Seal ring and mounting structure for said seal ring
The seal ring design with inward tabs addresses thickness variations and sealing issues by equalizing curing shrinkage rates, enhancing flatness and performance while simplifying manufacturing.
Patent Information
- Application Number
- JP2021114706
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-09-30
- Filing Date
- 2021-07-12
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2041-07-12
AI Technical Summary
Existing seal rings with filler fibers exhibit thickness variations near the abutment due to disordered filler orientation, leading to reduced flatness and sealing performance, and require additional resin puddle removal, increasing costs.
A seal ring design with radially inward protruding tabs near the abutment, reducing mold internal pressure and aligning filler orientation to equalize curing shrinkage rates, eliminating the need for resin puddle removal.
Improves flatness and sealing performance by equalizing thickness across the seal ring, reducing manufacturing time and costs by eliminating resin puddle removal steps.
Smart Images

Figure 0007595536000001 
Figure 0007595536000002 
Figure 0007595536000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a seal ring. And the mounting structure of this seal ring For example, a seal ring for sealing lubricating oil in a gap between a shaft and a housing used in an automatic transmission (AT) of an automobile. And the mounting structure of this seal ring Regarding. [Background technology]
[0002] For example, multiple seal rings are used in an automatic transmission (AT) for an automobile. An annular seal ring 100 as shown in Figures 8 and 9 is assembled between a shaft 300 and a housing 200 that move relative to each other in a hydraulic circuit of the transmission, and serves to seal in lubricating oil while sliding.
[0003] As shown in FIG. 8, this seal ring 100 may be provided with tabs 101 protruding radially inward at a plurality of positions on the inner circumferential surface 100a side of the seal ring 100. This tab 101 is intended to prevent the center of seal ring 100 from shifting significantly from the center of the shaft by having its tip abut against the bottom surface of annular groove 301 when shaft 300 is assembled inside housing 200.
[0004] 8, the seal ring 100 is formed with abutment portion 102. This abutment portion 102 is formed by cutting a portion of the seal ring 100, and when the seal ring 100 is attached to the shaft 300, the abutment portion 102 is expanded.
[0005] The seal rings that are often used are made by injection molding into a ring shape polyamide (PA), fluororesin (polytetrafluoroethylene (tetrafluorinated) (PTFE), tetrafluoroethylene-perfluoroalkylvinylether copolymer (PFA), tetrafluoroethylene-ethylene copolymer (ETFE), etc.) and their alloys, super engineering plastics such as liquid crystal polymer (LCP), polyimide (PI), polyetherketone (PEK), polyaryletherketone (PAEK), polyetherketoneetherketoneketone (PEKEKK), polyetheretherketone (PEEK), polyphenylene sulfide (PPS), and polybenzimidazole (PBI) mixed with reinforcing materials such as carbon fiber (called filler fiber).
[0006] Furthermore, with regard to injection molding of a seal ring, Patent Document 1 proposes arranging a gate 153 at a position offset from the opposing portion 152 on the seal ring 150 at the joint portion 151, as shown in FIG. 10, and providing a resin reservoir 154 on the side where the distance between the gate 153 and the joint portion 151 is shorter (the side of the flow length T1).
[0007] By adopting this configuration, in the manufacturing method of seal ring 150 shown in Patent Document 1, the amount of resin filled on the side where the distance between gate 153 and joint 151 is longer (flow length T2 side) and the side where the distance between gate 153 and joint 151 is shorter (flow length T1 side) can be made the same, so that resin can be filled without excess or deficiency and the occurrence of defects such as burrs can be prevented. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2004-205003 A Summary of the Invention [Problem to be solved by the invention]
[0009] However, even when a gate is located at the opposing end of the joint, when a seal ring is actually formed by injection molding a resin containing filler fibers, there was a problem that the thickness near the joint was thicker than other parts of the seal ring body. This phenomenon will be specifically explained with reference to Figures 11 and 12. Figure 11(a) is a cross-sectional view perpendicular to the axis of the seal ring body at a location other than the vicinity of the abutment of the seal ring body. Figure 11(b) is a partially enlarged view of Figure 11(a). Figure 12(a) is a cross-sectional view perpendicular to the axis of the seal ring body near the abutment of the seal ring body. Figure 12(b) is a partially enlarged view of Figure 12(a).
