Bipolar solid-state battery with porous support layer

The integration of a porous support layer in bipolar all-solid-state batteries addresses lithium dendrite issues, improving safety and performance by managing stress and enhancing density and lifespan.

JP7596013B2Active Publication Date: 2024-12-09LG ENERGY SOLUTION LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023501656
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-11-06
Filing Date
2021-10-29
Publication Date
2024-12-09
Estimated Expiration
2041-10-29

AI Technical Summary

Technical Problem

Bipolar all-solid-state batteries face issues with lithium dendrite formation leading to short circuits and internal stress, which compromises safety and reduces the battery's lifespan and density.

Method used

Incorporating a porous support layer between unit cells to manage stress and prevent lithium dendrite damage, using materials like olefin-based porous substrates and glass fibers to maintain constant pressure and improve ionic conductivity.

Benefits of technology

The porous support layer effectively reduces stress, prevents dendrite-induced short circuits, and enhances the battery's density and lifespan by maintaining consistent pressure and contact area.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007596013000008
    Figure 0007596013000008
  • Figure 0007596013000009
    Figure 0007596013000009
  • Figure 0007596013000010
    Figure 0007596013000010
Patent Text Reader

Abstract

The present invention relates to a bipolar all-solid-state battery including a porous support layer, and more specifically, to (a) a bipolar all-solid-state battery in which two or more unit cells each including a positive electrode, a solid electrolyte, and a negative electrode are connected in series and a first porous support layer is provided in the center of the connected part, or (b) a bipolar all-solid-state battery in which two or more unit cells each including a positive electrode, a solid electrolyte, and a second porous support layer are connected in series.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of priority based on Korean Patent Application No. 2020-0142129 filed on October 29, 2020, and Korean Patent Application No. 2020-0147423 filed on November 6, 2020, and all contents disclosed in the documents of the relevant Korean patent applications are incorporated herein by reference.

[0002] The present invention relates to a bipolar all-solid-state battery including a porous support layer, specifically, (a) a bipolar all-solid-state battery in which two or more unit cells including a positive electrode, a solid electrolyte, and a negative electrode are connected in series and a first porous support layer is provided in the center of the connected part, or (b) a bipolar all-solid-state battery in which two or more unit cells including a positive electrode, a solid electrolyte, and a second porous support layer are connected in series. [Background technology]

[0003] A bipolar battery has advantages such as minimizing the volume of the case, high energy density, stable performance, and low internal resistance. Such a bipolar battery generally has a bipolar electrode including a bipolar electrode layer and a biplate for connecting one unit cell to each adjacent unit cell in series. The biplate may be made of a material that has sufficient conductivity to transmit current between the unit cells, is chemically stable in the battery, and has excellent contact with the electrode. Such a biplate is easily corroded by a high dielectric electrolyte that is mainly used in lithium secondary batteries, and the corroded biplate reduces the electrolyte sealing and insulation between the unit cells, causing an internal short circuit, which ultimately reduces the safety of the battery.

[0004] To solve the above problems, bipolar all-solid-state batteries that do not use electrolytes have been proposed as an alternative. Unlike existing secondary batteries, bipolar all-solid-state batteries have a solid electrolyte, which is disposed between the positive and negative electrodes and serves as a separator.

[0005] Since solid-state batteries use a solid electrolyte instead of a liquid electrolyte used in conventional batteries, they are safe from explosions and fires as they do not evaporate electrolyte due to temperature changes or leak due to external impact. A drawback of solid-state batteries is that the contact area between the solid electrolyte and the positive or negative electrode is limited, making it difficult to form interfaces between the positive and negative electrodes and the solid electrolyte. When the contact area between the positive and negative electrodes and the solid electrolyte is small as described above, the unit cell including the solid electrolyte is pressurized to reduce the interfacial resistance.

[0006] Meanwhile, in order to increase the density and capacity of the bipolar solid-state battery and extend its lifespan, the bipolar solid-state battery can be manufactured using lithium. When lithium is used, lithium dendrites are formed during charging and discharging, damaging the separator (solid electrolyte) or causing a short circuit within the unit cell when the lithium dendrites meet the positive electrode. In particular, when the bipolar solid-state battery is pressurized, the growth of the lithium dendrites brings the positive electrode, solid electrolyte, and negative electrode closer to each other, causing damage to the solid electrolyte or a short circuit due to a reaction between the lithium dendrites and the positive electrode.

[0007] FIG. 1 is a perspective view of a bipolar all-solid-state battery according to the prior art before charging and discharging, and FIG. 2 is a perspective view of the bipolar all-solid-state battery according to the prior art after charging and discharging.

[0008] The bipolar all-solid-state battery 10 according to the related art includes a first unit cell 100 including a first positive electrode 110 including a first positive electrode active material 111 and a first positive electrode current collector 112, and a first negative electrode 130 including a first solid electrolyte 120, a first negative electrode active material 131, and a first negative electrode current collector 132; a second unit cell 200 including a second positive electrode 210 including a second positive electrode active material 211 and a second positive electrode current collector 212, and a second negative electrode 230 including a second solid electrolyte 220, a second negative electrode active material 231, and a second negative electrode current collector 232; and a bipolar electrode 300 for connecting the first unit cell 100 and the second unit cell 200 in series.

[0009] At this time, unlike FIG. 1 and FIG. 2, the first positive electrode active material 111, the first negative electrode active material 131, the second positive electrode active material 211, and the second negative electrode active material 231 may be applied only to one surface of the first positive electrode current collector 112, the first negative electrode current collector 132, the second positive electrode current collector 212, and the second negative electrode current collector 232, or a separate electrode active material may not be applied.

[0010] In addition, in the above configuration, a bipolar solid-state battery in which a first negative electrode active material, a bipolar electrode, and a second positive electrode active material are disposed between the first solid electrolyte 120 and the second solid electrolyte 220 is also possible, which also has the same problems as described below.

[0011] In order to reduce the interfacial resistance between the first positive electrode 110, the first solid electrolyte 120, and the first negative electrode 130 and the second positive electrode 210, the second solid electrolyte 220, and the second negative electrode 230, the bipolar all-solid-state battery 10 according to the prior art is pressurized by a pressure force F1 in the y-axis direction from a jig during charging and discharging.

[0012] However, in the bipolar all-solid-state battery 10, when the first unit cell 100 and the second unit cell 200 are charged and discharged, the lithium layer 400 generated is inserted into the first anode 130 and / or the second anode 230, causing the active material to expand, or lithium is deposited in the first anode 130 and / or the second anode 230, causing the thickness of the bipolar all-solid-state battery 10 to increase.

[0013] When the thickness of the bipolar solid-state battery 10 increases, the internal pressure F2 of the bipolar solid-state battery 10 increases, and the pressure F1 applied to the first unit cell 100 and the second unit cell 200 also increases. Generally, the pressure F1 is generated by a jig, and the jig occupies a certain position, because the internal volume increases.

[0014] As the lithium layer 400 formed by the initial charge and discharge increases, the reaction force between the first solid electrolyte 120 and the second solid electrolyte 220 and the lithium layer 400 increases, and the lithium metal of the lithium layer 400 flows into the first solid electrolyte 120 and the second solid electrolyte 220 through defects, which increases the possibility of causing a short circuit in the bipolar all-solid-state battery 10.

[0015] In addition, if the pressurizing force F1 increases, the positions and shapes of the first unit cell 100 and the second unit cell 200 in the bipolar all-solid-state battery 10 may be deformed. If the shape of the bipolar all-solid-state battery 10 or the positions of the first unit cell 100 and the second unit cell 200 change, the pressurizing force F1 may not be applied evenly to the first unit cell 100 and the second unit cell 200, so that some of the cells may not be pressurized or some of the cells may be overly pressurized.

[0016] Patent Document 1 relates to an all-solid-state thin-film laminated battery and refers to a case where a plurality of power generating elements are connected in series. However, unlike the bipolar battery of the present invention, this case connects the power generating elements in series via electrode terminals, and although it relieves stress inside the thin-film laminated battery, it is not possible to improve the density of the battery.

[0017] As described above, it is necessary to reduce the internal stress of a bipolar solid-state battery, which has superior performance relative to its density, while preventing damage to the solid electrolyte caused by lithium dendrites, but no clear solution has been presented. [Prior art documents] [Patent documents]

[0018] [Patent Document 1] JP 2004-273436 A Summary of the Invention [Problem to be solved by the invention]

[0019] The present invention is intended to solve the above problems, and aims to prevent damage to the solid electrolyte caused by the formation of lithium dendrites and short circuits in unit cells caused by the contact of the lithium dendrites with the positive electrode.

[0020] Another object of the present invention is to obtain a high-density bipolar all-solid-state battery while reducing stress inside the bipolar all-solid-state battery, improving ion conductivity, and improving life span. [Means for solving the problem]

[0021] In order to solve the above problems, the present invention provides a battery comprising: (a) two or more unit cells each including a positive electrode, a solid electrolyte, and a negative electrode connected in series, and a first porous support layer is provided at the center of the connected part; (b) A bipolar all-solid-state battery is provided in which two or more unit cells, each unit cell including a positive electrode, a solid electrolyte, and a second porous support layer, are connected in series.

