Advanced heterogeneous fibrous monolithic wafer-like silicon anodes
A monolithic heterogeneous fibrous silicon anode with an artificial SEI layer and tailored structural features addresses the challenges of uncontrolled expansion in silicon-based anodes, enhancing energy density and cycle life while enabling rapid charging.
Patent Information
- Application Number
- JP2023516478
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-04-09
- Filing Date
- 2021-09-16
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2041-09-16
AI Technical Summary
Existing silicon-based anodes in lithium-ion batteries suffer from uncontrolled volumetric expansion during charge/discharge cycles, leading to structural instability, irreversible capacity loss, and safety issues due to rapid lithium plating, which limits their cycle life and charging rate acceptance.
A heterogeneous fibrous silicon anode with a monolithic structure and tailored weak and stiff points is developed, featuring an artificial SEI layer formed during ex-situ prelithiation, allowing for controlled volume expansion and efficient lithium distribution, thereby maintaining structural integrity and enhancing charging rates.
The anode achieves high coulombic efficiency, gravimetric and volumetric energy density, and improved cycle life, enabling fast charging capabilities and reducing irreversible capacity loss, thus addressing the limitations of traditional silicon-based anodes.
Smart Images

Figure 0007595753000001 
Figure 0007595753000002 
Figure 0007595753000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an advanced ex-situ (before battery assembly) pre-lithiated anode (body) based on group IV semiconductors according to claim 1. The silicon anode of the present invention as an alkaline ion battery, preferably a lithium ion secondary battery, exhibits a free-standing and / or heterogeneous fibrous and / or wafer-like and / or monolithic structure with a high degree of structural order. The present invention offers the possibility to design thick silicon electrodes featuring weak and stiff points tailored to their structure in order to buffer the volume expansion during charge / discharge cycles in a predicted way, overcoming the uncontrolled volume expansion in state-of-the-art silicon anodes. [Background technology]
[0002] A definition of the invention is provided for each embodiment of the anode of the invention after "Objectives of the Invention."
[0003] From US patent application 20180331341A1 a spun silicon-based mat is known which is made from a mixture of a liquid silicon precursor and a polymer, whereby lithium is introduced into the resulting nanotubular silicon matrix of the spun mat.
[0004] The rapid growth of the e-mobility sector along with portable smart electronic devices is driving the demand for advanced secondary batteries with higher energy and high charge rate acceptance addressing real challenges arising from users of BEV battery-powered electric vehicles, which demand a much larger operating range on a single charge, and the shortest possible charging time, defined as 30 minutes or less from 15% SoC (State of Charge) to 100% SoC, with negligible adverse impact on cycle life, defined as SoH (State of Health). - SoH indicates the ratio of the current maximum usable capacity to the nominal capacity.
[0005] Lithium-ion batteries with long cycle life and high charge rate acceptance are at least in direct conflict with current types of alkali-ion anodes, which are primarily based on the Li+ intercalation reaction into graphite. The slow diffusion of Li+ upon intercalation into graphite and the presence of a concentration polarization gradient impede the rate of Li+ transport from the electrolyte to the anode, further restricting access to Li+. This phenomenon then exceeds the Li diffusion intercalation rate, inducing the accumulation of more charge carriers at the anode surface, driving the anode potential below 0 V. This is the region where lithium plating is kinetically more favorable than the Li+ intercalation reaction, and because the operating potential of graphite is close to 0.1 V, deposition of metallic Li occurs, with subsequent battery degradation and safety issues. Recently, the growing field of portable electronic devices has coincided with a trend towards "small" and "compact" energy carriers, defined herein as batteries with a desirable high volumetric energy density (>750 Wh / l), and "lightweight" as batteries with a desirable high gravimetric energy density (>300 Wh / kg), which is met by the anode of the present invention. There is a discrepancy in understanding the definition of the term "high energy battery". The most desirable requirement for a battery is to have a high gravimetric energy in Wh / kg. However, in reality, its opposite, volumetric capacity Wh / l, is more demanding due to the fact that there is available space: for example, providing the available space / volume to insert the battery into a smartphone, notebook, or electric vehicle platform, the most limiting factor is the need for a battery with both high volumetric and gravimetric energy density, defined herein as a compact and lightweight battery.
[0006] Silicon is one of the most promising types of anode for post-lithium batteries, with theoretical room temperature gravimetric / volumetric capacities of 3579 mAh / g and 8334 mAh / cm in the delithiated (discharged) state. 3 and lithium Li3.75Si (charged) state 1857mAh / g, 2193mAh / cm 3On the other hand, the average discharge potential is Li / Li + Compared to the most common types of anodes, graphite is defined herein as the state of the art anode used in commercial lithium-ion batteries, with gravimetric (graphite) 372 mAh / g vs. (silicon) 3579 mAh / g and volumetric (graphite) 837 mAh / cm 3 (silicon) 8334mAh / cm 3 It is defined as capacity.
[0007] The volumetric capacity of a lithium metal anode in a fully discharged state is 0 mAh / cm 3 , so all the lithium is stripped off the Cu foil etc. during discharge and moves towards the cathode, so that fully charged lithium has 2061 mAh / cm compared to silicon. 3 and silicon has a capacity of 8334mAh / cm when fully discharged. 3 When fully charged, it has a capacity of 2193mAh / cm 3 These figures therefore disclose the advantage of using a lithiated silicon anode instead of an LMA (lithium metal anode), since the theoretical volumetric variation of lithium metal averages 0.205 mAh / cm per micron of thickness. 2 The LMA anode is therefore dimensionally unstable, so that the thickness of the lithium metal foil decreases when it is discharged (stripped off) and increases when it is charged (plated). In comparison with graphite, the most commonly used anode material, all volume variations during cycling of the anode of the present invention are compensated within the internal voids / porosity of the anode (about 30% of the volume), and the thickness of the anode changes only slightly.
[0008] LMA foil is a hostless anode. Therefore, to charge it, there are large irreversible losses due to the formation of the SEI (solid electrolyte interface), but the most important factor is the defragmentation of lithium and the subsequent expansion of the SEI layer. This is only 50% even with advanced electrolytes and gradually increases with each cycle (lithium consumption). Thus, the theoretical minimum volume variation of LMA is 150% against 276% for silicon in the best scenario, but the practical situation is different. LMA (foil) loses Li during cycling. + It is desirable to use in excess because the SEI that consumes Li accumulates. + When it is consumed, the battery is dead.
