Image forming apparatus and unit for image forming apparatus

The image forming apparatus enhances electrical properties and abrasion resistance of the inorganic protective layer by using a specific elemental composition ratio and charging device configurations, addressing the limitations of existing systems.

JP7947737B2Active Publication Date: 2026-11-11FUJIFILM BUSINESS INNOVATION CORP
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2022052248
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-03-28
Publication Date
2026-11-11
Estimated Expiration
2042-03-28

AI Technical Summary

Technical Problem

Existing image forming apparatuses face challenges in achieving superior electrical properties and abrasion resistance of the inorganic protective layer in electrophotographic photoreceptors, particularly when the elemental composition ratio of oxygen to metal element in the surface layer is less than 1.3.

Method used

The image forming apparatus includes an electrophotographic photoreceptor with a conductive substrate, photosensitive layer, and an inorganic protective layer containing metal element M, oxygen O, and hydrogen H, with an elemental composition ratio of oxygen O to metal element M ranging from 1.3 to 1.5, and employs a charging device with a contact-type charging member and AC voltage application, along with specific voltage and frequency settings to enhance electrical properties and wear resistance.

Benefits of technology

The apparatus achieves superior electrical properties and wear resistance of the inorganic protective layer, outperforming conventional systems by maintaining optimal electron transport and photoelectric conversion functions while reducing wear.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007947737000005
    Figure 0007947737000005
  • Figure 0007947737000006
    Figure 0007947737000006
  • Figure 0007947737000007
    Figure 0007947737000007
Patent Text Reader

Abstract

To provide an image forming apparatus that is excellent in electrical characteristics and wear resistance of an inorganic protective layer in an electrophotographic photoreceptor.SOLUTION: An image forming apparatus comprises: an electrophotographic photoreceptor that has in this order a conductive substrate, a photosensitive layer, and an inorganic protective layer including a metal element M, oxygen O, and hydrogen H, wherein the element component ratio of the oxygen O to the metal element M (oxygen O / metal element M) in a layer forming a surface of the inorganic protective layer is 1.3 or more and 1.5 or less; an electrifying device having an electrifying member of a contact system that electrifies a surface of the electrophotographic photoreceptor, and an AC voltage application unit that applies AC voltage to the electrifying member of a contact system; an electrostatic charge image forming device that forms an electrostatic charge image on the electrified surface of the electrophotographic photoreceptor; a developing device that supplies electrostatic charge image developer to develop the electrostatic charge image formed on the surface of the electrophotographic photoreceptor as a toner image; and a transfer device that transfers the toner image formed on the surface of the electrophotographic photoreceptor to a surface of a recording medium.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an image forming apparatus and a unit for an image forming apparatus.

Background Art

[0002] Image formation by electrophotography is performed, for example, by charging the surface of a photoreceptor, forming an electrostatic charge image on the surface of the photoreceptor according to image information, then developing this electrostatic charge image with a developer containing toner to form a toner image, and transferring and fixing this toner image onto the surface of a recording medium.

[0003] Here, Patent Document 1 discloses "An electrophotographic photoreceptor, wherein in an electrophotographic apparatus having an electrophotographic photoreceptor, a toner supply member, and a charging imparting member, or a process cartridge detachably attachable to the main body of an electrophotographic apparatus, the outer surface of the electrophotographic photoreceptor has two protective layers, the protective layers each contain metal or metal oxide particles and a binder resin, and the relationship between the proportion of the metal or metal oxide particles contained in the protective layer 1 on the photoreceptor layer side and the proportion of the metal or metal oxide particles contained in the protective layer 2 laminated on the protective layer 1 satisfies the following formula (1)." P1>P2 Formula (1) P1 Weight % of the metal or metal oxide particles contained in the protective layer 1 P2 Weight % of the metal or metal oxide particles contained in the protective layer 2

Prior Art Documents

Patent Documents

[0004]

Patent Document 1

Summary of the Invention

Problem to be Solved by the Invention

[0005] An object of the present invention is to provide an image forming apparatus that is superior in the electrical properties of the electrophotographic photoreceptor and the abrasion resistance of the inorganic protective layer, compared to a case where the elemental composition ratio of oxygen O to metal element M (oxygen O / metal element M) in the layer constituting the surface of the inorganic protective layer is less than 1.3, the image forming apparatus comprising: an electrophotographic photoreceptor having a conductive substrate, a photosensitive layer, and an inorganic protective layer containing a metal element M, oxygen O and hydrogen H in this order; a charging device having a charging member that charges the surface of the electrophotographic photoreceptor; an electrostatic latent image forming apparatus that forms an electrostatic latent image on the surface of the charged electrophotographic photoreceptor; a developing device that supplies an electrostatic latent image developer to develop the electrostatic latent image formed on the surface of the electrophotographic photoreceptor as a toner image; and a transfer device that transfers the toner image formed on the surface of the electrophotographic photoreceptor to the surface of a recording medium. [MEANS FOR SOLVING THE PROBLEMS]

[0006] Means for solving the above problem include the following aspects. <1> An electrophotographic photoreceptor having a conductive substrate, a photosensitive layer, and an inorganic protective layer containing a metal element M, oxygen O and hydrogen H in this order, wherein the elemental composition ratio of the oxygen O to the metal element M (oxygen O / metal element M) in the layer constituting the surface of the inorganic protective layer is 1.3 or more and 1.5 or less; and A charging device having a contact-type charging member that charges the surface of the electrophotographic photoreceptor, and an AC voltage applying unit that applies an AC voltage to the contact-type charging member; An electrostatic latent image forming apparatus that forms an electrostatic latent image on the surface of the charged electrophotographic photoreceptor; A developing device that supplies an electrostatic latent image developer to develop the electrostatic latent image formed on the surface of the electrophotographic photoreceptor as a toner image; A transfer device that transfers the toner image formed on the surface of the electrophotographic photoreceptor to the surface of a recording medi um; and An image forming apparatus comprising the above. <2> The image forming apparatus according to <1>, wherein the elemental composition ratio of the oxygen O to the metal element M (oxygen O / metal element M) in the layer constituting the surface of the inorganic protective layer is 1.4 or more and 1.5 or less. <3> The inorganic protective layer is a single layer of the layer constituting the surface of the inorganic protective layer, wherein the elemental composition ratio (oxygen O / metal element M) of oxygen O to the metal element M is 1.3 or more and less than 1.5. <1> or <2> The image forming apparatus described above. <4> The thickness of the single layer constituting the surface of the inorganic protective layer is 0.5 μm or more and 1.0 μm or less. <3> The image forming apparatus described above. <5> The AC voltage applied to the contact-type charging member by the AC voltage application unit, the peak voltage V pp The voltage is between 350V and 4000V, and the frequency is 100Hz or higher. <1> ~ <4> An image forming apparatus as described in any one of the items. <6> The aforementioned peak voltage V pp The voltage is between 800V and 1500V, and the frequency is 2500Hz or higher. <5> The image forming apparatus described above. <7> The charging member is more effective than the contact-type charging member in the rotational direction of the electrophotographic photoreceptor. Downstream It is provided with a non-contact charging member that charges the surface of the electrophotographic photoreceptor, and a DC voltage application unit that applies a DC voltage to the non-contact charging member. <1> ~ <4> An image forming apparatus as described in any one of the items. <8> The AC voltage applied to the contact-type charging member by the AC voltage application unit, the peak voltage V pp The voltage is between 1000V and 4000V, and the frequency is 2500Hz or higher. The DC voltage applied to the non-contact charging member by the DC voltage application unit is such that the voltage V is 600V or more and 1000V or less. <7> The image forming apparatus described above. <9> The light transmittance of the inorganic protective layer is 90% or more. <1> ~ <8> An image forming apparatus as described in any one of the items. <10> An electrophotographic photoreceptor having, in this order, a conductive substrate, a photosensitive layer, and an inorganic protective layer containing a metal element M, oxygen O, and hydrogen H, wherein the elemental composition ratio (oxygen O / metal element M) of oxygen O to the metal element M in the layer constituting the surface of the inorganic protective layer is 1.3 or more and 1.5 or less, A charging device having a contact-type charging member that charges the surface of the electrophotographic photoreceptor and an AC voltage application unit that applies an AC voltage to the contact-type charging member, A unit for an image forming apparatus, comprising the above. [Effects of the Invention]

[0007] <1> According to the present invention, an image forming apparatus is provided that comprises an electrophotographic photoreceptor having a conductive substrate, a photosensitive layer, and an inorganic protective layer containing a metal element M, oxygen O, and hydrogen H in that order; a charging device having a charging member for charging the surface of the electrophotographic photoreceptor; an electrostatic image forming device for forming an electrostatic image on the surface of the charged electrophotographic photoreceptor; a developing device for supplying an electrostatic image developer and developing the electrostatic image formed on the surface of the electrophotographic photoreceptor as a toner image; and a transfer device for transferring the toner image formed on the surface of the electrophotographic photoreceptor to the surface of a recording medium. The image forming apparatus is provided that exhibits superior electrical properties and wear resistance of the inorganic protective layer in the electrophotographic photoreceptor compared to the case where the elemental composition ratio (oxygen O / metal element M) of oxygen O to metal element M in the layer constituting the surface of the inorganic protective layer is less than 1.3.

[0008] <2> According to the invention, an image forming apparatus is provided in which the electrical properties and wear resistance of the inorganic protective layer of the electrophotographic photoreceptor are superior to those in which the elemental composition ratio of oxygen O to metal element M (oxygen O / metal element M) is less than 1.4.

[0009] <3> According to the present invention, compared to a laminate in which the inorganic protective layer is a laminate including a layer constituting the surface of the inorganic protective layer, in which the elemental composition ratio of oxygen O to metal element M (oxygen O / metal element M) is 1.3 or more and less than 1.5, an image forming apparatus is provided in which the electrical properties and wear resistance of the inorganic protective layer are superior in the electrophotographic photoreceptor.

[0010] <4> According to the invention, an image forming apparatus is provided that exhibits superior electrical properties and wear resistance of the inorganic protective layer in an electrophotographic photoreceptor compared to a case where the thickness of a single layer constituting the surface of the inorganic protective layer is less than 0.5 μm.

[0011] <5> According to the invention, the peak-to-peak voltage V in the AC voltage applied to a contact-type charged member by the AC voltage application unit pp Compared to cases where the voltage is less than 350V or more than 4000V, or the frequency is less than 100Hz, an image forming apparatus is provided that has superior electrical characteristics and wear resistance of the inorganic protective layer in the electrophotographic photoreceptor. <6> According to the invention, the peak-to-peak voltage V in the AC voltage applied to a contact-type charged member by the AC voltage application unit pp Compared to cases where the voltage is less than 800V or more than 1500V, or the frequency is less than 2500Hz, an image forming apparatus is provided that has superior electrical characteristics and wear resistance of the inorganic protective layer in the electrophotographic photoreceptor.

[0012] <7> According to the present invention, an image forming apparatus is provided which has a conductive substrate, a photosensitive layer, and an inorganic protective layer containing a metal element M, oxygen O, and hydrogen H in that order; a charging device having a charging member for charging the surface of the electrophotographic photoreceptor; an electrostatic image forming device for forming an electrostatic image on the surface of the charged electrophotographic photoreceptor; a developing device for supplying an electrostatic image developer and developing the electrostatic image formed on the surface of the electrophotographic photoreceptor as a toner image; and a transfer device for transferring the toner image formed on the surface of the electrophotographic photoreceptor to the surface of a recording medium. Compared to the case where the elemental composition ratio of oxygen O to metal element M (oxygen O / metal element M) in the layer constituting the surface of the inorganic protective layer is less than 1.3, the image forming apparatus has a contact-type charging member and a non-contact-type charging member, and is superior in electrical properties of the electrophotographic photoreceptor and wear resistance of the inorganic protective layer. <8> According to the invention, the peak voltage V in the AC voltage applied to a contact-type charging member by the AC voltage application unit ppCompared to cases where the voltage is less than 1000V or more than 4000V, or the frequency is less than 2500Hz, or where the voltage V in the DC voltage applied to the non-contact type charged member by the DC voltage application unit is less than 600V or more than 1000V, an image forming apparatus is provided that has superior electrical characteristics and wear resistance of the inorganic protective layer in the electrophotographic photoreceptor.

[0013] <9> According to the invention, an image forming apparatus is provided in which the electrical properties and wear resistance of the inorganic protective layer are superior to those of an electrophotographic photoreceptor compared to a case where the light transmittance of the layer constituting the surface of the inorganic protective layer is less than 90%.

[0014] <10> According to the present invention, an image forming unit is provided that comprises an electrophotographic photoreceptor having a conductive substrate, a photosensitive layer, and an inorganic protective layer containing a metal element M, oxygen O, and hydrogen H in that order, and a charging device having a charging member for charging the surface of the electrophotographic photoreceptor, wherein the electrophotographic photoreceptor has superior electrical properties and wear resistance of the inorganic protective layer compared to a case where the elemental composition ratio (oxygen O / metal element M) of oxygen O to metal element M in the layer constituting the surface of the inorganic protective layer is less than 1.3. [Brief explanation of the drawing]

[0015] [Figure 1] This is a schematic diagram showing an example of an image forming apparatus according to this embodiment. [Figure 2] This is a schematic diagram showing another example of the image forming apparatus according to this embodiment. [Figure 3] This is a schematic diagram showing an example of a film deposition apparatus used to form an inorganic protective layer on an electrophotographic photoreceptor in this embodiment. [Figure 4] This is a schematic diagram showing an example of a plasma generator used for forming the inorganic protective layer of the electrophotographic photoreceptor in this embodiment. [Figure 5] This is a schematic cross-sectional view showing an example of the layer configuration of an electrophotographic photoreceptor in an image forming apparatus according to this embodiment. [Figure 6]This is a schematic cross-sectional view showing another example of the layer configuration of the electrophotographic photoreceptor in the image forming apparatus according to this embodiment. [Modes for carrying out the invention]

[0016] The following describes in detail an example embodiment of the present invention. These descriptions and examples are illustrative and not limiting to the present invention.

