Piping and method for manufacturing the same

The method uses non-carbon pigments in hard vinyl chloride resin pipes to maintain heat-shielding properties during processing, addressing discoloration and warping issues, achieving a pipe joint with superior heat-shielding and appearance.

JP7596474B2Active Publication Date: 2024-12-09SEKISUI CHEMICAL CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2023160167
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-09-25
Publication Date
2024-12-09
Estimated Expiration
2039-06-03

AI Technical Summary

Technical Problem

Hard vinyl chloride resin pipes containing carbon black deteriorate due to heat absorption, leading to warping and discoloration during processing, and existing weather-resistant coatings lose heat-shielding properties when peeled off.

Method used

A method for manufacturing a pipe joint using a gray hard vinyl chloride resin composition with non-carbon inorganic and organic pigments, achieving infrared reflectance of 20% or more, and specific SDR and heating conditions to maintain heat-shielding properties without discoloration.

Benefits of technology

The method allows for heat-processing of pipes without impairing heat-shielding properties, resulting in a pipe joint with excellent appearance and heat-shielding capabilities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007596474000004
    Figure 0007596474000004
  • Figure 0007596474000005
    Figure 0007596474000005
  • Figure 0007596474000006
    Figure 0007596474000006
Patent Text Reader

Abstract

To provide piping composed of a gray hard vinyl chloride-based resin composition, subjected to heating processing, and having excellent heat insulation and appearance.SOLUTION: Piping is composed of a gray hard vinyl chloride-based resin composition including a hard vinyl chloride-based resin and a pigment and has a processed portion on which heating processing is performed and a non-processed portion on which the heating processing is not performed. The pigment is composed of a non-carbon-based inorganic pigment and an organic pigment, the organic pigment includes at least a blue organic pigment, and color difference between the processed portion and the non-processed portion is 5 or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a pipe joint and to a pipe joint. [Background technology]

[0002] It is known that resin pipes have problems such as warping and deterioration due to heat. In particular, pipes containing carbon black as a pigment are prone to the above problems when exposed to sunlight because the carbon black easily absorbs infrared rays and accumulates heat. General-purpose rigid polyvinyl chloride resin pipes contain carbon black and are regulated to be gray in color. In view of this, rigid polyvinyl chloride resin pipes using organic pigments and rigid polyvinyl chloride resin pipes using inorganic pigments have been proposed (Patent Documents 1 and 2).

[0003] Meanwhile, in order to suppress deterioration of a cylindrical resin base material due to ultraviolet rays, a conduit has been proposed in which a weather-resistant paint is applied to the outer periphery of the base material (Patent Document 3). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2003-329176 A [Patent Document 2] JP 2013-159774 A [Patent Document 3] International Publication No. 2011 / 058965 Summary of the Invention [Problem to be solved by the invention]

[0005] However, according to the inventors' investigations, when attempting to manufacture a pipe fitting by subjecting the rigid polyvinyl chloride resin pipes of Patent Documents 1 and 2 to heat processing such as socketing and bending, the processed portion may whiten, resulting in a poor appearance. The rigid polyvinyl chloride resin pipes in Patent Documents 1 and 2 use a pigment that has a lower heat storage capacity than carbon black, so they have heat insulation properties and are less likely to rise in temperature when heated. This is thought to be the cause of whitening. If the heating temperature is increased or the heating time is extended in order to sufficiently increase the temperature, discoloration such as burning will occur, resulting in a poor appearance.

[0006] Patent Document 3 describes the inclusion of a heat-shielding pigment in a weather-resistant paint. A coating film formed from a weather-resistant paint containing a heat-shielding pigment has heat-shielding properties, and is therefore thought to be able to suppress temperature rise when exposed to sunlight. However, when a pipe coated with a weather-resistant paint is processed in an oil bath, the coating film on the surface peels off. In the area where the coating film has peeled off, the heat-shielding properties are lost. Furthermore, the peeling of the coating film also deteriorates the appearance.

[0007] One aspect of the present invention aims to provide a method for manufacturing a pipe fitting that is made of a gray rigid polyvinyl chloride resin composition and that can subject a heat-insulating pipe to heat processing without impairing the heat-insulating properties, thereby producing a pipe fitting with excellent heat-insulating properties and appearance. Another aspect of the present invention has an object to provide a pipe joint which is made of a gray rigid polyvinyl chloride resin composition, which is subjected to heat processing, and which has excellent heat insulation properties and appearance. [Means for solving the problem]

[0008] The present invention has the following aspects. [1] A process for producing a pipe made of a gray rigid polyvinyl chloride resin composition containing a polyvinyl chloride resin and a pigment, comprising the steps of: The pigment includes at least one selected from the group consisting of non-carbon-based inorganic pigments and organic pigments, The infrared reflectance of the surface of the processed tube is 20% or more; The ratio SDR of the outer diameter (mm) to the wall thickness (mm) of the processed tube is 30 to 36; A method for manufacturing a pipe fitting, characterized in that the heating time during the heat processing is set so that the ratio T / SDR of the heating time T (seconds) converted into the ratio SDR when an infrared heater with an output of 500 W is used is 40 to 150. [2] The method for manufacturing the pipe fitting according to [1] above, wherein the heating process is either one or both of bending and receiving. [3] A pipe joint made of a gray rigid polyvinyl chloride resin composition containing a polyvinyl chloride resin and a pigment, the pipe joint having a processed portion that has been subjected to a heat processing and an unprocessed portion that has not been subjected to the heat processing, The pigment includes at least one selected from the group consisting of non-carbon-based inorganic pigments and organic pigments, The surface has an infrared reflectance of 20% or more. A pipe fitting characterized in that the ratio SDR of the outer diameter (mm) to the wall thickness (mm) of the unmachined portion is 30 to 36. [4] The pipe fitting of [3] above, wherein the color difference between the processed portion and the unprocessed portion is 5 or less. [5] The pipe fitting according to [3] or [4], wherein the pigment is substantially free of carbon black. [6] The pipe fitting according to any one of [3] to [5] above, wherein the pigment consists solely of a non-carbon-based inorganic pigment. [7] The pipe fitting according to any one of [3] to [5], wherein the pigments that exhibit color are made entirely of organic pigments. [8] The pipe fitting according to any one of [3] to [5] above, wherein the pigment comprises a mixture of a non-carbon-based inorganic pigment and an organic pigment. Effect of the Invention

