Polymerization of ethylene in solution processes using Ziegler-Natta and hydrogenation catalysts

A catalyst system with a heterogeneous procatalyst and hydrogenation procatalyst produces high molecular weight polymers efficiently at high temperatures, addressing the limitations of existing systems by improving molecular weight and reactivity.

JP7596357B2Active Publication Date: 2024-12-09DOW GLOBAL TECHNOLOGIES LLC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2022504156
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-07-31
Filing Date
2020-07-28
Publication Date
2024-12-09
Estimated Expiration
2040-07-28

AI Technical Summary

Technical Problem

Existing catalyst systems struggle to produce high molecular weight polymers efficiently at high polymerization temperatures (120°C to 250°C) with high reactivity and molecular weight greater than 100,000 g/mol.

Method used

A catalyst system comprising a heterogeneous procatalyst with a titanium species, an aluminum species, and a magnesium chloride component, along with a hydrogenation procatalyst of formula Cp2TiX2, where Cp is cyclopentadienyl substituted with C1-C10 alkyl and X is a halogen atom, is used to polymerize ethylene and alpha-olefins.

Benefits of technology

The catalyst system achieves high molecular weight polymers with improved efficiency and reactivity at elevated temperatures, enhancing molecular weight distribution and polymer properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007596357000012
    Figure 0007596357000012
  • Figure 0007596357000001
    Figure 0007596357000001
  • Figure 0007596357000002
    Figure 0007596357000002
Patent Text Reader

Abstract

The catalyst system includes a heterogeneous procatalyst and a hydrogenation procatalyst. The heterogeneous procatalyst includes a titanium species, an aluminum species, and a magnesium chloride component. The hydrogenation procatalyst has the formula Cp2TiX2. In the formula Cp2TiX2, each Cp is represented by at least one R 1 cyclopentadienyl substituted with R 1 However, (C1-C 10 ) alkyl, and each X is independently a halogen atom.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority to U.S. Provisional Patent Application No. 62 / 881,004, filed July 31, 2019, the entire disclosure of which is incorporated herein by reference.

[0002] SUMMARY OF THE DISCLOSURE Embodiments of the present disclosure relate generally to catalyst compositions for the polymerization of ethylene, and optionally one or more α-olefins, and polymerization processes utilizing such catalyst compositions. [Background technology]

[0003] Olefin-based polymers, such as polyethylene, ethylene-based polymers, polypropylene, and propylene-based polymers, are produced by various catalyst systems. The selection of such catalyst system used in the polymerization process of an olefin-based polymer is an important factor that contributes to the characteristics and properties of such an olefin-based polymer.

[0004] Ethylene- and propylene-based polymers are produced for a wide variety of articles. The polyethylene and polypropylene polymerization processes can be modified in many ways to produce a wide variety of resulting polyethylene resins with different physical properties that make the various resins suitable for use in a variety of applications. The ethylene monomer and optionally one or more comonomers are present in a liquid diluent (such as a solvent), such as an alkane or isoalkane, e.g., isobutene. Hydrogen can also be added to the reactor. Catalyst systems for producing ethylene-based polymers can typically include chromium-based catalyst systems, Ziegler-Natta catalyst systems, and / or molecular (either metallocene or nonmetallocene) catalyst systems. The diluent and reactants in the catalyst system are circulated in the reactor at elevated polymerization temperatures, thereby producing an ethylene-based homopolymer or copolymer. Either periodically or continuously, a portion of the reaction mixture, including the polyethylene product dissolved in the diluent, is removed from the reactor, along with unreacted ethylene and one or more optional comonomers. Once removed from the reactor, the reaction mixture may be treated to remove the polyethylene product from the diluent and unreacted reactants, which are typically recycled back into the reactor. Alternatively, the reaction mixture may be sent to a second reactor connected in series to the first reactor, where a second polyethylene fraction may be produced.

[0005] Titanocene hydrogenation catalysts have been used (1) in metallocene-catalyzed polymerization reactions to remove H2 generated by the metallocene polymerization catalyst, and (2) in one reactor of a coupled reactor system to remove H2 carried over from the previous reactor. However, these applications of titanocene catalysts to remove H2 are limited to gas-phase and slurry-phase polymerization reactions, where the reaction temperatures are typically in the range of 60°C to 120°C. Summary of the Invention

[0006] There is a continuing need to create catalyst systems or procatalysts that produce high molecular weight polymers at high polymerization temperatures (temperatures between 120° C. and 250° C.). Additionally, the catalyst system should have high efficiency, high reactivity, and the ability to produce polymers with high molecular weights (greater than 100,000 g / mol).

[0007] An embodiment of the present disclosure includes a catalyst system. The catalyst system includes a heterogeneous procatalyst and a hydrogenation procatalyst. The heterogeneous procatalyst includes a titanium species, an aluminum species, and a magnesium chloride component. The hydrogenation procatalyst has the formula Cp2TiX2. In the formula Cp2TiX2, each Cp is represented by at least one R 1 cyclopentadienyl substituted with R 1 But, (C1-C 10 ) alkyl and each X is independently a halogen atom.

[0008] The embodiments of the present disclosure include a pre-process of polymerizing. The polymerization process to produce a polyolefin polymer comprises the steps of: 12 ) an α-olefin. [Brief description of the drawings]

[0009] [Figure 1] 1 is a graph of gel permeation chromatography. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] An embodiment of the present disclosure includes a catalyst system. The catalyst system includes a heterogeneous procatalyst and a hydrogenation procatalyst. The heterogeneous procatalyst includes a titanium species, an aluminum species, and a magnesium chloride component. The hydrogenation procatalyst has the formula Cp2TiX2. In the formula Cp2TiX2, each Cp is represented by at least one R 1 cyclopentadienyl substituted with R 1 But, (C1-C 10 ) alkyl and each X is independently a halogen atom.

