Barrier material forming composition and method for manufacturing the same, barrier material and method for manufacturing the same, and product and method for manufacturing the same
The barrier material forming composition addresses the limitations of conventional laminates by providing moisture-resistant and visible barrier materials on variously shaped objects, enhancing visibility and reliability.
Patent Information
- Application Number
- JP2025169927
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2025-10-08
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2040-08-19
AI Technical Summary
Conventional barrier film laminates are limited in applicability and do not allow for clear visibility of markings on objects after application, and they suffer from moisture resistance issues under high temperature and humidity conditions.
A barrier material forming composition comprising a mixture of a hydrolyzed polycondensate of a silane compound, a curing catalyst, and a polyether-modified polydimethylsiloxane, with specific ratios of polydimethylsiloxane to polyether portions, allowing for moisture-resistant and visible barrier materials on variously shaped objects.
The composition forms a barrier material with excellent moisture resistance, enabling good visibility and improved long-term reliability under high temperature and humidity conditions, suitable for objects of diverse shapes.
Smart Images

Figure 0007948391000001 
Figure 0007948391000002 
Figure 0007948391000003
Abstract
Description
[Technical Field]
[0001] The present invention relates to a composition for forming a barrier material and a method for producing the same, a barrier material and a method for producing the same, and a product and a method for producing the same. [Background technology]
[0002] Conventionally, in order to prevent moisture from entering voids formed in electronic components, sealing electronic components with barrier films or the like has been considered. For example, Patent Document 1 describes a barrier film laminate in which a barrier film having an inorganic oxide layer is laminated. [Prior art documents] [Patent Documents]
[0003] [Patent Document 1] Japanese Patent Publication No. 2011-093195 [Overview of the project] [Problems that the invention aims to solve]
[0004] However, the barrier film laminate described in Patent Document 1 is in film form, and therefore its applicability is limited to specific applications.
[0005] Furthermore, in recent years, with the increasing precision and diversification of electronic components, there is a growing need to be able to clearly see the markings, markers, etc., on the surface of an object after forming a barrier material on the object, through the barrier material.
[0006] Therefore, the present invention aims to provide a barrier material that has excellent moisture resistance, is applicable to objects of various shapes, and allows for good visibility of the object's surface after application. The present invention also aims to provide a barrier material forming composition that can easily form the above barrier material. The present invention further aims to provide a method for manufacturing the barrier material forming composition, a method for manufacturing the barrier material, a product comprising the barrier material, and a method for manufacturing the product. [Means for solving the problem]
[0007] The present invention provides a barrier material forming composition comprising a mixture of a hydrolyzed polycondensate of a silane compound containing a silane oligomer and a silane monomer, a curing catalyst, and a polyether-modified polydimethylsiloxane. Such a composition can easily form a moisture-resistant barrier material on an object by application. Furthermore, by appropriately selecting the ratio of the polydimethylsiloxane portion to the polyether portion in the polyether-modified polydimethylsiloxane as described later, it is possible to form a barrier material on the object surface that allows for good visibility.
[0008] In one embodiment, the composition has a ratio (N2 / N1) of 2 to 4 between the total number of carbon atoms bonded to oxygen atoms and the total number of carbon atoms bonded to silicon atoms (N1) in the polyether-modified polydimethylsiloxane. In such a composition, the ratio of the polydimethylsiloxane portion to the polyether portion is appropriately adjusted, and the polyether-modified polydimethylsiloxane functions well as a leveling agent, resulting in a smooth surface for the barrier material formed on the object. This significantly improves the visibility of the object surface after the barrier material is formed.
[0009] A composition according to one embodiment contains a polyether-modified polydimethylsiloxane. 13 In the 1C-NMR spectrum, peak P corresponds to the carbon atom bonded to the silicon atom. C1 Peak area S C1 The peak P corresponds to the carbon atom bonded to the oxygen atom. C2 Peak area S C2 The ratio (S C2 / S C1 The ratio of the polydimethylsiloxane portion to the polyether portion in such compositions is appropriately adjusted, and the polyether-modified polydimethylsiloxane functions well as a leveling agent, resulting in a smooth surface for the barrier material formed on the object. This significantly improves the visibility of the object surface after the barrier material is formed.
[0010] A composition according to one aspect is a polyether-modified polydimethylsiloxane 1 In the H-NMR spectrum, the peak P corresponding to the hydrogen atom on the carbon atom bonded to the silicon atom H1 has a peak area S H1 relative to the peak P corresponding to the hydrogen atom on the carbon atom bonded to the oxygen atom H2 has a peak area S H2 the ratio (S H2 / S H1 ) is from 1.0 to 1.8. In such a composition, the ratio of the polydimethylsiloxane moiety to the polyether moiety is appropriately adjusted, the polyether-modified polydimethylsiloxane functions satisfactorily as a leveling agent, and the surface of the barrier material formed on the target object is smoothed. As a result, the visibility of the surface of the target object after the formation of the barrier material is significantly improved.
[0011] In one aspect, the silane oligomer may have a silicon atom bonded to three oxygen atoms.
[0012] In one aspect, the ratio of the total number of silicon atoms bonded to three oxygen atoms and silicon atoms bonded to four oxygen atoms to the total number of silicon atoms in the silane oligomer may be 30% or more.
[0013] In one aspect, the silane monomer may contain at least one selected from the group consisting of alkyltrialkoxysilanes, aryltrialkoxysilanes and tetraalkoxysilanes.
[0014] In one aspect, the content of the silane monomer in the silane compound may be 5 to 40 parts by mass with respect to 100 parts by mass of the silane oligomer.
[0015] In one aspect, the silane compound may further contain a linear polysiloxane.
[0016] In one aspect, the kinematic viscosity of the linear polysiloxane at 25°C is 50 mm2 It can be / s or greater.
[0017] In one embodiment, the linear polysiloxane may have a diorganopolysiloxane chain.
[0018] In one embodiment, the linear polysiloxane may have groups selected from the group consisting of silanol groups and alkoxy groups at both ends.
[0019] In one embodiment, the content of the linear polysiloxane in the silane compound may be 1 to 30 parts by mass per 100 parts by mass of the silane oligomer.
[0020] The present invention also provides a method for producing the above composition. This method comprises the steps of: heating the silane compound in the presence of an acid catalyst to obtain the hydrolyzed polycondensate; and mixing the hydrolyzed polycondensate, the curing catalyst, and the polyether-modified polydimethylsiloxane.
[0021] In one embodiment, the acid catalyst may contain at least one selected from the group consisting of acetic acid, phosphoric acid, hydrochloric acid, and nitric acid.
[0022] The present invention also provides a method for manufacturing a barrier material, comprising the step of curing the above composition to form a barrier material.
[0023] The present invention also provides a method for manufacturing a product having a moisture-proofed component. This manufacturing method comprises a first step of applying the composition onto the component, and a second step of curing the applied composition to form a barrier material on the component.
[0024] The present invention also provides a method for manufacturing a product having a first member and a second member joined to the first member, wherein the joint between the first member and the second member is treated to prevent moisture. This manufacturing method comprises a first step of placing the composition between the first member and the second member, and a second step of curing the composition to form a barrier material and joining the first member and the second member via the barrier material.
[0025] The present invention also provides a method for manufacturing a product comprising a moisture-proof member. This manufacturing method comprises a first step of curing the above composition to produce a moisture-proof member having a barrier material, and a second step of assembling a plurality of members including the moisture-proof member.
[0026] The present invention also provides a barrier material which is a cured product of the above composition.
[0027] The present invention also provides a product comprising a member and a barrier material formed on the member.
[0028] The present invention also provides a product comprising a first member, a second member, and the barrier material provided between the first member and the second member. In this product, the first member and the second member may be joined via the barrier material.
