Sulfide-based inorganic solid electrolyte material, solid electrolyte, solid electrolyte membrane and lithium-ion battery
By optimizing the composition and incorporating a glass structure in sulfide-based inorganic solid electrolytes, the ionic conductivity is enhanced, addressing the limitations of conventional materials and improving battery performance.
Patent Information
- Application Number
- JP2022565226
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-11-30
- Filing Date
- 2021-11-12
- Publication Date
- 2024-12-09
- Estimated Expiration
- 2041-11-12
AI Technical Summary
Conventional sulfide-based inorganic solid electrolyte materials exhibit room for improvement in terms of ionic conductivity, which is crucial for enhancing the performance of all-solid-state lithium-ion batteries.
A sulfide-based inorganic solid electrolyte material is developed with a specific composition and manufacturing process that includes adjusting the raw material ratios and incorporating a glass structure to enhance ionic conductivity, as indicated by the sum of peak areas derived from P-NMR measurements exceeding a certain threshold.
The material achieves high ionic conductivity, suitable for use in lithium-ion batteries, particularly in all-solid-state configurations, improving safety and manufacturing efficiency.
Smart Images

Figure 0007596404000004 
Figure 0007596404000005 
Figure 0007596404000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a sulfide-based inorganic solid electrolyte material, a solid electrolyte, a solid electrolyte membrane, and a lithium ion battery. [Background technology]
[0002] Lithium-ion batteries are generally used as power sources for small portable devices such as mobile phones and laptops, etc. Recently, lithium-ion batteries have also begun to be used as power sources for electric vehicles, power storage, and other devices in addition to small portable devices.
[0003] Currently available lithium-ion batteries use electrolytes that contain flammable organic solvents. Meanwhile, research is underway into lithium-ion batteries that have been made all-solid by replacing the electrolyte with a solid electrolyte (hereinafter referred to as all-solid-state lithium-ion batteries).Since all-solid-state lithium-ion batteries do not contain flammable organic solvents, safety devices can be simplified and they are thought to have excellent manufacturing costs and productivity. As a solid electrolyte material used for the solid electrolyte, for example, a sulfide-based inorganic solid electrolyte material is known.
[0004] Specific prior art for solid electrolyte materials include Patent Documents 1 and 2, 31 Inorganic solid electrolyte materials that focus on the spectra obtained by P-NMR measurements are known.
[0005] Patent Document 1 describes a solid electrolyte that satisfies all of the following requirements: -Contains lithium, phosphorus and sulfur as components. The following formula (A) is satisfied. Li a P c S d X e (A) [In formula (A), a to e represent the composition ratio of each element, and a:c:d:e satisfies 1-9:1:3-7:0-9. X is I.] ·31 In P-NMR, it has a peak (first peak) in the region of 83.0 ppm or more and 88.0 ppm or less, and has no peaks outside the region of 83.0 ppm or more and 88.0 ppm or less, or if it has a peak, the peak intensity ratio to the first peak is 0.5 or less. Ionic conductivity is 5×10 -4 S / cm or more. When 0.1 g of solid electrolyte is placed in a 100 ml container and air with a humidity of 80-90% is passed through the container at a rate of 500 ml / min for 60 minutes, the average concentration of hydrogen sulfide in the air is 200 ppm or less.
[0006] Patent Document 2 describes a sulfide solid electrolyte material containing phosphorus and sulfur. 31 In a spectrum obtained by P-NMR measurement, a peak appearing within the range of 87.5 ppm to 88.5 ppm is defined as a first peak, and a peak appearing within the range of 84.2 ppm to 85.2 ppm is defined as a second peak in the same spectrum. When the ratio of the integrated intensity of the first peak to the integrated intensity of the second peak is expressed as x:1-x, 0.00926≦x≦0.37 is satisfied. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Patent No. 6077740 [Patent Document 2] JP 2019-3927 A Summary of the Invention [Problem to be solved by the invention]
[0008] One of the performance requirements for solid electrolyte materials is high ionic conductivity. According to the findings of the present inventors, there is room for improvement in terms of ion conductivity in conventional sulfide-based inorganic solid electrolyte particles.
[0009] The present invention has been made in view of the above circumstances. One of the objects of the present invention is to provide sulfide-based inorganic solid electrolyte particles having high ionic conductivity. [Means for solving the problem]
[0010] The present inventors have completed the invention provided below and have solved the above problems.
[0011] According to the present invention, A sulfide-based inorganic solid electrolyte material containing Li, P and S as constituent elements, 31 A sulfide-based inorganic solid electrolyte material in which, when the sum of the areas of the peaks derived from the PS4 structure in a spectrum obtained by P-NMR measurement is taken as 1, the sum of the areas of the peaks derived from the P2S6 glass structure is 0.1 or more. is provided.
[0012] Further, according to the present invention, A solid electrolyte comprising the above sulfide-based inorganic solid electrolyte material is provided.
[0013] Further, according to the present invention, A solid electrolyte membrane containing the above solid electrolyte as a main component is provided.
[0014] Further, according to the present invention, A lithium ion battery comprising a positive electrode including a positive electrode active material layer, an electrolyte layer, and a negative electrode including a negative electrode active material layer, A lithium ion battery in which at least one of the positive electrode active material layer, the electrolyte layer, and the negative electrode active material layer contains the inorganic solid electrolyte material described above. is provided. Effect of the Invention
[0015] According to the present invention, there are provided sulfide-based inorganic solid electrolyte particles having high ionic conductivity. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is a cross-sectional view showing an example of the structure of a lithium ion battery. [Diagram 2] 3 is a 31P-NMR spectrum of the sulfide-based inorganic solid electrolyte material of Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. The drawings are for illustrative purposes only. The shapes and dimensional ratios of the components in the drawings do not necessarily correspond to the actual products.
[0018] In this specification, unless otherwise specified, the expression "X to Y" in the explanation of a numerical range means from X to Y. For example, "1 to 5% by mass" means "from 1% by mass to 5% by mass."
[0019] In the description of groups (atomic groups) in this specification, when a description is made without specifying whether the group is substituted or unsubstituted, the description includes both groups having no substituents and groups having a substituent. For example, an "alkyl group" includes not only an alkyl group having no substituents (unsubstituted alkyl group) but also an alkyl group having a substituent (substituted alkyl group). In this specification, the term "(meth)acrylic" refers to a concept that includes both acrylic and methacrylic. The same applies to similar terms such as "(meth)acrylate."
[0020] <Sulfide-based inorganic solid electrolyte materials> The sulfide-based inorganic solid electrolyte material of this embodiment contains Li, P and S as constituent elements. The sulfide-based inorganic solid electrolyte material of this embodiment 31 In the spectrum obtained by P-NMR measurement, when the sum of the areas of the peaks derived from the PS4 structure is set to 1, the sum of the areas of the peaks derived from the P2S6 glass structure is 0.1 or more.
[0021] The present inventors have investigated the improvement of the ionic conductivity of sulfide-based inorganic solid electrolyte materials from various viewpoints. As a result, 31 It was found that the area of the peak derived from the P2S6 glass structure in the spectrum obtained by P-NMR measurement seems to correlate with the ionic conductivity. Based on this finding, the inventors conducted further research and found that ionic conductivity is improved when the area of the peak derived from the P2S6 glass structure is relatively large when the sum of the areas of the peaks derived from the PS4 structure is used as the standard. Therefore, the inventors have devised a method for producing a soluble cellulose acetate by devising a raw material composition and a manufacturing method. 31 We have created a new sulfide-based inorganic solid electrolyte material in which the sum of the areas of the peaks derived from the P2S6 glass structure is equal to or greater than 0.1 when the sum of the areas of the peaks derived from the PS4 structure in the spectrum obtained by P-NMR measurement is set to 1. We have also been able to increase the ionic conductivity. ("PS4 Structure" includes both PS4 Crystal Structure and PS4 Glass Structure.)
[0022] The reason why the sulfide-based inorganic solid electrolyte material of the present embodiment exhibits good ion conductivity can be explained as follows. Just to be clear, the following explanation includes speculation, and the present invention is not limited by the following explanation.
[0023] Theoretically, since the ionic conductivity of a crystalline structure is higher than that of a glassy structure, it would seem that the ionic conductivity would be improved if the sulfide-based inorganic solid electrolyte material were entirely made of crystalline structures. However, in real systems, the movement of Li ions is suppressed at the interfaces between the crystalline structures due to lattice mismatch. In order to suppress the decrease in ionic conductivity due to this "lattice mismatch," it is considered effective to fill the "gaps" between the crystal structures with a glass structure. In this embodiment, "the sum of the areas of the peaks derived from the P2S6 glass structure is 0.1 or more" is considered to represent the presence of a sufficient amount of P2S6 glass between the crystal structures to increase the mobility of Li ions.
[0024] As a supplementary note, the "peak area due to PS4 structure" and "peak area due to P2S6 glass structure" are 31 It is obtained by "waveform separation" of the NMR spectrum obtained by P-NMR measurement using a Gaussian function. Waveform separation can be performed, for example, using commercially available software that can curve fit various types of spectral data. Software capable of curve fitting includes software that comes with the NMR instrument and software that is sold separately from the NMR instrument. An example of the former is ALICE2 by JOEL. Also, well-known software for the latter include OriginPro and IgorPro. In Patent Document 1, 31 There is no mention of analyzing the P-NMR spectrum by waveform separation. 31 No mention is made of the area of the peaks in the P-NMR spectrum attributable to the P2S6 glass structure. 31 The inventors' original idea was to perform waveform separation on the P-NMR spectrum and then to "precisely" examine it, and then to focus on the area of the peak derived from the P2S6 glass structure relative to the area of the peak derived from the PS4 structure.