[0011] In embodiments of the catalyst system, the heterogeneous procatalyst comprises a titanium species. In some embodiments, the titanium species of the heterogeneous procatalyst may have catalytic activity. In some embodiments, the titanium species is TiCl 4-c (OR) c or TiCl 3-d (OR) d wherein R is selected from the group consisting of (C1-C 20 ) hydrocarbyl, where subscript c is 0, 1, 2, 3, or 4, and subscript d is 0, 1, 2, or 3. In some embodiments, the titanium species is, for example, titanium(IV) tetrachloride, titanium(III) trichloride, tris(2,2,6,6-tetramethyl-3,5-heptanedionato)titanium(III), trichlorotris(tetrahydrofuran)titanium(III), di-n-butoxytitanium(IV) dichloride, diethoxytitanium(IV) dichloride, diisopropoxytitanium(IV) dichloride, diisobutoxytitanium(IV) dichloride, triisopropoxytitanium(IV) chloride, tri-n-butoxytitanium(IV) chloride, triisobutoxytitanium(IV) chloride, titanium(IV) tetraisopropoxide (Ti(O i Titanium(IV) ethoxide, titanium(IV) n-butoxide, titanium(IV) isobutoxide, titanium(IV) 2-ethylhexoxide, dichlorobis(2,2,6,6-tetramethyl-3,5-heptanedionato)titanium(IV), tetrachlorobis(tetrahydrofuran)titanium(IV), methyltitanium(IV) trichloride, or combinations thereof. In some embodiments, the titanium species is titanium(IV) tetrachloride or titanium(IV) tetraisopropoxide (Ti(O i For example, in some embodiments, the titanium species can include titanium halides, titanium alkoxides, or combinations thereof. For example, in some embodiments, the titanium species can include titanium tetrachloride (TiCl4), titanium(IV) tetraisopropoxide (Ti(OPr)4). i Pr)4), other titanium halides, or titanium alkoxides, or combinations thereof.

[0012] In an embodiment of the catalyst system, the heterogeneous procatalyst comprises an aluminum species. In one or more embodiments, the aluminum species is selected from trialkylaluminum, dialkylaluminum chloride, alkylaluminum dichloride, alkylaluminum alkoxides, and alkylaluminoxanes.

[0013] In an embodiment of the catalyst system, the heterogeneous procatalyst comprises a magnesium chloride component. In one or more embodiments of the catalyst system, the magnesium chloride component of the heterogeneous catalyst comprises 100 ml of magnesium chloride as measured according to the BET method. 2 In some embodiments, the magnesium chloride component has a surface area of ​​150 m 2 / g or more, or 200m 2 In another embodiment, the magnesium chloride component has a surface area of ​​100 m 2 / g~800m 2 / g, or 200m 2 / g~600m 2 / g, or 300m 2 / g~500m 2 / g surface area.

[0014] In one or more embodiments, magnesium chloride comprises a high surface area that can be obtained from the chlorination of magnesium compounds. Such magnesium compounds include organomagnesium, organomagnesium halides, magnesium alkoxides, magnesium carbonate alkoxides, magnesium carboxylates, and combinations thereof. In embodiments, magnesium chloride can be obtained from the conversion of magnesium chloride adducts. Suitable magnesium chloride adducts include magnesium chloride adducts with alcohols and magnesium chloride adducts with ethers. In some embodiments, the magnesium chloride adduct is magnesium chloride adduct with ethanol. In some embodiments, the magnesium chloride adduct is magnesium chloride adduct with tetrahydrofuran.

[0015] In one or more embodiments, the magnesium chloride component includes, for example, the reaction product of a chloride source and a hydrocarbon soluble hydrocarbyl magnesium compound, or mixture of compounds. Exemplary organomagnesium compounds include di(C1-C 20 ) alkylmagnesium or di(C1-C 20 )arylmagnesium compounds, particularly di(n-butyl)magnesium, di(sec-butyl)magnesium, diisopropylmagnesium, di-n-hexylmagnesium, isopropyl-n-butyl-magnesium, ethyl-n-hexylmagnesium, ethyl-n-butylmagnesium, di-n-octylmagnesium, and combinations thereof. Exemplary suitable magnesium diaryls include diphenylmagnesium, dibenzylmagnesium, and ditolylmagnesium. The organomagnesium compounds may be optionally treated with organoaluminum compounds to improve solubility, reduce solution viscosity, or improve solubility and reduce solution viscosity. Stabilizers may also be present, such as those derived from substituted phenolic compounds. Additional suitable organomagnesium compounds include alkyl and arylmagnesium alkoxides, aryloxides, and chlorides, as well as mixtures of the foregoing. Highly preferred organomagnesium compounds are halogen-free organomagnesium compounds.

[0016] Chloride sources that may be used in the preparation of the magnesium chloride component of the heterogeneous procatalyst include metal and non-metal chlorides, including organic chlorides and hydrogen chloride. Examples of metal chlorides include MR y-a Cl a where M is a metal in Group 13, 14, or 15 of the Periodic Table of the Elements, R is a monovalent organic radical, and y has a value equal to the valence of M and has a value from 1 to y.

[0017] In various embodiments, the magnesium chloride component is made by chlorination of a solution of a hydrocarbon soluble magnesium precursor to obtain a MgCl2 slurry in the same hydrocarbon solvent used to make the magnesium precursor solution.

[0018] In one or more embodiments, the heterogeneous procatalyst can be prepared by first preparing a magnesium chloride component (MgCl2 component). The MgCl2 component can be prepared by selecting an organomagnesium compound or a complex containing an organomagnesium compound and reacting the organomagnesium compound with a chloride compound to make the MgCl2 component. Examples of organomagnesium compounds and / or organomagnesium complexes can include, but are not limited to, magnesium C2-C8 alkyls and aryls, magnesium alkoxides and aryloxides, carboxylated magnesium alkoxides, and carboxylated magnesium aryloxides, or combinations thereof. In some embodiments, the organomagnesium compound can include magnesium C2-C8 alkyls, magnesium C1-C4 alkoxides, or combinations thereof. In some embodiments, the organomagnesium compound can be butylethylmagnesium.

[0019] To prepare the magnesium chloride component, the organomagnesium compound may be dispersed in a hydrocarbon diluent. The concentration of the organomagnesium compound in the hydrocarbon diluent may be sufficient such that when the metal or nonmetal chloride compound and the organomagnesium compound are combined, the resulting slurry may contain a concentration of magnesium from 0.05 mol / L to 10.0 mol / L. The slurry of the organomagnesium compound dispersed in the hydrocarbon diluent may be contacted with a chloride compound to produce MgCl2. The chloride compound may be a metal or nonmetal chloride. For example, in some embodiments, the chloride compound may be hydrochloride gas. In some embodiments, the slurry of the organomagnesium compound and the chloride compound may be contacted at a temperature of -25°C to 100°C, or 0°C to 50°C. In some embodiments, the slurry of the organomagnesium compound and the metal or nonmetal chloride may be contacted for a time period of 1 hour to 12 hours, or 4 hours to 6 hours.