[0029] The present invention further provides a product which is an assembly of multiple components including a moisture-proof member having the above-mentioned barrier material. [Effects of the Invention]
[0030] The present invention provides a barrier material that has excellent moisture resistance, can be applied to objects of various shapes, and allows for good visibility of the object's surface after application. Furthermore, the present invention provides a barrier material forming composition that can easily form the above barrier material. Moreover, the present invention provides a method for manufacturing the barrier material forming composition, a method for manufacturing the barrier material, a product comprising the barrier material, and a method for manufacturing the product. [Modes for carrying out the invention]
[0031] Preferred embodiments of the present invention will be described below. In this specification, numerical ranges indicated using "~" indicate a range that includes the numerical values before and after "~" as the minimum and maximum values, respectively. "A or B" means that either A or B is included, or both are included. Unless otherwise specified, the materials exemplified in this embodiment can be used individually or in combination of two or more.
[0032] <Composition for forming barrier materials> The barrier material forming composition of this embodiment comprises a mixture of a hydrolysis polycondensate of a silane compound containing a silane oligomer and a silane monomer, a curing catalyst, and a polyether-modified polydimethylsiloxane. In this embodiment, the ratio of the polydimethylsiloxane portion to the polyether portion of the polyether-modified polydimethylsiloxane is adjusted to a predetermined range.
[0033] Such compositions, when applied to an object, can easily form a barrier material with excellent moisture resistance on the object. Furthermore, the composition, in which polyether-modified polydimethylsiloxane functions well as a leveling agent, smooths the surface of the barrier material formed on the object. Therefore, according to the above composition, it is possible to form a barrier material on the object surface that allows for good visibility.
[0034] Furthermore, conventional siloxane-based barrier materials sometimes suffered from weight loss due to hydrolysis under high temperature and high humidity conditions, resulting in poor long-term reliability. In contrast, barrier materials formed from the above composition exhibit sufficient suppression of weight loss due to hydrolysis even under high temperature and high humidity conditions, resulting in superior long-term reliability.
[0035] The ratio of the polydimethylsiloxane portion to the polyether portion can be defined, for example, by the ratio (N2 / N1) of the total number of carbon atoms bonded to oxygen atoms to the total number of carbon atoms bonded to silicon atoms N1 in the polyether-modified polydimethylsiloxane. The ratio (N2 / N1) is, for example, 2 to 4, and preferably 2.2 to 3.8.
[0036] The ratio of the polydimethylsiloxane portion to the polyether portion is, for example, that of polyether-modified polydimethylsiloxane. 13 In the 1C-NMR spectrum, peak P corresponds to the carbon atom bonded to the silicon atom. C1 Peak area S C1 The peak P corresponds to the carbon atom bonded to the oxygen atom. C2 Peak area S C2 The ratio (S C2 / S C1 ) may also be specified by the ratio (S C2 / S C1 ) is, for example, 2 to 4, preferably 2.2 to 3.8.
[0037] The ratio of the polydimethylsiloxane portion to the polyether portion is, for example, that of polyether-modified polydimethylsiloxane. 1 In the H-NMR spectrum, peak P corresponds to the hydrogen atom on the carbon atom bonded to the silicon atom. H1 Peak area S H1 Peak P corresponds to the hydrogen atom on the carbon atom bonded to the oxygen atom. H2 Peak area S H2 The ratio (S H2 / S H1 ) may also be specified by the ratio (S H2 / S H1 ) is, for example, 0.8 to 2.0, and preferably 1.0 to 1.8.
[0038] In other words, the composition of this embodiment may satisfy the following formula (1). 2 <N2 / N1<4 …(1)
[0039] Furthermore, the composition of this embodiment may satisfy either formula (2) or formula (3) below, and it is preferable that it satisfies both. 2 C2 / S C1 <4 …(2) 0.8 H2 / S H1 <2.0 …(3)
[0040] In this specification, 13 The 1C-NMR spectrum is measured using the following method. (solution 13 C-NMR measurement conditions) Equipment name: JEOL RESONANCE ECX400II Observed nucleus: 13C Observation frequency: 10.052MHz Measurement temperature: Room temperature (23℃) Measurement solvent: CDCl3 Pulse width: 11.4 μs (45°) Pulse repetition time: 2.0 seconds Total number of times: 700 Sample concentration (sample / solvent): 100 mg / 1.0 ml
[0041] 13 In the 1C NMR spectrum, peak P C1 The peak may have a chemical shift in the range of 5 ppm to -5 ppm (preferably 3 ppm to -3 ppm). That is, the peak area S C1 This may be the sum of the peak areas of peaks with a chemical shift in the range of 5 ppm to -5 ppm (preferably 3 ppm to -3 ppm).
[0042] Also, 13 In the 1C NMR spectrum, peak P C2 The peak may have a chemical shift in the range of 47 ppm to 65 ppm (preferably 50 ppm to 65 ppm). That is, the peak area S C2 This may be the sum of the peak areas of peaks with a chemical shift in the range of 47 ppm to 65 ppm (preferably 50 ppm to 65 ppm).
[0043] In this specification, 1 The H-NMR spectrum is measured using the following method. (solution 1 H-NMR measurement conditions) Equipment name: JEOL RESONANCE ECX400II Observed nucleus: 1H Observation frequency: 399.78MHz Measurement temperature: Room temperature (23℃) Measurement solvent: CDCl3 Pulse width: 6.64 μs (90°) Pulse repetition time: 5.0 seconds Total number of times: 8 Sample concentration (sample / solvent): 10 mg / 1.0 ml
[0044] 1 In the H-NMR spectrum, peak P H1 The peak may have a chemical shift in the range of 0.5 ppm to -0.5 ppm (preferably 0.3 ppm to -0.3 ppm). That is, the peak area S H1 This may be the sum of the peak areas of peaks with a chemical shift in the range of 0.5 ppm to -0.5 ppm (preferably 0.3 ppm to -0.3 ppm).
[0045] Also, 1 In the H-NMR spectrum, peak P H2 The peak may have a chemical shift in the range of 4.5 ppm to 2.5 ppm (preferably 4 ppm to 2 ppm). That is, the peak area S H2 This may be the sum of the peak areas of peaks with a chemical shift in the range of 4.5 ppm to 2.5 ppm (preferably 4 ppm to 2 ppm).
[0046] The barrier material forming composition may be in liquid or paste form, but it is preferable to be in liquid form from the viewpoint of making it easier to apply to the target object.
[0047] Silane oligomers have a structure in which multiple silicon atoms are linked via oxygen atoms, and can also be described as polymers of silane monomers. In this specification, silane oligomers refer to polymers with a molecular weight of 100,000 or less.
[0048] The silicon atoms contained in silane oligomers can be distinguished into silicon atoms bonded to one oxygen atom (M unit), silicon atoms bonded to two oxygen atoms (D unit), silicon atoms bonded to three oxygen atoms (T unit), and silicon atoms bonded to four oxygen atoms (Q unit). The following formulas (M), (D), (T), and (Q) can be used as examples of M, D, T, and Q units, respectively.
[0049] [ka]
[0050] In the above formula, R represents an atom other than the oxygen atom bonded to silicon (such as a hydrogen atom) or an atomic group (such as an alkyl group). Information regarding the content of these units can be obtained by Si-NMR.
[0051] In the silane oligomer, the ratio of the total number of T units and Q units to the total number of silicon atoms may be, for example, 30% or more, preferably 50% or more, more preferably 70% or more, even more preferably 90% or more, and may be 100%. Such a silane oligomer provides a barrier material with even better moisture resistance.
[0052] In one preferred embodiment, the silane oligomer preferably contains T units. The T unit content in the silane oligomer is, for example, 10% or more, preferably 20% or more, 30% or more, 40% or more, 50% or more, 70% or more, 80% or more, or 90% or more, and may be 100%, relative to the total number of silicon atoms. Such a silane oligomer tends to further improve the flexibility of the barrier material.