[0009] A commonly used overage is 200% to account for the cycle life of a realistic Li-ion battery using LMA, thus exceeding the theoretical volumetric capacity of silicon by 2193 mAh / cm. 3 Comparing this to the best possible scenario of 100% excess LMA foil, there is a factor of two reduction, resulting in a theoretical capacity of 1031 mAh / cm 3 So the excess lithium in the anode / cell compartment represents its own weight / volume, and the excess in the battery is mainly to compensate for its consumption and extend cycle life. Here, a realistic LMA anode would have a capacity of 1031mAh / cm 3 and graphite volumetric capacity of 837mAh / cm 3 When comparing the LMA with an additional 50% expansion contribution from the SEI, it is clear that using claims such as "lithium metal is the holy grail of batteries" shows a lack of understanding of fundamental electrochemistry and cell-battery-module-pack-systems.
[0010] A key element of a solid-state battery with LMA anodes is the need to use a specific device capable of applying uniaxial pressure to the battery module. This is because LMA is dimensionally unstable, so a lithium metal foil needs to be pressed against the solid electrolyte to exchange ions, resulting in an increase in its own weight / volume. However, this time it is not from the cell components, but from additional auxiliary components associated with the battery module or pack, stacking them to distribute forces such as 10 MPA evenly over the surface. Thus, in a realistic battery design, the energy content is further reduced by about 18%, and also significant safety concerns arise due to the presence of pre-compressed battery modules, for example in electric vehicles, which may release the extreme energy present in such batteries in the event of a crash event.
[0011] In the scope of the previous analysis, the present invention's ex situ pre-lithiated heterogeneous fibrous silicon anode with mixed ionic-electronic conductivity, preferably with an artificial SEI layer, is a new viable solution for next generation batteries, capable of accepting high charging rates and realizing ultra-compact batteries with lithium-rich LLS cathodes with capacities exceeding 1200 Wh / l and 350 Wh / kg.
[0012] The high density of silicon gives it 10 times the volumetric energy content of graphite anodes, but at the cost of high volume expansion upon lithiation defined as (graphite) 11.2% and (silicon) 276%; the challenge is clearly the nature of silicon expansion. (See ELSEVIER Journal of Industrial and Engineering Chemistry, Journal Volume: 74, Journal Issue: 25; Journal ID: ISSN1226-086X, page numbers 216-222). Since this is a highly anisotropic process, the point of interaction / input of electrons / ions into / and reaction with silicon, and the subsequent alloying reaction, is different from that of conventional intercalation type anodes, graphite.
[0013] As the second most abundant element in the Earth's crust after oxygen (~28% by mass), silicon's low cost, combined with Si's high volume / weight energy, gives it a significant advantage for use in batteries, the next generation of energy carriers. Si has an energy density of 1.6x10 -3 Conductivity in S / m is 1.9x10 -14 cm 2 / s Li + Although it is a group IV semiconductor with a diffusivity, Li in Si + The diffusion proceeds at different rates depending on the crystal orientation of the Si, so the direction is 3D. <100> and <111> The critical force of orientation (1) is <110> This is about 40% and 15% lower than <110> This means that the two materials have favorable diffusion rates in the opposite direction. This mismatch in diffusion would therefore result in rapid capacity fade due to non-uniform anisotropic expansion / contraction of silicon at the particle level and subsequently in the electrode. This would result in different rates of lithiation within the internal electrode structure, with the electronic conduction pathway being provided primarily by physical interactions between the active Si, the binder, and the conductive additives. Li + The location of the Si particles within the current anode structure is not precise as the Si anode cycle proceeds through repeatable charge / discharge cycles, since the points of Si interaction with the Si and electrons define the reaction rate. Thus, each contraction / expansion in subsequent cycles redistributes the internal ionic / electronic conduction paths due to the presence of the flexible polymer binder. Thus, the silicon-electron interaction points are constantly changing due to the complex nature of the slurry-based Si anode. The active Si particles need to interact with the binder and conductive additives to create the conduction paths for electrons and ions.
[0014] Current technical solutions for silicon-based anodes are based on using Si as a minor additive to existing slurry-based anodes, where the internal porosity of the anode is used to compensate for volumetric variations during cycling. Due to existing limitations resulting from the preferential use of slurry-based anodes, such volumetric changes are only partially compensated for by the internal porosity of the anode, where most of the pressure increase in the anode is converted into mechanical forces. This further destabilizes the structural bond between Si-graphite-binder-conductive additives. In conventional silicon-based lithium-ion batteries, the electronic conduction path is provided by the interaction of silicon with billions of conductive nanoparticles that transport electrons to and from the electrode. There is no steady-state Li-Si alloy point, as morphological changes occur in silicon-based anodes. Therefore, amorphous Li x The direction in which lithium enters the silicon crystal structure while forming the Si phase and the presence of local Si anisotropy lead to further deformation, followed by a redistribution of mechanical forces, which ultimately leads to cracking and delamination of the Si structure. Thus, the Si surface is exposed to the electrolyte and is in direct contact with the available electrolyte and Li. + This consumes more current to form a new SEI layer, which causes irreversible capacity loss and impedance gain, and generates excessive heat during cycling, making the rapid charge rate the most limiting factor (solid electrolyte interlayer). Summary of the Invention [Problem to be solved by the invention]
[0015] In order to solve the above problems, the objective of the present invention is to provide a negative electrode, preferably a heterogeneous fibrous lithiated silicon anode exhibiting hierarchical electrode porosity, for an alkali ion battery exhibiting significantly improved cycle life, high coulombic efficiency, gravimetric and volumetric energy density, activity utilization level, and to provide an innovative manufacturing method, preferably characterized as solvent-free and / or binder-free and / or drying-free and / or slurry mixing and degassing-free and / or slurry coating-free and / or anode current collector foil to tab welding-free and / or calendar-free (and preparation process), which leads to high energy, cost-effective and environmentally beneficial effects of such advanced silicon anodes. The high charge rate acceptance of the heterogeneous fibrous, preferably anisotropically lithiated (preferably n-type) silicon wafer anode, defined at the cell level as full charging of the cell from 15% SoC to 100% SoC, preferably in 12 minutes or less, will have a global impact on the alkali ion battery market. (Monolithic) wafer may refer to free-standing and / or heterogeneous fibrous and / or silicon (or group IV semiconductor in general) based anodes and / or integrated anode bodies made from heterogeneous fibrous silicon materials, preferably with tailored hierarchical open porosity. [Means for solving the problem]
[0016] Self-supporting can be understood as a structural property in that such an anode can maintain its structure without external support, such as an external backbone, which serves only the purpose of structural rigidity and takes away space within the anode that could otherwise be used for active material, in the same way that it is expected from a wafer.
