Manufacturing method of electronic modules

A liquid composition with conductive nanoparticles and a rheology control agent addresses the issues of high costs and inadequate coverage in conventional methods, enabling efficient and uniform conductive film formation on electronic components using inkjet printing.

JP7947728B2Active Publication Date: 2026-11-11RICOH CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2022044170
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-03-18
Publication Date
2026-11-11
Estimated Expiration
2042-03-18

AI Technical Summary

Technical Problem

Conventional methods for forming conductive films on electronic components face issues such as high costs, poor material utilization, and inadequate coverage of three-dimensional structures, with existing inks causing dripping and sagging due to viscosity gradients.

Method used

A liquid composition comprising conductive nanoparticles, a metal complex, and a rheology control agent, with specific viscosity ranges to ensure effective dispensing and film formation without dripping, using inkjet printing for precise application.

Benefits of technology

The composition enables the formation of uniform conductive films on complex surfaces with improved material efficiency and reduced costs, maintaining shape and preventing sagging, while ensuring high conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007947728000002
    Figure 0007947728000002
  • Figure 0007947728000003
    Figure 0007947728000003
  • Figure 0007947728000001
    Figure 0007947728000001
Patent Text Reader

Abstract

To provide a liquid composition that has excellent discharge properties and can form a good coating film without dripping when forming a conductive film on the side surface of an electronic component.SOLUTION: A liquid composition includes at least one of conductive nanoparticles and metal complexes, and a rheology control agent, and the viscosity at 25°C when sheared at a shear rate of 1 sec-1 is 100 mPa s or more, and the viscosity at 25°C when sheared at a shear rate of 100 sec-1 is 20 mPa s or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This invention , electric This relates to a method for manufacturing child modules. [Background technology]

[0002] In electronic circuit boards, electromagnetic noise has become a problem due to increased integration and speed, and various methods for suppressing noise are being considered. For example, technologies have been disclosed that involve covering the board with conductive materials or electromagnetic wave absorbers such as shielding films, metal shielding cans, conductive paints, or plated covers. Furthermore, electromagnetic shielding methods are known that involve dry film deposition such as sputtering or the direct application of conductive paint to electronic components in order to save space, reduce weight, and improve productivity.

[0003] However, conventional dry deposition methods have problems such as high running costs, poor material utilization efficiency, and high overall costs due to deposition being performed under vacuum. On the other hand, in film formation methods for applying conductive paints, there is a problem in that the sides of three-dimensional structures such as electronic components are not adequately covered. Conventional conductive coatings have been proposed using inkjet technology, which allows printing at any location, has high material utilization efficiency, and low running costs (see, for example, Patent Document 1). Furthermore, a method of applying high-viscosity ink by spray coating has been proposed. Due to the high viscosity of the ink, a film with high viscosity is formed after application that does not drip even on the sides (see, for example, Patent Document 2). [Overview of the project] [Problems that the invention aims to solve]

[0004] The present invention aims to provide a liquid composition that has excellent dispensing properties and can form a good coating film without dripping when forming a conductive film on the side surface of an electronic component. [Means for solving the problem]

[0005] The liquid composition of the present invention, as a means for solving the aforementioned problems, comprises at least one of conductive nanoparticles and a metal complex, and a rheology control agent. Shear rate 1 sec -1 The viscosity at 25°C when sheared is 100 mPa·s or higher, and the shear rate is 100 sec. -1 The viscosity at 25°C when sheared is 20 mPa·s or less. [Effects of the Invention]

[0006] According to the present invention, it is possible to provide a liquid composition that has excellent discharge properties and can form a good coating film without dripping when forming a conductive film on the side surface of an electronic component. [Brief explanation of the drawing]

[0007] [Figure 1] Figure 1 is a schematic diagram showing an example of a coating film formed when a liquid composition without a rheology control agent is applied to a substrate. [Figure 2] Figure 2 is a schematic diagram showing an example of a coating film formed when the liquid composition of the present invention, which contains a rheology control agent, is applied to a substrate. [Modes for carrying out the invention]

[0008] (liquid composition) The liquid composition of the present invention comprises at least one of conductive nanoparticles and a metal complex, and a rheology control agent, and preferably further comprises a solvent, a binder, etc., as needed. Furthermore, the liquid composition of the present invention has a shear rate of 1 sec. -1 The viscosity at 25°C when sheared is 100 mPa·s or higher, and the shear rate is 100 sec. -1 The viscosity at 25°C when sheared is 20 mPa·s or less. There are no particular restrictions on the method for measuring the viscosity of the liquid composition, and it can be appropriately selected depending on the purpose. For example, it can be measured in accordance with JIS Z 8803. There are no particular restrictions on the apparatus used for the measurement, and it can be appropriately selected depending on the purpose. For example, a TV25 type viscometer (cone plate type viscometer, manufactured by Toki Sangyo Co., Ltd.) can be used.

