Electrode catalyst for fuel cell

Modifying fuel cell catalysts with oxide nanoparticles addresses the issues of low humidity and ionomer poisoning, ensuring high activity and durability by enhancing proton conduction and preventing catalyst deterioration.

JP7596044B2Active Publication Date: 2024-12-09KK TOYOTA CHUO KENKYUSHO +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2022030249
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-02-28
Publication Date
2024-12-09
Estimated Expiration
2042-02-28

AI Technical Summary

Technical Problem

Fuel cell electrode catalysts face challenges in maintaining high activity in low humidity environments and are susceptible to ionomer poisoning and catalyst particle deterioration due to contact with ionomers, leading to reduced performance.

Method used

The catalyst is modified with oxide nanoparticles on the surface of catalyst particles to enhance proton conduction and prevent ionomer poisoning, using a carrier made of electronically conductive material with supported catalyst particles and oxide nanoparticles.

Benefits of technology

The modification with oxide nanoparticles retains water for proton conduction and suppresses ionomer poisoning and catalyst particle deterioration, maintaining catalyst activity and durability even in low humidity conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007596044000002
    Figure 0007596044000002
  • Figure 0007596044000003
    Figure 0007596044000003
  • Figure 0007596044000004
    Figure 0007596044000004
Patent Text Reader

Abstract

To provide a fuel cell electrode catalyst that exhibits relatively high activity even under low humidity environments and is capable of suppressing reduction of activity due to ionomer poisoning and degradation of catalyst particles caused by ionomer.SOLUTION: A fuel cell electrode catalyst includes a support including an electron conductive material, catalyst particles supported on the surface of the support, and oxide nanoparticles that modify the surface of the catalyst particles. The oxide nanoparticles are preferably tin oxide nanoparticles and / or tin oxide nanoparticles including dopants. The preferred content of the oxide nanoparticles is 1 mg / m2 or more and 20 mg / m2 or less.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electrode catalyst for a fuel cell, and more specifically to an electrode catalyst for a fuel cell which has high activity in a low humidity environment and excellent durability. [Background technology]

[0002] A polymer electrolyte fuel cell includes a membrane electrode assembly (MEA) in which catalyst layers are bonded to both sides of an electrolyte membrane. A gas diffusion layer is usually disposed on the outside of the catalyst layer. Furthermore, a current collector (separator) having a gas flow path is disposed on the outside of the gas diffusion layer. A polymer electrolyte fuel cell usually includes a structure (fuel cell stack) in which a plurality of unit cells each consisting of such an MEA, gas diffusion layer, and current collector are stacked.

[0003] In a solid polymer electrolyte fuel cell, the catalyst layer generally consists of a mixture of an electrode catalyst in which catalytic particles such as platinum are supported on the surface of a carrier, and an ionomer. Carbon materials such as carbon black and acetylene black are usually used for the carrier. However, when exposed to a high potential, the carbon carrier is oxidized and corroded, causing the catalytic particles supported on the carrier to fall off, and this causes the electrode performance to deteriorate. In addition, in the operating environment of the fuel cell, the catalytic particles are repeatedly dissolved and reprecipitated, causing them to become coarse, resulting in a decrease in the effective surface area of ​​the catalyst.

[0004] In order to solve this problem, various proposals have been made in the past. For example, Patent Document 1 discloses a composite catalyst comprising carbon, platinum microparticles supported on the surface of the carbon, and a metal oxide layer formed so as to surround the platinum microparticles, in which the platinum atoms in the platinum microparticles are bonded to the metal oxide. The same document states: (A) Such a composite catalyst can exhibit superior catalytic performance and catalytic durability compared to conventional platinum alloy catalysts and core-shell catalysts; and (B) In order for the platinum fine particles to be free from being buried in the metal oxide layer and to exhibit oxygen reduction ability, the thickness of the metal oxide layer is preferably 20 to 60% of the average particle diameter of the platinum fine particles. is stated.

[0005] Patent Document 2 discloses a composite electrode catalyst comprising a tin oxide-modified carbon material in which the surface of a carbon material is modified with tin oxide having a particle size of 20 nm or less, and platinum fine particles having a particle size of 5 nm or less supported on the surface of the tin oxide-modified carbon material. The document describes that a composite electrode catalyst having such a configuration has improved performance and is more than twice as durable as conventional composite electrode catalysts.

[0006] Furthermore, Non-Patent Document 1 discloses a SnOx / Pt-Cu-Ni heterojunction catalyst obtained by modifying the surface of a Pt-Cu-Ni alloy with tin oxide particles. The document describes that the apparent specific activity of the SnOx / Pt-Cu-Ni heterojunction catalyst is improved by up to 40% compared to pure Pt-Cu-Ni.