[0017] In this specification, numerical ranges indicated using "~" represent a range that includes the numbers before and after "~" as the minimum and maximum values, respectively. In numerical ranges described stepwise within this specification, the upper or lower limit of one numerical range may be replaced by the upper or lower limit of another numerical range described stepwise. Furthermore, in numerical ranges described in this disclosure, the upper or lower limit of that range may be replaced by the values ​​shown in the examples.

[0018] In this specification, the term "process" includes not only independent processes but also processes that cannot be clearly distinguished from other processes, provided that their intended purpose is achieved.

[0019] When embodiments are described herein with reference to the drawings, the configuration of such embodiments is not limited to that shown in the drawings. Furthermore, the sizes of the components in each figure are conceptual, and the relative relationships between the components are not limited thereto.

[0020] In this specification, each component may contain multiple types of the corresponding substance. When referring to the amount of each component in a composition in this disclosure, if there are multiple types of the substance corresponding to each component in the composition, unless otherwise specified, it means the total amount of those multiple types of substances present in the composition.

[0021] <Image forming apparatus> The image forming apparatus according to this embodiment comprises an electrophotographic photoreceptor (hereinafter also simply referred to as "photoreceptor"), a charging device for charging the surface of the photoreceptor, an electrostatic image forming device for forming an electrostatic image on the charged surface of the photoreceptor, a developing device for supplying an electrostatic image developer and developing the electrostatic image formed on the surface of the photoreceptor as a toner image, and a transfer device for transferring the toner image formed on the surface of the photoreceptor to the surface of a recording medium. The photoreceptor comprises, in this order, a conductive substrate, a photosensitive layer, and an inorganic protective layer containing a metal element M, oxygen O, and hydrogen H, with the elemental composition ratio (oxygen O / metal element M) of oxygen O to metal element M in the layer constituting the surface of the inorganic protective layer being 1.3 or more and 1.5 or less. The charging device includes a contact-type charging member that charges the surface of an electrophotographic photoreceptor and an AC voltage application unit that applies an AC voltage to the contact-type charging member.

[0022] Here, the image forming apparatus according to this embodiment may be a well-known image forming apparatus such as a direct transfer apparatus that directly transfers a toner image formed on the surface of a photoreceptor to a recording medium; an intermediate transfer apparatus that first transfers a toner image formed on the surface of a photoreceptor to the surface of an intermediate transfer body, and secondarily transfers the toner image transferred to the surface of the intermediate transfer body to the surface of a recording medium; or an apparatus equipped with a static elimination device that irradiates the surface of the photoreceptor with static elimination light to eliminate static charge after the transfer of the toner image and before charging. In the case of an intermediate transfer method apparatus, the transfer apparatus may be configured to include, for example, an intermediate transfer body on which a toner image is transferred; a primary transfer apparatus that first transfers the toner image formed on the surface of the photoreceptor to the surface of the intermediate transfer body; and a secondary transfer apparatus that secondarily transfers the toner image transferred to the surface of the intermediate transfer body to the surface of the recording medium.

[0023] In addition, in the image forming apparatus according to this embodiment, the portion including at least a photoreceptor and a charging device may constitute a unit for the image forming apparatus and may be a cartridge structure (process cartridge) that can be attached to and detached from the image forming apparatus.

[0024] The image forming apparatus according to this embodiment exhibits excellent electrical properties and wear resistance of the inorganic protective layer in the photoreceptor, thanks to the above configuration. The reason for this is presumed to be as follows.

[0025] In a photoreceptor, the inorganic protective layer containing a metal element M, oxygen O, and hydrogen H, which functions as an electron transport layer, needs to have the functions of surface electron injection to obtain charging properties, and photoelectric conversion and electron transport functions to obtain electrical properties. Furthermore, in order to inject electrons into the inorganic protective layer on the surface of the photoreceptor, the layers constituting the surface of the inorganic protective layer are made to have low resistance. However, reducing the resistance of the layers constituting the surface of the inorganic protective layer requires increasing the amount of metallic elements to lower surface resistance, which reduces light transmittance and impairs photoelectric conversion and electron transport functions. As a result, the electrical properties of the photoreceptor deteriorate. Furthermore, the wear resistance of the inorganic protective layer decreases.

[0026] Therefore, in this embodiment, the elemental composition ratio (oxygen O / metal element M) of oxygen O to metal element M in the layer constituting the surface of the inorganic protective layer of the photoreceptor is set to 1.3 or more and 1.5 or less. This improves wear resistance along with the photoelectric conversion function and electron transport function. On the other hand, the charging device employs a charging device that includes a contact-type charging member that charges the surface of the photoreceptor and an AC voltage application unit that applies an AC voltage to the contact-type charging member. This allows the charging member to inject electrons into the surface of the photoreceptor, i.e., the inorganic protective layer. This also ensures the charging characteristics.

[0027] From the above, it is presumed that the image forming apparatus according to this embodiment has excellent electrical properties and abrasion resistance of the inorganic protective layer in the photoreceptor.

[0028] Next, the configuration of the image forming apparatus according to this embodiment will be described in detail.

[0029] The following is an example of an image forming apparatus according to this embodiment, but it is not limited to this example. The main parts shown in the figure will be described, and other parts will be omitted from the explanation.

[0030] Figure 1 is a schematic diagram showing an example of an image forming apparatus according to this embodiment. As shown in Figure 1, the image forming apparatus 10 according to this embodiment is provided with, for example, a photoreceptor 12. The photoreceptor 12 is cylindrical and is connected to a drive unit 27 such as a motor via a drive force transmission member (not shown) such as a gear, and is rotationally driven by the drive unit 27 around a rotation axis indicated by a black dot. In the example shown in Figure 1, it is rotationally driven in the direction of arrow A.

[0031] Around the photoreceptor 12, for example, a charging device 15 (an example of a charging device), an electrostatic image forming device 16 (an example of an electrostatic image forming device), a developing device 18 (an example of a developing device), a transfer device 31 (an example of a transfer device), a cleaning device 22 (an example of a cleaning device), and a static elimination device 24 are arranged in order along the rotational direction of the photoreceptor 12. The image forming apparatus 10 also includes a fixing device 26 having a fixing member 26A and a pressurizing member 26B positioned in contact with the fixing member 26A. The image forming apparatus 10 also has a control device 36 that controls the operation of each device (each part). The unit including the photoreceptor 12, charging device 15, electrostatic image forming device 16, developing device 18, transfer device 31, and cleaning device 22 corresponds to the image forming unit.

[0032] In the image forming apparatus 10, at least the photoreceptor 12 may be provided as a process cartridge integrated with other devices.

[0033] The details of each device (part) of the image forming apparatus 10 will be described below.

[0034] [Electrophotographic photoconductor] A photoreceptor has a photosensitive layer and an inorganic protective layer on a conductive substrate, in that order. The photosensitive layer may be a single-layer photosensitive layer that integrates the functions of a charge generating material and a charge transporting material within the same photosensitive layer, or it may be a multilayer photosensitive layer with separate functions having a charge generating layer and a charge transporting layer. When the photosensitive layer is a multilayer photosensitive layer, the order of the charge generation layer and the charge transport layer is not particularly limited, but it is preferable that the photoreceptor has a charge generation layer, a charge transport layer, and an inorganic protective layer in this order on a conductive substrate. The photoreceptor may also contain layers other than these.

[0035] Figure 5 is a schematic cross-sectional view showing an example of the layer configuration of a photoreceptor in an image forming apparatus according to this embodiment. The photoreceptor 107A shown in Figure 5 has a structure in which a base layer 101 is provided on a conductive substrate 104, and a charge generation layer 102, a charge transport layer 103, and an inorganic protective layer 106 are sequentially formed thereon. In the photoreceptor 107A, a photoreceptor layer 105 is configured in which the functions of the charge generation layer 102 and the charge transport layer 103 are separated.

[0036] Figure 6 is a schematic cross-sectional view showing another example of the layer configuration of a photoreceptor in an image forming apparatus according to this embodiment. The photoreceptor 107B shown in Figure 6 has a structure in which an undercoat layer 101 is provided on a conductive substrate 104, and a photosensitive layer 105 and an inorganic protective layer 106 are formed sequentially. In the photoreceptor 107B, a single-layer photosensitive layer is constructed in which a charge generating material and a charge transporting material are contained in the same photosensitive layer 105, integrating their functions. In this embodiment, the photoreceptor may or may not have an undercoat layer 101.

[0037] The details of the photoreceptor in this embodiment will be described below, but reference numerals will be omitted.

[0038] (Conductive substrate) Examples of conductive substrates include metal plates, metal drums, and metal belts containing metals (aluminum, copper, zinc, chromium, nickel, molybdenum, vanadium, indium, gold, platinum, etc.) or alloys (stainless steel, etc.). Other examples of conductive substrates include paper, resin films, and belts coated, vapor-deposited, or laminated with conductive compounds (e.g., conductive polymers, indium oxide, etc.), metals (e.g., aluminum, palladium, gold, etc.) or alloys. Here, "conductive" refers to a volume resistivity of 10⁻¹⁰. 13This refers to a value less than Ωcm.

[0039] When an electrophotographic photoreceptor is used in a laser printer, the surface of the conductive substrate is preferably roughened to a center-line average roughness Ra of 0.04 μm to 0.5 μm in order to suppress interference fringes that occur when irradiated with laser light. While roughening to prevent interference fringes is not particularly necessary when using non-interfering light as the light source, it is beneficial for extending the lifespan by suppressing the occurrence of defects due to surface irregularities of the conductive substrate.

[0040] Methods for roughening a surface include, for example, wet honing, which involves suspending an abrasive in water and spraying it onto a support; centerless grinding, which involves pressing a conductive substrate against a rotating grinding wheel and continuously grinding it; and anodizing.

[0041] One method for roughening the surface is to disperse conductive or semiconductive powder in a resin without roughening the surface of the conductive substrate, to form a layer on the surface of the conductive substrate, and then roughen the surface with the particles dispersed in that layer.

[0042] Anodizing roughening treatment involves forming an oxide film on the surface of a conductive substrate (e.g., aluminum) by anodizing it in an electrolyte solution. Examples of electrolyte solutions include sulfuric acid solution and oxalic acid solution. However, the porous anodic oxide film formed by anodizing is chemically active, easily contaminated, and exhibits large resistance fluctuations depending on the environment. Therefore, it is preferable to perform a sealing treatment on the porous anodic oxide film to block the micropores of the oxide film by volume expansion due to a hydration reaction using pressurized steam or boiling water (metal salts such as nickel may be added), thereby converting it into a more stable hydrated oxide.

[0043] The thickness of the anodic oxide film is preferably, for example, 0.3 μm to 15 μm. When the film thickness is within this range, it tends to exhibit barrier properties against injection and tends to suppress the increase in residual potential due to repeated use.

[0044] The conductive substrate may be subjected to a treatment with an acidic treatment liquid or a boehmite treatment. The treatment with an acidic treatment liquid is performed, for example, as follows. First, an acidic treatment liquid containing phosphoric acid, chromic acid and hydrofluoric acid is prepared. The mixing ratio of phosphoric acid, chromic acid and hydrofluoric acid in the acidic treatment liquid is, for example, in the range of 10 mass% to 11 mass% for phosphoric acid, 3 mass% to 5 mass% for chromic acid, and 0.5 mass% to 2 mass% for hydrofluoric acid, and the total concentration of these acids is preferably in the range of 13.5 mass% to 18 mass%. The treatment temperature is preferably, for example, 42°C to 48°C. The film thickness of the coating is preferably 0.3 μm to 15 μm.

[0045] The boehmite treatment is performed, for example, by immersing the substrate in pure water at 90°C to 100°C for 5 minutes to 60 minutes, or bringing the substrate into contact with heated steam at 90°C to 120°C for 5 minutes to 60 minutes. The film thickness of the coating is preferably 0.1 μm to 5 μm. This may further be subjected to an anodic oxidation treatment using an electrolyte solution with low coating solubility, such as adipic acid, boric acid, borate, phosphate, phthalate, maleate, benzoate, tartrate, and citrate.

[0046] (Undercoat layer) The undercoat layer is, for example, a layer containing inorganic particles and a binder resin.

[0047] Examples of the inorganic particles include inorganic particles having a powder resistance (volume resistivity) of 10 2 Ωcm to 10 11 Ωcm. Among these, as the inorganic particles having the above resistance value, metal oxide particles such as tin oxide particles, titanium oxide particles, zinc oxide particles, and zirconium oxide particles are preferable, and zinc oxide particles are particularly preferable.

[0048] The specific surface area of the inorganic particles measured by the BET method is preferably, for example, 10 m 2 / g or more. The volume average particle diameter of the inorganic particles is preferably, for example, 50 nm to 2000 nm (preferably 60 nm to 1000 nm).

[0049] The inorganic particle content is preferably 10% by mass or more and 80% by mass or less relative to the binder resin, and more preferably 40% by mass or more and 80% by mass or less.

[0050] The inorganic particles may be surface-treated. Two or more types of inorganic particles with different surface treatments or particle sizes may be mixed and used.

[0051] Examples of surface treatment agents include silane coupling agents, titanate-based coupling agents, aluminum-based coupling agents, and surfactants. Silane coupling agents are particularly preferred, and silane coupling agents having an amino group are more preferred.

[0052] Examples of silane coupling agents having an amino group include, but are not limited to, 3-aminopropyltriethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, and N,N-bis(2-hydroxyethyl)-3-aminopropyltriethoxysilane.

[0053] Silane coupling agents may be used in combination of two or more types. For example, a silane coupling agent having an amino group may be used in combination with another silane coupling agent. Examples of other silane coupling agents include, but are not limited to, vinyltrimethoxysilane, 3-methacrylateoxypropyl-tris(2-methoxyethoxy)silane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, vinyltriacetoxysilane, 3-mercaptopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N,N-bis(2-hydroxyethyl)-3-aminopropyltriethoxysilane, and 3-chloropropyltrimethoxysilane.