[0022] The negative electrode of one unit cell may be disposed on one surface of the first porous support layer, and the positive electrode of another unit cell may be disposed on the opposing surface thereof, and the negative electrode may be a current collector without lithium metal or an active material layer.

[0023] The surface of the second porous support layer facing the solid electrolyte may serve as an anode, and the surface of the second porous support layer facing the cathode may serve as a separator. The second porous support layer may include a lithium anode or an anode current collector. The anode current collector may be a metal or a metal oxide, and the lithium anode or an anode current collector may not include a separate active material layer.

[0024] The first porous support layer may include at least one of a sheet or nonwoven fabric made of one or more selected from the group consisting of an olefin-based porous substrate, glass fiber, and polyethylene.

[0025] The first porous support layer may be formed by laminating one or more layers of the olefin-based porous substrate, sheet or nonwoven fabric. When the first porous support layer has two or more layers, each layer of the first porous support layer may be made of a different material, or each layer of the first porous support layer may be made of the same material.

[0026] The first porous support layer and the second porous support layer reduce in thickness when pressure is applied and return to their original thickness when the pressure is removed, thereby adjusting stress inside the all-solid-state battery, and the pressure may be generated when lithium ions from the positive electrode move to the negative electrode upon charging and accumulate between the negative electrode and the solid electrolyte or between the second porous support layer and the solid electrolyte.

[0027] The first porous support layer may adjust stress due to thickness changes caused by lithium deposition, and the thickness of the second porous support layer may be greater than the thickness of the deposited lithium.

[0028] The stress may be adjusted in proportion to the thickness and porosity of the first and second porous supporting layers, and the first porous supporting layer may have a thickness of 20 μm to 50 μm.

[0029] The positive electrode may include a positive electrode current collector and a positive electrode active material coated on one surface of the positive electrode current collector, the positive electrode active material facing the solid electrolyte, and the positive electrode current collector facing the first porous support layer and the second porous support layer.

[0030] The negative electrode of one unit cell disposed on one side of the first porous support layer may be lithium metal without a separate active material layer, and the positive electrode of the other unit cell disposed on the opposite side of the first porous support layer may be a positive electrode current collector.

[0031] The positive electrode disposed between the second porous support layer and the solid electrolyte may be composed of only a positive electrode active material, and in this case, the outermost positive electrode may be a positive electrode current collector and a positive electrode active material applied to a surface of the positive electrode current collector facing the solid electrolyte.

[0032] The two or more unit cells may be housed in a pouch-type battery case, and pressure may be applied to the two or more unit cells by an external jig during charging and discharging.

[0033] A bipolar all-solid-state battery in which two or more unit cells, each including a positive electrode, a solid electrolyte, and a second porous support layer, are connected in series may be formed by repeating one or more units in which a second porous support layer-anode active material-solid electrolyte are stacked between an outermost positive electrode, a solid electrolyte facing the outermost positive electrode, and an outermost negative electrode.

[0034] A bipolar all-solid-state battery in which two or more unit cells, each including a positive electrode, a solid electrolyte, and a second porous support layer, are connected in series may be formed by repeating one or more units, each of which includes a second porous support layer-anode current collector-anode active material-solid electrolyte, stacked between an outermost positive electrode, a solid electrolyte facing the outermost positive electrode, and an outermost negative electrode.

[0035] The present invention may be a battery module or a battery pack including the bipolar all-solid-state battery mentioned above, or a device equipped with the bipolar all-solid-state battery.

[0036] The present invention can select and combine one or more of the above-mentioned configurations that are not contradictory. Effect of the Invention

[0037] As described above, the bipolar solid-state battery according to the present invention reduces stress generated in the bipolar solid-state battery by forming a lithium layer, and can prevent damage to the solid electrolyte and reaction between the positive electrode and lithium dendrites of the lithium layer, thereby reducing cell shorts in the bipolar solid-state battery.

[0038] In addition, the bipolar solid-state battery uses only an anode current collector as an anode, and a cathode current collector and a cathode active material coated on one surface thereof as a cathode, and connects unit cells formed of these in series via a first porous support layer, thereby improving capacity and performance relative to the density of the battery.

[0039] In addition, the bipolar all-solid-state battery has a second porous supporting layer that serves as an anode and a separator, and the second porous supporting layer relieves internal stress, thereby improving safety and providing a high-density bipolar all-solid-state battery.

[0040] Furthermore, the pressure applied to the unit cells inside the bipolar solid-state battery is maintained constant, preventing damage to the unit cells, improving the ionic conductivity of the unit cells, and improving the life of the battery. [Brief description of the drawings]

[0041] [Figure 1] FIG. 1 is a perspective view of a bipolar all-solid-state battery according to the prior art before charging and discharging. [Diagram 2] FIG. 1 is a perspective view of a bipolar all-solid-state battery according to the prior art after charging and discharging. [Diagram 3] FIG. 1 is a perspective view of a bipolar all-solid-state battery according to a first example of the present invention before charging and discharging. [Figure 4] 1A to 1C are perspective views of a bipolar all-solid-state battery according to a first example of the present invention after charging and discharging. [Diagram 5] FIG. 2 is a cross-sectional view of an all-solid-state battery used in Experimental Example 2 of the present invention. [Figure 6]FIG. 2 is a perspective view of a bipolar all-solid-state battery according to a second example of the present invention before charging and discharging. [Figure 7] 1A to 1C are perspective views of a bipolar all-solid-state battery according to a second example of the present invention after charging and discharging. [Figure 8] FIG. 1 is a cross-sectional view of an all-solid-state battery used in Experimental Example 4 of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0042] Hereinafter, the present invention will be described in detail with reference to the accompanying drawings, in which a person having ordinary skill in the art to which the present invention pertains can easily carry out the present invention. However, in describing the operation principle of the preferred embodiment of the present invention in detail, if it is determined that the detailed description of related well-known functions or configurations may unnecessarily obscure the gist of the present invention, the detailed description thereof will be omitted.

[0043] In addition, the same reference numerals are used throughout the drawings for parts having similar functions and actions. Throughout the specification, when one part is said to be connected to another part, this includes not only a direct connection but also an indirect connection via another element between them. In addition, the inclusion of one component does not mean the exclusion of other components, but may further include other components, unless otherwise specified.

[0044] Furthermore, descriptions that specify or limit components by adding them are applicable to all inventions unless otherwise specified, and are not limited to a particular invention.

[0045] Furthermore, throughout the description of the present invention and the claims, the singular includes the plural unless specifically stated otherwise.

[0046] Furthermore, throughout the description of the present invention and the claims, unless otherwise stated, "or" includes "and." Therefore, "including A or B" means all three cases of including A, including B, or including A and B.

[0047] Additionally, all numerical ranges include the endpoints and all intermediate values ​​therebetween unless expressly stated to exclude.

[0048] The active material, current collector, and solid electrolyte referred to in relation to FIGS. 1 to 8 do not simply mean materials, but rather mean layers formed of these materials.

[0049] The bipolar all-solid-state battery according to the present invention comprises: (a) two or more unit cells each including a positive electrode, a solid electrolyte, and a negative electrode connected in series; and a first porous support layer is provided at the center of the connected unit cells; (b) Two or more unit cells each including a positive electrode, a solid electrolyte, and a second porous support layer are connected in series.

[0050] The negative electrode of one unit cell may be disposed on one surface of the first porous support layer, and the positive electrode of another unit cell may be disposed on the opposing surface thereof, and the negative electrode may be a current collector without a lithium metal or active material layer.

[0051] A first example of the bipolar all-solid-state battery according to the present invention (a) will be described with reference to FIG. 3 and FIG. 4, in which two or more unit cells including a positive electrode, a solid electrolyte, and a negative electrode are connected in series and a first porous support layer is provided at the center of the connected part.

[0052] FIG. 3 is a perspective view of the bipolar all-solid-state battery 1000 according to the first example of the present invention before charge and discharge, and FIG. 4 is a perspective view of the bipolar all-solid-state battery 1000 according to the first example of the present invention after charge and discharge.

[0053] In FIGS. 3 and 4, for convenience of explanation, the unit cells are illustrated as a first unit cell 1100 and a second unit cell 1200. However, the unit cell may include a plurality of the first unit cells 1100 and the second unit cells 1200.

[0054] The bipolar all-solid-state battery 1000 according to the present invention includes a first unit cell 1100 and a second unit cell 1200. The first unit cell 1100 includes a first positive electrode 1110 including a first positive electrode active material 1111 and a first positive electrode current collector 1112, a first solid electrolyte 1120, and a first negative electrode 1130 including a first negative electrode current collector 1132, and the second unit cell 1200 includes a second positive electrode 1210 including a second positive electrode active material 1211 and a second positive electrode current collector 1212, a second solid electrolyte 1220, and a second negative electrode 1230 including a second negative electrode current collector 1232. A first porous support layer 1300 for connecting the unit cells in series is disposed between the first unit cell 1100 and the second unit cell 1200. A first anode 1130 of a first unit cell 1100 is disposed on one surface of the first porous support layer 1300, and a second anode 1210 of a second unit cell 1200 is disposed on the other surface of the first porous support layer 1300, i.e., the surface facing the first anode 1130.