[0007] Patent Documents 1 and 2 state that coating the surface of carbon with a certain metal oxide improves the performance of the electrode catalyst. However, in the electrode catalysts described in Patent Documents 1 and 2, the metal oxide is supported on the carbon surface and does not coat the active species (platinum fine particles). Therefore, when such an electrode catalyst is used in the catalyst layer of a fuel cell, contact between the ionomer, which is a proton conductor, and the active species cannot be avoided. As a result, the catalyst may be poisoned by the ionomer, resulting in a decrease in catalytic activity. In addition, since the ionomer has a low pH, it is believed that contact between the catalyst particles and the ionomer accelerates the dissolution of the active species (platinum fine particles) during the operation of the fuel cell.

[0008] On the other hand, Non-Patent Document 1 reports that the oxygen reduction activity is improved by coating the active species (Pt-Cu-Ni alloy) with tin oxide. However, this effect is obtained because separate elementary reactions occur on both the tin oxide surface and the Pt-Cu-Ni alloy surface, and the energy barrier of the total oxygen reduction reaction is reduced as a result, and is not due to the suppression of ionomer poisoning. In addition, the amount of tin oxide coating per carrier surface area is 0.3 mg / m 2 Therefore, it is considered that there is no effect of suppressing ionomer poisoning. Therefore, even if this is applied to an actual cell, the catalytic activity is not exhibited.

[0009] Furthermore, the activity of catalyst layers containing conventional electrode catalysts is likely to decrease in low-humidity environments, which is believed to be because the proton conductivity of the ionomer decreases in low-humidity environments, making it difficult for protons to be supplied to the catalyst particles. However, there have been no examples of electrode catalysts proposed to date that exhibit relatively high activity even in low humidity environments and that are capable of suppressing the decrease in activity due to ionomer poisoning and the deterioration of catalyst particles caused by ionomers. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] JP 2013-098091 A [Patent Document 2] JP 2012-000525 A [Non-patent literature]

[0011] [Non-Patent Document 1] J.Am.Chem.Soc. 2019, 141, 9463-9467:Dual-Site Cascade Oxygen Reduction Mechanism on SnOx / Pt-Cu-Ni for Promoting Reaction Kinetics Summary of the Invention [Problem to be solved by the invention]

[0012] The problem to be solved by the present invention is to provide an electrode catalyst for a fuel cell that exhibits relatively high activity even in a low humidity environment, and that is capable of suppressing a decrease in activity due to ionomer poisoning and deterioration of catalyst particles caused by the ionomer. [Means for solving the problem]

[0013] In order to solve the above problems, the fuel cell electrode catalyst according to the present invention comprises: A carrier made of an electronic conductive material; Catalyst particles supported on the surface of the support; Oxide nanoparticles that modify the surface of the catalyst particles; It is equipped with: Effect of the Invention

[0014] When the surface of catalyst particles is modified with oxide nanoparticles, the decrease in activity in low-humidity environments is suppressed. This is thought to be because the hydrophilic nature of oxide nanoparticles makes it easier for water necessary for proton conduction to be retained around the catalyst particles even in low-humidity environments. In addition, when the surface of the catalyst particles is modified with oxide nanoparticles, the decrease in activity due to ionomer poisoning is suppressed. This is believed to be because the modification of the surface of the catalyst particles with oxide nanoparticles suppresses the adsorption of the acid groups of the ionomer onto the surface of the catalyst particles. Furthermore, when the surface of the catalyst particles is modified with oxide nanoparticles, the deterioration of the catalyst particles caused by dissolution and reprecipitation of the catalyst particles is suppressed. This is thought to be because the contact between the catalyst particles and the low-pH ionomer is suppressed, making the dissolution of the catalyst particles difficult to occur. [Brief description of the drawings]

[0015] [Figure 1]1 shows a high-angle annular dark field (HAADF) image (upper left), elemental mapping of Pt (lower left), elemental mapping of O (upper right), and elemental mapping of Sn (lower right) of the fuel cell electrode catalyst obtained in Example 1. [Diagram 2] FIG. 1 is a graph showing the ECSA maintenance rate versus the number of cycles in a potential fluctuation test. [Diagram 3] FIG. 1 shows mass activity before and after a potential fluctuation test under conditions of temperature: 60° C., humidity: 80% RH, and voltage: 0.84 V. [Figure 4] FIG. 1 shows mass activity before and after a potential fluctuation test under conditions of temperature: 82° C., humidity: 30% RH, and voltage: 0.84 V. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] An embodiment of the present invention will be described in detail below. [1. Electrode catalyst for fuel cells] The fuel cell electrode catalyst according to the present invention comprises: A carrier made of an electronic conductive material; Catalyst particles supported on the surface of the support; Oxide nanoparticles that modify the surface of the catalyst particles; It is equipped with:

[0017] [1.1. Carrier] [1.1.1. Materials] In the present invention, the material of the support is not particularly limited as long as it is a material having electronic conductivity. Here, "having electronic conductivity" means an electronic conductivity of 1.0×10 -5 S / cm or higher.

