Non-aqueous electrolyte secondary battery

JP7652759B2Active Publication Date: 2025-03-27SANYO ELECTRIC CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2022509364
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-03-26
Filing Date
2021-02-08
Publication Date
2025-03-27
Estimated Expiration
2041-02-08

Smart Images

  • Figure 0007652759000002
    Figure 0007652759000002
  • Figure 0007652759000003
    Figure 0007652759000003
  • Figure 0007652759000004
    Figure 0007652759000004
Patent Text Reader

Abstract

A non-aqueous electrolyte secondary battery that comprises an electrode body that includes a positive electrode plate and a negative electrode plate, a square packaging body that has an opening and houses the electrode body, a sealing plate that seals the opening, and an electrode terminal that is provided to the sealing plate. The positive electrode plate comprises a positive electrode core body and a positive electrode active material that is applied to both surfaces of the positive electrode core body. The circumference per unit capacity of the battery of the portion of the positive electrode core body to which the positive electrode active material is applied is no more than 0.28 m / Ah.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a non-aqueous electrolyte secondary battery. [Background technology]

[0002] A non-aqueous electrolyte secondary battery such as a lithium ion battery has a structure in which an electrode assembly is housed in an exterior body having an opening, and the opening is sealed with a sealing plate. The electrode assembly has a structure in which a positive electrode and a negative electrode are stacked with a separator interposed therebetween.

[0003] In recent years, the demand for lithium-ion batteries for vehicles has been increasing. Lithium-ion batteries for vehicles, especially those for EVs, are required to have various characteristics such as large capacity, compatibility with rapid charging, high capacity recovery rate, and high level of safety. For example, if a lithium-ion battery is stored for a certain period of time without being operated after being charged, the battery capacity will decrease, so it is necessary to improve the characteristics to prevent this capacity decrease. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2019-160587 A [Patent Document 2] JP 2012-43752 A Summary of the Invention

[0005] To address the decline in battery capacity caused by long-term storage, various measures have been implemented from a materials perspective, but as lithium-ion batteries for EVs become more powerful, there is a demand for further improvements in their characteristics.

[0006] The nonaqueous electrolyte secondary battery of the present disclosure is a nonaqueous electrolyte secondary battery comprising an electrode assembly including a positive electrode plate and a negative electrode plate, a rectangular exterior body having an opening and housing the electrode assembly, a sealing plate sealing the opening, and an electrode terminal provided on the sealing plate, the positive electrode plate comprises a positive electrode core and a positive electrode active material applied to at least one surface of the positive electrode core, and the perimeter of the applied portion of the positive electrode active material on the positive electrode core is 0.28 m / Ah or less per unit capacity of the battery. It is even more preferable that the perimeter of the applied portion of the positive electrode active material on the positive electrode core is 0.11 m / Ah or less per unit capacity of the battery.

[0007] When the positive electrode active material is applied to both sides of the positive electrode core, the circumferential length of the portion on the positive electrode core where the positive electrode active material is applied means the sum of the circumferential lengths of both sides.

[0008] The electrode body may have a shape in which the positive electrode plate and the negative electrode plate are wound facing each other.

[0009] The negative electrode plate includes a negative electrode core and a negative electrode active material applied to the negative electrode core, and in the electrode body, the positive electrode plate and the negative electrode plate are stacked with a separator interposed between them, and an area of ​​a portion of the coating portion of the negative electrode active material in the negative electrode plate that faces the coating portion of the positive electrode active material may be 85% or more and 95% or less of a total area of ​​the coating portion of the negative electrode active material.

[0010] The battery may include one or more electrode bodies, and each electrode body may have a capacity of 30 Ah or more.

[0011] The battery capacity per unit area of ​​the applied portion of the positive electrode active material on the positive electrode core is 40 Ah / m 2 The area of ​​the positive electrode active material applied on the positive electrode core means the total applied area of ​​both sides when the positive electrode active material is applied to both sides of the positive electrode core.

[0012] The battery comprises a first current collector arranged between the electrode body and the sealing plate and connected to the electrode terminal, a second current collector arranged between the electrode body and a side wall of the rectangular exterior body and connected to the first current collector, and a tab group extending from the electrode body toward the side wall and connected to the second current collector, wherein the second current collector is made of a flat plate having a surface parallel to the side wall, and the tab group has a positive electrode tab group bundling a plurality of positive electrode tabs extending from the positive electrode plate and a negative electrode tab group bundling a plurality of negative electrode tabs extending from the negative electrode plate, and is preferably bent parallel to the side wall at the connection side with the second current collector.

