Artificial leather and method for manufacturing the same
A semi-grain-like artificial leather with a multi-layer resin structure and polycarbonate-based polyurethane outermost layer addresses lightfastness and abrasion resistance issues, ensuring uniform color and durability for outdoor applications.
Patent Information
- Application Number
- JP2026512248
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2025-02-26
- Filing Date
- 2026-02-17
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2046-02-17
AI Technical Summary
Existing artificial leathers used in outdoor applications lack sufficient lightfastness and abrasion resistance, with uneven color development due to surface irregularities and dye usage.
A semi-grain-like artificial leather with a discontinuous resin layer comprising three or more layers, where the outermost layer is polycarbonate-based polyurethane and the intermediate layer contains a pigment, with specific thickness ratios and minimal dye content, ensuring uniform color development and improved durability.
The solution achieves both lightfastness and abrasion resistance suitable for outdoor use, with uniform color development, making it suitable for furniture, vehicle interiors, and clothing.
Smart Images

Figure 0007948488000005 
Figure 0007948488000006 
Figure 0007948488000001
Abstract
Description
[Technical Field]
[0001] This invention relates to artificial leather. [Background technology]
[0002] Artificial leather has been used in a wide range of applications, including clothing, furniture, and automotive interior materials, due to its superior properties compared to natural leather, such as durability and uniform appearance. In recent years, there has been a growing need for greater diversification of appearance, and in addition to artificial leather with a resin layer on the surface, so-called grain-like artificial leather with a discontinuous resin layer, so-called semi-grain-like artificial leather, has also been proposed.
[0003] For example, Patent Document 1 proposes a sheet-like material in which at least one surface of a fibrous structure containing ultrafine fibers is napped, and resin layers are intermittently formed on the napped surface, with two or more resin layers comprising the sheet, wherein at least the resin layer on the fibrous structure side is colored, and the outermost surface resin layer is not colored. It is stated that according to this invention, it is possible to obtain a leather-like sheet-like material that can express the feel of natural nubuck leather, the napped texture of suede leather, and melange-like colors, depth of color, and luster that are not found in natural leather.
[0004] Furthermore, Patent Document 2 proposes a leather-like fabric characterized by a fibrous structure comprising ultrafine fibers with an average single fiber diameter within a specific range, having a pile on at least one surface of the fibrous structure, having a discontinuous resin layer formed on the pile surface, the resin layer consisting of two or more layers, and containing a pigment in at least one of the resin layers. It is stated that this invention makes it possible to obtain a leather-like fabric that has a tactile feel similar to natural nubuck leather, a piled feel similar to suede leather, and also excellent lightfastness. [Prior art documents] [Patent Documents]
[0005] [Patent Document 1] Japanese Patent Publication No. 2019-65450 [Patent Document 2] Japanese Patent Publication No. 2018-123437 [Overview of the project] [Problems that the invention aims to solve]
[0006] Incidentally, as the applications for artificial leather diversify, it is increasingly being used in furniture installed outdoors. Such applications require a higher level of lightfastness and abrasion resistance than before.
[0007] In this regard, the sheet-like material related to the technology proposed in Patent Document 1 certainly combines the tactile feel of natural nubuck leather with the napped texture of suede leather, and has a melange-like color, and has been suitably used in conventional applications. However, because the fibrous structure is prone to discoloration and fading due to ultraviolet light and is colored with dyes, further improvements are needed in terms of lightfastness and abrasion resistance.
[0008] Furthermore, while the leather-like fabric proposed in Patent Document 2 exhibits a certain degree of lightfastness by incorporating pigments into the resin layer, there is still room for further improvement in terms of lightfastness and abrasion resistance.
[0009] Therefore, the object of the present invention, made in view of the above problems, is to provide a semi-grain-like artificial leather that achieves both lightfastness and abrasion resistance suitable for outdoor use, and has uniform color development. [Means for solving the problem]
[0010] The inventors initially attempted to create a discontinuous resin layer consisting of multiple layers on the surface of a fibrous base material, either without using dyes or with an extremely low dye content, and to incorporate a pigment into one of these layers. However, they found that this alone did not provide sufficient abrasion resistance for outdoor use, and the color development was uneven. Through further investigation, they discovered that the unevenness of the surface of the fibrous base material caused variations in the thickness of the pigment-containing resin layer, significantly affecting the uniformity of the color development. They then found that the configuration of multiple resin layers in the discontinuous resin layer is crucial for improving abrasion resistance. The inventors conducted further studies and ultimately found that by using three or more resin layers, setting the thickness of the resin layer closest to the fibrous base material to a specific range, and reducing surface irregularities of the fibrous base material, they could obtain an artificial leather that exhibits uniform color development. Furthermore, by using a polycarbonate-based polyurethane as the constituent resin of the outermost resin layer among the multiple resin layers of the discontinuous resin section, and containing a pigment in the intermediate layer of the discontinuous resin section, they were able to obtain an artificial leather that achieves both lightfastness and abrasion resistance suitable for outdoor use.
[0011] This invention was completed based on these findings, and according to this invention, the following inventions are provided.
[0012] [1] Artificial leather comprising a fibrous base material containing ultrafine fibers and a polymeric elastic material, The aforementioned artificial leather is The artificial leather has a discontinuous resin portion on at least one surface, The artificial leather does not contain dye, or it contains dye, and the proportion of dye in the artificial leather is 1.0% by mass or less. The discontinuous resin portion is arranged in order from the fibrous substrate side, Innermost layer, One or more intermediate layers, outermost layer It has at least 3 layers, The outermost layer is made of polycarbonate-based polyurethane. The aforementioned intermediate layer contains a pigment, The content ratio of the pigment in the discontinuous resin portion is 0.5% by mass or more and 5.0% by mass or less. Furthermore, artificial leather that satisfies the following equation 1.
[0013] 0.35≦D b / D≦0.60 (Formula 1) Here, D is the thickness (μm) of the discontinuous resin portion, and D b This is the thickness (μm) of the innermost layer.
[0014] [2] The artificial leather according to [1], wherein the constituent resin of the intermediate layer or the constituent resin of the innermost layer is polycarbonate polyurethane.
[0015] [3] The artificial leather according to [1], wherein the constituent resin of the intermediate layer and the constituent resin of the innermost layer of the discontinuous resin portion are polycarbonate-based polyurethane.
[0016] [4] The artificial leather according to any one of [1] to [3] above, wherein the pigment is carbon black.
[0017] [5] The artificial leather according to any one of [1] to [4], wherein the average particle size of the pigment is 0.05 μm or more and 0.20 μm or less.
[0018] [6] The artificial leather according to any one of [1] to [5], wherein the polymeric elastic body is a polycarbonate-based polyurethane.
[0019] [7] The artificial leather according to any one of [1] to [6], wherein the polymeric elastic body contains a black pigment.
[0020] [8] The artificial leather according to [7], wherein the proportion of the black pigment contained in the polymer elastic material is 0.1% by mass or more and 5.0% by mass or less in the polymer elastic material.
[0021] [9] The artificial leather according to [7] or [8], wherein the average particle size of the black pigment contained in the polymer elastic material is 0.05 μm or more and 0.20 μm or less.
[0022]
[10] A method for manufacturing artificial leather according to any of the above [1] to [9], A process for forming a sheet-like material comprising a fibrous base material containing ultrafine fibers and a polymeric elastic material, The process of forming, on at least one surface of the sheet-like material, in order from the fibrous substrate side, an innermost layer that does not contain pigment, one or more intermediate layers that contain pigment, and an outermost layer that does not contain pigment. A method for manufacturing artificial leather, including [the specified component].
[0023]
[11] Furniture containing artificial leather as described in any of [1] to [9] above.
[0024]
[12] A seat comprising artificial leather as described in any of [1] to [9] above.
[0025]
[13] Clothing containing artificial leather as described in any of [1] to [9] above.
[0026]
[14] Vehicle interior material including artificial leather as described in any of [1] to [9] above. [Effects of the Invention]
[0027] According to the present invention, it is possible to obtain a semi-grain-like artificial leather that achieves both lightfastness and abrasion resistance suitable for outdoor use, and also has uniform color development. Furthermore, the artificial leather according to the present invention can be used in a wide range of applications, from furniture, chairs, and vehicle interior materials to clothing, but is particularly suitable for furniture intended for outdoor use. [Brief explanation of the drawing]
[0028] [Figure 1] Figure 1 is a conceptual diagram illustrating a method for measuring and calculating the twist count of a multifilament in a woven fabric according to one embodiment of the present invention. [Figure 2] Figure 2 is a cross-sectional conceptual diagram illustrating and explaining the structure of artificial leather according to one embodiment of the present invention. [Modes for carrying out the invention]
[0029] The present invention relates to artificial leather comprising a fibrous base material containing ultrafine fibers and a polymeric elastic body, wherein the artificial leather has a discontinuous resin portion on at least one surface, does not contain dye, or the dye content in the artificial leather is 1.0% by mass or less, the discontinuous resin portion has at least three layers in order from the fibrous base material side: an innermost layer, one or more intermediate layers, and an outermost layer, the constituent resin of the outermost layer is polycarbonate-based polyurethane, the intermediate layer contains a pigment, the pigment content in the discontinuous resin portion is 0.5% by mass or more and 5.0% by mass or less, and furthermore satisfies the following formula 1.
[0030] 0.35≦D b / D≦0.60 (Formula 1) Here, D is the thickness (μm) of the discontinuous resin portion, and D b This is the thickness (μm) of the innermost layer.
[0031] The components will be described in detail below, but the present invention is not limited in any way to the scope described below, as long as it does not exceed the spirit of the invention, and various modifications are possible without departing from the spirit of the invention.
[0032] [Fibrous base material containing ultrafine fibers] The artificial leather according to one embodiment of the present invention (hereinafter also referred to as "this embodiment") includes a fibrous base material containing ultrafine fibers. Further details of these are described below.
[0033] (Ultrafine fibers) The fibrous base material according to this embodiment contains ultrafine fibers. In the present invention, "ultrafine fibers" refers to fibers with a single fiber diameter of 10 μm or less, as measured by the method described later.
[0034] The components that make up these ultrafine fibers include polyester resins, polyamide resins, acrylic resins, cellulose resins, polyolefin resins, and silicone resins. However, from the viewpoint of durability, and especially mechanical strength, polyester resins and polyamide resins are preferably used, and polyester resins, which have excellent heat resistance, are even more preferable.
[0035] In this invention, "polyester resin" refers to a resin in which the mole fraction of the polyester unit in the repeating unit is 80 mol% or more and 100 mol% or less. Unless otherwise specified, the same applies to any other resins that are described as "...-type resin".
[0036] Generally, polyester resins can be obtained, for example, from dicarboxylic acids and / or their ester-forming derivatives and diols, or by ring-opening polymerization of lactones.
[0037] In this embodiment, examples of dicarboxylic acids and / or their ester-forming derivatives used in the polyester resin include terephthalic acid, isophthalic acid, 2,6-naphthalenedicarboxylic acid, diphenyl-4,4'-dicarboxylic acid and its ester-forming derivatives. In this invention, ester-forming derivatives refer to lower alkyl esters, acid anhydrides, acyl chlorides, etc. of dicarboxylic acids. Specifically, methyl esters, ethyl esters, hydroxyethyl esters, etc., are preferably used. A more preferred embodiment of the dicarboxylic acid and / or its ester-forming derivative used in this invention is terephthalic acid and / or its dimethyl ester.
[0038] Furthermore, examples of diols used in the polyester resin according to this embodiment include ethylene glycol, 1,3-propanediol, 1,4-butanediol, and cyclohexanedimethanol. Among these, ethylene glycol is preferred.
[0039] Examples of lactones used in the polyester resin according to this embodiment include lactic acid, γ-butyrolactone, and ε-caprolactone. Among these, lactic acid, which is derived from plants, is preferred.
[0040] In this embodiment, the polyester resins that are preferred include polyethylene terephthalate, polybutylene terephthalate, polytrimethylene terephthalate, polyethylene naphthalate, polylactic acid, polycaprolactone, and mixtures and copolymers of these polyester resins. Among these, polyethylene terephthalate, polybutylene terephthalate, polytrimethylene terephthalate, polylactic acid, and mixtures and copolymers of these polyester resins are preferred because they can be used to produce artificial leather with excellent heat resistance, light resistance, and other properties.
[0041] Furthermore, the polyester resin according to this embodiment may contain inorganic particles such as titanium dioxide particles, lubricants, pigments, heat stabilizers, ultraviolet absorbers, conductive agents, heat storage agents, and antibacterial agents, depending on the purpose.
[0042] Furthermore, the cross-sectional shape of the ultrafine fibers can be either round or irregular. Specific examples of irregular cross-sections include elliptical, flat, triangular polygons (including those with rounded corners), sectors, and cross shapes.
[0043] In this embodiment, the ultrafine fibers preferably have an average single fiber diameter of 0.1 μm or more and 10.0 μm or less. A range where the upper limit of the average single fiber diameter of the ultrafine fibers is preferably 10.0 μm or less, more preferably 7.0 μm or less, and even more preferably 5.0 μm or less results in an artificial leather with superior flexibility. On the other hand, a range where the lower limit of the average single fiber diameter of the ultrafine fibers is preferably 0.1 μm or more, more preferably 0.5 μm or more, and even more preferably 1.0 μm or more results in an artificial leather with superior abrasion resistance.
