Semiconductor nanoparticles, their production method, and light-emitting device
The production of core-shell semiconductor nanoparticles with specific elemental compositions and heat treatment processes addresses the need for superior luminous efficiency, resulting in nanoparticles with efficient band-edge emission for light-emitting devices.
Patent Information
- Application Number
- JP2021542896
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-08-26
- Filing Date
- 2020-08-24
- Publication Date
- 2024-12-09
- Estimated Expiration
- 2040-08-24
AI Technical Summary
There is a need for semiconductor nanoparticles that exhibit superior luminous efficiency through band-edge emission.
The production of core-shell type semiconductor nanoparticles is achieved by forming a core with elements like Ag, Cu, Au, or alkali metals, and a shell with elements like Al, Ga, In, and Tl, using specific compounds and heat treatment to create a mixture with a defined atomic ratio, followed by a heat treatment process to form a shell on the core.
The method produces semiconductor nanoparticles with excellent luminous efficiency, capable of band-edge emission and narrow half-width light emission, suitable for applications in light-emitting devices.
Smart Images

Figure 0007595881000005 
Figure 0007595881000006 
Figure 0007595881000007
Abstract
Description
[Technical field]
[0001] The present disclosure relates to semiconductor nanoparticles, methods for producing the same, and light-emitting devices. [Background technology]
[0002] It is known that semiconductor particles exhibit a quantum size effect when their particle size is, for example, 10 nm or less, and such nanoparticles are called quantum dots (also called semiconductor quantum dots). The quantum size effect refers to the phenomenon in which the valence band and conduction band, which are considered continuous in bulk particles, become discrete when the particle size is nanosized, and the band gap energy changes depending on the particle size.
[0003] Since quantum dots can absorb light and convert the wavelength of the light into light corresponding to the band gap energy, white light emitting devices utilizing the emission of quantum dots have been proposed (see, for example, JP 2012-212862 A and JP 2010-177656 A). In addition, core-shell type semiconductor nanoparticles capable of band edge emission and having a low toxicity composition and a method for producing the same have been proposed (see, for example, JP 2018-044142 A). Summary of the Invention [Problem to be solved by the invention]
[0004] As quantum dots exhibiting band-edge emission, semiconductor nanoparticles with superior luminescence efficiency are in demand. One aspect of the present disclosure aims to provide a method for producing semiconductor nanoparticles capable of band-edge emission and with superior luminescence efficiency. [Means for solving the problem]
[0005] The first aspect is a method for producing core-shell type semiconductor nanoparticles. 1 , M 2 and a core comprising a semiconductor containing Z, 1is at least one element selected from the group consisting of Ag, Cu, Au and alkali metals, and contains at least Ag; M 2 The method includes preparing a core in which Z is at least one element selected from the group consisting of Al, Ga, In, and Tl, and includes at least one of In and Ga, and Z is at least one element selected from the group consisting of S, Se, and Te, obtaining a mixture containing the core, at least one compound containing a first element selected from the group consisting of Al, Ga, In, and Tl, and at least one simple substance of a second element selected from the group consisting of S, Se, and Te, and at least one compound containing the second element, and heat-treating the mixture to obtain core-shell type semiconductor nanoparticles. The mixture contains the compound containing the first element and the simple substance of the second element or the compound containing the second element in a mixing ratio such that the ratio of the total number of atoms of the first element to the sum of the total number of atoms of the first element and the total number of atoms of the second element is greater than 0.5.
[0006] The second aspect is a core-shell type semiconductor nanoparticle that has a core and a shell disposed on the surface of the core and emits light when irradiated with light. 1 , M 2 and semiconductors containing Z, 1 is at least one element selected from the group consisting of Ag, Cu, Au and alkali metals, and contains at least Ag; M 2 is at least one element selected from the group consisting of Al, Ga, In and Tl, and includes at least one of In and Ga, and Z includes at least one element selected from the group consisting of S, Se and Te. 1 The total content of M is 10 mol % or more and 30 mol % or less, 2 The total content of is 15 mol% or more and 35 mol% or less, and the total content of Z is 35 mol% or more and 55 mol% or less. The shell is essentially composed of a first element which is at least one selected from the group consisting of Al, Ga, In, and Tl, a second element which is at least one selected from the group consisting of S, Se, and Te, and an O element.
[0007] A third aspect is a light-emitting device comprising a light conversion member containing the core-shell type semiconductor nanoparticles and a semiconductor light-emitting element. Effect of the Invention
[0008] According to one aspect of the present disclosure, it is possible to provide a method for producing semiconductor nanoparticles capable of band edge emission and having excellent luminous efficiency. [Brief description of the drawings]
[0009] [Figure 1] FIG. 2 is a diagram showing the absorption spectrum of core-shell semiconductor nanoparticles. [Diagram 2] FIG. 2 is a diagram showing the emission spectrum of core-shell type semiconductor nanoparticles. [Diagram 3] FIG. 2 is a diagram showing the absorption spectrum of core-shell semiconductor nanoparticles. [Figure 4] FIG. 2 is a diagram showing the emission spectrum of core-shell type semiconductor nanoparticles. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] In this specification, the term "step" includes not only an independent step, but also a step that cannot be clearly distinguished from other steps, as long as the intended purpose of the step is achieved. Furthermore, the content of each component in the composition means the total amount of the multiple substances present in the composition when multiple substances corresponding to each component are present in the composition, unless otherwise specified. Hereinafter, the embodiments of the present invention will be described in detail. However, the embodiments shown below are examples of core-shell type semiconductor nanoparticles, their manufacturing method, and light-emitting devices for embodying the technical idea of the present invention, and the present invention is not limited to the core-shell type semiconductor nanoparticles, their manufacturing method, and light-emitting devices shown below.
[0011] Method for producing core-shell semiconductor nanoparticles The method for producing core-shell type semiconductor nanoparticles includes a preparation step of preparing a core, a mixing step of obtaining a mixture containing a core- and shell-forming material, and a heat treatment step of heat-treating the mixture to obtain core-shell type semiconductor nanoparticles. 1 , element M 2 and semiconductors containing element Z. 1 contains at least one element selected from the group consisting of silver (Ag), copper (Cu), gold (Au) and alkali metals, and contains at least Ag. 2 contains at least one selected from the group consisting of aluminum (Al), gallium (Ga), indium (In) and thallium (Tl), and contains at least one of In and Ga. The element Z contains at least one selected from the group consisting of sulfur (S), selenium (Se) and tellurium (Te). The mixture contains a core and at least one compound containing a first element, which is at least one selected from the group consisting of Al, Ga, In and Tl, as a shell forming material, and at least one simple substance of a second element, which is at least one selected from the group consisting of S, Se and Te, and at least one compound containing the second element. The mixture contains a compound containing a first element (hereinafter also referred to as a first element source) and a simple substance of the second element or a compound containing the second element (hereinafter collectively referred to as a second element source) in a mixing ratio such that the ratio of the total number of atoms of the first element to the sum of the total number of atoms of the first element and the total number of atoms of the second element is greater than 0.5.
[0012] In the method for producing core-shell semiconductor nanoparticles, when forming a shell on the core surface, a mixture containing a first element source and a second element source, which are shell forming materials, is heat-treated so that the content of the first element is in excess of the second element on a molar basis, thereby producing core-shell semiconductor nanoparticles with excellent luminous efficiency. This can be considered, for example, because the first element contained in excess reacts with an element other than the second element, such as oxygen, to form the shell.
[0013] Core preparation process In the core preparation process, element M 1 , element M 2and a core containing a semiconductor containing element Z. The core may be a semiconductor nanoparticle. The core may be prepared by appropriately selecting from commercially available semiconductor nanoparticles, or may be prepared by manufacturing semiconductor nanoparticles having a desired composition.
[0014] Core element M 1 The element M contains Ag and may further contain at least one element selected from the group consisting of Cu, Au and alkali metals. 1 The alkali metals in include lithium (Li), sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), etc. Alkali metals can become monovalent cations like Ag, and can therefore substitute for a portion of Ag in the composition of the semiconductor nanoparticles. In particular, Li has an ionic radius similar to that of Ag, and is preferably used. In the composition of the semiconductor nanoparticles, for example, by substituting a portion of Ag with an alkali metal, for example, the band gap is widened and the emission peak wavelength is shifted to a shorter wavelength. The element M 2 contains at least one of In and Ga, and may further contain at least one element selected from the group consisting of Al and Tl. The element Z contains at least one element selected from the group consisting of S, Se, and Te, and may contain at least S.
[0015] The core is, for example, the element M 1 Ag as the element M 2 The core may be a semiconductor nanoparticle containing at least one of In and Ga as the element Z, and S as the element Z. The core may be, for example, a semiconductor nanoparticle having a composition represented by the following formula (1). M 1 q M 2 Z (q+3) / 2 (1) Here, 0.2 <q≦1.2である。
[0016] The core semiconductor nanoparticles can be produced by the following production method. For example, the first core production method uses an element M 1 and a salt containing element M 2The second core production method may include a raw material preparation step of obtaining a first raw material mixture containing a salt containing element M, a source of element Z, and an organic solvent, and a heat treatment step of heat treating the first raw material mixture to obtain semiconductor nanoparticles. 1 and a salt containing element M 2 and an organic solvent; a temperature increasing step of heating the second raw material mixture to a predetermined temperature; and an adding step of adding a source of element Z to the heated second raw material mixture.
[0017] In the first core manufacturing method, element M 1 and a salt containing element M 2 The core may be produced by preparing a first raw material mixture by adding a salt containing the element M and a source of the element Z to an organic solvent at once, and then heat-treating the mixture. According to this method, the core semiconductor nanoparticles can be synthesized reproducibly in one pot by a simple operation. 1 Then, the organic solvent is reacted with a salt containing element M to form a complex. 2 The core may be produced by reacting the compound with a salt containing the element Z to form complexes, reacting these complexes with a source of element Z, and growing the crystals of the resulting reaction product. In this case, the heat treatment may be carried out at the stage of reaction with the source of element Z.
[0018] element M 1 Salts containing the element M 2 The salt containing the element M may be either an organic acid salt or an inorganic acid salt. Specifically, examples of inorganic acid salts include nitrates, sulfates, hydrochlorides, and sulfonates. Examples of organic acid salts include formates, acetates, oxalates, and acetylacetonates. 1 Salts containing the element M 2 The salt containing is preferably at least one selected from the group consisting of these, and more preferably an organic acid salt such as an acetate salt, an acetylacetonate salt, etc. This is believed to be because the organic acid salt has high solubility in an organic solvent and tends to allow the reaction to proceed more uniformly.