[0053] In another preferred embodiment, the Q unit content in the silane oligomer is, for example, 50% or more, preferably 70% or more, more preferably 80% or more, even more preferably 90% or more, and may be 100%, relative to the total number of silicon atoms. Such silane oligomers tend to have improved moisture resistance and transparency of the barrier material.
[0054] The silane oligomer preferably has an alkyl group or an aryl group as R in the above-mentioned formulas (M), (D), (T), and (Q).
[0055] As the alkyl group, alkyl groups having 6 or fewer carbon atoms are preferred, and alkyl groups having 4 or fewer carbon atoms are more preferred. Specific examples of alkyl groups include methyl, ethyl, propyl, and butyl groups, of which methyl, ethoxy, and propyl groups are preferred, and methyl groups are more preferred.
[0056] Examples of aryl groups include phenyl groups and substituted phenyl groups. Examples of substituents on substituted phenyl groups include alkyl groups, vinyl groups, mercapto groups, amino groups, nitro groups, and cyano groups. Phenyl groups are preferred as the aryl group.
[0057] The weight-average molecular weight of the silane oligomer may be, for example, 400 or more, preferably 600 or more, and more preferably 1000 or more. Alternatively, the weight-average molecular weight of the silane oligomer may be, for example, 30000 or less, preferably 10000 or less, and more preferably 6000 or less. A higher weight-average molecular weight of the silane oligomer tends to improve flexibility, while a lower weight-average molecular weight tends to improve moisture resistance and transparency. In this specification, the weight-average molecular weight of the silane oligomer refers to the weight-average molecular weight expressed in polystyrene equivalent as measured by gel permeation chromatography (GPC).
[0058] The silane oligomer content in the silane compound may be, for example, 30% by mass or more, preferably 40% by mass or more, more preferably 45% by mass or more, and even more preferably 50% by mass or more, based on the total amount of the silane compound. This allows the effects of the invention described above to be more pronounced. Alternatively, the silane oligomer content in the silane compound may be, for example, 95% by mass or less, 90% by mass or less, 85% by mass or less, or 80% by mass or less, based on the total amount of the silane compound.
[0059] In this embodiment, the silane compound contains a silane monomer. By incorporating a silane monomer, for example, the content of T units and Q units in the barrier material can be easily adjusted, and effects such as transparency and flexibility can be imparted to the barrier material depending on the application. Furthermore, incorporating a silane monomer tends to result in a barrier material with even better moisture resistance.
[0060] Examples of silane monomers include at least one silane monomer selected from the group consisting of alkyltrialkoxysilanes, aryltrialkoxysilanes, and tetraalkoxysilanes (hereinafter also referred to as the first silane monomer).
[0061] By incorporating the first silane monomer, for example, the content of T units and Q units in the barrier material can be adjusted, and effects such as transparency and flexibility can be imparted to the barrier material depending on the application. Furthermore, incorporating the first silane monomer tends to result in a barrier material with even better moisture resistance.
[0062] When the silane compound contains a first silane monomer, the content of the first silane monomer in the silane compound is not particularly limited and may be, for example, 5 parts by mass or more, preferably 8 parts by mass or more, and more preferably 10 parts by mass or more, per 100 parts by mass of silane oligomer. This tends to further improve the flexibility of the cured product. Alternatively, the content of the first silane monomer may be, for example, 40 parts by mass or less, preferably 35 parts by mass or less, and more preferably 30 parts by mass or less. This tends to reduce the volatility of the coating liquid and further improve workability.
[0063] Alkyltrialkoxysilanes are silane compounds in which one alkyl group and three alkoxy groups are bonded to a silicon atom.
[0064] The alkyl group of the alkyltrialkoxysilane is preferably an alkyl group having 6 or fewer carbon atoms, and more preferably an alkyl group having 4 or fewer carbon atoms. Specific examples of alkyl groups include methyl, ethyl, propyl, and butyl groups, of which methyl, ethyl, and propyl groups are preferred, and methyl groups are more preferred. Furthermore, the alkoxy group of the alkyltrialkoxysilane is preferably an alkoxy group having 6 or fewer carbon atoms, and more preferably an alkoxy group having 4 or fewer carbon atoms. Specific examples of alkoxy groups include methoxy, ethoxy, propoxy, and butoxy groups, of which methoxy, ethoxy, and propoxy groups are preferred, and methoxy and ethoxy groups are more preferred.
[0065] Aryltrialkoxysilanes are silane compounds in which one aryl group and three alkoxy groups are bonded to a silicon atom.
[0066] Examples of the aryl group in aryltrialkoxysilane include phenyl groups and substituted phenyl groups. Examples of substituents on the substituted phenyl group include alkyl groups, vinyl groups, mercapto groups, amino groups, nitro groups, and cyano groups. The phenyl group is preferred as the aryl group. Furthermore, the alkoxy group in aryltrialkoxysilane is preferably an alkoxy group having 6 or fewer carbon atoms, and more preferably an alkoxy group having 4 or fewer carbon atoms. Specific examples of alkoxy groups include methoxy groups, ethoxy groups, propoxy groups, and butoxy groups, of which methoxy groups, ethoxy groups, and propoxy groups are preferred, and methoxy groups and ethoxy groups are more preferred.
[0067] Tetraalkoxysilanes are silane compounds in which four alkoxy groups are bonded to a silicon atom.
[0068] The alkoxy group of the tetraalkoxysilane is preferably an alkoxy group having 6 or fewer carbon atoms, and more preferably an alkoxy group having 4 or fewer carbon atoms. Specific examples of alkoxy groups include methoxy, ethoxy, propoxy, and butoxy groups, of which methoxy, ethoxy, and propoxy groups are preferred, and methoxy and ethoxy groups are more preferred.
[0069] Specific examples of the first type of silane monomer include methyltrimethoxysilane, methyltriethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, and tetrabutoxysilane.
[0070] Examples of silane monomers include silane monomers having at least one reactive functional group selected from the group consisting of vinyl group, epoxy group, glycidyl group, (meth)acryloyl group, amino group, isocyanate group, isocyanurate group, and mercapto group (hereinafter also referred to as the second silane monomer). When the above composition contains such a silane monomer, a barrier material with even better conformability and adhesion to the target object tends to be formed.
[0071] The reason why the second silane monomer produces the above effects is not entirely clear, but it is thought that during the formation of the barrier material, cross-linking structures other than siloxane bonds are formed through reactions between reactive functional groups, reactions between reactive functional groups and silanol groups, etc., thereby achieving excellent moisture resistance and flexibility. Furthermore, it is also thought that during the formation of the barrier material, the reactive functional groups of the second silane monomer bond with functional groups present on the surface of the object, resulting in even better moisture resistance and flexibility.
[0072] From the viewpoint of further improving the flexibility of the barrier material and its adhesion to the component, the reactive functional group of the second silane monomer is preferably selected from the group consisting of vinyl group, epoxy group (more preferably glycidyl group), (meth)acryloyl group, amino group, isocyanate group, isocyanurate group, and mercapto group, with the amino group being more preferred.
[0073] The second silane monomer preferably has a silicon atom bonded to three oxygen atoms.
[0074] As the second silane monomer, for example, a silane monomer represented by the following formula (A-1) can be suitably used.
[0075] [ka]
[0076] In the formula, R A1 L indicates a reactive functional group. 1 is an alkanediyl group or an oxyalkanediyl group (-OL 2 - A group represented by L 2 represents an alkanediyl group. ) where p represents an integer greater than or equal to 0 (preferably an integer from 0 to 3), R A2 This indicates an alkyl group or an aryl group.