[0044] In this invention, the single fiber diameter and average single fiber diameter of the ultrafine fibers are measured and calculated by the following method. That is, (i) Cut out three 1cm x 0.1cm test pieces randomly from the artificial leather using a razor blade. (ii) The exposed cross-sections cut out with a razor blade are photographed using a scanning electron microscope (SEM, Keyence Corporation "VHX-D500 / D510" or a scanning electron microscope with equivalent performance) at a magnification (approximately 500x to 2000x) that allows for clear observation of 100 to 1000 cross-sections. (iii) Randomly select 50 fibers that appear to be ultrafine fibers (fibers with a single fiber diameter of 10 μm or less) from the captured SEM image, and measure the single fiber diameter of those fibers. If the cross-sectional shape is a perfect circle, the diameter can be measured directly. However, if the cross-sectional shape is irregular, the equivalent diameter of the circle is used. That is, first measure the cross-sectional area of the fiber, and then use the value obtained by calculating the diameter of the circle that gives that cross-sectional area using the following formula. Single fiber diameter (μm) = (4 × (cross-sectional area of single fiber (μm) 2 )) / π) 1 / 2 ···(formula) Furthermore, if the measurement and calculation results show that the single fiber diameter exceeds 10 μm, that fiber will be excluded as not being an ultrafine fiber, and a fiber that appears to be an ultrafine fiber (a fiber with a single fiber diameter of 10 μm or less) will be randomly selected again. (iv) Repeat steps (ii) and (iii) for the remaining specimens. (v) Calculate the arithmetic mean (μm) of the single fiber diameters (μm) of the 150 points obtained, round it to the second decimal place, and take this as the average single fiber diameter (μm) of the ultrafine fibers.
[0045] (Fibrous base material) The fibrous base material according to this embodiment contains 50% by mass or more of the ultrafine fibers. Examples of this fibrous base material include woven or knitted fabrics, nonwoven fabrics, and combinations thereof, such as an entanglement of a nonwoven fabric and a woven or knitted fabric. In this invention, "woven or knitted fabric" is a general term for both woven and knitted fabrics.
[0046] In this embodiment, when the fibrous base material is a woven or knitted fabric made of ultrafine fibers, examples of woven fabrics include plain weave, twill weave, satin weave, and various woven fabrics based on these weave structures. Examples of knitted fabrics include warp knitting, weft knitting represented by tricot knitting, lace knitting, and various knitted fabrics based on these knit structures.
[0047] In this embodiment, if the fibrous base material is a nonwoven fabric made of ultrafine fibers, the nonwoven fabric may be either a long-fiber nonwoven fabric or a short-fiber nonwoven fabric, but it is more preferable to use a short-fiber nonwoven fabric because it is easier to obtain an artificial leather with excellent flexibility.
[0048] When the fibrous base material according to this embodiment is a short-fiber nonwoven fabric made of ultrafine fibers, the fiber length of the ultrafine fibers is preferably 25 mm or more and 90 mm or less. When the fiber length of the ultrafine fibers is 25 mm or more, preferably 35 mm or more, and more preferably 40 mm or more, an artificial leather with excellent mechanical strength is obtained. On the other hand, when the fiber length of the ultrafine fibers is 90 mm or less, preferably 80 mm or less, and more preferably 70 mm or less, an artificial leather with excellent flexibility is obtained.
[0049] Furthermore, as described above, the fibrous base material according to this embodiment may also be an entanglement of a nonwoven fabric made of ultrafine fibers and a woven or knitted fabric. The fineness of the woven or knitted fabric used here is not limited to the ultrafine fibers as defined in this invention. Having such a fibrous base material results in artificial leather with higher abrasion resistance as well as superior mechanical strength. In this case as well, the woven or knitted fabric may be in the form exemplified above. In particular, woven fabrics are preferred because they have less dimensional change and are less prone to wrinkling during the manufacturing of artificial leather, resulting in artificial leather with excellent uniformity in appearance, and in particular, plain weave woven fabrics are preferred from the viewpoint of mechanical strength.
[0050] When the fibrous base material is an entanglement of a nonwoven fabric and a woven or knitted fabric, it is preferable to use multifilaments as the fibers constituting the woven or knitted fabric. Examples of components constituting the filaments (single threads) of the multifilament include polyester resins and polyamide resins. Among these, polyester resins, which have excellent durability and heat resistance, are preferred. Specific examples of polyester resins in this case include polyalkylene terephthalates such as polyethylene terephthalate, polybutylene terephthalate, and polytrimethylene terephthalate, polylactic acid, and mixtures and copolymers of these polyester resins.
[0051] When the fibrous base material is an entanglement of a nonwoven fabric and a woven or knitted fabric, composite fibers (hereinafter sometimes referred to as side-by-side or similar composite fibers) composed of two or more polymers compounded in a side-by-side or eccentric core-sheath type can also be used as the fibers constituting the woven or knitted fabric. For example, in side-by-side or similar composite fibers composed of two or more polymers with different intrinsic viscosity (IV), stress concentration on the high-viscosity side during stretching causes different internal strains between the two components. Due to this internal strain, the high-viscosity side shrinks significantly due to the difference in elastic recovery rate after stretching and the difference in thermal shrinkage during the heat treatment process, causing strain within the single fiber and resulting in three-dimensional coil-type crimping. This three-dimensional coil-type crimping improves the stretchability as artificial leather.
[0052] If the woven fabric is a woven fabric, the average single fiber diameter of the filaments (single yarns) of the multifilaments constituting the woven fabric is preferably 1.0 μm or more and 30.0 μm or less. By setting the upper limit of the average single fiber diameter range of the multifilaments constituting the woven fabric to preferably 30.0 μm or less, more preferably 15.0 μm or less, and even more preferably 13.0 μm or less, an artificial leather with excellent flexibility is obtained. On the other hand, by setting the lower limit of the average single fiber diameter range of the multifilaments constituting the woven fabric to preferably 1.0 μm or more, more preferably 8.0 μm or more, and even more preferably 9.0 μm or more, an artificial leather with even better mechanical strength is obtained.
[0053] In this invention, the average single fiber diameter of the filaments of the multifilament constituting the fabric is measured and calculated by the following method. That is, (i) Randomly cut out test pieces of approximately 10 cm x 10 cm from the artificial leather, sand the back surface of the test pieces with sandpaper to expose the fabric, identify the direction of the multifilaments constituting the fabric, designate one multifilament direction as the warp direction and the direction perpendicular to it as the weft direction. However, if the warp and weft directions of the multifilaments constituting the fabric in the artificial leather can be clearly identified, such as when artificial leather is available in roll form, then those directions shall be designated as the warp and weft directions of the multifilaments constituting the fabric in the artificial leather. (ii) From the artificial leather, cut out three random test pieces measuring 1 cm in the weft direction and 0.1 cm in the warp direction of the multifilament of the woven fabric for measuring the warp threads of the woven fabric, and three random test pieces measuring 0.1 cm in the weft direction and 1 cm in the warp direction of the multifilament of the woven fabric for measuring the weft threads of the woven fabric, using a razor blade. (iii) The exposed cross-sections cut out with a razor blade are photographed using a scanning electron microscope (SEM, Keyence Corporation "VHX-D500 / D510" or a scanning electron microscope with equivalent performance) at a magnification (approximately 500x to 2000x) that allows for clear observation of 20 to 50 cross-sections. (iv) Randomly select 10 filaments from the captured SEM image and measure the diameter of each individual fiber. If the cross-sectional shape is a perfect circle, the diameter can be measured directly. However, if the cross-sectional shape is irregular, the equivalent diameter is used. This is obtained by first measuring the cross-sectional area of the fiber and then calculating the diameter of the circle that corresponds to that cross-sectional area using the following formula. Single fiber diameter (μm) = (4 × (cross-sectional area of single fiber (μm) 2 )) / π) 1 / 2 ···(formula) (v) Repeat steps (iii) and (iv) for the remaining specimens. (vi) Calculate the arithmetic mean (μm) of the single fiber diameters (μm) of the 30 points obtained, round to the second decimal place, and take this as the average single fiber diameter (μm) of the filament.
[0054] The number of filaments included in the multifilament constituting the fabric, i.e., the filament count, is preferably 30 to 300. A range where the upper limit of the filament count is preferably 30 or more, and more preferably 50 or more, results in artificial leather with excellent mechanical strength. On the other hand, a range where the lower limit of the filament count is preferably 300 or less, more preferably 250 or less, and even more preferably 100 or less, results in artificial leather with excellent flexibility. In this case, the number of filaments in the warp threads and the number of filaments in the weft threads may be the same or different.
[0055] Furthermore, it is preferable that the twist count of the multifilaments constituting the fabric is between 1000 T / m and 4000 T / m. Regarding the range of twist counts, an upper limit of preferably 4000 T / m or less, more preferably 3500 T / m or less, and even more preferably 3000 T / m or less results in an artificial leather with excellent flexibility, while an lower limit of preferably 1000 T / m or more, more preferably 1500 T / m or more, and even more preferably 2000 T / m or more results in an artificial leather with excellent mechanical strength.
[0056] In the present invention, the twist number of filaments of the multifilament constituting the woven fabric is measured and calculated by the following method. That is, (i) A test piece of about 10 cm × 10 cm is randomly cut out from the artificial leather, the back surface of the test piece is ground with sandpaper to expose the woven fabric, and three small pieces of about 1 cm × 1 cm are randomly cut out while avoiding the end portions of the test piece. (ii) Using a scanning electron microscope (SEM, "VHX-D500 / D510" manufactured by Keyence Corporation, or a scanning electron microscope having equivalent performance) on the back surface of the small piece with the exposed woven fabric, photographing is performed at a magnification (about 500 to 2000 times) at least such that ten multifilaments in each of one fiber direction of the woven fabric and the direction perpendicular thereto are included in the same image, and one single yarn in the multifilament can be clearly observed. (iii) From the captured SEM image, ten multifilaments are randomly selected for each of one fiber direction of the woven fabric and the direction perpendicular thereto. (iv) As shown in Figure 1, one twist section 12 is randomly selected from the selected multifilament 11, and the distance L between the intersection point 14a of the perpendicular line drawn from one end 14 to the fiber direction 13 of the multifilament and the intersection point 15a of the perpendicular line drawn from the other end 15 to the fiber direction 13 of the multifilament T (16) is measured. (v) The distance L T corresponds to the distance for 0.5 twist of the multifilament, so the twist number of the multifilament is calculated using the following formula Twist number (T / m) = 0.5 / L T (m) ···(Formula) (vi) Steps (iii) to (v) are similarly repeated for the remaining small pieces. (vii) The arithmetic mean value (T / m) of the obtained twist numbers (T / m) at a total of 30 points is calculated, and rounded off to the first decimal place.
[0057] In artificial leather, the weave density of the fabric is preferably 70 threads / 2.54cm or more and 120 threads / 2.54cm or less in both the warp and weft directions. A lower limit of the weave density of the fabric is preferably 70 threads / 2.54cm or more, more preferably 80 threads / 2.54cm or more, resulting in artificial leather with excellent mechanical strength. On the other hand, a weave density of 120 threads / 2.54cm or less, preferably 110 threads / 2.54cm or less, results in artificial leather with excellent flexibility.
[0058] [Polymer elastic material] The artificial leather according to this embodiment includes a polymeric elastic material. Further details of these materials are described below.
[0059] First, the main component of the polymeric elastic body according to this embodiment is preferably selected from the group consisting of polyurethane, styrene-butadiene rubber (SBR), nitrile rubber (NBR), silicone rubber, and acrylic resin. Here, in the present invention, the "main component" of the polymeric elastic body means that the mass of the component is 50% by mass or more of the total mass of the polymeric elastic body. In particular, it is more preferable that the main component of the polymeric elastic body is polyurethane, as this results in an artificial leather with a more substantial feel and superior durability that can withstand actual use. It is even more preferable that the mass of polyurethane relative to the total mass of the polymeric elastic body is 90% by mass or more and 100% by mass or less.
[0060] In this embodiment, when the main component of the polymeric elastic material is polyurethane, this polyurethane may be either an organic solvent-based polyurethane used in a dissolved state in an organic solvent, or a water-dispersible polyurethane used in a dispersed state in water. Furthermore, it is preferable that this polyurethane is obtained by the reaction of a polymer diol, an organic diisocyanate, and a chain extender.
[0061] First, examples of polyurethane polymer diols according to this embodiment include polycarbonate diols, polyester diols, polyether diols, silicone diols, and fluorine diols, as well as copolymers of these. Among these, polycarbonate diols are preferred from the viewpoint of light resistance, hydrolysis resistance, and heat resistance. These polycarbonate diols can be produced by transesterification of alkylene glycol and carbonate ester, or by reaction of phosgene or chlorformate ester with alkylene glycol. Examples of alkylene glycols include, Linear alkylene glycols such as ethylene glycol, propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,9-nonanediol, and 1,10-decanediol, Branched alkylene glycols such as neopentyl glycol, 3-methyl-1,5-pentanediol, 2,4-diethyl-1,5-pentanediol, and 2-methyl-1,8-octanediol. Alicyclic diols such as 1,4-cyclohexanediol, Aromatic diols such as bisphenol A, Furthermore, examples include glycerin, trimethylolpropane, and pentaerythritol. In this embodiment, either a polycarbonate diol obtained from a single alkylene glycol or a copolymerized polycarbonate diol obtained from two or more alkylene glycols may be used.
[0062] Next, as an organic diisocyanate of the polyurethane according to this embodiment, for example, Aliphatic diisocyanates such as hexamethylene diisocyanate, dicyclohexylmethane diisocyanate, isophorone diisocyanate, and xylylene diisocyanate, Aromatic diisocyanates such as diphenylmethane diisocyanate and tolylene diisocyanate, Furthermore, combinations (mixtures) of these materials are also possible. In particular, when durability and heat resistance are important, aromatic polyisocyanates such as diphenylmethane diisocyanate are preferred, and when light resistance is important, aliphatic polyisocyanates such as hexamethylene diisocyanate, dicyclohexylmethane diisocyanate, and isophorone diisocyanate are preferred.