[0009] The ink described in Patent Document 1 (Japanese Patent Publication No. 2021-72438) is an inkjet ink with low viscosity, which causes it to drip due to gravity when printing on the sides, resulting in a film thickness gradient between the upper and lower parts of the side. In particular, the upper corners become thinner, causing a problem where conductivity with the top surface is interrupted. Furthermore, the ink described in Patent Document 2 (Japanese Patent Publication No. 2020-139019) had the problem that spray application was inefficient in terms of material utilization and increased costs because unnecessary parts had to be covered with a mask or the like to spray the paint over the entire surface.

[0010] Therefore, after diligent research, the inventors have concluded that the liquid composition of the present invention, by comprising at least one of conductive nanoparticles and a metal complex, and a rheology control agent, has a shear rate of 1 sec. -1 The viscosity at 25°C when sheared is 100 mPa·s or higher, and the shear rate is 100 sec. -1 We found that when sheared, the viscosity at 25°C is 20 mPa·s or less (i.e., viscosity is lower when shear force is applied and higher when no shear force is applied). Therefore, when ejecting ink to print on equipment, the viscosity decreases, resulting in improved ejection efficiency. On the other hand, after the ink has been printed, the viscosity increases, which suppresses ink dripping and flow, allowing the shape to be maintained.

[0011] Figure 1 is a schematic diagram of a coating film when a liquid composition containing no rheology control agent is applied to a substrate, and Figure 2 is a schematic diagram of a coating film when the liquid composition of the present invention containing a rheology control agent is applied to a substrate. In printing on the side surface of a three-dimensional object, if the viscosity of the liquid composition after printing is low, sagging of the liquid composition occurs as shown in Figure 1. On the other hand, as shown in Figure 2, when the viscosity of the liquid composition after printing is high, sagging does not occur. In inkjet printing, the viscosity of the liquid composition needs to be low at the time of ejection from the viewpoint of ejection performance, and general Newtonian fluid inks remain low in viscosity after printing, so there is a problem that sagging occurs. In contrast, the liquid composition of the present invention has an increased viscosity after printing, and thus can suppress sagging. In addition to adjusting viscosity, a method of adding a UV curable resin for immediate curing is conceivable, but when the conductive particles in the present invention are colored, this method cannot be used because it does not transmit UV light.

[0012] <Conductive Nanoparticles and Metal Complexes> The conductive nanoparticles and metal complexes are not particularly limited as long as they have conductivity, and can be appropriately selected according to the purpose. Examples thereof include metal particles such as silver, copper, gold, aluminum, nickel, and stainless steel, carbonaceous substances such as carbon black, graphite, and graphene, and conductive oxides such as ITO, ATO, and Ab2O5. Among these, silver and ITO are preferred from the viewpoint of shielding properties.

[0013] The volume average particle diameter of the conductive nanoparticles is not particularly limited and can be appropriately selected according to the purpose, but is preferably 1 nm or more and 1,000 nm or less, and more preferably 5 nm or more and 500 nm or less. There are no particular restrictions on the content of the conductive nanoparticles and metal complex, and they can be appropriately selected depending on the purpose. However, it is preferable that the content be 5% by mass or more and 80% by mass or less, and more preferably 10% by mass or more and 60% by mass or less, relative to the total amount of the liquid composition. When the content of the conductive nanoparticles and metal complex is 5% by mass or more, the conductivity is improved. This is thought to be because the interparticle distance of the nanoparticles decreases after coating, and conductivity can be obtained even in the presence of a rheology control agent. When the content of the conductive nanoparticles and metal complex is 80% by mass or less, the film uniformity is improved. This is thought to be because the fluidity of the liquid composition increases.

[0014] <Rheology control agent> The rheology control agent is a substance whose viscosity decreases when a shear force is applied and increases when no shear force is applied. By containing the rheology control agent, the liquid composition becomes thixotropic, and when the ink is ejected to print on the equipment, the viscosity decreases, making ejection possible. On the other hand, after the ink has been printed, the viscosity increases, suppressing ink dripping and flow and maintaining the shape.