[0019] Among the sources of the element Z, examples of the source of S include elemental sulfur and sulfur-containing compounds. Specific examples of the sulfur-containing compounds include β-dithiones such as 2,4-pentanedithione, dithiols such as 1,2-bis(trifluoromethyl)ethylene-1,2-dithiol, dialkyldithiocarbamate such as diethyldithiocarbamate, and alkylthioureas having an alkyl group having 1 to 18 carbon atoms, such as thiourea, monoalkylthiourea, 1,3-dialkylthiourea, 1,1-dialkylthiourea, 1,1,3-trialkylthiourea, and 1,1,3,3-tetraalkylthiourea.
[0020] Examples of the Se supply source include simple selenium, Se-containing compounds such as selenourea, selenoacetamide, and alkylselenol, etc. Examples of the Te supply source include simple tellurium, Te-phosphine complexes, and alkyltellurols, etc.
[0021] Examples of the organic solvent include amines having a hydrocarbon group having 4 to 20 carbon atoms, such as alkylamines or alkenylamines having 4 to 20 carbon atoms, thiols having a hydrocarbon group having 4 to 20 carbon atoms, such as alkylthiols or alkenylthiols having 4 to 20 carbon atoms, phosphines having a hydrocarbon group having 4 to 20 carbon atoms, such as alkylphosphines or alkenylphosphines having 4 to 20 carbon atoms, and it is preferable to include at least one selected from the group consisting of these. These organic solvents may, for example, ultimately modify the surface of the semiconductor nanoparticles obtained. Two or more organic solvents may be used in combination, and for example, a mixed solvent may be used that combines at least one selected from thiols having a hydrocarbon group having 4 to 20 carbon atoms and at least one selected from amines having a hydrocarbon group having 4 to 20 carbon atoms. These organic solvents may be used in combination with other organic solvents. When the organic solvent contains the thiol and the amine, the volume ratio of the thiol to the amine (thiol / amine) is, for example, greater than 0 and equal to or less than 1, and preferably equal to or greater than 0.007 and equal to or less than 0.2.
[0022] The first raw material mixture contains the element M 1 and at least one salt containing an element M 2 The first raw material mixture may contain at least one salt containing the element M and at least one source of the element Z without reacting with each other, or may contain a complex formed from the salt and the source of the element M. 1 M formed from a salt containing 1 Complex, element M 2 M formed from a salt containing 2 The complex formation may include a complex formed from a source of element Z, etc. The complex formation may be, for example, a complex formed from a source of element M in a suitable organic solvent. 1 and a salt containing element M 2 The mixing is carried out by mixing a salt containing the element Z with a source of the element Z. The mixing atmosphere may be an inert gas atmosphere, such as an argon atmosphere or a nitrogen atmosphere. By using an inert gas atmosphere, the by-production of oxides can be reduced or prevented.
[0023] The first raw material mixture contains the element M 2 The total number of atoms of element M 1 The ratio of the total number of atoms (M 1 / M 2 ) is, for example, 0.1 or more and 2.5 or less, preferably 0.2 or more and 2.0 or less, and more preferably 0.3 or more and 1.5 or less. In addition, in the composition of the first raw material mixture, the ratio of the number of In atoms to the total number of In and Ga atoms (In / (In+Ga)) is, for example, 0.1 or more and 1.0 or less, and preferably 0.25 or more and 0.99 or less. In addition, in the composition of the first raw material mixture, the ratio of the number of In atoms to the total number of In atoms and Ga atoms (In / (In+Ga)) is, for example, 0.1 or more and 1.0 or less, and preferably 0.25 or more and 0.99 or less. 1 The ratio of the total number of atoms (M 1 / Z) is, for example, 0.27 or more and 1.0 or less, and preferably 0.35 or more and 0.5 or less. By using a supply source of each element so that the composition of the first raw material mixture satisfies these conditions, semiconductor nanoparticles that are likely to give band edge emission can be produced.
[0024] The heat treatment step in the first manufacturing method may be a one-stage heat treatment step in which the first raw material mixture is heat-treated at a predetermined temperature, or a two-stage heat treatment step in which the first raw material mixture is heat-treated at the first temperature and then at a second temperature higher than the first temperature. By carrying out the heat treatment in two stages, for example, semiconductor nanoparticles having a relatively high band edge emission intensity can be produced with better reproducibility. Here, the heat treatment at the first temperature and the heat treatment at the second temperature may be carried out continuously, or the heat treatment at the first temperature may be followed by lowering the temperature and then raising the temperature to the second temperature for heat treatment.
[0025] When the heat treatment of the first raw material mixture is carried out in a single heat treatment step, the heat treatment temperature may be, for example, 180°C or higher, and preferably 200°C or higher or 260°C or higher. The heat treatment temperature may be, for example, 370°C or lower, and preferably 350°C or lower or 320°C or lower. The heat treatment time may be, for example, 1 minute or more, preferably 5 minutes or more, and more preferably 7 minutes or more. The heat treatment time may be, for example, 120 minutes or less, and preferably 60 minutes or less, and more preferably 30 minutes or less or 20 minutes or less.
[0026] In addition, when the heat treatment of the first raw material mixture is performed in a two-stage heat treatment process, the first temperature may be, for example, 30° C. or higher, and preferably 100° C. or higher. In addition, the first temperature may be, for example, 200° C. or lower, and preferably 180° C. or lower. The time of the heat treatment at the first temperature may be, for example, 1 minute or more, preferably 5 minutes or more, and more preferably 10 minutes or more. In addition, the time of the heat treatment at the first temperature may be, for example, 120 minutes or less, preferably 60 minutes or less, and more preferably 30 minutes or less.
[0027] The second temperature may be, for example, 180° C. or higher, and preferably 200° C. or higher. The second temperature may be, for example, 370° C. or lower, and preferably 350° C. or lower. The time of the heat treatment at the second temperature may be, for example, 1 minute or more, and preferably 5 minutes or more, and more preferably 10 minutes or more. The time of the heat treatment at the second temperature may be, for example, 120 minutes or less, and preferably 60 minutes or less, and more preferably 30 minutes or less.
[0028] The time of the heat treatment is defined as the start time of the heat treatment when a predetermined temperature is reached, and the end time of the heat treatment at the predetermined temperature is defined as the time when the operation for lowering or raising the temperature is performed. The rate of temperature rise until the predetermined temperature is reached may be, for example, 1°C / min to 100°C / min, or 1°C / min to 50°C / min. The rate of temperature fall after the heat treatment is, for example, 1°C / min to 100°C / min, and the material may be cooled as necessary, or the heat source may be stopped and the material may be allowed to cool.
[0029] The atmosphere in the heat treatment step is preferably an inert atmosphere such as a rare gas atmosphere such as argon atmosphere, a nitrogen atmosphere, etc. By performing the heat treatment in an inert atmosphere, it is possible to suppress the by-production of oxides.
[0030] In the preparation step of the second core manufacturing method, element M 1 and at least one salt containing an element M 2 A second raw material mixture is prepared, the second raw material mixture containing at least one salt containing the element M 1 and a salt containing element M 2 The second raw material mixture can be prepared by mixing a salt containing element M with an organic solvent. 1 Salt containing element M 2 The second raw material mixture may be prepared by mixing a salt containing the above with an organic solvent, and then mixing the remaining components. The resulting second raw material mixture may be in a solution state without undissolved matter at an elevated temperature. The mixing atmosphere may be an inert gas atmosphere, such as an argon atmosphere or a nitrogen atmosphere. By using an inert gas atmosphere, the by-production of oxides can be reduced or prevented.
[0031] Element M used in the second core manufacturing method 1 Salts containing element M 2 The salt containing and the organic solvent are the same as those used in the first core production method.
[0032] The second raw material mixture contains element M 1 and at least one salt containing an element M 2 The second raw material mixture may contain at least one salt containing the element M without reacting with each other, or may contain a complex formed from the element M. 1 M formed from a salt containing 1 Complex, element M 2 M formed from a salt containing 2 The complex formation may include a complex, etc., for example, by dissolving an element M in a suitable organic solvent. 1 and a salt containing element M 2 This is carried out by mixing with a salt comprising
[0033] The second raw material mixture contains the element M 2 The total number of atoms of element M 1 The ratio of the total number of atoms (M 1 / M 2 ) is, for example, 0.1 or more and 2.5 or less, preferably 0.2 or more and 2.0 or less, and more preferably 0.3 or more and 1.5 or less. In addition, in the composition of the second raw material mixture, the ratio of the number of In atoms to the total number of In and Ga atoms (In / (In+Ga)) is, for example, 0.1 or more and 1.0 or less, and preferably 0.25 or more and 0.99 or less. By using a supply source of each element so that the composition of the mixture satisfies these conditions, semiconductor nanoparticles that are likely to give band edge emission can be produced.
[0034] In the temperature-raising step in the second core production method, the prepared second raw material mixture is heated to a temperature in the range of, for example, 120° C. to 300° C. The temperature reached by the temperature rise is preferably 125° C. or higher, more preferably 130° C. or higher, even more preferably 135° C. or higher, and preferably 175° C. or lower, more preferably 160° C. or lower, even more preferably 150° C. or lower. The temperature rise rate is, for example, 1° C. / min to 50° C. / min, and preferably 10° C. / min to 50° C. / min.
[0035] The atmosphere in the temperature increasing step of the second raw material mixture is preferably an inert gas atmosphere, for example, an argon atmosphere, a nitrogen atmosphere, etc. By using an inert gas atmosphere, the by-production of oxides can be reduced or prevented.
[0036] In the addition step in the second core production method, a source of element Z is added to a second raw material mixture heated to a predetermined temperature while maintaining the predetermined temperature. 1 The element Z is gradually added so that the rate of increase in the ratio of the number of atoms of element Z to the number of atoms of element M in the mixture is, for example, 10 / min or less. 1 The ratio of the number of Z atoms to the number of M atoms (Z / M 1 The rate of increase of Z / M 1 The ratio is Z / M after that unit time. 1 The unit time is arbitrarily selected, for example, between 1 second and 1 minute. 1 From the viewpoint of controlling the particle growth of the particles to be produced, the rate of increase in the ratio of the number of atoms of Z to the number of atoms of is preferably 0.0001 / min to 2 / min, more preferably 0.0001 / min to 1 / min, even more preferably 0.001 / min to 0.2 / min, and particularly preferably 0.001 / min to 0.1 / min. Also, it is preferably 0.0002 / min to 2 / min, more preferably 0.002 / min to 0.2 / min.