[0063] And, as the chain extender for polyurethane according to this embodiment, for example, Amine-based chain extenders such as ethylenediamine and methylenebisaniline, Diol-based chain extenders such as ethylene glycol, or Polyamines obtained by reacting polyisocyanate with water, Furthermore, combinations (mixtures) of these can be cited.
[0064] Furthermore, when the main component of the polymeric elastic body according to this embodiment is a water-dispersible polyurethane, it is preferable to use an internal emulsifier to disperse the water-dispersible polyurethane in water. In other words, the polymeric elastic body according to this embodiment may contain an internal emulsifier. Examples of such internal emulsifiers include cationic internal emulsifiers such as quaternary amine salts, anionic internal emulsifiers such as sulfonates and carboxylates, and nonionic internal emulsifiers such as polyethylene glycol. In addition, a combination of cationic and nonionic internal emulsifiers, or a combination of anionic and nonionic internal emulsifiers, may be used.
[0065] The polymeric elastic material according to this embodiment may contain a black pigment. Examples of black pigments that have good lightfastness include carbon-based black pigments such as carbon black and graphite, and oxide-based black pigments such as iron tetroxide, copper and chromium composite oxides. Among these, carbon black is preferred because it is easy to obtain black pigment with a fine particle size and has excellent dispersibility in the polymer.
[0066] In the case where the polymeric elastic body according to this embodiment contains a black pigment, the average particle diameter of the black pigment contained in the polymeric elastic body is preferably 0.05 μm or more and 0.20 μm or less. The average particle diameter of the black pigment as used in this invention refers to the average particle diameter when the black pigment is present in the polymeric elastic body, and is generally called the secondary particle diameter, and is a value measured and calculated by the method described later. By having a lower limit of 0.05 μm or more, and more preferably 0.07 μm or more, for the range of the average particle diameter of the black pigment, the black pigment is more easily grasped inside the polymeric elastic body, and thus the detachment of the black pigment from the polymeric elastic body is suppressed. As a result, an artificial leather with excellent wash fastness and friction fastness is obtained. On the other hand, by having an upper limit of 0.20 μm or less, more preferably 0.18 μm or less, and even more preferably 0.16 μm or less, for excellent dispersibility when impregnating with the polymeric elastic body, an artificial leather with excellent mechanical strength is obtained.
[0067] In the case where the polymeric elastic body according to this embodiment contains a black pigment, the coefficient of variation (CV) of the particle size of the black pigment contained in the polymeric elastic body is preferably 75% or less. The upper limit of the CV is preferably 75% or less, more preferably 60% or less, and even more preferably 50% or less. This reduces the particle size distribution, suppressing the shedding of small particles from the surface of the polymeric elastic body and the precipitation of significantly aggregated particles into the impregnation tank. As a result, an artificial leather with excellent wash fastness and abrasion fastness is obtained. While there is no particular lower limit to the coefficient of variation in this invention, it is preferably 0.1% or more from the viewpoint of operability when impregnating the polymeric elastic body.
[0068] In this invention, the average particle size and coefficient of variation (CV) of the black pigment are measured and calculated by the following method. (i) 5 mm x 10 μm test pieces are randomly cut from the artificial leather using an ultramicrotome such as the Sorvall MT6000. (ii) The cross-section exposed by cutting with an ultramicrotome is observed at 10,000x magnification using a transmission electron microscope (TEM, for example, Hitachi High-Tech Corporation's "H7700"). (iii) Using image analysis software (for example, "WinROOF" manufactured by Mitani Corporation), randomly select 20 black pigment particles contained within a 2.3 μm × 2.3 μm field of view of the observed image. If there are fewer than 20 black pigment particles contained within the 2.3 μm × 2.3 μm field of view, select the black pigment particles that exist. Measure the area of these black pigment particles, and use the value obtained by calculating the diameter of the circle corresponding to that area using the following formula as the particle size of the black pigment. Particle diameter (μm) = (4 × (Particle area (μm) 2 )) / π) 1 / 2 ···(formula) (iv) The arithmetic mean (μm) of all measured particle sizes is rounded to the third decimal place and taken as the average particle size (μm) of the black pigment. The value obtained by calculating the following formula is taken as the coefficient of variation (CV) of the particle size of the black pigment. Coefficient of variation of particle size (%) = [(standard deviation of particle size) / (arithmetic mean of particle size)] × 100 ... (formula).
[0069] In this embodiment, it is preferable that the content of the black pigment contained in the polymeric elastic material is 0.1% by mass or more and 5.0% by mass or less. A lower limit of the black pigment content is preferably 0.1% by mass or more, more preferably 1.0% by mass or more, resulting in an artificial leather with excellent dark color development. A higher upper limit of the black pigment content is preferably 5.0% by mass or less, more preferably 4.5% by mass or less, and even more preferably 4.0% by mass or less, resulting in an artificial leather with excellent mechanical strength.
[0070] In this invention, the content ratio of the black pigment contained in the polymeric elastic material is measured and calculated by the following method. That is, (i) Shave off the discontinuous resin portion from the surface of the artificial leather with a razor. (ii) The artificial leather from which the discontinuous resin portion has been scraped off is immersed in dimethylformamide or the like to dissolve the polymeric elastic material. (iii) The polymer elastic material is dissolved and filtered and isolated using a filter or the like to separate only the pigment, and the mass of the pigment is measured. (iv) The polymer elastic solution from which the pigment has been removed is heated to a temperature of 100°C for 50 minutes to dry the solvent, and the mass of the polymer elastic solute is measured. (v) The pigment content in the polymer elastic material is calculated using the following formula. The percentage of pigment contained in the aforementioned polymeric elastic material is given by: (mass of pigment) / (mass of polymeric elastic material) × 100 ... (formula).
[0071] The polymeric elastic material according to this embodiment may further contain various additives depending on the purpose, for example, Other pigments besides the aforementioned black pigment, such as inorganic or oxide-based pigments, Flame retardants such as phosphorus-based, halogen-based, and inorganic types, Antioxidants such as phenols, sulfurs, and phosphorus, UV absorbers such as benzotriazoles, triazines, benzophenones, salicylates, cyanoacrylates, and oxalic acid anilides, Light stabilizers such as hindered amines and benzoates, Hydrolysis-resistant agents such as polycarbodiimide, It may contain plasticizers, antistatic agents, surfactants, and coagulation modifiers.
[0072] Generally, the content of polymeric elastic material in artificial leather can be appropriately adjusted considering the type of polymeric elastic material used, the manufacturing method of the polymeric elastic material, and the texture and physical properties. In the artificial leather of this embodiment, the content of the polymeric elastic material is preferably 15% by mass or more and 50% by mass or less relative to the fibrous base material. By setting the lower limit of the polymeric elastic material content to preferably 15% by mass or more, and more preferably 20% by mass or more, the bonding between fibers by the polymeric elastic material can be strengthened, resulting in artificial leather with superior mechanical strength. On the other hand, by setting the upper limit of the polymeric elastic material content to preferably 50% by mass or less, more preferably 45% by mass or less, and even more preferably 40% by mass or less, the artificial leather becomes more flexible.
[0073] In the present invention, the content of polymeric elastic material in a fibrous substrate is measured and calculated by the following method. (1) Cut a 20g sample randomly from the artificial leather using scissors or the like, and completely shave off the discontinuous resin portion from the surface of the artificial leather with a razor. (2) The artificial leather from which the discontinuous resin portion has been scraped off is immersed in dimethylformamide or the like to dissolve the polymeric elastic material, and then separated into a fibrous base material and a polymeric elastic material solution. (3) The polymer elastic solution is heated to a temperature of 100°C for 50 minutes to allow the solvent to dry, and the mass of the polymer elastic solute is measured. (4) Determine the mass of the fibrous base material from the difference between the mass of the artificial leather from which the discontinuous resin portion has been removed and the mass of the extracted polymeric elastic material, and calculate the polymeric elastic material content relative to the fibrous base material using the following formula. The content (by mass) of the polymeric elastic material relative to the fibrous substrate = 100 × (mass of polymeric elastic material) / (mass of fibrous substrate) ... (formula).
[0074] [Discontinuous resin part] The artificial leather according to this embodiment has a discontinuous resin portion on at least one surface. This discontinuous resin portion is arranged sequentially from the fibrous base material side. Innermost layer, One or more intermediate layers, outermost layer It has at least 3 layers, The outermost layer is made of polycarbonate-based polyurethane. The aforementioned intermediate layer contains a pigment, The content ratio of the pigment in the discontinuous resin portion is 0.5% by mass or more and 5.0% by mass or less. Furthermore, the artificial leather according to this embodiment satisfies the following formula 1 with respect to the discontinuous resin portion.
[0075] 0.35≦D b / D≦0.6 (Formula 1) Here, D is the thickness (μm) of the discontinuous resin portion, and D b is the thickness (μm) of the innermost layer. By having the discontinuous resin portion described above on at least one surface of the artificial leather, cracks in the resin layer do not occur when the artificial leather is bent, maintaining good quality and texture, and the portion that is not a discontinuous resin portion becomes an artificial leather with sufficient breathability. Further details of these will be explained below. In this invention, "discontinuous" in "discontinuous resin portion" refers to an embodiment as illustrated in the cross-sectional conceptual diagram of Figure 2 (note that polymer elastic bodies are not shown in this cross-sectional conceptual diagram), in which, when the artificial leather is viewed from the surface, there is a space between the resin portion 23a (23b) and the resin portion 23a (23b), and a part of the fibrous base material 22 constituting the artificial leather 21a (21b) is exposed.
[0076] First, as illustrated in Figure 2, the discontinuous resin portion according to this embodiment has at least three layers, in order from the fibrous substrate side: an innermost layer 231, one or more intermediate layers 232, and an outermost layer 233.
[0077] (Innermost layer, middle layer) In this embodiment, the innermost layer of the discontinuous resin portion refers to the layer that is in direct contact with the fibrous base material of the artificial leather in the discontinuous resin portion, and is closest to the fibrous base material. In this embodiment, the intermediate layer of the discontinuous resin portion refers to the layer located between the outermost layer and the innermost layer, which will be described later, in the discontinuous resin portion.
[0078] The constituent resins of the innermost and intermediate layers are preferably selected from the group consisting of polyurethane, styrene-butadiene rubber (SBR), nitrile rubber (NBR), silicone rubber, and acrylic resin. Here, in the present invention, the "constituent resin" of the innermost and intermediate layers refers to a resin in which the mass of the component is 50% by mass or more of the mass of the layer. In particular, the constituent resin of the innermost and intermediate layers is preferably polyurethane, and more preferably polycarbonate-based polyurethane, because it results in artificial leather with a flexible feel, a leather-like appearance, and excellent abrasion resistance that can withstand actual use. That is, it is also preferable that the constituent resin of the intermediate layer or the constituent resin of the innermost layer is polycarbonate-based polyurethane, and it is also preferable that the constituent resin of the intermediate layer and the constituent resin of the innermost layer of the discontinuous resin portion are polycarbonate-based polyurethane. In the present invention, "polycarbonate-based polyurethane" refers to polyurethane in which the chemical structure derived from polyols that constitute the polyurethane contains 50% by mass or more of a chemical structure derived from polycarbonate-based polyols.
[0079] In this embodiment, when the constituent resin of the innermost layer and intermediate layer of the discontinuous resin portion is polyurethane (this refers to any of the cases in which the constituent resin of the innermost layer of the discontinuous resin portion is polyurethane, the constituent resin of the intermediate layer is polyurethane, or both the constituent resin of the innermost layer and the constituent resin of the intermediate layer of the discontinuous resin portion are polyurethane; the same applies hereafter), this polyurethane may be either an organic solvent-based polyurethane used in a dissolved state in an organic solvent, or a water-dispersible polyurethane used in a dispersed state in water. Furthermore, it is preferable that this polyurethane is a polyurethane obtained by the reaction of a polymer diol, an organic diisocyanate, and a chain extender.
[0080] In this embodiment, when the constituent resin of the innermost and intermediate layers of the discontinuous resin portion is polyurethane, examples of polymer diols include polycarbonate-based diols, polyester-based diols, polyether-based diols, silicone-based diols, and fluorine-based diols, as well as copolymers combining these. Among these, from the viewpoint of light resistance, hydrolysis resistance, and heat resistance, polycarbonate-based diols are preferred for the polyurethane polymer diols. These polycarbonate-based diols can be produced by transesterification of alkylene glycol and carbonate ester, or by reaction of phosgene or chlorformate ester with alkylene glycol. Examples of alkylene glycols include: Linear alkylene glycols such as ethylene glycol, propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,9-nonanediol, and 1,10-decanediol, Branched alkylene glycols such as neopentyl glycol, 3-methyl-1,5-pentanediol, 2,4-diethyl-1,5-pentanediol, and 2-methyl-1,8-octanediol. Alicyclic diols such as 1,4-cyclohexanediol, Aromatic diols such as bisphenol A, Furthermore, examples include glycerin, trimethylolpropane, and pentaerythritol. In this embodiment, either a polycarbonate diol obtained from a single alkylene glycol or a copolymerized polycarbonate diol obtained from two or more alkylene glycols may be used.
[0081] Next, in the case where the innermost layer and intermediate layer of the discontinuous resin portion according to this embodiment are polyurethane, the organic diisocyanate can be, for example, Aliphatic diisocyanates such as hexamethylene diisocyanate, dicyclohexylmethane diisocyanate, isophorone diisocyanate, and xylylene diisocyanate, Aromatic diisocyanates such as diphenylmethane diisocyanate and tolylene diisocyanate, Furthermore, combinations (mixtures) of these materials are also possible. In particular, when durability and heat resistance are important, aromatic polyisocyanates such as diphenylmethane diisocyanate are preferred, and when light resistance is important, aliphatic polyisocyanates such as hexamethylene diisocyanate, dicyclohexylmethane diisocyanate, and isophorone diisocyanate are preferred.
