370).

[0010] Known mitigating Li plating involves modifying the graphite anode to improve the diffusion rate, as reported in Cheng, Q., et al. Cheng, Q., et 1., KOH etched graphite for fast chargeable lithium-ion batteries Journal of Power Sources (2015); 284(Supplement C): p. 258-263; Deng, T. and X. Zhou, Porous graphite prepared by molybdenum oxide catalyzed gasification as anode material for lithium ion batteries Materials Letters (2016); 176 (Supplement C): p. 151-154; Park, J.-S., et al., Edge-Exfoliated Graphites for Facile Kinetics of Delithiation ACS Nano (2012); 6(12): p. 10770-10775; Shim, J.-H. and S. Lee, Characterization of graphite etched with potassium hydroxide and its application in fast-rechargeable lithium ion batteries. Journal of Power Sources (2016); 324(Supplement C): p. 475-483, and optimization of charging protocol. T. Waldmann, et al.J Electrochem. Soc ., 163, A1232 (2016); Ahmed, S., et al., Enabling fast charging - A battery technology gap assessment Journal of Power Sources (2017); 367(Supplement C): p. 250-262. Somerville, L., et al., The effect of charging rate on the graphite electrode of commercial lithium-ion cells: A post-mortem study Journal of Power Sources (2016); 335 (Supplement C): p. 189-196; Zhang, SS, The effect of the charging protocol on the cycle life of a Li-ion battery Journal of Power Sources (2006); 161(2): p. 1385-1391. Waldmann, T., M. Kasper, and M. Wohlfahrt-Mehrens, Optimization of Charging Strategy by Prevention of Lithium Deposition on Anodes in high-energy Lithium-ion Batteries-Electrochemical Experiments. Electrochimica Acta (2015); 178 (Supplement C): p.525-532. Based on the current body of research, none of the above strategies can provide sufficient benefit to enable cycling at extremely fast charging rates. Thus, exploration of new approaches to inhibit Li deposition during fast charging is warranted.

[0011] Control of Li deposition overpotential using Ni and Cu metal substrates During the deposition of lithium by the electrocrystallization process, there is a free energy barrier that must be overcome for Li nuclei to form on the electrode surface. To overcome this thermodynamic cost and promote the reaction, an overpotential is required. Theoretically, the total overpotential for electrocrystallization can be calculated from four separate contributions: (Formula 1) η=ηct+ηd+ηr+ηc where ηct, ηd, ηr, and ηc are the charge transfer, diffusion, reaction, and crystallization overpotentials reported by Winand, R., Electrocrystallization: Fundamental considerations and application to high current density continuous steel sheet plating, Journal of Applied Electrochemistry, 1991. 21(5): p. 377-385.

[0012] However, in practice, it is difficult to extract all four of these parameters from experimental data. As shown in a recent study by Pei, A., et al., Nanoscale Nucleation and Growth of Electrodeposited Lithium Metal, Nano Letters (2017); 17(2): p. 1132-1139, the electrode polarization during the electrocrystallization of Li can be more simply described as the sum of two terms: the nucleation overpotential (ηn), which is related to the initial nucleation of Li clusters and observed as an initial voltage drop, and the plateau overpotential (ηp), which describes the continuous growth of Li on the existing nuclei (Figure 7). It is noteworthy that the value of ηp is higher than ηn, because the addition of Li atoms to preformed nuclei has a lower thermodynamic cost than the initial nucleation. Sagane, F., et al., Effects of current densities on the lithium plating morphology at a lithium phosphorus oxynitride glass electrolyte / copper thin film interface. Journal of Power Sources, 2013. 233 (Supplement C): p. 34-42.

[0013] The overpotential of Li electrocrystallization is highly dependent on the electrode substrate, especially nickel (Ni) and copper (Cu) metal substrates, which show high overpotentials that are unfavorable for lithium deposition (Figure 2a). As reported by Yan, K., et al., Selective deposition and stable encapsulation of lithium through heterogeneous seeded growth, Nat. Energy, 2016. 1(3): p. 16010, at low current densities (10 mA cm -2The overpotentials for Li deposition on Cu and Li at 1000 K were determined to be -40 mV and -30 mV, respectively, compared to an overpotential of -15 mV on a carbon substrate. The proposed approach would take advantage of the high overpotentials on Cu and Ni substrates to suppress Li plating on metal-coated electrodes.

[0014] The driving force for the overpotential during Li nucleation is the interfacial energy difference between the substrate and Li metal, which depends on the dissimilarity of the crystal structures between Li and the substrate for deposition. Both Cu and Ni crystallize in the FCC structure, while Li metal is BCC. Furthermore, the atomic radii of Cu and Ni are 1.28A and 1.24A, respectively, compared to 1.55A for Li metal. Pauling, L., Atomic Radii and Interatomic Distances in Metals, Journal of the American Chemical Society, 1947. 69(3): p. 542-553.

