Positive electrode slurry, positive electrode plate and battery including said positive electrode plate
By using polyether siloxane in the positive electrode slurry, the stability and flexibility of lithium-ion battery plates are improved, enabling higher coating weights and increased energy density with reduced manufacturing risks.
Patent Information
- Application Number
- JP2023516224
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-11-23
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2041-11-23
AI Technical Summary
Increasing the coating weight of positive electrode plates in lithium-ion batteries to enhance energy density leads to manufacturing yield reduction and safety risks.
Incorporating a polyether siloxane additive into the positive electrode slurry, which improves the stability, flexibility, and dispersibility of the electrode plate, allowing for increased coating weight without compromising manufacturing integrity.
The addition of polyether siloxane enhances the energy density of lithium-ion batteries while reducing material costs and minimizing manufacturing defects such as tearing and cracking.
Smart Images

Figure 0007595752000015 
Figure 0007595752000016 
Figure 0007595752000017
Abstract
Description
[Technical field]
[0001] The present application relates to the field of lithium batteries, in particular to a positive plate comprising polyethersiloxane, and further to a secondary battery comprising the positive plate, and a battery pack, a battery module and a power consuming device comprising the secondary battery. [Background technology]
[0002] In recent years, with the ever-widening application range of lithium-ion batteries, lithium-ion batteries are widely used in energy storage power systems such as hydroelectric, thermal, wind and solar power stations, as well as in multiple fields such as electric tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace, etc. As lithium-ion batteries have made great strides in development, there are also higher requirements for improving their energy density and reducing their costs.
[0003] At present, one of the effective ways to improve the energy density of lithium-ion batteries is to increase the coating weight of the positive plate, but the common way of increasing the coating weight of the positive plate reduces the yield of plate production and potential safety risks, which leads to difficulties in manufacturing lithium-ion batteries.
[0004] Therefore, the positive plate still needs to be improved. Summary of the Invention
[0005] The present application has been made in view of the above-mentioned problems, and an object of the present application is to provide a positive electrode slurry containing a specific polyether siloxane and a positive electrode plate manufactured using the positive electrode slurry.
[0006] As such, a first aspect of the present invention provides a cathode slurry comprising an active cathode material and a polyether siloxane, the polyether siloxane comprising at least [ka] The structural unit includes Where: D is a methyl group or an ethyl group; A is hydrogen, a halogen or a halogenated alkyl group, said halogen being optionally fluorine, chlorine or bromine, said A is optionally hydrogen or a fluoromethyl group; B is hydroxyl, R, OR, or ROR', where R, R' are each independently a straight or branched chain alkyl group containing 1 to 8 carbons; and optionally B is a methyl group, an ethyl group, or an ethoxymethyl group; E is a phenyl group, an alkyl-substituted phenyl group, an etherified phenyl group, or a halogenated phenyl group, and said E is optionally a phenyl group or a fluorophenyl group.
[0007] By adding a flexibility additive, i.e., the polyether siloxane described in the present application, to the positive electrode slurry, the stability of the positive electrode slurry can be improved, the flexibility of the positive electrode plate can be improved, and the coating weight of the positive electrode plate can be increased by ensuring the dispersibility of each material in the positive electrode plate.
[0008] In any embodiment of the present application, after adding the polyether siloxane to the cathode slurry, the resulting lithium ion battery has improved energy density.
[0009] In any embodiment, the number average molecular weight of the polyether siloxane is in the range of 10,000 to 60,000, and the selectable range is 20,000 to 60,000.
[0010] The molecular weight affects the processing performance of the positive electrode plate, so the number average molecular weight of the polyether siloxane must be controlled within the above range.
[0011] In any embodiment, in the polyether siloxane described in the present application, the molar ratio of the structural unit (I) is 0 to 75 mol %, the molar ratio of the structural unit (II) is 0 to 70 mol %, the molar ratio of the structural unit (III) is 5 to 65 mol %, and the molar ratio of the structural unit (IV) is 4 to 10 mol %, based on the total molar amount of the structural units (I) to (IV), and the molar ratios of the structural units (I) and (II) are not simultaneously zero.
[0012] The molar ratios of the structural units (I) to (IV) ensure that sufficient hydrogen bonds and an appropriate amount of covalent bonds are formed between the obtained polyether siloxane and the positive electrode active material, current collector, etc., and further ensure stability in the manufacturing process of the positive electrode plate, flexibility of the positive electrode plate, and dispersibility of various positive electrode materials, thereby improving the energy density of the battery.
[0013] In any embodiment, the weight ratio of the polyether siloxane to the positive electrode active material is 0.0005 to 0.030, a selectable range is 0.001 to 0.02, a further selectable range is 0.001 to 0.01, and a most selectable range is 0.001 to 0.006.
[0014] If the ratio value is too small, the positive plate will crack at high coating weight, and if the ratio value is too large, it will adversely affect the performance of the battery.
[0015] In any embodiment, the active cathode material is selected from at least one of lithium iron phosphate, lithium manganese iron phosphate, lithium manganate, lithium cobalt oxide, lithium nickel cobalt manganate, lithium nickel cobalt aluminate, lithium nickel oxide, or mixtures thereof.
[0016] The inventors of the present application have discovered that when the positive electrode active material is at least one of lithium iron phosphate, lithium manganese iron phosphate, lithium manganate, lithium cobaltate, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminate, lithium nickelate or a mixture thereof, the addition of the polyether siloxane can better achieve effects such as improving the flexibility of the electrode plate and increasing the coating weight of the electrode plate.
[0017] In any embodiment, the stability factor of the positive electrode slurry is 0 < V ≤ 6, and optionally 0 < V ≤ 4, where V = (V2 - V1) / V1 × 100%, V1 is the initial viscosity of the positive electrode slurry, i.e., the viscosity 0 hours after production, V2 is the viscosity of the positive electrode slurry 48 hours after production, where The positive electrode slurry used to measure V1 and the positive electrode slurry used to measure V2 are the same lot of positive electrode slurry.
[0018] The closer the viscosity of the positive electrode slurry 48 hours after production is to the initial viscosity, the more stable the slurry viscosity is. When the stability factor V ≤ 6, it is determined that the slurry viscosity is stable, and when V > 6, it is determined that the slurry viscosity is unstable. According to the measurement, after adding the polyether siloxane within the scope of the present application, the stability factor of the positive electrode slurry is all 0 < V ≤ 6, and optionally 0 < V ≤ 4, while when some other polyether siloxanes in the prior art are adopted, the stability factor is basically greater than 6.
[0019] The second aspect of the present application provides a positive electrode plate, which a positive electrode current collector, and and a positive electrode film layer located on at least one surface of the positive electrode current collector, the positive electrode film layer comprising the positive electrode slurry according to the first aspect of the present application. As described above, by adding the polyether siloxane, the present application allows for an improvement in the coating weight of the positive electrode plate. This is also manifested in an increase in the maximum weight of the positive electrode film layer per unit plate. In some embodiments, the mass of the positive electrode film layer per unit area of the plate is in the range of 13 to 45 mg / cm. 2 The selectable range is 20 to 43 mg / cm 2 and the selectable range is 22 to 33 mg / cm 2 The most selectable range is 25-31 mg / cm 2 where the mass is the mass of the positive electrode film layer on one side of the plate. If the positive electrode plate has a positive electrode film layer on both sides, the mass range of the positive electrode film layer per unit area on the plate is twice the above range, i.e., the range is 26 to 90 mg / cm. 2 The selectable range is 40 to 86 mg / cm 2 and the selectable range is 44 to 66 mg / cm 2 The most selectable range is 50-62mg / cm 2 where the mass is the mass of the positive electrode film layer on the two surfaces of the plate.
[0020] If the weight of the positive electrode film layer on the electrode plate per unit area is too small, the uniformity of the electrode plate will be low, and if the weight of the positive electrode film layer on the electrode plate per unit area is too large, the electrode plate will experience cracking during the coating process, making it impossible to continue production.
[0021] The positive plate described in the present application has excellent flexibility and significantly improved coating weight, so that the positive plate can be applied to secondary batteries, for example, by directly adding it to the positive electrode slurry during production, to improve the energy density of the battery.
[0022] In any embodiment, the weight ratio of elemental lithium to elemental silicon in the positive electrode plate corresponds to the weight ratio of elemental lithium to elemental silicon in the positive electrode slurry, i.e., in the range of 60 to 3875, a selectable range is 60 to 1950, a further selectable range is 90 to 1950, and a most selectable range is 380 to 1950.
[0023] In any embodiment, in the positive electrode slurry (or positive electrode plate), when only the polyethersiloxane contains silicon and only the active material contains lithium element, the weight ratio of lithium element to silicon element corresponds to the weight ratio of the positive electrode active material to the polyethersiloxane. Therefore, for such a case, the present application further limits the weight ratio of lithium element to silicon element. If the weight ratio of lithium element to silicon element is too large, the positive electrode plate will crack at high coating weight, and if the weight ratio is too small, it will have a negative impact on the battery performance.
[0024] In any embodiment, the positive electrode membrane layer includes two sublayers parallel to the positive electrode current collector and stacked on top of each other, wherein the weight content of silicon in the sublayer closest to the positive electrode current collector is in the range of 0 to 60 relative to the weight ratio of silicon in the sublayer furthest from the positive electrode current collector, with a selectable range being 0.1 to 30 and a further selectable range being 0.1 to 9.
[0025] Coating weight is 23mg / cm 2 or more (i.e., the mass of the positive electrode film layer per unit area of the electrode plate is 23 mg / cm 2 In some cases, applying multiple coats compared to a single thick coat can reduce the material cost of the flexibility additive and allow the polyether siloxane to perform better without affecting electrical performance.
[0026] In any embodiment, when the flexibility of the electrode plate is determined by folding the electrode plate in half and pressing it with a roller, The plate break length of the positive plate is 0; or The breaking length of the positive electrode plate is greater than 0 and less than or equal to 2 mm.
[0027] In this application, the method for determining the flexibility of the electrode plate by folding the electrode plate in half and performing roller pressing is as follows. Along the direction perpendicular to the machine direction (TD), a cold-pressed electrode plate with a size of 10 cm × 5 cm is measured, folded in half, and roller-pressed three times with a 2 kg hand roller, and the breaking length L of the electrode plate is inspected.
[0028] The method for determining the flexibility level of the electrode plate by folding the electrode plate in half and performing roller pressing is as follows.
