Pig iron production method

The method addresses the challenge of reducing coke usage in blast furnaces by stacking layers of low-basicity reduced iron compacts and high-basicity iron ore pellets, enhancing air permeability and maintaining furnace stability, thereby reducing CO2 emissions.

JP7596194B2Active Publication Date: 2024-12-09KOBE STEEL LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2021053067
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-26
Publication Date
2024-12-09
Estimated Expiration
2041-03-26

AI Technical Summary

Technical Problem

Existing blast furnace operations face limitations in reducing coke usage while maintaining stable operation, as the role of coke as a spacer cannot be fully replaced by auxiliary fuels, and the charging position of reduced iron is limited, hindering further reductions in CO2 emissions.

Method used

A method for manufacturing pig iron using a blast furnace that alternately stacks layers of ore raw material and coke, incorporating reduced iron compacts with low basicity and iron ore pellets with high basicity to enhance air permeability, reducing the need for coke by promoting melt-through and maintaining furnace stability.

Benefits of technology

This method reduces coke usage while ensuring stable blast furnace operation by improving air permeability and reducing CO2 emissions, achieved through the use of reduced iron compacts with low basicity and high-basicity iron ore pellets, which enhance melt-through and suppress viscosity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007596194000007
    Figure 0007596194000007
  • Figure 0007596194000008
    Figure 0007596194000008
  • Figure 0007596194000009
    Figure 0007596194000009
Patent Text Reader

Abstract

To provide a pig iron production method capable of reducing the used amount of cokes while maintaining the stable operation of a blast furnace.SOLUTION: A pig iron production method according to one aspect is a pig iron production method for producing a pig iron using a blast furnace having a tuyere and comprises the steps in which: a first layer comprising ore raw material and a second layer comprising cokes are alternately laminated inside the blast furnace; and, while blowing an auxiliary fuel into the blast furnace by hot wind fed from the tuyere, the ore raw material in the laminated first layer is reduced and melted. An aggregate comprising a reduced iron molded body obtained by compressively molding reduced iron is mixed into the first layer, the ore raw material uses iron ore pellets as the main raw material, the average basicity of the reduced iron molded body is 0.5 or less and the average basicity of the ore raw material is 0.9 or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing pig iron. [Background technology]

[0002] A method for producing pig iron is known in which a first layer containing raw ore and a second layer containing coke are alternately stacked in a blast furnace, and the raw ore is reduced and melted while auxiliary fuel is blown into the blast furnace by hot air blown from a tuyere. In this process, the coke serves as a heat source for melting the raw ore, a reducing agent for the raw ore, a recarburizer for carburizing the molten iron to lower its melting point, and a spacer for ensuring gas permeability in the blast furnace. By maintaining gas permeability with the coke, the lowering of the charge is stabilized, and stable operation of the blast furnace is achieved.

[0003] In blast furnace operation, it is desirable to have a low coke ratio from the viewpoint of cost reduction. However, if the coke ratio is reduced, the role of the coke described above is also reduced. For example, as a method for reducing the coke ratio, i.e., increasing the ratio of the ore raw material, a blast furnace operation method has been proposed in which reduced iron of small particle size is charged only to the periphery of the blast furnace (see JP-A-11-315308). In the above blast furnace operation method, it is said that by charging reduced iron that does not need to be reduced only to the periphery of the furnace, it is possible to increase the raw material filling rate while maintaining the roles of coke as a heat source, reducing agent, recarburizer, and spacer in the center of the furnace. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 11-315308 Summary of the Invention [Problem to be solved by the invention]

[0005] Due to the recent demand for reducing CO2 emissions, further reduction in the amount of coke used in blast furnace operation is required. In the above-mentioned conventional blast furnace operation method, the roles of coke as a heat source, reducing agent, and recarburizer can be replaced by auxiliary fuel injected from the tuyere. On the other hand, the role of spacer is played by only coke. In the above-mentioned conventional blast furnace operation method, the position where reduced iron is charged is limited to only the periphery of the furnace. Furthermore, the amount of coke used is only relatively reduced by charging reduced iron. Therefore, the above-mentioned conventional blast furnace operation method has a limit to the reduction in the amount of coke used, and it cannot be said that it can fully meet the recent demand for reducing CO2.

[0006] The present invention has been made in view of the above-mentioned circumstances, and has an object to provide a method for producing pig iron that can reduce the amount of coke used while maintaining stable operation of a blast furnace. [Means for solving the problem]

[0007] A method for producing pig iron according to one embodiment of the present invention is a method for producing pig iron using a blast furnace having a tuyere, the method comprising the steps of alternately stacking a first layer containing an ore raw material and a second layer containing coke in the blast furnace, and reducing and melting the stacked ore raw material in the first layer while blowing auxiliary fuel into the blast furnace with hot air blown from the tuyere, wherein aggregate including reduced iron molded bodies formed by compressing reduced iron is mixed into the first layer, the ore raw material is mainly made of iron ore pellets, the average basicity of the reduced iron molded bodies is 0.5 or less, and the average basicity of the iron ore pellets is 0.9 or more.

