Anode and all-solid-state secondary battery including same

The novel negative electrode structure with a high-hardness coating layer and sulfide-based electrolyte in all-solid-state batteries addresses the issues of electrode deterioration and micro-cracks, enhancing the battery's cycle characteristics and safety.

JP7596166B2Active Publication Date: 2024-12-09SAMSUNG SDI CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2021023693
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-02-18
Filing Date
2021-02-17
Publication Date
2024-12-09
Estimated Expiration
2041-02-17

AI Technical Summary

Technical Problem

Lithium-ion batteries using flammable organic solvents are prone to fires due to short circuits, and existing all-solid-state batteries face issues with negative electrode deterioration and micro-cracks in the solid electrolyte layer, leading to reduced cycle characteristics.

Method used

A negative electrode with a novel structure featuring a first metal base material coated with a second metal layer having higher Mohs hardness, combined with a sulfide-based solid electrolyte layer, to prevent electrode deterioration and micro-cracks, thereby improving cycle characteristics.

Benefits of technology

The novel electrode structure enhances the durability of the negative electrode and suppresses short circuits, resulting in improved cycle characteristics and safety of all-solid-state secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007596166000002
    Figure 0007596166000002
  • Figure 0007596166000003
    Figure 0007596166000003
  • Figure 0007596166000004
    Figure 0007596166000004
Patent Text Reader

Abstract

To provide a negative electrode and an all-solid-state secondary battery including the same.SOLUTION: A negative electrode includes a negative electrode current collector, and a first negative electrode active material layer arranged on the negative electrode current collector, and the negative electrode current collector includes a first metal base material, and a coating layer that is placed on the first metal base material and includes a second metal, the Mohs hardness of the second metal is higher than the Mohs hardness of the first metal, and there is also provided an all-solid-state secondary battery including the negative electrode.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a negative electrode and an all-solid-state secondary battery. [Background technology]

[0002] Recently, due to industrial demand, there has been active development of batteries with high energy density and safety. For example, lithium ion batteries have been put to practical use not only in the fields of information-related devices and communication devices, but also in the field of automobiles. In the field of automobiles, safety is particularly important because life is at stake.

[0003] Currently available lithium-ion batteries use electrolytes containing flammable organic solvents, which can lead to overheating and fires if a short circuit occurs. Therefore, all-solid-state batteries that use solid electrolytes instead of electrolytes have been proposed.

[0004] Since the all-solid-state battery does not use flammable organic solvents, the possibility of fire or explosion can be significantly reduced even if a short circuit occurs, and therefore the all-solid-state battery can be significantly safer than lithium-ion batteries that use electrolytes. Summary of the Invention [Problem to be solved by the invention]

[0005] The problem to be solved by the present invention is to provide a negative electrode having a novel structure.

[0006] Another problem to be solved by the present invention is to provide an all-solid-state secondary battery including a negative electrode having a novel structure. [Means for solving the problem]

[0007] From one aspect, a negative electrode current collector; and a first negative electrode active material layer disposed on the negative electrode current collector, the negative electrode current collector includes a first metal substrate and a coating layer disposed on the first metal substrate and including a second metal; A negative electrode is provided in which the second metal has a higher Mohs hardness than the first metal.

[0008] From another perspective, A positive electrode and The negative electrode; a solid electrolyte layer disposed between the positive electrode and the negative electrode; An all-solid-state secondary battery is provided, in which the solid electrolyte layer includes a sulfide-based solid electrolyte. Effect of the Invention

[0009] According to the present invention, by employing a negative electrode having a novel structure, it is possible to provide an all-solid-state secondary battery in which deterioration of the negative electrode current collector is prevented and cycle characteristics are improved. [Brief description of the drawings]

[0010] [Figure 1] FIG. 2 is a cross-sectional view of a negative electrode according to an exemplary embodiment. [Diagram 2] FIG. 2 is a cross-sectional view of a negative electrode according to another exemplary embodiment. [Diagram 3] FIG. 1 is a cross-sectional view of an all-solid-state secondary battery according to an exemplary embodiment. [Figure 4] FIG. 1 is a cross-sectional view of a bi-cell all-solid-state secondary battery according to an exemplary embodiment. [Diagram 5] FIG. 2 is a schematic diagram of a positive electrode layer of an all-solid-state secondary battery according to an exemplary embodiment. [Figure 6] FIG. 1 is a schematic diagram partially illustrating the inside of an all-solid-state secondary battery according to an exemplary embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] In the charge and discharge process of the all-solid-state secondary battery, the lithium-containing metal layer is precipitated on the negative electrode current collector, and the precipitated lithium-containing metal layer is dissolved. The lithium-containing metal layer precipitated on the negative electrode current collector by repeated charge and discharge of the all-solid-state secondary battery contains impurities remaining in the electrode, decomposition products of the solid electrolyte, and the like. Therefore, by containing such impurities, the surface of the lithium-containing metal layer becomes rough and hard. The lithium-containing metal layer having such a rough surface forms unevenness such as scratches on the negative electrode current collector, and the lithium-containing metal layer is further precipitated unevenly due to the unevenness such as scratches on the negative electrode current collector. Such uneven deposition of the lithium-containing metal layer applies uneven pressure to the solid electrolyte layer in contact with the negative electrode, generating fine cracks in the solid electrolyte layer, and such cracks in the solid electrolyte layer grow during repeated charge and discharge processes. The growth of lithium through such cracks causes a short circuit between the positive electrode and the negative electrode.

[0012] The negative electrode according to one embodiment has a novel structure, which prevents deterioration of the negative electrode current collector, suppresses the occurrence of a short circuit in an all-solid-state secondary battery using such a negative electrode, and improves cycle characteristics.

[0013] The present inventive concept described below can be modified in various ways and can have various embodiments, but specific embodiments are illustrated in the drawings and described in detail. However, it should be understood that the present inventive concept is not limited to the specific embodiments, but includes all modifications, equivalents, or alternatives included in the technical scope of the present inventive concept.

[0014] The terms used below are merely used to describe specific embodiments and are not intended to limit the inventive idea. A singular expression includes a plural expression unless otherwise clearly indicated in the context. In the following, terms such as "comprise" or "have" indicate the presence of a feature, number, step, operation, component, part, ingredient, material, or combination thereof described in the specification, and should be understood not to preclude the presence or addition of one or more other features, numbers, steps, operations, components, parts, ingredients, materials, or combinations thereof. In the following, " / " can be interpreted as "and" or "or" depending on the context.

[0015] In the drawings, the thickness of the various layers and regions is exaggerated or reduced for clarity. Similar parts are designated by the same reference numerals throughout the specification. Throughout the specification, when a part, such as a layer, film, region, or plate, is described as being "on" or "above" another part, it includes not only when it is directly on top of the other part, but also when there is an intermediate part or other part. Throughout the specification, terms such as first and second may be used to describe various components, but the components are not limited by the terms. The terms are used only to distinguish one component from another. In this specification and the drawings, components having substantially the same functional configuration are referred to by the same reference numerals to avoid redundant description.

[0016] The negative electrodes and all-solid-state secondary batteries according to the exemplary embodiments will be described in further detail below.

[0017] [Negative electrode] The negative electrode according to one embodiment includes a negative electrode current collector and a first negative electrode active material layer disposed on the negative electrode current collector, the negative electrode current collector including a first metal substrate and a coating layer disposed on the first metal substrate and including a second metal, the second metal having a higher Mohs hardness than the first metal. The coating layer including the second metal having a higher Mohs hardness than the first metal, i.e., harder, is disposed on the first metal substrate included in the negative electrode current collector, thereby suppressing the formation of irregularities such as scratches on the first metal substrate due to the lithium-containing metal layer deposited during the charge and discharge process. This can improve the uniformity of the lithium-containing metal layer formed on the negative electrode current collector during the charge and discharge process. Therefore, during the charge and discharge process, cracks in the solid electrolyte layer in contact with the negative electrode are suppressed, and short circuits of the all-solid-state secondary battery using such a negative electrode are suppressed. As a result, the cycle characteristics of the all-solid-state secondary battery using such a negative electrode can be improved.

[0018] 1 and 2, the negative electrode 20 includes a negative electrode current collector 21 and a first negative electrode active material layer 24 disposed on the negative electrode current collector 21, the negative electrode current collector 21 includes a first metal substrate 22 and a coating layer 23 disposed on the first metal substrate 22 and including a second metal, the Mohs hardness of the second metal being higher than the Mohs hardness of the first metal.

[0019] [Negative electrode: negative electrode current collector] 1, the negative electrode 20 includes a negative electrode current collector 21. The negative electrode current collector 21 includes a first metal substrate 22 and a coating layer 23 including a second metal disposed on the first metal substrate 22. The second metal has a higher Mohs hardness than the first metal. That is, since the coating layer including the second metal is harder than the substrate including the first metal, deterioration of the first metal substrate can be prevented.

[0020] The first metal substrate 22 preferably contains the first metal as a main component or is made of the first metal. The content of the first metal contained in the first metal substrate 22 may be, for example, 90% by weight or more, 95% by weight or more, 99% by weight or more, or 99.9% by weight or more with respect to the total weight of the first metal substrate 22. The first metal substrate 22 may be made of, for example, a material that does not react with lithium, i.e., does not form an alloy and / or compound with lithium. The Mohs hardness of the material constituting the first metal substrate 22 is preferably 5.5 or less. For example, the Mohs hardness of the first metal is preferably 6.0 or less, 5.5 or less, 5.0 or less, 4.5 or less, 4.0 or less, 3.5 or less, or 3.0 or less. For example, the Mohs hardness of the first metal is preferably 2.0 or more. The Mohs hardness of the first metal may be, for example, 2.0 to 6.0, or 2.0 to 5.5.