[0054] The surface treatment method using the surface treatment agent may be any known method, and may be either a dry or wet method.

[0055] The amount of surface treatment agent applied is preferably, for example, 0.5% by mass or more and 10% by mass or less relative to the inorganic particles.

[0056] In this case, it is preferable for the underlayer to contain electron-accepting compounds (acceptor compounds) along with inorganic particles, from the viewpoint of improving the long-term stability of electrical properties and carrier blocking ability.

[0057] Examples of electron-accepting compounds include quinone compounds such as chloranil and bromonil; tetracyanoquinodimethane compounds; fluorenone compounds such as 2,4,7-trinitrofluorenone and 2,4,5,7-tetranitro-9-fluorenone; oxadiazole compounds such as 2-(4-biphenyl)-5-(4-t-butylphenyl)-1,3,4-oxadiazole, 2,5-bis(4-naphthyl)-1,3,4-oxadiazole, and 2,5-bis(4-diethylaminophenyl)-1,3,4-oxadiazole; xanthone compounds; thiophene compounds; and diphenoquinone compounds such as 3,3',5,5'-tetra-t-butyldiphenoquinone; as well as other electron-transporting substances. In particular, compounds having an anthraquinone structure are preferred as electron-accepting compounds. Examples of compounds having an anthraquinone structure include hydroxyanthraquinone compounds, aminoanthraquinone compounds, and aminohydroxyanthraquinone compounds, and specifically, for example, anthraquinone, alizarin, quinizalin, anthralphine, and purpurin are preferred.

[0058] The electron-accepting compound may be dispersed in the underlayer together with inorganic particles, or it may be present attached to the surface of the inorganic particles.

[0059] Methods for attaching electron-accepting compounds to the surface of inorganic particles include, for example, dry methods or wet methods.

[0060] The dry method involves, for example, adding an electron-accepting compound, either directly or dissolved in an organic solvent, dropwise while stirring inorganic particles with a mixer that has a high shear force, or spraying it with dry air or nitrogen gas, to adhere the electron-accepting compound to the surface of the inorganic particles. When adding or spraying the electron-accepting compound, it is preferable to do so at a temperature below the boiling point of the solvent. After adding or spraying the electron-accepting compound, further baking at 100°C or higher may be performed. The baking temperature and time are not particularly limited as long as electrophotographic characteristics can be obtained.

[0061] The wet method involves dispersing inorganic particles in a solvent using methods such as stirring, ultrasound, sand milling, attritoring, and ball milling, while adding an electron-accepting compound. After stirring or dispersion, the solvent is removed to adhere the electron-accepting compound to the surface of the inorganic particles. Solvent removal methods include, for example, filtration or distillation. After solvent removal, further baking at 100°C or higher may be performed. The baking temperature and time are not particularly limited as long as electrophotographic characteristics can be obtained. In the wet method, the water content of the inorganic particles may be removed before adding the electron-accepting compound. Examples of this include removing water while stirring and heating in the solvent, or removing water by azeotrope with the solvent.

[0062] Furthermore, the attachment of the electron-accepting compound may be performed before or after surface treatment with a surface treatment agent on the inorganic particles, or it may be performed simultaneously with the attachment of the electron-accepting compound and surface treatment with the surface treatment agent.

[0063] The content of the electron-accepting compound is preferably, for example, 0.01% by mass or more and 20% by mass or less relative to the inorganic particles, and more preferably 0.01% by mass or more and 10% by mass or less.

[0064] Examples of known polymer compounds used as the binder resin for the undercoat include acetal resin (e.g., polyvinyl butyral), polyvinyl alcohol resin, polyvinyl acetal resin, casein resin, polyamide resin, cellulose resin, gelatin, polyurethane resin, polyester resin, unsaturated polyester resin, methacrylic resin, acrylic resin, polyvinyl chloride resin, polyvinyl acetate resin, vinyl chloride-vinyl acetate-maleic anhydride resin, silicone resin, silicone-alkyd resin, urea resin, phenol resin, phenol-formaldehyde resin, melamine resin, urethane resin, alkyd resin, epoxy resin, zirconium chelate compounds, titanium chelate compounds, aluminum chelate compounds, titanium alkoxide compounds, organic titanium compounds, and silane coupling agents. Examples of binder resins used in the undercoat include charge-transporting resins having charge-transporting groups, conductive resins (e.g., polyaniline), and the like.

[0065] Among these, a resin insoluble in the coating solvent of the upper layer is preferred as the binder resin used for the undercoat layer. In particular, a resin obtained by the reaction of a curing agent with at least one resin selected from the group consisting of thermosetting resins such as urea resin, phenol resin, phenol-formaldehyde resin, melamine resin, urethane resin, unsaturated polyester resin, alkyd resin, and epoxy resin is preferred. When using two or more of these binder resins in combination, the mixing ratio is set as needed.

[0066] The undercoat may contain various additives to improve electrical properties, environmental stability, and image quality. Examples of known additives include electron-transporting pigments such as polycyclic condensation and azo pigments, zirconium chelate compounds, titanium chelate compounds, aluminum chelate compounds, titanium alkoxide compounds, organic titanium compounds, and silane coupling agents. As mentioned above, silane coupling agents are used for surface treatment of inorganic particles, but they may also be added to the undercoat as additives.

[0067] Examples of silane coupling agents used as additives include vinyltrimethoxysilane, 3-methacrylateoxypropyl-tris(2-methoxyethoxy)silane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, vinyltriacetoxysilane, 3-mercaptopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N,N-bis(2-hydroxyethyl)-3-aminopropyltriethoxysilane, and 3-chloropropyltrimethoxysilane.

[0068] Examples of zirconium chelate compounds include zirconium butoxide, ethyl zirconium acetate, zirconium triethanolamine, acetylacetonate zirconium butoxide, ethyl acetate zirconium butoxide, zirconium acetate, zirconium oxalate, zirconium lactate, zirconium phosphonate, zirconium octanoate, zirconium naphthenate, zirconium laurate, zirconium stearate, zirconium isostearate, methacrylate zirconium butoxide, stearate zirconium butoxide, and isostearate zirconium butoxide.

[0069] Examples of titanium chelate compounds include tetraisopropyl titanate, tetran-butyl titanate, butyl titanate dimer, tetra(2-ethylhexyl) titanate, titanium acetylacetonate, polytitanium acetylacetonate, titanium octylene glycolate, titanium lactate ammonium salt, titanium lactate, titanium lactate ethyl ester, titanium triethanolamine, and polyhydroxytitanium stearate.

[0070] Examples of aluminum chelating compounds include aluminum isopropylate, monobutoxyaluminum diisopropylate, aluminum butyrate, diethylacetoacetate aluminum diisopropylate, and aluminum tris(ethylacetoacetate).

[0071] These additives may be used individually or as a mixture or polycondensate of multiple compounds.

[0072] The underlayer should ideally have a Vickers hardness of 35 or higher. The surface roughness (ten-point average roughness) of the undercoat layer should be adjusted to between 1 / (4n) (where n is the refractive index of the upper layer) and 1 / 2 of the exposure laser wavelength λ used, in order to suppress moiré patterns. Resin particles may be added to the undercoat to adjust the surface roughness. Examples of resin particles include silicone resin particles and cross-linked polymethyl methacrylate resin particles. The surface of the undercoat may also be polished to adjust the surface roughness. Polishing methods include buffing, sandblasting, wet honing, and grinding.

[0073] There are no particular restrictions on the formation of the undercoat, and well-known formation methods can be used. For example, it can be carried out by forming a coating film of an undercoat-forming solution obtained by adding the above components to a solvent, drying the coating film, and heating it if necessary.

[0074] Solvents for preparing the coating solution for forming the undercoat include known organic solvents such as alcohol-based solvents, aromatic hydrocarbon solvents, halogenated hydrocarbon solvents, ketone-based solvents, ketone alcohol-based solvents, ether-based solvents, and ester-based solvents. Specific examples of these solvents include common organic solvents such as methanol, ethanol, n-propanol, iso-propanol, n-butanol, benzyl alcohol, methyl cellsolve, ethyl cellsolve, acetone, methyl ethyl ketone, cyclohexanone, methyl acetate, ethyl acetate, n-butyl acetate, dioxane, tetrahydrofuran, methylene chloride, chloroform, chlorobenzene, and toluene.

[0075] Known methods for dispersing inorganic particles when preparing a coating solution for forming an undercoat include, for example, roll mills, ball mills, vibrating ball mills, attritors, sand mills, colloid mills, and paint shakers.

[0076] Conventional methods for applying the undercoating solution onto a conductive substrate include, for example, the blade coating method, wire bar coating method, spray coating method, immersion coating method, bead coating method, air knife coating method, and curtain coating method.

[0077] The thickness of the undercoat layer is preferably set to a range of 15 μm or more, and more preferably 20 μm to 50 μm.

[0078] (Middle class) Although not shown in the diagram, an intermediate layer may be further provided between the undercoat layer and the photosensitive layer. The intermediate layer is, for example, a layer containing a resin. Examples of resins that can be used in the intermediate layer include polymer compounds such as acetal resin (e.g., polyvinyl butyral), polyvinyl alcohol resin, polyvinyl acetal resin, casein resin, polyamide resin, cellulose resin, gelatin, polyurethane resin, polyester resin, methacrylic resin, acrylic resin, polyvinyl chloride resin, polyvinyl acetate resin, vinyl chloride-vinyl acetate-maleic anhydride resin, silicone resin, silicone-alkyd resin, phenol-formaldehyde resin, and melamine resin. The intermediate layer may contain an organometallic compound. Examples of organometallic compounds used in the intermediate layer include those containing metal atoms such as zirconium, titanium, aluminum, manganese, and silicon. The compounds used in these intermediate layers may be used individually, as a mixture of multiple compounds, or as polycondensates.

[0079] Among these, the intermediate layer is preferably a layer containing an organometallic compound that contains zirconium atoms or silicon atoms.

[0080] There are no particular restrictions on the formation of the intermediate layer, and well-known formation methods can be used. For example, it can be carried out by forming a coating film of an intermediate layer-forming coating solution obtained by adding the above components to a solvent, drying the coating film, and heating it if necessary. Conventional methods such as immersion coating, push-up coating, wire bar coating, spray coating, blade coating, knife coating, and curtain coating are used to form the intermediate layer.

[0081] The thickness of the intermediate layer is preferably set to a range of 0.1 μm to 3 μm, for example. The intermediate layer may also be used as a base layer.

[0082] (Charge generation layer) The charge generation layer is, for example, a layer containing a charge generation material and a binder resin. Alternatively, the charge generation layer may be a vapor-deposited layer of the charge generation material. A vapor-deposited layer of the charge generation material is suitable when using non-coherent light sources such as LEDs (Light Emitting Diodes) or organic EL (Electro-Luminescence) image arrays.

[0083] Examples of charge-generating materials include azo pigments such as bisazo and trisazo; fused aromatic pigments such as dibromoanthonthrone; perylene pigments; pyrrolopyrrole pigments; phthalocyanine pigments; zinc oxide; and trigonal selenium.

[0084] Among these, in order to accommodate laser exposure in the near-infrared region, it is preferable to use a metal phthalocyanine pigment or a metal-free phthalocyanine pigment as the charge generating material. Specifically, for example, hydroxygallium phthalocyanine; chlorogallium phthalocyanine; dichlorotin phthalocyanine; and titanyl phthalocyanine are more preferable.

[0085] On the other hand, to accommodate laser exposure in the near-ultraviolet region, preferred charge-generating materials include fused aromatic pigments such as dibromoanthoten; thioindigo pigments; porphyrazine compounds; zinc oxide; trigonal selenium; and bisazo pigments.

[0086] Even when using non-coherent light sources such as LEDs and organic EL image arrays with a central emission wavelength between 450 nm and 780 nm, the above charge generating materials may be used. However, from the viewpoint of resolution, when using a thin film of 20 μm or less for the photosensitive layer, the electric field strength in the photosensitive layer becomes high, making it easier for charge reduction due to charge injection from the substrate to occur, resulting in image defects known as black spots. This is particularly noticeable when using charge generating materials that are p-type semiconductors that easily generate dark current, such as trigonal selenium and phthalocyanine pigments.

[0087] In contrast, when n-type semiconductors such as fused aromatic pigments, perylene pigments, and azo pigments are used as charge-generating materials, dark currents are less likely to occur, and image defects called black spots can be suppressed even in thin films. Furthermore, the n-type is determined using the commonly used time-of-flight method, based on the polarity of the photocurrent that flows. Those that are more likely to carry electrons as carriers than holes are classified as n-type.

[0088] The binder resin used in the charge generation layer can be selected from a wide range of insulating resins, or it may be selected from organic photoconductive polymers such as poly-N-vinylcarbazole, polyvinylanthracene, polyvinylpyrene, and polysilane. Examples of binder resins include polyvinyl butyral resin, polyarylate resin (polycondensate of bisphenols and aromatic divalent carboxylic acids, etc.), polycarbonate resin, polyester resin, phenoxy resin, vinyl chloride-vinyl acetate copolymer, polyamide resin, acrylic resin, polyacrylamide resin, polyvinylpyridine resin, cellulose resin, urethane resin, epoxy resin, casein, polyvinyl alcohol resin, and polyvinylpyrrolidone resin. Here, "insulating properties" refers to a volume resistivity of 10 13 This refers to a value of Ωcm or greater. These binder resins can be used individually or in combination of two or more types.

[0089] Furthermore, the mixing ratio of the charge-generating material to the binder resin is preferably within the range of 10:1 to 1:10 by mass ratio.

[0090] The charge generation layer may also contain other well-known additives.

[0091] The formation of the charge generation layer is not particularly limited, and well-known formation methods can be used. For example, it can be carried out by forming a coating film of a charge generation layer forming solution obtained by adding the above components to a solvent, drying the coating film, and heating it as necessary. The charge generation layer may also be formed by vapor deposition of the charge generation material. Formation of the charge generation layer by vapor deposition is particularly suitable when using fused aromatic pigments or perylene pigments as the charge generation material.