[0013] In the nonaqueous electrolyte secondary battery disclosed herein, the perimeter of the coating portion of the positive electrode active material is 0.28 m / Ah or less per unit capacity of the battery. This makes it possible to reduce the proportion of lithium ions present in the region of the negative electrode plate facing the positive electrode plate after charging that diffuse to the region not facing the positive electrode plate during storage, thereby making it possible to increase the recovery rate of the battery capacity. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 is a perspective view showing a nonaqueous electrolyte secondary battery according to an embodiment of the present disclosure. [Diagram 2] FIG. 2 is a cross-sectional view of the battery in FIG. [Diagram 3] FIG. 3 is a diagram showing a second current collector according to an embodiment of the present disclosure. [Figure 4] FIG. 4 is a plan view of a positive electrode plate according to an embodiment of the present disclosure. [Diagram 5] FIG. 5 is a plan view of a negative electrode plate according to an embodiment of the present disclosure. [Figure 6] FIG. 6 is a plan view of an electrode assembly according to an embodiment of the present disclosure. [Figure 7] FIG. 7 is a perspective view that typically illustrates a positive electrode plate and a negative electrode plate of a nonaqueous electrolyte secondary battery. [Figure 8] FIG. 8 is a perspective view that shows the state of the negative electrode plate immediately after charging (the positive electrode plate is not shown). [Figure 9] FIG. 9 is a perspective view showing the state of a negative electrode plate that has been left for a long period of time after charging without being discharged (the positive electrode plate is not shown). [Figure 10] FIG. 10 is a perspective view that shows a schematic state of the negative electrode plate immediately after discharging from the state shown in FIG. 9 (with the positive electrode plate not shown). [Figure 11] FIG. 11 is a perspective view that shows the state of the negative electrode plate that has been left as is from the state shown in FIG. 10, with the positive electrode plate not shown. [Figure 12] FIG. 12 is a view showing the vicinity of the connection portion between the second current collector and the tab group before the tab group is folded. [Figure 13] FIG. 13 is a view showing the vicinity of the connection portion between the second current collector and the tab group after the tab group is folded. [Figure 14] FIG. 14 is a perspective view showing an electrode assembly in which the tab group is connected to a second current collector before the tab group is folded. [Figure 15] FIG. 15 is a diagram showing an electrode assembly group including a plurality of electrode bodies. [Figure 16] FIG. 16 is a diagram showing a group of multiple electrode assemblies connected to each other by first and second current collectors, and a sealing plate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Hereinafter, the embodiments of the present disclosure will be described in detail with reference to the drawings. The following description of the preferred embodiments is merely illustrative in nature and is not intended to limit the present disclosure, its application or its uses. In the following drawings, for the sake of simplicity, components having substantially the same functions are designated by the same reference numerals.

[0016] <Overall battery configuration> Fig. 1 is a perspective view showing a nonaqueous electrolyte secondary battery according to the present disclosure. Fig. 2 is a cross-sectional view of the battery in Fig. 1 taken parallel to the paper surface. As shown in Figs. 1 and 2, a nonaqueous electrolyte secondary battery 20 includes a battery case 100 including a rectangular exterior body 1 having an opening and a bottomed rectangular cylinder shape, and a sealing plate 2 that seals the opening of the rectangular exterior body 1.

[0017] The rectangular exterior body 1 has a bottom 1a, a pair of first side walls 1b, 1c, and a pair of second side walls 1d, 1e. The pair of first side walls 1b, 1c are arranged facing each other. The pair of second side walls 1d, 1e are arranged facing each other. The pair of first side walls 1b, 1c are perpendicular to the longitudinal direction of the sealing plate 2, and the area of ​​the pair of first side walls 1b, 1c is smaller than the area of ​​the pair of second side walls 1d, 1e.

[0018] An electrode body 3 including a positive electrode plate 4 and a negative electrode plate 5 is housed in the rectangular exterior body 1 together with an electrolyte. In this embodiment, the electrode body 3 is a flat electrode body in which the positive electrode plate 4 and the negative electrode plate 5 are wound with a separator interposed therebetween. The winding axis of the electrode body 3 extends perpendicular to the first side walls 1b, 1c and parallel to the second side walls 1d, 1e. Note that the electrode body 3 is not limited to a wound electrode body, and may be, for example, a laminated electrode body in which a plurality of positive electrode plates 4 and negative electrode plates 5 are stacked with a separator interposed therebetween.