[0008] In the pig iron manufacturing method, the first layer containing the ore raw material contains a reduced iron molded body obtained by compressing and molding reduced iron as an aggregate. The reduced iron molded body facilitates the passage of hot air when the first layer is softened and fused in the melting process, so that the pig iron manufacturing method requires a small amount of coke to ensure gas permeability. In addition, the pig iron manufacturing method uses reduced iron molded bodies having an average basicity of 0.5 or less, so that the reduced iron molded bodies can be obtained relatively inexpensively. Furthermore, in the pig iron manufacturing method, iron ore pellets having an average basicity of 0.9 or more are used as the main raw material, which suppresses an increase in viscosity when the reduced iron molded bodies having a low basicity are melted, and promotes melt-through. This mainly improves the gas permeability of the cohesive zone, and further reduces the amount of coke used. Therefore, the pig iron manufacturing method can reduce the amount of coke used while maintaining stable operation of the blast furnace.

[0009] The content of the iron ore pellets in the raw ore is preferably 50% by mass or more. By setting the content of the iron ore pellets to the lower limit or more, the air permeability can be further improved.

[0010] The iron ore pellets are preferably self-fluxed. By making the iron ore pellets self-fluxed in this way, melt-through of the reduced iron cast is promoted, and the breathability can be further improved.

[0011] It is preferable that the ratio R of the unit consumption of the iron ore pellets to the unit consumption of the reduced iron cast bodies satisfies the following formula 1. When the ratio R of the unit consumption of the iron ore pellets to the unit consumption of the reduced iron cast bodies satisfies the following formula 1, the effect of improving the air permeability due to the melt-through of the reduced iron cast bodies can be more reliably achieved.

number

[0012] Here, "main raw material" refers to the raw material with the largest content by mass. "Basicity" refers to the ratio of the mass of CaO to the mass of SiO2. In addition, when the target substance is composed of multiple granules, "average basicity" refers to the ratio of the total mass of CaO to the total mass of SiO2 of the multiple granules.

[0013] The "critical basicity" refers to the average basicity at which the maximum pressure drop starts to decrease when the pressure drop of the sample packed bed is continuously measured and the maximum value (maximum pressure drop) is plotted using the average basicity of HBI as a parameter, as shown in Figure 3. The sample packed bed can be composed of an upper coke layer 72a (height 20 mm), an ore layer 72b (height 110 mm), and a lower coke layer 72c (height 40 mm) from the top, using a large-scale load reduction experimental furnace 7 in which the graphite crucible 71 in which the sample is packed has an inner diameter of φ75 mm, as shown in Figure 5, for example. Effect of the Invention

[0014] As described above, by using the pig iron manufacturing method of the present invention, it is possible to reduce the amount of coke used while maintaining stable operation of the blast furnace. [Brief description of the drawings]

[0015] [Figure 1] FIG. 1 is a flow diagram showing a method for producing pig iron according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing the inside of a blast furnace used in the pig iron manufacturing method of FIG. [Diagram 3] FIG. 3 is a graph showing the relationship between the average basicity of the reduced iron cast and the maximum pressure drop. [Figure 4] FIG. 4 is a schematic enlarged partial view of the vicinity of the cohesive zone and the dripping zone in FIG. [Diagram 5] FIG. 5 is a schematic cross-sectional view showing the configuration of the large-scale load reduction experimental reactor used in the examples. [Figure 6] FIG. 6 is a graph showing a temperature profile for heating the sample-packed layer in the example. [Figure 7]FIG. 7 is a graph showing the relationship between the temperature of the sample-packed layer and the flow rate of the supplied gas in the examples. [Figure 8] FIG. 8 is a graph showing the results of the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, a method for producing pig iron according to each embodiment of the present invention will be described.

[0017] The pig iron manufacturing method shown in FIG. 1 is a pig iron manufacturing method for manufacturing pig iron using a blast furnace 1 shown in FIG. 2, and includes a laminating step S1 and a melting step S2.

[0018] <Blast furnace> As shown in FIG. 2, the blast furnace 1 has a tuyere 1a and a tap hole 1b provided at the bottom of the furnace. Usually, a plurality of tuyere 1a are provided. The blast furnace 1 is a solid-gas counterflow type shaft furnace, in which hot air, which is high-temperature air and, as necessary, high-temperature or room-temperature oxygen, is blown into the furnace from the tuyere 1a to carry out a series of reactions such as reduction and melting of the ore raw material 11 described later, and pig iron can be taken out from the tap hole 1b. The blast furnace 1 is also equipped with a Bell-Armor type raw material charging device 2. This raw material charging device 2 will be described later.

