Powder hot isostatic pressing cycle
By controlling pore morphology through adjusted temperature, pressure, and duration in the HIP process, the method addresses the issue of gas pores in metal powders, enhancing the mechanical properties and fatigue resistance of powder metallurgy articles.
Patent Information
- Application Number
- JP2023519050
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-09-24
- Filing Date
- 2021-09-21
- Publication Date
- 2024-12-09
- Estimated Expiration
- 2041-09-21
AI Technical Summary
Gas pores entrained during the production of metal powders, particularly through gas atomization, adversely affect the mechanical properties of powder metallurgy-fabricated articles, especially fatigue properties, and cannot be fully eliminated by conventional hot isostatic pressing (HIP).
A method and apparatus for HIP that involves isostatically compressing a precursor metal with closed pores, followed by controlled adjustments of temperature, pressure, and duration to modify the morphology of these pores, favoring spherical shapes, thereby reducing stress concentrations and enhancing mechanical properties.
The method effectively reduces the detrimental effects of gas pores on the mechanical properties of fabricated articles, improving fatigue resistance and overall performance by controlling pore morphology during the HIP process.
Smart Images

Figure 0007596519000009 
Figure 0007596519000010 
Figure 0007596519000011
Abstract
Description
[Technical field]
[0001] This invention relates to hot isostatic pressing. [Background technology]
[0002] Powder metallurgy (PM), including powder forging, hot isostatic pressing (HIP), metal injection molding (MIM), electric current assisted sintering (ECAS), and additive manufacturing (AM), provides near-net-shape (NNS) fabrication of articles from metal powders, preferably spherical metal powders. Spherical metal powders are typically produced by plasma spheroidization or spraying, including gas atomization (GA), plasma spheroidization (PS), plasma spraying (PA), and plasma rotating electrode process (PREP). GA and PA typically produce relatively finer powders compared to PREP and are therefore preferred for some PM techniques. Contaminant levels in GA powders are relatively lower than PA powders and therefore may be preferred for some metals. However, GA can result in gas entrapment as pores in the GA powder. These gas pores are detrimental to the mechanical properties, especially fatigue properties, of PM-produced articles and cannot be completely eliminated using HIP.
[0003] Therefore, PM needs to be improved. Summary of the Invention
[0004] One object of the present invention is, inter alia, to provide an apparatus and method for HIP that at least partially eliminates or mitigates at least some of the disadvantages of the prior art, whether identified herein or elsewhere. For example, it is an object of an embodiment of the present invention to provide a method of HIP that reduces the effect of entrapped gas porosity on the mechanical properties of PM-produced articles. For example, it is an object of an embodiment of the present invention to provide an apparatus for at least partially producing an article using HIP that improves control of its mechanical properties. For example, it is an object of an embodiment of the present invention to provide an article that is at least partially produced using HIP and has improved mechanical properties compared to an article that is at least partially produced using conventional HIP.
[0005] A first aspect provides a method of at least partially fabricating an article from a precursor thereof, the method comprising: providing a precursor, wherein the precursor comprises a metal having closed pores therein; isostatically pressing the precursor, thereby providing a pressed precursor; hot isostatically pressing (HIP) the compressed precursor at an Nth temperature of the set of temperatures, an Nth pressure of the set of pressures, and for an Nth duration of the set of durations, thereby at least partially producing the article; Equipped with.
[0006] A second aspect provides a hot isostatic pressing (HIP) apparatus for at least partially fabricating an article from a precursor thereof, the apparatus comprising: The method is configured to HIP a precursor comprising a metal having closed pores therein at an Nth temperature of the set of temperatures, at an Nth pressure of the set of pressures, and for an Nth duration of the set of durations by adjusting the set of temperatures, the set of pressures, and / or the set of durations to at least partially control the morphology of the closed pores, thereby at least partially producing the article.
[0007] A third aspect provides an article formed according to the method of the first aspect and / or the apparatus of the second aspect.
[0008] A fourth aspect provides a computer comprising a processor and a memory configured to at least partly carry out a method according to the first aspect.
[0009] A fifth aspect provides a computer program comprising instructions which, when executed by a computer comprising a processor and a memory, cause the computer to perform, at least in part, a method according to the first aspect.
[0010] A sixth aspect provides a non-transitory computer-readable storage medium comprising instructions that, when executed by a computer comprising a processor and a memory, cause the computer to perform, at least in part, a method according to the first aspect.
[0011] A seventh aspect provides a method of at least partially fabricating an article from a precursor thereof, the method comprising: providing a precursor, wherein the precursor comprises a metal having closed porosity therein; hot isostatically pressing (HIPing) the precursor at an Nth temperature of a set of temperatures, an Nth pressure of a set of pressures, and for an Nth duration of a set of durations, thereby at least partially fabricating the article, wherein HIPing the precursor comprises adjusting the set of temperatures, the set of pressures, and / or the set of durations to at least partially control the morphology of the closed porosity.
[0012] [Detailed Description of the Invention] According to the present invention there is provided a method, and also an apparatus and an article, as set out in the accompanying claims. Further features of the invention will be apparent from the dependent claims and the following description.
[0013] [method] A first aspect provides a method of at least partially fabricating an article from a precursor thereof, the method comprising: providing a precursor, wherein the precursor comprises a metal having closed pores therein; isostatically pressing the precursor, thereby providing a pressed precursor; hot isostatically pressing (HIP) the compressed precursor at an Nth temperature of the set of temperatures, an Nth pressure of the set of pressures, and for an Nth duration of the set of durations, thereby at least partially producing the article; Equipped with.
[0014] In one preferred example, the first aspect provides a method of making an article from a precursor thereof, the method comprising: providing a precursor comprising: enclosing a powder of an α+β Ti alloy in a container, wherein the powder is formed by electrode-induced gas atomization (EIGA); cold pressing the precursor by isostatically pressing the precursor at a first pressure, thereby providing a compressed precursor; hot isostatically pressing (HIP) the compressed precursor at an Nth pressure in the range of 75 MPa to 150 MPa and at an Nth temperature in the range of 850°C to 950°C, thereby producing an article. wherein the ratio of the first pressure to the Nth pressure is in the range of 1:2 to 9:10.
[0015] In this way, by isostatically pressing the precursor prior to or as part of the HIP of the precursor, the morphology (i.e., shape) of the closed pores in the metal is controlled during HIP, thereby defining the morphology of the remaining closed pores in the article. In particular, by controlling the morphology of the closed pores in this way, the remaining closed pores in the article may be relatively more spherical, thereby reducing the deleterious effects resulting therefrom. In particular, relatively more spherical, ideally spherical, closed pores result in relatively lower stress concentrations compared to, for example, ellipsoidal or toroidal closed pores. In this way, the effect of closed pores on the mechanical properties of the produced article, e.g., the deleterious effects on fatigue properties, is attenuated compared to articles at least partially produced using conventional HIP.
[0016] In other words, the method comprises modifying the HIP cycle when, for example, using titanium alloy powder to manufacture aircraft components (i.e., articles). The method is particularly beneficial when using powders produced by GA, such as EIGA, which may result in argon gas entrapment, but which may be preferred over using powders produced by PA due to reduced contamination. In particular, argon is substantially insoluble in titanium, and thus remains as an entrapped gas even after HIP. The method is also suitable for PM articles made using any powder that is susceptible to gas entrapment, since gas may remain entrapped in pores therein, even when PM involves a melting process such as electron beam powder bed selective melting or laser powder bed selective melting.
[0017] It is understood that temperatures, pressures, and times defined herein are in SI units unless otherwise stated. It is understood that, in general, the temperature change applied to the precursor during HIP requires equilibration across the precursor, the duration of which depends at least in part on the rate of temperature change, the magnitude of temperature change, the thermal mass of the precursor, the thermal conductivity of the precursor, and / or the dimensions of the precursor. It is understood that pressure is the pressure applied to the precursor during HIP (see pressure in closed pores). In contrast to temperature changes, pressure changes are experienced immediately by the entire precursor.
[0018] Modifications to the HIP cycle are intended to control the way in which entrapped bubbles of argon or the like (i.e., closed pores) within the powder granules (i.e., particles) are compressed and the subsequent shape that these bubbles develop, as well as to avoid damage caused by subsequent high temperature heat treatment cycles (e.g., annealing or stress relieving) or exposure to high temperatures during service.
[0019] [Manufacture] The method is to at least partially fabricate an article from its precursor. That is, fabricating (i.e., manufacturing, shaping) the article from its precursor includes HIP as described herein. It is understood that fabricating the article may include other steps before and / or after HIP. For example, fabricating the article may include additive manufacturing, thereby providing a precursor before HIP. For example, fabricating the article may include heat treating, thermo-mechanical forming, and / or machining (i.e., subtractive manufacturing) the article after HIP.
[0020] [Goods] The method comprises fabricating the article at least in part from a precursor thereof.