[0029] When L = 0, there is a fold but no light transmission, and the flexibility of the electrode plate is of the first level. When 0 < L ≤ 2 mm, the light transmittance is weak, and the flexibility of the electrode plate is of the second level. When 2 mm < L ≤ 10 mm, it is defined that the light transmittance is strong, and the flexibility is of the third level. When 10 mm < L ≤ 20 mm, it is defined as slightly broken, and the flexibility is of the fourth level. When L > 20 mm, it is defined as broken, and the flexibility is of the fifth level.
[0030] The closer the breaking length of the positive electrode plate is to 0, the better the flexibility of the electrode plate is shown, and the larger the breaking length of the electrode plate is, the worse the flexibility of the electrode plate is shown.
[0031] In the manufacture of the positive electrode plate, the hydrogen bonds formed in the positive electrode plate are broken during the cold pressing process. After adding the polyether siloxane described in this application, the flexible main chain of the polyether siloxane extends, and by reducing the cold pressing pressure, cracks can be reduced and the risk of tape breakage can be reduced, so the flexibility is improved.
[0032] In any embodiment, the range of the adhesion improvement rate S between the positive electrode film layer and the positive electrode current collector in the positive electrode plate is 2% to 50%, and the selectable range is 10% to 20%. Here, S = (S2 - S1) / S1 × 100%. S2 is the adhesive strength between the positive electrode film layer of the positive electrode plate and the positive electrode current collector; S1 is the adhesion between the positive electrode film layer of the positive electrode plate not containing the polyethersiloxane and the positive electrode current collector, where The positive electrode plate used when measuring S1 is the same as the positive electrode plate used when measuring S2, and the only difference is that the positive electrode plate used when measuring S1 does not contain the polyether siloxane, whereas the positive electrode plate used when measuring S2 contains the polyether siloxane.
[0033] The greater the adhesive strength between the positive electrode film layer in the positive electrode plate and the positive electrode current collector, the stronger the interaction between the active material in the positive electrode plate and the current collector, and conversely, the weaker the interaction between the active material in the positive electrode plate and the current collector, which may lead to the active material being peeled off from the current collector in some cases, making it impossible to manufacture a battery cell. In this application, the addition of polyether siloxane can improve the interaction between the active material and the current collector.
[0034] In any embodiment, the resistance reduction rate Ω of the positive electrode film in the positive electrode plate is in the range of 0 to 18%, and the selectable range is 6 to 15%, where Ω=(Ω1-Ω2) / Ω1×100%, Ω2 is the resistance of the positive electrode film, Ω1 is the resistance of the positive electrode film that does not contain the polyethersiloxane; Here, the positive electrode film used when measuring Ω1 is the same as the positive electrode film used when measuring Ω2, and the only difference is that the positive electrode film used when measuring Ω1 does not contain the polyether siloxane, whereas the positive electrode film used when measuring Ω2 contains the polyether siloxane.
[0035] The film resistance of the plate can also reflect the dispersibility of the slurry. The higher the dispersibility, the smaller the film resistance Ω of the plate. The positive plate described in this application has a reduced film resistance after adding polyether siloxane.
[0036] The third aspect of the present application provides a secondary battery, comprising a positive electrode plate according to the second aspect of the present application, or a positive electrode plate made from the positive electrode slurry according to the first aspect of the present application. The energy density of the secondary battery described in the present application is significantly improved. Moreover, the total material cost is reduced when manufacturing the battery. [Brief description of the drawings]
[0037] [Figure 1] 1 is a schematic diagram of the principle of interaction between the polyether siloxane in the positive plate of the present application and other materials in the positive plate, where the polyether siloxane is a polyether siloxane described in the present application. [Diagram 2] FIG. 1 is a schematic diagram of a process in the prior art in which a positive plate is torn during coating due to capillary tension, where the active material is a positive active material and the acting force is the acting force during the coating process, where the polyether siloxane described in the present application is not used. [Diagram 3] 1 is a schematic diagram of a positive electrode plate described in the present application that does not tear during the coating process, where the active material is a positive electrode active material, the acting force is the acting force during the coating process, and where the polyether siloxane described in the present application is used. [Figure 4] FIG. 1 is a schematic diagram of the increase in maximum coating weight per unit area in a positive electrode plate after using the polyethersiloxane of the present application, where the positive electrode material represents the positive electrode active material, SP represents the conductive agent used in the positive electrode plate, and PVDF represents the adhesive used in the positive electrode plate, where X represents the maximum coating thickness of a positive electrode slurry that does not contain polyethersiloxane, and Y represents the maximum coating thickness of a positive electrode slurry that contains polyethersiloxane under similar conditions, and obviously, Y is greater than X. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0038] Hereinafter, with appropriate reference to the drawings, embodiments specifically disclosing the positive electrode slurry, positive electrode plate, negative electrode plate, secondary battery, battery module, battery pack, and electric device of the present application will be described in detail. However, unnecessary detailed description may be omitted. For example, detailed description of well-known matters and duplicated description of structures that are actually the same may be omitted. This is to avoid the following description becoming unnecessarily long and to allow those skilled in the art to easily understand. Note that the drawings and the following description are provided to allow those skilled in the art to fully understand the present application, and are not intended to limit the subject matter described in the claims.
[0039] The "ranges" disclosed in this application are defined in the form of lower and upper limits, and a given range is defined by selecting one lower limit and one upper limit that define the boundaries of the particular range. Such defined ranges may or may not include the end values, and may be arbitrarily combined, i.e., any lower limit and any upper limit may be combined to form a range. For example, if ranges of 60-120 and 80-110 are listed for a particular parameter, it is also conceivable that they are understood as ranges of 60-110 and 80-120. It is to be noted that if minimum range values 1 and 2 are listed, and maximum range values 3, 4, and 5 are listed, all of the ranges 1-3, 1-4, 1-5, 2-3, 2-4, and 2-6 are conceivable. In this application, unless otherwise stated, the numerical range "a-b" is a shorthand expression representing all real number combinations between a and b, where a and b are both real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed herein, with "0-5" being merely a shorthand for combinations of these numbers. Also, when a parameter is described as an integer ≧2, this is equivalent to disclosing that the parameter is, for example, the integers 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0040] Unless otherwise stated, all the embodiments and optional embodiments in the present application may be combined with each other to form a new technical solution.
[0041] Unless otherwise stated, all technical features and optional technical features in the present application may be combined with each other to form a new technical solution.
[0042] Unless otherwise stated, all steps in the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b) to mean that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method mentioned above further includes step (c) to mean that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), may include steps (a), (c) and (b), may include steps (c), (a) and (b), etc.
[0043] Unless otherwise specified, the terms "comprise" and "comprises" referred to in this application may be open ended or closed ended. For example, the terms "comprise" and "comprises" may further include or include other ingredients not listed, or may include or include only the listed ingredients.
[0044] Unless otherwise stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, any one of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist), A is false (or does not exist) and B is true (or exists), or both A and B are true (or exist).
[0045] For lithium-ion batteries, the trend is to improve the energy density, and one of the ways to improve the energy density is to increase the coating weight of the positive plate. However, as the inventors of the present application have found, as shown in FIG. 2, in the coating process of a general positive electrode slurry, the positive plate will tear during or after the solvent evaporation due to the action of capillary tension, and the tear will further propagate to cause a large-area tear. In addition, this process is accompanied by the phenomenon of curling the edge of the plate. In addition, since the positive plate is hard and brittle, the tape will break during the cold pressing process, and the inner ring will break during the winding process. Based on this, the inventors of the present application have designed and synthesized a flexible polymer material, polyether siloxane, and by adding the flexible material, the coating weight can be improved, the coating mass can be improved, the risk problems caused by the cold pressing and winding processes can be eliminated, and the total cost of materials used in battery manufacturing can be reduced.
[0046] Thus, a first aspect of the present application provides a cathode slurry, comprising an active cathode material and a polyether siloxane, the polyether siloxane comprising at least [ka] The structural unit includes Where: D is a methyl group or an ethyl group; A is hydrogen, a halogen or a halogenated alkyl group, said halogen being optionally fluorine, chlorine or bromine, said A is optionally hydrogen or a fluoromethyl group; B is hydroxyl, R, OR, or ROR', where R, R' are each independently a straight or branched chain alkyl group containing 1 to 8 carbons; and optionally B is a methyl group, an ethyl group, or an ethoxymethyl group; E is a phenyl group, an alkyl-substituted phenyl group, an etherified phenyl group, or a halogenated phenyl group, and said E is optionally a phenyl group or a fluorophenyl group.
[0047] In the polyether siloxanes described in this application, the structural unit (IV) is present as a terminal group.
[0048] Optionally, in some embodiments, the polyether siloxane is (a) Unsubstituted or halogen or halogenated C 1-8 ethylene oxide substituted with an alkyl group; (b) ethylene oxide substituted with hydroxyl, hydroxyalkyl, R, OR, or ROR', where R and R' are each independently C 1-8 alkyl group, where the alkyl group in the hydroxyalkyl group is C 1-8 an alkyl group; (c) ethylene oxide substituted with a halogenated phenyl group, a halogenated alkylphenyl group, or a phenyl group; (d) C 1-8 Alkyl group or C 1-8 A component obtained by polymerizing triethoxysilane or trimethoxysilane substituted with an alkenyl group, wherein, with respect to the total molar amount of components (a) to (d), the molar ratio of component (a) is 0 to 75 mol%, and optionally 10 to 40 mol%, the molar ratio of component (b) is 0 to 70 mol%, and optionally 40 to 65 mol%, the molar ratio of component (c) is 5 to 65 mol%, and the molar ratio of component (d) is 4 to 10 mol%, Here, components (a) and (b) are not simultaneously zero.
[0049] In some embodiments, optionally, component (a) is selected from ethylene oxide, epifluorohydrin, epichlorohydrin, epibromohydrin.
[0050] In some embodiments, optionally, component (b) is selected from propylene oxide, ethyl glycidyl ether, isopropyl glycidyl ether, butyl glycidyl ether, isopropyl glycidyl ether, butylene oxide, 1,2-epoxybutane, 1,2-epoxypentane, 1,2-epoxyheptane, 1,2-epoxyoctane, 1,2-epoxydecane, 1,2-epoxy-3-methylbutane, and glycidol.
[0051] In some embodiments, optionally, component (c) is selected from styrene oxide, a phenyl group.
[0052] In some embodiments, optionally, component (d) is selected from vinyltriethoxysilane.