[0020] The reaction of a metal or non-metal chloride with an organomagnesium compound can produce a MgCl2 component, which can be a MgCl2 slurry including MgCl2 particles dispersed in a hydrocarbon diluent. In some embodiments, the MgCl2 slurry can have a concentration of MgCl2 between 0.05 mol / L and 10.0 mol / L, or between 0.2 mol / L and 1.0 mol / L, or between about 0.1 mol / L and 0.3 mol / L.

[0021] In an embodiment, the process for producing a heterogeneous procatalyst includes preparing a MgCl2 slurry in a hydrocarbon solvent. The process further includes mixing aluminum seeds with the MgCl2 slurry. The mixture of aluminum seeds and the MgCl2 slurry is heated, and then titanium seeds are added into the mixture of aluminum seeds and the MgCl2 slurry, which is heated and stirred, and then washed and placed in a hydrocarbon solvent to form a heterogeneous procatalyst.

[0022] In one or more embodiments, when preparing the magnesium chloride component or the heterogeneous procatalyst, the hydrocarbon solvent is a non-halogenated (C3-C 30 ) alkyl or non-halogenated (C3-C 30 ) cycloalkyl solvents. In some embodiments, the hydrocarbon solvent may include an isoparaffinic solvent. Examples of isoparaffinic solvents may include, but are not limited to, ISOPAR™ synthetic paraffinic solvents available from ExxonMobil (e.g., ISOPAR™ E paraffinic solvents), and special boiling point (SBP) solvents by Shell Chemicals (e.g., SBP 100 / 140 high purity dearomatized hydrocarbon solvents). Other examples of hydrocarbon solvents may include isobutene, pentane, isopentane, cyclopentane, hexane, 2-methylpentane, 3-methylpentane, cyclohexane, methylcyclopentane, heptane, 2-methylhexane, 3-methylhexane, octane, 2,2,4-trimethylpentane, tetradecane, and combinations thereof.

[0023] In one or more embodiments of the catalyst system, the heterogeneous procatalyst is an unsupported bulk catalyst. In some embodiments, the heterogeneous procatalyst comprises heterogeneous procatalyst particles having uncontrolled morphology.

[0024] In some embodiments of the catalyst system, the heterogeneous procatalyst comprises particles having an average particle size of 0.1 microns to 10 microns. In one or more embodiments, the average particle size is 8 microns or less, or 6 microns or less. In various embodiments, the heterogeneous procatalyst comprises heterogeneous procatalyst particles, where 10% or more of the particles have a particle size of 1 micron or less, as measured by light scattering. In some embodiments, 20% or more, 30% or more, or 40% or more of the particles have a particle size of 1 micron or less.

[0025] In an embodiment of the catalyst system, the hydrogenation procatalyst has the formula Cp2TiX2. In the formula Cp2TiX2, each Cp is represented by at least one R 1 cyclopentadienyl optionally substituted with 1 But, (C1-C 10 ) alkyl, each X is independently (C-C 40 ) Hydrocarbons, (C1-C 40 ) Heterohydrocarbons, (C1-C 40 ) hydrocarbyl, (C1-C 40 ) heterohydrocarbyl, or a halogen atom. In one or more embodiments, each Cp is at least one R selected from methyl, ethyl, propyl, 2-propyl, n-butyl, tert-butyl, iso-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, 2-ethylhexyl, tert-octyl, n-nonyl, or n-decyl. 1 In one or more embodiments, the hydrogenation procatalyst is selected from methylated Cp2TiCl2, butylated Cp2TiCl2, and ethylated Cp2TiCl2.

[0026] In one or more embodiments, the hydrogenation procatalyst is selected from bis(methylcyclopentadienyl)titanium chloride, bis(ethylcyclopentadienyl) chloride, bis(butylcyclopentadienyl)titanium chloride.

[0027] In embodiments of the catalyst system, each X is bonded to M through a covalent bond, a dative bond, or an ionic bond. In some embodiments, each X has an identity. The metal-ligand complex has six or fewer metal-ligand bonds and may be neutral in overall charge or may have a positive charge associated with the metal center. In some embodiments, the catalyst system comprises a metal-ligand complex according to the formula: 20 ) alkyl, (C1-C 20 )heteroalkyl, (C6-C 20 )Aryl, (C4-C 20 )heteroaryl, (C4-C 12 ) a diene, or a halogen. In one or more embodiments, each X is independently benzyl, phenyl, or chloro.

[0028] In some embodiments, the monodentate ligands can be monoanionic ligands. The monoanionic ligands have a net formal oxidation state of -1. Each monoanionic ligand can independently be a hydride, (C1-C 40 ) hydrocarbyl carbanion, (C1-C 40 ) Heterohydrocarbyl carbanions, halides, nitrates, carbonates, phosphates, sulfates, HC(O)O - , HC(O)N(H) - , (C1-C 40 ) Hydrocarbyl C(O)O - , (C1-C 40 ) HydrocarbylC(O)N((C1-C 20 )hydrocarbyl) - , (C1-C 40 ) Hydrocarbyl C(O)N(H) - , R K R L B - , RK R L N - , R K O - , R K S - , R K R L P - , or R M R K R L S - wherein each R K , R L , and R M are independently hydrogen, (C1-C 40 ) hydrocarbyl or (C1-C 40 ) heterohydrocarbyl, or R K and R L Together, (C2-C 40 ) hydrocarbylene or (C1-C 20 ) forms a heterohydrocarbylene, R M is as defined above.

[0029] In other embodiments, at least one monodentate ligand X, independently of any other ligand X, may be a neutral ligand. In certain embodiments, a neutral ligand is R Q NR K R L , R K OR L , R K S.R. L , or R Q PR K R L wherein each R Q are independently hydrogen, [(C1-C 10 )hydrocarbyl]3Si(C1-C 10 ) hydrocarbyl, (C1-C 40 ) hydrocarbyl, [(C1-C 10 )hydrocarbyl]3Si, or (C1-C 40 ) heterohydrocarbyl, each R K and R L are independently as defined above.