[0092] Solvents for preparing the coating solution for forming the charge generation layer include methanol, ethanol, n-propanol, n-butanol, benzyl alcohol, methyl cellsolve, ethyl cellsolve, acetone, methyl ethyl ketone, cyclohexanone, methyl acetate, n-butyl acetate, dioxane, tetrahydrofuran, methylene chloride, chloroform, chlorobenzene, and toluene. These solvents may be used individually or in mixtures of two or more.

[0093] Methods for dispersing particles (e.g., charge-generating materials) in a coating solution for forming a charge-generating layer include, for example, media dispersers such as ball mills, vibrating ball mills, attritors, sand mills, and horizontal sand mills, as well as media-less dispersers such as stirrers, ultrasonic dispersers, roll mills, and high-pressure homogenizers. Examples of high-pressure homogenizers include collision methods, which disperse the dispersion by causing liquid-liquid collisions or liquid-wall collisions under high pressure, and penetration methods, which disperse the dispersion by penetrating fine channels under high pressure. Furthermore, during this dispersion, it is effective to set the average particle size of the charge-generating material in the coating solution for forming the charge-generating layer to 0.5 μm or less, preferably 0.3 μm or less, and more preferably 0.15 μm or less.

[0094] Conventional methods for applying the charge-generating layer forming coating solution onto the undercoat (or intermediate layer) include, for example, the blade coating method, wire bar coating method, spray coating method, immersion coating method, bead coating method, air knife coating method, and curtain coating method.

[0095] The thickness of the charge generation layer is preferably set to a range of 0.1 μm to 5.0 μm, more preferably 0.2 μm to 2.0 μm.

[0096] (charge transport layer) The charge transport layer is, for example, a layer containing a charge transport material and a binder resin. The charge transport layer may also contain a polymer charge transport material.

[0097] Examples of charge transport materials include quinone compounds such as p-benzoquinone, chloranil, bromanil, and anthraquinone; tetracyanoquinodimethane compounds; fluorenone compounds such as 2,4,7-trinitrofluorenone; xanthone compounds; benzophenone compounds; cyanovinyl compounds; and ethylene compounds, which are electron transport compounds. Other examples of charge transport materials include hole transport compounds such as triarylamine compounds, benzidine compounds, arylalkane compounds, aryl-substituted ethylene compounds, stilbene compounds, anthracene compounds, and hydrazone compounds. These charge transport materials may be used individually or in combination of two or more, but are not limited to these.

[0098] As charge transport materials, from the viewpoint of charge mobility, the triarylamine derivative shown in the following structural formula (a-1) and the benzidine derivative shown in the following structural formula (a-2) are preferred.

[0099] [ka]

[0100] In structural formula (a-1), Ar T1 Ar T2 , and Ar T3 Each is independently a substituted or unsubstituted aryl group, -C6H4-C(R T4 )=C(R T5 )(R T6 ), or -C6H4-CH=CH-CH=C(R T7 )(R T8 ) indicates RT4 , R T5 , R T6 , R T7 , and R T8 Each of these independently represents a hydrogen atom, a substituted or unsubstituted alkyl group, or a substituted or unsubstituted aryl group. Substituents for each of the above groups include halogen atoms, alkyl groups having 1 to 5 carbon atoms, and alkoxy groups having 1 to 5 carbon atoms. Furthermore, substituted amino groups substituted with alkyl groups having 1 to 3 carbon atoms are also examples of substituents for each of the above groups.

[0101] [ka]

[0102] In structural formula (a-2), R T91 and R T92 Each of these independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 5 carbon atoms, or an alkoxy group having 1 to 5 carbon atoms. T101 , R T102 , R T111 and R T112 Each of these independently consists of a halogen atom, an alkyl group having 1 to 5 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, an amino group substituted with an alkyl group having 1 to 2 carbon atoms, a substituted or unsubstituted aryl group, and -C(R T12 )=C(R T13 )(R T14 ), or -CH=CH-CH=C(R T15 )(R T16 ) shows R T12 , R T13 , R T14 , R T15 and R T16 Each of these independently represents a hydrogen atom, a substituted or unsubstituted alkyl group, or a substituted or unsubstituted aryl group. Tm1, Tm2, ​​Tn1, and Tn2 each independently represent an integer between 0 and 2. Substituents for each of the above groups include halogen atoms, alkyl groups having 1 to 5 carbon atoms, and alkoxy groups having 1 to 5 carbon atoms. Furthermore, substituted amino groups substituted with alkyl groups having 1 to 3 carbon atoms are also examples of substituents for each of the above groups.

[0103] Here, among the triarylamine derivative represented by structural formula (a-1) and the benzidine derivative represented by structural formula (a-2), in particular, "-C6H4-CH=CH-CH=C(R T7 )(R T8 Triarylamine derivatives having ")" and "-CH=CH-CH=C(R T15 )(R T16 A benzidine derivative having ) is preferred from the viewpoint of charge mobility.

[0104] As polymer charge transport materials, known charge transport materials such as poly-N-vinylcarbazole and polysilane can be used. Polyester-based polymer charge transport materials are particularly preferred. Polymer charge transport materials may be used alone or in combination with a binder resin.

[0105] Examples of binder resins used in the charge transport layer include polycarbonate resin, polyester resin, polyarylate resin, methacrylic resin, acrylic resin, polyvinyl chloride resin, polyvinylidene chloride resin, polystyrene resin, polyvinyl acetate resin, styrene-butadiene copolymer, vinylidene chloride-acrylonitrile copolymer, vinyl chloride-vinyl acetate copolymer, vinyl chloride-vinyl acetate-maleic anhydride copolymer, silicone resin, silicone alkyd resin, phenol-formaldehyde resin, styrene-alkyd resin, poly-N-vinylcarbazole, and polysilane. Among these, polycarbonate resin or polyarylate resin is preferred as the binder resin. These binder resins can be used individually or in combination of two or more. The preferred mixing ratio of the charge transport material to the binder resin is between 10:1 and 1:5 by mass.

[0106] Among the above-mentioned binder resins, polycarbonate resins (monopolymers of bisphenol A, bisphenol Z, bisphenol C, bisphenol TP, etc., or copolymers thereof) are preferred because they more easily reduce the surface roughness of the charge transport layer and more effectively suppress the occurrence of image flow. One type of polycarbonate resin may be used alone, or two or more types may be used in combination. Similarly, among the polycarbonate resins, it is more preferable to include a monopolymerized polycarbonate resin of bisphenol Z.

[0107] The charge transport layer may contain inorganic particles in addition to the charge transport material and binder resin, as needed. The inclusion of inorganic particles in the charge transport layer (i.e., the outermost layer of the organic photosensitive layer) suppresses cracking of the inorganic protective layer. Specifically, by incorporating inorganic particles into the layer that constitutes the surface of the organic photosensitive layer, the inorganic particles function as a reinforcing material for the organic photosensitive layer, making the organic photosensitive layer less prone to deformation and thus suppressing cracking of the inorganic protective layer. Furthermore, the inclusion of inorganic particles in the charge transport layer (i.e., the organic photosensitive layer) makes dielectric breakdown of the charge transport layer (i.e., the organic photosensitive layer) less likely to occur even at high electric field strengths.

[0108] Inorganic particles used in the charge transport layer include silica particles, alumina particles, titanium oxide particles, potassium titanate, tin oxide particles, zinc oxide particles, zirconium oxide particles, barium sulfate particles, calcium oxide particles, calcium carbonate particles, and magnesium oxide particles. Inorganic particles may be used individually or in combination of two or more types. Among these, silica particles are particularly preferred because they have a high dielectric loss rate, are less likely to reduce the electrical properties of the photoreceptor, and suppress the occurrence of cracking in the inorganic protective layer. The following describes in detail the silica particles suitable for charge transport layers.

[0109] Examples of silica particles include dry silica particles and wet silica particles. Examples of dry silica particles include fumed silica obtained by burning silane compounds, and deflagration silica obtained by explosively burning metallic silicon powder. Examples of wet silica particles include wet silica particles obtained by the neutralization reaction of sodium silicate and mineral acid (sedimentation silica synthesized and aggregated under alkaline conditions, gel silica particles synthesized and aggregated under acidic conditions, etc.), colloidal silica particles obtained by polymerizing acidic silicic acid in an alkaline state (silica sol particles, etc.), and sol-gel silica particles obtained by hydrolysis of organosilane compounds (e.g., alkoxysilanes, etc.). Among these, combustion-processed silica particles are preferable because they have fewer silanol groups on the surface and a low void structure, from the viewpoint of suppressing image defects due to the generation of residual potential and deterioration of other electrical properties (suppression of deterioration of fine line reproducibility).

[0110] It is preferable that the silica particles have their surfaces treated with a hydrophobic treatment agent. This reduces the number of silanol groups on the surface of the silica particles, making it easier to suppress the generation of residual potential. Examples of hydrophobic treatment agents include well-known silane compounds such as chlorosilanes, alkoxysilanes, and silazanes. Among these, silane compounds having a trimethylsilyl group, a decylsilyl group, or a phenylsilyl group are preferred as hydrophobic treatment agents, from the viewpoint of easily suppressing the generation of residual potential and suppressing image density unevenness caused by charging unevenness on the photoreceptor surface. In other words, it is preferable for the surface of silica particles to have a trimethylsilyl group, a decylsilyl group, or a phenylsilyl group. Examples of silane compounds containing a trimethylsilyl group (trimethylsilane compounds) include trimethylchlorosilane, trimethylmethoxysilane, and 1,1,1,3,3,3-hexamethyldisilazane. Examples of silane compounds containing a decylsilyl group (decylsilane compounds) include decyltrichlorosilane, decyldimethylchlorosilane, and decyltrimethoxysilane. Examples of silane compounds containing a phenyl group (phenylsilane compounds) include triphenylmethoxysilane and triphenylchlorosilane.

[0111] Condensation rate of hydrophobized silica particles (SiO in silica particles) 4- The ratio of Si-O-Si in the bonding (hereinafter also referred to as the "condensation rate of the hydrophobic treatment agent") is, for example, 90% or more relative to the silanol groups on the surface of the silica particles, preferably 91% or more, and more preferably 95% or more. By setting the condensation rate of the hydrophobic treatment agent within the above range, the silanol groups of the silica particles are further reduced, making it easier to suppress the generation of residual potential.

[0112] The condensation rate of the hydrophobic treatment agent indicates the ratio of condensed silicon to all bondable silicon sites in the condensation region detected by NMR (Nuclear Magnetic Resonance), and is measured as follows. First, silica particles are separated from the layer. Si CP / MAS NMR analysis is performed on the separated silica particles using a Bruker AVANCE III 400 to determine the peak area corresponding to the number of SiO substitutions. The values ​​for 2-substituted (Si(OH)2(0-Si)2-), 3-substituted (Si(OH)(0-Si)3-), and 4-substituted (Si(0-Si)4-) are defined as Q2, Q3, and Q4, respectively. The condensation ratio of the hydrophobic treatment agent is calculated using the formula: (Q2×2+Q3×3+Q4×4) / 4×(Q2+Q3+Q4).

[0113] The volume resistivity of silica particles is, for example, 10 11 Ω·cm or more is preferable, preferably 10 12 Ω·cm or more, more preferably 10 13 It is greater than or equal to Ω·cm. By keeping the volume resistivity of the silica particles within the above range, the deterioration of electrical properties is suppressed.

[0114] The volume resistivity of silica particles is measured as follows. The measurement environment is set to a temperature of 20°C and a humidity of 50% RH. First, separate the silica particles from the layer. Then, 20 cm2 On the surface of a circular jig on which electrode plates are arranged, the separated silica particles to be measured are placed to a thickness of approximately 1 mm to 3 mm to form a silica particle layer. A 20 cm layer is then placed on top of this, as described above. 2 An electrode plate is placed on top of the silica particle layer, sandwiching it between the two plates. To eliminate the gaps between the silica particles, a 4 kg load is applied to the electrode plate placed on the silica particle layer, and then the thickness (cm) of the silica particle layer is measured. Both electrodes, above and below the silica particle layer, are connected to an electrometer and a high-voltage power generator. A high voltage is applied to both electrodes so that the electric field reaches a predetermined value, and the volume resistivity (Ω·cm) of the silica particles is calculated by reading the current value (A) that flows at this time. The formula for calculating the volume resistivity (Ω·cm) of silica particles is as shown in the formula below. In the formula, ρ represents the volume resistivity of the silica particles (Ω·cm), E represents the applied voltage (V), I represents the current value (A), I0 represents the current value at an applied voltage of 0V (A), and L represents the thickness of the silica particle layer (cm). In this evaluation, the volume resistivity at an applied voltage of 1000V was used. Formula: ρ = E × 20 / (I - I0) / L

[0115] The volume-average particle size of the inorganic particles containing silica particles is, for example, 20 nm to 200 nm, preferably 40 nm to 150 nm, more preferably 50 nm to 120 nm, and even more preferably 50 nm to 110 nm. When the volume-average particle size is within the above range, cracking of the inorganic protective layer and the generation of residual potential are more easily suppressed.

[0116] The volume-average particle size of inorganic particles is measured as follows. The measurement method for silica particles is shown below, but a similar method is used for other particles. The volume-average particle size of silica particles is determined by separating the silica particles from the layer, observing 100 primary silica particles at 40,000x magnification using a Scanning Electron Microscope (SEM), and measuring the longest and shortest diameters of each particle through image analysis. The equivalent spherical diameter is then calculated from the midpoint of these two values. The 50% diameter (D50v) at the cumulative frequency of the obtained equivalent spherical diameters is determined and measured as the volume-average particle size of the silica particles.