[0015] Thus, as reported by Yan, K., et al., Selective deposition and stable encapsulation of lithium through heterogeneous seeded growth, Nat. Energy, 2016. 1(3): p. 16010, an overpotential is necessary to overcome the energy barrier associated with the structural mismatch during Li nucleation on metal surfaces. Further insight into the high overpotential for Li deposition on Ni and Cu is gained by inspection of the binary phase diagrams between Li and Cu or Ni (Fig. 5). Neither Cu nor Ni form alloy compound phases with Li at room temperature. Furthermore, there is no single-phase solubility of Cu or Ni in Li at room temperature, which would otherwise reduce the energy barrier for Li nucleation. Thus, a high overpotential is necessary to drive the Li deposition reaction on Cu and Ni surfaces.

[0016] As reported by Pei, A., et al., Nanoscale Nucleation and Growth of Electrodeposited Lithium Metal, Nano Letters, 2017. 17(2): p. 1132-1139, the overpotential for Li electrodeposition also depends on the current density. As shown in Figure 2b, for the electrodeposition of Li on Cu foil substrate, ηn is 0.1 mA / cm 2 (Red / solid line) -50mV, current density 5mA / cm 2 (purple / thick dotted line) increases to -350 mV, but ηp is 0.1 mA / cm 2 From -30mV at 5mA / cm 2 As shown, the voltage increases to about -140 mV at 0.3 mA / cm 2 , 0.5mA / cm 2 , 1mA / cm 2 The current densities at and are shown in orange (wavy line), green (dashed dotted line), and blue (thick solid line) in Figure 2b, respectively.

[0017] For comparison, the 3C rate (2mAhcm 2 Approximately 6mAcm for a graphite load of 2 The electrode overpotentials for graphite / NMC cells cycled at 1000 s (current densities of 1000 s) have been reported to be in the range of -50 mV to -150 mV (Figure 3). Thus, at similar current densities, the overpotential for Li deposition on Cu is greater than the overpotential for lithiation of graphite. The overpotential values ​​strongly suggest that Li metal nucleation and growth on metal-coated graphite electrodes is significantly suppressed at high charge rates, with Li ion intercalation into graphite being the more favored process. DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]

[0018] The present invention provides an entirely new concept in anodes for use in lithium-ion battery cells, where the overpotential for Li metal deposition at the surface is intentionally increased, thus suppressing Li metal deposition during ultra-fast charging of lithium-ion battery cells manufactured with the anode. This is achieved by coating the graphite anode substrate with an ultra-thin coating of Cu and / or Ni metal, which has a high overpotential unfavorable to lithium deposition. The nanometer-scale thickness of the metal coating (in the range of 2200 nm, preferably in the range of 2-10 nm (e.g., 5 nm)) allows the functionality of the graphite anode to be maintained, preserving the state-of-the-art energy density. By suppressing Li plating, the resulting NCM / graphite battery addresses the EERE goal of achieving 500 cycles with less than 20% fade of specific energy using a 10-minute fast charge protocol. [Brief description of the drawings]

[0019] Further features and advantages of the present invention will become apparent from the following description of embodiments, taken in conjunction with the accompanying drawings, in which: [Figure 1] 1A-1C are schematic diagrams of (a) prior art Li-plating on graphite surface during fast charging rates, and (b) preferential intercalation into graphite due to increased overpotential for Li nucleation provided by Cu or Ni surface coverage in accordance with the present invention. [Diagram 2] Figure 2 graphically illustrates (a) the voltage profile for Li deposition under galvanostatic control on Ni and Cu substrates at a current density of 10 mA cm2 with scaling on the vertical axis of 50 mV, and (b) the voltage profile for Li deposition on a copper substrate at current potentials up to 5 mA / cm2. [Diagram 3]Figure 3 graphically shows the anode potential measurements versus (Li / Li+) for three electrode cells with a graphite anode, lithium nickel cobalt manganese oxide (LiwNixCoyMnz02) (NMC) cathode, Li reference electrode, and 1:1 (ethylene carbonate:dimethyl carbonate (EC:DMC) 1 M LiPF6 charged at (a) 5 °C, (b) 20 °C, and (b) 45 °C, respectively. Measurements were collected for cells with charge rates ranging from 0.2 °C to 3 °C. [Figure 4] Figure 4 graphically illustrates the voltage profiles of galvanostatic (black) and double-pulse potentiostatic (red / solid) Li deposition showing the nucleation overpotential (F[n] and plateau overpotential (I]p) associated with the electrodeposition process. Pei, A., et ak, Nanoscale Nucleation and Growth of Electrodeposited Lithium Metal, Nano Letters, 2017. 17(2): p. 1132-

[0020] [Diagram 5] Figure 5 shows Li with (a) Cu and (b) Ni (from 2: Yan, K., et al., Selective deposition and stable encapsulation of lithium through heterogeneous seeded growth. Nat. Energy, 2016. 1(3): p. 16010.).

[0021] [Figure 6] Figure 6(a) shows the CV of pristine carbon fiber. Figure 6(b) shows carbon fiber with a 40 nm thick Cu film deposited by physical vapor deposition. Figure 6(c) shows the relationship between Cu film thickness and anodic peak height for Li-only intercalation from Cu-coated carbon fiber.

[0022] [Figure 7]Figure 7 graphs the energy obtained at various discharge rates for Si and Cu-coated Si, where the values ​​are normalized versus energy obtained at a C / 8 rate.