[0082] Furthermore, in the case where the innermost and intermediate layers of the discontinuous resin portion according to this embodiment are made of polyurethane, the chain extender can be, for example, Amine-based chain extenders such as ethylenediamine and methylenebisaniline, Diol-based chain extenders such as ethylene glycol, or Polyamines obtained by reacting polyisocyanate with water, Furthermore, combinations (mixtures) of these can be cited.
[0083] Furthermore, the intermediate layer of the discontinuous resin portion according to this embodiment contains a pigment. By including a pigment in the intermediate layer of the discontinuous resin portion, the artificial leather becomes vividly colored even without the inclusion of dyes, and also exhibits superior lightfastness compared to artificial leather colored with dyes. The innermost and outermost layers of the discontinuous resin portion may also contain a pigment, but it is more preferable that the discontinuous resin portion contains a pigment only in the intermediate layer. This improves the adhesion between the fibrous base material and the innermost layer, and also reduces the amount of pigment exposed from the outermost layer, resulting in an artificial leather with higher abrasion resistance.
[0084] Examples of pigments according to this embodiment include: Phthalocyanine, anthraquinone, quinacridone, dioxazine, isoindolinone, isoindoline, indigo, quinophthalone, diketopyrrolopyrrole, perylene, perinone, and other condensed polycyclic organic pigments. Insoluble azo organic pigments such as benzimidazolone, condensed azo, and azomethine azo. Carbon-based black pigments such as carbon black and graphite, Oxide-based black pigments such as iron tetroxide, copper, and chromium composite oxides, Furthermore, combinations of these can be considered. Among these, carbon black is preferred as the pigment because it is easy to obtain a pigment with a fine particle size and has excellent dispersibility in polymers.
[0085] The average particle size of the pigment according to this embodiment is preferably 0.05 μm or more and 0.20 μm or less. The average particle size of the pigment referred to here is the average particle size when the pigment is present in the discontinuous resin portion, and is generally called the secondary particle size. By having a lower limit of 0.05 μm or more, and more preferably 0.07 μm or more, the pigment is held inside the discontinuous resin portion, so the shedding of the pigment from the discontinuous resin portion is suppressed, resulting in artificial leather with less reduction in lightfastness due to abrasion. Furthermore, by having an upper limit of 0.20 μm or less, more preferably 0.18 μm or less, and even more preferably 0.16 μm or less, the artificial leather has excellent dispersibility when the discontinuous resin portion is applied and has uniform color development.
[0086] In this embodiment, the coefficient of variation (CV) of the particle size of the pigment is preferably 75% or less. The lower limit of the CV is preferably 75% or less, more preferably 60% or less, and even more preferably 50% or less. This reduces the particle size distribution, suppressing the shedding of small particles from the surface of the discontinuous resin portion and the sedimentation of significantly aggregated particles in the resin liquid tank. This results in artificial leather with less change in lightfastness due to abrasion and good lightfastness. While the lower limit of the coefficient of variation in this invention is not particularly limited, it is preferably 0.1% or more from the viewpoint of operability when applying the discontinuous resin portion.
[0087] The average particle size and coefficient of variation (CV) of the pigment according to this embodiment are calculated by the following method. That is, (i) A 10 μm thick test piece is cut from the surface of the artificial leather using an ultramicrotome such as the Sorvall MT6000. (ii) The surface of the discontinuous resin portion in the ultrathin section is observed at 10,000x magnification using a transmission electron microscope (TEM, for example, Hitachi High-Tech Corporation's "H7700"). (iii) Using image analysis software (for example, "WinROOF" manufactured by Mitani Corporation), measure the equivalent circular diameter of the pigment particles contained within a 2.3 μm × 2.3 μm field of view of the observed image at 20 points. If there are fewer than 20 pigment particles contained within a 2.3 μm × 2.3 μm field of view, measure the equivalent circular diameter of all the pigment particles that are present. Measure the area of each of these pigment particles, and use the value obtained by calculating the diameter of the circle corresponding to that area using the following formula as the particle size of the pigment. Particle diameter (μm) = (4 × (Particle area (μm) 2 )) / π) 1 / 2 ···(formula) (iv) Calculate the arithmetic mean (μm) of all measured particle sizes, round it to the third decimal place, and use this as the average particle size (μm) of the pigment. Also, use the value obtained by the following formula as the coefficient of variation (CV) of the particle size of the pigment. Coefficient of variation of particle size (%) = [(Standard deviation of particle size) / (Arithmetic mean of particle size)] × 100 ... (Formula) (outermost layer) In this embodiment, the outermost layer of the discontinuous resin portion refers to the layer furthest from the fibrous base material of the artificial leather.
[0088] Furthermore, the outermost resin of the discontinuous resin portion according to this embodiment is a polycarbonate-based polyurethane. Because of this discontinuous resin portion, when the artificial leather is bent, cracks in the resin layer do not occur, maintaining good quality and texture, and the portion that is not the discontinuous resin portion becomes an artificial leather with sufficient breathability. This polycarbonate-based polyurethane may be either an organic solvent-based polyurethane or a water-dispersible polyurethane. Also, as the polycarbonate-based polyurethane, examples include polyurethanes obtained by the reaction of a polymer diol, an organic diisocyanate, and a chain extender as described above (innermost layer, intermediate layer), where the polymer diol of the polyurethane is the polycarbonate-based diol. The organic diisocyanate and chain extender may be those described above (innermost layer, intermediate layer). Furthermore, similar to the innermost layer and intermediate layer, it may also contain a pigment, in which case it is preferable that the pigment type, average particle size, and coefficient of variation (CV) of the particle size are within the range described above.
[0089] (Discontinuous resin section) The discontinuous resin portion according to this embodiment has the three layers described above. When viewed from the surface of the artificial leather, the outermost layer may cover the end faces of the innermost layer and / or intermediate layer without exposing them (as seen in cross-section, as shown in 23b of Figure 2). The constituent resins of each layer are as described above, but for example, they may also be in the following configurations. • An embodiment in which the constituent resin of the innermost layer, the intermediate layer, and the outermost layer of the discontinuous resin portion are all polycarbonate-based polyurethane. A configuration in which the mass of polyurethane relative to the mass of the discontinuous resin portion is 90% by mass or more and 100% by mass or less.
[0090] In addition, the constituent resins of each layer of the discontinuous resin portion may further contain various additives depending on the purpose, for example, Pigments other than the aforementioned pigments, such as inorganic or oxide-based pigments, Flame retardants such as phosphorus-based, halogen-based, and inorganic types, Antioxidants such as phenols, sulfurs, and phosphorus, UV absorbers such as benzotriazoles, triazines, benzophenones, salicylates, cyanoacrylates, and oxalic acid anilides, Light stabilizers such as hindered amines and benzoates, Hydrolysis-resistant agents such as polycarbodiimide, It may contain plasticizers, antistatic agents, surfactants, and coagulation modifiers.
[0091] Furthermore, in the discontinuous resin portion according to this embodiment, the content ratio of the pigment in the discontinuous resin portion is 0.5% by mass or more and 5.0% by mass or less. By setting the lower limit of the pigment content ratio to preferably 0.5% by mass or more, and more preferably 0.7% by mass or more, an artificial leather with excellent dark color development is obtained. By setting the upper limit of the pigment content ratio to preferably 5.0% by mass or less, and more preferably 4.5% by mass or less, an artificial leather with excellent physical properties and superior mechanical strength is obtained.
[0092] In this invention, the pigment content ratio in the discontinuous resin portion is measured and calculated by the following method. That is, (i) Completely shave off the discontinuous resin portion from the surface of the artificial leather with a razor and measure the mass of the discontinuous resin portion. At this time, at least 1 g or more of the discontinuous resin portion should be shaved off and collected. (ii) The constituent resin of the collected discontinuous resin portion is dissolved using dimethylformamide or the like, the residue is filtered off using a filter or the like, and the mass of the residue is measured to determine the mass of the pigment. (iii) Calculate the pigment content in the discontinuous resin portion using the following formula. The percentage of pigment contained in the discontinuous resin portion (by mass) = (mass of pigment) / (mass of discontinuous resin portion) × 100 ... (formula) Furthermore, with respect to the discontinuous resin portion according to this embodiment, the artificial leather of this embodiment satisfies the following formula 1. 0.35≦D b / D≦0.60 (Formula 1) Here, D is the thickness (μm) of the discontinuous resin portion, and Db is the thickness (μm) of the innermost layer. By satisfying the above formula, the innermost layer can reduce surface irregularities of the fibrous base material, and when the resin layer outside of that resin layer contains pigment, it results in artificial leather with more uniform color development. Furthermore, D shown in formula 1 b Regarding the range of / D, if its lower limit is 0.35 or higher, preferably 0.38 or higher, and more preferably 0.40 or higher, the artificial leather will have more uniform color development. On the other hand, D shown in Formula 1 b Regarding the range of / D, if its upper limit is 0.60 or less, preferably 0.55 or less, and more preferably 0.50 or less, it results in artificial leather with a flexible texture.
[0093] Insofar as the above formula 1 is satisfied, the thickness D (μm) of the discontinuous resin portion according to this embodiment is preferably 5.0 μm or more and 30.0 μm or less. Regarding the range of the thickness D (μm) of the discontinuous resin portion, an upper limit of preferably 30.0 μm or less, more preferably 25.0 μm or less, and even more preferably 20.0 μm or less results in an artificial leather with excellent flexibility. On the other hand, regarding the range of the thickness D (μm) of the discontinuous resin portion, a lower limit of preferably 5.0 μm or more, more preferably 6.0 μm or more, and even more preferably 7.0 μm or more results in an artificial leather with an elegant surface appearance.
[0094] Thickness D of the innermost layer according to this embodiment b The thickness (μm) is preferably between 2.0 μm and 15.0 μm. Innermost layer thickness D b Regarding the range of (μm), the upper limit is preferably 15.0 μm or less, more preferably 3.0 μm or less, and even more preferably 10.0 μm or less, resulting in an artificial leather with excellent flexibility and abrasion resistance. Innermost layer thickness D b Regarding the range of (μm), the lower limit is preferably 2.0 μm or more, more preferably 3.0 μm or more, and even more preferably 4.0 μm or more. This allows for surface smoothing during the application of the intermediate layer containing the pigment, resulting in a uniform resin coating and an artificial leather with uniform color development.
[0095] In this invention, the thickness D (μm) of the discontinuous resin portion and the thickness D of the innermost layer are as follows: b (μm) refers to the thickness measured by observing a cross-section of the obtained artificial leather, cut in the longitudinal or widthwise direction, using a scanning electron microscope (SEM, Keyence Corporation's "VHX-D500 / D510" or a scanning electron microscope with equivalent performance), and measuring the thickness using the scale bar on the screen.
[0096] [Artificial leather] The artificial leather according to this embodiment comprises the fibrous base material and the polymeric elastic body, and has the discontinuous resin portion on at least one surface.
[0097] The artificial leather according to this embodiment either does not contain dye, or contains dye, and the dye content in the artificial leather is 1.0% by mass or less. Here, in the present invention, embodiments in which the content percentage measured and calculated by the method described later is below the detection limit are also included in the "does not contain dye" embodiment. Furthermore, in the present invention, "contains dye" means that the content percentage measured and calculated by the method described later is above the detection limit, and this is the lower limit of the content percentage when dye is included. Generally, the detection limit for the content percentage measured and calculated by the method described later is 0.05% by mass.
[0098] While a form without dyes is most preferable, even when dyes are included, the upper limit of the dye content is preferably 1.0% by mass or less, preferably 0.7% by mass or less, and more preferably 0.5% by mass or less. This reduces the effect of discoloration due to light irradiation on the dye, resulting in artificial leather with excellent lightfastness.
[0099] In this invention, the percentage of dye content in the artificial leather is measured and calculated by the following method. That is, (i) 5 g of artificial leather is immersed in 30 mL of dimethylformamide, etc., and refluxed at a heating temperature of 160°C for 30 minutes to obtain a solution in which the polymeric elastic material and dye are dissolved. (ii) The solution is reprecipitated with 200 mL of methanol to separate it into methanol solution A containing the dissolved dye and a solidified polymeric elastic body. (iii) The solidified polymeric elastic material is dissolved in 20 mL of dimethylformamide, etc., and reprecipitated with 200 mL of methanol to obtain methanol solution B in which the dye is dissolved. (iv) Mix methanol solutions A and B, remove solid matter using a filter or the like, and measure the mass of the residue obtained by vacuum distillation of methanol as the dye. (v) Calculate the percentage of dye content in artificial leather using the following formula. Dye content (by mass) = (Mass of dye) / (Mass of artificial leather) × 100 ... (Formula).
[0100] In this embodiment, it is also preferable that the artificial leather has a napped surface on the side having the discontinuous resin portion. By having a napped surface on the side having the discontinuous resin portion, the discontinuous resin portion can penetrate the fibrous base material appropriately, preventing the discontinuous resin portion from existing in a clump-like state, resulting in an artificial leather with excellent flexibility.
[0101] Furthermore, the embodiment in which a surface having a non-continuous resin portion has a pile can be implemented, for example, by forming a non-continuous resin portion on a surface having a pile, such as a polyurethane-coated sheet as described later.