[0021] In one example, the article comprises and / or is an aerospace component, such as an airframe component, a vehicle component, such as an engine component, or a medical component, such as an implantable medical device.
[0022] [Precursor] The method involves fabricating an article at least in part from a precursor thereof, which should be understood to be a precursor to an article, such as a powder, an encapsulated powder, a casting, a sintered part, or a part produced by additive manufacturing (AM).
[0023] The method comprises providing a precursor, the precursor comprising a metal having closed porosity therein, i.e., the precursor has closed porosity in the metal, for example, the closed porosity can be in a powder particle, a casting, a sintered part, or a part produced by AM.
[0024] In one example, providing the precursor comprises additive manufacturing, e.g., selective laser melting a powder comprising a set of particles including the first particles. In one example, providing the precursor comprises additive manufacturing (AM) of the precursor from a feed material, e.g., the powder comprises a metal having closed pores therein, and / or the closed pores are formed during AM. That is, the precursor is provided by AM and then HIPed as described herein, e.g., to reduce porosity and / or increase its density.
[0025] In one example, the precursor comprises a powder comprising a set of particles including a first particle, the first particle comprising closed porosity. In one example, providing the precursor comprises enclosing a powder of a metal having closed porosity therein, for example in a container. Typically, the container is removed by machining after HIPing.
[0026] [Additive Manufacturing] ISO / ASTM 52900-15 defines seven categories of additive manufacturing processes, including binder jetting, directed energy deposition (DED), material extrusion, material jetting, powder bed fusion (PBF), sheet lamination, and bath photopolymerization. These additive manufacturing processes are well known.
[0027] In particular, DED and PBF techniques such as direct metal laser sintering (DLMS), selective thermal sintering (SHS), selective laser sintering (SLS), selective laser melting (SLM), laser metal deposition (LMD), and electron beam melting (EBM) are suitable for making (i.e., manufacturing, forming) metal articles, for example, from feed materials such as metal powders and / or wires (also known as filaments). Similarly, polymeric articles may be manufactured from feed materials such as powders and / or filaments comprising polymer compositions, including thermoplastics. The feed material may be heated to high temperatures, including melting thereof, for example, at temperatures of about 1000° C. to about 1000° C.
[0028]
number
[0029] is heated to a temperature T in the range of m is the absolute melting temperature of the feed material (K).
[0030] In one example, the AM comprises and / or is DED, such as wire or powder DED, and / or PBF, such as DMLS, SHS, SLS, SLM, LMD, or EBM.
[0031] metal In one example, the metal is a transition metal, e.g., a first, second, or third row transition metal. In one example, the metal is Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, or Zn. In one example, the metal is Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Ag, or Cd. In one example, the metal is Hf, Ta, W, Re, Os, Ir, Pt, Au, or Hg.
[0032] It should be understood that non-alloy metal refers to a metal having a relatively high purity, for example, a purity of at least 95%, at least 97%, at least 99%, at least 99.5%, at least 99.9%, at least 99.95%, at least 99.99%, at least 99.995%, or at least 99.999% by weight.
[0033] In one example, the metal comprises a ferrous or non-ferrous alloy, such as a stainless steel, an Al alloy, a Cu alloy, a Ti alloy, a Ni alloy, or a mixture of their respective alloys, preferably corresponding and / or compatible alloys thereof (e.g., having a similar or the same nominal composition).
[0034] In one example, the metal comprises a first row transition metal, such as Sc, Ti, Cr, Mn, Ni, or Cu, a second row transition metal, such as Zr or Nb, a Group III element, such as Al, and / or mixtures thereof, such as alloys.
[0035] In one preferred example, the metal comprises and / or consists of a Ti alloy, for example, Ti-6Al-4V alloy according to AMS 4911R, AMS 4928W, AMS 4965K, and AMS 4905F, as described below.
[0036] [Ti alloy] In one example, the metal may be a Ti alloy powder, such as an α+β Ti alloy, or an α+β Ti alloy having a beta transus temperature β transus The present invention comprises and / or is an α+β Ti alloy that has been heat treated beyond
[0037] [α+β Ti alloy] Elements with atomic radii within ±15% of the atomic radius of Ti are substitutional elements and have significant solubility in Ti. Elements with atomic radii less than 59% of the atomic radius of Ti, such as H, N, O, and C, occupy interstitial sites and also have substantial solubility. The relatively high solubility of substitutional and interstitial elements in Ti makes it difficult to design precipitation-hardened Ti alloys. However, B has a radius similar to but larger than C, O, N, and H, and is therefore capable of inducing Ti boride precipitation. In some alloys, Cu precipitation is also possible.
[0038] Substitutional elements can be classified according to their effect on the stability of the α and β phases. Thus, Al, O, N, and Ga are α stabilizers, while Mo, V, W, and Ta are all β stabilizers. Cu, Mn, Fe, Ni, Co, and H are also β stabilizers, but form eutectoids. The eutectoid reaction is often slow (because substitutional atoms are involved) and inhibited. Mo and V have the greatest effect on β stability and are common alloying elements. W is rarely added due to its high density. Cu is the most common alloying element in TiCu. 2 which makes such Ti alloys age hardenable and heat treatable. Zr, Sn and Si are neutral elements.
[0039] Interstitial elements do not fit properly into the Ti lattice, causing changes in the lattice parameters. Hydrogen is the most important interstitial element. Body-centered cubic (BCC) Ti has three octahedral interstices per atom, while hexagonal close-packed (CPH) Ti has one octahedral interstices per atom. The latter is therefore larger, and therefore the solubility of O, N, and C is much higher in the α phase.
[0040] Most α+β Ti alloys (also known as α-β Ti alloys, alpha-beta Ti alloys, dual-phase Ti alloys, or two-phase Ti alloys) have high strength and formability and contain 4-6 wt. % β stabilizers that allow a substantial amount of β to be retained upon quenching from the β→α+β phase. A typical α+β Ti alloy is Ti-6Al-4V (all nominal compositions by weight unless otherwise noted), while other α+β Ti alloys include Ti-6Al-6V-2Sn and Ti-6Al-2Sn-4Zr-Mo. Al reduces alloy density, stabilizes and strengthens the α phase, and increases the α+β→β transformation temperature, while V provides a greater amount of the more ductile β phase for hot working and reduces the α+β→β transformation temperature. Table 1 shows the nominal compositions of selected α+β Ti alloys.
[0041] [Table 1]
[0042] Table 1: Nominal composition of selected α+β Ti alloys; (a) Mechanical properties given for the annealed condition; may be solution-treated and aged to increase strength; (b) Mechanical properties given for the solution-treated and aged condition; alloys not typically applied in the annealed condition; (c) Semi-commercial alloys; mechanical properties and compositional limitations subject to negotiation with suppliers; (d) Primarily pipe alloys; may be cold drawn to increase strength; (e) Combined O 2 +2N 2= 0.27%; (f) similarly solution treated and aged using alternative aging temperatures (480°C or 900°F); (g) sum of other elements (wt%, max) 0.40; (h) each of other elements (wt%, max) 0.10; (i) Y (wt%, max) 0.005; (j) Y (wt%, max) 0.05; (k) Ru (wt%, min) 0.08, Ru (wt%, max) 0.14.
[0043] Ti-6Al-4V (martensitic α+β Ti alloy; K β =0.3) accounts for about half of all Ti alloys produced and is popular due to its strength (1100 MPa), creep resistance at 300°C, fatigue resistance, good castability, plastic workability, heat treatability, and weldability. Depending on the mechanical properties required, heat treatments applied to Ti-6Al-4V alloy, and more generally to α+β Ti alloys, include partial annealing (600-650°C for about 1 hour), full annealing (700-850°C followed by furnace cooling to about 600°C, followed by air cooling), or solutionizing (880-950°C followed by water quenching) and aging (400-600°C).
[0044] The α+β Ti alloys constitute a very important group of structural materials used in aerospace applications. The microstructure of these α+β Ti alloys can be significantly modified during thermomechanical processes and / or heat treatments, making it possible to tailor their mechanical properties, including fatigue behavior, to specific application requirements.
[0045] The main types of microstructures in α+β Ti alloys are: 1. A lamella having a beta transus temperature β transus formed after slow cooling when deformation or heat treatment is carried out at temperatures above 1000° C. in a single-phase β field, and comprising colonies of HCP α lamellae within large BCC β grains having diameters of several hundred microns; 2. Equiaxed, two-phase α + β field (i.e., β transus temperature β transus It is formed after deformation at 0.055 K or less and comprises spherical α phase dispersed in a β phase matrix.
[0046] In one example, the Mth temperature in the set of temperatures is the beta transus temperature β of an α+β Ti alloy. transus is less than.
[0047] Beta transus temperature β transus is the temperature at which the α+β→β transformation occurs. This means that the Ti alloy has a volume fraction of BCC β phase, V f = 1 is the lowest temperature.