[0018] Examples of the carrier material include: (a) Carbon, (b) Ti x O 2x-1 (x≧1), conductive oxides such as SnO2, (c) Conductive nitrides such as TiN, ZrN, and TaN, (d) Conductive borides such as TiB2, ZrB, TaB2, NbB2, WB, MoB, and CrB; (e) Conductive carbides such as TiC, SiC, WC, and ZrC, etc. The carrier may consist of any one of these, or may be a mixture of two or more of them.

[0019] [1.1.2. Average particle size] The term "average particle size" refers to the average length of particles in the minor axis direction, as measured by observing 100 or more particles under a microscope.

[0020] In the present invention, the average particle size of the carrier is not particularly limited, and an optimal value can be selected according to the purpose. In general, if the average particle size of the carrier is too small, the gap between the carrier particles constituting the electrode becomes small, and the movement resistance of the reactants and products moving through the gap may increase. Therefore, the average particle size of the carrier is preferably 10 nm or more. The average particle size is more preferably 30 nm or more, and more preferably 50 nm or more. On the other hand, if the average particle size of the carrier is too large, the surface area becomes small, and it may become impossible to support the active species in a fine particle form with high dispersion. Therefore, the average particle size of the carrier is preferably 500 nm or less. The average particle size is more preferably 200 nm or less, and even more preferably 100 nm or less.

[0021] [1.2. Catalyst particles] [1.2.1. Materials] In the present invention, the material of the catalyst particles is not particularly limited as long as it is a material that has activity in the oxygen reduction reaction and / or the hydrogen oxidation reaction.

[0022] Examples of materials for the catalyst particles include: (a) Precious metals (Pt, Au, Ag, Pd, Rh, Ir, Ru, Os), (b) Precious metal alloys containing two or more precious metal elements; (c) Precious metal-base metal alloys containing one or more precious metal elements and one or more base metal elements (e.g., Fe, Co, Ni, Cr, V, Ti, etc.); etc. The catalyst particles may consist of any one of these, or may be a mixture of two or more of them.

[0023] Among these, the catalyst particles are preferably made of Pt or a Pt alloy, since they have high activity in the electrode reaction of the fuel cell. Examples of Pt alloys include Pt-Fe alloys, Pt-Co alloys, Pt-Ni alloys, Pt-Pd alloys, Pt-Cr alloys, Pt-V alloys, Pt-Ti alloys, Pt-Ru alloys, and Pt-Ir alloys.

[0024] [1.2.2. Crystallite size] The term "crystallite size" refers to the size of the crystallite calculated by Scherrer's formula based on the X-ray diffraction peak.

[0025] In the present invention, the crystallite diameter of catalyst particles is not particularly limited, and can be selected as the most suitable value according to the purpose. In general, if the crystallite diameter of catalyst particles is too small, the catalyst particles are easily dissolved, and the durability of fuel cells may be reduced. Therefore, the crystallite diameter of catalyst particles is preferably 2 nm or more. The crystallite diameter is more preferably 3 nm or more. On the other hand, if the crystallite size of the catalyst particles is too large, the reaction surface area of ​​the catalyst particles will be small, and the amount of catalyst required to ensure performance may be large. Therefore, the crystallite size of the catalyst particles is preferably 10 nm or less. The crystallite size is more preferably 5 nm or less.

[0026] [1.2.3. Content] "Catalyst particle content" refers to the surface area of ​​the support (S[m 2 The mass of the catalyst particle (M1 [mg]) is the ratio (=M1 / S) of the mass of the catalyst particle (M1 [mg]) to the mass of the catalyst particle (M1 [mg]).

[0027] In the present invention, the content of the catalyst particles is not particularly limited, and an optimal value can be selected depending on the purpose. In general, if the content of the catalyst particles is too small, the electrode becomes thick, and the mass transfer resistance in the direction perpendicular to the surface of the electrode (thickness direction) may increase. Therefore, the content of the catalyst particles is preferably 0.1 mg / m 2 More preferably, the content is 0.40 mg / m or more. 2 More preferably, 1.0 mg / m 2 That's all. On the other hand, if the content of catalyst particles is excessive, the active species cannot be supported in a highly dispersed fine particle form, and the reaction surface area of ​​the catalyst may become small. Therefore, the content of catalyst particles is set to 10 mg / m 2 The content is preferably 5.0 mg / m or less. 2 More preferably, 2.0 mg / m 2 The following is the result.

