A method for manufacturing recycled plastics and recycled plastics manufactured by said manufacturing method.

A surfactant-based desorption method for multi-layer plastic laminates efficiently removes printed layers, producing high-quality recycled plastic with minimal impurities and discoloration, addressing the challenges of recycling complex plastic packaging.

JP7947758B2Active Publication Date: 2026-11-11TOYO INK
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2022094182
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-06-10
Publication Date
2026-11-11
Estimated Expiration
2042-06-10

Smart Images

  • Figure 0007947758000001
    Figure 0007947758000001
  • Figure 0007947758000002
    Figure 0007947758000002
  • Figure 0007947758000003
    Figure 0007947758000003
Patent Text Reader

Abstract

To provide a method for efficiently removing a printed layer from a packaging material containing the printed layer to obtain recycled plastic with less coloring, foreign matter and bubbles.SOLUTION: There is provided a manufacturing method of recycled plastic to obtain recycled plastic from a packaging material (A). The packaging material (A) has a plastic laminate body and a printed layer provided on at least one surface of the plastic laminate body, the printed layer is located on an outermost surface of the packaging material (A), the plastic laminate body does not include a chromatic ink layer, and a content of a polyester resin in the packaging material (A) is 80 mass% or more. The manufacturing method comprises steps of: obtaining a laminate body (B) by removing 85 mass% or more of the printed layer by immersing the packaging material (A) in a desorption liquid containing a surfactant (1); and melting and kneading the laminate body (B) using an extrusion device equipped with a screw and a discharge part (2).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] Packages made of plastic films, plastic bottles, and other plastic products are discarded and dumped as waste in the ocean, posing a problem of environmental pollution. Therefore, interest in the recycling of plastic products has been increasing in recent years. In general, plastic products mainly made from one type of resin, such as bottles, caps, and single-layer film bags, are relatively easy to recycle. In particular, for polyester (PET) bottles and polystyrene (PS) food trays, collection systems have been established by governments and retail stores such as supermarkets, and recycling such as bottle-to-bottle and tray-to-tray has been realized.

[0002] On the other hand, in the case of food packaging packages (packaging materials) having a multi-layer structure, plastic laminates in which various plastic base materials such as polyester base materials, nylon base materials (NY), polypropylene base materials (PP), and polyethylene base materials (PE) are bonded together are used as film base materials. Since different types of plastic base materials are not compatible with each other, material recycling is considered difficult.

[0003] Patent Document 1 discloses a recycling processing method for reusing waste material of biaxially stretched polyester films without a step of removing the printed layer, but does not disclose a technique related to a recycling processing method for a laminate using polyester having packaging material suitability as the main raw material. In addition, even if a package including a printed layer is recycled as it is, chromatic colors contained in the printed layer are mixed, and only plastic raw materials colored in dark colors such as black and gray can be obtained. Furthermore, once colored, it is difficult to make the material colorless and transparent. It is preferable that colorless and transparent polyester with no application restrictions can be obtained by material recycling.

[0004] On the other hand, Patent Document 2 discloses a technique for separating substrates in a plastic laminate having a printed layer between substrates. This technique involves peeling / removing the printed layer or adhesive layer with an ink cleaning agent containing a surfactant and an alkaline solution, but it relies on mechanical effects, such as being performed in a crusher, and it is considered difficult to peel the substrates and obtain a plastic substrate without impurities. In addition, the alkaline solution may hydrolyze the polyester film, potentially degrading the physical properties of the recycled material. There is a need for a method to produce high-quality recycled plastic with high moldability, mainly using polyester as the raw material. [Prior art documents] [Patent Documents]

[0005] [Patent Document 1] Japanese Patent Publication No. 2006-116857 [Patent Document 2] Patent No. 7004124 [Overview of the project] [Problems that the invention aims to solve]

[0006] The present invention aims to provide a method for efficiently removing the printed layer from packaging material containing the printed layer, thereby obtaining recycled plastic with less coloring, foreign matter, and air bubbles. [Means for solving the problem]

[0007] As a result of diligent research by the inventors, we have discovered that the above problems can be solved by using the recycled plastic manufacturing method described below, and have thus come to fruition with the present invention.

[0008] In other words, the present invention is a method for producing recycled plastic from packaging material (A), The packaging material (A) has a plastic laminate and a printed layer provided on at least one surface of the plastic laminate, the printed layer is on the outermost surface of the packaging material (A), The aforementioned plastic laminate does not contain a colored ink layer. The polyester resin content of packaging material (A) is 80% by mass or more. Step 1 involves immersing the packaging material (A) in a desorption solution containing a surfactant to remove 85% or more by mass of the printed layer and obtain a laminate (B), The present invention relates to a method for producing recycled plastic, comprising step 2 of melting and kneading the laminate (B) using an extruder equipped with a screw and a discharge unit.

[0009] The present invention also relates to a method for producing recycled plastic, wherein a plastic laminate has an adhesive layer, and the adhesive layer is formed from a dry laminate adhesive or a non-sol laminate adhesive with an acid value of 10 mg KOH / g or less.

[0010] Furthermore, the present invention relates to a method for producing recycled plastics, wherein the dry laminate adhesive or non-sol laminate adhesive comprises a polyester polyol and an isocyanate compound.

[0011] Furthermore, the present invention relates to the above-mentioned method for producing recycled plastic, wherein the dry coating amount of the adhesive layer is 6% by mass or less of the total mass of the laminate.

[0012] Furthermore, the present invention relates to the above-mentioned method for producing recycled plastic, wherein the surfactant comprises at least one selected from the group consisting of nonionic surfactants, amphoteric surfactants, and anionic surfactants.

[0013] The present invention also relates to the above-mentioned method for producing recycled plastic, wherein the desorbed liquid further comprises an antifoaming agent, and the antifoaming agent is at least one selected from the group consisting of emulsion-type silicone compounds, self-emulsifying silicone compounds, and non-silicone compounds.

[0014] Furthermore, the present invention relates to a method for producing recycled plastic, wherein the printed layer contains at least one set selected from the group consisting of urethane resin / vinyl chloride-vinyl acetate, urethane resin / cellulose resin, and polyamide resin / cellulose resin.

[0015] The present invention further relates to the above-mentioned recycled plastic production method, wherein the melting temperature is 260 to 290°C.

[0016] The present invention further relates to the above-mentioned recycled plastic production method, wherein the pressure at the discharge unit provided in the extrusion device is 15 MPa or less.

[0017] The present invention further relates to the above-mentioned recycled plastic production method, wherein the rotational speed of the screw provided in the extrusion device is 50 to 1000 RPM.

[0018] The present invention further relates to the above-mentioned recycled plastic production method, wherein the printed layer has a primer layer that is removable with a stripping liquid.

[0019] The present invention further relates to the above-mentioned recycled plastic production method, wherein the primer layer contains a water-dispersible resin.

[0020] The present invention further relates to the above-mentioned recycled plastic production method, which further comprises a drying step of adjusting the moisture content of the laminate (B) to 0.2 mass% or less.

[0021] The present invention further relates to the above-mentioned recycled plastic production, wherein the chlorine content of the laminate (B) is 0.4 mass% or less based on the total mass of the laminate.

[0022] The present invention further relates to a recycled plastic produced by the above-mentioned recycled plastic production method.

[0023] The present invention further relates to a recycled plastic produced by the above-mentioned recycled plastic production method. Effects of the Invention

[0024] According to the present invention, it has become possible to provide a method for efficiently stripping a printed layer from a packaging material including the printed layer to obtain a recycled plastic with less coloring, foreign matter, and bubbles. Modes for Carrying Out the Invention

[0025] The embodiments of the present invention will be described in detail below, but the descriptions of embodiments or requirements below are merely examples of embodiments of the present invention, and the present invention is not limited to these unless it exceeds the gist of the invention.

[0026] In this invention, "printed layer" refers to a layer formed from printing ink, an overcoat agent, etc. Furthermore, the "primer layer" described later is also an embodiment of the printed layer, and multiple stacked printed layers also constitute a printed layer. In the following, among the printed layer and primer layer, the layer that can be removed by a desorbing solution may be referred to as the "desorbing layer."

[0027] The present invention relates to a method for producing recycled plastic from packaging material (A), The packaging material (A) has a plastic laminate and a printed layer provided on at least one surface of the plastic laminate, the printed layer is on the outermost surface of the packaging material (A), The aforementioned plastic laminate does not contain a colored ink layer. The polyester resin content of packaging material (A) is 80% by mass or more. Step 1 involves immersing the packaging material (A) in a desorption solution containing a surfactant to remove 85% or more by mass of the printed layer and obtain a laminate (B), The method for producing recycled plastic is characterized by comprising step 2, which involves melting and kneading the laminate (B) using an extrusion device equipped with a screw and a discharge unit. The detachment liquid contains a surfactant, which promotes the detachment of the printed layer and suppresses its re-adhesion to the laminate (B) after detachment. Furthermore, by using a laminate (B) with minimal coloring, recycled plastic with less coloring, foreign matter, and air bubbles can be obtained.

[0028] <Packaging material (A)> The packaging material (A) in the present invention comprises a plastic laminate and a printed layer provided on at least one surface of the plastic laminate, the printed layer being on the outermost surface of the packaging material (A), the plastic laminate not containing a chromatic ink layer, and the polyester resin content of the packaging material (A) being 80% by mass or more. The "chromatic ink layer" in "the plastic laminate not containing a chromatic ink layer" refers to a layer formed from chromatic ink for the purpose of color or pattern, and means a layer in which the color is clearly visible. This does not exclude cases where the plastic laminate has a coating layer or the like without the intention of coloring, resulting in a very thin coloring. Details of the plastic laminate will be described in a separate section, but it has a laminated structure that includes a base material and layers other than the base material.

[0029] The packaging material (A) is exemplified below, but is not limited to these examples. The plastic laminate is preferably laminated by conventionally known methods such as dry lamination, non-solvent lamination, extrusion lamination, and co-extrusion molding. An intermediate substrate may also be provided as needed. The composition of the packaging material (A) can be exemplified by, but is not limited to, the following. In the compositional representations (1) to (16) below, " / " indicates the boundary between each layer. "( )" indicates the lamination structure of the plastic laminate. Note that when a "primer layer" is present, the "printed layer" refers to the "printed layer excluding the primer layer." Also, when multiple layers, such as the first printed layer and the second printed layer, are actually stacked in contact with each other, they are simply referred to as the "printed layer."