[0010] As shown in Figure 11(b), the filler fibers F in areas other than near the joint of the seal ring body are visually observed to be elongated and thin, and it can be seen that the axes of the filler fibers F are oriented perpendicular to the axis of the seal ring body (the axes of the filler fibers F are oriented parallel to the direction of the flow of the molten resin). In contrast, in FIG. 12(b), the state in which the axes of the filler fibers F are oriented perpendicular to the axis of the seal ring body as in FIG. 11(b) cannot be visually recognized. That is, it is found that the axis of the filler fibers in the vicinity of the joint of the seal ring body is oriented perpendicular to the direction of the flow of the molten resin.
[0011] The above phenomenon is caused by the collision of the resin with the end of the mold, which corresponds to the end of the joint of the seal ring body in the mold, causing a disturbance in the orientation of the filler fibers. In the vicinity of the joint of the seal ring, the filler fibers are oriented perpendicular to the direction of the flow of the molten resin, so the cure shrinkage rate of that part is smaller than the cure shrinkage rate of other parts (parts other than the vicinity of the joint). As a result, the thickness of the part near the joint becomes thicker than the other parts.
[0012] In this way, the thickness of the seal ring body near the abutment is greater than other portions of the seal ring body, which further deteriorates the flatness of the seal ring body and causes the problem of reduced sealing performance of the seal ring. Furthermore, when a gate is placed in a part of the mold corresponding to the opposing part of the joint of the seal ring body, and a resin containing filler fibers is injection molded from this gate to form a seal ring, if a resin pool as described above is formed, the resin pool must be removed with precision after injection molding, which requires more labor and materials and results in higher costs.
[0013] The present invention has been made to solve the above technical problems, and provides a seal ring made of a resin containing filler fibers, which does not require the formation of a resin pool that is to be removed after injection molding as in the conventional seal ring, and has good flatness and sealing properties. And the mounting structure of this seal ring The purpose is to provide. [Means for solving the problem]
[0014] In order to solve the above problems, the seal ring according to the present invention is a seal ring for sealing an annular gap between a housing and a shaft assembled therein, and is formed by injection molding. of A seal ring made of a resin containing filler fibers and free of resin pools is provided, the seal ring having an annular seal ring body having a joint and a plurality of tabs formed on an inner peripheral surface of the seal ring body so as to protrude radially inward, the tabs being formed at least in the vicinity of the joint. The length from the end of the joint, which is the position where the cross-sectional shape of the joint changes, to the end of the tab closest to the end of the joint is 0.5 mm or more and 2.5 mm or less. It is characterized by:
[0015] As described above, the seal ring of the present invention has a plurality of tabs formed on the inner surface of the seal ring body so as to protrude radially inward, and the tabs are formed at least near the joint. Therefore, when the seal ring is injection molded, molten resin flows into the tab forming portion of the mold, and the internal mold pressure in the area of the mold corresponding to the vicinity of the joint of the seal ring body is reduced. As described above, the cure shrinkage rate tends to be smaller in the vicinity of the joint where the filler orientation is disturbed than in other areas. In addition, the mold pressure is reduced near the joint, which tends to increase the cure shrinkage. Therefore, in the vicinity of the joint, the decrease in cure shrinkage due to the disturbance of the filler orientation and the increase in cure shrinkage due to the reduction in mold pressure are offset. As a result, the cure shrinkage rate near the joint and other parts of the seal ring body becomes approximately the same, and the thickness near the joint and other parts of the seal ring body become approximately uniform, improving the flatness and sealing performance of the seal ring. Furthermore, since no resin pool is formed as in the conventional method, there is no need to remove the resin pool after injection molding of the seal ring, which allows for a reduction in the number of steps and materials required.
[0016] In addition, the length from the end of the joint to the end of the tab closest to the end of the joint is 0.5 mm or more and 2.5 mm or less. This is one of the characteristics. When the length from the end of the joint to the end of the tab closest to the end of the joint exceeds 2.5 mm, the length becomes too large, so that the effect of reducing the internal mold pressure caused by the molten resin flowing into the tab formation portion of the mold is small. On the other hand, even if the length from the end of the joint to the end of the tab closest to the end of the joint is less than 0.5 mm, the effect of reducing the internal mold pressure can be obtained by the molten resin flowing into the tab forming portion of the mold. However, if the length is less than 0.5 mm, the shape of the joint becomes complex, making it difficult to manufacture the mold, which is not preferable.
[0017] The length dimension of the filler fibers is desirably 1000 μm or less. If the length of the filler fibers exceeds 1000 μm, the shrink anisotropy during injection molding becomes strong, which is undesirable.The average length of the filler fibers is preferably about 200 μm.