[0117] The amount of inorganic particles can be determined appropriately depending on their type, but in terms of suppressing cracking of the inorganic protective layer and the generation of residual potential, it is preferable that the amount be, for example, 30% by mass or more, more preferably 40% by mass or more, even more preferably 50% by mass or more, and particularly preferable to be 55% by mass or more relative to the total charge transport layer (solid content). Furthermore, while there is no particular upper limit to the inorganic particle content, from the standpoint of ensuring the characteristics of the charge transport layer, it is preferable to have 90% by mass or less, more preferably 80% by mass or less, more preferably 70% by mass or less, and even more preferably 65% ​​by mass or less. Furthermore, the inorganic particle content is preferably greater than the charge transport material content, for example, it is preferably 55% by mass or more and 90% by mass or less relative to the entire charge transport layer (solid content).

[0118] The charge transport layer may also contain other well-known additives.

[0119] -Characteristics of the charge transport layer- The surface roughness Ra (arithmetic mean surface roughness Ra) of the inorganic protective layer side of the charge transport layer is, for example, 0.06 μm or less, preferably 0.03 μm or less, and more preferably 0.02 μm or less. Setting the surface roughness Ra within the above range improves the smoothness of the inorganic protective layer and enhances its cleanability. To achieve a surface roughness Ra within the above range, methods such as increasing the thickness of the layer can be used.

[0120] This surface roughness Ra is measured as follows: First, the inorganic protective layer is removed to expose the layer to be measured. Then, a portion of that layer is cut out using a cutter or similar tool to obtain the sample for measurement. The surface roughness of this sample will be measured using a stylus-type surface roughness analyzer (e.g., Surfcom 1400A, manufactured by Tokyo Seimitsu Co., Ltd.). The measurement conditions will conform to JIS B0601-1994, with an evaluation length Ln = 4 mm, a reference length L = 0.8 mm, and a cutoff value of 0.8 mm.

[0121] The elastic modulus of the charge transport layer is, for example, 5 GPa or higher, preferably 6 GPa or higher, and more preferably 6.5 GPa or higher. If the elastic modulus of the charge transport layer is within the above range, cracking of the inorganic protective layer becomes easier to suppress. To achieve the elastic modulus of the charge transport layer within the above range, for example, methods such as adjusting the particle size and content of silica particles, or adjusting the type and content of charge transport material, can be used.

[0122] The elastic modulus of the charge transport layer is measured as follows: First, the inorganic protective layer is removed to expose the layer to be measured. Then, a portion of that layer is cut out using a cutter or similar tool to obtain the sample for measurement. For this sample, a depth profile is obtained using the continuous stiffness method (CSM) (U.S. Patent 4848141) with the Nano Indenter SA2 manufactured by MTS Systems, and the measurement is performed using the average value obtained from the indentation depth measurements from 30 nm to 100 nm.

[0123] The thickness of the charge transport layer is, for example, 10 μm to 40 μm, preferably 10 μm to 35 μm, and more preferably 15 μm to 30 μm. By keeping the thickness of the charge transport layer within the above range, cracking of the inorganic protective layer and the generation of residual potential become easier to suppress.

[0124] -Formation of a charge transport layer- The formation of the charge transport layer is not particularly limited, and well-known formation methods can be used. For example, it can be carried out by forming a coating film of a charge transport layer forming solution obtained by adding the above components to a solvent, drying the coating film, and heating it if necessary.

[0125] Suitable solvents for preparing the coating solution for forming the charge transport layer include common organic solvents such as aromatic hydrocarbons like benzene, toluene, xylene, and chlorobenzene; ketones like acetone and 2-butanone; halogenated aliphatic hydrocarbons like methylene chloride, chloroform, and ethylene chloride; and cyclic or linear ethers like tetrahydrofuran and ethyl ether. These solvents can be used individually or in mixtures of two or more.

[0126] Conventional methods for applying a charge transport layer forming coating solution onto a charge generation layer include blade coating, wire bar coating, spray coating, immersion coating, bead coating, air knife coating, and curtain coating.

[0127] When dispersing particles (e.g., silica particles or fluororesin particles) in a coating solution for forming a charge transport layer, the dispersion method may involve media dispersers such as ball mills, vibrating ball mills, attritors, sand mills, and horizontal sand mills, or media-less dispersers such as stirrers, ultrasonic dispersers, roll mills, and high-pressure homogenizers. Examples of high-pressure homogenizers include impact methods, which disperse the dispersion by causing liquid-liquid collisions or liquid-wall collisions under high pressure, and penetration methods, which disperse the dispersion by penetrating fine channels under high pressure.

[0128] Furthermore, after the formation of the charge transport layer and before the formation of the inorganic protective layer, if necessary, a step may be taken to replace the air contained in the organic photosensitive layer formed on the conductive substrate with a gas with a higher oxygen concentration than the air.

[0129] (Inorganic protective layer) -Composition of the inorganic protective layer- The inorganic protective layer has a surface layer that contains metal elements M, oxygen O, and hydrogen H. In other words, the surface layer of the inorganic protective layer is composed of an inorganic material containing metal elements M, oxygen O, and hydrogen H. Furthermore, the elemental composition ratio (oxygen O / metal element M) of oxygen O to metal element M in the layer constituting the surface of the inorganic protective layer is between 1.3 and 1.5. The inorganic protective layer may consist of a single layer of layers constituting the surface of the inorganic protective layer, wherein the elemental composition ratio of oxygen O to metal element M (oxygen O / metal element M) is 1.3 or more and 1.5 or less, or it may consist of a laminate including the layers constituting the surface of the inorganic protective layer. However, from the viewpoint of improving electrical properties, the inorganic protective layer is preferably composed of a single layer of the layer constituting the surface of the inorganic protective layer, in which the elemental composition ratio of oxygen O to metal element M (oxygen O / metal element M) is 1.3 or more and 1.5 or less.

[0130] Examples of metal elements M in the layers constituting the surface of the inorganic protective layer include elements from Group 13. Group 13 elements include boron, aluminum, gallium, and indium. Among these, from the viewpoint of electrical properties and wear resistance of the inorganic protective layer in the photoreceptor, Group 13 elements are preferred as the metal element M, and gallium is more preferred.

[0131] The elemental composition ratio (oxygen O / metal element M) of oxygen O to metal element M in the layer constituting the surface of the inorganic protective layer is 1.3 or more and 1.5 or less, but from the viewpoint of electrical properties in the photoreceptor and wear resistance of the inorganic protective layer, 1.4 or more and 1.5 or less is preferred, and 1.46 or more and 1.5 or less is more preferred. On the other hand, the elemental composition ratio (oxygen O / metal element M) of oxygen O to metal element M in the layer constituting the surface of the inorganic protective layer is more preferably 1.3 or more and 1.5 or less, from the viewpoint of suppressing peeling of the inorganic protective layer.

[0132] In the layer constituting the surface of the inorganic protective layer, the sum of the elemental composition ratios of metal element M, oxygen O, and hydrogen H relative to all elements constituting the layer constituting the surface of the inorganic protective layer is preferably 90% or more, more preferably 95%, and more preferably 98%, from the viewpoint of electrical properties in the photoreceptor and wear resistance of the inorganic protective layer.

[0133] In addition to the inorganic material mentioned above, the layer constituting the surface of the inorganic protective layer may contain, for example, one or more elements selected from C, Si, Ge, and Sn in the case of n-type, for control of conductivity. Alternatively, for example, in the case of p-type, it may contain one or more elements selected from N, Be, Mg, Ca, and Sr.

[0134] Here, when the layer constituting the surface of the inorganic protective layer is composed of metal elements M, oxygen O, and hydrogen H, the preferred elemental composition ratios for the photoreceptor, from the viewpoint of excellent electrical properties and wear resistance of the inorganic protective layer, are as follows. The elemental composition ratio of metal element M is, for example, often 15 atomic% to 50 atomic% of the total constituent elements of the inorganic protective layer, preferably 20 atomic% to 40 atomic% and more preferably 20 atomic% to 3 atomic%. The elemental composition ratio of oxygen (O) is, for example, often 30 to 70 atomic percent of the total constituent elements of the inorganic protective layer, preferably 40 to 60 atomic percent, and more preferably 45 to 55 atomic percent. The elemental composition ratio of hydrogen (H) is, for example, often 10 to 40 atomic percent relative to the total constituent elements of the inorganic protective layer, preferably 15 to 35 atomic percent, and more preferably 20 to 30 atomic percent.

[0135] When the inorganic protective layer is composed of a laminate, from the viewpoint of improving the electrical properties of the photoreceptor, the elemental composition ratio of oxygen O to metal element M (oxygen O / metal element M) in the layer below the layer constituting the surface of the inorganic protective layer is preferably 1.2 or more and less than 1.3. The layer beneath the surface layer of the inorganic protective layer should have the same composition as the layer constituting the surface layer of the inorganic protective layer, except for the elemental composition ratio of oxygen (O) to metal element (M) (oxygen O / metal element M).

[0136] The elemental composition ratios and atomic number ratios of each element in the inorganic protective layer, including their distribution in the thickness direction, are determined by Rutherford back scattering (hereinafter referred to as "RBS"). For RBS, the NEC 3SDH Pelletron will be used as the accelerator, the CE&A RBS-400 as the end station, and the 3S-R10 as the system. CE&A's HYPRA program and other software will be used for analysis. The measurement conditions for RBS are as follows: He++ ion beam energy of 2.275 eV, detection angle of 160°, and grazing angle of approximately 109° relative to the incident beam.

[0137] RBS measurement is performed as follows: First, a He++ ion beam is incident perpendicularly on the sample, and the detector is set at 160° to the ion beam to measure the signal of backscattered He. The composition ratio and film thickness are determined from the detected He energy and intensity. To improve the accuracy of determining the composition ratio and film thickness, spectra may be measured at two detection angles. Accuracy can be improved by measuring at two detection angles with different depth resolution and backscatter dynamics and cross-checking the results. The number of He atoms backscattered by the target atom is determined by only three factors: 1) the atomic number of the target atom, 2) the energy of the He atoms before scattering, and 3) the scattering angle. The density is assumed by calculation from the measured composition and used to calculate the thickness. The density error is within 20%.

[0138] The elemental composition ratio of hydrogen is determined by hydrogen forward scattering (hereinafter referred to as "HFS"). For HFS measurements, the NEC 3SDH Pelletron accelerator and the CE&A RBS-400 end station are used, along with the 3S-R10 system. The CE&A HYPRA program is used for analysis. The HFS measurement conditions are as follows: He++ ion beam energy: 2.275 eV • Detection angle: 160° relative to the incident beam; Grazing angle: 30°

[0139] HFS measurement involves setting the detector at a 30° angle to the He++ ion beam and the sample at a 75° angle from the normal, thereby picking up the hydrogen signal scattered in front of the sample. It is advisable to cover the detector with aluminum foil to remove He atoms scattered along with the hydrogen. Quantitative analysis is performed by normalizing the hydrogen counts of the reference sample and the sample under test using their stopping power, and then comparing them. A sample of Si with H ion implanted and muscovite are used as reference samples. Muscovite is known to have a hydrogen concentration of 6.5 atomic percent. The amount of hydrogen adsorbed on the outermost surface is corrected by subtracting, for example, the amount of hydrogen adsorbed on a clean Si surface.

[0140] Furthermore, the inorganic protective layer may have a distribution of compositional ratios in the thickness direction, or it may consist of multiple layers, depending on the purpose.

[0141] -Characteristics of the inorganic protective layer- The light transmittance of the inorganic protective layer is preferably 90% or higher, and more preferably 95%. When the light transmittance of the inorganic protective layer is within the above range, the electrical properties are improved. The light transmittance of the inorganic protective layer is measured as follows: First, a sample is collected by simultaneously forming an inorganic protective layer on quartz glass while depositing the protective layer on the photoreceptor to be measured. Light transmittance is measured for samples of an inorganic protective layer on quartz glass using a spectrophotometer (Shimadzu UV-26000). The volume resistivity of the inorganic protective layer is 5.0 × 10⁻⁶.9 Ωcm or greater: 1.0 × 10 13 A value less than Ωcm is preferable. The volume resistivity of the inorganic protective layer should be 8.0 × 10⁻⁶ in terms of improving electrical properties. 10 Ωcm or more, 7.0× 12 Less than 1 cm is preferable.

[0142] This volume resistivity is calculated based on the electrode area and sample thickness from the resistance value measured using an nF Corporation LCR meter ZM2371 under conditions of a frequency of 100 Hz and a voltage of 1 V. The measurement sample may be a sample obtained by forming a film on an aluminum substrate under the same conditions as when the inorganic protective layer to be measured was formed, and then forming a gold electrode on the film by vacuum deposition, or it may be a sample obtained by peeling off the inorganic protective layer from a fabricated electrophotographic photoreceptor, partially etching it, and sandwiching it between a pair of electrodes.

[0143] The inorganic protective layer is preferably a non-single-crystal film, such as a microcrystalline film, polycrystalline film, or amorphous film. Among these, amorphous films are particularly desirable for their surface smoothness, while microcrystalline films are more desirable in terms of hardness. The growth cross-section of the inorganic protective layer may have a columnar structure, but from the viewpoint of slipperiness, a highly flat structure is desirable, and an amorphous structure is preferable. Crystalline and amorphous properties are determined by the presence or absence of dots or lines in the diffraction pattern obtained by RHEED (Reflection High-Frequency Electron Diffraction) measurement.

[0144] The elastic modulus of the inorganic protective layer is preferably between 30 GPa and 80 GPa, and more preferably between 40 GPa and 65 GPa. By keeping the elastic modulus within the above range, the occurrence of depressions (dent-like scratches), peeling, and cracking of the inorganic protective layer becomes easier to suppress. This modulus of elasticity is calculated using the Nano Indenter SA2 manufactured by MTS Systems, Inc., with a depth profile obtained by the continuous stiffness method (CSM) (U.S. Patent 4848141), and the average value obtained from measurements taken from an indentation depth of 30 nm to 100 nm is used. The measurement conditions are as follows. • Measurement environment: 23℃, 55%RH • Indenter used: Diamond triangular pyramidal indenter (Berkovic indenter) • Test mode: CSM mode The measurement sample may be a sample prepared by depositing the inorganic protective layer on a substrate under the same conditions as when the inorganic protective layer to be measured was deposited, or it may be a sample prepared by peeling off the inorganic protective layer from an electrophotographic photoreceptor after fabrication and partially etching it.