[0019] In FIG. 2, reference numeral 10 denotes an external insulating member disposed between the sealing plate 2 and the positive electrode terminal 8, and reference numeral 12 denotes an external insulating member disposed between the sealing plate 2 and the negative electrode terminal 9. Reference numeral 11 denotes an internal insulating member disposed between the sealing plate 2 and the first positive electrode current collector 61, and reference numeral 13 denotes an internal insulating member disposed between the sealing plate 2 and the first negative electrode current collector 71. Reference numeral 14 denotes a box-shaped or bag-shaped insulating sheet disposed inside the rectangular exterior body 1 and accommodating the electrode body 3. Reference numeral 15 denotes an electrolyte injection hole provided in the sealing plate 2. Reference numeral 16 denotes a sealing member that seals the electrolyte injection hole 15. Reference numeral 17 denotes a gas exhaust valve provided in the sealing plate 2.

[0020] In the nonaqueous electrolyte secondary battery 20, one side is a positive electrode side and the other side is a negative electrode side in the extension direction of the winding axis of the electrode body 3. Below, the positive electrode side will be mainly described, and a description of the negative electrode side may be omitted.

[0021] <Electrode body configuration> The positive electrode plate 4 is a long strip as shown in FIG. 4, and has a region where a positive electrode active material layer 4a is formed on both sides of a positive electrode core (for example, aluminum foil). A plurality of positive electrode tabs 4b extend in a convex shape from the positive electrode core at one end in the short side direction of the positive electrode plate 4. The surface of the positive electrode core at one end in the short side direction of the positive electrode plate 4 and in the vicinity thereof is covered with a protective layer 4c. That is, the protective layer 4c is provided with a constant width from one side (end) extending in the longitudinal direction of the positive electrode plate 4 to the longitudinal central axis direction of the positive electrode plate 4c. In addition, a protective layer is provided at the base portion of the positive electrode tab 4b. The protective layer 4c contains an insulator, and may be, for example, a resin insulating layer, or a layer containing ceramic, which is an inorganic oxide, and a resin binder. An example of the protective layer 4c is a layer containing alumina powder, a carbon material as a conductive material, and polyvinylidene fluoride as a binder. The protective layer 4c may not be provided.

[0022] 5, the negative electrode plate 5 is in the form of a long strip, and has a region in which a negative electrode active material layer 5a is formed on both sides of a negative electrode core (e.g., copper foil). A plurality of negative electrode tabs 5b extend in a convex shape from the negative electrode core at one end in the short side direction of the negative electrode plate 5.

[0023] As shown in Fig. 6, the positive electrode plate 4 and the negative electrode plate 5 are stacked with a separator between them, and then wound to form the electrode body 3. In the electrode body 3, the winding axis extends in the direction connecting the positive electrode tab group 40 and the negative electrode tab group 50 (the horizontal direction in Fig. 6), and of the end faces of the electrode body 3 perpendicular to the winding axis, the positive electrode tab group 40 is located on one end face, and the negative electrode tab group 50 is located on the other end face opposite thereto. This positional relationship makes it easy to prevent short circuits within the battery.

[0024] <Relationship between positive and negative plates> In general, in order to ensure safety and extend the life of a battery, the negative electrode active material is designed to have a larger capacity than the positive electrode active material. In a battery in which a positive electrode plate and a negative electrode plate are stacked facing each other, the battery is designed so that the area where the active material of the positive electrode plate is applied is within the area where the active material of the negative electrode plate is applied, and the area where the active material of the negative electrode is applied exceeds (protrudes from) the area where the active material of the positive electrode is applied.

[0025] 7 is a schematic diagram showing a positive electrode plate 44 and a negative electrode plate 55 of a nonaqueous electrolyte secondary battery. An active material is provided on the entire surface of both the positive electrode plate 44 and the negative electrode plate 55. The negative electrode plate 55 has a larger area than the positive electrode plate 44, and the surface of the positive electrode plate 44 facing the negative electrode plate 55 faces the surface of the negative electrode plate 55 entirely, and the negative electrode plate 55 has a non-facing region 57 that does not face the positive electrode plate 44.