[0055] The first positive electrode 1110 may be manufactured, for example, by applying a positive electrode mixture, which is a mixture of a positive electrode active material composed of positive electrode active material particles, a conductive material, and a binder, to a first positive electrode collector 1112 to form a first positive electrode active material 1111, and if necessary, a filler may be further added to the positive electrode mixture.

[0056] The first positive electrode current collector 1112 is generally manufactured to a thickness of 3 μm to 500 μm, and is not particularly limited as long as it does not induce chemical changes in the battery and has high conductivity, and for example, the positive electrode current collector 1112 may be one selected from stainless steel, aluminum, nickel, titanium, and aluminum or stainless steel surface-treated with carbon, nickel, titanium, or silver, and more specifically, aluminum may be used. The current collector may have fine irregularities on its surface to increase the adhesive force of the positive electrode active material, and may be in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0057] The positive electrode active material contained in the first positive electrode active material 1111 may be, for example, a layered compound such as lithium nickel oxide (LiNiO2) or a compound substituted with one or more transition metals, in addition to the positive electrode active material particles; 1+x Mn 2-x Lithium manganese oxides such as LiMnO4 (where x is 0 to 0.33), LiMnO3, LiMn2O3, and LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, LiV3O4, V2O5, and Cu2V2O7; 1-x M x O2 (where M=Co, Mn, Al, Cu, Fe, Mg, B, or Ga, and x=0.01 to 0.3); 2-x M x The lithium manganese composite oxides can be represented by Li2Mn3MO8 (where M=Co, Ni, Fe, Cr, Zn, or Ta, and x=0.01 to 0.1) or Li2Mn3MO8 (where M=Fe, Co, Ni, Cu, or Zn); LiMn2O4 in which part of the Li in the chemical formula is replaced with an alkaline earth metal ion; disulfide compounds; Fe2(MoO4)3, and the like, but are not limited to these.

[0058] However, it is preferable that the positive electrode active material 1111 used in the present invention uses or contains a metal oxide containing lithium in order to deposit lithium on the first negative electrode 1130 .

[0059] The conductive material is usually added in an amount of 0.1% by weight to 30% by weight based on the total weight of the mixture including the positive electrode active material. The conductive material is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity, and examples of the conductive material include graphite such as natural graphite and artificial graphite; carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers and metal fibers; metal powders such as carbon fluoride, aluminum, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.

[0060] The binder included in the first positive electrode 1110 is a component that promotes binding between the active material and the conductive material and between the active material and the current collector, and is typically added in an amount of 0.1% by weight to 30% by weight based on the total weight of the mixture including the positive active material. Examples of such binders include polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, fluororubber, and various copolymers.

[0061] The first positive electrode 1110 may have a form in which the first positive electrode active material 1111 is formed on at least one surface of the first positive electrode current collector 1112. In this case, when the first positive electrode 1110 is located at the outermost periphery of the bipolar all-solid-state battery 1000, the first positive electrode 1110 may have a form in which the first positive electrode active material 1111 is coated on both surfaces of the first positive electrode current collector 1112. In addition, when the first positive electrode 1110 faces another unit cell of the bipolar all-solid-state battery 1000, the first positive electrode 1110 may have the first positive electrode active material 1111 coated on only one surface of the first positive electrode current collector 1112.

[0062] The second positive electrode 1210 may be formed in the same manner as the first positive electrode 1110. However, the second positive electrode 1210 faces a unit cell of the bipolar all-solid-state battery 1000, and has a configuration in which the second positive electrode active material 1211 is formed only on one surface of a second positive electrode current collector 1212 of the second positive electrode 1210.

[0063] A second positive electrode active material 1211 of a second positive electrode 1210 disposed on the other side of the first porous support layer 1300 faces the second solid electrolyte 1220, and the second positive electrode current collector 1212 faces the first porous support layer 1300, such that the first porous support layer 1300 connects unit cells of the bipolar all-solid-state battery 1000 in series.

[0064] The first solid electrolyte 1120 and the second solid electrolyte 1220 may be, but are not limited to, an organic solid electrolyte or an inorganic solid electrolyte.

[0065] Examples of the organic solid electrolyte that can be used include polyethylene derivatives, polyethylene oxide derivatives, polypropylene oxide derivatives, phosphate polymers, polyagitation lysine, polyester sulfide, polyvinyl alcohol, polyvinylidene fluoride, and polymers containing ionic dissociation groups.

[0066] Examples of the inorganic solid electrolyte include a sulfide-based solid electrolyte and an oxide-based solid electrolyte.

[0067] As an oxide-based solid electrolyte, for example, Li 6.25 La3Zr2Al 0.25 O 12 , Li3PO4, Li3+xPO4-xN x Nitrides and halides of Li, such as (LiPON), Li3N, LiI, Li5NI2, Li3N-LiI-LiOH, LiSiO4, LiSiO4-LiI-LiOH, Li2SiS3, Li4SiO4, and Li4SiO4-LiI-LiOH, may be used.

[0068] The sulfide particles are not particularly limited in the present invention, and all known sulfide materials used in the field of lithium batteries can be used. The sulfide materials can be purchased from the market or manufactured through a crystallization process of an amorphous sulfide material. For example, the sulfide solid electrolyte can be a crystalline sulfide solid electrolyte, an amorphous sulfide solid electrolyte, or any one or a mixture of these. Examples of usable composite compounds include sulfur-halogen compounds, sulfur-germanium compounds, and sulfur-silicon sulfides. Specifically, sulfides such as SiS2, GeS2, and B2S3 may be included, and Li3PO4, halogens, halogen compounds, etc. may be added. Preferably, 10 -4 A sulfide-based electrolyte capable of realizing lithium ion conductivity of S / cm or more may be used.

[0069] Representative examples include Li6PS5Cl (LPSCl), Thio-LISICON (Li 3.25 Ge 0.25 P 0.75 S4), Li2S-P2S5-LiCl, Li2S-SiS2, LiI-Li2S-SiS2, LiI-Li2S-P2S5, LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, Li2S-P2S5, Li3PS4, Li7P3S 11 , LiI-Li2S-B2S3, Li3PO4-Li2S-Si2S, Li3PO4-Li2S-SiS2, LiPO4-Li2S-SiS, Li 10 GeP2S 12 , Li 9.54 S 1.74 P 1.44 S 11.7 Cl 0.3 , Li7P3S 11 Including The first and second solid electrolytes 1120 and 1220 may have a coating layer on their surfaces facing the first and second anodes 1130 and 1230 to induce the formation of lithium dendrites.

[0070] The coating layer may include a metal to improve electrical conductivity and ionic conductivity. The type of the metal is not limited as long as it improves the performance of the first negative electrode 1130 or the second negative electrode 1230 and allows lithium dendrites to be formed between the coating layer and the first negative electrode current collector 1132 or between the coating layer and the second negative electrode current collector 1232. In this case, the metal has lithium affinity and can induce lithium dendrites to be formed between the coating layer and the first negative electrode current collector 1132 or between the coating layer and the second negative electrode current collector 1232.

[0071] In this case, in order to prevent lithium dendrites from growing toward the first solid electrolyte 1120 or the second solid electrolyte 1220, the lithium-affinity metal may be disposed on the side of the coating layer facing the first anode 1130 or the second anode 1230.

[0072] When a metal with a lithium affinity is located in the coating layer, lithium plating occurs on the metal with a lithium affinity to form lithium nuclei, and lithium dendrites that grow from the lithium nuclei grow only in the coating layer.

[0073] The lithium affinity metal may be at least one of a metal and a metal oxide, for example, the metal may be gold (Au), silver (Ag), platinum (Pt), zinc (Zn), silicon (Si), magnesium (Mg), etc., and the metal oxide may be a non-metal such as copper oxide, zinc oxide, cobalt oxide, etc.

[0074] The first negative electrode 1130 according to the present invention may consist of only the first negative electrode current collector 1132 .

[0075] The negative electrode current collector 1132 is generally formed to a thickness of 3 μm to 500 μm. The first negative electrode current collector 1132 is not particularly limited as long as it does not induce a chemical change in the battery and has conductivity, and may be a current collector without a lithium metal or a separate negative electrode active material layer. For example, the first negative electrode current collector 1132 may be made of copper, stainless steel, aluminum, nickel, titanium, baked carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, or aluminum-cadmium alloy. In addition, the first negative electrode current collector 1132 may be formed with fine irregularities on the surface to strengthen the binding force of the negative electrode active material, similar to the first positive electrode current collector 1112, and may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, or the like.

[0076] The second negative electrode 1230 may have the same shape as the first negative electrode 1130 .

[0077] The first unit cell 1100 and the second unit cell 1200 have the above-mentioned configuration, and can be connected in series to obtain a bipolar all-solid-state battery 1000 having high energy density.

