All solid state battery

The all-solid-state battery design with a carbon-based material, metal particles, and a polymer binder composition addresses the conductivity and adhesion issues of solid electrolytes, enhancing battery performance and capacity.

JP7596517B2Active Publication Date: 2024-12-09SAMSUNG SDI CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023515816
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-09-09
Filing Date
2021-06-22
Publication Date
2024-12-09
Estimated Expiration
2041-06-22

AI Technical Summary

Technical Problem

Lithium secondary batteries with solid electrolytes face issues of lower ionic conductivity, increased interfacial resistance due to poor adhesion of the solid electrolyte with active materials, and reduced output and capacitance characteristics, especially at low temperatures.

Method used

An all-solid-state battery design incorporating a negative electrode with a carbon-based material, metal particles, and a specific polymer binder composition, including butadiene-based rubber and carboxyalkyl cellulose, to enhance adhesion and reduce resistance.

Benefits of technology

The design achieves improved adhesion of the active material layer to the base material, resulting in lower resistance and enhanced battery performance, including increased capacity and lifespan.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007596517000003
    Figure 0007596517000003
  • Figure 0007596517000004
    Figure 0007596517000004
  • Figure 0007596517000005
    Figure 0007596517000005
Patent Text Reader

Abstract

An all-solid-state battery includes: an electrode assembly including a negative electrode, a positive electrode, and a solid electrolyte positioned between the negative electrode and the positive electrode; and a case that houses the electrode assembly, wherein the negative electrode includes a negative electrode current collector and a negative electrode active material layer including a negative electrode active material and a binder, the negative electrode active material including a carbon-based material and metal particles, and the binder includes a first polymer of butadiene-based rubber and a second polymer selected from carboxyalkyl cellulose (wherein the alkyl is an alkyl having 1 to 6 carbon atoms), a salt thereof, and a combination thereof, and the first polymer and the second polymer are included in a weight ratio of 1:1 to 6:1.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This relates to all-solid-state batteries. [Background technology]

[0002] Recently, with the rapid spread of electronic devices that use batteries, such as mobile phones, laptops, and electric vehicles, the demand for secondary batteries that are small, lightweight, and have relatively high capacity is rapidly increasing. In particular, lithium secondary batteries are in the spotlight as a driving power source for portable devices because of their light weight and high energy density. As a result, research and development to improve the performance of lithium secondary batteries is being actively conducted.

[0003] Among lithium secondary batteries, all-solid-state batteries that use solid electrolytes have the advantages of being safe as there is no risk of electrolyte leakage, and being easy to manufacture as thin batteries. However, lithium secondary batteries that use solid electrolytes are different from lithium-ion batteries that use liquid electrolytes.

[0004] Compared to batteries, the ion conductivity is lower, which causes a problem of a decrease in output characteristics, especially at low temperatures. In addition, compared to liquid electrolytes, the solid electrolyte has poorer surface adhesion to the active material, which increases the interface resistance, and the output characteristics and capacity characteristics are decreased compared to the amount of active material added because the solid electrolyte is distributed in a non-contact state with the electrode active material. Summary of the Invention [Problem to be solved by the invention]

[0005] One embodiment provides an all-solid-state battery including an electrode having excellent adhesion of an active material layer to a substrate and low resistance. [Means for solving the problem]

[0006] One embodiment provides an all-solid-state battery including: an electrode assembly including a negative electrode, a positive electrode, and a solid electrolyte located between the negative electrode and the positive electrode; and a case housing the electrode assembly, in which the negative electrode includes a negative electrode current collector and a negative electrode active material layer including a negative electrode active material and a binder, the negative electrode active material including a carbon-based material and metal particles, the binder including a first polymer of butadiene-based rubber and a second polymer selected from carboxyalkyl cellulose (wherein the alkyl is an alkyl having 1 to 6 carbon atoms), a salt thereof, and a combination thereof, and the first polymer and the second polymer are included in a weight ratio of 1:1 to 6:1.

[0007] The metal particles may be any one selected from Ag, Zn, Al, Sn, Mg, Ge, Cu, In, Ni, Bi, Au, Si, Pt, Pd, and combinations thereof.

[0008] The metal particles may have a size of 5 nm to 800 nm.

[0009] The carbon-based material may be a non-graphitic carbon.

[0010] The non-graphitic carbon may have a secondary particle form in which a plurality of primary particles are aggregated.

[0011] The primary particles may have a particle size of 20 nm to 100 nm.

[0012] The non-graphitic carbon may be any one selected from carbon black, activated carbon, acetylene black, denka black, ketjen black, and combinations thereof.

[0013] The binder may be included in an amount of 0.01 to 40 parts by weight based on 100 parts by weight of the negative electrode active material.

[0014] The first polymer of the butadiene-based rubber may be any one selected from styrene butadiene rubber (SBR), nitrile butadiene rubber (NBR), acrylate butadiene rubber (ABR), methacrylate butadiene rubber, acrylonitrile-butadiene-styrene (ABS) rubber, styrene-butadiene-styrene (SBS) rubber, and combinations thereof.

[0015] The solid electrolyte may be a sulfide-based solid electrolyte.

[0016] The solid electrolyte is Li a M b P c S d A e (wherein a, b, c, d and e are all from 0 to 12, inclusive; M is Ge, Sn, Si or a combination thereof; and A is one of F, Cl, Br, or I).

[0017] The negative electrode may not have a solid electrolyte.

[0018] The negative electrode may have an electrode plate binding strength of 10 gf / mm or more.

[0019] The negative electrode may further include a lithium deposition layer formed by depositing lithium between the negative electrode current collector and the negative electrode active material layer during charging.

[0020] The lithium deposit layer may have a thickness of 10 μm to 50 μm.