[0048] The lamellar microstructure is characterized by relatively low tensile ductility, moderate fatigue properties, and good creep and crack growth resistance. Important parameters of the lamellar microstructure with respect to mechanical properties include the β-grain size D, the size of the colonies of α-phase lamellae d, the thickness t of the α-phase lamellae, and the morphology of the interlamellar interfaces (β-phase). In general, an increase in the cooling rate leads to a refinement of the microstructure, with both the α-phase colony size d and the α-phase lamella thickness t being reduced. In addition, new α-phase colonies tend to nucleate not only on the β-phase boundaries, but also on the boundaries of other α-phase colonies, growing perpendicular to the existing α-phase lamellae. This leads to the formation of a characteristic microstructure called the "basket weave" or Widmanstätten microstructure.
[0049] Equiaxed microstructures have a better balance of room temperature strength and ductility, and fatigue properties that depend significantly on the crystallographic texture of the HCP α phase.
[0050] A favorable balance of properties can be obtained by the development of a bimodal microstructure consisting of primary α-grains and fine lamellar α-colonies within relatively small β-grains (10-20 μm in diameter).
[0051] The phase composition of an α+β Ti alloy after cooling from the β phase is at least partially controlled by the cooling rate. The kinetics of the phase transformation is governed by the β phase stability factor K βThe range of α + β → β phase transformation temperatures at least partially determines the conditions of the thermomechanical processes intended to develop the desired microstructure. The start and end temperatures of the α + β → β phase transformation vary at least partially as a function of the amount of β stabilizing elements (Table 2).
[0052] [Table 2]
[0053] Table 2: Onset and end temperatures of the α+β→β phase transformation in selected α+β Ti alloys (v h =v c =0.08℃ -1 );ns: nucleation start;ps: precipitation start;s: start;f: end.
[0054] Beta transus temperature β transus The microstructure of α+β Ti alloys after deformation or heat treatment beyond 18°C depends at least in part on the cooling rate. -1 ) is the β-phase stability coefficient K β <1, resulting in a martensitic α' (α'') microstructure and a higher β-phase stability factor, K β In the case of alloys with metastable β M Low and moderate cooling rates lead to the development of a lamellar microstructure consisting of colonies of α lamellae within large β grains. A decrease in cooling rate causes an increase in both the thickness t of the individual α lamellae and the size d of the α colonies. These in turn reduce the yield stress and tensile strength of these α+β Ti alloys.
[0055] The lamellar α-phase microstructure of α+β Ti alloys heat treated in the β-phase has a beneficial effect on fatigue behavior due to frequent changes in crack direction and secondary crack branching. If the α-phase lamellae are too large, the thin layer of β-phase cannot absorb a large amount of energy and slows down the crack propagation. In this case, the α-phase colonies behave as a single element of the microstructure. This phenomenon is consistent with the smaller β-phase stability factor K, such as Ti-6Al-4V.β This is more pronounced in α+β Ti alloys. If the β phase is thick enough, it can absorb energy during the plastic deformation of the region ahead of the crack tip, slowing down the crack propagation speed and thus contributing to increasing the fatigue life.
[0056] In one example, the metal may be Tekna Ti64® available in ASTM Grade 5 and Grade 23 with particle size distributions of -25 / 5, -45 / 15, -53 / 20, -105 / 45, and -250 / 90 available from Tekna Plasma Systems Inc. (Canada); Carpenter CT PowderRange Ti64 S® available in ASTM Grade 5 and Grade 23 available from Carpenter Technology Corporation (USA); Osprey Ti-6Al-4V Grade 5® and / or Osprey Ti-6Al-4V Grade 23® available from Sandvik AB (Sweden) and produced by EIGA; CPTi-Gr.1, Gr.2, Ti64-Gr.5, Gr.23, Ti6242, Ti5553, and / or Beta available from GKN Sinter Metals Engineering GmbH (Germany). 21S. Similar Ti alloys include LPW Ti6-4 High Performance Titanium, UNS R56400 / R56407, 3D Systems Ti Gr.23, Concept Laser CL 41 TI ELI, EOS Ti64ELI, Renishaw Ti6Al4V ELI-0406, SLM Solutions TiAl6V4, and TRUMPF TitaniumT:64 ELI-A LMF. In one example, the metal comprises and / or is a Ni alloy selected from Osprey Alloy 625® and / or Osprey Alloy 718® available from Sandvik AB (Sweden), IN625, IN718, and / or Ni-Ti available from GKN Sinter Metals Engineering GmbH (Germany). In one example, the metal comprises and / or is an Al alloy selected from AlSi7Mg, AlSi10Mg, and / or Al4047 available from GKN Sinter Metals Engineering GmbH (Germany).In one example, the metal comprises and / or is an Al alloy selected from 304L, 316L, 420, and / or 17-4PH available from GKN Sinter Metals Engineering GmbH, Germany. In one example, the metal comprises and / or is an Fe alloy selected from 4340, 4630, 5120, 8620, 20MnCr5, 42CrMo4, 1.2709, H13, Fe-Si, and / or Fe-Ni available from GKN Sinter Metals Engineering GmbH, Germany.
[0057] In one example, the metal comprises and / or is a Ti alloy, such as an α+β Ti alloy, the Nth pressure is in the range of 75 MPa to 150 MPa, preferably in the range of 90 MPa to 125 MPa, and / or the Nth temperature is in the range of 850°C to 950°C, preferably in the range of 875°C to 925°C.
[0058] [Powder] It should be understood that a powder comprises particles that are solid and may include discrete and / or aggregated particles. In one example, the particles have a regular shape, such as a spherical shape. In one example, the particles have an irregular shape, such as a spheroidal, flaky, or granular shape.
[0059] In general, the powder may comprise any material suitable for fusing by melting. The powder may comprise a metal such as Al, Ti, Cr, Fe, Co, Ni, Cu, W, Ag, Au, Pt, and / or alloys thereof. In general, the powder may comprise any metal from which particles can be produced by atomization. The particles can be produced by atomization, such as gas atomization, close-coupled gas atomization, plasma atomization, or water atomization, or other processes known in the art. The particles can have regular shapes, such as spherical, and / or irregular shapes, such as spheroidal, flaky, or granular.
[0060] These particles may have a size of at most 300 μm, at most 250 μm, at most 200 μm, at most 150 μm, at most 100 μm, at most 75 μm, at most 50 μm, at most 25 μm, at most 15 μm, at most 10 μm, at most 5 μm, or at most 1 μm. These particles may have a size of at least 150 μm, at least 100 μm, at least 75 μm, at least 50 μm, at least 25 μm, at least 15 μm, at least 10 μm, at least 5 μm, or at least 1 μm. Preferably, these particles have a size in the range of 10 μm to 200 μm. More preferably, these particles have a size in the range of 60 μm to 150 μm. In one example, the powder comprises particles having a size in the range of 5 μm to 200 μm, preferably 10 μm to 150 μm. For example, in the case of L-PBF of Ti alloys, the powder preferably comprises particles having a size in the range of 15 μm (D10) to 45 μm (D90) and / or in the range of 20 μm (D10) to 63 μm (D90), while in the case of EBM of Ti alloys, the powder preferably comprises particles having a size in the range of 45 μm (D10) to 105 μm (D90). For example, in the case of L-PBF of Ni, Al alloys, and stainless steels, the powder preferably comprises particles having a size in the range of 15 μm (D10) to 53 μm (D90), while in the case of EBM of Ni, Al alloys, and stainless steels, the powder preferably comprises particles having a size in the range of 50 μm (D10) to 150 μm (D90).
[0061] In the case of regular shapes, size may refer to, for example, the diameter of a sphere or rod, or the side of a rectangular prism. Size may also refer to the length of a rod. In the case of irregular shapes, size may refer to, for example, the largest dimension of the particle. Particle size distribution may be measured by the use of light scattering measurement of particles in an instrument such as a Malvern Mastersizer 3000 configured to measure particle sizes from 10 nm to 3500 micrometers, where the particles are wet dispersed (with a suitable dispersant that matches the particle surface chemistry and the liquid chemistry) in a suitable carrier liquid according to the instrument manufacturer's instructions and assuming the particles are of uniform density. Particle size distribution may be measured according to ASTM B822-17 Standard Test Method for Particle Size Distribution of Metal Powders and Related Compounds by Light Scattering.
[0062] In one example, the particles have a relatively small particle size D, for example, up to 50 μm, preferably up to 20 μm. In one example, the particles have a relatively wide particle size D distribution, including non-monomodal (e.g., bimodal) particles / or non-monodisperse (i.e., not a single particle size) size distribution, for example, D90 / D10 is at least 3, preferably at least 5, more preferably at least 10. In one example, the particles have a relatively high angle of repose, for example, at least 30°, more preferably at least 40°. In one example, the particles have a relatively high powder anisotropy, such that the stresses in the powder are not equal in all directions, and / or have a relatively high friction, such that the shear stresses in the powder may be near the wall.