[0019] <Lamination process> In the stacking step S1, as shown in Fig. 2, the first layers 10 and the second layers 20 are alternately stacked in the blast furnace 1. That is, the number of layers of each of the first layers 10 and the second layers 20 is two or more.

[0020] (1st layer) The first layer 10 includes raw ore 11. The first layer 10 is also mixed with aggregate 12. In addition to the raw ore 11 and aggregate 12, auxiliary materials such as limestone, dolomite, and silica stone may be charged into the first layer 10.

[0021] The raw ore 11 refers to ores that are used as iron raw materials. The raw ore 11 is heated and reduced by hot air blown in from the tuyere 1a in the melting step S2 to become molten pig iron. In this pig iron manufacturing method, iron ore pellets are used as the main raw material. "Iron ore pellets" are made from fine iron ore powder of several tens of μm, and are produced by improving the quality to have properties suitable for blast furnaces (e.g. size, strength, reducibility, etc.). In this pig iron manufacturing method, it is preferable that the iron ore pellets do not contain fine powder of sintered ore.

[0022] The lower limit of the average basicity of the iron ore pellets is 0.9, more preferably 1.0, which is basic, and even more preferably 1.4. If the basicity of the iron ore pellets is less than the lower limit, it is difficult to promote the melting through of the reduced iron molded body, and the air permeability may be reduced. Although the upper limit of the average basicity of the iron ore pellets is not particularly limited, the average basicity of the iron ore pellets is usually 2.0 or less.

[0023] The lower limit of the content of the iron ore pellets in the raw ore 11 is preferably 50 mass%, more preferably 90 mass%, and even more preferably 100 mass%, i.e., the raw ore 11 is entirely made of iron ore pellets. By setting the content of the iron ore pellets to be equal to or more than the lower limit, the air permeability can be further improved.

[0024] The iron ore pellets are preferably self-fluxed. By making the iron ore pellets self-fluxed in this way, melt-through of the reduced iron cast is promoted, and the breathability can be further improved.

[0025] The iron ore pellets preferably have a porosity of 21% or more for coarse open pores having a pore diameter of 4 μm or more. By including iron ore pellets having a porosity of 21% or more for coarse open pores having a pore diameter of 4 μm or more in the raw ore, the reduction rate of the raw ore can be increased, and the amount of coke used can be further reduced. Here, the "porosity of coarse open pores having a pore diameter of 4 μm or more" refers to the ratio of the volume of coarse open pores having a pore diameter of 4 μm or more to the apparent volume of the iron ore pellets, and is calculated by using a mercury intrusion porosimeter (e.g., Shimadzu Corporation's "Autopore III9400") to determine the open porosity ε0 [%] of the iron ore pellets and the total pore volume A [cm3] per unit weight of the iron ore pellets. 3 / g], total pore volume A of pores with a diameter of 4 μm or more per unit weight of iron ore pellet +4 [cm 3 / g], then ε0×A +4 / A [%]. Note that open pores refer to pores that are open to the outside of the iron ore pellets, and closed pores refer to pores that are closed inside the iron ore pellets.

[0026] The iron ore pellets preferably contain MgO. MgO has the effect of increasing the desulfurization ability of the slag at the hearth level and increasing the reducibility at high temperatures. For this reason, it is considered that MgO has the effect of accelerating the burn-through of the reduced iron cast by making the burn-through behavior of the raw ore 11 closer to that of the reduced iron cast. The lower limit of the content of MgO in the raw ore 11 is preferably 1 mass%, more preferably 1.5 mass%. On the other hand, the upper limit of the content of MgO is preferably 4 mass%, more preferably 3 mass%. If the content of MgO is less than the lower limit, the effect of accelerating the burn-through of the reduced iron cast may not be sufficiently obtained. Conversely, if the content of MgO exceeds the upper limit, the strength of the iron ore pellets may be reduced.

[0027] In addition to the iron ore pellets, the raw ore 11 may contain sinter, lump ore, carbonaceous composite agglomerated ore, metal, etc. From the viewpoint of improving permeability, the content of sinter in the raw ore 11 is preferably 10% by mass or less, and more preferably 0% by mass, i.e., the raw ore 11 does not contain sinter.

[0028] Although the reduced iron casts contained in the aggregate 12 described later can also be used as an iron raw material, the reduced iron casts are not included in the raw ore 11 in this specification.

[0029] The aggregate 12 is intended to improve the air permeability of the cohesive zone D described later and to allow the hot air to pass to the center of the blast furnace 1. The aggregate 12 includes reduced iron molded bodies (HBI, hot briquette iron) obtained by compression molding reduced iron.