[0078] A first porous support layer 1300 may be disposed between the first unit cell 1100 and the second unit cell 1200 to connect the unit cells in series.

[0079] The first porous support layer 1300 may be any material having electrical conductivity and ionic conductivity to connect the first unit cell 1100 and the second unit cell 1200 in series. As an example, the first porous support layer 1300 may include at least one of a sheet or nonwoven fabric made of one or more materials selected from a group including an olefin-based porous substrate, glass fiber, or polyethylene. In this case, the first porous support layer 1300 is preferably a sheet made of one or more materials selected from a group including an olefin-based porous substrate, glass fiber, or polyethylene. This is because the nonwoven fabric has a large porosity, but since the nonwoven fabric must be laminated in many layers in order for the first porous support layer 1300 to have a certain strength, the thickness change rate is not large compared to the porous substrate or sheet when the thickness is the same.

[0080] Specifically, the first porous support layer 1300 may contain a resin such as a polyolefin resin (polyethylene, polypropylene, polybutene, polyvinyl chloride) and a mixture or copolymer thereof, or may contain a resin such as polyethylene terephthalate, polycycloolefin, polyethersulfone, polyamide, polyimide, polyimideamide, polyaramid, nylon, polytetrafluoroethylene, etc. Among these, polyolefin resins are preferable because they can reduce the thickness and increase the capacity per volume in the bipolar all-solid-state battery 1000.

[0081] The first porous support layer 1300 is made of a material having elasticity and capable of relieving stress generated inside the bipolar all-solid-state battery 1000, or the stress generated inside the bipolar all-solid-state battery 1000 can be relieved through the pores of the first porous support layer 1300.

[0082] The first porous support layer may be the olefin-based porous substrate, or one or more layers of sheets or nonwoven fabrics laminated together.

[0083] When the first porous support layer is formed in multiple layers, the range of stress that the first porous support layer can relieve can be increased.

[0084] When the first porous support layer has two or more layers, each layer of the first porous support layer may be made of a different material, or each layer of the first porous support layer may be made of the same material.

[0085] The first porous support layer 1300 may have a pore diameter of generally 0.01 μm to 10 μm, a thickness of generally 20 μm to 50 μm, and a porosity of the first porous support layer 1300 may be 30% to 90%.

[0086] The first porous support layer 1300 adjusts stress caused by thickness change due to lithium deposition. In order for the first porous support layer 1300 to relieve stress as described above, the elastic range of the first porous support layer 1300 must be greater than the deformation range caused by the deposited lithium. The elastic range of the first porous support layer 1300 is proportional to the thickness and porosity of the first porous support layer 1300.

[0087] That is, the elastic range of the first porous support layer 1300 can be expressed as follows.

[0088] Elastic range of the first porous support layer = thickness of the first porous support layer x porosity of the first porous support layer At this time, the elasticity of the material used for the first porous support layer 1300 must be greater than the driving pressure of the jig.

[0089] The first porous support layer 1300 is disposed between the first negative electrode current collector 1132 of the first unit cell 1100 and the second positive electrode current collector 1212 of the second unit cell 1200, and the first porous support layer 1300, the first negative electrode current collector 1132, and the second positive electrode current collector 1212 can be used as a bipolar electrode of the bipolar all-solid-state battery 1000. As such, the first unit cell 1100, the second unit cell 1200, and the bipolar electrode share a portion with each other, thereby improving the density of the bipolar all-solid-state battery 1000. For this purpose, the first porous support layer 1300 is formed by pressing the first unit cell 1100 and the second unit cell 1200.

[0090] The first unit cell 1100, the second unit cell 1200, and the first porous support layer 1300 are pressed with a constant pressure F1 by a jig, which is maintained even when the bipolar solid-state battery 1000 is used.

[0091] In the bipolar all-solid-state battery 1000 according to the present invention, a lithium layer 1400 is formed after charging and discharging, as shown in Fig. 4. The lithium layer 1400 is formed by accumulating lithium between the first negative electrode 1130 or the second negative electrode 1230 and the first solid electrolyte 1120 or the second solid electrolyte 1220 due to charging and discharging. This is because lithium ions of the first positive electrode 1110 or the second positive electrode 1210 move to the first negative electrode 1130 or the second negative electrode 1230 and are accumulated between the first negative electrode 1130 and the first solid electrolyte 1120 or the second negative electrode 1230 and the second solid electrolyte 1220.

[0092] The lithium layer 1400 is charged under a constant current / constant voltage (CC / CV) condition, and the applied pressure F1 to the entire lithium secondary battery at this time may vary depending on the amount of lithium formed in the battery, the charge / discharge rate, time, etc. This is because the lithium layer 1400 is formed and an internal pressure F2 is generated.

[0093] In the bipolar all-solid-state battery 1000 according to the present invention, stress caused by an internal pressure F2 applied by the lithium layer 1400 is relieved through the first porous support layer 1300. The first porous support layer 1300 allows a constant pressure F1 to be applied to the entire bipolar all-solid-state battery 1000 through deformation of the shape including a reduction in the number of pores in the first porous support layer 1300 or a reduction in the thickness of the first porous support layer 1300.

[0094] The reduction in the pores or the change in shape of the first porous support layer 1300 is controlled by the formation and / or disappearance of the lithium layer 1400. For example, when the lithium layer 1400 is formed and an internal pressure F2 is generated, the pores of the first porous support layer 1300 may be reduced and the thickness may be reduced. Also, when the lithium layer 1400 disappears, the first porous support layer 1300 returns to its initial state, and the thickness m of the bipolar all-solid-state battery before and after compression is maintained the same.

[0095] In order to apply a constant pressure to the unit cells even during use, the bipolar all-solid-state battery 1000 may be formed by housing each unit cell in a battery case that can apply pressure to the entire unit cell of the bipolar all-solid-state battery 1000, or the unit cells may be housed in a pouch-type battery case, and then the bipolar all-solid-state battery 1000 may be pressurized outside the pouch-type battery case.

[0096] A bipolar all-solid-state battery according to a second embodiment of the present invention (b) in which two or more unit cells each including a positive electrode, a solid electrolyte, and a second porous support layer are connected in series will be described with reference to FIGS. 6 and 7.

[0097] FIG. 6 is a perspective view of a bipolar all-solid-state battery 2000 according to a second example of the present invention before charge and discharge, and FIG. 7 is a perspective view of the bipolar all-solid-state battery 2000 according to the second example of the present invention after charge and discharge.

[0098] In FIGS. 6 and 7, for convenience of explanation, the unit cells are illustrated as the first unit cell 2100 and the second unit cell 2200. However, the unit cell may include a plurality of the first unit cells 2100 and the second unit cells 2200.

[0099] The bipolar all-solid-state battery 2000 according to the second embodiment of the present invention includes a first unit cell 2100 and a second unit cell 2200. The first unit cell 2100 includes a first positive electrode 2110 including a first positive electrode active material 2111 and a first positive electrode current collector 2112, a first solid electrolyte 2120, and a second porous support layer 2140, and the second unit cell 2200 includes a second positive electrode 2210 including a second positive electrode active material 2211 and a second positive electrode current collector 2212, a second solid electrolyte 2220, and a second porous support layer 2240. The first unit cell 2100 and the second unit cell 2200 are connected in series via the second porous support layer 2140 and the second porous support layer 2240.

[0100] In this case, the second positive electrode current collector 2212 of the second unit cell 2200 may be omitted. When the second positive electrode current collector 2212 is omitted, the positive electrode 2210 disposed between the second porous support layer 2140 and the solid electrolyte 2220 is composed of only the positive electrode active material 2211, and the current collector 2212 is omitted. The first positive electrode 2110, which is the outermost positive electrode, may also be in the form of only the positive electrode current collector 2112 and the positive electrode active material 2111 applied to the side of the positive electrode current collector 2112 facing the solid electrolyte 2120, as shown in the drawing, or may be in the form of the positive electrode active material being applied to both sides of the positive electrode current collector 2112. Meanwhile, in the case of the second porous support layer 2240 corresponding to the outermost negative electrode, an additional current collector (not shown) may be added to the outer surface.

[0101] 6 and 7, the bipolar all-solid-state battery according to the present invention may be in a form in which only the second porous support layer is laminated with the solid electrolyte sandwiched therebetween, without using the first positive electrode, the second positive electrode, and the second negative electrode. In this case, a positive electrode active material may be applied to one surface of the second porous support layer.

[0102] 6 and 7 include a structure in which a second porous support layer-anode current collector-anode active material-solid electrolyte is laminated, except for the outermost cathode 2110, the outermost solid electrolyte 2120, and the opposite outermost anode 2240, and may have a structure in which this is repeated. In this case, the repeated structure may be second porous support layer-anode current collector-anode active material-solid electrolyte or second porous support layer-anode active material-solid electrolyte. Figures 6 and 7 show the most basic form in which there is one layer that can be repeated.

[0103] A first solid electrolyte 2120 of a first unit cell 2100 is disposed on one side of the second porous support layer 2140, and a second positive electrode 2210 of a second unit cell 2200 is disposed on the other side of the second porous support layer 2140, i.e., the side facing the first solid electrolyte 2120.