[0030] (1) Printing layer / (Substrate / Adhesive layer / Sealant) (2) Printing layer / (Substrate / Adhesive layer / Intermediate substrate / Adhesive layer / Sealant) (3) Printing layer / (Substrate / Adhesive layer / First intermediate substrate / Adhesive layer / Second intermediate substrate / Adhesive layer / Sealant) (4) Printing layer / (base material / AC agent layer / adhesive layer) (5) Printing layer / (Substrate / AC agent layer / Adhesive layer / Sealant) (6) Printing layer / (Substrate / AC agent layer / Adhesive layer / Intermediate substrate / AC agent layer / Adhesive layer / Sealant) (7) Printing layer / (Substrate / Adhesive layer / Intermediate substrate / AC agent layer / Adhesive layer / Sealant) (8) Printing layer / (Substrate / AC agent layer / Adhesive layer / Intermediate substrate / Adhesive layer / Sealant) (9) Printing layer / Primer layer / (Substrate / Adhesive layer / Sealant) (10) Printing layer / Primer layer / (Substrate / Adhesive layer / Intermediate substrate / Adhesive layer / Sealant) (11) Printing layer / Primer layer / (Substrate / Adhesive layer / First intermediate substrate / Adhesive layer / Second intermediate substrate / Adhesive layer / Sealant) (12) Printing layer / Primer layer / (Substrate / AC agent layer / Adhesive layer) (13) Printing layer / Primer layer / (Substrate / AC agent layer / Adhesive layer / Sealant) (14) Printing layer / Primer layer / (Substrate / AC agent layer / Adhesive layer / Intermediate substrate / (AC agent layer) / Adhesive layer / Sealant) (15) Printing layer / Primer layer / (Substrate / Adhesive layer / Intermediate substrate / AC agent layer / Adhesive layer / Sealant) (16) Printing layer / Primer layer / (Substrate / AC agent layer / Adhesive layer / Intermediate substrate / Adhesive layer / Sealant)

[0031] The "adhesive layer" mentioned above refers to an adhesive used to bond substrates together, such as a urethane-based adhesive used in dry lamination and non-solvent lamination, or a heat-meltable resin ("adhesive layer") used in extruded lamination. The "adhesive layer" is one embodiment of the adhesive layer. In the above configuration, the "AC agent layer" refers to an anchor coat layer, which is used to improve the adhesion between the substrate and the adhesive layer. The "AC agent layer" may or may not be present.

[0032] Since the present invention primarily focuses on the production of recycled polyester resin, the packaging material (A) contains polyester resin in an amount of 80% by mass or more of the total mass of the packaging material (A). The content is more preferably 85% or more, even more preferably 90% by mass or more, and still more preferably 95% by mass or more. By including the above-mentioned range in the polyester resin of the packaging material (A), it is possible to obtain a molding material that is easy to separate, highly recyclable, has good moldability, and can be used for various applications. The polyester resin is preferably polyethylene terephthalate (PET) or polybutylene terephthalate (PBT). Furthermore, in order to make it a monomaterial, it is even more preferable that the polyester resin is the same.

[0033] <Base material> The base material is preferably a plastic base material mainly containing polyester resin as a raw material, and is preferably in the form of a film or sheet for use in packaging materials. It is even more preferable that it is made of the same material as the intermediate base material and sealant. Examples of the polyester substrate include polyethylene terephthalate (PET) film and polybutylene terephthalate (PBT) film. The thickness of the substrate is preferably 5 to 30 μm, and more preferably 10 to 30 μm. If the thickness of the substrate is 5 μm or more, better dimensional stability and heat resistance can be obtained, and if it is 30 μm or less, better bending resistance can be obtained.

[0034] The substrate may also be a gas barrier substrate, such as a plastic substrate having an inorganic vapor-deposited layer of aluminum, silica, alumina, etc., or a plastic substrate having a layer of mixed organic and inorganic components.

[0035] The substrate is preferably in the form of (coated or kneaded) containing additives such as antistatic agents, anti-fogging agents, and UV-blocking agents, or in the form of having an easily adhering coating layer (for example, a layer containing polyvinyl alcohol and its derivatives), or in the form of having the surface of the substrate treated with corona or low-temperature plasma. The above additives and processing are also applied for the purpose of improving the wettability of printing inks and other coating agents, or for the purpose of giving the film specific functionality. For example, it is also suitably used to provide packaging with excellent visibility of the contents by preventing fogging of the packaging due to moisture.

[0036] <Adhesive layer, adhesive layer> The packaging material (A) may further have an adhesive layer and / or a bonding layer. The adhesive layer and / or bonding layer is not particularly limited as long as it can bond each layer. Suitable adhesive layers include olefin-based adhesives, acrylic-based adhesives, and reactive urethane adhesives, and are more preferably reactive urethane adhesives which are reaction products of polyisocyanate and polyol. Suitable bonding layers include meltable resins used in extrusion lamination. In addition, imine-based anchor coating agents and other anchor coating agents may be used to improve the adhesion between the substrate and the bonding layer. The method for bonding each layer is not particularly limited and can be conventionally known methods such as dry lamination, non-sol lamination, and extrusion lamination.

[0037] [Reactive urethane adhesive] As a reactive urethane adhesive, a two-component urethane adhesive consisting of a polyol as the main component and a polyisocyanate as the curing agent is preferred. In this case, the adhesive layer becomes the reactant of this urethane adhesive. The polyol can be any compound having two or more hydroxyl groups and can be selected from known polyols. Examples of polyols include polyester polyols, polycarbonate polyols, polycaprolactone polyols, polyether polyols, polyester polyols, acrylic polyols, silicone polyols, castor oil-based polyols, and fluorine-based polyols. Among these, it is preferable to include polyether polyols and / or polyester polyols, and polyester polyols are even more preferable from the viewpoint of compatibility. The polyol may be an acid-modified product in which some of the hydroxyl groups in the polyol are acid-modified, or a polyol in which urethane bonds are introduced by reacting some of the hydroxyl groups in the polyol with diisocyanate. Polyisocyanates can be any compound having two or more isocyanate groups and can be selected from known polyisocyanates. Examples of polyisocyanates include aromatic polyisocyanates, aromatic aliphatic polyisocyanates, aliphatic polyisocyanates, alicyclic polyisocyanates, and modified versions thereof. Polyols may be used individually or in combination of two or more types. The same applies to polyisocyanates.

[0038] From the viewpoint of compatibility during the melting and kneading of the laminate (B), the amount of adhesive layer applied is preferably 6% or less of the total packaging material (A), more preferably 5% or less, and even more preferably 4% or less.

[0039] The acid value of the adhesive layer is preferably 10 mg KOH / g or less, more preferably 8 mg KOH / g or more, even more preferably 6 mg KOH / g or less, and particularly preferably 5 mg KOH / g or less. When the above acid value is present, the substrate and sealant of the plastic laminate are less likely to separate during the immersion step in the desorption solution, and only the desorption layer is efficiently desorbed, thus shortening the time of step 1.

[0040] [Other ingredients] The adhesive layer may contain silane coupling agents, phosphorus oxygen acids or their derivatives, leveling agents, defoaming agents, reaction accelerators, as well as inorganic fillers (e.g., silica, alumina, mica, talc, aluminum flakes, glass flakes), layered inorganic compounds, stabilizers (e.g., antioxidants, heat stabilizers, UV absorbers, hydrolysis inhibitors), rust inhibitors, thickeners, plasticizers, antistatic agents, lubricants, antiblocking agents, colorants, fillers, nucleating agents, catalysts for adjusting the curing reaction, etc.

[0041] <Intermediate material> The packaging material (A) may further have an intermediate substrate layer. The intermediate substrate preferably contains a polyester resin, and more preferably is made of the same material as the substrate and sealant. Examples include polyethylene terephthalate (PET) film and polybutylene terephthalate (PBT) film. It is also preferable that the intermediate substrate be a gas barrier substrate, such as a plastic substrate having an inorganic vapor-deposited layer of aluminum, silica, alumina, etc., or a plastic substrate having a layer of mixed organic and inorganic components.

[0042] <Sealant> The packaging material (A) may further have a sealant. The sealant's inner layer surface comes into direct contact with the packaged object and plays a role in protecting the packaged object. In order to form the laminate into a bag shape, it is preferable that the innermost layer of the sealant has heat-sealing properties. A substrate coated with a heat-sealing agent to impart heat-sealing properties is also included in the sealant. A polyethylene terephthalate film with heat-sealing properties is preferred as the material constituting the sealant.

[0043] The thickness of the sealant is not particularly limited and is set appropriately according to the application of the laminate and the type and properties of the packaged material, but it is generally preferably 10 to 80 μm. In the case of pouches (especially retort pouches), the thickness of the sealant is preferably 20 to 60 μm.

[0044] The sealant may be, for example, an inorganic vapor-deposited layer such as aluminum, silica, and alumina, or a sealant having a layer of mixed organic and inorganic components.

[0045] <Co-extruded film> The plastic laminate is preferably a co-extruded film. A co-extruded film is one in which resin layers are laminated by extrusion molding, and the resin layers may be made of polyester resin, or resin layers of a different resin may be laminated. The method for forming the co-extruded film by laminating the resin layers is not particularly limited and conventionally known methods such as the T-die method and the inflation method of co-extrusion can be used.

[0046] <Plastic laminate> The plastic laminate of the packaging material (A) is preferably a plastic laminate or co-extruded film formed from at least a base material and a sealant. It may also have a base material (intermediate base material) as an intermediate layer. It is preferable that the base material, intermediate base material, sealant, and co-extruded layer constituting the co-extruded film are made of the same material. The thickness of the plastic laminate is not particularly limited, but considering processability for packaging containers, it is preferably 20 μm to 250 μm, more preferably 30 μm to 200 μm, and even more preferably 40 μm to 150 μm.

[0047] The plastic laminate may also include a gas barrier substrate, such as a plastic substrate having an inorganic vapor-deposited layer of aluminum, silica, alumina, etc.; or a plastic substrate having an organic layer of ethylene-vinyl alcohol copolymer, polyvinyl alcohol, etc.

[0048] Furthermore, the plastic laminate is preferably in a form that includes additives such as antistatic agents, anti-fogging agents, and UV-blocking agents (coated or kneaded), or in a form that has an easily adhering coating layer (for example, a layer containing polyvinyl alcohol and its derivatives), or in a form in which the surface of the substrate has been corona-treated or low-temperature plasma-treated. The above-mentioned additives and processing are also applied for the purpose of improving the wettability of printing inks and other coating agents, or for the purpose of giving the film specific functionality. For example, it is also suitably used to provide packaging materials with excellent visibility of the contents by preventing fogging of the packaging material due to moisture.

[0049] <Manufacturing of packaging material (A)> The method for manufacturing the packaging material (A) is not particularly limited and can be done by methods described in, for example, Japanese Patent Publication No. 2019-142037, Japanese Patent Publication No. 2019-142039, Japanese Patent Publication No. 2021-160270, etc. The printed layer described below may be formed in advance on the substrate by printing or the like before manufacturing the plastic laminate, or the printed layer may be formed after the plastic laminate is formed, or the printed layer may be formed after the plastic laminate is processed into the form of a packaging bag.

[0050] <Print layer> The printed layer is, for example, a layer that forms an arbitrary printed pattern, and is preferably a layer intended for decoration, aesthetic enhancement, displaying contents, expiration date, manufacturer, or seller information, etc. This also includes solid print layers. Furthermore, the printed layer in this invention can be removed by immersion in a desorption solution containing a surfactant. The printed layer can be formed with a printing ink, and the printing ink preferably contains a urethane resin and / or a polyamide resin and other resins. The other resin preferably contains a hard resin. Hard resin refers to a resin other than urethane resin and polyamide resin that can act as a binder resin soluble in organic solvents. Hard resins preferably have a glass transition temperature of 40 to 260°C, more preferably 50 to 250°C, and even more preferably 60 to 240°C. Examples of hard resins include cellulose resins, vinyl chloride copolymer resins (vinyl chloride-vinyl acetate copolymer resin, vinyl chloride-acrylic copolymer resin, etc.), dimer acid resins, rosin resins (rosin-modified maleic acid resin, rosin ester resin, etc.), maleic acid resins, petroleum resins, terpene resins, ketone resins, dammer resins, copal resins, etc. Among these, it is preferable that at least one resin selected from vinyl chloride copolymer resins and cellulose resins be used. When these hard resins are used in combination, adhesion to plastic laminates is improved. In particular, the other resin is preferably a vinyl chloride-vinyl acetate copolymer resin and / or a cellulose-based resin, and is preferably contained in a solid content of 0.1 to 6% by mass in the total mass of the printing ink, and more preferably 0.5 to 5% by mass. By using the above resin in combination, a printing layer with excellent printability and delamination properties can be formed. The printing ink can be, for example, a printing ink described in JP 2016-043600, JP 2019-043085, etc., as appropriate. The acid value of the printing layer is preferably 70 mgKOH / g or less, and more preferably 50 mgKOH / g or less. Suitable resin combinations include urethane resin / vinyl chloride-vinyl acetate, urethane resin / cellulose resin, and polyamide resin / cellulose resin.