[0021] The all-solid-state battery may further include a buffer material between the negative electrode and the case. Effect of the Invention

[0022] The all-solid-state battery has excellent adhesion of the active material layer to the substrate and has improved battery performance due to the inclusion of an electrode with low resistance. [Brief description of the drawings]

[0023] [Figure 1] FIG. 1 is a schematic cross-sectional view of an all-solid-state battery according to an embodiment. [Diagram 2] FIG. 1 is a schematic cross-sectional view of an all-solid-state battery during charging. [Diagram 3] 1 is a graph showing the results of measuring the capacity retention rate versus the initial discharge capacity of all-solid-state batteries according to Examples 1, 2, and 4 and Comparative Example 1. [Figure 4] 1 is a graph showing the results of measuring the life span of all-solid-state batteries according to Examples 1 and 2 and Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, preferred embodiments of the present invention will be described in detail, but they are given by way of example only and are not intended to limit the present invention, which is defined only by the scope of the following claims.

[0025] Unless otherwise specified in this specification, when a part such as a layer, film, region, plate, etc. is said to be "on" another part, this includes not only the case where it is "directly on" the other part, but also the case where there is another part in between.

[0026] In the present invention, the "particle size" or "particle diameter" may be defined as the average particle diameter (D50) based on 50% of the cumulative volume in a particle size distribution curve. The particle diameter may be measured by electron microscopy using, for example, a scanning electron microscopy (SEM) or a field emission scanning electron microscopy (FE-SEM), or by a laser diffraction method. When measuring by the laser diffraction method, more specifically, the particles to be measured are dispersed in a dispersion medium, and then introduced into a commercially available laser diffraction particle size measuring device (e.g., MT 3000 by Microtrac) and irradiated with ultrasonic waves of about 28 kHz at an output of 60 W, and the average particle diameter (D50) based on 50% of the particle size distribution in the measuring device may be calculated.

[0027] Hereinafter, the all-solid-state battery will be described with reference to Fig. 1. Fig. 1 is a cross-sectional view of an all-solid-state battery according to one embodiment.

[0028] 1, the all-solid-state battery 100 can be manufactured by stacking an anode 400 including an anode current collector 401 and an anode active material layer 403, a solid electrolyte layer 300, and a cathode 200 including a cathode active material layer 203 and a cathode current collector 201, and housing the stacked electrode assembly in a case 500. Although FIG. 1 shows one electrode assembly including the anode 400, the solid electrolyte layer 300, and the cathode 200, two or more electrode assemblies can also be stacked to manufacture an all-solid-state battery.

[0029] The negative electrode active material layer 403 includes a negative electrode active material and a binder. The negative electrode active material includes a carbon-based material and metal particles.

[0030] The carbon-based material may be crystalline carbon or non-graphitic carbon, and is not limited to a specific carbon. In one embodiment, the carbon-based material is preferably non-graphitic carbon. The non-graphitic carbon is a carbon-based material having a d002 This means that the value exceeds 0.337 nm.

[0031] The crystalline carbon may be any one selected from natural graphite, artificial graphite, mesophase carbon microbeads, and combinations thereof, and the non-graphitic carbon may be any one selected from carbon black, activated carbon, acetylene black, denka black, ketjen black, and combinations thereof. An example of the carbon black is Super P (TIMCAL).

[0032] The non-graphite carbon may have a secondary particle form in which a plurality of primary particles are aggregated, the primary particles may have a particle size of 20 nm to 100 nm, and the secondary particles may have a particle size of 1 μm to 20 μm.

[0033] In one embodiment, the particle size of the primary particles may be 20 nm or more, 30 nm or more, 40 nm or more, 50 nm or more, 60 nm or more, 70 nm or more, 80 nm or more, or 90 nm or more, and 100 nm or less, 90 nm or less, 80 nm or less, 70 nm or less, 60 nm or less, 50 nm or less, 40 nm or less, 30 nm or less, or 20 nm or less.

[0034] In one embodiment, the particle size of the secondary particles may be 1 μm or more, 3 μm or more, 5 μm or more, 7 μm or more, 10 μm or more, or 15 μm or more, and 20 μm or less, 15 μm or less, 10 μm or less, 7 μm or less, 5 μm or less, or 3 μm or less.

[0035] The morphology of the primary particles may be spherical, elliptical, plate-like, and combinations thereof, and in one embodiment, the morphology of the primary particles may be spherical, elliptical, and combinations thereof.

[0036] The metal particles may be any one selected from Ag, Zn, Al, Sn, Mg, Ge, Cu, In, Ni, Bi, Au, Si, Pt, Pd, and combinations thereof. The metal particles may be used in the negative electrode active material to improve the electrical conductivity of the electrode plate. In one embodiment, the metal particles are preferably Ag.

[0037] The metal particles may have a size of 5 nm to 800 nm. The size of the metal particles may be 5 nm or more, 50 nm or more, 100 nm or more, 150 nm or more, 200 nm or more, 250 nm or more, 300 nm or more, 350 nm or more, 400 nm or more, 450 nm or more, 500 nm or more, 550 nm or more, 600 nm or more, 650 nm or more, 700 nm or more, or 750 nm or more. The size of the metal particles may be 800 nm or less, 750 nm or less, 700 nm or less, 650 nm or less, 600 nm or less, 550 nm or less, 500 nm or less, 450 nm or less, 400 nm or less, 350 nm or less, 300 nm or less, 250 nm or less, 200 nm or less, 150 nm or less, 100 nm or less, or 50 nm or less. When the size of the metal particles is within the above range, the battery characteristics (e.g., life characteristics) of the all-solid-state battery can be improved.

[0038] The negative electrode active material may contain the carbonaceous material and the metal particles in a weight ratio of 1:1 to 99:1. For example, the weight of the carbonaceous material may be 1 or more, 2 or more, 3 or more, 4 or more, 5 or more, 10 or more, 15 or more, 20 or more, 25 or more, 30 or more, 35 or more, 40 or more, 45 or more, 50 or more, 55 or more, 60 or more, 65 or more, 70 or more, 75 or more, 80 or more, 85 or more, 90 or more or 95 or more, and 99 or less, 95 or less, 90 or less, 85 or less, 80 or less, 75 or less, 70 or less, 65 or less, 60 or less, 55 or less, 50 or less, 45 or less, 40 or less, 35 or less, 30 or less, 25 or less, 20 or less, 15 or less, 10 or less, 5 or less, 4 or less, 3 or less, or 2 or less, based on the weight of the metal particles. For example, the weight ratio of the carbon-based material to the metal particles may be 1:1 to 5:1, 1:1 to 10:1, 1:1 to 20:1, 1:1 to 30:1, 1:1 to 40:1, 1:1 to 50:1, 1:1 to 60:1, 1:1 to 70:1, 1:1 to 80:1, or 1:1 to 90:1. When the carbon-based material and the metal particles are included in the above weight ratio, the electrical conductivity of the all-solid-state electrode plate can be improved. In one embodiment, the weight ratio may be 3:1.

