Aluminum cans for filling wine and aluminum cans for filling wine
A laminated resin film with dimer acid copolymerized polyester resin and calcium carbonate in the adhesive layer addresses the corrosion and flavor deterioration issues in aluminum wine cans by controlling sulfite reactions, maintaining wine quality.
Patent Information
- Application Number
- JP2023510051
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-31
- Publication Date
- 2024-12-09
- Estimated Expiration
- 2041-03-31
AI Technical Summary
The corrosion of aluminum cans due to sulfurous acid in wine and the deterioration of wine flavor caused by hydrogen sulfide generation during the redox reaction between sulfurous acid and aluminum are significant issues in wine packaging in aluminum cans.
A combination of a specific coating on the inner side of aluminum cans, comprising a resin film with a laminated structure of dimer acid copolymerized polyester resin layers and an adhesive layer containing calcium carbonate, which prevents the corrosion of aluminum cans and deterioration of wine flavor by reacting with sulfite in wine.
The solution effectively reduces the likelihood of aluminum can corrosion and wine flavor deterioration by maintaining low molecular SO2 and chloride ion concentrations, ensuring the quality of wine over extended storage periods.
Smart Images

Figure 0007596514000003 
Figure 0007596514000004 
Figure 0007596514000005
Abstract
Description
[Technical field]
[0001] The present invention relates to an aluminum can for filling wine and an aluminum can for filling wine. [Background technology]
[0002] In wine, an appropriate amount of sulfurous acid is usually added as an essential additive for suppressing wild yeast during fruit juice fermentation and for regulating aging. When such wine is filled into aluminum cans, there are problems in that the sulfurous acid added to the wine is corrosive and easily corrodes the aluminum cans, and that hydrogen sulfide is generated by an oxidation-reduction reaction between sulfurous acid and aluminum, deteriorating the flavor of the wine.
[0003] Some of the sulfurous acid added to wine is combined with sugars, aldehydes, anthocyanins, etc., and exists in the form of "combined sulfurous acid," while the remaining sulfurous acid exists in the form of "free sulfurous acid." Most of the free sulfurous acid is HSO3 - (bisulfite ion), and the rest is in the form of SO2 (molecular SO2). The ratio of bisulfite ion to molecular SO2 varies depending on the pH.
[0004] For example, U.S. Patent No. 5,393,633 discloses a method for packaging wine in aluminum cans, producing wine having less than 35 ppm free sulfurous acid, less than 300 ppm chloride, and less than 800 ppm sulfate, and providing an anti-corrosion coating to the inside surface of the aluminum can. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] WO 03 / 029089 Summary of the Invention [Problem to be solved by the invention]
[0006] In view of the above problems, an object of the present invention is to provide wine packed in an aluminum can and an aluminum can for filling wine, which are less susceptible to corrosion of the aluminum can and flavor deterioration of the wine. [Means for solving the problem]
[0007] The inventors have newly discovered that the above-mentioned problems (i.e., the problem of corrosion of aluminum cans and the problem of flavor deterioration of wine) can be solved by combining a specific coating on the inner surface of an aluminum can with a specific composition of wine, and have completed the present invention.
[0008] That is, according to one aspect of the present invention, an aluminum can comprising an aluminum plate, a resin film provided on a surface of the aluminum plate that will become an inner surface of the can, and an adhesive layer interposed between the aluminum plate and the resin film to bond them together, the resin film comprising a first resin layer as an outermost layer and a second resin layer containing a dimer acid copolymerized polyester resin, and at least one of the resin layers and the adhesive layer that constitute the resin film contains calcium carbonate; Wine sealed in the aluminum can containing 4.3 mg / L or less of molecular SO2 and 350 mg / L or less of chloride ions; Aluminum cans containing wine is provided.
[0009] According to another aspect of the present invention, An aluminum can for filling wine, comprising: an aluminum plate; a resin film provided on a surface of the aluminum plate that will become the inner surface of the can; and an adhesive layer interposed between the aluminum plate and the resin film to bond them together, the resin film comprising a first resin layer as an outermost layer and a second resin layer containing a dimer acid copolymerized polyester resin, and at least one of the resin layers and the adhesive layer that constitute the resin film contains calcium carbonate. is provided. Effect of the Invention
[0010] According to the present invention, it is possible to provide wine packed in an aluminum can and an aluminum can for filling wine which are less susceptible to corrosion of the aluminum can and flavor deterioration of the wine. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a partially cutaway side view showing an example of an aluminum can for filling wine. [Diagram 2] FIG. 2 is a cross-sectional view showing an example of the layer structure of an aluminum can for filling wine. [Diagram 3] FIG. 3 is a cross-sectional view showing another example of the layer structure of an aluminum can for filling wine. [Figure 4] Figure 4 is a scatter plot showing the effect of molecular SO2 and chloride ion concentrations in wine on its applicability to aluminum cans. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The present invention will be described below. However, the following description is intended to explain the present invention in detail and is not intended to limit the present invention.
[0013] 1.Aluminum cans filled wine According to one aspect, there is provided an aluminum can filled wine, the aluminum can filled wine comprising: an aluminum can comprising an aluminum plate, a resin film provided on a surface of the aluminum plate that will become an inner surface of the can, and an adhesive layer interposed between the aluminum plate and the resin film to bond them together, the resin film comprising a first resin layer as an outermost layer and a second resin layer containing a dimer acid copolymerized polyester resin, and at least one of the resin layers and the adhesive layer that constitute the resin film contains calcium carbonate; Wine sealed in the aluminum can containing 4.3 mg / L or less of molecular SO2 and 350 mg / L or less of chloride ions; Includes.
[0014] As described above, the present invention can reduce corrosion of aluminum cans and flavor deterioration of wine by combining a specific coating on the inner surface of an aluminum can (i.e., the above-mentioned resin film) with a specific composition of wine (i.e., the above-mentioned molecular SO2 concentration and chloride ion concentration).