[0051] The printed layer can be obtained by forming printing ink on a substrate using various printing methods. The printing method is not particularly limited, but screen printing, gravure printing, flexographic printing, offset printing, and inkjet printing are preferred, with gravure printing being the most preferred.

[0052] <Primer layer> To further promote delamination, the printed layer may have a primer layer in contact with the plastic laminate. Note that the primer layer is also an embodiment of the printed layer. The primer layer is positioned in contact with the substrate and plays a role in delaminating the printed layer from the substrate by dissolution, peeling, etc., using a delamination solution. The primer layer preferably contains a water-dispersible resin and / or an acidic compound having an acidic group. The thickness of the primer layer is preferably in the range of 0.5 to 3.0 μm, more preferably 0.6 to 2.0 μm, and even more preferably 0.8 to 1.5 μm, and can be formed using known methods.

[0053] [Water dispersible resin] Any water-dispersible resin can be used that swells or dissolves in water and can be detached from the substrate. The water may be heated to a temperature of approximately 25-100°C. This allows the primer layer to be detached with water (including warm water). The water-soluble resin described later refers to a resin that exhibits water dispersibility regardless of the presence of acidic groups. Such resins can be selected from known resins, and examples include water-soluble polyester resins, water-soluble polyamide resins, water-soluble polyimide resins, water-soluble acrylic resins, water-soluble polyurethane resins, water-soluble polyallylamine resins, water-soluble phenolic resins, water-soluble epoxy resins, water-soluble phenoxy resins, water-soluble urea resins, water-soluble melamine resins, polyvinyl alcohol resins, and modified products of these resins. These can be used individually or in combination of two or more.

[0054] [Compounds containing acidic groups] The compound having an acidic group may be a resin having an acidic group, or a low-molecular-weight compound having an acidic group. This allows the primer layer to be removed.

[0055] Resins having acidic groups are not particularly limited as long as they have acidic groups, except in the case of low molecular weight compounds having acidic groups as described below. Examples of acidic groups include carboxyl groups, phosphate groups, sulfonic acid groups, sulfino groups, etc., and they may form salts. The following are preferred examples of resins having acidic groups. Examples include cellulose resins, urethane resins, acrylic resins, polyamide resins, vinyl chloride / vinyl acetate copolymers, ketone resins, polyester resins, and (meth)acrylic resins, all of which have acidic groups. For example, rosin-modified resins with acid values, such as maleated rosin and fumarated rosin, can be used. For example, radical copolymers such as styrene-(meth)acrylic resin, styrene-(anhydride)maleic acid resin, terpene-(anhydride)maleic acid resin, or acid-modified polyester resins can be used, which are copolymers of polymerizable monomers having acidic groups, such as polymerizable monomers having carboxyl groups, such as itaconic acid, maleic acid, fumaric acid, and cinnamic acid; polymerizable monomers that are acid anhydrides, such as itaconic acid anhydride and maleic anhydride; polymerizable monomers having sulfonic acid groups, such as sulfonated styrene; and polymerizable monomers having sulfonamide groups, such as vinylbenzenesulfonamide. These can be used individually or in combination of two or more.

[0056] Low molecular weight compounds having an acidic group refer to compounds that do not have a molecular weight distribution and have a molecular weight of 1,000 or less. Examples of such compounds include saturated fatty acids such as lauric acid, myristic acid, palmitic acid, margaric acid, and stearic acid; unsaturated fatty acids such as oleic acid, linoleic acid, linolenic acid, arachidonic acid, eicosapentaenoic acid, docosahexaenoic acid, and sorbic acid; hydroxy acids such as lactic acid, malic acid, and citric acid; aromatic carboxylic acids such as benzoic acid, phthalic acid, isophthalic acid, terephthalic acid, salicylic acid, gallic acid, melitic acid, and cinnamic acid; dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, fumaric acid, and maleic acid; tricarboxylic acids such as aconitic acid; oxocarboxylic acids such as pyruvic acid and oxaloacetate; carboxylic acid derivatives such as amino acids and nitrocarboxylic acids; and acid anhydrides such as trimellitic anhydride and pyromellitic anhydride. Low molecular weight compounds having acidic groups can be used in combination with the aforementioned acidic resins or known resins that constitute known primer layers to form a primer layer.

[0057] From the viewpoint of recoatability, the primer layer preferably contains a compound having an acidic group. Furthermore, from the viewpoint of printability, it is preferable to contain a urethane resin having an acidic group, an acrylic resin having an acidic group, or a rosin-modified resin.

[0058] (Urethane resin containing acidic groups) The urethane resin having acidic groups is not particularly limited, and for example, urethane resins described in JP 2020-90627, JP 2021-80431, etc., can be used as appropriate. An acid value derived from carboxyl groups can be imparted to the urethane resin, improving its desorption properties. The acid value of the urethane resin is preferably 15 mg KOH / g or more, more preferably 15 to 70 mg KOH / g, and even more preferably 20 to 50 mg KOH / g. A value of 15 mg KOH / g or more is preferred because it results in good desorption properties with desorption liquid, and a value of 70 mg KOH / g or less is preferred because it results in good substrate adhesion and retort resistance. The hydroxyl value of the urethane resin is preferably 1 to 35 mg KOH / g, more preferably 10 to 30 mg KOH / g. A value of 1 mg KOH / g or more is preferred because it results in good desorption properties with desorption liquid, and a value of 35 mg KOH / g or less is preferred because it results in good substrate adhesion.

[0059] The weight-average molecular weight of the urethane resin having acidic groups is preferably 10,000 to 100,000, more preferably 15,000 to 70,000, and even more preferably 15,000 to 50,000. The molecular weight distribution (Mw / Mn) of the urethane resin is preferably 6 or less. Mw represents the weight-average molecular weight, and Mn represents the number-average molecular weight. A molecular weight distribution of 6 or less results in excellent desorption properties and drying properties of the primer composition. Furthermore, the smaller the molecular weight distribution, i.e., the sharper the molecular weight distribution, the more uniformly the dissolution and peeling action by the desorption liquid occurs, improving the desorption properties of the polyester substrate. The molecular weight distribution is more preferably 5 or less, and even more preferably 4 or less. Furthermore, the molecular weight distribution is preferably 1.5 or more, and even more preferably 1.2 or more. In this invention, Mw, Mn, and molecular weight distribution (Mw / Mn) are polystyrene-equivalent values ​​determined by gel permeation chromatography (GPC).

[0060] Urethane resins having acidic groups may also have an amine value. When the urethane resin has an amine value, it is preferably 0.1 to 20 mg KOH / g, and more preferably 1 to 10 mg KOH / g. Within this range, excellent adhesion to the substrate is achieved.

[0061] The number of urethane bonds in the polyurethane resin having acidic groups is preferably 1 to 3 mmol / g, more preferably 1.5 to 2 mmol / g. The number of urea bonds is preferably 0 to 3 mmol / g, more preferably 0.2 to 1 mmol / g. The total number of urethane bonds and urea bonds is preferably 1 to 6 mmol / g, more preferably 1.7 to 3 mmol / g. By setting the number of urethane bonds and urea bonds within these ranges, the deleaciability and adhesion to the substrate are improved.

[0062] (Acrylic resin containing acidic groups) Examples of acrylic resins having acidic groups include polymers obtained by polymerizing monomers containing (meth)acrylic monomers having acidic groups such as (meth)acrylic acid and maleic acid; and resins obtained by polymerizing monomers containing (meth)acrylic monomers having hydroxyl groups or glycidyl groups, and then modifying those functional groups to introduce carboxyl groups (for example, maleic anhydride modified resins). The acid value of the acrylic resin having an acidic group is preferably 50 mg KOH / g or more, more preferably 100 mg KOH / g or more.

[0063] (Rosin-modified resin) Rosin-modified resins are resins prepared using rosin as one of the raw materials. Rosin contains a mixture of resin acids such as abietic acid, palastic acid, isopimal acid, and levopimal acid. These resin acids contain hydrophilic and chemically active carboxyl groups, and some also possess conjugated double bonds. Therefore, various rosin-modified resins are prepared by combining polyhydric alcohols and polybasic acids for condensation polymerization, by adding resol (a phenol condensate) to the benzene ring contained in the rosin skeleton, or by performing a Diels-Alder reaction with dienophiles such as maleic anhydride or maleic acid to add a maleic acid or maleic anhydride skeleton. Various types of such rosin-modified resins are commercially available and can be obtained and used.

[0064] Examples of rosin-modified resins include maleated rosin, fumarated rosin, rosin-modified maleic acid resin, rosin-modified fumaric acid resin, rosin-modified phenolic resin, rosin-modified alkyd resin, and rosin-modified polyester resin. In the present invention, any of these rosin-modified resins may be used, but among them, those that contain a moiety in their structure derived from at least one selected from the group consisting of maleic acid, maleic anhydride, fumaric acid, and fumaric anhydride are preferably used. A resin that "contains a moiety in its structure derived from at least one selected from the group consisting of maleic acid, maleic anhydride, fumaric acid, and fumaric anhydride" is a resin prepared using at least one selected from the group consisting of maleic acid, maleic anhydride, fumaric acid, and fumaric anhydride as part of the raw materials. Examples include rosin-modified maleic acid resins and rosin-modified fumaric acid resins obtained by condensation polymerization of maleic acid or fumaric acid as part of the polybasic acid, maleated rosin and fumarated rosin having a structure obtained by adding maleic acid, maleic anhydride, fumaric acid, or fumaric anhydride as a dienophile in a Diels-Alder reaction, and resins obtained by further polymerization of other chemical species using the functional groups contained therein. The acid value of the rosin-modified resin is preferably 10 to 400 mg KOH / g, and more preferably 100 to 300 mg KOH / g.

[0065] <Method for manufacturing recycled plastics> The present invention provides a method for producing recycled plastics, comprising at least a step 1 to obtain a laminate (B), and a step 2 to melt and knead the material.

[0066] <Step 1 to obtain the laminate (B)> Step 1 for obtaining the laminate (B) of the present invention includes immersing the packaging material (A) in a desorption solution containing a surfactant and recovering the laminate (B) from which the printed layer has been removed. When the packaging material (A) is immersed in the desorption solution, it is preferable that the printed layer is exposed in its cross-section. For this reason, it is more preferable to include a step of fragmenting the packaging material (A) by cutting or crushing. Furthermore, it is preferable that the laminate (B) obtained by detaching and recovering the printed layer from the packaging material (A) is further subjected to washing, dewatering, and drying. In this invention, "detachment" refers to the detachment of the printed layer from the plastic laminate by a detachment solution, and includes both forms: (1) when the detachment layer dissolves and the plastic laminate detaches, and (2) when the detachment layer does not dissolve but peels off due to neutralization, swelling, etc., and the plastic laminate detaches.