[0053] In this application, 1-8 The alkyl group is a straight-chain or branched-chain alkyl group containing 1 to 8 carbon atoms, and examples of the straight-chain or branched-chain alkyl group containing 1 to 8 carbon atoms include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, an isopropyl group, an isobutyl group, a t-butyl group, an isopentyl group, a t-pentyl group, a neopentyl group, a 2-methylpentyl group, a 3-methylpentyl group, a 2,2-dimethylbutyl group, a 2,3-dimethylbutyl group, a 2-methylhexyl group, a 3-methylhexyl group, a 2,2-dimethylpentyl group, a 3,3-dimethylpentyl group, a 2,3-dimethylpentyl group, a 2,4-dimethylpentyl group, and the like. may be selected from among butyl, 3-ethylpentyl, 2,2,3-trimethylbutyl, 2-methylheptyl, 3-methylheptyl, 4-methylheptyl, 2,2-dimethylhexane, 3,3-dimethylhexane, 2,3-dimethylhexane, 2,4-dimethylhexane, 2,5-dimethylhexane, 3,4-dimethylhexane, 3-ethylhexane, 2,2,3-trimethylpentane, 2,2,4-trimethylpentane, 2,3,3-trimethylpentane, 2,3,4-trimethylpentane, 2-methyl-3-ethylpentane, 3-methyl-3-ethylpentane, 2,2,3,3-tetramethylbutane.
[0054] In this application, 1-8 The alkenyl group is a straight or branched alkenyl group containing 1 to 8 carbons, which may include, but is not limited to, vinyl, propenyl, allyl, 1-methylprop-2-en-1-yl, 2-methylprop-2-en-1-yl, but-2-en-1-yl, but-3-en-1-yl, 1-methylbut-3-en-1-yl, and 1-methylbut-2-en-1-yl.
[0055] In the present application, the alkyl substituent may be a straight or branched chain alkyl group containing 1 to 8 carbons, which is optionally selected from methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, and t-butyl groups. Optionally, the alkyl substitution is mono- or di-substituted. In some embodiments, the phenyl group substituted with an alkyl group may be selected from, for example, 3,4-dimethylphenyl, 2-methylphenyl, 3,5-dimethylphenyl, and 4-(2-methylpropyl)phenyl.
[0056] In the present application, the alkyl group in the halogenated alkyl group is optionally a straight or branched alkyl group containing 1 to 8 carbons, for example, the alkyl group in the halogenated alkyl group is optionally a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, an isopropyl group, an isobutyl group, a t-butyl group, an isopentyl group, a t-pentyl group, a neopentyl group, a 2-methylpentyl group, a 3-methylpentyl group, a 2,2-dimethylbutyl group, a 2,3-dimethylbutyl group, a 2-methylhexyl group, a 3-methylhexyl group, a 2,2-dimethylpentyl group, a 3,3-dimethylpentyl group, a 2 ... ethylpentyl, 2,4-dimethylpentyl, 3-ethylpentyl, 2,2,3-trimethylbutyl, 2-methylheptyl, 3-methylheptyl, 4-methylheptyl, 2,2-dimethylhexane, 3,3-dimethylhexane, 2,3-dimethylhexane, 2,4-dimethylhexane, 2,5-dimethylhexane, 3,4-dimethylhexane, 3-ethylhexane, 2,2,3-trimethylpentane, 2,2,4-trimethylpentane, 2,3,3-trimethylpentane, 2,3,4-trimethylpentane, 2-methyl-3-ethylpentane, 3-methyl-3-ethylpentane, 2,2,3,3-tetramethylbutane. The halogen in the halogenated alkyl group may be selected from fluorine, chlorine, bromine, and iodine.
[0057] In this application, the ether substituent may be a straight or branched chain alkoxy group containing 1 to 8 carbons, and is optionally selected from methoxy, ethoxy, propoxy, or butoxy groups. In some embodiments, the etherified phenyl group may be selected from, for example, 4-methoxyphenyl, 3-methoxyphenyl, and the like.
[0058] In this application, a halogenated alkylphenyl group refers to a phenyl group substituted with a halogenated alkyl group, where the halogenated alkyl group refers to an alkyl group substituted with a halogen, where the alkyl group is C 1-8 It is an alkyl group.
[0059] In the present application, the halogenated phenyl group represents a phenyl group substituted with a halogen. In the present application, the halogen may be selected from fluorine, chlorine, bromine, and iodine. In some embodiments, the halogenated phenyl group may be selected from, for example, 4-fluorophenyl, 2-fluorophenyl, 2,6-difluorophenyl, 4-(trifluoromethyl)phenyl, 4-chlorophenyl, 3-chlorophenyl, 4-bromophenyl, 3-bromophenyl, or 2-bromophenyl.
[0060] In the polyethersiloxane described in the present application, the structural unit (IV) (or the structural unit formed by component (d)) can ensure the stability and dispersibility of the polymer and improve the strength of the polymer; the structural unit (I) (or the structural unit formed by component (a)) can improve the ability of the polymer to form hydrogen bonds with the positive electrode particle surface, conductive carbon, and aluminum foil; the structural unit (II) (or the structural unit formed by component (b)) extends the molecular branching to ensure that the polyethersiloxane forms covalent bonds with the positive electrode particle surface, conductive carbon, and aluminum foil surface, and ensures that the positive electrode particles do not move during the coating process; and the structural unit (III) (or the structural unit formed by component (c)) improves the rigidity of the polyethersiloxane and gives it a certain strength and hardness, thereby improving the oxidation resistance and electrolyte resistance of the polyethersiloxane, and the benzene ring forms an interaction with the positive electrode particle surface to ensure the dispersibility of the polyethersiloxane.
[0061] As shown in FIG. 1, the polyether siloxane described in the present application is a long main chain flexible chain, which may form a hydrogen bond with the positive electrode active material and the positive electrode current collector through the structural unit (I) (or the structural unit formed by component (a)), may form a covalent bond with the positive electrode active material and the positive electrode current collector through the structural unit (II) (or the structural unit formed by component (b)), and may interact with the positive electrode active material particle surface through the benzene ring in the structural unit (III) (or the structural unit formed by component (c)). Covalent bonds may also be formed between the polyether siloxanes described in the present application. Therefore, by adding the polyether siloxane described in the present application to the positive electrode slurry, the stability of the positive electrode slurry can be improved, the flexibility of the positive electrode plate can be improved, and the coating weight of the positive electrode plate can be improved by ensuring the dispersibility of each material in the positive electrode plate. As shown in FIG. 3, after the addition of the polyether siloxane, the positive electrode slurry of the present application was not torn during the coating process. As shown in FIG. 4, after adding the polyether siloxane of the present application, the maximum coating thickness (weight) on the positive plate was obviously improved.
[0062] The polyether siloxanes described in this application may be obtained by common technical means in the art or may be prepared by the following steps: Step (1): preparing polyether from alkylene oxide monomer under alkaline condition, where optionally, the reaction is carried out in a reactor, optionally, the solvent used is one or more of dimethyl sulfoxide, acetone, diethyl ether, optionally, the basic substance that can be added during the preparation is, for example, NaOH, KOH, dicyclohexylcarbodiimide, optionally, the reaction temperature range of the reaction is 80-160°C, the reaction time range is 3-7h, optionally, the stirring speed range during the reaction is 1000-2000 rpm, and optionally, after the reaction is completed, a vacuum distillation purification step is carried out.
[0063] Step (2): reacting the polyether in step (1) with a silane coupling agent to produce polyether siloxane, where optionally, the reaction is carried out in a reactor, optionally, the silane coupling agent includes one of vinyltrimethoxysilane, vinyltriethoxysilane, optionally, the reaction temperature range is 60-130°C, optionally, the reaction time range is 2-15h, optionally, stirring is performed during the reaction, the stirring time range is optionally 1-10h, and the stirring speed range is optionally 1000-2000r / min, and optionally, a reduced pressure distillation purification step is performed after the reaction is completed.
[0064] In some embodiments, the positive electrode slurry described herein has a pH range of about 6 to 9 at 20 to 60° C. The pH value can be measured by common means in the art.
[0065] In any embodiment of the present application, after adding the polyethersiloxane to the positive electrode slurry, the resulting lithium ion battery has an obviously improved energy density.In addition, the improvement of the positive electrode plate can save the amount of battery cells used, thereby reducing the total cost of materials used in battery production.
[0066] In some embodiments, the number average molecular weight range of the polyether siloxane is 10,000 to 60,000, with a selectable range being 20,000 to 60,000. In other embodiments, the number average molecular weight of the polyether siloxane is optionally selected from the ranges of 10,000 to 50,000, 20,000 to 50,000, 20,000 to 30,000, or 20,000 to 40,000.
[0067] The molecular weight affects the processing performance of the positive plate. If the molecular weight is small, the flexibility of the positive plate is not significantly improved, the phenomenon of tearing during application still occurs, and the problem of cold press tape breakage and winding breakage may occur. If the molecular weight is too small, the stability of the positive electrode slurry is low, the physical gelation phenomenon is easy to occur, and the resistance of the positive electrode film is deteriorated, which also has a negative impact on the battery performance. If the molecular weight is too large, it is disadvantageous to the dispersion of the polyether siloxane in the positive electrode slurry. Therefore, the number average molecular weight of the polyether siloxane needs to be controlled within the above range.
[0068] In some embodiments, in the polyether siloxane described herein, the molar ratio of the structural unit (I) is 0 to 75 mol%, the molar ratio of the structural unit (II) is 0 to 70 mol%, the molar ratio of the structural unit (III) is 5 to 65 mol%, and the molar ratio of the structural unit (IV) is 4 to 10 mol%, based on the total molar amount of the structural units (I) to (IV), and the molar ratios of the structural units (I) and (II) are not zero at the same time.
[0069] Optionally, the molar ratio of the structural unit (I) to the total molar amount of the structural units (I) to (IV) (or the molar ratio of the component (a) to the total molar amount of the components (a) to (d)) may be about 0 mol%, about 5 mol%, about 10 mol%, about 15 mol%, about 17 mol%, about 20 mol%, about 25 mol%, about 26 mol%, about 27 mol%, about 28 mol%, about 29 mol%, about 30 mol%, about 31 mol%, about 32 mol%, about 35 mol%, about 40 mol%, about 45 mol%, about 50 mol%, about 55 mol%, about 60 mol%, about 65 mol%, about 70 mol%, about 72 mol%, or about 75 mol%. Or, the molar ratio of the structural unit (I) may be within any range consisting of any of the above values.
[0070] Optionally, the molar ratio of the structural unit (II) to the total molar amount of the structural units (I) to (IV) (or the molar ratio of the component (b) to the total molar amount of the components (a) to (d)) may be about 0 mol%, about 5 mol%, about 10 mol%, about 15 mol%, about 17 mol%, about 20 mol%, about 25 mol%, about 30 mol%, about 31 mol%, about 35 mol%, about 40 mol%, about 43 mol%, about 45 mol%, about 50 mol%, about 53 mol%, about 54 mol%, about 55 mol%, about 56 mol%, about 58 mol%, about 60 mol%, about 63 mol%, about 65 mol%, or about 70 mol%. Or, the molar ratio of the structural unit (II) may be within any range consisting of any of the above values.