[0009] According to the method for manufacturing a pipe fitting of the present invention, a pipe to be processed which is made of a gray rigid polyvinyl chloride resin composition and has heat-insulating properties can be subjected to heat processing without impairing the heat-insulating properties, and a pipe fitting which has excellent heat-insulating properties and appearance can be obtained. The pipe joint of the present invention is made of a gray rigid polyvinyl chloride resin composition, is heat-processed, and has excellent heat insulation properties and appearance. [Brief description of the drawings]

[0010] [Figure 1] FIG. 2 is a partially cutaway side view showing an example of a pipe joint. [Diagram 2] FIG. 4 is a partially cutaway side view showing another example of a pipe joint. [Diagram 3] FIG. 4 is a partially cutaway side view showing another example of a pipe joint. [Figure 4] 1 is a graph showing the measurement results of the spectral reflectance of the surface of the pipe fittings of Examples 1 and 3 and Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] [Method of manufacturing pipe joint] A method for producing a pipe fitting according to one embodiment of the present invention includes a step of subjecting a processed pipe made of a gray rigid polyvinyl chloride resin composition to a heat processing step (heat processing step). Therefore, the resulting pipe fitting has a processed portion that has been subjected to the heat processing. The method for producing the pipe joint of this embodiment may include a step (molding step) of molding the gray rigid polyvinyl chloride resin composition to obtain a pipe to be processed, prior to the heat processing step. The method for producing the pipe joint of this embodiment may include a step of preparing a gray rigid vinyl chloride resin composition (preparation step) prior to the molding step.

[0012] (Gray rigid polyvinyl chloride resin composition) The gray rigid vinyl chloride resin composition (hereinafter also referred to as "the present resin composition") contains a vinyl chloride resin and a pigment. The present resin composition may contain additives as necessary within the range that does not impair the effects of the present invention.

[0013] <Vinyl chloride resin> Examples of vinyl chloride resins include homopolymers of vinyl chloride, copolymers of vinyl chloride, and chlorinated products thereof. These may be used alone or in combination of two or more kinds. Examples of the copolymer of vinyl chloride include copolymers of vinyl chloride monomer and a monomer or polymer copolymerizable with vinyl chloride monomer.

[0014] Examples of monomers copolymerizable with vinyl chloride monomers include α-olefin compounds such as ethylene, propylene, and butylene; vinyl ester compounds such as vinyl propionate; vinyl ether compounds such as ethyl vinyl ether and butyl vinyl ether; (meth)acrylate compounds such as methyl (meth)acrylate, butyl (meth)acrylate, and hydroxyethyl (meth)acrylate; aromatic vinyl compounds such as styrene and α-methylstyrene; and N-substituted maleimide compounds such as N-phenylmaleimide and N-cyclohexylmaleimide. These copolymerizable monomers may be used alone or in combination of two or more. Examples of polymers copolymerizable with vinyl chloride monomers include acrylic copolymers made of alkyl (meth)acrylate monomers, etc. These copolymerizable polymers may be used alone or in combination of two or more kinds. (Meth)acrylate means acrylate or methacrylate. In the vinyl chloride copolymer, the ratio of the vinyl chloride monomer to the above-mentioned copolymerizable monomer or polymer may be appropriately determined depending on the performance and purpose of the rigid polyvinyl chloride resin pipe, and is not particularly limited.

[0015] The vinyl chloride resin may be a commercially available product or may be produced by a known production method. In the production of a vinyl chloride homopolymer or copolymer, the vinyl chloride may be polymerized by a conventionally known method, such as a suspension polymerization method.

[0016] The average degree of polymerization of the vinyl chloride resin is preferably 800 to 3000, more preferably 900 to 1500, further preferably 950 to 1200, and most preferably 1000 to 1100. When the average degree of polymerization is 800 or more, the mechanical strength is superior. When the average degree of polymerization is 3000 or less, the resin is easily molded by extrusion molding and easily heat-processed. The above-mentioned average degree of polymerization means an average degree of polymerization measured in accordance with the "Testing method for vinyl chloride resins" of Japanese Industrial Standard JIS K 6721 using a resin obtained by dissolving a vinyl chloride resin in tetrahydrofuran (THF), removing insoluble components by filtration, and then drying and removing the THF in the filtrate.

[0017] <Pigments> In the present resin composition, the pigment is used to give the present resin composition a gray color tone as specified in JIS K 6741. The pigment includes a pigment that exhibits color (non-white) so as to impart a gray hue to the resin composition. The pigment typically includes a pigment that exhibits color and a pigment that exhibits white.

[0018] The pigment contains at least one pigment selected from the group consisting of non-carbon inorganic pigments and organic pigments (hereinafter, these are also collectively referred to as "pigment (I)"). Pigment (I) has lower infrared absorption than carbon black. Therefore, by containing pigment (I), it is possible to increase infrared reflectance. The pigment may contain other pigments other than the pigment (I) as necessary.

[0019] The non-carbon-based inorganic pigment is a compound (oxide, etc.) obtained by a chemical reaction of minerals or metals. Examples of the non-carbon-based inorganic pigment include non-carbon-based inorganic pigments that exhibit color (non-white), non-carbon-based inorganic pigments that exhibit white, etc. These non-carbon-based inorganic pigments can be appropriately combined within a range that allows the resin composition to be toned to a gray color.