[0015] Aluminum canned wine can be produced by filling an aluminum can body with wine, and then seaming a separate cap onto the aluminum can body according to a known seaming process.
[0016] Below, we will explain "wine" having a specific composition and "aluminum cans" having a specific coating on the inside surface.
[0017] 1-1.Wine Wine packaged in aluminum cans contains less than 4.3 mg / L of molecular SO2 and less than 350 mg / L of chloride ions.
[0018] In this specification, "molecular SO2 concentration" refers to a value calculated by the following formula.
number
[0019] The values of "pH," "alcohol concentration," and "free sulfite concentration" used to calculate the molecular SO2 concentration refer to values measured as follows.
[0020] In other words, "pH" refers to the value measured with a pH meter for wine at 20°C. "Alcohol concentration" refers to the value measured by liquid chromatography. "Free sulfite concentration" refers to the value measured by aeration distillation and titration method (Rankine method).
[0021] The molecular SO2 concentration in wine is 0 to 4.3 mg / L, preferably 1 to 3 mg / L, and more preferably 1 to 2 mg / L. If the molecular SO2 concentration in wine exceeds 4.3 mg / L, corrosion of aluminum cans and deterioration of the flavor of wine are likely to occur.
[0022] As used herein, the term "chloride ion concentration" refers to a value measured by potentiometric titration.
[0023] The chloride ion concentration in wine is 0 to 350 mg / L, preferably 0 to 200 mg / L, and more preferably 0 to 100 mg / L. If the chloride ion concentration in wine exceeds 350 mg / L, corrosion of aluminum cans and deterioration of the flavor of wine are likely to occur.
[0024] 1-2.Aluminum cans FIG. 1 shows an example of an aluminum can for filling wine (hereinafter, also simply referred to as an aluminum can). The aluminum can 1 shown in FIG. 1 is composed of a container body 2, a bottom lid 3, and a cap (not shown). The container body 2 and the bottom lid 3 are collectively referred to as an aluminum can body. The container body 2 has a neck portion 2a, a shoulder portion 2b, and a body portion 2c as an integral part. The bottom lid 3 is integrally roll-sewn and fixed to the container body 2 so as to close the lower end opening of the body portion 2c. Although not shown, a pill-proof cap, which is a separate part, is attached to the neck portion 2a by roll-on molding using a well-known capper so as to be resealable (reclosed) by screwing. Although a three-piece type bottle can is shown in FIG. 1, the aluminum can 1 may be a two-piece type bottle can, i.e., a bottle can in which the container body 2 and the bottom lid 3 are integrally formed.
[0025] In order to prevent corrosion of the aluminum can 1, the aluminum can has a resin coating described below on the inner surface of the can (i.e., the inner surface of the container body 2, the inner surface of the bottom lid 3, and the inner surface of the cap). The aluminum can 1 may also have a resin coating on the outer surface of the can (i.e., the outer surface of the container body 2, the outer surface of the bottom lid 3, and the outer surface of the cap).
[0026] Specifically, the aluminum can includes an aluminum plate, a resin film provided on a surface of the aluminum plate that will become the inner surface of the can, and an adhesive layer that is interposed between the aluminum plate and the resin film and bonds them together, the resin film includes a first resin layer as an outermost layer and a second resin layer including a dimer acid copolymerized polyester resin, At least one of the resin layer and the adhesive layer constituting the resin film contains calcium carbonate.
[0027] An example of the layer structure of such an aluminum can is shown in FIG. 2, and another example of the layer structure of such an aluminum can is shown in FIG.
[0028] An aluminum can having the layer structure shown in FIG. 2 (hereinafter also referred to as the aluminum can according to the first embodiment) includes an aluminum plate 10, a resin film 12 provided on a surface of the aluminum plate 10 that will become the inner surface of the can, and an adhesive layer 11 that is interposed between the aluminum plate 10 and the resin film 12 and bonds them together. The resin film 12 is a laminated film having a two-layer structure, and is composed of a first resin layer 12a as an outermost layer and a second resin layer 12b containing a dimer acid copolymerized polyester resin, The adhesive layer 11 contains calcium carbonate 14 .
[0029] An aluminum can having the layer structure shown in FIG. 3 (hereinafter also referred to as an aluminum can according to a second embodiment) includes an aluminum plate 10, a resin film 12 provided on a surface of the aluminum plate 10 that will become the inner surface of the can, and an adhesive layer 11 that is interposed between the aluminum plate 10 and the resin film 12 and bonds them together. the resin film 12 is a laminated film having a three-layer structure, and is composed of a first resin layer 12a as an outermost layer, a second resin layer 12b containing a dimer acid copolymer polyester resin as an intermediate layer, and a third resin layer 12c as an outermost layer on a surface facing the adhesive layer 11; The adhesive layer 11 contains calcium carbonate 14 .
[0030] The aluminum can according to the first embodiment is the same as the aluminum can according to the second embodiment except that the third resin layer 12c included in the aluminum can according to the second embodiment is omitted. Therefore, the aluminum can according to the second embodiment will be described below.
[0031] 1-2-1.Resin film 12 In the second embodiment, the resin film 12 provided on the surface of the aluminum plate 10 that faces the can inner surface is a laminated film having a three-layer structure. As shown in the figure, the laminated film having a three-layer structure is composed of a first resin layer 12a, a second resin layer 12b, and a third resin layer 12c. Specifically, the first resin layer 12a can be a resin film mainly containing (i.e., at a content rate of 50% by mass or more) an isophthalic acid copolymerized polyester resin containing 3 to 15 mol% of isophthalic acid with respect to the total acid amount of the first resin layer 12a. The second resin layer 12b can be a resin film mainly containing (i.e., at a content rate of 50% by mass or more) a dimer acid copolymerized polyester resin containing 5 to 50 mol% of dimer acid with respect to the total acid amount of the second resin layer 12b. The third resin layer 12c may be a resin film mainly containing (i.e., at a content of 50 mass % or more) isophthalic acid copolymerized polyester resin containing 3 to 15 mol % of isophthalic acid with respect to the total acid amount of the third resin layer 12c. The first resin layer 12a, the second resin layer 12b, and the third resin layer 12c each have a thickness of, for example, 3 to 10 μm. The resin film 12 preferably has a dimer acid ratio of 3 to 30 mol % with respect to the total acid amount in the entire film.