[0030] Additionally, each X may be, independently of any other ligand X, a halogen, unsubstituted (C 20 ) Hydrocarbyl, unsubstituted (C1-C 20 ) hydrocarbylC(O)O-, or R K R L R may be a monodentate ligand that is N- K and R L Each of is independently unsubstituted (C-C 20 In some embodiments, each monodentate ligand X is a chlorine atom, (C-C 10 ) hydrocarbyl (e.g., (C1-C6) alkyl or benzyl), unsubstituted (C1-C 10 ) hydrocarbylC(O)O-, or R K R L N- and R K and R L Each of is independently unsubstituted (C-C 10 ) hydrocarbyl. In one or more embodiments, X is benzyl, chloro, —CH2SiMe3, or phenyl.

[0031] In further embodiments, each X is selected from methyl, ethyl, 1-propyl, 2-propyl, 1-butyl, 2,2-dimethylpropyl, trimethylsilylmethyl, phenyl, benzyl, or chloro. In some embodiments, each X is the same. In some cases, at least two X are different from each other. In embodiments where at least two X are different from at least one X, X is different from methyl, ethyl, 1-propyl, 2-propyl, 1-butyl, 2,2-dimethylpropyl, trimethylsilylmethyl, phenyl, benzyl, and chloro. In further embodiments, the bidentate ligand is 2,2-dimethyl-2-silapropane-1,3-diyl or 1,3-butadiene.

[0032] In some embodiments, in the formula Cp2TiX2, each X is substituted benzyl or substituted heteroarylbenzyl. In other embodiments, X is selected from the group consisting of: [ka]

[0033] Cocatalyst Component In some embodiments, the catalyst system may further include a cocatalyst. A heterogeneous procatalyst according to the present disclosure may be combined with a cocatalyst to form a Ziegler-Natta catalyst. A Ziegler-Natta catalyst including a heterogeneous procatalyst may be made catalytically active by any technique known in the art for activating Ziegler-Natta type procatalysts for olefin polymerization reactions. In one example, but not intended to be limiting, a heterogeneous procatalyst may be made catalytically active by contacting the procatalyst with an activating cocatalyst or combining the procatalyst with an activating cocatalyst. Activating cocatalysts suitable for use herein include alkylaluminums including polymeric or oligomeric alumoxanes (also known as aluminoxanes). Combinations of one or more of the foregoing activating cocatalysts are also contemplated. The term "alkylaluminum" means monoalkylaluminum dihydrides or dihalides, dialkylaluminum hydrides or halides, or trialkylaluminums. Examples of polymeric or oligomeric alumoxanes include methylalumoxane, triisobutylaluminum modified methylalumoxane, and isobutylalumoxane. In some embodiments, the cocatalyst may be selected from aluminum alkyls, aluminum haloalkyls, alkylaluminum halides, and mixtures thereof. In some embodiments, the cocatalyst may be selected from triethylaluminum, trimethylaluminum, tri-n-butylaluminum, triisobutylaluminum, tri-n-hexylaluminum, tri-n-octylaluminum, diethylaluminum chloride, MAO, MMAO, diethylaluminum ethoxide, and mixtures thereof.

[0034] Preparation of the catalytic system In one or more embodiments, the catalyst system is prepared by mixing the heterogeneous procatalyst, the hydrogenation procatalyst, and optionally the cocatalyst in a hydrocarbon solvent. The catalyst system can then be used in a polymerization process.

[0035] In some embodiments, the catalyst system is prepared by feeding each of the heterogeneous procatalyst, the hydrogenation procatalyst, and the cocatalyst into a reactor via a separate feed line and mixing at least two of the heterogeneous procatalyst, the hydrogenation procatalyst, and the cocatalyst at ambient temperature for 0.5 minutes to 60 minutes before adding the third component to the reactor.

[0036] In other embodiments, the catalyst system is prepared by feeding each of the heterogeneous procatalyst, the hydrogenation procatalyst, and the cocatalyst into a reactor through separate feed lines and mixing the catalyst system at ambient temperature for 0.5 minutes to 60 minutes before adding the third component to the reactor.

[0037] Some embodiments of the present disclosure include a polymerization process for producing a polyolefin polymer comprising reacting one or more α-olefin monomers in solution in the presence of a catalyst system of the present disclosure, wherein the catalyst system comprises a heterogeneous procatalyst and a hydrogenation procatalyst as previously disclosed.

[0038] In one or more embodiments of the polymerization process, the one or more α-olefins are selected from the group consisting of (C2-C 12 In some embodiments, there is only a single type of olefin, ethylene, in the polymerization process. In some embodiments, there can be multiple (C-C 12 ) α-olefin monomers can be incorporated into the polymerization process. In various embodiments, (C2-C 12) The α-olefin monomers include, but are not limited to, ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, and 4-methyl-1-pentene. For example, the one or more α-olefin comonomers can be selected from the group consisting of propylene, 1-butene, 1-hexene, and 1-octene, or from the group consisting of 1-hexene and 1-octene.

[0039] In one or more embodiments of the polymerization process, (C2-C 12 ) The α-olefins react in a solution in a reactor at a reaction temperature of 150°C to 350°C.

[0040] Polymerization process embodiments include, but are not limited to, solution polymerization processes using one or more conventional reactors, such as loop reactors, isothermal reactors, stirred tank reactors, batch reactors, etc., in parallel, in series, or any combination thereof. In one embodiment, the polymerization process can include solution polymerization in a dual reactor system, such as a dual loop reactor system, where ethylene and optionally one or more α-olefins are polymerized in the presence of the catalyst system described herein, and optionally one or more cocatalysts. The catalyst system described herein, optionally in combination with one or more other catalysts, can be present in the first reactor or the second reactor. In one embodiment, the ethylene-based polymer can be produced by solution polymerization in a dual reactor system, such as a dual loop reactor system, where ethylene and optionally one or more α-olefins are polymerized in both reactors in the presence of the catalyst system described herein.

[0041] In another embodiment, the polymerization process can include solution polymerization in a single reactor system, for example a single loop reactor system or a single stirred tank reactor system, where ethylene, and optionally one or more α-olefins, are polymerized in the presence of a catalyst system as described within this disclosure, optionally in combination with one or more cocatalysts as described in the previous section, and optionally one or more other catalysts.