[0077] R A1When the group is a vinyl group, p is preferably 0 to 3, and more preferably 0.
[0078] R A1 When p is an epoxy group, a glycidyl group, a (meth)acryloyl group, an amino group, an isocyanate group, an isocyanurate group, or a mercapto group, p is preferably an integer of 1 or more, more preferably 1 to 3, and even more preferably 1.
[0079] R A1 When L is a vinyl group, a glycidyl group, or a (meth)acryloyl group, 1 It is preferable that the group is an oxyalkanediyl group.
[0080] R A1 When L is an amino group, isocyanate group, isocyanurate group or mercapto group, 1 It is preferable that the group is an alkanediyl group.
[0081] L 1 and L 2 The alkanediyl group in this case is preferably an alkanediyl group having 2 to 10 carbon atoms, and more preferably an alkanediyl group having 2 to 8 carbon atoms.
[0082] R A2 The alkyl group in is preferably one having 6 or fewer carbon atoms, and more preferably one having 4 or fewer carbon atoms. Specific examples of alkyl groups include methyl group, ethyl group, propyl group (n-propyl group, isopropyl group), and butyl group (n-butyl group, sec-butyl group, isobutyl group, tert-butyl group).
[0083] R A2 A phenyl group is preferred as the aryl group in this compound.
[0084] R A2 It is preferable that it be an alkyl group.
[0085] When the silane compound contains a silane monomer, the content of the second silane monomer in the silane compound may be, for example, 0.01 parts by mass or more, preferably 0.05 parts by mass or more, and more preferably 0.1 parts by mass or more, per 100 parts by mass of the silane oligomer. This tends to further improve conformability and adhesion. Alternatively, the content of the second silane monomer in the silane compound may be, for example, 5 parts by mass or less, preferably 4 parts by mass or less, and more preferably 2 parts by mass or less. This tends to further improve the thermal stability of the cured product.
[0086] In this embodiment, the silane compound may further contain a linear polysiloxane. This results in a barrier material that exhibits superior conformability to the target object and has fewer defects such as cracks.
[0087] A linear polysiloxane can be defined as a compound having a linear main chain formed by siloxane bonds, and it is preferable that this main chain is a diorganopolysiloxane chain. In other words, it is preferable that a linear polysiloxane has a polysiloxane chain composed of repeating D units.
[0088] The organic group (i.e., R in formula (D)) that bonds to the silicon atom in the main chain of the linear polysiloxane is preferably an alkyl group or an aryl group.
[0089] As the alkyl group, alkyl groups having 6 or fewer carbon atoms are preferred, and alkyl groups having 4 or fewer carbon atoms are more preferred. Specific examples of alkyl groups include methyl, ethyl, propyl, and butyl groups, of which methyl, ethoxy, and propyl groups are preferred, and methyl groups are more preferred.
[0090] Examples of aryl groups include phenyl groups and substituted phenyl groups. Examples of substituents on substituted phenyl groups include alkyl groups, vinyl groups, mercapto groups, amino groups, nitro groups, and cyano groups. Phenyl groups are preferred as the aryl group.
[0091] Linear polysiloxanes preferably have a group selected from the group consisting of silanol groups and alkoxy groups at at least one end, and more preferably have such groups at both ends. The silicon atoms at the ends bonded to the group are preferably Q units or D units, and more preferably D units.
[0092] As for the alkoxy group, an alkoxy group having 6 or fewer carbon atoms is preferred, and an alkoxy group having 4 or fewer carbon atoms is more preferred. Specific examples of alkoxy groups include methoxy, ethoxy, propoxy, and butoxy groups, of which methoxy, ethoxy, and propoxy groups are preferred, and methoxy and ethoxy groups are more preferred.
[0093] The kinematic viscosity of linear polysiloxane at 25°C is 50 mm². 2 It is preferable that the ratio is 1 / s or higher. Since such linear polysiloxanes have a sufficient chain length, the above-mentioned effects can be significantly obtained by incorporating linear polysiloxanes.
[0094] From the viewpoint of obtaining the above-mentioned effects more significantly, the kinematic viscosity of linear polysiloxane at 25°C is preferably 60 mm². 2 / s or more, more preferably 70 mm 2 It is / s or greater.
[0095] Furthermore, the kinematic viscosity of linear polysiloxane at 25°C is 500 mm². 2 It is preferable that the kinematic viscosity of the linear polysiloxane is less than or equal to / s. This improves the compatibility of the linear polysiloxane with other components in the composition, thereby improving the transparency of the barrier material forming composition and the barrier material obtained as a cured product. From the viewpoint of obtaining this effect more significantly, the kinematic viscosity of the linear polysiloxane at 25°C is 300 mm². 2 It is more preferable that it be less than or equal to / s, and 100mm 2 It is even more preferable that the time is less than or equal to / s.
[0096] When the silane compound contains linear polysiloxane, the content of linear polysiloxane in the silane compound may be, for example, 0.1 parts by mass or more, preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, and even more preferably 2 parts by mass or more, per 100 parts by mass of silane oligomer. This results in a more pronounced effect than described above. Alternatively, the content of linear polysiloxane in the silane compound may be, for example, 40 parts by mass or less, preferably 30 parts by mass or more, more preferably 20 parts by mass or less, and even more preferably 10 parts by mass or less, per 100 parts by mass of silane oligomer. This results in improved density of the coating film and a particularly excellent moisture resistance.
[0097] The composition according to this embodiment contains a hydrolyzed polycondensate of a silane compound. In this specification, a hydrolyzed polycondensate of a silane compound can be said to be a silane mixture obtained by subjecting a silane compound to a hydrolysis-polycondensation reaction (hereinafter also simply referred to as a hydrolysis reaction). Alternatively, a hydrolyzed polycondensate of a silane compound can also be said to be a silane mixture formed by the polycondensation of hydrolyzed products obtained by hydrolyzing the hydrolyzable groups in a silane compound.
[0098] The hydrolyzable group can be any group that can produce a silanol group upon hydrolysis, such as an alkoxy group like a methoxy group or an ethoxy group. Preferably, the hydrolyzable group is a group that is directly bonded to a silicon atom in the silane compound.
[0099] The reaction conditions for the hydrolysis reaction are not particularly limited, and any conditions that convert the hydrolyzable group to a silanol group are acceptable. The hydrolysis reaction is preferably carried out, for example, by heating the silane compound in the presence of an acid catalyst.
[0100] Examples of acid catalysts include acetic acid, phosphoric acid, hydrochloric acid, nitric acid, carbonic acid, and sulfuric acid, with at least one selected from the group consisting of acetic acid, phosphoric acid, hydrochloric acid, and nitric acid being preferred.
[0101] The amount of acid catalyst may be, for example, 0.001 parts by mass or more, preferably 0.005 parts by mass or more, more preferably 0.01 parts by mass or more, and even more preferably 0.05 parts by mass or more, per 100 parts by mass of silane compound. Alternatively, the amount of acid catalyst may be, for example, 5 parts by mass or less, preferably 4 parts by mass or less, more preferably 3 parts by mass or less, and even more preferably 2 parts by mass or less, per 100 parts by mass of silane compound.
[0102] The heating temperature during the hydrolysis reaction may be, for example, 40°C or higher, and preferably 60°C or lower. Alternatively, the heating temperature during the hydrolysis reaction may be, for example, 100°C or lower, and preferably 90°C or lower.
[0103] The reaction time for the hydrolysis reaction may be, for example, 30 minutes or more, preferably 1 hour or more. Alternatively, the reaction time for the hydrolysis reaction may be, for example, 10 hours or less, preferably 5 hours or less.
[0104] Hydrolysis reactions are preferably carried out in a liquid medium. Examples of liquid media include water and organic solvents. Examples of organic solvents include alcohols, ethers, ketones, esters, and hydrocarbons. In addition to these, acetonitrile, acetamide, N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, etc., can also be used.