[0023] [Figure 8] Figures 8(a) and (b) are Nyquist plots as a function of electrode potential for (a) a pure graphite electrode and (b) a graphite electrode coated with a 5 nm Cu layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] Hereinafter, the embodiments of the present invention will be described in detail with reference to the drawings. In describing the present invention, in order to clearly understand the concept of the present invention, the description of related functions or configurations known in the art will be omitted in order to avoid obscuring the present invention with unnecessary details.

[0025] The present invention provides an electrode (e.g., an anode), a method for forming the electrode for fast charging a lithium ion battery fabricated with the electrode, the electrode or anode formed by the method, and a cell or battery (or cell) fabricated with the electrode / anode for fast charging.

[0026] In one form, the invention embodies a graphite electrode (i.e., anode) coated with an ultra-thin layer of Cu and / or Ni metal nanoparticles to achieve a coating thickness of about 2-10 nm to increase the overpotential for Li metal nucleation at the electrode / anode surface when operating in a cell or battery fabricated with the coated graphite anode. The coating relies on the anode of the invention (of the cell or battery) to inhibit Li metal plating during ultra-fast charging. By mitigating Li plating, the resulting graphite / nano-coated material (NMC) cell or battery addresses the U.S. Office of Energy Efficiency and Renewable Energy (EERE) goal of achieving 500 cycles with less than 20% fade in specific energy using a 10 minute fast charge protocol.

[0027] Graphite anodes are coated with nanometer-scale (<20 nm) layers of Ni and Cu metals that are applied to the surface of the anode substrate via DC magnetron sputtering. Ni and Cu metal substrates have high overpotentials that are unfavorable for lithium deposition. Yan, K., et al., Selective deposition and stable encapsulation of lithium through heterogeneous seeded growth, Nat. Energy, 2016. 1(3): p. 16010; Pei, A., et al., Nanoscale Nucleation and Growth of Electrodeposited Lithium Metal. During charging of a cell or battery fabricated with the coated graphite anodes, the overpotentials for Li deposition on the metal-coated anode substrate surface are greater in magnitude than the overpotentials for intercalation into the graphite (Figure la), resulting in favorable lithiation of graphite and inhibited Li plating (Figure lb). The suppression of Li deposition allows the battery to be charged using a 10 min protocol over extended cycles (>500 cycles).

[0028] Metal-coated graphite anode: LiNi 0.6 Mn 0.2 Co 0.2 It was paired with a O2 (622 NCM) cathode, a polymer separator and a 1M LiPF63:7EC:EMC based electrolyte. The proposed battery (or cell) will utilize the current state-of-the-art electrode materials (graphite and 622 NCM) with the only difference being the modification of the graphite anode substrate surface via DC magnetron sputtering method. Therefore, the cost of the proposed battery will be comparable to the current state-of-the-art. Furthermore, since the ultra-thin metal coating will be deposited only on the surface of the graphite anode substrate, there will be no significant increase in the inert anode mass. 8mg / cm2 For a graphite anode with a loading of 0.01 μm, the mass of a 5 nm Cu coating on the anode (substrate) surface is less than 1 mg Cu per gram of graphite. Thus, the cell specific energy is also maintained relative to the current state of the art.

[0029] We have prepared and characterized graphite anodes coated with nanometer-scale Ni layers, nanometer Cu layers, or composite nanolayers of Cu and Ni. Electrochemical evaluations are performed on the coated graphite anodes in half- and full-cell configurations by comparing the fast charging behavior of cells containing Cu / Ni coated electrodes (i.e., anodes) with uncoated graphite anodes.

[0030] As known in the art, materials with high overpotentials hinder Li metal deposition. In that regard, recent reports have shown that nickel (Ni) and copper (Cu) metal substrates have high overpotentials that are unfavorable for lithium deposition (Figures 2a, 2b). K. Yan, et al. Nat. Energy, 1, 16010 (2016); A. Pei, et al. Nano Lett., 17, 1132 (2017).

[0031] The anodes and methods of fabricating the anodes of the present invention take advantage of this high overpotential for Li deposition on Cu and Ni metal substrates to inhibit Li plating during fast charging protocols in battery cells and batteries fabricated with the anodes. The methods of the present invention utilize DC magnetron sputtering to deposit nanometer-scale layers of Ni and / or Cu onto prefabricated graphite anodes, where the controlled ultra-thin metal coverage increases the overpotential for Li metal deposition, thus inhibiting Li plating during very fast charging while still maintaining the functionality of a graphite (or graphite) electrode (Figures la and lb).

[0032] The specific overpotential value for Li deposition on Ni and Cu substrates depends on the current density, and at a current density of 5 mA cm 2The reported value for Cu substrate at 1000V is -350mV (Figure 2b). Ahmed, S., et al., Enabling fast charging - A battery technology gap assessment. Journal of Power Sources, 2017. 367 (Supplement C): p. 250-262.