[0102] [Manufacturing method for artificial leather] The method for manufacturing artificial leather according to this embodiment is: A process for forming a sheet-like material comprising a fibrous base material composed of ultrafine fibers and a polymeric elastic material, The process of forming, on at least one surface of the sheet-like material, in order from the fibrous substrate side, an innermost layer that does not contain pigment, one or more intermediate layers that contain pigment, and an outermost layer that does not contain pigment. It is preferable that the following be included. Artificial leather obtained by such a manufacturing method has lightfastness and abrasion resistance that can withstand outdoor use, and as described later, it can be used in a wide range of applications from furniture, chairs and vehicle interior materials to clothing, but it is particularly suitable for outdoor furniture. The following describes each step of the preferred embodiment in more detail.
[0103] (A) Process of forming a sheet-like material In this process, a sheet-like material is formed comprising a fibrous base material composed of ultrafine fibers and a polymeric elastic material. Specifically, A step (A-1) to form a fibrous substrate composed of ultrafine fiber-generating fibers, The process (A-2) involves applying a polymeric elastic material to this fibrous base material to form a polymeric elastic material-attached sheet, A step (A-3) is to generate ultrafine fibers from ultrafine fiber-generating fibers of a polymer elastic material-attached sheet, and to form a sheet-like material containing a fibrous base material composed of ultrafine fibers and a polymer elastic material, A manner having, or A step (A-1) to form a fibrous substrate composed of ultrafine fiber-generating fibers, The process (A-4) involves generating ultrafine fibers from the ultrafine fiber-generating fibers of this fibrous base material to form an ultrafine fiber sheet composed of ultrafine fibers, The process (A-5) involves applying a polymeric elastic material to this ultrafine fiber sheet to form a polymeric elastic material-attached sheet, thereby forming a sheet-like material containing a fibrous base material composed of ultrafine fibers and a polymeric elastic material. An embodiment having the above is preferred. Each of these will be described in further detail below.
[0104] (A-1) Process for forming a fibrous base material In this process, a fibrous substrate composed of ultrafine fiber-generating fibers is formed.
[0105] First, ultrafine fiber-generating fibers are formed. In this embodiment, it is preferable to use a sea-island type composite fiber in which thermoplastic resins with different solvent solubility are used as a sea portion (easily soluble polymer) and an island portion (poorly soluble polymer), and the sea portion is dissolved and removed using a solvent or the like to form ultrafine fibers in the island portion. By using a sea-island type composite fiber, when the sea portion is removed, appropriate voids can be provided between the island portions, that is, between the ultrafine fibers inside the fiber bundle, making it possible to obtain artificial leather with a better texture.
[0106] As a method for spinning ultrafine fibers having a sea-island type composite structure, a method using a polymer interconnected array that uses a spinneret for sea-island type composite fibers and spins the sea portion and island portion in an interconnected manner is preferred from the viewpoint of obtaining ultrafine fibers with uniform single fiber fineness.
[0107] In this process, when using sea-island type composite fibers, the sea portion may be, for example, Polyethylene, polypropylene, polystyrene, Examples include copolymerized polyesters obtained by copolymerizing sodium sulfoisophthalic acid or polyethylene glycol, and polylactic acid. Among these, polystyrene and copolymerized polyesters are preferred from the viewpoint of spinnability and ease of elution.
[0108] In this process, when using sea-island composite fibers, it is preferable to use sea-island composite fibers in which the tensile strength of the island portion (corresponding to the tensile strength of the ultrafine fiber) is 2.2 cN / dtex or higher. By setting the lower limit of the tensile strength range of the island portion to preferably 2.2 cN / dtex or higher, more preferably 2.5 cN / dtex or higher, and even more preferably 3.0 cN / dtex or higher, it is possible to obtain artificial leather with superior mechanical strength, improve the abrasion resistance of the artificial leather, and suppress the decrease in friction fastness due to fiber shedding.
[0109] In this invention, the tensile strength of the island portion of the sea-island type composite fiber (tensile strength of the ultrafine fiber) is calculated by the following method. That is, (i) Prepare 10 bundles of 20 cm long sea-island type composite fibers, each bundled with 10 fibers. (ii) Of the 10 bundles of sample from (i), the seaweed is dissolved and removed from one bundle, and then air-dried. (iii) The test shall be conducted according to JIS L1013:2010 "Test Methods for Chemical Fiber Filaments," "8.5 Tensile Strength and Elongation," "8.5.1 Standard Time Test," under the conditions of a grip length of 5 cm, a tensile speed of 5 cm / min, and a load of 2 N. (iv) After dissolving and removing the sea portion from the remaining 9 bundles, the same tensile tests are performed, and the arithmetic mean (cN / dtex) of the obtained test results is rounded to two decimal places to obtain the value which is taken as the tensile strength of the island portion of the sea-island type composite fiber and the tensile strength of the ultrafine fibers.
[0110] In this process, the formed ultrafine fiber-generating fibers are used to form a fibrous base material composed of ultrafine fiber-generating fibers. This fibrous base material will be composed of ultrafine fibers through a process described later, and the form of this fibrous base material may be a woven or knitted fabric, a nonwoven fabric, or a combination thereof, for example, an entanglement of a nonwoven fabric and a woven or knitted fabric. Therefore, it is preferable that the fibrous base material composed of ultrafine fiber-generating fibers take the form of a woven or knitted fabric, a nonwoven fabric, or a combination thereof, for example, an entanglement of a nonwoven fabric and a woven or knitted fabric.
[0111] In this embodiment, when a fibrous base material composed of ultrafine fiber-generating fibers is made into a nonwoven fabric, as described above, either a long-fiber nonwoven fabric or a short-fiber nonwoven fabric can be used as the form of the nonwoven fabric, but a short-fiber nonwoven fabric is preferable because it is easier to obtain an artificial leather with excellent flexibility.
[0112] In this process, when a short-fiber nonwoven fabric is used as the nonwoven fabric for a fibrous base material composed of ultrafine fiber-generating fibers, the obtained ultrafine fiber-generating fibers are preferably crimped and cut to a predetermined length to obtain raw fibers, which are then opened, laminated, and entangled to obtain a short-fiber nonwoven fabric. Specifically, the spun ultrafine fiber-generating fibers are opened and then formed into a fiber web using a cross wrapper or the like, and the nonwoven fabric is obtained by entangling them. As a method for entangling the fiber web to obtain a nonwoven fabric, needle punching or water jet punching can be used. In addition, known methods can be used for crimping and cutting.
[0113] Furthermore, in this process, if the fibrous base material composed of ultrafine fiber-generating fibers includes a woven or knitted fabric, it is preferable to use an entangled body of nonwoven fabric and woven or knitted fabric as the fibrous base material. As for methods of entangling and integrating the nonwoven fabric and woven or knitted fabric, Either laminate a woven or knitted fabric onto one or both sides of the nonwoven fabric, or Either sandwich a woven or knitted fabric between multiple fiber webs, After performing one of the above steps, methods such as needle punching or water jet punching are used to entangle the fibers of the nonwoven fabric and the woven or knitted fabric.
[0114] In this process, if a nonwoven fabric is included in the fibrous substrate composed of ultrafine fiber-generating fibers, the apparent density of the nonwoven fabric made of ultrafine fiber-generating fibers after needle punching or water jet punching is set to 0.15 g / cm³. 3 More than 0.45g / cm 3 The following is preferable: The lower limit of the apparent density range of the nonwoven fabric is preferably 0.15 g / cm³. 3 By doing so, artificial leather with sufficient morphological and dimensional stability can be obtained. The upper limit of the apparent density range of the nonwoven fabric is preferably 0.45 g / cm³. 3 By doing the following, it is possible to maintain sufficient space for imparting a polymeric elastic material.
[0115] In this embodiment, the fibrous substrate composed of ultrafine fiber-generating fibers may also be subjected to a heat shrinkage treatment using hot water or steam in order to improve the density of the fibers.
[0116] In this embodiment, a fibrous substrate composed of ultrafine fiber-generating fibers can also be impregnated with a water-soluble resin by impregnating it with an aqueous solution of a water-soluble resin and drying it. By impregnating the nonwoven fabric with a water-soluble resin, the fibers are fixed and dimensional stability is improved.
[0117] (A-2) Process for forming a polymer elastic sheet In this process, a polymeric elastic material is applied to a fibrous substrate composed of the obtained ultrafine fiber-generating fibers to form a polymeric elastic material-attached sheet. Specifically, a fibrous substrate composed of ultrafine fiber-generating fibers is impregnated with a polymeric elastic material solution or emulsion, solidified, and the polymeric elastic material is applied to obtain a polymeric elastic material-attached sheet containing a fibrous substrate composed of ultrafine fiber-generating fibers and a polymeric elastic material.
[0118] In this embodiment, when the main component of the polymeric elastic material is solvent-based polyurethane, N,N-dimethylformamide (DMF) or dimethyl sulfoxide (DMSO) are preferably used as the solvent for the solution of the polymeric elastic material. It is preferable to use a wet coagulation method in which the solvent-based polyurethane is applied to the fibrous substrate by methods such as nipping in the liquid, generating a liquid flow by stirring, or spraying onto a sheet, and the polyurethane is solidified by replacing and removing the solvent in a water bath.
[0119] On the other hand, if the main component of the polymeric elastic material according to this embodiment is water-dispersible polyurethane, a water-dispersible polyurethane liquid may be used, which is obtained by dispersing polyurethane in water to form an emulsion. It is preferable to use dry coagulation, in which the water-dispersible polyurethane liquid is applied to the fibrous substrate by methods such as nipping in the liquid, generating a liquid flow by stirring, or spraying onto a sheet, and then heating to solidify the polyurethane.
[0120] In this case, it is also preferable to include a monovalent cation-containing inorganic salt, such as sodium sulfate, for the purpose of imparting heat-sensitive solidification properties to the water-dispersible polyurethane. Heat-sensitive solidification refers to the property that when the water-dispersible polyurethane liquid is heated, the fluidity of the water-dispersible polyurethane liquid decreases and the polyurethane solidifies when it reaches a certain temperature (heat-sensitive solidification temperature). By imparting heat-sensitive solidification properties, it is possible to suppress the phenomenon of migration, where moisture migrates to the sheet surface as it evaporates.
[0121] Furthermore, to improve color development, a polymeric elastic material containing a black pigment can be fixed to a fibrous substrate. One method for this is to impregnate a nonwoven fabric (fibrous substrate) with a solution of the polymeric elastic material containing the black pigment, followed by wet or dry coagulation. These methods can be appropriately selected depending on the type of polymeric elastic material used. Preferably, the black pigment used has a primary particle diameter number average of 0.01 μm or more and 0.05 μm or less, and a coefficient of variation (CV) of the primary particle diameter of the black pigment of 0.1% or more and 30% or less. By using a black pigment with a primary particle diameter within the above range, the particle diameter (secondary particle diameter) of the black pigment contained in the polymeric elastic material and the coefficient of variation (CV) of the particle diameter of the black pigment contained in the polymeric elastic material can be set to an appropriate range.
[0122] (A-3) Process for forming a sheet-like material In this process, ultrafine fibers are generated from ultrafine fiber-generating fibers of a polymer elastic material-attached sheet to form a sheet-like material containing a fibrous base material composed of ultrafine fibers and a polymer elastic material. Specifically, the polymer elastic material-attached sheet is immersed in a solvent or the like, and if sea-island type composite fibers are used, the sea portion is dissolved and removed to generate ultrafine fibers.
[0123] In the case of the ultrafine fiber-generating fiber according to this embodiment being a sea-island type composite fiber, if the sea portion is polyethylene, polypropylene, or polystyrene, an organic solvent such as toluene or trichloroethylene can be used as the solvent to dissolve and remove the sea portion. On the other hand, if the sea portion is copolymerized polyester or polylactic acid, an alkaline aqueous solution such as sodium hydroxide can be used. Furthermore, if the sea portion is a water-soluble thermoplastic polyvinyl alcohol-based resin, hot water (here meaning water at 80°C to 100°C) can be used.
[0124] (A-4) Process for forming an ultrafine fiber sheet This process involves generating ultrafine fibers from the ultrafine fiber-generating fibers of a fibrous substrate, which is made up of ultrafine fiber-generating fibers obtained in process (A-1), to form an ultrafine fiber sheet composed of ultrafine fibers. This is the same as process (A-3), except that instead of the polymer elastic sheet obtained in process (A-2), the fibrous substrate made up of ultrafine fiber-generating fibers obtained in process (A-1) is immersed in a solvent, etc., and if sea-island type composite fibers were used, the sea portion is dissolved and removed to generate ultrafine fibers and form an ultrafine fiber sheet.
[0125] (A-5) Process for forming a sheet-like material This process involves applying a polymeric elastic material to the ultrafine fiber sheet obtained in step (A-4) to form a polymeric elastic material-attached sheet, thereby forming a sheet-like material containing a fibrous base material composed of ultrafine fibers and a polymeric elastic material. This is the same as step (A-2), except that instead of using the fibrous base material composed of ultrafine fiber-generating fibers obtained in step (A-1), the ultrafine fiber sheet obtained in step (A-4) is impregnated with a polymeric elastic material solution or emulsion, solidified, and then a sheet-like material containing a fibrous base material composed of ultrafine fibers and a polymeric elastic material is obtained.
[0126] (A-6) Other post-processing steps Before forming the discontinuous resin portion on the sheet material obtained in step (A-3) or step (A-5), the surface of the sheet material on which the discontinuous resin portion will be formed may be smoothed. To smooth the surface of the sheet material, methods such as physically pressing the surface of the sheet material or pressing while heating with a hot roll or steam can be used. When pressing the surface of the sheet material using a hot roll or steam, the temperature is preferably 40°C to 200°C. By setting the lower limit of the temperature range when pressing to preferably 40°C or higher, more preferably 45°C or higher, and even more preferably 50°C or higher, the surface of the sheet material can be maintained in a smoother state even after time has passed since pressing. On the other hand, by setting the upper limit of the temperature range when pressing to preferably 200°C or lower, more preferably 190°C or lower, and even more preferably 180°C or lower, the thermal decomposition of the components of the sheet material can be further suppressed, and consequently, artificial leather with better mechanical properties can be obtained.