[0037] The total amount of the source of element Z added is the amount of element M in the final mixture. 1The amount of the element Z to be added is such that the ratio of the number of atoms of element Z to the number of atoms of element Z is 0.1 or more and 5.0 or less, and preferably 1.0 or more and 2.5 or less. The time required for adding the source of element Z may be, for example, 1 minute or more, preferably 5 minutes or more, more preferably 15 minutes or more, even more preferably 20 minutes or more, and is preferably 120 minutes or less, more preferably 60 minutes or less, and even more preferably 40 minutes or less.
[0038] The total amount of the source of element Z added is the amount of element M in the mixture. 1 When the ratio of the number of atoms of element Z to the number of atoms of is 0.1 or more and 2.5 or less, Z / M 1 The rate of increase of the ratio is, for example, 0.0001 / min to 1 / min, preferably 0.001 / min to 0.1 / min. In addition, when the total amount of the source of element Z is 0.001 / min to 0.1 / min, the total amount of the source of element M in the mixture is 0.001 / min to 0.1 / min. 1 When the ratio of the number of atoms of element Z to the number of atoms of is more than 2.5 and is 5.0 or less, Z / M 1 The rate of increase of the ratio is, for example, 0.0002 / min or more and 2 / min or less, and preferably 0.002 / min or more and 0.2 / min or less.
[0039] The supply source of element Z may be added so that the amount added per unit time is approximately the same over the required time. That is, the unit amount obtained by dividing the total amount added of the supply source of element Z by the number obtained by dividing the required time by the unit time may be added as the amount added per unit time. The unit time may be, for example, 1 second, 5 seconds, 10 seconds, 30 seconds, or 1 minute. The supply source of element Z may be added continuously or stepwise. The supply source of element Z may also be added to the mixture, for example, under an inert gas atmosphere.
[0040] The supply source of element Z is the same as the supply source of element Z used in the first core production method. In particular, in the second core production method, a sulfur-containing compound soluble in an organic solvent is preferred as the supply source of element Z, and from the viewpoint of solubility and reactivity, alkylthiourea is preferably used, and 1,3-alkylthiourea is more preferably used. The alkyl group of the alkylthiourea preferably has 1 to 12 carbon atoms, more preferably 1 to 8 carbon atoms, more preferably 1 to 6 carbon atoms, more preferably 1 to 4 carbon atoms, and even more preferably 1 to 3 carbon atoms. When the alkylthiourea has multiple alkyl groups, they may be the same or different.
[0041] The source of element Z may be added to the heated second raw material mixture as a simple substance of element Z or as a solution in which a compound containing element Z is dispersed or dissolved in an organic solvent. When the source of element Z is a solution of a compound containing element Z, the amount of the source of element Z added per unit time in the adding step can be easily controlled, and semiconductor nanoparticles with a narrower particle size distribution can be efficiently produced.
[0042] Examples of organic solvents for dissolving the compound containing element Z, which is the supply source of element Z, include the same organic solvents as those described above, and for example, an amine having a hydrocarbon group having 4 to 20 carbon atoms can be used.
[0043] When the source of element Z is a solution of a compound containing element Z, the concentration of the compound containing element Z is, for example, 1 mmol / L or more and 500 mmol / L or less, and preferably 10 mmol / L or more and 50 mmol / L or less.
[0044] The second core production method may further include a heat treatment step of heat treating the mixture after the addition of the supply source of element Z is completed at a temperature in the range of 120°C to 300°C. The temperature of the heat treatment may be the same as or different from the temperature to which the mixture is heated. From the viewpoint of quantum yield, the temperature of the heat treatment is, for example, 120°C to 300°C, preferably 125°C to 175°C, more preferably 130°C to 160°C, and even more preferably 135°C to 150°C.
[0045] The time of the heat treatment is, for example, 3 seconds or more, preferably 5 minutes or more, 10 minutes or more, or 20 minutes or more, from the viewpoint of the quantum efficiency of the semiconductor nanoparticles. The upper limit of the heat treatment time is not particularly limited, but can be, for example, 60 minutes or less. The time of the heat treatment is set to the time when a predetermined temperature is reached (for example, the time when 140°C is reached in the case of 140°C), and the time when the operation for lowering the temperature is performed is set to the time when the heat treatment is ended.
[0046] The heat treatment is preferably performed in an inert gas atmosphere, such as an argon atmosphere or a nitrogen atmosphere, which can reduce or prevent the production of oxides as by-products.
[0047] The second core production method may include a cooling step of lowering the temperature of the solution containing semiconductor nanoparticles following the above steps. The cooling step is started when an operation for lowering the temperature is performed and is ended when the temperature is cooled to 50° C. or less.
[0048] The cooling step may include a period during which the temperature is lowered at a rate of 50° C. / min or more in order to suppress the generation of silver sulfide from unreacted Ag salts. For example, the rate may be 50° C. / min or more at the time when the temperature lowering operation is started after the temperature lowering operation is performed.
[0049] The cooling step is preferably performed in an inert gas atmosphere, such as an argon atmosphere or a nitrogen atmosphere. By using an inert gas atmosphere, the production of oxides as by-products can be reduced or prevented.
[0050] The first core manufacturing method or the second core manufacturing method may further include a separation step of separating the obtained semiconductor nanoparticles from the solution, and may further include a purification step as necessary. In the separation step, for example, the solution containing the semiconductor nanoparticles may be centrifuged to extract a supernatant containing the semiconductor nanoparticles. In the purification step, for example, an appropriate organic solvent such as alcohol may be added to the supernatant obtained in the separation step and centrifuged to extract the semiconductor nanoparticles as a precipitate. The semiconductor nanoparticles can also be extracted by volatilizing the organic solvent from the supernatant. The extracted precipitate may be dried, for example, by vacuum degassing, natural drying, or a combination of vacuum degassing and natural drying. Natural drying may be performed, for example, by leaving the mixture in the air at room temperature and normal pressure, and in that case, the mixture may be left for 20 hours or more, for example, about 30 hours. The extracted precipitate may also be dispersed in an appropriate organic solvent.
[0051] In the first core production method or the second core production method, a purification step involving addition of an organic solvent such as alcohol and centrifugation may be carried out multiple times as necessary. As the alcohol used for purification, a lower alcohol having 1 to 4 carbon atoms such as methanol, ethanol, or n-propyl alcohol may be used. When dispersing the precipitate in an organic solvent, as the organic solvent, a halogen-based solvent such as chloroform, or a hydrocarbon-based solvent such as toluene, cyclohexane, hexane, pentane, or octane may be used.
[0052] Mixing process In the mixing step in the method for producing core-shell semiconductor nanoparticles, a compound (first element source) containing at least one first element selected from the group consisting of Al, Ga, In, and Tl, and at least one simple substance of a second element and a compound containing the second element (second element source) which is at least one selected from the group consisting of S, Se, and Te are mixed in a mixing ratio in which the ratio of the total number of atoms of the first element to the sum of the total number of atoms of the first element and the total number of atoms of the second element (hereinafter also referred to as the first element ratio) is, for example, greater than 0.5, to obtain a mixture for forming a shell. The first element ratio in the mixture for forming a shell is preferably 0.6 or more, or 0.7 or more. The upper limit of the first element ratio is, for example, less than 1, and is preferably 0.98 or less, or 0.95 or less.
[0053] The mixture for forming the shell may be obtained by mixing the prepared core, the first element source, and the second element source in an organic solvent. The organic solvent may be at least one selected from nitrogen-containing compounds having a hydrocarbon group with a carbon number of 4 to 20, or at least one selected from sulfur-containing compounds having a hydrocarbon group with a carbon number of 4 to 20, or may be a mixture of these.
[0054] The cores to be prepared may be used as a dispersion to form the mixture for forming the shell. In the liquid in which the cores, which are semiconductor nanoparticles, are dispersed, no scattered light occurs, so the dispersion is generally obtained as a transparent (colored or colorless) one. The solvent for dispersing the cores can be any organic solvent, as in the case of preparing the cores. For example, the organic solvent can be at least one selected from nitrogen-containing compounds having a hydrocarbon group with 4 to 20 carbon atoms, or at least one selected from sulfur-containing compounds having a hydrocarbon group with 4 to 20 carbon atoms, or a combination of at least one selected from nitrogen-containing compounds having a hydrocarbon group with 4 to 20 carbon atoms and at least one selected from sulfur-containing compounds having a hydrocarbon group with 4 to 20 carbon atoms. The nitrogen-containing compound is preferably higher than the reaction temperature, in particular because it is easy to obtain a compound with a particularly high purity and because its boiling point exceeds 290°C. Specific examples of the organic solvent include oleylamine, n-tetradecylamine, dodecanethiol, and combinations thereof.
[0055] The core dispersion has a particle concentration of, for example, 5.0×10 -8 mol / liter or more 5.0 x 10 -4 moles / liter or less, especially 1.0 x 10 -7 mol / liter or more 5.0 x 10 -5 The particle ratio in the dispersion may be adjusted to 5.0×10 -8 If the concentration is more than 5.0×10 -4 If the concentration is less than mol / L, Ostwald ripening of the material that constitutes the core and fusion due to collisions are suppressed, and the particle size distribution tends to be suppressed from becoming broad. The particle concentration is calculated based on the value obtained by dividing the number of particles contained in the dispersion by the Avogadro number.
[0056] The first element source is a compound containing at least one of Group 13 elements selected from the group consisting of Al, Ga, In, and Tl, and is, for example, an organic acid salt, an inorganic acid salt, or an organometallic compound of the first element. Specific examples of the first element source include inorganic acid salts such as nitrates, sulfates, hydrochlorides, and sulfonates; and organic acid salts such as acetates and acetylacetonate complexes, with organic acid salts such as acetates and acetylacetonate complexes being preferred. This is believed to be because organic acid salts have high solubility in organic solvents and tend to facilitate the reaction to proceed more uniformly.
[0057] The first element source may be a salt containing at least one of In and Ga. The salt containing at least one of In and Ga may be an organic acid salt such as an acetate or an acetylacetonate complex, or an inorganic acid salt such as a sulfate, a hydrochloride, or a sulfonate. Preferably, the salt may be an acetate or an acetylacetonate complex.
[0058] The second element source is a simple substance of a Group 16 element selected from the group consisting of S, Se, and Te, or a compound containing a Group 16 element. For example, when S is used as the second element to constitute the shell, the sulfur source may be simple sulfur such as high-purity sulfur, or a sulfur-containing compound such as thiols such as n-butanethiol, isobutanethiol, n-pentanethiol, n-hexanethiol, octanethiol, decanethiol, dodecanethiol, hexadecanethiol, and octadecanethiol, a disulfide such as dibenzyl sulfide, an alkylthiourea such as thiourea and 1,3-dimethylthiourea, and a thiocarbonyl compound. Among them, when thiourea, alkylthiourea, or the like is used as the sulfur source, a shell is sufficiently formed, and it is easy to obtain core-shell type semiconductor nanoparticles that give strong band edge emission.