[0017] The term "heterogeneous fibrous" fibers refers to possible variations in fiber length and / or diameter.
[0018] Monolithic can refer to the shape and / or structure of the anode active material made from layers of fibers by fusing the layers of fibers together in the manner of the present invention, resulting in a unified body of the anode active material.
[0019] This problem is solved according to the invention by an anode as claimed in claim 1.
[0020] The negative electrodes of the present invention may be used in alkaline ion rechargeable batteries and include the electrochemically active material of the anode. the active material is selected from Group IV semiconductors, and / or the active material is provided as a heterogeneous fibrous and / or wafer-like and / or free-standing and / or monolithic anode body, and / or the anode body comprises at least two (individual / discrete) layers of aligned and / or stacked and / or entangled fibers, and / or the at least two layers are arranged parallel on top of each other, and / or the layers are interconnected at a plurality of individual interconnection sites, preferably interconnection points, via metallic bonds, and / or the metallic bonds comprise or consist of a Li-Group IV semiconductor alloy and / or lithium or a mixture of the two, and / or the individual interconnection sites are distributed throughout the anode body, preferably distributed discretely throughout the area of the layers, more preferably throughout the area of the layers, and / or the metallic bonds extend in an out-of-plane direction relative to the individual layers, providing spacers between the layers, and the anode body, and in particular the layers thereof, is preferably non-uniformly lithiated with unlithiated, under-lithiated and stoichiometrically lithiated regions.
[0021] The electrode of the present invention also has a negative Li + It may be described as a host-type alloyed electrode.
[0022] The present invention may also refer to an anode comprising at least two (individual / discrete) layers of aligned and / or stacked and / or entangled fibers, at least two layers being arranged parallel on top of each other, the layers being interconnected via metallic bonds at a plurality of individual interconnection sites, preferably interconnection points, the metallic bonds comprising or consisting of Li-IV group semiconductor alloys and / or lithium or a mixture of the two, the metallic bonds extending in the out-of-plane direction relative to the individual layers, being spacers between the layers, the gaps between the layers formed by said spaces can be filled with silicon-lithium alloy formed during charging / lithiation of the anode, the anode comprising an SEI layer, the volume / expansion of which matches the volume of the anode in the maximum lithiation state. Such an SEI layer may be formed by overlithiation of the anode followed by the formation of an artificial SEI layer with dopants or electrolyte, which is formed by the excess lithium (preferably Li 21 Si5 to Li 15 Although the silicon-lithium alloy consumes a large amount of silicon (up to about 10 ...
[0023] Within the scope of our invention, we apply an innovative method for the fabrication of highly ordered ex situ pre-lithiated silicon structures, monolithic heterogeneous fibrous anodes that allow fine-tuning the content of lithium in the silicon anode active material to match lithium-free or lithiated cathodes. All subsequent processes are applied at the wafer (anode active material body) level, so that all irreversible losses due to SEI formation are internally compensated by the ex situ method.
[0024] The non-uniformly distributed lithiation or anisotropic lithiation of a layer includes unlithiated regions, underlithiated regions, and stoichiometrically lithiated regions.
[0025] Spot fusion, which may also be referred to synonymously as interconnect sites, refers to metallic bonds from the Li-IV semiconductor alloy and / or lithium or a mixture of the two, where the layers are interconnected at multiple discrete points by metallic bonds, with the discrete points of interconnection spanning the entire anode body and therefore the entire area of the layers.
[0026] According to the present invention, discrete can mean separated from one another, introduced separately, having spaces between them, or a combination thereof.
[0027] The interconnect sites are located between the layers and can extend into the layers to improve fixation.
[0028] Spot fusion at a specific location is Li x S (y) During cycling, the Li in the anode is controlled by how it redistributes in the anode. x S (y) This can further induce the subsequent distribution of .theta.. Thus dispersing the mechanical stress resulting from the charge / discharge cycles of lithiation and delithiation.
[0029] The "anisotropy" is due to the fact that during further charge / discharge cycles, x S (y) "The question is how can we predict and direct the deposition of Li in the anode as a thermal stabilizer? It's like the chassis of a modern car, where structural engineers insert weak spots to direct how the chassis deforms in the event of an accident and absorbs the energy from the crash. Spot fusion can do the same thing by inserting weak spots into the structurally rigid LixSi anode body."
[0030] The metallic bonds are preferably introduced by electrochemically induced Li fusion or by the introduction of molten lithium. The location, distribution, shape, size and number of these fusion spots are determined by the Li x S (y)This can be extracted from the analysis of the non-uniformity of the current distribution within the anode. Current analytical techniques include galvanostatic, potentiostatic, and impedance spectroscopy techniques. Additionally, the distribution of fusion spots can be derived via in situ and / or ex situ imaging techniques such as scanning electron microscopy and transmission electron microscopy, which reveal the location of metallic bonds and the presence of density gradients through elemental mapping by energy dispersive X-ray spectroscopy.
[0031] The twisting of the anode is caused by the electrolyte present in the internal void of the electrode, which causes Li + The amount of charge and activity is directly related to the accessibility of the most linear and shortest possible electronic and ionic conduction pathways established for the direct physical interaction of electrons with conductive additives such as carbon black or conductive polymers and / or their combinations. Conventional slurry-based electrodes lack the structural ordering important for efficient electronic and ionic pathways, but monolithic silicon anodes with a high degree of structural ordering are defined as hierarchical structures. It is composed of layers of aligned silicon fibers stacked in a monolithic anode structure, so that efficient pathways can be established. Monolithic silicon anodes with ordered porosity replace the traditional mediated electronic conduction pathways characteristic of slurry-based electrodes, which are based on direct physical contact between silicon, conductive agent, binder and current collector foil by the direct lithium fused fibrous low resistance heterogeneous fibrous silicon anode body of the present invention. This type of open structure allows for fast charging of the anode beyond the critical limit of existing intercalation type anodes that exists at 80% SoC.