[0104] The first positive electrode 2110 is made of the same material and manufactured by the same method as the first positive electrode 1110, the first positive electrode collector 2112 is made of the same material and manufactured by the same method as the first positive electrode collector 1112, and the first positive electrode active material 2111 is made of the same material and manufactured by the same method as the first positive electrode active material 1111.

[0105] However, the positive electrode active material 2111 used in the present invention preferably uses or contains a metal oxide containing lithium in order to deposit lithium on one side of the second porous support layer 2140 .

[0106] The first positive electrode 2110 may have a form in which the first positive electrode active material 2111 is formed on at least one surface of the first positive electrode current collector 2112. In this case, when the first positive electrode 2110 is located at the outermost periphery of the bipolar all-solid-state battery 2000, the first positive electrode 2110 may have a form in which the first positive electrode active material 2111 is coated on both surfaces of the first positive electrode current collector 2112. In terms of battery performance, it is more preferable that the positive electrode active material is coated on both surfaces of the solid electrolyte, rather than being coated on both surfaces of the positive electrode current collector.

[0107] When the first positive electrode 2110 faces a second porous support layer of another bipolar all-solid-state battery, the first positive electrode 2110 may have the first positive electrode active material 2111 applied only to the surface of the first positive electrode current collector 2112 that faces the first solid electrolyte 2120, or may be composed of only the first positive electrode active material 2111 and may be stacked continuously with another bipolar all-solid-state battery.

[0108] The material used for the second positive electrode 2210 may be the same as that of the first positive electrode 2110. The second positive electrode 2210 is formed by stacking a second positive electrode current collector 2212 and the second positive electrode active material 2211 in this order while facing a second porous support layer 2140. The second positive electrode 2210 may include only the second positive electrode active material 2211 without including the second positive electrode current collector 2212.

[0109] Specifically, the second positive electrode active material 2211 faces the second solid electrolyte 2220, and the second positive electrode current collector 2212 faces the second porous support layer 2140, such that the second porous support layer 2140 can serially connect unit cells of the bipolar all-solid-state battery 2000. The second porous support layer 2140 serves as an anode, a separator, and a cathode, or serves as an anode, a current collector, and a cathode.

[0110] The first solid electrolyte 2120 and the second solid electrolyte 2220 are made of the same material and are manufactured by the same method as the first solid electrolyte 1120 and the second solid electrolyte 1220.

[0111] The first solid electrolyte 2120 and the second solid electrolyte 2220 may have a coating layer on the opposite side of the second porous support layer 2140 and the second porous support layer 2240 to induce the formation of lithium dendrites.

[0112] The coating layer may include a metal to improve electrical conductivity and ionic conductivity. The metal is not limited to a specific type as long as it improves the negative electrode performance of the surface of the second porous support layer 2140 or the second porous support layer 2240 that serves as the negative electrode and allows lithium dendrites to be formed between the coating layer and the second porous support layer 2140 or between the coating layer and the second porous support layer 2240. In this case, the metal has an affinity for lithium and can induce lithium dendrites to be formed between the coating layer and the second porous support layer 2140 or between the coating layer and the second porous support layer 2240.

[0113] In this case, in order to prevent lithium dendrites from growing toward the first solid electrolyte 2120 or the second solid electrolyte 2220, the lithium-affinity metal may be disposed on the side of the second porous support layer 2140 or the second porous support layer 2240 facing the first solid electrolyte 2120 or the second solid electrolyte 2220.

[0114] When a metal with a lithium affinity is located in the coating layer, lithium plating occurs on the metal with a lithium affinity to form lithium nuclei, and lithium dendrites that grow from the lithium nuclei grow only in the coating layer.

[0115] The lithium affinity metal may be at least one of a metal and a metal oxide, for example, the metal may be gold (Au), silver (Ag), platinum (Pt), zinc (Zn), silicon (Si), magnesium (Mg), etc., and the metal oxide may be a non-metal such as copper oxide, zinc oxide, cobalt oxide, etc.

[0116] According to the present invention, the surface of the second porous support layer 2140 facing the first solid electrolyte 2120 may serve as an anode, and the surface of the second porous support layer 2140 facing the second cathode 2210 may serve as a separator and / or a current collector. When only the second cathode active material 2211 is used as the second cathode 2210, the surface of the second porous support layer 2140 facing the second cathode 2210 may simultaneously serve as a separator and a cathode current collector.

[0117] The second porous support layer 2140 may include a lithium anode or anode current collector. The lithium anode or anode current collector included in the second porous support layer 2140 is not particularly limited as long as it does not cause a chemical change in the battery and has high conductivity. The anode current collector may be a metal or a metal oxide. For example, the anode current collector may be copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, or silver, or an aluminum-cadmium alloy. In addition, the anode current collector may be formed with fine irregularities on its surface, similar to the first positive current collector 2112, to strengthen the binding force with the part of the second porous support layer 2140 that serves as a separator, and may be used in various forms such as a film, a sheet, a foil, a net, a porous body, a foam, or a nonwoven fabric. The lithium anode or anode current collector may be included in the second porous support layer 2140 as particles or particles in a core-shell form, rather than in the form of a layer.

[0118] The lithium anode or anode current collector of the second porous support layer 2140 according to the present invention may not include a separate active material. Since the lithium anode or anode current collector does not include a separate active material, the second porous support layer 2140 can be formed thin, thereby improving the density of the battery.

[0119] The second porous support layer 2140 may be formed to a thickness of generally 3 μm to 500 μm. In this case, the second porous support layer 2140 may be thicker than the lithium layer 2400 formed by depositing lithium.

[0120] The lithium anode or anode current collector of the second porous support layer 2140 may be distributed primarily on a surface facing the first solid electrolyte 2120 .

[0121] An electrically conductive material may be disposed on the second porous support layer 2140 facing the second positive electrode 2210. As an example, the second porous support layer 2140 facing the second positive electrode 2210 may include at least one of a sheet or a nonwoven fabric made of one or more materials selected from the group including an olefin-based porous substrate, glass fiber, or polyethylene.

[0122] Specifically, the second porous support layer 2140 may contain a resin such as polyolefin (polyethylene, polypropylene, polybutene, polyvinyl chloride) and a mixture or copolymer thereof, or may contain a resin such as polyethylene terephthalate, polycycloolefin, polyethersulfone, polyamide, polyimide, polyimideamide, polyaramid, nylon, polytetrafluoroethylene, etc. Among these, polyolefin resins are preferable because they can reduce the thickness and increase the capacity per volume in the bipolar all-solid-state battery 2000.

[0123] In addition, the second porous support layer 2140 facing the second positive electrode 2210 may include a component similar to the component of the first positive electrode current collector 2112 mentioned above.

[0124] The second porous support layer 2140 may be made of a material having elasticity and capable of relieving stress generated within the bipolar all-solid-state battery 2000, or may be capable of relieving stress generated within the bipolar all-solid-state battery 2000 through pores of the second porous support layer 2140. The second porous support layer 2140 may be in the form of a foam having a porous interior, made of a metal material.

[0125] The second porous support layer 2140 may have a pore diameter of generally 0.01 μm to 10 μm and a thickness of generally 20 μm to 50 μm.

[0126] The second porous support layer 2140 is disposed between the first solid electrolyte 2120 of the first unit cell 2100 and the second positive electrode current collector 2212 of the second unit cell 2200, and the second porous support layer 2140 and the second positive electrode current collector 2212 may serve as a bipolar electrode of the bipolar all-solid-state battery 2000. As such, the bipolar electrode constitutes a part of the first unit cell 2100 together with the first unit cell 2100 and the second unit cell 2200, thereby improving the density of the bipolar all-solid-state battery 2000. If the second positive electrode current collector 2212 is not present, further improvement in density may be achieved.

[0127] The second porous support layer 2140 is formed by pressing the first unit cell 2100 and the second unit cell 2200 .

[0128] The second porous support layer 2240 may have the same shape as the second porous support layer 2140 .

[0129] A separate metal current collector may be further included between the first unit cell 2100 and the second unit cell 2200 according to the present invention. That is, the metal current collector may be included between the second porous support layer 2140 and the second positive electrode 2210. The metal current collector is used to prevent lithium ions transferred from the first positive electrode 2110 from directly transferring to the second positive electrode 2210. In this case, the metal current collector may be the same material as that used for the first positive electrode current collector 2112. For example, the metal current collector may be one selected from stainless steel, aluminum, nickel, titanium, and aluminum or stainless steel surface-treated with carbon, nickel, titanium, or silver.

[0130] Also, a separate metal current collector may be further included in the outermost periphery of the second unit cell 2200. The current collector may be a metal or a metal oxide. For example, the current collector may be copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, or aluminum-cadmium alloy. The current collector may have fine irregularities on its surface to strengthen the bonding force with the second porous support layer 2140, and may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, or the like.

[0131] The first unit cell 2100 and the second unit cell 2200 are pressed with a constant pressure F1 by a jig, which is maintained even when the bipolar solid-state battery 2000 is used.