[0015] The rheology control agent is not particularly limited as long as it is a known substance whose viscosity decreases when a shear force is applied and increases when no shear force is applied. It can be appropriately selected depending on the purpose, and examples include layered clay minerals, modified ureas, amide waxes, castor oil, and silica particles. Among these, layered clay minerals are preferred.

[0016] Examples of the aforementioned layered clay minerals include serpentine-kaolin group, talcumpyrophyllite group, smectite group, vermiculite group, mica group, brittle mica group, chlorite group, and mixed layer minerals. Commercially available products can be used as the layered clay mineral, and examples of such commercial products include Kunipia-F, Kunipia-G, Kunipia-G4, Smecton-SA, Smecton-SWN, Smecton-SWF, Kunibis-110, Kunibis-127, Moistonite-QO, Smecton-SA, Smecton-STN, Smecton-SEN (Kunimine Industries Co., Ltd.), CLAYTONE-3, CLAYTONE-34, CLAYTONE-40, CLAYTONE-AF, CLAYTONE-APA, CLAYTONE-EM, CLAYTONE-ER, CLAYTONE-HT, CLAYTONE-HY, CLAYTONE-II, CLAYTONE-IMG400, CLAYTONE-MPZ, CLAYTONE-PS3, CLAYTONE-SF, CLAYTONE-VP V, and CLAYTONE-VZ (Big Chemie Japan).

[0017] There are no particular restrictions on the content of the rheology control agent, and it can be appropriately selected depending on the purpose, but it is preferable that it be 3 parts by weight or more and 5 parts by weight or less of the total volume of the liquid composition. When the content of the rheology control agent is 3 parts by weight or more of the total volume of the liquid composition, the film uniformity is improved. Furthermore, when the content of the rheology control agent is 5 parts by weight or less of the total volume of the liquid composition, the discharge performance is improved. Depending on the circulation conditions of the pump provided in the nozzle when discharging the liquid composition, the liquid composition may contain 5 parts by weight or more of the rheology control agent.

[0018] <organic solvents> The aforementioned organic solvent is not particularly limited and can be appropriately selected depending on the purpose. Examples include alcohols such as ethanol and butanol, ketones such as cyclohexanone and methyl ethyl ketone, aromatics such as toluene and ethylbenzene, glycols such as ethylene glycol and diethylene glycol, glycol ethers such as diethylene glycol monoethyl ether and ethylene glycol monobutyl ether, and esters such as butyl acetate and γ-butyl lactone. There are no particular restrictions on the content of the organic solvent, and it can be appropriately selected depending on the purpose, but it is preferably 20% by mass or more and 95% by mass or less, and more preferably 40% by mass or more and 90% by mass or less, based on the total amount of the liquid composition. When the content is 20% by mass or more and 95% by mass or less, fluidity is ensured and ink ejection performance is good.

[0019] <Method for producing a liquid composition> The liquid composition can be produced by dissolving or dispersing each of the above components in the above organic solvent. Specifically, a liquid composition can be prepared by mixing the above components with the above organic solvent using a mixing machine such as a ball mill, sand mill, bead mill, pigment disperser, lye crusher, ultrasonic disperser, homogenizer, planetary mixer, or film mixer.

[0020] <Binding agent> The binder is not particularly limited and can be appropriately selected depending on the purpose. Examples include acrylic resin, urethane resin, epoxy resin, ethylcellulose resin, polyvinyl alcohol resin, and olefin resin.

[0021] (Conductive film) The conductive film of the present invention comprises at least one of conductive nanoparticles and a metal complex, and a rheology control agent. The same conductive nanoparticles, metal complex, and rheology control agent as those used in the liquid composition can be used.

[0022] There are no particular restrictions on the thickness of the conductive film, and it can be appropriately selected depending on the purpose. However, when metal particles are used as the rheology control agent, a thickness of 0.05 μm to 50 μm is preferred, and when a carbonic substance is used as the rheology control agent, a thickness of 1 μm to 300 μm is preferred.

[0023] There are no particular restrictions on the volume resistivity of the conductive film, and it can be appropriately selected according to the purpose, but it is preferably 1 mΩ·cm or less, and more preferably 0.1 mΩ·cm or less.