[0032] The artificial SEI layer can be fabricated by the following steps.
[0033] The interconnected layers of Si fibers are 21It is lithiated (overlithiated) to Si5. Such lithiation can be carried out under high temperatures, preferably above 100°C, in a protective solvent, such as, for example, a linear, branched or cyclic alkane (Adv. Energy Mater. 2019, 1902116; DOI: 10.1002 / aenm.201902116). Suitable solvents may be binary or ternary mixtures of polar and non-polar solvents, more preferably, the non-polar solvent is a hydrocarbon, such as decane, and the solvent is a polar solvent, such as DEGDME diethylene glycol dimethyl ether, with a boiling point above 130°C.
[0034] The (over)lithiated Si layer is then treated with a dopant to form an artificial SEI layer, preferably at the maximum lithiation state of the Si anode. The reaction of the dopant with the lithiated anode reduces the lithium content. Li 15 The Si4 stoichiometry can be achieved by / after artificial SEI formation that is stable at room temperature. Because the SEI layer is artificially induced after lithiation of the Si anode, the aSEI layer will have fewer defects (cracks, weak spots, thickening, etc.), and there is only SEI formation at the end of the first lithiation process, and therefore no volume expansion occurs after SEI formation occurs (as in the case where the SEI is formed before or during the initial lithiation process). The protective solvent prevents the formation of a thick SEI layer during the initial stages / during lithiation.
[0035] The SEI formation can be carried out in a protective solvent, and liquid / dissolved and / or gaseous dopants such as group V pnictogens or low concentration electrolytes (e.g., As-, P-, (H)F-compounds) can alternatively or additionally be introduced, and the SEI layer can be overlithiated with Li 21 It may be introduced by reaction of Si5 with an electrolyte such as that used in the final battery. Such electrolyte may be selected, for example, from ceramic solid electrolytes, polymer electrolytes, ionic liquids, as known to those skilled in the art. The dopant and / or electrolyte may be (over)lithiated Li 21Upon contact with Si5, lithium reacts with the dopant and / or electrolyte to form a tailored (artificial) SEI layer that includes, for example, Li3P, Li3As, Li4As, and / or LiF, depending on the dopant and / or electrolyte used. 21 After consuming some of the Li from Si5, the room temperature active alloy (Li 15 The resulting artificial SEI layer experiences mixed ionic and electronic conduction properties. The amount of dopants in the Si layer is determined by the ratio of Li 21 The amount of Li present in the Si5 can be adapted to obtain the desired degree of lithiation.
[0036] This method reduces the loss of Li during the initial formation of the SEI layer, as compared to conventional lithiation of the final battery, for example by initial charging. 21 Li such as Si5 x S (y) The SEI forms when the species has a higher volume so that the volume expansion of the silicon does not cause cracking of the SEI, which is common during silicon anode operation.
[0037] A typical lithium-ion battery contains a certain amount of lithium inserted / intercalated into the NMC cathode, which means that when the battery is in a fully discharged state, all of the lithium is on the cathode side. + To transfer Li from the cathode to the anode, the anode needs to be initially charged, but during this process there is a large irreversible loss of Li. This Li is consumed by the SEI construction as the inactive part of the SEI layer, and due to the high reactivity of lithium, a thick highly resistive R SEI is formed. Furthermore, this is R ctThis typical in situ process uses only the Li present in the battery as part of the energy storage matrix. For Si anodes, lithiation is done in situ by mixing a suitable lithium precursor that can be part of a slurry or can be sprayed onto the surface of the electrode to lithiate it, followed by calendaring and activating the protective layer of the SLMP as in "2010 DOE Vehicle Technologies Program Review" PI Marina Yakovleva Co-PIDr. Yuan Gao FMC June 8, 2010 (https: / / www.energy.gov / sites / prod / files / 2014 / 03 / f11 / es011_yakovleva_2010_o.pdf). However, in situ lithiated electrodes build a protective layer over finely divided lithium metal powder introduced ex situ during battery assembly, which then needs to be activated, leading to a very expensive method.
[0038] In contrast, the preferred ex situ introduced lithium supplied from an external source a. is provided in excess, thus allowing 100% of the theoretical battery capacity to be achieved, and b. provides a uniform SEI layer with little to no cracks, weak spots, thickening, etc. The formation of the SEI layer occurs when the anode reaches its maximum expansion state (by volume), i.e., the (over)lithiated state (Li 21 This method is carried out in the Li x S (y) It is also possible to avoid inclusion of the SEI layer material within the body.
[0039] Conventional silicon-based anodes are based on intrinsic silicon with various shapes such as 0D, 1D, or more complex 3D host structures of silicon nanoparticles or micro-mesoporous 3D silicon or etched silicon anode bodies. 0D silicon particles below a critical diameter that prevents the particles from bursting during lithiation (expansion) have a protective carbon coating on their surface, more preferably carbon. This type of protective coating provides a barrier for lithium-initiated self-fusion of surrounding silicon structures with which it is in close physical contact. Conventional silicon anodes have used protective coatings based on partial oxidation of the silicon surface or carbon coatings, but these processes are applied to address the pyrophoric nature of nano-sized silicon particles and their ability to be processed as slurries using suitable solvents without significant side reactions. The presence of a barrier layer between silicon particles in a slurry-based electrode prevents lithium from efficiently propagating the self-fusion process throughout the electrode. While slurry-based silicon electrodes maintain internal electronic conduction pathways governed by physical contact between active mass particles-silicon and surrounding particles, conductive additives such as 1D shapes as CNTs and / or 0D as carbon black and / or polymer binders, our inventive heterogeneous fibrous anisotropically prelithiated monolithic silicon anodes preferably use the advantageous lithium-initiated self-fusion process of silicon to build innovative fully interconnected monolithic 3D (wafer-like) anodes. Preferably, the physical contacts mediated by conductive additives and polymer binders typical of slurry-based silicon anodes are completely eliminated by fusing lithium with cross-contacting silicon fibers and / or by (perfect) metallic bonding / joints created by artificial SEI before lithiation (Figure 13).