[0025] In this embodiment, the values in the table below (unit: ppm) can be used as the chemical shifts of each chemical species. That is, when the obtained NMR spectrum is separated into peaks corresponding to each chemical species, it is preferable to use a Gaussian function that shows a maximum value within the numerical range shown in the table below.
[0026] [Table 1]
[0027] The sulfide-based inorganic solid electrolyte material of the present embodiment can be obtained by using appropriate raw materials and an appropriate manufacturing method. Although preferred materials and manufacturing methods will be described in detail later, for example, (i) P2S5 having a P content greater than 27.87 mass% defined by stoichiometry is used as a raw material, (ii) the composition of the final sulfide-based inorganic solid electrolyte material is Li 10 P3S 12 or (iii) adjusting the molar ratio of each raw material so that it is close to this range, (iii) performing an appropriate annealing treatment, etc. By paying attention to these points, it is easy to produce the sulfide-based inorganic solid electrolyte material of this embodiment.
[0028] The sulfide-based inorganic solid electrolyte material of this embodiment will be described further.
[0029] (About NMR spectrum) As mentioned earlier, 31 When the sum of the areas of the peaks originating from the PS4 structure (both the PS4 crystal structure and the PS4 glass structure) in the P-NMR spectrum is taken as 1, the sum of the areas of the peaks originating from the P2S6 glass structure is 0.1 or more. This value is preferably 0.15 or more, more preferably 0.25 or more. The upper limit of this value is, for example, 2.0 or less, preferably 1.0 or less. Having this value appropriate is considered to mean that an appropriate amount of P2S6 glass is present in the "gaps" between the crystal structures. In other words, by appropriately adjusting this value, the ionic conductivity can be further increased.
[0030] 31In the P-NMR spectrum, when the sum of the peak areas derived from the PS4 glass structure is taken as 1, the sum of the peak areas derived from the P2S6 glass structure is preferably 0.15 or more, more preferably 0.25 or more. The upper limit of this value is, for example, 3.0 or less, preferably 1.0 or less. Although the details are unclear, it is presumed that the sulfide-based inorganic solid electrolyte material contains both the P2S6 glass structure and the PS4 glass structure as glass structures, and the ratio of these glass structures is appropriate, so that various types of lattice mismatches between crystal structures can be filled by the glass structure. As a result, it is considered that there are cases where the ion conductivity can be further improved.
[0031] 31 In the P-NMR spectrum, when the sum of the peak areas due to the PS4 glass structure is taken as 1, the sum of the peak areas due to the PS4 crystal structure is preferably 0.3 to 1, and more preferably 0.3 to 0.5. As mentioned above, it is believed that the mobility of Li ions is enhanced by the presence of a moderate amount of glass structure between the crystal structures. The fact that this value is 0.3 to 1 is presumed to indicate that a moderate amount of glass structure exists between the crystal structures in the composition of PS4.
[0032] 31 In the P-NMR spectrum, when the sum of the areas of the peaks derived from the PS4 structure is taken as 1, the sum of the areas of the peaks derived from the P2S7 glass structure is usually 0.05 to 0.25, and preferably 0.05 to 0.2. 31 In the P-NMR spectrum, when the sum of the areas of the peaks derived from the PS4 structure is taken as 1, the sum of the areas of the peaks derived from the P2S7 crystal structure is usually 0.05 to 0.25, and preferably 0.05 to 0.2. 31 In the P-NMR spectrum, when the sum of the areas of the peaks derived from the PS4 structure is taken as 1, the sum of the areas of the peaks derived from the P2S6 crystal structure is usually 0.005 to 0.02, and preferably 0.01 to 0.1.
[0033] 31In the P-NMR spectrum, when the sum of the areas of the peaks derived from the PS4 glass structure is taken as 1, the sum of the areas of the peaks derived from the P2S7 glass structure is usually 0.05 to 0.3, and preferably 0.08 to 0.25. 31 In the P-NMR spectrum, when the sum of the areas of the peaks derived from the PS4 glass structure is taken as 1, the sum of the areas of the peaks derived from the P2S7 crystal structure is usually 0.05 to 0.3, and preferably 0.08 to 0.25. 31 In the P-NMR spectrum, when the sum of the areas of the peaks derived from the PS4 glass structure is taken as 1, the sum of the areas of the peaks derived from the P2S6 crystal structure is usually 0.01 to 0.2, preferably 0.01 to 0.15, and more preferably 0.01 to 0.1.
[0034] By appropriately adjusting each peak area, the ionic conductivity can be increased in some cases.
[0035] (Constituent elements and their composition) The sulfide-based inorganic solid electrolyte material of this embodiment contains Li, P and S as constituent elements from the viewpoints of electrochemical stability, stability in moisture and air, ease of handling, and the like. In addition, from the viewpoint of further improving the lithium ion conductivity, electrochemical stability, stability in moisture and air, ease of handling, and the like, the sulfide-based inorganic solid electrolyte material of this embodiment has a molar ratio Li / P of the Li content to the P content in the sulfide-based inorganic solid electrolyte material of preferably 1.0 or more and 5.0 or less, more preferably 2.0 or more and 4.0 or less, even more preferably 2.5 or more and 3.8 or less, even more preferably 2.8 or more and 3.6 or less, even more preferably 3.0 or more and 3.5 or less, even more preferably 3.1 or more and 3.4 or less, and particularly preferably 3.2 or more and 3.4 or less. In addition, the molar ratio S / P of the S content to the P content is preferably 2.0 or more and 6.0 or less, more preferably 3.0 or more and 5.0 or less, even more preferably 3.5 or more and 4.5 or less, even more preferably 3.8 or more and 4.2 or less, even more preferably 3.9 or more and 4.1 or less, and particularly preferably 4.0. The contents of Li, P and S in the sulfide-based inorganic solid electrolyte material can be determined by, for example, ICP emission spectrometry or X-ray analysis.
[0036] The composition formula of the sulfide-based inorganic solid electrolyte material of this embodiment is preferably Li 10 P3S 12 In other words, when producing the sulfide-based inorganic solid electrolyte material of this embodiment, the composition formula of the finally obtained sulfide-based inorganic solid electrolyte material is Li 10 P3S 12 It is preferable to optimize the mixing ratio of each raw material so that the mixture ratio is equal to or close to that range.
[0037] (Particle size distribution) The sulfide-based inorganic solid electrolyte material of the present embodiment is usually composed of particles from the viewpoint of applicability to lithium ion batteries, etc. In other words, the property of the sulfide-based inorganic solid electrolyte material of the present embodiment is usually particulate.
[0038] By appropriately designing the particle size distribution of the particles constituting the sulfide-based inorganic solid electrolyte material, it may be possible to further increase the ionic conductivity. Regarding particle size distribution, the median diameter d 50 can be used as an indicator. 50 is preferably 0.1 to 10 μm, more preferably 0.1 to 6.0 μm. 50 It is believed that by making d appropriately large, the contact surface (interface) between particles is reduced, resulting in better ionic conductivity. 50 It is believed that by not making the particle size too large, gaps are less likely to form between the particles, and thus better ionic conductivity can be obtained.
[0039] Median diameter d 50The particle size distribution on a number basis, which is the basis for calculating the above, can be obtained, for example, by the following procedures: (1) photographing particles with an electron microscope, (2) measuring the tangential diameter (Ferret diameter) of each particle in the photographed image, and (3) plotting the tangential diameter (Ferret diameter) of each particle on the horizontal axis and the frequency on a number basis on the vertical axis.
[0040] (Other matters) The sulfide-based inorganic solid electrolyte material of this embodiment is usually excellent in electrochemical stability. Electrochemical stability refers to, for example, the property of being difficult to be oxidized and reduced in a wide voltage range. More specifically, in the sulfide-based inorganic solid electrolyte material of this embodiment, the maximum value of the oxidative decomposition current of the sulfide-based inorganic solid electrolyte material measured under the conditions of a temperature of 25°C, a sweep voltage range of 0 to 5V, and a voltage sweep rate of 5mV / sec is preferably 0.50μA or less, more preferably 0.20μA or less, even more preferably 0.10μA or less, even more preferably 0.05μA or less, and particularly preferably 0.03μA or less. It is preferable that the maximum value of the oxidative decomposition current of the sulfide-based inorganic solid electrolyte material is equal to or less than the above upper limit value, since the oxidative decomposition of the sulfide-based inorganic solid electrolyte material in the lithium ion battery can be suppressed. The lower limit of the maximum value of the oxidative decomposition current of the sulfide-based inorganic solid electrolyte material is not particularly limited, but is, for example, 0.0001 μA or more.
[0041] The sulfide-based inorganic solid electrolyte material of this embodiment can be used in any application requiring lithium ion conductivity. In particular, the sulfide-based inorganic solid electrolyte material of this embodiment is preferably used in a lithium ion battery. More specifically, it is used in a positive electrode active material layer, a negative electrode active material layer, an electrolyte layer, etc. in a lithium ion battery. Furthermore, the sulfide-based inorganic solid electrolyte material of this embodiment is preferably used in a positive electrode active material layer, a negative electrode active material layer, a solid electrolyte layer, etc. constituting an all-solid-state lithium ion battery, and is particularly preferably used in a solid electrolyte layer constituting an all-solid-state lithium ion battery. An example of an all-solid-state lithium ion battery using the sulfide-based inorganic solid electrolyte material according to this embodiment is one in which a positive electrode, a solid electrolyte layer, and a negative electrode are laminated in this order. Incidentally, lithium ion conductivity can be used as a quantitative index of lithium ion conductivity. The lithium ion conductivity of the sulfide-based inorganic solid electrolyte material according to this embodiment is, for example, 1.0×10 -3 S / cm or more, preferably 1.5×10 -3 The higher the lithium ion conductivity, the better. However, in reality, the upper limit of the lithium ion conductivity is, for example, 5.0×10 -3 S / cm, specifically 3.0×10 -3 S / cm, more specifically 2.0×10 -3 The lithium ion conductivity is expressed as 1.0 S / cm. The lithium ion conductivity can be measured, for example, as described in the Examples below.