[0032] This three-layer laminate film contains a dimer acid copolymer polyester resin, which allows the resin film 12 to have flexibility. The use of such a resin film 12 has excellent flexibility, which results in good film formability, and is less susceptible to film breakage (hair) and chipping (galling) during the drawing and ironing process during can manufacturing. Furthermore, even if the can is dropped or subjected to an external impact (dent) after the contents are sealed in the can and manufactured, the film surface is not damaged and the aluminum can is less susceptible to corrosion. In other words, the quality of the inner surface of the aluminum can can be ensured.
[0033] In addition, in this three-layer laminate film, the second resin layer 12b contains a dimer acid copolymer polyester resin, has high-temperature adhesion, and is soft and easily damaged at room temperature, but the second resin layer 12b is sandwiched between the first resin layer 12a and the third resin layer 12c, each of which contains an isophthalic acid copolymer polyester resin, so that the ease of handling of the resin film 12 can be improved. That is, the first resin layer 12a and the third resin layer 12c are non-adhesive even at high temperatures and have relatively robust properties at room temperature, so there is no trouble of winding around a high-temperature stretching roll during film formation, and there is no risk of damage during transportation during aluminum can formation. However, the aforementioned winding around the stretching roll and damage during aluminum can transportation may be solved by taking special measures such as surface treatment of the parts where the trouble occurs or by taking measures such as reducing the production speed, and the first resin layer 12a and the third resin layer 12c can be omitted by taking measures in production technology.
[0034] Although not shown, a resin film may be provided on the surface of the aluminum plate 10 that will become the outer surface of the can. This outer resin film may be, for example, a blend resin of polybutylene terephthalate and isophthalic acid copolymerized polyethylene terephthalate (PBT / copolymerized PET). The outer resin film has a thickness of, for example, 5 to 20 μm.
[0035] 1-2-2. Adhesive layer 11 The above-mentioned resin film 12 can be adhered to the aluminum plate 10 by the adhesive layer 11. The adhesive layer 11 can be, for example, an adhesive made of a thermosetting epoxy resin. It is preferable that the adhesive layer 11 does not contain bisphenol A type epoxy resin. There is a concern that bisphenol A type epoxy resin is an endocrine disrupting substance. For this reason, not containing bisphenol A type epoxy resin is preferable in that it is possible to reliably prevent the elution of bisphenol A type epoxy resin into the contents of the can container. In order to increase the adhesiveness without containing bisphenol A type epoxy resin, for example, it is preferable that the content ratio (mass ratio) of polyester resin to phenol resin is 10 to 40:0 to 20. The adhesive layer 11 has a thickness of, for example, 2 to 20 μm.
[0036] In the first and second embodiments, calcium carbonate 14 is contained in the adhesive layer 11 in the form of particles. Calcium carbonate 14 functions as an acid scavenger that reacts with sulfurous acid. Therefore, calcium carbonate 14 can prevent sulfurous acid contained in wine from permeating through the resin film 12 and reaching the aluminum plate 10. As a result, it is possible to prevent corrosion of aluminum cans and to prevent deterioration of the flavor of wine caused by the generation of hydrogen sulfide due to the reaction between sulfurous acid and aluminum.
[0037] The particles of calcium carbonate 14 have an average particle size of, for example, 0.01 to 4.0 μm, and preferably an average particle size of 0.01 to 0.1 μm. The amount of calcium carbonate 14 added can be, for example, 5 to 50 parts by mass with respect to 100 parts by mass of the adhesive resin. If the amount of calcium carbonate added is small, the above effects tend to decrease, and if the amount of calcium carbonate added is large, the formability of the resin film 12 tends to decrease.
[0038] The calcium carbonate 14 is preferably contained in the adhesive layer 11. In this case, the calcium carbonate 14 can effectively capture sulfurous acid contained in wine. The calcium carbonate 14 may be further contained in any layer of the resin film 12 in addition to the adhesive layer 11. Alternatively, the calcium carbonate 14 may be contained in any layer of the resin film 12 instead of the adhesive layer 11. In this case, it is preferable that the resin film 12 is composed of multiple layers, and contains the calcium carbonate 14 in a layer other than the outermost layer. If the calcium carbonate 14 is contained in a layer of the resin film 12 other than the outermost layer, the possibility of microscopic defects occurring during the forming process of the aluminum can can be eliminated.
[0039] 1-2-3. Details of Resin Film 12 The resin film 12 in the second embodiment will be described in detail below.
[0040] <First resin layer 12a> The first resin layer 12a may be a resin film containing, for example, 50 to 100 mass % of isophthalic acid copolymerized polyester resin, which contains 3 to 15 mol % of isophthalic acid relative to the total acid content of the first resin layer 12a. Such a resin film is non-adhesive at around 130°C.
[0041] The "isophthalic acid copolymerized polyester resin" is, for example, composed of dicarboxylic acid units containing 85 to 97 mol % of a terephthalic acid component and 15 to 3 mol % of an isophthalic acid component, and diol units containing 90 mol % or more of an ethylene glycol component. That is, the "isophthalic acid copolymerized polyester resin" is, for example, composed mainly of ethylene terephthalate, with 3 to 15 mol % of an isophthalic acid component copolymerized therein. Copolymerization of an isophthalic acid component can impart flexibility to the film. This can prevent fine cracks from occurring on the surface during the molding of aluminum cans.