[0030] HBI is made by forming reduced iron DRI (Direct Reduced Iron) in a hot state. DRI has a high porosity and has the drawback of oxidizing and generating heat during marine transportation and outdoor storage, while HBI has a low porosity and is difficult to reoxidize. After ensuring the breathability of the first layer 10, the aggregate 12 functions as metal and becomes molten iron. Since the aggregate 12 has a high metallization rate and does not require reduction, not much reducing agent is required to become this molten iron. Therefore, CO2 emissions can be reduced. Note that the "metallization rate" refers to the ratio [mass %] of metallic iron to the total iron content.

[0031] The upper limit of the average basicity of the reduced iron cast is 0.5, and 0.4 is more preferable. The reduced iron cast contains SiO2 and Al2O3 as slag components derived from iron ore, and generally tends to have a low average basicity. In the pig iron production method, a reduced iron cast having an average basicity equal to or lower than the upper limit is used, so that it is not necessary to prepare a high-quality reduced iron cast having an increased basicity by removing SiO2 or Al2O3 or adding CaO. Therefore, pig iron can be produced at low cost. On the other hand, the lower limit of the average basicity of the reduced iron cast is not particularly limited, and may be 0.

[0032] It is preferable that the ratio R of the unit consumption of the iron ore pellets to the unit consumption of the reduced iron cast bodies satisfies the following formula 1. When the ratio R of the unit consumption of the iron ore pellets to the unit consumption of the reduced iron cast bodies satisfies the following formula 1, the effect of improving the air permeability due to the melt-through of the reduced iron cast bodies can be more reliably achieved.

number

[0033] The above formula 1 will be explained in detail. FIG. 3 is a graph showing the relationship between the average basicity of HBI and the maximum pressure drop of a packed bed in which the first layer 10 and the second layer 20 are alternately laminated. It can be determined that the smaller the maximum pressure drop, the higher the air permeability. From FIG. 3, it can be seen that when the average basicity of HBI exceeds a certain value, the air permeability is improved. This certain value is the critical basicity. When CaO with a basicity equal to or higher than the critical basicity is present, it is considered that SiO2 in HBI changes into a calcium silicate-based melt, which reduces the viscosity of the molten iron generated from HBI and promotes melting. In other words, it can be said that CaO with a basicity equal to or higher than the critical basicity is necessary to obtain the effect of promoting melting of HBI.

[0034] In Figure 3, CaO is supplied from HBI, but it is also possible to supply CaO from iron ore pellets. In that case, if the amount of CaO exceeds the critical basicity with respect to the amount of SiO2 of the combined HBI and iron ore pellets, it is considered that the meltdown of HBI is promoted and the permeability of the packed bed is improved.

[0035] The SiO2 and CaO amounts of HBI and iron ore pellets combined are calculated based on the unit cost of reduced iron compacts. HBI (kg), and the unit of iron ore pellets is M P (kg) and is expressed by the following formula 2.

number

[0036] Here, as described above, CaO content / SiO2 content ≧ (C / S) criticalis satisfied, it is believed that the melting of HBI will be accelerated. Therefore, by substituting Equation 2 into this inequality, R = M P / M HBI By solving this, we obtain the above equation 1.

[0037] The lower limit of the charging amount of the reduced iron casts is preferably 100 kg, more preferably 150 kg, per ton of pig iron. If the charging amount of the reduced iron casts is less than the lower limit, the aggregate 12 in the cohesive zone D may not be able to sufficiently ensure the gas permeability in the melting step S2. On the other hand, the upper limit of the charging amount of the reduced iron casts is appropriately determined within a range in which the aggregate effect is not reduced due to an excess of aggregate, and the upper limit of the charging amount of the reduced iron casts is set to, for example, 700 kg per ton of pig iron.

[0038] The lower limit of the ratio of the average particle diameter of the reduced iron cast to the average particle diameter of the raw ore 11 is preferably 1.3, more preferably 1.4. As shown in FIG. 4, even when a part of the raw ore 11 in the first layer 10 melts and moves downward in the blast furnace 1 as dripping slag 13, and the raw ore 11 softens and shrinks, the reduced iron cast having a high melting point does not soften. If the reduced iron cast that is larger than the raw ore 11 by a certain amount is mixed as aggregate 12, the aggregate effect of the reduced iron cast is easily exhibited, and the first layer 10 as a whole can be prevented from shrinking. Therefore, by setting the ratio of the average particle diameter to the lower limit or more, a flow path of hot air as shown by the arrow in FIG. 4 can be secured, and the air permeability in the melting step S2 can be improved. On the other hand, the upper limit of the ratio of the average particle diameter is preferably 10, more preferably 5. If the ratio of the average particle diameter exceeds the upper limit, it becomes difficult to uniformly mix the reduced iron cast in the first layer 10, and segregation may increase. The term "average particle size" refers to the particle size at which the cumulative mass is 50% in the particle size distribution.