[0020] Examples of colored non-carbon inorganic pigments include compounds containing one (single salt) or multiple (double salt) metals selected from the group consisting of chromium, iron, cobalt, copper, manganese, magnesium, bismuth, yttrium, aluminum, and vanadium. Specific examples of double salts include Fe-Co-Cr, Cu-Cr, Fe-Cr, Fe-Mn, Cu-Mn, Cu-Mg, Cu-Bi, Mn-Bi, Y-Mn, Co-Al, and Fe-Co-Al-Mg salts. Examples of compounds containing the above metals include oxides, hydroxides, sulfides, silicates, and ferrocyanides of the above metals. These compounds may be used alone or in combination of two or more. As the colored non-carbon-based inorganic pigment, a chromium-containing compound is preferred, and an Fe-Cr-based compound is more preferred, since it can reduce the infrared reflectance. As the colored non-carbon inorganic pigment, oxides are preferred because they have superior color stability.

[0021] Examples of non-carbon-based inorganic pigments that exhibit a white color include metal oxides such as titanium dioxide, aluminum oxide, zinc oxide, etc. Among these, titanium dioxide is preferred because of its high refractive index and high whiteness.

[0022] When pigment (I) is a non-carbon-based inorganic pigment, the non-carbon-based inorganic pigment is preferably a mixed pigment of a colored non-carbon-based inorganic pigment and a white non-carbon-based inorganic pigment, from the viewpoint of toning the resin composition to a gray color. In the mixed pigment, the colored non-carbon-based inorganic pigment is preferably a pigment that exhibits black color by using one or a combination of a plurality of the colored non-carbon-based inorganic pigments described above. Examples of black pigments include mixed pigments of two or more pigments that have complementary or nearly complementary colors; double salt pigments that contain multiple metal ions that constitute two or more pigments that have complementary or nearly complementary colors; and mixtures thereof. From the viewpoint of obtaining high infrared reflectance and color stability, the colored non-carbon-based inorganic pigment is preferably a mixed pigment toned black by combining green chromium oxide (Cr2O3) with a red pigment (e.g., iron oxide) that is its complementary color; a composite oxide containing chromium oxide and iron oxide; or a mixture thereof, and more preferably a composite oxide containing chromium oxide and iron oxide. In the mixed pigment, the content ratio of the colored non-carbon-based inorganic pigment to the total content of the colored non-carbon-based inorganic pigment and the white non-carbon-based inorganic pigment can be appropriately adjusted within a range in which the resin composition is gray, and is not particularly limited, and may be, for example, 18 to 58 mass %.

[0023] Organic pigments are synthesized from petroleum, etc. Examples of organic pigments include colored (non-white) organic pigments. The colored organic pigment is not particularly limited, and examples thereof include azo pigments, phthalocyanine pigments (e.g., copper phthalocyanine), threne pigments, dye lake pigments, etc. These may be used alone or in combination of two or more. As the colored organic pigment, phthalocyanine pigments are preferred, and copper phthalocyanine is more preferred, in that they have superior color stability.

[0024] The pigment (I) may be a pigment that exhibits a color (non-white), may be a pigment that exhibits a white color, or may be a mixture of a pigment that exhibits a color and a pigment that exhibits a white color. Of the pigments (I), the pigments exhibiting a white color are preferably non-carbon-based inorganic pigments exhibiting a white color. The colored pigment among the pigments (I) may be a colored non-carbon-based inorganic pigment, a colored organic pigment, or a mixture of a colored non-carbon-based inorganic pigment and a colored organic pigment.

[0025] When the pigment (I) is a non-carbon-based inorganic pigment, the content of the non-carbon-based inorganic pigment is preferably 0.050 parts by mass or more relative to 100 parts by mass of the vinyl chloride resin from the viewpoint of suppressing the non-uniformity of the color tone due to the non-uniformity of the pigment dispersion. In addition, the content of the non-carbon-based inorganic pigment is more preferably 0.050 to 0.500 parts by mass relative to 100 parts by mass of the vinyl chloride resin from the viewpoint of further suppressing the contamination of the equipment in the extrusion molding. In order to obtain these effects more effectively, the content of the non-carbon-based inorganic pigment is preferably 0.055 to 0.450 parts by mass, more preferably 0.065 to 0.350 parts by mass, and even more preferably 0.070 to 0.250 parts by mass.

[0026] When the pigment (I) is an organic pigment, the content of the organic pigment is preferably 0.01 parts by mass or more relative to 100 parts by mass of the vinyl chloride resin from the viewpoint of providing infrared reflectivity. Moreover, the content of the organic pigment is more preferably 0.01 to 1.0 parts by mass relative to 100 parts by mass of the vinyl chloride resin from the viewpoint of providing more sufficient infrared reflectivity. From the viewpoint of obtaining these effects more satisfactorily, the content of the organic pigment is preferably 0.02 to 0.8 parts by mass, more preferably 0.02 to 0.6 parts by mass, and even more preferably 0.02 to 0.4 parts by mass.

[0027] When the pigment (I) is a mixture of a non-carbon inorganic pigment and an organic pigment, the total content of the non-carbon inorganic pigment and the organic pigment is preferably 0.01 parts by mass or more per 100 parts by mass of the vinyl chloride resin from the viewpoint of providing infrared reflectivity. Moreover, the total content of the non-carbon inorganic pigment and the organic pigment is more preferably 0.01 to 1.0 parts by mass per 100 parts by mass of the vinyl chloride resin from the viewpoint of providing more sufficient infrared reflectivity. From the viewpoint of obtaining these effects more satisfactorily, the total content of the non-carbon inorganic pigment and the organic pigment is preferably 0.02 to 0.8 parts by mass, more preferably 0.02 to 0.6 parts by mass, and even more preferably 0.02 to 0.4 parts by mass. The content ratio of the non-carbon-based inorganic pigment to the total content of the non-carbon-based inorganic pigment and the organic pigment is preferably from 10 to 100 mass %, more preferably from 50 to 99 mass %, and further preferably from 70 to 98 mass %.

[0028] Other pigments include, for example, carbon black. In the present resin composition, it is preferable that the pigment does not substantially contain carbon black. Since carbon black has high infrared ray absorption, by making the pigment substantially free of carbon black, it is easy to make the infrared ray reflectance of the inner peripheral surface of the tube body 21 20% or more. By "substantially free" it is meant that the infrared reflectance is not less than 20%. The content of carbon black is preferably 0.1 part by mass or less, more preferably 0.01 part by mass or less, and particularly preferably 0 part by mass, based on 100 parts by mass of the vinyl chloride resin.