[0059] When Se is used as the second element of the shell, the second element source may be selenium alone, or a compound such as a selenized phosphine oxide, an organic selenium compound (dibenzyl diselenide, diphenyl diselenide, etc.), or a hydride.When Te is used as the second element of the shell, the second element source may be tellurium alone, a tellurized phosphine oxide, or a hydride.
[0060] The mixture for forming the shell may contain an alkali metal salt in addition to the first element source and the second element source. The alkali metal includes lithium (Li), sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), etc. The alkali metal salt may be either an organic acid salt or an inorganic acid salt. Specifically, the salt may be a nitrate, acetate, sulfate, hydrochloride, sulfonate, acetylacetonate, etc., and is preferably at least one selected from the group consisting of these, and more preferably an organic acid salt such as acetate.
[0061] When the shell-forming mixture contains an alkali metal salt, the ratio of the alkali metal salt to the first element source may be, for example, 0.1 to 5, or 0.2 to 4. The ratio of the second element source to the sum of the alkali metal salt and the first element source may be, for example, 0.3 to 3, or 0.5 to 2.
[0062] The amounts of the first and second element sources in the shell-forming mixture may be selected in consideration of the amount of cores contained in the dispersion, so that a shell of desired thickness is formed on the cores present in the dispersion. For example, the amounts of the first and second element sources may be determined so that 0.1 μmol to 10 mmol, particularly 5 μmol to 1 mmol, of a semiconductor compound having a stoichiometric composition consisting of the first and second elements is generated per 10 nmol of substance as core particles. Note that the amount of substance as particles refers to the molar amount when one particle is regarded as a giant molecule, and the number of nanoparticles contained in the dispersion is determined using Avogadro's number (NA=6.022×10 23 ) divided by
[0063] The content of the first element source relative to the amount of substance of the core in the mixture for forming the shell is, for example, 1.6 or more, preferably 1.6×10 3 More preferably, it is 1×10 4 or more, for example, 2.5 × 10 5 or less, preferably 1.3×10 5 The content of the second element source relative to the content of the core is, for example, 5.3 × 10 or more, preferably 5.3 × 10 or less, as a molar ratio of the second element source to the number of particles (moles) of the core. 2 or more, for example, 8.5×10 4 or less, preferably 4.3×10 4 The following is the result.
[0064] Heat Treatment Process In one embodiment of the heat treatment step in the method for producing core-shell semiconductor nanoparticles, for example, the mixture for forming the shell is heat-treated at a predetermined temperature to form a semiconductor layer as the shell on the surface of the semiconductor nanoparticle as the core to obtain the core-shell semiconductor nanoparticle (heating-up method). Specifically, the mixture for forming the shell may be gradually heated to a peak temperature of 200°C or more and 310°C or less, and the mixture may be heated in such a manner that the peak temperature is maintained for a predetermined time, and then the temperature is gradually lowered. The heating rate may be, for example, 1°C / min or more and 50°C / min or less, but in order to minimize the deterioration of the core caused by continuing the heat treatment in the absence of a shell, it is preferable that the heating rate is 50°C / min or more and 100°C / min or less up to 200°C. In addition, if it is desired to further increase the temperature to 200°C or more, it is preferable that the heating rate is 1°C / min or more and 5°C / min or less thereafter. The heating rate may be, for example, 1°C / min or more and 50°C / min or less. If the peak temperature is above the above temperature, the surface modifier modifying the semiconductor nanoparticles is sufficiently removed, or the chemical reaction for generating the shell proceeds sufficiently, so that the semiconductor layer (shell) tends to be sufficiently formed. If the peak temperature is below the above temperature, the semiconductor nanoparticles are prevented from being altered, and good band edge emission tends to be obtained. The time for holding the peak temperature can be, for example, from 1 minute to 300 minutes, particularly from 10 minutes to 120 minutes. The holding time of the peak temperature is selected in relation to the peak temperature, and if the holding time is longer when the peak temperature is lower, and shorter when the peak temperature is higher, a good shell layer is likely to be formed.
[0065] Another embodiment of the heat treatment step in the method for producing core-shell semiconductor nanoparticles may be a one-stage heat treatment step in which the mixture for forming the shell is heat-treated at a predetermined temperature, or a two-stage heat treatment step in which the mixture is heat-treated at a first temperature and then at a second temperature higher than the first temperature. By carrying out the heat treatment in two stages, for example, it is possible to produce core-shell semiconductor nanoparticles having high band edge emission intensity with better reproducibility. Here, the heat treatment at the first temperature and the heat treatment at the second temperature may be carried out continuously, or the heat treatment at the first temperature may be followed by lowering the temperature and then raising the temperature to the second temperature for heat treatment.
[0066] When the heat treatment of the shell-forming mixture is carried out in a two-stage heat treatment process, the first temperature may be, for example, 30° C. or higher, and preferably 100° C. or higher. The first temperature may be, for example, 200° C. or lower, and preferably 180° C. or lower. The time of the heat treatment at the first temperature may be, for example, 1 minute or higher, and preferably 5 minutes or higher, and more preferably 7 minutes or higher. The time of the heat treatment at the first temperature may be, for example, 120 minutes or lower, and preferably 60 minutes or lower, and more preferably 30 minutes or lower or 20 minutes or lower.
[0067] The second temperature may be, for example, 180° C. or higher, and preferably 200° C. or higher. The second temperature may be, for example, 350° C. or lower, and preferably 330° C. or lower or 310° C. or lower. The time of the heat treatment at the second temperature may be, for example, 1 minute or more, and preferably 5 minutes or more, and more preferably 10 minutes or more or 20 minutes or more. The time of the heat treatment at the second temperature may be, for example, 120 minutes or less, and preferably 90 minutes or less, and more preferably 60 minutes or less or 40 minutes or less.
[0068] The time of the heat treatment is defined as the start time of the heat treatment when a predetermined temperature is reached, and the end time of the heat treatment at the predetermined temperature is defined as the time when the operation for lowering or raising the temperature is performed. The rate of temperature rise until the predetermined temperature is reached is, for example, 1°C / min to 100°C / min, or 1°C / min to 50°C / min. The rate of temperature fall after the heat treatment is, for example, 1°C / min to 100°C / min, and the material may be cooled as necessary, or the heat source may be stopped and the material may be allowed to cool.
[0069] The heat treatment is preferably performed in an inert gas atmosphere, such as an argon atmosphere or a nitrogen atmosphere, which can reduce or prevent the production of oxides as by-products.
[0070] In this way, the shell is formed to form core-shell type semiconductor nanoparticles having a core-shell structure. The obtained core-shell type semiconductor nanoparticles may be separated from the solvent, and may be further purified and dried as necessary. The methods of separation, purification and drying are as described above in relation to the method for producing the core, which is the semiconductor nanoparticle, and therefore detailed description thereof will be omitted here.
[0071] In one embodiment, the method for producing core-shell semiconductor nanoparticles may include a step of adding an oxygen source to a shell-forming mixture. That is, the method for producing core-shell semiconductor nanoparticles may include a core preparation step, a mixing step, and a heat treatment step, and the mixing step may include obtaining a shell-forming mixture containing an oxygen source. By including an oxygen source in the shell-forming mixture subjected to the heat treatment step, core-shell semiconductor nanoparticles having superior luminous efficiency can be produced.
[0072] In the present embodiment, the mixture for forming the shell obtained in the mixing step contains an oxygen source. In the mixing step, the prepared core, the first element source, the second element source, and the oxygen source are mixed to obtain the mixture for forming the shell.
[0073] In one embodiment, the method for producing core-shell semiconductor nanoparticles may include a step of adding an oxygen source to the shell-forming mixture in the heat treatment step. That is, the method for producing core-shell semiconductor nanoparticles may include a core preparation step, a mixing step, and a heat treatment step, and the heat treatment step may include adding an oxygen source to the shell-forming mixture. By adding an oxygen source to the heated shell-forming mixture, core-shell semiconductor nanoparticles with superior luminous efficiency can be produced.
[0074] In this embodiment, the oxygen source is added while the mixture for forming the shell obtained in the mixing step is heat-treated. When the shell is formed by a single-stage heat treatment, the oxygen source may be added during the heat treatment at the peak temperature, during the temperature rise to the peak temperature, or during the temperature fall from the peak temperature. When the heat treatment for forming the shell is performed in two stages, the oxygen source may be added during the heat treatment at the first temperature, after the heat treatment at the first temperature, or during the heat treatment at the second temperature. In addition to adding the oxygen source in the heat treatment step, the mixture for forming the shell before the heat treatment may already contain the oxygen source.
[0075] In one embodiment, the method for producing core-shell semiconductor nanoparticles may include a step of contacting an oxygen source with the core-shell semiconductor nanoparticles obtained in the heat treatment step. That is, the method for producing core-shell semiconductor nanoparticles may include a core preparation step, a mixing step, and a heat treatment step, and may include a step of contacting an oxygen source with the core-shell semiconductor nanoparticles obtained after the heat treatment step. By contacting the oxygen source with the core-shell semiconductor nanoparticles obtained from the shell-forming mixture to introduce oxygen atoms into the shell, it is possible to produce core-shell semiconductor nanoparticles with superior luminous efficiency.
[0076] In this embodiment, an oxygen source is contacted with the core-shell semiconductor nanoparticles obtained in the heat treatment step to introduce oxygen atoms into the shell. The core-shell semiconductor nanoparticles to be contacted with the oxygen source may be unpurified after the heat treatment step, or may be purified. The core-shell semiconductor nanoparticles to be contacted with the oxygen source may be obtained from a shell-forming mixture containing an oxygen source, or may be obtained by adding an oxygen source to the shell-forming mixture in the heat treatment step.
[0077] The oxygen source is not particularly limited as long as it can introduce oxygen atoms into the shell composition. Specific examples of the oxygen source include compounds containing oxygen atoms and gases containing oxygen atoms. Examples of compounds containing oxygen atoms include water and alcohol, and at least one selected from the group consisting of these is preferable. Examples of gases containing oxygen atoms include oxygen gas and ozone gas, and at least one selected from the group consisting of these is preferable. The oxygen source may be added by dissolving or dispersing a compound containing oxygen atoms in the mixture for forming the shell, or by blowing a gas containing oxygen atoms into the mixture for forming the shell.
[0078] The amount of the oxygen source added or used is, for example, in the case of water, 6000 ppm or less, preferably 3000 ppm or less, or 1000 ppm or less based on the weight of the solvent.