[0039] The upper limit of the air permeability resistance index of the reduced iron cast after the tumbler rotation test is preferably 0.1, more preferably 0.08. The reduced iron cast is generally transported between a factory where it is manufactured and a factory where it is used. During this transport, the volumetric destruction may occur and the particle size distribution may change. Therefore, by using a reduced iron cast that is guaranteed to have an air permeability resistance index of a certain value or less even after the tumbler rotation test, the air permeability in the lumpy zone E described later can be improved in actual blast furnace operation. On the other hand, the lower limit of the air permeability resistance index is not particularly limited and may be a value close to 0, which is the theoretical limit value by definition, but is usually about 0.03. It is sufficient to use a reduced iron cast having a property that the air permeability resistance index is a predetermined value or less, and this does not mean that the pig iron production method requires a tumbler rotation test.

[0040] Here, the "air permeability index after tumbler rotation test" of the reduced iron molded body is calculated as follows. First, a tumbler rotation test is performed according to the rotation strength measurement method for iron ores (JIS-M8712:2000), and the particle size distribution of the reduced iron molded body is obtained by sieving. This particle size distribution is calculated by dividing the representative particle size (median value) between the sieve openings by d i [cm], representative particle size d i The weight fraction of the reduced iron compacts belonging to i Using this particle size distribution, the harmonic mean diameter D p [cm], particle size composition index I sp is calculated using the following formula 3. Furthermore, the gravity conversion coefficient g c [9.807(g cm) / (G sec 2 )] to calculate the airflow resistance index K using the following formula 3. Note that the tumbler rotation conditions in the above tumbler rotation test are 24±1 rpm and 600 rotations.

number

[0041] In addition, when the reduced iron cast contains aluminum oxide, the upper limit of the content of the aluminum oxide in the reduced iron cast is preferably 1.5 mass %, more preferably 1.3 mass %. If the content of the aluminum oxide exceeds the upper limit, the melting point of the slag may be increased and the viscosity may be increased, which may make it difficult to ensure gas permeability in the lower part of the furnace. For this reason, by setting the content of the aluminum oxide in the reduced iron cast to the upper limit or less, it is possible to prevent an increase in the amount of coke used. The content of the aluminum oxide may be 0 mass %, i.e., the reduced iron cast may not contain aluminum oxide, but the lower limit of the content of the aluminum oxide is preferably 0.5 mass %. If the content of the aluminum oxide is less than the lower limit, the reduced iron cast may be expensive, which may increase the production cost of pig iron.

[0042] (2nd layer) The second layer 20 includes coke 21 .

[0043] The coke 21 serves as a heat source for melting the raw ore 11, as a generator of CO gas which is a reducing agent necessary for reducing the raw ore 11, as a recarburizer for carburizing the molten iron to lower its melting point, and as a spacer for ensuring ventilation within the blast furnace 1.

[0044] (Layering method) Various methods can be used to alternately stack the first layers 10 and the second layers 20. Here, the method will be described using as an example a blast furnace 1 equipped with a Bell-Armor type raw material charging device 2 (hereinafter, also simply referred to as "raw material charging device 2") as shown in Figure 2.

[0045] The raw material charging device 2 is provided at the top of the furnace. That is, the first layer 10 and the second layer 20 are charged from the top of the furnace. As shown in FIG. 2, the raw material charging device 2 has a bell cup 2a, a lower bell 2b, and an armor 2c.

[0046] Bell cup 2a is filled with the raw materials to be charged. When charging first layer 10, the raw materials constituting first layer 10 are charged into bell cup 2a, and when charging second layer 20, the raw materials constituting second layer 20 are charged into bell cup 2a.

[0047] Lower bell 2b is cone-shaped and spreads downward, and is disposed within bell cup 2a. Lower bell 2b can move up and down (in Fig. 2, the upward movement is shown by a solid line, and the downward movement is shown by a dashed line). When lower bell 2b moves upward, it seals the bottom of bell cup 2a, and when moved downward, a gap is formed on the extension of the side wall of bell cup 2a.

[0048] The armor 2c is provided below the lower bell 2b on the furnace wall of the blast furnace 1. When the lower bell 2b is moved downward, raw materials fall from the gap, and the armor 2c is a repulsion plate for repelling the falling raw materials. The armor 2c is configured to be able to move in and out toward the inside (center) of the blast furnace 1.

[0049] Using this raw material charging device 2, the first layer 10 can be laminated as follows. The same applies to the second layer 20. The first layer 10 and the second layer 20 are laminated alternately.

[0050] First, the lower bell 2b is positioned upward, and the raw material for the first layer 10 is charged into the bell cup 2a. When the lower bell 2b is positioned upward, the lower part of the bell cup 2a is sealed, so the raw material is filled into the bell cup 2a. The amount of the raw material filled is the amount of each layer stacked.