[0042] In the isophthalic acid copolymerized polyester resin, dicarboxylic acid units other than the terephthalic acid component and the isophthalic acid component may be contained within a range that does not impair lamination properties to an aluminum plate or the properties of an aluminum can, for example, within a range of 10 mol % or less. Examples of such dicarboxylic acid units include succinic acid, adipic acid, azelaic acid, sebacic acid, 1,4-naphthalenedicarboxylic acid, 4,4'-biphenyldicarboxylic acid, 1,12-dodecanoic acid, 1,2-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, and 1,4-cyclohexanedicarboxylic acid, and these may be used alone or in combination of two or more kinds.
[0043] In addition, the isophthalic acid copolymerized polyester resin may contain diol units other than the ethylene glycol component in an amount of 10 mol % or less. Examples of such diol units include aliphatic diols such as diethylene glycol, triethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, and neopentyl glycol, and alicyclic diols such as 1,4-cyclohexanedimethanol and 1,4-cyclohexanediethanol, which may be used alone or in combination of two or more.
[0044] The isophthalic acid copolymerized polyester resin is obtained by esterification reaction of the dicarboxylic acid component and the diol component by a known method. For example, a method of carrying out an ester exchange reaction with the diol component by adding a catalyst using a starting material in which a methyl group is added to the end of the dicarboxylic acid component, or a method of carrying out a direct esterification reaction with the diol component using a dicarboxylic acid component whose end is unmodified as a starting material. Alternatively, a commercially available isophthalic acid copolymerized polyethylene terephthalate resin may be used, and examples of commercially available products include IP121B, PIFG8, and PIFG10 (all manufactured by Bell Polyester Products Co., Ltd.). The intrinsic viscosity of the isophthalic acid copolymerized polyester resin is not particularly limited, but is preferably 0.7 to 0.9.
[0045] The above-mentioned isophthalic acid copolymerized polyester resin can be used by forming it into a film alone, but other polyester resins, such as polyethylene terephthalate resin, polybutylene terephthalate resin, polytrimethylene terephthalate resin, etc., may be used alone or in combination as a blend in a proportion of less than 50 mass % relative to the isophthalic acid copolymerized polyester resin.
[0046] <Second resin layer 12b> The second resin layer 12b may be a resin film containing a dimer acid copolymerized polyester resin at a content of, for example, 50 to 100% by mass.
[0047] The "dimer acid copolymer polyester resin" is, for example, 50 to 93 mass % of an ester oligomer (A) having a number average molecular weight of 700 or less, the ester oligomer (A) comprising dicarboxylic acid units (a1) containing 70 mol % or more of a terephthalic acid component and diol units (a2) containing 70 mol % or more of an ethylene glycol component; 7 to 50% by mass of a polyester polyol (B) which is composed of hydrogenated dimer acid units (b1) and 1,4-butanediol units (b2) and has a number average molecular weight of 1500 to 3000; is a constituent unit.
[0048] [Ester Oligomer (A)] In the above dimer acid copolymerized polyester resin, the dicarboxylic acid unit (a1) contains 70 mol% or more of terephthalic acid units. The total amount of the dicarboxylic acid units may be terephthalic acid units. Alternatively, dicarboxylic acid components other than terephthalic acid may be contained in a range of less than 30 mol% as long as the lamination property to the aluminum plate and the characteristics during molding of the aluminum can are not impaired. Examples of dicarboxylic acid components other than terephthalic acid include isophthalic acid, succinic acid, adipic acid, azelaic acid, sebacic acid, 1,4-naphthalenedicarboxylic acid, 4,4'-biphenyldicarboxylic acid, 1,12-dodecanoic acid, 1,2-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, and 1,4-cyclohexanedicarboxylic acid, and these may be used alone or in a mixture of two or more kinds. Among these, from the viewpoint of improving the dent resistance of aluminum cans including a film coating (i.e., the property that the film surface is not broken and the aluminum plate is not easily corroded even when subjected to an external impact (dent)), for example, isophthalic acid can be suitably used in the range of about 1 to 30 mol %.
[0049] In the above dimer acid copolymerized polyester resin, the diol unit (a2) contains 70 mol% or more of ethylene glycol units. The total amount of the diol units may be ethylene glycol units. Alternatively, a diol component other than ethylene glycol may be contained in a range of less than 30 mol%. Examples of the diol component other than ethylene glycol include propylene glycol, butanediol, neopentyl glycol, diethylene glycol, cyclohexane dimethanol, etc., and these may be used alone or in a mixture of two or more kinds.
[0050] In the above dimer acid copolymerized polyester resin, the number average molecular weight of the ester oligomer (A) is 700 or less, preferably 300 to 700. By copolymerizing using the ester oligomer (A) having a number average molecular weight of 700 or less, the polyester polyol (B) is randomly bonded in the polymer chain, and a copolymerized polyester resin with a transparent appearance is obtained. In addition, since the obtained copolymerized polyester resin has good compatibility with other resins, problems such as a surging phenomenon (unstable extrusion phenomenon) do not occur when blended with other resins and melt extrusion is performed, and a film can be stably formed.
[0051] On the other hand, for example, when an ester oligomer having a number average molecular weight of more than 700 and around 1000 is used, the polymerization reaction plateaus in the copolymerization reaction with the polyester polyol (B), so that a copolymerized polyester resin having a high viscosity, for example, an intrinsic viscosity of about 0.7 to 0.9, cannot be obtained. In addition, when a polyester having a number average molecular weight of more than 5000 is used, the polymerization reaction plateaus and a high molecular weight copolymerized polyester resin can be obtained, but the copolymerized polyester resin obtained becomes a block copolymer of -(A)-(B)-type because the molecular weight of the ester (A) unit is large, and the appearance of the resin becomes cloudy due to phase separation. Furthermore, such a block copolymer has poor compatibility with other resins, so that a surging phenomenon (unstable discharge phenomenon) occurs during melt extrusion, and there is also a problem that a sheet or film cannot be formed.