[0039] Conventional all-solid-state batteries often incorporate a highly reactive solid electrolyte into the electrode plate, making it difficult to manufacture the plate using an aqueous binder, so unlike conventional lithium-ion batteries, non-aqueous binders such as PVDF, which are not aqueous binders, are mainly used. However, because non-aqueous binders have low conductivity, there was a problem that the electrode material surrounded by the non-aqueous binder had low lithium ion conductivity and electrical conductivity.

[0040] In order to solve this problem, one embodiment provides an anode 400 that does not include a solid electrolyte in the anode 400 plate and includes a carbon-based material, metal particles, and a specific binder. Since the anode 400 does not include a solid electrolyte, it is possible to ensure excellent electrical conductivity, high adhesion, and low electrical resistance, thereby improving the characteristics of the all-solid-state battery.

[0041] The binder may include a first polymer of butadiene rubber and a second polymer selected from carboxyalkyl cellulose, a salt thereof, and a combination thereof. The binder improves the dispersibility of the negative electrode active material in the composition (slurry) for forming the negative electrode active material layer, and has a strong adhesive force, so that the binder content can be reduced and the negative electrode active material content can be increased to increase the capacity of the all-solid-state battery. In addition, the structural stability of the negative electrode 400 can be improved to improve various characteristics of the battery.

[0042] The butadiene-based rubber may include a substituted alkylene structural unit and a butadiene-derived structural unit, and may be any one selected from styrene butadiene rubber (SBR), nitrile butadiene rubber (NBR), acrylate butadiene rubber (ABR), methacrylate butadiene rubber, acrylonitrile-butadiene-styrene (ABS) rubber, styrene-butadiene-styrene (SBS) rubber, and combinations thereof.

[0043] The butadiene-based rubber may contain a substituted alkylene structural unit and a butadiene-derived structural unit in a molar ratio of 1:1 to 3:1. For example, the molar ratio may be 1:1 to 1.5:1, 1:1 to 2:1, or 1:1 to 2.5:1. When the molar ratio of the butadiene-based rubber is within the above range, the adhesive strength improving effect and the negative electrode structural stability effect can be improved.

[0044] The substituted alkylene structural unit may be derived from a substituted or unsubstituted styrene-based monomer. Specific examples of the substituted or unsubstituted styrene-based monomer include styrene, α-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2,4-dimethylstyrene, 2,5-dimethylstyrene, 2-methyl-4-chlorostyrene, 2,4,6-trimethylstyrene, cis-β-methylstyrene, trans-β-methylstyrene, 4-methyl-α-methylstyrene, 4-fluoro-α-methylstyrene, 4-chloro-α-methylstyrene, Examples of suitable styrene copolymers include 4-bromo-α-methylstyrene, 4-t-butylstyrene, 2-fluorostyrene, 3-fluorostyrene, 4-fluorostyrene, 2,4-difluorostyrene, 2,3,4,5,6-pentafluorostyrene, 2-chlorostyrene, 3-chlorostyrene, 4-chlorostyrene, 2,4-dichlorostyrene, 2,,6-dichlorostyrene, octachlorostyrene, 2-bromostyrene, 3-bromostyrene, 4-bromostyrene, 2,4-dibromostyrene, α-bromostyrene, β-bromostyrene, or combinations thereof.

[0045] In another embodiment, the substituted alkylene structural unit may be derived from a substituted or unsubstituted nitrile monomer, and specific examples of the substituted or unsubstituted nitrile monomer include acrylonitrile, methacrylonitrile, fumaronitrile, α-chloronitrile, α-cyanoethyl acrylonitrile, or a combination thereof.

[0046] The butadiene-derived structural unit may be a structural unit derived from a butadiene monomer, and specific examples of the butadiene monomer include 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, or 2-ethyl-1,3-butadiene, or a combination thereof.

[0047] The second polymer is selected from carboxyalkyl cellulose, a salt thereof, and a combination thereof. The alkyl of the carboxyalkyl cellulose may be a lower alkyl having 1 to 6 carbon atoms. In one embodiment, the carboxyalkyl cellulose may be carboxy methyl cellulose (CMC) or a salt thereof.

[0048] The carboxyalkyl cellulose has high viscosity and excellent coating properties, and at the same time contributes to improving adhesion, preventing the active material from falling off the current collector, and exhibiting excellent cycle characteristics. In addition, since the alkyl group of the carboxyalkyl cellulose is a lower alkyl group, the carboxyalkyl cellulose has high water solubility and is suitable for producing an aqueous electrode.

[0049] More specifically, the carboxymethyl cellulose may have a molecular weight (Mw) of 100,000 to 4,000,000. When the molecular weight is within the above range, the attractive force between the polymers is improved, so that the negative electrode active material can be uniformly dispersed, the adhesive force of the active material is also improved, so that the life characteristics can be improved, and the viscosity of the slurry is suitable for coating, so that the productivity of the electrode can be improved.

[0050] The first and second polymers of the binder may be contained in the negative electrode in a weight ratio of 1:1 to 6:1. The weight of the first polymer relative to the second polymer may be 1.1 or more, 1.2 or more, 1.3 or more, 1.4 or more, 1.5 or more, 1.6 or more, 1.7 or more, 1.8 or more, 1.9 or more, 2.0 or more, 2.1 or more, 2.2 or more, 2.3 or more, 2.4 or more, 2.5 or more, 2.6 or more, 2.7 or more, 2.8 or more, 2.9 or more, or 3.0 or more and 5 or less, 4.9 or less, 4.8 or less, 4.7 or less, 4.6 or less, 4.5 or less, 4.4 or less, 4.3 or less, 4.2 or less, 4.1 or less, 4.0 or less, 3.9 or less, 3.8 or less, 3.7 or less, 3.6 or less, 3.5 or less, 3.4 or less, 3.3 or less, 3.2 or less, 3.1 or less, or 3.0 or less. In one embodiment, the weight ratio of the first polymer to the second polymer of the binder may be 1:1 to 5:1 or 1:1 to 6:1.