[0067] <Laminated body (B)> In this invention, the laminate (B) is specifically obtained by removing 85% or more of the printed layer of the packaging material (A) from 100% by mass, more preferably 90% or more by mass, even more preferably 95% or more by mass, and particularly preferably 99% or more by mass. By removing 85% or more by mass of the printed layer, a high-quality recycled plastic with less discoloration and foreign matter can be obtained.

[0068] Furthermore, halogen elements derived from the printing layer and adhesive layer that may be contained in the laminate (B) may generate halogen gases or acidic gases such as hydrogen chloride during pellet manufacturing, potentially damaging equipment or endangering human health. Moreover, if air bubbles are generated during pellet manufacturing, when molded products are manufactured using the manufactured pellets, surface irregularities are likely to occur, potentially degrading the surface condition of the molded products. For this reason, the chlorine content of the laminate (B) is preferably 0.4% by mass or less, preferably 0.2% by mass or less, and even more preferably 0.1% by mass or less of the total mass of the laminate.

[0069] The chlorine content in the laminate (B) can be measured using known methods such as ion chromatography (IC) or ICP-MS.

[0070] <Separated liquid> The desorption solution only needs to contain water and a surfactant, and it desorbs the printed layer. The desorption solution can be appropriately selected considering the ease of desorption of the printed layer, as described later. Examples of such desorption solutions include water containing a surfactant, a basic aqueous solution, and an acidic aqueous solution, but water is preferred considering the hydrolysis properties of polyester. These desorption solutions may be heated. Furthermore, the desorption solution may contain other components besides the surfactant, as long as it does not impair the effects of the present invention. Examples of other components include defoamers, and the appropriate type and amount can be selected and used according to the required characteristics.

[0071] The temperature of the desorption solution when immersing the packaging material (A) is preferably in the range of 25 to 120°C, more preferably 30 to 120°C, and particularly preferably 30 to 80°C. The immersion time in the desorption solution is preferably in the range of 1 minute to 24 hours, more preferably 1 minute to 12 hours, and preferably 1 minute to 6 hours. The amount of desorption solution used is preferably in the range of 50,000 to 100,000 times the mass of the packaging material (A), more preferably 100,000 to 10,000 times, and it is preferable to stir or circulate the desorption solution in order to improve the desorption efficiency. The rotation speed is preferably 80 to 5,000 rpm, more preferably 80 to 4,000 rpm.

[0072] <Surfactants> The desorbing liquid in the present invention contains a surfactant. From the viewpoint of desorbing the printed layer, anionic surfactants, cationic surfactants, amphoteric surfactants, and nonionic surfactants are preferred, at least one selected from the group consisting of nonionic surfactants, amphoteric surfactants, and anionic surfactants is more preferred, and nonionic surfactants are particularly preferred.

[0073] Surfactants primarily play a role in improving the desorption properties of the printed layer. This is thought to be because the surfactant facilitates the penetration of the desorption liquid into the printed layer, thereby promoting desorption. Furthermore, it is believed that the surfactant adsorbs onto the desorbed components and the surface of the substrate, preventing the re-adhesion of the finely dispersed printed layer and other materials. Furthermore, as the amount of packaging material (A) relative to the desorption liquid is increased, the plastic laminate tends to curl, trapping the desorbed ink fragments, making it difficult to cleanly remove the ink fragments trapped in the curl. However, when the desorption liquid contains a surfactant, the surfactant is adsorbed onto the surface of the plastic laminate, suppressing curling. As a result, desorption is improved, and re-adhesion is suppressed.

[0074] The HLB value of a surfactant can be expressed as an index value related to its affinity for water and oil. The HLB value is an index value related to the affinity of a surfactant for water and oil, and is calculated by dividing the HLB value of a substance without hydrophilic groups into 0 and the HLB value of a substance with only hydrophilic groups into 20. The concept of HLB was proposed in 1949 by William Griffin of Atlas Powder Company. Several methods for determining the HLB value by calculation have been proposed. For example, there are the Griffin method, Atlas method, Davis method, and Kawakami method. For the nonionic surfactant used in this invention, the HLB value calculated using the Griffin method was adopted. For the ionic surfactant, the HLB value calculated using the Davis method was adopted.

[0075] In this invention, surfactants with an HLB value of 3 or higher are preferred, and preferably 7 or higher. An HLB value of 7 or higher exhibits excellent deinking and readhesion properties as described above. The HLB value of nonionic surfactants is preferably 8 or higher, more preferably 10 or higher. Furthermore, the HLB value of surfactants is preferably 20 or lower, more preferably 19 or lower, and even more preferably 17 or lower. An HLB value of 20 or lower is preferred because it exhibits excellent foam suppression.

[0076] The surfactant may be used alone or in combination of two or more types. The surfactant content of the eluent is preferably in the range of 0.1 to 10% by mass, and more preferably in the range of 0.3 to 5% by mass, based on the mass of the eluent. A content of 0.1% by mass or more is preferable because it provides excellent deinking and re-adhesion properties, and a content of 10% by mass or less is preferable from the viewpoint of suppressing foaming.

[0077] [Nonionic surfactants] The nonionic surfactant is not particularly limited, but is preferably an alkylene oxide adduct to which alkylene oxide (hereinafter also referred to as AO) has been added. More preferably, it is a compound obtained by adding alkylene oxide to alcohols having active hydrogen, a compound obtained by adding alkylene oxide to amines, or a compound obtained by adding alkylene oxide to fatty acids. The above addition may be random addition or block addition. The number of carbon atoms in the alkylene oxide is preferably 2 to 4. More preferably, the nonionic surfactant is an alcohol-based nonionic surfactant obtained by adding an alkylene oxide having 2 to 4 carbon atoms to an alcohol.

[0078] (Alcohol-based nonionic surfactant) Examples of alcohol-based nonionic surfactants include alkylene oxide adducts of primary or secondary alcohols having a total of 8 to 24 carbon atoms, or alkylene oxide adducts of alkylphenols having a total of 8 to 12 carbon atoms. The primary or secondary alcohols having a total of 8 to 24 carbon atoms may be saturated or unsaturated. Examples of primary or secondary alcohols with a total of 8 to 24 carbon atoms include lauryl alcohol, stearyl alcohol, oleyl alcohol, dodecyl alcohol, arachidyl alcohol, behenyl alcohol, lignoceryl alcohol, myristyl alcohol, and the like. Furthermore, examples of alkylene oxides to be added to alcohols include ethylene oxide, propylene oxide, and butylene oxide, with ethylene oxide being preferred as essential. The number of moles of alkylene oxide to be added is preferably 1 to 100 moles, more preferably 2 to 50 moles, per mole of alcohol or alkylphenol. This range is particularly preferred because it exhibits excellent desorption properties.

[0079] (Fatty acid-based nonionic surfactant) The structure of the fatty acid-based nonionic surfactant is not particularly limited, but examples include alkylene oxide adducts of higher fatty acids having a total of 10 to 24 carbon atoms, oils and fats consisting of esters of the aforementioned saturated or unsaturated higher fatty acids having a total of 10 to 24 carbon atoms with glycerol, and alkylene oxide adducts of mixtures of the aforementioned oils and fats with 2 to 10 polyhydric alcohols. The above higher fatty acids having a total of 10 to 24 carbon atoms may be either saturated or unsaturated. Examples of higher fatty acids with a total of 10 to 24 carbon atoms include saturated higher fatty acids such as lauric acid, myristic acid, palmitic acid, stearic acid, arachidic acid, and behenic acid; and unsaturated higher fatty acids such as palmitoleic acid, oleic acid, elaidic acid, linoleic acid, linolenic acid, erucic acid, and ricinoleic acid. Examples of polyhydric alcohols with a total of 2 to 10 valencies include ethylene glycol, propylene glycol, glycerin, polyglycerin, sorbitol, sorbitan, and sucrose. The type and number of moles of alkylene oxide added are the same as described in the section on [alcohol-based nonionic surfactants] above.

[0080] (Amine-based nonionic surfactant) Examples of amine-based nonionic surfactants include AO adducts of saturated or unsaturated primary or secondary amines with a total of 8 to 36 carbon atoms. Examples of amines include 2-ethylhexylamine, di-2-ethylhexylamine, laurylamine, dilaurylamine, tetradecylamine, ditetradecylamine, hexadecylamine, dihexadecylamine, stearylamine, distearylamine, oleylamine, and dioleylamine. The type of AO and the number of moles added are the same as described above.

[0081] [Anionic surfactants] Anionic surfactants are preferably non-soap-based, and examples include sulfonic acid-based anionic surfactants, sulfate ester-based anionic surfactants, carboxylic acid-based anionic surfactants, and phosphate ester-based anionic surfactants.

[0082] (Sulfonic acid-based anionic surfactant) Examples of the above-mentioned sulfonic acid-based anionic surfactants include alkyl sulfonic acid, alkylbenzene sulfonic acid, alkyl naphthalene sulfonic acid, alkyl diphenyl ether disulfonic acid, alkyl methyl taurine, sulfosuccinate diesters, alkylene oxide adducts of sulfonic acid, and salts thereof. Specific examples include hexane sulfonic acid, octanesulfonic acid, decane sulfonic acid, dodecane sulfonic acid, toluene sulfonic acid, cumene sulfonic acid, octylbenzene sulfonic acid, dodecylbenzene sulfonic acid, dinitrobenzene sulfonic acid, and lauryl dodecylphenyl ether disulfonic acid.

[0083] (Sulfate-based anionic surfactant) Examples of the above-mentioned sulfate ester-based anionic surfactants include sulfate esters (alkyl ether sulfates), alkylene oxide adducts of sulfate esters, and salts thereof. Specific examples include lauryl sulfate, myristyl sulfate, and polyoxyethylene lauryl ether sulfate.

[0084] (Carboxylic acid-based anionic surfactant) Examples of the carboxylic acid-based anionic surfactants mentioned above include alkyl carboxylic acids, alkylbenzene carboxylic acids, alkylene oxide adducts of carboxylic acids, and salts thereof. Specific examples include lauric acid, myristic acid, palmitic acid, stearic acid, polyoxyethylene lauryl ether acetate, and polyoxyethylene tridecyl ether acetate.

[0085] (Phosphate ester-based anionic surfactant) Examples of the above-mentioned phosphate ester-based anionic surfactants include phosphate esters (alkyl ether phosphate esters), alkylene oxide adducts of phosphate esters, and salts thereof. Specific examples include octyl phosphate esters, lauryl phosphate esters, tridecyl phosphate esters, myristyl phosphate esters, cetyl phosphate esters, stearyl phosphate esters, polyoxyethylene octyl ether phosphate esters, and polyoxyethylene lauryl ether phosphate esters.