[0079] When the shell surface of the core-shell semiconductor nanoparticles is modified with a specific modifying agent described below, the core-shell semiconductor nanoparticles obtained by the above manufacturing method may be subjected to a modification step. In the modification step, the core-shell semiconductor nanoparticles are contacted with a specific modifying agent containing phosphorus (P) having a negative oxidation number to modify the shell surface of the core-shell particles. This produces core-shell semiconductor nanoparticles that exhibit band edge emission with a better quantum yield.
[0080] The contact between the core-shell type semiconductor nanoparticles and the specific modifier can be carried out, for example, by mixing a dispersion of the core-shell type semiconductor nanoparticles with the specific modifier. The core-shell particles may also be mixed with a liquid specific modifier. The specific modifier may be used in its solution. The dispersion of the core-shell type semiconductor nanoparticles can be obtained by mixing the core-shell type semiconductor nanoparticles with a suitable organic solvent. Examples of the organic solvent used for dispersion include halogenated solvents such as chloroform; aromatic hydrocarbon solvents such as toluene; and aliphatic hydrocarbon solvents such as cyclohexane, hexane, pentane, and octane. The concentration of the substance amount in the dispersion of the core-shell type semiconductor nanoparticles is, for example, 1×10 -7 mol / L or more 1×10 -3mol / L or less, preferably 1×10 -6 mol / L or more 1×10 -4 mol / L or less.
[0081] The amount of the specific modifier used relative to the core-shell type semiconductor nanoparticles is, for example, 1 to 50,000 times in terms of molar ratio. -7 mol / L or more 1.0×10 -3 When a dispersion of core-shell type semiconductor nanoparticles having a concentration of mol / L or less is used, the dispersion and the specific modifying agent may be mixed at a volume ratio of 1:1000 to 1000:1.
[0082] The temperature during contact between the core-shell semiconductor nanoparticles and the specific modifying agent is, for example, from -100°C to 100°C or from 30°C to 75°C. The contact time may be appropriately selected depending on the amount of the specific modifying agent used, the concentration of the dispersion liquid, and the like. The contact time is, for example, 1 minute or more, preferably 1 hour or more, and 100 hours or less, preferably 48 hours or less. The atmosphere during contact is, for example, an inert gas atmosphere such as nitrogen gas or a rare gas.
[0083] Core-shell type semiconductor nanoparticles The core-shell semiconductor nanoparticles have a core and a shell disposed on the surface of the core, and emit light when irradiated with light. 1 , element M 2 and the element Z. 1 is at least one element selected from the group consisting of silver (Ag), copper (Cu), gold (Au) and alkali metals, and contains at least Ag. 2 is at least one element selected from the group consisting of aluminum (Al), gallium (Ga), indium (In) and thallium (Tl), and includes at least one of In and Ga. Z includes at least one element selected from the group consisting of sulfur (S), selenium (Se) and tellurium (Te). The composition of the core is 1 The total content of M is 10 mol % or more and 30 mol % or less, 2The total content of is 15 mol% or more and 35 mol% or less, and the total content of Z is 35 mol% or more and 55 mol% or less. The shell is essentially composed of a first element which is at least one selected from the group consisting of Al, Ga, In, and Tl, a second element which is at least one selected from the group consisting of S, Se, and Te, and oxygen (O).
[0084] In the core-shell type semiconductor nanoparticles, the core itself contains semiconductor nanoparticles, and the shell contains oxygen in addition to the first and second elements, so that excellent luminous efficiency can be achieved. The core-shell type semiconductor nanoparticles emit light having an emission peak wavelength in the range of 500 nm to 1000 nm and a half width in the emission spectrum of, for example, 250 meV or less when irradiated with light having a wavelength in the range of, for example, 200 nm to less than 500 nm. The half width is preferably 200 meV or less, more preferably 150 meV or less. The lower limit of this half width is, for example, 30 meV or more. The half width being 250 meV or less means that when the emission peak wavelength is 600 nm, the half width is 73 nm or less, when the emission peak wavelength is 700 nm, the half width is 100 nm or less, and when the emission peak wavelength is 800 nm, the half width is 130 nm or less, which means that the core-shell type semiconductor nanoparticles emit light at the band edge.
[0085] Core-shell type semiconductor nanoparticles, whose core composition includes Ag, at least one of In and Ga, and S, Se, or Te, and whose shell composition includes a first element, a second element, and an oxygen element, provide band edge emission due to their shape and size. Furthermore, the core-shell type semiconductor nanoparticles can be made to have a composition that does not include Cd and Pb, which are considered to be highly toxic, and can be applied to products in which the use of Cd, etc. is prohibited. Therefore, these semiconductor nanoparticles can be suitably used as wavelength conversion materials for light-emitting devices used in liquid crystal displays, as well as biomolecular markers, etc.
[0086] The total content of Ag, Cu, Au and alkali metals in the core composition is, for example, 10 mol% to 30 mol%, preferably 15 mol% to 25 mol%. The total content of Al, Ga, In and Tl in the core composition is, for example, 15 mol% to 35 mol%, preferably 20 mol% to 30 mol%. The total content of S, Se and Te in the core composition is, for example, 35 mol% to 55 mol%, preferably 40 mol% to 55 mol%.
[0087] When the core contains In and Ga, the ratio of the number of In atoms to the sum of the number of In and Ga atoms in the composition (In / (In+Ga)) is, for example, 0.01 or more and 1.0 or less, preferably 0.1 or more and 0.99 or less. In addition, the ratio of the sum of the number of Ag atoms to the sum of the number of In and Ga atoms in the core composition (Ag / (In+Ga)) is, for example, 0.3 or more and 1.2 or less, preferably 0.5 or more and 1.1 or less. When the core contains S, the ratio of the number of S atoms to the sum of the number of Ag, In and Ga atoms in the core composition (S / (Ag+In+Ga)) is, for example, 0.8 or more and 1.5 or less, preferably 0.9 or more and 1.2 or less.
[0088] The composition of the core is identified, for example, by energy dispersive X-ray spectrometry (EDX), X-ray fluorescence spectrometry (XRF), inductively coupled plasma (ICP) optical emission spectrometry, etc. The composition ratios such as (Ag) / (In+Ga), S / (Ag+In+Ga), etc. are calculated based on the composition identified by any of these methods.
[0089] In the composition of the core, Ag may be partially substituted with at least one of Cu and Au, but it is preferable that the core is substantially composed of Ag. Here, "substantially" means that the ratio of elements other than Ag to Ag is, for example, 10 mol % or less, preferably 5 mol % or less, and more preferably 1 mol % or less.
[0090] When the core contains an alkali metal, the content of the alkali metal is, for example, less than 30 mol %, and preferably 1 mol % or more and 25 mol % or less. a ) relative to the total number of atoms of alkali metals (M a ) atomic number ratio (M a / (Ag+M a )) is, for example, less than 1, preferably 0.8 or less, more preferably 0.4 or less, and even more preferably 0.2 or less. The ratio is, for example, greater than 0, preferably 0.05 or more, and more preferably 0.1 or more. The alkali metal preferably contains at least Li, and is preferably substantially Li. Here, "substantially" means that the ratio of alkali metals other than Li to Li is, for example, 10 mol % or less, preferably 5 mol % or less, and more preferably 1 mol % or less.
[0091] In the core composition, at least one of In and Ga may be partially substituted with at least one of Al and Tl, but it is preferable that the core is substantially composed of at least one of In and Ga. Here, "substantially" means that the ratio of elements other than In or Ga to In and Ga is, for example, 10 mol % or less, preferably 5 mol % or less, and more preferably 1 mol % or less.
[0092] When the core contains S, the S may be partially substituted with at least one of Se and Te, or may be substantially composed of S. Here, "substantially" means that the ratio of elements other than S to S is, for example, 10 mol % or less, preferably 5 mol % or less, and more preferably 1 mol % or less.
[0093] The core may be composed substantially of at least one of Ag, In, and Ga, and S. Here, the term "substantially" is used in consideration of the fact that elements other than Ag, In, Ga, and S are inevitably included due to the inclusion of impurities, etc.
[0094] The crystal structure of the core may include at least one selected from the group consisting of tetragonal, hexagonal, and orthorhombic. For example, semiconductor nanoparticles containing Ag, In, and S and having a tetragonal, hexagonal, or orthorhombic crystal structure are generally introduced in literature as being represented by the composition formula AgInS2. The core according to this embodiment can be considered to be, for example, a group 13 element, with Ga substituted for a part of In. The composition of the core may be, for example, represented by Ag-In-Ga-S.
[0095] In addition, among semiconductor nanoparticles represented by a composition formula such as Ag-In-Ga-S, those having a hexagonal crystal structure are wurtzite type, and those having a tetragonal crystal structure are chalcopyrite type. The crystal structure is identified, for example, by measuring an XRD pattern obtained by X-ray diffraction (XRD) analysis. Specifically, the XRD pattern obtained from the semiconductor nanoparticles is compared with a known XRD pattern assuming that the semiconductor nanoparticles are represented by a composition of AgInS2, or an XRD pattern obtained by performing a simulation from crystal structure parameters. If any of the known patterns and the simulation patterns match the pattern of the semiconductor nanoparticles, the crystal structure of the semiconductor nanoparticles can be said to be the crystal structure of the matching known or simulation pattern.
[0096] In the core aggregate, cores of different crystal structures may be mixed in part, in which case peaks derived from a plurality of crystal structures are observed in the XRD pattern.
[0097] The core may have an average particle size of, for example, 50 nm or less. The average particle size of the core may be, for example, 20 nm or less, 10 nm or less, or less than 10 nm. When the average particle size of the core is 50 nm or less, quantum size effect tends to be easily obtained, and band edge emission tends to be easily obtained. The lower limit of the average particle size of the core is, for example, 1 nm.
[0098] The particle size of the core can be determined, for example, from a TEM image taken using a transmission electron microscope (TEM). Specifically, the particle size of a particle is determined as the length of the longest line segment among the line segments that connect any two points on the periphery of a particle observed in a TEM image and that pass through the inside of the particle.
[0099] However, when the particle has a rod shape, the length of the short axis is regarded as the particle size. Here, a rod-shaped particle refers to a particle having a short axis and a long axis perpendicular to the short axis in a TEM image, and the ratio of the length of the long axis to the length of the short axis is greater than 1.2. A rod-shaped particle is observed in a TEM image, for example, as a quadrangle including a rectangular shape, an ellipse, or a polygon. The shape of the cross section, which is a surface perpendicular to the long axis of the rod shape, may be, for example, a circle, an ellipse, or a polygon. Specifically, for a particle having a rod-like shape, the length of the long axis refers to the length of the longest line segment among the line segments connecting any two points on the periphery of the particle in the case of an ellipse, and refers to the length of the longest line segment among the line segments that are parallel to the longest side that defines the periphery and connect any two points on the periphery of the particle in the case of a rectangular or polygonal shape. The length of the short axis refers to the length of the line segment that is perpendicular to the line segment that defines the length of the longest axis among the line segments connecting any two points on the periphery.