[0033] By comparison, a 3C rate (2mAh cm 2 For a graphite loading of about 6mAcm 2 Electrode overpotentials for graphite / nanomaterial (NMC) cells cycled at 1000 V (current density of 1000 V) have been reported to range from -50 mV to -150 mV (Figures 3a, 3b, and 3c). T. Waldmann, et al. J Electrochem. Soc ., 163 (7), A1232 (2016). As shown, solid gray (thin solid line) indicates 0.2C cell 1, solid red (solid line) indicates 0.5 cell 1, solid orange (thick solid line) indicates 1C cell 1, solid blue (thick solid line) indicates 2C cell 1, solid gray (thickest solid line) indicates 3C cell 1, dashed gray (thin line) indicates 0.2C cell 2, dashed red (wavy line) indicates 0.5 cell 2, dashed orange (thick wavy line) indicates 1C cell 2, dashed blue (thick wavy line) indicates 2C cell 2, and dashed gray (thickest wavy line) indicates 3C cell 2. The overpotential for Li deposition on Cu substrates is larger in magnitude than the graphite electrode overpotentials reported at similar current densities, and therefore, graphite anode substrates coated with thin Ni and / or Cu metal layers may mitigate Li surface deposition and favor lithium intercalation into graphite, allowing ultrafast charging by inhibited Li plating.

[0034] The anode of the present invention is fabricated using the current state-of-the-art anode materials (graphite and 622NMC) and 1M LiPF63:7EC:EMC electrolyte. The only difference in fabrication compared to the current state-of-the-art Li-ion batteries is the modification of the graphite electrode surface via DC magnetron sputtering deposition. Thus, the cost of the proposed battery made with the anode of the invention is comparable to the current state of the art. And, the battery specific energy is maintained, since the ultra-thin metal coating is deposited only on the surface of the graphite anode, i.e., on the substrate surface. 8mg / cm2 coated with a 5nm Cu layer. 2 For a graphite anode with a loading of 1000 Li, the inert mass on the electrode surface is <1 mg Cu per gram of graphite. Suppressing Li deposition allows the battery to be charged using a 10 min protocol over extended cycling (>500 cycles).

[0035] In the device and method of the present invention, the overpotential for Li metal nucleation at the surface of the anode is intentionally increased, thus suppressing Li metal deposition during ultra-fast charging while maintaining the functionality of known graphite electrodes / anodes (Figure la).

[0036] As is known, the driving force of overpotential during heterogeneous nucleation of Li is the interfacial energy difference between the substrate and Li metal, which depends on the dissimilarity of the crystal structures between Li and the substrate for deposition. Both Cu and Ni crystallize in face-centered cubic (FCC) structure, while Li metal is in base-centered cubic (BCC) structure. Thus, an overpotential is required to overcome the energy barrier associated with the structural mismatch during Li nucleation on the metal surface.

[0037] In the method of the present invention, graphite / carbon black / polyvinylidene fluoride (PVDF) electrodes are fabricated using a slurry casting method. The surface of the electrode, i.e., the electrode substrate, is coated with Cu and Ni using a physical vapor deposition (PVD) method in which metals are evaporated under vacuum from a heated tungsten crucible. F. Nobili, et al. J Power Sources, 180, 845 (2008); M. Mancini, et al. . / . Power Sources, 190, 141 (2009); J. Suzuki, et al. Electrochem. Solid-State Lett., 4, Al (2001); F. Nobili, et al. Fuel Cells (Weinheim, Ger.), 9, 264 (2009).

[0038] Monitor the deposition rate and thickness by measuring the electrode mass using a quartz crystal microbalance (QCM) and adjust the temperature and deposition time to obtain Ni and Cu layers in the range of 2-10 nm. In our understanding, 8 mg / cm 2 For a graphite anode with a loading of 0.1 μm, for a 5 nm Cu coating the metal mass is less than 1 mg per gram of graphite.

[0039] High-resolution transmission electron microscopy (HR-TEM) was used to determine the uniformity and thickness of the metal film. The coated anodes were LiNi 0.6A cathode (622 NCM) paired with MnO2CoO2O2 is used and evaluated using a 1M LiPF63:7EC:EMC based electrolyte. Vinylene carbonate (VC) as reported by JC Burns et al. (J. Electrochem. Soc., 160, A1668 (2013); D. Aurbach, et al. Electrochim. Acta, 47, 1423 (2002)) and fluoroethylene carbonate as reported by H. Shin et al. (J. Electrochem. Soc., 162, A1683 (2015); B. Liu, et al. Electrochem. Solid-State Lett., 15, A77 (2012)), which have been used to form a more robust anode SEI in Li-ion cells, are evaluated to modify the solid-electrolyte interface (SEI).

[0040] A systematic investigation of the effect of Ni and Cu coating thickness, cell temperature, charge rate, and state of charge (SOC) on Li plating cycle life was performed in two and three electrode cell configurations. As reported by JP Jones, et al. ECS Trans., 75, 1 (2017); M. Petzl Journal of Power Sources, 254, 80 (2014), the anode potential in the three electrode cell configuration was measured (T. Waldmann, et al. J. Electrochem. Soc., 163, A2149 (2016); SS Zhang, J. Power Sources, 161, 1385 (2006)) and the heat flow associated with Li deposition was monitored using isothermal microcalorimetry (LE Downie, et al. J. Electrochem. Soc., 160, A588 (2013)) to detect and quantify Li deposition by plotting at different voltages. The extended cycling performance of the coated anode, which exhibited optimal electrochemical behavior, was further evaluated in a 2 Ah pouch cell.