[0052] The ester oligomer (A) can be obtained by esterifying a dicarboxylic acid component (a1) mainly composed of terephthalic acid with a diol component (a2) mainly composed of ethylene glycol by a known method. For example, a method of obtaining an oligomer by using a starting material in which a methyl group is added to the end of the dicarboxylic acid component (a1) and carrying out an ester exchange reaction with the diol component (a2) by adding a catalyst, or a method of obtaining an oligomer by directly esterifying a dicarboxylic acid component (a1) with an unmodified end and a diol component (a2) using the dicarboxylic acid component (a1) as a starting material.
[0053] In the production of the ester oligomer (A), for example, after a predetermined esterification rate is reached at a reaction temperature of 230 to 250°C, 3 to 10% by mass of diol (ethylene glycol) is added to the system relative to the total oligomer obtained, and the depolymerization reaction is preferably carried out for about 30 minutes to 1 hour while maintaining the internal temperature at 230 to 250°C. By carrying out a depolymerization reaction using a diol (ethylene glycol) after the esterification reaction, it is possible to adjust the number average molecular weight of the ester oligomer (A) to 700 or less. On the other hand, if the depolymerization reaction is not carried out, the number average molecular weight of the ester oligomer becomes high, exceeding 700, under normal conditions. Alternatively, if the depolymerization reaction is not carried out, the number average molecular weight can be controlled to 700 or less by setting the molar ratio of the diol component to the dicarboxylic acid component in a high range of 1.25 to 1.60, but if the molar ratio of the diol component is less than 1.25, the number average molecular weight will exceed 700.
[0054] [Polyester polyol (B)] In the above dimer acid copolymerized polyester resin, the polyester polyol (B) has a dicarboxylic acid unit composed of a hydrogenated dimer acid unit (b1). The dimer acid is, for example, a dicarboxylic acid compound having 36 carbon atoms obtained by dimerizing an unsaturated fatty acid having 18 carbon atoms, such as oleic acid or linoleic acid. The dimer acid in which the unsaturated double bonds remaining after dimerization are saturated by hydrogenation is a hydrogenated dimer acid, and the dicarboxylic acid unit of the polyester polyol (B) is composed of this hydrogenated dimer acid unit (b1). Note that hydrogenated dimer acid is usually obtained as a mixture of compounds having a linear branched structure and an alicyclic structure, and although the contents of these vary depending on the production process, the contents of these are not particularly limited in the present invention. The diol unit of the polyester polyol (B) is composed of a 1,4-butanediol unit (b2). Note that the ends of the polyester polyol (B) are all hydroxyl groups derived from the 1,4-butanediol unit (b2).
[0055] The number average molecular weight of the polyester polyol (B) is 1500 to 3000, preferably 1800 to 2500. When the average molecular weight is within this range, the reactivity during copolymerization is excellent, and the obtained copolymerized polyester resin also has excellent performance as a film for covering metal sheets. On the other hand, when the average molecular weight is less than 1500, the reactivity during copolymerization is good, but the dent resistance of aluminum cans including the film coating tends to be poor. On the other hand, when the average molecular weight exceeds 3000, the reactivity during copolymerization is poor, and a copolymerized polyester resin with a desired molecular weight may not be obtained.
[0056] The polyester polyol (B) can be obtained by esterifying hydrogenated dimer acid units (b1) and 1,4-butanediol units (b2) by a known method, but it is necessary to adjust the molar ratio during the reaction so that the terminals are hydroxyl groups. Alternatively, a commercially available product may be used as the polyester polyol (B). For example, Priplast 3199 (manufactured by Croda) is commercially available as a polyester polyol having a number average molecular weight of 2200 and consisting of hydrogenated dimer acid and 1,4-butanediol. Other commercially available polyester polyols include Priplast 3162, 3192, 3196, 2101, and 2104 (all manufactured by Croda).
[0057] [Copolymer polyester resin] The above dimer acid copolymerized polyester resin can be obtained by copolymerizing 50 to 93% by mass of an ester oligomer (A) and 7 to 50% by mass of a polyester polyol (B). Here, the content of the polyester polyol (B) in the total polymer is 7 to 50% by mass, preferably 15 to 35% by mass. If the content of the polyester polyol (B) is within the above range, the copolymerization reactivity is excellent and the dent resistance of aluminum cans, particularly those containing film coating, is excellent. Furthermore, since a copolymerized polyester resin in which the polyester polyol (B) is randomly bonded in the polymer chain is obtained, the appearance is colorless and transparent or pale yellow and transparent. On the other hand, if the content of the polyester polyol (B) is less than 7% by mass, the dent resistance of aluminum cans containing film coating is poor, and if it exceeds 50% by mass, the copolymerization reactivity is poor and the obtained copolymerized polyester resin may have a cloudy appearance due to phase separation of the polyester polyol (B).
[0058] The copolymerization reaction of the ester oligomer (A) and the polyester polyol (B) can be carried out by a conventional method. For example, the pressure in the reaction system to which each component is added is gradually reduced from atmospheric pressure to a high vacuum of 133.3 Pa or less to carry out a series of reactions. The temperature during the reaction is preferably controlled between 250 and 270°C. If the temperature exceeds 270°C, a decrease in viscosity due to deterioration occurs in the latter half of the copolymerization reaction, and if the temperature is less than 250°C, the copolymerization reaction may not proceed. In addition, as a polymerization catalyst used in the copolymerization reaction, antimony trioxide, germanium dioxide, titanium compounds, etc. can be used, and among these, titanium compounds such as tetrabutyl titanate and tetraisopropoxy titanate are preferably used from the standpoint of reactivity, safety, and cost. In addition, the intrinsic viscosity of the above-mentioned dimer acid copolymerized polyester resin is not particularly limited, but is preferably 0.7 to 0.9.