[0132] In the bipolar all-solid-state battery 2000 according to the present invention, a lithium layer 2400 is formed after charging and discharging, as shown in Fig. 7. The lithium layer 2400 is formed by depositing lithium between the second porous support layer 2140 or the second porous support layer 2240 and the first solid electrolyte 2120 or the second solid electrolyte 2220 by charging and discharging.

[0133] The lithium layer 2400 is charged under a constant current / constant voltage (CC / CV) condition, and the pressure F1 applied to the entire lithium secondary battery at this time may vary depending on the amount of lithium formed in the battery, the charge / discharge rate, time, etc. This is because the lithium layer 2400 is formed and an internal pressure F2 is generated.

[0134] In the bipolar all-solid-state battery 2000 according to the present invention, stress generated by the internal pressure F2 applied by the lithium layer 2400 is relieved through the second porous support layer 2140 or the second porous support layer 2240. The second porous support layer 2140 or the second porous support layer 2240 reduces the number of pores in the second porous support layer 2140 or the second porous support layer 2240 or changes the shape of the second porous support layer 2140 or the second porous support layer 2240, so that a constant pressure F1 is applied to the entire bipolar all-solid-state battery 2000.

[0135] Hereinafter, the present invention will be described with reference to an experimental example that compares the present invention with a comparative example according to the prior art.

[0136] (Experimental Example 1) Elasticity Test of the First Porous Support Layer The thickness change of the first porous support layer was measured in response to pressure changes due to jig pressure and / or lithium deposition during charging of the all-solid-state battery. First porous support layer #1 and first porous support layer #2, which have similar porosity but different thicknesses, and first porous support layer #3, which has different porosity and thickness, were used as the first porous support layer.

[0137] The first porous support layer was made of polyethylene.

[0138] The first porous support layer was punched out to a size of 2.5 cm x 2.5 cm, and the solid-state battery was sequentially pressurized at 5 MPa, 10 MPa, 15 MPa, and 20 MPa using a jig. The thickness change at each step was measured and is shown in Table 1 below.

[0139] [Table 1]

[0140] The thickness of the first porous support layer decreases as the pressure increases, but in the case of a thin ultra-thin porous support layer such as first porous support layer #1, the thickness change due to pressure is small, while in the case of a thick porous support layer with high porosity such as first porous support layer #3, the thickness change due to pressure is large. The deformation of the porous support layer due to the pressure applied during evaluation of an all-solid-state battery and the pressure change due to lithium generated during charging was simulated for the first porous support layers #1 to #3, and the porous support layers were pressurized at 5 MPa once, twice, three times, five times, and ten times, respectively, and the thicknesses were measured. The results are shown in Table 2.

[0141] In this case, the first porous support layer #1 was pressurized at 20 MPa, the first porous support layer #2 was prepared by laminating one, two, or three layers pressurized at 10 MPa, and the first porous support layer #3 was prepared by pressing one that was not pressurized or one that was pressurized at 10 MPa at 5 MPa once, twice, three times, five times, or ten times, respectively.

[0142] [Table 2]

[0143] In order to reduce the stress generated in the bipolar solid-state battery as intended in the present invention, the deformation range due to pressure must be within the elastic range of the first porous support layer. As shown in Table 2, the first porous support layer according to the present invention is a thin film type with a low absolute value of thickness change, i.e., deformation range. In particular, the first porous support layer #1 is an ultra-thin porous support layer with a theoretically possible deformation range of 4 μm. Therefore, it can be seen that when a thin porous support layer is used, the porous support layer absorbs the stress inside the bipolar solid-state battery without a large change in thickness.

[0144] Even excluding jig pressure, charging typically requires 1mAh / cm 2When lithium is deposited, the lithium is deposited on the negative electrode as a layer having a thickness of 4 μm. The present invention relates to a battery used in a large-capacity battery used in a small or automobile battery, and generally, the capacity of the electrode is larger than that of a thin-film battery, and the thickness of lithium deposited on the negative electrode is also increased with the increase in the capacity of the electrode. Therefore, when a first porous support layer having a small deformation range as in the present invention is used to relieve the stress inside the bipolar all-solid-state battery, the stress inside the bipolar all-solid-state battery can be relieved by using a plurality of first porous support layers according to the thickness of the deposited lithium. As shown in Table 2, even when two or three first porous support layers #2 are laminated, it can be seen that the battery operates in the same manner as when one first porous support layer #2 is laminated.

[0145] When comparing the first porous support layer #3 and the first porous support layer #3 pressurized at 10 MPa, the thickness of the unpressurized first porous support layer #3 is reduced from 41 μm to 38 μm when pressurized once at 5 MPa, and then as the number of pressurizations increases, the thickness continues to decrease and the deformation becomes small, but when this is used after primary molding at a pressure higher than the driving pressure, i.e., when the first porous support layer #3 is pressurized at 10 MPa, there is no change in thickness even if additional pressure is continued thereafter. Therefore, it can be seen that when a thin first porous support layer such as the first porous support layer #2 is laminated in multiple layers, or a thick first porous support layer such as the first porous support layer #3 is molded at a pressure higher than the driving pressure and then used, the stress inside the bipolar all-solid-state battery can be reduced.

[0146] (Experimental Example 2) Measurement of Thickness Increase Rate In Experimental Example 2, a battery formed as described below was charged and discharged five times, and the thickness change rate was calculated. The initial capacity of the battery was measured by charging and discharging at 60°C, and the charging conditions were CC / CV (8.5V, 0.05C, 0.01C current cutoff) and the discharging conditions were CC (6V, 0.05C, 60°C). The thickness increase rate was calculated as (battery thickness after charging / battery thickness before charging) x 100, and is shown in Table 3 below. In addition, the capacity retention rate after five charging and discharging cycles was measured and is shown in Table 3 below.

[0147] The capacity retention rate was calculated as follows.

[0148] Capacity retention rate (%) = (Capacity after 5 cycles / Initial capacity) x 100

[0149] (Example 1-1) The positive electrode active material is NCM811 (LiNi 0.8 Co 0.1 Mn 0.1 A positive electrode slurry was prepared by dispersing and stirring the positive electrode slurry in anisole in a weight ratio of 77.5:19.5:1.5:1.5, which is a weight ratio of 77.5:19.5:1.5:1.5. The positive electrode slurry was applied to an aluminum current collector having a thickness of 15 μm using a doctor blade, and then vacuum-dried at 100° C. for 12 hours to obtain a positive electrode slurry with a capacity of 2 mAh / cm. 2 A positive electrode having a capacity of 1000 g / m2 was produced.

[0150] The solid electrolyte layer was fabricated by mixing argyrodite (Li6PS5Cl) and PTFE binder in a weight ratio of 95:5.

[0151] As the negative electrode current collector, nickel having a thickness of 11 μm was used.

[0152] FIG. 5 is a cross-sectional view of the all-solid-state battery 1000 used in Experimental Example 2.

[0153] The all-solid-state battery of Experimental Example 2 is formed by stacking a first unit cell 1100 in which a first positive electrode 1110 having a first positive electrode active material 1111 formed on one side of a first positive electrode collector 1112, a first solid electrolyte layer 1120, and a negative electrode consisting of only a first negative electrode collector 1132, and a second unit cell 1200 in which a negative electrode consisting of only a second positive electrode 1210 having a second positive electrode active material 1211 formed on one side of a second positive electrode collector 1212, a second solid electrolyte layer 1220, and a second negative electrode collector 1232 is stacked, and a first porous support layer 1300 is stacked between the first unit cell 1100. In this case, the first positive electrode active material 1111 is stacked so as to face the first solid electrolyte layer 1120, which is the same as the case of the second positive electrode active material 1211. At this time, the first positive electrode current collector 1112 faces the jig, and the second positive electrode current collector 1212 faces the first porous support layer 1300 .

[0154] The first porous support layer 1300 used in Example 1-1 of the present invention was prepared by laminating three of the first porous support layers #2 after pressurizing them at 10 MPa.

[0155] (Example 1-2) The first porous support layer 1300 was prepared and evaluated in the same manner as in Example 1-1, except that the first porous support layer #2 was pressurized at 10 MPa and one sheet was used as the first porous support layer 1300.

[0156] (Examples 1-3) In the above Example 1-1, the capacity is 3 mAh / cm 2 The fabrication and evaluation were performed in the same manner as in Example 1-1, except that the positive electrode was made of 1-1.

[0157] (Comparative Example 1-1) The fabrication and evaluation were performed in the same manner as in Example 1-1, except that the first porous supporting layer was not used.

[0158] (Comparative Example 1-2) The first porous support layer 1300 was prepared and evaluated in the same manner as in Example 1-1, except that the first porous support layer #1 was pressurized at 20 MPa and one sheet was used as the first porous support layer 1300.

[0159] (Comparative Example 1-3) The fabrication and evaluation were performed in the same manner as in Example 1-1, except that one sheet of the first porous support layer #3 was used as the first porous support layer 1300 in Example 1-1.