[0105] In a preferred embodiment, the hydrolysis reaction may be carried out in a liquid medium containing water and alcohols. Using such a liquid medium makes it easier to obtain a barrier material with excellent transparency.
[0106] The alcohols used are preferably those that can be vaporized by heating during barrier material formation. For example, alcohols with 6 or fewer carbon atoms are preferred, and alcohols with 1 to 4 carbon atoms are more preferred.
[0107] The composition of this embodiment includes a curing catalyst. The curing catalyst can be any catalyst that can promote the further polymerization reaction of the hydrolysis polycondensate of the silane compound and can cure the composition by heating or other means.
[0108] Examples of curing catalysts include acid catalysts such as hydrochloric acid, nitric acid, sulfuric acid, acetic acid, and phosphoric acid; metal catalysts containing metal elements such as tin, titanium, aluminum, zinc, iron, cobalt, manganese, and zirconium; and base catalysts such as aliphatic amines, ammonium hydroxide, tetraethylammonium hydroxide, sodium carbonate, and sodium hydroxide. The curing catalyst may be used individually or in combination of two or more types.
[0109] Examples of metal catalysts include metal alkoxides and metal complexes. Any metal catalyst that can promote the dehydration condensation reaction of silane compounds having a silanol group (for example, the further dehydration condensation reaction of the hydrolysis polycondensate of the silane compound mentioned above) is acceptable, and any known metal catalyst can be used without particular limitation. One metal catalyst may be used alone, or two or more may be used in combination.
[0110] As the metal catalyst, a metal catalyst selected from the group consisting of aluminum catalysts (metal catalysts containing aluminum), nickel catalysts (metal catalysts containing nickel), titanium catalysts (metal catalysts containing titanium), and zirconium catalysts (metal catalysts containing zirconium) is preferred, and a metal catalyst selected from the group consisting of aluminum catalysts, nickel catalysts, and zirconium catalysts is more preferred.
[0111] Examples of aluminum catalysts, nickel catalysts, titanium catalysts, and zirconium catalysts include metal alkoxides and metal complexes. The metal catalyst can be any catalyst that can promote the dehydration condensation reaction of silane compounds having a silanol group (for example, the further dehydration condensation reaction of the hydrolysis polycondensate of the silane compound mentioned above), and may be, for example, a known catalyst that can promote the dehydration condensation reaction. Examples of aluminum catalysts include aluminum alkyl acetate diisopropylate, aluminum monoacetylacetonate bis(ethyl acetate), and aluminum tris(acetylacetonate).
[0112] The amount of curing catalyst added may be, for example, 0.001 parts by mass or more, preferably 0.005 parts by mass or more, more preferably 0.01 parts by mass or more, and even more preferably 0.02 parts by mass or more, per 100 parts by mass of the silane compound. This further shortens the curing time. Alternatively, the amount of curing catalyst added may be, for example, 1 part by mass or less, preferably 0.9 parts by mass or less, more preferably 0.6 parts by mass or less, and even more preferably 0.5 parts by mass or less, per 100 parts by mass of the silane compound. This tends to further improve the long-term reliability of the barrier material.
[0113] Polyether-modified polydimethylsiloxane can be described as a compound in which some of the methyl groups of polydimethylsiloxane are replaced with groups containing a polyether structure.
[0114] A polyoxyalkylene structure is preferred as the polyether structure. Preferred polyoxyalkylene structures include polyoxyethylene structures, polyoxypropylene structures, and combinations thereof.
[0115] Examples of polyether-modified polydimethylsiloxanes include compounds having a structural unit represented by the following formula (1-1) (hereinafter also referred to as structural unit (1-1)) and a structural unit represented by the following formula (1-2) (hereinafter also referred to as structural unit (1-2)).
[0116] [ka]
[0117] In the formula, R 1 and R 2 R indicates an alkanediyl group, 3 represents an alkyl group, and n represents an integer greater than or equal to 2.
[0118] R 1 The alkanediyl group in is preferably an alkanediyl group having 2 to 15 carbon atoms, more preferably an alkanediyl group having 2 to 10 carbon atoms, and even more preferably an alkanediyl group having 2 to 8 carbon atoms.
[0119] R 2 The alkanediyl group in is preferably an alkanediyl group having 2 to 6 carbon atoms, more preferably an alkanediyl group having 2 to 4 carbon atoms, and even more preferably an alkanediyl group having 2 or 3 carbon atoms. 2 They may be the same or different from each other.
[0120] R 3 The alkyl group in is preferably an alkyl group having 10 or fewer carbon atoms, more preferably an alkyl group having 8 or fewer carbon atoms, and even more preferably an alkyl group having 1 or more carbon atoms.
[0121] n is not particularly limited as long as it is 2 or greater, but is preferably 5 or greater, more preferably 8 or greater, and even more preferably 10 or greater. Also, n may be, for example, 35 or less, preferably 30 or less, and even more preferably 25 or less.
[0122] The ratio of structural unit (1-1) to structural unit (1-2) is not particularly limited and may be appropriately changed, for example, to satisfy at least one (preferably two or more, more preferably all three) of the above formulas (1) to (3).
[0123] In the polyether-modified polydimethylsiloxane, the ratio (C2 / C1) of the content of structural unit (1-2) to the content of structural unit (1-1) (C1) may be, for example, 0.01 or more, and may be 0.02 or more, or 0.03 or more. Furthermore, the ratio (C2 / C1) may be, for example, 0.3 or less, and may be 0.25 or less, or 0.2 or less.
[0124] The terminals of the polyether-modified polydimethylsiloxane (i.e., the terminals of the polydimethylsiloxane) are not particularly limited, but are preferably trialkylsilyl groups, and more preferably trimethylsilyl groups.
[0125] The weight-average molecular weight of the polyether-modified polydimethylsiloxane may be, for example, 100 or more, preferably 200 or more, and more preferably 500 or more. Alternatively, the weight-average molecular weight of the polyether-modified polydimethylsiloxane may be, for example, 100,000 or less, preferably 50,000 or less, and more preferably 10,000 or less.
[0126] The amount of polyether-modified polydimethylsiloxane blended may be, for example, 0.001 parts by mass or more, preferably 0.005 parts by mass or more, more preferably 0.01 parts by mass or more, and even more preferably 0.02 parts by mass or more, per 100 parts by mass of the silane compound. This tends to further improve surface uniformity. Alternatively, the amount of polyether-modified polydimethylsiloxane blended may be, for example, 2.0 parts by mass or less, preferably 1.0 part by mass or less, more preferably 0.7 parts by mass or less, and even more preferably 0.5 parts by mass or less, per 100 parts by mass of the silane compound. This reduces the cost of the barrier material by reducing the manufacturing cost of the polyether-modified polydimethylsiloxane.
[0127] The composition of this embodiment may further contain a liquid medium. The liquid medium incorporated into the composition of this embodiment may be the liquid medium used in the hydrolysis reaction. That is, the liquid medium used in the hydrolysis reaction may be incorporated into the composition of this embodiment together with the hydrolysis polycondensate. Examples of liquid media include those described above.
[0128] The content of the liquid medium in the composition is not particularly limited; for example, it may be set to a content that gives the composition a viscosity suitable for coating. The viscosity of the composition is not particularly limited and may be adjusted as appropriate depending on the thickness of the barrier material to be prepared, the coating method, the shape of the object, etc.
[0129] The viscosity of the composition at 25°C may be, for example, 1 to 6000 mPa·s, and preferably 5 to 3000 mPa·s. Such a composition makes it easier to apply to an object and to form a barrier material on the object.