[0042] (Method of manufacturing inorganic solid electrolyte material) The sulfide-based inorganic solid electrolyte material of this embodiment can be obtained by a manufacturing method including the following steps (A), (B) and (C). In addition, the manufacturing method of the sulfide-based inorganic solid electrolyte material of this embodiment preferably further includes the following step (D) as necessary. In that case, step (C) may be performed before step (D), may be performed after step (D), or may be performed both. Step (A): Preparing a raw material composition Step (B): A step of mechanically treating the raw material composition of the sulfide-based inorganic solid electrolyte material to vitrify the raw material composition while causing a chemical reaction, thereby obtaining a sulfide-based inorganic solid electrolyte material in a glassy state. Step (C): A step of classifying the obtained sulfide-based inorganic solid electrolyte material Step (D): Heating (annealing) the obtained sulfide-based inorganic solid electrolyte material in a glassy state to crystallize at least a portion of it.
[0043] These steps will now be described in detail.
[0044] A step (A) of preparing a raw material composition First, raw materials are appropriately mixed to prepare a raw material composition for the sulfide-based inorganic solid electrolyte material. Here, the mixing ratio of each raw material in the raw material composition is adjusted so that the resulting sulfide-based inorganic solid electrolyte material has a desired composition ratio. The raw material composition of the sulfide-based inorganic solid electrolyte material typically contains lithium sulfide and phosphorus sulfide, and preferably further contains lithium nitride.
[0045] As already mentioned, the final composition of the sulfide-based inorganic solid electrolyte material is Li 10 P3S 12 It is preferable to adjust the molar ratio of each raw material so that it is equal to or close to this range. In other words, it is preferable to adjust the composition of the raw materials so that the molar amount of Li relative to the molar amount of P (Li / P) is 3.2 to 3.4, and the molar amount of S relative to the molar amount of P (S / P) is 3.9 to 4.1. By the way, Li 10 P3S 12 is a lithium-rich composition. Therefore, by using lithium nitride as a raw material, it is easy to optimize the composition.
[0046] The method for mixing the raw materials is not particularly limited as long as it is a method that can uniformly mix the raw materials. For example, mixing can be performed using a ball mill, a bead mill, a vibration mill, an impact grinding device, a mixer (a pug mixer, a ribbon mixer, a tumbler mixer, a drum mixer, a V-type mixer, etc.), a kneader, a two-shaft kneader, an airflow grinder, etc. At the laboratory level, mixing can be performed using a mortar made of agate or alumina. The mixing conditions when mixing the raw materials, such as the stirring speed, processing time, temperature, reaction pressure, and gravitational acceleration applied to the mixture, can be appropriately determined depending on the processing amount of the mixture.
[0047] The lithium sulfide used as the raw material is not particularly limited. Commercially available lithium sulfide may be used, or lithium sulfide obtained by reacting lithium hydroxide with hydrogen sulfide may be used. From the viewpoint of obtaining a high-purity sulfide-based inorganic solid electrolyte material and suppressing side reactions, it is preferable to use lithium sulfide with few impurities. In this embodiment, the lithium sulfide includes lithium polysulfide. The lithium sulfide is preferably Li2S.
[0048] As already mentioned, it is preferable to use P2S5, which has a P content higher than the stoichiometrically defined 27.87% by mass, as the phosphorus sulfide used as the raw material. Although the details are unclear, it is speculated that the use of such P2S5 containing "excess P" as the raw material promotes not only the formation of ordered crystals but also the formation of glass, which is more disordered than crystals, in steps (B) and (D), resulting in the formation of an appropriate amount of P2S6 glass structure. From the viewpoint of improving the availability of the raw material and the ionic conductivity of the final sulfide-based inorganic solid electrolyte material, the P content in the raw material P2S5 is preferably 28.0 to 28.3 mass %.
[0049] Lithium nitride may be used as the raw material. Here, since the nitrogen in lithium nitride is discharged into the system as N2, by using lithium nitride as the raw inorganic compound, it becomes possible to increase only the Li composition in a sulfide-based inorganic solid electrolyte material that contains Li, P, and S as constituent elements. The lithium nitride that can be used is not particularly limited. Commercially available lithium nitride (e.g., Li3N, etc.) may be used, or lithium nitride obtained by reacting metallic lithium (e.g., Li foil) with nitrogen gas may be used. From the viewpoint of obtaining a high-purity solid electrolyte material and suppressing side reactions, it is preferable to use lithium nitride with few impurities.
[0050] Step (B) of obtaining a sulfide-based inorganic solid electrolyte material in a glassy state The raw material composition obtained in step (A) is mechanically treated to chemically react and vitrify the raw materials, lithium sulfide, phosphorus sulfide, and preferably lithium nitride, to obtain a sulfide-based inorganic solid electrolyte material in a glassy state.
[0051] In mechanical treatment, two or more inorganic compounds are mechanically collided with each other to cause a chemical reaction and vitrification. Examples of mechanical treatment include mechanochemical treatment. Mechanochemical treatment is a method of vitrification by applying mechanical energy such as shear force or collision force to a target composition. In the step (B), the mechanochemical treatment is preferably a dry mechanochemical treatment, from the viewpoint of easily realizing an environment in which moisture and oxygen are removed to a high level. By applying the mechanochemical treatment, the raw materials can be mixed while being pulverized into fine particles. Therefore, the contact area of the raw materials can be increased. This can promote the reaction of the raw materials. Therefore, the sulfide-based inorganic solid electrolyte material of the present embodiment can be obtained more efficiently.
[0052] Mechanochemical processing is a method of vitrification while applying mechanical energy such as shear force, impact force, or centrifugal force to the mixture. Examples of equipment (vitrification equipment) for vitrification by mechanochemical processing include crushing and dispersing machines such as ball mills, bead mills, vibration mills, turbo mills, mechanofusion, disk mills, and roll mills; rotary and impact crushing equipment consisting of a mechanism combining rotation (shear stress) and impact (compressive stress) represented by rock drills, vibration drills, impact drivers, etc.; high-pressure gliding rolls; and the like. Among these, ball mills and bead mills are preferred from the viewpoint of efficiently generating very high impact energy, and ball mills are particularly preferred. In addition, from the viewpoint of excellent continuous productivity, roll mills; rotary and impact crushing equipment consisting of a mechanism combining rotation (shear stress) and impact (compressive stress) represented by rock drills, vibration drills, impact drivers, etc.; high-pressure gliding rolls; vertical mills such as roller-type vertical mills and ball-type vertical mills, etc. are preferred. In this embodiment, it is particularly preferable to carry out step (B) using a ball mill. More specifically, it is preferable to carry out the mechanochemical treatment for a total of about 10 to 1500 hours using zirconia balls with a diameter of 5 to 50 mm. When carrying out step (B) using a ball mill, the powder adhering to the inner wall and balls of the ball mill device may be scraped off during the process, and the scraped powder may be returned to the ball mill to resume the mechanochemical treatment.
[0053] It is preferable that step (B) is carried out in an atmosphere in which the amount and inflow of moisture and oxygen are highly suppressed, thereby making it possible to highly suppress contact of the raw material composition with moisture and oxygen. An atmosphere in which the presence and inflow of moisture and oxygen are highly suppressed can be created, for example, by the following method. First, the mixing vessel and the sealed vessel for the vitrification apparatus are placed in the glove box, and then the injection of inert gas such as high-purity dry argon gas or dry nitrogen gas obtained through a gas purification device and vacuum degassing are performed multiple times (preferably three times or more) into the glove box. Here, in the glove box after the above operation, the inert gas such as high-purity dry argon gas or dry nitrogen gas is circulated through the gas purification device to adjust the oxygen concentration and moisture concentration to preferably 1.0 ppm or less, more preferably 0.8 ppm or less, and even more preferably 0.6 ppm or less, respectively. Next, lithium sulfide and phosphorus sulfide are charged into the mixing vessel in the glove box, and then mixed to prepare a raw material composition (referring to step (A)). Here, charging of lithium sulfide and phosphorus sulfide into the mixing vessel in the glove box is performed according to the following procedure. First, with the door inside the glove box body closed, lithium sulfide and phosphorus sulfide are charged into the side box of the glove box. Next, an inert gas such as high-purity dry argon gas or dry nitrogen gas drawn from inside the glove box is injected into the side box and vacuum degassed multiple times (preferably three or more times), and then the door inside the glove box body is opened, lithium sulfide and phosphorus sulfide are charged into the mixing vessel inside the glove box body, and the mixing vessel is sealed. Next, after mixing the lithium sulfide and phosphorus sulfide, the obtained raw material composition is removed from the mixing vessel, transferred to a vessel for a vitrification apparatus, and sealed. By carrying out such an operation, the amount of moisture and oxygen present in the sealed container containing the raw material composition can be suppressed to a higher level than in the past, and as a result, in step (B), an atmosphere in which the amount of moisture and oxygen present is highly suppressed can be created. Next, the sealed container containing the raw inorganic composition is taken out from the glove box. The sealed container is then set in a vitrification apparatus placed in an atmosphere filled with dry gas such as dry argon gas, dry nitrogen gas, or dry air (for example, in a box filled with dry argon gas, dry nitrogen gas, dry air, or the like), and vitrification is performed. Here, during vitrification, it is preferable to continue to introduce a constant amount of dry gas into the atmosphere filled with dry gas. By such measures, an atmosphere in which the inflow of moisture and oxygen is highly suppressed can be created in step (B). In order to highly suppress the inflow of moisture and oxygen into the sealed container, it is preferable to use a gasket with excellent sealing properties, such as an O-ring or ferrule gasket, for the lid of the sealed container in order to achieve higher airtightness.