[0100] The average core diameter is the arithmetic mean of the diameters of all measurable particles observed in a TEM image at magnifications of 50,000 to 150,000. Here, measurable particles are those whose entirety can be observed in a TEM image. Therefore, particles that are not partly included in the imaging range in a TEM image and are cut off are not measurable. If the number of measurable particles in one TEM image is 100 or more, the average diameter is determined using that TEM image. On the other hand, if the number of measurable particles in one TEM image is less than 100, the imaging location is changed, another TEM image is obtained, and the diameters of 100 or more measurable particles in two or more TEM images are measured to determine the average diameter.
[0101] The core, which is a semiconductor nanoparticle, may be capable of band edge emission. The core may emit light with an emission peak wavelength in the range of 500 nm to 650 nm by irradiating light with a wavelength in the range of 200 nm to less than 500 nm. The half width in the emission spectrum of the core is 250 meV or less, preferably 200 meV or less, more preferably 150 meV or less. The lower limit of this half width is, for example, 30 meV or more. The half width being 250 meV or less means that when the emission peak wavelength is 600 nm, the half width is 73 nm or less, when the emission peak wavelength is 700 nm, the half width is 100 nm or less, and when the emission peak wavelength is 800 nm, the half width is 130 nm or less, which means that the semiconductor nanoparticle emits band edge light.
[0102] The core may provide other emission such as defect emission in addition to the band edge emission. Defect emission generally has a long emission lifetime and a broad spectrum, with its peak at a longer wavelength than the band edge emission. When both band edge emission and defect emission are obtained, it is preferable that the intensity of the band edge emission is greater than that of the defect emission.
[0103] The peak position of the band edge emission of the core can be changed by changing at least one of the shape and average grain size of the core, particularly the average grain size. For example, if the average grain size of the core is made smaller, the band gap energy becomes larger due to the quantum size effect, and the peak wavelength of the band edge emission can be shifted to the shorter wavelength side.
[0104] In addition, the peak wavelength of the band edge emission of the core can be changed by changing the core composition. For example, the peak wavelength of the band edge emission can be shifted to the shorter wavelength side by increasing the Ga ratio (Ga / (In+Ga)), which is the ratio of the number of Ga atoms to the sum of the numbers of In and Ga atoms in the composition. In addition, by selecting Li as an alkali metal and increasing the number of Ag and alkali metals (M a ) relative to the sum of the number of atoms of alkali metals (M a) is the ratio of the number of atoms in a Ratio(M a / (Ag+M a ) can be increased to shift the emission peak wavelength of the band edge emission to the shorter wavelength side. In addition, for example, by substituting part of the S in the composition with Se and increasing the S ratio (S / (S+Se)), which is the ratio of the number of S atoms to the sum of the numbers of S and Se atoms, the emission peak wavelength of the band edge emission can be shifted to the shorter wavelength side.
[0105] The absorption spectrum of the core may show an exciton peak. The exciton peak is a peak obtained by exciton generation, and the fact that it appears in the absorption spectrum means that the core particle group is composed of particles suitable for band edge emission with a small particle size distribution and few crystal defects. In addition, the steeper the exciton peak, the more particles with uniform particle size and few crystal defects are contained in the core particle aggregate. Therefore, if the exciton peak is steep, the half width of the emission will be narrow, and it is expected that the emission efficiency will be improved. In the absorption spectrum of the core, the exciton peak is observed, for example, within the range of 350 nm to 900 nm.
[0106] The core may emit light having an emission peak wavelength on the longer wavelength side than the exciton peak of the absorption spectrum due to the Stokes shift. When the absorption spectrum of the core shows an exciton peak, the energy difference between the exciton peak and the emission peak wavelength is, for example, 300 meV or less.
[0107] Core-shell semiconductor nanoparticles have a core-shell structure in which a semiconductor constituting the shell is disposed on the surface of the core. The shell is a semiconductor having a larger band gap energy than the semiconductor constituting the core, and is composed of a semiconductor containing at least one first element selected from the group consisting of Al, Ga, In, and Tl, which are group 13 elements, at least one second element selected from the group consisting of S, Se, and Te, which are group 16 elements, and oxygen. The semiconductor constituting the shell may contain only one type of group 13 element or two or more types of group 16 element, and may contain only one type of group 16 element or two or more types of group 16 element.
[0108] The shell may be composed of a semiconductor substantially consisting of the first element, the second element, and oxygen, where "substantially" means that, when the total number of atoms of all elements contained in the shell is taken as 100%, the proportion of elements other than the first element, the second element, and oxygen is, for example, 10% or less, preferably 5% or less, and more preferably 1% or less.
[0109] The shell may be configured by selecting its composition depending on the band gap energy of the semiconductor constituting the core. Alternatively, when the composition of the shell is determined in advance, the core may be designed so that the band gap energy of the semiconductor constituting the core is smaller than that of the shell. For example, a semiconductor made of Ag-In-S has a band gap energy of about 1.8 eV or more and 1.9 eV or less.
[0110] Specifically, the semiconductor constituting the shell may have a band gap energy of, for example, 2.0 eV to 5.0 eV, or 2.5 eV to 5.0 eV. The band gap energy of the shell may be, for example, about 0.1 eV to 3.0 eV, about 0.3 eV to 3.0 eV, or about 0.5 eV to 1.0 eV, higher than the band gap energy of the core. If the difference between the band gap energy of the semiconductor constituting the shell and the band gap energy of the semiconductor constituting the core is equal to or greater than the lower limit, the proportion of emission other than band edge emission in the light emission from the core tends to be small, and the proportion of band edge emission tends to be large.
[0111] Furthermore, the band gap energy of the semiconductors constituting the core and shell is preferably selected so as to provide a type-I band alignment in which the band gap energy of the shell sandwiches the band gap energy of the core at the heterojunction of the core and the shell. By forming the type-I band alignment, it is possible to obtain better band edge emission from the core. In the type-I alignment, it is preferable that a barrier of at least 0.1 eV is formed between the band gap of the core and the band gap of the shell, and for example, a barrier of 0.2 eV or more or 0.3 eV or more may be formed. The upper limit of the barrier is, for example, 1.8 eV or less, particularly 1.1 eV or less. If the barrier is equal to or greater than the lower limit, the proportion of emission other than band edge emission in the emission from the core tends to be small, and the proportion of band edge emission tends to be large.
[0112] The semiconductor constituting the shell may contain In or Ga as the first element. The semiconductor constituting the shell may contain S as the second element. Furthermore, the semiconductor constituting the shell may contain oxygen (O). Semiconductors containing In or Ga, S, and O tend to be semiconductors with a larger band gap energy than the above-mentioned core.
[0113] The shell may have a semiconductor crystal system that is similar to that of the core semiconductor, and may have a lattice constant that is the same as or close to that of the core semiconductor. A shell made of a semiconductor that has a similar crystal system and a close lattice constant (here, a shell whose lattice constant is a multiple close to that of the core is also considered to have a close lattice constant) may well cover the periphery of the core. The shell may also be amorphous.
[0114] Whether or not an amorphous shell is formed can be confirmed by observing the core-shell structured semiconductor nanoparticles with HAADF-STEM. When an amorphous shell is formed, specifically, a part having a regular pattern (e.g., striped pattern, dot pattern, etc.) is observed in the center, and a part not observed as having a regular pattern is observed around it in HAADF-STEM. According to HAADF-STEM, a substance having a regular structure such as a crystalline substance is observed as an image having a regular pattern, and a substance not having a regular structure such as an amorphous substance is not observed as an image having a regular pattern. Therefore, when the shell is amorphous, the shell can be observed as a part that is clearly different from the core (which has a crystal structure such as a tetragonal system as described above) observed as an image having a regular pattern.
[0115] Furthermore, when the shell is made of Ga-SO, Ga is a lighter element than Ag and In contained in the core, so that the shell tends to be observed as a darker image than the core in an image obtained by HAADF-STEM.
[0116] Whether or not an amorphous shell is formed can also be confirmed by observing the semiconductor nanoparticles having the core-shell structure of this embodiment with a high-resolution transmission electron microscope (HRTEM). In an image obtained with HRTEM, the core portion is observed as a crystal lattice image (an image having a regular pattern), while the shell portion is observed as a portion in which a black and white contrast is observed but no regular pattern is visible.
[0117] On the other hand, the shell is preferably made of a semiconductor that does not form a solid solution with the core, since if the shell and the core form a solid solution, the two become one, and the mechanism of obtaining band-edge emission by covering the core with the shell and changing the surface state of the core may not be obtained.
[0118] The shell may include, as a combination of the first element and the second element, a combination of In and S, a combination of Ga and S, or a combination of In, Ga and S, but is not limited thereto. The combination of In and S may be in a form in which the shell contains indium sulfide, and the combination of Ga and S may be in a form in which the shell contains gallium sulfide, and the combination of In, Ga and S may be in a form in which the shell contains indium gallium sulfide. The indium sulfide that may constitute the shell does not have to be of stoichiometric composition (In2S3), and in this sense, indium sulfide is represented by the formula InS x (x may be any number, not limited to integers, such as 0.8 to 1.5). Similarly, gallium sulfide does not have to be stoichiometric (Ga2S3), in that sense, gallium sulfide has the formula GaS x (x is not limited to an integer, but may be any number, for example, 0.8 to 1.5). Indium gallium sulfide is represented by In 2(1-y) Ga 2y S3 (where y is any number greater than 0 and less than 1), or In a Ga 1-a S b (where a is any number greater than 0 and less than 1, and b is any number not limited to integers).
[0119] The form of the oxygen element that constitutes the shell is not clear, but may be, for example, Ga-OS, Ga2O3, or the like.
[0120] Indium sulfide has a band gap energy of 2.0 eV to 2.4 eV, and its lattice constant is 1.0775 nm when its crystal system is cubic. Gallium sulfide has a band gap energy of about 2.5 eV to 2.6 eV, and its lattice constant is 0.5215 nm when its crystal system is tetragonal. However, the crystal systems described here are all reported values, and the shell of an actual core-shell semiconductor nanoparticle does not necessarily contain a semiconductor that satisfies these reported values.