[0063] In one example, the powder comprises additives, alloying additives, fluxes, binders, and / or coatings. In one example, the powder comprises particles having different compositions, e.g., a mixture of particles having different compositions.
[0064] Generally, spherical metal powders are the preferred feedstock for near-net-shape (NNS) fabrication via powder metallurgy (PM), including powder forging, hot isostatic pressing (HIP), metal injection molding (MIM), electric current assisted sintering (ECAS), and additive manufacturing (AM).
[0065] For example, for titanium alloy powders, important properties for PM include particle size, particle size distribution, flowability, and chemical composition, including oxygen content. The particle size distribution (PSD) requirements vary depending on the application: ≦45 μm (325 mesh) for MIM, 15 μm-45 μm for SLM, 10-45 μm for cold spray, and 45 μm-106 μm for EBM. Oxygen is a strong solution strengthener for titanium alloys, but in excess, ductility and fracture toughness will be compromised. To meet the oxygen requirements of industrial standards for the final manufactured components, which are typically less than 0.2 wt%, the oxygen content of the titanium alloy powder should be ≦0.15 wt%. Preferably, the powder has high purity, high sphericity, and flowability, as well as no entrapped gas bubble porosity. However, in general, the oxygen content of titanium alloy powders is inversely proportional to the particle size. Furthermore, most NNS processes require the powder to have good flowability, which is influenced by powder shape and size, interparticle friction, material type, and environmental factors. In general, powders with good flowability should preferably have a spherical shape and the particle size should be relatively large; that is, as the particle size decreases, the flowability also decreases. Furthermore, the powder preferably has good apparent density and tap density, which also affects the density and uniformity of the manufactured parts.
[0066] Typically, spherical titanium powders are produced by plasma spheroidization or atomization, including gas atomization (GA), plasma spheroidization (PS), plasma atomization (PA), and plasma rotating electrode process (PREP). Gas atomization includes free-fall gas atomization (FFGA), close-coupled gas atomization (CCGA), and electrode-induced gas atomization (EIGA). PREP powders are considered to have very high purity and nearly perfect sphericity. However, the particle size of PREP powders is typically relatively coarse, e.g., 50 μm to 350 μm, which is coarser than desired for SLM, EBM, and MIM applications. However, relatively finer spherical titanium alloy powders can be produced via the GA and PA processes. Typical particle sizes of GA and PA titanium alloy powders range from 10 μm to 300 μm.
[0067] All atomization processes involve melting, atomization, and solidification. Melting is typically by vacuum induction melting, plasma arc melting, including RF plasma arc melting, induction drip melting, or direct plasma heating. Atomization breaks up the liquid metal into droplets that solidify in flight in an inert atmosphere, typically accomplished using high pressure gas, usually argon, to break up the liquid metal stream through a nozzle. The inert atmosphere is usually ultra-high purity argon or helium to reduce oxygen contamination.
[0068] EIGA generally produces ceramic-free powders, where the liquid metal does not come into contact with any refractory metal or other ceramic components that may introduce contamination. In particular, in contrast to PA, EIGA powders are free of tungsten contamination and may therefore be preferred.
[0069] However, GA typically results in the formation of satellite particles, which are fine particles that bounce off and collide with the partially molten particles as a result of the circulation of gas in the atomization chamber. The satellite particles are detrimental to the free flow of the particles. Furthermore, GA typically results in the formation of gas porosity or gas bubbles in the powder as a result of the high pressure gas used for atomization being entrained in the liquid metal. These gas porosity are detrimental to the mechanical properties, especially the fatigue properties, of the PM article and cannot be completely eliminated by using HIP. Furthermore, these gas porosity may remain after PBF and subsequent HIP of the article.
[0070] More specifically, argon entrapment in EIGA powder takes the form of, for example, a single nominally spherical bubble formed during the solidification process. In the EIGA powder manufacturing process, argon is used to generate particles by being blown into a gas stream of molten titanium (or titanium alloy). Bubbles tend to occur only in particles above a certain size, and are typically not found in powder particles less than about 50 μm in diameter. For powder bed selective laser melting AM, the EIGA powder used typically has a particle size distribution (PSD) of 15 μm to 45 μm, thus avoiding the problem of argon entrapment. However, this relatively narrow particle size distribution used in SLM is not suitable for powder HIP, where a relatively wide particle size distribution is required to increase the "tap density" (i.e., density of the uncompressed powder). This is necessary because powder HIP relies on filling, evacuating, and sealing a molding canister containing the powder, and subsequent overall compression during HIP, to create the desired near-net-shape product. Too low a tap density will result in excessive compaction during HIP, which will be more costly, however, EIGA titanium alloy powders are desirable for HIP because tungsten contamination is avoided.
[0071] In one example, the powder is formed by gas atomization, and optionally the first particles have a dimension of at least 50 μm.
[0072] [Closed pores]It should be understood that the closed pores contain the entrapped gas. For example, the gas can be entrapped during the production of the metal, such as being entrapped in the GA of the metal powder. For example, the gas can be entrapped in the AM of the metal powder or other feedstock in a protective atmosphere comprising the gas (more generally known as porosity). It should be understood that the pores are closed, i.e., the entrapped gas is contained within the pores. In one example, the gas is an inert gas, such as a noble gas like argon, helium, or neon. In one example, the gas has a relatively low solubility in the metal. In one example, the closed pores in the precursor metal have dimensions, such as diameters, in the range of 1 μm to 250 μm, preferably in the range of 10 μm to 100 μm, more preferably in the range of 25 μm to 75 μm. It should be understood that the volume of the closed pores is smaller than the volume of the metal having the closed pores therein. In one example, the closed pores in the precursor metal are spherical or substantially spherical. In one example, the closed pores in the precursor metal are substantially spherical, for example, an oblate spheroid, where a / 2 < c < a, or a prolate spheroid, where a < c < 2a. The morphology of the closed pores in the precursor metal can be determined using optical microscopy of the mounted and polished metal microstructure sample in combination with image analysis software, for example, using an OLYMPUS digital microscope DSX1000 (available from Olympus Corporation, Japan) equipped with a DP27 digital camera in combination with OLYMPUS (registered trademark) Stream image analysis software. In this way, a 2D morphological determination of the closed pores in the precursor metal can be provided. It should be understood that this determination of the morphology of the closed pores in the precursor metal is destructive, and thus the morphological determination of the closed pores in the precursor metal is of that sample and is thus a statistical determination.Additionally and / or alternatively, the morphology of the closed pores in the precursor metal can be determined using CT, such as X-ray computed tomography (CT), for example using an XT H 225 ST (available from Nikon Metrology Europe NV, Belgium) equipped with a Varian 2520Dx detector with a focal spot size of 3 μm at up to 7 W and a focal spot size of 225 μm at 225 W, 1950×1500 active pixels and a pixel size of 127 μm. In this way, for example by reconstruction of 2D slices, a 3D morphological determination of the closed pores in the precursor metal can be provided. It should be understood that this determination of the morphology of the closed pores in the precursor metal is non-destructive.
[0073] [HIP] The method comprises HIPing a precursor at an Nth temperature of a set of temperatures, an Nth pressure of a set of pressures, and for an Nth duration of a set of durations, thereby at least partially producing an article.
[0074] HIP is known. Generally, HIP is used to reduce porosity and thus densify metals, thereby improving their mechanical properties and / or workability. During HIP, the precursor is exposed to high temperatures, typically 480°C for aluminum to over 1300°C for nickel-based superalloys, at high isostatic gas pressures, typically 50 MPa to 300 MPa, for a given time. The gas is inert, typically Ar. The simultaneous heat and pressure reduce internal voids through a combination of plastic deformation, creep, and diffusion bonding, resulting in near 100% densification. HIP can be used as a post-processing step in AM.
[0075] It should be understood that the Nth temperature of the set of temperatures, the Nth pressure of the set of pressures, and the Nth duration of the set of durations are determined at least in part according to the precursor, metal, and / or article, as known to those of skill in the art, i.e., the Nth temperature of the set of temperatures, the Nth pressure of the set of pressures, and the Nth duration of the set of durations may be determined in a conventional manner.
[0076] [Adjustment] Isostatically pressing the precursor and HIPing the compressed precursor comprises adjusting a set of temperatures, a set of pressures, and / or a set of durations to at least partially control the closed pore morphology. That is, in contrast to conventional HIPing, a set of temperatures, a set of pressures, and / or a set of durations are adjusted to at least partially control the closed pore morphology. For example, heating and / or pressurization to an Nth temperature of the set of temperatures and an Nth pressure of the set of pressures, respectively, can be adjusted to at least partially control the closed pore morphology. For example, cooling and / or depressurization from an Nth temperature of the set of temperatures and an Nth pressure of the set of pressures, respectively, can be adjusted to at least partially control the closed pore morphology.