[0130] The composition of this embodiment may further contain other components not listed above. Examples of other components include resins having hydroxyl groups in their molecular structure, metal oxide particles, and metal oxide fibers. Examples of resins having hydroxyl groups in their molecular structure include polyvinyl alcohol. Examples of metal oxide particles include silica particles and alumina particles, and these particles are preferably nano-sized (for example, with a particle size of 1 nm or more and less than 1000 nm) (i.e., nanosilica particles and nanoalumina particles are preferred). Examples of metal oxide fibers include alumina fibers, and the fiber diameter of these metal oxide fibers is preferably nano-sized (for example, with a fiber diameter of 1 nm or more and less than 1000 nm) (i.e., alumina nanofibers are preferred).
[0131] The amount of the other components mentioned above is not particularly limited as long as the above-described effects are obtained. For example, it may be 50 parts by mass or less, preferably 40 parts by mass or less, per 100 parts by mass of the silane compound. Alternatively, the amount of the other components may be, for example, 10 parts by mass or more, or 20 parts by mass or more, per 100 parts by mass of the silane compound.
[0132] The following are examples of methods for producing the composition according to this embodiment. <Method for producing the composition> This manufacturing method comprises a first step of heating the above-mentioned silane compound in the presence of an acid catalyst to obtain a hydrolyzed polycondensate of the silane compound, and a second step of mixing the hydrolyzed polycondensate of the silane compound with a curing catalyst and a polyether-modified polydimethylsiloxane.
[0133] The first step is to hydrolyze the silane compound by heating in the presence of an acid catalyst. The preferred conditions for the hydrolysis reaction are as described above.
[0134] The second step involves mixing the hydrolyzed polycondensate obtained in the first step with a curing catalyst, a polyether-modified polydimethylsiloxane, and other components as needed, to obtain a composition. The mixing method in the second step is not particularly limited and may be done by known methods.
[0135] <Barrier material> The barrier material in this embodiment may be a cured product of the barrier material forming composition described above. Alternatively, this barrier material may be formed by heating the barrier material forming composition described above. Upon heating, the hydrolysis polycondensates of the silane compounds in the composition undergo further polymerization to form a polysiloxane compound.
[0136] The barrier material has a low water vapor permeability and excellent moisture resistance. The water vapor permeability of the barrier material per 25 μm thickness (40°C, 95% RH) is, for example, 5000 g / m². 2 • May be less than or equal to 4000g / m² 2·day or less, more preferably 3000 g / m 2 ·day or less.
[0137] Further, the water vapor transmission rate (40°C, 95%RH) of the barrier material per 25 μm thickness may be, for example, 100 g / m 2 ·day or more, preferably 500 g / m 2 ·day or more. Such a barrier material has dehumidifying properties, and can sufficiently suppress breakage due to expansion of moisture that has entered the interior even when used in a high-temperature environment.
[0138] The water vapor transmission rate of the barrier material refers to a value measured by the humidity sensor method (Lyssy method) in accordance with JIS K7129.
[0139] The barrier material may have transparency. Such a barrier material can be suitably used in applications requiring transparency, for example, as a covering material for covering an image sensor in an image sensor package. Here, "having transparency" means that the visible light transmittance (light transmittance at 550 nm) per 1 mm thickness is 80% or more.
[0140] The visible light transmittance (light transmittance at 550 nm) of the barrier material per 1 mm thickness is preferably 80% or more, more preferably 85% or more, and even more preferably 90% or more. The visible light transmittance of the barrier material is measured with a spectrophotometer.
[0141] The barrier material has excellent insulating properties, and can be suitably used in applications requiring insulating properties, for example, as a moisture-proof barrier material for electronic components.
[0142] The volume resistivity of the barrier material may be, for example, 1×10 10 Ω·cm or more, and from the viewpoint of securing sufficient insulating properties as a moisture-proof barrier material for electronic components, it is preferably 1×10 12 Ω·cm or more, more preferably 1×10 14 Ω·cm or more. In addition, the volume resistivity of the barrier material is, for example, 1×1019 It may be less than or equal to Ωcm, and 1 × 10 18 It may be less than or equal to Ωcm. In this specification, the volume resistivity of the barrier material is the value measured in accordance with JIS K 6911.
[0143] The dielectric breakdown strength of the barrier material may be, for example, 10 kV / mm or more, and from the viewpoint of ensuring sufficient insulation as a moisture-proof barrier material for electronic components, 50 kV / mm or more is preferred, and 100 kV / mm or more is more preferred. Furthermore, the dielectric breakdown strength of the barrier material may be, for example, 1000 kV / mm or less, or 500 kV / mm or less. In this specification, the dielectric breakdown strength of the barrier material is expressed as a value measured in accordance with JIS C 2110.
[0144] The barrier material has excellent heat resistance and can be suitably used in applications requiring heat resistance, such as as a moisture-proof barrier material for electronic components that undergo high-temperature processes (e.g., reflow processes) during mounting. The barrier material can be suitably used, for example, as a moisture-proof barrier material that is placed on a component before heating in a reflow oven and subjected to the reflow oven together with the component. Because the barrier material has excellent heat resistance, it can maintain sufficient moisture protection even after heating in a reflow oven.
[0145] Temperature at which barrier material loses 5% of its weight (T d5 The temperature may be, for example, 260°C or higher, preferably 280°C or higher, and more preferably 300°C or higher. The 5% weight loss temperature of the barrier material may be, for example, 500°C or lower, and may be 450°C or lower. In this specification, the 5% weight loss temperature of the barrier material refers to the value measured by a thermogravimetric differential thermal analyzer.
[0146] The shape of the barrier material is not particularly limited. The barrier material may be formed, for example, into a film, and such a barrier material can be used as a moisture-proof barrier film. The barrier material may also be formed to fill gaps between members, in which case it can prevent moisture from entering through the gaps. The barrier material may also be formed to cover members, in which case it can prevent the members from coming into contact with moisture.
[0147] <Method for manufacturing barrier materials> The method for producing the barrier material according to this embodiment includes a heating step of heating the above-mentioned composition to form the barrier material. In this production method, heating causes the hydrolysis polycondensates of the silane compounds in the composition to further polymerize and form a polysiloxane compound.
[0148] In the heating step, the liquid medium in the composition may be removed by heating. That is, the heating step may be a step in which a barrier material containing a polysiloxane compound is formed by heating and drying the composition.
[0149] The heating temperature in the heating process is not particularly limited and should be any temperature at which the silane oligomer can polymerize. Furthermore, if the composition contains a liquid medium, the heating temperature is preferably the temperature at which the liquid medium volatilizes. The heating temperature may be, for example, 70°C or higher, preferably 100°C or higher. Alternatively, the heating temperature may be, for example, 200°C or lower, preferably 180°C or lower.
[0150] This manufacturing method may further include a coating step for applying the composition. In this case, the heating step can be defined as a step for heating the coated composition.
[0151] The method of applying the composition is not particularly limited and may be modified as appropriate depending on the shape of the object to be coated, the thickness of the barrier material, etc.
[0152] In this manufacturing method, the composition may be applied to an object to which moisture resistance is to be imparted, thereby forming a barrier material on the object. Alternatively, in this manufacturing method, a barrier material of a predetermined shape may be manufactured first, and then the manufactured barrier material may be applied to the object.
[0153] <Applications of barrier materials> The applications of the barrier material according to this embodiment are not particularly limited and can be suitably applied to various applications requiring moisture resistance. For example, the barrier material can be suitably used as a moisture-proof barrier material for electronic components.
[0154] The barrier material according to this embodiment has excellent moisture resistance even in high-temperature environments (e.g., 100°C or higher). Therefore, the barrier material according to this embodiment can be suitably used in applications such as moisture-proof barrier materials for electronic components used in high-temperature environments, and moisture-proof barrier materials for electronic components that undergo high-temperature processes during mounting. Specifically, it can be suitably used as, for example, a moisture-proof barrier material for power semiconductors, a moisture-proof barrier material for image sensors, and a moisture-proof barrier material for displays.