[0026] 8 shows a schematic diagram of the state of negative electrode plate 55 immediately after charging (positive electrode plate 44 is not shown). Lithium ions 48 move from positive electrode plate 44 to negative electrode plate 55 due to charging. Since the diffusion speed of lithium ions 48 within negative electrode plate 55 is not very high, lithium ions 48 are present only in facing region 56 facing positive electrode plate 44 immediately after charging. Note that in FIG. 8, outer perimeter line 46 indicating the perimeter of positive electrode plate 44 is shown by a dashed line, and facing region 56 is the region surrounded by this outer perimeter line 46.

[0027] If the battery is left for a long time without being discharged after charging, as shown in Fig. 9 (positive electrode plate 44 is not shown), lithium ions 48 diffuse within negative electrode plate 55, and the probability of lithium ions 48 being present becomes the same in any part of negative electrode plate 55. That is, the distribution ratio of lithium ions 48 becomes the same in both facing region 56 and non-facing region 57.

[0028] FIG. 10 (the positive electrode plate 44 is not shown) shows the state of the negative electrode plate 55 after it has been left for a long time without discharging after charging and then fully discharged. All of the lithium ions 48 that were present in the facing region 56 move to the positive electrode plate 44 due to the discharge, and the lithium ions 48 are no longer present in the facing region 56. Meanwhile, the lithium ions 48 that were present in the non-facing region 57 cannot move to the positive electrode plate 44 during discharge due to the diffusion speed of the lithium ions 48, and therefore remain in the non-facing region 57. If the negative electrode plate 55 is left for a long time without being charged or discharged, some of the lithium ions 48 move (diffuse) from the non-facing region 57 into the facing region 56 as shown in FIG. 11 (the positive electrode plate 44 is not shown).

[0029] From the above explanation, it can be understood that if a battery is left to stand after charging and stored, the battery capacity will decrease compared to immediately after charging. In order to reduce the rate of decrease in battery capacity and increase the capacity recovery rate, it is necessary to reduce the length of the outer periphery 46 per unit capacity of the battery (more precisely, the periphery of the positive electrode active material application portion on the positive electrode core body in the positive electrode plate). That is, when moving from FIG. 8 to FIG. 9, if the outer periphery 46 per unit capacity of the battery is short, the number of lithium ions 48 that move to the non-facing region 57 decreases, and the capacity recovery rate increases.

[0030] Specifically, when the perimeter of the applied portion of the positive electrode active material on the positive electrode core is 0.28 m / Ah or less per unit capacity of the battery, the capacity recovery rate is practically sufficient for an EV battery. When the perimeter of the applied portion of the positive electrode active material on the positive electrode core is 0.11 m / Ah or less per unit capacity of the battery, a further improvement in the capacity recovery rate can be expected. In addition, in the negative electrode plate 55, the area ratio of the facing region / (facing region+non-facing region) is preferably 85% or more and 95% or less. More precisely, the area ratio of the facing region / (facing region+non-facing region) is the ratio of the area of ​​the applied portion of the negative electrode active material facing the applied portion of the positive electrode active material to the total area of ​​the applied portion of the negative electrode active material. In addition to the circumferential length of the application portion of the positive electrode active material per unit capacity of the present disclosure, by setting the area ratio of the facing area / (facing area+non-facing area) in the negative electrode plate 55 to 85% or more and 95% or less, the diffusion area of ​​lithium ions during long-term storage as shown in FIG. 9 can be suppressed, and the capacity recovery rate can be improved.

[0031] The capacity of each electrode body is preferably 30 Ah or more. The capacity of the battery per unit area of ​​the positive electrode active material coating on the positive electrode core is preferably 40 Ah / m 2 The improvement in capacity recovery rate, which is the object of the present disclosure, is particularly required for lithium-ion batteries for EVs, and furthermore, in these batteries, the above-mentioned configuration improves the energy density, leading to an extension of the EV driving distance.

[0032] Patent Document 1 discloses a battery with a capacity of 8.4 Ah, a width of the positive active material applied is 11.0 cm, and a positive plate length is 440 cm, and the perimeter of the positive active material applied portion per unit capacity is 1.07 m / Ah. Patent Document 2 discloses a battery with a capacity of 4.6 Ah, a width of the positive active material applied is 50 mm, and a positive plate length is 3000 mm, and the perimeter of the positive active material applied portion per unit capacity is 1.33 m / Ah.