[0059] Another method for obtaining a dimer acid copolymerized polyester resin is to carry out an esterification reaction between a dicarboxylic acid containing 50 to 95 mol % of a terephthalic acid component and 50 to 5 mol % of a dimer acid component and a diol containing 90 mol % or more of an ethylene glycol component by a known method.
[0060] In the dimer acid copolymerized polyester resin, dicarboxylic acid units other than the terephthalic acid component and the dimer acid component may be contained within a range that does not impair lamination properties to an aluminum plate or the properties of an aluminum can, for example, within a range of 10 mol % or less. Examples of such dicarboxylic acid units include isophthalic acid, succinic acid, adipic acid, azelaic acid, sebacic acid, 1,4-naphthalenedicarboxylic acid, 4,4'-biphenyldicarboxylic acid, 1,12-dodecanoic acid, 1,2-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, and 1,4-cyclohexanedicarboxylic acid, and these may be used alone or in combination of two or more kinds.
[0061] In addition, the dimer acid copolymerized polyester resin may contain diol units other than the ethylene glycol component in an amount of 10 mol% or less. Examples of such diol units include aliphatic diols such as diethylene glycol, triethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, and neopentyl glycol, and alicyclic diols such as 1,4-cyclohexanedimethanol and 1,4-cyclohexanediethanol, which may be used alone or in combination of two or more.
[0062] The above dimer acid copolymerized polyester resin can be used by forming a film alone, but may also be used by blending with other polyester resins. Examples of other polyester resins include polyethylene terephthalate resin, isophthalic acid copolymerized polyester resin, polybutylene terephthalate resin, and polytrimethylene terephthalate resin, and may be used alone or in combination at a ratio of less than 50% by mass of the dimer acid copolymerized polyester resin.
[0063] <Third resin layer 12c> The third resin layer 12c may be a resin film containing, for example, 50 to 100 mass % of isophthalic acid copolymerized polyester resin containing 3 to 15 mol % of isophthalic acid with respect to the total acid amount of the third resin layer 12c. The third resin layer 12c may have the same composition as the first resin layer 12a.
[0064] In the copolymer polyester resin of the first resin layer 12a, the second resin layer 12b, and the third resin layer 12c, metal salts such as magnesium acetate, calcium acetate, and magnesium chloride can be added as additives to stabilize the electrostatic adhesion to the cooling roll when forming a melt-extrusion film. Furthermore, as an anti-blocking agent for the film roll, it is also possible to blend an appropriate amount of inert particles such as silica, alumina, calcium carbonate, and titanium dioxide, and the average particle size of the inert particles is preferably 1.0 to 4.0 μm. If it is less than 1.0 μm, the anti-blocking property is poor, and if it exceeds 4.0 μm, the particles may fall off due to wear or the film may break when stretched.
[0065] The copolymer polyester resins of the first resin layer 12a, the second resin layer 12b, and the third resin layer 12c may contain additives such as color pigments, waxes, heat stabilizers, antioxidants, and ultraviolet absorbers, as necessary. Examples of antioxidants include hindered phenol-based antioxidants, phosphorus-based antioxidants, and sulfur-based antioxidants, with hindered phenol-based antioxidants being particularly preferred. Several types of these antioxidants may be added in combination, and the content is preferably 100 to 5000 ppm.
[0066] <Laminated film> The resin film 12 can be obtained by laminating the copolymer polyester resins of the first resin layer 12a, the second resin layer 12b, and the third resin layer 12c by a known method. For example, the copolymer polyester resin of the first resin layer 12a, the copolymer polyester resin of the second resin layer 12b, and the copolymer polyester resin of the third resin layer 12c are each fed into separate extruders and co-extruded simultaneously from one die (co-extrusion lamination). Alternatively, the copolymer polyester resin of the second resin layer 12b is melt-extruded onto the surface of a film of the first resin layer 12a (or the third resin layer 12c) previously produced by a T-die method or an inflation method, and cooled and solidified. The copolymer polyester resin of the third resin layer 12c (or the first resin layer 12a) is melt-extruded onto the surface of the film while being fed and cooled and solidified (extrusion lamination). The thickness of the resin film 12 is not particularly limited, but is preferably 9 to 30 μm in total including the first resin layer 12a, the second resin layer 12b, and the third resin layer 12c.
[0067] 2.Aluminum cans for filling wine According to another aspect, there is provided an aluminum can for filling wine, which includes an aluminum plate, a resin film provided on a surface of the aluminum plate that will become the inside surface of the can, and an adhesive layer interposed between the aluminum plate and the resin film to bond them together, the resin film including a first resin layer as an outermost layer and a second resin layer containing a dimer acid copolymerized polyester resin, and at least one of the resin layers and the adhesive layer that constitute the resin film contains calcium carbonate.
[0068] For details of aluminum cans for filling wine, please refer to the explanation in the above section "1-2. Aluminum cans." Such aluminum cans have a specific resin film on the inside of the can, so they are excellent in that they are less likely to corrode and the flavor of the wine to deteriorate when filled with wine.
[0069] Preferred embodiments of the aluminum can for filling wine are summarized below.
[0070] [1] An aluminum can for filling wine, comprising: an aluminum plate; a resin film provided on the surface of the aluminum plate that will become the inside of the can; and an adhesive layer interposed between the aluminum plate and the resin film to adhere them together, wherein the resin film comprises a first resin layer as an outermost layer and a second resin layer containing a dimer acid copolymer polyester resin, and at least one of the resin layers and the adhesive layer that constitute the resin film contains calcium carbonate.
[0071] [2] The aluminum can for filling wine according to [1], wherein the resin film has a two-layer structure consisting of the first resin layer and the second resin layer. [3] The aluminum can for filling wine according to [1] or [2], wherein the first resin layer contains an isophthalic acid copolymer polyester resin.