[0054] Regarding the degree of vitrification, it can be generally determined that the raw material inorganic composition has been vitrified and the desired sulfide-based inorganic solid electrolyte material has been obtained if the diffraction peaks derived from the raw material disappear or decrease when X-ray diffraction analysis is performed using Cu-Kα radiation as a radiation source.
[0055] In step (B), the lithium ion conductivity of the sulfide-based inorganic solid electrolyte material is preferably 1.0×10 or less by an AC impedance method under the measurement conditions of 27.0° C., an applied voltage of 10 mV, and a measurement frequency range of 0.1 Hz to 7 MHz. -4 S cm -1 More preferably, 2.0×10 -4 S cm -1 More preferably, 3.0×10 -4 S cm -1 More preferably, 4.0×10 -4 S cm -1 It is preferable to carry out the vitrification treatment until the lithium ion conductivity is increased to 100%, whereby a sulfide-based inorganic solid electrolyte material having even better lithium ion conductivity can be obtained.
[0056] Classification (sieving) process (C) It is preferable to classify (screen) the obtained sulfide-based inorganic solid electrolyte material. By this processing, for example, d 50 can be adjusted. The sulfide-based inorganic solid electrolyte material may be further pulverized to adjust the particle size, etc. As a specific method for the pulverization, known pulverization methods such as airflow pulverization, mortar, rotary mill, coffee mill, etc. can be used. Step (C) is preferably carried out in an inert gas atmosphere or a vacuum atmosphere, since this can prevent contact with moisture in the air.
[0057] (D) a step of crystallizing at least a portion of the sulfide-based inorganic solid electrolyte material; In this embodiment, it is preferable to carry out a step of crystallizing at least a part of the sulfide-based inorganic solid electrolyte material. In step (D), the sulfide-based inorganic solid electrolyte material in a glass state is heated (annealed) to crystallize at least a part of the sulfide-based inorganic solid electrolyte material, thereby producing a sulfide-based inorganic solid electrolyte material in a glass ceramic state (also called crystallized glass). By appropriately selecting the heating conditions, it is possible to adjust the ratio of each glass structure or each crystal structure in the sulfide-based inorganic solid electrolyte material. Then, it is possible to obtain a sulfide-based inorganic solid electrolyte material having even better lithium ion conductivity. In other words, the sulfide-based inorganic solid electrolyte material of the present embodiment is preferably in a glass ceramic state (crystallized glass state) because it has excellent lithium ion conductivity.
[0058] The temperature at which the sulfide-based inorganic solid electrolyte material in a glassy state is heated (annealed) is preferably 220 to 500°C, and more preferably 250 to 350°C. The time for heating (annealing) the sulfide-based inorganic solid electrolyte material in a glass state is not particularly limited as long as it is a time that can obtain a sulfide-based inorganic solid electrolyte material in a desired glass-ceramic state, and is, for example, 0.5 to 24 hours, preferably 1 to 18 hours, more preferably 1 to 15 hours, and even more preferably 1 to 10 hours. The heating method is not particularly limited, and may be, for example, a method using a calciner. The heating conditions such as temperature and time can be appropriately adjusted to optimize the properties of the sulfide-based inorganic solid electrolyte material.
[0059] The heating (annealing) of the sulfide-based inorganic solid electrolyte material in a glassy state is preferably performed under an inert gas atmosphere. This can prevent the deterioration (e.g., oxidation) of the sulfide-based inorganic solid electrolyte material. Examples of the inert gas include argon gas, helium gas, and nitrogen gas. These inert gases are preferably as high in purity as possible to prevent impurities from being mixed into the product, and the dew point is preferably -70°C or less, and more preferably -80°C or less, to avoid contact with moisture. The method of introducing the inert gas is not particularly limited as long as the system is filled with an inert gas atmosphere. For example, a method of purging with an inert gas, a method of continuously introducing a constant amount of an inert gas, etc. may be mentioned.
[0060] In order to obtain the sulfide-based inorganic solid electrolyte material of this embodiment, it is preferable to appropriately adjust each of the above steps. However, the method for producing the sulfide-based inorganic solid electrolyte material of this embodiment is not limited to the above method, and the sulfide-based inorganic solid electrolyte material of this embodiment can be obtained by appropriately adjusting various conditions.
[0061] <Solid electrolyte> The solid electrolyte of the present embodiment includes the sulfide-based inorganic solid electrolyte material of the present embodiment described above. The solid electrolyte of the present embodiment may or may not contain, as a component other than the sulfide-based inorganic solid electrolyte material of the present embodiment, for example, a solid electrolyte material of a type different from the sulfide-based inorganic solid electrolyte material of the present embodiment described above, within a range that does not impair the object of the present invention.
[0062] The solid electrolyte of this embodiment may or may not contain a solid electrolyte material of a different type from the sulfide-based inorganic solid electrolyte material of this embodiment described above. The solid electrolyte material of a different type from the sulfide-based inorganic solid electrolyte material of this embodiment is not particularly limited as long as it has ion conductivity and insulating properties, and can be one generally used in lithium ion batteries. For example, inorganic solid electrolyte materials such as sulfide-based inorganic solid electrolyte materials, oxide-based inorganic solid electrolyte materials, and other lithium-based inorganic solid electrolyte materials of a different type from the sulfide-based inorganic solid electrolyte material of this embodiment; organic solid electrolyte materials such as polymer electrolytes can be mentioned.
[0063] Examples of sulfide-based inorganic solid electrolyte materials different from the sulfide-based inorganic solid electrolyte material of the present embodiment described above include Li2S-P2S5 material, Li2S-SiS2 material, Li2S-GeS2 material, Li2S-Al2S3 material, Li2S-SiS2-Li3PO4 material, Li2S-P2S5-GeS2 material, Li2S-Li2O-P2S5-SiS2 material, Li2S-GeS2-P2S5-SiS2 material, Li2S-SnS2-P2S5-SiS2 material, Li2S-P2S5-Li3N material, Li2S 2+X -P4S3 material, Li2S-P2S5-P4S3 material, etc. These may be used alone or in combination of two or more. Among these, the Li2S-P2S5 material is preferred because it has excellent lithium ion conductivity and is stable over a wide voltage range without decomposition, etc. Here, for example, the Li2S-P2S5 material refers to an inorganic material obtained by chemically reacting inorganic compositions containing at least Li2S (lithium sulfide) and P2S5 with each other through mechanical treatment. In this embodiment, lithium sulfide also includes lithium polysulfide.
[0064] Examples of the oxide-based inorganic solid electrolyte material include NASICON-type, such as LiTi2(PO4)3, LiZr2(PO4)3, and LiGe2(PO4)3, (La 0.5+x Li 0.5-3x)Examples include perovskite types such as TiO3, Li2O-P2O5 materials, Li2O-P2O5-Li3N materials, etc. As other lithium-based inorganic solid electrolyte materials, for example, LiPON, LiNbO3, LiTaO3, Li3PO4, LiPO 4-x N x (where x is 0 < x ≤ 1), LiN, LiI, LISICON, etc. Furthermore, glass ceramics obtained by precipitating crystals of these inorganic solid electrolytes can also be used as inorganic solid electrolyte materials.
[0065] As the above organic solid electrolyte materials, for example, polymer electrolytes such as dry polymer electrolytes and gel electrolytes can be used. As the polymer electrolyte, those generally used in lithium-ion batteries can be used.
[0066] <Solid electrolyte membrane> The solid electrolyte membrane of this embodiment mainly contains a solid electrolyte containing the sulfide-based inorganic solid electrolyte material of this embodiment described above.
[0067] The solid electrolyte membrane of this embodiment is used, for example, in the solid electrolyte layer constituting an all-solid-state lithium-ion battery. Examples of all-solid-state lithium-ion batteries applying the solid electrolyte membrane of this embodiment include those in which a positive electrode, a solid electrolyte layer, and a negative electrode are laminated in this order. In this case, the solid electrolyte layer is constituted by the solid electrolyte membrane.
[0068] The average thickness of the solid electrolyte membrane of this embodiment is preferably 5 μm or more and 500 μm or less, more preferably 10 μm or more and 200 μm or less, and even more preferably 20 μm or more and 100 μm or less. When the average thickness of the solid electrolyte membrane is equal to or more than the lower limit, the loss of the solid electrolyte and the occurrence of cracks on the surface of the solid electrolyte membrane can be further suppressed. When the average thickness of the solid electrolyte membrane is equal to or less than the upper limit, the impedance of the solid electrolyte membrane can be further reduced. As a result, the battery characteristics of the obtained all-solid-state lithium ion battery can be further improved.
[0069] The solid electrolyte membrane of the present embodiment is preferably a pressure-molded body of a particulate solid electrolyte containing the sulfide-based inorganic solid electrolyte material according to the present embodiment described above. That is, it is preferable to pressurize the particulate solid electrolyte to form a solid electrolyte membrane having a certain strength by the anchor effect between the solid electrolyte materials. By forming the solid electrolyte into a pressure-molded body, the solid electrolyte particles bond together, and the strength of the resulting solid electrolyte membrane is further increased, which further suppresses chipping of the solid electrolyte and the occurrence of cracks on the surface of the solid electrolyte membrane.
[0070] The content of the sulfide-based inorganic solid electrolyte material of the present embodiment in the solid electrolyte membrane of the present embodiment is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, even more preferably 80% by mass or more, and particularly preferably 90% by mass or more, when the entire solid electrolyte membrane is taken as 100% by mass. This improves the contact between the solid electrolytes, and reduces the interface contact resistance of the solid electrolyte membrane. As a result, the lithium ion conductivity of the solid electrolyte membrane can be further improved. And, by using such a solid electrolyte membrane having excellent lithium ion conductivity, the battery characteristics of the obtained all-solid-state lithium ion battery can be further improved. The upper limit of the content of the sulfide-based inorganic solid electrolyte material of the present embodiment in the solid electrolyte membrane of the present embodiment is not particularly limited, but is, for example, 100 mass % or less.