[0033] <Structure of current collection from electrode body> The sealing plate 2 is provided with a positive electrode terminal 8 and a negative electrode terminal 9 as electrode terminals to the outside. The positive electrode terminal 8 is electrically connected to the positive electrode tab group 40 via a positive electrode current collector 6, which is composed of a first positive electrode current collector 61 and a second positive electrode current collector 62. The negative electrode terminal 9 is electrically connected to the negative electrode tab group 50 via a negative electrode current collector 7, which is composed of a first negative electrode current collector 71 and a second negative electrode current collector 72.

[0034] The first positive electrode current collector 61 has a generally L-shaped cross section and is disposed between the electrode body 3 and the sealing plate 2. Specifically, the first positive electrode current collector 61 has a first region disposed along the sealing plate 2 and a second region bent from an end of the first region. The second region extends along the first side wall 1b toward the bottom 1a. The first positive electrode current collector 61 is connected to the positive electrode terminal 8. The negative electrode side has a similar configuration.

[0035] The second positive electrode current collector 62 is disposed between the electrode body 3 and the first side wall 1b of the rectangular exterior body 1. Specifically, the second positive electrode current collector 62 is made of a flat plate having a surface parallel to the first side wall 1b, and extends along the first side wall 1b toward the bottom 1a. The second positive electrode current collector 62 is connected to the first positive electrode current collector 61. The negative electrode side has a similar configuration.

[0036] 3 shows the second positive electrode current collector 62. The second positive electrode current collector 62 has a structure in which a part of a substantially rectangular flat plate is bent, and has a current collector connection part 62a, an inclined part 62b, and a tab connection part 62c. The current collector connection part 62a is connected to the first positive electrode current collector 61. The tab connection part 62c is connected to the positive electrode tab group 40. The inclined part 62b connects the current collector connection part 62a and the tab connection part 62c, and is inclined with respect to both of them.

[0037] The current collector connection portion 62a is provided with a recess 62d. A through hole 62e is provided in the recess 62d. The current collector connection portion 62a is joined to the first positive electrode current collector 61 in the recess 62d. Furthermore, the second positive electrode current collector 62 is provided with a fuse portion 66.

[0038] Next, the bending of the positive electrode tab group 40 and the connection between the positive electrode tab group 40 and the second positive electrode current collector 62 will be described. Note that the negative electrode side has almost the same configuration and structure as the positive electrode side, so only the positive electrode side will be described below. Fig. 12 shows the vicinity of the connection between the second positive electrode current collector 62 and the positive electrode tab group 40 before the positive electrode tab group 40 is folded. Fig. 14 shows the electrode assembly 3 in which the positive electrode tab group 40 is connected to the second positive electrode current collector 62 and the negative electrode tab group 50 is connected to the second negative electrode current collector 72 before the positive electrode tab group 40 and the negative electrode tab group 50 are folded.

[0039] The positive electrode tab group 40 is connected to the tab connection portion 62c of the second positive electrode current collector 62. Specifically, as shown in Fig. 12, before bending the positive electrode tab group 40, in a state in which the positive electrode tab group 40 is disposed on the tab connection portion 62c of the second positive electrode current collector 62, the tab connection portion 62c and the positive electrode tab group 40 are joined (welded) to each other, thereby forming the connection portion 63.

[0040] 12, the positive electrode tab group 40 is connected to the tab connection portion 62c of the second positive electrode current collector 62, closer to one side in the width direction of the flat plate constituting the second positive electrode current collector 62 (the right side in FIG. 12). That is, the connection portion 63 between the positive electrode tab group 40 and the tab connection portion 62c is closer to the base side of the positive electrode tab group 40 in the width direction of the flat plate (one side in the width direction, the right side in FIG. 9). This makes it possible to more reliably form a curved shape near the base of the positive electrode tab group 40 when the positive electrode tab group 40 is bent.

[0041] 13 is a diagram showing the vicinity of the connection part between the second positive electrode current collector 62 and the positive electrode tab group 40 after the positive electrode tab group 40 is folded. The tab connection part 62c of the second positive electrode current collector 62, which was disposed substantially parallel to the first main surface 3a and the second main surface 3b of the electrode body 3 (see FIGS. 12 and 14), is oriented substantially perpendicular to the winding axis of the electrode body 3 by folding the positive electrode tab group 40. That is, the positive electrode tab group 40 is folded parallel to the first side wall 1b on the side of the connection part 63 with the second positive electrode current collector 62. The positive electrode tab group 40 in the folded state is fixed to the electrode body 3 by tape 80.