[0071] Optionally, the molar ratio of the structural unit (III) to the total molar amount of the structural units (I) to (IV) (or the molar ratio of the component (c) to the total molar amount of the components (a) to (d)) is about 5 mol%, about 6 mol%, about 7 mol%, about 10 mol%, about 11 mol%, about 15 mol%, about 20 mol%, about 24 mol%, about 25 mol%, about 26 mol%, about 30 mol%, about 31 mol%, about 35 mol%, about 40 mol%, about 45 mol%, about 50 mol%, about 55 mol%, about 59 mol%, about 60 mol%, or about 65 mol%. Or, the molar ratio of the structural unit (III) is within any range consisting of any of the above values.
[0072] Optionally, the molar ratio of structural unit (IV) relative to the total molar amount of structural unit (I) to structural unit (IV) (or the molar ratio of component (d) relative to the total molar amount of components (a) to (d)) is about 4 mol%, about 5 mol%, about 6 mol%, about 7 mol%, about 8 mol%, about 9 mol%, or about 10 mol%, or the molar ratio of structural unit (IV) is within any range consisting of any of the above values.
[0073] In this application, the term "about" a certain value refers to a range, namely, a range of ±3% of the given value.
[0074] The molar ratios of the structural units (I) to (IV) (or components (a) to (d)) ensure that sufficient hydrogen bonds and an appropriate amount of covalent bonds are formed between the resulting polyether siloxane and the positive electrode active material, current collector, etc., and further ensure stability in the manufacturing process of the positive electrode plate, flexibility of the positive electrode plate, and dispersibility of various positive electrode materials, thereby improving the energy density of the battery.
[0075] In some embodiments, the weight ratio of the polyether siloxane to the positive electrode active material is 0.0005 to 0.030, a selectable range is 0.001 to 0.02, a further selectable range is 0.001 to 0.01, and a most selectable range is 0.001 to 0.006.
[0076] If the weight ratio of polyether siloxane to the positive active material is too small, the positive plate will crack at high application weights, and if the ratio is too large, it will adversely affect the battery performance.
[0077] In some embodiments, the weight ratio of lithium to silicon in the positive electrode slurry is in the range of 60 to 3875, with a selectable range being 60 to 1950, a further selectable range being 90 to 1950, and a most selectable range being 380 to 1950.
[0078] In some embodiments, in the positive electrode slurry, only the polyethersiloxane contains silicon, and only the active material contains lithium element, and in such a case, the weight ratio of lithium element to silicon element represents the weight ratio of the positive electrode active material to the polyethersiloxane.Therefore, for such a case, the present application further limits the weight ratio of lithium element to silicon element.Similarly, if the weight ratio of lithium element to silicon element is too large, the positive electrode plate will crack at high coating weight, and if the weight ratio is too small, it will have a negative impact on battery performance.
[0079] In some embodiments, the active cathode material is selected from at least one of lithium iron phosphate, lithium manganese iron phosphate, lithium manganate, lithium cobalt oxide, lithium nickel cobalt manganate, lithium nickel cobalt aluminate, lithium nickel oxide, or mixtures thereof.
[0080] Theoretically, for the positive electrode of the secondary battery, the present application may adopt a positive electrode active material for batteries well known in the art. As an example, the positive electrode active material may include at least one material of lithium-containing phosphate with an olivine structure, lithium transition metal oxide, and each modified compound. However, the present application is not limited to these materials, and may further use other conventional materials that can be used as a positive electrode active material of a battery. These positive electrode active materials may be used alone or in combination of two or more. Here, examples of the lithium transition metal oxide include lithium cobalt oxide (e.g., LiCoO2), lithium nickel oxide (e.g., LiNiO2), lithium manganese oxide (e.g., LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (e.g., LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2(NCM 333 (may be abbreviated as LiNi 0.5 Co 0.2 Mn 0.3 O2(NCM 523 (may be abbreviated as LiNi 0.5 Co 0.25 Mn 0.25 O2(NCM 211 (may be abbreviated as LiNi 0.6 Co 0.2 Mn 0.2 O2(NCM 622 (may be abbreviated as LiNi 0.8 Co 0.1 Mn 0.1 O2(NCM 811 Lithium nickel cobalt aluminum oxide (e.g., LiNi0.85 Co 0.15 Al 0.05 It may contain, but is not limited to, at least one of O2) and its modified compounds. Examples of lithium-containing phosphates having an olivine structure include lithium iron phosphate (e.g., LiFePO4 (which may be abbreviated as LFP)), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (e.g., LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium manganese iron phosphate, and a composite material of lithium manganese iron phosphate and carbon, but are not limited thereto.
[0081] However, the inventors of the present application have discovered that when the positive electrode active material is at least one of lithium iron phosphate, lithium manganese iron phosphate, lithium manganate, lithium cobaltate, lithium nickel cobalt manganate, lithium nickel cobalt aluminate, lithium nickelate, or a mixture thereof, the addition of the polyether siloxane can better achieve effects such as improving the flexibility of the electrode plate and increasing the coating weight of the electrode plate.
[0082] In some embodiments, the stability factor of the positive electrode slurry is 0 < V ≤ 6, and optionally, 0 < V ≤ 4, where V = (V2 - V1) / V1 × 100%, V1 is the initial viscosity of the positive electrode slurry, i.e., the viscosity 0 hours after production, V2 is the viscosity of the positive electrode slurry 48 hours after production, where The positive electrode slurry used when measuring V1 and the positive electrode slurry used when measuring V2 are of the same lot of positive electrode slurry.
[0083] In this application, the viscosity is measured at room temperature (20 - 35°C) using a viscometer (for example, a viscometer with model number DVESLVTJ0 purchased from Brookfield). The closer the viscosity of the positive electrode slurry is to the initial viscosity 48 hours after the production of the positive electrode slurry, the more stable the slurry viscosity is indicated. When the stability factor V ≤ 6, it is determined that the slurry viscosity is stable, and when V > 6, it is determined that the slurry viscosity is unstable. According to the measurement, after adding the polyether siloxane within the scope of this application, the stability factors of the positive electrode slurries are all 0 < V ≤ 6, and optionally 0 < V ≤ 4. In contrast, when some other polyether siloxanes in the prior art are adopted, the stability factor is basically greater than 6.
[0084] The second aspect of this application provides a positive electrode plate, a positive electrode current collector, and a positive electrode film layer located on at least one surface of the positive electrode current collector, wherein the positive electrode film layer contains the positive electrode slurry described in the first aspect of this application. As described above, this application realizes an improvement in the coating weight in the positive electrode plate by adding the polyether siloxane. This is also manifested in terms of an increase in the maximum weight per unit electrode plate of the positive electrode film layer. In some embodiments, the mass of the electrode plate per unit area of the positive electrode film layer is in the range of 13 - 45 mg / cm 2 and the selectable range is 20 - 43 mg / cm 2 and the further selectable range is 22 - 33 mg / cm 2 and the most selectable range is 25 - 31 mg / cm 2 and the mass is the mass of the positive electrode film layer on one side of the electrode plate. If there are positive electrode film layers on both surfaces of the positive electrode plate, the mass range of the electrode plate per unit area of the positive electrode film layer is twice the above range, that is, the range is 26 - 90 mg / cm 2 and the selectable range is 40 - 86 mg / cm 2 and the further selectable range is 44 - 66 mg / cm 2 and the most selectable range is 50 - 62 mg / cm 2where the mass is the mass of the positive electrode film layer on the two surfaces of the plate.
[0085] In some embodiments, the addition of the polyether siloxane allows the coating weight (single side) of the positive plate described herein to be up to 45 mg / cm 2 , optionally up to 23-45 mg / cm 2 and optionally up to 28-43 mg / cm 2 may be also possible.
[0086] If the weight of the positive electrode film layer on the electrode plate per unit area is too small, the uniformity of the electrode plate is low, and if the weight of the positive electrode film layer on the electrode plate per unit area is too large, the electrode plate will have a tear phenomenon during the coating process, making it impossible to continue production. This application limits the weight of the positive electrode film layer on the electrode plate per unit area to the above range, ensuring that the highest effect is achieved within this range.
[0087] The positive electrode current collector has two surfaces opposing each other in the thickness direction of the positive electrode current collector, and the positive electrode film layer is provided on either one or both of the two opposing surfaces of the positive electrode current collector.
[0088] In the lithium ion battery of the present application, the positive electrode current collector may adopt a metal foil sheet or a composite current collector. For example, an aluminum foil may be adopted as the metal foil sheet. The composite current collector may include a polymeric material base layer and a metal layer formed on at least one surface of the polymeric material base layer. The composite current collector may be formed by forming a metal material (such as aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy) on a polymeric material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0089] In the positive electrode plate, the mass content of the positive electrode active material in the positive electrode film layer is 90-97% relative to the positive electrode film layer. The content may be measured by EDS. If the mass content is too small, the battery produced will have low energy density and cannot meet the demand for battery capacity, and if the mass content is too large, the adhesive and conductive agent will be insufficient, resulting in poor battery performance.
[0090] In the positive electrode plate, the mass content of the adhesive in the positive electrode film layer is 2 to 5% with respect to the total mass of the positive electrode film layer. As an example, the adhesive may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene ternary copolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene ternary copolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylic ester resin. In the conventional general positive electrode plate, an adhesive with a specific crystallinity or a similar crystallinity is used, and after coating and drying, the plate is brittle and easily cracks under stress, but in the positive electrode plate of the present application, an adhesive with a similar crystallinity is used, and the plate does not crack.
[0091] In some embodiments, the positive electrode membrane layer optionally further comprises a conductive agent, which may include at least one of superconducting carbon, acetylene black, carbon black, ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers, by way of example only.
[0092] In some embodiments, the positive electrode plate can be manufactured in the following manner. The components for manufacturing the positive electrode plate, such as the positive electrode active material, the polyether siloxane additive described in the present application, the conductive agent, the adhesive, and any other components, are dispersed in a solvent (e.g., N-methylpyrrolidone) to form a positive electrode slurry, and the positive electrode slurry is applied to a positive electrode current collector, and the positive electrode plate is obtained after processes such as drying and cold pressing.
[0093] The positive electrode plate described in the present application has a very high flexibility and a significantly improved coating weight, for example, an improvement of about 36% in the positive electrode coating weight can be achieved. The positive electrode plate can be applied to a secondary battery, for example, by directly adding it to the positive electrode slurry during the manufacturing process, to improve the energy density of the battery.