[0018] Furthermore, it is desirable that the cross-sectional area parallel to the axis of the tab and the seal ring body at the position of the tab formed near the joint portion is larger than the cross-sectional area parallel to the axis of the seal ring body at both the left and right sides of the tab. In this way, since the cross-sectional area parallel to the axis of the tab and the seal ring body is larger than the cross-sectional area parallel to the axis of the seal ring body at both the left and right sides of the tab, the internal mold pressure in the region of the mold corresponding to the vicinity of the joint can be reduced.
[0019] It is also desirable that the joint portion is formed by opposing one end and the other end of the seal ring body, and that the one end and the other end have engaging protrusions or engaging recesses that can engage with each other and have a cross-sectional area parallel to the axis that is smaller than the cross-sectional area parallel to the axis of the seal ring body.
[0020] In this way, even if an engaging protrusion or engaging recess is formed at one end and the other end of the joint, whose cross-sectional area parallel to the axis is smaller than the cross-sectional area parallel to the axis of the seal ring body, during injection molding of the seal ring, molten resin flows into the tab forming portion of the mold, and the internal mold pressure in the area of the mold corresponding to the vicinity of the joint of the seal ring body is reduced. Therefore, as described above, the cure shrinkage rate tends to be smaller near the joint where the filler orientation is disturbed compared to other areas, but the internal mold pressure is reduced near the joint, and this reduction in internal mold pressure tends to increase the cure shrinkage rate. As a result, near the joint, the decrease in the cure shrinkage rate due to disturbance in the filler orientation and the increase in the cure shrinkage rate due to reduced internal mold pressure are offset, making the thickness near the joint and the thickness of other parts of the seal ring body approximately uniform, improving the flatness and sealing properties of the seal ring.
[0021] It is also preferable that the inclination angle of the side surface of the tab relative to the circumferential direction of the seal ring body is set within a range of 100° to 150°. If the inclination angle of the side surface of the tab is less than 100°, the orientation of the filler fibers in the tab tends to become disordered, which is not preferable. Also, if the inclination angle of the side surface of the tab exceeds 150°, the circumferential length of the tab becomes long, and the cure shrinkage rate increases in areas other than the vicinity of the joint, which leads to deterioration of flatness, which is not preferable.
[0022] It is also preferable that the radial thickness of the tab is smaller than the radial thickness of the seal ring body. If the radial thickness of the seal ring body is smaller than the radial thickness of the tab, the mechanical strength of the seal ring body will be reduced, which is undesirable.
[0023] Also, The seal ring mounting structure according to the present invention is the above-mentioned seal ring mounting structure for sealing an annular gap between a housing and a shaft assembled therein, The seal ring body is fitted into an annular groove formed in a shaft inserted into the housing. Installed , the above Seal ring When installing, A feature of this invention is that in the event of misalignment between the seal ring body and the shaft, the tip of a tab formed on the inner surface of the seal ring body so as to protrude radially inward comes into contact with the bottom surface of the annular groove. Effect of the Invention
[0024] According to the present invention, in a seal ring made of a resin containing filler fibers, it is not necessary to form a resin pool that is removed after injection molding as in the conventional seal ring, and the seal ring has good flatness and sealing properties. And the mounting structure of this seal ring can be obtained. [Brief description of the drawings]
[0025] [Figure 1] FIG. 1 is a perspective view of a seal ring according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a perspective view of the seal ring of FIG. 1 as seen from a different direction. [Diagram 3] FIG. 3(a) is a plan view of the seal ring of FIGS. 1 and 2, and FIG. 3(b) is a side view of the seal ring as viewed from the outside. [Figure 4] FIG. 4 is a cross-sectional view parallel to the axis of a seal ring body in a state in which the seal ring according to one embodiment of the present invention is mounted in an annular groove of a shaft. [Diagram 5] FIG. 5(a) is an enlarged perspective view of the joint and the tabs in the vicinity thereof, and FIG. 5(b) is a cross-sectional view taken along line II of FIG. 5(a). [Figure 6] FIG. 6(a) is an enlarged plan view of the abutment and the tabs in the vicinity thereof, and FIG. 6(b) is a side view of the abutment as viewed from the outside of the seal ring. [Figure 7] 7A and 7B show another embodiment of the abutment, and FIG. 7(a) is