[0042] With such a configuration, the positive electrode tab group 40 can be folded without bending the second positive electrode current collector 62. This makes it possible to fabricate a nonaqueous electrolyte secondary battery with high volumetric energy density by a simple method.

[0043] As described above, the negative electrode side has the same configuration as the positive electrode side, and in FIG. 14, 72a is a current collector connection portion, 72b is an inclined portion, and 72c is a tab connection portion.

[0044] In the nonaqueous electrolyte secondary battery according to this embodiment, by folding the positive electrode tab group 40 and the negative electrode tab group 50, a battery with high volumetric energy density can be obtained without folding the second current collectors 62, 72, and one end 5e of the negative electrode plate 5 is positioned opposite the protective layer 4c of the positive electrode plate 4, thereby preventing a short circuit within the battery.

[0045] (Example) <Example 1> [Preparation of positive electrode plate] A lithium nickel cobalt manganese composite oxide as a positive electrode active material, polyvinylidene fluoride (PVdF) as a binder, a carbon material as a conductive material, and N-methyl-2-pyrrolidone (NMP) as a dispersion medium were mixed and kneaded so that the mass ratio of lithium nickel cobalt manganese composite oxide:PVdF:carbon material was 97.5:1:1.5, to prepare a positive electrode active material layer slurry.

[0046] Alumina powder, carbon material as a conductive material, polyvinylidene fluoride (PVdF) as a binder, and N-methyl-2-pyrrolidone (NMP) as a dispersion medium were mixed together so that the mass ratio of alumina powder:carbon material:PVdF was 83:3:14 to prepare a protective layer slurry.

[0047] The positive electrode active material layer slurry and the positive electrode protective layer slurry prepared by the above-mentioned method were applied to both sides of an aluminum foil as a positive electrode core by a die coater. At this time, the positive electrode active material layer slurry was applied to the center of the positive electrode core in the width direction. In addition, the positive electrode protective layer slurry was applied to the end of the region in the width direction where the positive electrode active material layer slurry was applied.

[0048] The positive electrode core coated with the positive electrode active material layer slurry and the positive electrode protective layer slurry was dried, and the NMP contained in the positive electrode active material layer slurry and the positive electrode protective layer slurry was removed. This resulted in the formation of a positive electrode active material layer and a positive electrode protective layer. The positive electrode active material layer was then compressed to form a positive electrode original plate. This positive electrode original plate was cut so that the active material layer coating portion was a rectangle with a width of 88 mm and a length of 4600 mm, to form a positive electrode plate. The cutting of the positive electrode plate could be performed by irradiation of energy rays such as a laser, a mold, or a cutter.

[0049] [Preparation of negative electrode plate] Graphite as the negative electrode active material, styrene butadiene rubber (SBR) and carboxymethyl cellulose (CMC) as binders, and water as a dispersion medium were kneaded together so that the mass ratio of graphite:SBR:CMC was 98:1:1 to prepare a negative electrode active material layer slurry.

[0050] The negative electrode active material layer slurry prepared by the above-mentioned method was applied to both sides of a copper foil serving as a negative electrode core by a die coater.

[0051] The negative electrode core coated with the negative electrode active material layer slurry is dried to remove water contained in the negative electrode active material layer slurry. This forms a negative electrode active material layer. The negative electrode active material layer is then compressed to form a negative electrode base plate. This negative electrode base plate is cut so that the active material layer coating portion has a width of 92 mm and a length of 4900 mm to form a negative electrode plate. The negative electrode base plate can be cut by irradiation of energy rays such as a laser, a mold, a cutter, or the like.

[0052] [Preparation of electrode body] The strip-shaped positive electrode plate and strip-shaped negative electrode plate prepared by the above-mentioned method are wound with a strip-shaped separator made of polyolefin interposed therebetween to prepare a flat wound electrode body. The electrode body has a flat region in the center and curved portions at both ends of the flat region.

[0053] A positive electrode tab group having multiple stacked positive electrode tabs is provided at one end in the direction in which the winding axis of the electrode body extends. A negative electrode tab group having multiple stacked negative electrode tabs is provided at the other end in the direction in which the winding axis of the electrode body extends. Note that the center of the positive electrode tab group and the center of the negative electrode tab group are shifted to one side from the winding axis in a direction perpendicular to the extension direction of the winding axis of the electrode body and in a direction perpendicular to the thickness direction of the electrode body.