[0024] The conductive film can be formed by coating the liquid composition of the present invention onto a substrate. The coating method is not particularly limited and can be appropriately selected depending on the purpose. Examples include spin coating, casting, microgravure coating, gravure coating, bar coating, roll coating, wire bar coating, dip coating, slit coating, capillary coating, spray coating, nozzle coating, dispense coating, gravure printing, screen printing, flexographic printing, offset printing, reverse printing, and inkjet printing. Among these, inkjet printing is preferred. In particular, inkjet printing allows for on-demand printing of diverse patterns in minute areas, and is preferable for printing on electronic components or modules because it offers high material efficiency and can accommodate a variety of patterns. Furthermore, in inkjet printing, a flow-through head can be used to prevent ink stagnation within the print head. A flow-through head has a structure in which the liquid composition circulates within the ejection head. In this process, the liquid composition is made to flow in a way that applies a shearing velocity within the head, thereby reducing its viscosity and enabling ink ejection.

[0025] A commercially available product can be used as the flow-through head; for example, the MH5421F manufactured by Ricoh Co., Ltd. can be used.

[0026] The conductive film can be a surface treatment layer. The aforementioned surface treatment layer is formed as a layer to adjust the wettability or surface energy of the film surface, and is formed as a resin film having hydrophilic or hydrophobic groups on its surface. As the material for the surface treatment layer, materials having carboxyl groups, amino groups, keto groups, OH groups, fluorine groups, silanol groups, etc. in the resin structure can be used. Furthermore, inorganic particles such as ceramics (SiO2, Al2O3, AlN, BN, etc.), metals (Ag, Cu, Au, Al, etc.), and carbon can also be mixed in. The thickness of the surface treatment layer is preferably 0.5 μm or more and 10 μm or less. There are no particular restrictions on the method for forming the surface treatment layer, and it can be appropriately selected depending on the purpose. For example, it can be formed by coating a resin material or inorganic material mixed with at least an organic monomer material having a reactive group and an initiator, and then performing a curing treatment such as UV irradiation, heat treatment, or dehydration treatment. Various printing methods can be used for coating, such as spin coating, casting, microgravure coating, gravure coating, bar coating, roll coating, wire bar coating, dip coating, slit coating, capillary coating, spray coating, nozzle coating, dispense coating, gravure printing, screen printing, flexographic printing, offset printing, reverse printing, and inkjet printing.

[0027] The conductive film can form a surface protective layer. The aforementioned surface protective layer is mainly formed of a resin material. Examples of the aforementioned resin materials include photocurable resins, thermosetting resins, and materials to which inorganic particles have been added. As the inorganic particles, ceramic materials such as SiO2, Al2O3, AlN, and BN can be used to provide the function of suppressing thermal expansion when the temperature rises. Specific examples of curing resin materials include, for example, urethane resins, epoxy resins, phenolic resins, polyimide resins, ester resins, vinyl resins, silicone resins, styrene resins, cellulose resins, amide resins, fluororesins, and mixtures thereof. Among these, epoxy resins, silicone resins, and polyimide resins are preferred due to their good heat resistance, and epoxy resins are more preferred due to their low curing shrinkage. Furthermore, commercially available products can be used as the material for the surface protective layer. Examples include ink materials such as IJSR4000 and IJSR9000 from Taiyo Ink Co., Ltd., PR1205 from Go-O Chemical Co., Ltd., and PA1210 from JNC Corporation. [Examples]

[0028] The following describes embodiments of the present invention, but the present invention is not limited in any way to these embodiments.

[0029] (Example 1) 100 parts by weight of Ag nanoparticles (FlowMetal SR7000, manufactured by Bando Chemical Co., Ltd., Ag nanoparticle content 50% by mass) as a conductive ink and 3 parts by weight of a rheology control agent (Smecton-SEN, manufactured by Kunimine Industries Co., Ltd.) were mixed and mixed for 3 hours using a roller mill (50 rpm). After that, coarse particles were removed using a 2.5 μm filter to obtain a liquid composition. The viscosity of the obtained liquid composition was measured using a viscometer while varying the shear rate, and at a shear rate of 1 sec -1 The pressure was 210 mPa·s, and the shear rate was 100 sec. -1 The pressure was 11 mPa·s. Furthermore, the volume resistivity of the obtained liquid composition was measured using a Loresta GP (manufactured by Dia Instruments), and the shielding characteristics were measured using a WM7300 EMC NOISE SCANNER1 (manufactured by Morita Tech Co., Ltd.). The volume resistivity was 80 μΩ·cm, and the shielding characteristics were 48 dB.