[0040] In one embodiment, the object of the invention is an engineered heterogeneous fibrous and / or monolithic silicon anode body with functional anisotropy represented by the introduction of specific regions (Figure 7) in the monolithic silicon body, which structurally further comprises a combination of rigid spots (fused parts of the lithiated layer) and weak spots (non-lithiated and / or partially lithiated and / or fully lithiated and / or over-lithiated parts of the layer). Together they may form an electrode superstructure designed to be able to redistribute the volumetric variations of silicon by allowing the weak regions to absorb and redistribute the volumetric variations of silicon. These regions may preferably be oriented in the plane of the electrode to accommodate the volumetric changes and redistribute them, preferably following a predetermined direction interconnecting the silicon layers, with the rigid spots preferably oriented out of the plane. The diameter of the fused spots or lines is preferably in the range of 1 to 1500 μm, more preferably in the range of 375 μm. The outer distance of the fused spots or lines is preferably in the range of 50-3000 μm, more preferably in the range of 750 μm, whereby the fused points and / or lines may be characterized by a specific geometric pattern (spiral, star, hexagon, etc.) and / or a non-uniform distribution.
[0041] The fusion spots may be provided as part of the structural integrity of the (wafer-like) stack of layers of Si fibers. Thus, the number of fusion spots may be appropriately selected to provide at least an initial support of the entire anode structure. Anisotropic lithiation may be provided by the separate lithiation process described above, since the lithiation is oriented within and / or between the provided layers, thus providing a defined plane and extension direction. The spots may also add a high degree of structural strength and partial flexibility to deal with silicon anisotropy upon cycling. Furthermore, (anisotropic) fusion spots FIG. 7, preferably anisotropically aligned Si-Li alloy patterns are provided on and within the (wafer) structure / layer structure / Si fibers, preferably with lithiated portions distributed throughout the anode body (wafer) / layer structure, while at the same time non-lithiated or lithium-deficient portions are distributed throughout the anode body (wafer) / layer structure in the first process step (see FIG. 2 for an example).
[0042] Such an arrangement may be referred to as functional anisotropy by forming Li-Si alloys with a gradient, also known as a bending modulus gradient, between the lithiation and structural spot fusion pillars. Lithiation can generally be established by print fusion methods using liquid lithium and / or its alloys and / or electrochemical lithiation and / or a combination thereof, more preferentially two-step lithiation.
[0043] Spot fusion can mean: the layers are interconnected at multiple discrete points by metallurgical bonds, and / or ○ Individual single locations and / or areas and / or lines connecting them At each interconnection point, a Li-IV semiconductor alloy and / or lithium, or a mixture of the two, is provided as the metallic bonding material; and / or ○ Individual points of interconnection are distributed throughout the anode body, so that the entire area of the layer and / or the layers are preferably spaced apart from one another by the material of the individual interconnections, and / or Metallic bonds extend out of plane with respect to the individual layers. The meaning of spot fusion goes beyond simply connecting dots and can also include lines and / or areas and / or columns, which may have the properties outlined in this patent application.
[0044] According to a preferred embodiment, the distribution or degree of lithiation within the layer varies, and the degree of lithiation of the anode body across the extension plane of the layer is similar.
[0045] According to one embodiment, the present invention is directed to a negative electrode for use in an alkali-ion rechargeable battery, the electrochemically active material of the anode being selected from group IV semiconductors. The active material may be provided as a heterogeneous fibrous and / or wafer-like and / or free-standing and / or monolithic anode body. The anode body comprises at least two layers of aligned and / or stacked and / or entangled fibers, which are spot fused by the presence of lithium at multiple discrete points of physical contact to form individual lithium group IV semiconductor alloy (e.g. LiSi alloy) bonds between the layers. Instead of or in addition to spot fusing the anode body, particularly the layers, the layers are anisotropically lithiated. Spot fusion may represent at least a part of the anisotropic lithiation, at least in one aspect of the present invention. The above-mentioned anodes may contain, at least in the charged state, an excess of lithium in the anode body that may not necessarily participate in the bonding of the layers. This additional lithium may be present, for example as a charge carrier, preferably in the individual layers. The objective of this invention is to introduce an innovative way to efficiently address volumetric variations in silicon-based anodes by introducing strategically placed weak and stiff spots, structures that work synergistically together. This can be visualized in a similar way to the structural weak spots that engineers originally placed in car chassis to absorb the impact forces during a car crash, saving lives, and converting them into mechanical deformations in the car chassis and surrounding structural components. Weak spots are sometimes called expansion / contraction zones, where the anode material can expand during lithiation (charging) and contract during delithiation (discharging).
[0046] It is a preferred object of the present invention to introduce structural and / or material anisotropy represented by changes in anode density caused by lithiation (and / or lithium alloy formation) of a heterogeneous fibrous silicon anode body (wafer) and / or electrical anisotropy represented by conductive (lithium, lithium alloy) lines, dots, regions, pillars (collectively referred to herein as pillars, see e.g. FIG. 2 ) preferably oriented perpendicularly to the electrode base (in the elongation direction of the silicon fiber layer).
[0047] In one embodiment, the object of the present invention is the production of well-aligned and / or entangled and / or stacked free-standing layers comprising (preferably consisting of) silicon nano- or micro-fibers and / or silicon nano- or micro-rods, and thus comprising (preferably consisting of) crystalline silicon and / or amorphous silicon and / or polycrystalline silicon, preferably from suitable hydrogenated silicon precursors, which are preferably liquid within the operating window of the nano- and / or micro-fiber manufacturing equipment, preferably defined between mp -55°C and bp 420°C. Silicon precursors include cyclic silanes (Si n H 2n , n>3), for example, cyclohexasilane, SiH 12 (mp+16.5, bp+226°C) or Hexasilane Si6H 14(mp -44.7°C to +bp 193.6°C) n H 2n+2 where n>3). A general concept of how to convert silanes into crystalline or polymeric silicon, i.e. fibers, can be found, for example, in ACS Applied Materials and Interfaces, Journal Volume: 4; Journal Issue: 5, pages 2680-2685; Journal ID: ISSN 1944-8244 (Solution-based synthesis of microcrystalline silicon). According to an embodiment, the Si precursor can also carry a dopant and / or dopant(s), which is crosslinked with the Si precursor, for example to form a copolymerized Si / dopant solution prior to the fiber spinning process or to grow Si rods, wires with nano- and / or micro-dimensions.
[0048] The information above and below regarding Si and Si fibers is meant to apply to any Group IV semiconductor or mixtures thereof.