[0028] [1.3. Oxide nanoparticles] [1.3.1. Qualification] The surface of the catalyst particles is modified with oxide nanoparticles. Here, "the surface of the catalyst particle is modified with oxide nanoparticles" means that the oxide nanoparticles are arranged on the outside of the catalyst particle so as to prevent contact between the ionomer and the catalyst particle, and does not necessarily mean that the catalyst particle and the oxide nanoparticle are in contact. However, if there is a large gap between the catalyst particle and the oxide nanoparticle, the ionomer may enter through the large gap and poison the catalyst particle. Therefore, it is preferable that the catalyst particle and the oxide nanoparticle are in contact with each other.

[0029] An electrode catalyst in which the surface of the catalyst particle is modified with oxide nanoparticles can be obtained by supporting the catalyst particle on a support surface, and then supporting the oxide nanoparticles on the support surface on which the catalyst particle is supported. The details of the manufacturing method of the electrode catalyst will be described later.

[0030] [1.3.2. Materials] When the surface of catalyst particles is modified with oxide nanoparticles, the decrease in activity in low-humidity environments is suppressed. This is thought to be because the hydrophilic nature of oxide nanoparticles makes it easier for water necessary for proton conduction to be retained around the catalyst particles even in low-humidity environments.

[0031] In the present invention, the material of the oxide nanoparticles is not particularly limited. The oxide nanoparticles may be a material having electronic conductivity or may be an insulating material. Even if the oxide nanoparticles are an insulating material, there is no problem with the electrode reaction as long as an electron conduction path for supplying electrons to the catalyst particles is secured. However, when the oxide nanoparticles are an insulating material, if the amount of modification with the oxide nanoparticles is excessive, the electron conduction path to the catalyst particle may be interrupted. Therefore, the oxide nanoparticles are preferably made of a material having electron conductivity.

[0032] Examples of materials for oxide nanoparticles include: (a) Tin oxide nanoparticles, soot oxide nanoparticles containing dopants, (b) Titanium oxide nanoparticles, titanium oxide nanoparticles containing dopants The oxide nanoparticles may be made of any one of these materials, or may be a mixture of two or more of these materials. Among these, the oxide nanoparticles are preferably tin oxide nanoparticles and / or soot oxide nanoparticles containing a dopant, because the nanoparticles can be easily formed by the oxygen dissolved in the reaction solution or the oxygen-containing functional groups on the support surface, and the particle size of the nanoparticles can be controlled by the temperature and time of the heat treatment after the nanoparticles are generated.

[0033] [1.3.3. Crystallite size] In the present invention, the crystallite diameter of the oxide nanoparticles is not particularly limited, and an optimal value can be selected according to the purpose. In general, if the crystallite diameter of the oxide nanoparticles is too small, the size of the gap between the oxide nanoparticles when the closest packing is assumed becomes excessively small. As a result, the mass transfer resistance from the outside to the catalyst particles may increase. Therefore, the crystallite diameter of the oxide nanoparticles is preferably 2 nm or more. The crystallite diameter is more preferably 3 nm or more. On the other hand, if the crystallite diameter of the oxide nanoparticles is too large, the size of the gap between the oxide nanoparticles when they are assumed to be closely packed becomes excessively large. As a result, the ionomer may enter through the gap and poison the catalyst particles. Therefore, the crystallite diameter of the oxide nanoparticles is preferably 10 nm or less. The crystallite diameter is more preferably 5 nm or less.

[0034] [1.3.4. Content] The "content of oxide nanoparticles" refers to the surface area of ​​the support (S[m 2 The mass of oxide nanoparticles (M2 [mg]) is the ratio (=M2 / S) of the mass of oxide nanoparticles (M2 [mg]) to the mass of oxide nanoparticles (M2 [mg]).

[0035] In the present invention, the content of oxide nanoparticles is not particularly limited, and an optimal value can be selected depending on the purpose. In general, if the content of oxide nanoparticles is too small, the ratio of catalyst particles whose surfaces are not modified with oxide nanoparticles increases. As a result, performance degradation in low humidity environments, catalyst poisoning by ionomers, or catalyst deterioration is likely to occur. Therefore, the content of oxide nanoparticles is preferably 1 mg / m 2 More preferably, the content is 1.5 mg / m 2 That's all. On the other hand, if the content of oxide nanoparticles is excessive, the surface of the catalyst particles is covered with a thick layer of oxide nanoparticles, which may increase the mass transfer resistance. Therefore, the content of oxide nanoparticles is set to 20 mg / m 2 The content is preferably 5 mg / m or less. 2 The following is the result.