[0021] The first metal may be, for example, copper (Cu), nickel (Ni), stainless steel (SUS), iron (Fe), cobalt (Co), etc., but is not necessarily limited thereto, and may be any metal used as a current collector in the art, preferably having a Mohs hardness of 5.5 or less. The first metal substrate 22 may be, for example, one of the above-mentioned metals, or may be an alloy of two or more metals. The first metal substrate 22 may be, for example, in the form of a sheet or foil.

[0022] The coating layer 23 includes a second metal. The coating layer 23 preferably includes the second metal as a main component or is made of the second metal. The content of the second metal in the coating layer 23 may be, for example, 90% by weight or more, 95% by weight or more, 99% by weight or more, or 99.9% by weight or more with respect to the total weight of the coating layer 23. The coating layer 23 may be made of a material that does not react with lithium, i.e., does not form an alloy and / or compound with lithium. The Mohs hardness of the material that constitutes the coating layer 23 is preferably, for example, 6.0 or more. For example, the Mohs hardness of the second metal is 6.0 or more, 6.5 or more, 7.0 or more, 7.5 or more, 8.0 or more, 8.5 or more, or 9.0 or more. For example, the Mohs hardness of the second metal is preferably 12 or less. The Mohs hardness of the second metal may be, for example, 6.0 to 12, 6.5 to 12, 7.0 to 12, 7.5 to 12, 8.0 to 12, 8.5 to 12, or 9.0 to 12. For example, the Mohs hardness of the second metal may be 12 or less. The Mohs hardness of the second metal may be, for example, 6.0 to 10, 6.5 to 10, 7.0 to 10, 7.5 to 10, 8.0 to 10, 8.5 to 10, or 9.0 to 10. If the Mohs hardness of the second metal is excessively low, it may be difficult to suppress the deterioration of the negative electrode current collector. If the Mohs hardness of the second metal is excessively high, the processability may be reduced.

[0023] The second metal is preferably at least one selected from the group consisting of titanium (Ti), manganese (Mn), niobium (Nb), tantalum (Ta), iridium (Ir), vanadium (V), rhenium (Re), osmium (Os), tungsten (W), chromium (Cr), boron (B), ruthenium (Ru) and rhodium (Rh). The coating layer 23 may be made of one of the above-mentioned metals, or may be made of an alloy of two or more metals.

[0024] The difference in Mohs hardness between the first metal contained in the first metal substrate 22 and the second metal contained in the coating layer 23 may be, for example, 2 or more, 2.5 or more, 3 or more, 3.5 or more, or 4 or more. When the first metal and the second metal have such a difference in Mohs hardness, deterioration of the negative electrode current collector 21 can be more effectively suppressed.

[0025] The coating layer 23 may have a single-layer structure or a multi-layer structure of two or more layers. The coating layer 23 may have, for example, a two-layer structure including a first coating layer and a second coating layer. The coating layer 23 may have, for example, a three-layer structure including a first coating layer, a second coating layer, and a third coating layer.

[0026] The thickness of the coating layer 23 is, for example, 1 μm or less, 900 nm or less, 800 nm or less, 700 nm or less, 600 nm or less, 500 nm or less, 400 nm or less, 300 nm or less, 200 nm or less, or 150 nm or less. The thickness of the coating layer 23 is, for example, preferably 10 nm to 1 μm, 20 nm to 900 nm, 30 nm to 800 nm, 40 nm to 700 nm, 50 nm to 600 nm, 50 nm to 500 nm, 50 nm to 500 nm, 50 nm to 300 nm, 50 nm to 200 nm, or 50 nm to 150 nm. If the thickness of the coating layer 23 is too thin, it is difficult to suppress the uneven growth of the lithium-containing metal layer. The thicker the coating layer 23, the more the cycle characteristics of the all-solid-state secondary battery can be improved, but if the coating layer 23 is excessively thick, the energy density of the all-solid-state secondary battery decreases, and it may become difficult to form the coating layer 23. The coating layer 23 is also disposed on the first metal base material 22 by, for example, a vacuum deposition method, a sputtering method, a plating method, or the like, but is not necessarily limited to such methods, and any method that can form the coating layer 23 in the relevant technical field is possible.

[0027] The coating layer 23 may be, for example, inert to the solid electrolyte. The coating layer 23 may be, for example, inert to the sulfide-based solid electrolyte. Since the coating layer 23 is inert to the sulfide-based solid electrolyte, the first metal substrate 22, which is reactive to the sulfide-based solid electrolyte, can be protected from the sulfide-based solid electrolyte. That is, the coating layer 23 can act as a protective layer for the first metal substrate 22. For example, in an all-solid-state secondary battery including an anode 20 including copper (Cu) as the first metal substrate 22 and a sulfide-based solid electrolyte as the solid electrolyte, the protective layer 23 inert to the sulfide-based solid electrolyte is disposed on the first metal substrate 22, thereby effectively preventing deterioration such as corrosion of the copper (Cu) substrate, which is the first metal substrate 22, caused by the sulfide-based solid electrolyte.

[0028] 2, the coating layer 23 is further disposed on a third surface A3, i.e., a side surface, between a first surface A1 of the first metal substrate 22 facing the coating layer 23 and a second surface A2 facing the first surface A1. By disposing the coating layer 23 simultaneously on the first surface A1 and the third surface A3 of the first metal substrate 22, deterioration of the first metal substrate 22 can be more effectively prevented. The coating layer 23 is also disposed on the third surface A3 of the first metal substrate 22, i.e., the entire side surface.

[0029] The thickness of the negative electrode current collector 21 including the first metal substrate 22 and the coating layer 23 may be, for example, 5 μm to 50 μm, 10 μm to 50 μm, 10 μm to 40 μm, or 10 μm to 30 μm, but is not necessarily limited to such ranges and is selected depending on the required characteristics of the all-solid-state secondary battery.

[0030] [Negative electrode: negative electrode active material] 1 to 4 and 6, the negative electrodes 20, 20a, 20b include first negative electrode active material layers 24, 24a, 24b disposed on negative electrode current collectors 21, 21a, 21b. The first negative electrode active material layer 24 includes, for example, a negative electrode active material and a binder.

[0031] The negative electrode active material contained in the first negative electrode active material layer 24 has, for example, a particulate form. The average particle size of the negative electrode active material having a particulate form may be, for example, 4 μm or less, 3 μm or less, 2 μm or less, 1 μm or less, 900 nm or less, 800 nm or less, 700 nm or less, 600 nm or less, 500 nm or less, 400 nm or less, 300 nm or less, 200 nm or less, or 100 nm or less. The average particle size of the negative electrode active material having a particle form may be, for example, 10 nm to 4 μm, 10 nm to 3 μm, 10 nm to 2 μm, 10 nm to 1 μm, 10 nm to 900 nm, 10 nm to 800 nm or less, 10 nm to 700 nm, 10 nm to 600 nm, 10 nm to 500 nm, 10 nm to 400 nm, 10 nm to 300 nm, 10 nm to 200 nm, 10 nm to 100 nm, or 20 nm to 80 nm. When the negative electrode active material has an average particle size in such a range, it can further facilitate reversible absorbing and / or desorbing of lithium during charging and discharging. The average particle size of the negative electrode active material is, for example, a median diameter (D50) measured using a laser type particle size distribution meter.

[0032] The negative electrode active material contained in the first negative electrode active material layers 24, 24a, 24b may include, for example, one or more selected from the group consisting of a carbon-based negative electrode active material, and a metallic negative electrode active material or a semi-metallic negative electrode active material.

[0033] The carbon-based negative electrode active material may be, in particular, amorphous carbon. The amorphous carbon may be, for example, carbon black (CB), acetylene black (AB), furnace black (FB), Ketjen black (KB), graphene, etc., but is not necessarily limited thereto, and may be any material that is classified as amorphous carbon in the relevant technical field. The amorphous carbon is carbon that has no crystallinity or has very low crystallinity, and is classified as crystalline carbon or graphite-based carbon.

[0034] The metal negative electrode active material or the semi-metal negative electrode active material may include one or more selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn) and zinc (Zn), but is not necessarily limited thereto, and any metal negative electrode active material or semi-metal negative electrode active material that forms an alloy or compound with lithium in the art is possible. For example, nickel (Ni) does not form an alloy with lithium, so it is not a metal negative electrode active material in this specification.

[0035] The first negative electrode active material layer 24, 24a, 24b may include one of these negative electrode active materials, or may include a mixture of a plurality of different negative electrode active materials. For example, the first negative electrode active material layer 24, 24a, 24b may include only amorphous carbon, or may include one or more selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn). Alternatively, the first negative electrode active material layer 24, 24a, 24b may include a mixture of amorphous carbon and one or more selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn). The mixing ratio of the mixture of the amorphous carbon and gold or the like may be, for example, 10:1 to 1:2, 10:1 to 1:1, 7:1 to 1:1, 5:1 to 1:1, or 4:1 to 2:1 by weight, but is not necessarily limited to such ranges and is selected depending on the required characteristics of the all-solid-state secondary battery 1. When the negative electrode active material has such a composition, the cycle characteristics of the all-solid-state secondary battery 1 can be further improved.

[0036] The negative electrode active material included in the first negative electrode active material layer 24, 24a, 24b may include, for example, a mixture of first particles made of amorphous carbon and second particles made of a metal or a semi-metal. The metal or semi-metal may include, for example, gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn). The semi-metal may also be a semiconductor. The content of the second particles may be, for example, 8 to 60 wt%, 10 to 50 wt%, 15 to 40 wt%, or 20 to 30 wt%, based on the total weight of the mixture. When the second particles have a content in such a range, for example, the cycle characteristics of the all-solid-state secondary battery 1 can be further improved.

[0037] [Negative electrode: binder] The binder contained in the first negative electrode active material layer 24, 24a, 24b may be, for example, styrene-butadiene rubber (SBR), polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), polyethylene, vinylidene fluoride / hexafluoropropylene copolymer, polyacrylonitrile, polymethyl methacrylate, etc., but is not necessarily limited thereto, and any binder used as a binder in the relevant technical field may be used. The binder may be composed of a single binder or a plurality of different binders.