[0051] When the first polymer and the second polymer are included in the above weight ratio, the binder can provide the electrode layer with appropriate flexibility to prevent cracking of the electrode layer and increase the adhesion of the electrode layer surface, whereas when the first polymer and the second polymer are present in a range exceeding the above range, the rigidity of the electrode may decrease.

[0052] The binder may be included in an amount of 0.01 to 40 parts by weight relative to 100 parts by weight of the negative electrode active material. The binder may be included in an amount of 1 to 15 parts by weight relative to 100 parts by weight of the negative electrode active material, and for example, the binder may be included in an amount of 1 part by weight or more, 2 parts by weight or more, 3 parts by weight or more, 4 parts by weight or more, 5 parts by weight or more, 6 parts by weight or more, 7 parts by weight or more, 8 parts by weight or more, 9 parts by weight or more, 10 parts by weight or more, 11 parts by weight or more, 12 parts by weight or more, 13 parts by weight or more, or 14 parts by weight or more, and 15 parts by weight or less, 14 parts by weight or less, 13 parts by weight or less, 12 parts by weight or less, 11 parts by weight or less, 10 parts by weight or less, 9 parts by weight or less, 8 parts by weight or less, 7 parts by weight or less, 6 parts by weight or less, 5 parts by weight or less, 4 parts by weight or less, 3 parts by weight or less, or 2 parts by weight or less relative to 100 parts by weight of the negative electrode active material.

[0053] When the binder is contained in the negative electrode 400 of the all-solid-state battery 100 in the above content range, the electrical resistance and adhesive strength are improved, and the characteristics (battery capacity and output characteristics) of the all-solid-state battery can be improved.

[0054] In addition to the above-mentioned negative electrode active material and binder, additives such as a conductive material, a filler, a dispersant, and an ion conductive material may be appropriately blended into the negative electrode active material layer 403. Examples of conductive materials that can be contained in the negative electrode active material layer 403 include graphite, carbon black, acetylene black, ketjen black, carbon fiber, and metal powder. In addition, known materials that are generally used in all-solid-state batteries can be used as the filler, dispersant, ion conductive material, and the like that can be contained in the negative electrode active material layer 403.

[0055] The negative electrode active material layer 403 can be formed on a negative electrode current collector 401. Examples of the negative electrode current collector 401 include a plate-shaped body or a foil-shaped body made of indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof. The negative electrode current collector 401 may be omitted.

[0056] The negative electrode 400 is 5.0·10 -2 The negative electrode may have a plate electrical resistance of 5.0·10 ohm·cm or less. -2 ohm·cm or less, 4.9·10 -2 ohm cm or less, 4.8·10 -2 ohm cm or less, 4.7·10 -2 ohm·cm or less, 4.6·10 -2 ohm·cm or less, 4.5·10 -2 ohm·cm or less, 4.4·10 -2 ohm cm or less, 4.3·10 -2 ohm cm or less, 4.2·10 -2 ohm cm or less, 4.1·10 -2 ohm cm or less, 4.0·10 -2The negative electrode may have an electrical resistance of 5.0·10 ohm·cm or less. -2 The low electrical resistance of the electrodes (less than ohm·cm) increases the electrical conductivity of the electrodes, improving the performance of solid-state batteries.

[0057] The negative electrode 400 may have a negative plate binding strength of 10 gf / mm or more. For example, the negative electrode may have a negative plate binding strength of 10 gf / mm or more, 20 gf / mm or more, 30 gf / mm or more, 40 gf / mm or more, 50 gf / mm or more, 60 gf / mm or more, 70 gf / mm or more, 80 gf / mm or more, or 90 gf / mm or more. Since the negative electrode has a high negative plate binding strength of 10 gf / mm or more, the stability of the plate is increased, and the characteristics of the all-solid-state battery can be improved.

[0058] The all-solid-state battery 100 can exhibit high characteristics over a wider temperature range by including the solid electrolyte layer 300. The solid electrolyte layer 300 includes a solid electrolyte. The solid electrolyte included in the solid electrolyte layer 300 may be an inorganic solid electrolyte such as a sulfide-based solid electrolyte or an oxide-based solid electrolyte, or a solid polymer electrolyte.

[0059] In one embodiment, the solid electrolyte may be a sulfide-based solid electrolyte having excellent ion conductivity, and the solid electrolyte may be Li a M b P c S d A e (a, b, c, d and e are all from 0 to 12, M is Ge, Sn, Si or a combination thereof, and A is one of F, Cl, Br, or I), specifically Li3PS4, Li7P3S 11 For example, x may be 0 to 7. The higher the ionic conductivity of the sulfide-based solid electrolyte used in the all-solid-state battery, the more preferable. -4 ~10 -2 S / cm. Within this range, the charge / discharge capacity can be improved.

[0060] The sulfide-based solid electrolyte can be obtained by mixing Li2S and P2S5 in a mixing ratio of 50:50 to 80:20. Within the above mixing ratio range, a sulfide-based solid electrolyte having a preferable ionic conductivity can be provided. The ionic conductivity can be further improved by including other components such as SiS2, GeS2, and B2S3. The sulfide solid electrolyte may be amorphous or crystalline, but it is preferable to use an amorphous sulfide-based solid electrolyte that has good contact with the active material.

[0061] The mixing method may be mechanical milling or a solution method. Mechanical milling is a method in which the starting materials are placed in a reactor and vigorously stirred with a ball mill, etc., to finely disperse the starting materials and mix them. When a solution method is used, the starting materials are mixed in a solvent to obtain a solid electrolyte as a precipitate. In addition, additional calcination may be performed. When additional calcination is performed, the crystals of the solid electrolyte may become even stronger.