[0121] In semiconductor nanoparticles having a core-shell structure, the shell thickness may be in the range of 0.1 to 50 nm, in the range of 0.1 to 10 nm, and particularly in the range of 0.3 to 3 nm. When the shell thickness is equal to or greater than the lower limit, the effect of the shell covering the core is sufficiently obtained, and band edge emission with excellent luminous efficiency is easily obtained.
[0122] The surface of the core-shell type semiconductor nanoparticles may be modified with any compound. The compound that modifies the surface of the semiconductor nanoparticles is also called a surface modifier. The surface modifier has at least one of the following functions: stabilizing the core-shell type semiconductor nanoparticles to prevent particle aggregation or growth, improving the dispersibility of the core-shell type semiconductor nanoparticles in a solvent, and compensating for surface defects of the core-shell type semiconductor nanoparticles to improve the luminous efficiency.
[0123] The surface modifier may be, for example, a nitrogen-containing compound having a hydrocarbon group having 4 to 20 carbon atoms, a sulfur-containing compound having a hydrocarbon group having 4 to 20 carbon atoms, an oxygen-containing compound having a hydrocarbon group having 4 to 20 carbon atoms, a phosphorus-containing compound having a hydrocarbon group having 4 to 20 carbon atoms, etc. Examples of the hydrocarbon group having 4 to 20 carbon atoms include saturated aliphatic hydrocarbon groups such as butyl group, isobutyl group, pentyl group, hexyl group, octyl group, ethylhexyl group, decyl group, dodecyl group, hexadecyl group, and octadecyl group; unsaturated aliphatic hydrocarbon groups such as oleyl group; alicyclic hydrocarbon groups such as cyclopentyl group and cyclohexyl group; aromatic hydrocarbon groups having 6 to 10 carbon atoms such as phenyl group and naphthyl group; and arylalkyl groups such as benzyl group and naphthylmethyl group, among which saturated aliphatic hydrocarbon groups and unsaturated aliphatic hydrocarbon groups are preferred. Examples of the nitrogen-containing compounds include amines and amides, examples of the sulfur-containing compounds include thiols, examples of the oxygen-containing compounds include fatty acids, and examples of the phosphorus-containing compounds include phosphines and phosphine oxides.
[0124] The surface modifier is preferably a nitrogen-containing compound having a hydrocarbon group having a carbon number of 4 to 20. Examples of such nitrogen-containing compounds include alkylamines such as butylamine, isobutylamine, pentylamine, hexylamine, octylamine, ethylhexylamine, decylamine, dodecylamine, hexadecylamine, and octadecylamine, and alkenylamines such as oleylamine.
[0125] The surface modifier is preferably a sulfur-containing compound having a hydrocarbon group having 4 to 20 carbon atoms. Examples of such sulfur-containing compounds include butanethiol, isobutanethiol, pentanethiol, hexanethiol, octanethiol, ethylhexanethiol, decanethiol, dodecanethiol, hexadecanethiol, and octadecanethiol.
[0126] The surface modifier may be used alone or in combination of two or more different types. For example, a compound selected from the nitrogen-containing compounds exemplified above (e.g., oleylamine) may be used in combination with a compound selected from the sulfur-containing compounds exemplified above (e.g., dodecanethiol).
[0127] The shell surface of the core-shell semiconductor nanoparticles may be modified with a surface modifier containing phosphorus (P) having a negative oxidation number (hereinafter also referred to as a "specific modifier"). When the shell surface modifier contains the specific modifier, the quantum efficiency of the band edge emission of the core-shell semiconductor nanoparticles is further improved.
[0128] The specific modifier contains P, which has a negative oxidation number as a Group 15 element. The oxidation number of P is -1 when one hydrogen atom or a hydrocarbon group is bonded to P, and +1 when one oxygen atom is bonded to P via a single bond, and changes depending on the substitution state of P. For example, the oxidation number of P in trialkylphosphine and triarylphosphine is -3, and in trialkylphosphine oxide and triarylphosphine oxide, it is -1.
[0129] The specific modifier may contain other Group 15 elements in addition to P having a negative oxidation number. Examples of other Group 15 elements include N, As, and Sb.
[0130] The specific modifying agent may be, for example, a phosphorus-containing compound having a hydrocarbon group having 4 to 20 carbon atoms. Examples of the hydrocarbon group having 4 to 20 carbon atoms include linear or branched saturated aliphatic hydrocarbon groups such as n-butyl, isobutyl, n-pentyl, n-hexyl, octyl, ethylhexyl, decyl, dodecyl, tetradecyl, hexadecyl, and octadecyl groups; linear or branched unsaturated aliphatic hydrocarbon groups such as oleyl; alicyclic hydrocarbon groups such as cyclopentyl and cyclohexyl groups; aromatic hydrocarbon groups such as phenyl and naphthyl groups; and arylalkyl groups such as benzyl and naphthylmethyl groups. Of these, saturated aliphatic hydrocarbon groups and unsaturated aliphatic hydrocarbon groups are preferred. When the specific modifying agent has a plurality of hydrocarbon groups, they may be the same or different.
[0131] Specific examples of the specific modifying agent include tributylphosphine, triisobutylphosphine, tripentylphosphine, trihexylphosphine, trioctylphosphine, tris(ethylhexyl)phosphine, tridecylphosphine, tridodecylphosphine, tritetradecylphosphine, trihexadecylphosphine, trioctadecylphosphine, triphenylphosphine, tributylphosphine oxide, triisobutylphosphine oxide, tripentylphosphine oxide, trihexylphosphine oxide, trioctylphosphine oxide, tris(ethylhexyl)phosphine oxide, tridecylphosphine oxide, tridodecylphosphine oxide, tritetradecylphosphine oxide, trihexadecylphosphine oxide, trioctadecylphosphine oxide, and triphenylphosphine oxide. At least one selected from the group consisting of these is preferred.
[0132] Light Emitting Device The light-emitting device includes a light conversion member and a semiconductor light-emitting element, and the light conversion member contains the core-shell type semiconductor nanoparticles described above. According to this light-emitting device, for example, a part of the light emitted from the semiconductor light-emitting element is absorbed by the core-shell type semiconductor nanoparticles to emit light of a longer wavelength. Then, the light from the core-shell type semiconductor nanoparticles and the remaining part of the light emitted from the semiconductor light-emitting element are mixed, and the mixed light can be used as the light emitted by the light-emitting device.
[0133] Specifically, a light-emitting device that emits white light can be obtained by using a semiconductor light-emitting element that emits blue-violet or blue light with a peak wavelength of about 400 nm to 490 nm and semiconductor nanoparticles that absorb blue light and emit yellow light. Alternatively, a white light-emitting device can be obtained by using two types of semiconductor nanoparticles, one that absorbs blue light and emits green light, and one that absorbs blue light and emits red light.
[0134] Alternatively, a white light-emitting device can be obtained by using a semiconductor light-emitting element that emits ultraviolet light with a peak wavelength of 400 nm or less and three types of semiconductor nanoparticles that absorb the ultraviolet light and emit blue light, green light, and red light, respectively. In this case, it is desirable to have all the light from the light-emitting element absorbed and converted by the semiconductor nanoparticles so that the ultraviolet light emitted from the light-emitting element does not leak to the outside.
[0135] Alternatively, a device that emits white light can be obtained by using a semiconductor light-emitting element that emits blue-green light with a peak wavelength of approximately 490 nm or more and 510 nm or less, and using semiconductor nanoparticles that absorb the blue-green light and emit red light.
[0136] Alternatively, a light-emitting device that emits near-infrared radiation can be obtained by using a semiconductor light-emitting element that emits red light with a wavelength of 700 nm or more and 780 nm or less, and semiconductor nanoparticles that absorb the red light and emit near-infrared radiation.
[0137] The core-shell semiconductor nanoparticles may be used in combination with other semiconductor quantum dots, or may be used in combination with other phosphors that are not quantum dots (e.g., organic phosphors or inorganic phosphors). Other semiconductor quantum dots are, for example, binary semiconductor quantum dots described in the Background Art section. As phosphors that are not quantum dots, garnet phosphors such as aluminum garnet phosphors can be used. Garnet phosphors include yttrium-aluminum-garnet phosphors activated with cerium, and lutetium-aluminum-garnet phosphors activated with cerium. Other examples include nitrogen-containing calcium aluminosilicate phosphors activated with europium and / or chromium, silicate phosphors activated with europium, β-SiAlON phosphors, nitride phosphors such as CASN or SCASN, LnSi3N 11 rare earth nitride phosphors such as BaSi2O2N2:Eu or Ba3Si6O 12 Examples of phosphors that can be used include oxynitride phosphors such as N2:Eu, sulfide phosphors such as CaS, SrGa2S4, SrAl2O4, and ZnS, chlorosilicate phosphors, SrLiAl3N4:Eu phosphors, SrMg3SiN4:Eu phosphors, and K2SiF6:Mn phosphors as manganese-activated fluoride complex phosphors.
[0138] In a light-emitting device, the light conversion member containing the core-shell semiconductor nanoparticles may be, for example, a sheet or plate-like member, or may be a member having a three-dimensional shape. An example of a member having a three-dimensional shape is a sealing member formed by filling a resin into a recess formed in a package of a surface-mounted light-emitting diode in order to seal the light-emitting element when the semiconductor light-emitting element is disposed on the bottom surface of the recess.
[0139] Another example of the light conversion member is a resin member formed to surround the upper and side surfaces of the semiconductor light emitting element with a substantially uniform thickness when the semiconductor light emitting element is disposed on a planar substrate.Alternatively, yet another example of the light conversion member is a resin member formed in a plate shape with a predetermined thickness on the upper part of the semiconductor light emitting element and the resin member containing the reflector when the semiconductor light emitting element is surrounded by a resin member containing a reflector whose upper end forms the same plane as the semiconductor light emitting element.
[0140] The light conversion member may be in contact with the semiconductor light emitting element, or may be provided at a distance from the semiconductor light emitting element. Specifically, the light conversion member may be a pellet-shaped member, a sheet member, a plate-shaped member, or a rod-shaped member that is disposed at a distance from the semiconductor light emitting element, or may be a member provided in contact with the semiconductor light emitting element, such as a sealing member, a coating member (a member that covers the light emitting element and is provided separately from the molding member), or a molding member (including, for example, a member having a lens shape).
[0141] In addition, when two or more types of core-shell semiconductor nanoparticles that emit light of different wavelengths are used in a light-emitting device, the two or more types of semiconductor nanoparticles may be mixed in one light conversion member, or two or more light conversion members containing only one type of quantum dot may be combined and used. In this case, the two or more types of light conversion members may form a laminated structure or may be arranged in a dot-like or stripe-like pattern on a plane.