[0054] [Battery construction] As shown in Fig. 14, a second positive electrode current collector 62 is joined to the positive electrode tab group 40, and a second positive electrode current collector 72 is joined to the negative electrode tab group 50. Furthermore, as shown in Figs. 15 and 16, two electrode bodies 3 in which the positive electrode tab group 40 and the negative electrode tab group 50 are folded are stacked and fixed with tape 90. Each positive electrode tab group 40 is arranged on the same side, and each negative electrode tab group 50 is arranged on the same side. In each electrode body 3, each positive electrode tab group 40 is folded in the same direction. In each electrode body 3, each negative electrode tab group 50 is folded in the same direction.

[0055] In the stacking direction of the electrode bodies 3, the second positive electrode current collectors 62 attached to each electrode body 3 are arranged at intervals and connected onto the second region 61b of the first positive electrode current collector 61. The same is true for each second negative electrode current collector 72.

[0056] These two electrode bodies 3 are inserted into the rectangular exterior body 1. Then, a sealing plate 2 is joined to the rectangular exterior body 1, and the opening of the rectangular exterior body 1 is sealed with the sealing plate 2. An electrolyte is injected through an electrolyte injection hole 15 provided in the sealing plate 2, and the electrolyte injection hole 15 is sealed with a sealing member 16. This completes the nonaqueous electrolyte secondary battery 20.

[0057] [Initial charge / discharge conditions] The non-aqueous electrolyte secondary battery thus fabricated was charged and discharged at 0.5 C, and adjusted to an SOC of 20% or less, to be ready for shipment.

[0058] [High temperature storage test conditions] The point when the shippable nonaqueous electrolyte secondary battery was charged to SOC 90% was set as storage day 0, and the battery was left in a 60°C environment for 56 days and 300 days, after which the discharge capacity was checked. The capacity recovery rate after storage was determined as the ratio of the discharge capacity before storage to 100%.

[0059] <Example 2> A battery was fabricated in the same manner as in Example 1, except that the active material layer-coated portion of the positive electrode plate in one electrode assembly was 262 mm wide and 2900 mm long, and the active material layer-coated portion of the negative electrode plate in one electrode assembly was 272 mm wide and 3100 mm long, and a high-temperature storage test was carried out. This was designated Example 2.

[0060] <Comparative Example> A battery was fabricated in the same manner as in Examples 1 and 2, except that in one electrode assembly, the active material layer-coated portion of the positive electrode plate was 76 mm wide and 4600 mm long, and the active material layer-coated portion of the negative electrode plate was 80 mm wide and 4900 mm long, and a high-temperature storage test was carried out. This was used as a comparative example.

[0061] Examples of the present disclosure will be described in detail below with reference to Table 1.

[0062] [Table 1]

[0063] Table 1 shows the perimeter of the positive electrode active material-coated portion per unit battery capacity, the ratio of the area of ​​the portion facing the positive electrode active material-coated portion to the total area of ​​the negative electrode active material-coated portion, the capacity per electrode body, the capacity per unit area of ​​the positive electrode active material-coated portion, and the capacity recovery rate after a high-temperature storage test for the nonaqueous electrolyte secondary batteries of Examples 1 and 2 and the Comparative Example.

[0064] It was found that if the perimeter of the positive electrode active material coating portion per unit capacity of the battery is 0.28 m / Ah or less, as in Example 1, a capacity recovery rate of 80% can be maintained even after 300 days of storage. It is considered that a capacity recovery rate of more than 80% even after 300 days of storage in a 60°C environment is suitable for an EV battery. Furthermore, if the perimeter of the positive electrode active material coating portion per unit capacity of the battery is 0.11 m / Ah or less, as in Example 2, the capacity recovery rate becomes 86% even after 300 days of storage, and storage resistance is further improved.

[0065] On the other hand, when the circumference of the positive electrode active material application area per unit battery capacity is greater than 0.28 m / Ah, as in the comparative example, the capacity recovery rate after 300 days of storage drops to 78%, which does not satisfy the performance level required for an EV battery.

[0066] (Other embodiments) The above-mentioned embodiments are merely examples of the present invention, and the present invention is not limited to these examples, and these examples may be combined with well-known, commonly used, or publicly known technologies, or may be partially replaced. In addition, modified inventions that can be easily conceived by a person skilled in the art are also included in the present invention.