an enlarged plan view of the abutment and the tabs in the vicinity thereof, and FIG. 7(b) is a side view of the abutment as viewed from the outside of the seal ring. [Figure 8] FIG. 8 is a perspective view of a conventional seal ring. [Figure 9] FIG. 9 is a cross-sectional view parallel to the axis of a seal ring body in a state in which a shaft on which a conventional seal ring is mounted is assembled into a housing. [Figure 10] FIG. 10 is a plan view of a conventional seal ring. [Figure 11] FIG. 11 shows a conventional seal ring, where (a) is a cross-sectional view perpendicular to the axis of the seal ring body at a location other than the vicinity of the abutment of the seal ring body, and (b) is an enlarged view of a portion of (a). [Figure 12] FIG. 12 shows a conventional seal ring, where (a) is a cross-sectional view perpendicular to the axis of the seal ring body in the vicinity of the abutment of the seal ring body, and (b) is an enlarged view of a portion of (a). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] The seal ring according to the present invention will be described below. And the mounting structure of this seal ring The seal ring according to the present embodiment is mounted between a shaft and a housing that move relative to each other in a hydraulic circuit of an automatic transmission of an automobile, for example, and serves to seal in lubricating oil while sliding. Fig. 1 is a perspective view of a seal ring according to an embodiment of the present invention, and Fig. 2 is a perspective view of the seal ring of Fig. 1 seen from another direction. Fig. 3(a) is a plan view of the seal ring of Fig. 1 and Fig. 2, and Fig. 3(b) is a side view of the seal ring seen from the outside. Fig. 4 is a cross-sectional view parallel to the axis of a seal ring body in a state in which the seal ring according to an embodiment of the present invention is mounted in an annular groove of a shaft. The axis of the seal ring body is the annular axis of the seal ring according to the embodiment of the present invention. The seal ring passes through the center C (center of the ring) of the annular seal ring when it is installed in the groove. A line extending perpendicular to a plane including the first sealing surface.
[0027] The illustrated seal ring 1 includes an annular seal ring body 1A formed of a material such as polyamide (PA), fluororesin (polytetrafluoroethylene (tetrafluoride) (PTFE), tetrafluoroethylene-perfluoroalkylvinylether copolymer (PFA), tetrafluoroethylene-ethylene copolymer (ETFE), etc.) and alloys thereof, super engineering plastics such as liquid crystal polymer (LCP), polyimide (PI), polyetherketone (PEK), polyaryletherketone (PAEK), polyetherketoneetherketoneketone (PEKEKK), polyetheretherketone (PEEK), polyphenylene sulfide (PPS), polybenzimidazole (PBI), etc., mixed with filler fibers such as carbon fibers as a reinforcing material, and a plurality of tabs 10 formed on the inner peripheral surface of the seal ring body 1A. The cross section of the seal ring body 1A parallel to the axis of the seal ring body at the portion where the tabs 10 are not formed is rectangular. The seal ring 1 is a resin seal ring in which no resin pool is formed as shown in Patent Document 1. As described above, the resin in the seal ring 1 contains filler fibers, and therefore the seal ring 1 has high wear resistance.
[0028] More specifically, as shown in Fig. 4, the oil seal side (seal surface side) of the seal ring body 1A is provided with a first seal surface 2. This first seal surface 2 comes into sliding contact with a side wall surface (the side surface of the annular groove on the oil seal side) 21a of annular groove 21 of shaft 20, and seals the side wall surface 21a. Moreover, the outer peripheral surface of the seal ring body 1A is a second seal surface 5. This second seal surface 5 comes into contact with an inner peripheral surface 31 of a housing 30 to provide a seal.
[0029] As described above, a plurality of tabs 10 (six in the figure) are provided at predetermined intervals on the inner peripheral surface 7 of the seal ring 1 shown in FIGS. Each tab 10 protrudes radially inward from the inner surface 7 as shown in Figure 3, and when the seal ring 1 is attached to the annular groove 21 of the shaft 20 as shown in Figure 4, if misalignment occurs between the seal ring body 1A and the shaft 20, the tip portion 10a of the tab 10 will abut against the groove bottom surface 21b of the annular groove 21. Thus, one of the functions of the tab 10 is to prevent the center C of the seal ring main body 1A from being significantly displaced from the center of the shaft 20 when the shaft 20 is assembled inside the housing 30.
[0030] As shown in Figures 1 to 3, a joint portion 15 (separation portion) is formed at one circumferential location of the seal ring 1, and when attaching the seal ring 1 to the shaft 20, the seal ring 1 can be easily attached to the annular groove 21 of the shaft 20 by expanding the seal ring 1 in the direction of separating this joint portion 15. The tabs 10 are provided near both ends of the seal ring body 1A that are separated by at least the joint portion 15.