[0071] The planar shape of the solid electrolyte membrane is not particularly limited and can be appropriately selected according to the shapes of the electrodes and current collectors. The planar shape can be, for example, rectangular.
[0072] The solid electrolyte membrane of the present embodiment may contain a binder resin. When the binder resin is contained, the content thereof is preferably less than 0.5 mass%, more preferably 0.1 mass% or less, even more preferably 0.05 mass% or less, and even more preferably 0.01 mass% or less, when the entire solid electrolyte membrane is taken as 100 mass%. Moreover, it is even more preferable that the solid electrolyte membrane of the present embodiment does not substantially contain a binder resin, and it is most preferable that the solid electrolyte membrane does not contain a binder resin. This improves the contact between the solid electrolytes, and reduces the interface contact resistance of the solid electrolyte film. As a result, the lithium ion conductivity of the solid electrolyte film can be further improved. By using such a solid electrolyte film with excellent lithium ion conductivity, the battery characteristics of the obtained all-solid-state lithium ion battery can be improved. Just to be clear, "substantially free of binder resin" means that the binder resin may be contained to the extent that the effect of the present embodiment is not impaired. In addition, when an adhesive resin layer is provided between the solid electrolyte layer and the positive electrode or the negative electrode, the adhesive resin originating from the adhesive resin layer present in the vicinity of the interface between the solid electrolyte layer and the adhesive resin layer is excluded from the "binder resin in the solid electrolyte membrane."
[0073] The binder resin is a binder that is generally used in lithium-ion batteries to bind inorganic solid electrolyte materials together, such as polyvinyl alcohol, poly(meth)acrylic acid, carboxymethyl cellulose, polytetrafluoroethylene, polyvinylidene fluoride, styrene-butadiene rubber, polyimide, etc.
[0074] The solid electrolyte membrane of the present embodiment can be obtained, for example, by (i) first depositing particulate solid electrolyte in the form of a membrane on the cavity surface of a mold or on the surface of a substrate, and then (ii) applying pressure to the solid electrolyte deposited in the form of a membrane. In the above (ii), the method of pressing the solid electrolyte is not particularly limited. For example, when the particulate solid electrolyte is deposited on the cavity surface of a mold, pressing with a mold and a stamping die can be used, and when the particulate solid electrolyte is deposited on the surface of a substrate, pressing with a mold and a stamping die, roll pressing, flat plate pressing, etc. can be used. The pressure for pressing the solid electrolyte is, for example, 10 to 500 MPa.
[0075] If necessary, the inorganic solid electrolyte deposited in the form of a film may be heated while being pressurized. By applying heat and pressure, the solid electrolytes are fused and bonded to each other, and the strength of the obtained solid electrolyte film is further increased. As a result, chipping of the solid electrolyte and the occurrence of cracks on the surface of the solid electrolyte film can be further suppressed. The temperature to which the solid electrolyte is heated is, for example, 40 to 500°C.
[0076] <Lithium-ion battery> FIG. 1 is a cross-sectional view showing an example of the structure of a lithium ion battery according to this embodiment (lithium ion battery 10). The lithium ion battery 100 includes, for example, a positive electrode 110 including a positive electrode active material layer 101, an electrolyte layer 120, and a negative electrode 130 including a negative electrode active material layer 103. At least one of the positive electrode active material layer 101, the negative electrode active material layer 103, and the electrolyte layer 120 contains the sulfide-based inorganic solid electrolyte material of this embodiment. It is preferable that all of the positive electrode active material layer 101, the negative electrode active material layer 103, and the electrolyte layer 120 contain the sulfide-based inorganic solid electrolyte material of this embodiment. In this embodiment, a layer containing a positive electrode active material is called a positive electrode active material layer 101 unless otherwise specified. The positive electrode 110 may further include a current collector 105 in addition to the positive electrode active material layer 101, as necessary, or may not include the current collector 105. In this embodiment, unless otherwise specified, a layer including a negative electrode active material is called a negative electrode active material layer 103. The negative electrode 130 may further include a current collector 105 in addition to the negative electrode active material layer 103, as necessary, or may not include the current collector 105. There is no particular limitation on the shape of the lithium ion battery 100. Examples of the shape include a cylindrical shape, a coin shape, a square shape, a film shape, and any other shape.
[0077] The lithium ion battery 100 is generally manufactured according to a known method, for example, by forming a stack of a positive electrode 110, an electrolyte layer 120, and a negative electrode 130 into a cylindrical, coin, square, film, or other arbitrary shape, and sealing a nonaqueous electrolyte solution therein as necessary.
[0078] (positive electrode) The material constituting the positive electrode 110 is not particularly limited, and any material generally used in lithium ion batteries can be used. The method for producing the positive electrode 110 is not particularly limited, and the positive electrode 110 can be produced according to a generally known method. For example, the positive electrode 110 can be obtained by forming a positive electrode active material layer 101 containing a positive electrode active material on the surface of a current collector 105 such as aluminum foil. The thickness and density of the positive electrode active material layer 101 are appropriately determined depending on the intended use of the battery, and are not particularly limited, and can be set in accordance with generally known information.
[0079] The positive electrode active material layer 101 contains a positive electrode active material. The positive electrode active material is not particularly limited, and generally known materials can be used. For example, lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMn2O4), solid solution oxide (Li2MnO3-LiMO2 (M=Co, Ni, etc.)), lithium-manganese-nickel oxide (LiNi 1 / 3 Mn 1 / 3 Co 1 / 3O2), composite oxides such as olivine-type lithium phosphate oxide (LiFePO4); conductive polymers such as polyaniline and polypyrrole; sulfide-based positive electrode active materials such as Li2S, CuS, Li-Cu-S compounds, TiS2, FeS, MoS2, Li-Mo-S compounds, Li-Ti-S compounds, Li-VS compounds, and Li-Fe-S compounds; materials using sulfur as an active material such as sulfur-impregnated acetylene black, sulfur-impregnated porous carbon, and mixed powder of sulfur and carbon; and the like can be used. These positive electrode active materials may be used alone or in combination of two or more. Among these, from the viewpoint of having a higher discharge capacity density and superior cycle characteristics, a sulfide-based positive electrode active material is preferred, and one or more selected from a Li-Mo-S compound, a Li-Ti-S compound, and a Li-VS compound are more preferred.
[0080] Here, the Li-Mo-S compound contains Li, Mo, and S as the constituent elements, and can usually be obtained by chemically reacting the raw materials, molybdenum sulfide and an inorganic composition containing lithium sulfide, with each other through a mechanical treatment. In addition, the Li-Ti-S compound contains Li, Ti, and S as constituent elements, and can usually be obtained by chemically reacting inorganic compositions containing titanium sulfide and lithium sulfide, which are raw materials, with each other through mechanical processing. Li-VS compounds contain the constituent elements Li, V, and S, and are usually obtained by chemically reacting the raw materials vanadium sulfide and lithium sulfide with each other through mechanical processing.
[0081] The positive electrode active material layer 101 may or may not contain, as a component other than the positive electrode active material, one or more materials selected from, for example, a binder resin, a thickener, a conductive assistant, a solid electrolyte material, etc. Each material, such as the binder resin, the thickener, the conductive assistant, and the solid electrolyte material, will be described below.
[0082] The positive electrode active material layer 101 may contain a binder resin that serves to bind the positive electrode active materials together and between the positive electrode active material and the current collector 105 . The binder resin is not particularly limited as long as it is a typical binder resin that can be used in lithium ion batteries. Examples include polyvinyl alcohol, poly(meth)acrylic acid, carboxymethyl cellulose, polytetrafluoroethylene, polyvinylidene fluoride, styrene-butadiene rubber, polyimide, etc. The binder may be used alone or in combination of two or more.
[0083] The positive electrode active material layer 101 may contain a thickener in order to ensure the fluidity of the slurry suitable for application. The thickener is not particularly limited as long as it is a normal thickener that can be used in lithium ion batteries. Examples of the thickener include cellulose-based polymers such as carboxymethyl cellulose, methyl cellulose, and hydroxypropyl cellulose, and ammonium salts and alkali metal salts thereof, polycarboxylic acids, polyethylene oxide, polyvinylpyrrolidone, poly(meth)acrylates, and water-soluble polymers such as polyvinyl alcohol. The thickener may be used alone or in combination of two or more.
[0084] The positive electrode active material layer 101 may contain a conductive assistant from the viewpoint of improving the conductivity of the positive electrode 110. The conductive assistant is not particularly limited as long as it is a normal conductive assistant that can be used in lithium ion batteries. For example, carbon black such as acetylene black and ketjen black, and carbon materials such as vapor grown carbon fiber can be mentioned. When a conductive assistant is used, one type may be used alone, or two or more types may be used in combination.
[0085] The positive electrode 110 may contain a solid electrolyte containing the sulfide-based inorganic solid electrolyte material of the present embodiment described above, or may contain a solid electrolyte containing a solid electrolyte material of a type different from the sulfide-based inorganic solid electrolyte material of the present embodiment. The solid electrolyte material of a type different from the sulfide-based inorganic solid electrolyte material of the present embodiment is not particularly limited as long as it has ion conductivity and insulating properties, and can be one generally used in lithium ion batteries. For example, inorganic solid electrolyte materials such as sulfide-based inorganic solid electrolyte materials, oxide-based inorganic solid electrolyte materials, and other lithium-based inorganic solid electrolyte materials; organic solid electrolyte materials such as polymer electrolytes can be mentioned. More specifically, the inorganic solid electrolyte materials mentioned in the description of the solid electrolyte of the present embodiment can be used.
[0086] The blending ratio of the various materials in the positive electrode active material layer 101 is appropriately determined depending on the intended use of the battery, and is not particularly limited, and can be set in accordance with generally known information.