[0038] The first negative electrode active material layers 24, 24a, 24b contain a binder, and thus the first negative electrode active material layers 24, 24a, 24b are stabilized on the negative electrode current collectors 21, 21a, 21b. In addition, cracks in the first negative electrode active material layers 24, 24a, 24b are suppressed despite volume changes and / or relative position changes of the first negative electrode active material layers 24, 24a, 24b during charge / discharge processes. For example, when the first negative electrode active material layers 24, 24a, 24b do not contain a binder, the first negative electrode active material layers 24, 24a, 24b can be easily separated from the negative electrode current collectors 21, 21a, 21b. When the first negative electrode active material layer 24, 24a, 24b is detached from the negative electrode current collector 21, 21a, 21b, the negative electrode current collector 21, 21a, 21b comes into direct contact with the solid electrolyte layer 30, 30a, 30b at the exposed portion of the negative electrode current collector 21, 21a, 21b, increasing the possibility of short circuit. The first negative electrode active material layer 24, 24a, 24b is produced, for example, by applying a slurry in which the material constituting the first negative electrode active material layer 24, 24a, 24b is dispersed onto the negative electrode current collector 21, 21a, 21b and drying the slurry. By including a binder in the first negative electrode active material layer 24, 24a, 24b, the negative electrode active material can be stably dispersed in the slurry. For example, when the slurry is applied onto the negative electrode current collectors 21, 21a, 21b by a screen printing method, clogging of the screen (for example, clogging due to aggregates of the negative electrode active material) can be suppressed.

[0039] The content of the binder contained in the first negative electrode active material layers 24, 24a, and 24b may be, for example, 1 to 20 wt %, 2 to 15 wt %, or 3 to 10 wt % relative to the total weight of the first negative electrode active material layers 24, 24a, and 24b, but is not necessarily limited to such ranges and is selected depending on the characteristics of the all-solid-state secondary battery.

[0040] [Negative electrode: Other additives] The first negative electrode active material layers 24, 24a, 24b may further include additives used in the conventional all-solid-state secondary battery 1, such as a filler, a coating agent, a dispersant, an ion-conductive auxiliary, etc., within the range in which the physical properties of the all-solid-state secondary battery 1 are maintained or improved.

[0041] As the filler, coating agent, dispersant, and ion-conductive auxiliary contained in the negative electrode active material layers 24, 24a, and 24b, known materials generally used for the negative electrodes of all-solid-state secondary batteries can be used.

[0042] [Negative electrode: first negative electrode active material layer] The thickness of the first negative electrode active material layer 24, 24a, 24b may be, for example, 1 μm to 20 μm, 1 μm to 15 μm, 2 μm to 10 μm, or 3 μm to 7 μm. The thickness of the first negative electrode active material layer 24, 24a, 24b may be, for example, 50% or less, 40% or less, 30% or less, 20% or less, 10% or less, or 5% or less of the thickness of the positive electrode active material layer. If the thickness of the first negative electrode active material layer 24, 24a, 24b is excessively thin, lithium dendrites formed between the first negative electrode active material layer 24, 24a, 24b and the negative electrode current collector 21, 21a, 21b collapse the first negative electrode active material layer 24, 24a, 24b, making it difficult to improve the cycle characteristics of the all-solid-state secondary battery. If the thickness of the first negative electrode active material layers 24, 24a, 24b is excessively large, the energy density of the all-solid-state secondary battery in which the negative electrode 20 is used decreases, and the internal resistance of the all-solid-state secondary battery due to the first negative electrode active material layers 24, 24a, 24b increases, making it difficult to improve the cycle characteristics of the all-solid-state secondary battery.

[0043] If the thickness of the first negative electrode active material layer 24, 24a, 24b is reduced, the charge capacity of the first negative electrode active material layer 24, 24a, 24b is also reduced. The charge capacity of the first negative electrode active material layer 24, 24a, 24b may be, for example, 50% or less, 40% or less, 30% or less, 20% or less, 10% or less, 5% or less, or 2% or less, compared to the charge capacity of the positive electrode active material layer. The charge capacity of the first negative electrode active material layer 24, 24a, 24b may be, for example, 0.1% to 50%, 0.1% to 40%, 0.1% to 30%, 0.1% to 20%, 0.1% to 10%, 0.1% to 5%, or 0.1% to 2% compared to the charge capacity of the positive electrode active material layer. If the charge capacity of the first negative electrode active material layer 24, 24a, 24b is excessively small, the thickness of the first negative electrode active material layer 24, 24a, 24b becomes very thin, and thus lithium dendrites formed between the first negative electrode active material layer 24, 24a, 24b and the negative electrode current collector 21, 21a, 21b during repeated charge and discharge processes collapse the first negative electrode active material layer 24, 24a, 24b, making it difficult to improve the cycle characteristics of the all-solid-state secondary battery. If the charge capacity of the first negative electrode active material layer 24, 24a, 24b is excessively large, the energy density of the all-solid-state secondary battery decreases, and the internal resistance of the all-solid-state secondary battery due to the first negative electrode active material layer 24, 24a, 24b increases, making it difficult to improve the cycle characteristics of the all-solid-state secondary battery.

[0044] The charge capacity of the positive electrode active material layer is obtained by multiplying the charge capacity density (mAh / g) of the positive electrode active material by the mass of the positive electrode active material in the positive electrode active material layer. When multiple types of positive electrode active materials are used, the charge capacity density mass value is calculated for each positive electrode active material, and the sum of these values ​​is the charge capacity of the positive electrode active material layer. The charge capacity of the first negative electrode active material layer 24, 24a, 24b is also calculated by the same method. That is, the charge capacity of the first negative electrode active material layer 24, 24a, 24b is obtained by multiplying the charge capacity density (mAh / g) of the negative electrode active material by the mass of the negative electrode active material in the first negative electrode active material layer 24, 24a, 24b. When multiple types of negative electrode active materials are used, the charge capacity density mass value is calculated for each negative electrode active material, and the sum of these values ​​is the capacity of the first negative electrode active material layer 24, 24a, 24b. Here, the charge capacity density of the positive electrode active material and the negative electrode active material is a capacity estimated using an all-solid-state half-cell using lithium metal as a counter electrode. The charge capacity of the positive electrode active material layer and the first negative electrode active material layer 24, 24a, 24b is directly measured by measuring the charge capacity using the all-solid-state half-cell. The charge capacity density is obtained by dividing the measured charge capacity by the mass of each active material. Alternatively, the charge capacity of the positive electrode active material layer and the first negative electrode active material layer 24, 24a, 24b may be an initial charge capacity measured during the first cycle charge.

[0045] [All-solid-state secondary battery] The all-solid-state secondary battery according to one embodiment includes a positive electrode, the above-mentioned negative electrode, and a solid electrolyte layer disposed between the positive electrode and the negative electrode, the solid electrolyte layer including a sulfide-based solid electrolyte. The first metal substrate of the negative electrode current collector included in the negative electrode is covered with a coating layer including a second metal having high hardness, so that the sulfide-based solid electrolyte can suppress deterioration of the first metal substrate, particularly the Cu substrate. In addition, during the charge / discharge process, the uniformity of the lithium-containing metal layer deposited on the negative electrode current collector is improved, so that microcracks in the solid electrolyte layer due to the non-uniform lithium-containing metal layer can be suppressed. Therefore, short-circuiting of the solid electrolyte layer is suppressed during charge / discharge of the all-solid-state secondary battery. As a result, the cycle characteristics of the all-solid-state secondary battery can be improved.

[0046] 3, 4, and 6, the all-solid-state secondary battery 1 includes a positive electrode 10, the above-mentioned negative electrode 20, and a solid electrolyte layer 40 disposed between the positive electrode 10 and the negative electrodes 20, 20a, and 20b, and the solid electrolyte layer 40 includes a sulfide-based solid electrolyte.

[0047] According to FIG. 3, the all-solid-state secondary battery 1 can have a single-cell structure including, for example, a positive electrode active material layer 12 arranged on one surface of a positive electrode current collector 11, a solid electrolyte layer 30, and a negative electrode 20.

[0048] 4, the all-solid-state secondary battery 1 may have a bi-cell structure including, for example, positive electrode active material layers 12a, 12b, solid electrolyte layers 30a, 30b, and negative electrodes 20a, 20b, which are respectively disposed on both sides of a positive electrode current collector 11. In the all-solid-state secondary battery 1 having a bi-cell structure, pressure is applied symmetrically in both directions of the all-solid-state secondary battery 1 during the battery manufacturing process, so that cracks that may occur due to pressure being applied in one direction during the manufacturing process of the all-solid-state secondary battery 1 can be more effectively suppressed.

[0049] [Positive electrode] [Positive electrode: Positive electrode active material] 3 to 6, the positive electrode 10 includes a positive electrode current collector 11 and positive electrode active material layers 12, 12a, and 12b disposed on the positive electrode current collector. The positive electrode active material layers 12, 12a, and 12b include a positive electrode active material.

[0050] The positive electrode active material can reversibly absorb and release lithium ions. The positive electrode active material may be, for example, lithium transition metal oxides such as lithium cobalt oxide (LCO), lithium nickel oxide, lithium nickel cobalt oxide, lithium nickel cobalt aluminum oxide (NCA), lithium nickel cobalt manganese oxide (NCM), lithium manganese oxide, and lithium iron phosphate oxide; nickel sulfide; copper sulfide; lithium sulfide; iron oxide or vanadium oxide; but is not necessarily limited thereto, and any material that is used as a positive electrode active material in the technical field is possible. The positive electrode active material may be each alone or may be a mixture of two or more kinds.