[0142] An example of the semiconductor light-emitting element is an LED chip. The LED chip may have a semiconductor layer made of one or more kinds selected from the group consisting of GaN, GaAs, InGaN, AlInGaP, GaP, SiC, ZnO, etc. A semiconductor light-emitting element that emits blue-violet light, blue light, or ultraviolet light may have a composition of, for example, In. X Al Y Ga 1-X-Y The semiconductor layer is made of a GaN-based compound represented by N (0≦X, 0≦Y, X+Y<1).
[0143] The light-emitting device is preferably incorporated into a liquid crystal display device as a light source. Since the band-edge emission by the core-shell type semiconductor nanoparticles has a short emission life, the light-emitting device using the core-shell type semiconductor nanoparticles is suitable for the light source of a liquid crystal display device that requires a relatively fast response speed. In addition, the core-shell type semiconductor nanoparticles of this embodiment can show an emission peak with a small half-width as the band-edge emission. Therefore, in the light-emitting device, blue light having a peak wavelength in the range of 420 nm to 490 nm is obtained by the blue semiconductor light-emitting element, and green light having a peak wavelength in the range of 510 nm to 550 nm, preferably 530 nm to 540 nm, and red light having a peak wavelength in the range of 600 nm to 680 nm, preferably 630 nm to 650 nm are obtained by the semiconductor nanoparticles. Alternatively, in the light-emitting device, the semiconductor light-emitting element is used to obtain ultraviolet light with a peak wavelength of 400 nm or less, and the semiconductor nanoparticles are used to obtain blue light with a peak wavelength of 430 nm to 470 nm, preferably 440 nm to 460 nm, green light with a peak wavelength of 510 nm to 550 nm, preferably 530 nm to 540 nm, and red light with a peak wavelength of 600 nm to 680 nm, preferably 630 nm to 650 nm. This allows a liquid crystal display device with good color reproducibility to be obtained without using a dark color filter. The light-emitting device is used, for example, as a direct-type backlight or an edge-type backlight.
[0144] Alternatively, a sheet, plate-like member, or rod made of resin, glass, or the like, containing core-shell semiconductor nanoparticles may be incorporated into a liquid crystal display device as a light conversion member independent of the light emitting device. EXAMPLES
[0145] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0146] Example 1 Preparation of semiconductor nanoparticles (core) 0.0833 mmol of silver acetate (AgOAc), 0.05 mmol of indium acetylacetonate (In(acac)3)), 0.075 mmol of gallium acetylacetonate (Ga(acac)3)) and 0.2292 mmol of sulfur powder were added to a 0.25 cm 3 of 1-dodecanethiol and 2.75 cm 3 The mixture was poured into a mixture of oleylamine and dispersed. The dispersion was placed in a test tube together with a stirrer, and after nitrogen replacement, the contents in the test tube were stirred under a nitrogen atmosphere and heat-treated at 300°C for 10 minutes. After the heat treatment, the resulting suspension was left to cool, then centrifuged (radius 146 mm, 4000 rpm, 5 minutes) to remove the precipitate. 3 ml of methanol was added to this, and centrifuged (radius 146 mm, 4000 rpm, 5 minutes) to precipitate the semiconductor nanoparticles, and the supernatant was discarded. 3 ml of ethanol was further added thereto, and centrifuged under the same conditions to precipitate the semiconductor nanoparticles. The precipitate was removed, dried, and then dispersed in chloroform to obtain a semiconductor nanoparticle dispersion, and a dispersion of the cores was obtained.
[0147] Fabrication of core-shell semiconductor nanoparticles From the obtained semiconductor nanoparticle dispersion, 1 × 10 -5 The mixture was collected so that it contained 1 mmol of semiconductor nanoparticles, and dried under reduced pressure. 0.16 mmol of acetylacetonate gallium (Ga(acac)3) and 0.0533 mmol of thiourea were weighed out, 3.0 mL of oleylamine (water content 480 ppm) was added, and the inside of the test tube was replaced with nitrogen. After the nitrogen replacement, the contents in the test tube were stirred under a nitrogen atmosphere, and the first stage of heat treatment was performed at 150°C for 10 minutes, and the second stage of heat treatment was performed at 300°C for 30 minutes, and the mixture was allowed to cool to room temperature. The precipitate was removed by centrifugation (4000 rpm, 5 minutes). The supernatant was filtered through a membrane filter with a pore size of 0.20 μm. Methanol was added and centrifuged (4000 rpm, 5 minutes), and ethanol was added to the obtained precipitate and centrifuged (4000 rpm, 5 minutes) to obtain core-shell type semiconductor nanoparticles as a precipitate.
[0148] (Examples 2 to 4 and Comparative Example 1) Core-shell semiconductor nanoparticles were obtained in the same manner as in Example 1, except that the charged composition and the heating time in the second stage during the production of the core-shell semiconductor nanoparticles were changed as shown in Table 1.
[0149] [Table 1]
[0150] (Average particle size) The shapes of the core-shell type semiconductor nanoparticles obtained in Examples 1 to 4 and Comparative Example 1 were observed using a transmission electron microscope (TEM, Hitachi High-Technologies Corporation, product name H-7650), and the average particle size was measured from TEM images at 80,000 to 200,000 magnifications. Here, a Hi-Res Carbon HRC-C10 STEM Cu100P grid (Oken Shoji Co., Ltd.) was used as the TEM grid. The shape of the obtained particles was spherical or polygonal. The average particle size was determined by selecting TEM images at three or more locations, measuring the particle sizes of a total of 100 or more points of the nanoparticles contained therein, excluding those in which the particle images are cut off at the edge of the images, and determining the arithmetic average.
[0151] (Absorption and emission characteristics) The absorption spectrum and emission spectrum were measured for the core-shell type semiconductor nanoparticles obtained in Examples 1 to 4 and Comparative Example 1. The absorption spectrum was measured using a diode array spectrophotometer (Agilent Technologies, product name Agilent 8453A) at a wavelength of 190 nm to 1100 nm. The emission spectrum was measured using a multichannel spectrometer (Hamamatsu Photonics, product name PMA11) at an excitation wavelength of 365 nm. The absorption spectrum is shown in FIG. 1, and the emission spectrum is shown in FIG. 2. Table 2 shows the emission peak wavelength (band edge emission) of the steep emission peak observed in each emission spectrum, the half width of the band edge emission, the emission quantum yield of the band edge emission, and the Stokes shift of the band edge emission (the energy value of the absorption peak obtained from the absorption spectrum minus the energy value of the emission peak obtained from the emission spectrum). From Table 2, it can be seen that the core-shell type semiconductor nanoparticles obtained in Examples 1 to 4 have a higher band edge emission quantum yield than Comparative Example 1. I confirmed it would be higher.
[0152] [Table 2]
[0153] Example 5 Fabrication of core-shell semiconductor nanoparticles From the semiconductor nanoparticle dispersion liquid obtained in Example 1, 1×10 -5 A sample containing 10 mmol of semiconductor nanoparticles was taken and dried under reduced pressure. 0.16 mmol of acetylacetonate gallium (Ga(acac)3) and 0.0533 mmol of thiourea were weighed out, and 3.0 mL of dehydrated oleylamine (moisture value 50 ppm) was added, and the inside of the test tube was replaced with nitrogen. After the nitrogen replacement, the contents in the test tube were stirred in a nitrogen atmosphere while being heat-treated at 150°C for 10 minutes as the first stage of heat treatment, and then 5.35 x 10 mmol of pure water was added. -5mol was added, followed by a second heat treatment at 300°C for 30 minutes, and then allowed to cool at room temperature for 45 minutes. The precipitate was removed by centrifugation (4000 rpm, 5 minutes). The supernatant was filtered through a membrane filter with a pore size of 0.20 μm. Methanol was added and centrifuged (4000 rpm, 5 minutes), and ethanol was added to the resulting precipitate and centrifuged (4000 rpm, 5 minutes) to obtain core-shell type semiconductor nanoparticles as precipitates.
[0154] (Examples 6 to 9, Comparative Example 2) A core-shell semiconductor nanoparticle dispersion was obtained in the same manner as in Example 1, except that the amount of pure water added was changed as shown in Table 3.
[0155] [Table 3]
[0156] The average particle size and luminescence characteristics of the core-shell semiconductor nanoparticles obtained in Examples 5 to 9 and Comparative Example 2 were measured in the same manner as in Example 1. The results are shown in Table 4. FIG. 3 shows the absorption spectrum, and FIG. 4 shows the emission spectrum. It was confirmed from Table 3 that the core-shell semiconductor nanoparticles obtained in Examples 5 to 9 had a higher band edge luminescence quantum yield than Comparative Example 2.
[0157] [Table 4]
[0158] Example 10 The core-shell semiconductor nanoparticles obtained in Example 7 were dispersed in chloroform to prepare a dispersion. Then, an equal amount of trioctylphosphine (TOP) was added to the dispersion and mixed, and the mixture was allowed to stand at room temperature for 24 hours to obtain a dispersion of TOP-modified core-shell semiconductor nanoparticles. The luminescence properties of the TOP-modified core-shell semiconductor nanoparticles were measured in the same manner as in Example 1, and the quantum yield of the band edge emission was 88.8%.
[0159] The disclosure of Japanese Patent Application No. 2019-153625 (filing date: August 26, 2019) is incorporated herein by reference in its entirety. All documents, patent applications, and technical standards described herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard was specifically and individually indicated to be incorporated by reference.
Claims
1. M 1 , M. 2 and a core comprising a semiconductor comprising Z, 1 is at least one element selected from the group consisting of Ag, Cu, Au and alkali metals, and contains at least Ag; M 2 preparing a core in which Z is at least one element selected from the group consisting of Al, Ga, In, and Tl, and contains at least one of In and Ga, and Z is at least one element selected from the group consisting of S, Se, and Te; Obtaining a mixture including the core, at least one compound including a first element selected from the group consisting of Al, Ga, In, and Tl, and at least one simple substance of a second element selected from the group consisting of S, Se, and Te and at least one compound including the second element; and heat treating the mixture to obtain core-shell type semiconductor nanoparticles. The mixture contains a compound containing the first element and the second element alone or a compound containing the second element in a mixing ratio such that the ratio of the total atomic number of the first element to the sum of the total atomic number of the first element and the total atomic number of the second element is 0.6 or more.
2. The process of claim 1 , wherein the mixture includes an added source of oxygen.
3. The method of claim 1 or 2, wherein the heat treatment comprises adding an oxygen source to the mixture.
4. The method according to claim 1 , further comprising contacting the core-shell type semiconductor nanoparticles obtained by the heat treatment with an oxygen source.
Citation Information
Patent Citations
Semiconductor nanoparticle and manufacturing method therefor