[0031] Specifically, the tab 10 is provided at least near an end of the abutment 15 of the seal ring body 1A (a portion where the cross-sectional area changes at the abutment 15). As a result, when the seal ring 1 is injection molded, molten resin containing the filler fibers flows into the tab forming portion of the mold, reducing the internal mold pressure in the region of the mold corresponding to the vicinity of the joint of the seal ring body 1A. As described above, the cure shrinkage rate tends to be smaller in the vicinity of the joint where the filler orientation is disturbed, compared to other areas. The mold internal pressure is reduced in the vicinity of the joint, and this reduction in mold internal pressure tends to increase the cure shrinkage rate. Therefore, in the vicinity of the joint, the decrease in the cure shrinkage rate due to the disturbance in the filler orientation and the increase in the cure shrinkage rate due to the reduction in the internal mold pressure are offset. As a result, the cure shrinkage rate near the joint and other parts of the seal ring body becomes approximately the same, and the thickness near the joint and other parts of the seal ring body become approximately uniform, improving the flatness and sealing performance of the seal ring.
[0032] It is desirable that the length of the filler fibers contained in the resin forming the seal ring 1 is 1000 μm or less. If the length of the filler fibers exceeds 1000 μm, the shrinkage anisotropy during injection molding becomes strong, which is not preferable. The average length of the filler fibers is preferably about 200 μm. The length of the filler fiber is not limited to the above, and the shape and dimensions may be any shape that can exhibit the effect of wear resistance. Although carbon fiber is exemplified as the filler fiber, the present invention is not limited to carbon fiber, and glass fiber and CNF (cellulose nanofiber) may be used, for example.
[0033] Next, the structure of the joint portion 15 and the tab 10 will be described in detail. Fig. 5(a) is an enlarged perspective view of the abutment 15 and the tab 10 in the vicinity thereof, and Fig. 5(b) is a cross-sectional view taken along line II of Fig. 5(a). Fig. 6(a) is an enlarged plan view of the abutment 15 and the tab 10 in the vicinity thereof, and Fig. 6(b) is a side view of the abutment 15 as viewed from the outside of the seal ring body 1A.
[0034] The joint portion 15, i.e., the portion where one end and the other end of the seal ring main body 1A face each other, has a mutually engageable engaging protrusion or engaging recess whose cross-sectional area parallel to the axis is smaller than the cross-sectional area parallel to the axis of the seal ring main body 1A. Specifically, one end side of the seal ring body 1A is formed with an inner peripheral side wall 15a extending in a circumferential direction in a wall-like shape on the inner peripheral surface of the seal ring body 1A. Further, a lower step portion 15b is formed on the radially outer side of the inner peripheral side wall 15a, extending in the circumferential direction in a stepped shape. By forming the lower step portion 15b, an upper step recess portion 15c is formed thereon.
[0035] On the other hand, at the other end side of the seal ring body 1A, an inner peripheral recess 15d is formed on the inner peripheral surface of the seal ring body 1A, with which the inner peripheral side wall 15a is engageable. Further, an upper step portion 15e is formed so as to be engageable with the lower step portion 15b and extends radially outward from the inner peripheral recess portion 15d and engages with the upper step recess portion 15c. By forming the upper step portion 15e, a lower step recess 15f is formed below, and the lower step portion 15b is adapted to engage therewith. In this manner, at the joint 15, both ends of the seal ring main body 1A are formed in a stepped shape and have a structure in which they engage with each other. When the joint 15 is closed, the first seal surface 2 and the non-seal surface 6, which are the seal surfaces, are not in communication with each other, and the second seal surface 5 and the non-seal surface 7 are not in communication with each other, thereby improving the sealing performance.
[0036] 6(a), as described above, the tab 10 is provided at least near the end of the abutment 15 of the seal ring body 1A (the portion where the cross-sectional area changes at the abutment 15). Preferably, the length dimension L1 from the end of the abutment 15 to the end of the tab 10 closest to the end of the abutment 15 is formed to be 0.5 mm or more and 2.5 mm or less. The length dimension L1 from the end of this joint 15 to the tab 10 closest to it is the length dimension from the position where both ends of the seal ring main body 1A are formed in a stepped shape, i.e., the position where the cross-sectional shape changes at the joint 15 of the seal ring main body 1A (the joint end) to the tab 10 closest to it.