[0077] In this way, by adjusting the temperature set, pressure set, and / or duration set during isostatic pressing and HIPing of the precursor, the morphology (i.e., shape) of the closed pores in the metal is controlled during isostatic pressing and HIPing, thereby defining the morphology of the residual closed pores in the article. In particular, by controlling the morphology of the closed pores during isostatic pressing and HIPing in this way, the residual closed pores in the article may be relatively more spherical, thereby reducing the deleterious effects resulting therefrom. In particular, relatively more spherical, ideally spherical, closed pores result in relatively lower stress concentrations, as compared to, for example, ellipsoidal or toroidal closed pores. In this way, the effect of closed pores on the mechanical properties of the produced article, such as the potentially deleterious effects on fatigue properties, is attenuated as compared to articles at least partially produced using conventional HIPing.
[0078] In one example, the closed pores in the metal of the article are spherical or substantially spherical. In one example, the closed pores in the metal of the article are oblate spheroids, where a / 2 < c < a, or prolate spheroids, where a < c < 2a. The morphology of the closed pores in the metal of the article can be determined as previously described for the closed pores in the metal of the precursor, with necessary modifications. For example, by using CT, the change in the morphology of the closed pores in the metal as a result of HIP can be examined. In one example, the sphericity Ψ a of the closed pores in the metal of the article is within 50%, preferably within 20%, more preferably within 10% of the sphericity Ψ p of the closed pores in the metal of the precursor. Generally, the sphericity Ψ of a closed pore having a volume V and a surface area A can be defined by the following formula:
[0079]
Number
[0080] In one example, the sphericity Ψ of the closed pores in the metal of the article a is at least 0.9, preferably at least 0.95, more preferably at least 0.975, and most preferably at least 0.99.
[0081] [Heating and Pressurization] In one example, adjusting the set of temperature, the set of pressure, and / or the set of duration comprises, for example, pressurizing to the Nth pressure in the set of pressure (e.g., at least 90%) without heating substantially, and then heating to the Nth temperature in the set of temperature by heating to the Nth temperature in the set of temperature, and / or adjusting pressurizing to the Nth pressure in the set of pressure. In this way, the precursor particles are isotropically compressed from the start of HIP before significant heating, so that, for example, sintering or diffusion bonding is relatively little or none.
[0082] In one example, isostatically pressing the precursor comprises pressurizing the precursor from a zero pressure of the set of pressures, e.g., ambient pressure, to a first pressure of the set of pressures for a first duration of the set of durations, i.e., the precursor is first pressed, e.g., isostatically pressed, to the first pressure for the first duration.
[0083] In one example, the ratio of the first pressure to the Nth pressure is in the range of 1:5 to 1:1, preferably in the range of 1:4 to 19:20, more preferably in the range of 1:2 to 9:10, and most preferably in the range of 2:3 to 17:20, for example, 3:4, i.e., the first pressure is relatively high compared to the HIP pressure (i.e., the Nth pressure).
[0084] In one example, pressing the precursor from the zeroth pressure of the set of pressures to the first pressure of the set of pressures during the first duration of the set of durations comprises substantially isothermal pressing the precursor from the zeroth pressure of the set of pressures to the first pressure of the set of pressures during the first duration of the set of durations, e.g., at a first temperature of the set of temperatures, e.g., ambient temperature, without applying heating or cooling, and / or such that the temperature is constant within 5%. That is, the temperature is maintained during the initial pressing, e.g., maintained at about ambient temperature (i.e., the first temperature). This may be referred to as cold pressing at a relatively high pressure, e.g., as described above. In this manner, the particles of the precursor are isostatically pressed from the start of HIPing, prior to significant heating, so that, e.g., there is relatively little or no sintering or diffusion bonding. More generally, it should be noted that cold pressing may occur without applying external heating, i.e., without supplying heat to the precursor or gas, and the temperature of the precursor and / or gas may increase as a result of pressing. In contrast, cold pressing in conventional HIPing is typically at a relatively low pressure.
[0085] In one example, adjusting the set of temperatures, the set of pressures, and / or the set of durations comprises pressurizing the precursor from a first pressure in the set of pressures to an Nth pressure in the set of pressures for a second duration in the set of durations by heating the precursor to a second temperature in the set of temperatures, i.e., increasing the pressure from the first pressure to the Nth pressure may be achieved by heating the precursor (and thus the gas) to the second temperature.
[0086] In one example, adjusting the set of temperatures, the set of pressures, and / or the set of durations comprises, for example, heating the precursor from a second temperature in the set of temperatures to an Nth temperature in the set of temperatures at an Nth pressure in the set of pressures, i.e., the precursor may be heated to a HIP temperature, and the precursor is HIPed at the Nth temperature in the set of temperatures, at the Nth pressure in the set of pressures, and for the Nth duration in the set of durations.
[0087] [Cooling and decompression] In one example, the method comprises isothermally depressurizing the article from an Nth pressure to ambient pressure, and then cooling the depressurized article from an Nth temperature to ambient temperature.
[0088] In one example, adjusting the set of temperatures, the set of pressures, and / or the set of durations comprises adjusting the cooling from the Nth temperature of the set of temperatures and / or adjusting the decompression from the Nth pressure of the set of pressures, for example, by substantially isothermal decompression from the Nth pressure of the set of pressures, for example, to ambient pressure (e.g., so that the temperature is constant within 5%), and then cooling from the Nth temperature of the set of temperatures, for example, toward ambient temperature. That is, the precursor is decompressed while relatively hot, and then cooled at a relatively low pressure. In this way, spheroidization of closed pores is promoted, since the precursor is maintained at a relatively high temperature during decompression.
[0089] In one example, adjusting the set of temperatures, the set of pressures, and / or the set of durations comprises cooling the precursor from an Nth temperature of the set of temperatures to an N+1th temperature of the set of temperatures, optionally the N+1th temperature of the set of temperatures being at least 80%, preferably at least 85%, more preferably at least 90%, most preferably at least 90% of the Nth temperature, e.g., at least 97.5% of the Nth temperature, during the N+1th duration of the set of durations, i.e., the precursor may be initially cooled, but the temperature remains relatively high compared to the Nth temperature.
[0090] In one example, cooling the precursor from an Nth temperature in the set of temperatures to an N+1th temperature in the set of temperatures comprises isobarically cooling the precursor from an Nth temperature in the set of temperatures to an N+1th temperature in the set of temperatures, i.e., the initial cooling does not involve, for example, the application or release of pressure.
[0091] In one example, adjusting the set of temperatures, the set of pressures, and / or the set of durations comprises depressurizing the precursor to an N+2th pressure of the set of pressures for an N+2th duration of the set of durations at a first depressurization rate of the set of depressurization rates, depressurizing the precursor to an N+3th pressure of the set of pressures for an N+3th duration of the set of durations at a second depressurization rate of the set of depressurization rates, and optionally depressurizing the precursor to an N+4th pressure of the set of pressures for an N+4th duration of the set of durations at a third depressurization rate of the set of depressurization rates, the first depressurization rate being slower than the second depressurization rate, and optionally the second depressurization rate being slower than the third depressurization rate, and optionally depressurizing the precursor comprises substantially isothermally depressurizing the precursor at, for example, the Nth temperature of the set of temperatures or the N+1th temperature of said temperatures, for example, without applying heating or cooling and / or such that the temperature is constant within 5%. That is, the precursor is depressurized at a relatively lower initial rate and then at a relatively higher rate. Additionally and / or alternatively, in one example, the first depressurization rate, the second depressurization rate, and optionally the third depressurization rate are substantially equal or equal. Additionally and / or alternatively, in one example, the first depressurization rate is faster than the second depressurization rate, and optionally the second depressurization rate is faster than the third depressurization rate.
[0092] Maintaining the precursor at a relatively high temperature during depressurization promotes spheroidization of closed pores that may expand during depressurization. It should be understood that depressurization may comprise continuous depressurization, gradual depressurization at a predetermined rate, e.g., as defined by a flow controller, and / or stepwise depressurization, e.g., depressurization by partial release, hold for a predetermined duration, and repeat. In general, inserting periodic holds at a constant applied pressure may provide an opportunity for the system to reach or approach some equilibrium. In this way, the closed pores may expand to or toward equilibrium expansion as the applied pressure is reduced. If the depressurization rate is too fast, the closed pores may tear and form cracks. However, because the pressure in the closed pores decreases as they expand, the driving force to expand decreases so that there is some self-correction. Nevertheless, a dwell at a constant pressure may be an opportunity to allow the process to reach some equilibrium before another pressure reduction ramp. Thus, in one example, pressurizing the precursor to a pressure of the set of pressures comprises holding the precursor at that pressure for a duration of the set of durations, e.g., the duration is in the range of 0.05 hours to 1 hour, preferably in the range of 0.1 hours to 0.5 hours. Additionally and / or alternatively, depressurization may be continuous or gradual at a relatively slow rate during which such equilibration may occur.