[0160] [Table 3]

[0161] As shown in Table 3, when the elasticity of the first porous support layer is greater than the battery operating pressure as in Examples 1-1 to 1-3 of the present invention, the first porous support layer absorbs the thickness change caused by lithium during charging, and the first porous support layer relieves the stress within the all-solid-state battery. It can be seen that this elimination of thickness change continues even after five charge / discharge cycles. Theoretically, the deformation amount of the first porous support layer can be calculated based on the thickness and porosity of the first porous support layer to be used, and when the capacity of the positive electrode is 3 mAh / cm as in Example 1-3, the deformation amount of the first porous support layer can be calculated based on the thickness and porosity of the first porous support layer to be used. 2 It can be seen that even when the capacity of the positive electrode is increased as in the case of (a), there is almost no increase in thickness during charging and discharging.

[0162] On the other hand, in the case of Comparative Example 1-1 where the first porous support layer is not applied, the thickness of the all-solid-state battery increases, and the resistance inside the all-solid-state battery increases, and the life span is also inferior to that of Examples 1-1 to 1-3. Also, in the case of Comparative Example 1-2 where the first porous support layer is used, which has a smaller deformation amount than the increased thickness, and Comparative Example 1-3 where the elasticity is low and the thickness changes continuously during operation, it can be seen that the effect of using the first porous support layer is negligible. Therefore, it can be seen that the elastic range of the first porous support layer must be larger than the deformation range caused by the deposited lithium.

[0163] That is, the capacity of the all-solid-state battery is 1 mAh / cm 2 Since lithium is deposited to a thickness of 4 μm per layer, the deformation range can be calculated based on the thickness and porosity of the first porous support layer, and one or more layers can be laminated for use.

[0164] (Experimental Example 3) Elasticity Test of the Second Porous Support Layer Two types of nickel foam (Ni foam #1 and Ni foam #2) were selected as the second porous support layer to be used as a porous current collector of an all-solid-state battery. The second porous support layer was punched out to 2.0 cm x 2.0 cm, and then pressurized at 5 MPa, 10 MPa, 15 MPa, 25 MPa, and 50 MPa, and the thickness change at each step was measured and shown in Table 4 below.

[0165] [Table 4]

[0166] The thickness of nickel foam #1 and nickel foam #2 gradually decreased as the pressure increased. After being pressurized at 50 MPa, nickel foam #1 had a thickness of 165 μm and a porosity of 48%, while nickel foam #2 had a thickness of 109 μm and a porosity of 83%.

[0167] In order to simulate the deformation of the second porous support layer due to the pressure applied during evaluation of the all-solid-state battery and the pressure change caused by lithium during charging, the second porous support layer was pressurized several times at 5 MPa, and the second porous support layer that had been pressurized several times was pressurized at 10 MPa, and then the second porous support layer that had been pressurized at 10 MPa was pressurized in sequence at 15 MPa and 25 MPa. After pressing, the thickness of the second porous support layer was measured, and the results are shown in Tables 5 and 6 below.

[0168] At this time, the nickel foam #1, the nickel foam #1 pressurized at 50 MPa, and the nickel foam #2 pressurized at 50 MPa were used as the second porous support layer.

[0169] [Table 5]

[0170] [Table 6]

[0171] In the case of nickel foam #1 without any treatment, the thickness was continuously reduced when the second porous support layer was sequentially pressurized at a pressure of 5 MPa. This thickness reduction occurs because the pressure is greater than the elasticity of the second porous support layer, and composition deformation occurs continuously. In particular, when the pressure increases to 10 MPa or 15 MPa, the deformation rate increases continuously. That is, when a battery is manufactured using the second porous support layer, the thickness of the second porous support layer decreases due to an increase in pressure caused by lithium deposition during continuous charging and discharging, and the thickness of the second porous support layer cannot be restored even when the lithium deposition is removed. If the thickness of the second porous support layer cannot be restored as described above, the lithium deposited during discharge moves to the positive electrode and the thickness of the lithium layer decreases, and the contact between the second porous support layer, the solid electrolyte, and the positive electrode decreases, and the interface resistance in the battery increases, thereby reducing the overall performance of the all-solid-state battery.

[0172] On the other hand, in the case of nickel foam #1 and nickel foam #2 pressurized at 50 MPa, the thickness does not change even when pressurized at 5 MPa several times. This is because the deformation of nickel foam #1 and nickel foam #2 pressurized at 50 MPa is already completed and the strength is improved by pressing, and a larger pressure is required to deform the deformed second porous support layer. In the case of nickel foam #1 and nickel foam #2 pressurized at 50 MPa, as shown in Tables 5 and 6, deformation does not occur up to 25 MPa, and it can be seen that they can fully withstand the pressure generated during operation of the all-solid-state battery. As described above, when the second porous support layer does not deform, the initial thickness and initial shape can be maintained even during charging and discharging, and when the second porous support layer is applied, the contact between the positive electrode-solid electrolyte-second porous support layer is constantly maintained, and the performance of the battery does not deteriorate. In this case, it is more effective to use a second porous support layer that has a large shape retention force that maintains its shape when deformed by pressure.

[0173] The second porous support layer mentioned above can be applied to various other components used in batteries, and although the material is not described in the description of the invention in this specification, any material that can be used in batteries can be used. In addition, the second porous support layer can be applied to batteries that use electrolytes and all other products for storing electricity, in addition to all-solid-state batteries.

[0174] (Experimental Example 4) Measurement of Thickness Increase Rate In Experimental Example 4, the all-solid-state battery formed in the following configuration was charged and discharged, and the thickness change rate was calculated. The initial capacity was measured by charging and discharging at 60°C, and the charging conditions were CC / CV (8.5V, 0.05C, 0.01C current cutoff), and the discharging conditions were CC conditions (6V, 0.05C, 60°C). At this time, the thickness increase rate was calculated as battery thickness after charging / battery thickness before charging×100, and is shown in Table 7 below.

[0175] (Example 2-1) The positive electrode active material is NCM811 (LiNi 0.8 Co 0.1 Mn 0.1 A positive electrode slurry was prepared by dispersing and stirring the positive electrode slurry in anisole in a weight ratio of 77.5:19.5:1.5:1.5, which is a weight ratio of 77.5:19.5:1.5:1.5. The positive electrode slurry was applied to an aluminum current collector having a thickness of 15 μm using a doctor blade, and then vacuum-dried at 100° C. for 12 hours to obtain a positive electrode slurry with a capacity of 4 mAh / cm. 2 This was used as the outermost positive electrode.

[0176] The solid electrolyte layer was fabricated by mixing argyrodite (Li6PS5Cl) and PTFE binder in a weight ratio of 95:5.

[0177] The nickel foam #1 pressurized at 50 MPa in Experimental Example 3 was used as the second porous support layer.

[0178] The positive electrode active material facing one side of the second porous support layer is NCM811 (LiNi 0.8 Co 0.1 Mn 0.1 The cathode was formed using a cathode slurry prepared by dispersing and stirring anisole in a weight ratio of 77.5:19.5:1.5:1.5, which consisted of 02), a solid electrolyte called argyrodite (Li6PS5Cl), a conductive material called carbon, and a PTFE binder.

[0179] In Example 2-1 of the present invention, nickel was used as the outermost negative electrode current collector.

[0180] FIG. 8 is a cross-sectional view of an all-solid-state battery 2000 used in Experimental Example 4.

[0181] The all-solid-state battery according to Experimental Example 4 is formed by stacking a first unit cell 2100 in which a first positive electrode 2110 having a first positive electrode active material 2111 formed on one surface of a first positive electrode current collector 2112, a first solid electrolyte 2120, and a second porous support layer 2140 are stacked, and a second unit cell 2200 in which a second positive electrode active material 2211, a second solid electrolyte 2220, and a second negative electrode current collector 2232 are stacked. At this time, the first positive electrode active material 2111 faces the first solid electrolyte 2120. The all-solid-state battery is pressed by a jig, and the first positive electrode current collector 2112 and the second negative electrode current collector 2232 face the jig.

[0182] Using the material according to Example 2-1, an all-solid-state battery as shown in FIG. 8 was manufactured.

[0183] The jig was fastened so as to apply a force of 5 MPa to the all-solid-state battery, and then charging and discharging were performed.

[0184] (Example 2-2) The fabrication and evaluation were performed in the same manner as in Example 2-1, except that nickel foam #2 pressurized at 50 MPa was used as the second porous support layer.

[0185] (Example 2-3) In the above Example 2-1, the capacity of the positive electrode is 6 mAh / cm 2 The second porous support layer was fabricated and evaluated in the same manner as in Example 2-1, except that nickel foam #2 pressurized at 50 MPa was used.

[0186] (Comparative Example 2-1) The fabrication and evaluation were performed in the same manner as in Example 2-1, except that a nickel foil having a thickness of 10 μm was used as the second porous supporting layer.

[0187] (Comparative Example 2-2) In the above Example 2-1, the capacity of the positive electrode is 6 mAh / cm 2The second porous support layer was fabricated and evaluated in the same manner as in Example 2-1, except that a nickel foil having a thickness of 10 μm was used as the second porous support layer.