[0087] (Negative electrode) The material constituting the negative electrode 130 is not particularly limited, and any material generally used in lithium ion batteries can be used. The method for producing the negative electrode 130 is not particularly limited, and the negative electrode 130 can be produced according to a generally known method. For example, the negative electrode 130 can be obtained by forming a negative electrode active material layer 103 containing a negative electrode active material on the surface of a current collector 105 such as copper. The thickness and density of the negative electrode active material layer 103 are not particularly limited since they are appropriately determined depending on the intended use of the battery, and can be set in accordance with generally known information.
[0088] The negative electrode active material layer 103 contains a negative electrode active material. The negative electrode active material is not particularly limited as long as it is a normal negative electrode active material that can be used for the negative electrode of a lithium ion battery. For example, carbonaceous materials such as natural graphite, artificial graphite, resin carbon, carbon fiber, activated carbon, hard carbon, and soft carbon; metal-based materials mainly composed of lithium, lithium alloys, tin, tin alloys, silicon, silicon alloys, gallium, gallium alloys, indium, indium alloys, aluminum, and aluminum alloys; conductive polymers such as polyacene, polyacetylene, and polypyrrole; lithium titanium composite oxides (e.g., Li4Ti5O 12 These negative electrode active materials may be used alone or in combination of two or more.
[0089] The negative electrode active material layer 103 is not particularly limited, but may contain, as a component other than the negative electrode active material, one or more materials selected from, for example, a binder resin, a thickener, a conductive assistant, a solid electrolyte material, etc. These materials are not particularly limited, but may be, for example, the same materials as those used for the positive electrode 110 described above. The blending ratio of the various materials in the negative electrode active material layer 103 is appropriately determined depending on the intended use of the battery, and is not particularly limited, and can be set in accordance with generally known information.
[0090] (electrolyte layer) The electrolyte layer 120 is a layer formed between the positive electrode active material layer 101 and the negative electrode active material layer 103 . The electrolyte layer 120 may be a separator impregnated with a non-aqueous electrolyte solution or a solid electrolyte layer containing a solid electrolyte.
[0091] The separator is not particularly limited as long as it electrically insulates the positive electrode 110 and the negative electrode 130 and allows lithium ions to pass through, and for example, a porous membrane can be used.
[0092] As the porous membrane, a microporous polymer film is preferably used, and examples of the material include polyolefin, polyimide, polyvinylidene fluoride, polyester, etc. In particular, a porous polyolefin film is preferable, and specific examples thereof include a porous polyethylene film, a porous polypropylene film, etc.
[0093] The non-aqueous electrolyte to be impregnated into the separator is an electrolyte dissolved in a solvent. Any known lithium salt can be used as the electrolyte, and it may be selected according to the type of active material. For example, LiClO4, LiBF6, LiPF6, LiCF3SO3, LiCF3CO2, LiAsF6, LiSbF6, LiB 10 Cl 10 , LiAlCl4, LiCl, LiBr, LiB(C2H5)4, CF3SO3Li, CH3SO3Li, LiCF3SO3, LiC4F9SO3, Li(CF3SO2)2N, and lithium lower fatty acid carboxylates.
[0094] The solvent for dissolving the electrolyte is not particularly limited as long as it is a solvent that is usually used as a liquid for dissolving electrolytes. For example, carbonates such as ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), dimethyl carbonate (DMC), diethyl carbonate (DEC), methyl ethyl carbonate (MEC), vinylene carbonate (VC), etc.; lactones such as γ-butyrolactone, γ-valerolactone, etc.; ethers such as trimethoxymethane, 1,2-dimethoxyethane, diethyl ether, 2-ethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, etc.; sulfoxides such as dimethyl sulfoxide, etc.; 1,3- Examples of such oxolanes include dioxolane and 4-methyl-1,3-dioxolane; nitrogen-containing compounds such as acetonitrile, nitromethane, formamide, and dimethylformamide; organic acid esters such as methyl formate, methyl acetate, ethyl acetate, butyl acetate, methyl propionate, and ethyl propionate; phosphoric acid triesters and diglymes; triglymes; sulfolanes such as sulfolane and methylsulfolane; oxazolidinones such as 3-methyl-2-oxazolidinone; sultones such as 1,3-propane sultone, 1,4-butane sultone, and naphtha sultone; etc. These may be used alone or in combination of two or more.
[0095] The solid electrolyte layer is a layer formed between the positive electrode active material layer 101 and the negative electrode active material layer 103, and is a layer formed of a solid electrolyte containing a solid electrolyte material. The solid electrolyte contained in the solid electrolyte layer is not particularly limited as long as it has lithium ion conductivity. However, in this embodiment, it is preferable that the solid electrolyte contains the sulfide-based inorganic solid electrolyte material of this embodiment. The content of the solid electrolyte in the solid electrolyte layer of the present embodiment is not particularly limited as long as the desired performance is obtained, and is, for example, 10% by volume or more and 100% by volume or less, preferably 50% by volume or more and 100% by volume or less. In particular, in the present embodiment, it is preferable that the solid electrolyte layer is composed only of a solid electrolyte containing the sulfide-based inorganic solid electrolyte material of the present embodiment.
[0096] The solid electrolyte layer of the present embodiment may contain a binder resin. By containing the binder resin, a solid electrolyte layer having flexibility can be obtained. Examples of the binder resin include fluorine-containing binders such as polytetrafluoroethylene and polyvinylidene fluoride. The thickness of the solid electrolyte layer is, for example, 0.1 μm or more and 1000 μm or less, preferably 0.1 μm or more and 300 μm or less.
[0097] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can be adopted. Furthermore, the present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of the present invention are included in the present invention. Below, examples of reference forms are given. 1. A sulfide-based inorganic solid electrolyte material containing Li, P and S as constituent elements, 31 In the spectrum obtained by P-NMR measurement, PS 4 When the sum of the areas of the peaks due to the structure is set to 1, P 2 S 6 A sulfide-based inorganic solid electrolyte material in which the sum of the areas of peaks derived from a glass structure is 0.1 or more. 2. 1. The sulfide-based inorganic solid electrolyte material according to claim 1, In the above spectrum, PS 4 When the sum of the peak areas due to the glass structure is set to 1, P 2 S 6 A sulfide-based inorganic solid electrolyte material in which the sum of the peak areas derived from the glass structure is 0.15 or more. 3. 1. or 2. The sulfide-based inorganic solid electrolyte material according to claim 1, In the above spectrum, PS 4 When the sum of the peak areas due to the glass structure is set to 1, PS 4 A sulfide-based inorganic solid electrolyte material in which the sum of the peak areas derived from the crystal structure is 0.3 to 1. 4. The sulfide-based inorganic solid electrolyte material according to any one of 1. to 3., Lithium ion conductivity is 1.5×10 -3 Sulfide-based inorganic solid electrolyte material with a dielectric constant of S / cm or higher. 5. The sulfide-based inorganic solid electrolyte material according to any one of 1. to 4., A sulfide-based inorganic solid electrolyte material composed of particles with a median diameter of 0.1 to 10 μm. 6. The sulfide-based inorganic solid electrolyte material according to any one of 1. to 5., The sulfide-based inorganic solid electrolyte material has a molar ratio Li / P of the Li content to the P content of 1.0 or more and 5.0 or less, and a molar ratio S / P of the S content to the P content of 2.0 or more and 6.0 or less. 7. The sulfide-based inorganic solid electrolyte material according to any one of 1. to 6., A sulfide-based inorganic solid electrolyte material used in lithium-ion batteries. 8. A solid electrolyte comprising the sulfide-based inorganic solid electrolyte material according to any one of 1. to 7. 9. 8. A solid electrolyte membrane containing the solid electrolyte according to claim 8 as a main component. 10. 9. The solid electrolyte membrane according to claim 9, A solid electrolyte membrane which is a pressure-molded body of the particulate solid electrolyte. 11. 9. or 10. The solid electrolyte membrane according to claim 10, A solid electrolyte membrane having a binder resin content of less than 0.5% by mass when the entire solid electrolyte membrane is taken as 100% by mass. 12. 9. The solid electrolyte membrane according to any one of 9. to 11., A solid electrolyte membrane, wherein the content of the sulfide-based inorganic solid electrolyte material in the solid electrolyte membrane is 50% by mass or more when the entire solid electrolyte membrane is taken as 100% by mass. 13. A lithium ion battery comprising a positive electrode including a positive electrode active material layer, an electrolyte layer, and a negative electrode including a negative electrode active material layer, A lithium ion battery in which at least one of the positive electrode active material layer, the electrolyte layer, and the negative electrode active material layer contains the sulfide-based inorganic solid electrolyte material according to any one of 1. to 7. EXAMPLES
[0098] The embodiments of the present invention will be described in detail based on Examples and Comparative Examples. It should be noted that the present invention is not limited to the Examples.
[0099] <Production of sulfide-based inorganic solid electrolyte materials> Example 1 First, Li2S (Furukawa Co., Ltd., purity 99.9%), P2S5 (Perimeter Solutions), and Li3N (Furukawa Co., Ltd.) were prepared as raw materials. For P2S5, a product with a P content of 28.1 mass% was selected from several P2S5 products with different lot numbers obtained from Perimeter Solutions. The P content was measured by ICP emission spectrometry using an ICP emission spectrometer (Seiko Instruments Inc., SPS3000).
[0100] Next, Li2S powder, P2S5 powder, and Li3N powder (Li2S:P2S5:Li3N=27:9:2 (molar ratio)) were precisely weighed in an argon glove box. These powders were then mixed in an agate mortar for 10 minutes. Thus, a mixed powder was obtained.