[0094] In some embodiments, the weight ratio of lithium and silicon in the positive plate corresponds to the weight ratio of lithium and silicon in the positive electrode slurry, i.e., the range is 60-3875, the selectable range is 60-1950, the more selectable range is 90-1950, and the most selectable range is 380-1950. The effect of the weight ratio of lithium and silicon is as described above. The weights of lithium and silicon may be measured by energy dispersive spectroscopy (EDS) or inductively coupled plasma spectroscopy (ICP).
[0095] In some embodiments, the positive electrode membrane layer includes two sublayers parallel to the positive electrode current collector and stacked on top of each other, wherein the weight content of silicon in the sublayer closest to the positive electrode current collector is in the range of 0 to 60, with a selectable range being 0.1 to 30, and further selectable range being 0.1 to 9, relative to the weight content of silicon in the sublayer furthest from the positive electrode current collector.
[0096] Optionally, when preparing a positive electrode membrane layer having two sublayers, two positive electrode slurries containing different amounts of polyether siloxane are first prepared and one slurry is applied to the current collector and dried, and then the other slurry is applied and dried.
[0097] The thicknesses of the two sublayers may be the same or different. The thickness of the sublayer closest to the positive electrode current collector may be smaller or larger than the thickness of the sublayer furthest from the positive electrode current collector. For example, the thicknesses of the two sublayers may be measured by a cross section using an ion milling device in combination with SEM, and when detecting the manufactured positive electrode membrane layer, the silicon content in the sublayer closest to the positive electrode current collector and the silicon content in the sublayer furthest from the positive electrode current collector can be detected by a method in which elemental analysis is performed on the cross section using an ion milling device and combined with EDS.
[0098] When a positive electrode plate is manufactured under the condition of the same content of polyether siloxane, the maximum coating weight of the positive electrode slurry per unit area achieved by multi-layer coating is greater than the maximum coating weight of the positive electrode slurry per unit area achieved by single-layer coating. For example, when the positive electrode slurry is coated on one surface of the positive electrode current collector, the coating weight in one application is 36 mg / cm2. 2 During the coating process, the capillary tension and stress can easily cause the plate to crack, so the coating density is 36mg / cm 2 When a second coating is performed, two cathode slurries are prepared, each containing a different amount of polyether siloxane, specifically, the polyether siloxane content in each layer satisfies the above conditions. In the first layer, 18 mg / cm 2 The plate was not cracked due to the small capillary tension and stress caused by the application, and the first layer was applied with a coating weight of 18 mg / cm2. 2 When the second layer is applied with a coating weight of 36mg / cm, the plate still does not crack due to the action of polyether siloxane. 2 Therefore, the secondary coating increases the maximum coating weight of the positive electrode slurry per unit area of the plate, further increasing the energy density of the battery.
[0099] In some embodiments, when the flexibility of a plate is determined by folding the plate in half and pressing it with a roller, The fracture length of the positive electrode plate is 0, or the fracture length of the positive electrode plate is greater than 0 and less than or equal to 2 mm.
[0100] In this application, the method for determining the flexibility of the electrode plate by folding the electrode plate in half and performing roller pressing is as follows. Along the direction perpendicular to the machine direction (TD), a cold-pressed electrode plate with a size of 10 cm × 5 cm is measured, folded in half, and roller-pressed three times with a 2 kg hand roller, and the fracture length L of the electrode plate is inspected.
[0101] The method for judging the flexibility level is as follows.
[0102] L = 0 means there is a fold but light does not pass through, and the flexibility of the electrode plate is of the first level. 0 < L ≤ 2 mm means weak light transmittance, and the flexibility of the electrode plate is of the second level. 2 mm < L ≤ 10 mm is defined as strong light transmittance, and the flexibility is of the third level. 10 mm < L ≤ 20 mm is defined as slightly broken, and the flexibility is of the fourth level. L > 20 mm is defined as broken, and the flexibility is of the fifth level.
[0103] The closer the fracture length of the positive electrode plate is to 0, the better the flexibility of the electrode plate is shown, and the larger the fracture length is, the worse the flexibility of the electrode plate is shown.
[0104] In the manufacture of the positive electrode plate, during the cold pressing process, the hydrogen bonds formed in the positive electrode plate are broken, and the flexible main chain extends. However, after adding the polyether siloxane described in this application, by reducing the cold pressing pressure, cracks can be reduced and the risk of tape breakage can be reduced, so the flexibility is improved.
[0105] In some embodiments, the range of the adhesion improvement rate S between the positive electrode film layer and the positive electrode current collector in the positive electrode plate is 2% to 50%, and the selectable range is 10% to 20%. Here, S = (S2 - S1) / S1 × 100%, S2 is the adhesive strength between the positive electrode film layer of the positive electrode plate and the positive electrode current collector; S1 is the adhesion between the positive electrode film layer of the positive electrode plate not containing the polyethersiloxane and the positive electrode current collector, where The positive electrode plate used when measuring S1 is the same as the positive electrode plate used when measuring S2, and the only difference is that the positive electrode plate used when measuring S1 does not contain the polyether siloxane, whereas the positive electrode plate used when measuring S2 contains the polyether siloxane.
[0106] In the present application, the method for measuring S1 and S2 is as follows.
[0107] The test plate is weighed along the direction perpendicular to the machine direction (TD), a sample with a size of 20 mm (width) x (100-160) mm (length) is cut out, and a special double-sided tape is attached to a steel plate, the size of the tape being 20 mm (width) x (90-150) mm (length). After attaching the cut plate sample to the double-sided tape, it is rolled three times in the same direction with a 2 kg hand roller. The adhesive strength of the plate is tested with a tensile machine, and the plate without the polyether siloxane has an adhesive strength of S1, and the plate with the polyether siloxane has an adhesive strength of S2.
[0108] In the test, for example, a 2Kg hand roller purchased from Guangdong Iris Technology Co., Ltd. can be used, with a roller width of 45mm, a roller diameter of 83mm, a rubber thickness of 6mm, and a rubber hardness of HS80±5.
[0109] In the test, for example, a tensile machine with model number 336, purchased from INSTRON, USA, can be used.
[0110] The greater the adhesive strength between the positive electrode film layer in the positive electrode plate and the positive electrode current collector, the stronger the interaction between the active material in the positive electrode plate and the current collector, and conversely, the weaker the interaction between the active material in the positive electrode plate and the current collector, which may lead to the active material being peeled off from the current collector in some cases, making it impossible to manufacture a battery cell. In this application, the addition of polyether siloxane can improve the interaction between the active material and the current collector.
[0111] In some embodiments, the resistance reduction rate Ω of the positive electrode film in the positive electrode plate is in the range of 0 to 18%, and a selectable range is 6 to 15%, where Ω=(Ω1-Ω2) / Ω1×100%, Ω2 is the resistance of the positive electrode film, Ω1 is the resistance of the positive electrode film that does not contain the polyethersiloxane; Here, the positive electrode film used when measuring Ω1 is the same as the positive electrode film used when measuring Ω2, and the only difference is that the positive electrode film used when measuring Ω1 does not contain the polyether siloxane, whereas the positive electrode film used when measuring Ω2 contains the polyether siloxane.
[0112] In this application, the measurement of Ω2 and Ω1 is performed using a film resistance meter with model number BER1100 purchased from Xiamen Yuan Neng Technology Co., Ltd., and the specific measurement method is as follows:
[0113] Take a plate with an area of 4cm x 25cm (longitudinal) along the mechanical tension (MD) direction, place the current collector of the test plate in the middle of the probe, press the operation button first, then press the switch valve down, after 15 seconds, a data will be automatically collected, and when it changes to another point, the test method is as above, and the test is continued until 20 points have been tested, and the resistances of the 20 points obtained respectively are averaged to obtain the values of Ω2 and Ω1 respectively.
[0114] The film resistance of the electrode plate can reflect the dispersibility of the slurry. The higher the dispersibility, the smaller the film resistance Ω of the electrode plate. After adding polyethersiloxane, the film resistance of the positive electrode plate described in the present application is reduced, and is reduced by about 0-18%, optionally by about 6-15%, compared with the film resistance of a general positive electrode plate, which means that the dispersibility of each material in the positive electrode plate manufactured after adding polyethersiloxane is improved.
[0115] The third aspect of the present application provides a secondary battery, comprising a positive electrode plate according to the second aspect of the present application, or a positive electrode plate made from the positive electrode slurry according to the first aspect of the present application. The energy density of the secondary battery described in the present application is significantly improved. Moreover, the total material cost is reduced when manufacturing the battery.
[0116] The secondary battery, battery module, battery pack and power consuming device of the present application are described below.
[0117] secondary battery Typically, a secondary battery includes a positive electrode plate, a negative electrode plate, an electrolyte, and a separator. During the charge and discharge process of the battery, active ions shuttle between the positive electrode plate and the negative electrode plate to perform intercalation and deintercalation. The electrolyte serves to conduct ions between the positive electrode plate and the negative electrode plate. The separator is provided between the positive electrode plate and the negative electrode plate, and serves mainly to prevent short-circuiting between the positive and negative electrodes, while allowing ions to pass through.
[0118] [Positive plate] The positive electrode plate according to the second aspect of the present application is employed, or the positive electrode plate is manufactured with the positive electrode slurry according to the first aspect of the present application.
[0119] [Negative plate] The negative electrode plate includes a negative electrode current collector and a negative electrode film layer provided on at least one surface of the negative electrode current collector, the negative electrode film layer including a negative electrode active material.
[0120] For example, the negative electrode current collector has two surfaces opposing each other in the thickness direction of the negative electrode current collector, and the negative electrode film layer is disposed on either one or both of the two opposing surfaces of the negative electrode current collector.
[0121] In some embodiments, the negative electrode current collector may be a metal foil sheet or a composite current collector. For example, a copper foil may be used as the metal foil sheet. The composite current collector may include a polymeric base layer and a metal layer formed on at least one surface of the polymeric substrate. The composite current collector may be formed by forming a metal material (such as copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy) on a polymeric substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0122] In some embodiments, the negative electrode active material may be a negative electrode active material for batteries well known in the art. As an example, the negative electrode active material may include at least one of artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based material, tin-based material, and lithium titanate. The silicon-based material may be selected from at least one of silicon elemental, silicon oxide, silicon carbon composite, silicon nitrogen composite, and silicon alloy. The tin-based material may be selected from at least one of tin elemental, tin oxide, and tin alloy. However, the present application is not limited to these materials, and other conventional materials that can be used as a negative electrode active material for a battery may be used. These negative electrode active materials may be used alone or in combination of two or more.