[0051] Next, the lower bell 2b is moved downward. This creates a gap between the bell cup 2a and the raw material, which falls through this gap toward the furnace wall and collides with the armor 2c. The raw material collides with the armor 2c and is then loaded into the furnace. The raw material falls while moving toward the furnace interior due to the repulsion from the armor 2c, so it flows from the position where it fell toward the center of the furnace and accumulates. The armor 2c is configured to be able to move in and out toward the center, so the falling position of the raw material can be adjusted by moving the armor 2c in and out. This adjustment allows the first layer 10 to be accumulated in a desired shape.

[0052] <Dissolution process> In the melting step S2, the ore raw material 11 in the stacked first layer 10 is reduced and melted while auxiliary fuel is blown into the blast furnace by hot air blown from the tuyere 1a. Note that the blast furnace is a continuous operation, and the melting step S2 is performed continuously. On the other hand, the stacking step S1 is performed intermittently, and new first layers 10 and second layers 20 to be treated in the melting step S2 are added depending on the status of the reduction and melting treatment of the first layer 10 and the second layer 20 in the melting step S2.

[0053] Fig. 2 shows the state in the melting step S2. As shown in Fig. 2, a raceway A, which is a hollow portion in which coke 21 swirls and exists in a significantly sparse state, is formed near the tuyere 1a by hot air from the tuyere 1a. The temperature of this raceway A is the highest in the blast furnace 1, at about 2000°C. Adjacent to the raceway A, there is a core B, which is a pseudo-stagnation region of the coke inside the blast furnace 1. Also, from the core B upward, there are a dripping zone C, a cohesive zone D, and a lumpy zone E, in that order.

[0054] The temperature inside the blast furnace 1 rises from the top towards the raceway A. In other words, the temperature is highest in the lumpy zone E, followed by the cohesive zone D and the dripping zone C. For example, the lumpy zone E is between 20°C and 1200°C, whereas the core B is between 1200°C and 1600°C. The temperature of the core B varies in the radial direction, and the temperature at the center of the core B may be lower than that of the dripping zone C. In addition, by stably circulating hot air in the center of the furnace, the cohesive zone D with an inverted V-shaped cross section is formed, ensuring the permeability and reducibility inside the furnace.

[0055] In the blast furnace 1, the iron ore raw material 11 is first heated and reduced in the lumpy zone E. In the cohesive zone D, the ore reduced in the lumpy zone E softens and shrinks. The softened and shrunk ore descends to become dripping slag and moves to the dripping zone C. In the smelting step S2, the reduction of the ore raw material 11 mainly proceeds in the lumpy zone E, and the melting of the ore raw material 11 mainly occurs in the dripping zone C. In the dripping zone C and the core B, direct reduction proceeds in which the descending liquid iron oxide FeO directly reacts with the carbon of the coke 21.

[0056] The aggregate 12 including the reduced iron casts exerts an aggregate effect in the cohesive zone D. In other words, even if the ore is in a softened and shrunk state, the reduced iron casts having a high melting point do not soften, and an air passage for reliably passing the hot air to the center of the blast furnace 1 is secured.

[0057] The reduced iron compact has a high melting point, but due to the carburization reaction caused by carbon monoxide (CO) in the reducing gas and carbon in the coke, the melting point is lowered to about 1500°C in the temperature range below the cohesive zone D. It becomes molten iron. At this point, the SiO2 slag component contained in the reduced iron molded body is still in a solid state, and it is in a solid-liquid coexistence state with the molten iron from the previously melted reduced iron molded body, and the viscosity is high, so the melt-down stagnates. Here, in the case of reduced iron molded bodies with high basicity, CaO reacts with SiO2 to form calcium silicate molten liquid, which eliminates the solid-liquid coexistence and promotes the melt-down. In the case of reduced iron molded bodies with low basicity, i.e., with a high SiO2 content, when SiO2 supplied from the reduced iron molded body reacts with CaO supplied from iron ore pellets with high basicity, i.e., with a high CaO content, the solid-liquid coexistence state is eliminated, and the melt-down of the reduced iron molded body is promoted.

[0058] Molten pig iron F, which is molten reduced iron, is piled up in the hearth, and molten slag G is piled up on top of the molten pig iron F. The molten pig iron F and molten slag G can be taken out from the tap hole 1b.

[0059] Examples of the auxiliary fuel injected from the tuyere 1a include pulverized coal made by pulverizing coal to a particle size of about 50 μm, heavy oil, natural gas, etc. The auxiliary fuel functions as a heat source, a reducing agent, and a recarburizer. In other words, it replaces the roles of the coke 21 except for the role of a spacer.