[0101] Next, 500 g of the mixed powder was weighed out and placed in an alumina pot (inner volume 5.0 L) together with 7500 g of zirconia balls with a diameter of 25 mm and 700 g of zirconia balls with a diameter of 10 mm, and then pulverized and mixed (mechanochemical treatment) for 48 hours in a ball mill (rotation speed 100 rpm). Next, the powder remaining on the inner wall of the pot and on the balls after grinding and mixing was scraped off. After that, the powder was placed in the same pot again together with the balls, and ground and mixed for the same time as before using a ball mill (rotation speed 100 rpm). This process from scraping to grinding was repeated for a total of 700 hours. Then, the glass-state sulfide-based inorganic solid electrolyte material (Li 10 P3S 12 ) was obtained. The grinding and mixing (mechanochemical treatment) was carried out in an atmosphere in which the presence and inflow of moisture and oxygen were suppressed at high levels.
[0102] Next, the sulfide-based inorganic solid electrolyte material in the glass state was annealed in argon at 300°C for 7 hours. This resulted in the formation of a sulfide-based inorganic solid electrolyte material in the glass ceramic state (Li 10 P3S 12 ) was obtained. The obtained sulfide-based inorganic solid electrolyte material in a glass ceramic state was classified using a sieve with 20 μm openings to remove coarse particles. In this manner, a sulfide-based inorganic solid electrolyte material was produced.
[0103] The composition of the obtained sulfide-based inorganic solid electrolyte material is Li 10 P3S 12 This was confirmed by ICP emission spectrometry using an ICP emission spectrometry analyzer (Seiko Instruments, SPS3000).
[0104] Example 2 First, Li2S (manufactured by Furukawa Co., Ltd., purity 99.9%), P2S5 (manufactured by Perimeter Solutions Co., Ltd.), and Li3N (manufactured by Furukawa Co., Ltd.) were used as raw materials. For P2S5, a product with a P content of 28.0 mass% was selected from several P2S5 products with different lot numbers obtained from Perimeter Solutions Co., Ltd. (The P content was measured in the same manner as in Example 1).
[0105] Next, Li2S powder, P2S5 powder, and Li3N powder (Li2S:P2S5:Li3N=27:9:2 (molar ratio)) were precisely weighed in an argon glove box. These powders were then mixed in an agate mortar for 10 minutes. Thus, a mixed powder was obtained. Next, 500 g of the mixed powder was weighed out and placed in an alumina pot (inner volume 5.0 L) together with 7500 g of zirconia balls with a diameter of 25 mm and 700 g of zirconia balls with a diameter of 10 mm, and then pulverized and mixed (mechanochemical treatment) for 48 hours in a ball mill (rotation speed 100 rpm). Next, the powder remaining on the inner wall of the pot and on the balls after grinding and mixing was scraped off. After that, the powder was placed in the same pot again together with the balls, and ground and mixed for the same time as before using a ball mill (rotation speed 100 rpm). This process from scraping to grinding was repeated for a total of 700 hours. Then, the glass-state sulfide-based inorganic solid electrolyte material (Li 10 P3S 12 ) was obtained. Next, the sulfide-based inorganic solid electrolyte material in the glass state was annealed in argon at 300°C for 7 hours. This resulted in the formation of a sulfide-based inorganic solid electrolyte material in the glass ceramic state (Li 10 P3S 12 ) was obtained. Next, the obtained sulfide-based inorganic solid electrolyte material in a glass ceramic state was classified using a sieve with 20 μm openings to remove coarse particles. In this manner, a sulfide-based inorganic solid electrolyte material was produced.
[0106] The composition of the obtained sulfide-based inorganic solid electrolyte material is Li10 P3S 12 This was confirmed by ICP emission spectrometry using an ICP emission spectrometry analyzer (Seiko Instruments, SPS3000).
[0107] Example 3 First, Li2S (manufactured by Furukawa Co., Ltd., purity 99.9%), P2S5 (manufactured by Kanto Chemical Co., Ltd.), and Li3N (manufactured by Furukawa Co., Ltd.) were used as raw materials. For P2S5, from among several P2S5 products with different lot numbers obtained from Kanto Chemical Co., Ltd., one with a P content of about 27.9 mass%, which is greater than 27.87 mass%, was used (the method for measuring the P content was the same as in Example 1).
[0108] Next, Li2S powder, P2S5 powder, and Li3N powder (Li2S:P2S5:Li3N=27:9:2 (molar ratio)) were precisely weighed in an argon glove box. These powders were then mixed in an agate mortar for 10 minutes. Thus, a mixed powder was obtained. Next, 500 g of the mixed powder was weighed out and placed in an alumina pot (inner volume 5.0 L) together with 7500 g of zirconia balls with a diameter of 25 mm and 700 g of zirconia balls with a diameter of 10 mm, and then pulverized and mixed (mechanochemical treatment) for 48 hours in a ball mill (rotation speed 100 rpm). Next, the powder remaining on the inner wall of the pot and on the balls after grinding and mixing was scraped off. After that, the powder was placed in the same pot again together with the balls, and ground and mixed for the same time as before using a ball mill (rotation speed 100 rpm). This process from scraping to grinding was repeated for a total of 700 hours. Then, the glass-state sulfide-based inorganic solid electrolyte material (Li 10 P3S 12 ) was obtained. Next, the sulfide-based inorganic solid electrolyte material in the glass state was annealed in argon at 300°C for 7 hours. This resulted in a sulfide-based inorganic solid electrolyte material in the glass ceramic state (Li 10 P3S 12 ) was obtained. Next, the obtained sulfide-based inorganic solid electrolyte material in a glass ceramic state was classified using a sieve with 20 μm openings to remove coarse particles. In this manner, a sulfide-based inorganic solid electrolyte material was produced.
[0109] The composition of the obtained sulfide-based inorganic solid electrolyte material is Li 10 P3S 12 This was confirmed by ICP emission spectrometry using an ICP emission spectrometry analyzer (Seiko Instruments, SPS3000).
[0110] Comparative Example 1 In Comparative Example 1, unlike Examples 1 to 3, Li3N was not used as a raw material, and Li9P3S was used. 12 A sulfide-based inorganic solid electrolyte material having a composition represented by the following formula was manufactured. The specific procedure is as follows.
[0111] First, Li2S (manufactured by Furukawa Co., Ltd., purity 99.9%) and P2S5 (manufactured by Perimeter Solutions, P content 28.1 mass%, P content measured by the same method as in Example 1) were prepared as raw materials. Next, Li2S powder and P2S5 powder (Li2S:P2S5=75:25 (molar ratio)) were precisely weighed in an argon glove box. These powders were then mixed in an agate mortar for 10 minutes. Thus, a mixed powder was obtained. Next, 500 g of the mixed powder was weighed out and placed in an alumina pot (inner volume 5.0 L) together with 7500 g of zirconia balls with a diameter of 25 mm and 700 g of zirconia balls with a diameter of 10 mm, and then pulverized and mixed (mechanochemical treatment) for 48 hours in a ball mill (rotation speed 100 rpm). Next, the powder remaining on the inner wall of the pot and on the balls after grinding and mixing was scraped off. After that, the powder was put into the same pot again together with the balls, and ground and mixed for the same time as before using a ball mill (rotation speed 100 rpm). This process from scraping to grinding was repeated for a total of 700 hours. Then, the glass-state sulfide-based inorganic solid electrolyte material (Li9P3S 12 ) was obtained. Next, the sulfide-based inorganic solid electrolyte material in the glass state was annealed in argon at 300°C for 7 hours. This resulted in a sulfide-based inorganic solid electrolyte material in the glass ceramic state (Li9P3S 12 ) was obtained. Next, the obtained sulfide-based inorganic solid electrolyte material in a glass ceramic state was classified using a sieve with 20 μm openings to remove coarse particles. In this manner, a sulfide-based inorganic solid electrolyte material was produced.
[0112] The composition of the obtained sulfide-based inorganic solid electrolyte material is Li9P3S 12 This was confirmed by ICP emission spectrometry using an ICP emission spectrometry analyzer (Seiko Instruments, SPS3000).
[0113] Comparative Example 2 In Comparative Example 2, unlike Examples 1 to 3, P2S5 having a relatively low P content was used as the raw material. The specific procedure was as follows.
[0114] First, Li2S (manufactured by Furukawa Co., Ltd., purity 99.9%), P2S5 (manufactured by Perimeter Solutions Co., Ltd.), and Li3N (manufactured by Furukawa Co., Ltd.) were prepared as raw materials. For P2S5, a product with a P content of 27.7 mass% was selected from several P2S5 products with different lot numbers obtained from Perimeter Solutions Co., Ltd. (The P content was measured in the same manner as in Example 1).
[0115] Next, Li2S powder, P2S5 powder, and Li3N powder (Li2S:P2S5:Li3N=27:9:2 (molar ratio)) were precisely weighed in an argon glove box. These powders were then mixed in an agate mortar for 10 minutes. Thus, a mixed powder was obtained. Next, 500 g of the mixed powder was weighed out and placed in an alumina pot (inner volume 5.0 L) together with 7500 g of zirconia balls with a diameter of 25 mm and 700 g of zirconia balls with a diameter of 10 mm, and then pulverized and mixed (mechanochemical treatment) for 48 hours in a ball mill (rotation speed 100 rpm). Next, the powder remaining on the inner wall of the pot and on the balls after grinding and mixing was scraped off. After that, the powder was placed in the same pot again together with the balls, and ground and mixed for the same time as before using a ball mill (rotation speed 100 rpm). This process from scraping to grinding was repeated for a total of 700 hours. Then, the glass-state sulfide-based inorganic solid electrolyte material (Li 10 P3S 12 ) was obtained. Next, the sulfide-based inorganic solid electrolyte material in the glass state was annealed in argon at 300°C for 7 hours. This resulted in the formation of a sulfide-based inorganic solid electrolyte material in the glass ceramic state (Li 10 P3S 12 ) was obtained. Next, the obtained sulfide-based inorganic solid electrolyte material in a glass ceramic state was classified using a sieve with 20 μm openings to remove coarse particles. In this manner, a sulfide-based inorganic solid electrolyte material was produced.