[0049] Suitable liquid silicon precursors may also be poly(silanes) such as dimethylpolysilane (DMPS), deca-phenyl-penta-silane (DPPS), and poly-methyl-phenylsilane (PMPS), and / or a suitable n-type dopant may be phosphorus bromine, PBr3.
[0050] A first possible method for producing a silicon layer is electrospinning of a (polymer) solution onto a substrate and subsequent pyrolysis by heating and / or laser and / or microwave treatment to obtain a silicon layer made of rods and / or wires with nano- and / or micro-dimensions, which may or may not be doped. The same operation is performed: a second layer of a (polymer) silicon precursor is electrospun, followed by pyrolysis to obtain a second silicon layer. This operation can be repeated X times to obtain X stacked / entangled silicon layers.
[0051] A second possible method is based on carbonaceous seed carriers decorated with a suitable catalyst (e.g., gold, silver nickel, etc.) capable of forming intermetallic compounds with silicon in the growth process. These seed carriers are in the form of 0D ((silicon)-nanocrystals, quantum dots), 1D (CNTs) and / or 2D (graphene, mxenes, silicon nanosheets) and / or 3D (reduced graphene oxide forms, MOFs) carbon-based materials. These seed materials decorated with the above nucleation seeds can be aligned by dielectrophoresis on top of a solution containing a copolymerized Si / dopant mixture, which can be dissolved in a hydrocarbon or a mixture of hydrocarbons, e.g., paraffin. The system of current collectors can be implemented in various shapes, e.g., a hexagon containing three cathodes and three anodes. The alignment of these seed carriers creates an electronic percolation network that short-circuits the cathode / anode pairs. This short circuit generates heat by the Joule effect at the surface of the seed carrier, which causes the thermal decomposition of the silicon precursor, resulting in a silicon layer made of rods and / or fibers and / or wires with nano- and / or micro-dimensions. Furthermore, this silicon layer can be doped with various n-type (e.g. phosphorus) or p-type (e.g. boron) by adding appropriate dopant precursors (e.g. B2H6, pnictogens) to the precursor solution. Several layers can be obtained by stacking the dielectrophoretic electrodes in a hexagonal system by an electrical insulator to obtain a stack of electrodes.
[0052] The successful production of the described anode can be monitored by scanning electron microscopy to confirm the morphology of the silicon monolith, and scanning microtomography to ensure good distribution and location of the melting points. As for the anode performance, cyclic voltammetry as well as the usual galvanostatic cycling method can be implemented, and the anodic and cathodic peaks should be contained below 0.2 V, transforming good kinetics of the electrochemical reactions and thus a morphology of the silicon anode suitable for ionic and electronic diffusion, as well as efficient charge transfer phenomena. Ex situ lithiated anode (Li15 Si4) represents the fully charged state of an electrochemical half-cell based on a fabricated silicon anode with a suitable lithium-free cathode; for example, in the case of sulfur, the electrochemical cell is characterized by an open circuit potential above 0 V, and in the case of sulfur, a potential of 2.1 V is observed. 15 To monitor the complete lithiation of a Si anode (e.g., 100 mg), the initial discharge is performed to the full theoretical capacity (100 mg Li 15 The capacity of the ex-situ fabricated SEI reaches 185mAh for the Si4 anode. The beneficial construction of the ex-situ fabricated SEI is demonstrated by repeated charge / discharge of such fabricated anodes without losing capacity due to the formation of lithium-consuming in-situ SEI construction. The combination of structural integrity of the ex-situ SEI and anisotropic lithiation results in a capacity retention of up to 90% of the initial discharge capacity over up to 1,000 charge / discharge cycles at a current density of 3C. Another approach to visualize the anisotropic Li distribution is realized by operando analysis of the charge distribution during charge / discharge, especially during the initial discharge, by X-ray microdiffraction (according to ACS The Journal of Physical Chemistry Letters, Journal Volume:1; Journal Issue:14; Pages 2120-2123; Journal ID: ISSN1948-7185).
[0053] Another object is the spot fusion of the resulting monolithic heterogeneous fibrous silicon anode, initiated by an alloying reaction between, for example, lithium and / or binary lithium alloys and / or ternary lithium alloys and / or lithium salts. Suitable solvents suitable for alloying Li with Si and capable of solubilizing the lithium salt are, more preferably, the lithium salt is LiTFSI, suitable solvents are, for example, binary and ternary mixtures of polar and non-polar alkane solvents, more preferably, the non-polar solvent is a hydrocarbon such as decane, and the polar solvent is diethylene glycol dimethyl ether, the boiling point of the solvent is above 130° C., and the molar concentration of LiTFSI in the electrolyte is 0.75M or less, more preferably 0.25M. Pre-lithiation is preferably the introduction of structure lithium (e.g., dots / lines - Figs. 1, 2, 3) before setting up the battery, so that the pre-lithiated silicon anode is a structure containing lithium and / or Li-Si alloys.
[0054] In accordance with embodiments of the previous subject matter, the present invention includes environmentally friendly positive electrodes manufactured from a slurry-free process and / or not based on anode material slurry and / or binder-free and / or drying-free and / or calendar-free manufacturing methods.
[0055] According to one embodiment of the present invention, a negative electrode - heterogeneous fibrous silicon anode is provided, where the selected active material is heterogeneous fibrous ex situ pre-lithiated and / or the content of silicon in the anode is 72% or more, more preferably 92% by weight, more preferably the pre-lithiation state of the silicon anode depends on the available lithium content in the cathode which together form a balanced lithium ion battery.
[0056] According to one embodiment of the present invention, a negative electrode-heterogeneous fibrous silicon anode is provided, in which the size of the fiber / rod / wire / tube is 120 nm-15 μm, and the thickness of the heterogeneous fibrous silicon (wafer-like) anode is 10 μm-800 μm.
[0057] This and other dimensional specifications may be determined by SEM (scanning electron microscope).
[0058] According to one embodiment of the present invention, a method for the preparation of a negative electrode - a heterogeneous fibrous silicon anode is provided, in which silicon fibers are preferably prepared from silicon precursors containing suitable dopants and / or dopants, preferably forming a homogeneous mixture that is preferably partially copolymerized prior to entering the fiber formation process.