[0127] Furthermore, it is preferable to grind the surface of the sheet-like material and apply a napping treatment before the process of forming the discontinuous resin portion described later. By applying the napping treatment, the resin of the discontinuous resin portion penetrates the sheet-like material appropriately, resulting in an artificial leather with excellent abrasion resistance and flexibility.
[0128] The napping process can be performed by grinding using sandpaper or a roll sander. The napping process can be applied to one side of the sheet material or to both sides. When performing the napping process, a silicone-based lubricant such as a silicone emulsion can be applied to the surface of the sheet material before napping to improve the release properties of the polymer elastic material and ultrafine fibers during the formation of the nap, to disperse the ultrafine fibers, and to form a uniform nap layer. In addition, applying an antistatic agent before napping can suppress the accumulation of grinding dust generated from the sheet material on the sandpaper.
[0129] Furthermore, prior to this grinding, it is also preferable to cut the sheet material in half in the thickness direction to obtain two thin sheets.
[0130] Furthermore, it is preferable to subject the sheet-like material to a heat shrinkage treatment using a liquid jet staining machine or the like to improve the surface density.
[0131] (B) Process for forming a discontinuous resin section In this process, on at least one surface of the sheet-like material (of course, the sheet-like material that has undergone the process described in (A-6) above is also included in the sheet-like material of this process), a pigment-free innermost layer, one or more pigment-containing intermediate layers, and a pigment-free outermost layer are formed in order from the fibrous substrate side. In this way, the discontinuous resin portion can be formed. Of course, the discontinuous resin portion may be formed on one surface of the sheet-like material, or on both surfaces.
[0132] In this process, the method for forming the innermost layer, intermediate layer, and outermost layer is not particularly limited as long as it allows for the discontinuous application of resin to the surface of the sheet-like material, but for example, Methods that involve applying resin using screen methods such as flat screens and rotary screens, or gravure coating methods, followed by drying to form each layer. Methods include forming a discontinuous resin film on a support substrate such as release paper, applying an adhesive to the surface of the resin film, bonding it to the surface of the sheet-like material, and then peeling off the release paper to form each layer, as well as combinations thereof.
[0133] In particular, when the main components of the innermost layer, intermediate layer, and outermost layer in this process are solvent-based polyurethane, and when using one of the above manufacturing methods, such as the screen method or gravure coating method, N,N-dimethylformamide, dimethyl sulfoxide, toluene, methyl ethyl ketone, ethyl acetate, acetone, or combinations thereof can be used as the solvent for the solvent-based polyurethane.
[0134] On the other hand, in this process, when the main components of the innermost layer, intermediate layer, and outermost layer are water-dispersible polyurethane, and when using one of the above manufacturing methods, such as the screen method or the gravure coating method, a water-dispersible polyurethane liquid, which is obtained by dispersing polyurethane in water to form an emulsion, may be used.
[0135] The amount of coating applied to each layer of the discontinuous resin section can be appropriately selected according to the desired purpose and pattern. In particular, when creating a semi-grain-like artificial leather that achieves both lightfastness and abrasion resistance suitable for outdoor use, and has uniform color development, it is preferable to set the amount of coating applied to each layer within the following range. • Innermost layer: 5.0g / m² 2 More than 15.0g / m 2 below ·Middle layer: 5.0g / m 2 More than 15.0g / m 2 below ·Outermost layer: 1.0g / m 2 More than 10.0g / m 2 below For example, if there are two intermediate layers, the total coating amount for the intermediate layers is twice the above range, which is 10.0 g / m². 2 More than 30.0g / m 2 The following is preferable. Furthermore, "coating amount" here refers to the mass per unit area of the remaining resin after the solvent used for coating has been removed. These points will be explained in more detail below.
[0136] First, the innermost and middle layers were coated at a rate of 5.0 g / m² each. 2 More than 15.0g / m 2 The following is preferable. The innermost layer can also be described as a layer that can bond the sheet-like material (fibrous base material) and the intermediate layer. The upper limit of the coating amount for the innermost layer is preferably 15.0 g / m². 2 More preferably, 14.0 g / m² 2 More preferably, 13.0 g / m² 2 By doing the following, a highly flexible artificial leather can be obtained. On the other hand, regarding the range of coating amount for the innermost layer, the lower limit is preferably 5.0 g / m².2 More preferably 6.0 g / m 2 More preferably 7.0 g / m² 2 By doing so, the artificial leather surface exhibits a resinous feel and texture, resulting in an artificial leather with an elegant surface appearance. Furthermore, the intermediate layer can be described as a layer that smooths the surface of the sheet-like material to which the innermost layer is applied, enabling the formation of a uniform outermost layer. Therefore, the intermediate layer can also be described as a layer that brings out the gloss and flexible texture of the artificial leather surface. The amount of the intermediate layer applied is 5.0 g / m². 2 More than 15.0g / m 2 The following is preferable: The upper limit of the application amount for the intermediate layer is preferably 15.0 g / m². 2 More preferably, 14.0 g / m² 2 More preferably, 13.0 g / m² 2 The following measures result in a highly flexible artificial leather. On the other hand, the lower limit of the application amount for the intermediate layer is preferably 5.0 g / m². 2 More preferably 6.0 g / m 2 More preferably 7.0 g / m² 2 By doing so, the artificial leather surface exhibits a resinous feel and texture, resulting in an artificial leather with an elegant surface appearance. Note that the amount of resin applied to the innermost and intermediate layers may be the same or different for each layer.
[0137] Furthermore, regarding the amount of discontinuous resin applied, the outermost layer is 1.0 g / m². 2 More than 10.0g / m 2 The following is preferable. The outermost resin layer can also be said to be a layer that can maintain the abrasion resistance of the artificial leather surface. The upper limit of the coating amount for the outermost layer is preferably 10.0 g / m². 2 More preferably, 9.0 g / m 2 More preferably, 7.0 g / m 2 By doing the following, a highly flexible artificial leather can be obtained. On the other hand, the lower limit of the coating amount for the outermost layer is preferably 1.0 g / m². 2 More preferably 2.0 g / m 2 More preferably 3.0 g / m 2By doing so, it is possible to obtain artificial leather with excellent abrasion resistance.
[0138] Therefore, the total coating amount of the discontinuous resin section is 11.0 g / m². 2 More than 40.0g / m 2 The following is preferable: The upper limit of the total coating amount for the discontinuous resin portion is preferably 40.0 g / m². 2 More preferably, 37.0 g / m² 2 More preferably, 33.0 g / m² 2 By following the instructions below, a highly flexible artificial leather can be obtained. The lower limit of the total coating amount for the discontinuous resin portion is preferably 11.0 g / m². 2 More preferably, 14.0 g / m² 2 More preferably 17.0 g / m² 2 By doing so, it is possible to obtain artificial leather that exhibits a resinous feel and surface texture on the surface, resulting in an artificial leather with an elegant surface appearance.
[0139] In this process, when forming each layer of the discontinuous resin portion, it is preferable to dry the resin after each layer is applied. Furthermore, it is preferable that the drying temperature after application be between 70°C and 180°C. By setting the upper limit of the drying temperature range after application to preferably 180°C or lower, more preferably 170°C or lower, and even more preferably 160°C or lower, thermal decomposition of the resin can be suppressed, resulting in artificial leather with excellent mechanical strength and an elegant surface appearance. On the other hand, by setting the lower limit of the drying temperature range after application to preferably 70°C or higher, more preferably 75°C or higher, and even more preferably 80°C or higher, the resin can be dried efficiently.
[0140] Furthermore, in the drying process described above, it is preferable that the drying time after application be between 10 seconds and 10 minutes. By setting the upper limit of the drying time after application to preferably 10 minutes or less, more preferably 8 minutes or less, and even more preferably 5 minutes or less, thermal decomposition of the resin can be suppressed, resulting in artificial leather with excellent mechanical strength and an elegant surface appearance. On the other hand, by setting the lower limit of the drying time after application to preferably 10 seconds or more, more preferably 30 seconds or more, and even more preferably 1 minute or more, the resin can be sufficiently dried.
[0141] (C) Other post-processing steps The artificial leather according to this embodiment can be further processed, to the extent that it does not impair the effects of the present invention. Of course, in this invention, the artificial leather obtained by performing this post-processing step is also considered to be the artificial leather according to the present invention. The artificial leather according to this embodiment can be given decorative features on its surface as needed. For example, post-processing treatments such as perforation, embossing, laser processing, pin sonic processing, and printing can be applied.
[0142] [Uses of artificial leather] The artificial leather according to this embodiment has excellent lightfastness and abrasion resistance, making it suitable for a wide range of applications, including furniture, clothing, general merchandise, shoes and bags, vehicle interior materials, seats, and more.
[0143] Among these, furniture containing the aforementioned artificial leather is particularly preferable because it can take advantage of its excellent lightfastness and abrasion resistance. Note that the term "furniture" as used herein does not include seats, which will be discussed later. Examples of such furniture include beds, mattresses, cushions, tables, carpets, cabinets, and television stands. It is even more preferable that at least a portion of these surface materials, for example, parts that the user can directly come into contact with or parts that are visible to the user, are made of the aforementioned artificial leather.
[0144] Furthermore, seats containing the aforementioned artificial leather are also preferable because they can take advantage of its particularly excellent lightfastness. In such seats, it is even more preferable that at least a part of the surface material of the headrest, seat, armrest, footrest, etc., for example, the part that comes into direct contact with the occupant, is made of the aforementioned artificial leather. Of course, the seats of the present invention can be used not only for vehicles such as automobiles, aircraft, railway cars, and ships, but also for seats in homes, offices, and shops. Note that the term "seat" as used in the present invention includes chairs, benches, sofas, couches, stools, and floor chairs.
[0145] Alternatively, clothing containing the aforementioned artificial leather is also preferable because it can take advantage of its excellent lightfastness and abrasion resistance. Examples of such clothing include: T-shirts, polo shirts, dress shirts, blouses, wrap tops, cut-and-sew tops, sweaters, vests, hoodies, sweatshirts, turtlenecks, cardigans, tank tops, tube tops, and other tops. Outerwear such as coats, blazers, jackets, windbreakers, cloaks, capes, aprons, and cloaks, Trousers such as slacks, jeans, and shorts, Skirts, cocktail dresses, one-piece dresses, gowns and other dresses, Clothing such as ceremonial robes, suits, uniforms, underwear, shoe uppers and trims, hats, bags, scarves, ties, wallets and other accessories, or, This includes clothing materials and accessories such as interlinings and pockets, as well as linings for the aforementioned clothing items.
[0146] Furthermore, vehicle interior materials including the aforementioned artificial leather are preferable because they can take advantage of their excellent lightfastness and abrasion resistance. Note that the term "vehicle interior material" as used herein does not include the seats mentioned above. Examples of such vehicle interior materials include floor carpets, floor mats, ceiling linings, and surface materials for vehicle parts such as steering wheels, horn switches, shift knobs, dashboards, instrument panels, glove boxes, sun visors, and assist grips. In this invention, "vehicle" includes automobiles, aircraft, railway vehicles, ships, as well as other vehicles such as carriages, palanquins, and rickshaws, and also certain industrial, construction, and agricultural machinery capable of carrying people or animals, such as excavators, cranes, tractors, and combine harvesters.
[0147] For these applications, embodiments comprising a laminate including the artificial leather and a backing material are also preferred. Examples of the backing material include woven fabrics, knitted fabrics, nonwoven fabrics, foamed resin sheets, and combinations thereof.
[0148] First, examples of the aforementioned textiles include plain weave, twill weave, satin weave, and various textiles based on these weaving structures.
[0149] Furthermore, knitted fabrics include warp knitting, weft knitting represented by tricot knitting, lace knitting, and various knitted fabrics based on these knitting structures.
[0150] Examples of resins that are the main components of fibers constituting woven or knitted fabrics include polyester resins, polyamide resins, acrylic resins, cellulose resins, polyolefin resins, silicone resins, or various copolymers containing these components, or mixtures thereof, or resins that form natural fibers such as cotton and wool. Hereinafter, in the present invention, the "main component" of fibers constituting woven or knitted fabrics means that the mass of the component is 50% by mass or more of the total mass of the fibers.
[0151] Examples of nonwoven fabrics include needle-punched nonwoven fabrics, papermaking nonwoven fabrics, spunbond nonwoven fabrics, meltblown nonwoven fabrics, spunlace nonwoven fabrics, air-through nonwoven fabrics, chemical bond nonwoven fabrics, flash-spun nonwoven fabrics, and nonwoven fabrics that combine these. Examples of resins that are the main components of the fibers constituting the nonwoven fabric include polyester resins, polyamide resins, acrylic resins, cellulose resins, polyolefin resins, silicone resins, or various copolymers containing these components, or mixtures thereof, or resins that form natural fibers such as cotton and wool. Here, in the present invention, the "main component" of the fibers constituting the nonwoven fabric means that the mass of the component is 50% by mass or more of the total mass of the fibers.
[0152] Furthermore, examples of the foamed resin sheet include a resin with internal bubbles molded into a sheet, or a resin sheet with a foaming agent encapsulated within it and then foamed. Examples of the resin for the foamed resin sheet include polyolefin resins, polyurethane resins, polyester resins, polyamide resins, polyphenylene sulfide resins, polycarbonate resins, polyetherketone resins, polyetherimide resins, etc., or various copolymers containing these components, or mixtures thereof. [Examples]
[0153] Next, the artificial leather of the present invention will be described in more detail using examples, but the present invention is not limited to these examples.