[0086] The anionic surfactant preferably has an alkyl group having 2 to 24 carbon atoms or an alkenyl group having 2 to 24 carbon atoms, and more preferably has an alkyl group having 8 to 18 carbon atoms. The alkyl group or alkenyl group may be linear or branched. Furthermore, when the anionic surfactant is an alkylene oxide adduct, examples of the alkylene oxide include ethylene oxide, propylene oxide, and butylene oxide, with ethylene oxide being preferred. The number of moles of alkylene oxide added is preferably 1 to 12 moles, more preferably 1 to 8 moles, per mole of alcohol or alkylphenol. This range is particularly preferred because it exhibits excellent desorption properties.

[0087] Examples of salts that constitute the anionic surfactants described above include metal salts such as sodium, potassium, magnesium, and calcium. These salts may be used individually or in combination of two or more. Among these, anionic surfactants are preferably sulfonate type or phosphate type, from the viewpoint of desorption and readhesion, and more preferably alkyl sulfonate, polyoxyalkylene alkyl ether sulfonate, polyoxyalkylene alkyl ether phosphate, etc.

[0088] [Cationic surfactants] Examples of cationic surfactants include alkylamine salts and quaternary ammonium salts. Specifically, stearylamine acetate, trimethyl coconut ammonium chloride, trimethyl beef tallow ammonium chloride, dimethyl dioleyl ammonium chloride, methyl oleyl diethanol chloride, tetramethyl ammonium chloride, laurylpyridinium chloride, laurylpyridinium bromide, laurylpyridinium disulfate, cetylpyridinium bromide, 4-alkyl mercaptopyridine, poly(vinylpyridine)-dodecyl bromide, dodecylbenzyltriethylammonium chloride, etc. can be used.

[0089] [Amphoteric surfactants] Examples of amphoteric surfactants include lauryldimethylaminoacetic acid betaine, 2-alkyl-N-carboxymethyl-N-hydroxyethylimidazolinium betaine, coconut oil fatty acid amidopropyl dimethylaminoacetic acid betaine, polyoctyl polyaminoethylglycine, and imidazoline derivatives.

[0090] These surfactants may be used individually in the desorbent solution, or two or more may be used in combination. The total surfactant content in the desorbent solution, based on the total mass of the desorbent solution, is preferably in the range of 0.1 to 10% by mass, and more preferably in the range of 0.3 to 5% by mass. A content of 0.1% by mass or more is preferable because it provides excellent deinking and re-adhesion properties, while a content of 10% by mass or less is preferable from the viewpoint of suppressing foaming.

[0091] [Antifoaming agent] Defoaming agents generally have extremely high lipophilicity, and in this invention, the defoaming agent refers to one with an HLB value in the range of 1 to less than 3. When used in combination with the above-mentioned surfactant, it can exhibit good defoaming properties without reducing delamination and readhesion, and can suppress foaming caused by the surfactant. Examples of the above-mentioned defoaming agents include silicone-based compounds and non-silicone-based compounds.

[0092] (Silicone-based compounds) Examples of the above-mentioned silicone compounds include emulsion type, self-emulsifying type, oil type, oil compound type, and solvent type. Emulsion-type silicone defoamers are silicone-based defoamers that are formed by emulsifying a silicone oil compound with an activator to create an O / W type emulsion. Examples include "KM-89" and "KM-98" from Shin-Etsu Chemical Co., Ltd., "FC2913" and "SILFOAM SE47" from Asahi Kasei Wacker Silicone Co., Ltd., and "BYK-015" and "BYK-1640" from Big Chemie Japan Co., Ltd. Self-emulsifying silicone-based defoamers are 100% active ingredients that form an emulsion when diluted and mixed with water. Examples include "KS-540" and "X-50-1176" from Shin-Etsu Chemical Co., Ltd., and "SILFOAM SD670" and "SILFOAM SD850" from Asahi Kasei Wacker Silicone Co., Ltd. Oil-type defoamers are 100% silicone oil defoamers that do not contain solvents or additives. Examples include "KM-89" and "KM-98" from Shin-Etsu Chemical Co., Ltd., "AK350" and "AK12500" from Asahi Kasei Wacker Silicone Co., Ltd., and "BYK-1770" from Big Chemie Japan Co., Ltd. Oil compound type defoamers are silicone-based defoamers that combine silicone oil with silica particles. Examples include "KM-89" and "KM-98" from Shin-Etsu Chemical Co., Ltd., "SILFOAM SC370" and "PULPSIL22274VP" from Asahi Kasei Wacker Silicone, and "BYK-017" and "BYK-018" from Big Chemie Japan. Solvent-type defoamers are silicone-based defoamers in which silicone oil is dissolved in a solvent. Examples include "KM-89" and "KM-98" from Shin-Etsu Chemical Co., Ltd., and "BYK-019" and "BYK-025" from Big Chemie Japan.

[0093] (Non-silicone compounds) Examples of the above-mentioned non-silicone compounds include fatty acid ester compounds, urea resin compounds, paraffin compounds, polyoxyalkylene glycol compounds, acrylic ester copolymers, ester polymers, ether polymers, amide polymers, emulsified mineral oils, polysiloxane adducts, fluorine compounds, vinyl polymers, acetylene alcohol, acrylic polymers, special vinyl polymers, ethylene glycol, and higher alcohols (octyl alcohol, cyclohexanol, etc.).

[0094] The defoaming agent may be used alone or in combination of two or more types. The defoaming agent content in the detached liquid is preferably in the range of 0.01 to 5% by mass, and more preferably in the range of 0.03 to 3% by mass, based on the total mass of the detached liquid. A content of 0.01% by mass or more provides excellent foam suppression, while a content of 5% by mass or less provides excellent deinking and re-adhesion properties. From the viewpoint of not reducing deinking properties or re-adhesion properties when combined with the above-mentioned surfactants with an HLB of 7 or higher, the defoaming agent is preferably at least one selected from the group consisting of emulsion-type silicone compounds, self-emulsifying silicone compounds, and non-silicone compounds.

[0095] <Process of fragmentation by cutting or crushing> Embodiments of the present invention preferably include a step of fragmenting the packaging material (A) by cutting or crushing. By fragmenting the packaging material (A) by cutting or crushing, the printed layer can be detached from the packaging material (A) in a shorter time. More specifically, the detachment liquid penetrates from the surface and edges of the packaging material (A), comes into contact with the printed layer, and detaches the printed layer by dissolving or swelling it. Therefore, it is preferable that the packaging material (A) is fragmented by cutting or crushing and the printed layer is exposed in the cross-section when immersed in the detachment liquid.

[0096] To fragment the shape of the packaging material (A), cutting or crushing is effective. The cutting or crushing method is not particularly limited and examples include using a jaw crusher, impact crusher, cutter mill, stamp mill, ring mill, roller mill, jet mill, or hammer mill. The size of the fragments of the packaging material (A) is preferably 5 mm to 60 mm in side length, more preferably 10 mm to 50 mm, and even more preferably 20 mm to 40 mm. If the size is 5 mm or larger, the stretching of the sealant due to stress during cutting or crushing can be suppressed. Stretching of the sealant reduces the exposure of the printed layer on the cross-section of the packaging material (A), which can reduce the immersion efficiency during delamination or impair delamination properties. If the crushing size is 60 mm or less, the exposed area of ​​the printed layer of the packaging material (A) increases, which promotes contact and penetration of the delamination liquid and shortens the time of the delamination process. Furthermore, in order to prevent a decrease in the molecular weight of the polyester, it is preferable to crush the material at a temperature of 220°C or lower, more preferably at a temperature of 200°C or lower, and even more preferably at a temperature of 180°C or lower.

[0097] <Washing, dewatering, and drying process> Embodiments of the present invention preferably include a step of detaching the printed layer from the packaging material (A), recovering the laminate (B) obtained therefrom, washing the attached detached liquid with water, dewatering, and drying. The washing method can be a batch type or a continuous type, and water, detergent, neutralizing agent, or alkaline aqueous solution may be used. Centrifugal dewatering is preferred as the dewatering method, and hot air drying is preferred as the drying method. The purpose of adjusting the moisture content in the laminate (B) is to prevent foaming of the recycled plastic obtained by the extruder. If bubbles occur during pellet production, when molded products are manufactured using the manufactured pellets, surface irregularities are likely to occur, potentially degrading the surface condition of the molded products. Furthermore, if the polyester undergoes hydrolysis due to the effects of moisture, the molecular weight decreases, reducing viscosity during injection molding and making it difficult to manufacture molded products. The moisture content in the laminate (B) is preferably 0.2% by mass or less, more preferably 0.1% by mass or less, and even more preferably 0.05% by mass or less.

[0098] <Step 2: Melting and kneading> The laminate (B) obtained in step 1 is melted and kneaded using an extrusion device equipped with a screw and a discharge unit.

[0099] [Extrusion device equipped with a screw and a discharge section] The extrusion apparatus used in the present invention is equipped with a screw. The extrusion apparatus is a device that can melt and mold commonly used thermoplastic resins, etc., and for example, a known extrusion apparatus described in Japanese Patent Application Publication No. 2017-148997 can be used. Specifically, it has a supply port for supplying materials, a melt-kneading section for melting and kneading materials such as thermoplastic resin supplied from the supply port, and a discharge section for discharging the thermoplastic resin that has been melted and kneaded in the melt-kneading section. The melting and mixing section is equipped with a screw, and the material is melted and mixed by shear heat generated by the rotation of the screw, a heat source such as an electric heater, and the material itself. The molten material passes through the mesh of the discharge section and is discharged. Examples of the extrusion device include a twin-screw extruder, a single-screw extruder, and a rotor-type twin-screw mixer.

[0100] Embodiments of the present invention more specifically include the steps of supplying a laminate (B) from a supply port, melting and kneading the laminate (B) supplied from the supply port to form a resin composition (b), discharging the resin composition (b) that has been melted and kneaded in a melt-kneading section, and cooling the resin composition (b) that has been discharged from the discharge section to 40°C or below, and it is preferable to obtain recycled plastic.

[0101] [Process of supplying from the supply port] The laminate (B) obtained in step 1 is supplied from the feed port of the extruder. If necessary, various additives may be added to the laminate (B) before processing with the extruder. Mixing of the laminate (B) with optional components can be performed using a Henschel mixer, tumbler, disper, etc.

[0102] (Additives) The recycled plastic of the present invention may contain known additives, etc., to the extent that they do not impair the effects of the present invention. Examples of additives include modifiers. Modifiers suppress the decrease in viscosity of the recycled plastic due to the hydrolysis of polyester resin. Examples of modifiers include carbodiimide compounds and acrylic compounds. Other additives include at least one antioxidant selected from the group consisting of phenolic and phosphorus-based agents; at least one lubricant selected from the group consisting of fatty acid amides, alkylene fatty acid amides, metal soaps, and esters; hindered amine-based weather stabilizers; waxes with an acid value of 5 mg KOH / g or less; and at least one antistatic agent selected from the group consisting of fatty acid sulfonates and fatty acid esters.

[0103] [Step to obtain resin composition (b)] The laminate (B) supplied from the supply port is heated, melted, and kneaded in the melt-kneading section of the extruder to become a resin composition (b). The temperature range in this process must take into account the glass transition temperature of the laminate (B), the melting temperature, the shape of the recycled plastic, and the pressure applied during the molding process. The melting temperature is preferably 260 to 290°C, and more preferably 270 to 290°C. At this temperature range, it is heated, melted, and kneaded to become a uniform recycled plastic.