[0051] The positive electrode active material is, for example, Li a A 1-b B' b D2 (in the chemical formula, 0.90≦a≦1 and 0≦b≦0.5); Li a E 1-b B' b O 2-c D c (In the chemical formula, 0.90≦a≦1, 0≦b≦0.5, and 0≦c≦0.05); LiE 2-b B' b O 4-c D c (In the chemical formula, 0≦b≦0.5, 0≦c≦0.05); Li a Ni 1-b-c Co b B' c D α (In the chemical formula, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α≦2);Li a Ni 1-b-c Co b B' c O 2-α F' α (In the chemical formula, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2);Li a Ni 1-b-c Co b B' c O 2-αF'2 (in the chemical formula, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, 0<α<2); Li a Ni 1-b-c Mn b B' c D α (In the chemical formula, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α≦2);Li a Ni 1-b-c Mn b B' c O 2-α F' α (In the chemical formula, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2);Li a Ni 1-b-c Mn b B' c O 2-α F'2 (in the chemical formula, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, 0<α<2); Li a Ni b E c G d O2 (wherein the chemical formula is 0.90≦a≦1, 0≦b≦0.9, 0≦c≦0.5, and 0.001≦d≦0.1); Li a Ni b Co c Mn d GeO2 (in the chemical formula, 0.90≦a≦1, 0≦b≦0.9, 0≦c≦0.5, 0≦d≦0.5, 0.001≦e≦0.1); Li a NiG b O2 (in the chemical formula, 0.90≦a≦1, 0.001≦b≦0.1); Li a CoG b O2 (in the chemical formula, 0.90≦a≦1, 0.001≦b≦0.1); Li a MnG b O2 (in the chemical formula, 0.90≦a≦1, 0.001≦b≦0.1); Li a Mn2G b O4 (in the chemical formula, 0.90≦a≦1, 0.001≦b≦0.1); QO2; QS2; LiQS2; V2O5; LiV2O5; LiI'O2; LiNiVO4; Li 3-f J2(PO4)3(0≦f≦2);Li3-f The compound may be a compound represented by any one of the chemical formulas Fe2(PO4)3(0≦f≦2);LiFePO4. In such a compound, A is Ni, Co, Mn, or a combination thereof, B' is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element, or a combination thereof, D is O, F, S, P, or a combination thereof, E is Co, Mn, or a combination thereof, F' is F, S, P, or a combination thereof, G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, or a combination thereof, Q is Ti, Mo, Mn, or a combination thereof, I' is Cr, V, Fe, Sc, Y, or a combination thereof, and J is V, Cr, Mn, Co, Ni, Cu, or a combination thereof. A compound having a coating layer added to the surface of such a compound can also be used, and a mixture of the above-mentioned compound and a compound having a coating layer added can also be used. The coating layer added to the surface of such a compound may include, for example, a coating element compound such as an oxide of a coating element, a hydroxide of a coating element, an oxyhydroxide of a coating element, an oxycarbonate of a coating element, or a hydroxycarbonate of a coating element. The compound forming such a coating layer may be amorphous or crystalline. The coating element contained in the coating layer may be, for example, Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or a mixture thereof. The method of forming the coating layer is selected within a range that does not adversely affect the physical properties of the positive electrode active material. The coating method is, for example, a spray coating method, a dipping method, etc. Specific coating methods are well understood by those skilled in the art, so detailed explanations will be omitted.

[0052] The positive electrode active material may include, for example, a lithium salt of a transition metal oxide having a layered rock salt type structure among the aforementioned lithium transition metal oxides. The "layered rock salt type structure" is, for example, a structure in which oxygen atom layers and metal atom layers are regularly arranged alternately in the <111> direction of a cubic rock salt type structure, whereby each atomic layer forms a two-dimensional plane. The "cubic rock salt type structure" refers to a sodium chloride type (NaCl type) structure which is a kind of crystal structure. Specifically, it shows a structure in which face-centered cubic lattices (fcc) formed by cations and anions respectively are arranged with a shift of about 1 / 2 of the ridge of the unit lattice from each other. Such a lithium transition metal oxide having a layered rock salt type structure is, for example, LiNi x Co y Al z O2 (NCA; 0 < x < 1, 0 < y < 1, 0 < z < 1, x + y + z = 1), LiNi x Co y Mn z O2 (NCM; 0 < x < 1, 0 < y < 1, 0 < z < 1, x + y + z = 1), LiNi x Co y Al v Mn w O2 (NCAM; 0 < x < 1, 0 < y < 1, 0 < v < 1, 0 < w < 1, x + y + v + w = 1), LiNi a Co b Al c O2 (0.5 ≦ a < 1, 0 < b < 0.5, 0 < c < 0.5, a + b + c = 1) or LiNi a Co b Mn c O2 (0.5 ≦ a < 1, 0 < b < 0.5, 0 < c < 0.5, a + b + c = 1), which may be a ternary lithium transition metal oxide. When the positive electrode active material includes a ternary lithium transition metal oxide having a layered rock salt type structure, the energy density and thermal stability of the all-solid-state secondary battery 1 can be further improved.

[0053] The positive electrode active material may be covered with a coating layer as described above. The coating layer may be any known coating layer for a positive electrode active material of an all-solid-state secondary battery. The coating layer may be, for example, Li2O-ZrO2 (LZO).

[0054] The positive electrode active material is, for example, LiNi x Co y Al z O2(NCA), LiNi x Co y Mn z O2(NCM), or LiNi x Co y Al v Mn w It may be a ternary lithium transition metal oxide such as O2 (NCAM), and when it contains nickel (Ni), it is possible to increase the capacity density of the all-solid-state secondary battery 1 and reduce metal elution from the positive electrode active material in a charged state. As a result, it is possible to improve the cycle characteristics of the all-solid-state secondary battery 1 in a charged state.

[0055] The shape of the positive electrode active material may be, for example, a particulate shape such as a perfect sphere or an oval sphere. The particle size of the positive electrode active material is not particularly limited, and is within the range applicable to the positive electrode active material of a conventional all-solid-state secondary battery. The content of the positive electrode active material in the positive electrode layer 10 is also not particularly limited, and is within the range applicable to the positive electrode layer of a conventional all-solid-state secondary battery.

[0056] The content of the positive electrode active material contained in the positive electrode active material layers 12, 12a, 12b may be, for example, 80 to 99 wt %, 80 to 95 wt %, or 80 to 90 wt % of the total weight of the positive electrode active material layers 12, 12a, 12b.

[0057] [Positive electrode: solid electrolyte] The positive electrode active material layers 12, 12a, and 12b may further include a solid electrolyte in addition to the positive electrode active material. The solid electrolyte included in the positive electrode 10 may be the same as or different from the solid electrolyte included in the solid electrolyte layers 30, 30a, and 30b. For details about the solid electrolyte included in the positive electrode 10, please refer to the section on the solid electrolyte layers 30, 30a, and 30b.

[0058] The solid electrolyte used in the positive electrode active material layers 12, 12a, and 12b has a smaller D50 average particle size than the solid electrolyte used in the solid electrolyte layers 30, 30a, and 30b. For example, the D50 average particle size of the solid electrolyte used in the positive electrode active material layers 12, 12a, and 12b may be 90% or less, 80% or less, 70% or less, 60% or less, 50% or less, 40% or less, 30% or less, or 20% or less of the D50 average particle size of the solid electrolyte used in the solid electrolyte layers 30, 30a, and 30b. The D50 average particle size of the solid electrolyte used in the positive electrode active material layers 12, 12a, and 12b may be, for example, 0.1 μm to 2 μm, 0.2 μm to 1.5 μm, or 0.3 μm to 1.0 μm.

[0059] The content of the solid electrolyte contained in the positive electrode active material layers 12, 12a, 12b may be, for example, 1 to 15 wt %, 5 to 15 wt %, or 8.0 to 12.0 wt % of the total weight of the positive electrode active material layers 12, 12a, 12b.

[0060] [Positive electrode: binder] The positive electrode active material layers 12, 12a, and 12b may contain a binder, which may be, for example, styrene-butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, or the like, but is not necessarily limited thereto, and any material that can be used as a binder in the art is possible.

[0061] The content of the binder in the positive electrode active material layers 12, 12a, 12b may be, for example, 0.1 to 5 wt %, 0.5 to 3 wt %, or 1.0 to 2.0 wt % of the total weight of the positive electrode active material layers 12, 12a, 12b.

[0062] [Positive electrode: Conductive material] The positive electrode active material layers 12, 12a, and 12b may contain a conductive agent. The conductive agent may be, for example, a carbon-based conductive agent or a metal-based conductive agent. The conductive agent may be, for example, graphite, carbon black (CB), acetylene black (AB), ketjen black (KB), carbon fiber, carbon tube, metal powder, etc., but is not necessarily limited thereto, and any conductive agent that can be used as a conductive agent in the relevant technical field is possible.

[0063] The content of the conductive agent in the positive electrode active material layers 12, 12a, 12b may be, for example, 0.1 to 10 wt %, 0.5 to 5 wt %, or 1.0 to 4.0 wt % of the total weight of the positive electrode active material layers 12, 12a, 12b.

[0064] [Positive electrode: Other additives] The positive electrode active material layers 12, 12a, 12b may further contain additives such as a filler, a coating agent, a dispersant, and an ion-conductive auxiliary in addition to the above-mentioned positive electrode active material, solid electrolyte, binder, and conductive agent.

[0065] As the filler, coating agent, dispersant, and ion-conductive auxiliary contained in the positive electrode active material layers 12, 12a, and 12b, known materials generally used for the positive electrodes of all-solid-state secondary batteries can be used.

[0066] [Positive electrode: Positive electrode current collector] The positive electrode current collector 11 may be, for example, a plate or foil made of indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof. The positive electrode current collector 11 may not be provided.

[0067] The positive electrode current collector 11 may further include a carbon layer disposed on one or both surfaces of the metal substrate. By further disposing the carbon layer on the metal substrate, the metal of the metal substrate is prevented from being corroded by the solid electrolyte contained in the positive electrode layer, and the interface resistance between the positive electrode active material layer 12, 12a, 12b and the positive electrode current collector 11 can be reduced. The thickness of the carbon layer may be, for example, 0.1 μm to 5 μm, 0.5 μm to 5 μm, 1 μm to 5 μm, 1 μm to 4 μm, or 1 μm to 3 μm. If the thickness of the carbon layer is too thin, it is difficult to completely block the contact between the metal substrate and the solid electrolyte. If the thickness of the carbon layer is too thick, the energy density of the all-solid-state secondary battery may be reduced. The carbon layer may include amorphous carbon, crystalline carbon, etc.