[0036] [1.4. Electronic conductivity of powder compacts] The "electronic conductivity of the compact" refers to the electronic conductivity calculated using the current and voltage obtained by applying a pressing pressure of 2 MPa to a compact made of a fuel cell electrode catalyst and measuring the voltage while passing a constant current through the compact.

[0037] Generally, for an electrode reaction to proceed on the surface of a catalyst particle, electrons must be supplied to the catalyst surface or electrons must be removed from the catalyst surface, so the higher the electronic conductivity of the electrode catalyst for fuel cells, the better. By using the method described below, a fuel cell electrode catalyst having an electronic conductivity of 0.15 S / cm or more for the compact can be obtained.

[0038] [1.5. Purpose] The fuel cell electrode catalyst according to the present invention can be used as either an air electrode catalyst or a fuel electrode catalyst. The fuel cell electrode catalyst according to the present invention is suitable as an air electrode catalyst because the catalyst particles are not easily deteriorated even when potential fluctuation occurs.

[0039] [2. Manufacturing method of fuel cell electrode catalyst] The fuel cell electrode catalyst according to the present invention comprises: (a) supporting catalyst particles on a support surface; (b) Oxide nanoparticles are further supported on the surface of the support on which the catalyst particles are supported. It can be produced by the above method.

[0040] [2.1. 1st step] First, catalyst particles are supported on the surface of the carrier. The method for supporting the catalyst particles on the surface of the carrier is not particularly limited, and a known method can be used. In addition, a commercially available electrode catalyst (one in which catalyst particles are supported on the surface of the carrier) may be used as it is.

[0041] [2.2. 2nd process] Next, oxide nanoparticles are further supported on the surface of the support on which the catalyst particles are supported. The method for supporting the oxide nanoparticles is not particularly limited, and any method can be used as long as it is possible to modify the surface of the catalyst particles with oxide nanoparticles.

[0042] For example, when the oxide nanoparticles are tin oxide nanoparticles, a carrier carrying catalyst particles is dispersed in an aqueous tin chloride solution and stirred in the air, whereby the tin chloride is oxidized by the oxygen-containing functional groups on the carrier surface and dissolved oxygen to form tin oxide nanoparticles, and when stirred for a predetermined time, the catalyst particle surfaces are modified with tin oxide nanoparticles. After the predetermined time has elapsed, the solid content is separated from the dispersion and dried to obtain the fuel cell electrode catalyst according to the present invention.

[0043] Other methods for modifying the surface of catalyst particles with oxide nanoparticles include, for example: (a) Atomic layer deposition method, (b) Sol-gel method, etc.

[0044] [3. Effect] The catalyst layer is made of a composite of an electrode catalyst and an ionomer. When generating electricity in a fuel cell, protons are supplied to the surface of the catalyst particles via the ionomer. However, in a low-humidity environment, the proton conductivity of the ionomer decreases, making it difficult for protons to be supplied to the surface of the catalyst particles. Therefore, in general, when generating electricity in a low-humidity environment, the activity of the catalyst particles is likely to decrease.

[0045] It is also known that the catalytic activity decreases when the sulfonic acid groups of the ionomer are adsorbed on the surface of the catalyst particles. Moreover, it is known that the decrease in activity due to catalyst poisoning is greater in a low humidity environment. Furthermore, it is known that when catalyst particles are exposed to potential fluctuations, the metal elements contained in the catalyst particles are repeatedly dissolved and reprecipitated, causing the catalyst particles to become coarse. In particular, since the ionomer has a low pH, when the ionomer comes into contact with the catalyst particles, the dissolution of the catalyst particles may be accelerated.

[0046] On the other hand, Patent Document 1 discloses an electrode catalyst obtained by forming a metal oxide layer so as to surround platinum fine particles supported on the surface of a support. Patent Document 2 discloses an electrode catalyst obtained by modifying the surface of a carbon support with tin oxide and further supporting platinum fine particles on the surface. However, in both of the electrode catalysts described in Patent Documents 1 and 2, the platinum fine particles are exposed on the outermost surface, and it is considered difficult to suppress the decrease in activity in a low humidity environment, the decrease in activity due to ionomer poisoning, and / or the decrease in activity due to the coarsening of catalyst particles.