[0062] The all-solid-state battery 100 includes a cathode 200 including a cathode active material layer 203 and a cathode current collector 201. The cathode active material layer 203 can include a cathode active material. The cathode active material is preferably a cathode active material capable of reversibly absorbing and releasing lithium ions. For example, the cathode active material can be one or more of composite oxides of lithium and a metal selected from cobalt, manganese, nickel, and combinations thereof. Specific examples of the composite oxides include Li a A 1-b B 1 b D 1 2 (wherein 0.90≦a≦1.8, and 0≦b≦0.5); Li a E 1-b B 1 b O 2-c D 1 c (wherein, 0.90≦a≦1.8, 0≦b≦0.5, and 0≦c≦0.05); LiE 2-b B 1 b O4-c D 1 c (wherein 0≦b≦0.5 and 0≦c≦0.05); Li a Ni 1-b-c Co b B 1 c D 1 α (wherein, 0.90≦a≦1.8, 0≦b≦0.5, 0≦c≦0.05, and 0<α≦2); Li a Ni 1-b-c Co b B 1 c O 2-α F 1 α (wherein, 0.90≦a≦1.8, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Li a Ni 1-b-c Co b B 1 c O 2-α F 1 2 (wherein, 0.90≦a≦1.8, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Li a Ni 1-b-c Mn b B 1 c D 1 α (wherein, 0.90≦a≦1.8, 0≦b≦0.5, 0≦c≦0.05, and 0<α≦2); Li a Ni 1-b-c Mn b B 1 c O 2-α F 1 α (wherein, 0.90≦a≦1.8, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Li a Ni 1-b-c Mn b B 1 c O 2-α F 1 2 (wherein, 0.90≦a≦1.8, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Li a Ni b E c Gd O2 (wherein 0.90≦a≦1.8, 0≦b≦0.9, 0≦c≦0.5, and 0.001≦d≦0.1); Li a Ni b Co c Mn d GeO2 (wherein, 0.90≦a≦1.8, 0≦b≦0.9, 0≦c≦0.5, 0≦d≦0.5, and 0.001≦e≦0.1); Li a NiG b O2 (wherein 0.90≦a≦1.8, 0.001≦b≦0.1); Li a CoG b O2 (wherein 0.90≦a≦1.8, 0.001≦b≦0.1); Li a MnG b O2 (wherein 0.90≦a≦1.8, 0.001≦b≦0.1); Li a Mn2G b O4 (wherein 0.90≦a≦1.8, 0.001≦b≦0.1); QO2; QS2; LiQS2; V2O5; LiV2O5; LiI 1 O2;LiNiVO4;Li (3-f) J2(PO4)3(0≦f≦2);Li (3-f) A compound represented by any one of the following chemical formulas can be used: Fe2(PO4)3(0≦f≦2);LiFePO4:

[0063] In the above formula, A is Ni, Co, Mn, or a combination thereof; 1 is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, rare earth elements or combinations thereof; D 1 is O, F, S, P, or a combination thereof; E is Co, Mn, or a combination thereof; F 1 is F, S, P, or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, or a combination thereof; Q is Ti, Mo, Mn, or a combination thereof; I 1 is Cr, V, Fe, Sc, Y, or a combination thereof; J is V, Cr, Mn, Co, Ni, Cu, or a combination thereof.

[0064] For example, the positive electrode active material can be formed using lithium cobalt oxide (hereinafter referred to as LCO), lithium nickel oxide, lithium nickel cobalt oxide, lithium nickel cobalt aluminum oxide (hereinafter referred to as NCA), lithium nickel cobalt manganese oxide (hereinafter referred to as NCM), etc. These positive electrode active materials can be used alone or in combination of two or more.

[0065] In addition, a lithium salt of a transition metal oxide having a layered rock salt structure can be used as the positive electrode active material. Here, "layered" indicates a thin layered shape. Also, "rock salt structure" refers to a sodium chloride type structure which is a kind of crystal structure, specifically, a structure in which the face-centered cubic lattices formed by cations and anions are arranged with a shift of only 1 / 2 of the unit lattice angle.

[0066] Examples of such transition metal composite oxides having a layered rock salt structure include LiNi x Co y Al z O2 (NCA), LiNi x Co y Mn z O2 (NCM) (where 0 < x < 1, 0 < y < 1, 0 < z < 1, x + y + z = 1), etc., are ternary lithium transition metal oxides.

[0067] When the positive electrode active material contains the ternary lithium transition metal composite oxide having the above-mentioned layered rock salt structure, the energy density and thermal stability of the all-solid-state battery 100 can be improved.

[0068] The positive electrode active material may be covered with a coating layer. Any coating layer known as a coating layer for a positive electrode active material of an all-solid-state battery can be used as the coating layer. An example of the coating layer is Li2O-ZrO2.

[0069] In addition, when the positive electrode active material is formed of a ternary lithium transition metal composite oxide such as NCA or NCM and contains nickel (Ni) as the positive electrode active material, the capacity density of the all-solid-state battery 100 increases and metal elution of the positive electrode active material in a charged state can be reduced. As a result, the all-solid-state battery 100 can have improved long-term reliability and cycle characteristics in a charged state.

[0070] Here, examples of the shape of the positive electrode active material include particle shapes such as spherical and elliptical. The average particle size of the positive electrode active material is not particularly limited, and may be within a range applicable to the positive electrode active material of existing all-solid-state secondary batteries. The content of the positive electrode active material in the positive electrode active material layer 203 is also not particularly limited, and may be within a range applicable to the positive electrode layer of existing all-solid-state secondary batteries.

[0071] The positive electrode active material layer 203 may further include a solid electrolyte. The solid electrolyte included in the positive electrode layer may be the same as or different from the solid electrolyte included in the solid electrolyte layer 300. The solid electrolyte may be included in an amount of 10 to 30 wt % based on the total weight of the positive electrode layer.

[0072] The positive electrode active material layer 203 may be formed on the positive electrode current collector 201. At this time, the positive electrode active material layer 203 may be formed on the positive electrode current collector 201 by a dry or wet coating method. The positive electrode current collector 201 may be, for example, a plate or foil made of indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof. The positive electrode current collector 201 may be omitted.