[0068] The thickness of the positive electrode current collector 11 including the metal substrate and, optionally, the carbon layer may be, for example, 10 μm to 50 μm, 10 μm to 40 μm, or 10 μm to 30 μm, but is not necessarily limited to such ranges and is selected depending on the required characteristics of the all-solid-state secondary battery.

[0069] [Positive electrode: inactive material] 3 to 6, the positive electrode 10 may further include positive electrode current collectors 11, 11a, and 11b, positive electrode active material layers 12, 12a, and 12b disposed on the positive electrode current collectors, and an inactive member 40 disposed on one surface of the positive electrode active material layers.

[0070] The inactive member 40 is a member that does not contain a material having electrochemical activity, for example, an electrode active material. The electrode active material is a material that absorbs / desorbs lithium. The inactive member is a material other than the electrode active material, and is a member made of a material used in the art.

[0071] The inactive member 40 can surround the side surfaces of the positive electrode active material layers 12, 12a, 12b and contact the solid electrolyte layers 30, 30a, 30b. By surrounding the side surfaces of the positive electrode active material layers 12, 12a, 12b with the inactive member and contacting the solid electrolyte layers 30, 30a, 30b, cracks in the solid electrolyte layers 30, 30a, 30b that are not in contact with the positive electrode active material layers 12, 12a, 12b due to a pressure difference during the pressing process can be effectively suppressed.

[0072] The inactive member 40 is extended to the end portions of the solid electrolyte layers 30, 30a, and 30b. By extending the inactive member 40 to the end portions of the solid electrolyte layers 30, 30a, and 30b, it is possible to suppress cracks occurring at the end portions of the solid electrolyte layers 30, 30a, and 30b. The end portions of the solid electrolyte layers 30, 30a, and 30b are the outermost portions that contact the side surfaces of the solid electrolyte layers 30, 30a, and 30b. That is, the inactive member 40 is extended to the outermost portions that contact the side surfaces of the solid electrolyte layers 30, 30a, and 30b.

[0073] The area (e.g., surface area) S1 of the positive electrode active material layers 12, 12a, 12b is narrower than the area (e.g., surface area) S2 of the solid electrolyte layers 30, 30a, 30b in contact with the positive electrode active material layers 12, 12a, 12b, and the inactive member 40 is disposed surrounding the side surfaces of the positive electrode active material layers 12, 12a, 12b, so that the area difference (area error) between the positive electrode active material layers 12, 12a, 12b and the solid electrolyte layers 30, 30a, 30b can be corrected. The area (e.g., surface area) S3 of the inactive member 40 corrects the difference between the area (e.g., surface area) S1 of the positive electrode active material layers 12, 12a, 12b and the area (e.g., surface area) S2 of the solid electrolyte layers 30, 30a, 30b, so that cracks in the solid electrolyte layers 30, 30a, 30b caused by the pressure difference during the pressurization process can be effectively suppressed. For example, the area (e.g., surface area) S1 of the positive electrode active material layers 12, 12a, 12b may be less than 100%, 99% or less, 98% or less, 97% or less, 96% or less, 93% or less, or 85% or less of the area S2 of the solid electrolyte layers 30, 30a, 0b. For example, the area (e.g., surface area) S1 of the positive electrode active material layers 12, 12a, 12b may be 50% to less than 100%, 50% to 99%, 55% to 98%, 60% to 97%, 70% to 96%, 80% to 95%, or 85% to 95% of the area (e.g., surface area) S2 of the solid electrolyte layers 30, 30a, 30b. If the area S1 of the positive electrode active material layers 12, 12a, 12b is the same as or larger than the area (e.g., surface area) S2 of the solid electrolyte layers 30, 30a, 30b, the positive electrode active material layers 12, 12a, 12b will come into physical contact with the negative electrode active material layers 22, 22a, 22b, causing a short circuit, or the possibility of a short circuit occurring due to overcharging of lithium, etc. will increase.

[0074] The area (e.g., surface area) S3 of the inactive member 40 may be, for example, 50% or less, 40% or less, 30% or less, 20% or less, or 10% or less of the area S1 of the active material layers 12, 12a, and 12b. For example, the area (e.g., surface area) S3 of the inactive member 40 may be 1% to 50%, 5% to 40%, 5% to 30%, 5% to 20%, or 5% to 15% of the area S1 of the positive electrode active material layers 12, 12a, and 12b. The sum of the area (e.g., surface area) S3 of the inactive member 40 and the area (e.g., surface area) S1 of the positive electrode active material layers 12, 12a, and 12b may be the same as the area (e.g., surface area) S2 of the solid electrolyte layers 30, 30a, and 30b.

[0075] The inactive member 40 is disposed between the positive electrode current collector 11 and the solid electrolyte layers 30, 30a, 30b facing each other, or between the two solid electrolyte layers 30, 30a, 30b facing each other. The inactive member 40 can act as a filler that fills the space between the positive electrode current collector 11 and the solid electrolyte layers 30, 30a, 30b facing each other, or the space between the two solid electrolyte layers 30, 30a, 30b facing each other.

[0076] The area (e.g., surface area) S1 of the positive electrode active material layers 12, 12a, 12b is smaller than the area (e.g., surface area) S4 of the negative electrode current collectors 21, 21a, 21b. For example, the area (e.g., surface area) S1 of the positive electrode active material layers 12, 12a, 12b may be less than 100%, 99% or less, 98% or less, 97% or less, 96% or less, 93% or less, or 85% or less of the area (e.g., surface area) S4 of the negative electrode current collectors 21, 21a, 21b. For example, the area (e.g., surface area) S1 of the positive electrode active material layers 12, 12a, 12b may be 50% to less than 100%, 50% to 99%, 55% to 98%, 60% to 97%, 70% to 96%, 80% to 95%, or 85% to 95% of the area (e.g., surface area) S4 of the negative electrode current collectors 21, 21a, 21b.

[0077] The area (e.g., surface area) S4 of the negative electrode current collectors 21, 21a, and 21b may be the same as the area (e.g., surface area) S5 and / or shape of the positive electrode current collector 11. For example, the area (e.g., surface area) S4 of the negative electrode current collectors 21, 21a, and 21b may be in the range of 100±1% or 100±0.5% of the area S5 of the positive electrode current collector 11. The area (e.g., surface area) S5 of the positive electrode current collector 11 may be the same as the area (e.g., surface area) S2 and / or shape of the solid electrolyte layers 30, 30a, and 30b. For example, the area (e.g., surface area) S5 of the positive electrode current collector 11 may be in the range of 100±1% or 100±0.5% of the area (e.g., surface area) S2 of the solid electrolyte layers 30, 30a, and 30b. As used herein, "same" area and / or shape includes all cases having "substantially the same" area and / or shape, except where the area and / or shape is intentionally made different.

[0078] The inactive member 40 may include one or more selected from the group consisting of a lithium ion insulator and a lithium ion conductor. The inactive member 40 may be an electronic insulator. That is, the inactive member 40 does not have to be an electronic conductor.

[0079] The inactive member 40 may be an organic material, an inorganic material, or an organic-inorganic composite material. The organic material may be, for example, a polymer. The inorganic material may be, for example, a ceramic such as a metal oxide. The organic-inorganic composite material may be a composite of a polymer and a metal oxide. The inactive member 40 may include, for example, one or more selected from the group consisting of an insulating polymer, an ion-conducting polymer, an insulating inorganic material, an oxide-based solid electrolyte, and a sulfide-based solid electrolyte. The inactive member 40 may be, for example, an olefin-based polymer such as polypropylene (PP) or polyethylene (PE).

[0080] The density of the inactive member 40 may be, for example, 10% to 200%, 10% to 150%, 10% to 140%, 10% to 130%, or 10% to 120% of the density of the positive electrode active material contained in the positive electrode active material layers 12, 12a, and 12b. The density of the inactive member 40 may be, for example, 90 to 110% of the density of the positive electrode active material contained in the positive electrode active material layers 12, 12a, and 12b. The density of the inactive member 40 may be, for example, substantially the same as the density of the positive electrode active material contained in the positive electrode active material layers 12, 12a, and 12b.

[0081] The inactive member 40 may be, for example, a gasket. By using a gasket as the inactive member 40, cracks in the solid electrolyte layers 30, 30a, and 30b caused by the pressure difference during the pressurization process can be effectively suppressed.

[0082] The thickness of the inactive member 40 may be the same as the thickness of the positive electrode active material layers 12, 12a, and 12b, or may be close to the thickness of the positive electrode active material layers 12, 12a, and 12b.

[0083] [Solid electrolyte layer] [Solid electrolyte layer: solid electrolyte] 3 to 6, the solid electrolyte layers 30, 30a, 30b are disposed between the positive electrode 10 and the negative electrodes 20, 20a, 20b and include a sulfide-based solid electrolyte.

[0084] Examples of the sulfide-based solid electrolyte include Li2S-P2S5, Li2S-P2S5-LiX (X is a halogen element), Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, and Li2S-P2S5-Z. m S n (m and n are positive numbers, and Z is one of Ge, Zn, or Ga), Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li pMO q (p and q are positive numbers, and M is one of P, Si, Ge, B, Al, Ga, and In), Li 7-x P.S. 6-x Cl x (0≦x≦2), Li 7-x P.S. 6-x Br x (0≦x≦2) and Li 7-x P.S. 6-x I x (0≦x≦2). The sulfide-based solid electrolyte may be prepared by processing starting materials such as Li2S and P2S5 by melt quenching or mechanical milling. After such processing, heat treatment may be performed. The solid electrolyte may be amorphous, crystalline, or a mixture of these. The solid electrolyte may be, for example, the above-mentioned sulfide-based solid electrolyte material containing at least sulfur (S), phosphorus (P), and lithium (Li) as constituent elements. For example, the solid electrolyte may be a material containing Li2S-P2S5. When a sulfide-based solid electrolyte material containing Li2S-P2S5 is used as the sulfide-based solid electrolyte material forming the solid electrolyte, the mixture molar ratio of Li2S and P2S5 is, for example, in the range of Li2S:P2S5=50:50 to 90:10.