[0047] In contrast, when the surface of the catalyst particles is modified with oxide nanoparticles, the decrease in activity in low-humidity environments is suppressed. This is thought to be because the oxide nanoparticles are hydrophilic, which makes it easier for the water necessary for proton conduction to be retained around the catalyst particles even in low-humidity environments. In addition, when the surface of the catalyst particles is modified with oxide nanoparticles, the decrease in activity due to ionomer poisoning is suppressed. This is believed to be because the modification of the surface of the catalyst particles with oxide nanoparticles suppresses the adsorption of the acid groups of the ionomer onto the surface of the catalyst particles. Furthermore, when the surface of the catalyst particles is modified with oxide nanoparticles, the deterioration of the catalyst particles caused by dissolution and reprecipitation of the catalyst particles is suppressed. This is thought to be because the contact between the catalyst particles and the low-pH ionomer is suppressed, making the dissolution of the catalyst particles difficult to occur. EXAMPLES

[0048] (Example 1, Comparative Example 1) [1. Sample preparation] [1.1. Preparation of electrode catalyst] 1.1.1. Example 1 Pt / C (Tanaka Kikinzoku Kogyo Co., Ltd., TEC10V30E) was used as the electrode catalyst before supporting tin oxide nanoparticles (hereinafter, also referred to as the "unmodified catalyst"). To wash the unmodified catalyst, the unmodified catalyst was dispersed in hot water at 80°C and subjected to ultrasonic treatment for 5 minutes. The unmodified catalyst was then collected by suction filtration. This treatment was carried out three times, and the unmodified catalyst was then vacuum dried at 100°C for 2 hours.

[0049] Next, 5.6 mL of 35 mass% HCl solution was added to 200 mL of pure water, and 1.4 g of tin(II) chloride and 0.2 g of unmodified catalyst (Pt / C) were added thereto, and the mixture was stirred for 2 hours at room temperature in the air using a stirrer. The residue recovered by suction filtration was then washed and vacuum dried under the same conditions as those for washing and vacuum drying the unmodified catalyst, to obtain an electrode catalyst. Hereinafter, the electrode catalyst obtained in Example 1 is also referred to as a "tin oxide modified catalyst."

[0050] [1.1.2. Comparative Example 1] The unmodified catalyst obtained in Example 1 after washing and drying in vacuum was directly subjected to the test.

[0051] [1.2. Preparation of MEA] [1.2.1. Preparation of catalyst sheet] A water / ethanol mixed solvent (volume ratio: 0.65) and an ionomer (D2020, manufactured by Chemours) were added to the electrode catalyst obtained in Example 1 or Comparative Example 1, and a catalyst dispersion was prepared by ultrasonic treatment. The amount of the ionomer added was set so that the ratio of the mass of the ionomer to the mass of the support carbon (I / C) was 0.7. Next, the catalyst dispersion was applied onto a polytetrafluoroethylene sheet using a coater, and the sheet was left in the air for 1 hour, after which it was further dried in a dryer at 80°C for 1 hour to obtain an air electrode catalyst sheet. The anode catalyst sheet was prepared in the same manner as the cathode catalyst sheet, except that a commercially available electrode catalyst was used.

[0052] [1.2.2. Hot pressing] The air electrode catalyst layer and the anode catalyst layer were cut out to 1 cm square from the air electrode catalyst sheet and the anode catalyst sheet, respectively. An electrolyte membrane (NR211, manufactured by Chemours) was sandwiched between the air electrode catalyst layer and the anode catalyst layer, and hot pressed to obtain an MEA. The hot pressing was performed under the following conditions: preheating at 120°C for 5 minutes, pressing pressure: 50 kPa, and pressing time: 5 minutes.

[0053] 2. Test Method [2.1. Characterization of electrocatalysts] [2.1.1. Crystallite size] X-ray diffraction (XRD) was performed on the tin oxide modified catalyst and the unmodified catalyst. For the XRD measurement, a Rigaku Ultima IV was used. The crystallite size of the tin oxide nanoparticles was calculated from the (211) diffraction peak by the Scherrer equation, while the crystallite size of the Pt particles was calculated from the (111) diffraction peak.

[0054] [2.1.2. Amount of modification (Pt or tin oxide content per unit surface area)] Thermogravimetry (TG) was performed on the tin oxide modified catalyst and the unmodified catalyst. For TG measurement, a Rigaku Thermplus II was used, and the temperature was raised to 900°C at a rate of 5°C / min under air flow (100mL / m).

[0055] Next, the mass ratio of Pt to carbon (R Pt ) and the mass ratio of tin oxide to carbon (R SnO2 The mass ratio was then calculated based on the surface area (250 m) of 1 g of carbon. 2 ) to calculate the modification amount (mass of Pt or tin oxide per unit surface area).

[0056] R Pt (mass%)=W2×100 / (W1-W2) …(1) R SnO2 (mass%)=Q2×100 / (Q1-Q2)-R Pt…(2) however, W1 is the mass of the unmodified catalyst before TG measurement, W2 is the mass of the unmodified catalyst after TG measurement, Q1 is the mass of the tin oxide modified catalyst before TG measurement, Q2 is the mass of the tin oxide modified catalyst after TG measurement.