[0073] In addition to the above-mentioned positive electrode active material and solid electrolyte, additives such as a conductive material, a binder, a filler, a dispersant, and an ion conductive material can be appropriately mixed into the positive electrode active material layer 203 .

[0074] The filler, dispersant, and ion conductive material that can be contained in the positive electrode active material layer 203 may be the same as the additives blended in the negative electrode active material layer 403. In this case, the conductive material may be present in an amount of 1 to 10% by weight based on the total weight of the positive electrode active material layer 203. Examples of binders that can be contained in the positive electrode active material layer 203 include styrene butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, and polyethylene.

[0075] The thickness of the negative electrode 400 may be 1 μm to 30 μm. For example, the thickness of the negative electrode 400 may be 1 μm or more, 5 μm or more, 10 μm or more, 15 μm or more, 20 μm or more, or 25 μm or more, and 25 μm or less, 20 μm or less, 15 μm or less, 10 μm or less, or 5 μm or less. Since the thickness of the negative electrode 400 is small as described above, the life of the all-solid-state battery can be improved, and the energy density can also be increased.

[0076] The thickness of the positive electrode 200 may be 100 μm to 200 μm. For example, the thickness of the positive electrode 200 may be 100 μm or more, 110 μm or more, 120 μm or more, 130 μm or more, 140 μm or more, 150 μm or more, 160 μm or more, 170 μm or more, 180 μm or more, or 190 μm or more, and 200 μm or less, 190 μm or less, 180 μm or less, 170 μm or less, 160 μm or less, 150 μm or less, 140 μm or less, 130 μm or less, 120 μm or less, or 110 μm or less. As described above, the thickness of the positive electrode 200 is thicker than the thickness of the negative electrode 400, so that the capacity of the positive electrode 200 is greater than the capacity of the negative electrode 400.

[0077] The thickness ratio of the positive electrode 200 to the negative electrode 400 may be 3 to 200. For example, the thickness ratio of the positive electrode 200 to the negative electrode 400 may be 3 or more, 5 or more, 7 or more, 10 or more, 20 or more, 30 or more, 40 or more, 50 or more, 100 or more, or 150 or more, and 200 or less, 150 or less, 100 or less, 50 or less, 40 or less, 30 or less, 20 or less, 10 or less, 7 or less, or 5 or less. In one embodiment, the thickness ratio of the positive electrode 200 to the negative electrode 400 may be 3 to 10.

[0078] During charging of the battery, the negative electrode and the positive electrode may expand, and the thickness of the negative electrode and the positive electrode may increase. When the thickness of the negative electrode increases, the negative electrode may further include a lithium deposition layer. An all-solid-state battery having such a structure will be described with reference to FIG. 2. FIG. 2 is a schematic cross-sectional view of an all-solid-state battery during charging. In FIG. 2, the same components as those already described above are assigned the same reference numerals as in FIG. 1, and the description thereof will be omitted. Referring to FIG. 2, the negative electrode 400' of the all-solid-state battery 100 further includes a lithium deposition layer 405' formed between the negative electrode current collector 401' and the negative electrode active material layer 403'. During charging, the lithium deposition layer 405' may be formed by the lithium that moves from the positive electrode 200 to the negative electrode 400', and the safety and life of the all-solid-state battery may be increased through the lithium deposition layer 405'.

[0079] The thickness of the lithium deposit layer 405' may be 10 μm to 50 μm. For example, the thickness of the lithium deposit layer 405' may be 10 μm or more, 20 μm or more, 30 μm or more, or 40 μm or more, and 50 μm or less, 40 μm or less, 30 μm or less, or 20 μm or less. By including the lithium deposit layer 405', the thickness of the negative electrode 400' after charging can be increased by 2 to 5 times. That is, the thickness of the negative electrode after charging can be increased by 2 to 5 times compared to the initial thickness before charging or the thickness of the negative electrode during discharging.

[0080] In one embodiment, the all-solid-state battery 100 may further include a buffer material for buffering a change in thickness due to the lithium deposition layer 405'. The buffer material may be disposed between the negative electrode 400' and the case 500 or on the outer surface of the case 500, and in the case of a battery in which one or more electrode assemblies are stacked, the buffer material may be disposed between different electrode assemblies.

[0081] The buffer material has an elastic recovery rate of 50% or more and is insulating, and specifically includes silicone rubber, acrylic rubber, fluorine-based rubber, nylon, synthetic rubber, or a combination thereof. The buffer material may be in the form of a polymer sheet.

[0082] The present invention will be described in more detail with reference to the following examples and comparative examples. However, the examples are for illustrating the present invention and are not intended to limit the scope of the present invention. EXAMPLES

[0083] Example 1 (1) Manufacturing of positive electrode active material An LZO coating solution was prepared by mixing 100 parts by weight of anhydrous 2-propanol, 10 parts by weight of lithium methoxide (10% methanol solution), and 0.5 parts by weight of zirconium (IV) tetrapropoxide. 0.9 Co 0.05 Mn 0.05 O2) was mixed and stirred for 1 hour, and then vacuum dried at 50°C to prepare a positive electrode active material.

[0084] (2) Manufacturing of positive electrodes LZO-coated positive electrode active material NCM (LiNi 0.9 Co 0.05 Mn 0.05A mixture was prepared by mixing the positive electrode active material, the solid electrolyte, the conductive material, and the binder, polytetrafluoroethylene (PTFE), in which the weight ratio of the positive electrode active material, the solid electrolyte, the conductive material, and the binder was 85:15:3:1.5.

[0085] Then, xylene was added to the mixture, and the mixture was dried at 45° C. for 2 hours in a vacuum chamber to prepare a positive electrode having a thickness of 150 μm.

[0086] (3) Manufacturing of solid electrolyte layer Isobutylyl isobutyrate (IBIB) was added as a binder solution to the argyrodite-type solid electrolyte Li6PS5Cl and mixed. The mixture was then stirred in a Thinky mixer to adjust the viscosity to an appropriate level. After adjusting the viscosity, 2mm zirconia balls were added and the mixture was stirred again in the Thinky mixer to prepare a slurry. The slurry was cast on a release PET film and dried at room temperature to prepare a solid electrolyte layer.