[0030] (Example 2) In Example 1, a liquid composition was obtained in the same manner as in Example 1, except that Ag nanoparticles were changed to an Ag complex (TEC-IJ-010, manufactured by InkTec). When the viscosity was measured in the same manner as in Example 1, the shear rate was 1 sec -1 and 180 mPa·s, and the shear rate was 100 sec -1 and 10 mPa·s. Further, when the volume resistance value and shielding property of the obtained liquid composition were measured in the same manner as in Example 1, the volume resistance value was 75 μΩ·cm, and the shielding property was 45 dB.

[0031] (Example 3) In Example 1, a liquid composition was obtained in the same manner as in Example 1, except that the content of the rheology control agent was changed from 3 parts by weight to 5 parts by weight. When the viscosity was measured in the same manner as in Example 1, the shear rate was 1 sec -1 and 330 mPa·s, and the shear rate was 100 sec -1 and 18 mPa·s. Further, when the volume resistance value and shielding property of the obtained liquid composition were measured in the same manner as in Example 1, the volume resistance value was 200 μΩ·cm, and the shielding property was 40 dB.

[0032] (Example 4) In Example 1, a liquid composition was obtained in the same manner as in Example 1, except that Ag nanoparticles were changed to ITO nanoink (manufactured by Sigma-Aldrich). When the viscosity was measured in the same manner as in Example 1, the shear rate was 1 sec -1 and 200 mPa·s, and the shear rate was 100 sec -1 and 10 mPa·s. Further, when the volume resistance value and shielding property of the obtained liquid composition were measured in the same manner as in Example 1, the volume resistance value was 980 μΩ·cm, and the shielding property was 30 dB.

[0033] (Example 5) A liquid composition was obtained in the same manner as in Example 1, except that the rheology control agent was changed from 3 parts by weight of smectone-SEN to 5 parts by weight of modified urea (RHEOBYK-410: manufactured by Bic Chemie Japan). When the viscosity was measured in the same manner as in Example 1, the shear rate was 1 sec. -1 The pressure was 180 mPa·s, and the shear rate was 100 sec. -1 The pressure was 15 mPa·s. Furthermore, when the volume resistivity and shielding characteristics of the obtained liquid composition were measured in the same manner as in Example 1, the volume resistivity was 230 μΩ·cm and the shielding characteristics were 35 dB.

[0034] (Example 6) In Example 4, a liquid composition was obtained in the same manner as in Example 4, except that the content of the rheology control agent was changed from 3 parts by weight to 5 parts by weight. When the viscosity was measured in the same manner as in Example 4, the shear rate was 1 sec. -1 The pressure was 350 mPa·s, and the shear rate was 100 sec. -1 The pressure was 20 mPa·s. Furthermore, when the volume resistivity and shielding characteristics of the obtained liquid composition were measured in the same manner as in Example 1, the volume resistivity was 1,300 μΩ·cm and the shielding characteristics were 20 dB.

[0035] (Comparative Example 1) Comparative Example 1 was prepared in the same manner as in Example 1, except that the content of the rheology control agent was changed to 10 parts by weight. When the viscosity was measured in the same manner as in Example 1, the shear rate was 1 sec. -1 The pressure was 1,200 mPa·s, and the shear rate was 100 sec. -1 The pressure was 60 mPa·s. We also attempted to use the inkjet method for ejection, but it was unsuccessful.

[0036] (Comparative Example 2) A liquid composition was obtained in the same manner as in Example 1, except that the content of the rheology control agent was changed from 3 parts by weight to 6 parts by weight. When the viscosity was measured in the same manner as in Example 1, the shear rate was 1 sec. -1At 500 mPa·s, the shear rate was 100 sec. -1 The pressure was 24 mPa·s. We also attempted to use the inkjet method for ejection, but it was unsuccessful.

[0037] (Comparative Example 3) In Example 1, a liquid composition was obtained in the same manner as in Example 1, except that a rheology control agent was not added. When the viscosity was measured in the same manner as in Example 1, the shear rate was 1 sec. -1 The pressure was 5.6 mPa·s, and the shear rate was 100 sec. -1 The pressure was 5.0 mPa·s. Furthermore, when the volume resistivity and shielding characteristics of the obtained liquid composition were measured in the same manner as in Example 1, the volume resistivity was 8 μΩ·cm and the shielding characteristics were 28 dB.

[0038] Discharge properties and film uniformity were evaluated for Examples 1-6 and Comparative Examples 1-3. The results are shown in Table 1.