[0041] The presence of Ni and / or Cu coatings on graphite anodes increases the Li nucleation overpotential and inhibits Li deposition compared to uncoated graphite anodes. Furthermore, the metal layer reduces the charge transfer resistance of the graphite electrode (as shown in Figure 8) (F. Nobili, et al. J Power Sources, 180, 845 (2008)). Thus, this device and method enables ultrafast charging by inhibiting the kinetics of Li metal plating while simultaneously improving the charge transfer kinetics at the graphite anode.

[0042] Scientific and other principles The first objective is to prepare and characterize graphite electrodes coated with nanometer-scale Ni or Cu layers. The main scientific question under this objective is the control of the thickness and uniformity of the metal coating. The graphite electrodes are coated with a 6 mg / cm 2 The films were fabricated with a target active material loading of 100 nm. Nanometer-scale (<20 nm) Ni and Cu layers were deposited on the graphite electrodes using DC magnetron sputtering deposition. Film thickness and uniformity were optimized through control of sputter time and sputter power. Thickness was monitored during deposition using a quartz crystal microbalance mounted in the deposition vacuum chamber adjacent to the substrate as reported in Lindner, M. and M. Schmid, Thickness Measurement Methods for Physical Vapor Deposited Aluminum Coatings in Packaging Applications: A Review. Coatings (2017); 7(1): p. 9.

[0043] The metal coated electrodes are characterized via SEM measurements including secondary electrons, backscattered electrons, and energy dispersive spectroscopy (EDS) mapping techniques. EDS mapping is used to evaluate the coating homogeneity of the metal film by identifying the presence of cracks or voids.

[0044] The second objective was to perform an electrochemical evaluation of Ni-graphite and Cu-graphite electrodes in half- and full-cell configurations. 0.6 MnO2Co 0.2 The O2-utilizing electrodes (622 NCM) cathodes were prepared with a target cathode:anode capacity ratio of 1:1.2. Initial electrochemical evaluation of uncoated graphite electrodes, Ni-graphite and Cu-graphite electrodes, and NCM cathodes was performed using half cells in a coin cell format. AC impedance, galvanostatic cycling, and rate capability tests will be used to characterize the various electrode types.

[0045] The evidence of Li metal deposition on the working electrodes of cells containing uncoated and coated graphite anodes is examined after electrochemical testing by destructive analysis. Optical microscopy is used to examine the anode surface for lithium deposits as reported by Park, G. et al. A study of the electrochemical properties and lithium deposition on graphite at low temperatures. Park, G., et ah, The study of electrochemical properties and lithium deposition of graphite at low temperature. Journal of Power Sources (2012); 199(Supplement C): p. 293-299; Waldmann, T., et ah, Temperature dependent ageing mechanisms in Lithium-ion batteries - A Post-Mortem study. Journal of Power Sources (2014); 262(Supplement C): p.129-135; Gallagher, KG, et ah, Optimizing Areal Capacities through Understanding the Limitations of Lithium-Ion Electrodes. Journal of The Electrochemical Society (2016); 163(2): p. A138-A149.

[0046] The electrodes were also imaged using SEM to visualize the formation of Li dendrites on the graphite anode surface as reported by Honbo, LL, et al., Electrochemical properties and Li deposition morphologies of surface modified graphite after grinding, Journal of Power Sources (2009); 189 (1): p. 337-343. Single-layer full cells (NCM / graphite) were then prepared in a pouch cell format. The electrochemical performance of Ni-graphite and Cu-graphite electrodes in the full cell configuration was determined via galvanostatic cycling. Go / No-Go decisions were made based on the demonstration of at least one metal-coated anode capable of delivering 25 cycles at a C / 2 charge rate with less than 20% capacity fade.

[0047] The third objective was to optimize the battery rate capability and cycle life through a systematic study of metal coating type and thickness. The scientific focus of the third objective was to determine the relationship between electrochemical performance and metal coating type and thickness. Graphite electrodes coated with Ni or Cu at three thicknesses between 2 and 20 nm were prepared for a total of six unique coating types. Electrochemical evaluations were performed using single-layer pouch full cells. Testing included AC impedance, rate capability, and galvanostatic cycling. The coating type delivering the highest capacity at a 2C charge rate was determined after electrochemical characterization, with evidence of Li-metal deposition determined via optical microscopy and SEM and correlated with capacity loss.

[0048] The fourth objective was to evaluate the ultrafast charging of cells including benchmarks with metal coated graphite electrodes and cells using uncoated graphite electrodes by determining the ultrafast charging capabilities of the optimized metal coated graphite electrodes and benchmarks versus uncoated graphite. From the results of the third objective, monolayer full cells utilizing the two metal coatings identified as having the best cycling performance were prepared and tested at a 3°C rate. Additional downselections were made based on the metal coated anodes with the highest capacity after 100 cycles. Additional monolayer full cells were prepared using the optimized electrodes as well as the uncoated graphite electrodes. The cells were galvanostatically cycled at an extremely fast charge rate (6C) at multiple temperatures. The results of the testing were used to verify that the project goal was achieved, i.e., metal coated electrodes with functional capacity at a 6C rate greater than that of the uncoated graphite anodes.