[0085] The sulfide-based solid electrolyte may include, for example, an argyrodite-type solid electrolyte represented by the following chemical formula 1:

[0086] Li + 12-n-x A n+ X 2- 6-x Y - x (1)

[0087] In the chemical formula 1, A is P, As, Ge, Ga, Sb, Si, Sn, Al, In, Ti, V, Nb or Ta, X is S, Se or Te, Y is Cl, Br, I, F, CN, OCN, SCN or N3, and 1≦n≦5, 0≦x≦2. The sulfide-based solid electrolyte is, for example, Li 7-x P.S. 6-x Cl x (0≦x≦2), Li 7-x P.S. 6-x Br x (0≦x≦2) and Li 7-x P.S. 6-x I x (0≦x≦2). The sulfide-based solid electrolyte may be, for example, an argyrodite-type compound containing one or more selected from the group consisting of Li6PS5Cl, Li6PS5Br, and Li6PS5I.

[0088] The density of the argyrodite-type solid electrolyte may be, for example, 1.5 to 2.0 g / cc. By making the argyrodite-type solid electrolyte have a density of 1.5 g / cc or more, the internal resistance of the all-solid-state secondary battery can be reduced, and the penetration of the solid electrolyte layer by Li can be effectively suppressed.

[0089] The elastic modulus of the sulfide-based solid electrolyte, i.e., Young's modulus, may be, for example, 35 GPa or less, 30 GPa or less, 27 GPa or less, 25 GPa or less, or 23 GPa or less. The elastic modulus of the sulfide-based solid electrolyte, i.e., Young's modulus, may be, for example, 10 to 35 GPa, 10 to 30 GPa, 10 to 27 GPa, 10 to 25 GPa, or 10 to 23 GPa. When the sulfide-based solid electrolyte has an elastic modulus in such a range, the temperature and / or pressure required for sintering, etc., is reduced, making it easier to sinter the solid electrolyte.

[0090] The D50 average particle size of the solid electrolyte used in the solid electrolyte layers 30, 30a, 30b may be, for example, 1 μm to 10 μm, 1.5 μm to 7 μm, or 2 μm to 5 μm.

[0091] The content of the sulfide-based solid electrolyte contained in the solid electrolyte layers 30, 30a, 30b may be, for example, 97 to 100 wt %, 98 to 99.9 wt %, or 98.5 to 99.0 wt % of the total weight of the solid electrolyte layers 30, 30a, 30b.

[0092] [Solid electrolyte layer: binder] The solid electrolyte layers 30, 30a, and 30b may further include, for example, a binder. The binder included in the solid electrolyte layers 30, 30a, and 30b may be, for example, styrene-butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, and the like, but is not limited thereto, and any binder used as a binder in the relevant technical field is possible. The binder in the solid electrolyte layers 30, 30a, and 30b may be the same as or different from the binder included in the positive electrode active material layers 12, 12a, and 12b and the negative electrode active material layer 22.

[0093] The content of the binder contained in the solid electrolyte layers 30, 30a, 30b may be, for example, 0.1 to 3 wt %, 0.5 to 2 wt %, or 1.0 to 2.0 wt % of the total weight of the solid electrolyte layers 30, 30a, 30b.

[0094] [Negative electrode: second negative electrode active material layer (deposit layer or non-deposit layer)] 3, 4 and 6, the all-solid-state secondary battery 1 includes a positive electrode 10, the above-mentioned negative electrode 20, and solid electrolyte layers 30, 30a, and 30b disposed between the positive electrode 10 and the negative electrodes 20, 20a, and 20b.

[0095] The all-solid-state secondary battery 1 may further include a second negative electrode active material layer (not shown) disposed, for example, between the negative electrode current collector 21, 21a, 21b and the first negative electrode active material layer 24, 24a, 24b by charging. The all-solid-state secondary battery 1 may further include a second negative electrode active material layer (not shown) disposed, for example, between the solid electrolyte layer 30, 30a, 30b and the first negative electrode active material layer 24, 24a, 24b by charging. The second negative electrode active material layer may be a metal layer containing lithium or a lithium alloy. The metal layer may contain lithium or a lithium alloy. Thus, the second negative electrode active material layer is a metal layer containing lithium and acts, for example, as a lithium reservoir. The lithium alloy may be, for example, a Li·Al alloy, a Li·Sn alloy, a Li·In alloy, a Li·Ag alloy, a Li·Au alloy, a Li·Zn alloy, a Li·Ge alloy, a Li·Si alloy, etc., but is not limited thereto, and any alloy that is used as a lithium alloy in the art is possible. The second negative electrode active material layer may be made of one of these alloys, may be made of lithium, or may be made of multiple alloys.

[0096] The thickness of the second negative electrode active material layer is not particularly limited, and may be, for example, 1 μm to 1,000 μm, 1 μm to 500 μm, 1 μm to 200 μm, 1 μm to 150 μm, 1 μm to 100 μm, or 1 μm to 50 μm. If the thickness of the second negative electrode active material layer is too thin, it is difficult for the second negative electrode active material layer to function as a lithium storage. If the thickness of the second negative electrode active material layer is too thick, the mass and volume of the all-solid-state secondary battery 1 may increase, and the cycle characteristics may be deteriorated.

[0097] In the all-solid-state secondary battery 1, the second negative electrode active material layer is also deposited between the negative electrode current collectors 21, 21a, 21b and the first negative electrode active material layers 24, 24a, 24b by charging after the assembly of the all-solid-state secondary battery 1, for example. When the second negative electrode active material layer is deposited by charging after the assembly of the all-solid-state secondary battery 1, the energy density of the all-solid-state secondary battery 1 increases because the all-solid-state secondary battery 1 does not include the second negative electrode active material layer when assembled. For example, when the all-solid-state secondary battery 1 is charged, it is charged beyond the charge capacity of the first negative electrode active material layers 24, 24a, 24b. That is, the first negative electrode active material layers 24, 24a, 24b are overcharged. At the beginning of charging, lithium is absorbed into the first negative electrode active material layers 24, 24a, 24b. The negative electrode active material contained in the first negative electrode active material layer 24, 24a, 24b forms an alloy or a compound with the lithium ions transferred from the positive electrode layer 10. If the first negative electrode active material layer 24, 24a, 24b is charged beyond its capacity, for example, lithium is deposited on the back surface of the first negative electrode active material layer 24, 24a, 24b, that is, between the negative electrode current collector 21, 21a, 21b and the first negative electrode active material layer 24, 24a, 24b, and a metal layer corresponding to the second negative electrode active material layer is formed by the deposited lithium. The second negative electrode active material layer is a metal layer mainly composed of lithium (i.e., metallic lithium). Such a result is obtained, for example, by the negative electrode active material contained in the first negative electrode active material layer 24, 24a, 24b being composed of a material that forms an alloy or a compound with lithium. During discharge, lithium in the first negative electrode active material layer 24, 24a, 24b and the second negative electrode active material layer, i.e., the metal layer, is ionized and moves to the positive electrode layer 10. Therefore, in the all-solid-state secondary battery 1, lithium can be used as the negative electrode active material. In addition, since the first negative electrode active material layer 24, 24a, 24b covers the second negative electrode active material layer, it serves as a protective layer for the second negative electrode active material layer, i.e., the metal layer, and also serves to suppress the precipitation growth of lithium dendrites. Therefore, short-circuiting and capacity reduction of the all-solid-state secondary battery 1 are suppressed, and as a result, the cycle characteristics of the all-solid-state secondary battery 1 are improved.Furthermore, after the all-solid-state secondary battery 1 is assembled, when the second negative electrode active material layer is disposed by charging, the negative electrode current collectors 21, 21a, 21b, the first negative electrode active material layers 24, 24a, 24b, and the regions therebetween are Li-free regions that do not contain lithium (Li) in, for example, the initial state or post-discharge state of the all-solid-state secondary battery.

[0098] Alternatively, in the all-solid-state secondary battery 1, the second negative electrode active material layer is, for example, disposed between the negative electrode collector 21, 21a, 21b and the first negative electrode active material layer 24, 24a, 24b, or disposed between the solid electrolyte layer 30, 30a, 30b and the first negative electrode active material layer 24, 24a, 24b, before the assembly of the all-solid-state secondary battery 1. That is, the second negative electrode active material layer is disposed as a non-deposition layer between the negative electrode collector 21, 21a, 21b and the first negative electrode active material layer 24, 24a, 24b, or disposed between the solid electrolyte layer 30, 30a, 30b and the first negative electrode active material layer 24, 24a, 24b, before the assembly of the battery. By disposing the second negative electrode active material layer as a lithium reservoir before the assembly of the all-solid-state secondary battery 1, the charging and discharging of the all-solid-state secondary battery 1 is promoted, and lithium loss caused by side reactions and the like can be compensated for. The second negative electrode active material layer may be, for example, a lithium coating layer having a thickness in the above range, or may be a lithium metal foil. The lithium metal coating layer may be coated, for example, by a sputtering method. EXAMPLES

[0099] The present invention will be described in more detail with reference to the following examples and comparative examples, however, the examples are merely intended to illustrate the present invention and are not intended to limit the scope of the present invention.

[0100] <Example 1: Cu substrate / Ti coating layer 100 nm, first active material layer (metal-carbon layer) thickness 7 μm> (Negative electrode layer manufacturing) A Cu foil having a thickness of 10 μm was prepared as a first metal substrate. A Ti thin-film coating layer having a thickness of 100 nm was coated on the Cu foil by DC magnetron sputtering to prepare a negative electrode current collector. The Mohs hardness of Cu was 3.0, and the Mohs hardness of Ti was 6.0.