[0060] <Advantages> In the pig iron manufacturing method, the first layer 10 including the raw ore 11 includes a reduced iron molded body obtained by compressing reduced iron as the aggregate 12. The reduced iron molded body facilitates the passage of hot air when the first layer 10 is softened and fused in the melting step S1, so that the pig iron manufacturing method requires a small amount of coke to ensure gas permeability. In addition, the pig iron manufacturing method uses reduced iron molded bodies having an average basicity of 0.5 or less, so that the reduced iron molded bodies can be obtained relatively inexpensively. Furthermore, in the pig iron manufacturing method, iron ore pellets having an average basicity of 0.9 or more are used as the main raw material, which suppresses an increase in viscosity when the reduced iron molded bodies having a low average basicity are melted, and promotes melting through. This mainly improves the gas permeability of the cohesive zone D, and further reduces the amount of coke used. Therefore, the pig iron manufacturing method can reduce the amount of coke used while maintaining stable operation of the blast furnace 1.

[0061] [Other embodiments] It should be noted that the present invention is not limited to the above-described embodiment.

[0062] In the above embodiment, it has been explained on the premise that the ore raw material of all the stacked first layers is mainly made of iron ore pellets, the average basicity of the reduced iron casts is 0.5 or less, and the average basicity of the iron ore pellets is 0.9 or more, but the present invention includes a configuration in which the ore raw material of at least one first layer is mainly made of iron ore pellets, the average basicity of the reduced iron casts is 0.5 or less, and the average basicity of the iron ore pellets is 0.9 or more. However, it is preferable that 90% or more, more preferably 95% or more, and even more preferably 100%, i.e., all layers are first layers having the above configuration.

[0063] In the above embodiment, the pig iron manufacturing method of the present invention has been described as including only the lamination process and the melting process, but the pig iron manufacturing method may include other processes.

[0064] For example, the pig iron manufacturing method may include a step of charging a mixture of coke and reduced iron casts into the center of the blast furnace. In this case, it is preferable that the ratio of the reduced iron casts having a particle size of 5 mm or more among the reduced iron casts in the mixture is 90 mass % or more, and the content of the reduced iron casts in the mixture is 75 mass % or less. When the hot air reaches the center of the blast furnace, it rises in the center. By including reduced iron casts having a large particle size in the center at a content of the upper limit or less, sensible heat can be effectively utilized without impeding the flow of the hot air. Therefore, the amount of coke used can be further reduced. Here, the "center" of the blast furnace refers to a region that is 0.2Z or less away from the center, where Z is the radius of the furnace throat.

[0065] The pig iron manufacturing method may also include a step of pulverizing the powder derived from the reduced iron molded body and coal. In this case, it is preferable to include the fine powder obtained in the pulverizing step as the auxiliary fuel. The reduced iron molded body is partially crushed into powder during the transportation process or the like. Such powder reduces the gas permeability in the blast furnace, and is therefore not suitable for use as the first layer. In addition, this powder has a large specific surface area, so it is reoxidized to iron oxide. If the auxiliary fuel containing this iron oxide is injected from the tuyere, the gas permeability can be improved. Therefore, by pulverizing the powder derived from the reduced iron molded body together with coal and using the pulverized powder and the fine powder containing the coal as the auxiliary fuel to be injected from the tuyere, the reduced iron molded body can be effectively utilized and the gas permeability in the blast furnace can be improved.

[0066] Although the above embodiment has been described using the Bell-Armor method as the lamination process, other methods can also be used. One such method is the Bell-Less method. In the Bell-Less method, a rotating chute is used and lamination can be performed while adjusting the angle. EXAMPLES

[0067] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0068] The effect of the basicity of iron ore pellets on the permeability was investigated by conducting a large-scale load reduction experiment simulating the surrounding area of ​​a blast furnace.

[0069] FIG. 5 shows the large-scale load reduction experimental furnace 7 used in this experiment. The inner diameter of the graphite crucible 71 in which the samples were packed was φ75 mm. The sample packed layer 72 was composed of an upper coke layer 72a (height 20 mm), an ore layer 72b (height 110 mm), and a lower coke layer 72c (height 40 mm) from the top. The ore layer 72b corresponds to the first layer 10 of the present invention, and the upper coke layer 72a and the lower coke layer 72c correspond to the second layer 20.

[0070] The ore layer 72b was a mixture of reduced iron casts (HBI) and raw ore. The total iron content (T.Fe) of the ore layer 72b was constant.

[0071] The chemical properties of the HBI used are shown in Table 1. The average basicity of HBI was 0.46. The amount of HBI charged was 250 kg per ton of pig iron.

[0072] [Table 1]

[0073] Three types of ore raw materials were prepared: (1) iron ore pellets with an average basicity of 0.04 (SiO2 content = 5.44 mass%, MgO content = 0.54 mass%), (2) iron ore pellets with an average basicity of 1.20 (SiO2 content = 4.23 mass%, MgO content = 2.11 mass%), and (3) self-fluxed sinter with an average basicity of 2.10 (SiO2 content = 5.40 mass%, MgO content = 1.00 mass%).