[0029] The content ratio of the pigment (I) to the total content of the pigments in the present resin composition is preferably 60 mass% or more, more preferably 80 mass% or more, and particularly preferably 100 mass%. That is, it is particularly preferable that the pigment in the present resin composition consists only of the pigment (I).

[0030] The content ratio of the coloring pigment to the total pigment content is preferably from 10 to 60 mass %, and more preferably from 15 to 50 mass %. The content ratio of the white pigment to the total pigment content is preferably from 40 to 90 mass %, and more preferably from 50 to 85 mass %.

[0031] In a preferred embodiment of the present invention, the pigment of the resin composition is composed solely of a non-carbon-based inorganic pigment. Since non-carbon-based inorganic pigments have excellent color stability, discoloration is unlikely to occur if the pigment is composed solely of a non-carbon-based inorganic pigment.

[0032] In another preferred embodiment of the present invention, the pigments present in the resin composition are colored only by organic pigments, which have excellent dispersibility in vinyl chloride resins, and thus color unevenness is unlikely to occur if the colored pigments are made up of only organic pigments. In the present embodiment, when the pigment contains a pigment that exhibits a white color, the pigment that exhibits a white color preferably consists of only a non-carbon-based pigment that exhibits a white color.

[0033] In another preferred embodiment of the present invention, the pigment of the resin composition is a mixture of a non-carbon inorganic pigment and an organic pigment. If the pigment is a mixture of a non-carbon inorganic pigment and an organic pigment, color unevenness is unlikely to occur and fading can be suppressed.

[0034] When the pigment (I) is a mixture of a non-carbon-based inorganic pigment and an organic pigment, it is preferable that the organic pigment is blue and the other colors are non-carbon-based inorganic pigments. The blue organic pigment is an organic pigment and has excellent dispersibility and color stability compared to organic pigments of other colors. Therefore, it is possible to suppress fading while suppressing color unevenness. An example of a blue organic pigment is copper phthalocyanine (phthalocyanine blue). Examples of non-carbon-based inorganic pigments of other colors that can be combined with the blue organic pigment include the above-mentioned mixed pigments of a colored non-carbon-based inorganic pigment (particularly a black pigment) and a white non-carbon-based inorganic pigment. By combining this mixed pigment with a blue organic pigment, color unevenness can be further suppressed and color stability can be further improved.

[0035] <Additives> Examples of additives include dispersants, stabilizers, stabilizing aids, lubricants, processing aids, antioxidants, and fillers. These additives may be used alone or in combination of two or more. Among these additives, dispersants, stabilizers, and fillers are preferred. The dispersant is not particularly limited, and examples thereof include silica, sodium salts or ammonium salts of polycarboxylic acids (e.g., polyacrylic acid), surfactants, etc. These may be used alone or in combination of two or more kinds.

[0036] The stabilizer is not particularly limited, and examples thereof include organic tin stabilizers such as dimethyltin mercapto, dibutyltin mercapto, dioctyltin mercapto, dibutyltin maleate, dibutyltin maleate polymer, dioctyltin maleate, dioctyltin maleate polymer, dibutyltin laurate, and dibutyltin laurate polymer; lead-based stabilizers such as lead stearate, dibasic lead phosphite, and tribasic lead sulfate, calcium-zinc-based stabilizers, barium-zinc-based stabilizers, and barium-cadmium-based stabilizers; stearate-based stabilizers (metal soaps) such as calcium stearate, zinc stearate, barium stearate, and lead stearate; ultraviolet absorbers such as salicylic acid esters, benzophenones, benzotriazoles, and cyanoacrylates; and hindered amine-based light stabilizers. These may be used alone or in combination of two or more. Among these stabilizers, stearates (stearic acid stabilizers) are preferred, and lead stearate is more preferred.

[0037] When a stearate is contained in the present resin composition, the content of the stearate is preferably 0.5 to 2 parts by mass, more preferably 0.8 to 1.7 parts by mass, even more preferably 1 to 1.5 parts by mass, and particularly preferably 1.1 to 1.4 parts by mass, relative to 100 parts by mass of the vinyl chloride resin, from the viewpoint of obtaining even better color stability. When the present resin composition contains a colored non-carbon-based inorganic pigment, the content of the stearate is preferably 10 to 54 parts by mass, more preferably 15 to 53 parts by mass, even more preferably 20 to 52 parts by mass, and particularly preferably 22 to 52 parts by mass, per 1 part by mass of the colored non-carbon-based inorganic pigment, from the viewpoint of obtaining even better color stability.

[0038] The stabilizing aid is not particularly limited, and examples thereof include epoxidized soybean oil, epoxidized linseed oil, epoxidized tetrahydrophthalate, epoxidized polybutadiene, phosphate ester, etc. These may be used alone or in combination of two or more.

[0039] The lubricant includes an internal lubricant and an external lubricant. The internal lubricant is used for the purpose of reducing the flow viscosity of the molten resin during molding and preventing frictional heat generation. The internal lubricant is not particularly limited, and examples thereof include butyl stearate, lauryl alcohol, stearyl stearate, epoxidized soybean oil, glycerin monostearate, stearic acid, bisamide, etc. These may be used alone or in combination of two or more. The external lubricant is used for the purpose of increasing the sliding effect between the molten resin and the metal surface during molding. The external lubricant is not particularly limited, and examples thereof include montanic acid wax, paraffin wax, polyolefin wax, ester wax, etc. These may be used alone or in combination of two or more kinds.

[0040] The processing aid is not particularly limited, and examples thereof include acrylic processing aids that are alkyl acrylate-alkyl methacrylate copolymers having a weight average molecular weight of 100,000 to 2,000,000, and specific examples thereof include n-butyl acrylate-methyl methacrylate copolymers, 2-ethylhexyl acrylate-methyl methacrylate-butyl methacrylate copolymers, etc. These may be used alone or in combination of two or more kinds.