[0049] The expected outcomes are realized to achieve specific DOE technology objectives. The cell or battery of the present invention manufactured by the method of the invention is based on a graphite / NMC cell couple that utilizes nanometer-scale coatings of Ni or Cu coatings to enable long cycle life (500 cycles) at ultra-fast charge rates (6C) while maintaining state-of-the-art battery specific energy and cost. It has been found that the presence of Ni and / or Cu coatings on the graphite anode increases the Li nucleation overpotential compared to uncoated graphite anodes, thus inhibiting Li deposition and allowing charging at higher rates compared to unmodified graphite anodes. Since the cell or battery of the invention used state-of-the-art electrode materials (graphite and 622 NCM), with the only difference being the modification of the graphite electrode surface via a facile physical vapor deposition (PVD) method, the cost of the proposed cell will be similar to current technology. Furthermore, since the metal coating is primarily on the surface of the graphite anode electrode, there is no significant decrease in the cell specific energy. 8mg / cm 2For a graphite anode electrode of load, assuming surface deposition, the mass of a 5 nm Cu coating would be <1 mg Cu per g graphite. Another advantage of the proposed technique is that the physical vapor deposition step is favorable for industrial scale-up.

[0050] Feasibility Previous reports have shown that nickel (Ni) and copper (Cu) metal substrates are Yan, K., et al., Selective deposition and stable encapsulation of lithium through heterogeneous seeded growth. Nat. Energy (2016); 1(3): p. 16010,Pei, A., et al., Nanoscale Nucleation and Growth of Electrodeposited Lithium Metal Nano Letters (2017); 17 (2): p. 1132-1139; Wang, H.-C., et al., Fabrication and Characterization of Ni Thin Films Using Direct-Current Magnetron Sputtering Chinese Physics Letters (2005); 22(8): p. As reported by et al. (2013) this has been shown to exhibit a high overpotential that is unfavorable to lithium deposition (Figure 2).

[0051] Ultrathin surface coatings of Ni and Cu metals were applied to graphite electrodes via DC magnetron sputtering. Preparation of ultrathin films with controlled thicknesses below 10 nm by DC magnetron sputtering is reported in Prater, WL, et al., Microstructural comparisons of ultrathin Cu films deposited by ion beam and dc-magnetron sputtering, Journal of Applied Physics (2005); 97(9): p. 093301 and Ni Wang, H.-C., et al., Fabrication and Characterization of Ni Thin Films Using Direct-Current Magnetron Sputtering, Chinese Physics Letters (2005); 22 (8): p. 2106 metals. The sputtering equipment utilized for deposition can accommodate electrodes of suitable size for pouch cell assembly.

[0052] Surface modification of graphitic carbon anode materials with Cu and Ni metal coatings has been previously explored to modify the solderectrolite interphase (or solid-electrolyte interphase) (SEI) (F. Nobili, et al. J. Power Sources, 180, 845 (2008); M. Mancini, et al. J. Power Sources, 190, 141 (2009); M. Mancini, et al. J. Power Sources, 190, 141 (2009); P. Yu, et al. J. Electrochem. Soc., 147, 2081 (2000); F. Nobili, et al. Fuel Cells (Weinheim, Ger.), 9, 264 (2009)), providing proof of concept for intercalation of Li ions through metal films. This work, as exemplified in Figure 4 by J. Suzuki, et al. Electrochem. Solid-State Lett., 4, Al (2001), found that Li+ ions could be effectively (de)intercalated into the graphitized carbon fiber substrate through a 5-40 nm thick Cu film, facilitating the charge transfer process on the graphite oxide electrode, and a consistently lower impedance was observed over a range of voltages compared to the pure electrode. Sethuraman, VA, K. Kowolik, and V. Srinivasan, Increased cycling efficiency and rate capability of copper-coated silicon anodes in lithium-ion batteries, Journal of Power Sources (2011); 196(1): p. 393-398. See also Figure 6a-c. F. Nobili, et al. J. Power Sources, 180, 845 (2008). The improved kinetics was attributed to the catalytic effect of the metal coating for the desolvation of Li cations from the electrolyte.F. Nobili, et al. Fuel Cells (Weinheim, Ger.), 9, 264 (2009).

[0053] Further evidence for Li-ion intercalation through nm-scale Cu films is provided by reports of Cu-coated Si and Si / graphite composite electrodes as reported by Sethuraman, VA, K. Kowolik, and V. Srinivasan, Increased cycling efficiency and rate capability of copper-coated silicon anodes in lithium-ion batteries Journal of Power Sources 2011); 196(1): p. 393-398. Yen, J.-P., et al., Sputtered copper coating on silicon / graphite composite anode for lithium ion batteries Journal of Alloys and Compounds (2014); 598 (Supplement C): p. 184-190. In these reports, DC magnetron sputtering was used to deposit Cu films on the surface of the electrodes, with surface film thicknesses ranging from 10 to 100 nm. SEM and EDX analysis were used to confirm that the Cu film was uniform across the electrode. The presence of the Cu coating was found to improve cycling efficiency and deliverable energy compared to uncoated Si anodes at rates as high as 3C (Figure 7). Sethuraman, VA, K. Kowolik, and V. Srinivasan, Increased cycling efficiency and rate capability of copper-coated silicon anodes in lithium-ion batteries, Journal of Power Sources (2011); 196(1): p. 393-398.Diffusion of Li through Ni metal has been demonstrated in multilayer Ni / NiO thin film electrodes. Evmenenko, G., et al., Morphological Evolution of Multilayer Ni / NiO Thin Film Electrodes during Lithiation, ACS Applied Materials & Interfaces (2016 8(31): p.19979-19986. The results showed that Li ion transport is effective through Ni layers <~7.5 nm as reported by Evmenenko, G., et al., Lithiation of multilayer Ni / NiO electrodes: criticality of nickel layer thicknesses on conversion reaction kinetics, Phys. Chem. Chem. Phys. (2017); 19(30): p. 20029-20039.