[0037] Furthermore, when the length from the end of the joint to the end of the tab closest to the end of the joint exceeds 2.5 mm, the length becomes too large, and the effect of reducing the internal mold pressure caused by the molten resin flowing into the tab formation portion of the mold is small. On the other hand, even if the length from the end of the joint to the end of the tab closest to the end of the joint is less than 0.5 mm, the effect of reducing the internal mold pressure can be obtained by the molten resin flowing into the tab forming portion of the mold. However, if the length is less than 0.5 mm, the shape of the joint becomes complex, making it difficult to manufacture the mold, which is not preferable.
[0038] The inclination angle of the side surface of the tab relative to the circumferential direction of the seal ring body is set within a range of 100° to 150°. If the inclination angle of the side surface of the tab is less than 100°, the orientation of the filler fibers in the tab tends to become disordered, which is not preferable. Also, if the inclination angle of the side surface of the tab exceeds 150°, the circumferential length of the tab becomes long, and the cure shrinkage rate increases in areas other than the vicinity of the joint, which leads to deterioration of flatness, which is not preferable.
[0039] Furthermore, as shown in FIG. 6(a), a radial thickness dimension L2 of the tab 10 is formed to be smaller than a radial thickness dimension L3 of the seal ring body 1A. If the radial thickness dimension L3 of the seal ring body is formed smaller than the radial thickness dimension L2 of the tab, the radial thickness dimension of the seal surface 2 of the seal ring body 1A will be small, which is undesirable as it will result in a decrease in sealing performance. Therefore, from the viewpoint of the sealing performance of the seal ring body 1A, it is preferable that the radial thickness dimension L3 of the seal ring body 1A is formed to be larger than the radial thickness dimension L2 of the tab 10.
[0040] In addition, as shown in Figure 5(b), the cross-sectional area S1 parallel to the axis of the tab 10 and the seal ring body 1A is larger than the cross-sectional area S2 parallel to the axis of the seal ring body 10 at both the left and right sides of the tab 10 (positions where the tab is not formed). As a result, during injection molding of the seal ring 1, the molten resin containing the filler fibers flows into the tab forming portion of the mold, and the internal pressure of the mold is reduced in the region of the mold corresponding to the vicinity of the joint.
[0041] The seal ring 1 thus configured is obtained by injecting molten resin containing filler fibers into a mold (not shown). In the mold, a gate through which the resin flows is formed in a portion of the mold corresponding to the portion facing the abutment 15 of the seal ring 1. In the molded seal ring 1, as shown in FIG. 2, a gate mark 17 is formed on the inner circumferential surface 7 at the portion facing the abutment 15 on the seal ring 1.
[0042] The molten resin injected from an injection nozzle (not shown) flows into the mold through the gate of the mold, splits into left and right sides, and flows toward the portion where the joint 15 is formed due to a predetermined internal mold pressure.
[0043] Moreover, the molten resin flowing from the gate to both the left and right sides also flows into the tab forming portion of the mold corresponding to the tab 10, as described above. Furthermore, since a tab forming portion is provided in the vicinity of the joint forming portion of the mold corresponding to joint 15, the internal mold pressure of the molten resin passing through the tab forming portion, i.e., the molten resin in the vicinity of the joint forming portion, is reduced by the tab forming portion.
[0044] As described above, the cure shrinkage rate tends to be smaller in the vicinity of the joint where the filler orientation is disturbed than in other areas. Furthermore, the tab forming portion reduces the internal mold pressure of the molten resin in the vicinity of the joint forming portion, and this reduction in internal mold pressure tends to increase the cure shrinkage rate. Therefore, in the vicinity of the joint, the decrease in the cure shrinkage rate due to the disturbance in the filler orientation and the increase in the cure shrinkage rate due to the reduction in the internal mold pressure are offset. As a result, the thickness in the vicinity of the joint and the thickness of the other portions of the seal ring body become substantially uniform, thereby improving the flatness and sealing performance of the seal ring. Furthermore, since no resin pool is formed as in the conventional method, there is no need to remove the resin pool after injection molding of the seal ring, which allows for a reduction in the number of steps and materials required.
[0045] In addition, by positioning the gate at the opposing part of the joint, the amount of resin flowing to both the left and right sides of the seal ring body 1A is made the same, reducing the internal mold pressure of the molten resin and preventing the occurrence of burrs, etc.