[0041] The antioxidant is not particularly limited, and examples thereof include phenol-based antioxidants, etc. These may be used alone or in combination of two or more kinds.

[0042] The filler is not particularly limited, and examples thereof include calcium carbonate, talc, etc. These may be used alone or in combination of two or more kinds. Among these fillers, calcium carbonate is preferred from the viewpoint of obtaining better color stability.

[0043] When calcium carbonate is contained in the resin composition, the content of calcium carbonate is preferably 5 parts by mass or more relative to 100 parts by mass of vinyl chloride resin from the viewpoint of obtaining even better color stability. The upper limit of the content of calcium carbonate is not particularly limited, but is preferably 10 parts by mass or less, more preferably 9 parts by mass or less, and even more preferably 8 parts by mass or less relative to 100 parts by mass of vinyl chloride resin.

[0044] (To be processed pipe) The pipe to be processed is a pipe made of the above-mentioned gray rigid polyvinyl chloride resin composition. The processed pipe may be a single layer or a multi-layer pipe. If the processed pipe is a multi-layer pipe, the grey rigid polyvinyl chloride resin composition constituting each layer may be the same or different.

[0045] The infrared reflectance of the surface of the processed pipe is 20% or more, preferably 25% or more, and more preferably 30% or more. If the infrared reflectance of the surface of the processed pipe is 20% or more, a pipe fitting having a surface infrared reflectance of 20% or more can be obtained. If the surface of the pipe fitting has an infrared reflectance of 20% or more, the pipe fitting has excellent heat insulation properties, and the temperature of the pipe fitting is less likely to rise when exposed to sunlight, and the pipe fitting is less likely to warp or deteriorate. From the viewpoint of heat insulation, the higher the infrared reflectance of the surface of the processed tube, the better. There is no particular upper limit, but from the viewpoint of ease of heat processing, a reflectance of 60% or less is preferable.

[0046] The infrared reflectance of the surface of the processed pipe can be adjusted by the pigment of the rigid polyvinyl chloride resin composition constituting the processed pipe (if the processed pipe is multi-layered, the pigment of the rigid polyvinyl chloride resin composition constituting the outermost layer). The infrared reflectance of the surface of the processed pipe tends to increase as the content of pigment (I) in the pigment increases or the content of carbon black decreases. The infrared reflectance refers to the average value of the spectral reflectance in the wavelength range of 800 to 1600 nm, and the average value of the spectral reflectance in the wavelength range of 800 to 1100 nm is preferably 20% or more. The infrared reflectance is measured by an ultraviolet-visible-near infrared spectrophotometer. Details are as described in the Examples.

[0047] The ratio SDR (outer diameter / wall thickness, hereinafter also referred to simply as "SDR") of the outer diameter (mm) to the wall thickness (mm) of the processed pipe is 30 to 36, and preferably 31 to 34. If the SDR of the processed pipe is 30 or more, the physical strength such as compressive strength and tensile strength is excellent. If the SDR of the processed pipe is 36 or less, the workability is excellent.

[0048] The wall thickness and outside diameter of the processed pipe can be appropriately selected within the range of SDR 30-36 depending on the pipe joint to be manufactured. The outer diameter of the processed pipe is not particularly limited, but when at least one end of the pipe fitting is intended to be inserted into the socket portion of another pipe fitting, it is made the same as the inner diameter of the socket portion.

[0049] The processed pipe may be, for example, a VU pipe as specified in JIS K 6741. VU pipes are mainly used for drainage pipes (drainage pipes for detached houses, buried sewer pipes, etc.) and ventilation pipes. In general, the SDR of VU pipes is set to 30 to 38.

[0050] The shape of the processed pipe can be appropriately selected depending on the pipe joint to be manufactured. The processed tube may be, for example, straight. The cross-sectional shape of the processed tube may be, for example, circular, oval, square or rectangular.

[0051] From the viewpoint of manufacturing efficiency, the processed pipe is preferably an extrusion molded product. Unlike an injection molded product, the processed pipe, which is an extrusion molded product, does not have a gate mark, which is a mark left by introducing resin into a mold cavity (space), or a weld line, which indicates a location where resin flows in the mold cavity join together. Therefore, a pipe fitting obtained by subjecting the processed pipe to heat processing also does not have a gate mark or a weld line.

[0052] (Preparation process) In the preparation step, for example, a vinyl chloride resin, a pigment including the pigment (I), and, if necessary, additives are mixed together to prepare the present resin composition. The vinyl chloride resin, pigment, etc. can be mixed by a known method such as a hot blend method or a cold blend method.

[0053] (molding process) In the molding step, the resin composition is molded to obtain a processed pipe. In the molding step, the resin composition can be molded by a known molding method, and from the viewpoint of production efficiency, an extrusion molding method is preferred.

[0054] (heat processing process) In the heat processing step, the pipe to be processed is subjected to heat processing. Specifically, the processed portion of the pipe to be processed is heated to soften it and deform the processed portion.

[0055] Examples of the heat processing include bending and receiving. In the bending process, a bent portion is formed by bending a pipe to be processed. Thus, the resulting pipe joint has a bent portion. In the bending process, the bent portion is typically a portion other than the end portion of the pipe to be processed. In socket machining, the end of the pipe is enlarged to form a socket, so that the resulting pipe fitting has a socket. The heating process may include both bending and receiving of the pipe, in which case the resulting pipe joint has a bent portion and a receiving portion.

[0056] As a method for heating the processed part, from the viewpoint of productivity, a method of irradiating the processed part with infrared rays by an infrared heater is preferable. The output of the infrared heater can be, for example, in the range of 250 to 1000 W. The shape of the infrared heater can be, for example, a rod shape or a plate shape. The distance between the processed part and the infrared heater can be adjusted, for example, in the range of 5 cm to 50 cm. When irradiating infrared rays, the processed pipe and the infrared heater may be rotated relatively to heat the processed part uniformly. In this case, only the processed pipe may be rotated, only the infrared heater may be rotated, or both of them may be rotated. The rotation speed can be appropriately adjusted according to the output of the infrared heater and the distance between the processed part and the infrared heater. However, the heating method is not limited to the above method, and other heating methods may be adopted.