[0101] The DC magnetron sputtering conditions were: cathode power 125 W, sputtering pressure 1.1 Pa, and vacuum degree 4×10 -4 It was Pa.

[0102] As the negative electrode active material, carbon black (CB) with a primary particle size of about 30 nm and silver (Ag) particles with an average particle size of about 60 nm were prepared.

[0103] N-methylpyrrolidone (NMP) solvent and PVDF-HFP binder (Kureha #9300, Mw: 1,200,000 g / mol) were put into a container and stirred for 5 minutes at 1,300 rpm with a Thinky mixer to prepare an NMP solution in which the PVDF-HFP binder was dissolved. Silver (Ag) particles and carbon black (CB) were sequentially put into the NMP solution and stirred for 5 minutes at 1,300 rpm with a Thinky mixer to prepare a slurry. On a solids basis, the carbon black (CB) and silver (Ag) particles had a weight ratio of 3:1, and the PVDF-HFP binder content was 6 wt%.

[0104] The prepared slurry was applied onto the Ti coating layer of the negative electrode current collector using a bar coater, and dried in a convection oven at 80°C for 10 minutes to obtain a laminate. The obtained laminate was then vacuum-dried at 40°C for 10 hours to obtain a vacuum-dried laminate. The vacuum-dried laminate was roll-pressed at a pressure of 300 MPa for 10 ms to flatten the surface of the first negative electrode active material layer of the laminate. A negative electrode was produced by the above process. The thickness of the first negative electrode active material layer included in the negative electrode was about 7 μm.

[0105] (Positive electrode layer manufacturing) The positive electrode active material was LiNi coated with Li2O-ZrO2 (LZO). 0.8 Co 0.15 Mn 0.05 O2 (NCM) was prepared. The LZO-coated positive electrode active material was prepared by the method disclosed in Korean Patent Publication No. 10-2016-0064942. Argyrodite-type crystal Li6PS5Cl (D50=0.5μm, crystalline) was prepared as a solid electrolyte. Polytetrafluoroethylene (PTFE) binder (DuPont's Teflon (registered trademark) binder) was prepared as a binder. Carbon nanofiber (CNF) was prepared as a conductive agent. These materials were mixed with a paraxylene (p-xylene) solvent in a weight ratio of positive electrode active material: solid electrolyte: conductive agent: binder = 84: 11.5: 3: 1.5, and the mixture was formed into a sheet, and then vacuum dried at 40 ° C for 10 hours to prepare a positive electrode sheet. A polypropylene (PP) gasket was placed around the positive electrode sheet to surround the positive electrode sheet. The positive electrode sheet surrounded by the gasket was pressed onto one side of a positive electrode current collector made of 18 μm thick carbon-coated aluminum foil to produce a positive electrode. The positive electrode sheet and gasket were pressed together by roll pressing at a pressure of 450 MPa for 100 ms.

[0106] The thickness of the positive electrode active material layer and the gasket included in the positive electrode was about 100 μm.

[0107] The positive electrode active material layer was disposed at the center of the positive electrode current collector, and a gasket was disposed surrounding the positive electrode active material layer up to the end of the positive electrode current collector. The area of ​​the positive electrode active material layer was about 90% of the area of ​​the positive electrode current collector, and the gasket was disposed surrounding the positive electrode active material layer over the entire remaining 10% area of ​​the positive electrode current collector where the positive electrode active material layer was not disposed.

[0108] (Manufacturing of solid electrolyte layer) A mixture was prepared by adding 1.5 parts by weight of an acrylic binder to 98.5 parts by weight of the solid electrolyte (D50=3.0 μm, crystalline) of Li6PS5Cl, which is an argyrodite-type crystal. Octyl acetate was added to the prepared mixture while stirring to produce a slurry. The produced slurry was applied to a nonwoven fabric using a bar coater and dried in air at 80°C for 10 minutes to obtain a sheet-like solid material. The obtained solid material was vacuum-dried at 40°C for 10 hours. A solid electrolyte layer was produced by the above process.

[0109] (Manufacturing all-solid-state secondary batteries) A solid electrolyte layer was disposed on the positive electrode active material layer of the positive electrode, and a negative electrode was disposed on the solid electrolyte layer such that the first negative electrode active material layer was in contact with the solid electrolyte layer, to prepare a laminate.

[0110] The laminate was placed in a pouch and vacuum sealed, and then subjected to warm isostatic pressing (WIP) at 90° C. for 30 minutes under a pressure of 500 MPa to produce an all-solid-state secondary battery.

[0111] This pressure treatment sinters the solid electrolyte layer, improving the battery characteristics. The thickness of the sintered solid electrolyte layer was 60 μm.

[0112] <Example 2: Cu substrate / Ti coating layer 200 nm, first active material layer (metal-carbon layer) thickness 7 μm> A negative electrode and an all-solid-state secondary battery were manufactured in the same manner as in Example 1, except that the thickness of the Ti thin film coating layer disposed on the Cu foil was changed to 200 nm.

[0113] <Example 3: Cu substrate / Ti coating layer 300 nm, first active material layer (metal-carbon layer) thickness 7 μm> A negative electrode and an all-solid-state secondary battery were manufactured in the same manner as in Example 1, except that the thickness of the Ti thin film coating layer disposed on the Cu foil was changed to 300 nm.

[0114] <Example 4: Cu substrate / V coating layer 100 nm, first active material layer (metal-carbon layer) thickness 7 μm> A negative electrode and an all-solid-state secondary battery were manufactured in the same manner as in Example 1, except that the Ti thin film coating layer disposed on the Cu foil was replaced with a V thin film coating layer. The Mohs hardness of the Cu was 3.0, and the Mohs hardness of the V was 7.0.

[0115] <Example 5: Cu substrate / W ​​coating layer 100 nm, first active material layer (metal-carbon layer) thickness 7 μm> Except for changing the Ti thin film coating layer disposed on the Cu foil to a W thin film coating layer, a negative electrode and an all-solid-state secondary battery were manufactured in the same manner as in Example 1. The Mohs hardness of the Cu was 3.0, and the Mohs hardness of the W was 7.5.

[0116] <Example 6: Cu substrate / Cr coating layer 100 nm, first active material layer (metal-carbon layer) thickness 7 μm> Except for changing the Ti thin film coating layer disposed on the Cu foil to a Cr thin film coating layer, a negative electrode and an all-solid-state secondary battery were manufactured in the same manner as in Example 1. The Mohs hardness of the Cu was 3.0, and the Mohs hardness of the Cr was 8.5.

[0117] <Example 7: Ni substrate / Cr coating layer 100 nm, first active material layer (metal-carbon layer) thickness 7 μm> A negative electrode and an all-solid-state secondary battery were manufactured in the same manner as in Example 6, except that a 10 μm thick Ni foil was used instead of a Cu foil as the first metal substrate. The Mohs hardness of the Ni was 4.0, and the Mohs hardness of the Cr was 8.5.

[0118] <Example 8: SUS substrate / Cr coating layer 100 nm, first active material layer (metal-carbon layer) thickness 7 μm> A negative electrode and an all-solid-state secondary battery were manufactured in the same manner as in Example 6, except that a 10 μm thick stainless steel (SUS 304) sheet was used as the first metal substrate instead of the Cu foil. The Mohs hardness of the stainless steel was 5.5, and the Mohs hardness of Cr was 8.5.

[0119] <Example 9: Cu substrate / Ti coating layer 100 nm, first active material layer (metal-carbon layer) thickness 3 μm> A negative electrode and an all-solid-state secondary battery were manufactured in the same manner as in Example 1, except that the thickness of the first negative electrode active material layer was changed to 3 μm.

[0120] <Example 10: Cu substrate / Ti coating layer 100 nm, first active material layer (metal-carbon layer) thickness 15 μm> A negative electrode and an all-solid-state secondary battery were manufactured in the same manner as in Example 1, except that the thickness of the first negative electrode active material layer was changed to 15 μm.

[0121] Example 11: Bicell An all-solid-state secondary battery was manufactured in the same manner as in Example 1, except that a positive electrode active material layer and a gasket were disposed on both sides of a positive electrode current collector to prepare a positive electrode layer, and a solid electrolyte layer and a negative electrode layer were sequentially disposed on both sides of the positive electrode layer to manufacture a battery.

[0122] <Comparative Example 1: Cu substrate / first active material layer (metal-carbon layer) thickness 7 μm, no Ti coating layer member> Except for using a 10 μm thick Cu foil as it is as a negative electrode current collector, a negative electrode and an all-solid-state secondary battery were manufactured in the same manner as in Example 1. Therefore, no Ti thin film coating layer was provided.

[0123] <Comparative Example 2: Ni substrate / first active material layer (metal-carbon layer) thickness 7 μm, no Ti coating layer member> A negative electrode and an all-solid-state secondary battery were manufactured in the same manner as in Example 1, except that a 10 μm thick Ni foil was used as the negative electrode current collector as it was, and therefore no Ti thin film coating layer was provided.

[0124] <Comparative Example 3: SUS substrate / first active material layer (metal / carbon layer) thickness 7 μm, no Ti coating layer member> Except for using a 10 μm thick SUS sheet as it is as a negative electrode current collector, a negative electrode and an all-solid-state secondary battery were manufactured in the same manner as in Example 1. Therefore, no Ti thin film coating layer was provided.

[0125] <Reference Example 1: No gasket material> An all-solid-state secondary battery was manufactured in the same manner as in Example 1, except that no gasket was used during the manufacture of the positive electrode layer.

[0126] [Evaluation example 1: Charge / discharge test] The charge / discharge characteristics of the all-solid-state secondary batteries produced in Examples 1 to 11 and Comparative Examples 1 to 3 were evaluated by the following charge / discharge test. The charge / discharge test was performed by placing the all-solid-state secondary batteries in a thermostatic chamber at 60°C.