[0059] The present invention may also be directed to a negative electrode for use in an alkali ion rechargeable battery, the electrochemically active material of the anode being selected from Group IV semiconductors, characterized in that the active material is provided as a heterogeneous fibrous and / or wafer-like and / or free-standing and / or monolithic anode body, the anode body comprising at least two layers of aligned and / or stacked and / or entangled fibers spot-fused together at a plurality of discrete points with individual lithium Group IV semiconductor alloy and / or lithium bonding between the layers, and the anode body, in particular the layers, are anisotropically lithiated.
[0060] According to one embodiment, a new safety enhancement concept exploits the beneficial anisotropic properties of 2D graphene foil, also known as paper, FIG. 9, which has higher thermal and electronic conductivity in the in-plane direction than through the plane, such a net-shaped graphene current collector foil FIG. 8 is provided with integrated current collecting tabs or tabs, mimicking the geometry of the FIG. 7 electrode, and the anisotropy allows for efficient removal and redistribution of electrons and heat removal from or to the battery.
[0061] 10-13 model the effect of lithium on the active mass material of the anode during construction of the anode.
[0062] 14 and 15 show the effect of lithiation and delithiation on the structure of the anode layer, in particular between the melt spots according to claim 1 (structural expansion and contraction of the layer).
[0063] Preferably, the monolithic and / or wafer-like and / or free-standing architecture further comprises at least two, preferably at least three, heterogeneous fibrous silicon layers stacked and / or intertwined between each layer (FIGS. 4, 5). Preferably, such silicon structures can then be converted into a monolithic body by lithiation (FIG. 6).
[0064] The present invention may also be directed to a negative electrode for use in an alkaline ion rechargeable battery, comprising an anode electrochemically active material, and / or the active material is selected from group IV semiconductors, and / or the active material is provided as a heterogeneous fibrous and / or wafer-like and / or free-standing and / or monolithic anode body, and / or the anode body comprises at least two layers of aligned and / or stacked and / or entangled fibers, and / or the layers are spot fused (FIGS. 1 and / or 2 and / or 3). Individual lithium group IV semiconductor alloy and / or lithium bonds and / or layers are spaced apart from each other at a plurality of discrete points together, preferably by spot fused bonds, and / or the spot fused bonds are oriented in an out-of-plane direction relative to the layer plane of extension, and / or the portions of the layers outside the spot fused bonds are free to move and / or expand in an in-plane direction, and / or the anode body, particularly the layers, are anisotropically lithiated. Preferably, the anode body has an artificial ex-situ SEI layer on the entire surface of the anode body (wafer).
[0065] According to one embodiment of the present invention, the method for producing the negative electrode - the heterogeneous fibrous silicon anode, in which the anisotropic (over)lithiation of the silicon fibrous layer is performed, is provided by the molten lithium printing fusion method via a fusion printer and / or lithium dispenser, preferably within a temperature range of 45 °C to 750 °C, the fusion printer head preferably follows a predetermined trajectory to place the fusion spots, producing a functional anisotropy (anisotropic lithiation) in the anode, preferably defined as a pattern or spot. According to one embodiment of the present invention, a method for producing a negative electrode - a heterogeneous fibrous silicon anode, in which anisotropic (over)lithiation of the silicon fibrous layer is carried out, is provided, for example, by electrochemical methods in a suitable lithium electrolyte temperature range, preferably between 100°C and 250°C, into which the entire silicon anode body (wafer) is immersed. A glass, ceramic and / or glass-ceramic sheet of solid electrolyte can divide the operating prelithiation chamber into two independent cathode / anode compartments, which allows the prelithiation chamber to be filled with molten lithium metal and / or thick lithium metal foils, and / or Li2S6 in organic solvents and / or water or Cu. 2+ Suitable Li-ion donors of various types, such as liquid lithium-rich donor electrolytes such as Li2SO4 in polar protic solvents, as sacrificial electrodes, + Sources can be used: glass, ceramic, and / or glass-ceramic sheets of solid electrolytes that feature a pattern resembling the target distribution of anisotropic lithiation (see Figures 2, 4, 5, and 6).
[0066] According to one embodiment of the present invention, a method for manufacturing anode-silicon anodes is provided, in which the silicon fiber layers and / or printer heads are immersed in a liquid treatment medium. Preferably, each print-fuse head / nozzle is electrically connected to monitor the resistivity of the local spot area of the Si anode body (wafer) and / or monitor the pressure rise during expansion caused by prelithiation, and these parameters are used to create a balanced spot-fuse point. This allows for safer and faster lithiation of Si along the printer / dosing head / nozzle trajectory or spot printing / fusing. Preferably, Li spot printing / fusing rises through the layer of silicon during the spot-fusing process, preferably as droplets of molten lithium, interconnecting the individual Si fiber layers.
[0067] According to one embodiment of the present invention, a method for ex situ pre-lithiation (preferably first stage) anode - a heterogeneous fibrous silicon anode is provided, where the flow of molten lithium against gravity towards the silicon layer immersed in a solvent - is defined as suspended in a suitable process liquid, such as a hydrocarbon, as outlined above, compatible with molten lithium, such liquid having a density of 0.65 g / cm 3 or more, and is therefore higher than the density of molten lithium.
[0068] Preferably, according to the present invention, a negative electrode for use in an alkali ion rechargeable battery is claimed, wherein the electrochemically active material is selected from Group IV semiconductors, the active material forming a heterogeneous fibrous monolithic anode body, the anode body comprising at least three layers of aligned and / or stacked and / or entangled fibers.