[0093] In one example, adjusting the set of temperatures, the set of pressures, and / or the set of durations comprises cooling the precursor to an N+5th temperature of the set of temperatures during an N+5th duration of the set of durations at a first cooling rate of the set of cooling rates, and cooling the precursor to an N+6th temperature of the set of temperatures during an N+6th duration of the set of durations at a second cooling rate of the set of cooling rates, the first cooling rate being slower than the second cooling rate, and optionally cooling the precursor comprises isobarically cooling the precursor, for example, at ambient pressure. That is, the precursor is cooled at a relatively lower initial rate and then cooled at a relatively higher rate. In this manner, spheroidization of closed pores during cooling is promoted.
[0094] [Device] A second aspect provides a hot isostatic pressing (HIP) apparatus for at least partially fabricating an article from a precursor thereof, the apparatus comprising: The method is configured to HIP a precursor comprising a metal having closed pores therein at an Nth temperature of the set of temperatures, at an Nth pressure of the set of pressures, and for an Nth duration of the set of durations by adjusting the set of temperatures, the set of pressures, and / or the set of durations to at least partially control the morphology of the closed pores, thereby at least partially producing the article.
[0095] The HIP, article, precursor, metal, closed pores, Nth temperature, set of temperatures, Nth pressure, set of pressures, duration, set of durations, creating, adjusting, controlling, and / or closed pore morphology may be as described with respect to the first embodiment.
[0096] [Goods] A third aspect provides an article formed according to the method of the first aspect and / or the apparatus of the second aspect.
[0097] In one example, the article comprises and / or is an aerospace component, such as an airframe component, a vehicle component, such as an engine component, or a medical component, such as an implantable medical device.
[0098] Computer, computer program, and non-transitory computer-readable storage medium A fourth aspect provides a computer comprising a processor and a memory configured to at least partly carry out a method according to the first aspect.
[0099] A fifth aspect provides a computer program comprising instructions which, when executed by a computer comprising a processor and a memory, cause the computer to perform, at least in part, a method according to the first aspect.
[0100] A sixth aspect provides a non-transitory computer-readable storage medium comprising instructions that, when executed by a computer comprising a processor and a memory, cause the computer to perform, at least in part, a method according to the first aspect.
[0101] [Definition] Throughout this specification, the term "comprising" or "comprises" means including the specified component(s) but not excluding the presence of other components. The term "consisting essentially of" or "consists essentially of" means including the specified components but excluding other components, with the exception of materials present as impurities, unavoidable materials present as a result of the process used to provide the components, and components added for purposes other than achieving the technical effect of the invention, such as colorants. The term "consisting of" or "consists of" means including the specified components but excluding other components. Whenever appropriate, depending on the context, use of the term "comprises" or "comprising" may also be interpreted to include the meaning of "consist essentially of" or "consisting essentially of" and may also be interpreted to include the meaning of "consist of" or "consisting of".
[0102] The optional features described herein may, where appropriate, be used either individually or in combination with one another, particularly in such combinations as are described in the appended claims. Optional features for each aspect or exemplary embodiment of the invention as described herein are also applicable, where appropriate, to all other aspects or exemplary embodiments of the invention. In other words, a person skilled in the art reading this specification should consider the optional features for each aspect or exemplary embodiment of the invention as interchangeable and combinable between different aspects and exemplary embodiments.
[0103] For a better understanding of the present invention, and to show how illustrative embodiments thereof may be carried into effect, reference will be made, by way of example only, to the accompanying drawings, in which: [Brief description of the drawings]
[0104] [Figure 1] 1 illustrates a schematic diagram of isotropic HIP of a precursor comprising a metal having closed pores therein. [Diagram 2] 1 illustrates a schematic diagram of anisotropic HIP of a precursor comprising a metal having closed pores therein. [Diagram 3] 1 illustrates a schematic of uniaxial HIP of a precursor comprising a metal having closed pores therein. [Figure 4] 1 illustrates a schematic diagram of a method according to an illustrative embodiment; [Diagram 5] 1 illustrates a schematic diagram of a method according to an illustrative embodiment; [Figure 6] 1 illustrates a schematic diagram of a conventional method. [Figure 7] 1 illustrates a schematic diagram of a method according to an illustrative embodiment and a conventional method; [Figure 8] 1 illustrates a schematic diagram of a method according to an illustrative embodiment; [Figure 9] 9 illustrates generally the method of FIG. 8 in more detail; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0105] Figure 1 illustrates a schematic of isotropic HIP of a precursor P comprising a metal M having closed pores p therein. In particular, Figure 1 illustrates a schematic of isotropic collapse of a spherical bubble (i.e., closed pore p) from a diameter of 0.05 mm to 0.005 mm.
[0106] First, the spherical bubbles (i.e., closed pores) may simply be compressed in a perfectly symmetrical manner (as illustrated diagrammatically by the radial arrows of equal length, showing the compression of the closed pores p by the isostatic HIP pressure applied to the precursor P) into bubbles of much smaller diameter but still spherical in shape. Typically, a very large EIGA bubble of about 0.05 mm diameter, completely contained inside the largest EIGA particle in a given PSD (i.e., a granule with a diameter of 0.106 mm) subjected to HIP at 920° C. and 100 MPa pressure, is expected to be compressed such that the internal pressure approaches the externally applied HIP pressure, with the expectation being that such a bubble would reduce in diameter by about an order of magnitude (i.e., from D=0.05 mm at A to D=0.005 mm at B). Some expansion may occur upon removal of the HIP pressure, especially if the pressure is removed while still at very high temperatures. However, bubble collapse during HIP also results in diffusion bonding of the surrounding surfaces in a closed geometry, so any such expansion is expected to be relatively minor. This type of bubble compression with only limited or negligible post-HIP expansion is viewed as the most favorable outcome.
[0107] Second, Figure 2 illustrates diagrammatically the anisotropic HIP of a precursor P comprising a metal M having closed pores p therein (the longer arrows illustrating the preferential collapse direction). In particular, Figure 2 illustrates diagrammatically the partial isotropic collapse of an ellipsoidal bubble from a diameter of 0.05 mm (A) to a spherical bubble (i.e., pressure is not applied uniformly in all directions) (B) (as diagrammatically illustrated by radial arrows of unequal length indicating directional compression of the closed pores p by the anisotropic HIP pressure applied to the precursor P).
[0108] Thus, a spherical bubble may be partially asymmetrically compressed into a squashed sphere with an ellipsoid shape. This behavior is likely to occur when pressure transmission through the surrounding grains is not completely uniform. The degree of asymmetric collapse could potentially result in a highly exaggerated ellipsoid shape. This is of some concern because the internal gas pressure inside the ellipsoid after removal of the external HIP pressure will generate a higher stress concentration than would be the case for a purely spherical bubble. In an extremely squashed ellipsoid, it is possible that the combination of internal pressure and geometric stress concentration could cause the material to tear or split open, resulting in significant crack formation at the squashed radius.
[0109] Third, Figure 3 illustrates a more extreme case of anisotropic bubble compression by uniaxial pressure occurring during the "HIP process" of a precursor P comprising a metal M having closed pores p therein. In particular, Figure 3 illustrates the uniaxial collapse of a spherical bubble from a diameter of 0.05 mm (A) (as illustrated diagrammatically by the isometric parallel arrows showing the uniaxial compression of closed pores p by the uniaxial HIP pressure applied to the precursor P) into a donut-shaped toroidal double bubble (B through C) with a central diffusion bonding zone.
[0110] Therefore, if the transmission of HIP pressure were completely or nearly completely uniaxial, the bubbles could be crushed into quasi-two-dimensional platelets with opposing inner surfaces in close proximity. The HIP pressures involved would likely result in the very center regions contacting and diffusion bonding to each other, thus resulting in an annular shape. This is believed to be a most undesirable outcome, and one that would be expected to be actually detrimental to the integrity of the material.
[0111] The first approach is to "encourage" all particles to be isostatically pressed from the start (i.e., before any significant heating), thus limiting the opportunity for all surfaces to be in intimate contact and for sintering to begin when there is a significant temperature increase, ensuring an uninterrupted pressure path throughout the powder system.