[0127] The first cycle was 0.6 mA / cm until the battery voltage reached 3.9 V to 4.25 V. 2 The battery was charged for 12.5 hours at a constant current of 0.6 mA / cm until the battery voltage reached 2.5 V. 2 Discharge was carried out at a constant current of 1000 V for 12.5 hours.

[0128] From the second cycle onwards, the charge and discharge cycles were repeated under the same conditions as the first cycle.

[0129] The capacity retention rate was evaluated based on the number of cycles at which the discharge capacity was 95% or more of the discharge capacity (standard capacity) in the first cycle.

[0130] Some of the measurement results are shown in Table 1 below.

[0131] [Table 1]

[0132] The all-solid-state secondary batteries of Examples 1 to 8 and 10 maintained 95% or more of the discharge capacity for 70 or more cycles. Therefore, it was confirmed that the all-solid-state secondary batteries of Examples 1 to 8 and 10 had an improved capacity maintenance rate.

[0133] Also, as can be seen from Examples 1 to 3, the capacity retention rate was improved more as the thickness of the second coating layer increased.

[0134] In addition, as can be seen from Examples 4 to 8, the capacity retention rate was improved as the Mohs hardness of the second coating layer metal increased.

[0135] The all-solid-state secondary battery of Example 10 had an improved capacity retention rate compared to the all-solid-state secondary battery of Example 1, but the total capacity of the all-solid-state secondary battery was relatively reduced compared to Example 1 due to an increase in the irreversible capacity.

[0136] It can be understood that the life characteristics are improved by preventing deterioration of the first metal substrate by coating the first metal substrate with a high hardness second metal layer.

[0137] On the other hand, the all-solid-state secondary batteries of Comparative Examples 1 and 2, which used negative electrodes that did not include a high-hardness second metal layer, maintained a discharge capacity of 95% or more for a number of cycles of 50 or less. Therefore, it was confirmed that the capacity retention rate of the all-solid-state secondary batteries of Comparative Examples 1 and 2 was reduced.

[0138] In particular, the all-solid-state secondary battery of Comparative Example 1, which used a Cu current collector as the negative electrode, which has a low Mohs hardness and causes a side reaction with sulfides, had the worst life characteristics.

[0139] In the all-solid-state secondary batteries of Examples 1 to 10, after the first cycle charging was completed, a scanning electron microscope (SEM) image of the cross section of the battery was measured, and it was found that a lithium metal layer corresponding to the second negative electrode active material layer was formed between the first negative electrode active material layer and the negative electrode current collector.

[0140] It was confirmed that the all-solid-state secondary battery of Example 11 also exhibited excellent cycle characteristics.

[0141] [Evaluation example 2: Checking for cracks after fabrication of all-solid-state battery] Cross sections of the all-solid-state secondary batteries manufactured in Examples 1 to 11 and Comparative Examples 1 to 3 were observed with a scanning electron microscope (SEM) to observe whether cracks penetrating the solid electrolyte layer were generated.

[0142] In the all-solid-state secondary batteries produced in Examples 1 to 11 and Comparative Examples 1 to 3, no cracks were observed in the solid electrolyte layer.

[0143] On the other hand, in the all-solid-state secondary battery of Reference Example 1, many cracks were observed in the solid electrolyte layer at the edge of the positive electrode layer.

[0144] In addition, the all-solid-state secondary battery of Reference Example 1 experienced a short circuit in less than 10 cycles during charging and discharging under the conditions of Evaluation Example 1, and had poor life characteristics.

[0145] Therefore, it was confirmed that in the all-solid-state secondary batteries of Examples 1 to 11, by using an inactive material for the positive electrode, cracks in the solid electrolyte layer were prevented during the battery manufacturing process.

[0146] Although an exemplary embodiment has been described in detail with reference to the attached drawings, the present invention is not limited to such an example. It is obvious that a person skilled in the art in the technical field to which the present invention belongs can derive various modifications or alterations within the scope of the technical idea described in the claims, and it goes without saying that these also belong to the technical scope of the present invention. [Explanation of symbols]

[0147] 1 All-solid-state secondary battery 10 positive electrode 11 Positive electrode current collector 12, 12a, 12b positive electrode active material layer 20, 20a, 20b negative electrode 21, 21a, 21b negative electrode current collector 22, 22a, 22b First metal base material 23, 23a, 23b Coating layers 24, 24a, 24b First negative electrode active material layer 30, 30a, 30b solid electrolyte layer 40 Inert Materials

Claims

1. a negative electrode current collector; and a first negative electrode active material layer disposed on the negative electrode current collector, the negative electrode current collector includes a first metal substrate and a coating layer disposed on an upper surface and a side surface of the first metal substrate and including a second metal; The Mohs hardness of the second metal is higher than the Mohs hardness of the first metal, The first metal is at least one selected from the group consisting of copper (Cu), nickel (Ni), stainless steel (SUS), iron (Fe) and cobalt (Co); a negative electrode, further comprising a second negative electrode active material layer disposed between a negative electrode current collector and a first negative electrode active material layer included in the negative electrode, the second negative electrode active material layer being a metal layer containing lithium or a lithium alloy.

2. 2. The negative electrode of claim 1, wherein the first metal has a Mohs hardness of 5.5 or less.

3. The negative electrode according to claim 1 or 2, wherein the second metal has a Mohs hardness of 6.0 or more.

4. The second metal is one or more selected from the group consisting of titanium (Ti), manganese (Mn), niobium (Nb), tantalum (Ta), iridium (Ir), vanadium (V), rhenium (Re), osmium (Os), tungsten (W), chromium (Cr), boron (B), ruthenium (Ru) and rhodium (Rh). The negative electrode according to any one of claims 1 to 3.

5. The negative electrode according to any one of claims 1 to 4, wherein the coating layer has a thickness of 1 µm or less.

6. The negative electrode according to any one of claims 1 to 5, wherein the coating layer is inactive with respect to a sulfide-based solid electrolyte.

7. 7. The negative electrode according to claim 1, wherein the first negative electrode active material layer comprises a negative electrode active material and a binder, the negative electrode active material has a particulate form, and the negative electrode active material has an average particle size of 4 μm or less.

8. The negative electrode according to claim 7 , wherein the negative electrode active material comprises at least one selected from the group consisting of a carbon-based negative electrode active material, and a metallic or semi-metallic negative electrode active material.

9. The anode of claim 8 , wherein the carbon-based anode active material comprises amorphous carbon.

10. 9. The negative electrode according to claim 8, wherein the metal negative electrode active material or the semi-metallic negative electrode active material comprises one or more selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), and zinc (Zn).

11. 11. The anode of claim 1, wherein the anode active material comprises a mixture of first particles made of amorphous carbon and second particles made of a metal or semi-metal, and a content of the second particles is in a range of 8 to 60 wt % based on a total weight of the mixture.

12. The negative electrode according to any one of claims 1 to 11, wherein the first negative electrode active material layer has a thickness of 1 µm to 20 µm.

13. A positive electrode and The negative electrode according to any one of claims 1 to 12, a solid electrolyte layer disposed between the positive electrode and the negative electrode; The solid electrolyte layer includes a sulfide-based solid electrolyte.

14. the positive electrode includes a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector, The all-solid-state secondary battery according to claim 13 , further comprising an inactive member surrounding a side surface of the positive electrode active material layer, disposed in a peripheral portion of the positive electrode current collector, and extending to an end portion of the positive electrode current collector.

15. The sulfide-based solid electrolyte is Li 2 S-P 2 S 5 , Li 2 S-P 2 S 5 -LiX (X is a halogen element), Li 2 S-P 2 S 5 -Li 2 O., Li 2 S-P 2 S 5 -Li 2 O-LiI, Li 2 S-SiS 2 , Li 2 S-SiS 2 - LiI, Li 2 S-SiS 2 - LiBr, Li 2 S-SiS 2 -LiCl, Li 2 S-SiS 2 -B 2 S 3 - LiI, Li 2 S-SiS 2 -P 2 S 5 - LiI, Li 2 S-B 2 S 3 , Li 2 S-P 2 S 5 -Z m S n (m and n are positive numbers, and Z is one of Ge, Zn, and Ga), Li 2 S-GeS 2 , Li 2 S-SiS 2 -Li 3 P.O. 4 , Li 2 S-SiS 2 -Li p M.O. q (p and q are positive numbers, and M is one of P, Si, Ge, B, Al, Ga, and In), Li 7-x P.S. 6-x C x (0≦x≦2), Li 7-x P.S. 6-x B x (0≦x≦2) and Li 7-x P.S. 6-x I x The all-solid-state secondary battery according to claim 13 or 14, comprising one or more selected from the group consisting of (0≦x≦2).

16. The all-solid-state secondary battery according to any one of claims 13 to 15, wherein the sulfide-based solid electrolyte comprises an argyrodite-type solid electrolyte represented by the following chemical formula 1: Li + 12-n-x A n+ X 2- 6-x Y - x (1) In the formula 1, A is P, As, Ge, Ga, Sb, Si, Sn, Al, In, Ti, V, Nb, or Ta, X is S, Se, or Te, and Y is Cl, Br, I, F, CN, OCN, SCN, or N. 3 where 1≦n≦5 and 0≦x≦2.

17. The argyrodite-type solid electrolyte is Li 7-x P.S. 6-x C x (0≦x≦2), Li 7-x P.S. 6-x B x (0≦x≦2) and Li 7-x P.S. 6-x I x The all-solid-state secondary battery according to claim 16, wherein x is one or more selected from the group consisting of (0≦x≦2).

18. The all-solid-state secondary battery according to any one of claims 13 to 17, wherein the second negative electrode active material layer is further disposed between the solid electrolyte layer and the first negative electrode active material layer.

Citation Information

Patent Citations

  • Battery

    JP2012049023A

  • Electrode body and secondary battery

    JP2016048651A

  • All-solid battery manufacturing method

    JP2017130281A

  • All-solid type secondary battery

    JP2019145299A