[0155] The following describes in detail one preferred form of application for the barrier material, but the applications of the barrier material are not limited to those described below.
[0156] <Application example 1> One embodiment relates to a product having a moisture-proofed component. Such a product comprises a component and a barrier material formed on the component. The barrier material may be formed on one component or on multiple components. The barrier material may be formed, for example, to cover one or more components, or to cover the joint between two components.
[0157] Such products are manufactured by a manufacturing method comprising a first step of applying the barrier material forming composition onto a component, and a second step of heating the applied composition to form a barrier material on the component. This manufacturing method may further include a step of exposing the moisture-proofed component to high temperatures (for example, reflow soldering, heat curing of chip bonds, drying of materials by heating, etc.).
[0158] Specific examples of such applications include the following electronic components:
[0159] (Electronic component A-1) An electronic component according to one embodiment comprises a substrate, a cover glass, an image sensor disposed between the substrate and the cover glass, a support member that supports the cover glass and the image sensor on the substrate, and the barrier material provided on the joint between the cover glass and the support member.
[0160] Such electronic components can be manufactured, for example, by a manufacturing method comprising a coating step of applying a barrier material forming composition to the joint between a support member and a cover glass, and a barrier material forming step of heating the coated composition to form a barrier material on the joint.
[0161] (Electronic component A-2) One embodiment of the electronic component comprises a substrate, an image sensor disposed on the substrate, and the barrier material provided on the image sensor.
[0162] The above barrier material can be made to have excellent moisture resistance and transparency. For this reason, the above barrier material can also be suitably used as a sealing material for sealing image sensors. Since such electronic components can be used to construct an image sensor package without using a cover glass, it is expected that the size of the components will be reduced and handling will be improved.
[0163] In this application, the visible light transmittance (550nm) of the barrier material per 1mm thickness is preferably 95% or higher, more preferably 97% or higher, and even more preferably 99% or higher.
[0164] Such electronic components can be manufactured, for example, by a manufacturing method comprising a coating step of applying a barrier material forming composition onto an image sensor, and a barrier material forming step of heating the coated composition to form a barrier material on the image sensor.
[0165] <Application example 2> One embodiment relates to a product having a first member and a second member joined to the first member, wherein the joint between the first member and the second member is treated to prevent moisture. Such a product comprises a first member, a second member, and a barrier material provided between the first member and the second member, wherein the first member and the second member are joined via the barrier material.
[0166] Such a product can be manufactured by a manufacturing method comprising: a first step of placing a barrier material forming composition between a first member and a second member; and a second step of heating the composition to form a barrier material and joining the first member and the second member via the barrier material. This manufacturing method may further include a step of exposing the first member and the second member joined via the barrier material to high temperatures (e.g., reflow soldering, heat curing of chip bonds, drying of materials by heating, etc.).
[0167] Specific examples of such applications include the following electronic components:
[0168] (Electronic parts B-1) An electronic component according to one embodiment comprises a substrate, a cover glass, an image sensor disposed between the substrate and the cover glass, a support member that supports the cover glass and the image sensor on the substrate, and a barrier material that joins the cover glass and the support member.
[0169] Such electronic components can be manufactured, for example, by a manufacturing method comprising the steps of: placing a barrier material forming composition between a support member and a cover glass; heating the composition to form a barrier material; and joining the support member and the cover glass via the barrier material.
[0170] <Application example 3> One application relating to this embodiment concerns a product equipped with a moisture-proof component. Such a product may be an assembly of multiple components, for example, that include the moisture-proof component, and may be a moisture-proof component made of a barrier material.
[0171] Such a product can be manufactured by a manufacturing method comprising: a first step of heating the above-mentioned barrier material forming composition to produce a moisture-proof member made of the barrier material; and a second step of assembling a plurality of members including the moisture-proof member. This manufacturing method may further include a step of exposing the assembly obtained in the second step to high temperatures (for example, reflow soldering, heat curing treatment of chip bonds, drying of materials by heating, etc.).
[0172] Specific examples of such applications include the following electronic components:
[0173] (Electronic parts C-1) An electronic component according to one embodiment comprises a substrate, at least one component selected from the group consisting of a MEMS sensor, a wireless module, and a camera module, and a moisture-proof member having a barrier material.
[0174] The above barrier material has excellent moisture resistance. Therefore, the above electronic component has excellent moisture resistance, and the deterioration of sensing characteristics due to moisture absorption is sufficiently prevented.
[0175] Such electronic components can be manufactured, for example, by a manufacturing method comprising the steps of: producing a moisture-proof member having a barrier material by heating a barrier material forming composition; and assembling a plurality of members including the moisture-proof member. Here, the barrier material may be formed independently of the substrate and the component, or it may be formed integrally with the component by heating the barrier material forming composition applied to the component.
[0176] Although preferred embodiments of the present invention have been described above, the present invention is not limited to the above embodiments. [Examples]
[0177] (solution 13 C-NMR measurement conditions) Equipment name: JEOL RESONANCE ECX400II Observed nucleus: 13C Observation frequency: 10.052MHz Measurement temperature: Room temperature (23℃) Measurement solvent: CDCl3 Pulse width: 11.4 μs (45°) Pulse repetition time: 2.0 seconds Total number of times: 700 Sample concentration (sample / solvent): 100 mg / 1.0 ml
[0178] (solution 1 H-NMR measurement conditions) Equipment name: JEOL RESONANCE ECX400II Observed nucleus: 1H Observation frequency: 399.78MHz Measurement temperature: Room temperature (23℃) Measurement solvent: CDCl3 Pulse width: 6.64 μs (90°) Pulse repetition time: 5.0 seconds Total number of times: 8 Sample concentration (sample / solvent): 10 mg / 1.0 ml
[0179] (Example 1) <Preparation of polyether-modified polydimethylsiloxane> As the polyether-modified polydimethylsiloxane, a polyether-modified polydimethylsiloxane having N2 / N1 of 2.6, S C2 / S C1 of 2.6, S H2 / S H1 of 1.2 (hereinafter also referred to as polyether-modified polydimethylsiloxane (S-1)) was prepared.
[0180] <Preparation of barrier material-forming composition> 10 parts by mass of 2-BuOH (manufactured by FUJIFILM Wako Pure Chemical Corporation), 64.9 parts by mass of silane oligomer (manufactured by Shin-Etsu Chemical Co., Ltd., product name: X-40-9227), 14.3 parts by mass of methyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., product name: KBM-13, hereinafter abbreviated as "MTMS"), 2.0 parts by mass of linear polysiloxane (manufactured by Momentive Performance Materials Japan LLC, product name: YF3800, kinematic viscosity at 25°C: 80 mm 2 / s), 0.1 parts by mass of nitric acid, and 11.3 parts by mass of water were mixed, and the mixture was reacted at 70°C for 1 hour while stirring with a stir bar. Next, 0.28 parts by mass of a nickel catalyst (manufactured by Momentive Performance Materials Japan LLC, product name: CR12, solid content: 12% by mass), 0.02 parts by mass of an aluminum catalyst (aluminum alkylacetoacetate diisopropylate, manufactured by Matsumoto Fine Chemical Co., Ltd., product name: Aluminum Chelate M), and 0.5 parts by mass of the polyether-modified polydimethylsiloxane (S-1) were added and mixed to obtain a barrier material-forming composition.