[0112] Therefore, the method according to the first embodiment may work better by applying a very high level of "cold pressure" before heating begins, rather than the standard approach used in HIP, which is to pre-fill the pressure vessel with argon only to a relatively low initial gas pressure, and then use a temperature rise to achieve most of the required pressure increase. The latter approach is generally used in the HIP industry, where the initial cold pressure is capped and will not exceed 25% of the final target pressure. In the case of titanium powder HIP, the final target pressure is at least 100 MPa, so the initial pressure used is no more than 25 MPa. This pressure cap ensures that argon gas is not wasted, since any cold pressure (i.e., ambient pressure) that exceeds 25% of the final target pressure will require subsequent release as the pressure increases during the heating stage. For example, according to the Universal Gas Equation, if the final target temperature and pressure are 920°C and 100MPa, any cold pressurization above a pressure of 24.56MPa (i.e., for example, 20°C) would be expected to either result in overpressure or the need to release gas to stay within the target pressure range. In contrast, the method according to the first embodiment may cold pressurize to about 75% of the target pressure (e.g., 75MPa) and then heat to 920°C, and it is expected that when the temperature reaches about 118°C, the pressure will approach the final target pressure of 100MPa and then release will be required for the remainder of the heating stage. In doing so, as the titanium begins to plastically deform and the intragranular bubbles begin to collapse, a uniform isostatic pressure is present throughout the powder system and asymmetric bubble collapse is not expected to occur at any significant level.
[0113] The second approach is to modify the way in which the pressure and temperature are reduced once the HIP dwell at maximum pressure and temperature is finished. In the prior art, it is standard to reduce the temperature and pressure simultaneously. When the pressure is released, the HIP argon gas will expand and the temperature will decrease. This will aid in cooling. In addition, a "gas quench" (i.e., injecting cold gas) may also be applied to accelerate the cooling process. The proposed novel approach is to reduce the HIP pressure while maintaining the temperature at a high level to encourage re-spheroidization of any ellipsoidal bubbles that may be present. This may be done either substantially isothermally at the full HIP temperature (e.g., typically 920°C for titanium alloys) without applying, for example, heating or cooling, or alternatively, some level of pre-cooling to an intermediate temperature while remaining at full HIP pressure may be applied, after which the HIP pressure may then be reduced substantially isothermally (i.e., at the intermediate reduced temperature) without applying, for example, heating or cooling. The latter approach would provide increased flow stress for the titanium, providing some resilience to better withstand the subsequent positive pressure differential inside the entrapped argon bubbles once HIP depressurization has commenced, which would otherwise risk damage. In any case, the rate of HIP vessel depressurization should be controlled so that the initial rate of pressure decay is more limited and allowed to increase progressively according to a defined process. Only after the HIP vessel pressure has been substantially reduced would a full reduction in temperature be performed.
[0114] The rationale for the modified depressurization to a substantially reduced level (either at the full HIP temperature or at intermediate and partially reduced temperatures) followed by the main cooling stage is to allow spheroidization of any ellipsoidal gas bubbles that may have formed despite the use of a cold pressurization step. The controlled depressurization of the HIP vessel is therefore a preventative measure, but one that can also be used in the absence of a cold pressurization step (see below) to mitigate ellipsoidal gas bubble re-expansion that occurs in a damaging manner. Otherwise, without preventative gradual depressurization at high temperature, it would be of concern that any sudden reduction in the HIP pressure occurring during the cooling stage could result in a surprisingly high positive pressure difference between the inside of the gas bubble and the HIPed component. This could then create a tendency for the bubble to tear or split open, rather than the more desirable slow re-expansion and crack formation, or at least the preservation of non-spheroidized gas bubbles that could then act as sites of premature fatigue crack initiation in the component during service.
[0115] Figure 4 illustrates a schematic of a method according to an exemplary embodiment. In particular, Figure 4 shows the HIP temperature and pressure curves for the cycle of Table 3 ("cold fill" (75 MPa) to 75% of the final target pressure, and 40°C isobaric cooling prior to controlled (progressively increasing) rate depressurization). Note that the stabilization hold time of Table 3 can be extended to provide a safety margin and allow the gas bubbles to re-expand to optimal levels before the next depressurization stage begins.
[0116] [Table 3]
[0117] Table 3: HIP cycle using "cold fill" (75 MPa) to 75% of final target pressure, and isobaric cooling to 40°C prior to controlled (progressively increasing) rate depressurization (transient cooling at 75 MPa cold fill pressure and extended stabilization hold).
[0118] Figure 5 illustrates a schematic of a method according to an exemplary embodiment. In particular, Figure 5 shows the HIP temperature and pressure curves for the cycle of Table 4 (without "cold fill" to 75% of the final target pressure (75 MPa) and without isobaric cooling prior to controlled (progressively increasing) rate depressurization).
[0119] [Table 4]
[0120] Table 4: HIP cycle using a "cold fill" (75 MPa) to 75% of the final target pressure with no isobaric cooling prior to controlled (progressively increasing) rate of depressurization (isothermal cooling at 75 MPa cold fill pressure and extended stabilization hold).
[0121] A conventional method is illustrated diagrammatically in Figure 6. In particular, Figure 6 shows a conventional HIP cycle using a "cold fill" to 25% of the final target pressure (25 MPa) with simultaneous cooling and depressurization (see Table 5).
[0122] [Table 5]
[0123] Table 5: Conventional HIP cycle using "cold fill" to 25% of the final target pressure (25 MPa) with simultaneous cooling and depressurization (see Figure 6).
[0124] 7 is a schematic diagram illustrating a method according to an exemplary embodiment and a conventional method, in particular, FIG. 7 shows a comparison between the preferred embodiment and the conventional HIP cycle of FIG.
[0125] Note that the conventional HIP cycle is a shorter cycle (see FIG. 7). The preferred embodiment is the longest cycle as it also includes an isobaric cooling stage which adds approximately 44 minutes to the cycle without isobaric cooling and is 167 minutes longer than the conventional process described.
[0126] Applying conventional processes to powder HIP parts made from EIGA powders would potentially result in highly ellipsoidal and even toroidal gas bubbles, with the potential for cracking and / or splitting during the process, either during subsequent high temperature heat treatments or during service exposure. The enhanced process also has applicability to other processes that use HIP as a remedial treatment (e.g., for the elimination of internal porosity in additively manufactured parts). This includes both laser and electron beam selective powder bed processes. In the case of laser powder bed, argon gas entrapment can occur either through the use of a less than optimal set of laser build parameters, where the argon process gas used gets trapped in the porosity created by the inferior build process, or through argon entrapment already present in the powder stock. The latter is less likely, as SLM processes typically use powder grades between 15 and 45 microns and are generally not thought to suffer from the intragranular argon bubbles associated with the EIGA route. In contrast, electron beam powder bed processes typically use coarser powders and may well contain intragranular (i.e., within the precursor gas particles) argon gas entrapment. This form of gas entrapment is known to be capable of surviving the EB melting process despite the use of a vacuum environment.The present invention therefore has wider applicability than powder HIP alone.
[0127] FIG. 8 illustrates a method according to an illustrative embodiment.
[0128] The method comprises fabricating the article at least in part from a precursor thereof.
[0129] At S801, the method comprises providing a precursor, the precursor comprising a metal having closed pores therein.
[0130] In S802, the method comprises isostatically pressing a precursor, thereby providing a compressed precursor, and hot isostatically pressing (HIP) the compressed precursor at an Nth temperature of the set of temperatures, at an Nth pressure of the set of pressures, and for an Nth duration of the set of durations, thereby at least partially producing the article.
[0131] FIG. 9 illustrates generally the method of FIG. 8 in more detail, as summarized by Table 6.
[0132] [Table 6]
[0133] Table 6: HIP cycle using cold charging to 75% of the final target pressure and isobaric cooling prior to depressurization at a controlled (gradually increasing) rate.
[0134] In this example, adjusting the set of temperatures, the set of pressures, and / or the set of durations comprises adjusting the heating to an Nth temperature of the set of temperatures and / or adjusting the pressurizing to an Nth pressure of the set of pressures, for example, by pressurizing to substantially an Nth pressure of the set of pressures without heating and then heating to the Nth temperature of the set of temperatures.
[0135] In this example, adjusting the set of temperatures, the set of pressures, and / or the set of durations comprises pressurizing the precursor from a zeroth pressure in the set of pressures, e.g., ambient pressure, to a first pressure in the set of pressures for a first duration in the set of durations.
[0136] In this example, the ratio of the first pressure to the Nth pressure is 3:4.
[0137] In this example, pressurizing the precursor from the zeroth pressure of the set of pressures to the first pressure of the set of pressures during the first duration of the set of durations comprises substantially isothermal pressurizing the precursor from the zeroth pressure of the set of pressures to the first pressure of the set of pressures during the first duration of the set of durations, e.g., without applying heating or cooling, e.g., at a first temperature of the set of temperatures, e.g., ambient temperature.
[0138] In this example, adjusting the set of temperatures, the set of pressures, and / or the set of durations comprises pressurizing the precursor from a first pressure in the set of pressures to an Nth pressure in the set of pressures for a second duration in the set of durations by heating the precursor to a second temperature in the set of temperatures.
[0139] In this example, adjusting the set of temperatures, the set of pressures, and / or the set of durations comprises, for example, heating the precursor from a second temperature in the set of temperatures to an Nth temperature in the set of temperatures at an Nth pressure in the set of pressures.