[0039] <Dischargeability> The liquid compositions of Examples 1-6 and Comparative Examples 1-3 were loaded into an inkjet recording device equipped with an inkjet head (MH5421F, Ricoh Co., Ltd.) and a pump (CIMS HFR, Megnajet). While circulating the liquid composition at a flow rate of 450 ml / min, the inkjet head was tilted at 45 degrees to coat the liquid composition and form a conductive film with a thickness of 5 μm. The ejection performance at this time was evaluated based on the evaluation criteria below. The results are shown in Table 1. [Evaluation Criteria] ○: Possible to discharge ×: Unable to discharge

[0040] <Film uniformity> Using the liquid compositions of Examples 1-6 and Comparative Examples 1-3, conductive films were formed in the same manner as described in <Dischargeability> above. Film uniformity was measured by cross-sectional SEM, and the film thickness was evaluated based on the decrease in film thickness on the upper surface according to the following evaluation criteria. The results are shown in Table 1. When the film uniformity is good, a good coating film is formed without any sagging. [Evaluation Criteria] ○: Good film uniformity (reduction from top film thickness less than 10%) ×: Poor film uniformity (reduction of 10% or more from the top film thickness)

[0041] [Table 1]

[0042] The embodiments of the present invention are as follows. <1> The material comprises at least one of conductive nanoparticles and a metal complex, and a rheology control agent. Shear rate 1 sec -1 The viscosity at 25°C when sheared is 100 mPa·s or higher, and the shear rate is 100 sec. -1 This liquid composition is characterized by having a viscosity of 20 mPa·s or less at 25°C when sheared. <2> The rheological control agent is a layered clay mineral, <1> This is the liquid composition described in [the relevant document]. <3> The content of the rheology control agent is 3 parts by weight or more and 5 parts by weight or less relative to the liquid composition. <1> from <2> It is a liquid composition as described in any of the above. <4> A conductive film characterized by comprising at least one of conductive nanoparticles and a metal complex, and a rheology control agent. <5> The electronic module has a conductive film comprising at least one of conductive nanoparticles and a metal complex, and a rheology control agent. <6> The resistivity of the conductive film is 1 mΩ·cm or less, <5> This is the electronic module described in [the document]. <7> The aforementioned <1> from <3> This is a method for manufacturing an electronic module, characterized by forming an electromagnetic wave shielding film by coating with any of the liquid compositions described in the above by an inkjet method. <8> The aforementioned <1> from <3> The liquid composition described in any of the above is coated by an inkjet method by applying a shear force to the liquid composition such that its viscosity is 20 mPa·s or less at 25°C. <7> This is a method for manufacturing the electronic module described in [the document].

[0043] The aforementioned <1> from <3> A liquid composition according to any of the above, <4> The conductive film described above, <5> The electronic module described above, and the <7> from <8> According to the method for manufacturing an electronic module described in any of the above, the aforementioned problems of the conventional method can be solved and the objective of the present invention can be achieved. [Prior art documents] [Patent Documents]

[0044] [Patent Document 1] Japanese Patent Publication No. 2021-72438 [Patent Document 2] Japanese Patent Publication No. 2020-139019

Claims

1. A method for manufacturing an electronic module in which a liquid composition is applied to the side surface of a three-dimensional object by an inkjet method to form an electromagnetic wave shielding film, The liquid composition is The material comprises at least one of conductive nanoparticles and a metal complex, and a rheology control agent. Shear rate is 1 sec -1 The viscosity at 25°C when sheared is 100 mPa·s or more, and the shear rate is 100 sec. -1 The viscosity at 25°C when sheared is 20 mPa·s or less. A method for manufacturing an electronic module, characterized in that the rheology control agent is a layered clay mineral.

2. The method for manufacturing an electronic module according to claim 1, wherein the content of the rheology control agent is 3 parts by weight or more and 5 parts by weight or less relative to the liquid composition.

3. The method for manufacturing an electronic module according to Claim 1, wherein a shear force is applied to the liquid composition so that the viscosity of the liquid composition is 20 mPa·s or less at 25°C, and the module is coated by an inkjet method.

Citation Information

Patent Citations

  • Conductive paste and method for preparing conductive paste

    JP2013110010A

  • Rheology-modified inks and printing methods

    JP2013515826A

  • Photocatalytic coating composition

    JP2015193832A

  • Silver nanoparticle inks comprising aminomethylsilanes

    JP2016079396A

  • Ink composition, printer, and method for discharging ink composition

    JP2018024873A