[0046] In addition, in the above embodiment, as shown in FIG. 6, both ends of the seal ring main body 1A are formed in a stepped shape at the joint portion 15 so as to engage with each other, but the present invention is not limited to this configuration. For example, the joint portion 15 may be configured as shown in the plan view of Fig. 7(a) and the side view of Fig. 7(b). That is, on the inner peripheral surface of the seal ring, an inner peripheral side wall 15g is formed on one end side of the seal ring body 1A, extending in the circumferential direction like a wall. Also, an engagement protrusion 15h is formed on the radially outer side of the inner peripheral side wall 15g, extending in the circumferential direction like a step. By forming the engagement protrusion 15h, an upper step recess 15i (engagement recess) and a lower step recess 15j (engagement recess) are formed above and below the engagement protrusion 15h, respectively.
[0047] On the other hand, at the other end side of the seal ring body 1A, an inner peripheral recess 15k is formed on the inner peripheral surface of the seal ring, with which the inner peripheral side wall 15g is engageable. Further, on the radially outer side of the inner peripheral recess 15k, an upper step protrusion 15m (engagement protrusion) and a lower step protrusion 15n (engagement protrusion) are provided which can engage with the upper and lower parts of the engagement protrusion 15h and which engage with the upper step recess 15i and the lower step recess 15j, respectively. By forming the upper protrusion 15m and the lower protrusion 15n, an intermediate recess 15p (engagement recess) is formed therebetween, and the engagement protrusion 15h engages therewith.
[0048] In this manner, both ends of the seal ring body 1A may be formed in opposing concave and convex shapes at the joint 15, so as to be engaged with each other. Even in this case, when the joint portion 15 is closed, the first sealing surface 2, which is the sealing surface, and the non-sealing surface 6 are not in communication with each other, and the second sealing surface 5 and the non-sealing surface 7 are not in communication with each other, thereby improving the sealing performance.
[0049] In the above embodiment, as shown in FIG. 3, six tabs 10 are provided on the seal ring 1. However, the present invention is not particularly limited to the number of tabs 10 being six. In addition, in the above embodiment, a case where the sealing ring is injection molded using a resin containing filler fibers is described, but the present invention is not limited to this, and can also be applied to a case where the sealing ring is injection molded using a resin that does not contain filler fibers.
[0050] Example 1 The following seal rings were manufactured by injection molding. This seal ring has a step-shaped joint as shown in FIG. 6, is made of polyether ether ketone (PEEK), has an outer diameter of φ50 mm, and an inner diameter of φ46 mm. The length dimension of the filler fibers contained in the resin forming this seal ring is 1000 μm or less, with an average length dimension of 200 μm, the number of tabs 10 is 6, the length dimension L1 from the end of the joint to the end of the tab closest to the end of the joint is 1 mm, the radial thickness dimension L2 of the tab is 0.5 mm, the radial thickness dimension L3 of the seal ring body is 2 mm, and the inclination angle θ of the side of the tab is 120 degrees. Then, using a micrometer, the maximum and minimum values of the axial thickness of the seal ring body at 10 points in each seal ring were measured, and the difference between the maximum and minimum values was calculated as the flatness. As a result, the flatness was 0.014 (mm).
[0051] Example 2 A seal ring was produced by injection molding under the same conditions as in Example 1 above, except that the length dimension L1 from the end of the abutment to the end of the tab closest to the end of the abutment was set to 0.5 mm. Then, using a micrometer, the maximum and minimum values of the axial thickness of the seal ring body at 10 points in each seal ring were measured, and the difference between the maximum and minimum values was calculated as the flatness. As a result, the flatness was 0.01 (mm).
[0052] Example 3 A seal ring was produced by injection molding under the same conditions as in Example 1 above, except that the length dimension L1 from the end of the abutment to the end of the tab closest to the end of the abutment was set to 1.5 mm. Then, using a micrometer, the maximum and minimum values of the axial thickness of the seal ring body at 10 points in each seal ring were measured, and the difference between the maximum and minimum values was calculated as the flatness. As a result, the flatness was 0.017 (mm).
[0053] Example 4 A seal ring was produced by injection molding under the same conditions as in Example 1 above, except that the length dimension L1 from the end of the abutment to the end of the tab closest to the end of the abutment was set to 2.5 mm. Then, using a micrometer, the maximum and minimum values of the axial thickness of the seal ring body at 10 points in each seal ring were measured, and the difference between the maximum and minimum values was calculated as the flatness. As a result, the flatness was 0.019 (mm).
[0054] Example 5 In Example 5, an attempt was made to manufacture a seal ring under the same conditions as in Example 1 described above, except that the length dimension L1 from the end of the joint to the end of the tab closest to the joint end was set to 0.3 mm. However, the length dimension from the end of the joint of the mold to the end of the tab closest to the joint end was short, and the shape of the joint of the mold became complicated, so production of the mold was abandoned.