[0057] The heating time when the heat processing is performed is set so that the ratio T / SDR (hereinafter, also simply referred to as "T / SDR") of the heating time T (seconds) converted to the SDR of the processed pipe when an infrared heater with an output of 500 W is used is 40 to 150, preferably 50 to 140, and more preferably 60 to 130. In other words, the heating time (seconds) is set in consideration of the amount of heat per unit time when the heat processing is actually performed so that the value of "amount of heat per unit time x heating time (seconds)" when the heat processing is actually performed is equal to the value of "amount of heat per unit time x heating time T (seconds)" when an infrared heater with an output of 500 W is used. If T / SDR is 40 or more, the workability is excellent and whitening is unlikely to occur. If T / SDR is 150 or less, the productivity is excellent and discoloration (burning) is unlikely to occur.

[0058] When heating using an infrared heater, the amount of heat is proportional to the output, so the heating time (seconds) when heat processing is performed is calculated as "T x 500 (W) / output (W) of the infrared heater." For example, if the output of the infrared heater is 500W, the heating time when heat processing is performed is T (seconds). If the output of the infrared heater is 1000W, the heating time when heat processing is performed is T x 500 / 1000 (seconds). If the output of the infrared heater is 250W, the heating time when heat processing is performed is T x 500 / 250 (seconds). For example, when the SDR of the processed tube is 33 and the output of the infrared heater is 500 W, the heating time (infrared radiation irradiation time) is set to 1300 to 5000 seconds, and preferably 1600 to 4500 seconds.

[0059] The heating time during heat processing is preferably set so that the surface temperature after heating is 115 to 160°C, and more preferably 125 to 150°C. If the surface temperature after heating is equal to or higher than the lower limit, even if the thickness of the processed pipe is large, the temperature of the processed pipe is sufficiently high, the processed pipe can be favorably heat processed, and whitening is unlikely to occur. If the surface temperature after heating is equal to or lower than the upper limit, discoloration (burning) or unintended deformation is unlikely to occur in the portion to be bent.

[0060] The bending process can be carried out by a known method, except that the heating conditions during bending are as described above. The radius of curvature R of the curved portion formed by bending may be, for example, 450 to 2100 mm. The bending angle of the curved portion may be, for example, 15 to 90°.

[0061] The opening can be carried out by a known method, except that the heating conditions for the opening are as described above. The inner diameter of the socket part formed by processing the socket may be, for example, 114 to 630 mm. Note that this also includes cases where the inner surface of the socket is tapered, such as a TS socket, or where the inner diameter is made 1 to 10 mm larger than the above inner diameter to provide a gap between the inserted pipe and the inner surface of the socket for clearance. The inner diameter of the socket is preferably 114 mm or more, more preferably 165 mm or more, and particularly preferably 216 mm or more. Pipe fittings having a large-diameter socket with an inner diameter of 114 mm or more are difficult to manufacture by injection molding because it is difficult to fill the mold cavity (space) evenly with resin and the injection pressure of the resin by the injection molding machine becomes significantly high. According to the present invention, pipe fittings having such large-diameter sockets can be manufactured.

[0062] [Pipe fittings] The pipe joint of the present invention is made of a gray rigid polyvinyl chloride resin composition, and has a processed portion which has been subjected to a heat processing and an unprocessed portion which has not been subjected to the heat processing. The grey rigid polyvinyl chloride resin composition is as described above. The heat processing is as described above. The processed portion can be exemplified by a receiving portion and a curved portion. The unprocessed portion is typically a straight tube. The pipe joint of the present invention may be a single layer or a multilayer. When it is a multilayer, the grey rigid vinyl chloride resin composition constituting each layer may be the same or different.

[0063] The surface infrared reflectance of the pipe joint of the present invention is 20% or more, preferably 25% or more, and more preferably 30% or more. If the surface infrared reflectance is 20% or more, the pipe joint has excellent heat shielding properties, and the temperature of the pipe joint is less likely to increase when exposed to sunlight, and warping and deterioration are less likely to occur. From the viewpoint of heat insulation, the higher the infrared reflectance of the surface of the pipe fitting of the present invention, the better, and there is no particular upper limit. However, from the viewpoint of ease of application of the socket processing or bending processing when manufacturing the pipe fitting of the present invention, it is preferably 60% or less.

[0064] The SDR of the unprocessed part is 30-36, and 31-34 is preferable.

[0065] In the pipe joint of the present invention, the color difference between the processed portion and the unprocessed portion is preferably 5 or less, more preferably 3 or less, even more preferably 2 or less, and particularly preferably 1 or less. If the color difference between the processed portion and the unprocessed portion is 5 or less, the appearance is more excellent. The color difference can be adjusted by adjusting the heating conditions when the pipe to be processed is subjected to heat processing. The lower the heating temperature or the shorter the heating time, the smaller the color difference tends to be. The color difference refers to the color difference (ΔE) in the L*a*b* color system defined in JIS Z8781-4:2013.

[0066] The shape of the pipe joint of the present invention can be appropriately selected. A pipe fitting according to one aspect of the present invention includes a body portion and a socket portion. The main body is formed in a cylindrical shape having the same diameter. The main body may be straight or may have a bent portion. The cross-sectional shape of the main body may be, for example, circular, elliptical, square, or rectangular. The outer diameter of the main body is the same as the outer diameter of the processed tube. The socket portion is formed at the end of the pipe joint with a larger diameter than the body portion. The socket portion is typically thinner than the body portion. The cross-sectional shape of the socket portion may be, for example, circular or elliptical. The preferred inner diameter of the socket portion is as described above. The number of socket portions may be one or more.