[0087] (4) Manufacturing of negative electrodes A binder solution was prepared using SBR (styrene butadiene rubber) and CMC (sodium carboxymethyl cellulose) in water as a solvent. The binder solution was then mixed with Ag nanoparticles (D50:60nm) and carbon black. The weight ratio of Ag nanoparticles, carbon black, SBR, and CMC was 25:75:6:3.

[0088] The mixture was stirred in a Thinky mixer to adjust the viscosity to an appropriate level. After adjusting the viscosity, 2 mm zirconia balls were added and stirred again in the Thinky mixer to prepare a slurry. The stirred slurry was coated on SUS foil and then vacuum dried at 100°C to prepare a negative electrode with a thickness of 10 μm.

[0089] (5) Manufacturing of all-solid-state batteries The positive electrode produced in (2) above was placed on a 2.89 cm 2 The solid electrolyte layer produced in (3) was cut into a square shape of 4.41 cm 2 The negative electrode produced in (4) above was cut into a square shape of 3.61 cm 2 After cutting into a square shape, they were stacked to produce an all-solid-state battery.

[0090] Example 2 An all-solid-state battery was manufactured in the same manner as in Example 1, except that when manufacturing the negative electrode, a mixture of Ag nanoparticles (D50:60 nm), carbon black, SBR, and CMC was prepared in a weight ratio of 25:75:8:4.

[0091] Example 3 An all-solid-state battery was manufactured in the same manner as in Example 1, except that when manufacturing the negative electrode, a mixture of Ag nanoparticles (D50:60 nm), carbon black, SBR, and CMC was prepared in a weight ratio of 25:75:10:5.

[0092] Example 4 An all-solid-state battery was manufactured in the same manner as in Example 1, except that when manufacturing the negative electrode, a mixture of Ag nanoparticles (D50:60 nm), carbon black, SBR, and CMC was prepared in a weight ratio of 25:75:7.5:1.5.

[0093] Example 5 An all-solid-state battery was manufactured in the same manner as in Example 1, except that when manufacturing the negative electrode, a mixture of Ag nanoparticles (D50:60 nm), carbon black, SBR, and CMC was prepared in a weight ratio of 25:75:4.5:4.5.

[0094] Example 6 An all-solid-state battery was manufactured in the same manner as in Example 1, except that when manufacturing the negative electrode, Bi nanoparticles were used instead of Ag nanoparticles, and a mixture of Bi nanoparticles (D50:60 nm), carbon black, SBR, and CMC was prepared in a weight ratio of 25:75:6:3.

[0095] Example 7 An all-solid-state battery was manufactured in the same manner as in Example 1, except that when manufacturing the negative electrode, Sn nanoparticles were used instead of Ag nanoparticles, and a mixture of Sn nanoparticles (D50:60 nm), carbon black, SBR, and CMC was prepared in a weight ratio of 25:75:6:3.

[0096] Example 8 An all-solid-state battery was manufactured in the same manner as in Example 1, except that when manufacturing the negative electrode, Zn nanoparticles were used instead of Ag nanoparticles, and a mixture of Zn nanoparticles (D50:60 nm), carbon black, SBR, and CMC was prepared in a weight ratio of 25:75:6:3.

[0097] Comparative Example 1 An all-solid-state battery was manufactured in the same manner as in Example 1, except that a polymer binder solution prepared by dissolving polyvinylidene fluoride (PVDF) in N-methylpyrrolidone (NMP) was used as a binder when manufacturing the negative electrode.

[0098] At this time, the weight ratio of Ag nanoparticles (D50:60 nm), carbon black, and PVdF in the preparation was 25:75:7.

[0099] Comparative Example 2 An all-solid-state battery was manufactured in the same manner as in Example 1, except that when manufacturing the negative electrode, a mixture of Ag nanoparticles (D50:60nm), carbon black, SBR, and CMC was prepared in a weight ratio of 25:75:8.5:0.5. In this case, the viscosity of the slurry was not ensured, so a plate was not manufactured.

[0100] Comparative Example 3 An all-solid-state battery was manufactured in the same manner as in Example 1, except that when manufacturing the negative electrode, a mixture of Ag nanoparticles (D50:60nm), carbon black, SBR, and CMC was prepared in a weight ratio of 25:75:3:6. In this case, after the slurry coating, the slurry was separated from the SUS foil during the drying process, and the electrode plate was not manufactured.

[0101] Evaluation 1: Electrode plate electrical conductivity measurement The resistance of the negative electrodes produced in Examples 1 to 5 and Comparative Examples 1 to 3 was measured using a 46-pin multipoint electrode resistance measuring device. The measurement current was 1 mA, the voltage range was 0.7 V, and the resistance of the SUS foil substrate was 7*10 -5 It is ohm·cm.

[0102] The measurement results are shown in Table 1 below.

[0103] [Table 1]

[0104] Referring to Table 1, the resistance values ​​of the negative electrodes of Examples 1 to 5, which were prepared using a binder in which SBR and CMC were mixed in a weight ratio of 1:1 to 6:1, were 5.0 to 10. -2 On the other hand, in Comparative Example 1, where a PVDF binder was used instead of SBR and CMC, the negative electrode plate had a resistance of 5.6·10 -2 It was high, measured in ohms·cm.

[0105] These results indicate that the use of a binder in which SBR and CMC are mixed in a weight ratio of 1:1 to 6:1 for the negative electrode can reduce the plate resistance and improve the electrical conductivity of the negative electrode.

[0106] Evaluation 2: Electrode plate adhesion evaluation The negative electrode plates of Examples 1 to 5, 7, and 8 and the negative electrode plates of Comparative Examples 1 to 3 were cut to a width of 25 mm and fixed on a slide glass with double-sided tape. The fixed negative electrode plates were evaluated for adhesion using a tensile tester (UTM). At this time, the negative electrode plates were separated from the slide glass at 180° at a speed of 10 mm / min.

[0107] The measurement results are shown in Table 2 below.