[0067] The nonaqueous electrolyte secondary battery 20 may include a plurality of electrode bodies 3. In this case, the capacity of each electrode body is preferably 30 Ah or more. FIG. 15 is a diagram showing an electrode body group 300 including a plurality of electrode bodies 3. As shown in FIG. 15, the nonaqueous electrolyte secondary battery 20 includes a plurality of (two) electrode bodies 3. A second current collector 62 is connected to the positive electrode tab group 40 of each electrode body 3. The electrode body group 300 is formed by arranging a plurality of electrode bodies 3, 3 and fixing them together with a tape 90. FIG. 16 is a diagram showing the electrode body group 300 and the sealing plate 2 connected to each other by a first positive electrode current collector 61 and a second positive electrode current collector 62. [Explanation of symbols]

[0068] 1. Rectangular exterior body 1b 1st side wall (side wall) 1c 1st side wall (side wall) 2 Sealing plate 3 Electrode body 4 Positive plate 4b Positive electrode tab 5 Negative plate 5b Negative tab 8 Positive terminal (electrode terminal) 9 Negative terminal (electrode terminal) 20 Nonaqueous electrolyte secondary battery 40 Positive electrode tab group (tab group) 50 Negative electrode tab group (tab group) 61 First positive electrode collector (first collector) 62 Second positive electrode collector (second collector) 71 First negative electrode current collector (first current collector) 72 Second negative electrode current collector (second current collector)

Claims

1. an electrode assembly including a positive electrode plate and a negative electrode plate; A rectangular exterior body having an opening and housing the electrode body; a sealing plate that seals the opening; an electrode terminal provided on the sealing plate; A non-aqueous electrolyte lithium ion secondary battery comprising: The positive electrode plate includes a positive electrode core and a positive electrode active material applied to at least one surface of the positive electrode core, a circumferential length of the coating portion of the positive electrode active material on the positive electrode core per unit capacity of a battery is 0.28 m / Ah or less; The negative electrode plate includes a negative electrode core and a negative electrode active material applied to the negative electrode core, In the electrode assembly, the positive electrode plate and the negative electrode plate are stacked with a separator interposed therebetween, an area of ​​a portion of the coated portion of the negative electrode active material in the negative electrode plate that faces the coated portion of the positive electrode active material is 85% or more and 95% or less of a total area of ​​the coated portion of the negative electrode active material; The negative electrode active material is graphite, an active material application area of ​​the positive electrode plate is inside an active material application area of ​​the opposing negative electrode plate, A non-aqueous electrolyte lithium ion secondary battery comprising one or more of the electrode bodies, each of the electrode bodies having a capacity of 30 Ah or more.

2. 2. The nonaqueous electrolyte lithium ion secondary battery according to claim 1, wherein the circumferential length of the applied portion of the positive electrode active material on the positive electrode core per unit capacity of the battery is 0.11 m / Ah or less.

3. 3. The nonaqueous electrolyte lithium ion secondary battery according to claim 1, wherein the electrode assembly has a shape in which the positive electrode plate and the negative electrode plate are wound facing each other.

4. The battery capacity per unit area of ​​the applied portion of the positive electrode active material on the positive electrode core is 40 Ah / m 2 The nonaqueous electrolyte lithium ion secondary battery according to claim 1 .

5. a first current collector disposed between the electrode body and the sealing plate and connected to the electrode terminal; a second current collector disposed between the electrode body and a side wall of the rectangular exterior body and connected to the first current collector; a group of tabs extending from the electrode body toward the side wall and connected to the second current collector; Equipped with the second current collector is a flat plate having a surface parallel to the side wall, 5. The nonaqueous electrolyte lithium-ion secondary battery according to claim 1, wherein the tab group includes a positive electrode tab group formed by bundling a plurality of positive electrode tabs extending from the positive electrode plate and a negative electrode tab group formed by bundling a plurality of negative electrode tabs extending from the negative electrode plate, and is bent parallel to the side wall on a connection side with the second current collector.

Citation Information

Patent Citations

  • Battery

    JP1994349460A

  • Apparatus and method for measuring terahertz wave

    JP2009192524A

  • Cylindrical nickel-hydrogen storage battery

    JP2009211970A

  • Secondary battery and vehicle mounted with the same

    JP2012043752A

  • Separator for lithium ion battery, electrode-separator assembly for lithium ion battery and method for manufacturing the same, and lithium ion battery

    JP2014010970A