[0181] (Example 2) As the polyether-modified polydimethylsiloxane, a polyether-modified polydimethylsiloxane having N2 / N1 of 3.5, S C2 / S C1 of 3.5, S H2 / S H1A polyether-modified polydimethylsiloxane (hereinafter also referred to as polyether-modified polydimethylsiloxane (S-2)) with a ratio of 1.6 was prepared. A barrier material-forming composition was obtained in the same manner as in Example 1, except that polyether-modified polydimethylsiloxane (S-1) was replaced with polyether-modified polydimethylsiloxane (S-2).
[0182] (Comparative Example 1) As polyether-modified polydimethylsiloxane, the N2 / N1 ratio is 6.2, S C2 / S C1 6.2, S H2 / S H1 A polyether-modified polydimethylsiloxane (hereinafter also referred to as polyether-modified polydimethylsiloxane (X-1)) with a ratio of 2.9 was prepared. A barrier material-forming composition was obtained in the same manner as in Example 1, except that polyether-modified polydimethylsiloxane (S-1) was replaced with polyether-modified polydimethylsiloxane (X-1).
[0183] (Comparative Example 2) As polyether-modified polydimethylsiloxane, the N2 / N1 ratio is 4.4, S C2 / S C1 4.4, S H2 / S H1 A polyether-modified polydimethylsiloxane (hereinafter also referred to as polyether-modified polydimethylsiloxane (X-2)) with a ratio of 1.9 was prepared. A barrier material forming composition was obtained in the same manner as in Example 1, except that polyether-modified polydimethylsiloxane (S-1) was replaced with polyether-modified polydimethylsiloxane (X-2).
[0184] (Evaluation method) The barrier material-forming compositions obtained in the examples and comparative examples were evaluated for their moisture resistance (moisture absorption rate) and visibility using the following method. The results are shown in Table 1.
[0185] <Moisture resistance (moisture absorption rate)> A 40mm square base substrate was prepared by masking one side of a 0.4mm thick copper-clad laminate MCL-E-700G (manufactured by Hitachi Chemical Co., Ltd., product name) and immersing it in a copper etching solution to remove the copper foil from one side. Next, a barrier material forming composition was applied to the side of the base substrate from which the copper foil had been removed, so that the thickness after drying would be 30μm. The substrate was then dried at 150°C for 1 hour using a safety oven (manufactured by ESPEC Corporation, product name: SPHH-202). As a result, a barrier material was formed on the substrate, and an evaluation substrate with a barrier material was obtained. The evaluation substrate with barrier material was dried at 150°C for 1 hour using a safety oven (ESPEC Corporation, product name: SPHH-202) to obtain a measurement sample. The mass of the obtained measurement sample was measured to determine the initial mass m4. Next, the sample was treated in a constant temperature and humidity chamber (Kato Corporation, product name: SE-44CI-A) at 85°C / 85%RH for 120 hours to obtain a sample after constant temperature and humidity treatment. The mass of the measurement sample after constant temperature and humidity treatment was measured to determine the mass m5. From the initial mass m4 and the mass m5 after constant temperature and humidity treatment, the moisture absorption rate QB (%) was calculated using the following formula. QB = 100 × (m5 - m4) / m4
[0186] <Visibility> A barrier material-forming composition was applied to a three-terminal regulator (SOT-89 NJM78L05UA, manufactured by New Japan Radio Co., Ltd.) to a thickness of 30 μm after drying. The mixture was then dried at 150°C for 1 hour using a safety oven (ESPEC Corporation, product name: SPHH-202). Afterward, the label on the three-terminal regulator was visually evaluated to determine if it was recognizable.
[0187] [Table 1]
Claims
1. The mixture comprises a hydrolysis polycondensate of a silane compound containing a silane oligomer and a silane monomer, a curing catalyst, and a polyether-modified polydimethylsiloxane. The polyether-modified polydimethylsiloxane 1 In the 1H-NMR spectrum, peak P corresponds to the hydrogen atom on the carbon atom bonded to the silicon atom. H1 Peak area S H1 Peak P corresponds to the hydrogen atom on the carbon atom bonded to the oxygen atom. H2 Peak area S H2 The ratio (S H2 / S H1 ) is between 1.0 and 1.8, A barrier material forming composition wherein the polyether-modified polydimethylsiloxane has a structural unit (1-1) represented by the following formula (1-1) and a structural unit (1-2) represented by the following formula (1-2), and the terminal end of the polyether-modified polydimethylsiloxane is a trialkylsilyl group. 【Chemistry 1】 [In the formula, R1 and R2 represent alkanediyl groups, R3 represents an alkyl group, and n represents an integer of 2 or more.]
2. The composition according to claim 1, wherein the silane oligomer has a silicon atom bonded to three oxygen atoms.
3. The composition according to claim 1 or 2, wherein the ratio of the total number of silicon atoms bonded to three oxygen atoms and silicon atoms bonded to four oxygen atoms to the total number of silicon atoms in the silane oligomer is 30% or more.
4. The composition according to any one of claims 1 to 3, wherein the silane monomer comprises at least one selected from the group consisting of alkyltrialkoxysilane, aryltrialkoxysilane, and tetraalkoxysilane.
5. The composition according to any one of claims 1 to 4, wherein the content of the silane monomer in the silane compound is 5 to 40 parts by mass per 100 parts by mass of the silane oligomer.
6. The composition according to any one of claims 1 to 5, wherein the silane compound further contains a linear polysiloxane.
7. The kinematic viscosity of the linear polysiloxane at 25°C is 50 mm². 2 The composition according to claim 6, wherein the value is / s or greater.
8. The composition according to claim 6 or 7, wherein the linear polysiloxane has a diorganopolysiloxane chain.
9. The composition according to any one of claims 6 to 8, wherein the linear polysiloxane has a group selected from the group consisting of a silanol group and an alkoxy group at both ends.
10. The composition according to any one of claims 6 to 9, wherein the amount of the linear polysiloxane in the silane compound is 1 to 30 parts by mass per 100 parts by mass of the silane oligomer.
11. A method for producing the composition according to any one of claims 1 to 10, A step of heating the silane compound in the presence of an acid catalyst to obtain the hydrolyzed polycondensate, A step of mixing the hydrolyzed polycondensate, the curing catalyst, and the polyether-modified polydimethylsiloxane, A manufacturing method that includes the following features.
12. The production method according to claim 11, wherein the acid catalyst comprises at least one selected from the group consisting of acetic acid, phosphoric acid, hydrochloric acid, and nitric acid.
13. A method for producing a barrier material, comprising the step of curing a composition according to any one of claims 1 to 10 to form a barrier material.
14. A method for manufacturing a product having a moisture-proofed component, A first step of applying the composition according to any one of claims 1 to 10 onto a member, A second step involves curing the applied composition to form a barrier material on the member, A manufacturing method that includes the following features.
15. A method for manufacturing a product comprising a first member and a second member joined to the first member, wherein the joint between the first member and the second member is treated to prevent moisture damage, A first step of placing the composition according to any one of claims 1 to 10 between a first member and a second member, A second step involves curing the composition to form a barrier material, and joining the first member and the second member via the barrier material. A manufacturing method that includes the following features.
16. A method for manufacturing a product equipped with a moisture-proofing member, A first step of curing the composition according to any one of claims 1 to 10 to produce a moisture-proof member having a barrier material, A second step involves assembling a plurality of members, including the moisture-proof member, A manufacturing method that includes the following features.
17. A barrier material which is a cured product of the composition according to any one of claims 1 to 10.
18. Components and A barrier material according to claim 17 formed on the member, A product that possesses these features.
19. The invention comprises a first member, a second member, and a barrier material according to claim 17 provided between the first member and the second member, A product in which the first member and the second member are joined together via the barrier material.
20. A product that is an assembly of multiple members, including a moisture-proof member having the barrier material described in claim 17.
Citation Information
Patent Citations
Barrier film laminate
JP2011093195A
Antifouling system containing silicone hydrogel
JP2016510079A