[0055] Comparative Example 1 As Comparative Example 1, a seal ring similar to that of Example 1 was produced, except that the tab in Example 1 was not formed. Then, as in Example 1, the maximum and minimum values of the axial thickness at 10 points on the seal ring body in one seal ring were measured, and the difference between them was calculated as the flatness. As a result, the flatness was 0.024 (mm).
[0056] Comparative Example 2 A seal ring was produced by injection molding under the same conditions as in Example 1 above, except that the length dimension L1 from the end of the abutment to the end of the tab closest to the end of the abutment was set to 3 mm. Then, using a micrometer, the maximum and minimum values of the axial thickness of the seal ring body at 10 points in each seal ring were measured, and the difference between the maximum and minimum values was calculated as the flatness. As a result, the flatness was 0.024 (mm).
[0057] As described above, flatness was not measured in Example 5. However, even when the length from the end of the joint to the end of the tab closest to the end of the joint is short, as in Example 5, it can be inferred that the effect of reducing the internal mold pressure can be obtained by the molten resin flowing into the tab formation portion of the mold. However, if the length dimension from the end of the joint to the end of the tab closest to the end of the joint becomes too short, as in Example 5, the shape of the joint becomes complex and it becomes difficult to manufacture the mold, which is not preferable from the standpoint of mold manufacturing. Furthermore, compared with the seal rings of Examples 1 to 4 in which a tab is formed at least near the joint, and the seal rings of Comparative Examples 1 and 2, the seal rings of Examples 1 to 4 have superior flatness. Since the seal rings have superior flatness, it can be said that the seal performance is also superior. Therefore, it was confirmed that by forming the tab at least in the vicinity of the joint, the flatness and sealing performance were improved. [Explanation of symbols]
[0058] 1 Seal ring 1A Seal ring body 2 First Seal Surface 5 Second seal surface 6 Non-sealing surface 7 Inner surface 10 Tabs 15 Joint area 20 Axis 21 Annular groove 21a Side (oil seal side) 22 Gap 30 Housing 31 Housing inner surface
Claims
1. A seal ring for sealing an annular gap between a housing and a shaft assembled therein, the seal ring being made of a resin containing filler fibers and free of resin pools during injection molding, a ring-shaped seal ring body having a joint portion; a plurality of tabs formed on an inner circumferential surface of the seal ring body so as to protrude radially inward; The tab is formed at least near the joint, A seal ring characterized in that a length dimension from an end of the joint, which is a position where the cross-sectional shape of the joint changes, to the end of the tab closest to the end of the joint is 0.5 mm or more and 2.5 mm or less.
2. 2. The seal ring according to claim 1, wherein the length of the filler fibers is 1000 μm or less.
3. 3. A seal ring as described in claim 1 or claim 2, characterized in that a cross-sectional area parallel to the combined axis of the tab and the seal ring body at the position of a tab formed in the vicinity of the joint portion is larger than a cross-sectional area parallel to the axis of the seal ring body at both left and right sides of the tab.
4. The joint portion is formed such that one end and the other end of the seal ring body face each other, A seal ring as described in any one of claims 1 to 3, characterized in that the one end and the other end are formed with engaging convex portions or engaging concave portions that can engage with each other and whose cross-sectional area parallel to the axis is smaller than the cross-sectional area parallel to the axis of the seal ring body other than the joint portion.
5. 5. The seal ring according to claim 1, wherein an inclination angle of the side surface of the tab relative to the inner circumferential surface of the seal ring body is set within a range of 100° to 150°.
6. 6. The seal ring according to claim 1, wherein a radial thickness of the tab is smaller than a radial thickness of the seal ring body.
7. A mounting structure for a seal ring that seals an annular gap between a housing and a shaft assembled therein, comprising: The seal ring body is fitted into an annular groove formed in a shaft inserted into the housing. Installed, A seal ring mounting structure characterized in that if misalignment occurs between the seal ring body and the shaft when the seal ring is mounted, the tip of a tab formed on the inner surface of the seal ring body so as to protrude radially inward will abut against the bottom surface of the annular groove.
Citation Information
Patent Citations
Upper piston ring for large-scale two-stroke turbocharging uniflow type scavenging internal combustion engine with crosshead
CN105221291A
Seal ring for rotor
JP1998318375A
Resin seal ring and its manufacturing method
JP2004205003A
Seal ring
JP2015218790A
Seal ring
JP2015218791A