[0072] [4] The aluminum can for filling wine according to any one of [1] to [3], wherein the adhesive layer contains a thermosetting epoxy resin. [5] The aluminum can for filling wine described in [1], wherein the resin film further includes a third resin layer as an outermost layer on the surface facing the adhesive layer, and has a three-layer structure of the first resin layer, the second resin layer, and the third resin layer.
[0073] [6] The aluminum can for filling wine according to [5], wherein the first resin layer contains an isophthalic acid copolymer polyester resin. [7] The aluminum can for filling wine according to [5] or [6], wherein the adhesive layer contains a thermosetting epoxy resin.
[0074] [8] The aluminum can for filling wine according to any one of [5] to [7], wherein the third resin layer contains an isophthalic acid copolymerized polyester resin. [9] The aluminum can filled wine according to any one of [1] to [8], wherein the adhesive layer contains calcium carbonate. EXAMPLES
[0075] [Example 1] In Example 1, various types of wine were sealed in aluminum cans having a specific coating on the inside surface of the can, and a storage test was conducted.
[0076] [Obtaining pH, alcohol concentration, free sulfite concentration, and chloride ion concentration] The pH, alcohol concentration, free sulfite concentration, and chloride ion concentration were obtained for 38 types of wine. The pH was measured with a pH meter at 20°C. The alcohol concentration was measured by high performance liquid chromatography. The free sulfite concentration was measured by aeration distillation and titration method (Rankine method). The chloride ion concentration was measured by potentiometric titration method.
[0077] [Calculation of molecular SO2 concentration] From the obtained pH, alcohol concentration, and free sulfite concentration values, the molecular SO2 concentration of each of the 38 types of wine was calculated based on the molecular SO2 concentration calculation formula described above.
[0078] [Packaging in aluminum cans] Each wine was filled into an aluminum can, and a separate cap was then wrapped around the aluminum can to produce a canned wine.
[0079] The aluminum can used had the bottle-shaped can structure shown in Fig. 1, had a resin coating having the layer structure shown in Fig. 3 on the inner surface of the can, and had a resin coating on the outer surface of the can. Specifically, the aluminum can body had, from the outer surface of the can, an outer resin film, an aluminum plate 10, an adhesive layer 11, and an inner resin film 12 with a three-layer structure.
[0080] The three-layered inner resin film 12 was composed of an outer layer made of 10 mol% isophthalic acid copolymerized PET resin, an intermediate layer made of 21 mol% dimer acid copolymerized PET resin, and an inner layer made of 10 mol% isophthalic acid copolymerized PET resin. The inner resin film 12 had a thickness of 25 μm. The outer layer, intermediate layer, and inner layer had a thickness ratio of 1:1:0.5. The adhesive layer 11 was made of a thermosetting epoxy resin and contained calcium carbonate particles. The adhesive layer 11 had a thickness of 3 μm.
[0081] The outer resin film was made of a blend of polybutylene terephthalate and isophthalic acid copolymerized polyethylene terephthalate (PBT / copolymerized PET). The outer resin film had a thickness of 18 μm.
[0082] The aluminum can material was produced as follows: an inner resin film was prepared by a known co-extrusion film production method, an adhesive resin was applied to the inner resin film, and an outer resin film was prepared by a known film production method, and these two types of films were bonded to an aluminum plate by thermocompression bonding.
[0083] [Storage and quality evaluation of canned wine] The canned wine was stored and the quality of the canned wine was evaluated after storage. The storage was carried out for a period of 24 months at temperatures of 5°C, 20°C, and 38°C. The quality evaluation was carried out by visual observation of the corrosion state and by sensory evaluation.
[0084] If no corrosion was observed and the wine's flavor did not deteriorate under all storage conditions, the wine was rated as being suitable for filling into the aluminum cans tested, whereas if corrosion was observed or the wine's flavor deteriorated, the wine was rated as not suitable for filling into the aluminum cans tested.
[0085] [Determination of upper limits of molecular SO2 concentration and chloride ion concentration] The data for each wine was plotted with molecular SO2 concentration (mg / L) on the horizontal axis and chloride ion concentration (mg / L) on the vertical axis. Wines with good evaluation results (i.e., wines that were evaluated as suitable for use in the aluminum cans tested) were plotted with a "O" mark, and wines with bad evaluation results (i.e., wines that were evaluated as not suitable for use in the aluminum cans tested) were plotted with a "X" mark.
[0086] The evaluation results are shown in Figure 4. The evaluation results showed that when wine with a molecular SO2 concentration of 4.3 mg / mL or less and a chloride ion concentration of 350 mg / L or less is filled into the above-mentioned aluminum can with a specific coating on the inside of the can, it does not cause corrosion of the aluminum can or deterioration of the flavor of the wine during storage.
[0087] [Example 2] In Example 2, in addition to the aluminum can used in Example 1 (hereinafter referred to as aluminum can A), three types of wine shown in Table 1 below were packed in another aluminum can (hereinafter referred to as aluminum can B) and a storage test was carried out. The storage test was carried out as described in the column of Example 1 under "Storage and quality evaluation of canned wine".
[0088] Aluminum can B had a bottle-like can structure, and had a resin coating having the layer structure shown in Fig. 2 on the inner surface of the can, and had a resin coating on the outer surface of the can. Specifically, the body of aluminum can B had, from the outer surface of the can, an outer resin film, an aluminum plate 10, an adhesive layer 11, and an inner resin film 12 with a two-layer structure.
[0089] The two-layered inner resin film 12 was composed of an outer layer made of a blend resin of polybutylene terephthalate and polyethylene terephthalate (PBT / PET) and an inner layer made of 10 mol% isophthalic acid copolymer polyester resin. The inner resin film 12 had a thickness of 20 μm. The outer layer and the inner layer had a thickness ratio of 1:1. The adhesive layer 11 was made of a thermosetting epoxy resin and contained calcium carbonate particles. The adhesive layer 11 had a thickness of 3 μm.