[0140] In this example, adjusting the set of temperatures, the set of pressures, and / or the set of durations comprises adjusting the cooling from the Nth temperature of the set of temperatures and / or adjusting the decompression from the Nth pressure of the set of pressures, e.g., by substantially isothermal depressurization from the Nth pressure of the set of pressures, e.g., to ambient pressure, and then cooling from the Nth temperature of the set of temperatures, e.g., toward ambient temperature.
[0141] In this example, adjusting the set of temperatures, the set of pressures, and / or the set of durations comprises cooling the precursor from an Nth temperature of the set of temperatures to an N+1th temperature of the set of temperatures, optionally the N+1th temperature of the set of temperatures is at least 80%, preferably at least 85%, more preferably at least 90% of the Nth temperature during the N+1th duration of the set of durations.
[0142] In this example, cooling the precursor from an Nth temperature in the set of temperatures to an N+1th temperature in the set of temperatures comprises isobarically cooling the precursor from an Nth temperature in the set of temperatures to an N+1th temperature in the set of temperatures.
[0143] In this example, adjusting the set of temperatures, the set of pressures, and / or the set of durations comprises depressurizing the precursor to an N+2th pressure of the set of pressures for an N+2th duration of the set of durations at a first depressurization rate of the set of depressurization rates, depressurizing the precursor to an N+3th pressure of the set of pressures for an N+3th duration of the set of durations at a second depressurization rate of the set of depressurization rates, and optionally depressurizing the precursor to an N+4th pressure of the set of pressures for an N+4th duration of the set of durations at a third depressurization rate of the set of depressurization rates, wherein the first depressurization rate is slower than the second depressurization rate, and optionally the second depressurization rate is slower than the third depressurization rate, and optionally depressurizing the precursor comprises substantially isothermal depressurization of the precursor at, for example, the Nth temperature of the set of temperatures or the N+1th temperature of said temperatures, e.g., without applying heating or cooling.
[0144] In this example, adjusting the set of temperatures, the set of pressures, and / or the set of durations comprises cooling the precursor to an N+5th temperature of the set of temperatures for an N+5th duration of the set of durations at a first cooling rate of the set of cooling rates and cooling the precursor to an N+6th temperature of the set of temperatures for an N+6th duration of the set of durations at a second cooling rate of the set of cooling rates, where the first cooling rate is slower than the second cooling rate, and optionally cooling the precursor comprises isobarically cooling the precursor, for example at ambient pressure.
[0145] While preferred embodiments have been shown and described, it will be recognized by those skilled in the art that various changes and modifications can be made therein without departing from the scope of the invention as defined in the appended claims and described above.
[0146] Attention is directed to all documents and documents in connection with this application that are filed contemporaneously with or prior to this application and that are open to public inspection herewith, and the contents of all such documents and documents are incorporated herein by reference.
[0147] All of the features disclosed in this specification (including any accompanying claims and drawings), and / or all of the steps of any method or process so disclosed, may be combined in any combination, except combinations in which at most some of such features and / or steps are mutually exclusive.
[0148] Each feature disclosed in this specification (including any accompanying claims and drawings), unless expressly stated otherwise, may be replaced by alternative features serving the same, equivalent or similar purpose, and thus, unless expressly stated otherwise, each feature disclosed is only an example of a generic series of equivalent or similar features.
[0149] The invention is not limited to the details of the embodiment(s) described above.The invention extends to any novel one or any novel combination of the features disclosed in this specification (including any accompanying claims and drawings), or to any novel one or any novel combination of the steps of any method or process so disclosed. The following is a summary of the claims as originally filed: [1] A method for making an article from a precursor thereof, the method comprising: providing said precursor comprising enclosing a powder of an α+β Ti alloy in a container, wherein said powder is formed by electrode-induced gas atomization (EIGA); cold pressing the precursor by isostatically pressing the precursor at a first pressure, thereby providing a pressed precursor; hot isostatically pressing (HIP) the compressed precursor at an Nth pressure in the range of 75 MPa to 150 MPa and at an Nth temperature in the range of 850° C. to 950° C., thereby producing the article. wherein a ratio of the first pressure to the Nth pressure is in the range of 1:2 to 9:10. [2] The method according to [1], wherein a ratio of the first pressure to the Nth pressure is in the range of 2:3 to 17:20. [3] The method of [1] or [2], wherein cold pressing of the precursor by isostatically pressing the precursor at the first pressure does not involve the application of heat or cooling. [4] The method according to any one of [1] to [3], wherein the powder particles contain bubbles containing argon. [5] The method according to [4], wherein the particles of the powder have a dimension of at least 50 μm. [6] The method according to any one of [1] to [5], comprising isothermally depressurizing the article from the Nth pressure to ambient pressure, and then cooling the depressurized article from the Nth temperature to ambient temperature. [7] The method of [6], wherein isothermal depressurizing the article from the Nth pressure to ambient pressure comprises isothermal depressurizing the article from the Nth pressure to ambient pressure. [8] The method of [6] or [7], wherein cooling the reduced pressure article from the Nth temperature toward ambient temperature comprises cooling at a first cooling rate and then cooling at a second cooling rate, the first cooling rate being slower than the second cooling rate. [9] The method according to any one of [6] to [8], wherein cooling the precursor comprises isobarically cooling the precursor.
[10] The method of [9], wherein isobaric cooling of the precursor is carried out at ambient pressure.
[11] The method according to any one of [6] to
[10] , wherein cooling the reduced pressure article from the Nth temperature towards ambient temperature comprises isobarically cooling the precursor from the Nth temperature to an N+1th temperature, wherein the N+1th temperature is at least 80% of the Nth temperature.
[12] The method according to any one of [1] to
[11] , wherein the cold pressing of the precursor is carried out at ambient temperature.
[13] The method according to any one of [1] to
[12] , wherein the α+β Ti alloy is a Ti-6Al-4V alloy.
[14] The method according to any one of [1] to
[13] , wherein the Nth pressure is in the range of 90 MPa to 125 MPa, and the Nth temperature is in the range of 875°C to 925°C.
[15] The method according to any one of [1] to
[14] , wherein the article is an aerospace component, a vehicle component, or a medical component.
Claims
1. 1. A method of making an article from a precursor thereof, the method comprising: providing said precursor comprising enclosing a powder of α+β Ti alloy in a container, wherein said powder is formed by electrode induced gas atomization (EIGA); cold pressing the precursor by isostatically pressing the precursor at a first pressure, thereby providing a pressed precursor; hot isostatically pressing (HIP) the compressed precursor at an Nth pressure in the range of 75 MPa to 150 MPa and at an Nth temperature in the range of 850° C. to 950° C., thereby producing the article. wherein a ratio of the first pressure to the Nth pressure is in the range of 1:2 to 9:
10.
2. The method of claim 1 , wherein a ratio of the first pressure to the Nth pressure ranges from 2:3 to 17:
20.
3. 3. The method of claim 1 or 2, wherein cold pressing of the precursor by isostatically pressing the precursor at the first pressure does not involve the application of heat or cooling.
4. The method according to any one of claims 1 to 3, wherein the particles of the powder contain bubbles filled with argon.
5. The method of claim 4 , wherein the particles of the powder have a size of at least 50 μm.
6. 6. The method of any one of claims 1 to 5, comprising isothermally depressurizing the article from the Nth pressure to ambient pressure, and thereafter cooling the depressurized article from the Nth temperature to ambient temperature.
7. The method of claim 6 , wherein isothermal depressurizing the article from the Nth pressure to ambient pressure comprises isothermal depressurizing the article from the Nth pressure to ambient pressure.
8. 8. The method of claim 6 or 7, wherein cooling the reduced pressure article from the Nth temperature towards ambient temperature comprises cooling at a first cooling rate followed by cooling at a second cooling rate, the first cooling rate being slower than the second cooling rate.
9. The method of any one of claims 6 to 8, wherein cooling the precursor comprises isobarically cooling the precursor.
10. 10. The method of claim 9, wherein the isobaric cooling of the precursor is performed at ambient pressure.
11. 11. The method of any one of claims 6 to 10, wherein cooling the reduced pressure article from the Nth temperature towards ambient temperature comprises isobarically cooling the precursor from the Nth temperature to an N+1th temperature, wherein the N+1th temperature is at least 80% of the Nth temperature.
12. The method according to any one of claims 1 to 11, wherein the cold pressing of the precursor is carried out at ambient temperature.
13. The method according to any one of claims 1 to 12, wherein the α+β Ti alloy is a Ti-6Al-4V alloy.
14. The method according to any one of claims 1 to 13, wherein the Nth pressure is in the range of 90 MPa to 125 MPa and / or the Nth temperature is in the range of 875°C to 925°C.
15. The method of any one of claims 1 to 14, wherein the article is an aerospace component, a vehicle component, or a medical component.
Citation Information
Patent Citations
Hot isostatic pressing consolidation of powder derived parts
WO2020030906A1