[0054] Although the present invention has been shown and described with reference to specific embodiments thereof, it will be understood by those skilled in the art that various changes and details therefrom can be made therein without departing from the spirit and scope of the present invention and its equivalents. The following is an invention described at the beginning of the present application. <Claim 1> an anode substrate; a nanocoating formed on the surface of said anode substrate selected from the group of nanocoatings consisting of Cu, Ni, and composites of Cu and Ni; Including, 1. An anode configured for fast charging a lithium ion battery, wherein the coating increases an overpotential for Li metal nucleation on the coated surface of at least one electrode and inhibits Li metal plating during ultra-fast charging. <Claim 2> 10. The anode of claim 1, wherein ultra-fast charging occurs in less than 20 minutes. <Claim 3> 2. The anode of claim 1, wherein the coating is a nanocoating having a thickness in the range of 2 to 200 nm. <Claim 4> 4. The anode of claim 3, wherein the nanocoating has a thickness in the range of 2 to 10 nm. <Claim 5> 10. The anode of claim 1, wherein the anode substrate is selected from the group consisting of graphite, carbon black, and polyvinyl fluoride (PVDF). <Claim 6> The anode substrate is made of graphite and has a thickness of about 8 mg / cm 2 5. The anode of claim 4, wherein the coating has a thickness of about 5 nm at a loading of 1000 nm and the coating comprises a mass of metal less than 1 mg per gram of graphite. <Claim 7> 3. The anode of claim 2, wherein the ultra-fast charging occurs in about 10 minutes. <Claim 8> 2. The anode of claim 1, wherein the overpotential is determined by an interfacial energy difference between the substrate and Li metal, the interfacial energy difference being dependent on dissimilarity of crystal structures. <Claim 9> 10. The anode of claim 1, wherein the coating comprises a composite nanolayer of Cu and Ni on a surface of the anode substrate. <Claim 10> 1. A method for making an anode for fast charging of a lithium ion battery, comprising: coating a surface of an anode substrate with a Cu layer, a Ni layer, or a Cu layer and a Ni layer to form an anode having an increased overpotential for Li metal nucleation on the coated surface; whereby Li metal plating is inhibited during ultra-fast charging of a lithium ion battery formed with the anode. <Claim 11> 11. The method of claim 10, wherein the step of coating includes applying a nanolayer of Ni directly onto the anode substrate surface and applying a layer of Cu directly onto the layer of Ni to form a composite nanolayer. <Claim 12> The method of claim 10, comprising applying the coating to the anode by physical vapor deposition (PVD). <Claim 13> 13. The method of claim 12, comprising evaporating Cu, Ni, or both Cu and Ni under vacuum from a heated tungsten crucible. <Claim 14> 11. The method of claim 10, comprising applying the coating to a thickness in the range of about 2 to 200 nm. <Claim 15> The method of claim 14, wherein the coating is applied to a thickness of about 2 to 10 nm. <Claim 16> The coating is about 8 mg / cm 2 16. The method of claim 15, wherein the coating is applied at a loading of about 1000 nm to a thickness of about 5 nm and the coating comprises a mass of metal less than 1 mg per gram of graphite. <Claim 17> 11. The method of claim 10, wherein the increased overpotential is based on an interfacial energy difference between the Li metal and a substrate material from which the anode substrate is formed. <Claim 18> The method of claim 11 , comprising manufacturing the anode substrate using a slurry casting method. <Claim 19> an anode substrate; a nanocoating on the surface of said anode substrate selected from the group consisting of a Cu nanolayer, a Ni nanolayer, and a composite nanolayer of Cu and Ni; A lithium ion battery cell having: The coating increases the overpotential for Li metal nucleation on the coated surface of the anode substrate and inhibits Li metal plating during ultra-fast charging of the lithium ion battery cell. <Claim 20> 20. The lithium ion battery cell of claim 19, wherein the lithium ion battery cell is a lithium ion battery. <Claim 21> 20. The lithium ion battery cell of claim 19, wherein the coating comprises a composite nanolayer of Cu and Ni on the Cu anode substrate. <Claim 22> 1. An anode configured for fast charging a lithium ion battery, comprising: an anode substrate; A coating on the surface of an anode substrate for increasing the Li metal overpotential to inhibit Li metal plating during ultra-fast charging of the battery formed from said lithium ion battery. Including, The anode is manufactured by a process comprising the step of applying a nanocoating selected from the group consisting of a Cu nanolayer, a Ni nanolayer, and a composite nanolayer of Cu and Ni to the surface of the anode substrate. <Claim 23> 23. The anode of claim 22, wherein the applying step forms a nanocoating having a thickness of about 2-200 nm. <Claim 24> 24. The anode of claim 23, wherein the nanocoating has a thickness of 2 to 10 nm. <Claim 25> 23. The anode of claim 22, wherein the nanocoating is applied to the anode by physical vapor deposition (PVD). <Claim 26> 23. The anode of claim 22, wherein the applying step comprises evaporating Cu, Ni, or both Cu and Ni under vacuum from a heated tungsten crucible. <Claim 27> The nanocoating is about 8 mg / cm 2 25. The anode of claim 24, wherein the metal is applied at a loading of about 1000 nm to a thickness of about 5 nm and the mass of the metal including the coating is less than 1 mg per gram of graphite. <Claim 28> 25. The anode of claim 24, wherein the increased overpotential is based on an interfacial energy difference between a substrate material from which the anode substrate is formed and the Li metal. <Claim 29> 25. The anode of claim 24, comprising fabricating the anode substrate using a slurry casting process.