[0057] [2.1.3. Modification state] The modification state of the tin oxide modified catalyst was examined by STEM-EDX analysis using a JEM-2100F (manufactured by JEOL Ltd.).

[0058] [2.1.4. Electronic conductivity] The tin oxide modified catalyst and the unmodified catalyst were each pressed and their resistance was measured at a pressure of 2 MPa. The apparent electronic conductivity was calculated from the resistance and thickness.

[0059] [2.2. Cell evaluation] First, a break-in was performed using the following evaluation equipment. Then, the power generation performance was evaluated using the following evaluation equipment. The details of the evaluation are described below.

[0060] [2.2.1. Evaluation equipment] Details of the evaluation device are as follows. <Evaluation bench> CO evaluation bench (manufactured by CHINO) <Electrochemical measurement equipment> Potentiostat: 2100 (manufactured by Toho Giken Co., Ltd.) AC resistance measuring device: FC-100R (manufactured by CHINO) <Single cell> Cell: 1cm 2 Square cell for Diffusion layer: Carbon paper (with microporous layer) Current collector: gold-plated copper plate with integrated flow path (flow path: straight flow path with 0.4 mm pitch)

[0061] [2.2.2. Break-in] The MEA was run-in by sweeping the generated current under the following conditions: Cell temperature / relative humidity (both poles): 60℃ / 80%RH Air electrode gas: 21% O2 / N2, 1000mL / min, atmospheric pressure Fuel electrode gas: H2, 500mL / min, atmospheric pressure Current sweep: 50mA / (s cm) from open circuit voltage to -0.1V 2 ) 30 sweeps

[0062] [2.2.3. Power generation performance evaluation] The IV curve was measured by current sweep. To perform IR correction, the cell resistance was measured simultaneously with the current sweep. The measurement conditions were as follows: Cell temperature / relative humidity (both poles): Two conditions: 60℃ / 80%RH or 82℃ / 30%RH Air electrode gas: Air, 2000mL / min, 50kPa-G Fuel electrode gas: H2, 500mL / min, 30kPa-G Current sweep: 10mA / (s cm) from open circuit voltage to -0.1V 2 ) sweep was performed three times (the data from the third sweep was used as the power generation performance) Cell resistance measurement frequency: 10kHz

[0063] [2.2.4. Potential fluctuation test] A potential fluctuation test was conducted to examine the change in the ECSA retention rate during the test. The measurement conditions were as follows: Cell temperature / relative humidity (both poles): 60℃ / 80%RH Air electrode gas: N2, 1000mL / min Fuel electrode gas: 10% H2 / N2, 1000mL / min Potential control: Lower limit potential 0.6V vs RHE, held for 3s → Upper limit potential 1.0V vs RHE, held for 3s, 500 cycles, then cyclic voltammogram (115mV vs RHE⇔1000mV vs RHE, 50mV / s) was measured for 5 cycles. 20 sets of the above were performed.

[0064] In addition, the ECSA during the voltage fluctuation test was calculated by setting the charge in the hydrogen desorption region of the CV at 210 μC / cm, which is the charge of hydrogen adsorption and desorption per unit area of ​​polycrystalline Pt. 2 This was calculated by dividing by .

[0065] [3. Results] [3.1. Characterization of electrocatalysts] [3.1.1. Amount of modification, crystallite size, and electronic conductivity] The modification amount, crystallite size, and electronic conductivity of the tin oxide modified catalyst (Example 1) and the unmodified catalyst (Comparative Example 1) are shown in Table 1. From Table 1, the following can be seen.

[0066] (1) The amount of Pt modified in the tin oxide modified catalyst is 1.6 mg / m 2 The amount of tin oxide modification was 2.6 mg / m 2 It was. (2) The crystallite diameter of the tin oxide nanoparticles was 2.6 nm, which was slightly larger than the crystallite diameter of the Pt particles, 2.3 nm. (3) The electronic conductivity of the tin oxide modified catalyst was equivalent to that of the unmodified catalyst, and no decrease in electronic conductivity was observed due to the tin oxide modification layer.

[0067] [Table 1]

[0068] [3.1.2. Modification state] 1 shows a high angle annular dark field (HAADF) image (upper left), elemental mapping of Pt (lower left), elemental mapping of O (upper right), and elemental mapping of Sn (lower right) of the fuel cell electrode catalyst obtained in Example 1. Since Sn is distributed around Pt, it is considered that SnO2 modifies Pt.