[0108] [Table 2]

[0109] As shown in Table 2 above, the negative electrodes of Examples 1 to 5, 7, and 8, which were prepared using a binder in which the aqueous binder SBR and CMC were mixed in a weight ratio of 1:1 to 6:1, had high binding strengths of 39.3 gf / mm or more, whereas the negative electrode of Comparative Example 1, in which a PVDF binder was used instead of SBR and CMC, had a low binding strength of 7.9 gf / mm.

[0110] These results indicate that the use of a binder in which SBR and CMC are mixed in a weight ratio of 1:1 to 6:1 in the negative electrode can increase the plate binding strength and improve the stability of the electrode.

[0111] Evaluation 3: Battery output characteristics evaluation The all-solid-state batteries according to Examples 1, 2, and 4, and Comparative Example 1 were charged and discharged to evaluate the capacity retention rate relative to the initial discharge capacity. When evaluating the output characteristics, the first charge and discharge were performed at 0.1 C at 45° C., the second cycle was charged at 0.1 C and discharged at 0.33 C, and the third cycle was charged at 0.1 C and discharged at 1 C to evaluate the output characteristics.

[0112] The measurement results are shown in Fig. 3. Fig. 3 is a graph showing the results of measuring the capacity retention rate versus the initial discharge capacity of the all-solid-state batteries according to Examples 1, 2, and 4, and Comparative Example 1.

[0113] Referring to FIG. 3, it can be seen that the output characteristics of the batteries of Examples 1, 2 and 4, in which SBR and CMC were used as binders in a weight ratio of 1:1 to 6:1, are superior to the output characteristics of the battery of Comparative Example 1, in which PVDF binder was used instead of SBR and CMC.

[0114] Rating 4: Battery life rating The batteries manufactured in Examples 1 and 2 and Comparative Example 1 were charged and discharged to evaluate the battery life characteristics. When evaluating the battery life, the batteries were charged and discharged at 45° C. and 0.33 C to evaluate the battery life characteristics. The measurement results are shown in Figure 4.

[0115] Referring to FIG. 4, it can be seen that the life span of the batteries of Examples 1 and 2, which were manufactured using a binder in which SBR and CMC were mixed in a weight ratio of 1:1 to 6:1, was superior to that of the battery of Comparative Example 1, which used a PVDF binder instead of SBR and CMC.

[0116] Although the preferred embodiments of the present invention have been described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements made by those skilled in the art using the basic concept of the present invention defined in the appended claims also fall within the scope of the present invention. [Explanation of symbols]

[0117] 100: All-solid-state battery 200: Positive electrode 201: Positive electrode current collector 203: Positive electrode active material layer 300: Solid electrolyte layer 400, 400': Negative pole 401, 401': Negative electrode current collector 403, 403': Negative electrode active material layer 405': Lithium deposit layer 500: Case

Claims

1. an electrode assembly including a negative electrode, a positive electrode, and a solid electrolyte disposed between the negative electrode and the positive electrode; and A case for accommodating the electrode assembly An all-solid-state battery comprising: the negative electrode includes a negative electrode current collector and a negative electrode active material layer including a negative electrode active material and a binder, the negative electrode active material includes a carbon-based material and metal particles, the binder comprises a first polymer of a butadiene-based rubber and a second polymer selected from a carboxyalkyl cellulose, where the alkyl is an alkyl having 1 to 6 carbon atoms, a salt thereof, and a combination thereof; The first polymer and the second polymer are included in a weight ratio of 1:1 to 6:1, The metal particles have a size of 5 nm to 800 nm. All-solid-state battery.

2. 2. The all-solid-state battery according to claim 1, wherein the metal particles are any one selected from Ag, Zn, Al, Sn, Mg, Ge, Cu, In, Ni, Bi, Au, Si, Pt, Pd, or a combination thereof.

3. The all-solid-state battery of claim 1 , wherein the carbon-based material is a non-graphitic carbon.

4. The solid-state battery of claim 3 , wherein the non-graphitic carbon has a secondary particle form in which a plurality of primary particles are aggregated.

5. The all-solid-state battery according to claim 4, wherein the primary particles have a particle size of 20 nm to 100 nm.

6. The all-solid-state battery according to claim 3 , wherein the non-graphitic carbon is any one selected from the group consisting of carbon black, activated carbon, acetylene black, denka black, ketjen black, and combinations thereof.

7. The all-solid-state battery according to claim 1, wherein the binder is contained in an amount of 0.01 to 40 parts by weight based on 100 parts by weight of the negative electrode active material.

8. 2. The solid-state battery of claim 1, wherein the butadiene-based rubber is any one selected from the group consisting of styrene butadiene rubber (SBR), nitrile butadiene rubber (NBR), acrylate butadiene rubber (ABR), methacrylate butadiene rubber, acrylonitrile-butadiene-styrene (ABS) rubber, styrene-butadiene-styrene (SBS) rubber, and combinations thereof.

9. The all-solid-state battery according to claim 1 , wherein the solid electrolyte is a sulfide-based solid electrolyte.

10. The solid electrolyte is Li a M b P c S d A e (a, b, c, d, and e are all greater than or equal to 0 and less than or equal to 12; M is Ge, Sn, Si, or a combination thereof; and A is one of F, Cl, Br, or I.

11. 10. The all-solid-state battery of claim 1, wherein no solid electrolyte is present in the negative electrode.

12. The all-solid-state battery according to claim 1 , wherein the negative electrode has an adhesive strength of the electrode plate of 10 gf / mm or more.

13. The all-solid-state battery according to claim 1 , wherein the negative electrode further comprises a lithium deposition layer in which lithium is deposited during charging.

14. The all-solid-state battery according to claim 13, wherein the lithium deposition layer has a thickness of 10 μm to 50 μm.

15. The all-solid-state battery according to claim 1 , further comprising a buffer material between the negative electrode and the case.

Citation Information

Patent Citations

  • Negative electrode structure of lithium battery and preparation method thereof

    CN108336293A

  • Secondary battery and method for manufacturing secondary battery

    JP2016139608A

  • Lithium ion secondary battery

    JP2017152198A

  • Non-aqueous electrolyte secondary battery

    WO2017187638A1

  • Fully solid-state secondary battery and method of manufacturing same

    WO2019188487A1