[0145] The thickness of the inorganic protective layer is often, for example, 0.2 μm to 10.0 μm, and preferably 0.4 μm to 5.0 μm. When this film thickness is within the above range, the electrical properties and the abrasion resistance of the inorganic protective layer in the photoreceptor are improved.

[0146] -Formation of an inorganic protective layer- For forming the inorganic protective layer, known vapor deposition methods such as plasma CVD (Chemical Vapor Deposition), organometallic vapor deposition, molecular beam evaporation, vapor deposition, and sputtering are used.

[0147] The following explanation describes the formation of an inorganic protective layer, illustrating it with specific examples and illustrating an example of a film deposition apparatus in the drawings. While the following explanation focuses on the formation of an inorganic protective layer composed of gallium, oxygen, and hydrogen, it is not limited to this method; any known formation method should be applied depending on the desired composition of the inorganic protective layer.

[0148] Figure 3 is a schematic diagram showing an example of a film deposition apparatus used for forming an inorganic protective layer on an electrophotographic photoreceptor according to this embodiment. Figure 3(A) shows a schematic cross-sectional view of the film deposition apparatus viewed from the side, and Figure 3(B) shows a schematic cross-sectional view between A1 and A2 of the film deposition apparatus shown in Figure 3(A). In Figure 3, 210 is the film deposition chamber, 211 is the exhaust port, 212 is the substrate rotation section, 213 is the substrate support member, 214 is the substrate, 215 is the gas introduction pipe, 216 is the shower nozzle having an opening for injecting the gas introduced from the gas introduction pipe 215, 217 is the plasma diffusion section, 218 is the high-frequency power supply section, 219 is the flat plate electrode, 220 is the gas introduction pipe, and 221 is the high-frequency discharge pipe section.

[0149] In the film deposition apparatus shown in Figure 3, an exhaust port 211 connected to a vacuum exhaust device (not shown) is provided at one end of the film deposition chamber 210, and a plasma generator consisting of a high-frequency power supply unit 218, a flat plate electrode 219, and a high-frequency discharge tube unit 221 is provided on the side of the film deposition chamber 210 opposite to the side with the exhaust port 211. This plasma generator consists of a high-frequency discharge tube section 221, a flat plate electrode 219 positioned inside the high-frequency discharge tube section 221 with its discharge surface facing the exhaust port 211, and a high-frequency power supply section 218 positioned outside the high-frequency discharge tube section 221 and connected to the side of the flat plate electrode 219 opposite to the discharge surface. A gas introduction pipe 220 for supplying gas into the high-frequency discharge tube section 221 is connected to the high-frequency discharge tube section 221, and the other end of this gas introduction pipe 220 is connected to a first gas supply source (not shown).

[0150] Alternatively, the plasma generator shown in Figure 4 may be used instead of the plasma generator provided in the film deposition apparatus shown in Figure 3. Figure 4 is a schematic diagram showing another example of a plasma generator used in the film deposition apparatus shown in Figure 3, and is a side view of the plasma generator. In Figure 4, 222 represents a high-frequency coil, 223 represents a quartz tube, and 220 is the same as that shown in Figure 3. This plasma generator consists of a quartz tube 223 and a high-frequency coil 222 provided along the outer surface of the quartz tube 223, with one end of the quartz tube 223 connected to a film deposition chamber 210 (not shown in Figure 4). The other end of the quartz tube 223 is connected to a gas introduction pipe 220 for introducing gas into the quartz tube 223.

[0151] In Figure 4, a rod-shaped shower nozzle 216 extending along the discharge surface is connected to the discharge surface side of the flat electrode 219. One end of the shower nozzle 216 is connected to a gas introduction pipe 215, which is connected to a second gas supply source (not shown) located outside the film deposition chamber 210. Furthermore, a substrate rotation section 212 is provided within the film deposition chamber 210, and a cylindrical substrate 214 is attached to the substrate rotation section 212 via a substrate support member 213 so that the longitudinal direction of the shower nozzle 216 and the axial direction of the substrate 214 face each other. During film deposition, the substrate rotation section 212 rotates, causing the substrate 214 to rotate in the circumferential direction. For example, a photoreceptor with an organic photosensitive layer already laminated is used as the substrate 214.

[0152] The inorganic protective layer can be formed, for example, as follows: First, oxygen gas (or helium (He) diluted oxygen gas), helium (He) gas, and hydrogen (H2) gas as needed are introduced into the high-frequency discharge tube section 221 from the gas introduction tube 220, and a 13.56 MHz radio wave is supplied to the flat electrode 219 from the high-frequency power supply section 218. At this time, a plasma diffusion section 217 is formed so as to spread radially from the discharge surface side of the flat electrode 219 toward the exhaust port 211 side. Here, the gas introduced from the gas introduction tube 220 flows through the film deposition chamber 210 from the flat electrode 219 side toward the exhaust port 211 side. The flat electrode 219 may also be surrounded by an earth shield.

[0153] Next, trimethylgallium gas is introduced into the deposition chamber 210 via the gas introduction tube 215 and the shower nozzle 216 located downstream of the plate electrode 219, which is an activation device, thereby depositing a non-single-crystal film containing gallium, oxygen, and hydrogen on the surface of the substrate 214. As the substrate 214, for example, a substrate on which an organic photosensitive layer is formed is used.

[0154] The surface temperature of the substrate 214 during the deposition of the inorganic protective layer is preferably 150°C or lower, more preferably 100°C or lower, and particularly preferably between 30°C and 100°C, since an organic photoreceptor having an organic photosensitive layer is used. Even if the surface temperature of the substrate 214 is below 150°C at the start of film deposition, if it rises above 150°C due to the influence of plasma, the organic photosensitive layer may be damaged by heat. Therefore, it is desirable to control the surface temperature of the substrate 214 taking this effect into consideration. The surface temperature of the substrate 214 may be controlled by at least one of a heating device and a cooling device (not shown in the figure), or it may be left to the natural temperature rise during discharge. When heating the substrate 214, the heater may be installed on the outside or inside of the substrate 214. When cooling the substrate 214, a cooling gas or liquid may be circulated inside the substrate 214. To avoid a temperature rise on the substrate 214 surface due to electrical discharge, it is effective to adjust the high-energy gas flow hitting the substrate 214 surface. In this case, conditions such as gas flow rate, discharge output, and pressure are adjusted to achieve the desired temperature.

[0155] Alternatively, instead of trimethylgallium gas, organometallic compounds containing aluminum or hydrides such as diborane can be used, and two or more of these may be mixed. For example, in the initial stages of forming the inorganic protective layer, by introducing trimethylindium into the deposition chamber 210 via the gas introduction tube 215 and shower nozzle 216, a film containing nitrogen and indium is deposited on the substrate 214. This film absorbs ultraviolet light that is generated during continuous deposition and degrades the organic photosensitive layer. Therefore, damage to the organic photosensitive layer caused by ultraviolet light during deposition is suppressed.

[0156] Furthermore, for dopant doping during film formation, SiH3 and SnH4 are used in gaseous form for n-type films, and biscyclopentadienylmagnesium, dimethylcalcium, dimethylstrontium, etc., are used in gaseous form for p-type films. In addition, known methods such as thermal diffusion and ion implantation may be used to dopant elements into the surface layer. Specifically, for example, a conductive inorganic protective layer of the n-type, p-type, etc., is obtained by introducing a gas containing at least one dopant element into the film deposition chamber 210 via a gas introduction pipe 215 and a shower nozzle 216.

[0157] In the film deposition apparatus described using Figures 3 and 4, the activated nitrogen or activated hydrogen formed by the discharge energy may be independently controlled by providing multiple activation devices, or a gas containing both nitrogen and hydrogen atoms, such as NH3, may be used. Furthermore, H2 may be added. In addition, conditions in which activated hydrogen is liberated and generated from organometallic compounds may be used. In this way, activated carbon atoms, gallium atoms, nitrogen atoms, hydrogen atoms, etc., exist in a controlled state on the surface of substrate 214. The activated hydrogen atoms have the effect of removing hydrogen molecules from hydrocarbon groups such as methyl and ethyl groups that constitute organometallic compounds. Therefore, a hard film (inorganic protective layer) that constitutes a three-dimensional bond is formed.

[0158] The plasma generator in the film deposition apparatus shown in Figures 3 and 4 uses a high-frequency oscillator, but is not limited to this. For example, a microwave oscillator may be used, or an electrocyclotron resonance or helicon plasma system may be used. In the case of a high-frequency oscillator, it may be either an inductive or capacitive type. Furthermore, two or more types of these devices may be used in combination, or two or more devices of the same type may be used. A high-frequency oscillator is desirable to suppress the temperature rise of the substrate 214 surface due to plasma irradiation, but a device to suppress heat irradiation may also be provided.

[0159] When using two or more different plasma generators, it is desirable to ensure that discharges occur simultaneously at the same pressure. Alternatively, a pressure difference may be provided between the discharge region and the film deposition region (the area where the substrate is placed). These devices may be arranged in series with respect to the gas flow formed within the deposition apparatus from the gas introduction area to the gas discharge area, or each device may be arranged facing the film deposition surface of the substrate.

[0160] For example, when two types of plasma generators are installed in series with respect to a gas flow, taking the film deposition apparatus shown in Figure 3 as an example, the shower nozzle 216 is used as an electrode to generate a discharge in the film deposition chamber 210. In this case, for example, a high-frequency voltage is applied to the shower nozzle 216 via the gas introduction pipe 215 to generate a discharge in the film deposition chamber 210 using the shower nozzle 216 as an electrode. Alternatively, instead of using the shower nozzle 216 as an electrode, a cylindrical electrode is provided between the substrate 214 and the flat plate electrode 219 in the film deposition chamber 210, and this cylindrical electrode is used to generate a discharge in the film deposition chamber 210. Furthermore, when using two different types of plasma generators under the same pressure, for example, a microwave oscillator and a high-frequency oscillator, the excitation energy of the excited species can be significantly varied, which is effective for controlling the film quality. Also, the discharge may be performed near atmospheric pressure (70,000 Pa to 110,000 Pa). When performing the discharge near atmospheric pressure, it is desirable to use He as the carrier gas.

[0161] For example, the inorganic protective layer is formed by placing a substrate 214 with an organic photosensitive layer formed on it in a film deposition chamber 210, and introducing mixed gases with different compositions to form the inorganic protective layer.

[0162] Furthermore, regarding film deposition conditions, for example, when using high-frequency discharge, it is desirable to set the frequency in the range of 10 kHz to 50 MHz in order to deposit a high-quality film at low temperatures. Also, although the output depends on the size of the substrate 214, it is 0.01 W / cm² relative to the surface area of ​​the substrate. 2 More than 0.2W / cm 2 The following range is desirable: The rotational speed of the base 214 should preferably be in the range of 0.1 rpm to 500 rpm.

[0163] (Single-layer photosensitive layer) A single-layer photosensitive layer (charge generation / charge transport layer) is, for example, a layer comprising a charge generation material, a charge transport material, and, if necessary, a binder resin and other well-known additives. These materials are the same as those described for the charge generation layer and the charge transport layer. Furthermore, the content of the charge-generating material in the single-layer photosensitive layer is preferably 0.1% to 10% by mass, and more preferably 0.8% to 5% by mass, relative to the total solid content. In addition, the content of the charge-transporting material in the single-layer photosensitive layer is preferably 5% to 50% by mass, relative to the total solid content. The method for forming a single-layer photosensitive layer is the same as the method for forming a charge generation layer or a charge transport layer. The thickness of the single-layer photosensitive layer is, for example, preferably 5 μm to 50 μm, and more preferably 10 μm to 40 μm.

[0164] [Charging device] The charging device 15 charges the surface of the photoreceptor 12. The charging device 15 includes, for example, a contact-type charging member 14 provided in contact with the surface of the photoreceptor 12 and charging the surface of the photoreceptor 12, and an AC power supply 28 (an example of an AC voltage application unit for the charging member) that applies an AC voltage to the charging member 14. The AC power supply 28 is electrically connected to the charging member 14.

[0165] Examples of contact-type charging members 14 include contact-type chargers using conductive charging rolls, charging brushes, charging films, charging rubber blades, charging tubes, etc.

[0166] The AC voltage applied to the charged member 14 by the AC power supply 28 is the peak voltage V pp The voltage should be between 350V and 4000V (preferably between 800V and 1500V), and the frequency should be 100Hz or higher (preferably 2500V or higher). Here, the AC power supply 28 may apply a superimposed voltage to the charged member 14, which is a DC voltage superimposed with an AC voltage.

[0167] The charging device 15 is not limited to a configuration comprising a contact-type charging member 14 and an AC power supply 28 that applies an AC voltage to the charging member 14. As shown in Figure 2, along with the contact-type charging member 14 and the AC power supply 28, the rotational direction of the photoreceptor 12 is greater than that of the contact-type charging member 14. DownstreamThe device may also be configured to include a non-contact charging member 14A that charges the surface of the photoreceptor 12, and a DC power supply 28A (an example of a DC voltage application unit) that applies a DC voltage to the non-contact charging member 14A. Examples of non-contact charging members 14A include known charging devices such as non-contact roller chargers, scorotron chargers or corotron chargers utilizing corona discharge.

[0168] In this embodiment, the AC voltage applied to the contact-type charging member 14 by the AC power supply 28 is the peak voltage V pp The voltage should be between 1000V and 4000V, and the frequency should be 2500Hz or higher. On the other hand, the DC voltage applied to the non-contact type charging member 14A by the DC power supply 28A is preferably 600V or less and 1000V or less.

[0169] In this embodiment, the contact-type charging member 14 functions as an auxiliary charging member and plays the role of injecting electrons into the photoreceptor 12. Therefore, even if a non-contact type electrical member 14A is used, the electrical properties of the photoreceptor 12 and the wear resistance of the inorganic protective layer are improved.