[0067] A pipe joint according to another aspect of the present invention includes a main body portion having a straight pipe portion and a bent portion. The main body is similar to the main body of the pipe joint of the above-mentioned embodiment, except that it has a bent portion. The pipe fitting of this embodiment may include a socket portion similar to the socket portion of the pipe fitting of the embodiment described above.

[0068] An example of a pipe fitting is shown in Figure 1. The pipe fitting 1 in this example comprises a straight pipe section 2 (main body) formed in a cylindrical shape with the same diameter, and a socket section 3 formed with an enlarged diameter on one end side of the straight pipe section 2. The straight pipe section 2 and the socket section 3 are connected by a tapered pipe section 4. The other end of the straight pipe section 2 is an insertion section 5 that is inserted into a socket 3 of another pipe fitting 1. The outer peripheral surface of the tip of the insertion section 5 is an inclined surface 5a that is gradually tapered toward the tip. An insertion mark 6 is provided on the outer peripheral surface of the straight pipe section 2 to determine the depth of insertion into the socket 3 of the other pipe fitting 1. The receiving portion 3 has an expanded diameter portion 3a formed around the entire inner circumferential surface of the receiving portion 3 for accommodating a rubber ring 11 as a waterproofing material. The receiving portion 3 is formed with the same diameter except for the expanded diameter portion 3a. The inner diameter (minimum inner diameter) of the receiving portion 3 is the same as the outer diameter of the insertion portion 5.

[0069] Another example of a pipe fitting is shown in Figure 2. The pipe fitting 1 of this example is similar to the pipe fitting 1 of Figure 1 except for the shape of the socket portion 3. In this example, the socket portion 3 has a shape in which the diameter decreases from the tapered pipe portion 4 to the enlarged diameter portion 3a.

[0070] Another example of a pipe fitting is shown in Figure 3. The pipe fitting 1 of this example comprises a main body portion 7 formed in a cylindrical shape having the same diameter, and a socket portion 3 formed with an expanded diameter on one end side of the main body portion 7. The main body portion 7 and the socket portion 3 are connected by a tapered pipe portion 4. The main body 7 has a bent portion 7a, a first straight pipe portion 7b located at the other end side of the bent portion 7a, and a second straight pipe portion 7c located at one end side of the bent portion 7a. In this example, the bend angle of the bent portion 7a (the inclination angle of the axis l2 of the second straight pipe portion 7c with respect to the axis l1 of the first straight pipe portion 7b) is set to 15°. The other end of the first straight pipe section 7b is an insertion section 5 that is inserted into the receiving portion 3 of another pipe fitting 1, similar to the pipe fitting in Figure 1, and the outer peripheral surface of the tip of the insertion section 5 is an inclined surface 5a that is gradually tapered in diameter toward the tip. The inner diameter of the receiving portion 3 is the same as the outer diameter of the insertion portion 5 .

[0071] The pipe joint of the present invention preferably has no gate marks or weld lines. Typically, such a pipe joint is produced by subjecting a processed pipe formed by extrusion molding to heat processing. It is particularly preferred that the pipe joint of the present invention has a socket portion having an inside diameter of 114 mm or more and has no gate marks or weld lines. The more preferred inside diameter of the socket portion is as described above. EXAMPLES

[0072] The present invention will now be described in more detail with reference to the following examples, but the present invention is in no way limited to these examples. Examples 2 and 7 are reference examples.

[0073] (Examples 1 to 8, Comparative Examples 1 to 3) <Preparation of Rigid Polyvinyl Chloride Resin Composition> According to the formulations shown in Tables 1 to 3, pigments and dispersants were mixed to prepare pigment compositions, and the resulting pigment compositions, vinyl chloride resins, and additives were stirred and mixed by a cold blend method in a Super Mixer (100 L, manufactured by Kawata Corporation) to obtain rigid vinyl chloride resin compositions. Details of each component shown in Tables 1 to 3 are as follows.

[0074] · Vinyl chloride resin: Vinyl chloride homopolymer (product name "TS-1000R", manufactured by Tokuyama Sekisui Kogyo Co., Ltd., average degree of polymerization 1000). Lead stearate: Product name "SAK-NSBN", manufactured by Sun Ace Corporation. Calcium carbonate: Product name "Whiten 305S", manufactured by Shiraishi Calcium Co., Ltd. Titanium oxide: White inorganic pigment, product name "R-3L", manufactured by Sakai Chemical Industry Co., Ltd. Chromium compounds: A complex oxide of chromium oxide and iron oxide, a black inorganic pigment. ·Cobalt Blue: Blue inorganic pigment. · Copper Phthalocyanine: A blue organic pigment. ·Diketopyrrolopyrrole: Red organic pigment. ·Monoazo Yellow: Yellow organic pigment. Carbon black: Product name "Touka Black #7350", manufactured by Tokai Carbon Co., Ltd. Dispersant: Silica.

[0075] <Forming of processed pipes> The rigid polyvinyl chloride resin composition obtained above was fed to a twin-screw counter-rotating extruder (product name "SLM-50", manufactured by Nagata Manufacturing Co., Ltd.) and molded into a straight processed pipe having an outer diameter and wall thickness shown in Tables 1 to 3 and a length of 1 m. The SDR of the processed pipe is also shown in Tables 1 to 3.

[0076] <Processing of pipe to be processed> The obtained processed pipe was subjected to bending (heat processing) in the following manner to obtain a pipe joint. Using a rod-shaped infrared heater (quartz tube) with an output of 500 W and a reflector attached, the pipe to be processed was heated while rotating under the conditions (infrared heater output, heating time) shown in Tables 1 to 3. The T / SDR and surface temperature after heating at this time are also shown in Tables 1 to 3. Immediately after heating was completed, the pipe to be processed was fixed to a bending die set at an angle of 90° and the heated portion was bent to form a bend with a bending angle of 90° and a curvature radius of R1200 mm. After cooling, the pipe joint was removed from the bending die.

[0077] The obtained pipe joint was subjected to the following measurements.