[0042] Test Method The specific surface area of ​​the MgCl2 support is measured by the Brunauer, Emmett, Teller (BET) surface area method. A Tristar 3020 surface area analyzer by Micromeritics is used. A 30 mL amount of the MgCl2 slurry is filtered to remove the solvent, then reslurried in 30 mL of hexane. The resulting slurry is filtered again under inert atmosphere and washed with additional hexane. This process is repeated once to obtain a filter cake of MgCl2. Residual solvent is removed from the filter cake under vacuum. The filter cake is further dried in a Vac Prep 061 by Micromeritics by placing a 0.2 g sample of the vacuum dried MgCl2 into a tube with a Transeal stopper under inert atmosphere, using a 0.5 inch (1.27 cm) sample tube and a Transeal stopper designed for inert sample protection. The sample tube is connected to the Vac Prep 061 unit with nitrogen purging. The sample tube is vacuumed by opening the Transeal stopper and the evacuated tube is placed in a heating block with an aluminum tube protector. The sample is dried at 110 °C for 3 h under vacuum in a Vac Prep 061 unit. Nitrogen is then introduced into the sample tube. The dried sample is cooled to room temperature and then the sample tube is removed from the Vac Prep 061 unit to obtain a completely dried sample. Under an inert atmosphere, 0.1500 g to 0.2000 g of the completely dried sample is transferred into a clean sample tube with a tube filler rod. The sample tube is then sealed with a Transeal stopper and connected to a Tristar 3020 instrument for surface area measurement. The QUICKSTART method is used for data acquisition.

[0043] Melt Index (MI) or I2 was determined in accordance with ASTM D1238-10, Condition 190° C. / 2.16 kg, Procedure B, and is reported in grams dissolved per 10 minutes (g / 10 min).

[0044] Samples for density measurements were prepared according to ASTM D 4703-10. Samples were pressed at 374°F (190°C) for 5 minutes at 10,000 psi (68 MPa). The temperature was held at 374°F (190°C) for 5 minutes and then the pressure was increased to 30,000 psi (207 MPa) for 3 minutes. This was followed by a 1 minute hold at 70°F (21°C) and 30,000 psi (207 MPa). Measurements were performed within 1 hour of sample compression using ASTM D792-08, Method B.

[0045] Magnesium chloride particle size was determined with a Malvern Mastersizer 3000 laser particle size analyzer. The Mastersizer 3000 is calibrated with a wet standard (D50=60 micron silica beads) run through a Hydro MV cell using Malvern's QAS3001B Quality Audit Standard (bottle part number CRM0016). The sample cell is cleaned prior to use by stirring 140 mL of isopropanol at 3500 RPM for 5 minutes, followed by reducing the stirring to 1000 RPM, decanting the isopropanol, and repeating twice. The sample cell is then charged with 140 mL of mineral oil in preparation to receive the sample. Samples are prepared in an inert atmosphere glove box by adding 0.12 mL of the 0.2 mol / L slurry into a pre-dried GC vial. Then, 0.75 mL of additional mineral oil is added to the GC vial, vortexed to mix, and the entire contents are then added to the sample cell of the dispersion unit. Light scattering is performed with the refractive index of MgCl2 (1.68) entered into the software. The instrument is initialized and the background is measured. Light scattering of the sample is then performed and the D10, D50, and D90 are reported by the software.

[0046] For gel permeation chromatography (GPC), the chromatography system consisted of a PolymerChar GPC-IR (Valencia, Spain) high temperature GPC chromatograph equipped with an internal IR5 infrared detector (IR5) coupled to a Precision Detectors (now Agilent Technologies) two-angle laser light scattering (LS) detector model 2040. The autosampler oven compartment was set at 160 degrees Celsius and the column compartment was set at 150 degrees Celsius. The columns used were four Agilent "Mixed A" 30 cm, 20 micron linear mixed bed columns. The chromatography solvent used was 1,2,4-trichlorobenzene containing 200 ppm butylated hydroxytoluene (BHT). The solvent source was nitrogen sparged. The injection volume used was 200 microliters and the flow rate was 1.0 milliliters / min.

[0047] Calibration of the GPC column set was performed with 21 narrow molecular weight distribution polystyrene standards with molecular weights ranging from 580 g / mol to 8,400,000 g / mol arranged in six "cocktail" mixtures with at least one decade between the individual molecular weights. Standards were purchased from Agilent Technologies. Polystyrene standards were prepared at 0.025 grams in 50 milliliters of solvent for molecular weights equal to or greater than 1,000,000 g / mol, and 0.05 grams in 50 milliliters of solvent for molecular weights less than 1,000,000 g / mol. The polystyrene standards were dissolved at 80 degrees Celsius for 30 minutes with gentle agitation. The polystyrene standard peak molecular weights were converted to polyethylene molecular weights using Equation 1 (described in Williams and Ward, J. Polym. Sci., Polym. Let., 6, 621 (1968)):

number

[0048] A fifth order polynomial was used to fit each polyethylene equivalent calibration point. A small adjustment (approximately 0.405-0.440) was made to A to correct for column resolution and band broadening effects, such as the NIST standard NBS 1475, obtained at 52,000 Mw.

[0049] Total plate counts of the GPC column set were performed with decane (prepared at 0.04 g in 50 mL TCB). Plate counts (Equation 2) and symmetry (Equation 3) were measured with a 200 μL injection according to the following equations:

number

number

[0050] Samples were prepared semi-automatically using the PolymerChar "Instrument Control" software to target sample weights of 2 mg / ml and add solvent (containing 200 ppm BHT) via the PolymerChar high temperature autosampler to septa-capped vials that had been pre-sparged with nitrogen. Samples were dissolved at 160 degrees Celsius with "slow" shaking for 2 hours.

[0051] Calculations of Mn, Mw, and Mz were based on GPC results using the internal IR5 detector (measurement channel) of the PolymerChar GPC-IR chromatograph according to Equations 4-6 using PolymerChar GPCOne™ software, baseline-subtracted IR chromatograms at each equally spaced data collection point (i), and polyethylene equivalent molecular weights obtained from a narrow standard calibration curve at point (i).

number

number

number

[0052] To monitor deviations over time, a flow marker (decane) was introduced into each sample via a micropump controlled by the PolymerChar GPC-IR system. This flow marker (FM) was used to linearly calibrate the pump flow rate (Flow (apparent)) of each sample by RV matching the respective decane peak in the sample (RV (FM sample)) with the decane peak in the narrow standard calibration (RV (FM calibrated)). Any change in time of the decane marker peak is thus assumed to be related to a linear shift in flow rate (Flow (effective)). To facilitate the highest accuracy of the RV measurement of the flow marker peak, a least squares fitting routine is used to fit the peaks of the flow marker concentration chromatogram to a quadratic equation. The first derivative of the quadratic equation is then used to determine the true peak position. After calibrating the system based on the flow marker peaks, the effective flow rate (relative to the narrow standard calibration) is calculated as in Equation 7. Processing of the flow marker peaks was performed by PolymerChar GPCOne™ software. An acceptable flow correction is that the effective flow rate should be within + / - 2% of the apparent flow rate. Flow Rate (effective) = Flow Rate (nominal) * (RV(FM calibrated) / RV(FM sample)) (Equation 7)

[0053] Solution batch reactor copolymerization test method.