[0090] The outer resin film was made of a blend of polybutylene terephthalate and polyethylene terephthalate (PBT / PET) and had a thickness of 18 μm.
[0091] The evaluation results are shown in the table below. [Table 1]
[0092] Wine A had a molecular SO2 concentration of 2.2 mg / L and a chloride ion concentration of 170 mg / L. Wine B had a molecular SO2 concentration of 0.8 mg / L and a chloride ion concentration of 40 mg / L. Wine C had a molecular SO2 concentration of 2.7 mg / L and a chloride ion concentration of 50 mg / L.
[0093] When wine A was stored in aluminum can A, no corrosion occurred, but when it was stored in aluminum can B, corrosion occurred. Similarly, when wine C was stored in aluminum can A, no corrosion occurred, but when it was stored in aluminum can B, corrosion occurred.
[0094] These results show that even if the molecular SO2 concentration in the wine is 4.3 mg / mL or less and the chloride ion concentration in the wine is 350 mg / L or less, corrosion of the aluminum cans will occur during storage unless the aluminum can has a specific coating on the inside.
[0095] The results of Examples 1 and 2 show that a combination of a specific coating on the inner surface of an aluminum can and a specific composition of wine can prevent corrosion of the aluminum can and flavor deterioration of the wine. The following claims as originally filed of this application are given as embodiments. [1] An aluminum can comprising an aluminum plate, a resin film provided on a surface of the aluminum plate that will be the inner surface of the can, and an adhesive layer interposed between the aluminum plate and the resin film to bond them together, the resin film comprising a first resin layer as an outermost layer and a second resin layer containing a dimer acid copolymerized polyester resin, and at least one of the resin layers constituting the resin film and the adhesive layer contains calcium carbonate; The aluminum can is filled with 4.3 mg / L or less of molecular SO 2 and wine containing 350 mg / L or less of chloride ions. Aluminum cans containing filled wine. [2] An aluminum can filled wine as described in [1], wherein the resin film has a two-layer structure consisting of the first resin layer and the second resin layer. [3] An aluminum can filled wine according to [1] or [2], wherein the first resin layer contains an isophthalic acid copolymer polyester resin. [4] The aluminum can filled wine according to any one of [1] to [3], wherein the adhesive layer contains a thermosetting epoxy resin. [5] The aluminum-can filled wine described in [1], wherein the resin film further includes a third resin layer as the outermost layer on the surface facing the adhesive layer, and has a three-layer structure of the first resin layer, the second resin layer, and the third resin layer. [6] An aluminum can filled wine according to [5], wherein the first resin layer contains an isophthalic acid copolymer polyester resin. [7] An aluminum can filled with wine according to [5] or [6], wherein the adhesive layer contains a thermosetting epoxy resin. [8] The aluminum can filled wine according to any one of [5] to [7], wherein the third resin layer contains an isophthalic acid copolymer polyester resin. [9] A wine bottle packed in an aluminum can according to any one of [1] to [8], wherein the adhesive layer contains calcium carbonate.
[10] An aluminum can for filling wine, comprising: an aluminum plate; a resin film provided on the surface of the aluminum plate that will become the inside of the can; and an adhesive layer interposed between the aluminum plate and the resin film to adhere them together, wherein the resin film comprises a first resin layer as an outermost layer and a second resin layer containing a dimer acid copolymer polyester resin, and at least one of the resin layers and the adhesive layer that constitute the resin film contains calcium carbonate. [Explanation of symbols]
[0096] 1...aluminum can for filling wine, 2...container body, 2a...mouth neck portion, 2b...shoulder portion, 2c...body portion, 3...bottom lid Reference Signs List 10: aluminum plate, 11: adhesive layer, 12: resin film, 12a: first resin layer, 12b: second resin layer, 12c: third resin layer, 14: calcium carbonate
Claims
1. an aluminum can having a bottle-shaped can structure, comprising: an aluminum plate; a resin film provided on a surface of the aluminum plate that will become the inner surface of the can; and an adhesive layer interposed between the aluminum plate and the resin film to bond them together, wherein the resin film comprises a first resin layer as an outermost layer and a second resin layer containing a dimer acid copolymer polyester resin, and only the adhesive layer contains calcium carbonate; The aluminum can is sealed with 4.3 mg / L or less of molecular SO 2 and a wine containing 350 mg / L or less of chloride ions. Aluminum cans containing filled wine.
2. 2. The aluminum can filled wine container according to claim 1, wherein the resin film has a two-layer structure of the first resin layer and the second resin layer.
3. 3. The aluminum can filled wine container according to claim 1, wherein the first resin layer contains an isophthalic acid copolymer polyester resin.
4. 4. The aluminum can filled wine according to claim 1, wherein the adhesive layer comprises a thermosetting epoxy resin.
5. 2. The aluminum can filled wine container described in claim 1, wherein the resin film further includes a third resin layer as the outermost layer on the surface facing the adhesive layer, and has a three-layer structure of the first resin layer, the second resin layer, and the third resin layer.
6. The aluminum can filled wine bottle according to claim 5, wherein the first resin layer contains an isophthalic acid copolymer polyester resin.
7. 7. The aluminum can filled wine bottle according to claim 5, wherein the adhesive layer comprises a thermosetting epoxy resin.
8. The aluminum can filled wine bottle according to any one of claims 5 to 7, wherein the third resin layer contains an isophthalic acid copolymer polyester resin.
Citation Information
Patent Citations
Canned wine
JP1990076565A
How to package wine in aluminum cans
JP2005503971A
Polyester film for coating metal sheet, polyester film coated metal sheet and polyester film coated metal container
JP2006007746A
Metal can for canning wine
JP2006062688A
Paint for wine can, coated metal plate for wine can, and wine can
JP2011016570A