[0078] <Infrared reflectance measurement> The spectral reflectance of the surface of the pipe fitting was measured at wavelengths of 800 to 1100 nm using an ultraviolet-visible-near infrared spectrophotometer (Shimadzu Corporation, "UV-3600Plus"), and the average value was taken as the infrared reflectance of the surface of the pipe fitting. The results are shown in Tables 1 to 3. The spectral reflectance curves of Examples 1 and 3 and Comparative Example 1 are shown in Figure 4.

[0079] <Color difference measurement> The chromaticity of the surface of the processed part (bent part or socket part) of the pipe joint and the surface of the unprocessed part (straight pipe part) were measured in a dark room using a spectrophotometer (handy spectrophotometer "NF333" manufactured by Nippon Denshoku Industries Co., Ltd.) The results are shown in Tables 1 to 3. Here, the color difference (ΔE) is calculated by the following formula (1). ΔE=√((L1-L2) 2 +(a1-a2) 2 +(b1-b2) 2 ) · · · (1) In formula (1), L1, a1, and b1 respectively represent the lightness L of the processed part, the chromaticity a in the red direction, and the chromaticity b in the yellow direction, while L2, a2, and b2 respectively represent the lightness L of the unprocessed part, the chromaticity a in the red direction, and the chromaticity b in the yellow direction.

[0080] [Table 1]

[0081] [Table 2]

[0082] [Table 3]

[0083] In Examples 1 to 8, in which processed pipes containing pigment (I), with a surface infrared reflectance of 20% or more and an SDR of 40 to 150, were heated under predetermined heating conditions and subjected to heat processing, the processed pipes could be processed well. In addition, the color difference between the processed part and the unprocessed part was less than 5. [Explanation of symbols]

[0084] 1 Pipe fittings 2 Straight pipe section 3 Socket 4 Tapered pipe section 5 Insertion section 6 Insertion line 7 Main body 7a Bend 7b First straight pipe section 7c Second straight pipe section 11 Rubber Ring

Claims

1. A piping comprising a straight pipe which is an extrusion molded product of a gray rigid polyvinyl chloride resin composition containing a rigid polyvinyl chloride resin and a pigment and which has been subjected to a heat treatment, the piping having a processed portion which has been subjected to the heat treatment and a straight unprocessed portion which has not been subjected to the heat treatment, the processed portion being either a bent portion or a receiving portion, The pigment is composed of a non-carbon-based inorganic pigment and an organic pigment, and is substantially free of carbon black; the organic pigment includes at least a blue organic pigment, A pipe, wherein the color difference between the processed portion and the unprocessed portion is 5 or less.

2. A pipe made of a gray rigid polyvinyl chloride resin composition containing a rigid polyvinyl chloride resin and a pigment, the pipe having a bent portion formed by a heat processing and a straight pipe-shaped insertion portion to be inserted into another pipe, the pipe having no gate mark and / or weld line, The pigment is composed of a non-carbon-based inorganic pigment and an organic pigment, and is substantially free of carbon black; the organic pigment includes at least a blue organic pigment, A pipe having a color difference between the bent portion and the inserted portion of 5 or less.

3. A pipe made of a gray rigid polyvinyl chloride resin composition containing a rigid polyvinyl chloride resin and a pigment, the pipe having a processed portion that has been subjected to a heat processing and a straight, unprocessed portion that has not been subjected to the heat processing, the processed portion having no gate mark and / or weld line, the processed portion being either a bent portion or a receiving portion, The pigment is composed of a non-carbon-based inorganic pigment and an organic pigment, and is substantially free of carbon black; the organic pigment includes at least a blue organic pigment, A pipe, wherein the color difference between the processed portion and the unprocessed portion is 5 or less.

4. The piping according to any one of claims 1 to 3, wherein the organic pigment comprises a phthalocyanine-based pigment.

5. The piping according to any one of claims 1 to 4, wherein a total content of the non-carbon-based inorganic pigment and the organic pigment is 0.01 to 1.0 parts by mass per 100 parts by mass of the rigid polyvinyl chloride resin.

6. The pipe according to any one of claims 1 to 5, wherein the non-carbon-based inorganic pigment comprises a colored non-carbon-based inorganic pigment and a white non-carbon-based inorganic pigment.

7. The piping according to claim 1 or 3, wherein the processed portion is a bent portion.

8. The piping according to claim 7 , wherein the bend is formed at a location other than an end of the piping.

9. A method for producing a pipe for processing comprising a step of subjecting a straight pipe to a heat treatment, the straight pipe being made of a gray rigid polyvinyl chloride resin composition containing a rigid polyvinyl chloride resin and a pigment; The step of performing the heat processing is a step of heating and softening the processed portion of the processed pipe by irradiating the processed portion with infrared rays using an infrared heater, thereby deforming the processed portion; The pigment is composed of a non-carbon-based inorganic pigment and an organic pigment, and is substantially free of carbon black; the organic pigment includes at least a blue organic pigment, A manufacturing method for piping, characterized in that the heating time during the heat processing is set so that the ratio T / SDR of the heating time T (seconds) converted when an infrared heater with an output of 500 W is used as the infrared heater to the ratio SDR of the outer diameter (mm) to the wall thickness (mm) of the processed pipe is 40 to 150, thereby making the color difference between the processed part that has been heat processed and the unprocessed part that has not been heat processed 5 or less.

10. A method for manufacturing piping as described in claim 9, wherein in the heat processing step, the surface temperature of the processed part after heating by the infrared heater is 115 to 160°C.

11. A method for manufacturing piping as described in claim 9 or 10, wherein the heating process is either one or both of bending and receiving processing.

12. A method for manufacturing piping described in any one of claims 9 to 11, wherein the processed pipe does not have gate marks and / or weld lines.

Citation Information

Patent Citations

  • Vinyl chloride-based resin molded product and vinyl chloride-based resin composition

    JP1999310675A

  • Method for color-changing for resin pipe

    JP2000334801A

  • Conduit line forming method

    JP2001251747A

  • Hard vinyl chloride resin pipe

    JP2003329176A

  • Hard vinyl chloride resin tube

    JP2005155901A