[0054] A batch reactor is charged with 250 g of 1-octene and 1330 g of Isopar E. The reactor contents are heated to 190° C. and then the contents are saturated with ethylene in the presence of a specified amount of molecular hydrogen (H2). A suspension of procatalyst (e.g., PCAT in liquid (e.g., (C1)), cocatalyst triethylaluminum (TEA), and alkylating Cp2TiCl2 solution (e.g., E1 or E2) are mixed in a separate flask as needed, and the resulting mixture is immediately added to the batch reactor. The pressure in the reactor is maintained at 3100 kilopascals (kPa, equal to 450 pounds per square inch (psi)) with ethylene flow to compensate for the pressure drop due to ethylene consumption during the polymerization. After a reaction time of 10 minutes, the bottom valve is attached and the reactor contents are transferred to a glass kettle. The kettle contents are poured onto a Mylar-lined tray and allowed to cool. The contents are placed on the tray in a fume hood overnight to allow most of the liquid to evaporate. The remaining resin is dried in a vacuum oven to obtain the product poly(ethylene-co-1-octene) copolymer.

[0055] Continuous solution reactor copolymerization test method.

[0056] The continuous solution polymerization process included an adiabatic continuous stirred tank reactor (CSTR). The reactor contained independent control of all solvent, monomer, comonomer, hydrogen, and catalyst system component feeds. The total feed stream to the reactor, including solvent, monomer, comonomer, and hydrogen, was temperature controlled by sending the total feed stream through a heat exchanger prior to introducing the total feed stream into the reactor. The total feed stream to the reactor was injected into the reactor at one point. The catalyst system components were injected into the reactor separately from the other feeds. An agitator within the reactor was used to continuously mix the reactants. An oil bath provided additional fine adjustment of the reactor temperature control.

[0057] Ethylene monomer, 1-octene comonomer, and process solvent (SBP 100 / 140 by Shell Chemicals) are purified with molecular sieves before being introduced into the reactor. The monomer, solvent, and comonomer feed streams are pressurized through to a pressure higher than the reaction pressure. The monomer, comonomer, solvent, and hydrogen streams are combined and then introduced into the reactor. The individual components of the catalyst system are manually diluted batchwise with purified solvent / diluent and pressurized to a pressure higher than the reaction pressure. The feed lines for the procatalyst (PCAT), cocatalyst, and alkylated Cp2TiCl2 hydrogenation procatalyst (if used) are combined into a single line and the components are mixed together for approximately 2 minutes before entering the reactor. All reaction feed streams are measured with mass flow meters and independently controlled with metering pumps.

[0058] The final reactor effluent is sent to a zone where the catalyst system is deactivated by addition and reaction with water. Following catalyst deactivation, the reactor effluent is sent to a two-stage devolatilization system where the ethylene-based polymer is removed from the non-polymer stream (e.g., excess monomer or comonomer, solvent, etc.). The non-polymer stream is removed from the system and the isolated polymer melt is pelletized and collected. EXAMPLES

[0059] The following examples are provided to illustrate the embodiments described in this disclosure and are not intended to limit the scope of the disclosure or its appended claims.

[0060] Preparation of procatalyst Compound (C1). Isopar E fluid obtained from ExxonMobil Corporation and containing >99.75% to 99.9% by weight naphtha (petroleum), light alkylate, CAS 64741-66-8, and 0.1% to less than 0.25% by weight isooctane CAS 540-54-1 (isoalkane mixture) having a boiling range of 114° C. to 139° C.

[0061] Fine particle MgCl2(D1). 375m 2 / g~425m2 Solid particulate MgCl2 having a BET surface area of ​​1.00 g / g. The product was prepared by diluting a 20 wt% solution of butylethylmagnesium in heptane with a measured amount of (C1) to obtain a dilute solution, and slowly adding hydrogen chloride (HCl) to the dilute solution with stirring at 30°C while maintaining a temperature of 30±3°C until a molar ratio of Cl to Mg of 2.04:1.00 was reached to obtain a 0.20 mol / L suspension of (D1) in (C1).

[0062] Preparation of Heterogeneous Procatalysts ("PCATs") A 15 wt% solution of ethylaluminum dichloride (EADC) in heptane is slowly added to the above MgCl2 particulate slurry (D1) while stirring at 30°C until the EADC / Mg ratio reaches 0.3. The temperature of the reaction mixture is maintained at 30°C ± 3°C during the addition. The mixture is aged at 30°C for 4 hours. Then, a 51 wt% solution of (IV) isopropoxide in heptane is slowly added to the mixture while stirring at 30°C until the Ti / Mg ratio reaches 0.075. The temperature of the reaction mixture is maintained at 30°C ± 3°C during the addition. The mixture is aged at 30°C for at least 8 hours. Isopar E solvent (C1) is used for rinsing to ensure accuracy of the catalyst dosage. The final Ti concentration for the finished catalyst is 0.12 mol / L.

[0063] Preparation of hydrogenation procatalyst Example 1: Bis(ethylcyclopentadienyl)titanium chloride (E1). In a 2 oz bottle, place 1.000 g of Cp2TiCl2 and a stir bar. 20.1 mL of a 1.0 mol / L triethylaluminum (TEA) solution in heptane is added slowly over approximately 10 minutes with stirring. The solid Cp2TiCl2 becomes soluble and forms a blue solution.

[0064] Example 2: Bis(butylcyclopentadienyl)titanium chloride (E2). In a 4 oz bottle, place 0.544 g Cp2TiCl2, 4.0 mL Isopar E, and a stir bar. 38.0 mL of a 1.0 M solution of triisobutylaluminum (TiBAl) in hexanes is added slowly over approximately 10 minutes with stirring. The solid Cp2TiCl2 becomes soluble and forms a blue solution.