Claims

1. an anode substrate made of graphite; a nanocoating formed on a surface of the anode substrate, the nanocoating being selected from the group consisting of Cu, Ni, and a composite of Cu and Ni; Including, 1. An anode configured for fast charging a lithium ion battery, wherein the nanocoating increases the overpotential for Li metal nucleation at the coated surface of the anode substrate and inhibits Li metal plating during charging at charge rates of 6C or greater, the nanocoating enabling a lithium ion battery to achieve 500 cycles with a specific energy fade of less than 20%.

2. 10. The anode of claim 1, wherein the charging occurs in less than 20 minutes.

3. The anode of claim 1, wherein the nanocoating has a thickness in the range of 2 to 200 nm.

4. The anode of claim 3, wherein the nanocoating has a thickness in the range of 2 to 10 nm.

5. The anode substrate has a thickness of 8 mg / cm 2 13. The anode of claim 1, wherein the nanocoating has a thickness of 5 nm and a mass of metal comprising the nanocoating is less than 1 mg per gram of graphite.

6. 3. The anode of claim 2, wherein the charging occurs in 10 minutes.

7. 2. The anode of claim 1, wherein the overpotential is determined by an interfacial energy difference between the anode substrate and Li metal, the interfacial energy difference being dependent on dissimilarity of crystal structures.

8. The anode of claim 1 , wherein the nanocoating comprises a composite of the Cu and Ni.

9. an anode substrate made of graphite; A nanocoating on the surface of the anode substrate selected from the group consisting of a Cu nanolayer, a Ni nanolayer, and a composite nanolayer of Cu and Ni. A lithium ion battery cell having: The nano-coating increases the overpotential for Li metal nucleation on the coated surface of the anode substrate and inhibits Li metal plating during charging of the lithium ion battery cell at charge rates of 6C or higher, the nano-coating making it possible to obtain a lithium ion battery achieving 500 cycles with a specific energy fade of less than 20%.

10. 10. The lithium ion battery cell of claim 9, wherein the lithium ion battery cell is a lithium ion battery.

11. 10. The lithium ion battery cell of claim 9, wherein the coating comprises a composite nanolayer of Cu and Ni.

12. 1. An anode configured for fast charging a lithium ion battery, comprising: an anode substrate made of graphite; A nano-coating on a surface of the anode substrate for increasing the Li metal overpotential to inhibit Li metal plating during charging of the lithium ion battery at a charge rate of 6C or greater. Including, The anode is manufactured by a process comprising a step of applying a nano-coating to the surface of the anode substrate, the nano-coating being selected from the group of a Cu nano-layer, a Ni nano-layer, and a composite nano-layer of Cu and Ni, the nano-coating making it possible to obtain a lithium-ion battery achieving 500 cycles with a specific energy fade of less than 20%.

13. The anode of claim 12, wherein the nanocoating has a thickness of 2 to 200 nm.

14. The anode of claim 13, wherein the nanocoating has a thickness of 2 to 10 nm.

15. The anode of claim 12 , wherein the nanocoating is applied to the anode by physical vapor deposition (PVD).

16. The anode substrate has a thickness of 8 mg / cm 2 15. The anode of claim 14, wherein the nanocoating has a thickness of 5 nm and the mass of metal comprising the nanocoating is less than 1 mg per gram of graphite.

17. 15. The anode of claim 14, wherein the increased overpotential is due to an interfacial energy difference between the Li metal and a substrate material from which the anode substrate is formed.

Citation Information

Patent Citations

  • Negative electrode for secondary battery and secondary battery using the same

    JP2007026926A

  • Nonaqueous electrolyte secondary battery

    JP2007123246A

  • Lithium-ion rechargeable battery with high-speed charge / discharge performance

    JP2007522620A

  • Nonaqueous electrolyte secondary battery and battery pack

    JP2015065000A

  • Electrode, secondary battery, and manufacturing method for the same

    JP2015109270A