[0123] In some embodiments, the negative electrode membrane layer optionally further comprises an adhesive, which may be selected from at least one of styrene butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).
[0124] In some embodiments, the negative electrode membrane layer optionally further comprises a conductive agent, which may be selected from at least one of superconducting carbon, acetylene black, carbon black, ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0125] In some embodiments, the negative electrode membrane layer optionally further comprises other auxiliary agents, such as a thickening agent (eg, sodium carboxymethylcellulose (CMC-Na)).
[0126] In some embodiments, a negative electrode plate can be manufactured in the following manner. The components for manufacturing a negative electrode plate, such as the negative electrode active material, the conductive agent, the adhesive, and any other components, are dispersed in a solvent (e.g., deionized water) to form a negative electrode slurry, and the negative electrode slurry is applied to a negative electrode current collector. After undergoing processes such as drying and cold pressing, a negative electrode plate is obtained.
[0127] [Electrolyte] The electrolyte serves to conduct ions between the positive and negative plates. The present application does not specifically limit the type of electrolyte, and it can be selected according to needs. For example, the electrolyte may be selected from at least one of a solid electrolyte and a liquid electrolyte (i.e., an electrolyte solution).
[0128] In some embodiments, the electrolyte employs an electrolyte solution, the electrolyte solution including an electrolyte salt and a solvent.
[0129] In some embodiments, the electrolyte salt may be selected from one or more of lithium hexafluorophosphate (LiPF), lithium tetrafluoroborate (LiBF), lithium perchlorate (LiClO), lithium hexafluoroarsenate (LiAsF), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonylimide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluoro(oxalato)borate (LiDFOB), lithium bis(oxalato)borate (LiBOB), lithium difluorophosphate (LiPOF), lithium difluorobis(oxalato)phosphate (LiDFOP), and lithium tetrafluoro(oxalato)phosphate (LiTFOP).
[0130] In some embodiments, the solvent may be one or more selected from ethylene carbonate (EC), propylene carbonate (PC), methyl ethyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfone (SF), dimethyl sulfone (MSM), methyl ethyl sulfone (EMS), and diethyl sulfone (ESE).
[0131] In some embodiments, the electrolyte solution optionally further includes an additive. For example, the additive may include an anode film-forming additive, a cathode film-forming additive, or an additive that can improve some performance of the battery, such as an additive that improves the overcharge performance of the battery, an additive that improves the high temperature performance of the battery, or an additive that improves the low temperature performance of the battery.
[0132] [Separator] In some embodiments, the secondary battery further includes a separator. The separator is disposed between the positive and negative plates to provide an insulating effect. In the present application, there is no particular limitation on the type of separator, and any well-known separator with a porous structure having good chemical and mechanical stability may be selected.
[0133] In some embodiments, the separator may be made of at least one of glass fiber, nonwoven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator may be a single-layered thin film or a multi-layered composite thin film, without any particular limitation. When the separator is a multi-layered composite thin film, the materials of each layer may be the same or different, without any particular limitation.
[0134] [Exterior body] In some embodiments, the secondary battery may include an exterior body for packaging the positive electrode plate, the negative electrode plate, and the electrolyte. As an example, the positive electrode plate, the negative electrode plate, and the separator may be stacked or wound to form a stacked structure battery cell or a wound structure battery cell, and the battery cell may be packaged in the exterior body, and the electrolyte may adopt an electrolytic solution soaked in the battery cell. The number of battery cells in the secondary battery may be one or several, and may be adjusted according to demand.
[0135] In one embodiment, the present application provides an electrode assembly. In some embodiments, the positive and negative plates and the separator may be wound or stacked to produce the electrode assembly. The outer packaging may be used to package the electrode assembly and the electrolyte.
[0136] In some embodiments, the exterior of the secondary battery may be a soft package, for example, a bag-type soft package. The material of the soft package may be plastic, for example, one or more of polypropylene (PP), polybutylene terephthalate (PBT), polybutylene succinate (PBS), etc. In some embodiments, the exterior of the secondary battery may be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell.
[0137] Secondary battery manufacturing method In one embodiment, the present application provides a method for producing a secondary battery, in which a negative plate described in the present application or a negative plate produced according to the method described in the present application is used.
[0138] The manufacturing of the secondary battery may further include assembling the negative plate, the positive plate and the electrolyte of the present application to form a secondary battery. In some embodiments, the positive plate, the separator and the negative plate may be wound or stacked in order, with the separator being interposed between the positive plate and the negative plate to play the role of isolation, to obtain a battery cell, which is then inserted into an exterior body, injected with an electrolyte and sealed to obtain a secondary battery.
[0139] In some embodiments, the manufacturing of the secondary battery may further include a step of manufacturing a positive electrode plate. For example, a positive electrode active material, a conductive agent, and an adhesive may be dispersed in a solvent (e.g., N-methylpyrrolidone, abbreviated as NMP) to form a uniform positive electrode slurry, which is applied to a positive electrode current collector, and a positive electrode plate is obtained after processes such as drying and cold pressing.
[0140] In some embodiments, the manufacture of a secondary battery includes manufacturing a negative plate according to the methods described herein.
[0141] In the present application, there is no particular limitation on the shape of the secondary battery, which may be cylindrical, rectangular or any other shape.
[0142] In some embodiments, the present application provides a power consuming device, a battery module, or a battery pack, wherein the power consuming device, battery module, or battery pack includes a secondary battery described herein or manufactured according to a method described herein.
[0143] In some embodiments, the secondary batteries may be assembled into a battery module, and the number of secondary batteries included in the battery module may be one or more, with the specific number being selectable by one of ordinary skill in the art based on the application and capacity of the battery module.
[0144] In some embodiments, the battery modules may be further assembled into a battery pack, and the number of battery modules included in the battery pack may be one or more, and the specific number may be selected by one skilled in the art based on the application and capacity of the battery pack.
[0145] The present application further provides a power consuming device including at least one of the secondary battery, battery module, or battery pack according to the present application. The secondary battery, battery module, or battery pack may be used as a power source for the power consuming device, or may be used as an energy storage unit for the power consuming device. The power consuming device may include, but is not limited to, mobile equipment (e.g., mobile phone, laptop, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc. Another example of the device may be a mobile phone, a tablet computer, a laptop, etc. The device generally requires a reduction in weight, and may employ a secondary battery as a power source. The power consuming device may be a secondary battery, a battery module, or a battery pack according to the demands of its use.
[0146] Therefore, the present application provides a battery module including the secondary battery described in the present application.
[0147] The present application further provides a battery pack including the battery module.
[0148] The present application further provides a power consuming device including at least one of the secondary battery, the battery module, or the battery pack described in the present application.
[0149] <Example> The present application is described in detail below by examples, which are not limiting.
[0150] <Example 1> (Step 1, Production of polyether siloxane) 1) Precursor 1, precursor 2, and precursor 3 (see Table 1 for specific types and amounts) are reacted under alkaline conditions to produce polyether. When the number average molecular weight of the polyether reaches 2w (i.e., 20,000), the reaction is stopped. 2) The polyether produced in step 1) is reacted with a silane coupling agent (see Table 1 for the specific type and amount used) to produce polyether siloxane. After the reaction is completed, the polyether siloxane with a number average molecular weight of 1w~3w (i.e. 10,000~30,000) is cut out through filtration and dialysis.
[0151] (Step 2, Preparation of Positive Electrode Slurry) The positive electrode active material (lithium iron phosphate), conductive agent (conductive carbon black Super P), and adhesive PVDF are mixed for 30 minutes. The resulting mixture is then added to NMP and stirred for 180 minutes to disperse it uniformly. Finally, the polyether siloxane prepared in step 1 (see Table 2 for specific amount used) is added, and then thoroughly stirred for 60 minutes to form a uniform positive electrode slurry.
[0152] (Step 3, Manufacturing the Positive Plate) The positive electrode slurry is applied to the surface of the positive electrode current collector aluminum foil, and then dried and cold pressed to obtain a positive electrode plate. A series of positive electrode plate performance tests (mainly to test whether the plate breaks, refer to the positive electrode plate break length test method described in this specification, when the plate does not break, the maximum weight of the coating is the maximum coating weight per unit area) showed that the maximum coating weight per unit area was 30 mg / cm. 2 It was found to be the case.
[0153] (Step 4, Manufacturing the negative plate) Anode active material (graphite), conductive agent (Super P), adhesive (SBR), and thickener (CMC) are mixed in a mass ratio of 96.2:0.8:1.8:1.2 with an appropriate amount of deionized water and thoroughly stirred to form a uniform anode slurry. This anode slurry is applied to the two surfaces of anode current collector copper foil, and after drying and cold pressing, a cathode plate is obtained.
[0154] (Step 5, Electrolyte Production) Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) were mixed according to a volume ratio of 1:1:1, and then LiPF6 was uniformly dissolved in the above solution to obtain an electrolyte, in which the concentration of LiPF6 was 1 mol / L.
[0155] (Step 6, separator) Polyethylene (PE) film is used.
[0156] (Step 7, Manufacturing secondary batteries) The positive electrode plate, separator, and negative electrode plate are stacked in order and wound to obtain an electrode assembly, which is then inserted into an exterior body, the electrolyte is added, and the secondary battery of Example 1 is obtained after undergoing processes such as packaging, standing, chemical conversion, and aging. The exterior body is a hard case having a length x width x height of 148 mm x 28.5 mm x 97.5 mm.
[0157] <Examples 2 to 19 and Comparative Example 1> The same procedure as in Example 1 was carried out, except that the raw materials and amounts used were as shown in Tables 1 and 2, and the polyether siloxane was selected in the number average molecular weight range as shown in Tables 4 to 6, whereas no polyether siloxane was used in Comparative Example 1.
[0158] <Example 21> For the manufacturing process of steps 1 and 4 to 7, refer to Example 1, and select the polyether siloxane in the number average molecular weight range as shown in Table 7. The manufacturing process of steps 2 to 3 is changed as follows:
[0159] (Step 2, Preparation of Positive Electrode Slurry) 3134.63g of positive electrode active material (lithium iron phosphate), 32.5g of conductive agent (Super P), and 81.25g of adhesive PVDF are mixed for 30 minutes. Then, the resulting mixture is added to 1750g of NMP solvent and stirred for 180 minutes to disperse it uniformly. Finally, 1.63g of polyether siloxane prepared in step 1 is added, and then stirred thoroughly for 60 minutes to form a uniform positive electrode slurry 1.