[0065] Example 3: Bis(ethylcyclopentadienyl)titanium chloride (E3). In a 1 liter bottle, place 50.00 g of Cp2TiCl2 and a stir bar. Add 880 mL of a 1.0 M solution of triethylaluminum (TEA) in heptane over approximately 10 minutes with stirring. The solid Cp2TiCl2 becomes soluble and forms a blue solution.

[0066] Polymerizations of ethylene with one or more α-olefins, such as 1-octene, were carried out in the presence of various amounts of H2 to establish the relationships between (1) the weight average molecular weight (Mw) and H2 content of the polymers, (2) Mw / Mn and Mw, and (3) Mz / Mw and Mw, and the characteristics of the resulting polymer and catalyst systems are recorded in Tables 1-4. [Table 1]

[0067] As recorded in Table 1, molecular weight, molecular weight distribution, and Mz / Mw all increased for the polymers produced in the systems containing the comparative catalyst as the amount of hydrogen was decreased. [Table 2]

[0068] Ethylene polymerization reactions were carried out in the presence of a butylated Cp2TiCl2 hydrogenation procatalyst (E2) in the presence of 40 mmol of H2. The data in Table 2 show that a substantial portion of the H2 can be consumed by the hydrogenation catalyst. The amount of H2 consumed is evident from the weight average molecular weight of the polymer produced. For example, the catalyst system in run IE3 included a hydrogenation procatalyst having a 3:1 molar ratio of Cp2TiCl2 / Ti in the presence of 40 mmol of H2, and the weight average molecular weight of the polymer produced is 179,154 g / mol. With 40 mmol of H2 in the reactor system, the catalyst system in run IE3 produced a polymer with a weight average molecular weight approximately 70,000 g / mol greater than the weight average molecular weight of the polymer produced in run CE5 (Table 1) by the comparative catalyst system in the presence of 40 mmol of H2.

[0069] The comparative catalyst system lacked a hydrogenation procatalyst. As the amount of H2 increased, the weight average molecular weight decreased. In contrast, in the examples of Tables 2 and 3, in the presence of 40 mmol of H2, as the amount of hydrogenation procatalyst increased, the weight average molecular weight of the polymer produced increased. This trend supports the assertion that a substantial portion of the H2 can be consumed by the hydrogenation catalyst. Furthermore, as the weight average molecular weight of the polymer increased, the molecular weight distribution increased slightly, although the degree of increase was significantly less than that observed without the hydrogenation procatalyst (Table 1). [Table 3]

[0070] Ethylene polymerization reactions were carried out in the presence of 40 mmol of H2 and ethylated Cp2TiCl2 hydrogenation procatalyst (E1). The data in Table 3 also show that a substantial portion of H2 can be consumed by the hydrogenation catalyst. In particular, by adding a constant amount of H2, the weight average molecular weight of the polymer also generally increased as the ratio of hydrogenation procatalyst to titanium catalyst increased from 1:1 to 4:1. The increase in the weight average molecular weight of the polymer is evidence of hydrogen consumption by the hydrogenation catalyst, since the presence of H2 can terminate the polymer chains. [Table 4]

[0071] In a continuous reaction process, the catalyst system of run IE9, which contained both hydrogenation procatalyst E3 and a heterogeneous catalyst, produced polymers with molecular weights nearly 30% higher than the molecular weight of the polymers produced by the catalyst system without a hydrogenation catalyst. As shown in the figure, the polymers produced by the catalyst system containing hydrogenation procatalyst E3 and a heterogeneous catalyst had comparable molecular weight distributions and Mz / Mw values ​​lower than the corresponding values ​​for the polymers produced by the comparative catalyst system in run CE6. The hydrogenation procatalyst, E3, can be built to a specific region of molecular weight (near Mw) without affecting the distribution (or Mn or Mz). The present invention includes the following aspects. Section 1. 1. A catalyst system comprising: a heterogeneous procatalyst comprising a titanium species, an aluminum species, and a magnesium chloride component; Formula Cp2TiX2TiCp2 or Cp2TiX n and a hydrogenation procatalyst having During the ceremony, Each Cp has at least one (C1-C 10 ) cyclopentadienyl substituted with alkyl; Each X is independently monoanionic or neutral, and each X is independently selected from the group consisting of (C1-C 40 ) Hydrocarbons, (C1-C 40 ) Heterohydrocarbons, (C1-C 40 ) hydrocarbyl, (C1-C 40 ) heterohydrocarbyl, or a halogen atom; A catalyst system wherein n is 1 or 2. Section 2. Item 2. The catalyst system according to item 1, wherein the heterogeneous catalyst is an unsupported bulk catalyst. Section 3. 3. The catalyst system according to claim 1 or 2, wherein the heterogeneous procatalyst comprises heterogeneous procatalyst particles having an average particle size of 0.1 microns to 10 microns. Section 4. 4. The catalyst system according to any one of items 1 to 3, wherein the heterogeneous procatalyst comprises heterogeneous procatalyst particles having an uncontrolled morphology. Section 5. 5. The catalyst system according to any one of items 1 to 4, wherein the heterogeneous procatalyst comprises heterogeneous procatalyst particles, and 10% or more of the heterogeneous procatalyst particles have a particle size of 1 micron or less. Section 6. 6. The catalyst system according to any one of items 1 to 5, wherein the ratio of moles of titanium in the hydrogenation procatalyst to moles of titanium in the heterogeneous procatalyst is greater than 1:2. Section 7. Alkyl aluminum cocatalyst Al(R 2 )3, wherein each R 2 But independently, (C1-C 20 ) alkyl or halogen atom, provided that at least one R 2 (C1-C 20 ) alkyl. The catalyst system according to any one of items 1 to 6. Section 8. Item 7. The catalyst system according to any one of items 1 to 6, further comprising an alkylaluminum cocatalyst selected from the group consisting of trialkylaluminum compounds, dialkylaluminum chlorides, alkylaluminum dichlorides, alkylaluminum alkoxides, and alkylaluminoxanes. Section 9. Catalyst system item 7 or 8, wherein the ratio of moles of titanium in said heterogeneous procatalyst to moles of aluminum in said cocatalyst is greater than 2:1. Section 10. Item 9. The catalyst system according to item 7 or 8, wherein the ratio of moles of titanium in the heterogeneous procatalyst to moles of aluminum in the cocatalyst is 1000:1 to 2:1. Section 11. 1. A polymerization process comprising: In the presence of a catalytic system, (C2-C 12 ) reacting an α-olefin with a catalyst system comprising: a heterogeneous procatalyst comprising a titanium species, an aluminum species, and a magnesium chloride component; Formula Cp2TiX n TiCp2 or Cp2TiX n and a hydrogenation procatalyst having During the ceremony, Each Cp has at least one (C1-C 10 ) cyclopentadienyl substituted with alkyl; Each X is independently monoanionic or neutral, and each X is independently selected from the group consisting of (C1-C 40 ) Hydrocarbons, (C1-C 40 ) Heterohydrocarbons, (C1-C 40 ) hydrocarbyl, (C1-C 40 ) heterohydrocarbyl, or a halogen atom; The polymerization process wherein n is 1 or 2. Section 12. The catalyst system comprises a trialkylaluminum cocatalyst Al(R 2 )3, wherein each R 2 But independently, (C1-C 20 Item 12. The polymerization process according to item 11, wherein the alkyl is aryl. Section 13. Item 13. The polymerization process according to item 11 or 12, wherein the heterogeneous catalyst is a bulk catalyst. Section 14. Item 14. The polymerization process of any one of items 11 to 13, wherein the heterogeneous procatalyst comprises heterogeneous procatalyst particles, and 10% or more of the particles have a particle size of 1 micron or less. Section 15. Item 15. The polymerization process of any one of items 11 to 14, wherein the heterogeneous catalyst comprises heterogeneous procatalyst particles having an uncontrolled particle morphology. Section 16. (C2-C 12 16. The polymerization process according to any one of items 11 to 15, wherein the α-olefin is reacted in a reactor at a reaction temperature of 150°C to 350°C.