[0170] [Electrostatic image forming device] The electrostatic image forming apparatus 16 forms an electrostatic image on the surface of a charged photoreceptor 12. Specifically, for example, the electrostatic image forming apparatus 16 irradiates the surface of the photoreceptor 12, which has been charged by a charging member 14, with light L modulated based on the image information of the image to be formed, thereby forming an electrostatic image on the photoreceptor 12 that corresponds to the image information.

[0171] Examples of electrostatic image forming apparatus 16 include optical equipment having a light source that exposes an image-like object with light such as semiconductor laser light, LED light, or liquid crystal shutter light.

[0172] [Developing equipment] The developing device 18 is located, for example, downstream of the photoreceptor 12 in the rotational direction from the irradiation position of light L by the electrostatic image forming device 16. The developing device 18 has a storage section for containing the developer. This storage section contains an electrostatic image developer having toner. The toner is stored, for example, in a charged state within the developing device 18.

[0173] Furthermore, in the image forming apparatus shown in Figure 1, fatty acid metal salt particles are added to the developer (toner) contained in the developing device 18. In other words, the developing device 18 also serves as a supply device that supplies fatty acid metal salts to the contact area between the surface of the photoreceptor 12 and the cleaning blade 22A. Details regarding the fatty acid metal salt particles added to the developer (and its toner) will be described later.

[0174] The developing apparatus 18 includes, for example, a developing member 18A that develops the electrostatic image formed on the surface of the photoreceptor 12 using a developer containing toner, and a power supply 32 that applies a developing voltage to the developing member 18A. The developing member 18A is electrically connected to, for example, the power supply 32.

[0175] The developing element 18A of the developing device 18 is selected according to the type of developer, but an example is a developing roll having a developing sleeve with a magnet built in.

[0176] The developing device 18 (including the power supply 32) is electrically connected to, for example, a control device 36 provided in the image forming apparatus 10, and is driven and controlled by the control device 36 to apply a developing voltage to the developing member 18A. The developing member 18A, to which the developing voltage has been applied, is charged to a developing potential corresponding to the developing voltage. The developing member 18A, charged to the developing potential, then holds, for example, the developer contained in the developing device 18 on its surface and supplies the toner contained in the developer from inside the developing device 18 to the surface of the photoreceptor 12. On the surface of the photoreceptor 12 to which the toner has been supplied, the formed electrostatic charge image is developed as a toner image.

[0177] [Transfer device] The transfer device 31 is provided, for example, downstream of the developing member 18A in the rotational direction of the photoreceptor 12. The transfer device 31 includes, for example, a transfer member 20 that transfers the toner image formed on the surface of the photoreceptor 12 to the recording medium 30A, and a power supply 30 that applies a transfer voltage to the transfer member 20. The transfer member 20 is, for example, cylindrical and transports the recording medium 30A between itself and the photoreceptor 12. The transfer member 20 is electrically connected to, for example, the power supply 30.

[0178] Examples of the transfer member 20 include contact-type transfer chargers using belts, rollers, films, rubber cleaning blades, etc., and non-contact type transfer chargers that are known themselves, such as scorotron transfer chargers or corotron transfer chargers that utilize corona discharge.

[0179] The transfer device 31 (including the power supply 30) is electrically connected to, for example, a control device 36 provided in the image forming apparatus 10, and is driven and controlled by the control device 36 to apply a transfer voltage to the transfer member 20. The transfer member 20, to which the transfer voltage has been applied, is charged to a transfer potential corresponding to the transfer voltage.

[0180] When a transfer voltage with the opposite polarity to the toner that constitutes the toner image formed on the photoreceptor 12 is applied to the transfer member 20 from the power supply 30 of the transfer member 20, for example, a transfer electric field with an electric field strength that moves each toner constituting the toner image on the photoreceptor 12 from the photoreceptor 12 to the transfer member 20 side by electrostatic force is formed in the region where the photoreceptor 12 and the transfer member 20 face each other (see transfer region 32A in Figure 1).

[0181] The recording medium 30A is housed in, for example, a housing (not shown), and is transported from this housing along a transport path 34 by a plurality of transport members (not shown) to the transfer region 32A, which is the region where the photoreceptor 12 and the transfer member 20 face each other. In the example shown in Figure 1, it is transported in the direction of arrow B. Once the recording medium 30A reaches the transfer region 32A, the toner image on the photoreceptor 12 is transferred to the recording medium 30A by a transfer electric field formed in the region, for example, when a transfer voltage is applied to the transfer member 20. That is, for example, the toner image is transferred onto the recording medium 30A by the movement of toner from the surface of the photoreceptor 12 to the recording medium 30A. The toner image on the photoreceptor 12 is then transferred onto the recording medium 30A by the transfer electric field.

[0182] [Cleaning device] The cleaning device 22 is located downstream of the transfer area 32A in the rotational direction of the photoreceptor 12. After the toner image has been transferred to the recording medium 30A, the cleaning device 22 cleans any residual toner adhering to the photoreceptor 12. In addition to residual toner, the cleaning device 22 also cleans any other adhering substances such as paper dust.

[0183] The cleaning device 22 has a cleaning blade 22A, and removes deposits from the surface of the photoreceptor 12 by bringing the tip of the cleaning blade 22A into contact with the photoreceptor 12 in a direction opposite to the rotation direction of the photoreceptor 12.

[0184] [Static eliminator] The static elimination device 24 is, for example, located downstream of the cleaning device 22 in the rotational direction of the photoreceptor 12. After the toner image has been transferred, the static elimination device 24 exposes the surface of the photoreceptor 12 to remove static electricity. Specifically, for example, the static elimination device 24 is electrically connected to a control device 36 provided in the image forming apparatus 10, and is driven and controlled by the control device 36 to expose the entire surface of the photoreceptor 12 (specifically, for example, the entire image forming area) to remove static electricity.

[0185] Examples of static elimination devices 24 include devices having a light source such as a tungsten lamp that emits white light or a light-emitting diode (LED) that emits red light.

[0186] [Fusing device] The fixing device 26 is, for example, located downstream of the transfer area 32A in the transport direction of the transport path 34 of the recording medium 30A. The fixing device 26 includes a fixing member 26A and a pressurizing member 26B positioned in contact with the fixing member 26A, and fixes the toner image transferred onto the recording medium 30A at the contact point between the fixing member 26A and the pressurizing member 26B. Specifically, for example, the fixing device 26 is electrically connected to a control device 36 provided in the image forming apparatus 10, and is driven and controlled by the control device 36 to fix the toner image transferred onto the recording medium 30A to the recording medium 30A by heat and pressure.

[0187] Examples of the fixing device 26 include known fixing devices such as hot roller fixing devices and oven fixing devices. Specifically, for example, the fixing device 26 may be a well-known fixing device comprising a fixing roll or fixing belt as a fixing member 26A and a pressure roll or pressure belt as a pressure member 26B.

[0188] Here, the recording medium 30A, which has been transported along the transport path 34 and has the toner image transferred to it by passing through the area where the photoreceptor 12 and the transfer member 20 face each other (transfer area 32A), is further transported along the transport path 34 by a transport member (not shown) to the installation position of the fixing device 26, where the toner image on the recording medium 30A is fixed.

[0189] The recording medium 30A, on which the image has been formed by fixing the toner image, is discharged to the outside of the image forming apparatus 10 by a plurality of transport members (not shown in the figure). The photoreceptor 12 is then discharged by the static elimination device 24 and then recharged to a charging potential by the charging device 15.

[0190] [Operation of the image forming apparatus] An example of the operation of the image forming apparatus 10 according to this embodiment will be described. Note that various operations of the image forming apparatus 10 are performed by a control program executed in the control device 36.

[0191] The image forming operation of the image forming apparatus 10 will be described. First, the surface of the photoreceptor 12 is charged by the charging device 15. The electrostatic image forming device 16 exposes the charged surface of the photoreceptor 12 based on image information. This forms an electrostatic image on the photoreceptor 12 corresponding to the image information. In the developing device 18, the electrostatic image formed on the surface of the photoreceptor 12 is developed with a developer containing toner. This forms a toner image on the surface of the photoreceptor 12. In addition, fatty acid metal salt particles are added to the developer (and its toner) contained in the developing device 18, and these fatty acid metal salt particles are supplied to the surface of the photoreceptor 12 along with the toner. In the transfer device 31, the toner image formed on the surface of the photoreceptor 12 is transferred to the recording medium 30A. The toner image transferred to the recording medium 30A is fixed by the fuser device 26. Meanwhile, the surface of the photoreceptor 12 after the toner image has been transferred is cleaned by the cleaning blade 22A in the cleaning device 22, and then static electricity is removed by the static elimination device 24. Some of the fatty acid metal salt particles supplied to the surface of the photoreceptor 12 in the developing device 18 remain on the surface of the photoreceptor 12 even after the toner image has been transferred by the transfer device 31, and are supplied to the contact position between the cleaning blade 22A and the photoreceptor 12. Therefore, the presence of a fatty acid metal salt at the contact point between the cleaning blade 22A and the photoreceptor 12 enables the cleaning blade 22A to achieve high cleaning performance. [Examples]

[0192] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited in any way to these examples.

[0193] <Fabrication of electrophotographic photoreceptors> [Preparation of silica particles] 100 parts by mass of untreated (hydrophilic) silica particles (product name: OX50, manufactured by Aerosil, volume average particle size: 40 nm) were mixed with 30 parts by mass of a trimethylsilane compound (1,1,1,3,3,3-hexamethyldisilazane (manufactured by Tokyo Chemical Industry Co., Ltd.)) as a hydrophobic treatment agent. The mixture was reacted for 24 hours, and then filtered to obtain hydrophobic silica particles. These were designated as silica particles (1). The condensation rate of these silica particles (1) was 93%.

[0194] [Fabrication of electrophotographic photoreceptor 1] - Preparation of the lower layer - Zinc oxide: (Average particle size 70nm: Manufactured by Teika Co., Ltd.: Specific surface area value 15m²) 2 100 parts by mass of (g) was mixed with 500 parts by mass of tetrahydrofuran and stirred. 1.3 parts by mass of silane coupling agent (KBM503: manufactured by Shin-Etsu Chemical Co., Ltd.) was added and the mixture was stirred for 2 hours. Subsequently, the tetrahydrofuran was removed by vacuum distillation, and the mixture was baked at 120°C for 3 hours to obtain zinc oxide surface-treated with silane coupling agent.

[0195] 110 parts by mass of the surface-treated zinc oxide (silane coupling agent surface-treated zinc oxide) was stirred and mixed with 500 parts by mass of tetrahydrofuran. A solution of 0.6 parts by mass of alizarin dissolved in 50 parts by mass of tetrahydrofuran was added, and the mixture was stirred at 50°C for 5 hours. Subsequently, the zinc oxide to which alizarin had been added was filtered off by vacuum filtration, and the mixture was further dried under vacuum at 60°C to obtain alizarin-added zinc oxide.

[0196] A mixture was obtained by mixing 60 parts by mass of alizarin-modified zinc oxide, 13.5 parts by mass of a curing agent (blocked isocyanate Sumijule 3175, manufactured by Sumitomo Bayern Urethanes), 15 parts by mass of butyral resin (Eslec BM-1, manufactured by Sekisui Chemical Co., Ltd.), and 85 parts by mass of methyl ethyl ketone. 38 parts by mass of this mixture was mixed with 25 parts by mass of methyl ethyl ketone, and the mixture was dispersed for 2 hours using a sand mill with 1 mmφ glass beads to obtain a dispersion.

[0197] To the obtained dispersion, 0.005 parts by mass of dioctyltin dilaurate and 40 parts by mass of silicone resin particles (Tospar 145, manufactured by Momentive Performance Materials) were added as catalysts to obtain a coating solution for forming an undercoat. This coating solution was applied by immersion coating onto an aluminum substrate with a diameter of 60 mm, a length of 357 mm, and a wall thickness of 1 mm, and dried and cured at 170°C for 40 minutes to obtain an undercoat with a thickness of 19 μm.

[0198] -Fabrication of a charge generation layer- A mixture consisting of 15 parts by mass of hydroxygallium phthalocyanine, which has diffraction peaks at Bragg angles (2θ±0.2°) of at least 7.3°, 16.0°, 24.9°, and 28.0° in its X-ray diffraction spectrum using Cukα characteristic X-rays as a charge-generating material, 10 parts by mass of vinyl chloride / vinyl acetate copolymer (VMCH, manufactured by NUC Corporation) as a binder resin, and 200 parts by mass of n-butyl acetate was dispersed for 4 hours using glass beads with a diameter of 1 mmφ in a sand mill. To the obtained dispersion, 175 parts by mass of n-butyl acetate and 180 parts by mass of methyl ethyl ketone were added and stirred to obtain a coating solution for forming a charge-generating layer. This coating solution for forming a charge-generating layer was immersed and coated onto a base layer, and dried at room temperature (25°C) to form a charge-generating layer with a film thickness of 0.2 μm.

[0199] -Fabrication of a charge transport layer- 50 parts by mass of silica particles (1) were mixed with 250 parts by mass of tetrahydrofuran. While maintaining the liquid temperature at 20°C, 25 parts by mass of 4-(2,2-diphenylethyl)-4',4''-dimethyltriphenylamine as a charge transport material and 25 parts by mass of bisphenol Z type polycarbonate resin (viscosity average molecular weight: 30000) as a binder resin were added, and the mixture was stirred for 12 hours to obtain a coating solution for forming a charge transport layer.

[0200] This charge transport layer forming coating solution was applied onto the charge generation layer and dried at 135°C for 40 minutes to form a charge transport layer with a thickness of 30 μm, thereby obtaining an organic photoreceptor (1).

[0201] Through the above steps, an organic photoreceptor (1) was obtained, in which an undercoat layer, a charge generation layer, and a charge transport layer were sequentially laminated on an aluminum substrate.