[0154] [Evaluation Method] The evaluation methods and measurement conditions used in the examples are described below. Unless otherwise specified, the measurements and calculations for each physical property were performed based on the methods described above.
[0155] (1) Average single fiber diameter of ultrafine fibers (μm): The average single fiber diameter of the ultrafine fibers was measured and calculated using a scanning electron microscope (SEM) manufactured by Keyence Corporation, specifically the "VHX-D500 / D510," based on the method described above.
[0156] (2) Average single fiber diameter (μm) of the single filament of the multifilament of the woven fabric, and the number of twists (T / m) of the multifilament: The average single fiber diameter and twist count of the multifilament single yarns of the woven fabric were measured and calculated using a scanning electron microscope (SEM) manufactured by Keyence Corporation, specifically the "VHX-D500 / D510," based on the method described above.
[0157] (3) Average particle size (μm) and coefficient of variation (%) of particle size of black pigment in polymeric elastic material: The average particle size and coefficient of variation of particle size of black pigment in polymeric elastic materials were measured and calculated using the above method, employing a Sorvall MT6000 ultramicrotome, a Hitachi High-Tech H7700 transmission electron microscope (TEM), and WinROOF image analysis software from Mitani Corporation.
[0158] (4) Percentage of polymeric elastic material content relative to fibrous base material (mass%): The proportion of polymeric elastic material in the fibrous substrate was measured and calculated based on the definition and method described above.
[0159] (5) Average particle size (μm) of black pigment in the innermost, intermediate, and outermost layers, and coefficient of variation (%) of particle size: The average particle size and coefficient of variation of the black pigment in the innermost, intermediate, and outermost layers were measured and calculated using the methods described above, with a Sorvall MT6000 ultramicrotome, a Hitachi High-Tech H7700 transmission electron microscope (TEM), and WinROOF image analysis software from Mitani Corporation.
[0160] (6) Thickness D of the innermost layer b(μm), Thickness D of the discontinuous resin section (μm): Thickness D of the innermost layer b The thickness of the discontinuous resin section was measured and calculated using a scanning electron microscope (SEM) manufactured by Keyence Corporation, specifically the "VHX-D500 / D510," based on the method described above.
[0161] (7) Dye content in artificial leather (mass %): The proportion of dyes in the artificial leather was measured and calculated based on the method described above.
[0162] (8) Lightfastness (grade): Lightfastness was evaluated according to JIS L0843:2006 "Test Method for Color Fastness to Xenon Arc Light" "4. Test Type": Method B (High Temperature Method), in accordance with "7.2 Exposure Method" "c) Third Exposure Method". The size of the test specimen was 6.5 cm × 5.5 cm, and a Suga Test Instruments Co., Ltd. "NX25 / X25A" lightfastness tester using a xenon arc light source was used, with a black panel temperature of 89°C ± 3°C, and the test specimen was processed according to the standard. In this invention, a good level is Grade 4 or higher.
[0163] (9) Abrasion resistance [Wear loss after lightfastness test] (mg): As an evaluation of abrasion resistance, an abrasion resistance test was conducted on artificial leather after irradiation with xenon arc light under conditions in which a Grade 4 blue scale faded to its standard state in the lightfastness test described in (8). The evaluation was carried out as follows. (i)(8) In the lightfastness test, a circular specimen with a diameter of 3.8 cm was taken from a test specimen after irradiation with xenon arc light under conditions that caused standard fading of a Grade 4 blue scale, and its mass was measured. In the present invention, a good level was defined as a wear loss of 15 mg or less. (ii) In accordance with "8.19.5 Method E (Martindale method)" of JIS L1096:2020 "Test methods for woven and knitted fabrics", the surface with discontinuous resin parts was used as the friction surface under a pressing load (12 kPa) for "furniture, carpets, etc.", and this surface was set to the pilling position (THREE DRIVE ROLLERS = POSITION B) of the Martindale abrasion tester to perform an abrasion resistance test. (iii) The testing machine was stopped after 20,000 friction cycles, and the difference in mass of the test specimen before and after the test was evaluated.
[0164] (10) Uniformity of color development: The artificial leather was evaluated by 11 individuals skilled in sensory evaluation. The following evaluations were visually judged, and the level with the most votes was designated as the surface condition. In the event of a tie for the most votes for a particular level, the sensory evaluation was limited to the tied level, and the 11 participants were re-evaluated. This process was repeated until the final evaluation was determined. In this invention, a good level was designated as "A or B". A: Even upon close inspection, no color unevenness can be observed on the surface of the artificial leather, indicating uniform color development. B: While slight color variations can be observed on the artificial leather surface upon close inspection, the overall color development is uniform. C: Uneven coloring can be observed on the surface of the artificial leather, indicating uneven color development. D: Significant color unevenness can be observed on the surface of the artificial leather, and the color development is very inconsistent. Furthermore, the quantitative evaluation of the uniformity of color development was performed as follows. (i) JIS Z8781-4:2013 “Colorimetry-Part 4: CIE1976L * a * b * L, defined in the "color space" * value, a * value, b * The values were measured using a Konica Minolta CR-310 spectrophotometer. (ii) The measurement result of (i) is used as the standard color, and five L values different from the measurement location of the standard color are measured within the same fabric. * value, a *value, b * value was measured, and in accordance with JIS Z8781-4:2013 "Color measurement - Part 4: CIE 1976 L * a * b * color space", the ΔE with the standard color as specified in "3.12 CIE 1976 CIELAB 1976 L * a * b * color difference" was calculated, and the maximum value was defined as ΔE * ab . * abMax Incidentally, in the present invention, a favorable level is defined as ΔE * abMax < 1.0.
[0165] [Resins and the like used] For the resins and the like used in Examples and Comparative Examples, the following materials were used. Hereinafter, the abbreviations defined at the beginning are used, including those in Table 1 to Table 4. CB1: Carbon black with an average particle diameter of 0.09 μm and a coefficient of variation (CV) of particle diameter of 50%. CB2: Carbon black with an average particle diameter of 0.08 μm and a coefficient of variation (CV) of particle diameter of 20%. O-PCPU: Polycarbonate-based polyurethane, which is an organic solvent-based polyurethane. O-PEPU: Polyester-based polyurethane, which is an organic solvent-based polyurethane. O-PXPU: Polyether / polyester-based polyurethane, which is an organic solvent-based polyurethane (a polyurethane whose polymer diol is a copolymer obtained by combining a polyether-based diol and a polyester-based diol). PCB: Phthalocyanine blue with an average particle diameter of 0.12 μm and a coefficient of variation (CV) of particle diameter of 50%. PET: Polyethylene terephthalate with an intrinsic viscosity of 0.73. PVA: Polyvinyl alcohol with a saponification degree of 88%.
[0166] [Example 1] <Step (A-1) of forming fibrous base material> Using polystyrene as the sea component and PET as the island component, melt spinning was performed using a sea-island composite spinneret with 16 islands per hole under conditions of a spinning temperature of 285°C and an island / sea mass ratio of 80 / 20. Subsequently, the resulting fiber was drawn to 2.8 times its original length in an oil solution bath, then cut to a length of 51 mm, and passed through a carding machine and a cross-lapper process to form a laminated fiber web.
[0167] Then, the following plain woven fabric was prepared. Warp and weft yarns: · Component constituting the filament: PET · Average single filament diameter of the filament: 11.0 μm · Number of filaments contained in the multifilament (filament count): 72 · Twist count of the multifilament: 2500 T / m Weave density: · Warp direction: 95 ends / 2.54 cm · Weft direction: 76 picks / 2.54 cm This plain woven fabric was laminated on both sides of the aforementioned laminated fiber web, and needle-punched at a punch density of 3500 punches / cm 2 to form a fibrous base material composed of ultra-fine fiber developable fibers, having a basis weight of 700 g / m 2 and a thickness of 3.0 mm.
[0168] <Step (A-4) of forming an ultra-fine fiber sheet> After subjecting the aforementioned fibrous base material to a shrinkage treatment with hot water at a temperature of 96°C, it was impregnated with a 5 mass% concentration PVA aqueous solution and squeezed with a roll. Then, this was dried with hot air at a temperature of 120°C for 10 minutes to obtain a PVA-attached sheet in which the PVA mass relative to the mass of the fibrous base material composed of ultra-fine fiber developable fibers was 7.5 mass%. The PVA-attached sheet thus obtained was immersed in trichloroethylene, and subjected to 10 cycles of liquid squeezing and compression using a mangle, thereby dissolving and removing the sea component and performing compression treatment on the PVA-attached sheet, to form an ultra-fine fiber sheet containing a fibrous base material composed of developed ultra-fine fibers.
[0169] <Step (A-5) of forming a sheet-like article> The ultrafine fiber sheet was immersed in a DMF solution of CB1 and O-PCPU prepared to a solid content concentration of 11.3% (prepared such that CB1 accounted for 1.5 mass% relative to polyurethane). Thereafter, this was squeezed with rolls, then immersed in an aqueous solution with a DMF concentration of 30 mass% to coagulate the polyurethane. Subsequently, PVA and DMF were removed with hot water, followed by drying with hot air at 110°C for 10 minutes, to form a sheet-like material having a thickness of 2.2 mm and a polyurethane mass of 27 mass% relative to the mass of the fibrous base material.
[0170] <Other post-processing step (A-6)> The sheet-like material was cut in half perpendicularly to the thickness direction, and the surface formed by the half-cut (half-cut surface) was ground by 0.25 mm with an endless sandpaper of sandpaper grit No. 180 to form a napped surface, with the thickness adjusted to 0.85 mm. This was subjected to a shrinkage treatment using a jet dyeing machine at a liquid temperature of 125°C, and then dried with a dryer.
[0171] <Step (B) for forming discontinuous resin portion> A toluene solution of O-PCPU (containing no pigment) prepared to a solid content concentration of 30 mass% was applied onto the napped surface of the sheet-like material by a gravure coating method, and dried with hot air at a temperature of 80°C for 3 minutes, to give an application amount of 7.8 g / m 2 of the innermost layer was formed.
[0172] Next, one layer of a toluene solution of CB2 and O-PCPU (prepared such that CB2 accounted for 3.0 mass% relative to the total solid content in the toluene solution) prepared to a solid content concentration of 30 mass% was applied from above the innermost layer by a gravure coating method, and dried with hot air at a temperature of 80°C for 3 minutes, to give an application amount of 7.1 g / m 2 of the intermediate layer was formed.
[0173] Thereafter, a toluene solution of O-PCPU (containing no pigment) prepared to a solid content concentration of 30 mass% was applied from above the intermediate layer by a gravure coating method, and dried with hot air at a temperature of 80°C for 3 minutes, to give an application amount of 4.0 g / m 2The outermost layer was formed, and artificial leather was obtained. The results are shown in Table 1.
[0174] [Example 2] In the process (B) of forming a discontinuous resin section, The innermost polyurethane layer is made of O-PEPU, and the application amount is 8.9 g / m². 2 to, The amount of the intermediate layer to be applied is 7.2 g / m². 2 to, The outermost layer should be coated at 3.8 g / m². 2 to, Artificial leather was obtained in the same manner as in Example 1, except for the changes made. The results are shown in Table 1.
[0175] [Example 3] In the process (B) of forming a discontinuous resin section, The amount of coating applied to the innermost layer is 10.4 g / m². 2 to, The formation of the intermediate layer is as follows: The amount of resin applied to the outermost layer is 3.7 g / m². 2 to, Artificial leather was obtained in the same manner as in Example 1, except for the changes made. The results are shown in Table 1. (Formation of the intermediate layer) A toluene solution of CB2 and O-PCPU, prepared to a solid content concentration of 30% by mass (CB2 was adjusted to 3.0% by mass relative to the total solid content in the toluene solution), was applied as a single layer by gravure coating from the innermost layer and dried with hot air at 80°C for 3 minutes. Then, another layer of the same toluene solution was applied on top and dried with hot air at 80°C for 3 minutes, resulting in a coating amount of 13.6 g / m². 2 It formed an intermediate layer (consisting of two layers).
[0176] [Example 4] In the process (B) of forming a discontinuous resin section, The innermost polyurethane layer is made of O-PEPU, and the application amount is 8.2 g / m². 2 to, The intermediate polyurethane layer is made of O-PEPU, and the application amount is 7.8 g / m². 2 to, The outermost layer should be coated at 3.7 g / m².2 to, An artificial leather was obtained in the same manner as in Example 1 except for the change. The results are shown in Table 1.
[0177] [Example 5] In the step (A-5) of forming the sheet-like material, the DMF solution was changed to a DMF solution of O-PXPU (containing no CB1) adjusted to a solid content concentration of 11.3%, In the step (B) of forming the discontinuous resin portion, The coating amount of the innermost layer was set to 8.0 g / m 2 to, The coating amount of the intermediate layer was set to 7.1 g / m 2 to, The coating amount of the outermost layer was set to 4.2 g / m 2 to, An artificial leather was obtained in the same manner as in Example 1 except for the change. The results are shown in Table 1.
[0178] [Example 6] An artificial leather was obtained in the same manner as in Example 1 except that the step (B) of forming the discontinuous resin portion was changed as follows. The results are shown in Table 2. (Step (B) of forming the discontinuous resin portion) A toluene solution of O-PCPU (adjusted such that CB2 accounts for 2.0 mass% of the total solid content in the toluene solution) adjusted to a solid content concentration of 30 mass% was applied to the napped surface of the sheet-like material by a gravure coating method, and dried with hot air at a temperature of 80°C for 3 minutes, to give a coating amount of 8.4 g / m 2 to form the innermost layer.