[0104] Furthermore, the rotation speed of the screw during kneading is preferably 50 to 1000 RPM. More preferably 80 to 800 RPM, and even more preferably 100 to 500 RPM. Within this range, it is possible to suppress the generation of insoluble matter and burning in the resin composition (b) and thus the recycled plastic, and to obtain recycled plastic with high mechanical properties. As a result, good moldability can be maintained.

[0105] [Step of dispensing resin composition (b)] In the melt-kneading section of the extruder, the resin composition (b) is heated, melted, and kneaded, and the resulting resin composition (b) is discharged from the tip discharge section of the extruder. In the process of discharging the resin composition (b), the pressure at the tip discharge section of the extruder is preferably 15 MPa or less, more preferably 10 MPa, and even more preferably 8 MPa. This pressure makes it difficult for impurities to be included, and recycled plastic with stable purity can be continuously obtained. In the discharge section of the extruder, it is preferable to use a screen mesh (metal mesh) to remove foreign matter from the pellets to be formed. The type of screen mesh (metal mesh) is not particularly limited, and examples include woven types such as plain weave, twill weave, plain tatami weave and twill tatami, and perforated metal type, but plain weave is preferred. The size of the screen mesh is preferably 40 mesh or more, more preferably 80 mesh or more, and even more preferably 120 mesh or more, taking into consideration the pressure of the discharge section and clogging.

[0106] [Cooling process] Methods for cooling the extruded resin composition (b) include, for example, air cooling, wind cooling, and water cooling. It is preferable to cool the extruded resin composition (b) to 20°C to 80°C, and more preferably to 30°C to 60°C. It is also preferable to shred the extruded resin composition (b) before and / or after cooling. Examples of shredding methods include, but are not particularly limited to, hot cutting and strand cutting methods. The shape of the recycled plastic is not particularly limited and can be rod-shaped, granular, cubic, rectangular, irregular, etc.

[0107] <Molded products> The recycled plastic obtained by the manufacturing method described above can be used, for example, as a molding material to obtain molded products by heat molding. The heat molding method is not particularly limited and examples include injection molding, extrusion molding, blow molding, and compression molding. The molding material produced using the recycled plastic of the present invention is of high quality because the printed layer is removed and the re-adhesion of the removed components is suppressed. It can be used in a variety of fields, such as home appliances, stationery, automotive parts, toys, sporting goods, medical supplies, and building materials. [Examples]

[0108] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the present invention, parts and % refer to parts by mass and mass %, respectively, unless otherwise noted.

[0109] <Molecular weight and molecular weight distribution> The weight-average molecular weight (Mw), number-average molecular weight (Mn), and molecular weight distribution (Mw / Mn) are G Measurement was performed using PC (gel permeation chromatography), and polystyrene was labeled. The molecular weight was determined as the converted molecular weight used for the quasi-substance. The measurement conditions are shown below. GPC device: Showa Denko Shodex GPC-104 Columns: The following columns were used, connected in series. Two Shodex LF-404 tubes manufactured by Showa Denko. Showa Denko Shodex LF-G Detector: RI (Differential Refractometer) Measurement conditions: Column temperature 40°C Eluent: Tetrahydrofuran Flow rate: 0.3mL / min

[0110] <Acid value, hydroxyl value> The acid value and hydroxyl value were measured according to the method described in JIS K 0070 (1992).

[0111] <Chlorine content> The chlorine content was measured in accordance with JIS K0127 (2013). Specifically, the pulverized dried laminate (B) was pretreated by combustion, and the chlorine content of the resulting sample was quantified by ion chromatography to determine the chlorine content.

[0112] <Moisture content measurement method> The moisture content of the dried laminate (B) was measured in accordance with JIS K 0068 (2001). The measuring equipment and reagents are shown below. Measuring instrument: Karl Fischer moisture meter MKC-710D (manufactured by Kyoto Electronics Manufacturing Co., Ltd.) : Moisture vaporizer ADP-611 (manufactured by Kyoto Electronics Manufacturing Co., Ltd.) Karl Fischer Reagent: ChemAqua Water Standard 1 (manufactured by Kyoto Electronics Manufacturing Co., Ltd.)

[0113] <Measurement of total light transmittance> In accordance with JIS K7361, the total light transmittance was measured using HazeGuard Plus (manufactured by Gardner).

[0114] <Primer manufacturing> [Synthesis Example 1-1] (Polyurethane resin P1) In a reactor equipped with a reflux condenser, dropping funnel, gas inlet tube, stirrer, and thermometer, nitrogen gas was introduced while 108.6 parts of PPA (polyester polyol with a number average molecular weight of 2,000, consisting of a polycondensate of propylene glycol and adipic acid), 40.7 parts of PEG (polyether polyol with a number average molecular weight of 2,000, consisting of polyethylene glycol), 28.3 parts of DMPA (2,2-dimethylolpropanoic acid), 105.7 parts of IPDI (isophorone diisocyanate), and 200 parts of NPAC (n-propyl acetate) were charged. The mixture was reacted at 90°C for 5 hours to obtain a prepolymer solution having isocyanate groups at the ends. Next, a mixture of 16.7 parts AEA (2-(2-aminoethylamino)ethanol) and 150 parts IPA (isopropyl alcohol) was added dropwise at room temperature over 60 minutes. Then, 10.0 parts of 28% aqueous ammonia and 690 parts of deionized water were gradually added to neutralize the carboxyl groups in the resin, thereby making it water-soluble. Next, NPAC and IPA were removed by vacuum distillation to obtain an aqueous solution of polyurethane resin P3 with a solid content of 30%, a weight-average molecular weight of 32,000, Mw / Mn = 3.3, and an acid value of 39.3 mgKOH / g. However, the acid value of P1 is the value before neutralization.

[0115] [Synthesis Example 1-2] (Polyurethane resin P2) In a reactor equipped with a reflux condenser, dropping funnel, gas inlet tube, stirrer, and thermometer, 135.7 parts of PPA, 13.6 parts of PPG (polyether polyol made of polypropylene glycol with a number average molecular weight of 2,000), 28.3 parts of DMPA, 105.7 parts of IPDI, and 200 parts of NPAC were charged while introducing nitrogen gas, and the mixture was reacted at 90°C for 5 hours to obtain a urethane prepolymer solution having isocyanate groups at the ends. Next, a mixture of 16.7 parts AEA and 350 parts IPA was added dropwise at room temperature over 60 minutes, and then the mixture was reacted at 70°C for 3 hours to obtain a polyurethane resin solution. The obtained polyurethane resin solution was mixed with NPAC to adjust the solid content, resulting in a polyurethane resin P2 solution with a solid content concentration of 30%, a weight-average molecular weight of 30,000, Mw / Mn = 3.0, and an acid value of 39.3 mgKOH / g.

[0116] [Synthesis Example 1-3] (Polyurethane resin P3) Solutions of polyurethane resin P3 were obtained using the same method as in Synthesis Example 1-2, except that the raw materials and quantities listed in Table 1 were used.

[0117] [Table 1]

[0118] The abbreviations used in Table 1 are shown below. PPA: A polyester polyol with a number average molecular weight of 2,000, consisting of a polycondensate of propylene glycol and adipic acid. PPG: A polyether polyol with a number average molecular weight of 2,000, composed of polypropylene glycol. PEG: A polyether polyol composed of polyethylene glycol with a number average molecular weight of 2,000. DMPA: 2,2-Dimethylolpropanoic acid BD:1,4-butanediol IPDI: Isophorone diisocyanate NPAC: n-propyl acetate AEA: 2-(2-aminoethylamino)ethanol IPA: Isopropyl alcohol

[0119] <Primer preparation> [Preparation Example 2-1] (Primer S1) Primer S1 was obtained by stirring and mixing 87 parts of polyurethane resin P1 solution, 10 parts of water, and 3 parts of silica particles (P-73, manufactured by Mizusawa Chemical Co., Ltd.: hydrophilic silica particles with an average particle size of 3.8 μm) using a disperser.

[0120] [Preparation Examples 2-2, 2-3] (Primers S2, S3) Primers S2 and S3 were obtained using the same method as in Preparation Example 2-1, except that the raw materials and mixing ratios shown in Table 2 were changed.

[0121] [Table 2]

[0122] The abbreviations used in Table 2 are shown below. EA: Ethyl acetate IPA: Isopropyl alcohol

[0123] <Ink manufacturing> (Synthesis of urethane resin I1) In a reactor equipped with a reflux condenser, dropping funnel, gas inlet tube, stirrer, and thermometer, 103.2 parts of polyester polyol, a condensate of 3-methyl-1,5-pentanediol and sebacic acid with a number average molecular weight of 2000, 35.2 parts of neopentyl glycol, 121.4 parts of isophorone diisocyanate, 0.03 parts of stannous 2-ethylhexylate, and 65.1 parts of ethyl acetate were charged. The mixture was reacted at 90°C for 2 hours under a nitrogen atmosphere, and 165.3 parts of ethyl acetate was added and cooled to obtain 490.2 parts of a solvent solution of the terminal isocyanate prepolymer. Next, the obtained 490.2 parts of the terminal isocyanate prepolymer was gradually added at room temperature to a mixture of 33.6 parts of isophorone diamine, 1.2 parts of di-n-butylamine, 237.5 parts of ethyl acetate, and 200.6 parts of isopropyl alcohol, and the mixture was then reacted at 50°C for 1 hour. Subsequently, 5.3 parts of isophorone diisocyanate were added to adjust the viscosity, and then the solid content was adjusted to 30% with a solvent of ethyl acetate / isopropyl alcohol mixed in a mass ratio of 1 / 2, yielding a urethane resin I1 solution with an amine value of 8.2 mg KOH / g, an acid value of 0.2 mg KOH / g, and a weight-average molecular weight of 40,000.

[0124] (Polyamide resin I2) Twenty parts of polyamide resin I2 (weight-average molecular weight 15,000) were mixed and dissolved in 80 parts of a mixed solvent consisting of methylcyclohexane:isopropyl alcohol = 70:30 (weight ratio) to obtain a polyamide resin I2 solution with a solid content of 30%. The polyamide resin contains constituent units derived from polymerized fatty acids and / or dimer acids, and has an amine value of 3.0 mg KOH / g, an acid value of 1.0 mg KOH / g, and a softening point of 110°C.

[0125] (Vinyl chloride-vinyl acetate copolymer (PVC) solution) Thirty parts of vinyl chloride-vinyl acetate copolymer resin (manufactured by Nisshin Chemical Co., Ltd., product name Solvine TA5R) were mixed and dissolved in 70 parts of ethyl acetate to obtain a vinyl chloride-vinyl acetate copolymer resin solution (abbreviated as PVC solution) with a solid content of 30%.

[0126] (Cellulose resin solution) 43 parts of nitrocellulose isopropyl alcohol-wetted product (Nobel Enterprises, product name DLX5-8) were mixed and dissolved in 57 parts of a mixed solvent consisting of ethyl acetate and ethanol in a 50:50 (weight ratio) mixture to obtain a nitrocellulose solution with a solid content of 30%.

[0127] [Preparation Example 3-1] (Ink R1) Ten parts of blue pigment PB15 (CIPigment Blue 15), twenty-five parts of polyurethane resin I1 solution, five parts of PVC solution, ten parts of EA, and ten parts of IPA were mixed and stirred, and dispersed for 20 minutes using a sand mill as a bead mill. Subsequently, ten parts of polyurethane resin I1 solution, fifteen parts of EA, and fifteen parts of IPA were mixed and stirred to obtain ink R1. Table 3 shows the total amount of each compound in the dispersion and post-compounding stages.