[0202] -Formation of inorganic protective layer- Next, an inorganic protective layer composed of hydrogen-containing gallium oxide was formed on the surface of the organic photoreceptor (1). The formation of this inorganic protective layer was performed using a film forming apparatus having the configuration shown in Figure 3.

[0203] First, the organic photoreceptor (1) was placed on the substrate supporting member 213 inside the film forming chamber 210 of the film forming apparatus, and the inside of the film forming chamber 210 was evacuated through the exhaust port 211 until the pressure reached 0.1 Pa. Next, 40% oxygen gas diluted with He (flow rate 5.7 sccm) and hydrogen gas (flow rate 500 sccm) were introduced from the gas introduction pipe 220 into the high-frequency discharge tube section 221 provided with a flat plate electrode 219 having a diameter of 85 mm. A 13.56 MHz radio wave was set to an output of 500 W by the high-frequency power supply unit 218 and a matching circuit (not shown in Figure 3), matching was performed with a tuner, and discharge was generated from the flat plate electrode 219. The reflected wave at this time was 0 W. Next, trimethylgallium gas (flow rate 1.9 sccm) was introduced from the shower nozzle 216 through the gas introduction pipe 215 into the plasma diffusion section 217 inside the film forming chamber 210. At this time, the reaction pressure inside the film forming chamber 210 measured by a Baratron vacuum gauge was 5.3 Pa. In this state, film formation was performed for 68 minutes while rotating the organic photoreceptor (1) at a speed of 500 rpm, and an inorganic protective layer with a film thickness of 6 μm was formed on the surface of the charge transport layer of the organic photoreceptor (1). The surface roughness Ra on the outer peripheral surface of the inorganic protective layer was 1.9 nm.

[0204] In the inorganic protective layer, the elemental composition ratio of oxygen to gallium (O / M = oxygen / gallium) was 1.45.

[0205] Through the above steps, an electrophotographic photoreceptor 1 was obtained, in which an undercoat layer, a charge generation layer, a charge transport layer, and an inorganic protective layer were sequentially formed on a conductive substrate.

[0206] [Fabrication of Electrophotographic Photoreceptor 2] Electrophotographic photoreceptor 2 was obtained in the same manner as electrophotographic photoreceptor 1, except that the flow rate of 40% oxygen gas diluted with He was set to 4.8 sccm in the formation of the inorganic protective layer.

[0207] [Fabrication of electrophotographic photoreceptor 3] Electrophotographic photoreceptor 3 was obtained in the same manner as electrophotographic photoreceptor 1, except that the flow rate of 40% oxygen gas diluted with He was set to 5.3 sccm in the formation of the inorganic protective layer.

[0208] [Fabrication of the electrophotographic photoreceptor 4] In forming the inorganic protective layer, an electrophotographic photoreceptor 4 was obtained in the same manner as for electrophotographic photoreceptor 1, except that the flow rate of 40% oxygen gas diluted with He was set to 8.6 sccm.

[0209] [Fabrication of electrophotographic photoreceptors 5-8] Electrophotographic photoreceptors 5 to 8 were obtained in the same manner as electrophotographic photoreceptor 1, except that the film deposition time was adjusted to achieve the film thickness shown in Table 1 during the formation of the inorganic protective layer.

[0210] [Fabrication of the electrophotographic photoreceptor 9] An electrophotographic photoreceptor 9 was obtained in the same manner as electrophotographic photoreceptor 1, except that trimethylaluminum was used as the raw material gas in the formation of the inorganic protective layer.

[0211] [Fabrication of the electrophotographic photoreceptor 10] Electrophotographic photoreceptor 10 was obtained in the same manner as electrophotographic photoreceptor 1, except that dimethylzinc was used instead of trimethylgallium as the raw material gas in the formation of the inorganic protective layer.

[0212] [Fabrication of the electrophotographic photoreceptor 11] In forming the inorganic protective layer, the electrophotographic photoreceptor 11 was obtained in the same manner as electrophotographic photoreceptor 1, except that the flow rate ratio of trimethylgallium gas and He-diluted 40% oxygen gas was changed midway through the process so that the film thickness and composition of the surface layer and the lower layer matched those shown in Table 1.

[0213] [Fabrication of electrophotographic photoreceptor C1] Electrophotographic photoreceptor C1 was obtained in the same manner as electrophotographic photoreceptor 1, except that the flow rate of 40% oxygen gas diluted with He was set to 1.5 sccm in the formation of the inorganic protective layer.

[0214] [Fabrication of electrophotographic photoreceptor C2] Electrophotographic photoreceptor C2 was obtained in the same manner as electrophotographic photoreceptor 1, except that the flow rate of 40% oxygen gas diluted with He was set to 12.5 sccm in the formation of the inorganic protective layer.

[0215] <Examples 1-20, Comparative Examples 1-3> As the image forming apparatus (1), a modified version of the image forming apparatus "VERSANT180Press (manufactured by Fujifilm Business Innovation Co., Ltd.)" was prepared (as shown in Figure 1, an image forming apparatus equipped with a contact-type electrostatic roller and an AC power supply that applies an AC voltage to the electrostatic roller). The photoreceptors for each example were mounted in the prepared image forming apparatus. The peak-to-peak voltage Vpp and frequency of the AC voltage applied to the charging roll by the AC power supply were as shown in Table 1, and the following evaluation was performed. However, Comparative Example 3 was an image forming apparatus modified from the "VERSANT180Press" image forming apparatus (manufactured by Fujifilm Business Innovation Co., Ltd.), equipped with a contact-type charging roll and a DC power supply that applies a DC voltage to the charging roll.

[0216] The abbreviations in Table 1 are as follows: • O / M: Elemental composition ratio of oxygen (O) to the aforementioned metal element (M) (oxygen O / metal element M) • IR CH / MO: Indicates the ratio of C + H elements to M + O elements ((C+H) / (M+O)) in the inorganic protective layer. The evaluation method is IR measurement, and it is defined by the intensity ratio of infrared spectral absorption. Specifically, it is as follows: CH is a 3000 cm³ compound caused by the addition of C and H elements. -1 This is the intensity of infrared spectral absorption in the vicinity, and MO is due to the combination of M and O elements at 500 cm². -1 This is the intensity of infrared spectral absorption in the vicinity. For infrared absorption spectrum measurement, a Spectrum One Fourier transform infrared absorption measurement system manufactured by PerkinElmer with a S / N ratio of 30000:1 and a resolution of 4 cm⁻¹ was used. A sample deposited on a crystalline Si substrate was placed on a sample stage equipped with a beam condenser, and then the measurement was performed. A silicon wafer without a deposited film was used as a reference.

[0217] (Electrical characteristics of photoreceptor) The in-machine potential and density gradation property on the VERSANT180Press were evaluated. And evaluation was performed according to the following criteria. A: Photoreceptor surface potential after exposure of -250 V or lower B: Photoreceptor surface potential after exposure higher than -250 V and -300 V or lower C: Photoreceptor surface potential after exposure higher than -300 V and -350 V or lower D: Electrical characteristics problem exists, density output deterioration

[0218] (Abrasion resistance of photoreceptor) Judgment was made based on the abrasion rate on the VERSANT180Press. Specifically, the abrasion amount (unit: nm) per 1000 rotations of the photoreceptor (expressed as kcycle) was evaluated according to the following criteria. A: 0.08 nm / kcycle or less B: Greater than 0.08 nm / kcycle and 0.1 nm / kcycle or less C: Greater than 0.1 nm / kcycl and 0.13 nm / kcycl or less D: Crack defect occurrence due to abrasion

[0219] [Table 1]

[0220] <Examples 101 to 111> Except for using a modified image forming apparatus, the "VERSANT180Press" (manufactured by Fujifilm Business Innovation Co., Ltd.), as the image forming apparatus (as shown in Figure 2, an image forming apparatus equipped with a contact-type charging roll and an AC power supply that applies an AC voltage to the charging roll, and a non-contact type scorotron charger and a DC power supply that applies a DC voltage to the scorotron charger), the electrical characteristics and wear resistance of the photoreceptor were evaluated in the same manner as in Example 1. However, the peak-to-peak voltage Vpp and frequency of the AC voltage applied to the charging roll by the AC power supply, and the DC voltage applied to the scorotron charger by the DC power supply were as shown in Table 2, and the same evaluation as in Example 1 was performed.

[0221] [Table 2]

[0222] From the above results, it can be seen that this embodiment exhibits superior electrical properties and wear resistance of the inorganic protective layer in the electrophotographic photoreceptor compared to the comparative example. [Explanation of symbols]

[0223] 10 Image forming apparatus 12 Photoreceptor 14. Contact-type charging member 15. Charging device 16 Electrostatic image forming device 18. Developing device 20 Transfer Member 22 Cleaning device 22A Cleaning Blade 24 Static eliminator 26 Fixing device 30A recording medium 31 Transfer device 36 Control device 64 External supply device 66A Fatty acid metal salts 101 Sublayer 102 Charge generation layer 103 Charge transport layer 104 Conductive substrate 105 Photosensitive layer 106 Inorganic protective layer 107A, 107B Electrophotographic photoreceptor (photoreceptor) 210 Deposition chamber 211 Exhaust port 212 Base Rotating Section 213 Base support member 214 Base 215 Gas inlet pipe 216 Shower Nozzle 217 Plasma Diffusion Section 218 High-frequency power supply unit 219 Flat electrode 220 Gas inlet pipe 221 High-frequency discharge tube section 222 High-Frequency Coil 223 Quartz tube

Claims

1. An electrophotographic photoreceptor having, in this order, a conductive substrate, a photosensitive layer, and an inorganic protective layer containing a metal element M, oxygen O, and hydrogen H, wherein the elemental composition ratio (oxygen O / metal element M) of oxygen O to the metal element M in the layer constituting the surface of the inorganic protective layer is 1.3 or more and 1.5 or less, The following charging device (A) or (B), A static charge image forming apparatus for forming a static charge image on the surface of the charged electrophotographic photoreceptor, A developing apparatus that supplies an electrostatic image developer and develops the electrostatic image formed on the surface of the electrophotographic photoreceptor as a toner image, A transfer device for transferring a toner image formed on the surface of the electrophotographic photoreceptor to the surface of a recording medium, An image forming apparatus equipped with the following features. (A): A charging device comprising: a contact-type charging member that charges the surface of the electrophotographic photoreceptor; an AC voltage application unit that applies an AC voltage to the contact-type charging member; a non-contact-type charging member provided downstream of the contact-type charging member in the rotational direction of the electrophotographic photoreceptor and that charges the surface of the electrophotographic photoreceptor; and a DC voltage application unit that applies a DC voltage to the non-contact-type charging member, wherein the AC voltage applied to the contact-type charging member by the AC voltage application unit has a peak voltage Vpp of 800V or more and 1500V or less, a frequency of 2500Hz or more and 3000Hz or less, and the DC voltage applied to the non-contact-type charging member by the DC voltage application unit has a voltage V of 600V or more and 1000V or less. (B): A charging device having only a contact-type charging member as a charging member for charging the surface of the electrophotographic photoreceptor, and having only an AC voltage application unit for applying an AC voltage to the contact-type charging member as a voltage application unit for applying a voltage to the charging member, wherein the peak voltage Vpp of the AC voltage applied to the contact-type charging member by the AC voltage application unit is 800V or more and 1500V or less, and the frequency is 2500Hz or more and 3000Hz or less.

2. The image forming apparatus according to claim 1, wherein the elemental composition ratio (oxygen O / metal element M) of oxygen O to the metal element M in the layer constituting the surface of the inorganic protective layer is 1.4 or more and 1.5 or less.

3. The image forming apparatus according to claim 1 or claim 2, wherein the inorganic protective layer is a single layer of a layer constituting the surface of the inorganic protective layer, wherein the elemental composition ratio (oxygen O / metal element M) of oxygen O to the metal element M is 1.3 or more and less than 1.

5.

4. The image forming apparatus according to claim 3, wherein the thickness of the single layer constituting the surface of the inorganic protective layer is 0.5 μm or more and 1.0 μm or less.

5. The image forming apparatus according to any one of claims 1 to 4, wherein the light transmittance of the inorganic protective layer is 90% or more.

6. An electrophotographic photoreceptor having, in this order, a conductive substrate, a photosensitive layer, and an inorganic protective layer containing a metal element M, oxygen O, and hydrogen H, wherein the elemental composition ratio (oxygen O / metal element M) of oxygen O to the metal element M in the layer constituting the surface of the inorganic protective layer is 1.3 or more and 1.5 or less, The following charging device (A) or (B), A unit for an image forming apparatus, comprising the above. (A): A charging device comprising: a contact-type charging member that charges the surface of the electrophotographic photoreceptor; an AC voltage application unit that applies an AC voltage to the contact-type charging member; a non-contact-type charging member provided downstream of the contact-type charging member in the rotational direction of the electrophotographic photoreceptor and that charges the surface of the electrophotographic photoreceptor; and a DC voltage application unit that applies a DC voltage to the non-contact-type charging member, wherein the AC voltage applied to the contact-type charging member by the AC voltage application unit has a peak voltage Vpp of 800V or more and 1500V or less, a frequency of 2500Hz or more and 3000Hz or less, and the DC voltage applied to the non-contact-type charging member by the DC voltage application unit has a voltage V of 600V or more and 1000V or less. (B): A charging device having only a contact-type charging member as a charging member for charging the surface of the electrophotographic photoreceptor, and having only an AC voltage application unit for applying an AC voltage to the contact-type charging member as a voltage application unit for applying a voltage to the charging member, wherein the peak voltage Vpp of the AC voltage applied to the contact-type charging member by the AC voltage application unit is 800V or more and 1500V or less, and the frequency is 2500Hz or more and 3000Hz or less.

Citation Information

Patent Citations

  • Electrifier for image forming device

    JP1997222768A

  • Electrophotographic photoreceptor, electrophotographic apparatus using same and process cartridge

    JP2004133044A

  • Electrification controller, electrifying device, image forming apparatus, and electrification control program

    JP2008164737A

  • Electrophotographic photoreceptor, process cartridge and image forming apparatus