[0116] The composition of the obtained sulfide-based inorganic solid electrolyte material is Li 10 P3S 12 This was confirmed by ICP emission spectrometry using an ICP emission spectrometry analyzer (Seiko Instruments, SPS3000).
[0117] < 31 P-NMR measurement> The sulfide-based inorganic solid electrolyte materials obtained in each of the Examples and Comparative Examples were used as samples to carry out phosphorus-31 nuclear magnetic resonance spectroscopy analysis as described below. Then, waveform separation was carried out.
[0118] In a glove bag purged with N2, a 3.2 mm diameter sample tube was filled with the sample. This was set in the instrument and rotated (Magic Angle Spinning: MAS) at a magic angle (54.7°) with respect to the external magnetic field for measurement. The details of the NMR measurement conditions are as follows. Observation frequency: 242.95MHz Pulse width: 90° pulse Pulse waiting time: 2800sec Number of times accumulated: 64 Measurement mode: Single pulse method ·MAS speed: 12kHz ·Standard substance: (NH4)2HPO41.33ppm Equipment: JNM-ECA600 manufactured by JEOL RESONANCE Co., Ltd.
[0119] The obtained NMR spectrum was separated into a peak derived from the PS4 glass structure, a peak derived from the PS4 crystal structure, a peak derived from the P2S7 glass structure, a peak derived from the P2S7 crystal structure, a peak derived from the P2S6 glass structure, and a peak derived from the P2S6 crystal structure by Gaussian functions using software capable of waveform separation. The area of each Gaussian function was then taken as the sum of the areas of the peaks derived from each structure. In the waveform separation, the maximum position (corresponding to the chemical shift of each structure), half-width, and maximum value of each Gaussian function were optimized so as to reproduce the obtained NMR spectrum as faithfully as possible. However, the maximum position of each Gaussian function was optimized within the numerical ranges listed in Table 1 above.
[0120] For reference, the sulfide-based inorganic solid electrolyte material of Example 1 31 The P-NMR spectra (original data and waveform separated data) are shown in Figure 2.
[0121] <Measurement of particle size / calculation of particle size distribution> The SEM images of the obtained sulfide-based inorganic solid electrolyte material were analyzed using image processing software (public freeware, ImageJ, v1.52a) published by the National Institutes of Health. Based on this analysis, the particle size distribution was calculated. From the obtained particle size distribution, d 50 asked for.
[0122] The procedure was as follows: first, carbon tape was attached to the sample stage of the SEM, and then a minute amount of sulfide-based inorganic solid electrolyte material particles were attached to the carbon tape so that they were thinly and widely dispersed. Next, an SEM image of the sulfide-based inorganic solid electrolyte material was taken (resolution: 1280 pixels horizontal x 960 pixels vertical). The obtained SEM image was loaded into ImageJ. Calibration was performed from the scale displayed in the SEM image. Next, the image was converted into a black and white binary image. At that time, a threshold was set so that the outline of the particles would be clear. If there were overlapping particles in the obtained black and white image, the overlapping particles were separated by the watershed method as image processing by ImageJ. Then, particle analysis was performed as image analysis by ImageJ, and the measurement results of the particle size by the Feret's diameter were obtained. In each example and comparative example, the particle sizes of 3000 or more particles were measured. The particle size measurement results were read into Microsoft's spreadsheet software EXCEL (registered trademark) to obtain the particle size distribution. From the particle size distribution, the median diameter d 50 asked for.
[0123] In all the examples and comparative examples, d 50 was in the range of 0.1-10 μm.
[0124] <Evaluation: Measurement of lithium ion conductivity> The lithium ion conductivity of the sulfide-based inorganic solid electrolyte materials obtained in each of the Examples and Comparative Examples was measured by an AC impedance method. The lithium ion conductivity was measured using a potentiostat / galvanostat SP-300 manufactured by Biologic Corp. The sample size was 9.5 mm in diameter and 1.2 to 2.0 mm in thickness, and the measurement conditions were an applied voltage of 10 mV, a measurement temperature of 27.0°C, a measurement frequency range of 0.1 Hz to 7 MHz, and a Li foil electrode. As a sample for measuring lithium ion conductivity, a plate-shaped sulfide-based inorganic solid electrolyte material having a diameter of 9.5 mm and a thickness of 1.2 to 2.0 mm was used, which was obtained by pressing 150 mg of the powdered sulfide-based inorganic solid electrolyte material obtained in each Example and Comparative Example at 270 MPa for 10 minutes using a pressing device.
[0125] Various information is summarized in Tables 2 and 3. Both Tables 2 and 3 summarize the information for Examples 1 to 3 and Comparative Examples 1 and 2. (i) Table 2 shows the area of the peaks derived from each structure when the sum of the peak areas derived from the PS4 structure (both the PS4 crystal structure and the PS4 glass structure) is set to 1, and (ii) Table 3 shows the area derived from each structure when the sum of the peak areas derived from the PS4 glass structure is set to 1.
[0126] [Table 2]
[0127] [Table 3]
[0128] As shown in Tables 2 and 3, 31 In the spectrum obtained by P-NMR measurement, the sulfide-based inorganic solid electrolyte materials (Examples 1 to 3) exhibited high lithium ion conductivity in which the sum of the areas of the peaks derived from the P2S6 glass structure was 0.1 or more when the sum of the areas of the peaks derived from the PS4 structure was set to 1. On the other hand, the sulfide-based inorganic solid electrolyte materials (Comparative Examples 1 and 2) in which the sum of the areas of the peaks derived from the P2S6 glass structure was less than 0.1 exhibited poor lithium ion conductivity. In addition, a comparison between Examples 1 and 2 and Example 3 reveals a tendency that the lithium ion conductivity increases as the total area of the peaks derived from the P2S6 glass structure increases.
[0129] This application claims priority based on Japanese Patent Application No. 2020-197943, filed on November 30, 2020, the disclosure of which is incorporated herein in its entirety. [Explanation of symbols]
[0130] 100 Lithium-ion batteries 101 Cathode active material layer 103 Negative electrode active material layer 105 Current collector 110 Positive electrode 120 Electrolyte layer 130 negative electrode
Claims
1. A sulfide-based inorganic solid electrolyte material containing only Li, P and S as constituent elements, 31 In the spectrum obtained by P-NMR measurement, PS 4 When the sum of the areas of the peaks due to the structure is set to 1, P 2 S 6 A sulfide-based inorganic solid electrolyte material, in which the sum of the areas of peaks derived from a glass structure is 0.1 or more.
2. The sulfide-based inorganic solid electrolyte material according to claim 1, In the spectrum, PS 4 When the sum of the peak areas due to the glass structure is set to 1, P 2 S 6 A sulfide-based inorganic solid electrolyte material, in which the sum of peak areas derived from a glass structure is 0.15 or more.
3. The sulfide-based inorganic solid electrolyte material according to claim 1 or 2, In the spectrum, PS 4 When the sum of the peak areas due to the glass structure is set to 1, PS 4 A sulfide-based inorganic solid electrolyte material having a sum of peak areas derived from a crystal structure of 0.3 to 1.
4. The sulfide-based inorganic solid electrolyte material according to any one of claims 1 to 3, Lithium ion conductivity is 1.5 x 10 -3 A sulfide-based inorganic solid electrolyte material having a specific surface area (S / cm) or more.
5. The sulfide-based inorganic solid electrolyte material according to any one of claims 1 to 4, A sulfide-based inorganic solid electrolyte material composed of particles with a median diameter of 0.1 to 10 μm.
6. The sulfide-based inorganic solid electrolyte material according to any one of claims 1 to 5, The sulfide-based inorganic solid electrolyte material has a molar ratio Li / P of the Li content to the P content of 1.0 or more and 5.0 or less, and a molar ratio S / P of the S content to the P content of 2.0 or more and 6.0 or less.
7. The sulfide-based inorganic solid electrolyte material according to any one of claims 1 to 6, A sulfide-based inorganic solid electrolyte material used in lithium-ion batteries.
8. A solid electrolyte comprising the sulfide-based inorganic solid electrolyte material according to any one of claims 1 to 7.
9. A solid electrolyte membrane comprising the solid electrolyte according to claim 8 as a main component.
10. The solid electrolyte membrane according to claim 9, A solid electrolyte membrane which is a pressure-molded body of the particulate solid electrolyte.
11. The solid electrolyte membrane according to claim 9 or 10, A solid electrolyte membrane, wherein the content of the binder resin in the solid electrolyte membrane is less than 0.5% by mass, where the entire solid electrolyte membrane is taken as 100% by mass.
12. The solid electrolyte membrane according to any one of claims 9 to 11, A solid electrolyte membrane, wherein the content of the sulfide-based inorganic solid electrolyte material in the solid electrolyte membrane is 50 mass % or more when the entire solid electrolyte membrane is taken as 100 mass %.
13. A lithium ion battery comprising a positive electrode including a positive electrode active material layer, an electrolyte layer, and a negative electrode including a negative electrode active material layer, At least one of the positive electrode active material layer, the electrolyte layer, and the negative electrode active material layer comprises the sulfide-based inorganic solid electrolyte material according to any one of claims 1 to 7. A lithium ion battery.
Citation Information
Patent Citations
Optical fiber sensor
JP1985077740A
Sulfide solid electrolyte glass, lithium solid state battery, and method for producing sulfide solid electrolyte glass
JP2014035865A
Sulfide solid electrolyte material and cell using the same
JP2019003927A
Sulfide-based solid electrolyte, Solid state secondary battery comprising sulfide-based solid electrolyte, and Method for preparing sulfide-based solid electrolyte
KR1020200107396A