[0128] [Preparation Examples 3-2 to 3-4] (Ink R2 to R4) Inks R2 to R4 were obtained using the same method as in ink preparation example 3-1, except that the raw materials and mixing ratios shown in Table 3 were used. The mixing amounts in Table 3 are the sum of the mixing during dispersion and the mixing afterward.

[0129] [Table 3]

[0130] The abbreviations used in Table 3 are shown below.

[0131] PB15: CIPigment Blue 15 EA: Ethyl acetate IPA: Isopropyl alcohol

[0132] <Adhesive manufacturing> [Production Example 4-1] (Polyol Solution B1) In a reaction vessel equipped with a stirrer, thermometer, reflux condenser, dropping tank, and nitrogen gas inlet, 188 parts ethylene glycol, 316 parts neopentyl glycol, 179 parts 1,6-hexanediol, 315 parts terephthalic acid, 315 parts isophthalic acid, 64 parts adipic acid, and 323 parts sebacic acid were charged. The mixture was heated to 250°C while stirring under a nitrogen stream, and the esterification reaction was carried out. After a predetermined amount of water was distilled off, the pressure was gradually reduced, and the deglycolization reaction was carried out at a pressure of 1 mmHg or less for 5 hours to obtain a polyester polyol. Subsequently, 8.5 parts isophorone diisocyanate was gradually added, and the reaction was carried out at 150°C for approximately 2 hours to obtain a polyester polyurethane polyol. 0.4 parts trimellitic anhydride was added to 100 parts of this polyester polyurethane polyol, and the mixture was reacted at 180°C for about 2 hours. After that, the mixture was diluted with ethyl acetate until the solid content concentration reached 50%, thereby obtaining polyol solution B1 containing a partially acid-modified polyester polyol with an acid value of 2.2 mg KOH / g.

[0133] [Manufacturing Example 4-2] (Polyol Solution B2) In a reaction vessel equipped with a stirrer, thermometer, reflux condenser, dropping tank, and nitrogen gas inlet, 682 parts isophthalic acid, 274 parts sebacic acid, 72 parts adipic acid, 202 parts ethylene glycol, 506 parts neopentyl glycol, and 493 parts 1,6-hexanediol were charged. The mixture was heated to 250°C while stirring under a nitrogen stream to carry out the esterification reaction. After a predetermined amount of water was distilled off, the pressure was gradually reduced, and the deglycolization reaction was carried out at a pressure of 1 mmHg or less for 5 hours. Subsequently, 95 parts isophorone diisocyanate was gradually added, and the reaction was carried out at 150°C for about 2 hours to obtain a polyester polyurethane polyol. 2.0 parts ethylene glycol anhydrotrimellitate was added to 100 parts of this polyester polyurethane polyol, and the reaction was carried out at 180°C for about 2 hours. After that, the mixture was diluted with ethyl acetate until the solid content concentration reached 50%, to obtain polyol solution B2 containing a partially acid-modified polyester polyol with an acid value of 7.8 mg KOH / g.

[0134] [Manufacturing Example 4-3] (Polyol Solution B3) In a reaction vessel equipped with a stirrer, thermometer, reflux condenser, dropping tank, and nitrogen gas inlet tube, 40 parts of bifunctional polypropylene glycol with a number average molecular weight of approximately 2,000, 30 parts of bifunctional polypropylene glycol with a number average molecular weight of approximately 400, 10 parts of trifunctional polypropylene glycol with a number average molecular weight of approximately 400, 20 parts of bifunctional polyether polyol ECOPROL 2000 with a number average molecular weight of approximately 2,000, and 26 parts of tolylene diisocyanate were charged. The reaction was carried out by heating at 80-90°C for 5 hours while stirring under a nitrogen gas stream. During the reaction, 0.1% of dibutyltin dilaurate (DBTDL) was added as a reaction catalyst to accelerate the reaction and obtain a polyether urethane polyol. The obtained polyether urethane polyol was adjusted to a solid content concentration of 75% with ethyl acetate to obtain polyol solution B3.

[0135] [Manufacturing Example 4-4] (Polyol B4) In a reaction vessel equipped with a stirrer, thermometer, reflux condenser, dropping tank, and nitrogen gas inlet, 84.4 parts of triol with a number average molecular weight of approximately 400 (formed by adding polypropylene glycol to glycerin), 6.9 parts of trimethylolpropane, 207.7 parts of polypropylene glycol with a number average molecular weight of approximately 2,000, 235.4 parts of polypropylene glycol with a number average molecular weight of approximately 400, 205.4 parts of polytetramethylene glycol with a number average molecular weight of approximately 2,000, and 60.2 parts of tolylene diisocyanate were charged. The mixture was heated at 80°C to 90°C for 3 hours while stirring under a nitrogen gas stream to carry out the urethane formation reaction, yielding polyol B4 having urethane bonds.

[0136] [Production Example 4-5] (Polyisocyanate solution C1) Coronate 2785 (a biuret-type polyisocyanate derived from hexamethylene diisocyanate, manufactured by Tosoh Corporation) was diluted with ethyl acetate until the solid content concentration reached 50% to obtain polyisocyanate solution C1.

[0137] [Production Example 4-6] (Polyisocyanate solution C2) In a reaction vessel equipped with a stirrer, temperature gauge, reflux condenser, dropping tank, and nitrogen gas inlet, 23 parts of bifunctional polypropylene glycol with a number average molecular weight of approximately 2,000, 18 parts of bifunctional polypropylene glycol with a number average molecular weight of approximately 400, 2 parts of trifunctional polypropylene glycol with a number average molecular weight of approximately 400, and 30 parts of 4,4'-diphenylmethane diisocyanate were charged into the reaction vessel. The reaction was carried out by heating at 70-80°C for 7 hours with stirring under a nitrogen gas stream. After the reaction was complete, 7 parts of the trimethylolpropane adduct of tolylene diisocyanate were mixed in. Subsequently, the mixture was diluted with ethyl acetate to a solid content of 75% to obtain a polyisocyanate solution containing polyether urethane polyisocyanate. 80 parts of the above polyisocyanate solution and 20 parts of Desmodule L75 (manufactured by Sumika Covestro Urethane Co., Ltd., a trimethylolpropane adduct of toluene diisocyanate, with an NCO group content of 13% and a solid content of 75%) were mixed to obtain polyisocyanate solution C2.

[0138] [Manufacturing Example 4-6] (Polyisocyanate C3) In a reaction vessel equipped with a stirrer, temperature gauge, reflux condenser, dropping tank, and nitrogen gas inlet, 371.0 parts of a mixture of 2,4-diphenylmethane diisocyanate and 4,4'-diphenylmethane diisocyanate (mass ratio 50:50), 27.4 parts of triol with a number average molecular weight of approximately 400 obtained by adding polypropylene glycol to glycerin, 2.6 parts of trimethylolpropane, 31.8 parts of polypropylene glycol with a number average molecular weight of approximately 400, 289.4 parts of polypropylene glycol with a number average molecular weight of approximately 2,000, and 77.8 parts of polytetramethylene glycol with a number average molecular weight of approximately 1,000 were charged. The mixture was heated at 80°C to 90°C for 3 hours while stirring under a nitrogen gas stream to carry out the urethane reaction, yielding polyisocyanate C3 with an isocyanate group content of 11.1% and containing urethane bonds.

[0139] <Adhesive adjustment> [Preparation Example 4-1] (Adhesive D1) 100 parts of polyol solution B1 and 8 parts of polyisocyanate solution C1 were mixed, and EA was added to obtain adhesive D1 with a solid content of 30%.

[0140] [Preparation Example 4-2] (Adhesive D2) 100 parts of polyol solution B2 and 8 parts of polyisocyanate solution C1 were mixed, and EA was added to obtain adhesive D2 with a solid content of 30%.

[0141] [Preparation Example 4-3] (Adhesive D3) 100 parts of polyol solution B3 and 100 parts of polyisocyanate solution C2 were mixed, and EA was added to obtain adhesive D3 with a solid content of 30%.

[0142] [Preparation Example 4-4] (Adhesive D4) Adhesive D4 was obtained by mixing 50 parts of polyol B4 and 100 parts of polyisocyanate C3.

[0143] [Table 4]

[0144] <Manufacturing of laminates> The manufacturing method for the laminate is described below. The primer and printing ink were each diluted using a mixed solvent of EA / IPA (mass ratio 70 / 30) so that the viscosity of the primer was 14 seconds and the viscosity of the printing ink was 16 seconds (25°C, Zahn Cup #3 (manufactured by Rigosha)) before gravure printing. The coating amount after drying of the primer layer was approximately 1.0 g / m². 2 The coating amount after drying of the printed layer is approximately 2.0 g / m². 2 I adjusted it so that it would be as follows.

[0145] [Manufacturing Example 5-1] (Laminate L1) A diluted printing ink R1 was applied to a PET (double-sided corona-treated polyethylene terephthalate, 12 μm thick) film using a gravure printing press equipped with a gravure plate with a plate depth of 30 μm. The film was dried at 50°C to obtain a printed material consisting of a printed layer (R1) and a polyester substrate layer (PET). Next, adhesive D1 was applied to the PET surface of the printed material using a dry laminating machine, with a dry application amount of 2.5 g / m². 2After coating and drying to achieve the desired result, the material was laminated with an HSPET (heat-sealable polyethylene terephthalate, 30 μm thick) film to obtain a laminate L1 with the configuration R1 / PET / D1 / HSPET.

[0146] [Manufacturing Examples 5-2 to 5-8] (Laminated Structures L2 to L8) Laminates L2 to L8 were obtained using the same method as in Manufacturing Example 5-1, except that the base material and ink were changed to those listed in Table 5.

[0147] [Manufacturing Example 5-9] (Laminate L9) A diluted primer S1 was printed onto a PET (corona-treated polyethylene terephthalate, 12 μm thick) film using a gravure printing press equipped with a gravure plate with a plate depth of 30 μm. The print was dried at 60°C to obtain a printed material consisting of a primer layer (S1) and a polyester substrate layer (PET). Next, printing ink R1 was printed onto the primer layer using the same procedure to obtain a printed layer (R1) / primer layer (S1) / polyester substrate layer (PET). Then, adhesive D1 was applied to the PET surface using a dry laminating machine, with a dry application amount of 2.5 g / m². 2 After coating and drying to achieve the desired result, the material was laminated with an HSPET (heat-sealable polyethylene terephthalate, 30 μm thick) film to obtain a laminate L9 with the configuration R1 / S1 / PET / D1 / HSPET.

[0148] [Manufacturing Examples 5-10, 5-11] (Laminates L10, L11) Laminates L10 and L11 were obtained using the same method as in Manufacturing Example 5-9, except that the primer was changed to the one described in Table 5.

[0149] [Manufacturing Examples 5-12~14] (Laminate L12~14) Laminates L12 to L14 were obtained using the same method as in Manufacturing Example 5-1, except that the adhesive and the amount of adhesive applied were changed to those described in Table 5.