[0179] Next, a toluene solution of CB2 and O-PCPU (adjusted such that CB2 accounts for 2.0 mass% of the total solid content in the toluene solution) adjusted to a solid content concentration of 30 mass% was applied as one layer from above the innermost layer by a gravure coating method, and dried with hot air at a temperature of 80°C for 3 minutes, to give a coating amount of 7.2 g / m 2 to form the intermediate layer.
[0180] Subsequently, a toluene solution of CB2 and O-PCPU (adjusted to have CB2 at 1.5% by mass relative to the total solid content in the toluene solution), prepared to a solid content concentration of 30% by mass, was applied to the intermediate layer using a gravure coating method. The mixture was then dried with hot air at 80°C for 3 minutes, resulting in a coating amount of 4.3 g / m². 2 It formed the outermost layer.
[0181] [Example 7] In the other post-processing steps (A-6), when shrinking treatment is performed using a liquid flow dyeing machine, the process is modified to also include adding black dye to the artificial leather in an amount of 0.9% by mass relative to its mass. In the process (B) of forming a discontinuous resin section, The amount of coating applied to the innermost layer is 8.2 g / m². 2 to, The formation of the intermediate layer is as follows: The outermost layer coating amount is 4.1 g / m². 2 to, Artificial leather was obtained in the same manner as in Example 1, except for the changes made. The results are shown in Table 2. (Formation of the intermediate layer) A toluene solution of PCB and O-PCPU (adjusted so that PCB accounts for 3.0% by mass relative to the total solid content in the toluene solution), prepared to a solid content concentration of 30% by mass, was applied as a single layer using gravure coating from the innermost layer. The mixture was then dried with hot air at 80°C for 3 minutes, resulting in a coating amount of 6.9 g / m². 2 It formed an intermediate layer.
[0182] [Example 8] In the process (B) of forming a discontinuous resin section, The formation of the innermost layer is as follows: The amount of the intermediate layer to be applied is 6.8 g / m². 2 to, The outermost layer coating amount is 3.6 g / m². 2 to, Artificial leather was obtained in the same manner as in Example 1, except for the changes made. The results are shown in Table 2. (Formation of the innermost layer) A toluene solution of O-PCPU (without pigment), prepared to a solid content concentration of 45% by mass, was applied in a single layer to the pile surface of the aforementioned sheet-like material by gravure coating, and dried with hot air at 80°C for 5 minutes, resulting in a coating amount of 14.0 g / m². 2 It formed the innermost layer.
[0183] [Example 9] In the process (B) of forming a discontinuous resin section, The amount of coating applied to the innermost layer is 7.9 g / m². 2 to, The formation of the intermediate layer is as follows: The outermost layer coating amount is 4.4 g / m². 2 to, Artificial leather was obtained in the same manner as in Example 1, except for the changes made. The results are shown in Table 2. (Formation of the intermediate layer) A toluene solution of CB2 and O-PCPU (adjusted so that CB2 accounts for 1.5% by mass relative to the total solid content in the toluene solution), prepared to a solid content concentration of 30% by mass, was applied as a single layer by gravure coating from the innermost layer. The mixture was then dried with hot air at 80°C for 3 minutes, resulting in a coating amount of 7.7 g / m². 2 It formed an intermediate layer.
[0184] [Example 10] In the process (B) of forming a discontinuous resin section, The amount of coating applied to the innermost layer is 8.1 g / m². 2 to, The formation of the intermediate layer is as follows: The outermost layer should be coated at 3.9 g / m². 2 to, Artificial leather was obtained in the same manner as in Example 1, except for the changes made. The results are shown in Table 2. (Formation of the intermediate layer) A toluene solution of CB2 and O-PCPU, prepared to a solid content concentration of 30% by mass (CB2 was adjusted to 12.0% by mass relative to the total solid content in the toluene solution), was applied as a single layer using gravure coating from the innermost layer. The mixture was then dried with hot air at 80°C for 3 minutes, resulting in a coating amount of 7.6 g / m². 2 It formed an intermediate layer.
[0185] [Comparative Example 1] In the process (B) of forming a discontinuous resin section, The amount of coating applied to the innermost layer is 8.1 g / m². 2 to, The formation of the intermediate layer is as follows: The outermost layer coating amount is 4.4 g / m². 2 to, Artificial leather was obtained in the same manner as in Example 1, except for the changes made. The results are shown in Table 3. (Formation of the intermediate layer) A toluene solution of O-PCPU (without pigment), prepared to a solid content concentration of 30% by mass, was applied as a single layer using gravure coating from the innermost layer, and dried with hot air at 80°C for 3 minutes, resulting in a coating amount of 7.2 g / m². 2 It formed an intermediate layer.
[0186] [Comparative Example 2] In the process (B) of forming a discontinuous resin section, The amount of coating applied to the innermost layer is 8.1 g / m². 2 to, The amount of the intermediate layer to be applied is 7.0 g / m². 2 to, The formation of the outermost layer is as follows: Artificial leather was obtained in the same manner as in Example 1, except for the changes made. The results are shown in Table 3. (Formation of the outermost layer) A toluene solution of O-PEPU (without pigment), prepared to a solid content concentration of 30% by mass, was applied as a single layer using gravure coating over the intermediate layer, and dried with hot air at 80°C for 3 minutes, resulting in a coating amount of 5.2 g / m². 2 It formed the outermost layer.
[0187] [Comparative Example 3] In the process (B) of forming a discontinuous resin section, The amount of coating applied to the innermost layer is 7.8 g / m². 2 to, The formation of the intermediate layer is as follows: The outermost layer should be coated at 3.9 g / m². 2 to, Artificial leather was obtained in the same manner as in Example 1, except for the changes made. The results are shown in Table 3. (Formation of the intermediate layer) A toluene solution of O-PCPU (adjusted so that CB2 accounts for 1.0% by mass relative to the total solid content in the toluene solution), prepared to a solid content concentration of 30% by mass, was applied as a single layer by gravure coating from the innermost layer. The mixture was then dried with hot air at 80°C for 3 minutes, resulting in a coating amount of 6.7 g / m². 2 It formed an intermediate layer.
[0188] [Comparative Example 4] In the process (B) of forming a discontinuous resin section, The amount of coating applied to the innermost layer is 8.0 g / m². 2 to, The formation of the intermediate layer is as follows: The outermost layer should be coated at 3.7 g / m². 2 to, Artificial leather was obtained in the same manner as in Example 1, except for the changes made. The results are shown in Table 3. (Formation of the intermediate layer) A toluene solution of O-PCPU (adjusted so that CB2 accounts for 15.0% by mass of the total solids in the toluene solution), prepared to a solid content concentration of 30% by mass, was applied as a single layer by gravure coating from the innermost layer. The mixture was then dried with hot air at 80°C for 3 minutes, resulting in a coating amount of 7.5 g / m². 2 It formed an intermediate layer.
[0189] [Comparative Example 5] In the process (B) of forming a discontinuous resin section, The amount of coating applied to the innermost layer is 5.5 g / m². 2 to, The amount of the intermediate layer to be applied is 8.2 g / m². 2 to, The outermost layer should be coated at 5.2 g / m². 2 to, Artificial leather was obtained in the same manner as in Example 1, except for the changes made. The results are shown in Table 4.
[0190] [Comparative Example 6] In the process (B) of forming a discontinuous resin section, The formation of the innermost layer is as follows: The amount of the intermediate layer to be applied is 7.0 g / m². 2to, The outermost layer should be coated at 3.7 g / m². 2 to, Artificial leather was obtained in the same manner as in Example 1, except for the changes made. The results are shown in Table 4. (Formation of the innermost layer) A toluene solution of O-PCPU (without pigment), prepared to a solid content concentration of 45% by mass, was applied in a single layer to the pile surface of the aforementioned sheet-like material by gravure coating, and dried with hot air at 80°C for 5 minutes, resulting in a coating amount of 18.1 g / m². 2 It formed the innermost layer.
[0191] [Comparative Example 7] In the other post-processing steps (A-6), when shrinking treatment is performed using a liquid flow dyeing machine, the process is modified to also include adding black dye to the artificial leather in an amount of 1.5% by mass relative to its mass. In the process (B) of forming a discontinuous resin section, The amount of coating applied to the innermost layer is 8.0 g / m². 2 to, The amount of the intermediate layer to be applied is 7.2 g / m². 2 to, The outermost layer coating amount is 4.4 g / m². 2 to, Artificial leather was obtained in the same manner as in Example 1, except for the changes made. The results are shown in Table 4.
[0192] [Comparative Example 8] In the process (B) of forming a discontinuous resin section, The amount of coating applied to the innermost layer is 7.7 g / m². 2 to, The amount of the intermediate layer to be applied is 6.9 g / m². 2 And make this the outermost layer, By not applying the outermost layer, Artificial leather was obtained in the same manner as in Example 1, except for the changes made. The results are shown in Table 4.
[0193] [Comparative Example 9] In the process (B) of forming a discontinuous resin section, By not applying the innermost layer, The amount of the intermediate layer to be applied is 7.0 g / m². 2 And make this the innermost layer, The outermost layer coating amount is 4.1 g / m². 2 to, Artificial leather was obtained in the same manner as in Example 1, except for the changes made. The results are shown in Table 4.
[0194] [Table 1]
[0195] [Table 2]
[0196] [Table 3]
[0197] [Table 4]
[0198] As shown in Tables 1 and 2, the artificial leathers of Examples 1 to 10 had a lightfastness of grade 5 or higher, a uniformity of color development of grade B or higher, and abrasion loss of 15 mg or less after the lightfastness test. This indicates that it was possible to obtain semi-grain-like artificial leather that is suitable for outdoor use, has both lightfastness and abrasion resistance, and uniform color development. In particular, the artificial leather of Example 1 is a more preferable form because it has high levels of lightfastness, uniformity of color development, and abrasion resistance after the lightfastness test.
[0199] On the other hand, as shown in Tables 3 and 4, the artificial leathers of Comparative Examples 1 to 9 satisfy at least one of the following conditions: lightfastness of grade 3 or lower, uniformity of color development of grade C or lower, and abrasion loss of 20 mg or more after the lightfastness test. Therefore, they cannot be said to be semi-grain artificial leathers that have both lightfastness and abrasion resistance suitable for outdoor use, as well as uniform color development. [Explanation of symbols]
[0200] 11: Multifilament 12: One twisted section 13: Fiber direction of multifilaments 14: One end 14a: Intersection of perpendiculars 15: The other end 15a: Intersection of perpendiculars 16: Distance L T 21a, 21b: Artificial leather 22: Fibrous base material 23a, 23b: Discrete resin section 231: Innermost layer 232: Mesopotamia 233: Outermost layer
Claims
1. Artificial leather comprising a fibrous base material containing ultrafine fibers and a polymeric elastic material, The aforementioned artificial leather is The artificial leather has a discontinuous resin portion on at least one surface, The artificial leather does not contain dye, or it contains dye, and the proportion of dye in the artificial leather is 1.0% by mass or less. The discontinuous resin portion is arranged in order from the fibrous substrate side, Innermost layer, One or more intermediate layers, outermost layer It has at least three layers, The outermost layer is made of polycarbonate-based polyurethane. The aforementioned intermediate layer contains a pigment, The content ratio of the pigment in the discontinuous resin portion is 0.5% by mass or more and 5.0% by mass or less. Furthermore, artificial leather that satisfies the following equation 1. 0.35≦D b / D≦0.60 ・・・(Equation 1) Here, D is the thickness (μm) of the discontinuous resin portion, b This is the thickness (μm) of the innermost layer.
2. Furthermore, the artificial leather according to claim 1, wherein the constituent resin of the intermediate layer or the constituent resin of the innermost layer is a polycarbonate-based polyurethane.
3. The artificial leather according to claim 1, wherein the constituent resin of the intermediate layer and the constituent resin of the innermost layer of the discontinuous resin portion are polycarbonate-based polyurethane.
4. The artificial leather according to any one of claims 1 to 3, wherein the pigment is carbon black.
5. The artificial leather according to any one of claims 1 to 3, wherein the average particle size of the pigment is 0.05 μm or more and 0.20 μm or less.
6. The artificial leather according to any one of claims 1 to 3, wherein the polymeric elastic body is a polycarbonate-based polyurethane.
7. The artificial leather according to any one of claims 1 to 3, wherein the polymeric elastic body contains a black pigment.
8. The artificial leather according to claim 7, wherein the proportion of the black pigment contained in the polymeric elastic material is 0.1% by mass or more and 5.0% by mass or less.
9. The artificial leather according to claim 7, wherein the average particle size of the black pigment contained in the polymer elastic material is 0.05 μm or more and 0.20 μm or less.
10. A method for producing artificial leather according to any one of claims 1 to 3, A process for forming a sheet-like material comprising a fibrous base material composed of ultrafine fibers and a polymeric elastic material, The process of forming, on at least one surface of the sheet-like material, in order from the fibrous substrate side, an innermost layer that does not contain pigment, one or more intermediate layers that contain pigment, and an outermost layer that does not contain pigment. A method for manufacturing artificial leather, including [the specified component].
11. Furniture comprising artificial leather as described in any one of claims 1 to 3.
12. A seat comprising artificial leather according to any one of claims 1 to 3.
13. Clothing comprising artificial leather as described in any one of claims 1 to 3.
14. A vehicle interior material comprising artificial leather according to any one of claims 1 to 3.
Citation Information
Patent Citations
Leather-like fabric
JP2018123437A
Sheet material
JP2019065450A
Napped artificial leather and manufacturing method therefor
WO2021131591A1