[0160] 3131.38g of positive electrode active material (lithium iron phosphate), 32.5g of conductive agent (Super P), and 81.25g of adhesive PVDF are mixed for 30 minutes. Then, the resulting mixture is added to 1750g of NMP solvent and stirred for 180 minutes to disperse it uniformly. Finally, 14.63g of polyether siloxane prepared in step 1 is added, and then stirred thoroughly for 60 minutes to form a uniform positive electrode slurry 2.
[0161] (Step 3, Manufacturing the Positive Plate) In step 2, the positive electrode slurry 1 is applied to the surface of the positive electrode current collector aluminum foil, and after drying, the positive electrode slurry 2 is applied to the surface of the dried slurry 1, and the coating thickness of the positive electrode slurry 1 and the positive electrode slurry 2 is kept the same. A series of positive electrode plate performance tests (mainly testing whether the plate breaks or not, refer to the positive electrode plate breaking length test method described in this specification, when no break occurs, the maximum coating weight is the maximum coating weight per unit area) showed that the total unit area coating weight was 31 mg / cm 2 It was found to be the case.
[0162] <Example 20> The difference from Example 21 is that the positive electrode slurry 1 does not contain polyether siloxane, and other manufacturing processes are similar to those of Example 21. For specific process parameters, see Tables 1 and 3. For polyether siloxane, select the number average molecular weight range as shown in Table 7.
[0163] <Examples 22 to 26> The manufacturing process is similar to that of Example 21, except that the raw materials and amounts used are as shown in Tables 1 and 3, and the polyether siloxane has a number average molecular weight range as shown in Table 8.
[0164] In the present application, in all the positive electrode plates in the examples and comparative examples, the positive electrode slurry is applied to both surfaces of the positive electrode current collector, that is, double-sided application.
[0165] See Tables 1 to 3 for the materials and amounts used in the preparation of Examples 1 to 26. [Table 1] [Table 2]
[0166] In the preparation of the positive electrode slurry, 32.5 g of the conductive agent Super P, 81.25 g of the adhesive PVDF, and 1750 g of the solvent NMP were used in each of Example 1 and Examples 13 to 19. In the preparation of the positive electrode slurry, the materials and amounts used in Examples 1 to 12 were the same as those in Example 1. [Table 3]
[0167] IV. Performance evaluation of positive electrode slurry and positive electrode plate <Slurry parameter testing> 1. Stability of the cathode slurry The stability of the positive electrode slurry was evaluated by the following method: The stability factor of the cathode slurry is denoted as V, where V=(V2-V1) / V1, where: V1 is the initial viscosity of the fresh cathode slurry; V2 is the viscosity of the fresh cathode slurry 48 hours after it is prepared.
[0168] The viscosity of the fresh positive electrode slurry and that after standing for 48 hours are measured at room temperature (20 to 35°C) using a DVESLVTJ0 viscometer (manufacturer: Brookfield). If V≦6, the slurry viscosity is determined to be stable, and if V>6, the slurry viscosity is determined to be unstable.
[0169] 2. Weight ratio of lithium element to silicon element in the positive electrode slurry The test methods for the weight ratio of silicon element to lithium element in the positive electrode slurry and the weight ratio of polyether siloxane to positive electrode active material in the positive electrode slurry are as follows.
[0170] This test was performed using the Thermo Fisher Scientific ICAP7400 instrument. Take a certain weight of the above slurry, dry it, perform an ICP-OES (Inductively Coupled Plasma Optical Emission Spectrometer) test on the obtained dry powder to obtain the weight ratio of silicon element to lithium element in the positive electrode slurry, and further estimate the weight ratio of polyether siloxane to positive electrode active material in the slurry based on the weight ratio of the silicon element to the lithium element.
[0171] The weight ratio of silicon element to lithium element in the positive electrode slurry and the weight ratio of polyether siloxane to positive electrode active material in the positive electrode slurry correspond to the weight ratio of silicon element to lithium element in the positive electrode plate and the weight ratio of polyether siloxane to positive electrode active material in the positive electrode plate.
[0172] <Test of Positive Electrode Plate Parameters> 1. Test of Positive Electrode Plate Breaking Length Determine the flexibility of the electrode plate by folding the electrode plate in half and roller pressing it. That is, along the direction perpendicular to the machine direction (TD), measure a 10 cm × 5 cm cold-pressed electrode plate, fold it in half, and roller press it three times with a 2 kg hand roller, and inspect the breaking length L of the electrode plate.
[0173] Judge the flexibility level based on the following method. When L = 0, there is a fold but light does not pass through, and the flexibility of the electrode plate is grade one. When 0 < L ≤ 2 mm, the light transmittance is weak, and the flexibility of the electrode plate is grade two. When 2 mm < L ≤ 10 mm, it is defined that the light transmittance is strong, and the flexibility is grade three. When 10 mm < L ≤ 20 mm, it is defined that it is slightly broken, and the flexibility is grade four. When L > 20 mm, it is defined that it is broken, and the flexibility is grade five.
[0174] 2. Test of Positive Electrode Slurry Adhesion Improvement Rate Evaluate the adhesion improvement rate of the positive electrode plate by the following method. The adhesion improvement rate of the positive electrode plate is denoted as S, and S = (S2 - S1) / S1 × 100%, where S2 is the adhesion between the positive electrode film layer and the positive electrode current collector of the positive electrode plate of this application. S1 is the adhesion between the positive electrode film layer of the positive electrode plate not containing the polyethersiloxane and the positive electrode current collector, where The positive electrode plate used when measuring S1 is the same as the positive electrode plate used when measuring S2, and the only difference is that the positive electrode plate used when measuring S1 does not contain the polyether siloxane, whereas the positive electrode plate used when measuring S2 contains the polyether siloxane.
[0175] The 2Kg pressure roller used in this test was purchased from Guangdong Iris Technology Co., Ltd., with a roller width of 45mm, a roller diameter of 83mm, a coating rubber thickness of 6mm, and a coating rubber hardness of HS80±5.
[0176] This test uses a tensile machine, model number 336, purchased from INSTRON, USA.
[0177] The measurement method for S1 and S2 is as follows.
[0178] The test plate is weighed along the direction perpendicular to the machine direction (TD), a sample with a size of 20 mm (width) x 100-160 mm (length) is cut out, and a special double-sided tape is attached to a steel plate, the size of the tape being 20 mm (width) x 90-150 mm (length). After the cut plate sample is attached to the double-sided tape, it is rolled three times in the same direction with a 2 kg pressure roller. The adhesive strength of the plate is tested with a tensile machine, and the plate without the polyether siloxane has an adhesive strength of S1, and the plate with the polyether siloxane has an adhesive strength of S2.
[0179] 3.Resistance drop rate of positive plate The resistance drop rate of the positive plate is expressed as Ω, and is expressed as Ω=(Ω1-Ω2) / Ω1×100%, where: Ω2 is the resistance of the positive plate of the present application; Ω1 is the resistance of the positive plate without polyethersiloxane, Here, the positive electrode plate used in measuring Ω1 has the same characteristics as the positive electrode plate used in measuring Ω2, except that it does not contain polyether siloxane.
[0180] The measurement method for Ω2 and Ω1 is as follows.
[0181] This test uses a film resistance meter with model number BER1100, purchased from Xiamen Yuan Neng Technology Co., Ltd.
[0182] Take a plate with an area of 4cm x 25cm (longitudinal) along the mechanical tension (MD) direction, place the current collector of the test plate in the middle of the probe, press the operation button in the software first, then press the switch valve down, after 15 seconds, a data will be automatically collected, and when it changes to another point, the test method is as above, and the test is continued until 20 points have been tested, and the resistances of the 20 points obtained respectively are averaged to obtain the values of Ω2 and Ω1 respectively.
[0183] 4. Maximum application weight test per unit area A blank aluminum foil and a positive plate that had been dried during the coating process (both sides of the positive electrode current collector of this positive plate had a coating) were prepared. The area of the positive plate was 1540.25 mm 2 The coating weight per unit area is obtained by trimming 15 small discs from each of the small discs, subtracting the average mass of the small blank aluminum foil discs from the average mass of the small discs, and dividing the result by 2. The "single side" refers to coating only on one surface of the current collector, and is not the same concept as the number of "sublayers" described in this application. The maximum coating weight per unit area in the table refers to the weight on one side.
[0184] All coating weight data in the table examples of this application refer to maximum coating weight data per unit area on one side, and both plate performance and battery performance are measured at maximum coating weight.
[0185] The maximum coating weight per unit area refers to the maximum coating weight when the electrode plate is maintained without cracking or breaking through a positive electrode plate breaking length test during and after coating of the electrode plate.
[0186] 5. The ratio of silicon content between the two sublayers in the positive electrode film layer The silicon content in the two sublayers of the positive electrode membrane is obtained by cross-sectional ion milling and EDS examination and compared.
[0187] <Battery-related performance tests> 1.Energy density measurement The batteries manufactured in the examples and comparative examples are weighed, the mass of the whole battery is obtained, the capacity of the battery is formed, the battery is left at 25°C for 10 minutes, then charged at 0.33C until it reaches 100% SOC, depolarized with a small current, left at rest for 10 minutes, then discharged at 0.33C until it reaches 0% SOC, the capacity obtained is the 0.33C capacity of the battery. The battery is left at rest for 30 minutes, then charged to 100% SOC, then left at rest for 30 minutes, then discharged at a constant current of 0.01C for 30 minutes, the voltage has a stable process, this stable value is the charge and discharge plateau, that is, the plateau voltage is obtained, and finally, the weight energy density of the battery is calculated, that is, the battery weight energy density = battery capacity x discharge plateau voltage / weight of the whole battery, the basic unit is Wh / kg (watt-hours / kilogram).
[0188] 2. Measurement of Direct Current Resistance (DCR) The capacity test is performed on the battery at 25℃, and the capacity test method is as described above. Then, charge the battery at a constant voltage of 0.05C, leave it for 60min, discharge it at 0.33C until it reaches 50% SOC, leave it for 60min, discharge it at 0.33C until it reaches 20% SOC, leave it for 60min, discharge it at 0.33C until it reaches 0% SOC, test the open circuit voltage at 0% SOC, and compile the DCR data for 30s.
[0189] For the measurement results, please refer to Tables 4 to 7, where " / " in the tables represents that the item was not present, not added, or not detected.
[0190] In Tables 4 to 7, "(I) / (II) / (III) / (IV)" represents the molar amount of structural unit (I) / the molar amount of structural unit (II) / the molar amount of structural unit (3) / the molar amount of structural unit (IV), where the molar amount of structural unit (I) corresponds to the molar amount of precursor 1 in each Example, the molar amount of structural unit (II) corresponds to the molar amount of precursor 2 in each Example, the molar amount of structural unit (3) corresponds to the molar amount of precursor 3 in each Example, and the molar amount of structural unit (IV) corresponds to the molar amount of the silane coupling agent in each Example.