[0150] [Manufacturing Example 5-15] (Laminate L15) A printed material consisting of a printed layer (R1) / polyester substrate layer (PET) was obtained using the same method as in Manufacturing Example 5-1. Next, adhesive D4 was applied to the PET surface of the printed material using a non-sol laminating machine at a rate of 2.0 g / m². 2 After coating the material in this manner, it was laminated with an HSPET (heat-sealable polyethylene terephthalate, 30 μm thick) film to obtain a laminate L15 with the configuration R1 / PET / D4 / HSPET.

[0151] [Comparative Manufacturing Example 5-A] (Laminate L16) Diluted printing ink R1 was applied to PET (double-sided corona-treated polyethylene terephthalate, 12 μm thick) using a gravure printing press equipped with a gravure plate with a plate depth of 30 μm. The print was dried at 50°C to obtain a printed material consisting of a printed layer (R1) and a polyester substrate layer (PET). Next, adhesive D1 was applied to the printed surface using a dry laminating machine, with a dry application amount of 2.5 g / m². 2 After coating and drying to achieve the desired result, the material was laminated with an HSPET (heat-sealable polyethylene terephthalate, 30 μm thick) film to obtain a laminate L16 with the composition PET / R1 / D1 / HSPET.

[0152] [Comparative Manufacturing Example 5-B] (Laminate L17) A diluted printing ink R1 was applied to PET (double-sided corona-treated polyethylene terephthalate film, 25 μm thick) using a gravure printing press equipped with a gravure plate with a plate depth of 30 μm. The print was dried at 50°C to obtain a printed material consisting of a printed layer (R1) and a polyester substrate layer (PET). Next, adhesive D1 was applied to the PET surface using a dry laminating machine, with a dry application amount of 2.5 g / m². 2 After coating and drying to achieve the desired result, the material was laminated with CPP (unoriented polypropylene film, 30 μm thick) to obtain a laminate L17 with the composition R1 / PET / D1 / CPP.

[0153] [Table 5]

[0154] The abbreviations used in Table 5 are shown below. The number in parentheses after the abbreviation indicates the thickness (μm). PET(12): Double-sided corona-treated polyethylene terephthalate film, 12 μm thick PET(25): Double-sided corona-treated polyethylene terephthalate film, 25 μm thick HSPET(12): Heat-sealable polyethylene terephthalate, 12 μm thick Matte PET (12): Matte polyethylene terephthalate film, 12 μm thick PVDCPET(12): Polyvinylidene chloride resin-coated polyethylene terephthalate film, 12 μm thick VMPET(12): Transparent vapor-deposited polyethylene terephthalate film, 12 μm thick (manufactured by Toppan Printing Co., Ltd.) CPP(30): Unoriented polypropylene film, 30 μm thickness

[0155] <Preparation of the eluent> [Preparation Example 6-1] (Abstract Solution A1) One part of POE stearyl ether (polyoxyethylene stearyl ether, POE addition number: 12, HLB: 13.9) as a surfactant, 0.1 parts of BYK-1650 (manufactured by Bic Chemie Japan, silicone emulsion type defoamer, solid content concentration 27.5%) as an antifoaming agent, and 98.9 parts of water were mixed and stirred with a disperser to obtain eluent A1.

[0156] [Preparation Examples 6-2 to 6-8, Comparative Preparation Example 6-A] (Detachment liquid A2 to A9) Eliminated liquids A2 to A9 were obtained using the same method as in Production Example 6-1, except that the formulation was changed to the one shown in Table 6.

[0157] [Table 6]

[0158] The abbreviations used in Table 6 are shown below. (Nonionic surfactant) POE stearyl ether, POE addition number: 12, HLB: 13.9 (Anionic surfactant) POE lauryl ether phosphate; POE addition number: 4, HLB: 10.0 (Cationic surfactant) Stearylamine acetate HLB; 11.0 (Amphoteric surfactant) Lauryldimethylaminoacetic acid betaine HLB; 10.0 (Antifoaming agent / emulsion type) BYK-1650: Manufactured by Big Chemie Japan, silicone-based emulsion type, solids content concentration 27.5%, main solvent: water (Antifoaming agent / Self-emulsifying type) KS-540: Manufactured by Shin-Etsu Chemical Co., Ltd., silicone-based self-emulsifying type, solid content concentration 100%, (Antifoaming agent / non-silicone type) BYK-1640: Manufactured by Big Chemie Japan, non-silicone type, solids content concentration 62%, main solvent: water

[0159] <Evaluation of desorption properties of the desorption layer> [Examples 1-27, Comparative Examples 1-4] Using the laminate (L) and desorption liquid (A) described in Step 1 of Table 7, the separation and recovery state of the plastic laminate was evaluated for laminates L1 to L17 equipped with a desorption layer as follows. In a 50L kettle, 40L of desorbent liquid and 1.6kg of samples (each of laminate L1-L17 cut to 3cm x 3cm) were added and stirred at 70°C and 2000rpm. After stirring for 60 minutes, samples were taken and washed and dehydrated. From the obtained samples, 10 sheets of separated laminate (B) were sampled, and the removal rate (area %) of the printed layer was visually confirmed and evaluated according to the following criteria. The evaluation results are shown in Table 7. A (Excellent): More than 95% of the printed layer peels off from the plastic laminate. B (Good): 90% to less than 95% of the printed layer peels off from the plastic laminate. C (Acceptable): 85% to less than 90% of the printed layer peels off from the plastic laminate. D (Not acceptable): 10% to less than 85% of the printed layer peels off from the plastic laminate. E (Poor): Less than 10% of the printed layer peels off from the plastic laminate, or does not peel off at all.

[0160] <Manufacturing of recycled plastics> [Example 1] The laminate (B) obtained using the above desorption evaluation method was further dried with hot air until its moisture content was 0.2% or less. The moisture content and chlorine content measurements of the obtained laminate (B) are shown in Table 7. Subsequently, the dried laminate (B) was fed into a twin-screw extruder, melted and kneaded at a screw rotation speed of 250 rpm and a temperature of 280°C, and extruded from the extruder at a discharge pressure of 3 MPa. A 150-mesh filter was used in the discharge section. The material was then immediately cut with a pelletizer and cooled by immersion in cold water. In this way, pellets, which are recycled plastics, were obtained from the packaging material (A).

[0161] [Examples 2-27] For Examples 2 to 27, recycled plastic pellets were obtained using the same procedure as in Example 1, except that the conditions described in Table 7 were changed.

[0162] [Comparative Example 1] For Comparative Example 1, the laminate L1 was cut to a size of 3 cm x 3 cm, and the sample was used after washing and dewatering only, without immersion in the desorption solution. Recycled plastic pellets were obtained using the same procedure as in Example 1 under all other conditions.

[0163] [Comparative Examples 2-4] For Comparative Examples 2 to 4, recycled plastic pellets were obtained using the same procedure as in Example 1, except that the conditions described in Table 7 were changed.

[0164] <Transmittance Evaluation> [Examples 1-27, Comparative Examples 1-4] The recycled plastic pellets obtained as described above were extruded at 270°C using a T-die extruder to produce film-like molded bodies with a thickness of 60 μm. Subsequently, the coloration of the molded bodies was evaluated by measuring the total light transmittance using a haze meter (SH7000, manufactured by JEOL Ltd.) and according to the following criteria. The evaluation results are shown in Table 7. A (Excellent): Total light transmittance is 80% or higher. B (Good): Total light transmittance is 70% or more but less than 80% C (Acceptable): Total light transmittance is 60% or more but less than 70% D (Not acceptable): Total light transmittance is 50% or more but less than 60% E (Inferior): Total light transmittance is less than 50%

[0165] <Foreign matter detection and foaming evaluation> The recycled plastic pellets obtained as described above were extruded at 270°C using a T-die extruder to produce film-like molded bodies with a thickness of 60 μm. The number of visually identifiable foreign objects and foams per 0.5 m² of the obtained molded bodies was counted and evaluated according to the following criteria. The evaluation results are shown in Table 7. A (Excellent): Fewer than 20 foreign objects or bubbles. B (Good): Number of foreign objects and foams is 20 or more but less than 40. C (Acceptable): Number of foreign objects or bubbles is between 40 and 80. D (Not acceptable): Number of foreign objects or foam particles is 80 or more but less than 120. E (Inferior): More than 120 foreign objects or bubbles.

[0166] [Table 7]

[0167] The evaluation results above demonstrate that the manufacturing method of the present invention allows for easy removal of the printed layer, resulting in a plastic laminate with minimal re-adhesion, and furthermore, a high-quality recycled plastic material with minimal discoloration can be obtained.

Claims

1. A method for producing recycled plastic from a packaging material (A) comprising a plastic laminate including a base material, an adhesive layer and a sealant, and a printed layer formed from printing ink, wherein The printed layer contains at least one set selected from the group consisting of urethane resin / vinyl chloride-vinyl acetate, urethane resin / cellulose resin, and polyamide resin / cellulose resin. The printing layer is located on the outermost surface of the packaging material (A), The aforementioned plastic laminate does not contain a colored ink layer. The polyester resin content of packaging material (A) is 80% by mass or more. Step 1 involves immersing the packaging material (A) in a desorption solution containing water and a surfactant with an HLB value of 7 or higher to remove 85% or more by mass of the printed layer and obtain a laminate (B), A method for producing recycled plastic, comprising step 2 of melting and kneading the laminate (B) using an extrusion device equipped with a screw and a discharge unit.

2. The method for producing recycled plastic according to Claim 1, wherein the adhesive layer is formed from a dry laminate adhesive or a non-sol laminate adhesive with an acid value of 10 mg KOH / g or less.

3. The method for producing recycled plastic according to claim 1, wherein the dry coating amount of the adhesive layer is 6% by mass or less of the total mass of the laminate.

4. The method for producing recycled plastic according to claim 1, wherein the surfactant comprises at least one selected from the group consisting of nonionic surfactants, amphoteric surfactants, and anionic surfactants.

5. The method for producing recycled plastic according to claim 4, wherein the desorbing liquid further contains an antifoaming agent, and the antifoaming agent is at least one selected from the group consisting of emulsion-type silicone compounds, self-emulsifying silicone compounds, and non-silicone compounds.

6. The method for producing recycled plastic according to claim 1, wherein the melting temperature is 260 to 290°C.

7. The method for producing recycled plastic according to claim 1, wherein the pressure of the discharge section of the extrusion apparatus is 15 MPa or less.

8. The method for producing recycled plastic according to claim 1, wherein the rotational speed of the screw of the extrusion apparatus is 50 to 1000 RPM.

9. The method for producing recycled plastic according to claim 1, wherein the printed layer has a primer layer that can be removed by a desorption solution.

10. The method for producing recycled plastic according to claim 9, wherein the primer layer contains a water-dispersible resin.

11. Furthermore, the method for producing recycled plastic according to claim 1, further comprising a drying step to reduce the moisture content of the laminate (B) to 0.2% by mass or less.

12. The method for producing recycled plastic according to claim 1, wherein the chlorine content of the laminate (B) is 0.4% by mass or less of the total mass of the laminate.

Citation Information

Patent Citations

  • Method for removing ink layer from heat shrinkable label

    JP2001350411A

  • Processing method for reclaiming biaxially oriented polyester film and equipment therefor

    JP2006116857A

  • Ink cleaner used to regenerate plastic laminates into recycled raw materials, ink film peeling / removal method, and method for separating and recovering peeled or removed ink film

    JP7004124B1

  • Separation / recovery method for laminated film

    WO2020066652A1

  • Layered film and layered film separation and recovery method

    WO2021090690A1