[0188] [Table 7]

[0189] As shown in Table 7, when the elasticity of the second porous support layer is greater than the driving pressure of the battery as in Examples 2-1 to 2-3 of the present invention, the second porous support layer absorbs the thickness change caused by lithium during charging, and the second porous support layer relieves the stress within the all-solid-state battery. It can be seen that this elimination of thickness change continues even after five charge / discharge cycles. This shows that the amount of deformation of the nickel foam is sufficient due to the stress caused by the increase in thickness of lithium deposited during charging, as well as the elasticity of the second porous support layer. Theoretically, the amount of deformation of the second porous support layer can be predicted from its thickness and porosity, and in Example 2-3, when the capacity of the positive electrode is 6 mAh / cm 2 Even when the capacity of the positive electrode is increased as in the case of FIG. 1, the thickness of the second porous support layer is 109 μm and the porosity is 83%, and it can be confirmed that there is almost no increase in thickness during charging and discharging.

[0190] On the other hand, in the case of Comparative Example 2-1 in which a general nickel foil was applied, the thickness increased by 11.4% even after one charge because there was no factor to eliminate the thickness increase due to the deposited lithium. This thickness change rate increases with the number of charges. In addition, in the case of Comparative Example 2-2 in which the capacity of the positive electrode was increased, the thickness change rate further increased to 15.8%, confirming that the stress due to lithium deposition could not be eliminated. Based on the above results, it can be seen that the second porous support layer according to the present invention is effective in minimizing the thickness change rate of a battery due to charging and discharging of an all-solid-state battery that operates by a lithium plating / stripping mechanism.

[0191] The present invention also provides a battery module including the bipolar solid-state battery, a battery pack, and a device including the battery pack. However, since the battery module, battery pack, and device are well known in the art, detailed description thereof will be omitted in this specification.

[0192] Of course, the device may be, for example, a laptop, a netbook, a tablet PC, a mobile phone, an MP3, a wearable electronic device, a power tool, an electric vehicle (EV), a hybrid electric vehicle (HEV), a plug-in hybrid electric vehicle (PHEV), an electric bicycle (E-bike), an electric scooter, an electric golf cart, or a power storage system, but is not limited to these.

[0193] Those skilled in the art will appreciate that various applications and modifications within the scope of the present invention are possible based on the above content. [Explanation of symbols]

[0194] 10, 1000, 2000: Bipolar solid-state battery 100, 1100, 2100: 1st unit cell 110, 1110, 2110: 1st positive electrode 111, 1111, 2111: First positive electrode active material 112, 1112, 2112: first positive electrode current collector 120, 1120, 2120: First solid electrolyte 130, 1130: first negative electrode 131, 1131: First negative electrode active material 132, 1132: First negative electrode current collector 2140, 2240: Second porous support layer 200, 1200, 2200: Second unit cell 210, 1210, 2210: 2nd positive electrode 211, 1211, 2211: Second positive electrode active material 212, 1212, 2212: second positive electrode current collector 220, 1220, 2220: Second solid electrolyte 230, 1230: second negative electrode 231, 1231: Second negative electrode active material 232, 1232: Second negative electrode current collector 300: Bipolar electrode 1300: First porous support layer 400, 1400, 2400: Lithium layer F1: Pressure F2: Internal pressure m: thickness before compression M: Thickness after pressing JIG: Jig [Industrial Applicability]

[0195] The present invention relates to a bipolar all-solid-state battery including a porous support layer, specifically, (a) a bipolar all-solid-state battery in which two or more unit cells including a positive electrode, a solid electrolyte, and a negative electrode are connected in series and a first porous support layer is provided in the center of the connected part, or (b) a bipolar all-solid-state battery in which two or more unit cells including a positive electrode, a solid electrolyte, and a second porous support layer are connected in series, and thus the present invention is industrially applicable.

Claims

1. (a) Two or more unit cells each including a positive electrode, a solid electrolyte, and a negative electrode are connected in series, and a first porous support layer having a thickness of 20 μm to 50 μm is provided at the center of the connected part; or (b) A bipolar all-solid-state battery in which two or more unit cells each including a positive electrode, a solid electrolyte, and a second porous support layer are connected in series, The first porous support layer and the second porous support layer reduce in thickness when pressure is applied and return to their original thickness when the pressure is removed, thereby adjusting stress inside the bipolar solid-state battery; the negative electrode of one of the unit cells disposed on one surface of the first porous support layer is lithium metal without a separate active material layer, and the positive electrode of the other of the unit cells disposed on an opposite surface of the first porous support layer is a positive electrode current collector; a surface of the second porous support layer facing the solid electrolyte serves as an anode, and a surface of the second porous support layer facing the cathode serves as a separator.

2. The bipolar all-solid-state battery according to claim 1 , wherein the negative electrode of one of the unit cells is disposed on one surface of the first porous support layer, and the positive electrode of the other unit cell is disposed on an opposing surface thereof.

3. (b) A bipolar all-solid-state battery in which two or more unit cells each including a positive electrode, a solid electrolyte, and a second porous support layer are connected in series, the second porous support layer reduces in thickness when pressure is applied and returns to its original thickness when the pressure is removed, adjusting stress within the bipolar solid-state battery; the second porous support layer comprises a lithium anode or an anode current collector; a surface of the second porous support layer facing the solid electrolyte serves as an anode, and a surface of the second porous support layer facing the cathode serves as a separator.

4. The bipolar all-solid-state battery according to claim 3 , wherein the negative electrode current collector is a metal or a metal oxide.

5. The bipolar all-solid-state battery of claim 3 , wherein the lithium anode or the anode current collector does not include a separate active material layer.

6. The first porous support layer comprises: An olefin-based porous substrate; and Sheets and nonwoven fabrics made from one or more materials selected from the group including glass fiber or polyethylene; The bipolar solid-state battery according to claim 1 , comprising at least one of:

7. The first porous support layer comprises: The bipolar all-solid-state battery according to claim 6 , wherein the olefin-based porous substrate, the sheet, or the nonwoven fabric is laminated in one or more layers.

8. The first porous support layer is two or more layers, The first porous support layer may be made of different materials. The bipolar solid-state battery according to claim 7 , wherein each layer of the first porous support layer is made of the same material.

9. 2. The bipolar all-solid-state battery according to claim 1, wherein the pressure is generated by lithium ions of the positive electrode moving to the negative electrode upon charging and accumulating between the negative electrode and the solid electrolyte, or between the second porous support layer and the solid electrolyte.

10. The bipolar solid-state battery of claim 9 , wherein the first porous support layer adjusts stress due to thickness changes caused by lithium deposition.

11. 10. The bipolar solid-state battery of claim 9, wherein the thickness of the second porous support layer is greater than the thickness of the deposited lithium.

12. 2. The bipolar solid-state battery of claim 1, wherein the first and second porous support layers have a porosity of 30% to 90%.

13. The bipolar all-solid-state battery according to claim 1 , wherein the positive electrode comprises a positive electrode current collector and a positive electrode active material coated on one surface of the positive electrode current collector.

14. 14. The bipolar all-solid-state battery according to claim 13, wherein the positive electrode active material faces the solid electrolyte, and the positive electrode current collector faces the first porous support layer and the second porous support layer.

15. The positive electrode disposed between the second porous support layer and the solid electrolyte is composed of only a positive electrode active material, The bipolar all-solid-state battery according to claim 1 , wherein the outermost positive electrode at this time is a positive electrode current collector and a positive electrode active material applied to the positive electrode current collector facing the solid electrolyte.

16. A bipolar solid-state battery as described in claim 1, wherein two or more of the unit cells are housed in a single pouch-type battery case.

17. The bipolar solid-state battery as described in claim 1, wherein pressure is applied to the two or more unit cells by an external jig during charging and discharging.

18. The bipolar all-solid-state battery, in which two or more unit cells each including the positive electrode, the solid electrolyte, and the second porous support layer are connected in series, comprises: Between an outermost positive electrode, a solid electrolyte facing the outermost positive electrode, and an outermost negative electrode, 2. The bipolar all-solid-state battery according to claim 1, wherein one or more units each including a second porous support layer, a positive electrode active material, and a solid electrolyte are repeated.

19. The bipolar all-solid-state battery, in which two or more unit cells each including the positive electrode, the solid electrolyte, and the second porous support layer are connected in series, comprises: Between an outermost positive electrode, a solid electrolyte facing the outermost positive electrode, and an outermost negative electrode, 2. The bipolar all-solid-state battery according to claim 1, wherein one or more units each including a second porous support layer, a positive electrode current collector, a positive electrode active material, and a solid electrolyte are repeated.

Citation Information

Patent Citations

  • All solid thin film laminated battery

    JP2004273436A

  • Biploar battery and its manufacturing method

    JP2006190649A

  • Silicon secondary battery unit and battery module for electric vehicle using same

    JP2017522709A

  • Bipolar type all-solid battery

    JP2021197219A

  • Method of improving cycle life of a rechargeable lithium metal battery