[0069] [3.2. Cell performance] Figure 2 shows the ECSA retention rate versus the number of cycles in the potential fluctuation test. Figure 3 shows the mass activity before and after the potential fluctuation test under conditions of temperature: 60°C, humidity: 80% RH, and voltage: 0.84 V. Figure 4 shows the mass activity before and after the potential fluctuation test under conditions of temperature: 82°C, humidity: 30% RH, and voltage: 0.84 V. The following can be seen from Figures 2 to 4.

[0070] (1) The MEA using the tin oxide modified catalyst (Example 1) at the air electrode showed a smaller decrease in ECSA retention rate against voltage fluctuation than the MEA using the unmodified catalyst (Comparative Example 1). This shows that modifying Pt with tin oxide can suppress the decrease in the surface area of ​​Pt.

[0071] (2) Under high humidity conditions (temperature: 60°C, humidity: 80% RH), the mass activity of the MEA of Example 1 before the potential fluctuation test was equivalent to that of Comparative Example 1. On the other hand, under low humidity conditions (temperature: 82°C, humidity: 30% RH), the mass activity of the MEA of Example 1 before the potential fluctuation test was higher than that of Comparative Example 1. It was found from Figures 3 and 4 that modifying Pt with tin oxide has almost no effect on the mass activity under high humidity conditions, but modifying Pt with tin oxide improves the mass activity under low humidity conditions.

[0072] (3) Under both high and low humidity conditions, the mass activity after the durability test of the MEA of Example 1 was higher than that of Comparative Example 1. This is believed to be because the dissolution and reprecipitation of Pt was suppressed by modifying Pt with tin oxide.

[0073] Although the embodiment of the present invention has been described in detail above, the present invention is not limited to the above embodiment, and various modifications are possible without departing from the gist of the present invention. [Industrial Applicability]

[0074] The fuel cell electrode catalyst according to the present invention can be used as an electrode catalyst for an air electrode catalyst layer of a polymer electrolyte fuel cell, or as an electrode catalyst for an anode catalyst layer.

Claims

1. A carrier made of an electronic conductive material; Catalyst particles supported on the surface of the support; Oxide nanoparticles that modify the surface of the catalyst particles; Equipped with The crystallite size of the oxide nanoparticles is 2 nm or more and 10 nm or less; The content of the oxide nanoparticles is 1 mg / m 2 or more and 20 mg / m 2 or more. Electrode catalyst for fuel cells. Here, the "content of oxide nanoparticles" refers to the ratio (=M 2 / S) of the mass of the oxide nanoparticles (M 2 [mg]) to the surface area of ​​the support (S [m 2 ]).

2. 2. The fuel cell electrode catalyst according to claim 1, wherein the support comprises at least one selected from the group consisting of carbon, a conductive oxide, a conductive nitride, a conductive boride, and a conductive carbide.

3. 3. The fuel cell electrode catalyst according to claim 1, wherein the average particle diameter of the carrier is from 10 nm to 500 nm.

4. The catalyst particles are (a) Precious metals; (b) a precious metal alloy containing two or more precious metal elements; and (c) A precious metal-base metal alloy containing one or more precious metal elements and one or more base metal elements.

4. The fuel cell electrode catalyst according to claim 1, comprising at least one selected from the group consisting of:

5. 5. The fuel cell electrode catalyst according to claim 1, wherein the catalyst particles have a crystallite size of 2 nm or more and 10 nm or less.

6. The content of the catalyst particles is 0.1 mg / m 2 10mg / m or more 2 6. The fuel cell electrode catalyst according to claim 1, wherein: However, the "content of catalyst particles" refers to the surface area (S [m 2 ]) relative to the mass of the catalyst particles (M 1 [mg]) ratio (=M 1 / S).

7. 7. The fuel cell electrode catalyst according to claim 1, wherein the oxide nanoparticles comprise tin oxide nanoparticles and / or soot oxide nanoparticles containing a dopant.

8. 8. The fuel cell electrode catalyst according to claim 1, wherein the powder compact has an electronic conductivity of 0.15 S / cm or more. Here, the "electronic conductivity of the compact" refers to the electronic conductivity calculated using a current and a voltage measured while a constant current is passed through the compact made of the fuel cell electrode catalyst in a state where a pressing pressure of 2 MPa is applied to the compact.

Citation Information

Patent Citations

  • Membrane electrode complex for polymer electrolyte fuel cell

    JP2003036857A

  • Fuel cell electrode catalyst and manufacturing method therefor

    JP2005270864A

  • Membrane-electrode structure for solid polymer fuel cell

    JP2011253723A

  • Composite electrode catalyst and method for manufacturing the same

    JP2012000525A

  • Platinum-metal oxide composite catalyst for fuel cell, and method for producing the same