[0191] [Table 4]
[0192] (Data Analysis) As can be seen from Table 4, compared with Comparative Example 1, after adding polyether siloxane to the positive electrode slurry corresponding to the Example, the maximum coating weight per unit area was increased by 36.4%, the energy density was increased by 6.5%, the DCR was significantly decreased, and the battery performance was significantly improved.
[0193] [Table 5-1] [Table 5-2]
[0194] (Data Analysis) As can be seen from Table 5, the molecular weight of polyethersiloxane affects the coating weight per unit area and the battery energy density. When the molecular weight of polyethersiloxane is <1w (for example, Example 6), the stability of the positive electrode slurry is low, the physical gelation phenomenon is easy to occur, the positive electrode plate is torn, the plate breakage length of the positive electrode plate is long, and the energy density of the corresponding battery is low; when the molecular weight of polyethersiloxane is >7w (for example, Example 7), the polyethersiloxane is easy to crosslink, so the stability of the corresponding positive electrode slurry is low, the positive electrode plate resistance is large, and the DCR of the corresponding battery is large.
[0195] [Table 6-1] [Table 6-2]
[0196] (Data Analysis) As can be seen from Table 6, when the weight ratio of polyether siloxane to the positive electrode active material is less than 0.0005 (for example, Example 18), the maximum coating weight of the positive electrode plate is 22 mg / cm 2 The corresponding battery energy density is low; when the coating weight exceeds this value, the positive plate is severely torn; when the weight ratio of polyethersiloxane to positive active material is >0.03 (e.g., Example 19), the film resistance of the positive plate is deteriorated, and the battery resistance DCR is high.
[0197] [Table 7-1] [Table 7-2] [Table 7-3]
[0198] (Data Analysis) As can be seen from Table 7, the maximum coating weight per unit area of the positive electrode plate corresponding to Example 1 is 30 mg / cm 2 , which is lower than those of Examples 20 to 26, and the corresponding energy densities are also lower than those of Examples 20 to 26. Furthermore, as can be seen by comparing Examples 20 to 26, when the weight content of silicon in the sublayer closest to the positive current collector is >60 (Example 26) relative to the weight content of silicon in the sublayer furthest from the positive current collector, the excessive distribution of polyether siloxane in the sublayer closest to the positive current collector affects the stability of the slurry and the membrane resistance of the plate, and the corresponding battery DCR increases.
[0199] It should be noted that the present application is not limited to the above embodiment. The above embodiment is merely an example, and any embodiment having substantially the same configuration as the technical idea and having similar actions and effects within the scope of the technical proposal of the present application is included in the technical scope of the present application. In addition, various modifications that a person skilled in the art can conceive of to the embodiment are implemented within the scope of the gist of the present application, and other forms constructed by combining some of the components in the embodiment are also included in the scope of the present application.
Claims
1. a positive electrode slurry comprising a positive electrode active material and a polyether siloxane; The polyether siloxane comprises at least [Formula 1] At least one of (I) and (II), (III) and (IV) in the structural unit Where: D is a methyl group or an ethyl group; A is hydrogen, halogen or a halogenated alkyl group; B is a hydroxyl group, R, OR, or ROR', where R, R' are each independently a straight or branched chain alkyl group containing 1 to 8 carbons; E is a phenyl group, an alkyl-substituted phenyl group, an etherified phenyl group, or a halogenated phenyl group.
2. The positive electrode slurry of claim 1, wherein the halogen is fluorine, chlorine or bromine.
3. The positive electrode slurry of claim 1, wherein A is hydrogen or a fluoromethyl group, B is a methyl group, an ethyl group or an ethoxymethyl group, and E is a phenyl group or a fluorophenyl group.
4. The positive electrode slurry according to any one of claims 1 to 3, wherein the polyether siloxane has a number average molecular weight in the range of 10,000 to 60,000.
5. The positive electrode slurry according to claim 4, wherein the number average molecular weight range of the polyether siloxane is 20,000 to 60,000.
6. The positive electrode slurry according to any one of claims 1 to 5, wherein the molar ratio of the structural unit (I) is 0 to 75 mol%, the molar ratio of the structural unit (II) is 0 to 70 mol%, the molar ratio of the structural unit (III) is 5 to 65 mol%, and the molar ratio of the structural unit (IV) is 4 to 10 mol%, based on the total molar amount of the structural units (I) to (IV), and wherein the molar ratios of the structural units (I) and (II) are not simultaneously zero.
7. The positive electrode slurry according to any one of claims 1 to 6, wherein a weight ratio of the polyether siloxane to the positive electrode active material is 0.0005 to 0.
030.
8. The positive electrode slurry according to claim 7, wherein the weight ratio of the polyether siloxane to the positive electrode active material is 0.001 to 0.
02.
9. The positive electrode slurry according to claim 8, wherein the weight ratio of the polyether siloxane to the positive electrode active material is 0.001 to 0.
01.
10. The positive electrode slurry according to claim 9, wherein the weight ratio of the polyether siloxane to the positive electrode active material is 0.001 to 0.
006.
11. The positive electrode slurry according to any one of claims 1 to 10, wherein the positive electrode active material is selected from at least one of lithium iron phosphate, lithium manganese iron phosphate, lithium manganate, lithium cobalt oxide, lithium nickel cobalt manganate, lithium nickel cobalt aluminate, lithium nickel oxide, or a mixture thereof.
12. the stability factor of the cathode slurry is 0<V≦6, optionally 0<V≦4; Here, V=(V2-V1) / V1×100%. V1 is the initial viscosity of the positive electrode slurry; V2 is the viscosity of the cathode slurry 48 hours after it is prepared, where The positive electrode slurry according to any one of claims 1 to 11, wherein the positive electrode slurry used when measuring V1 and the positive electrode slurry used when measuring V2 are positive electrode slurries of the same lot.
13. A positive electrode plate, A positive electrode current collector; and a positive electrode film layer located on at least one surface of the positive electrode current collector, the positive electrode film layer being manufactured from the positive electrode slurry according to any one of claims 1 to 12, and the positive electrode film layer has a mass range of 13 to 45 mg / cm in the electrode plate per unit area. 2 wherein the mass is the mass of a positive electrode film layer on one side of the plate.
14. The positive electrode plate according to claim 13, wherein the positive electrode film layer has a mass per unit area of the plate in the range of 20 to 43 mg / cm 2 .
15. The positive electrode plate according to claim 14, wherein the positive electrode film layer has a mass per unit area of the plate in the range of 22 to 33 mg / cm 2 .
16. The positive electrode plate according to claim 15, wherein the positive electrode film layer has a mass per unit area of the plate in the range of 25 to 31 mg / cm 2 .
17. The positive electrode plate according to any one of claims 13 to 16, wherein the weight ratio range of lithium element to silicon element in the positive electrode plate is 60 to 3875.
18. The positive electrode plate according to claim 17, wherein the weight ratio range of lithium element to silicon element in the positive electrode plate is 60 to 1950.
19. The positive electrode plate according to claim 18, wherein the weight ratio range of lithium element to silicon element in the positive electrode plate is 90 to 1950.
20. The positive electrode plate according to claim 19, wherein the weight ratio range of lithium element to silicon element in the positive electrode plate is 380 to 1950.
21. 21. The positive electrode plate according to claim 17, wherein the positive electrode film layer comprises two sublayers parallel to the positive electrode current collector and stacked on top of each other, wherein the weight content of silicon in the sublayer closest to the positive electrode current collector ranges from 0 to 60 relative to the weight content of silicon in the sublayer furthest from the positive electrode current collector.
22. The positive electrode plate of claim 21, wherein the weight content of silicon in the sublayer closest to the positive electrode collector is 0.1 to 30 times the weight content of silicon in the sublayer furthest from the positive electrode collector.
23. The positive electrode plate of claim 22, wherein the weight content of silicon in the sublayer closest to the positive electrode collector is 0.1 to 9 relative to the weight content of silicon in the sublayer furthest from the positive electrode collector.
24. When determining the flexibility of a plate by folding the plate in half and pressing it with a roller, The plate break length of the positive plate is 0; or The positive electrode plate according to any one of claims 13 to 23, wherein the positive electrode plate has a plate break length greater than 0 and less than or equal to 2 mm.
25. The range of the adhesive strength improvement rate S of the positive electrode plate is 2 to 50%, Here, S=(S2-S1) / S1×100%. S2 is the adhesive strength between the positive electrode film layer of the positive electrode plate and the positive electrode current collector; S1 is the adhesion between the positive electrode film layer of the positive electrode plate not containing the polyether siloxane and the positive electrode current collector, where The positive electrode plate used when measuring S1 is the same as the positive electrode plate used when measuring S2, and the positive electrode plate used when measuring S1 does not contain the polyether siloxane, whereas the positive electrode plate used when measuring S2 contains the polyether siloxane. The positive electrode plate according to any one of claims 13 to 24, which is different only in that.
26. A positive electrode plate as described in claim 25, wherein the range of the adhesive strength improvement rate S of the positive electrode plate is 10 to 20%.
27. The range of the resistance reduction rate Ω of the positive electrode film in the positive electrode plate is 0 to 18%, Here, Ω = (Ω1 - Ω2) / Ω1 x 100%, Ω2 is the resistance of the positive electrode film, Ω1 is the resistance of the positive electrode film that does not contain the polyethersiloxane; Here, the positive electrode film used when measuring Ω1 is the same as the positive electrode film used when measuring Ω2, and the positive electrode film used when measuring Ω1 does not contain the polyether siloxane, whereas the positive electrode film used when measuring Ω2 contains the polyether siloxane. The positive electrode plate according to any one of claims 13 to 26, wherein the positive electrode plate is different only in that the positive electrode film used when measuring Ω1 does not contain the polyether siloxane.
28. The positive electrode plate according to claim 27, wherein the range of the resistance reduction rate Ω of the positive electrode film in the positive electrode plate is 6 to 15%.
29. A secondary battery comprising the positive electrode plate according to any one of claims 13 to 28, or the positive electrode plate obtained with the positive electrode slurry according to any one of claims 1 to 12.
Citation Information
Patent Citations
Siloxane polymer for bonding self-repairing lithium battery electrode and preparation method of siloxane polymer
CN112094413A
Secondary battery
CN113644275A
Aqueous polyvinylidene fluoride composition
JP2012528466A
Nonaqueous electrolyte secondary battery
JP2014078341A
Polysiloxane binder for lithium ion battery electrodes
US20120153219A1