[0074] Each of the sample packed beds 72 using the ore raw materials (1) to (3) described above was heated using an electric furnace 73 according to the temperature profile shown in FIG. 6, while a gas (reducing gas) having the composition shown in FIG. 7 was supplied. The gas was supplied from a gas supply pipe 74 provided at the bottom of the large-scale load reduction experimental furnace 7, and discharged from a gas discharge pipe 75 provided at the top. The total supply rate of the gas was 40 NL / min, and temperature control was performed using two thermocouples 76. The load applied to the sample packed beds 72 was 1 kgf / cm. 2 This load was applied by applying the weight of a weight 78 via a load rod 77.

[0075] The pressure drop of the sample packed bed 72 was continuously measured under the above-mentioned conditions, and the time integral value of the pressure drop (S value) was calculated. The S value can be used as an evaluation index of the softening and melting behavior of the ore layer 72b, and it is considered that the smaller the S value, the higher the permeability. The results are shown in Figure 8.

[0076] The results in Figure 8 show that the S value is in the following order: iron ore pellets with an average basicity of 1.20 < iron ore pellets with an average basicity of 0.04 < self-fluxed sintered ore with an average basicity of 2.10. It is clear that air permeability is improved by using iron ore pellets with an average basicity of 0.9 or more as the ore raw material.

[0077] The average basicity (=CaO amount / SiO2 amount) determined from the amount of CaO and SiO2 calculated based on the above formula 2 was 0.10 when (1) iron ore pellets with an average basicity of 0.04 were used, and 1.13 when (2) iron ore pellets with an average basicity of 1.20 were used. The critical basicity of the HBI used was 0.88, and it can be said that the air permeability is improved by setting the basicity determined from the amount of CaO and SiO2 calculated based on the above formula 2 as the critical basicity of the HBI, i.e., by satisfying the above formula 1. [Industrial Applicability]

[0078] By using the pig iron manufacturing method of the present invention, it is possible to reduce the amount of coke used while maintaining stable operation of the blast furnace. [Explanation of symbols]

[0079] 1 blast furnace 1a tuyere 1b Taphole 2 Raw material charging device 2a Bell Cup 2b Lower Bell 2c Armor 10 1st layer 11 Mineral ore 12 Aggregate 13 Dripping slag 20 2nd layer 21 Coke 7. Large-scale load reduction experimental reactor 71 Graphite crucible 72 Sample Packing Bed 72a Upper coke layer 72b Ore layer 72c Lower coke layer 73 Electric Furnace 74 Gas supply pipe 75 Gas exhaust pipe 76 Thermocouple 77 Load rod 78 Weight A Raceway B Core C. Droplet zone D Cohesive zone E. Lumpy Zone F Molten iron G Molten slag

Claims

1. A method for producing pig iron using a blast furnace having a tuyere, comprising the steps of: stacking alternately first layers including raw ore and second layers including coke in the blast furnace; reducing and melting the ore raw material of the first layer stacked while blowing auxiliary fuel into the blast furnace with hot air blown from the tuyere; Equipped with an aggregate including a reduced iron molded product obtained by compressing reduced iron is mixed into the first layer; The ore raw material is mainly iron ore pellets, The average basicity of the reduced iron cast body is 0.5 or less, The iron ore pellets have an average basicity of 0.9 or more; A method for producing pig iron, wherein the ratio of the average particle size of the reduced iron cast bodies to the average particle size of the raw ore is 1.4 or more and 10 or less.

2. A method for producing pig iron using a blast furnace having a tuyere, comprising the steps of: stacking alternately first layers including raw ore and second layers including coke in the blast furnace; reducing and melting the ore raw material of the first layer stacked while blowing auxiliary fuel into the blast furnace with hot air blown from the tuyere; Equipped with an aggregate including a reduced iron molded product obtained by compressing reduced iron is mixed into the first layer; The ore raw material is mainly iron ore pellets, The average basicity of the reduced iron cast body is 0.5 or less, The iron ore pellets have an average basicity of 0.9 or more; A method for producing pig iron, wherein a ratio R of a unit consumption of the iron ore pellets to a unit consumption of the reduced iron cast satisfies the following formula 1: [0010] In formula 1, (C / S) is the average basicity, (%SiO 2 ) is SiO 2 The subscript HBI indicates reduced iron compact, and P indicates iron ore pellet. critical represents the critical basicity of HBI.

3. 3. The method for producing pig iron according to claim 1 or 2, wherein the content of the iron ore pellets in the raw ore is 50 mass% or more.

4. 4. A method for producing pig iron as claimed in any one of claims 1 to 3, wherein the iron ore pellets are self-fluxed.

Citation Information

Patent Citations

  • Operation of blast furnace

    JP1999315308A

  • Method for producing pig iron

    JP2009102746A

  • Self-fluxing pellet for blast furnace, and its manufacturing method

    JP2009149942A