[0069] In the following, the invention is further explained by the provided figures. [Brief description of the drawings]
[0070] [Figure 1] FIG. 1 is a diagram illustrating an example of a fusion spot distribution for interconnecting individual layers of aligned and / or stacked and / or entangled Group IV, particularly silicon, fibers. [Diagram 2] FIG. 2 shows an exemplary setup for the lithiation of a spot-fused layered silicon anode body (wafer), a patterned solid (glass) ceramic electrolyte (hexagon) as a lithiation mask. The lithiation is carried out stepwise, for example, in four steps as shown in FIG. 2, but is not limited to this number of steps. The steps can be from 1 to 100 steps. The lithiation is preferably started first in the central portion 1, followed by the subsequent regions, then 3, 4, etc. [Diagram 3] FIG. 3 shows an abstract representation of an overlithiated silicon anode body. [Figure 4]Figure 4 shows a patterned solid (glass) ceramic electrolyte as a lithiation mask, similar to ex situ lithiation in a process solvent / electrolyte. Figure 4 shows the initial state, which contains only a limited lithiated layer and a non-expanded silicon layer. These layers are mechanically linked to each other by fusion spots. [Diagram 5] Figure 5 shows a patterned solid (glass) ceramic electrolyte as a lithiation mask, similar to ex situ lithiation in a process solvent / electrolyte. Figure 5 shows a partially lithiated intermediate state and an expanded silicon layer that is anisotropically spot fused with lithium induced metallic bonding. Arrows indicate the lithiation pathway. [Figure 6] Figure 6 shows a patterned solid (glass) ceramic electrolyte as a lithiation mask, analogous to ex situ lithiation in a process solvent / electrolyte. Figure 6 shows the integrity of (over)lithiated and fully expanded silicon layers, which are anisotropically spot fused by lithium induced metallic bonds. Arrows indicate the lithiation pathways. [Figure 7] FIG. 7 shows a lithiated (5-100%) silicon wafer monolithic body containing an ex situ fabricated artificial SEI layer. [Figure 8] FIG. 8 illustrates a graphene and / or reduced graphene oxide current collector foil that includes three tabs. [Figure 9] Figure 9 illustrates a lithiated (5-100%) silicon wafer anode monolith containing an ex situ fabricated artificial SEI layer mounted on top of a three-tab graphene and / or reduced graphene oxide current collector foil. [Figure 10]Figures 10-13 are diagrams showing the relative volume ranges of layered silicon anodes (later silicon wafers) in various unlithiated, partially lithiated, and overlithiated states. The size of the circles may simply represent an increase in volume, but not necessarily an actual percentage of the volume or increase. Figure 10 shows a silicon wafer anode in its most dense state. [Figure 11] FIG. 11 shows a lithiated silicon wafer anode in the (electrochemical) room temperature active phase Li15Si4. [Figure 12] FIG. 12 shows an overlithiated silicon wafer anode in the high temperature active phase Li21Si5 characterized by the largest volume (electrochemically) possible. [Figure 13] Figure 13 shows an SEI produced ex situ by disproportionating the high-temperature Li21Si5 phase to the room-temperature phase Li15Si4. The excess Li thus released is consumed to build an artificial SEI layer (red). [Figure 14] FIG. 14 is a top view of the relative orientation of three representative layers with aligned silicon fibers, each aligned along the direction of an individual arrow of the same color, in a layer of aligned, preferably 120° entangled, silicon fibers prior to the prelithiation process. [Figure 15] FIG. 15 shows the layer setup according to FIG. 14 after the prelithiation (spot fusion) process.
Claims
1. 1. A negative electrode for an alkaline ion rechargeable battery, comprising: - comprising an anode electrochemically active material, said active material is chosen from group IV semiconductors; the active material is provided as a heterogeneous fibrous, wafer-like, free-standing monolithic anode body; said anode body comprises at least two layers of aligned and / or stacked and / or entangled fibers, the at least two layers are arranged parallel to one another, the layers are interconnected at a plurality of discrete interconnect sites via metallurgical bonds; said metallic bond comprises or consists of a Li-IV group element alloy and / or lithium or a mixture of the two, the individual interconnect sites are distributed discretely throughout the anode body and therefore in the layer; a negative electrode, wherein the metallic bonds extend out-of-plane relative to the individual layers and provide spacers between the layers;
2. 10. The negative electrode of claim 1, wherein the anode body is characterized as being non-uniformly lithiated with unlithiated and / or underlithiated and / or stoichiometrically lithiated regions.
3. 3. The negative electrode according to claim 1 or 2, characterized in that the anode body has an artificial ex situ introduced SEI layer on the entire surface of the wafer, the volume / extension of which is adapted to the volume of the anode in the maximum lithiation state and / or is provided in the highly lithiated state of the anode.
4. 4. The negative electrode according to claim 1, wherein the group IV semiconductor is or contains silicon.
5. 5. The negative electrode of claim 1, wherein at the individual interconnect points of the layers, there is stoichiometric access of lithium with respect to the amount of lithium required to form a lithium-group IV element alloy within the metallic bond.
6. 6. The anode according to claim 1, wherein the length of said fibers is 120 nm to 15 μm, and the thickness of said heterogeneous fibrous silicon wafer anode is 10 μm to 800 μm.
7. 7. The negative electrode according to claim 1 , characterized in that the individual Li-IV element alloy bonds and thus the individual interconnection points are provided as placeholders between the layers, such that the layers experience at least partial voids between them at least in a discharged state, and that in a charged state of the anode, the voids are at least partially filled with the active material.
8. 8. A negative electrode according to claim 1, characterized in that the individual interconnection points or sites are in the form of points and / or lines and / or pillars and / or patches.
9. 9. The negative electrode of claim 1, wherein the layers are spaced apart from one another.
10. 10. The negative electrode of claim 1, wherein the individual interconnection sites are at least partially arranged as spacers between the layers, such that the layers include at least some regions having gaps between the layers provided by the spacers.
11. at least one Group IV semiconductor material is provided as individual layers of aligned and / or stacked and / or entangled fibers; the layers are arranged parallel to one another and are interconnected together at a plurality of individual interconnect sites via spot fusion, i.e., metallurgical bonding; the metallic bond comprises or consists of a Li-IV element alloy and / or lithium or a mixture of the two, and is formed by fusing the layers together by lithium fusion or by the introduction of lithium in liquid form into the disposed layers; 11. A method for producing an anode according to any one of claims 1 to 10, wherein the individual interconnect sites are introduced across the anode body and thus are individually disposed in the layers, and the metallurgical bonds are provided such that they extend out-of-plane relative to the individual layers and thus form spacers between the layers.
12. The anode body is lithiated to an overlithiated state, i.e., Li 21 X 5 and X is at least one of the group IV elements, and is treated with one or more SEI layer-forming dopants, such as As-, P-, (H)F-compounds, and / or SEI layer-forming electrolytes, to form an artificial SEI layer on the anode in its maximum volume expansion state.
Citation Information
Patent Citations
Method of manufacturing fibers comprising silicon or silicon material, and use of the same in lithium storage battery
JP2011082179A
Porous electrode active materials
JP2013538777A
Negative electrode active material for lithium ion secondary battery, and lithium ion secondary battery
WO2016075798A1