Claims

1. 1. A catalyst system comprising: a heterogeneous procatalyst comprising a titanium species, an aluminum species, and a magnesium chloride component, said titanium species represented by TiCl 4-c (OR) c or TiCl 3-d (OR) d , R is a (C 1 -C 20 )hydrocarbyl, subscript c is 0, 1, 2, 3 or 4, and subscript d is 0, 1, 2 or 3, said heterogeneous procatalyst comprising heterogeneous procatalyst particles having an average particle size of from 0.1 microns to 10 microns; Formula Cp 2 TIX 2 TiCp 2 Or Cp 2 TIX n and a hydrogenation procatalyst having During the ceremony, Each Cp is at least one (C 1 -C 10 ) cyclopentadienyl substituted with alkyl; Each X is independently monoanionic or neutral, and each X is independently selected from the group consisting of: 1 -C 40 ) Hydrocarbons, (C 1 -C 40 ) heterohydrocarbons, (C 1 -C 40 ) hydrocarbyl, (C 1 -C 40 ) heterohydrocarbyl, or a halogen atom; A catalyst system wherein n is 1 or 2.

2. The catalyst system of claim 1, wherein the heterogeneous procatalyst is an unsupported bulk catalyst.

3. 10. The catalyst system of claim 1, wherein the heterogeneous procatalyst comprises heterogeneous procatalyst particles having uncontrolled particle morphology.

4. 10. The catalyst system of claim 1, wherein said heterogeneous procatalyst comprises heterogeneous procatalyst particles, and at least 10% of said heterogeneous procatalyst particles have a particle size of 1 micron or less.

5. 10. The catalyst system of claim 1, wherein the ratio of moles of titanium in said hydrogenation procatalyst to the moles of titanium in said heterogeneous procatalyst is greater than 1:

2.

6. Alkyl aluminum cocatalyst Al(R 2 ) 3 wherein each R 2 But independently, (C 1 -C 20 ) an alkyl or halogen atom, provided that at least one R 2 But (C 1 -C 20 2. The catalyst system of claim 1, provided that:

7. 10. The catalyst system of claim 1 further comprising an alkylaluminum cocatalyst selected from the group consisting of trialkylaluminum compounds, dialkylaluminum chlorides, alkylaluminum dichlorides, alkylaluminum alkoxides, and alkylaluminoxanes.

8. 7. The catalyst system of claim 6, wherein the ratio of moles of titanium in said heterogeneous procatalyst to moles of aluminum in said cocatalyst is greater than 2:

1.

9. 7. The catalyst system of claim 6, wherein the ratio of moles of titanium in said heterogeneous procatalyst to moles of aluminum in said cocatalyst is from 1000:1 to 2:

1.

10. 1. A polymerization process comprising: In a reactor at a reaction temperature of 150° C. to 350° C., in the presence of a catalyst system, (C 2 -C 12 ) reacting an α-olefin with a catalyst system comprising: a heterogeneous procatalyst comprising a titanium species, an aluminum species, and a magnesium chloride component, said titanium species represented by TiCl 4-c (OR) c or TiCl 3-d (OR) d , R is a (C 1 -C 20 )hydrocarbyl, subscript c is 0, 1, 2, 3 or 4, and subscript d is 0, 1, 2 or 3, said heterogeneous procatalyst comprising heterogeneous procatalyst particles having an average particle size of from 0.1 microns to 10 microns; Formula Cp 2 TIX n TiCp 2 Or Cp 2 TIX n and a hydrogenation procatalyst having During the ceremony, Each Cp is at least one (C 1 -C 10 ) cyclopentadienyl substituted with alkyl; Each X is independently monoanionic or neutral, and each X is independently selected from the group consisting of: 1 -C 40 ) Hydrocarbons, (C 1 -C 40 ) heterohydrocarbons, (C 1 -C 40 ) hydrocarbyl, (C 1 -C 40 ) heterohydrocarbyl, or a halogen atom; The polymerization process wherein n is 1 or 2.

11. The catalyst system comprises a trialkylaluminum cocatalyst Al(R 2 ) 3 wherein each R 2 But independently, (C 1 -C 20 11. The polymerization process of claim 10, wherein:

12. The polymerization process of claim 10, wherein the heterogeneous procatalyst is a bulk catalyst.

13. 11. The polymerization process of claim 10, wherein the heterogeneous procatalyst comprises heterogeneous procatalyst particles, with 10% or more of the particles having a particle size of 1 micron or less.

14. 11. The polymerization process of claim 10, wherein the heterogeneous procatalyst comprises heterogeneous procatalyst particles having uncontrolled particle morphology.

Citation Information

Patent Citations

  • Novel catalyst and method for producing olefin polymer having relatively narrow molecular weight distribution

    JP1986287909A

  • Method for producing propylene single polymer or propylene random copolymer

    JP2010275382A